Polylactic acid modifier, polylactic acid resin composition, and method for manufacturing molding
A block copolymer of L-type or D-type polylactic acid and polyol addresses the complexity of conventional modifiers by enhancing flexibility and crystallinity with a single additive, achieving faster crystallization and improved production efficiency.
Patent Information
- Application Number
- JP2023066678
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-25
AI Technical Summary
Conventional polylactic acid modifiers require multiple additives to improve flexibility and crystallinity, complicating the manufacturing process and reducing production efficiency due to the need for separate equipment and time-consuming solvent dissolution.
A block copolymer containing structural units from L-type or D-type polylactic acid and polyol, which forms stereocomplex crystals, improving flexibility and crystallinity with a single additive and enhancing production efficiency.
The block copolymer reduces crystallization time by over 30% and increases flexibility by 5% or more, allowing for easier mixing and improved production efficiency without the need for special equipment.
Smart Images

Figure 2024152464000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a polylactic acid modifier, a polylactic acid resin composition, and a method for producing a molded article. [Background technology]
[0002] Polylactic acid is a resin material that is biodegradable and has biomass properties, and demand for it as a material that can address environmental issues is growing. However, it has known problems such as its hard and brittle nature, poor impact resistance and flexibility, and poor crystallinity, which means it takes a long time to solidify or crystallize, and poor heat resistance.
[0003] It is known that various modifiers are used to improve the physical properties of these polylactic acids. For example, it is known that plasticizers and crystal nucleating agents are added as additives to improve flexibility and heat resistance (e.g., Patent Document 1).
[0004] Another known modification method is to use a compound containing an optical isomer as an additive to form a stereocomplex (sc crystal) to improve crystallinity (for example, Patent Document 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2014-118452 A [Patent Document 2] International Publication No. 2011 / 030766 Summary of the Invention [Problem to be solved by the invention]
[0006] However, in order to improve flexibility and crystallinity, it was necessary to use a combination of multiple additives with conventional additives. Furthermore, the general dosage forms of the above additives are liquid or powder, so when using them with polylactic acid, which is generally in pellet form, separate mixing equipment is required. This causes a problem of the manufacturing process becoming complicated.
[0007] In addition, in the compound disclosed in Patent Document 2, polylactic acid and additives need to be dissolved in a solution, which takes time for mixing and requires special equipment for dissolving, complicating the production process. In addition, the need to remove the solvent reduces production efficiency.
[0008] Therefore, an object of the present disclosure is to provide a polylactic acid modifier that can improve flexibility and crystallinity by a single additive and can produce a polylactic acid resin composition with excellent production efficiency. [Means for solving the problem]
[0009] In other words, the present disclosure provides a polylactic acid modifier that is a block copolymer that contains at least a constituent unit derived from either L-type or D-type polylactic acid and a constituent unit derived from a polyol and has a polylactic acid / polyol / polylactic acid structure.
[0010] The polylactic acid modifier preferably has an average particle size of 0.5 mmΦ or more.
[0011] The polylactic acid modifier preferably does not exhibit fluidity at room temperature.
[0012] The polylactic acid modifier preferably has polycaprolactone as the polyol.
[0013] The present disclosure also provides a polylactic acid resin composition which is a mixture of L- or D-type polylactic acid and a block copolymer which is a polylactic acid modifier containing at least a polylactic acid of a type different from the above polylactic acid and a polyol, the block copolymer exhibiting no fluidity at room temperature and having an average particle size of 0.5 mmΦ or more, which can reduce the time required for crystallization when cooled from a molten state to 100 to 110°C and kept at that temperature by 30% or more compared to the above polylactic acid alone, and which has a flexibility improvement rate at room temperature of 5% or more.
[0014] In the polylactic acid resin composition, the content of the block copolymer in the total amount of the polylactic acid resin composition is preferably 0.5 to 50% by mass.
[0015] In the polylactic acid resin composition, the polyol is preferably polycaprolactone.
[0016] The present disclosure also provides a method for producing a molded product obtained by molding the polylactic acid resin composition using any one of molding methods selected from the group consisting of injection molding, extrusion molding, compression molding, transfer molding, lamination molding, cast molding, powder molding, calendar molding, foam molding, blow molding, vacuum / pressure molding, and melt spinning. Effect of the Invention
[0017] The polylactic acid modifier of the present disclosure can improve flexibility and crystallinity as a single additive, making it possible to prepare a polylactic acid resin composition with excellent production efficiency. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] [Polylactic acid modifier] The polylactic acid modifier according to one embodiment of the present disclosure is a block copolymer that contains at least a constitutional unit derived from either L-type or D-type polylactic acid and a constitutional unit derived from a polyol, and contains a structure of polylactic acid / polyol / polylactic acid (hereinafter, the block copolymer may be referred to as the "block copolymer of the present disclosure"). Only one type of block copolymer of the present disclosure may be used, or two or more types may be used.
[0019] The block copolymer of the present disclosure contains at least a constituent unit derived from either L-type or D-type polylactic acid and a constituent unit derived from a polyol, and is a block copolymer containing a polylactic acid / polyol / polylactic acid structure, and forms sc crystals with the polylactic acid, thereby improving the crystallinity of the polylactic acid, and since it contains a polyol, flexibility can also be improved.
[0020] In this disclosure, "crystallinity" refers to the ease with which a polylactic acid resin composition crystallizes, and "good crystallinity" means that the composition crystallizes quickly.
[0021] In addition, the block copolymer of the present disclosure preferably further contains a structural part derived from a polymerization initiator. As the polymerization initiator, a known or conventional polymerization initiator can be used, for example, a low molecular weight diol compound or a low molecular weight diamine. In addition, the molecular weight of the polymerization initiator is preferably 500 or less.
[0022] Examples of the low molecular weight diol compound include ethylene glycol, propylene glycol, 1,4-butylene glycol, 2-methylpropanediol, neopentyl glycol, pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 3-methyl-1,5-pentanediol, 3,3-dimethylolheptane, neopentyl glycol, diethylene glycol, dipropylene glycol, cyclohexane-1,4-diol, cyclohexane-1,4-dimethanol, dimer acid diol, etc. Among these, diethylene glycol is particularly preferred.
[0023] The content of the polymerization initiator is preferably 0.2 to 2.0 mass %, more preferably 0.1 to 1.0 mass %, and even more preferably 0.2 to 0.5 mass %, based on the total amount of the block copolymer of the present disclosure.
[0024] The polyol in the block copolymer of the present disclosure is preferably one having a thermal decomposition temperature of 200° C. or higher from the viewpoint of dissolving both polylactic acid and, specifically, for example, polylactone polyols, polyester polyols, polyether polyols, polycarbonate polyols, polyolefin polyols, poly(meth)acrylic polyols, etc. Only one type of the polyol may be used, or two or more types may be used.
[0025] Examples of the polylactone polyols include polybutyrolactone, polyvalerolactone, and polycaprolactone.
[0026] Examples of the polyester polyols include polyethylene adipate diol, polybutylene adipate diol, polyhexamethylene adipate diol, polyhexamethylene isophthalate diol, polyneopentyl adipate diol, polyethylene propylene adipate diol, polyethylene butylene adipate diol, polybutylene hexamethylene adipate diol, poly(polyoxytetramethylene) adipate diol, poly(3-methylpentylene adipate) diol, polyethylene azelate diol, polyethylene sebacate diol, polybutylene azelate diol, polybutylene sebacate diol, and polyneopentyl terephthalate diol.
[0027] Examples of the polyether polyols include polyalkylene glycols such as polyethylene glycol, polypropylene glycol, poly-1,2-butylene glycol, polytetramethylene glycol (poly-1,4-butanediol), poly-3-methyltetramethylene glycol, and polyneopentyl glycol.
[0028] Examples of the polycarbonate polyols include polyhexamethylene carbonate diol, polypentamethylene carbonate diol, polytetramethylene carbonate diol, and poly(tetramethylene / hexamethylene) carbonate diol (e.g., a diol obtained by condensing 1,4-butanediol and 1,6-hexanediol with a dialkyl carbonate while causing a dealcoholization reaction).
[0029] The poly(meth)acrylic polyols include, for example, homopolymers and copolymers of (meth)acrylic acid esters having a hydroxyl group. Poly(meth)acrylic polyols can also be obtained by copolymerizing compounds having polymerizable unsaturated bonds in addition to (meth)acrylic acid esters having a hydroxyl group. In the present invention, "(meth)acrylic" means "methacrylic and / or acrylic".
[0030] The (meth)acrylic acid ester having a hydroxy group includes those having one (meth)acryloyl group, and examples thereof include those having a hydroxyalkyl group having 2 to 20 carbon atoms {for example, hydroxyalkyl (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate}, and (meth)acrylic acid monoesters of trihydric alcohols {for example, a (meth)acrylic acid monoester of glycerin and a (meth)acrylic acid monoester of trimethylolpropane}.
[0031] Among these, from the viewpoint of imparting flexibility to the polylactic acid resin composition, the polyol is preferably the polylactone polyol, and among these, polycaprolactone is particularly preferred since it does not use any components harmful to the human body.
[0032] The number average molecular weight (Mn) of the polyol in the block copolymer of the present disclosure is preferably 1800 to 22000, more preferably 1300 to 10000, and even more preferably 3000 to 15000. When the number average molecular weight (Mn) is 2000 or more, it becomes easy to impart flexibility to the polylactic acid resin composition, and when it is 30000 or less, it becomes possible to suppress the formation of a continuous crystal structure of the polyol, and to easily maintain the flexibility of the material.
[0033] The content of polyol in the block copolymer of the present disclosure is preferably 15 to 90% by mass, more preferably 20 to 85% by mass, and even more preferably 30 to 80% by mass, based on the total amount of the block copolymer of the present disclosure. When the content of polyol is 15% by mass or more, the amount of polyol becomes sufficient, and it becomes easy to impart flexibility to the polylactic acid resin composition. When the content of polyol is 90% by mass or less, it becomes easy to improve the crystallinity.
[0034] The polylactic acid in the block copolymer of the present disclosure is preferably a type of polylactic acid different from the polylactic acid to be modified. That is, when the polylactic acid to be modified is L-type polylactic acid, the polylactic acid in the block copolymer of the present disclosure preferably contains D-type polylactic acid as a main component, and when the polylactic acid to be modified is D-type polylactic acid, the polylactic acid in the block copolymer of the present disclosure preferably contains L-type polylactic acid as a main component.
[0035] When the polylactic acid in the block copolymer of the present disclosure is an L-type polylactic acid mainly composed of L-type lactic acid, the content of the L-type lactic acid unit is preferably 90% by mass or more, more preferably 99% by mass or more of a homopolymer. Similarly, when the polylactic acid is a D-type polylactic acid mainly composed of D-type lactic acid, the content of the D-type lactic acid unit is preferably 90% by mass or more, more preferably 99% by mass or more of a homopolymer.
[0036] The number average molecular weight (Mn) of the polylactic acid in the block copolymer of the present disclosure is preferably 4000 to 15000, more preferably 5000 to 12000, and even more preferably 6000 to 10000. When the number average molecular weight (Mn) is 4000 or more, it becomes easy to form sc crystals with the polylactic acid of the present disclosure and improve the crystallinity, and when it is 15000 or less, it is possible to prevent the sudden growth of the sc crystals and the excessive expansion of the sc crystal domains from forming non-uniform crystals and destabilizing the physical properties.
[0037] The content of polylactic acid in the block copolymer of the present disclosure is preferably 10 to 85% by mass, more preferably 15 to 80% by mass, and even more preferably 20 to 75% by mass, based on the total amount of the block copolymer of the present disclosure. When the content of polylactic acid is 10% by mass or more, the amount of polylactic acid becomes sufficient, making it easy to impart crystallinity. When the content of polylactic acid is 85% by mass or less, it makes it easy to impart flexibility. The content of polylactic acid above represents the total amount of polylactic acid added to both ends of the polyol.
[0038] The number average molecular weight (Mn) of the block copolymer of the present disclosure is preferably 10,000 to 50,000, more preferably 12,000 to 45,000, and even more preferably 14,000 to 40,000. When the number average molecular weight of the block copolymer is 10,000 or more, it is easy to impart flexibility and crystallinity. In addition, when the number average molecular weight is 50,000 or less, it is possible to suppress variations in product quality caused by an increase in viscosity, which leads to an increase in the load on the stirring blades, and uneven heat conduction in the reaction system.
[0039] The weight average molecular weight (Mw) of the block copolymer of the present disclosure is preferably 10,000 to 100,000, more preferably 15,000 to 90,000, and even more preferably 20,000 to 80,000. When the weight average molecular weight of the block copolymer is 10,000 or more, it is easy to impart flexibility and crystallinity. In addition, when the weight average molecular weight is 100,000 or less, it is possible to suppress variations in product quality caused by the load on the stirring blade due to an increase in viscosity and uneven heat conduction in the reaction system.
[0040] The total amount of the polyol, the polylactic acid, and the polymerization initiator in the block copolymer of the present disclosure is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 100% by mass, based on the total amount of the block copolymer of the present disclosure.
[0041] The block copolymer of the present disclosure may contain other components other than the polymerization initiator, the polylactic acid, and the polyol. Examples of the other components include antioxidants, fillers, flame retardants, pigments, antistatic agents, processing aids, and viscosity improvers. The content of the other compounds is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, even more preferably 1 part by mass or less, and particularly preferably 0 parts by mass, relative to 100 parts by mass of the total amount of the block copolymer of the present disclosure. The block copolymer of the present disclosure may contain a solvent, but it is preferable that the block copolymer does not contain a solvent in order to maintain the pellet shape.
[0042] The block copolymer of the present disclosure preferably does not exhibit fluidity at room temperature (25° C.). In the present disclosure, "has fluidity" means a liquid or paste-like property that exhibits fluidity at room temperature, and is not solid. Since the block copolymer of the present disclosure does not exhibit fluidity at room temperature, it can be easily mixed with the polylactic acid of the present disclosure and has excellent handleability.
[0043] The block copolymer of the present disclosure preferably has an average particle size of 0.5 mmΦ or more, more preferably 1 mmΦ or more, and even more preferably 1.5 mmΦ or more. By having an average particle size of 0.5 mm or more, the block copolymer of the present disclosure can be easily mixed with other resin compounds. The pellet shape of the block copolymer of the present disclosure is not particularly limited, but may be circular, spherical, or sliced. In the present disclosure, the average particle size is determined by shaking sieves with openings of 2.8 mm, 2.36 mm, 2.0 mm, 1.7 mm, and 1.4 mm and a tray stacked in this order for 30 seconds, selecting 10 pellets from the sieve with the largest amount of pellets remaining, measuring their sizes with a vernier caliper, and calculating the average value.
[0044] The block copolymer of the present disclosure can be synthesized by a known or conventional method. Specifically, for example, depending on the block copolymer to be obtained, polyol and polylactic acid can be melt-mixed or solution-mixed in a predetermined ratio, solidified, and then solid-phase polymerized to produce the block copolymer. As another method, it can be produced by synthesizing polyol in advance, preferably by heating to 140 to 200 ° C, and heating polylactic acid to its molecular end, preferably at 150 to 250 ° C, to sequentially polymerize and grow the polyol. Conversely, it can also be produced by synthesizing polylactic acid in advance, sequentially polymerizing and growing the polyol to its molecular end, and then sequentially polymerizing and growing the polylactic acid.
[0045] In particular, when the polyol is a polylactone polyol, it is preferable to produce the polylactone by ring-opening polymerization of lactone at the terminal of a polymerization initiator to obtain the polylactone, and then by sequentially polymerizing and growing polylactic acid at the molecular terminal of the polylactone.
[0046] [Polylactic acid resin composition] A polylactic acid resin composition according to one embodiment of the present disclosure is a mixture of L- or D-type polylactic acid and a block copolymer which is a polylactic acid modifier containing at least a type of polylactic acid different from the polylactic acid and a polyol, the block copolymer exhibiting no fluidity at room temperature and having an average particle size of 0.5 mmφ or more, and compared to the polylactic acid alone, the time required for crystallization when cooled from a molten state to 100 to 110°C and kept at that temperature can be reduced by 30% or more, and the flexibility improvement rate at room temperature is 5% or more.
[0047] The polylactic acid resin composition contains the L- or D-type polylactic acid, a type of polylactic acid different from the polylactic acid, and a block copolymer containing at least a polyol, and thus can form sc crystals. Compared to polylactic acid alone, the time required for crystallization when the temperature is lowered from a molten state to 100 to 110°C and the temperature is kept at 100°C to 110°C can be reduced by 30% or more, thereby improving the crystallinity. In addition, the block copolymer contains the polyol, and the flexibility improvement rate is 5% or more compared to polylactic acid alone, thereby improving the flexibility. Furthermore, the block copolymer has no fluidity and has an average particle size of 0.5 mmΦ or more, so that it can be easily mixed with the polylactic acid, and the production efficiency is excellent.
[0048] The time required for crystallization when the polylactic acid resin composition is cooled from a molten state to 100 to 110°C and kept at this temperature (hereinafter, sometimes referred to as "half crystallization time") is preferably within 100 seconds, more preferably within 80 seconds, and even more preferably within 70 seconds. In addition, compared with the half crystallization time of polylactic acid alone (145 seconds), the half crystallization time of the polylactic acid resin composition can be shortened by 30% or more, preferably by 40% or more, and even more preferably by 50% or more. Since the half crystallization time of the polylactic acid resin composition can be shortened by 30% or more compared to the half crystallization time of polylactic acid alone, crystallization can be performed early and production efficiency can be improved. In addition, in the present disclosure, the temperature when the temperature is lowered from the molten state to 100 to 110°C means that any temperature within the above range can be used as long as the objects to be compared are the same temperature.
[0049] In the present disclosure, the half-crystallization time is calculated by heating the polylactic acid resin composition to 190°C by differential scanning calorimetry (DSC), holding it for 5 minutes to dissolve it, rapidly cooling it to 100 to 110°C, and holding it for 15 minutes, and then calculating the time it takes for the peak area of the exothermic peak of the polylactic acid resin composition to reach half.
[0050] The flexural modulus of the polylactic acid resin composition measured by the method described in the Examples below is preferably 3700 MPa or less, more preferably 3600 MPa or less, and even more preferably 3500 MPa or less. The reduction rate of the flexural modulus of the polylactic acid resin composition relative to the flexural modulus of the polylactic acid alone (flexibility improvement rate) is 5% or more, preferably 7% or more, and even more preferably 10% or more. By having the flexibility improvement rate of the polylactic acid resin composition relative to the polylactic acid alone of 5% or more, the polylactic acid resin composition can easily exhibit flexibility.
[0051] In addition, the difference between the mass ratio of the polylactic acid and the block copolymer in the polylactic acid resin composition measured by the method in the Examples described later and the designed mass ratio is preferably within ±20%, more preferably within ±10%. By keeping the difference between the actual mass ratio and the designed mass ratio within ±20%, mixing can be easily performed.
[0052] <Polylactic acid> The polylactic acid resin composition contains either L-type or D-type polylactic acid (hereinafter, sometimes referred to as "polylactic acid of the present disclosure"). It is also preferable to use the block copolymer of the present disclosure together with the polylactic acid of the present disclosure. The polylactic acid of the present disclosure is a polymer compound obtained by polymerizing a plurality of lactic acids through ester bonds, with lactic acid (CH3CH(OH)COOH) as a constituent unit.
[0053] Lactic acid, which is a structural unit of the polylactic acid of the present disclosure, is known to have two types of optical isomers, L-type and D-type. In the present disclosure, both L-type and D-type lactic acid can be used as structural units. In addition, in order to form sc crystals with the block copolymer described below, the polylactic acid of the present disclosure is preferably a polymer mainly composed of either L-type or D-type, and in the case of an L-type polylactic acid mainly composed of L-type lactic acid, the content of the L-type lactic acid unit is preferably 90% by mass or more, more preferably 99% by mass or more of a homopolymer. Similarly, in the case of a D-type polylactic acid mainly composed of D-type lactic acid, the content of the D-type lactic acid unit is preferably 90% by mass or more, more preferably 99% by mass or more of a homopolymer.
[0054] The polylactic acid of the present disclosure may contain other components within a range that does not impair its properties. Examples of the other components include catalysts, end-capping agents, additives, etc. The content of the other components is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 0 parts by mass, based on the total amount of the polylactic acid.
[0055] The polylactic acid of the present disclosure can be produced by a known method for polymerizing polylactic acid, such as ring-opening polymerization of lactide, dehydration condensation of lactic acid, or a combination of these with solid-phase polymerization, followed by melting and solidifying.
[0056] The number average molecular weight (Mn) of the polylactic acid of the present disclosure is preferably 2,000 to 50,000,000, and more preferably 3,000 to 20,000,000. The weight average molecular weight (Mw) of the polylactic acid of the present disclosure is preferably 2,000 to 80,000,000, and more preferably 3,000 to 40,000,000.
[0057] The content of the polylactic acid of the present disclosure relative to the total amount of the polylactic acid resin composition is preferably 50 to 99.5% by mass, more preferably 60 to 99% by mass, and even more preferably 70 to 98% by mass. By having the content of the polylactic acid of the present disclosure be 50% by mass or more, it is possible to improve the crystallinity and flexibility while maintaining the physical properties of polylactic acid. In addition, by having the content be 99.5% by mass or less, it becomes easy to improve the flexibility and crystallinity of the polylactic acid resin composition.
[0058] The polylactic acid of the present disclosure has an average particle size of preferably 0.5 mmΦ or more, more preferably 1.0 mmΦ or more, and even more preferably 1.5 mmΦ or more. By having an average particle size of 0.5 mmΦ or more, the polylactic acid of the present disclosure can be easily kneaded.
[0059] <Block copolymer> The polylactic acid resin composition contains a block copolymer containing at least a polylactic acid of a type different from that of the polylactic acid of the present disclosure and a polyol as a polylactic acid modifier. Only one type of the block copolymer may be used, or two or more types may be used.
[0060] In addition, the block copolymer preferably further contains a structural portion derived from a polymerization initiator, and depending on the structure of the polymerization initiator, a structure such as a diblock copolymer, a triblock copolymer, a star block copolymer, or a comb block copolymer can be formed.
[0061] As the polymerization initiator, known or commonly used polymerization initiators can be used, such as low molecular weight hydroxyl group-containing compounds, low molecular weight amines, etc. The molecular weight of the polymerization initiator is preferably 500 or less.
[0062] Examples of the low molecular weight hydroxyl group-containing compound include monool compounds such as ethanol, propanol, butanol, pentanol, and hexanol; diol compounds such as ethylene glycol, propylene glycol, 1,4-butylene glycol, 2-methylpropanediol, neopentyl glycol, pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 3-methyl-1,5-pentanediol, 3,3-dimethylolheptane, neopentyl glycol, diethylene glycol, dipropylene glycol, cyclohexane-1,4-diol, cyclohexane-1,4-dimethanol, and dimer acid diol; alkanetriols having 2 to 8 carbon atoms such as 1,2,4-butanetriol and 1,2,6-hexanetriol; and triol compounds such as 5- to 6-membered cycloalkanetriols such as 1,2,3-cyclohexanetriol, as well as low molecular weight hydroxyl group-containing compounds having 4 or more hydroxyl groups. Among these, diol compounds are preferred because they can produce a triblock copolymer, and diethylene glycol is particularly preferred.
[0063] By using the monol compound as the polymerization initiator, a diblock copolymer containing the polyol and the polylactic acid on one side of the polymerization initiator can be prepared, by using the diol compound, a triblock copolymer containing the polyol and the polylactic acid on both ends of the polymerization initiator can be prepared, and by including a triol compound or a low molecular weight hydroxyl group-containing compound having 4 or more hydroxyl groups, a star-shaped or comb-shaped block copolymer can be prepared. Among these, the block copolymer is preferably the block copolymer of the present disclosure.
[0064] The block copolymer does not exhibit fluidity at room temperature (25° C.). In the present disclosure, "having fluidity" means a liquid or paste-like property that exhibits fluidity at room temperature, and is not solid. Since the block copolymer does not exhibit fluidity at room temperature, it can be easily mixed with the polylactic acid of the present disclosure and has excellent handleability.
[0065] The block copolymer has an average particle size of 0.5 mmΦ or more, preferably 1 mmΦ or more, more preferably 1.5 mmΦ or more. By having an average particle size of 0.5 mm or more, it becomes easy to knead other resin compounds. The pellet shape of the block copolymer is not particularly limited, but may be circular, spherical, or sliced.
[0066] The content of the block copolymer in the polylactic acid resin composition is preferably 0.5 to 50% by mass, more preferably 1 to 40% by mass, and even more preferably 2 to 30% by mass. When the content of the block copolymer is 0.5% or more, it becomes easy to improve the flexibility and crystallinity of the polylactic acid resin composition. When the content is 50% by mass or less, it is possible to improve the crystallinity and flexibility while maintaining the physical properties of polylactic acid.
[0067] Moreover, the block copolymer can be prepared in the same manner as the block copolymer of the present disclosure described above.
[0068] The polylactic acid resin composition can be produced by mixing the polylactic acid of the present disclosure and the block copolymer by a known or conventional method. Specifically, the polylactic acid of the present disclosure and the block copolymer are fed through a main feeder of a twin-screw kneading extruder, and kneaded and melted in the extruder to prepare the composition. The block copolymers of the polylactic acid resin composition do not show fluidity at room temperature, and can be fed in the form of pellets with an average particle size of 0.5 mm or more, so that the polylactic acid resin composition can be easily mixed with polylactic acid in the form of pellets.
[0069] In addition, it is preferable that the polylactic acid resin composition is produced without using a solvent, since the polylactic acid resin composition does not require a step for dissolving or removing the solvent, and therefore the production efficiency can be excellent.
[0070] [Method of manufacturing molded products] In addition, the polylactic acid resin composition prepared by the above method can be molded into a molded product by a method such as injection molding, extrusion molding, compression molding, transfer molding, lamination molding, cast molding, powder molding, calendar molding, foam molding, blow molding, vacuum / pressure molding, or melt spinning.
[0071] It is known that when polylactic acid is used as a raw material, the crystallization of polylactic acid is slow in the molding process, and the cooling process takes time, resulting in poor production efficiency, but since the above-mentioned polylactic acid resin composition contains a block copolymer, it can form sc crystals, which allows for early crystallization, thereby improving production efficiency.In addition, since it contains a polyol structural part, it has excellent flexibility.
[0072] Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification. In addition, each configuration in each embodiment and their combinations are merely examples, and addition, omission, and other modifications of configurations are possible as appropriate within the scope of the present disclosure. The present disclosure is not limited by the embodiments, but is limited only by the claims. EXAMPLES
[0073] Hereinafter, one embodiment of the present disclosure will be described in more detail based on examples.
[0074] Manufacturing Example 1 (Synthesis of block copolymers) As raw materials, 246.77 g of ε-caprolactone (manufactured by Daicel Corporation) and 2.19 g of diethylene glycol (manufactured by Tokyo Chemical Industry Co., Ltd.) were placed in a separable flask and heated to 100°C, after which 0.0314 g of stannous octoate (trade name "Stanoct", manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added. The temperature was then raised to 150°C, and stirring and heating were continued until the concentration of ε-caprolactone became less than 1% by mass. After cooling to 60°C, 60.60 g of D-lactide (D-isomer purity: 96.4%) was added, and the temperature was raised to 170°C at normal pressure, followed by stirring and heating until the concentration of D-lactide became less than 4% by mass. Through the above steps, 306.1 g of a triblock copolymer of D-type polylactic acid (PDLA) / polycaprolactone (PCL) / D-type polylactic acid (PDLA) (weight average molecular weight (Mw): 31,000, number average molecular weight (Mn): 15,000, hereinafter sometimes referred to as "block copolymer A") was obtained.
[0075] Block copolymer A was placed in the melting cylinder (500 ml) of a simple extrusion device and melted by heating with a heating jacket at 170°C to 190°C for 10 minutes. The pressurized cylinder was operated, and the resin was passed through a (circular) die with a hole diameter of 2.5 mmΦ and pelletized with a small pelletizer to obtain pellets of the block copolymer of Production Example 1 with an average particle diameter of 2.3 mmΦ.
[0076] Manufacturing Example 2 Except for using 108.56 g of ε-caprolactone (manufactured by Daicel Corporation) and 488.5 g of D-lactide (D-isomer purity: 96.4%) as raw materials, 531 g of block copolymer pellets of Production Example 2 were obtained under the same conditions as Production Example 1. The block copolymer of Production Example 2 was a PDLA / PCL / PDLA triblock copolymer (weight average molecular weight (Mw): 34,000, number average molecular weight (Mn): 20,000; hereinafter, sometimes referred to as "block copolymer B").
[0077] Production Example 3 Except for using 238.91 g of ε-caprolactone (manufactured by Daicel Corporation) and 358.4 g of D-lactide (D-isomer purity: 96.4%) as raw materials, 583 g of block copolymer pellets of Production Example 3 were obtained under the same conditions as Production Example 1. The block copolymer of Production Example 3 was a PDLA / PCL / PDLA triblock copolymer (weight average molecular weight (Mw): 44,000, number average molecular weight (Mn): 30,000; hereinafter, sometimes referred to as "block copolymer C").
[0078] Production Example 4 Except for using 413.68 g of ε-caprolactone (manufactured by Daicel Corporation) and 413.7 g of D-lactide (D-isomer purity: 96.4%) as raw materials, 814 g of block copolymer pellets of Production Example 4 were obtained under the same conditions as Production Example 1. The block copolymer of Production Example 4 was a PDLA / PCL / PDLA triblock copolymer (weight average molecular weight (Mw): 73,000, number average molecular weight (Mn): 39,000; hereinafter, sometimes referred to as "block copolymer D").
[0079] Example 1 The pellets of block copolymer A and L-type polylactic acid (PLLA) pellets (L-form purity 99% or more, average particle size 2.5 mmΦ) of Production Example 1 were each dried in a constant temperature dryer at 80°C for 3 hours or more. After drying, they were allowed to cool in a desiccator, and a ratio of 3% by mass of block copolymer A and 97% by mass of PLLA was measured and placed in a shaker and blended. The cylinder temperature of a small resin kneading device (product name: Labo Plastomill 4M150, manufactured by Toyo Seiki Seisakusho) was set to 190°C, and 30 g of the measured pellets were placed in the kneading chamber while rotating the cylinder at 10 rpm. Thereafter, the lid was closed, the cylinder rotation speed was increased to 50 rpm, and kneading was performed for 5 minutes. The cylinder was stopped, and the uniformly kneaded molten resin was taken out, placed in a metal vat, and cooled in a desiccator to prepare the polylactic acid resin composition of Example 1.
[0080] Example 2 A polylactic acid resin composition of Example 2 was prepared in the same manner as in Example 1, except that the blending amounts shown in Table 1 were used.
[0081] Examples 3 and 4 Polylactic acid resin compositions of Examples 3 and 4 were prepared in the same manner as in Example 1, except that the block copolymer B prepared in Production Example 2 was used in the amounts shown in Table 1.
[0082] Examples 5 and 6 Polylactic acid resin compositions of Examples 5 and 6 were prepared in the same manner as in Example 1, except that the block copolymer C prepared in Production Example 3 was used in the amounts shown in Table 1.
[0083] Examples 7 and 8 Polylactic acid resin compositions of Examples 7 and 8 were prepared in the same manner as in Example 1, except that the block copolymer D prepared in Production Example 4 was used in the amounts shown in Table 1.
[0084] Comparative Example 1 A polylactic acid resin composition of Comparative Example 1 was prepared in the same manner as in Example 1, except that simple poly-L lactic acid was used.
[0085] Comparative Example 2 Powdered crystallinity improver B (aromatic sulfonate, average particle size 35 μm) and L-type polylactic acid (PLLA) pellets (L-purity 99% or more, average particle size 2.5 mmΦ) were dried in a constant temperature dryer at 80 ° C. for 3 hours or more. The cylinder temperature of a small resin kneading device (product name "Labo Plastomill (Labo Plastomill 4M150), manufactured by Toyo Seiki Seisakusho) was set to 190 ° C., and 29.1 g of PLLA pellets were weighed and placed in the kneading chamber while rotating the cylinder at 10 rpm, and then 0.9 g of crystallinity improver B was added. Thereafter, the lid was closed, the cylinder rotation speed was increased to 50 rpm, and kneading was performed for 5 minutes. The cylinder was stopped, and the uniformly kneaded molten resin was taken out, placed in a metal vat, and cooled in a desiccator to prepare a polylactic acid resin composition of Comparative Example 2.
[0086] Comparative Example 3 A polylactic acid resin composition of Comparative Example 3 was prepared in the same manner as in Comparative Example 2, except that a powdery physical property improver A (acrylic compound, average particle size 100 μm) was used.
[0087] Comparative Example 4 A polylactic acid resin composition of Comparative Example 4 was prepared in the same manner as in Comparative Example 2, except that a liquid property improving agent B (aliphatic ester surfactant) was used.
[0088] Comparative Example 5 D-type polylactic acid (PDLA, granular crystal improver A, average particle size 2.5 mmΦ) and the above powder physical property improver A and L-type polylactic acid (PLLA) pellets (L-form purity 99 % or more) was dried at 80°C for 3 hours or more in a constant temperature dryer. The cylinder temperature of a small resin kneading device (product name: Labo Plastomill 4M150, manufactured by Toyo Seiki Seisakusho) was set to 190°C, and 29.1 g of the measured PLLA pellets were placed in the kneading chamber while rotating the cylinder at 10 rpm, and then 0.3 g of the granular crystal improver A and 0.6 g of the powdery physical property improver A were added. Thereafter, the lid was closed, the cylinder rotation speed was increased to 50 rpm, and kneading was performed for 5 minutes. The cylinder was stopped, and the uniformly kneaded molten resin was taken out, placed in a metal vat, and cooled in a desiccator to prepare a polylactic acid resin composition of Comparative Example 5.
[0089] Comparative Example 6 A polylactic acid resin composition of Comparative Example 6 was prepared in the same manner as in Comparative Example 5, except that the liquid property improver B was used instead of the powdery property improver A.
[0090] Comparative Example 7 A polylactic acid resin composition of Comparative Example 7 was prepared in the same manner as in Comparative Example 5, except that the powdery crystallinity improving agent B was used instead of the granular crystallinity improving agent A.
[0091] Comparative Example 8 A polylactic acid resin composition of Comparative Example 8 was prepared in the same manner as in Comparative Example 7, except that the liquid property improver B was used instead of the powdery property improver A.
[0092] [evaluation] The polylactic acid resin compositions prepared in the Examples and Comparative Examples were subjected to the following evaluations, and the results are shown in Table 1. In Table 1, " / " indicates that measurement was not possible, and "-" indicates that measurement was not possible.
[0093] (1) Half-crystallization time and crystallization time reduction rate The polylactic acid resin compositions prepared in the examples and comparative examples were dried at 80°C for 3 hours, and 5 mg was sampled and measured by DSC under the following conditions. The half-crystallization time was calculated by counting the integral time from the start of the formation of an exothermic peak formed with the crystallization of PLLA, the main component of the polylactic acid resin composition, to the time when the peak area reached half of the peak area, and the results were recorded. Measurement equipment: DSC Q2000 manufactured by TA Instruments Measurement conditions: Heat from room temperature to 190°C (heating rate: 86°C / min), and hold for 5 minutes. Then, cool to 100°C (cooling rate: 83°C / min), and hold for 15 minutes.
[0094] The shortening rate of the half-crystallization time relative to the poly-L lactic acid alone of Comparative Example 1 was calculated as the shortening rate of the crystallization time.
[0095] (2) Flexural modulus and flexibility improvement rate The polylactic acid resin compositions prepared in the examples and comparative examples were sheared to a particle size of 1 to 3 mm and dried in a constant temperature dryer at 80°C for 3 hours. A mold having a plurality of frames of 1 x 10 x 55 mm in size was placed on a metal plate, 1 g of the above polylactic acid resin composition was placed in each frame, and a metal plate was placed on top of it and set in a hot press machine (product name "Mini Test Press 10, manufactured by Toyo Seiki Co., Ltd.) previously set at 190°C. The metal plate and the mold were placed between the hot press machine and preheated for 3 minutes without applying pressure, and then the pressure was increased to 10 MPa and held for 5 minutes. Thereafter, the metal plate and the mold were transferred to a water circulation cooling press and cooled for 5 minutes, and the test piece was removed from the mold. The test piece of 1 x 10 x 55 mm in size was placed in a constant temperature dryer and subjected to a crystallization treatment at 100°C for 20 minutes. The test piece prepared by the above method was subjected to Tensilon bending elastic modulus measurement under the following conditions. Equipment: RTC-1350A manufactured by ORENTEC Measurement conditions: Test type: 3-point bending test Distance between the two lower supports: 32mm - Testing machine body rigidity: 0mm / kgf Load full scale: 5N Test speed: 1mm / min Control method: Constant speed control ·Measurement temperature: room temperature
[0096] The reduction rate of the flexural modulus relative to the L-type polylactic acid alone in Comparative Example 1 was calculated as the flexibility improvement rate.
[0097] (3) Handling and manufacturing stability For the polylactic acid resin compositions prepared in the examples and comparative examples, the additive was colored red with a dye and the PLLA pellets were colored blue in advance. When two additives were used, the crystal improver was colored red and the physical property improver was colored blue. The additives were mixed in the same manner except for coloring and heating, and samples were taken from five random locations in a 10 ml bottle. The pellets taken out of the 10 ml bottle were visually separated by color with tweezers, the mass of the pellets of each color was measured, and the difference between the mass ratio of the pellets of each color measured and the mass ratio of the designed pellets was evaluated as follows. When a powder additive was used, the additives were sieved and separated by color and measured. ○: The difference between the measured mass ratio and the design mass ratio is 10% or less △+: The difference between the measured mass ratio and the design mass ratio is more than 10% to 20%. △: The difference between the measured mass ratio and the designed mass ratio is more than 20% to 30%. △-: The difference between the measured mass ratio and the design mass ratio is more than 30% to 40%. ×: The difference between the measured mass ratio and the designed mass ratio is more than 40%, or mixing is difficult in the actual equipment.
[0098] (4) Injection molding demolding time and demolding time reduction rate The polylactic acid resin composition of Example 4 was dried in a constant temperature dryer at 80°C for 3 hours, and a test piece was prepared using an injection molding machine under the following conditions. The pellets were melted once on the extruder side of the injection molding machine, injected into a mold, and held at a constant pressure after injection. The shortest time from the timing at which the pressure was released to the timing at which the test piece was sufficiently crystallized and solidified so that it could be removed from the mold without deformation was defined as the injection molding demolding time. Injection molding machine: Electric injection molding machine (product name: J110AD-180H, manufactured by Japan Steel Works) Screw diameter: Φ35mm Mold shape: JIS K 7139 (ISO 20753) Type A1 dumbbell specimen shape Cylinder temperature: 40 to 200°C (average temperature: 190°C) Mold temperature: 100~105℃ (Set temperature: 100℃)
[0099] Also, the reduction rate (mold release time reduction rate) of the injection molding demold time of the poly-L lactic acid alone in Comparative Example 1 was calculated.
[0100] [Table 1]
[0101] It was confirmed that the flexibility and crystallinity of the polylactic acid resin composition using the polylactic acid modifier of the embodiment were improved compared to conventional additives. In addition, it was confirmed that the polylactic acid resin composition of the embodiment can be easily mixed without special kneading equipment, and the crystallization time is also shortened, so that the production efficiency is excellent. On the other hand, when polylactic acid alone was used, it took a long time for semi-crystallization, and the bending modulus was also poor (Comparative Example 1). In addition, when only a powdery crystallinity improving agent was used, the flexibility could not be improved, and kneading was difficult, resulting in poor handling (Comparative Example 2). When a powdery or liquid physical property improving agent was used, the flexibility and crystallinity could be improved, but the handling was poor (Comparative Examples 3 and 4). In addition, when the above-mentioned crystallinity improving agent and physical property improving agent were used in combination, the flexibility and crystallinity could be improved, but the handling was poor (Comparative Examples 5 to 8).
[0102] Variations of the present disclosure are described below. [Appendix 1] Contains at least a structural unit derived from either L-type or D-type polylactic acid and a structural unit derived from a polyol, A polylactic acid modifier that is a block copolymer with a polylactic acid / polyol / polylactic acid structure. [Appendix 2] 2. The polylactic acid modifier according to claim 1, having an average particle size of 0.5 mmΦ or more. [Appendix 3] 3. The polylactic acid modifier according to claim 1 or 2, which does not exhibit fluidity at room temperature. [Appendix 4] 4. The polylactic acid modifier according to any one of claims 1 to 3, wherein the polyol is polycaprolactone. [Appendix 5] A mixture of L-type or D-type polylactic acid and a block copolymer which is a polylactic acid modifier containing at least a polylactic acid of a type different from the polylactic acid and a polyol; The block copolymer does not exhibit fluidity at room temperature and has an average particle size of 0.5 mmΦ or more; Compared to the polylactic acid alone, the time required for crystallization when the temperature is lowered from a molten state to 100 to 110°C and kept at that temperature can be reduced by 30% or more, A polylactic acid resin composition having a flexibility improvement rate of 5% or more at room temperature. [Appendix 6] 6. The polylactic acid resin composition according to claim 5, wherein the content of the block copolymer in the total amount of the polylactic acid resin composition is 0.5 to 50% by mass. [Appendix 7] 7. The polylactic acid resin composition according to claim 5, wherein the polyol is polycaprolactone. [Appendix 8] A method for producing a molded product obtained by molding the polylactic acid resin composition according to any one of claims 5 to 7 by any one of molding methods selected from the group consisting of injection molding, extrusion molding, compression molding, transfer molding, lamination molding, cast molding, powder molding, calendar molding, foam molding, blow molding, vacuum / pressure molding, and melt spinning.
Claims
1. Contains at least a structural unit derived from either L-type or D-type polylactic acid and a structural unit derived from a polyol, A polylactic acid modifier which is a block copolymer having a polylactic acid / polyol / polylactic acid structure.
2. 2. The polylactic acid modifier according to claim 1, having an average particle size of 0.5 mmΦ or more.
3. 3. The polylactic acid modifier according to claim 1, which does not exhibit fluidity at room temperature.
4. 3. The polylactic acid modifier according to claim 1, wherein the polyol is polycaprolactone.
5. A mixture of L- or D-type polylactic acid and a block copolymer which is a polylactic acid modifier containing at least a type of polylactic acid different from the polylactic acid and a polyol; The block copolymer does not exhibit fluidity at room temperature and has an average particle size of 0.5 mmΦ or more; Compared to the polylactic acid alone, the time required for crystallization when the temperature is lowered from a molten state to 100 to 110°C and kept at that temperature can be reduced by 30% or more, A polylactic acid resin composition having a flexibility improvement rate of 5% or more at room temperature.
6. 6. The polylactic acid resin composition according to claim 5, wherein the content of said block copolymer in the total amount of said polylactic acid resin composition is 0.5 to 50% by mass.
7. The polylactic acid resin composition according to claim 5 or 6, wherein the polyol is polycaprolactone.
8. A method for producing a molded product obtained by molding the polylactic acid resin composition according to claim 5 or 6 by any one of molding methods selected from the group consisting of injection molding, extrusion molding, compression molding, transfer molding, lamination molding, cast molding, powder molding, calendar molding, foam molding, blow molding, vacuum / pressure molding, and melt spinning.
Citation Information
Patent Citations
Polylactic acid resin composition and its resin molded article
JP2014118452A
Method for producing stereo complex crystals of polylactic acid, polylactic acid, and molded body, synthetic fiber, porous body and ion conductor comprising same
WO2011030766A1