Electronic component and manufacturing method for the same

By controlling the surface treatment of tin-plated external electrodes to limit tin hydroxide and maintain a specific water contact angle, void formation in solder connections is prevented, ensuring reliable and durable electronic components.

JP2024152301APending Publication Date: 2024-10-25KOA CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023066416
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Void formation in solder connections during surface mounting of electronic components with tin-plated external electrodes leads to reliability issues, which existing technologies fail to adequately address.

Method used

The surface of the external electrode is treated to maintain a specific amount of tin hydroxide (SnO2·nH2O) within 100 μmol/m², ensuring a water contact angle of 80 to 110°, thereby suppressing hydroxylation and oxidation, thus preventing void formation during soldering.

Benefits of technology

This approach effectively suppresses void generation in solder connections, maintaining connection reliability for extended periods, reducing waste, and enhancing the longevity of electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152301000001_ABST
    Figure 2024152301000001_ABST
Patent Text Reader

Abstract

To provide an electronic component that can prevent a void from occurring in a solder during surface mounting.SOLUTION: The electronic component includes a component body made of ceramic and an external electrode provided on the component body. The surface of the external electrode is formed of tin. The amount of tin hydroxide (SnO2.nH2O) is 100 μmol / m2 or less. The external electrode is used for surface mounting with solder.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electronic component and a method for manufacturing the same. [Background technology]

[0002] There are known electronic components that are surface-mounted on a circuit board. Such electronic components are usually provided with external electrodes. The external electrodes are required to be connected to a wiring pattern provided on the circuit board via solder with high reliability.

[0003] In relation to the above, Patent Document 1 discloses an invention relating to a resistor electrode formation method capable of suppressing deterioration of solderability due to aging for more than five years. Patent Document 1 describes a resistor electrode formation method in which a side electrode is formed on at least the side of a substrate, and a plating layer is formed to cover the side electrode, in which after the plating layer is formed, the surface of the plating layer is ultrasonically cleaned with an aqueous solution of sodium triphosphate. By so-called neutralization treatment, the amount of plating solution residue on the plating surface is extremely reduced, thereby suppressing oxidation of the electrode surface. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 10-321420 Summary of the Invention [Problem to be solved by the invention]

[0005] The inventors have been studying electronic components having a ceramic component body and external electrodes provided on the component body, with the surfaces of the external electrodes being made of tin. In the course of the study, the inventors have found that in such electronic components, voids may occur in the solder when the electronic components are surface-mounted via solder. The occurrence of voids should be avoided because it can deteriorate connection reliability.

[0006] Therefore, an object of the present invention is to provide a technology that can suppress the generation of voids in the solder during surface mounting in an electronic component having a ceramic component body and an external electrode provided on the component body, with the surface of the external electrode formed from tin. [Means for solving the problem]

[0007] In one aspect of the present invention, an electronic component includes a component body made of ceramic and an external electrode provided on the component body. The surface of the external electrode is made of tin. The amount of tin hydroxide (SnO2·nH2O) on the surface of the external electrode is 100 μmol / m 2 The external electrodes are used for surface mounting by soldering.

[0008] In another aspect of the present invention, a method for manufacturing an electronic component is provided for use in surface mounting of external electrodes by soldering, the method comprising the steps of: preparing a component body made of ceramic; and forming external electrodes on the component body, the external electrodes being formed on the surface of the component body by tin plating; and treating the surface of the external electrodes with a treatment liquid to suppress the generation of tin hydroxide (SnO2·nH2O). Effect of the Invention

[0009] According to the above-described aspects, an electronic component capable of suppressing the occurrence of voids in the solder during surface mounting and a method for manufacturing the electronic component are provided. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a perspective view showing an electronic component according to an embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view of an electronic component. [Diagram 3] FIG. 3 is a cross-sectional view that illustrates a schematic configuration of an end portion of an electronic component in a surface-mounted state. [Figure 4]FIG. 4 is a graph showing the results of voltammetry measurements for the comparative examples and the examples. [Diagram 5] FIG. 5 is a graph showing the water contact angle before and after the PCT treatment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] An embodiment of the present invention will be described below. The electronic component according to this embodiment is an electronic component that is surface mounted via solder for use. This electronic component has a component body made of ceramic, and external electrodes provided on the component body. The surfaces of the external electrodes are made of tin. During surface mounting, the external electrodes are mounted on an electronic board via solder. That is, the external electrodes are used for surface mounting by solder.

[0012] Here, one of the features of this embodiment is the amount of tin hydroxide (SnO2·nH2O) on the surface of the external electrode. Specifically, the amount of tin hydroxide on the surface of the external electrode is 100 μmol / m 2 According to the findings of the present inventors, by adopting such a configuration, the generation of voids in the solder during surface mounting is suppressed. It is believed that a small amount of tin hydroxide suppresses the reaction between the hydroxyl groups of tin hydroxide and the components contained in the solder (especially the carboxyl groups of the flux components), and the fluidity of the flux is not lost, resulting in the generation of voids being suppressed.

[0013] (1) Electronic Components The electronic component according to this embodiment will be described in detail below, taking as an example a case where the electronic component is a chip resistor. Fig. 1 is a perspective view showing an electronic component 1 (chip resistor) according to this embodiment. Fig. 2 is a schematic cross-sectional view of the electronic component 1.

[0014] As shown in Figures 1 and 2, the electronic component 1 has a component body 2, a pair of internal electrodes 3, a pair of back surface electrodes 4, a pair of end surface electrodes 5, a pair of external electrodes 6, a resistor 9, and a protective film 10.

[0015] The component body 2 is made of ceramic (e.g., Al2O3, etc.). The component body 2 is insulating and substrate-like. That is, the component body 2 has a main surface 2-1, a back surface 2-2, and an end surface 2-3. In the example shown in FIGS. 1 and 2, the component body 2 is a thin rectangular parallelepiped (the main surface 2-1 and the back surface 2-2 are rectangular). However, the component body 2 does not necessarily have to be rectangular, and may be, for example, coin-shaped (disc-shaped), etc.

[0016] The resistor 9 is provided on the main surface 2-1. The resistor 9 may be made of, for example, ruthenium oxide.

[0017] The pair of internal electrodes 3 are provided on the main surface 2-1 so as to sandwich the resistor 9. Each of the pair of internal electrodes 3 is connected to the resistor 9.

[0018] A pair of rear surface electrodes 4 are provided on the rear surface 2-2.

[0019] A pair of end electrodes 5 are provided so as to connect each of the internal electrodes 3 and each of the back electrodes 4. One end of each of the end electrodes 5 is disposed on the internal electrode 3. The end electrodes 5 are provided so as to extend from one end thereof around the end face 2-3 to the back surface 2-2. Each of the end electrodes 5 is located on the back surface electrode 4 on the back surface 2-2 side.

[0020] The protective film 10 is provided to protect the resistor element 9. That is, the protective film 10 is disposed on the main surface 2-1 so as to cover the resistor element 9. Note that a portion of the internal electrode 3 is also covered by the protective film 10.

[0021] Specifically, the protective film 10 has a glass protective film 10-2 and a resin protective film 10-1. The glass protective film 10-2 is provided so as to cover the resistor 9. The resin protective film 10-1 is provided so as to cover the glass protective film 10-2.

[0022] A pair of external electrodes 6 are provided so as to cover the respective end surface electrodes 5. One end of each external electrode 6 is located on the main surface 2-1, and the other end is located on the back surface 2-2. In detail, each external electrode 6 extends from the main surface 2-1, around the end surface 2-3, and to the back surface 2-2.

[0023] Each external electrode 6 is a portion that comes into contact with solder during surface mounting, and therefore the surface of the external electrode 6 is exposed.

[0024] Each external electrode 6 has an underlayer 7 and a tin plating layer 8 provided on the underlayer 7. The underlayer 7 is, for example, a nickel plating layer. The underlayer 7 has a thickness of, for example, 1 to 20 μm, preferably 2 to 10 μm. The tin plating layer 8 has a thickness of, for example, 1 to 20 μm, preferably 2 to 10 μm.

[0025] In this specification, the tin plating layer 8 is a layer substantially made of tin. Specifically, the tin content in the tin plating layer 8 is, for example, 98% by mass or more, and preferably 99% by mass or more. If the surface of the external electrode 6 is formed of the tin plating layer 8 having such a composition, unless special measures are taken, tin hydroxide is formed on the surface of the external electrode, and the hydroxyl group of the tin hydroxide reacts with the flux, which may cause a problem of void generation during surface mounting. However, according to this embodiment, the amount of tin hydroxide is set to a specific value or less, so that the generation of voids can be suppressed. Note that suppressing the amount of tin hydroxide as in this embodiment is effective against deterioration caused by water, and is therefore suitable for electronic components in which the surface of the external electrode, which is particularly susceptible to hydroxide, is made of a layer made of tin.

[0026] Next, a method for surface mounting the electronic component 1 will be described. FIG. 3 is a cross-sectional view that shows a schematic configuration of an end portion of the electronic component 1 in a surface-mounted state. In the example shown in FIG. 3, the electronic component 1 is mounted on a circuit board 11. Specifically, a wiring pattern is formed on the circuit board 11, and lands 12 are provided. During surface mounting, solder paste is printed or applied on the lands 12. Then, the electronic component 1 is mounted on the circuit board 11 so that the external electrodes 6 are in contact with the solder paste. Thereafter, a reflow process is performed. As a result, the external electrodes 6 are connected to the lands 12 via the solder 13, as shown in FIG. 3. After reflow, the tin-plated layer 8 melts, and the boundary between the tin-plated layer 8 and the solder 13 is no longer distinguishable.

[0027] In the chip resistor having the above-mentioned configuration, the surface of the tin plating layer 8 becomes rough due to the surface roughness of the internal electrode 3, the back electrode 4, and the underlayer 7, and since the tin plating layer 8 melts into the solder during surface mounting by solder, the surface roughness of the underlayer 7 affects the difficulty of voids escaping to the outside. Furthermore, multiple layers (internal electrode 3, back electrode 4, end electrode 5, underlayer 7) are overlapped inside the tin plating layer 8, and due to these overlaps, there is a height difference of about several μm to several tens of μm on the surface. In that case, if a void occurs in the solder 13 during reflow, the generated void is more difficult to escape to the outside due to the unevenness caused by the height difference. Therefore, in chip resistors, it is more strongly desired to suppress voids during surface mounting than in other electronic components (capacitors, varistors, etc.). The electronic component 1 according to this embodiment can meet such a demand, and is therefore particularly useful in chip resistors.

[0028] Next, the surface state of the external electrode 6 will be described in detail.

[0029] As described above, the amount of tin hydroxide on the surface of the external electrode 6 is 100 μmol / m 2 Preferably, the amount of tin hydroxide on the surface of the external electrode 6 is 90 μmol / m 2 Less than or equal to 85 μmol / m 2The amount of tin hydroxide on the surface of the external electrode 6 can be measured by the method described in the examples below.

[0030] Preferably, the surface of the external electrode 6 has a water contact angle of 80 to 110°. More preferably, the surface of the external electrode 6 has a water contact angle of 90 to 110°. If the water contact angle is in this range, the formation of tin hydroxide can be suppressed for a long period of time. As a result, the occurrence of voids during surface mounting can be suppressed for a long period of time. For example, by having a water contact angle of 80 to 110°, even when an accelerated life test is performed by PCT treatment (121°C, 2 atm, 5 hours, humidity = unsaturated 100%), the amount of tin hydroxide is 100 μmol / m 2 It is possible to realize a surface as described below. It is also possible to obtain an electronic component 1 that can be used even after being stored for three years or more after production, or for five years or more after production. The water contact angle can be measured by a method that will be described in the examples below.

[0031] Preferably, the surface of the external electrode 6 has a water contact angle change rate before and after PCT treatment (121°C, 2 atm, 5 hours, humidity=100% unsaturated) within ±10% (amount of change in water contact angle before and after PCT treatment, assuming that the water contact angle before PCT treatment is 100%). Note that the PCT treatment conditions are merely an example and do not limit the present invention.

[0032] As described above, according to this embodiment, since the surface of the external electrode 6 has a specific state, hydroxylation of the surface of the tin plating layer 8 is suppressed, and the occurrence of voids in solder surface mounting can be suppressed. Furthermore, according to this embodiment, oxidation of the surface of the tin plating layer 8 can also be suppressed. In other words, both oxidation and hydroxylation of the surface of the tin plating layer 8 are suppressed, and it is possible to achieve both the effect of preventing discoloration of the tin plating layer 8 and the effect of preventing the occurrence of voids in solder surface mounting.

[0033] In addition, according to the present embodiment, the occurrence of voids is suppressed for a long period of time, so that surface mounting is possible while maintaining connection reliability even after storage for, for example, three years or more after manufacture. This eliminates the need to discard electronic components, leading to a reduction in the amount of waste.

[0034] In this embodiment, the electronic component 1 is described as a chip resistor; however, the present invention is not limited to chip resistors, and can be applied to any electronic component whose main body is made of ceramic, such as a capacitor or varistor.

[0035] (2) Manufacturing methods for electronic components The electronic component 1 having the above-described configuration can be obtained by employing a specific manufacturing method. The manufacturing method of the electronic component 1 according to this embodiment will be described below with reference to an example.

[0036] First, prepare a component body 2. Specifically, a large insulating substrate for producing a plurality of chip resistors is prepared as the component body 2. Then, dividing grooves are formed in the component body 2 for ultimately dividing it into individual chip resistors.

[0037] Next, the internal electrodes 3 and the back surface electrodes 4 are formed at predetermined positions on the main surface 2-1 and the back surface 2-2 of the component body 2. The internal electrodes 3 and the back surface electrodes 4 can be formed, for example, by screen printing a silver-based paste and firing it.

[0038] Next, the resistor 9 is formed on the main surface 2-1 of the component body 2, overlapping a part of the internal electrode 3. The resistor 9 can be formed, for example, by screen printing a paste containing a constituent material such as ruthenium oxide, followed by firing. Note that the internal electrode 3 and the back electrode 4 may be formed after the resistor 9, in which case the end of the resistor 9 is overlapped with a part of the internal electrode 3 for electrical connection.

[0039] Next, a glass protective film 10-2 is formed so as to cover the resistor 9 and a part of the internal electrode 3.

[0040] Next, a trimming groove (notch) is formed in part of resistor 9 using a laser or the like, and the resistance value of resistor 9 is adjusted to a desired value.

[0041] Next, a resin protective film 10-1 (eg, epoxy resin) is formed so as to cover the glass protective film 10-2.

[0042] Next, the component body 2 is divided into rectangular shapes so that the end faces 2-3 are formed in the component body 2.

[0043] Next, an NiCr alloy material is sputtered onto the end surface 2-3 of the component body 2 to form an end surface electrode 5.

[0044] Next, the component body 2 is divided into individual pieces.

[0045] Next, the external electrode 6 is formed on the end electrode 5. Specifically, first, a base layer 7 is formed on the end electrode 5. The base layer 7 can be formed, for example, by electrolytic nickel plating. Next, a tin plating layer 8 is formed on the base layer 7. The tin plating layer 8 can be formed, for example, by electrolytic plating. After the tin plating layer 8 is formed, the external electrode 6 is washed with water and dried. As a result, the external electrode 6 is formed.

[0046] The water contact angle on the surface of the tin plating layer 8 after drying (which is also the surface of the external electrode 6) is usually less than 80°. Therefore, the surface of the external electrode 6 is treated with a treatment liquid so that the water contact angle becomes 80 to 110°. In this case, for example, by using Metas HB-15 (manufactured by Yuken Industry Co., Ltd.) as the treatment liquid, the water contact angle on the surface of the external electrode 6 can be made 80 to 110°. By treating the surface so that the water contact angle becomes 80 to 110°, the subsequent generation of tin hydroxide can be suppressed. In other words, when the amount of tin hydroxide on the surface is 100 μmol / m 2 The following controlled external electrodes 6 can be obtained:

[0047] The treatment with the treatment liquid may be performed by immersion or spraying. The immersion method is preferred because it allows the treatment liquid to be uniformly brought into contact with the surfaces of the electronic component 1 (particularly the external electrodes 6). In other words, it is preferred to immerse the external electrodes 6 in a chemical solution containing the treatment liquid. EXAMPLES

[0048] In the following, examples carried out by the inventors will be described in more detail in order to explain the present invention in more detail. However, the present invention should not be construed as being limited to the following examples.

[0049] Comparative Example 1 As an electronic component according to Comparative Example 1, a chip resistor having the configuration shown in FIG. 1 and FIG. 2 was obtained. Specifically, a sample was prepared in which a resistor, a protective film, an internal electrode, a back electrode, and an end electrode were formed on a ceramic component body. After the sample was prepared, a nickel plating layer was formed as a base layer by barrel plating. Specifically, the component body and a dummy ball, which is a current-carrying assistant, were put into a barrel, and nickel plating (20 A, 25 minutes) was performed while rotating the barrel. A Watts bath without additives was used as the plating bath. The film thickness of the base layer was about 8 μm. Subsequently, tin electrolytic plating (7 A, 15 minutes) was performed on the base layer by barrel plating to form a tin plating layer with a thickness of about 5 μm. A methanesulfonic acid-based semi-gloss bath was used as the tin plating bath. Thus, an external electrode was formed. After tin plating, the surface of the external electrode was washed with water at room temperature. After washing, a drying process was performed at 70° C. for 10 minutes. Thus, an electronic component according to Comparative Example 1 was obtained.

[0050] Comparative Example 2 After tin plating, the electrodes were washed with water at room temperature in the same manner as in Comparative Example 1. Furthermore, the surfaces of the external electrodes were treated with a 50°C aqueous solution of sodium phosphate tribasic (10 g / L) for 60 seconds. After treatment, the electrodes were washed with water and further dried at 70°C for 10 minutes. This produced an electronic component according to Comparative Example 2.

[0051] Example 1 After tin plating, the electrodes were washed with water at room temperature in the same manner as in Comparative Example 1. After washing with water, the surfaces of the external electrodes were treated with a treatment liquid (Metas HB-15, 5 ml / L, manufactured by Yuken Industry Co., Ltd.) at room temperature for 60 seconds. Specifically, the external electrodes were treated by immersing them in the treatment liquid. After treatment, the electrodes were washed with water and further dried at 70°C for 10 minutes. This resulted in the electronic component of Example 1.

[0052] Example 2 The treatment liquid was changed to prototype HB-30 (5 ml / L). The electronic device according to Example 2 was obtained by using the same method as in Example 1. Note that prototype HB-30 is obtained by partially changing the components contained in "Metas HB-15 manufactured by Yuken Industry Co., Ltd."

[0053] Example 3 As in Example 2, the prototype HB-30 was used as the treatment liquid. However, the concentration was changed to (20 ml / L). Other than that, the same method as in Example 2 was used to obtain an electronic device according to Example 3.

[0054] Example 4 As in Example 3, the prototype HB-30 (20 ml / L) was used as the treatment liquid. However, the temperature of the treatment liquid was set to 50° C. Other than that, the same method as in Example 3 was used to obtain an electronic device according to Example 4.

[0055] Example 5 The treatment temperature with the treatment liquid was set to 50° C. Other than that, the same method as in Example 1 was used to obtain an electronic device according to Example 5.

[0056] (Measurement of tin hydroxide content after PCT treatment) The electronic components according to the comparative example and the example were subjected to PCT treatment. Specifically, the electronic components were left in an atmosphere of 121°C and 2 atm (humidity=100% unsaturated) for 5 hours. This PCT treatment is an accelerated life test in which 1 hour is roughly equivalent to 1 year. The conditions of the PCT treatment are merely an example and are not intended to limit the present invention.

[0057] After the PCT treatment, the amount of tin hydroxide on the surface of the external electrode was measured according to the method described in the literature (Analysis of the chemical state of tin oxide film by voltammetry using ammonia buffer as the electrolyte, Nakayama et al., Materials and the Environment, Vol. 62, p. 16-21, (2013)). Specifically, the reduction of SnO2·nH2O (SnO2·nH2O+2H2O+4e - →Sn+nH2O+4OH - The amount of SnO2·nH2O was measured. A chip resistor with a tin-plated external electrode was used as the working electrode, an Ag / AgCl electrode was used as the reference electrode, and a Pt / Ti plate was used as the counter electrode, and the measurement was performed using a three-electrode method. An ammonia buffer solution (0.5M NH4OH + 0.5M NH4Cl) was used, and the potential was swept from -06V to -1.8V to -0.6V at a sweep rate of 20mV / s for two cycles. The results of the voltammetry measurement are shown in Figure 4. The amount of SnO2·nH2O was calculated from the difference in the amount of electricity between the first cycle and the second cycle (after removal of SnO2·nH2O) in the range from -1.4V to -1.8V, where reduction of SnO2·nH2O is said to occur according to the above literature.

[0058] Specifically, the difference in the quantity of electricity per unit area [C / m 2 Here, according to Faraday's law of electrolysis, the amount of substance can be calculated by the following formula 1 using the amount of electricity, the ion valence, and the Faraday constant. (Equation 1) Amount of substance [mol] = (Amount of electricity [C]) / (Ion valence × Faraday constant [C / mol]) In the above-mentioned reaction to form tin hydroxide, the ionic valence is 4. The Faraday constant is 96485 [C / mol]. Therefore, the difference in the quantity of electricity per unit area [C / m 2 ], the amount of tin hydroxide per unit area [mol / m 2 ] was requested. (Equation 2) Tin hydroxide content [mol / m 2 ]=(Difference in electrical quantity [C / m 2]) / (4×96485[C / mol])

[0059] As a specific measurement example, in Comparative Example 1, the difference in the amount of electricity per unit area was 277.6 [C / m 2 ]. Therefore, 277.6[C / m 2 ] / (4×96485[C / mol])=719μmol / m 2 The amount of tin hydroxide per unit area is 719 μmol / m 2 For the other comparative examples and examples, the amount of tin hydroxide was determined in the same manner.

[0060] (Measurement of void occurrence rate after PCT treatment) The void ratio during surface mounting was measured for the electronic components according to the comparative example and the example after the PCT treatment. Specifically, a circuit board having gold-plated lands was prepared. Solder paste was applied onto the lands. Next, the electronic components were mounted on the circuit board using a desktop mounter so that the external electrodes were in contact with the solder paste. Next, a reflow process was performed at a peak temperature of 245°C. After the reflow process was completed, the solder was observed using an X-ray microscope, and the area of ​​the void portion relative to the electrode area was calculated as the void generation rate.

[0061] (Measurement of water contact angle before and after PCT treatment) Instead of a chip resistor, a sample was prepared in which fired Ag was printed as a back electrode on the entire back surface of an alumina substrate. Then, nickel plating, tin plating, and post-treatment were performed on the back electrode under the same conditions as those of Comparative Example 1 and Examples 4 to 5 to form an external electrode. The obtained sample was cut to approximately 1 x 5 cm. Then, the water contact angle of the obtained sample was measured before and after PCT treatment (121°C, 2 atm, humidity = 100% unsaturated, 5 hours). The water contact angle was measured with reference to the description of JISR3257 (static drop method). Specifically, first, ultrasonic cleaning (200W, 35kHz, 10 minutes) was performed to remove air bubbles adsorbed on the unevenness of the electrode surface. After ultrasonic cleaning, a DMo-502 manufactured by Kyowa Interface Science was used to drop 2μL of water, and the water contact angle 1 second after the drop was measured by the θ / 2 method. The samples used in this measurement were different from those used in the measurement of the amount of tin hydroxide, etc., in that they were not chip resistors, but there was no change in the method of producing and processing the external electrodes, and therefore the results of this measurement were used as the results of the water contact angles of Comparative Example 1 and Examples 4 to 5. Note that for each Comparative Example and Example, the measurement was repeated multiple times to determine the minimum, maximum, and average values.

[0062] (Results and Discussion) The measurement results of the amount of tin hydroxide and the void generation rate are shown in Table 1. As shown in Table 1, when the amount of tin hydroxide was 100 μmol / m 2 In the following Examples 1 to 5, the amount of tin hydroxide is 100 μmol / m 2 The void generation rate was lower than that of Comparative Examples 1 and 2, which were more than 100 μmol / m 2 It was confirmed that the void generation rate can be reduced by controlling the following:

[0063] FIG. 5 shows the results of the water contact angle before and after the PCT treatment for Comparative Example 1 and Examples 4 to 5. The water contact angle before the PCT treatment was less than 80° in Comparative Example 1, whereas it was within the range of 80 to 110° in Examples 4 to 5. From this result, it can be understood that by treating the surface of the external electrode so that the water contact angle is within the range of 80 to 110°, the formation of tin hydroxide is suppressed for a long period of time, and as a result, the void generation rate can be reduced for a long period of time. In Comparative Example 1, the water contact angle changed significantly before and after the PCT treatment, and the rate of change exceeded ±10%. In contrast, in Examples 4 and 5, the rate of change of the water contact angle before and after the PCT treatment was within ±10%, and the rate of change was small.

[0064] In addition, in Comparative Examples 1 and 2, slight discoloration was visually observed after the PCT treatment, whereas in Examples 1 to 5, no discoloration occurred even after the PCT treatment.

[0065] [Table 1] [Explanation of symbols]

[0066] REFERENCE SIGNS LIST 1 electronic component, 2 component body, 3 internal electrode, 4 back electrode, 5 end electrode, 6 external electrode, 7 undercoat layer, 8 tin plating layer, 9 resistor, 10 protective film, 11 electronic board, 12 land, 13 solder

Claims

1. A component body made of ceramic; an external electrode provided on the component body; Equipped with the surface of the external electrode is formed of tin; The tin hydroxide (SnO 2 ・nH 2 O) is 100 μmol / m 2 is as follows: The electronic component is used such that the external electrodes are surface-mounted by soldering.

2. 2. The electronic component according to claim 1 , Even when the surface of the external electrode is subjected to PCT treatment, tin hydroxide (SnO 2 ・nH 2 O) is 100 μmol / m 2 A surface such that Electronic components.

3. 3. The electronic component according to claim 1, The external electrode has a base layer, The tin is provided on the underlayer. Electronic components.

4. 3. The electronic component according to claim 1, The surface of the external electrode is formed by tin plating. Electronic components.

5. 3. The electronic component according to claim 1, The water contact angle on the surface of the external electrode is 80° to 110°. Electronic components.

6. 3. The electronic component according to claim 1, Used after being stored for more than three years after manufacture, Electronic components.

7. 3. The electronic component according to claim 1, A chip resistor, Electronic components.

8. 1. A method for manufacturing an electronic component in which external electrodes are surface-mounted by solder, comprising the steps of: Providing a component body made of ceramic; forming the external electrodes on the component body, the surfaces of the external electrodes being formed by tin plating; The surface of the external electrode is treated with a treatment liquid to form a tin hydroxide (SnO 2 ・nH 2 O) suppression; Equipped with A method for manufacturing electronic components.

9. The method according to claim 8, further comprising the steps of: The tin hydroxide (SnO 2 ・nH 2 The step of suppressing the generation of tin hydroxide (SnO 2 ・nH 2 O) at a concentration of 100 μmol / m 2 The method includes controlling Manufacturing method.

10. The method according to claim 8 or 9, The tin hydroxide (SnO 2 ・nH 2 O) includes treating the surface of the external electrode with the treatment liquid so that the surface of the external electrode has a water contact angle of 80 to 110°. Manufacturing method.

11. The method according to claim 8 or 9, the step of suppressing the generation of tin hydroxide includes a step of immersing the external electrodes in the treatment liquid. Manufacturing method.