Recycled base material manufacturing method

A laminate with an anchor layer and cured ink layer on non-absorbing substrates allows for efficient deinking by dissolving the anchor layer in an alkaline solution, improving recyclability and reducing environmental impact.

JP2024152215AActive Publication Date: 2024-10-25TOYO INK MFG CO LTD +1

Patent Information

Application Number
JP2023066274
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-25
Estimated Expiration
2043-04-14

AI Technical Summary

Technical Problem

Existing methods are inadequate for recycling non-absorbing substrates coated with active energy ray-curable inks and varnishes, particularly due to difficulties in separating and removing these coatings, which leads to reduced recyclability and increased environmental impact.

Method used

A laminate structure is developed with an anchor layer containing an aqueous resin and a cured ink layer of active energy ray-curable inks, where the anchor layer is dissolved in an alkaline solution to facilitate easy removal of the ink layer from non-absorbing substrates.

Benefits of technology

The laminate exhibits excellent blocking resistance, scratch resistance, and effective deinking properties, enhancing the recyclability of non-absorbing substrates coated with active energy ray-curable inks and varnishes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152215000001
    Figure 2024152215000001
  • Figure 2024152215000002
    Figure 2024152215000002
  • Figure 2024152215000003
    Figure 2024152215000003
Patent Text Reader

Abstract

To provide a laminate that has excellent physical properties such as blocking resistance and scratch resistance as the laminate, has an excellent deinking property in a recycling process of non-absorbent base material, and is obtained by using an active energy ray-curable ink, and a manufacturing method for a laminate, and to provide a method for deinking the laminate.SOLUTION: There is provided a laminate having an anchor layer and an ink layer in this order on a non-absorbing base material, wherein the anchor layer contains an aqueous resin; and the aqueous resin has an acid value of 25 to 300 mgKOH / g and a glass transition temperature of 10 to 150°C; and the ink layer is a cured product of at least one ink selected from an active energy ray-curable offset printing ink, an active energy ray-curable flexographic printing ink, and an active energy ray-curable resin letterpress printing ink.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate, a method for manufacturing a laminate, and a method for deinking a laminate. [Background technology]

[0002] Compared to oxidative polymerization, penetration drying, and hot air drying oil-based inks and varnishes, active energy ray curing inks and varnishes are convenient in that they cure instantly, have the ability to form a strong cured film, and are non-VOC, containing no petroleum-based volatile compounds. As a result, they are widely used in the package printing industry for applications ranging from beverage and food packaging, pharmaceutical packaging, and cosmetic packaging, to general paper containers.

[0003] In the food packaging field in particular, the ideal form of active energy ray curable ink / varnish would be electron beam (hereafter also referred to as "EB") curable ink, which does not contain photopolymerization initiators and takes into consideration safety and security for humans and the environment; however, due to the large initial capital investment required, it is difficult to say that this is common, and ultraviolet ray (hereafter also referred to as "UV") curable ink is more prevalent on the market.

[0004] In recent years, it is known that there has been a gradual shift to LED curing systems that use UV-LED light sources that are energy-saving and suppress the generation of ozone and heat, energy-saving UV systems that use a single metal halide lamp that eliminates the infrared range that generates heat and the ultraviolet range that generates ozone, and energy-saving UV systems that reduce the number of UV lamps from the usual 3 to 4 to just 1.

[0005] Energy-saving UV-curable inks and varnishes designed to accommodate these new systems have recently been increasingly replaced by ordinary oil-based inks and varnishes, especially in commercial printing, and are required to have the same performance as ordinary oil-based inks and varnishes, including printability and print quality. An increasing number of inks are being certified as "recyclable UV-curable inks" with a rank A certification for recyclability. However, not all UV systems on the market will be replaced by energy-saving UV systems, and many still use conventional UV systems (many of which are rated B in recyclability). UV-curable inks and varnishes are generally considered to be more difficult to recycle than general oil-based inks and varnishes, except for recyclable energy-saving UV-curable inks and some recyclable UV-curable inks. In order to simplify recycling when collecting printed materials, it is considered to be extremely difficult and nearly impossible to separate printed materials that are printed with non-recyclable UV-curable or other active energy ray-curable inks and varnishes.

[0006] Similarly, there is an urgent need to develop methods to make it easier to recycle substrates, even if they are non-absorbent substrates other than paper. This is because in recent years, UV curing devices, UV-LED curing devices, and EB curing devices that are less susceptible to heat have been developed, and even if the substrate is thin, it is now possible to irradiate it with active energy rays without causing thermal damage, resulting in an increase in the use of active energy ray-curable inks and varnishes.

[0007] In particular, measures against marine pollution are required as part of global environmental measures for plastic substrates, and there is an urgent need to develop a plastic recovery system that does not allow microplastics, which cause marine pollution, to flow into the ocean. Compared to chemical recycling, which chemically decomposes and reuses materials such as plastics, material recycling, which pelletizes and reuses materials, is easier and more convenient. However, if the active energy ray-curable ink / varnish is not removed from the substrate, the remaining ink / varnish will get into the melting process of the substrate, making it difficult for the substrate to return to its original color, and there is a high possibility that the uses of the recycled substrate will be limited. Therefore, the development of a simple method to remove additives such as active energy ray-curable ink / varnish and adhesives from packaging materials such as plastics will lead to an increase in the efficiency of material recycling.

[0008] Furthermore, if it becomes possible to easily remove active energy ray-curable inks and varnishes from all non-absorbing substrates, not only soft packaging materials but also hard plastic substrates such as PET bottle caps, nonwoven fabrics and metals, and thereby easily reuse the substrate materials, it will be possible to reduce the use of fossil resources by improving recycling efficiency, and ultimately contribute to a reduction in carbon dioxide emissions.

[0009] For example, Patent Document 1 discloses an organic solvent-based ink for a release layer that can be removed by alkali treatment, a laminate such as a printed matter that includes a release layer using this ink, and a method for recycling this laminate. However, the ink that can be removed is limited to ink that uses a solvent, and there is no simple deinking method for active energy ray-curable ink that is generally considered to be solvent-free, so there is a need to establish a printed matter that is excellent in deinking suitability using a general active energy ray-curable ink / varnish, and a method for manufacturing the printed matter.

[0010] Patent Document 2 refers to an aqueous anchoring agent for a release layer that can be removed by alkali treatment, and a laminate such as a printed matter that includes a release layer using this. However, the substrate that can be removed is limited to paper or synthetic paper, and the technology has not been established for non-absorbent substrates such as plastics. In particular, in the case of non-absorbent substrates such as plastics compared to paper substrates, the adhesion between the substrate and the anchor layer, and the blocking resistance of the anchor layer (blocking in areas where ink is not printed on the anchor layer, and blocking when the substrate is rolled up or stacked before printing the ink) are major issues. Among these, active energy ray curable offset printing inks, active energy ray curable flexographic printing inks, and active energy ray curable resin letterpress printing inks have high film strength among active energy ray curable inks, and are difficult to deink, so there is a demand for anchor agents that can be deinked even when these inks are used. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] JP 2020-090627 A [Patent Document 2] Patent No. 7070772 Summary of the Invention [Problem to be solved by the invention]

[0012] The object of the present invention is to provide a laminate which has excellent physical properties as a laminate, such as blocking resistance and scratch resistance, and which has excellent deinking properties in the recycling process of non-absorbing substrates, using an active energy ray-curable ink, and a method for producing said laminate, as well as to provide a method for deinking said laminate. [Means for solving the problem]

[0013] Means for Solving the Problems The present inventors conducted extensive research to solve the above problems and, as a result, discovered that the above problems can be solved by the laminate and the method for producing the laminate described below, thereby completing the present invention.

[0014] That is, the present invention provides a laminate having an anchor layer and an ink layer in this order on a non-absorbing substrate, The anchor layer comprises an aqueous resin, The acid value of the aqueous resin is 25 to 300 mgKOH / g; The glass transition temperature of the aqueous resin is 10 to 150° C., The present invention relates to a laminate, wherein the ink layer is a cured product of at least one type of ink selected from an active energy ray-curable offset printing ink, an active energy ray-curable flexographic printing ink, and an active energy ray-curable resin letterpress printing ink.

[0015] The present invention also relates to the above laminate, wherein the aqueous resin comprises at least one resin selected from the group consisting of an aqueous acrylic resin and an aqueous urethane resin.

[0016] The present invention also provides a method for producing a laminate, comprising the steps of: A step 1 of applying an anchor agent containing water and an aqueous resin to a non-absorbent substrate and drying the applied agent in an oven to obtain a laminate having an anchor layer on the substrate; a step 2 of printing at least one ink selected from an active energy ray-curable offset printing ink, an active energy ray-curable flexographic printing ink, and an active energy ray-curable resin letterpress printing ink on the anchor layer of the laminate having an anchor layer on the non-absorbing substrate, and curing the ink with active energy rays to obtain a laminate having an ink layer on the anchor layer; Including, The acid value of the aqueous resin is 25 to 300 mgKOH / g; The aqueous resin has a glass transition temperature of 10 to 150°C.

[0017] The present invention also relates to a method for producing the above laminate, wherein the aqueous resin comprises at least one resin selected from the group consisting of an aqueous acrylic resin and an aqueous urethane resin.

[0018] The present invention also provides a method for deinking a laminate having an anchor layer and an ink layer, in that order, on a non-absorbing substrate, comprising the steps of: The anchor layer comprises an aqueous resin, The acid value of the aqueous resin is 25 to 300 mgKOH / g; The glass transition temperature of the aqueous resin is 10 to 150° C., the ink layer is a cured product of at least one ink selected from an active energy ray-curable offset printing ink, an active energy ray-curable flexographic printing ink, and an active energy ray-curable resin letterpress printing ink, The present invention relates to a method for deinking a laminate, in which the laminate is stirred in an alkaline aqueous solution, the anchor layer is dissolved in the alkaline aqueous solution, and the ink layer is deinked from the non-absorbing substrate.

[0019] The present invention also relates to a method for deinking the above laminate, wherein the aqueous resin comprises at least one selected from the group consisting of an aqueous acrylic resin and an aqueous urethane resin.

[0020] The present invention also relates to a method for recovering ink, which comprises filtering and recovering the ink layer deinked by the above-mentioned deinking method. Effect of the Invention

[0021] The present invention has made it possible to provide a laminate which has excellent physical properties as a laminate, such as blocking resistance and scratch resistance, and which also has excellent deinking properties in the recycling process of non-absorbent substrates using an active energy ray-curable ink, a method for producing said laminate, and a method for deinking said laminate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The present invention will be described in detail below. Note that the present invention is not limited to the following embodiments, and can be practiced with various modifications within the scope of the spirit of the invention. In addition, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".

[0023] The present invention is a laminate having an anchor layer and an ink layer in this order on a non-absorbing substrate, in which the anchor layer is a layer obtained by drying an aqueous anchor agent containing an aqueous resin in an oven, and the ink layer is a layer obtained by curing an active energy ray-curable ink with active energy rays.

[0024] As described below, if the ink does not contain a colorant, it becomes varnish (also called clear ink), and the ink layer becomes a varnish layer (clear ink layer).

[0025] <Ink layer> <Active energy ray curable ink> The ink layer of the present invention is a cured product of at least one ink (also referred to as "active energy ray curable ink") selected from active energy ray curable offset printing ink, active energy ray curable flexographic printing ink, and active energy ray curable resin letterpress printing ink. The active energy ray curable ink (also referred to as "ink") will be described below.

[0026] The active energy ray-curable ink of the present invention is at least one type of ink selected from the group consisting of active energy ray-curable ink for offset printing, active energy ray-curable ink for flexographic printing, and active energy ray-curable ink for resin letterpress printing. These active energy ray curable offset printing inks, active energy ray curable flexographic printing inks, and active energy ray curable resin letterpress printing inks are inks that have high film strength and are considered to be difficult to deink, even among active energy ray curable inks.

[0027] [Coloring agent] In the present invention, the ink may contain a colorant. As the colorant, at least one of a pigment and a dye may be used. From the viewpoint of light resistance, a pigment is preferred. The pigment that can be used in the present invention is not particularly limited, and any known pigment can be used. The pigment can be either an inorganic pigment or an organic pigment. If the ink does not contain colorant, it becomes a varnish (clear ink).

[0028] Examples of inorganic pigments include carbon blacks such as furnace black, lamp black, acetylene black, and channel black, iron oxide, and titanium oxide.

[0029] Examples of organic pigments include soluble azo pigments such as β-naphthol, β-oxynaphthoic acid, β-oxynaphthoic acid anilide, acetoacetate anilide, and pyrazolone; Examples of the pigments include insoluble azo pigments such as β-naphthol, β-oxynaphthoic acid anilide, acetoacetate anilide monoazo, acetoacetate anilide disazo, and pyrazolone; phthalocyanine pigments such as copper phthalocyanine blue, halogenated (e.g., chlorinated or brominated) copper phthalocyanine blue, sulfonated copper phthalocyanine blue, and metal-free phthalocyanine; and polycyclic pigments and heterocyclic pigments such as quinacridone, dioxazine, threne (pyranthrone, anthranthrone, indanthrone, anthrapyrimidine, flavanthrone, thioindigo, anthraquinone, perinone, perylene, etc.), isoindolinone, metal complex, quinophthalone, and diketopyrrolopyrrole.

[0030] More specifically, in terms of the CI color index, black pigments include CI Pigment Black 1, 6, 7, 9, 10, 11, 28, 26, 31, and the like.

[0031] Examples of white pigments include CI Pigment White 5, 6, 7, 12, and 28.

[0032] Examples of yellow pigments include CI Pigment Yellow 1, 2, 3, 12, 13, 14, 16, 17, 18, 24, 73, 74, 75, 83, 93, 95, 97, 98, 100, 108, 109, 110, 114, 120, 128, 129, 138, 139, 174, 150, 151, 154, 155, 167, 174, 176, 180, 185, and 213.

[0033] Blue or cyan pigments include CI Pigment Blue 1, 2, 14, 15, 15:1, 15:2, 15:3, 15:4, 60, 62, and the like.

[0034] Red or crimson pigments include CI Pigment RED 1, 3, 5, 19, 21, 22, 31, 38, 42, 43, 48:1, 48:2, 48:3, 48:4, 48:5, 49:1, 50, 52, 53:1, 57:1, 57:2, 58:4, 63:1, 81, 81:1, 81:2, 81:3, 81:4, 83, 90, 104, 108, 11 2, 114, 122, 144, 146, 148, 149, 150, 166, 168, 169, 170, 172, 173, 176, 177, 178, 184, 185, 187, 193, 202, 209, 214, 242, 254, 255, 264, 266, 269, CI Pigment Violet 19, etc.

[0035] Green pigments include CI Pigment Green 1, 2, 3, 4, 7, 8, 10, 15, 17, 26, 36, 45, 50, and the like.

[0036] Purple pigments include CI Pigment Violet 1, 2, 3, 4, 5:1, 12, 13, 15, 16, 17, 19, 23, 25, 29, 31, 32, 36, 37, 39, and 42. Orange pigments include CI Pigment Orange 13, 16, 20, 34, 36, 38, 39, 43, 51, 61, 63, 64, 74, and the like.

[0037] In the present invention, the above pigments may be used alone or in combination of two or more.

[0038] In the present invention, the pigment can be used in any content as long as the desired concentration can be reproduced on the surface of the printing substrate, and the content is preferably 5 to 30 mass % and more preferably 10 to 25 mass % based on the total amount of the ink.

[0039] [(Meth)acrylate compounds] In this specification, unless otherwise specified, "(meth)acryloyl", "(meth)acrylic acid", "(meth)acrylate", and "(meth)acryloyloxy" respectively mean "acryloyl and / or methacryloyl", "acrylic acid and / or methacrylic acid", "acrylate and / or methacrylate", and "acryloyloxy and / or methacryloyloxy". In addition, "PO" stands for "propylene oxide" and "EO" stands for "ethylene oxide". In addition, X in EO-modified (X) and PO-modified (X) represents the number of moles of EO and PO modified, and Y in polyethylene glycol (Y) di(meth)acrylate represents the approximate molecular weight of the polyethylene glycol portion.

[0040] The active energy ray-curable ink of the present invention contains a (meth)acrylate compound. The (meth)acrylate compound that can be used in the present invention is not particularly limited as long as it is a compound having one or more (meth)acryloyl groups, and includes any form of monomer, oligomer, or polymer. Here, the term "monomer" refers to a compound that is the minimum structural unit for constituting an oligomer or a polymer, and the term "oligomer" refers to a polymer having structural units based on 2 to 100 monomers.

[0041] Specific examples of the (meth)acrylate compound used in the present invention include the compounds shown below.

[0042] [(Meth)acrylate compounds] (monomer) 2-Ethylhexyl (meth)acrylate, 2-Hydroxyethyl (meth)acrylate, 2-Hydroxypropyl (meth)acrylate, β-Carboxylethyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, tetrahydrofurfuryl acrylate, alkoxylated tetrahydrofurfuryl acrylate, caprolactone (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isoamyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, isodecyl (meth)acrylate, 3,3,5-trimethylcyclohexanol (meth)acrylate ) acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, norbornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (oxyethyl) (meth)acrylate, 1,4-cyclohexanedimethanol (meth)acrylate, cyclic trimethylolpropane formal (meth)acrylate, benzyl (meth)acrylate, EO-modified (2) nonylphenol acrylate, 2-methyl-2-ethyl-1,3-dioxolan-4-yl) methyl acrylate, and other monofunctional (meth)acrylate monomers having one (meth)acryloyl group in the molecule; 1,3-butylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, 1,2-dodecanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol (200) di(meth)acrylate, polyethylene glycol (300) di(meth)acrylate, polyethylene glycol (400) di(meth)acrylate, polyethylene glycol (600) di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate , dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, EO-modified (2) 1,6-hexanediol di(meth)acrylate, PO-modified (2) neopentyl glycol di(meth)acrylate, (neopentyl glycol-modified) trimethylolpropane di(meth)acrylate, dimethyloltricyclodecane di(meth)acrylate, EO-modified (4) bisphenol A di(meth)acrylate, PO-modified (4) bisphenol A di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, dimethylol-tricyclodecane di(meth)acrylate, dicyclopentanyl di(meth)acrylate, and other bifunctional (meth)acrylate monomers having two (meth)acryloyl groups in the molecule; Trimethylolpropane tri(meth)acrylate, EO modified (3) trimethylolpropane tri(meth)acrylate, EO modified (6) trimethylolpropane tri(meth)acrylate, PO modified (3) trimethylolpropane tri(meth)acrylate, trifunctional (meth)acrylate monomers having three (meth)acryloyl groups in the molecule, such as pentaerythritol tri(meth)acrylate, Pentaerythritol tetra(meth)acrylate, EO-modified (4) pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, and other tetrafunctional (meth)acrylate monomers having four acryloyl groups in the molecule; Pentafunctional (meth)acrylate monomers having five (meth)acryloyl groups in the molecule, such as dipentaerythritol penta(meth)acrylate; and hexafunctional (meth)acrylate monomers having six (meth)acryloyl groups in the molecule, such as dipentaerythritol hexa(meth)acrylate.

[0043] (Oligomer) Examples of the oligomer include urethane acrylate oligomers such as aliphatic urethane acrylate oligomers and aromatic urethane acrylate oligomers, acrylic ester oligomers, polyester acrylate oligomers, and epoxy acrylate oligomers having 1 to 6 (meth)acryloyl groups. [Other ingredients] In the present invention, the ink may contain, if necessary, in addition to the above-mentioned components, a polymerization initiator, an amine compound, a resin, a polymerization inhibitor, a surface tension adjuster, a wax, an extender pigment, a pigment dispersant, an antifoaming agent, an ultraviolet absorber, an antioxidant, an antistatic agent, and the like.

[0044] (Polymerization initiator) In the present invention, the ink may contain a polymerization initiator. The polymerization initiator preferably contains a polymerizable initiator for radical or cationic polymerization, and more preferably contains a photopolymerization initiator. The polymerization initiator in the present invention is a compound that undergoes a chemical change through the action of light or through interaction with the electronically excited state of the sensitizing dye to generate radicals or cations, and among these, a photoradical polymerization initiator is preferable from the viewpoint of being able to initiate polymerization by exposure to light.

[0045] In the present invention, the photo-radical polymerization initiator is not particularly limited, and known ones can be used. Specific examples include benzophenone compounds, dialkoxyacetophenone compounds, α-hydroxyalkylphenone compounds, α-aminoalkylphenone compounds, acylphosphine oxide compounds, oxime ester compounds, and thioxanthone compounds. The photo-polymerization initiator may be used alone or in combination of two or more.

[0046] Benzophenone compounds include benzophenone, 2-methylbenzophenone, 3-methylbenzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 4-phenylbenzophenone, 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(dimethylamino)benzophenone, [4-(methylphenylthio)phenyl]-phenylmethanone, 2-chloro-4-phenyl-benzophenone, 1-{4-[(4-benzoylphenylsulfanyl)phenyl]-2-methyl-2-(4-methylbenzenesulfonyl)propan-1-one, and polybutylene glycol bis(4-benzoylphenoxy)acetate.

[0047] Examples of the dialkoxyacetophenone compounds include 2,2-dimethoxy-2-phenylacetophenone, dimethoxyacetophenone, and diethoxyacetophenone.

[0048] The α-hydroxyalkylphenone compounds include 1-hydroxy-cyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxymethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, oligo[2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone], 2,3-dihydro-6-(2-hydroxy-2-methyl-1-oxopropyl)-1,1,3-trimethyl-3-[4-(2-hydroxy-2-methyl- 2-hydroxy-1-[4-[4-(2-hydroxy-2-methyl-1-oxopropyl)phenyl]-1H-indene and 2,3-dihydro-5-(2-hydroxy-2-methyl-1-oxopropyl)-1,1,3-trimethyl-3-[4-(2-hydroxy-2-methyl-1-oxopropyl)phenyl]-1H-indene mixture, 2-hydroxy-1-[4-[4-(2-hydroxy-2-methylpropynyl)benzyl]phenyl]-2-methylpropan-1-one, 2-hydroxy-1-[4-[4-(2-hydroxy-2-methylpropanoyl)phenoxy]phenyl]-2-methylpropan-1-one, 1-[4-(1,1-dimethylethyl)phenyl]-2-hydroxy-2-methylpropan-1-one, and the like.

[0049] Examples of α-aminoalkylphenone compounds include 2-methyl-1-[4-(methoxythio)-phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone, 1,2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, and 1-(9,9-dibutyl-9H-fluoren-2-yl)-2-methyl-2-morpholinopropan-1-one. phospho-4-yl-propan-1-one, polyethylene glycol di(β-4-[4-(2-dimethylamino-2-benzyl)butanonylphenyl]piperazine)propionate, 2-benzyl-2-dimethylamino-1-(4-piperidinylphenyl)-1-butanone, 1-(biphenyl-4-yl)-2-methyl-2-morpholinopropan-1-one, 1-(biphenyl-4-yl)-2-methoxy-2-morpholinopropan-1-one, and the like.

[0050] Examples of the acylphosphine oxide compound include diphenylacylphenylphosphine oxide, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, tris(phenyl(2,4,6-trimethylbenzoyl)phosphinic acid) polyethylene glycol ester, ethyl(2,4,6-trimethylbenzoyl)phenylphosphineate, and bis(2,4,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide.

[0051] The oxime ester compounds include 1-[4-(phenylthio)phenyl]octane-1,2-dione, 2-benzoyl oxime, ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(o-acetyl oxime), 3-cyclopentyl-1-(4-(phenylthio)phenyl)propane-1,2-dione-2-(o-benzoyl oxime), 1-[9-ethyl-6-(2-methylbenzoyl)-9H -carbazol-3-yl]-3-cyclopentylpropane-1-(o-acetyloxime), methanone, [8-[[(acetyloxy)imino][2-(2,2,3,3-tetrafluoropropoxy)phenyl]methyl]-11-(2-ethylhexyl)-11H-benzo[a]carbazol-5-yl]-, (2,4,6-trimethylphenyl), 1-phenyl-1,2-propanedione-2-(o-ethoxycarbonyl)oxime, and the like.

[0052] Examples of thioxanthone compounds include 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2,4-dichlorothioxanthone, 1-chloro-4-propylthioxanthone, 2-chlorothioxanthone, poly(oxy-1,4-butanediyl), α-[2-[(9-oxo-9H-thioxanthenyl)oxy]acetyl]-ω-[[2-[(9-oxo-9H-thioxanthenyl)oxy]acetyl]oxy]-, 1,3-di({α-[1-chloro-9-oxo-9H-thioxanthen-4-yl]oxy}acetylpoly[oxy(1-methylethylene)])oxy]-2,2-bis({α-[1-chloro-9-oxo-9H-thioxanthen-4-yl]oxy}acetylpoly[oxy(1-methylethylene)])oxymethyl)propane, and the like.

[0053] The content of the photopolymerization initiator is preferably from 1 to 20% by mass, and more preferably from 5 to 15% by mass, based on the total amount of the ink.

[0054] (Amine compounds) In the present invention, the ink may contain an amine compound. There is no particular limitation on the amine compound, and any known amine compound can be used. By using the amine compound as a component of the active energy ray-curable ink, it is expected that the effect of the hydrogen abstraction type photopolymerization initiator can be enhanced. Specific examples include N,N-dimethylaniline, N,N-diethylaniline, N,N-dimethyl-p-toluidine, ethyl 4-(dimethylamino)benzoate, N,N-dihydroxyethylaniline, triethylamine and N,N-dimethylhexylamine, poly(oxy-1,2-ethanediyl,α-[4-(dimethylamino)benzoyl]-ω-[[4-(dimethylamino)benzoyl]oxy]-, bis-N,N-[2-(4-dimethylaminobenzoyl)oxyethylene-1-yl ]methylamine, poly(oxy-1,2-ethanediyl), α-[4-(dimethylamino)benzoyl]-ω-[[4-(dimethylamino)benzoyl]oxy]-, poly[oxy(methyl-1,2-ethanediyl), α-[4-(dimethylamino)benzoyl-ω-butoxy-, 2-butoxyethyl-4-(dimethylamino)benzoate, 2-(dimethylamino)ethyl benzoate, etc. The amine compounds may be used alone or in combination of two or more kinds.

[0055] (resin) In the present invention, the ink may contain a resin, which reduces the cure shrinkage of the coating film that occurs during curing, suppresses curling of the substrate, and improves adhesion to the anchoring agent.

[0056] The resins may be used alone or in combination of two or more kinds. The content of the resin is preferably 1 to 20% by mass based on the total mass of the ink.

[0057] Specific examples of the resin include polyvinyl chloride, (meth)acrylic resin, styrene (meth)acrylic resin, epoxy resin, polyester resin, polyurethane resin, cellulose derivatives (e.g., ethyl cellulose, cellulose acetate, nitrocellulose), vinyl chloride-vinyl acetate copolymer, polyamide resin, polyvinyl acetal resin, diallyl phthalate resin, alkyd resin, rosin-modified alkyd resin, petroleum resin, urea resin, synthetic rubber such as butadiene-acrylonitrile copolymer, etc. Among them, diallyl phthalate resin and polyester resin are more preferable from the viewpoint of dispersibility.

[0058] (Polymerization inhibitor) In the present invention, the ink may contain a polymerization inhibitor, specific examples of which include 4-methoxyphenol, hydroquinone, methylhydroquinone, t-butylhydroquinone, 2,6-di-t-butyl-4-methylphenol, phenothiazine, and aluminum salt of N-nitrosophenylhydroxylamine.

[0059] The content of the polymerization inhibitor is preferably 0.01 to 2% by mass relative to the total mass of the ink, from the viewpoint of increasing the stability of the ink while maintaining the curability.

[0060] (wax) In the present invention, the ink may contain wax. By containing wax, it is possible to improve the abrasion resistance, scratch resistance, blocking prevention, smoothness, and scratch prevention. There is no particular limitation on the wax, and any known wax can be used. For example, natural wax and synthetic wax can be used. Examples of natural waxes include carnauba wax, Japan wax, lanolin, montan wax, paraffin wax, and microcrystalline wax. Examples of synthetic waxes include Fischer-Tropsch wax, polyethylene wax, polypropylene wax, and polytetrafluoroethylene wax.

[0061] The content of the wax is preferably 0.1 to 5% by mass based on the total mass of the ink.

[0062] (Extender pigment) In the present invention, the ink may contain an extender pigment, such as clay, talc, barium sulfate, calcium carbonate, ground calcium carbonate, barium carbonate, magnesium carbonate, silica, or bentonite.

[0063] (Pigment dispersant) In the present invention, the ink preferably contains a pigment dispersant in order to improve the pigment dispersibility. There is no particular limitation on the pigment dispersant, and any known pigment dispersant can be used. Among them, a resin-type pigment dispersant having a basic functional group is preferable, and examples of the basic functional group include a primary, secondary, or tertiary amino group, and nitrogen-containing heterocycles such as pyridine, pyrimidine, and pyrazine. Further, as the skeleton constituting the resin-type pigment dispersant, a fatty acid amine skeleton and / or a urethane skeleton are more preferable since good pigment dispersibility can be easily obtained.

[0064] Examples of the pigment dispersant include the Ajisper series (Ajisper PB821, PB822, PB824, etc.) manufactured by Ajinomoto Fine-Techno Co., Ltd., the Solsperse series (Solsperse 00, Solsperse 32000, Solsperse 38500, etc.) manufactured by Lubrizol, and the Disperbyk series (BYK-162, BYK-168, BYK-183, etc.) manufactured by BYK-Chemie.

[0065] The content of the pigment dispersant is preferably from 0.1 to 10% by mass, and more preferably from 0.2 to 5% by mass, based on the total mass of the ink.

[0066] The active energy ray curable ink in the present application is preferably at least one ink selected from active energy ray curable offset printing ink, active energy ray curable flexographic printing ink, and active energy ray curable resin letterpress printing ink, because these inks have high film strength and are difficult to deink among active energy ray curable inks, and are inks in which the effects of the present invention are particularly pronounced.

[0067] <Anchor layer> The anchor layer of the laminate of the present invention contains an aqueous resin. Such an anchor layer can be obtained by coating an aqueous anchor agent containing an aqueous resin and drying it.

[0068] [Water-based anchoring agent] The aqueous anchor agent in the present invention contains water and an aqueous resin.

[0069] [Water-based resin] Examples of the aqueous resin in the present invention include an aqueous acrylic resin, an aqueous urethane resin, an aqueous polyester resin, etc. Among them, it is preferable to use an aqueous acrylic resin or an aqueous urethane resin, and it is particularly preferable to use an aqueous acrylic resin.

[0070] [Acid value of water-based resin] The acid value of the aqueous resin is preferably 25 to 300 mgKOH / g. This is because an acid value in this range makes it possible to obtain a resin with good alkali solubility, and improves the deinking properties of UV ink. The acid value of the aqueous resin is preferably 30 to 275 mgKOH / g, and more preferably 30 to 250 mgKOH / g.

[0071] [Glass transition temperature of water-based resin] The glass transition temperature (Tg) of the aqueous resin is preferably 10 to 150°C. When the glass transition temperature is in this range, good anti-blocking performance and good adhesion to the substrate can be obtained. The glass transition temperature (Tg) of the aqueous resin is preferably 10 to 120°C, and more preferably 10 to 100°C.

[0072] [Water-based acrylic resin] The aqueous acrylic resin has an acrylic monomer unit. Furthermore, it is also preferable that the acrylic resin is obtained by copolymerizing a styrene-based monomer, a maleic acid-based monomer, or the like. The acrylic resin preferably has a carboxyl group and is made aqueous in the presence of an emulsifier and / or a basic compound.

[0073] Suitable examples of the acrylic monomer include alkyl esters of (meth)acrylic acid, alkylamides of (meth)acrylic acid, hydroxyalkyl esters of (meth)acrylic acid, etc. The alkyl groups constituting the alkyl esters etc. preferably have 1 to 18 carbon atoms.

[0074] Suitable examples of the styrene-based monomer include styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, m-methylstyrene, and the like, and suitable examples of the maleic acid-based monomer include maleic anhydride and maleic acid, which may be in the form of an alkyl ester having 1 to 18 carbon atoms, an alkylamide having 1 to 18 carbon atoms, or a hydroxyalkyl ester having 2 to 4 carbon atoms. Furthermore, the aqueous acrylic resin used in the present invention may further contain, as a reaction component, known monomers other than those mentioned above that are generally used as reaction components for aqueous acrylic resins.

[0075] Using these reaction components, acrylic resins can be produced by known production methods, and can be made aqueous by using known emulsifiers or polymer protective colloids, or by introducing carboxyl groups into the molecule and neutralizing with a basic compound. As the basic compound, amine compounds are preferred, and ammonia is preferred. The aqueous acrylic resin is preferably an aqueous emulsion, more preferably a core-shell type acrylic emulsion, and the core / shell ratio of the acrylic emulsion is preferably 10:90 to 70:30.

[0076] [Water-based urethane resin] The aqueous urethane resin is preferably in the form of a polyurethane resin synthesized from a polyol, a hydroxy acid, and a polyisocyanate, or in the form of a polyurethane urea resin containing a urethane prepolymer having an isocyanate group at its terminal, which is synthesized from a polyol, a hydroxy acid, and a polyisocyanate, and a polyurethane urea chain-extended with a polyamine.

[0077] Water-based urethane resins and polyurethane urea resins are made water-soluble by introducing ionic groups such as carboxyl groups and sulfone groups into the resin when polyol and polyisocyanate are reacted, and neutralizing the resin with a basic compound. From the viewpoint of water resistance, carboxyl groups are preferred as the ionic groups.

[0078] <Laminate> The laminate of the present invention can be obtained by printing an active energy ray-curable ink onto an anchor agent applied to a non-absorbing substrate, and curing the ink with active energy rays.

[0079] The method for producing this laminate includes the following steps: A step 1 of applying an aqueous anchoring agent containing an aqueous resin to a non-absorbent substrate and drying the applied aqueous anchoring agent in an oven to obtain a laminate having an anchoring layer on the non-absorbent substrate; a step 2 of printing an active energy ray curable ink on the anchor layer of the laminate having an anchor layer on the non-absorbing substrate, and curing the ink with active energy rays to obtain a laminate having an ink layer on the anchor layer; Includes.

[0080] As described above, by using an ink that does not contain a colorant (varnish or clear ink), a laminate having a varnish layer on an anchor layer can be obtained.

[0081] It is also possible to print an active energy ray-curable varnish on the ink and then cure it with active energy rays to form a laminate having a varnish layer on an ink layer.

[0082] The non-absorbing substrate is not particularly limited, and known substrates can be used. Specifically, polypropylene (PP), polyethylene (PET), polyethylene terephthalate (PET), plastic substrates having inorganic deposition layers such as aluminum, silica, and alumina, aluminum foil, polyvinyl chloride (PVC), polystyrene (PS), nylon, cellophane, metal sheets, etc., and the substrates may contain various additives such as antistatic agents, antifogging agents, and ultraviolet protection agents.

[0083] In the present invention, the method for printing the active energy ray-curable ink is not particularly limited as long as it is possible to print an active energy ray-curable offset printing ink, an active energy ray-curable flexographic printing ink, or an active energy ray-curable resin letterpress printing ink, but it is preferably any one of offset printing using an active energy ray-curable offset printing ink, resin letterpress printing using an active energy ray-curable resin letterpress printing ink, and flexographic printing using an active energy ray-curable flexographic printing ink.

[0084] In the present invention, the method for applying the aqueous anchor agent is not particularly limited, and any known method can be used.Specific examples include a roll coater, a gravure coater, a flexo coater, an air doctor coater, a blade coater, an air knife coater, a squeeze coater, an impregnation coater, a transfer roll coater, a kiss coater, a curtain coater, a cast coater, a spray coater, a die coater, offset printing, gravure printing, resin letterpress printing, and flexo printing.

[0085] The active energy ray source is not particularly limited and may be any known source, specifically including mercury lamps, xenon lamps, metal hydride lamps, excimer lamps, LEDs (light-emitting diodes) such as ultraviolet light-emitting diodes (UV-LEDs) and ultraviolet laser diodes (UV-LDs), electron beam (EB) irradiation devices, and gas / solid-state lasers.

[0086] <Deinking> In the present invention, deinking is a process for removing ink components from a printed non-absorbing substrate.

[0087] (Ink component removal process using alkaline aqueous solution) The laminate is, for example, brought into contact with an alkaline aqueous solution in a treatment tank containing the alkaline aqueous solution to remove the ink layer.

[0088] (Alkaline aqueous solution) In the present invention, the alkaline aqueous solution is an aqueous solution containing an alkaline compound, and the alkaline compound is preferably contained in an amount of 0.5 to 10 mass % of the entire aqueous solution, and more preferably 1 to 5 mass %. The alkaline compound is not particularly limited, but examples thereof include sodium hydroxide (NaOH), potassium hydroxide (KOH), calcium hydroxide (Ca(OH) 2 Ammonia, barium hydroxide (Ba(OH) 2 ), Sodium Carbonate (Na 2 CO 3 Preferred are NaOH and / or KOH.

[0089] (Ink component removal process) The mechanism by which the ink layer can be detached from the laminate by contacting the alkaline aqueous solution with the laminate is assumed to be that the presence of the resin allows the alkaline aqueous solution to penetrate through the surface of the anchor layer and / or the cross section of the laminate, dissolving the anchor layer. The laminate, which is formed into a packaging container after applying an anchor layer to a non-absorbent substrate and then printing an ink layer and then going through a bag-making process or the like, is preferably cut or crushed in the recycling process or before, so that the laminate comes into contact with the alkaline aqueous solution in a state where the cross section of the laminate is exposed.

[0090] The laminate and the alkaline aqueous solution are preferably contacted while being stirred. The stirring means is not particularly limited, and examples thereof include known stirring equipment such as a general dispersion, radial flow turbine blade, axial flow turbine blade, paddle blade, propeller blade, anchor blade, and high shear mixer. For example, in the case of a 2L flask scale, the stirring rotation speed is preferably 100 to 350 rpm, depending on the shape and size of the stirring blade. The stirring time is preferably 15 minutes or more and 24 hours or less.

[0091] (Base material recovery process) The method for producing recycled substrates of the present invention includes a step of recovering the non-absorbent substrate after the ink layer is removed from the laminate. The step of recovering the non-absorbent substrate refers to a step of separating and recovering the non-absorbent substrate from a treatment tank in which the alkaline aqueous solution, the peeled ink layer fragments, the non-absorbent substrate, and the like are mixed after the laminate is treated with an alkaline aqueous solution, and it is preferable to obtain the non-absorbent substrate with high purity. There are no particular limitations on the method for recovering the non-absorbent substrate, and for example, separation and recovery based on the size difference between the non-absorbent substrate and the ink layer fragments is preferable, and separation and recovery based on the specific gravity difference is also preferable. Alternatively, separation and recovery can be appropriately performed by a combination of these, and among them, it is preferable to include a separation and recovery step based on the specific gravity difference, and more preferably, a separation and recovery step based on the specific gravity difference and a separation and recovery step based on the size difference are used in combination. In the separation and recovery process based on the specific gravity difference, it is preferable to recover only the substrate floating in the alkaline aqueous solution in the treatment tank. It is also preferable if impurity components and fragments of the ink layer in the alkaline aqueous solution settle, which makes it easy to separate from the non-absorbent substrate, and allows only the non-absorbent substrate to be recovered more accurately. Therefore, the physical properties and transparency of the non-absorbent substrate recycled after recovery are improved. The method of separation based on the specific gravity difference may be a conventionally known method, such as one using a fluidized bed or one using a centrifuge.

[0092] After the ink layer is detached from the laminate and the non-absorbent substrate is recovered, the non-absorbent substrate is washed with water and dried to obtain a recycled non-absorbent substrate. In this case, it is preferable that the recycled non-absorbent substrate is free of any contaminants, including fragments of the detached ink layer, as much as possible. The recycled non-absorbent substrate can be processed into pellets using an extruder or the like and reused as recycled resin. The use of the recycled resin is not limited, and it may be processed into a colorless and transparent film, or may be processed into a molded product with a colorant added.

[0093] Available deinking agents include DI-7020, DI-7027, DI-7250, and DI-767 manufactured by Kao Corporation, the DIA-Z series and DIA-Y series manufactured by Nissin Chemical Co., Ltd., and the Riptor series manufactured by Lion Specialty Chemicals.

[0094] (Ink recovery process) In the above-mentioned substrate recovery step, the ink can be recovered by filtering the alkaline aqueous solution after substrate recovery. At this time, since the material of the anchor layer is soluble in the alkaline aqueous solution, it is possible to extract the ink components with high purity. EXAMPLES

[0095] The present invention will be specifically described below with reference to examples and comparative examples. However, the present invention is not limited to the following examples. In the examples and comparative examples, "parts" and "%" represent "parts by mass" and "% by mass", respectively.

[0096] <Preparation of anchoring agent> (Anchoring agent 1) 99.0 parts of resin 1 (Hi-Loss X436 manufactured by Seiko PMC Corporation) and 1.0 part of polyethylene wax (Chemipearl W500 manufactured by Mitsui Chemicals Inc.) were added and stirred with a disper for 10 minutes to obtain an aqueous anchor agent (AC1).

[0097] (Anchor agent 2-13) For the above resins 2 to 13, aqueous anchoring agents (AC2) to (AC13) were obtained by using the same formulation as anchoring agent 1, except that the resin was changed to the resin listed in Table 1 (for details, see paragraph 0114 of the original specification).

[0098] (Anchoring agent 14) 79.0 parts of resin 14 (Megapur IM30AL manufactured by MEGARA), 10.0 parts of ethyl acetate, 10.0 parts of isopropyl alcohol, and 1.0 part of polyethylene wax (Chemipearl W500 manufactured by Mitsui Chemicals) were added and stirred with a disperser for 10 minutes to obtain an oil-based anchor agent (AC14).

[0099] (Anchoring agent 15) 20.0 parts of TMPTA (EO), 60.0 parts of DiTMPTA, 10.0 parts of DPHA, 6.0 parts of 4MBP, 3.0 parts of TPO, and 1.0 part of EDB were mixed and stirred using a butterfly mixer to prepare a UV flexo acrylic anchor agent (AC15).

[0100] <Preparation of active energy ray-curable resin varnish> 65.0 parts of DPHA, 6.5 parts of TMPTA (EO), and 3.5 parts of DiTMPTA were mixed and heated to 100° C. with stirring. Next, 25.0 parts of diallyl phthalate resin (resin 15) was mixed and dissolved while keeping the temperature at 100° C. to prepare a diallyl phthalate resin varnish.

[0101] (Anchoring agent 16) 10.0 parts of TMPTA (EO), 18.0 parts of DiTMPTA, 7.0 parts of DPHA, 5.0 parts of 4MBP, 2.0 parts of TPO, 1.0 part of EDB, and 57.0 parts of the diallyl phthalate resin varnish were mixed and stirred using a butterfly mixer to produce a UV offset acrylic anchor agent (AC16).

[0102] <Ink manufacturing example> <Preparation of oil-based resin varnish> (Example of rosin modified phenolic resin production) In a reaction vessel, 54.3 parts of gum rosin was reacted with 30.8 parts of tertiary butylphenol and 9.4 parts of 92% by weight paraformaldehyde in a xylene solvent under sodium hydroxide catalyst at 100°C for 4 hours, and the phenolic resin from which moisture had been removed was added dropwise at 150°C and reacted for 2 hours. 5.4 parts of glycerin was then added, and the reaction was continued for 15 hours at 250°C using 0.1 parts of calcium oxide as a catalyst. During this time, the mixture was successively removed to obtain a rosin phenolic resin.

[0103] (Example of rosin modified phenolic resin varnish production) Next, 45.0 parts of the rosin-modified phenolic resin as a binder resin, 44.0 parts of soybean oil, 10.0 parts of soybean oil fatty acid normal butyl ester, and 1.0 parts of ALCH were placed in a four-neck flask equipped with a stirrer, a reflux condenser equipped with a water separator, and a thermometer, and heated and stirred at 190°C for 1 hour to obtain a rosin-modified phenolic resin varnish.

[0104] (Ink manufacturing example 1 (oil-based ink)) 17.0 parts of RAVEN 1080 Ultra, 3.0 parts of BA-2550, 59.0 parts of rosin-modified phenolic resin varnish, 20.0 parts of soybean oil, 0.5 parts of MK dryer, and 0.5 parts of drying inhibitor CP were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less to prepare an ink.

[0105] (Ink Manufacturing Example 2 (UV Ink 1)) (Active energy ray curable offset printing ink, active Energy-ray curable resin letterpress printing ink 17.0 parts of RAVEN 1080 Ultra, 3.0 parts of BA-2550, 6.0 parts of TMPTA (EO), 13.0 parts of DiTMPTA, 7.0 parts of DPHA, 3.0 parts of 379, 1.5 parts of DEABP, 1.5 parts of DETX, 1.0 part of EDB, and 47.0 parts of diallyl phthalate resin varnish were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less to prepare an ink.

[0106] (Ink Manufacturing Example 3 (UV Ink 2)) (Active energy ray curable offset printing ink, active Energy-ray curable resin letterpress printing ink 17.0 parts of RAVEN 1080 Ultra, 3.0 parts of BA-2550, 6.0 parts of TMPTA (EO), 13.0 parts of DiTMPTA, 7.0 parts of DPHA, 3.0 parts of 379, 1.5 parts of DEABP, 1.5 parts of DETX, 1.0 part of EDB, and 47.0 parts of MIRAMER PS-4500 were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less to prepare an ink.

[0107] (Ink manufacturing example 4 (LED ink)) (Active energy ray curable offset printing ink, active energy ray curable resin letterpress printing ink) 17.0 parts of RAVEN 1080 Ultra, 3.0 parts of BA-2550, 6.0 parts of TMPTA (EO), 10.0 parts of DiTMPTA, 7.0 parts of DPHA, 3.0 parts of 379, 2.0 parts of TPO, 2.0 parts of DEABP, 2.5 parts of 4MBP, 2.5 parts of DETX, 1.0 part of EDB, and 44.0 parts of diallyl phthalate resin varnish were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less to prepare an ink.

[0108] (Ink Manufacturing Example 5 (UV Flexographic Ink) (Active Energy Ray Curable Flexographic Printing Ink)) 15.0 parts of RAVEN 1080 Ultra, 1.0 part of BA-2550, 16.0 parts of TMPTA (EO), 5.0 parts of DiTMPTA, 7.0 parts of DPHA, 3.0 parts of 379, 2.0 parts of DEABP, 2.5 parts of 4MBP, 2.5 parts of DETX, 1.0 part of EDB, and 6.0 parts of Solsperse 24000 were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less to prepare an ink. Then, 39.0 parts of TMPTA (EO) were added and mixed and stirred using a butterfly mixer to prepare an ink.

[0109] (Ink Manufacturing Example 6 (UV Ink Yellow) (Active Energy Ray Curable Offset Printing Ink, Active Energy Ray Curable Resin Letterpress Printing Ink)) 15.0 parts of Permanent Yellow BHS, 6.0 parts of TMPTA (EO), 18.0 parts of DiTMPTA, 7.0 parts of DPHA, 3.0 parts of 379, 1.5 parts of DEABP, 1.5 parts of DETX, 1.0 part of EDB, and 47.0 parts of diallyl phthalate resin varnish were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less to prepare an ink.

[0110] (Ink Manufacturing Example 7 (UV Ink Red) (Active Energy Ray Curable Offset Printing Ink, Active Energy Ray Curable Resin Letterpress Printing Ink)) 20.0 parts of Permanent Rubine L5B-01, 6.0 parts of TMPTA (EO), 13.0 parts of DiTMPTA, 7.0 parts of DPHA, 3.0 parts of 379, 1.5 parts of DEABP, 1.5 parts of DETX, 1.0 part of EDB, and 47.0 parts of diallyl phthalate resin varnish were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less to prepare the ink.

[0111] (Ink Manufacturing Example 8 (UV Ink Blue) (Active Energy Ray Curable Offset Printing Ink, Active Energy Ray Curable Resin Letterpress Printing Ink)) 20.0 parts of Heliogen Blue D7088, 6.0 parts of TMPTA (EO), 13.0 parts of DiTMPTA, 7.0 parts of DPHA, 3.0 parts of 379, 1.5 parts of DEABP, 1.5 parts of DETX, 1.0 part of EDB, and 47.0 parts of diallyl phthalate resin varnish were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less to prepare an ink.

[0112] (Ink Production Example 9 (EB Ink) (Active Energy Ray Curable Offset Printing Ink, Active Energy Ray Curable Resin Letterpress Printing Ink)) 17.0 parts of RAVEN 1080 Ultra, 3.0 parts of BA-2550, 6.0 parts of TMPTA (EO), 13.0 parts of DiTMPTA, 7.0 parts of DPHA, and 54.0 parts of diallyl phthalate resin varnish were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less to prepare an ink.

[0113] (Varnish (clear ink) Manufacturing example 1 (UV varnish) (Active energy ray curable offset printing varnish, active energy ray curable Chemically-modified resin letterpress varnish 6.0 parts of TMPTA (EO), 13.0 parts of DiTMPTA, 7.0 parts of DPHA, 6.0 parts of 184, 2.0 parts of TPO, 1.0 part of EDB, 3.0 parts of filler, and 62.0 parts of diallyl phthalate resin varnish were mixed and stirred using a butterfly mixer, and then dispersed using a three-roll mill so that the maximum particle size was 7.5 μm or less to produce a varnish.

[0114] The descriptions of the materials used in the examples are as follows: [Coloring agent] ·Permanent Yellow BHS: Manufactured by Clariant, Permanent Yellow BHS (CIPigment Yellow 174) ·Permanent Rubine L5B-01: Manufactured by Clariant, Permanent Rubine L5B-01 (CIPigment Red 57:1) ·HELIOGEN BLUE D7088: Manufactured by BASF, HELIOGEN BLUE D7088 (CIPigment Blue 15:3) ·Raven 1080 Ultra: Manufactured by Bilra Carbon, Raven 1080 Ultra Powder (CIPigment Black 7) BA-2550: Morimura Shoji Co., Ltd., alkaline blue toner BA-2550 (CIPigmen t Blue 61) [Extender pigment] Filler: Matsumura Sangyo Co., Ltd., High Filler #5000PJ, talc [(Meth)acrylate compounds] TMPTA (EO): BASF, LAROMER LR8863, trimethylolpropane ethylene oxide modified triacrylate DiTMPTA: Daicel-Allnex, EBECRYL1142, ditrimethylolpropane tetraacrylate DPHA: MIWON, MIRAMER M600, dipentaerythritol hexaacrylate PS-4500: MIWON, MIRAMER PS-4500, polyester acrylate oligomer [resin] Resin 1: Seiko PMC's Hi-Loss X436 (acid value 33 mg KOH / g, glass transition temperature 21°C) Resin 2: BASF JONCRYL PDX-7615 (acid value 51 mg KOH / g, glass transition temperature 33°C) Resin 3: BASF JONCRYL 63D (acid value 213 mg KOH / g, glass transition temperature 73°C) Resin 4: Neocryl A-2091 manufactured by Covestro (acid value 62 mg KOH / g, glass transition temperature 98°C) Resin 5: BASF JONCRYL PDX-7732 (acid value 87 mg KOH / g, glass transition temperature 12°C) Resin 6: Emmapoly SG5157 manufactured by Gifu Ceramics Manufacturing Co., Ltd. (acid value 218 mgKOH / g, glass transition temperature 102°C) Resin 7: Acris TGV40 (acid value 54 mgKOH / g, glass transition temperature 109°C) manufactured by Gifu Ceramics Manufacturing Co., Ltd. Resin 8: Takelac W605 (acid value 25 mg KOH / g, glass transition temperature 100°C) manufactured by Mitsui Chemicals Resin 9: Seiko PMC Hi-Loss X J-140A (acid value 33 mg KOH / g, glass transition temperature 6°C) Resin 10: Neocryl A-1127 manufactured by Covestro (acid value 18 mg KOH / g, glass transition temperature 5°C) Resin 11: LIOCRYL PFX0302 manufactured by Toyochem Co., Ltd. (acid value 150 mg KOH / g, glass transition temperature 4°C) Resin 12: Taisei Fine Chemical Co., Ltd., Acrylit WEM200U (acid value 6 mg KOH / g, glass transition temperature 31°C) Resin 13: BASF JP-W2 (acid value 312 mg KOH / g, glass transition temperature 102°C) Resin 14: Megarpur IM30AL manufactured by MEGARA (acid value 0 mgKOH / g, glass transition temperature -10°C) Resin 15: Daisodap A manufactured by Osaka Soda Co., Ltd. (acid value 2 mg KOH / g, glass transition temperature 150°C) [Photopolymerization initiator] 379: IGM RESINS, Omnirad379, 1,2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone TPO: Chemark Chemical Company, CHEMARK TPO, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide DEABP: Chemark Chemical Company, CHEMARK DEABP, 4,4'-bis(dimethylamino)benzophenone 4MBP: Soho Industry Co., Ltd., SB-PI 712 DETX: Chemark Chemical Company, CHEMARK DETX, 2,4-diethylthioxanthone 184: IGM RESINS, Omnirad 184, 1-hydroxy-cyclohexyl phenyl ketone [Amine compounds] EDB: Chemark Chemical Company, CHEMARK EDB, Ethyl 4-(dimethylamino)benzoate [Pigment dispersant] Solsperse 24000: Lubrizol Solsperse 24000 [Metal dryer] MK Dryer: MK Dryer manufactured by Toyo Ink Co., Ltd. [Drying inhibitor] Drying inhibitor CP: Drying inhibitor CP manufactured by Toyo Ink Co., Ltd. [Aluminum gelling agent] ALCH: Manufactured by Kawaken Fine Chemicals Co., Ltd., ALCH, aluminum ethyl acetate diisopropylate [others] Soybean oil fatty acid normal butyl ester: Toshin Yushi Co., Ltd., SFB2

[0115] The performance of the obtained anchor agent coating was evaluated by the following method, and the results are shown in Table 1.

[0116] <Printing anchoring agent onto substrate> In Examples 1 to 29 and Comparative Examples 1, 4 to 8, and 11, an anchor agent shown in Table 1 was applied onto a substrate using a bar coater (No. 4, manufactured by Yasuda Seiki Co., Ltd.). Then, the substrate was dried in an oven at 60 degrees for 10 minutes to prepare a laminate having an anchor layer on the substrate. In Comparative Examples 9 and 10, an anchoring agent shown in Table 1 was applied onto the substrate using a bar coater (No. 4, manufactured by Yasuda Seiki Co., Ltd.). The coating was then cured using an ultraviolet curing device (160 W / cm metal halide lamp) manufactured by iGraphics Co., Ltd. at a conveyor speed of 30 m / min to produce a laminate having an anchoring layer on the substrate.

[0117] <Evaluation of Laminate Having Anchor Layer on Substrate> The physical properties of the laminates having an anchor layer on a substrate obtained in Examples 1 to 29 and Comparative Examples 1, 4 to 8, and 11 were evaluated. (Blocking resistance) The anchor agent-coated products obtained in Examples 1 to 29 and Comparative Examples 1, 4 to 8, and 11 were cut into pieces measuring 4 cm wide and 4 cm long, and the coated and uncoated surfaces were placed in close contact with each other and subjected to a load of 10 N / cm. 2 The coated objects were then peeled off from each other and evaluated. (Evaluation Criteria) Good: No noise or resistance when peeled off. ×: A crackling sound was heard when peeled off. There was a large resistance. In addition, ◯ is preferable in practical use. (Adhesion) An adhesive tape (Nichiban Cellotape (registered trademark), 18 mm wide) was attached to the ink surface of the laminate and peeled off vertically at 90 degrees. The adhesion to the substrate was evaluated from the percentage of the area of ​​the ink coating that was peeled off from the anchor layer. (Evaluation Criteria) ○: The ink film does not peel off from the anchor layer. ○△: Less than 10% of the ink film peeled off from the anchor layer. △: Peeling of the ink film from the anchor layer is 10% or more but less than 30%. △×: Peeling of the ink film from the anchor layer is 30% or more but less than 70%. ×: 70% or more of the ink film peels off from the anchor layer. ◯, ◯△, and △ are practically preferable.

[0118] <Ink and varnish printing> In Examples 1 to 21, 24 to 27 and Comparative Examples 1 and 4 to 10, the prepared laminate having an anchor layer on the substrate was printed with the sample ink shown in Table 1 using an RI tester (a simple printing machine manufactured by Mei Seisakusho Co., Ltd. (a printing machine capable of printing offset printing ink, flexographic printing ink, and resin letterpress printing ink)) with an ink gauge of 0.25 mL over only half the area of ​​the substrate, and the printed matter was then cured with an ultraviolet curing device manufactured by Eye Graphics Co., Ltd. (160 W / cm metal halide lamp) at a conveyor speed of 30 m / min to obtain a laminate having an anchor layer and an ink layer in this order on the substrate. In Example 22, the prepared laminate having an anchor layer on a substrate was printed with the sample ink shown in Table 1 using an RI tester with an ink gauge of 0.25 mL over only half the area of ​​the substrate, and the ink was then cured on the printed matter with an ultraviolet curing device (160 W / cm metal halide lamp) manufactured by iGraphics Co., Ltd. at a conveyor speed of 100 m / min to obtain a laminate having an anchor layer and an ink layer in this order on the substrate. In Example 23, the sample ink shown in Table 1 was printed on the prepared laminate having an anchor layer on the substrate using an RI tester with an ink gauge of 0.25 mL over only half the area of ​​the substrate, and the printed matter was then irradiated with 30 KGy of electron beams using a low-energy electron beam irradiation device manufactured by ESI Corporation (voltage of 175 KV, nitrogen-substituted atmosphere with an oxygen concentration of 50 ppm) to harden the ink, thereby obtaining a laminate having an anchor layer and an ink layer in that order on the substrate. In Example 28, a laminate having an anchor layer on a substrate was prepared by printing a UV varnish prepared by mixing two parts of UV ink 1 with an ink gauge of 0.25 mL using an RI tester over only half of the substrate's area, and then the coating was cured in an ultraviolet curing device (160 W / cm metal halide lamp) manufactured by iGraphics Co., Ltd. at a conveyor speed of 30 m / min to obtain a laminate having an anchor layer and a varnish layer in that order on the substrate. In Example 29, a laminate having an anchor layer on a substrate was prepared by printing UV ink 1 with an ink gauge of 0.25 mL using an RI tester over only half the area of ​​the substrate, and the printed matter was cured as a coating in an UV curing device manufactured by iGraphics (160 W / cm metal halide lamp) at a conveyor speed of 30 m / min. Further, using an RI tester, UV varnish was printed on the ink layer with an ink gauge of 0.25 mL, and the printed matter was cured as a coating in an UV curing device manufactured by iGraphics (160 W / cm metal halide lamp) at a conveyor speed of 30 m / min. Thus, a laminate having an anchor layer, ink layer, and varnish layer in that order on the substrate was obtained. In addition, in Comparative Example 11, the sample ink shown in Table 1 was printed using an RI tester with an ink gauge of 0.25 mL on half of the area of ​​the substrate on the prepared laminate having an anchor layer on the substrate, and then the ink was left to harden at room temperature for 24 hours to obtain a laminate having an anchor layer and an ink layer in that order on the substrate. In Comparative Examples 2 and 3, an RI tester was used to directly print the sample ink shown in Table 1 onto the substrate using an ink gauge of 0.25 mL, covering only half of the substrate's area. The ink was then cured using an ultraviolet curing device (160 W / cm metal halide lamp) manufactured by Eye Graphics Co., Ltd. at a conveyor speed of 30 m / min to obtain a laminate having an ink layer on the substrate.

[0119] The performance of the obtained laminate was evaluated by the following method, and the results are shown in Table 1.

[0120] The substrates used in the examples are as follows: PP1: Polypropylene sheet manufactured by Okamoto Corporation PP2: Novatec PP, manufactured by Japan Polypropylene Corporation PE1: Taiko FC, manufactured by Futamura Chemical Co., Ltd. PE2: Novatec HD, manufactured by Japan Polyethylene Corporation PET: Reshine manufactured by Toyobo Co., Ltd. Aluminum vapor deposition: Gojo Paper Co., Ltd., SPECIALITIES Aluminum foil: Toyo Aluminum Co., Ltd., Leadmax Synthetic paper: New Yupo FGS, manufactured by Yupo Corporation PVC: PVC80C P manufactured by Lintec Corporation PS: Styrofoam, manufactured by Oishi Sangyo Co., Ltd. Nylon: Made by Unitika Ltd., emblem Cellophane: Futamura Chemical Co., Ltd., PL Metal: Nippon Steel Corporation, ET2.8 / 2.8T2.5B

[0121] <Evaluation of a laminate having an ink layer on an anchor layer> (residual solvent) The resulting laminate was evaluated for residual solvent. The laminates of Examples 1 to 29 and Comparative Examples 1 to 11 were cut into pieces measuring 10 cm wide and 10 cm long, and 100 pieces were placed in an eggplant flask, sealed, and then heated (temperature: 80°C, 30 minutes). After that, 0.4 ml of air was removed from the flask and analyzed by gas chromatography (GC) to confirm the amount of solvent components. (Evaluation Criteria) ◯: The total amount of residual solvent is 0.5 mg / cm 2 It was less than. ○△: The total amount of residual solvent is 0.5 mg / cm 2 More than 1mg / cm 2 It was less than. △: The total amount of residual solvent is 1 mg / cm 2 More than 2mg / cm 2 It was less than. △×: The total amount of residual solvent is 2 mg / cm 2 More than 3mg / cm 2 It was less than. ×: The total amount of residual solvent is 3 mg / cm 2 That was all. In addition, ◯, ◯△, and △ are practically preferable.

[0122] (Evaluation of scratch resistance) The laminate was evaluated by rubbing the ink surface with cotton cloth. The less rubbing, the better the scratch resistance. The evaluation criteria are as shown below, with ◯, ◯△, and △ being practically preferable. ○: No rubbing on the printed surface where the ink has been applied 〇△: The ink is rubbed off to the surface of the printed surface. △: The ink is rubbed off to the middle of the printed surface. △×: The ink is rubbed off to the bottom of the printed surface. ×: The coating on the printed surface where the ink was spread disappears

[0123] (Evaluation of deinking ability) The laminates prepared in Examples 1 to 29 and Comparative Examples 1 to 11 were aged at 60° C. for one week, and then stored for an additional 10 days in an environment of room temperature 23±1° C. and humidity 50±2%. Then, the laminates were cut into 30×30 mm pieces, and 90 g of each piece was used as a test sample.

[0124] <Deinking test> In a 2L flask, 1.5L of 30°C hot water, 11mL of 3.75% sodium hydroxide solution, and 11mL of deinking agent (DI-7027 manufactured by Kao Corporation) diluted to 1.5% were added, and the sample was then added and stirred at 300 rpm for 20 minutes. Two minutes after the start of stirring, the sample adhering to the lid was washed away into the tank with a small amount of water. After the desorption was completed, the substrate was removed and the extent to which the area of ​​each 30 x 30 mm was covered with ink was visually evaluated. ○: Ink has come off from 99% or more of the substrate ○△: Ink has come off from 95% to less than 99% of the substrate △: Ink has come off from 90% to less than 95% of the substrate ×: Ink has come off from less than 90% of the substrate

[0125] (Blocking resistance) The laminate was cut into a piece 4cm wide and 4cm long, half of which was printed with ink and half was not, and the coated and uncoated surfaces were placed in close contact with each other and subjected to a load of 10N / cm. 2The coated objects were then peeled off from each other and evaluated. (Evaluation Criteria) Good: No noise or resistance when peeled off. ×: A crackling sound was heard when peeled off. There was a large resistance. In addition, ◯ is preferable in practical use.

[0126] In a laminate having an anchor layer on a substrate, the blocking resistance and adhesion are both evaluated as 〇, 〇△, or △. In a laminate having an ink layer on an anchor layer, those that are rated as ◯, ◯△, or △ in the three evaluations of residual solvent, scratch resistance, and deinking ability are considered to be practical.

[0127] From the above, it has been found that the laminate of the present invention has deinking properties while providing printing quality such as scratch resistance and adhesion required in the market, even when at least one type of ink selected from active energy ray-curable offset printing ink, active energy ray-curable flexographic printing ink, and active energy ray-curable resin letterpress printing ink is used.

[0128] [Table 1]

[0129] [Table 1]

[0130] [Table 1]

[0131] [Table 1]

Claims

1. A laminate having an anchor layer and an ink layer in this order on a non-absorbing substrate, The anchor layer comprises an aqueous resin, The acid value of the aqueous resin is 25 to 300 mgKOH / g; The glass transition temperature of the aqueous resin is 10 to 150° C., A laminate, wherein the ink layer is a cured product of at least one type of ink selected from an active energy ray-curable offset printing ink, an active energy ray-curable flexographic printing ink, and an active energy ray-curable resin letterpress printing ink.

2. 2. The laminate according to claim 1, wherein the aqueous resin comprises at least one selected from the group consisting of an aqueous acrylic resin and an aqueous urethane resin.

3. A method for producing a laminate, comprising the steps of: A step 1 of applying an anchor agent containing water and an aqueous resin to a non-absorbent substrate and drying the applied agent in an oven to obtain a laminate having an anchor layer on the substrate; a step 2 of printing at least one ink selected from an active energy ray-curable offset printing ink, an active energy ray-curable flexographic printing ink, and an active energy ray-curable resin letterpress printing ink on the anchor layer of the laminate having an anchor layer on the non-absorbing substrate, and curing the ink with active energy rays to obtain a laminate having an ink layer on the anchor layer; Including, The acid value of the aqueous resin is 25 to 300 mgKOH / g; The method for producing a laminate, wherein the aqueous resin has a glass transition temperature of 10 to 150° C.

4. The method for producing a laminate according to claim 3, wherein the aqueous resin comprises at least one selected from the group consisting of an aqueous acrylic resin and an aqueous urethane resin.

5. A method for deinking a laminate having an anchor layer and an ink layer, in that order, on a non-absorbing substrate, comprising the steps of: The anchor layer comprises an aqueous resin, The acid value of the aqueous resin is 25 to 300 mgKOH / g; The glass transition temperature of the aqueous resin is 10 to 150° C., the ink layer is a cured product of at least one ink selected from an active energy ray-curable offset printing ink, an active energy ray-curable flexographic printing ink, and an active energy ray-curable resin letterpress printing ink, A method for deinking a laminate, comprising agitating the laminate in an alkaline aqueous solution, dissolving the anchor layer in the alkaline aqueous solution, and deinking the ink layer from the non-absorbing substrate.

6. The method for deinking a laminate according to claim 5, wherein the aqueous resin comprises at least one selected from the group consisting of an aqueous acrylic resin and an aqueous urethane resin.

7. A method for recovering ink, comprising filtering and recovering the ink layer deinked by the deinking method according to claim 5 or 6.

Citation Information

Patent Citations

  • Laminate deinking method

    JP2023018605A

  • Heat-shrinkable film

    JP2023040698A

  • Organic solvent-based printing ink, printed material, and laminate

    JP2020090627A

  • Deinking method for laminate

    JP7070772B1

Cited By

  • Recycled plastic substrate, and method for manufacturing the recycled plastic substrate.

    JP2026110970A

  • Printed media and packaging

    JP7903743B2

  • Printed media and packaging

    JPWO2025249481A1