Method for producing support membrane containing recycled polysulfone
Regenerating the support membrane from recycled polysulfone in composite semipermeable membranes addresses the issue of waste and resource inefficiency by maintaining membrane performance through a method of isolating and recasting the porous support layer.
Patent Information
- Application Number
- JP2023066209
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-25
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The performance of composite semipermeable membranes deteriorates over time, leading to their disposal as industrial waste, which contributes to environmental impact and resource wastage, and they cannot be effectively reused due to the difficulty in separating the base material, porous support layer, and separation functional layer.
A method to regenerate a support membrane by isolating the porous support layer from the composite semipermeable membrane, crushing it, forming a resin solution, and casting it onto a base material to create a new support membrane using recycled polysulfone.
The regenerated support membrane maintains excellent water generation and separation performance, reducing waste and resource consumption while maintaining membrane efficiency.
Smart Images

Figure 2024152173000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a new support membrane using polysulfone contained in a composite semipermeable membrane. [Background technology]
[0002] Polysulfone resins are widely used in various fields such as the medical field, food industry, water treatment industry, etc., due to their high chemical, mechanical, and thermal stability. In the water treatment field, polysulfone resins have the advantage of being easily formed into membranes, and composite semipermeable membranes, which are formed by casting polysulfone resin onto a substrate and providing a separation functional layer on the support membrane, have high salt rejection and high permeation flux, and are therefore widely used in various fields such as the medical field, food manufacturing industry, and water treatment field.
[0003] Specifically, Patent Document 1 discloses a composite semipermeable membrane having a porous support having a nonwoven fabric layer and a polymer porous layer formed on one side of the nonwoven fabric layer, and a separation functional layer provided on the surface of the porous support, and discloses polysulfone as a material for forming the polymer porous layer. Also disclosed is a spiral membrane element including a plurality of membrane leaves with a permeation side channel material interposed between opposing composite semipermeable membranes, a feed side channel material interposed between the membrane leaves, a perforated central tube around which the membrane leaves and the feed side channel material are wound, and a sealing portion for preventing mixing of the feed side channel and the permeation side channel. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication WO2018 / 052124 Brochure Summary of the Invention [Problem to be solved by the invention]
[0005] The performance of the composite semipermeable membrane in a membrane element gradually deteriorates with use, so that membrane elements that no longer meet the required performance are replaced with new ones. Used membrane elements are currently disposed of as industrial waste. The main disposal methods include incineration and landfilling, but as the use of membrane elements increases, the amount of waste will also increase, and it is expected that the impact on the environment will become greater. In addition, there is a growing global demand for waste reduction and effective use of resources, and it is desirable to reuse used membrane elements as well.
[0006] On the other hand, since the performance of used composite semipermeable membranes has deteriorated, they cannot be reused as they are, and since it is difficult to separate the substrate, the porous support layer, and the separation functional layer, used composite semipermeable membranes cannot be reused as materials.
[0007] An object of the present invention is to provide a method for utilizing a used composite semipermeable membrane. [Means for solving the problem]
[0008] In order to achieve the above object, the present invention is characterized by the following configurations (1) to (4). (1) A method for regenerating a new support membrane from a composite semipermeable membrane having a substrate, a porous support layer formed on the substrate from a resin containing polysulfone, and a separation functional layer on the porous support layer, comprising the steps of: (a) isolating a porous support layer by removing a substrate and a separating functional layer from the composite semipermeable membrane; (b) crushing the porous support layer isolated in the step (a) to obtain a crushed material; (c) preparing a resin solution containing the crushed material; (d) casting the resin solution onto a substrate and solidifying it to form a porous support layer; A method for producing a support membrane containing recycled polysulfone, comprising: (2) The method for producing a support membrane according to (1) above, wherein the step (a) includes peeling off the substrate from the porous support layer. (3) The method for producing the support membrane according to (1) or (2) above, wherein the step (a) comprises decomposing the separation functional layer with chlorine. Effect of the Invention
[0009] According to the present invention, the porous support layer of the composite semipermeable membrane can be reused for the production of a new support membrane. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a cross-sectional view showing an example of the composite semipermeable membrane of the present invention. [Diagram 2] FIG. 2 is a partially developed perspective view showing an example of a separation membrane element. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described in detail.
[0012] [1. Composite semipermeable membrane] The structure of the composite semipermeable membrane will be described with reference to FIG.
[0013] The composite semipermeable membrane 1 separates components in a fluid supplied to the surface of the composite semipermeable membrane, and can obtain a permeated fluid that has permeated the composite semipermeable membrane. The composite semipermeable membrane 1 has a support membrane 14 and a separation functional layer 13. The support membrane 14 has a substrate 11 and a porous support layer 12 on the substrate. The composite semipermeable membrane 1 has a supply side surface 17 that faces the separation functional layer 13, and a permeation side surface 18 that faces the substrate 11. Each layer will be described below.
[0014] <Base material> From the viewpoint of strength and fluid permeability, it is preferable to use a fibrous substrate as the substrate 11. As the fibrous substrate, either a long fiber nonwoven fabric or a short fiber nonwoven fabric can be preferably used.
[0015] The nonwoven fabric may be made of polyolefin, polyester, cellulose, etc., and from the viewpoint of shape retention, polyolefin and polyester are preferred. A mixture of a plurality of materials may also be used.
[0016] The thickness of the substrate 11 is preferably set so that the total thickness of the substrate and the porous support layer is within the range of 30 to 300 μm, or within the range of 50 to 250 μm.
[0017] <Porous support layer> The porous support layer 12 is formed from a resin containing polysulfone.
[0018] The porous support layer 12 provides mechanical strength to the composite semipermeable membrane 1, and does not have separation performance for components with small molecular sizes such as ions. The size and distribution of the pores in the porous support layer 12 are not particularly limited. For example, the porous support layer 12 may have uniform and fine pores, or may have a distribution of pore sizes in which the diameter gradually increases from the surface on which the separation functional layer 13 is formed to the other surface. In either case, the projected area circle equivalent diameter of the pores measured using an atomic force microscope or an electron microscope on the surface on which the separation functional layer 13 is formed is preferably 1 nm or more and 100 nm or less. In particular, in terms of interfacial polymerization reactivity and retention of the separation functional layer, the pores on the surface on which the separation functional layer is formed in the porous support layer preferably have a projected area circle equivalent diameter of 3 to 50 nm.
[0019] The thickness of the porous support layer 12 is not particularly limited, but for reasons such as imparting strength to the separation membrane, it is preferably in the range of 15 μm or more and 300 μm or less, and more preferably 20 μm or more and 150 μm or less.
[0020] The morphology of the porous support layer 12 can be observed by a scanning electron microscope, a transmission electron microscope, or an atomic force microscope. For example, when observing by a scanning electron microscope, the porous support layer 12 is peeled off from the substrate 11, and then cut by freeze fracturing to obtain a sample for cross-sectional observation. This sample is thinly coated with platinum, platinum-palladium, or ruthenium tetrachloride, preferably ruthenium tetrachloride, and observed by a high-resolution field emission scanning electron microscope (UHR-FE-SEM) at an acceleration voltage of 3 to 6 kV. As the high-resolution field emission scanning electron microscope, a Hitachi S-900 type electron microscope or the like can be used. Based on the obtained electron microscope photograph, the film thickness of the porous support layer and the diameter of a circle equivalent to the projected area of the surface can be measured.
[0021] The thickness and pore size of the porous support layer are average values, and the thickness of the porous support layer is the average value of 20 measurements at 20 μm intervals in the direction perpendicular to the thickness direction by cross-sectional observation, and the pore size is the average value of the diameters equivalent to the projected area circles measured for 200 pores.
[0022] Next, a method for forming the porous support layer will be described. The porous support layer can be manufactured, for example, by casting a solution of the above-mentioned polysulfone in N,N-dimethylformamide (hereinafter, referred to as DMF) to a certain thickness on the above-mentioned substrate 11, for example, a tightly woven polyester fabric or a nonwoven fabric, and then wet-coagulating it in water.
[0023] For example, a predetermined amount of polysulfone is dissolved in DMF to prepare a polysulfone resin solution of a predetermined concentration, and then the polysulfone resin solution is applied to a substrate made of polyester fabric or nonwoven fabric to a substantially constant thickness, and the solvent on the surface is removed in air for a certain period of time, after which the polysulfone is coagulated in a coagulation liquid to obtain the polysulfone.
[0024] <Separation functional layer> The thickness of the separation functional layer 13 is not limited to a specific value, but is preferably 5 to 3000 nm in terms of separation performance and permeability, and is particularly preferably 5 to 300 nm for reverse osmosis membranes, forward osmosis membranes, and nanofiltration membranes.
[0025] The thickness of the separation functional layer 13 can be measured according to the conventional method for measuring the thickness of a composite semipermeable membrane. For example, the composite semipermeable membrane is embedded in a resin, cut to prepare an ultrathin slice, and the slice is then stained or otherwise processed. The thickness can then be measured by observing the slice with a transmission electron microscope. In addition, when the separation functional layer 13 has a pleated structure, the thickness can be determined by measuring the number of pleats at 20 measurements at 50 nm intervals in the cross-sectional length direction of the pleated structure located above the porous support layer 12, and averaging the measurements.
[0026] A polyamide separation functional layer obtained by polycondensing a polyfunctional amine and a polyfunctional acid halide, an organic-inorganic hybrid functional layer, or the like is preferably used as the separation functional layer 13, because of its excellent performance in separating components in the raw fluid. These separation functional layers can be formed by polycondensing a monomer on a porous support layer.
[0027] For example, the separation functional layer 13 can contain polyamide as a main component. Such a membrane is formed by interfacial polycondensation of a polyfunctional amine and a polyfunctional acid halide by a known method. For example, a polyfunctional amine aqueous solution is applied to a porous support layer, and the excess amine aqueous solution is removed with an air knife or the like, and then an organic solvent solution containing a polyfunctional acid halide is applied to obtain a polyamide separation functional layer.
[0028] The separation functional layer 13 may have an organic-inorganic hybrid structure containing an Si element or the like. The separation functional layer having an organic-inorganic hybrid structure may be, for example, a compound (A) or (B) below: (A) a silicon compound in which a reactive group having an ethylenically unsaturated group and a hydrolyzable group are directly bonded to a silicon atom, and (B) A compound other than the compound (A) having an ethylenically unsaturated group Specifically, the separation functional layer may contain a condensate of the hydrolyzable group of the compound (A) and a polymer of the ethylenically unsaturated group of the compound (A) and / or (B). That is, the separation functional layer may contain A polymer formed by condensation and / or polymerization of only compound (A), Polymers formed by polymerization of only compound (B), and Copolymer of compound (A) and compound (B) The copolymer may contain at least one polymer selected from the group consisting of the following. The polymer includes a condensation product. In the copolymer of the compound (A) and the compound (B), the compound (A) may be condensed via a hydrolyzable group.
[0029] The hybrid structure can be formed by a known method. An example of the method for forming the hybrid structure is as follows. A reaction liquid containing compound (A) and compound (B) is applied to a porous support layer. After removing excess reaction liquid, a heat treatment may be performed to condense the hydrolyzable groups. The ethylenically unsaturated groups of compound (A) and compound (B) may be polymerized by heat treatment, electromagnetic wave irradiation, electron beam irradiation, or plasma irradiation. In order to increase the polymerization rate, a polymerization initiator, a polymerization promoter, etc. may be added when forming the separation functional layer.
[0030] In addition, for any of the separation functional layers, the surface of the membrane may be hydrophilized, for example, with an alcohol-containing aqueous solution or an alkaline aqueous solution, before use.
[0031] [2. Separation Membrane Element] 2, the separation membrane element 10 includes a water collection pipe 6 and a composite semipermeable membrane 1 wound around the water collection pipe 6. The separation membrane element 10 further includes a feed-side flow path material 2, a permeate-side flow path material 4, end plates, and other components.
[0032] The composite semipermeable membrane 1 forms a rectangular envelope membrane 5 with the permeate side facing inward. The envelope membrane 5 has only one side open and the other three sides sealed so that the permeated water can flow into a water collection pipe 6. The permeated water is isolated from the feed water by this envelope membrane.
[0033] The feed-side flow passage material 2 is disposed between the envelope-like membranes 5, i.e., between the feed-side surfaces of the composite semipermeable membrane 1. The feed-side flow passage material 2 and the multiple envelope-like membranes 5 are wrapped around the water collection pipe 6 in an overlapping state.
[0034] The permeate-side flow passage material 4 is disposed inside the envelope-like membrane 5 , that is, between the permeate-side surfaces of the composite semipermeable membrane 1 .
[0035] Raw water (shown as "feed water 7" in the figure) supplied from one end in the longitudinal direction of the separation membrane element 10 is supplied to the composite semipermeable membrane 1 through a flow path formed by the feed-side flow path material 2. Water that has permeated the composite semipermeable membrane 1 (shown as "permeated water 8" in the figure) flows into the water collection pipe 6 through a flow path formed by the permeation-side flow path material 4. Thus, the permeated water 8 is recovered from one end of the water collection pipe 6. Meanwhile, water that has not permeated the composite semipermeable membrane 1 (shown as "concentrated water 9" in the figure) is recovered from the other end of the separation membrane element 1. The separation membrane element 1 shown in FIG. 2 is an example of the configuration of a spiral-type separation membrane element comprising a water collection pipe and a separation membrane wound around the water collection pipe, and the present invention is directed to this form. [4. Method for producing a support membrane containing regenerated polysulfone] (1) A process for obtaining recycled polysulfone from a porous support layer This process is (a) isolating a porous support layer by removing a substrate and a separating functional layer from the composite semipermeable membrane; (b) crushing the porous support layer isolated in the step (a) to obtain a crushed material; has. In the following steps, a used composite semipermeable membrane may be used, or a composite semipermeable membrane that is out of specification and has not been used may be used.
[0036] (Cleaning process) Since organic or inorganic impurities contained in the raw water are attached to the used composite semipermeable membrane, it is preferable to wash it with an acid or an alkali. As the acid, inorganic acids such as dilute hydrochloric acid, dilute sulfuric acid, phosphoric acid, nitric acid, and sodium hydrogen sulfite, and organic acids such as an aqueous oxalic acid solution and an aqueous citric acid solution can be used alone or in a mixture of two or more. As the alkali, an aqueous sodium hydroxide solution, an aqueous sodium hypochlorite solution, and an aqueous sodium carbonate solution can be used alone or in a mixture of two or more. For washing, a method of immersing the composite semipermeable membrane in an aqueous acid or alkali solution alone or alternately for a certain period of time, or a method of circulating an acid or alkali within the separation membrane element can be used.
[0037] In order to improve the cleaning efficiency, the chemical cleaning may be combined with physical cleaning such as backflow cleaning using a pump or air cleaning using a blower.
[0038] Since the support membrane or unused composite semipermeable membrane may contain impurities such as organic solvents, it is preferable to wash the membrane with a water-soluble organic solvent and then rinse the membrane with water.
[0039] (Process for removing the substrate) Among the above-mentioned steps (a), the step of removing the base material will be described.
[0040] When the support membrane includes a substrate and a porous support layer, the substrate and the porous support layer (which may be a laminate of a separation functional layer and a porous support layer) are separated to isolate the porous support layer. Specifically, the substrate may be peeled off from the porous support layer, or the porous support layer (which may be a laminate with a separation functional layer) may be ground to separate it from the substrate. Grinding may be performed using a grinder, a sander, a blaster, or the like. Peeling is particularly preferred because it can remove the substrate efficiently while suppressing noise, odor, and dust in a shorter time than grinding.
[0041] The peeling can be performed by supplying a high-pressure fluid to the permeation side surface (the surface on the substrate side) of the composite semipermeable membrane, or by peeling the interface between the substrate and the porous support layer manually or using a film peeling device, or by using a combination of these methods.
[0042] Furthermore, the step of removing the substrate contained in the composite semipermeable membrane may be carried out either before or after the step of removing the separating functional layer from the composite semipermeable membrane, which will be described later.
[0043] (Step of removing the separation functional layer) Among the above-mentioned steps (a), the step of removing the separation functional layer will be described.
[0044] To isolate the porous support layer from the composite semipermeable membrane, a step of removing the separation functional layer from the laminate of the porous support layer and the separation functional layer is carried out. As a removal method, a method of disassembling the separation functional layer or a method of removing the separation functional layer from the porous support layer by grinding can be used. The specific grinding method is as described above. Disassembly can remove the separation functional layer more easily and efficiently than grinding.
[0045] The decomposition can be performed by contacting the separation functional layer with a chemical that decomposes the separation functional layer but does not decompose the porous support layer, by decomposing the separation functional layer by plasma treatment, or by depolymerization using subcritical water. However, decomposition of the separation functional layer with a chemical is particularly preferred because it can be performed in a short time and at low cost.
[0046] As for the chemicals used for decomposing the separation functional layer, in the case where the separation functional layer is a polyamide separation functional layer formed by polycondensation of a polyfunctional amine and a polyfunctional acid halide, a chemical capable of oxidatively decomposing an amide bond is preferable, and for example, a chlorine-based chemical such as an aqueous sodium hypochlorite solution or an aqueous calcium hypochlorite solution, or an alkaline chemical such as hydrogen peroxide or sodium hydroxide can be used, and these can be used alone or as a mixture of two or more kinds. Among them, the method of removing the separation functional layer by the chlorine decomposition method using an aqueous sodium hypochlorite solution or an aqueous calcium hypochlorite solution is preferable because it is possible to remove the separation functional layer most simply and efficiently while suppressing chemical changes in the polysulfone to be regenerated.
[0047] The method of measuring the presence or absence of chemical changes in polysulfone can be performed by molecular weight distribution measurement, elemental analysis, melting point measurement, differential scanning calorimetry, heat weight loss analysis, nuclear magnetic resonance spectroscopy, infrared spectroscopy, ultraviolet spectroscopy, etc., but it can also be confirmed by processing the recycled polysulfone resin into its original shape and comparing its physical properties before and after the regeneration process. However, no matter which method is used, measurement errors will occur, so in analyses such as molecular weight distribution measurement, elemental analysis, melting point measurement, differential scanning calorimetry, heat weight loss analysis, nuclear magnetic resonance spectroscopy, infrared spectroscopy, and ultraviolet spectroscopy, the error is within 5%, and in the case of processing the recycled polysulfone resin into its original shape and comparing its physical properties before and after the regeneration process, an error of about 10% can be considered to be no chemical change.
[0048] As the pH of the chlorine-based aqueous solution used becomes more acidic, the proportion of the active species, hypochlorous acid, increases and the decomposition efficiency of the separation functional layer increases; however, at the same time, there is a higher risk of promoting corrosion of piping and equipment. Therefore, the pH is preferably in the range of 6.0 to 9.0, and more preferably in the range of 6.5 to 7.5.
[0049] The effective chlorine concentration of the chlorine-based aqueous solution used is preferably in the range of 1% to 15%, more preferably in the range of 3 to 10%, which allows efficient decomposition of the separating functional layer while suppressing decomposition of the chemical itself.
[0050] The higher the temperature of the chlorine-based aqueous solution used, the higher the decomposition efficiency. However, if the temperature is too high, gas will be generated or the decomposition of the chemical itself will be accelerated, making it difficult to control the concentration. Therefore, the temperature is preferably in the range of 10°C to 60°C, and more preferably in the range of 20°C to 40°C.
[0051] The decomposition of the separation functional layer with chemicals can be achieved by a method of immersing the composite semipermeable membrane obtained by disassembling the separation membrane element in an aqueous solution of a chlorine-based chemical for a certain period of time, by continuously or intermittently applying a chlorine-based aqueous solution to the surface of the composite semipermeable membrane, or by circulating an aqueous solution of a chlorine-based chemical within the separation membrane element to remove the separation functional layer.
[0052] The pH, available chlorine concentration, treatment temperature and treatment method of the above chlorine-based aqueous solution can be arbitrarily set depending on the degree of polymerization and thickness of the separating functional layer of the composite semipermeable membrane used.
[0053] (Process for crushing the porous support layer) Step (b) will be described. In order to efficiently dissolve the polysulfone in the solvent, it is preferable to crush the isolated porous support layer before dissolution. A crusher or pulverizer such as a ball mill, a high-speed cutter mill, a roll crusher, a rotary cutter, or a hydraulic cutter is usually used to crush the porous support layer, but it is particularly preferable to use a crushing means such as a high-speed cutter mill, a rotary cutter, or a hydraulic cutter, since it can be crushed finely. In addition, it is preferable to dry the porous support layer to be crushed in advance, since it can be crushed more uniformly.
[0054] By dissolving the crushed particles in a solvent, a polysulfone solution can be obtained in a short period of time.
[0055] (2) Support film formation process This process is (c) preparing a resin solution containing the crushed material; (d) casting the resin solution onto a substrate and solidifying it to form a porous support layer; That is, according to this process, an isolated porous support layer (i.e., regenerated polysulfone) can be used as at least a part of the resin that forms the porous support layer.
[0056] In step (c), the solvent contained in the resin solution, that is, the solvent in which the regenerated polysulfone is dissolved, is exemplified by DMF, as in the above-mentioned method for forming the porous support layer. Since the polysulfone solution obtained by dissolving the regenerated polysulfone in a solvent may contain impurities, a substrate, and a part of the separation functional layer that were not completely removed in the isolation step of the porous support layer, it is preferable to perform a purification step to remove these impurities. Centrifugation and / or filtration can be used to purify the polysulfone resin solution. Filtration, which can be inexpensive and continuously purified, is particularly preferable. The filter material used for filtration may be any filter material that is not corroded by solvents such as DMF and can remove impurities remaining in the regenerated polysulfone resin solution, and may be a felt filter, a membrane filter, a glass filter, a metal mesh, or the like, used alone or in combination.
[0057] The purified regenerated polysulfone resin solution can be poured onto a substrate to a certain thickness and wet-coagulated in water to regenerate a porous support membrane, similar to the method for producing the porous support membrane described above.
[0058] In step (d), the resin solution is cast onto a substrate and then immersed in a coagulation bath that contains a non-solvent for polysulfone, and more specifically, water.
[0059] The regenerated support membrane can be formed by polycondensing monomers on a porous support layer in the same manner as in the method for producing the separation functional layer described above, to form a composite semipermeable membrane. The regenerated composite semipermeable membrane can be used in the medical and food fields, as well as in water treatment membranes.
[0060] By using the polysulfone resin regenerated in the above manner as a part or whole of the support membrane, the polysulfone resin can be easily recycled as a material without changing its physical properties.
[0061] [3. Use of separation membrane elements] The separation membrane elements 10 may be connected in series or in parallel and housed in a pressure vessel to be used as a separation membrane module.
[0062] Furthermore, the above-mentioned separation membrane element and separation membrane module can be combined with a pump for supplying a fluid thereto, a device for pretreating the fluid, etc. to form a fluid separation device. By using this separation device, for example, it is possible to separate feed water into permeated water such as drinking water and concentrated water that did not permeate the membrane, thereby obtaining water suitable for the purpose.
[0063] The higher the operating pressure of the fluid separation device, the higher the removal rate. However, the energy required for operation also increases. In addition, taking into consideration the retention of the supply flow path and permeation flow path of the separation membrane element, the operating pressure when permeating the supply water to the separation membrane module is preferably 0.2 MPa or more and 6 MPa or less.
[0064] As the temperature of the feed water increases, the salt rejection rate decreases, but as the temperature decreases, the membrane permeation flux also decreases. Therefore, the temperature of the feed water is preferably 5°C or higher and 45°C or lower.
[0065] In addition, when the pH of the raw water is in the neutral range, even if the raw water is a liquid with a high salt concentration such as seawater, the formation of scale such as magnesium is suppressed, and deterioration of the membrane is also suppressed.
[0066] <Supplied water> The water supplied to the separation membrane element of this embodiment is not particularly limited, and may be tap water that has been treated in advance, or may be water with a large amount of impurities in the solution, such as seawater, brine, or sewage. For example, when used for water treatment, the raw water (supply water) may be a liquid mixture containing 500 mg / L to 100 g / L of TDS (Total Dissolved Solids), such as seawater, brine, or wastewater. In general, TDS refers to the total dissolved solids content, and is expressed as "mass / volume", but it may also be expressed as "weight ratio" assuming that 1 L is 1 kg. According to the definition, it can be calculated from the weight of the residue after evaporating a solution filtered through a 0.45 μm filter at a temperature of 39.5 to 40.5° C., but it is more convenient to convert it from the practical salinity (S). EXAMPLES
[0067] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. Measurements in the examples and reference examples were carried out as follows.
[0068] (Membrane desalination rate (TDS removal rate)) Seawater (TDS concentration 3.5%) adjusted to a temperature of 25°C and pH 6.5 was supplied to the composite semipermeable membrane at an operating pressure of 5.5 MPa. The practical salinity (S) of the resulting permeate was measured by measuring the electrical conductivity with a Toa Denpa Kogyo Co., Ltd. electrical conductivity meter. The practical salinity thus obtained was regarded as the salt concentration, and the TDS removal rate was calculated using the following formula. Salt rejection rate = 100 x {1-(salt concentration in permeate water / salt concentration in feed water)} (membrane flux) Seawater was used as the feed water, and the membrane permeation flux (m 3 / m 2 / day).
[0069] (Separation membrane element salt rejection rate (TDS removal rate)) Seawater (TDS concentration 3.5%) adjusted to a temperature of 25°C and pH 6.5 was supplied to the spiral separation membrane element at an operating pressure of 5.5 MPa. The practical salinity (S) of the resulting permeate was measured by measuring the electrical conductivity with a Toa Denpa Kogyo Co., Ltd. electrical conductivity meter. The practical salinity thus obtained was regarded as the salt concentration, and the TDS removal rate was calculated using the following formula. TDS removal rate (%) = 100 × {1 - (TDS concentration in permeate water / TDS concentration in feed water)}.
[0070] (Water production volume of separation membrane element) The amount of water permeated when the separation membrane element was operated under the same conditions as in the measurement of salt rejection was calculated as the amount of water produced (m3) per day per separation membrane element. 3 The data are expressed as 100 mg / day.
[0071] (Continuous operation test of separation membrane element) The spiral-type separation membrane element was operated continuously for 30 days at a pressure of 5.5 MPa with seawater (TDS concentration 3.5%) adjusted to a temperature of 25°C and pH 6.5, and then the operation was terminated. The salt rejection rate and water production volume were then measured.
[0072] (Reference example A) A 15.0 wt % polysulfone solution in N,N-dimethylformamide (DMF) was cast onto a nonwoven fabric made of polyester fibers (fiber diameter: 1 decitex, thickness: approximately 90 μm, air permeability: 1 cc / cm2 / sec) at room temperature (25°C) to a thickness of 180 μm, and then immediately immersed in pure water and left for 5 minutes to produce a roll of fiber-reinforced polysulfone support membrane (thickness 130 μm).
[0073] After that, the support membrane roll was unwound, and a polyfunctional amine aqueous solution prepared so that the polyfunctional amine was 5.5 wt% in total and the molar ratio of metaphenylenediamine / 1,3,5-triaminobenzene was 70 / 30 was applied to the polysulfone surface, and after removing excess aqueous solution from the support membrane surface by blowing nitrogen from an air nozzle, a 25°C n-decane solution containing 0.16 wt% trimesic acid chloride was applied so that the surface was completely wet. Then, excess solution was removed from the membrane by air blowing, and the membrane was washed with hot water at 90°C to obtain a separation membrane roll. The membrane performance evaluation of the obtained composite semipermeable membrane showed that the salt rejection rate was 99.82% and the membrane permeation flux was 0.91 m3 / m2 / day.
[0074] The separation membrane sheet was then cut, and a net (thickness: 800 μm, pitch 5 mm x 5 mm) was continuously laminated between the separation membrane sheets folded so that one side was open, as a supply side flow path material, and a urethane-based adhesive (isocyanate:polyol = 1:3) was applied to both longitudinal ends of the perforated water collection pipe of the separation membrane sheet, and then the sheets were stacked to produce six envelope-shaped membranes with a width of 930 mm so that the effective area of the separation membrane element was 8 m2.
[0075] Then, a predetermined portion of the opening side of the envelope-shaped membrane was attached to the outer periphery of a perforated water collection pipe, and further wound in a spiral shape to produce a wound body. After wrapping a film around the outer periphery of the wound body and fixing it with tape, the edges were cut, end plates were attached, and filament winding was performed to produce a 4-inch element.
[0076] The separation membrane element was placed in a cylindrical pressure vessel made of fiber-reinforced plastic, and the salt rejection rate and water production volume were measured by the above-mentioned method. The salt rejection rate was 99.80%, and the water production volume was 6.7 m 3 / day.
[0077] Example 1 The separation membrane element obtained in Reference Example A was continuously operated by the above-mentioned method, and the salt rejection rate and water production volume were measured. The salt rejection rate was 99.80%, and the water production volume was 5.2 m 3 / day. After this continuous operation, dilute sulfuric acid adjusted to pH 1 was passed through the separation membrane element at room temperature (20°C), and the pump was stopped and the element was left to stand for 24 hours. Next, the inside of the separation membrane element was rinsed with RO water, and then an aqueous sodium hydroxide solution adjusted to pH 14 was passed through and circulated at room temperature (20°C), and the pump was stopped and the element was left to stand for 24 hours. After that, the inside of the separation membrane element was rinsed with RO water to remove impurities adhering to the composite semipermeable membrane.
[0078] After washing, the filament windings and end plates of the separation membrane element were removed, and the composite semipermeable membrane was cut out from the separation membrane leaf so as to remove the adhesive portion. The cut composite semipermeable membrane was passed through a film peeling device to remove the substrate contained in the composite semipermeable membrane.
[0079] The composite semipermeable membrane with the substrate removed was immersed in an aqueous sodium hypochlorite solution with an available chlorine concentration of 5% adjusted to pH 7 for 24 hours at room temperature (20°C), and then rinsed with RO water to decompose and remove the polyamide separation functional layer.
[0080] The porous support layer from which the polyamide separation function layer had been decomposed and removed was dried and then crushed with a high-speed cutter mill to obtain regenerated polysulfone resin.
[0081] The crushed regenerated polysulfone resin was then dissolved in 15.0% by weight of polysulfone in N,N-dimethylformamide (DMF), and the solution was filtered and purified using a 400-mesh SUS metal plain-woven filter and a PTFE membrane filter with a pore size of 1 μm. The purified regenerated polysulfone resin solution was made into a support membrane in the same manner as in Reference Example A, and then a separation functional layer was formed to make a composite semipermeable membrane.
[0082] The membrane performance of the regenerated composite semipermeable membrane was evaluated, and the salt rejection rate was 99.78% and the membrane permeation flux was 0.89m 3 / m 2 / day.
[0083] In addition, this regenerated composite semipermeable membrane was made into a separation membrane element in the same manner as in Reference Example A, and placed in a cylindrical pressure vessel made of fiber-reinforced plastic. The salt rejection rate and water production volume were measured by the method described above. The salt rejection rate was 99.76%, and the water production volume was 6.3 m 3 / day.
[0084] Example 2 The separation membrane element obtained in Reference Example A was continuously operated by the above-mentioned method, and the salt rejection rate and water production volume were measured. The salt rejection rate was 99.80%, and the water production volume was 5.2 m 3 / day. After this continuous operation, dilute sulfuric acid adjusted to pH 1 was passed through the separation membrane element at room temperature (20°C), and the pump was stopped and the element was left to stand for 24 hours. Next, the inside of the separation membrane element was rinsed with RO water, and then an aqueous sodium hydroxide solution adjusted to pH 14 was passed through and circulated at room temperature (20°C), and the pump was stopped and the element was left to stand for 24 hours. After that, the inside of the separation membrane element was rinsed with RO water to remove impurities adhering to the composite semipermeable membrane.
[0085] Next, an aqueous solution of sodium hypochlorite with an available chlorine concentration of 5% and adjusted to pH 7 was circulated through the filter at room temperature (20°C), after which the pump was stopped and the filter was left to stand for 24 hours.Then, the inside of the separation membrane element was rinsed with RO water to decompose and remove the polyamide separation functional layer.
[0086] After washing, the filament winding and end plates of the separation membrane element were removed, and the support membrane was cut out from the separation membrane leaf so as to remove the adhesive portion. The cut support membrane was passed through a film peeling device to remove the substrate contained in the support membrane.
[0087] The porous support layer was then dried and crushed with a high-speed cutter mill to obtain regenerated polysulfone resin.
[0088] The crushed regenerated polysulfone resin was then dissolved in 15.0% by weight of polysulfone in N,N-dimethylformamide (DMF), and the solution was filtered and purified using a 400-mesh SUS metal plain-woven filter and a PTFE membrane filter with a pore size of 1 μm. The purified regenerated polysulfone resin solution was made into a support membrane in the same manner as in Reference Example A, and then a separation functional layer was formed to make a composite semipermeable membrane.
[0089] The membrane performance of the regenerated composite semipermeable membrane was evaluated, and the salt rejection rate was 99.77%, and the membrane permeation flux was 0.87m 3 / m 2 / day.
[0090] In addition, this regenerated composite semipermeable membrane was made into a separation membrane element in the same manner as in Reference Example A, and placed in a cylindrical pressure vessel made of fiber-reinforced plastic. The salt rejection rate and water production volume were measured by the method described above. The salt rejection rate was 99.75%, and the water production volume was 6.1 m 3 / day.
[0091] Example 3 The separation membrane element obtained in Reference Example A was continuously operated by the above-mentioned method, and the salt rejection rate and water production volume were measured. The salt rejection rate was 99.80%, and the water production volume was 5.2 m 3 / day.
[0092] After the continuous operation, the filament windings and end plates of the separation membrane element were removed, and the composite semipermeable membrane was cut out from the separation membrane leaf so as to remove the adhesive portion.
[0093] The cut composite semipermeable membrane was immersed in dilute sulfuric acid adjusted to pH 1 at room temperature (20°C) for 24 hours, and then rinsed with RO water. Next, it was immersed in an aqueous sodium hydroxide solution adjusted to pH 14 at room temperature (20°C) for 24 hours, and then rinsed with RO water to remove impurities attached to the composite semipermeable membrane.
[0094] Thereafter, the washed composite semipermeable membrane was passed through a film peeling device to remove the substrate contained in the composite semipermeable membrane.
[0095] Furthermore, the composite semipermeable membrane from which the substrate had been removed was immersed in an aqueous sodium hypochlorite solution with an effective chlorine concentration of 5% adjusted to pH 7 for 24 hours at room temperature (20°C), and then rinsed with RO water to decompose and remove the polyamide separation functional layer.
[0096] The porous support layer from which the polyamide separation function layer had been decomposed and removed was dried and then crushed with a high-speed cutter mill to obtain regenerated polysulfone resin.
[0097] The crushed regenerated polysulfone resin was then dissolved in 15.0% by weight of polysulfone in N,N-dimethylformamide (DMF), and the solution was filtered and purified using a 400-mesh SUS metal plain-woven filter and a PTFE membrane filter with a pore size of 1 μm. The purified regenerated polysulfone resin solution was made into a support membrane in the same manner as in Reference Example A, and then a separation functional layer was formed to make a composite semipermeable membrane.
[0098] The membrane performance of the regenerated composite semipermeable membrane was evaluated, and the salt rejection rate was 99.80%, and the membrane permeation flux was 0.90m 3 / m 2 / day.
[0099] In addition, this regenerated composite semipermeable membrane was made into a separation membrane element in the same manner as in Reference Example A, and placed in a cylindrical pressure vessel made of fiber-reinforced plastic. The salt rejection rate and water production volume were measured by the method described above. The salt rejection rate was 99.80%, and the water production volume was 6.6 m 3 / day.
[0100] As is clear from the results shown above, it can be said that the composite semipermeable membranes having a support membrane made of the regenerated polysulfone resin of Examples 1 to 3 stably have excellent water production performance and separation performance. [Industrial Applicability]
[0101] The present invention is preferably used as a method for regenerating a support membrane made of a polysulfone resin when discarding a used separation membrane element, without incinerating or burying it. Although the present invention has been described in detail using specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. [Explanation of symbols]
[0102] 1 Composite semipermeable membrane 2 Supply side channel material 4 Permeate side channel material 5 Envelope membrane 6 Water collection pipe 7 Supply water 8 Permeate water 9 Concentrated water 10 Separation membrane element 11 Base material 12 Porous support layer 13 Separation functional layer 14 Support membrane 17 Supply side 18 Transmitting side surface
Claims
1. A method for regenerating a new support membrane from a composite semipermeable membrane having a substrate, a porous support layer formed on the substrate from a resin containing polysulfone, and a separation functional layer on the porous support layer, comprising the steps of: (a) isolating a porous support layer by removing a substrate and a separating functional layer from the composite semipermeable membrane; (b) crushing the porous support layer isolated in the step (a) to obtain a crushed material; (c) preparing a resin solution containing the crushed material; (d) casting the resin solution onto a substrate and solidifying it to form a porous support layer; A method for producing a support membrane containing recycled polysulfone, comprising:
2. The step (a) includes peeling the substrate from the porous support layer. A method for producing the support membrane according to claim 1 .
3. The step (a) includes decomposing the separation functional layer with chlorine. A method for producing the support membrane according to claim 1 or 2.
Citation Information
Patent Citations
Spiral membrane element
WO2018052124A1