Embossing rubber roller, plastic film manufacturing method, and surface protection film
The rubber roller with a fluororesin layer and controlled concave portions addresses the issue of high haze in conventional embossing rollers by reducing surface shape transfer, facilitating easier inspection and bonding.
Patent Information
- Application Number
- JP2023066043
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-25
AI Technical Summary
Conventional embossing rollers transfer fine irregularities to plastic films, leading to high haze, making inspection processes difficult and complicating bonding to adherends.
A rubber roller with a fluororesin layer featuring curved concave portions and controlled depth and density, combined with a method to produce a plastic film that suppresses haze and minimizes surface shape transfer.
The solution effectively reduces haze to 60% or less, enabling easier inspection and bonding processes by preventing surface shape transfer to adherends.
Smart Images

Figure 2024152096000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an embossing rubber roller, a method for producing a plastic film using the same, and a surface protective film. [Background technology]
[0002] Conventionally, as an embossing roller for forming an uneven shape on the surface of a plastic film, for example, a rubber roller with a surface coated with silicone rubber as described in Patent Document 1 has been proposed. In Patent Document 1, spherical solid particles with a limited particle size are mixed into the silicone rubber constituting the rubber roller, so that a large number of unevennesses with uniform size are formed on the surface of the rubber roller. The manufactured plastic film can be used as a surface protection film that protects the surface of the adherend from scratches and dirt during the manufacturing process and transportation by bonding it to a sheet-like or web-like adherend such as an optical plastic film or a resin plate, and it is said that the use of the plastic film manufactured by the above manufacturing method can prevent the transfer of the matte surface to the adherend. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-55189 A Summary of the Invention [Problem to be solved by the invention]
[0004] On the other hand, plastic films produced using conventional embossing rollers have the characteristic of having a large haze because the dense unevenness of the embossing roller surface is transferred to the film. If a plastic film with a large haze is used as a surface protection film, there is a problem that the inspection process and appearance inspection after bonding to an adherend become difficult.
[0005] The present invention aims to improve upon the drawbacks of the conventional technology and to provide an embossing rubber roller that suppresses the transfer of an uneven surface to an adherend while suppressing haze in the produced plastic film, as well as a method for producing a plastic film using the same, and a surface protective film. [Means for solving the problem]
[0006] In order to achieve the above object, the rubber roller for embossing of the present invention has the following configuration: That is, the rubber roller for embossing is a rubber roller in which the surface of a core metal at the center of the roller is covered with at least a rubber layer and a fluororesin layer from the side closer to the core metal, the fluororesin layer being the outermost layer of the rubber roller, and a plurality of curved recesses having edges in the shape of a circle or an ellipse are formed on the surface of the fluororesin layer.
[0007] The recess has a depth of 2 μm or more and 10 μm or less, and the recess has a depth of 1 mm 2 It is preferable that the number of the recesses per unit area is 150 or more and 2500 or less.
[0008] In the method for producing a plastic film of the present invention, it is preferable to extrude molten resin from a die and cool the extruded molten resin while clamping it between the embossing rubber roller and a cooling roller, thereby solidifying the molten resin and obtaining a plastic film on a web.
[0009] The surface protective film of the present invention is a surface protective film composed of a single layer or multiple layers, at least one outermost surface of which has curved convex portions, and preferably has a haze of 60% or less.
[0010] The height of the protrusions is 2 μm or more and 10 μm or less, and the protrusions are formed within 1 mm 2 It is preferable that the number of the protrusions per unit area is 150 or more and 2500 or less.
[0011] The rubber roller for embossing of the present invention refers to a roller having irregularities formed on its surface, the irregularities being intended to be transferred to the surface of a plastic film, thereby forming irregularities on the surface of the plastic film.
[0012] In the present invention, the edge shape is a circle or an ellipse means that the edge shape of the recesses on the surface of the embossing rubber roller or the edge shape of the protrusions on the surface of the plastic film is a circle or an ellipse, or a shape of an edge in which a plurality of these overlap.
[0013] In the present invention, the cooling roller refers to a roller intended to come into contact with the molten resin and cool it to solidify the molten resin.
[0014] The surface protection film of the present invention refers to a plastic film that is attached to a sheet-like or web-like adherend, such as an optical plastic film such as a retardation film or a brightness enhancing film, or a metal foil, a glass plate, or a resin plate, to protect the surface of the adherend from damage such as scratches and dirt during the manufacturing process or transportation. Effect of the Invention
[0015] The present invention provides an embossing rubber roller capable of embossing a plurality of convex portions on the surface of a plastic film while suppressing the haze of the plastic film. Further, a method for producing a plastic film using the embossing rubber roller is provided. The present invention also provides a surface protection film that suppresses haze without transferring the surface shape to an adherend. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a schematic side view showing one embodiment of an embossing rubber roller of the present invention. [Diagram 2] FIG. 2 is an enlarged schematic side view showing one embodiment of the embossing rubber roller of the present invention. [Diagram 3]1 is a configuration example showing the surface shape of an embossing rubber roller of the present invention. [Figure 4] 1 is a schematic cross-sectional view showing one embodiment of a surface protection film of the present invention. [Diagram 5] FIG. 1 is a schematic side view showing one embodiment of the plastic film manufacturing method of the present invention. [Figure 6] FIG. 2 is a schematic side view showing another embodiment of the plastic film manufacturing method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an example of the best mode for carrying out the present invention will be described with reference to the drawings.
[0018] As shown in FIG. 1, the embossing rubber roller 100 of the present invention has a core metal 3 at the center of the roller, the surface of which is coated with at least a rubber layer 2 and a fluororesin layer 1 in that order from the side closest to the core metal 3.
[0019] The structure of the core metal 3 is not particularly limited, but it is preferable that the surface temperature of the embossing rubber roller 100 can be controlled by providing a heat medium flow path 4 for circulating a heat medium such as water inside as shown in FIG. 1. When the surface temperature of the embossing rubber roller 100 is lowered, when the embossing rubber roller 100 is used as the embossing rubber roller 13 in the manufacturing method of a plastic film as shown in FIG. 5, the releasability from the molten resin is improved, and the embossing rubber roller 13 is easily prevented from wrapping around the embossing rubber roller 13. Also, the speed at which the molten resin 12 is solidified is increased, so that the embossing speed can be improved. The surface temperature of the embossing rubber roller 13 can be lowered by providing a cooling backup roller on the opposite side of the cooling roller 14 to the embossing rubber roller 13, or by spraying air or mist-like water on the embossing rubber roller 13. Furthermore, if the surface temperature of the embossing rubber roller 100 is increased, when it is used as the embossing rubber roller 13 in a manufacturing method of a plastic film 16 as shown in Figure 6, the temperature of the plastic film surface can be increased, so that the surface of the plastic film 16 softens and the uneven shape of the embossing rubber roller 100 becomes easier to transfer.
[0020] The material of the core 3 is not particularly limited and may be appropriately selected from ordinary materials such as metal, plastic, or fiber-reinforced resin, but as in the above, it is preferable to select a metal material with high thermal conductivity from the viewpoint of temperature control. Examples of the metal material that can be selected include carbon steel, stainless steel, aluminum, and aluminum alloys.
[0021] The configuration of the embossing rubber roller 100 is such that at least a rubber layer 2 and a fluororesin layer 1 are coated on the side closer to the core metal 3, and the outermost layer is the fluororesin layer 1, as shown in FIG. 2, a layer of another material such as an adhesive layer 6 may be present between the core metal 3 and the rubber layer 2, or between the rubber layer 2 and the fluororesin layer 1.
[0022] The material of the rubber layer 2 located between the core metal 3 and the fluororesin layer 1 is not particularly limited and can be selected from normal rubber types such as natural rubber, butadiene rubber, and urethane rubber. However, it is preferable to use silicone rubber, whose main component is silicone, because of the ease of roller production and high heat resistance. Among silicone rubbers, when silicone rubber, which is generally called RTV (Room Temperature Vulcanization) silicone rubber or liquid silicone rubber, is used, which is in a liquid state before becoming a rubber-like elastic body by crosslinking, it is easy to obtain a surface without height differences due to seams, so there is an advantage that when a rubber roller is used as the embossing rubber roller 13, the seams are not transferred to the embossing surface of the plastic film 16. On the other hand, when silicone rubber, generally called HTV (High Temperature Vulcanization) silicone rubber or heat vulcanized silicone rubber, is used, it is easy to obtain high heat resistance and strength compared to RTV. In addition, by using these in a laminated state, it is possible to obtain the advantages of both.
[0023] Methods for covering the rubber layer 2 include a method of wrapping a sheet of uncrosslinked rubber around the core metal 3 and crosslinking it, as in the case of manufacturing various rubber rollers, a method of applying or spraying liquid uncrosslinked rubber onto the core metal 3 or filling a mold with the uncrosslinked rubber and then crosslinking it, and a method of inserting the core metal 3 into a crosslinked rubber tube and fixing it by tightening or bonding. In addition, when covering the rubber layer 2, an adhesive can be used to improve the adhesive strength. The adhesive used for bonding the core metal 3 and the rubber layer 2 is not particularly limited, and can be selected from ordinary adhesives whose main components are vinyl acetate resin, acrylic copolymer resin, epoxy resin, nitrile rubber, etc., but using an adhesive whose main component is the same as that of the rubber layer 2 often results in high adhesive strength.
[0024] The configuration of the rubber layer 2 is not particularly limited, but the number of layers is preferably in the range of 1 to 3. Within this range, peeling and shear fracture at the interface between the rubber layers during use can be easily controlled, and desired mechanical properties such as heat resistance and strength can be imparted.
[0025] The rubber hardness of the rubber layer 2 is not particularly limited, but a rubber hardness in the range of A 30 to 90 (JIS K 6253:2012) is preferably used. In the configuration in which different types of rubber layers 2 are laminated as exemplified above, it is preferable that the laminated rubber as a whole has a hardness in the above range. If the rubber hardness is within the above range, it is easier to alleviate unevenness in contact pressure due to the processing accuracy of the embossing rubber roller 100 and the opposing rollers and uneven thickness in the width direction of the film during embossing, which is preferable because it makes it easier to perform embossing uniformly.
[0026] The thickness of the rubber layer 2 is not particularly limited, but is preferably in the range of 1 to 15 mm. In addition, in the configuration in which different types of rubber layers 2 are laminated as exemplified above, it is preferable that the above range is satisfied for the entire laminated rubber. This range is preferable because it is easy to alleviate unevenness in contact pressure due to processing accuracy of the embossing rubber roller 100 and the opposing rollers and uneven thickness of the film 16 in the width direction during embossing, and it is easy to perform embossing uniformly. In addition, it is preferable because it is easy to control the temperature when controlling the surface temperature of the embossing rubber roller 100 by the heat medium flow path 4 inside the core metal 3, etc.
[0027] The embossing rubber roller 100 may have a so-called crown shape, in which the outer diameter is gradually reduced from the center to the end. By providing an appropriate crown shape according to the length and rigidity of the embossing rubber roller 100 and the pressure during embossing, a uniform pressure distribution is achieved in the width direction, making it easier to perform embossing uniformly in the width direction. As a method for processing the embossing rubber roller 100 into a crown shape, a method for gradually reducing the outer diameter of the rubber layer 2 from the center to the end, or a method for gradually reducing the outer diameter of the outermost fluororesin layer 1 from the center to the end can be used. In addition, as a method for obtaining the same effect as that of making the embossing rubber roller 100 into a crown shape, a method for making the core metal 3 into a crown shape and making the embossing rubber roller 100 into a constant outer diameter can also be used. In this case, since the outer diameter of the surface is constant, friction due to a difference in peripheral speed in the axial direction does not occur, which is preferable.
[0028] There are no particular limitations on whether or not the surface of the rubber layer 2 is removed, and on the method of the removal, but removal is preferred because it can eliminate irregularities that occur when covering or storing the rubber layer 2. The method of the removal can be appropriately selected from cutting with a cutting tool, polishing with sandpaper or a rotating grindstone, and the like.
[0029] The coating method and bonding method of the fluororesin layer 1 are not particularly limited, but a method can be used in which the embossing rubber roller 100 not coated with the fluororesin layer 1 is inserted into a heat-shrinkable tube made of fluororesin, heated from the outside with a hot air gun or heater, and tightened and fixed by heat shrinkage. If the rubber roller is coated with a heat-shrinkable tube made of fluororesin, a seamless surface can be easily obtained, so that when the rubber roller is used as the embossing rubber roller 13, the seam is not transferred to the embossing surface of the plastic film 16. In addition, an adhesive can be used to strengthen the adhesive force between the fluororesin layer 1 and the rubber layer 2 and suppress misalignment and slippage when used as the embossing rubber roller 13. The adhesive used to bond the fluororesin layer 1 and the rubber layer 2 is not particularly limited, and can be appropriately selected from ordinary adhesives whose main components are vinyl acetate resin, acrylic copolymer resin, epoxy resin, nitrile rubber, etc., but when an adhesive whose main component is the same as that of the rubber layer 2 is used, a high adhesive force is often obtained.
[0030] Although there is no particular limitation on the material of the fluororesin layer 1, it is preferable to use PFA (perfluoroalkoxyalkane) or FEP (tetrafluoroethylene-hexafluoropropylene copolymer), which are generally used in fluororesin heat-shrinkable tubes. By selecting such a material, it becomes possible to inexpensively cover the fluororesin layer 1 by heat shrinking.
[0031] The thickness of the fluororesin layer 1 is not particularly limited, but is preferably about 0.1 to 1.0 mm. Within this range, unevenness in contact pressure due to processing accuracy of the embossing rubber roller 100 and the opposing roller and uneven thickness of the film 16 in the width direction during embossing can be easily alleviated, making it easier to perform uniform embossing.
[0032] A plurality of curved recesses 7 with edges of a circle or ellipse are formed on the surface of the fluororesin layer 1 as shown in Figures 2 and 3. By transferring the recesses 7 of the above-mentioned shape to the surface protection film 101 by a method as shown in Figures 5 and 6, which will be described later, it is possible to form protrusions 8 on the embossing surface of the surface protection film 101. The height and number of the protrusions 8 on the surface of the surface protection film 101 are almost the same as the depth and number of the recesses 7 in the fluororesin layer 1 of the embossing rubber roller 100.
[0033] The present inventors have found that the reason why the haze of the surface protection film 101 having a dense uneven shape is large is that the inclination of the unevenness of the surface of the film 16 is steep and the proportion of the surface perpendicular to the incident light is small. In other words, when the proportion of the surface that is approximately parallel to the adhesive surface is small, most of the incident light that enters the film 16 is refracted, so the haze is large. In addition, when there is no unevenness or there are very few unevennesses on the surface of the film 16, the releasability of the embossed molded surface is greatly impaired, and when the unevenness is not dense, the contact pressure between the adherend and the surface protection film 101 is large, and the uneven shape of the surface protection film 101 is transferred to the adherend. Furthermore, when there is an unevenness whose depth or height is too large compared to the surrounding unevenness, the contact pressure is concentrated and a dent is generated on the adherend.
[0034] As a result of extensive research based on these findings, it was found that by making the recesses 7 on the surface of the embossing rubber roller 100 curved with a circular or elliptical edge shape, it is possible to reduce the haze of the film 16 while suppressing the transfer of the surface shape of the film 16 to the adherend. By reducing the haze of the film 16 to 60% or less, it becomes possible to easily carry out the inspection process and appearance inspection after the film 16 is attached to the adherend as the surface protection film 101. In addition, the recesses 7 on the surface of the embossing rubber roller 100 have a depth of 2 μm to 10 μm and a width of 1 mm. 2 Within the above range, the number of projections 8 on the surface of the surface protective film 101 is preferably in the range of 150 to 2500. 2By setting the number of recesses per unit area to 150 or more and 2500 or less, high releasability is easily obtained, and the surface protection film 101 can be easily peeled off without wrinkles or tears when unrolled. For the same reason, the height of the recesses 7 on the surface of the embossing rubber roller 100 is set to 3.5 μm or more and 5 μm or less, and 1 mm 2 It is more preferable that the number per unit is 200 or more and 1000 or less.
[0035] The method for forming the recesses 7 on the surface of the fluororesin layer 1 is not particularly limited, but it is preferable to perform so-called blasting, in which particles are sprayed at high pressure. Furthermore, the shape of the particles is preferably spherical, and blasting using spherical bodies is preferable for forming curved recesses with a circular or elliptical edge shape on the surface of the fluororesin layer 1. Furthermore, the material of the spherical bodies to be sprayed is not particularly limited, and can be appropriately selected from common abrasives such as steel, alumina, glass, and ceramic, but steel and alumina are preferably used. By spraying spherical bodies made of steel or alumina, it is easy to prevent the sprayed material from cracking when sprayed on the fluororesin layer 1, the edge shape of the recesses 7 from becoming other than a circle or an ellipse, the sprayed material from piercing the surface of the fluororesin layer 1, and the sprayed material from moving into the molten resin 12 during embossing, which is preferable. Furthermore, a 1 mm thick layer of the fluororesin layer 1, which is the outermost layer of the embossing rubber roller 100, is sprayed with a thickness of 1 mm. 2 When trying to obtain recesses 7 with a number of 150 to 2,500 per unit and a height of 2 μm to 10 μm, this can often be achieved by using a spray material with a diameter in the range of 30 μm to 120 μm, although this will vary depending on the spray pressure and the thickness and hardness of the fluororesin layer 1.
[0036] There are no particular limitations on whether or not the surface of the fluororesin layer 1 is subjected to a removal process, and on the method of removal, but it is preferable to perform the removal process before the blasting process, since this makes it possible to remove scratches and dents that occur during the fluororesin tube manufacturing process, etc. As the removal process, general polishing methods such as polishing with a rotating grindstone, buff polishing, and vertical polishing can be used.
[0037] FIG. 5 shows an example of a method for producing a plastic film using a rubber roller for embossing of the present invention. Molten resin 12 discharged from a T-die 11 is pressed and cooled by a cooling roller 14 and a rubber roller for embossing 13 to obtain a plastic film 16. Next, if necessary, the film 16 is cut by a blade such as a cutter 17, or the film edge 18 is trimmed, and the film is wound into a roll to become a film roll 21. Thereafter, if necessary, the film is again subjected to a slitting process or other processing process to become a product roll. The die is not limited to the T-die 11, but the T-die 11 is preferably used because it can extrude the molten resin 12 uniformly in the width direction at a high temperature.
[0038] The rubber rollers for embossing of the present invention are 13 and 100. In this way, the surface shape of the rubber roller for embossing 100 is transferred to the film 16, and as described above, the transfer of the surface shape to the adherend is suppressed, and the film 16 with suppressed haze can be obtained.
[0039] The T-die 11 extrudes the molten resin 12, which has been mixed by an extruder (not shown), from a slit provided in the depth direction of the drawing, so that the molten resin 12 is extruded into a sheet shape. It is preferable to provide a filtering device called a polymer filter between the extruder and the T-die 11, because it is easy to reduce the inclusion of foreign matter called fish eyes and deteriorated resin. The width of the slit of the T-die 11 is preferably adjustable in a constant direction in the width direction of the film 16, so as to control the unevenness in the thickness of the film 16. The thickness of the film 16 to be produced can be controlled by the ratio of the discharge speed of the molten resin 12 to the rotation speed of the cooling roller 14. When the film 16 to be produced has a multilayer structure, a lamination device for the molten resin 12 called a feed block is provided upstream of the T-die 11, or the T-die 11 has a structure having multiple manifolds called a multi-manifold structure, and is co-extruded. In addition, the width of the film 16 to be produced may be changed by regulating the flow path width of the molten resin 12 in the film width direction.
[0040] It is preferable that the positional relationship between the T-die 11, the cooling roller 14, and the embossing rubber roller 13 is an adjustable structure. Usually, in order to precisely transfer the surface shape of the embossing rubber roller 13 to the molten resin 12, it is preferable to nip and press the molten resin 12 in a molten state before cooling, so that it is preferable to adjust the position of the T-die 11 or the cooling roller 14 so that the molten resin 12 directly enters the nip point as shown in Fig. 5, but the positional relationship between the cooling roller 14 and the embossing rubber roller 13 may be adjusted as appropriate.
[0041] The temperature of the molten resin 12 is set appropriately depending on the type of resin used and the embossing speed, but for example, in the case of a general polyethylene resin, it can generally be set in the range of 130°C or higher and 300°C or lower.
[0042] The cooling roller 14 has a flow path inside for circulating a heat medium, and is structured to control the rise in surface temperature. The surface temperature of the cooling roller 14 is appropriately set depending on the type of molten resin 12, the contact time between the molten resin 12 and the cooling roller 14, and room temperature and humidity, but is preferably in the range of 10°C to 60°C from the viewpoint of the film-forming speed and the surface quality of the film 16. If the surface temperature of the cooling roller 14 is within the above range, it is easy to cool and solidify the molten resin 12 within a practical range of film-forming speed, and it is also easy to prevent deterioration of the surface quality of the film 16 due to condensation on the surface of the cooling roller 14 during film formation.
[0043] The material of the surface of the cooling roller 14 is not particularly limited, but metal, ceramics, resin, composite film of resin and metal, and carbon fiber-based film such as diamond-like carbon can be used. Rubber can also be used as the surface material of the cooling roller 14. Metals can be selected from iron, steel, stainless steel, aluminum, titanium, chromium, nickel, and ceramics can be selected from sintered bodies such as alumina, silicon carbide, and silicon nitride. The surface shape of the cooling roller 14 is transferred to the molten resin 12 and becomes the surface shape of the opposite side of the surface where the molten resin 12 and the embossing rubber roller 13 contact each other, so that industrial chrome plating or ceramics, which are excellent in durability and rust prevention, are preferably used from the viewpoint of suppressing deterioration of the appearance quality of the film 16 and the occurrence of convex defects. In order to make the surface of the cooling roller 14 metal, in addition to ordinary machining using a metal material, known surface treatment techniques such as electroplating and electroless plating can be appropriately used. Similarly, in order to obtain a ceramic surface, in addition to ordinary machining using a ceramic material, known surface treatment techniques such as thermal spraying and coating can be appropriately used.
[0044] The surface shape of the cooling roller 14 is transferred to the molten resin 12, and determines the surface shape of the opposite side of the surface of the molten resin 12 that comes into contact with the embossing rubber roller 13. Therefore, the surface shape of the cooling roller 14 is appropriately designed according to the plastic film 16 to be produced, but when producing the surface protection film 101 of the present invention, the arithmetic mean roughness Ra (JIS B B0601:2013) of the cooling roller 14 is preferably 0.2 μm or less, more preferably Ra 0.1 μm or less. When producing the surface protection film 101 of the present invention, the opposite side becomes an adhesive surface to be attached to an adherend, and the adhesive strength thereof decreases as the arithmetic mean roughness Ra of the adhesive surface increases, making it difficult to adhere to the adherend, so the above range is preferable. It is possible to increase adhesive strength by mixing additives such as tackifiers into the resin, but when the surface protection film 101 of the present invention is peeled off from the substrate, the additives may remain on the substrate, or the additives may make it difficult to reuse the resin. Therefore, it is preferable in terms of both quality and cost to keep the surface roughness within the above range and to allow the resin alone to exhibit sufficient adhesive strength as the surface protection film 101 of the present invention.
[0045] As a means for pressing the embossing rubber roller 13 against the cooling roller 14 to squeeze the molten resin 12, a method of controlling the gap between the cooling roller 14 and the embossing rubber roller 13 or the pressing amount of the embossing rubber roller 13, i.e., the relative position between the embossing rubber roller 13 and the cooling roller 14, by a method of sandwiching a taper block or the like may be used, or a method of controlling the pressing force of the embossing rubber roller 13 by an air cylinder or the like may be used. However, when producing a thin film in which the thickness of the molten resin 12 at the nip point is 100 μm or less, or when the hardness of the embossing rubber roller 13 is greater than A 90, a method of controlling the pressing force is preferable because the unevenness of the pressure may become too large when controlled by the pressing amount. The pressing pressure is appropriately set, but is preferably in the range of about 0.1 kN / m to 30 kN / m. If the pressing pressure is within the above range, the surface of the embossing rubber roller 13 is easily transferred to the molten resin.
[0046] Alternatively, as shown in Figure 6, an embossed plastic film 16 can be obtained in a similar manner by heating an already manufactured plastic film 32 to soften at least the surface to be embossed to a state where it can be processed, and then clamping the film between an embossing rubber roller 13 and a backing roller 34.
[0047] FIG. 4 shows a cross-sectional view of one embodiment of the surface protection film 101 of the present invention. The surface protection film 101 of the present invention can be manufactured by the embossing rubber roller of the present invention or by a method for manufacturing a plastic film using the same. As described above, the surface of the surface protection film 101 of the present invention has protrusions 8 formed thereon, which have almost the same shape, number, and height as the depth of the recesses 7 on the surface of the embossing rubber roller 100. This reduces the haze of the film 16 while suppressing the transfer of the surface shape of the film 16 to the adherend, making it possible to reduce the haze to 60% or less, and thus making it possible to easily carry out an inspection process or an appearance inspection after the film 101 is attached to the adherend. Furthermore, if the haze is 50% or less, it is preferable because the inspection after the film 101 is attached to the adherend can be carried out more accurately or easily. In addition, as described above, from the viewpoint of improving releasability, the protrusions 8 on the surface of the surface protection film 101 of the present invention have a height of 2 μm to 10 μm and a height of 1 mm or less. 2 The number of particles per mm is preferably 150 or more and 2500 or less. 2 It is more preferable that the number of protrusions 8 per unit area is 200 or more and 1000 or less, and the height of the protrusions 8 is 3.5 μm or more and 5 μm or less.
[0048] The thickness of the surface protection film 101 of the present invention is not particularly limited, but if it is in the range of 15 μm or more and 100 μm or less, the surface shape of the embossing rubber roller 100 can be sufficiently transferred to the surface of the surface protection film 101, and high handleability can be obtained during transportation after bonding to an adherend, so it is preferable. Also, if it is in the range of 20 μm or more and 50 μm or less, a good balance between the transferability of the surface shape and the handleability is obtained, so it is more preferable.
[0049] The surface protective film 101 of the present invention may have a single-layer structure or a multi-layer structure consisting of two or more layers. For example, when it has a single-layer structure, the device configuration is simple, so that the equipment cost and maintenance cost can be reduced. When it has a three-layer structure and recycled raw materials are used for the middle layer, the raw material cost can be reduced. In addition, when it has a single-layer structure or a multi-layer structure, raw materials can be easily reused if the resins of each layer are the same.
[0050] The surface protective film 101 of the present invention may have convex portions 8 formed on both sides, but at least the outermost surface of one side has a plurality of convex portions 8. It is preferable to use a plastic film 16 having convex portions 8 formed only on one side, with the surface to be bonded to an adherend being a smooth surface and the other surface being an uneven surface, as the surface protective film 101 of the present invention, because this prevents the front and back sides of the film from peeling off when the film is wound into a roll after bonding, or prevents the occurrence of wrinkles.
[0051] The resin constituting the surface protection film 101 of the present invention is not particularly limited, and can be appropriately selected from polyesters such as polyethylene terephthalate and polyethylene-2,6-naphthalate, polyolefins such as polyethylene and polypropylene, polyvinyls such as polyvinyl chloride and polyvinylidene chloride, polyamides, aromatic polyamides, polyphenylene sulfide, etc. according to the required characteristics, but it is preferable to use polyolefins. Among them, it is particularly preferable to use low-density polyethylene (LDPE) or linear low-density polyethylene (LLDPE) for the layer forming the protrusions 8 and the layer forming the adhesive surface. If the protrusions 8 are formed from a hard resin, when the film 16 is wound up in a roll, the shape of the protrusions 8 may be transferred to the adherend, reducing the adhesive strength, or when the film 16 is attached to the adherend and then wound up in a roll, the shape of the protrusions may be transferred to the surface of the adherend. It is preferable to use soft LDPE or LLDPE for the layer forming the protrusions 8, as these problems are less likely to occur. In addition, by making the arithmetic mean roughness Ra of the surface of these resins 0.1 μm or less, they can exert adhesive force on a smooth adherend without adding additives such as adhesives. This is preferable because when a resin such as LDPE or LLDPE is used on the adhesive surface, the adhesive is prevented from remaining on the surface of the adherend due to bleeding out of the adhesive when the surface protection film 101 is peeled off. On the other hand, other resins can be used for layers other than the layer forming the protrusions 8 and the layer forming the adhesive surface. For example, if the rigidity is insufficient when the film 16 is formed only from LDPE or LLDPE, the rigidity can be increased by using high density polyethylene or polypropylene. In the surface protection film 101 of the present invention, a certain degree of rigidity may be preferable because it is less likely to cause process problems such as wrinkles and curls and is easier to use. EXAMPLES
[0052] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Various evaluation and measurement methods are also shown below.
[0053] [Number of recesses on the surface of the embossing rubber roller] The surface of the embossing rubber roller was observed with a laser microscope (OLS4100, manufactured by Olympus Corporation) and 2 The number of recesses within the range was counted. The recesses were counted at a total of 20 locations over the entire circumference and width of the embossing rubber roller, and the average value was calculated. The magnification for counting was 20 times.
[0054] [Depth of the recesses on the surface of the embossing rubber roller] The embossed surface of the embossing rubber roller was observed with the laser microscope. 2 The depth of the recesses was measured within the range of 0.01 mm, and the average value was calculated. The depth of the recesses was measured at a total of 20 locations around the entire circumference and width of the embossing rubber roller. The magnification for measuring the depth was 20 times. The depth of the recesses was measured as the difference in average height between the deepest part of the recesses and the periphery of the recesses.
[0055] [Number of protrusions on the plastic film surface] The embossed surface of the surface protection film was observed with the laser microscope. 2 The number of protrusions within the range was counted. The protrusions were counted at a total of 20 locations across the entire surface protection film, and the average value was calculated. The counting was performed at a magnification of 20 times.
[0056] [Height of protrusions on plastic film surface] The embossed surface of the surface protection film was observed with the laser microscope. 2 The height of the convex parts within the range was measured and the average value was calculated. The height of the convex parts was measured at a total of 20 points across the entire surface protection film. The magnification for measuring the depth was 20 times. The height of the convex parts was measured as the difference between the highest part of the convex parts and the average height around the convex parts.
[0057] [Haze in plastic films] A surface protection film was produced using a rubber roller for embossing, and the haze of the surface protection film was measured at a total of 10 locations across the film using a haze meter (NDH-5000 manufactured by Nippon Denshoku Industries Co., Ltd.), and the average value was calculated.
[0058] [Transfer to substrate] The plastic film was attached to a retardation film made from acrylic resin, and stored in a rolled-up state at a temperature of 22 to 26°C for 30 days. Thereafter, the film was unrolled and the presence or absence of transfer was visually confirmed.
[0059] [Example 1] A stainless steel core containing a heat transfer medium passage was coated with HTV silicone rubber to a thickness of 8 mm, and then further coated with a PFA heat shrink tube with a thickness of 0.2 mm to create a rubber roller for embossing molding with a surface length of 1.5 m. The surface of the fluororesin layer, which is the outermost layer, was buffed, and then a steel spherical spray material was sprayed to create a concave shape with a depth of 1.6 to 2.0 μm and a width of 1 mm. 2 The embossing roller was sprayed so that the number of depressions per unit area was 4,000 to 4,500. As a result, the shape of the edges of the depressions formed on the surface of the embossing roller was a mixture of circles and ellipses, the depth of the depressions on the surface of the embossing roller was 2.0 μm, and the number of depressions was 1 mm. 2 The number of projections per unit area was 4060. Then, using the rubber roller for embossing that had been produced, a surface protection film mainly composed of LDPE was produced by the method shown in Figure 5. The number of projections, height of the projections, haze, and the presence or absence of transfer to the adherend were measured and confirmed for the surface protection film produced. The projections of the surface protection film were curved.
[0060] [Example 2] An embossing rubber roller was manufactured under the same conditions as in Example 1, and the depth of the recesses was 1.6 to 2.0 μm and 1 mm. 2 The steel spheres were sprayed onto the surface of the embossing rubber roller so that the number of spheres per unit area was 2300 to 2800. As a result, the shape of the edges of the recesses formed on the surface of the embossing rubber roller was a mixture of circles and ellipses, the depth of the recesses on the surface of the embossing rubber roller was 2.0 μm, and the number of recesses was 1 mm.2 The number of protrusions per unit area was 2480. The number of protrusions, the height of the protrusions, the haze, and the presence or absence of transfer to the adherend were measured and confirmed for the produced surface protection film. The protrusions of the surface protection film were curved.
[0061] [Example 3] An embossing rubber roller was manufactured under the same conditions as in Example 1, and the depth of the recesses was 10.2 to 10.6 μm and 1 mm. 2 The steel spheres were sprayed onto the surface of the embossing rubber roller so that the number of spheres was 100 to 500 per unit area. As a result, the shape of the edges of the recesses formed on the surface of the embossing rubber roller was a mixture of circles and ellipses, the depth of the recesses on the surface of the embossing rubber roller was 10.5 μm, and the number of recesses was 1 mm. 2 The number of protrusions per unit area was 140. The number of protrusions, the height of the protrusions, the haze, and the presence or absence of transfer to the adherend were measured and confirmed for the produced surface protection film. The protrusions of the surface protection film were curved.
[0062] [Example 4] An embossing rubber roller was manufactured under the same conditions as in Example 1, and the depth of the recesses was 4.2 to 4.6 μm and 1 mm. 2 The steel spheres were sprayed onto the surface of the embossing rubber roller so that the number of spheres was 500 to 1000 per unit area. As a result, the shape of the edges of the recesses formed on the surface of the embossing rubber roller was a mixture of circles and ellipses, the depth of the recesses on the surface of the embossing rubber roller was 4.5 μm, and the number of recesses was 1 mm. 2 The number of protrusions per unit area was 670. The number of protrusions, the height of the protrusions, the haze, and the presence or absence of transfer to the adherend were measured and confirmed for the produced surface protection film. The protrusions of the surface protection film were curved.
[0063] [Comparative Example 1] As described in Example 1 of Patent Document 1, spherical alumina particles with a volume average particle size of 3.5 μm were added to the RTV silicone rubber raw material so that the raw material did not contain particles with a particle size of 0.8 μm or less or 30 μm or more, and an embossing silicone rubber roller was produced. Furthermore, a surface protection film whose main component is LDPE was produced using the silicone rubber roller for embossing produced. The uneven shape of the surface of the silicone rubber roller for embossing originates from the size of the spherical solid particles contained in the silicone rubber, but since the uneven shape is different from the roller surfaces of Examples 1 to 4, the depth of the recesses could not be measured. Regarding the number of recesses, 2 The number of protrusions, the height of the protrusions, the haze, and the presence or absence of transfer onto the adherend were measured and confirmed for the produced surface protection films.
[0064] [Comparative Example 2] An embossing rubber roller was manufactured under the same conditions as in Example 1, and the depth of the recesses was 1.6 to 2.0 μm and 1 mm. 2 An abrasive made of silica sand was sprayed onto the surface of the embossing rubber roller so that the number of recesses per unit area was 4,000 to 4,500. As a result, the shape of the edges of the recesses formed on the surface of the embossing rubber roller was polygonal or overlapping polygonal shapes, and the internal shape was a polyhedron rather than a curved surface. The depth of the recesses on the surface of the embossing rubber roller was 2.0 μm, and the number of recesses was 1 mm. 2 The number of protrusions per unit area was 4,230. The number of protrusions, the height of the protrusions, the haze, and the presence or absence of transfer to the adherend were measured and confirmed for the manufactured surface protection film. The protrusions of the surface protection film had polygonal or overlapping polygonal edge shapes, and the external shape was polyhedral.
[0065] The results of Examples 1 to 4 and Comparative Examples 1 and 2 are shown in Table 1. The films produced in Comparative Examples 1 and 2 had a haze greater than 60%, whereas the films produced in Examples 1 to 4 all had a haze of 60% or less. Transfer to the adherend occurred only in Comparative Example 2, and in Comparative Example 2, it was also confirmed that the abrasive had stuck into the roller surface. With regard to Examples 1 to 4, in which the haze was 60% or less and no transfer was confirmed, a peeling sound was generated when the film was unwound in Examples 1 to 3, but no peeling sound was generated in Example 4, confirming that the film has high releasability.
[0066] [Table 1] [Industrial Applicability]
[0067] The present invention is not limited to a method for producing a surface protective film, but can also be applied to a method for producing a plastic film having at least one surface embossed, but the scope of application is not limited to these. [Explanation of symbols]
[0068] 1 Fluorine resin layer 2 Rubber layers 3 Core wire 4 Heat transfer passage 5. Bearings 6 Adhesive layer 7 Recess 8 Convex 11 T-die 12 Molten resin 13 Embossing rubber roller 14 Cooling roller 15 Peeling roller 16 Film 17 Cutter 18 Film Edge 19 Edge suction tube 20 Air Roller 21 Film Roll 31 Film roll before embossing 32 Film before embossing 33 Heating methods for plastic films 34 Receiving roller 100 Embossing rubber roller 101 Surface protection film A Film transport direction
Claims
1. A rubber roller for embossing, comprising at least a rubber layer and a fluororesin layer coated on the surface of a core metal at the center of the roller, in that order from the side closest to the core metal, the fluororesin layer being the outermost layer of the rubber roller, and a plurality of curved recesses, the edge of which has a circular or elliptical shape, formed on the surface of the fluororesin layer.
2. The depth of the recess is 2 μm or more and 10 μm or less, and the surface of the fluororesin layer is 1 mm 2 The embossing rubber roller according to claim 1 , wherein the number of the recesses per unit area is 150 to 2,500.
3. A method for producing a plastic film, comprising the steps of: discharging a molten resin from a die; and cooling the molten resin while clamping it between the embossing rubber roller according to claim 1 or 2 and a cooling roller, thereby solidifying the molten resin and obtaining a web-like plastic film.
4. A surface protection film composed of a single layer or multiple layers, at least one of the outermost surfaces having a curved convex portion and a haze of 60% or less.
5. The height of the protrusions is 2 μm or more and 10 μm or less, and the protrusions are formed within 1 mm 2 The surface protective film according to claim 4 , wherein the number of the protrusions per unit area is 150 or more and 2,500 or less.
Citation Information
Patent Citations
Decorative work
JP1980000189A