Electrophotographic receptor, process cartridge, and electrophotographic device

A polymer with specific structural units in the electron transport layer addresses electron transport deficiencies in conventional photoreceptors, improving electron mobility and reducing image defects like pattern memory and ghosts for high-speed printing.

JP2024152031APending Publication Date: 2024-10-25CANON KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023065931
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Conventional electrophotographic photoreceptors suffer from image defects such as pattern memory and ghosts during large-volume and high-speed printing due to insufficient electron transport ability and non-uniform film states caused by high concentrations of perylene imide structures.

Method used

The use of a polymer with specific structural units represented by formulas (1), (2), or (3) in the electron transport layer, having a glass transition temperature between -10°C and 50°C, to minimize stacking and promote uniform orientation of perylene imide structures, enhancing electron mobility and reducing trap sites.

Benefits of technology

This approach effectively suppresses pattern memory and ghosts, enabling high-sensitivity and durable electrophotographic photoreceptors suitable for large-scale and high-speed printing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152031000034
    Figure 2024152031000034
  • Figure 2024152031000035
    Figure 2024152031000035
  • Figure 2024152031000036
    Figure 2024152031000036
Patent Text Reader

Abstract

To provide an electrophotographic receptor capable of suppressing the occurrence of pattern memory and a ghost.SOLUTION: An electrophotographic receptor includes a support, an electron transport layer, a charge generation layer, and a hole transport layer in this order. The electron transport layer includes a polymer having a specific structural unit. The polymer has a glass transition temperature Tg of -10°C or more and 50°C or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrophotographic photoreceptor, and a process cartridge and an electrophotographic apparatus each having the electrophotographic photoreceptor. [Background technology]

[0002] In electrophotographic photoreceptors used in electrophotographic processes, a technique is known in which an undercoat layer containing an electron transport material is provided between the support and the photosensitive layer in order to suppress charge injection from the support side to the photosensitive layer side and to suppress the occurrence of image defects such as black spots. Patent Document 1 describes an electron transport layer containing a copolymer having a repeating unit including a structure having electron transport properties, and Patent Document 2 describes a resin having a repeating unit including a structure having electron transport properties. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2010-198014 A [Patent Document 2] JP 2003-345044 A Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, there has been a demand for large-volume and high-speed printing in electrophotographic processes. According to the study by the present inventors, it has been found that when large-volume and high-speed printing is performed with the electrophotographic photoreceptors described in Patent Documents 1 and 2, image defects called pattern memory and image defects called ghosts may occur.

[0005] Pattern memory is the following phenomenon. For example, after a large number of images 301 including vertical lines 306 shown in FIG. 1(a) are output continuously, a solid black image 302 shown in FIG. 1(b) is output. In this case, the output solid black image produces an image 304 including vertical lines 307 as shown in FIG. 1(c) due to the vertical lines 306 included in the image 301 shown in FIG. 1(a) being repeatedly recorded. Also, after a large number of images 301 shown in FIG. 1(a) are output continuously, a halftone image 303 shown in FIG. 1(d) is output. In this case, as in the case of outputting the solid black image 302 shown in FIG. 1(b), an image 305 including vertical lines 308 as shown in FIG. 1(e) is produced due to the vertical lines 306 included in the image 301 shown in FIG. 1(a) being repeatedly recorded.

[0006] A ghost is a phenomenon as follows. For example, as shown in Fig. 2(a), an image having a black background (black image) 52 in a white background (white image) 51 at the beginning of the image is output, followed by a halftone image 53 with a one-dot knight pattern as shown in Fig. 2(b). At this time, a ghost is a phenomenon in which a part with a different image density from the surroundings is generated in the halftone image 53 of the image shown in Fig. 2(a), as shown by ghost part 54. Therefore, an object of the present invention is to provide an electrophotographic photoreceptor capable of suppressing the occurrence of pattern memory and ghosts, a method for manufacturing the electrophotographic photoreceptor, a process cartridge having the electrophotographic photoreceptor, and an electrophotographic apparatus having the electrophotographic photoreceptor. [Means for solving the problem]

[0007] The above object can be achieved by the present invention, which is described below. That is, the electrophotographic photoreceptor according to the present invention is an electrophotographic photoreceptor having a support, an electron transport layer, a charge generating layer, and a hole transport layer in this order, characterized in that the electron transport layer contains a polymer having a structural unit represented by the following formula (1), (2), or (3), and the glass transition temperature Tg of the polymer is from -10°C to 50°C. [ka] [ka] [ka] (In formula (1), R 11 , R 12 , R 13 , R 14 , R 15 , R 16 , R 17 , and R 18 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, R 61 represents a hydrogen atom or a substituted or unsubstituted alkyl group, m 1 indicates an integer between 2 and 16.) (In formula (2), R 22 , R 23 , R 24 , R 26 , R 27 , and R 28 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, R 62 represents a hydrogen atom or a substituted or unsubstituted alkyl group, R 41 and R 42 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, m 2 indicates an integer between 2 and 16.) (In formula (3), R 31, R 33 , R 34 , R 35 , R 37 , and R 38 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, R 63 represents a hydrogen atom or a substituted or unsubstituted alkyl group, R 51 and R 52 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, m 3 indicates an integer between 2 and 16.) Effect of the Invention

[0008] According to the present invention, it is possible to provide an electrophotographic photoreceptor capable of suppressing the occurrence of pattern memory and ghosts, a method for manufacturing the electrophotographic photoreceptor, a process cartridge having the electrophotographic photoreceptor, and an electrophotographic apparatus having the electrophotographic photoreceptor. [Brief description of the drawings]

[0009] [Figure 1] FIG. 13 is a diagram showing an example of an image for explaining a pattern memory. [Diagram 2] FIG. 13 is a diagram showing an example of an image for explaining a ghost. [Diagram 3] FIG. 2 is a diagram showing an example of a layer structure of an electrophotographic photoreceptor according to the present invention. [Figure 4] 1 is a diagram showing an example of a schematic configuration of an electrophotographic apparatus provided with a process cartridge having an electrophotographic photosensitive member according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below with reference to preferred embodiments. In the case of large-volume and high-speed printing, when a conventional electrophotographic photoreceptor is used, image defects called pattern memory and image defects called ghosts may occur. The following are considered to be the causes of such defects. Electrophotographic photoreceptors are required to have high sensitivity and high durability in order to handle large-volume and high-speed printing, and therefore, charge generating substances having higher sensitivity are used as the charge generating substances contained in electrophotographic photoreceptors. As the sensitivity of the charge-generating material increases, the amount of charge generated increases. However, conventional electrophotographic photoreceptors do not have sufficient electron transport capacity, and it is believed that when a large number of identical images are output in a short period of time, charge tends to accumulate in exposed areas of the photosensitive layer.

[0011] The present inventors have investigated the use of highly π-conjugated perylene imide for the purpose of increasing the mobility of electrons in order to suppress pattern memory and ghosts. However, there are cases where the mobility of electrons is not increased sufficiently by merely forming a film containing a high concentration of perylene imide. Since perylene imide has a rigid planar structure, it is easy to stack. Therefore, when the content ratio of perylene imide as an electron transport material is high, stacks due to the planar structure of perylene are significantly likely to be formed. Therefore, the present inventors speculate that the film state becomes non-uniform, which is a factor that hinders the improvement of the electron mobility of the film as a whole. Therefore, we tried to make it difficult for the perylene imide structure to stack by making the perylene imide into a polymer with a repeating structural unit containing the perylene imide structure. However, we found that there were cases where the increase in electron mobility was only limited, and cases where the electron mobility was improved and the pattern memory was improved, but the suppression of ghosting was insufficient.

[0012] While the pattern memory is improved, the suppression of ghosts is insufficient. The inventors have hypothesized that this may be due to differences in the state of existence of the perylene imide structure, which contributes to electron transfer, in the film. As a result of further investigation, the inventors have found that when the above-mentioned polymer has a specific structural unit described below and is a polymer having a glass transition temperature Tg of -10°C or more and 50°C or less, both pattern memory and ghost can be improved.

[0013] The reasons why both pattern memory and ghosting can be improved by using the above polymer are considered to be as follows. First, it is considered that stacking of the perylene imide structure portion can be minimized by polymerization, and the formation of a non-uniform film state can be suppressed. In addition, the inventors speculate that in a uniform film state, the glass transition temperature Tg of the above polymer is low, which makes it easier for the perylene imide to assume a moderately oriented state, thereby reducing trap sites.

[0014] As a result of the above mechanism, even when the concentration of perylene imide is increased, the molecules do not stack and can be spaced apart from each other at an appropriate distance, thereby fully achieving the effect of increasing the concentration and thereby suppressing pattern memory and ghosting. Specifically, the present inventors have discovered an electrophotographic photoreceptor characterized in having an electron transport layer containing a polymer having a structural unit represented by the below-mentioned formula (1), formula (2) or formula (3) and having a glass transition temperature Tg of −10° C. or more and 50° C. or less.

[0015] The configuration of the electrophotographic photoreceptor according to the present invention will be described in detail below. [Electrophotographic photoreceptor] 3 is a diagram showing an example of the layer structure of the electrophotographic photoreceptor according to the present invention, which has a support 101, an electron transport layer 102, a charge generation layer 103, and a hole transport layer 104 in this order. The method for producing the electrophotographic photoreceptor according to the present invention includes a method in which the coating liquid for each layer described below is prepared, coated in the desired order, and dried. In this case, the coating liquid can be applied by dip coating, spray coating, inkjet coating, roll coating, die coating, blade coating, curtain coating, wire bar coating, ring coating, etc. Among these, dip coating is preferred from the viewpoint of efficiency and productivity. The support and each layer will be described below.

[0016] <Support> In the present invention, the electrophotographic photoreceptor has a support. In the present invention, the support is preferably a conductive support having electrical conductivity. The shape of the support may be a cylinder, a belt, a sheet, or the like. Among them, a cylindrical support is preferable. The surface of the support may be subjected to electrochemical treatment such as anodization, blasting, cutting, or the like. The support is preferably made of a metal, a resin, or a glass. Examples of the metal include aluminum, iron, nickel, copper, gold, stainless steel, and alloys thereof. Among them, an aluminum support using aluminum is preferable. Furthermore, the resin or glass may be made conductive by a process such as mixing with or coating with a conductive material.

[0017] <Conductive layer> In the present invention, a conductive layer may be provided on the support. By providing the conductive layer, scratches and irregularities on the surface of the support can be concealed and light reflection on the surface of the support can be controlled. The conductive layer preferably contains conductive particles and a resin. The conductive particles may be made of a material such as metal oxide, metal, or carbon black. Examples of metal oxides include zinc oxide, aluminum oxide, indium oxide, silicon oxide, zirconium oxide, tin oxide, titanium oxide, magnesium oxide, antimony oxide, bismuth oxide, etc. Examples of metals include aluminum, nickel, iron, nichrome, copper, zinc, silver, etc. Among these, it is preferable to use metal oxides as the conductive particles, and it is particularly preferable to use titanium oxide, tin oxide, or zinc oxide. When a metal oxide is used as the conductive particles, the surface of the metal oxide may be treated with a silane coupling agent or the like, or the metal oxide may be doped with an element such as phosphorus or aluminum or an oxide thereof. The conductive particles may have a laminated structure having a core particle and a coating layer that covers the core particle. Examples of the core particle include titanium oxide, barium sulfate, zinc oxide, etc. Examples of the coating layer include metal oxides such as tin oxide. When a metal oxide is used as the conductive particles, the volume average particle size is preferably 1 nm or more and 500 nm or less, and more preferably 3 nm or more and 400 nm or less. Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, acrylic resin, silicone resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, and alkyd resin. The conductive layer may further contain silicone oil, resin particles, a masking agent such as titanium oxide, and the like. The thickness of the conductive layer is preferably from 1 μm to 50 μm, and particularly preferably from 3 μm to 40 μm. The conductive layer can be formed by preparing a coating solution for the conductive layer containing the above-mentioned materials and solvent, forming a coating film of this, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Examples of the dispersion method for dispersing the conductive particles in the coating solution for the conductive layer include a method using a paint shaker, a sand mill, a ball mill, and a liquid collision type high-speed disperser.

[0018] <Electron transport layer> The electrophotographic photoreceptor according to the present invention has an electron transport layer on a support or a conductive layer.

[0019] The electron transport layer contains a polymer having a structural unit represented by the following formula (1), (2), or (3), and the glass transition temperature Tg of the polymer is from -10°C to 50°C. [ka] [ka] [ka] (In formula (1), R 11 , R 12 , R 13 , R 14 , R 15 , R 16 , R 17 , and R 18 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, R 61 represents a hydrogen atom or a substituted or unsubstituted alkyl group, m 1 indicates an integer between 2 and 16.) (In formula (2), R 22 , R 23 , R 24 , R 26 , R 27 , and R 28each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, R 62 represents a hydrogen atom or a substituted or unsubstituted alkyl group, R 41 and R 42 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, m 2 indicates an integer between 2 and 16.) (In formula (3), R 31 , R 33 , R 34 , R 35 , R 37 , and R 38 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, R 63 represents a hydrogen atom or a substituted or unsubstituted alkyl group, R 51 and R 52 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, m 3 indicates an integer between 2 and 16.)

[0020] In the structural unit represented by formula (1), the structural unit represented by formula (2), and the structural unit represented by formula (3), examples of the substituent that the substituted alkyl group has include an aryl group, a halogen atom, a nitro group, a cyano group, an amino group, and an alkoxy group. Examples of the substituent on the substituted aryl group include a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, an alkyl group, a halogen-substituted alkyl group, an alkoxy group, a hydroxy group, and a carboxyalkyl group. Examples of the substituent on the substituted alkoxy group include a halogen atom, an aryl group, a nitro group, a cyano group, a trifluoromethyl group, an alkyl group, a halogen-substituted alkyl group, and an alkoxy group. Examples of the substituent that the substituted thiol group has include a halogen atom, an aryl group, a nitro group, a cyano group, a trifluoromethyl group, an alkyl group, a halogen-substituted alkyl group, and an alkoxy group. Examples of the substituent on the substituted amino group include a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, an alkyl group, a halogen-substituted alkyl group, and an alkoxy group. Examples of the substituent on the substituted alkynyl group include a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, an alkyl group, a halogen-substituted alkyl group, and an alkoxy group.

[0021] In the structural unit represented by formula (1), the structural unit represented by formula (2), and the structural unit represented by formula (3), specific examples of the substituted or unsubstituted alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, a cyclopentyl group, an n-hexyl group, a 1-methyl group, a 2-methyl ... Examples of groups that can be used include aryl pentyl group, 4-methyl-2-pentyl group, 3,3-dimethylbutyl group, 2-ethylbutyl group, cyclohexyl group, hexyl group, isohexyl group, heptyl group, octyl group, nonyl group, decyl group, undecyl group, dodecyl group, tridecyl group, tetradecyl group, hexadecyl group, heptadecyl group, octadecyl group, nonadecyl group, icosyl group, henicosyl group, triacontyl group, benzyl group, and trityl group. Specific examples of the substituted or unsubstituted alkynyl group include an ethynyl group, a propynyl group, a butynyl group, a pentynyl group, a hexynyl group, a heptynyl group, and an octynyl group. Specific examples of the substituted or unsubstituted aryl group include a phenyl group, a biphenyl group, a fluorenyl group, a 1-naphthyl group, a 2-naphthyl group, and a tolyl group. Specific examples of the substituted or unsubstituted alkoxy group include a methoxy group, an ethoxy group, a propoxy group, a tert-butoxy group, a phenoxy group, a pentyloxy group, a cyclohexyloxy group, a benzyloxy group, an allyloxy group, and a 1-naphthyloxy group. Specific examples of the substituted or unsubstituted thiol group include a thiol group (sulfanyl group), a methylthio group, an ethylthio group, a propylthio group, a butylthio group, a pentylthio group, a hexylthio group, a heptylthio group, an octylthio group, and a phenylthio group. Specific examples of the substituted or unsubstituted amino group include an amino group, a methylamino group, a dimethylamino group, a trimethylamino group, an ethylamino group, a diethylamino group, a propylamino group, an isopropylamino group, a butylamino group, a pentylamino group, a hexylamino group, a heptylamino group, an octylamino group, a phenylamino group, and a pyrrolidinyl group.

[0022] The m in formula (1) can be selected because the concentration of the perylene imide structure can be increased and pattern memory can be more effectively suppressed. 1 , m in Eq. (2) 2 , and m in formula (3) 3 It is preferable that represents an integer of 2 or more and 6 or less.

[0023] m in formula (1) 1 , m in Eq. (2) 2 , and m in formula (3) 3 When the value is 6 or less, the concentration of the perylene imide structure portion can be increased, and pattern memory can be effectively suppressed.

[0024] In addition, the perylene imide structure is easily oriented in a uniform manner, so that R 61 , R in Eq. (2) 62 , and R in formula (3) 63 preferably represents a methyl group.

[0025] Specific examples of the structural unit represented by the formula (1), the structural unit represented by the formula (2), and the structural unit represented by the formula (3) are shown in Tables 1 to 4 below.

[0026] [Table 1]

[0027] [Table 2]

[0028] [Table 3]

[0029] [Table 4]

[0030] The weight average molecular weight of the polymer having the structural unit represented by formula (1), formula (2) or formula (3) is preferably 30,000 or less. When the average molecular weight of the polymer is 30,000 or less, the perylene imide structure is likely to assume an appropriate orientation state, and ghosts can be more effectively suppressed.

[0031] The glass transition temperature Tg of the polymer having a structural unit represented by formula (1), formula (2) or formula (3) was measured under the following conditions. The glass transition temperature Tg described in this application is the temperature at the intersection of the tangent of the temperature range before the inflection point and the tangent of the temperature range after the inflection point in the endothermic peak that appears during the second heating to 200°C under the following temperature conditions.

[0032] [Glass transition temperature measurement] Measuring device used: X-DSC7000 manufactured by Hitachi High-Tech Science Corporation Temperature conditions: Temperature drop from 25℃ to -50℃ at 10℃ / min -50℃ for 5 minutes -50℃ to 200℃ at 10℃ / min Maintain at 200℃ for 10 minutes Temperature drop from 200℃ to -50℃ at 50℃ / min -50℃ for 10 minutes -50℃ to 200℃ at 10℃ / min Sample size: approx. 2mg Measurement environment: N2 airflow

[0033] Table 5 shows specific examples of polymers having a structural unit represented by formula (1), (2), or (3), their weight average molecular weights, and their glass transition temperatures Tg.

[0034] [Table 5]

[0035] In order for the perylene imide structure of the above polymer to be in an appropriate orientation state that can obtain the effects of the present invention, it is preferable that the CuKα characteristic X-ray diffraction pattern obtained for the electron transport layer has a peak at 2θ=7.5°±2.5° (θ is the Bragg angle).

[0036] The X-ray diffraction measurements were carried out under the following conditions. (X-ray diffraction measurement) Measuring equipment used: Rigaku Electric Co., Ltd., X-ray diffraction device RINT-TTRII X-ray tube:Cu X-ray wavelength: Kα1 Tube voltage: 50KV Tube current: 300mA Scan method: θ scan Scan speed: 4.0° / min Sampling interval: 0.02° Start angle 2θ: 3.0° Stop angle 2θ: 35.0° Goniometer: Rotor horizontal goniometer (TTR-2) Attachment: Capillary rotating sample stage Filter: None Detector: Scintillation counter Incident Monochrome: Use Slit: Variable slit (parallel beam method) Counter monochromator: Not used Divergence slit: open Divergence vertical limit slit: 10.00mm Scattering slit: open Receiving slit: open

[0037] The coating liquid for the electron transport layer may contain a crosslinking agent in addition to the polymer having a structural unit represented by formula (1), formula (2), or formula (3) and having a glass transition temperature Tg of −10° C. or more and 50° C. or less.

[0038] As the crosslinking agent, any known material can be used, specifically, the compounds described in "Crosslinking Agent Handbook" edited by Shinzo Yamashita and Tosuke Kaneko, published by Taiseisha (1981) can be mentioned. In the present invention, the crosslinking agent is preferably an isocyanate compound having an isocyanate group or a blocked isocyanate group, or an amine compound having an N-methylol group or an alkyl-etherified N-methylol group. An isocyanate compound having 2 to 6 isocyanate groups or blocked isocyanate groups is preferred. Examples of the isocyanate compound as the crosslinking agent include the isocyanate compounds shown below, but the present invention is not limited thereto. In addition, the isocyanate compounds shown below may be used in combination. Examples of the isocyanate compound include isocyanurate modified products, biuret modified products, allophanate modified products, and adduct modified products with trimethylolpropane or pentaerythritol of diisocyanates such as triisocyanate benzene, triisocyanate methylbenzene, triphenylmethane triisocyanate, lysine triisocyanate, tolylene diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, naphthalene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, xylylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, methyl-2,6-diisocyanate hexanoate, and norbornane diisocyanate. The blocked isocyanate group is -NHCOX 1 (X 1 X is a protecting group). 1 may be any protecting group that can be introduced into an isocyanate group.

[0039] Examples of commercially available isocyanate compounds include isocyanate-based crosslinking agents such as Duranate MFK-60B, SBA-70B, 17B-60P, SBN-70D, and SBB-70P manufactured by Asahi Kasei Corporation, and Desmodur BL3175 and BL3475 manufactured by Sumika Bayer Urethane Co., Ltd.

[0040] The amine compound as the crosslinking agent preferably has an N-methylol group or an alkyl-etherified N-methylol group.More preferably, the amine compound has a plurality (two or more) of N-methylol groups or alkyl-etherified N-methylol groups.Examples of the amine compound include methylolated melamine, methylolated guanamine, methylolated urea derivatives, methylolated ethylene urea derivatives, methylolated glycoluril, and compounds in which the methylol moiety is alkyl-etherified, and derivatives thereof.

[0041] Examples of commercially available amine compounds (crosslinking agents) include Super Melami No. 90 (manufactured by NOF Corp. (formerly Nippon Oil & Fats)), Super Bekkamin® TD-139-60, L-105-60, L127-60, L110-60, J-820-60, and G-821-60 (manufactured by DIC Corp.), U-Ban 2020 (Mitsui Chemicals), Sumitex Resin M-3 (manufactured by Sumitomo Chemical Co., Ltd. (formerly Sumitomo Chemical Co., Ltd.)), and Ni Examples of such compounds include Karac MW-30, MW-390, and MX-750LM (manufactured by Sanwa Chemical Co., Ltd.), Super Beckamin(R) L-148-55, 13-535, L-145-60, and TD-126 (manufactured by DIC Corporation), Nikalac BL-60 and BX-4000 (manufactured by Sanwa Chemical Co., Ltd.), Nikalac MX-280, Nikalac MX-270, and Nikalac MX-290 (manufactured by Sanwa Chemical Co., Ltd.).

[0042] In the present invention, the content of the polymer having the structural unit represented by formula (1), formula (2) or formula (3) relative to the total mass of the electron transport layer is preferably 50% by mass or more from the viewpoint of improving the mobility of electrons in the electron transport layer. Moreover, the content of the polymer having the structural unit represented by formula (1), formula (2) or formula (3) relative to the total mass of the electron transport layer is more preferably 70% by mass or more.

[0043] The electron transport layer may contain a resin. Alternatively, the electron transport layer may be formed as a cured film by polymerizing a composition containing a monomer having a polymerizable functional group. Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, acrylic resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, polyvinyl phenol resin, alkyd resin, polyvinyl alcohol resin, polyethylene oxide resin, polypropylene oxide resin, polyamide resin, polyamic acid resin, polyimide resin, polyamideimide resin, and cellulose resin. Examples of the polymerizable functional group contained in the monomer having a polymerizable functional group include an isocyanate group, a blocked isocyanate group, a methylol group, an alkylated methylol group, an epoxy group, a metal alkoxy group, a hydroxy group, an amino group, a carboxy group, a thiol group, a carboxylic anhydride group, and a carbon-carbon double bond group.

[0044] For the purpose of improving electrical properties, the electron transport layer may further contain metal oxide particles, metal particles, conductive polymers, etc. Among these, it is preferable to use metal oxide particles. Metal oxide particles include particles of indium tin oxide, tin oxide, indium oxide, titanium oxide, strontium titanate, zinc oxide, aluminum oxide, etc. Silicon dioxide particles can also be used. Metal particles include particles of gold, silver, aluminum, etc. The metal oxide particles contained in the electron transport layer may be surface-treated with a surface treatment agent such as a silane coupling agent.

[0045] The surface treatment of the metal oxide particles can be carried out by a common method, such as a dry method or a wet method. In the dry method, metal oxide particles are stirred in a mixer capable of high-speed stirring, such as a Henschel mixer, while an alcohol aqueous solution, an organic solvent solution, or an aqueous solution containing a surface treatment agent is added to the metal oxide particles to uniformly disperse them, and then the particles are dried. In the wet method, the metal oxide particles and the surface treatment agent are stirred in a solvent or dispersed in a sand mill using glass beads or the like, and the solvent is removed by filtration or distillation under reduced pressure. After the solvent is removed, it is preferable to further bake the mixture at 100° C. or higher.

[0046] The electron transport layer may further contain additives, for example, known materials such as metal particles such as aluminum particles, conductive particles such as carbon black, hole transport substances, metal chelate compounds, and organometallic compounds.

[0047] The thickness of the electron transport layer is preferably from 0.1 μm to 10 μm, and more preferably from 0.5 μm to 5 μm. The electron transport layer has a function of suppressing charge injection from the support or the conductive layer, so the volume resistivity of the electron transport layer is 1×10 10 It is preferable that the resistance is Ω·cm or more, and 1×10 12 It is more preferable that the resistivity is Ω·cm or more.

[0048] The electron transport layer can be formed by preparing a coating solution for the electron transport layer containing the above-mentioned materials and solvent, forming a coating film, and drying and / or curing the coating solution. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Examples of the dispersion method for preparing the coating solution for the electron transport layer include a method using a homogenizer, an ultrasonic disperser, a ball mill, a sand mill, a roll mill, a vibration mill, an attritor, or a liquid collision type high-speed disperser. The temperature at which the coating film of the coating liquid for the electron transport layer is dried by heating is preferably 100 to 200°C.

[0049] <Charge generation layer> The charge generating layer preferably contains a charge generating material and a resin. Examples of the charge generating material include azo pigments, perylene pigments, polycyclic quinone pigments, indigo pigments, and phthalocyanine pigments. Among these, azo pigments and phthalocyanine pigments are preferred. Among phthalocyanine pigments, oxytitanium phthalocyanine pigments, chlorogallium phthalocyanine pigments, and hydroxygallium phthalocyanine pigments are preferred. The content of the charge generating material in the charge generating layer is preferably from 40% by mass to 85% by mass, and more preferably from 60% by mass to 80% by mass, based on the total mass of the charge generating layer. Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, polyvinyl butyral resin, acrylic resin, silicone resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, polyvinyl alcohol resin, cellulose resin, polystyrene resin, polyvinyl acetate resin, polyvinyl chloride resin, etc. Among these, polyvinyl butyral resin is more preferable. The charge generating layer may further contain additives such as an antioxidant and an ultraviolet absorbing agent, etc. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, and benzophenone compounds. The thickness of the charge generating layer is preferably from 0.1 μm to 1 μm, and more preferably from 0.15 μm to 0.4 μm. The charge generating layer can be formed by preparing a coating solution for the charge generating layer containing the above-mentioned materials and solvent, forming a coating film of this, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.

[0050] <Hole transport layer> The hole transport layer preferably contains a hole transport substance and a resin. Examples of hole transport substances include polycyclic aromatic compounds, heterocyclic compounds, hydrazone compounds, styryl compounds, enamine compounds, benzidine compounds, triarylamine compounds, and resins having groups derived from these substances. Among these, triarylamine compounds and benzidine compounds are preferred. The content of the hole transport material in the hole transport layer is preferably from 25% by mass to 70% by mass, and more preferably from 30% by mass to 55% by mass, based on the total mass of the hole transport layer.

[0051] Examples of the resin include polyester resin, polycarbonate resin, acrylic resin, polystyrene resin, etc. Among these, polycarbonate resin and polyester resin are preferable. As the polyester resin, polyarylate resin is particularly preferable. The content ratio (mass ratio) of the hole transport substance to the resin is preferably from 4:10 to 20:10, and more preferably from 5:10 to 12:10.

[0052] The hole transport layer may also contain additives such as antioxidants, ultraviolet absorbers, plasticizers, leveling agents, slipping agents, and abrasion resistance improvers. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane-modified resins, silicone oils, fluororesin particles, polystyrene resin particles, polyethylene resin particles, silica particles, alumina particles, and boron nitride particles. The thickness of the hole transport layer is preferably from 5 μm to 50 μm, more preferably from 8 μm to 40 μm, and particularly preferably from 10 μm to 30 μm. The hole transport layer can be formed by preparing a coating solution for the hole transport layer containing the above-mentioned materials and solvent, forming a coating film of this, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Among these solvents, ether-based solvents or aromatic hydrocarbon-based solvents are preferred.

[0053] <Protective layer> In the present invention, a protective layer may be provided on the hole transport layer. By providing the protective layer, durability can be improved. The protective layer preferably contains conductive particles and / or a hole transport substance, and a resin. The conductive particles include particles of metal oxides such as titanium oxide, zinc oxide, tin oxide, and indium oxide. Examples of the hole transport substance include polycyclic aromatic compounds, heterocyclic compounds, hydrazone compounds, styryl compounds, enamine compounds, benzidine compounds, triarylamine compounds, and resins having groups derived from these substances. Among these, triarylamine compounds and benzidine compounds are preferred. Examples of the resin include polyester resin, acrylic resin, phenoxy resin, polycarbonate resin, polystyrene resin, phenol resin, melamine resin, epoxy resin, etc. Among them, polycarbonate resin, polyester resin, and acrylic resin are preferable.

[0054] The protective layer may be formed as a cured film by polymerizing a composition containing a monomer having a polymerizable functional group. Examples of the reaction include thermal polymerization, photopolymerization, and radiation polymerization. Examples of the polymerizable functional group of the monomer having a polymerizable functional group include an acrylic group and a methacrylic group. A material having a hole transport function may be used as the monomer having a polymerizable functional group. The protective layer may contain additives such as antioxidants, ultraviolet absorbers, plasticizers, leveling agents, slipping agents, abrasion resistance improvers, etc. Specific examples of the additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane-modified resins, silicone oils, fluororesin particles, polystyrene resin particles, polyethylene resin particles, silica particles, alumina particles, and boron nitride particles. The thickness of the protective layer is preferably from 0.5 μm to 10 μm, and more preferably from 1 μm to 7 μm. The protective layer can be formed by preparing a coating solution for the protective layer containing the above-mentioned materials and solvent, forming a coating film from the coating solution, and drying and / or curing the coating solution. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, sulfoxide-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents.

[0055] [Method of Manufacturing Electrophotographic Photoreceptor] The method for producing an electrophotographic photoreceptor according to the present invention is a method for producing an electrophotographic photoreceptor having a support, an electron transport layer, a charge generating layer, and a hole transport layer in this order. The method includes a step of forming a coating film of a coating liquid for an electron transport layer, and drying and / or curing the coating film to form the electron transport layer. The coating liquid for an electron transport layer contains a polymer having a structural unit represented by formula (1), formula (2), or formula (3), and the glass transition temperature Tg of the polymer is from -10°C to 50°C.

[0056] [Process cartridges, electrophotographic devices] The process cartridge according to the present invention is characterized in that it integrally supports the electrophotographic photosensitive member described above and at least one means selected from the group consisting of a charging means, a developing means and a cleaning means, and is detachably attachable to the main body of the electrophotographic apparatus. The electrophotographic apparatus according to the present invention is characterized by comprising the electrophotographic photosensitive member described above, as well as a charging means, an exposing means, a developing means and a transferring means.

[0057] FIG. 4 shows an example of a schematic configuration of an electrophotographic apparatus having a process cartridge equipped with an electrophotographic photosensitive member. A cylindrical electrophotographic photoreceptor 1 is driven to rotate around an axis 2 at a predetermined peripheral speed in the direction of the arrow. The surface of the electrophotographic photoreceptor 1 is charged to a predetermined positive or negative potential by a charging means 3. Although the figure shows a roller charging method using a roller-type charging member, a corona charging method, a proximity charging method, an injection charging method, or other charging methods may be adopted. Exposure light 4 is irradiated from an exposure means (not shown) onto the charged surface of the electrophotographic photoreceptor 1, and an electrostatic latent image corresponding to the target image information is formed. The electrostatic latent image formed on the surface of the electrophotographic photoreceptor 1 is developed with toner contained in a developing means 5, and a toner image is formed on the surface of the electrophotographic photoreceptor 1. The toner image formed on the surface of the electrophotographic photoreceptor 1 is transferred to a transfer material 7 by a transfer means 6. The transfer material 7 to which the toner image has been transferred is transported to a fixing means 8, where the toner image is fixed, and the transfer material is printed out outside the electrophotographic device. The electrophotographic device may have a cleaning means 9 for removing deposits such as toner remaining on the surface of the electrophotographic photoreceptor 1 after transfer. Also, a so-called cleanerless system may be used in which the deposits are removed by the developing means 5 or the like without separately providing the cleaning means 9. The electrophotographic apparatus may have a charge eliminating mechanism that eliminates charge on the surface of the electrophotographic photoreceptor 1 by pre-exposure light 10 from a pre-exposure means (not shown). Also, in order to mount and remove the process cartridge 11 according to the present invention to the main body of the electrophotographic apparatus, a guide means 12 such as a rail may be provided. The electrophotographic photoreceptor of the present invention can be used in laser beam printers, LED printers, copiers, facsimiles, and combination machines thereof. EXAMPLES

[0058] The present invention will be described in more detail below using examples and comparative examples. The present invention is not limited to the following examples without departing from the gist of the present invention. In the following description of the examples, "parts" are based on mass unless otherwise specified. First, an example of polymer synthesis will be shown.

[0059] [Synthesis example of polymer 1] The following materials were prepared: 3,4,9,10-perylenetetracarboxylic dianhydride (Tokyo Chemical Industry Co., Ltd.): 1.96 parts Poly(propylene glycol) bis(2-aminopropyl ether) (Mn230, Sigma-Aldrich): 1.38 parts These were mixed with 50 parts of N-methylpyrrolidone and heated to 180° C. while stirring. After 48 hours of reaction, the mixture was cooled and poured into 50 mL of water, and the precipitate was filtered off. The precipitate obtained was washed with hot water and then dried to obtain 3.0 parts of perylene imide polymer 1. The obtained compound was identified by NMR. 1 Measurement was performed by H-NMR (400 MHz, JMN-EX400, JEOL) using CDCl3 as a solvent. As a result, the target product was confirmed to have the following peak positions. δ8.6-7.8ppm (broad m, perylene site) δ4.3-4.1ppm (broad m, alkyl moiety linked to imide nitrogen) δ4.0-3.2ppm (broad m, ether portion) δ1.60-1.11ppm (broad s, methyl group) The weight average molecular weight of the obtained polymer is shown in Table 5. The weight average molecular weight (Mw) was measured by GPC (gel permeation chromatography) using HLC-8220 manufactured by Tosoh Corporation, and expressed as a polystyrene equivalent value.

[0060] [Example 1] [Manufacturing of electrophotographic photoreceptors] <Support> An aluminum cylinder with a length of 260.5 mm and a diameter of 30 mm was prepared. This aluminum cylinder was machined (JIS B 0601:2014, ten-point average roughness Rzjis: 0.8 μm), and the machined aluminum cylinder was used as a support (conductive support).

[0061] <Electron transport layer> Next, the following materials were prepared: Electron transport material: polymer 1:5 parts Blocked isocyanate compound as a crosslinking agent (product name: SBB-70P (solid content 70%), isocyanate:blocking group=6.7:3.3 (mass ratio), manufactured by Asahi Kasei): 2 parts These were dissolved in a mixed solvent of 48 parts of chloroform and 24 parts of o-xylene. The obtained coating solution for the electron transport layer was dip-coated on a support, and the obtained coating film was heated at 170° C. for 40 minutes and dried to form an electron transport layer having a thickness of 2.0 μm.

[0062] <Charge generation layer> Next, hydroxygallium phthalocyanine crystals (charge generating material) having peaks at Bragg angles (2θ±0.2°) of 7.5°, 9.9°, 12.5°, 16.3°, 18.6°, 25.1°, and 28.3° in CuKα characteristic X-ray diffraction were prepared. 10 parts of this hydroxygallium phthalocyanine crystal, 5 parts of polyvinyl butyral resin (product name: S-LEC BX-1, manufactured by Sekisui Chemical Co., Ltd.), and 250 parts of cyclohexanone were placed in a sand mill using glass beads with a diameter of 1 mm, and dispersed for 2 hours. Next, 250 parts of ethyl acetate were added to this to prepare a coating liquid for a charge generating layer. This coating liquid for a charge generating layer was applied by dip coating on the electron transport layer to form a coating film, and the resulting coating film was dried at a temperature of 95° C. for 10 minutes to form a charge generating layer with a thickness of 0.15 μm.

[0063] <Hole transport layer> The following materials were prepared: A hole transport material represented by the following formula (B-1): 5 parts [ka] A hole transporting compound represented by the following formula (B-2): 5 parts [ka] Polycarbonate resin (product name: Iupilon Z-400, manufactured by Mitsubishi Engineering Plastics): 10 parts These were dissolved in a mixed solvent of 25 parts of ortho-xylene / 25 parts of methyl benzoate / 25 parts of dimethoxymethane to prepare a coating solution for the hole transport layer. The coating solution for the hole transport layer thus prepared was dip-coated on the above-described charge generation layer to form a coating film, and the coating film was heated and dried at a temperature of 120 ° C for 30 minutes to form a hole transport layer with a film thickness of 25 μm.

[0064] [Evaluation] [Method for Preparing Sample for X-ray Diffraction Pattern Measurement] An aluminum cylinder wrapped with an aluminum sheet having a thickness of 50 μm was used as a support instead of the aluminum cylinder, and an electron transport layer was formed in the same manner as the method described in the above [Manufacture of Electrophotographic Photoconductor]. Thereafter, the aluminum sheet was peeled off from the aluminum cylinder, fixed to the sample stage of the X-ray diffraction pattern using double-sided tape, and the X-ray diffraction pattern was measured under the conditions described above.

[0065] (Pattern Memory Evaluation) The evaluation of the pattern memory was performed using a laser beam printer (trade name: Laser Jet Enterprise M609dn) manufactured by Hewlett Packard as an evaluation apparatus. The evaluation of the pattern memory was performed as follows. The manufactured electrophotographic photoconductor was mounted on the above-described laser beam printer manufactured by Hewlett Packard. This was installed in a low temperature and low humidity (15 ° C / 10% RH) environment, and an image with a printing rate of 5% was continuously output 100,000 times in repetition. Subsequently, an image of a vertical line pattern of 3 dots and 100 spaces was continuously output 20 times in repetition, and then three types of halftone images and a solid black image shown in Table 6 were output. Based on the appearance of the vertical streaks caused by the output of the above vertical lines on these output images, the degree of generation of the pattern memory was ranked into five levels according to the criteria shown in Table 6. The better the suppression of the pattern memory, the larger the rank number. The three types of halftone images are a halftone of a 1-dot horse racing pattern, a halftone of a horizontal line of 1 dot and 1 space, and a halftone of a horizontal line of 1 dot and 2 spaces.

[0066] [Table 6]

[0067] (Ghost Rating) Using the same electrophotographic device as that used for the pattern memory evaluation, one solid white image was output as the first sheet without turning on the pre-exposure. Then, printing for ghost evaluation was performed. That is, as shown in FIG. 2(a), an image having a black background (black image) 52 in a white background (white image) 51 at the beginning of the image, followed by a series of images having a halftone image 53 of a one-dot knight pattern shown in FIG. 2(b) was output in succession for five sheets. In FIG. 2, the "ghost portion 54" is the portion to evaluate the presence or absence of ghost caused by the black background (black image) 52. In the ghost evaluation, the difference in image density between the halftone image 53 of a one-dot knight pattern and the ghost portion 54 in the ghost evaluation print was measured using a spectrodensitometer (product name: X-Rite504 / 508, manufactured by X-Rite Corporation). The image density of 10 points was measured for each of the halftone image 53 and the ghost portion 54 in the ghost evaluation print, and the average of these 10 points was calculated. This was performed in the same manner for all of the five ghost evaluation prints described above. The difference in density between the average image density of the halftone image 53 and the average image density of the ghost portion 54 was taken as the ghost image density difference. The smaller the ghost image density difference, the greater the effect of suppressing the occurrence of ghost images. The ghost evaluation was performed according to the following criteria. A is a ghost image density difference of less than 0.01, B is a ghost image density difference of 0.01 or more and less than 0.02, C is a ghost image density difference of 0.02 or more and less than 0.03, D is a ghost image density difference of 0.03 or more and less than 0.04, and E is a ghost image density difference of 0.04 or more. The results are shown in Table 7.

[0068] [Examples 2 to 37] An electrophotographic photoreceptor was produced and evaluated in the same manner as in Example 1, except that the type of polymer used in Example 1 was changed to the polymer shown in Table 7. The results are shown in Table 7.

[0069] [Examples 38 to 40] Except for changing the amount of the crosslinking agent in the electron transport layer liquid from 2 parts to 3 parts (Example 38), 1 part (Example 39), and 0 part (Example 40), electrophotographic photoreceptors were produced and evaluated in the same manner as in Example 27. The results are shown in Table 7.

[0070] [Example 41] The support was changed to that described below, a conductive layer was formed on the support as described below, and an electron transport layer, a charge generating layer, and a hole transport layer were further formed on the conductive layer in the same manner as in Example 27 to produce an electrophotographic photoreceptor and evaluate it. The results are shown in Table 7.

[0071] <Support> An aluminum cylinder having a diameter of 30 mm and a length of 260.5 mm was used as a support (cylindrical support).

[0072] <Conductive layer> An anatase-type titanium oxide having an average primary particle size of 200 nm was used as the substrate, and a titanium niobium sulfate solution containing 33.7 parts of titanium in terms of TiO2 and 2.9 parts of niobium in terms of Nb2O5 was prepared. 100 parts of the substrate was dispersed in pure water to prepare a suspension of 1000 parts, which was then heated to 60°C. The titanium niobium sulfate solution and 10 mol / L sodium hydroxide were dropped into the suspension over 3 hours so that the pH of the suspension was 2 to 3. After the entire amount was dropped, the pH was adjusted to near neutral, and a polyacrylamide-based flocculant was added to precipitate the solids. The supernatant was removed, filtered, washed, and dried at 110°C to obtain an intermediate containing 0.1 mass% of organic matter derived from the flocculant in terms of C. This intermediate was calcined in nitrogen at 750°C for 1 hour, and then calcined in air at 450°C to produce titanium oxide particles. The resulting particles had a volume average particle size (average primary particle size) of 220 nm as determined by a particle size measurement method using a scanning electron microscope. Next, a phenolic resin (phenolic resin monomer / oligomer) was used as a binder (product name: Plyofen J-325, manufactured by DIC, resin solid content: 60%, density after curing: 1.3 g / cm 250 parts of this phenol resin was dissolved in 35 parts of 1-methoxy-2-propanol as a solvent to obtain a solution. To this solution, 60 parts of titanium oxide particles were added, and the mixture was placed in a vertical sand mill using 120 parts of glass beads with an average particle size of 1.0 mm as a dispersion medium, and dispersion treatment was carried out for 4 hours under conditions of a dispersion temperature of 23±3°C and a rotation speed of 1500 rpm (circumferential speed of 5.5 m / s) to obtain a dispersion. The glass beads were removed from this dispersion using a mesh. Next, the following materials were prepared: Silicone oil as a leveling agent (product name: SH28 PAINT ADDITIVE, manufactured by Toray Dow Corning): 0.01 part Silicone resin particles (product name: KMP-590, manufactured by Shin-Etsu Chemical Co., Ltd., average particle size: 2 μm, density: 1.3 g / cm) were used as a surface roughening agent. 3 ):8 parts These were added to the dispersion liquid after removing the glass beads, stirred, and filtered under pressure using PTFE filter paper (product name: PF060, manufactured by Advantec Toyo) to prepare a coating liquid for the conductive layer. The conductive layer coating liquid thus prepared was dip-coated onto the above-mentioned support to form a coating film, and the coating film was heated at 150° C. for 20 minutes to be cured, thereby forming a conductive layer having a thickness of 25 μm.

[0073] [Comparative Example 1] An electrophotographic photoreceptor was produced and evaluated in the same manner as in Example 1, except that the polymer 1 in Example 1 was changed to a polymer A having a repeating structural unit represented by the following formula (C-1). The results are shown in Table 7. Polymer A (molecular weight 3469, glass transition temperature Tg 52°C) [ka]

[0074] [Comparative Example 2] An electrophotographic photoreceptor was prepared and evaluated in the same manner as in Example 1, except that the electron transport layer was formed as follows. The results are shown in Table 7. <Electron transport layer> To 40 parts of copolymer B having a repeating structural unit represented by the following formula (C-2) and a repeating structural unit represented by the following formula (C-3), 300 parts by mass of distilled water, 500 parts by mass of methanol, and 8 parts by mass of triethylamine were added as a dispersion medium. This was dispersed for 2 hours using a sand mill device using glass beads with a diameter of 1 mm to prepare a coating liquid (dispersion) for an electron transport layer. This coating liquid for an electron transport layer was dip-coated on a support and heated at 120°C for 10 minutes to evaporate the dispersion medium and melt or aggregate (dry) the particles of the copolymer to form an electron transport layer having a thickness of 1.0 μm. Polymer B (molecular weight 11,000, glass transition temperature Tg 70°C, copolymerization ratio (mol%) formula (C-2): formula (C-3) = 19:1) [ka] [ka]

[0075] [Comparative Example 3] An electrophotographic photoreceptor was prepared and evaluated in the same manner as in Example 1, except that the electron transport layer was formed as follows. The results are shown in Table 7. <Electron transport layer> A polymer (10 parts) consisting of a mixture of two materials, a polymer having a repeating structural unit represented by the following formula (C-4) and a polymer having a structural unit represented by the following formula (C-5), was prepared. The polymer (10 parts) was dissolved in a mixed solvent of 30 parts by mass of N-methyl-2-pyrrolidone and 60 parts by mass of cyclohexanone to prepare a coating solution for an electron transport layer. This electron transport coating liquid was dip-coated onto a support, and the resulting coating film was heated at 150°C for 30 minutes to evaporate the solvent and cause condensation to form an electron transport layer having a thickness of 1.0 μm and containing polymer C having a structural unit represented by the following formula (C-6). The molecular weight of the polymer having a repeating structural unit represented by formula (C-4) and the polymer having a repeating structural unit represented by formula (C-5) were each 20000. The glass transition temperature Tg of the polymer C having a repeating structural unit represented by formula (C-6) was not observed in the range of -50°C to 200°C. [ka] [ka] [ka]

[0076] [Table 7]

[0077] The disclosure according to an embodiment of the present invention includes the following configuration. (Configuration 1) An electrophotographic photoreceptor having a support, an electron transport layer, a charge generating layer, and a hole transport layer in this order, The electron transport layer contains a polymer having a structural unit represented by the following formula (1), the following formula (2), or the following formula (3), The glass transition temperature Tg of the polymer is -10°C or more and 50°C or less. 1. An electrophotographic photoreceptor comprising: [ka] [ka] [ka] (In formula (1), R 11 , R 12 , R 13 , R 14 , R 15 , R 16 , R 17 , and R 18each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, R 61 represents a hydrogen atom or a substituted or unsubstituted alkyl group, m 1 indicates an integer between 2 and 16.) (In formula (2), R 22 , R 23 , R 24 , R 26 , R 27 , and R 28 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, R 62 represents a hydrogen atom or a substituted or unsubstituted alkyl group, R 41 and R 42 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, m 2 indicates an integer between 2 and 16.) (In formula (3), R 31 , R 33 , R 34 , R 35 , R 37 , and R 38 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, R 63represents a hydrogen atom or a substituted or unsubstituted alkyl group, R 51 and R 52 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, m 3 indicates an integer between 2 and 16.) (Configuration 2) m in formula (1) 1 , m in Eq. (2) 2 , and m in formula (3) 3 represents an integer of 2 or more and 6 or less. (Configuration 3) R in formula (1) 61 , R in Eq. (2) 62 , and R in formula (3) 63 3. The electrophotographic photoreceptor according to embodiment 1 or 2, wherein represents a methyl group. (Configuration 4) 4. The electrophotographic photoreceptor according to any one of configurations 1 to 3, wherein the polymer has a weight average molecular weight of 30,000 or less. (Configuration 5) 5. The electrophotographic photoreceptor according to any one of Configurations 1 to 4, wherein a CuKα characteristic X-ray diffraction pattern obtained for the electron transport layer has a peak at a position of 2θ=7.5°±2.5° (θ is the Bragg angle). (Method 1) A method for producing an electrophotographic photoreceptor having a support, an electron transport layer, a charge generating layer, and a hole transport layer in this order, comprising the steps of: forming a coating film of a coating liquid for an electron transport layer, and drying and / or curing the coating film to form the electron transport layer; The coating liquid for an electron transport layer contains a polymer having a structural unit represented by the following formula (1), the following formula (2), or the following formula (3), The glass transition temperature Tg of the polymer is -10°C or more and 50°C or less. 2. A method for producing an electrophotographic photoreceptor comprising the steps of: [ka] [ka] [ka] (In formula (1), R 11 , R 12 , R 13 , R 14 , R 15 , R 16 , R 17 , and R 18 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, R 61 represents a hydrogen atom or a substituted or unsubstituted alkyl group, m 1 indicates an integer between 2 and 16.) (In formula (2), R 22 , R 23 , R 24 , R 26 , R 27 , and R 28 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, R 62 represents a hydrogen atom or a substituted or unsubstituted alkyl group, R 41 and R 42 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, m 2 indicates an integer between 2 and 16.) (In formula (3), R 31 , R 33, R 34 , R 35 , R 37 , and R 38 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, R 63 represents a hydrogen atom or a substituted or unsubstituted alkyl group, R 51 and R 52 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, m 3 indicates an integer between 2 and 16.) (Method 2) the coating liquid for the electron transport layer further contains a crosslinking agent, The process includes curing the coating. A method for producing an electrophotographic photoreceptor according to method 1. (Configuration 8) A process cartridge which integrally supports the electrophotographic photosensitive member according to any one of Configurations 1 to 5 and at least one means selected from the group consisting of a charging means, a developing means and a cleaning means, and is detachably mountable to a main body of an electrophotographic apparatus. (Configuration 9) 6. An electrophotographic apparatus comprising the electrophotographic photoreceptor according to any one of Configurations 1 to 5, a charging means, an exposing means, a developing means and a transferring means. [Explanation of symbols]

[0078] 101 Support 102 Electron transport layer 103 Charge generating layer 104 Hole transport layer 1. Electrophotographic photoreceptor 2-axis 3. Charging means 4 Exposure light 5. Developing method 6 Transfer Method 7 Transfer material 8 Fixing Method 9 Cleaning Method 10 Pre-exposure light 11 Process cartridge 12 Guidance means

Claims

1. An electrophotographic photoreceptor having a support, an electron transport layer, a charge generating layer, and a hole transport layer in this order, The electron transport layer contains a polymer having a structural unit represented by the following formula (1), the following formula (2), or the following formula (3), The glass transition temperature Tg of the polymer is −10° C. or more and 50° C. or less.

1. An electrophotographic photoreceptor comprising: [Formula 1] [chemical 2] [C3] (In formula (1), R 11 , R 12 , R 13 , R 14 , R 15 , R 16 , R 17 , and R 18 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, R 61 represents a hydrogen atom or a substituted or unsubstituted alkyl group, m 1 represents an integer of 2 or more and 16 or less.) (In formula (2), R 22 , R 23 , R 24 , R 26 , R 27 , and R 28 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, R 62represents a hydrogen atom or a substituted or unsubstituted alkyl group, R 41 and R 42 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, m 2 represents an integer of 2 or more and 16 or less.) (In formula (3), R 31 , R 33 , R 34 , R 35 , R 37 , and R 38 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, R 63 represents a hydrogen atom or a substituted or unsubstituted alkyl group, R 51 and R 52 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, m 3 represents an integer of 2 or more and 16 or less.)

2. m in formula (1) 1 , m in formula (2) 2 and m in formula (3) 3 The electrophotographic photoreceptor according to claim 1 , wherein represents an integer of 2 or more and 6 or less.

3. R in formula (1) 61 , R in formula (2) 62 and R in formula (3) 63 The electrophotographic photoreceptor according to claim 1 , wherein represents a methyl group.

4. 2. The electrophotographic photoreceptor according to claim 1, wherein the polymer has a weight average molecular weight of 30,000 or less.

5. 2. The electrophotographic photoreceptor according to claim 1, wherein a CuKα characteristic X-ray diffraction pattern obtained for the electron transport layer has a peak at a position of 2θ=7.5°±2.5° (θ is the Bragg angle).

6. A method for producing an electrophotographic photoreceptor having a support, an electron transport layer, a charge generating layer, and a hole transport layer in this order, comprising the steps of: forming a coating film of a coating liquid for an electron transport layer, and drying and / or curing the coating film to form the electron transport layer; The coating liquid for the electron transport layer contains a polymer having a structural unit represented by the following formula (1), the following formula (2), or the following formula (3): The glass transition temperature Tg of the polymer is −10° C. or more and 50° C. or less.

2. A method for producing an electrophotographic photoreceptor comprising the steps of: [C4] [C5] [C6] (In formula (1), R 11 , R 12 , R 13 , R 14 , R 15 , R 16 , R 17 , and R 18 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, R 61 represents a hydrogen atom or a substituted or unsubstituted alkyl group, m 1 represents an integer of 2 or more and 16 or less.) (In formula (2), R 22 , R 23 , R 24 , R 26 , R 27 , and R 28 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, R 62 represents a hydrogen atom or a substituted or unsubstituted alkyl group, R 41 and R 42 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, m 2 represents an integer of 2 or more and 16 or less.) (In formula (3), R 31 , R 33 , R 34 , R 35 , R 37 , and R 38 each independently represents a hydrogen atom, a halogen atom, a nitro group, a cyano group, a trifluoromethyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted thiol group, a substituted or unsubstituted amino group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkynyl group, or a substituted or unsubstituted aryl group, R 63 represents a hydrogen atom or a substituted or unsubstituted alkyl group, R 51 and R 52 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group, m 3 represents an integer of 2 or more and 16 or less.)

7. the coating liquid for the electron transport layer further contains a crosslinking agent, The process includes curing the coating. The method for producing an electrophotographic photoreceptor according to claim 6 .

8. 6. A process cartridge which integrally supports the electrophotographic photosensitive member according to any one of claims 1 to 5 and at least one means selected from the group consisting of a charging means, a developing means and a cleaning means, and is detachably mountable to a main body of an electrophotographic apparatus.

9. 6. An electrophotographic apparatus comprising the electrophotographic photoreceptor according to claim 1, a charging means, an exposure means, a developing means and a transfer means.

Citation Information

Patent Citations

  • Electrophotographic photoreceptor, process cartridge and electrophotographic device possessing it

    JP2003345044A

  • Electrophotographic photosensitive member, process cartridge, and electrophotographic apparatus

    JP2010198014A