Nonaqueous gel electrolyte, nonaqueous electrolyte storage element, and method for manufacturing nonaqueous electrolyte storage element
A non-aqueous gel electrolyte with a crosslinked polymer and specific solvents addresses complexity and solvent leakage issues, providing stable and oxidation-resistant gel electrolytes for energy storage.
Patent Information
- Application Number
- JP2023066723
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-25
AI Technical Summary
Existing methods for producing non-aqueous gel electrolytes are complex and face challenges with solvent leakage and low oxidation resistance, particularly when using solvents like fluoroethylene carbonate, which hinder long-term gel stability.
A non-aqueous gel electrolyte is produced using a crosslinked polymer with a polyethylene oxide skeleton, a base catalyst, and a non-aqueous solvent comprising sulfones and propylene carbonate, which allows for a simpler process and enhances oxidation resistance and gel stability.
The solution results in a non-aqueous gel electrolyte that can be manufactured easily and maintains high oxidation resistance and stable gel state, ensuring effective performance in energy storage devices.
Smart Images

Figure 2024152495000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a nonaqueous gel electrolyte, a nonaqueous electrolyte storage element, and a method for producing a nonaqueous electrolyte storage element. [Background technology]
[0002] Non-aqueous electrolyte secondary batteries, such as lithium ion secondary batteries, are widely used in electronic devices such as personal computers and communication terminals, automobiles, etc., due to their high energy density. Non-aqueous electrolyte secondary batteries generally have a pair of electrically isolated electrodes and a non-aqueous electrolyte interposed between the electrodes, and are configured to charge and discharge by transferring charge-transporting ions between the electrodes. As non-aqueous electrolyte storage elements other than non-aqueous electrolyte secondary batteries, capacitors such as lithium ion capacitors and electric double layer capacitors are also widely used.
[0003] In recent years, nonaqueous electrolyte storage elements using a gel-like nonaqueous electrolyte as the nonaqueous electrolyte instead of a nonaqueous electrolytic solution have also attracted attention (hereinafter, the gel-like nonaqueous electrolyte is also referred to as a "nonaqueous gel electrolyte"). Nonaqueous electrolyte storage elements using a nonaqueous gel electrolyte have advantages such as being less susceptible to leakage. Patent Document 1 describes a nonaqueous gel electrolyte that includes an electrolyte salt, a nonaqueous solvent, and a polymer having a polyethylene glycol skeleton, the polymer having a network structure due to crosslinking of the polyethylene glycol chains. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-170992 A Summary of the Invention [Problem to be solved by the invention]
[0005] The nonaqueous gel electrolyte described in Patent Document 1 is produced by the following method. First, a hydrogel is obtained by a crosslinking reaction in an aqueous solution containing a monomer. Water is volatilized from the obtained hydrogel to obtain a dry gel. The obtained dry gel is immersed in a nonaqueous electrolyte solution in which an electrolyte salt is dissolved in a nonaqueous solvent, and the nonaqueous gel electrolyte is obtained by swelling the nonaqueous gel electrolyte.
[0006] In the above method, many steps must be taken. In addition, in the above method, it is difficult to obtain a nonaqueous gel electrolyte by preparing a hydrogel in a container of a nonaqueous electrolyte storage element and replacing water with a nonaqueous electrolyte. Therefore, the present inventors have studied a method of obtaining a nonaqueous gel electrolyte by using a base catalyst to crosslink monomers in a nonaqueous electrolyte to form a crosslinked polymer and gel the nonaqueous gel electrolyte. On the other hand, when considering application to a nonaqueous electrolyte storage element with a high energy density, it is desirable to use a nonaqueous solvent with high oxidation resistance for the nonaqueous gel electrolyte. However, it was found that gelation does not occur when fluoroethylene carbonate, a nonaqueous solvent with high oxidation resistance, is used in the method using a base catalyst. In addition, depending on the type of nonaqueous solvent, even if gelation occurs, the nonaqueous solvent may seep out of the gel over time, making it impossible to maintain the gel state for a long period of time.
[0007] The present invention has been made in light of the above circumstances, and an object of the present invention is to provide a nonaqueous gel electrolyte that can be produced by a relatively simple process and has high oxidation resistance and stability in its gel state, a nonaqueous electrolyte storage element including such a nonaqueous gel electrolyte, and a method for producing such a nonaqueous electrolyte storage element. [Means for solving the problem]
[0008] A non-aqueous gel electrolyte according to one aspect of the present invention comprises a crosslinked polymer having a polyethylene oxide skeleton, a base catalyst, and a non-aqueous solvent, the non-aqueous solvent being selected from the group consisting of sulfones and carbonates including propylene carbonate, and having a solubility parameter of 10.0 (cal / cm 3 ) 1 / 2The main component is at least one of the above components.
[0009] A nonaqueous electrolyte storage element according to another aspect of the present invention includes the nonaqueous gel electrolyte according to the aspect of the present invention.
[0010] A method for producing a nonaqueous electrolyte storage element according to another aspect of the present invention includes crosslinking a first compound with a second compound in a container in the presence of a base catalyst and a nonaqueous solvent, wherein at least one of the first compound and the second compound has a polyethylene oxide skeleton, and the first compound and the second compound have functional groups that undergo a crosslinking reaction with each other in the presence of the base catalyst, the nonaqueous solvent is selected from the group consisting of sulfones and carbonates including propylene carbonate, and has a solubility parameter of 10.0 (cal / cm 3 ) 1 / 2 The main component is at least one of the above components. Effect of the Invention
[0011] According to any one aspect of the present invention, it is possible to provide a nonaqueous gel electrolyte that can be produced by a relatively simple process and has high oxidation resistance and stability in a gel state, a nonaqueous electrolyte storage element including such a nonaqueous gel electrolyte, and a method for producing such a nonaqueous electrolyte storage element. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a perspective view showing one embodiment of a nonaqueous electrolyte electricity storage element. [Diagram 2] FIG. 2 is a schematic diagram showing one embodiment of an electricity storage device formed by assembling a plurality of nonaqueous electrolyte electricity storage elements. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] First, an outline of the nonaqueous gel electrolyte, the nonaqueous electrolyte storage element, and the method for producing the nonaqueous electrolyte storage element disclosed in this specification will be described.
[0014] [1] A nonaqueous gel electrolyte according to one aspect of the present invention comprises a crosslinked polymer having a polyethylene oxide skeleton, a base catalyst, and a nonaqueous solvent, the nonaqueous solvent being selected from the group consisting of sulfones and carbonates including propylene carbonate, and having a solubility parameter of 10.0 (cal / cm 3 ) 1 / 2 The main component is at least one of the above components.
[0015] The nonaqueous gel electrolyte described in [1] above can be produced by a relatively simple process, and has high oxidation resistance and stability in the gel state. The reason why such an effect occurs is unclear, but the following reasons are presumed. When producing the nonaqueous gel electrolyte described in [1] above, for example, a crosslinking reaction of a monomer in a nonaqueous electrolyte solution mainly composed of a nonaqueous solvent containing a base catalyst is performed to obtain a crosslinked polymer having a polyethylene oxide skeleton, and this crosslinked polymer and the nonaqueous solvent form a gel-like nonaqueous electrolyte. In this way, the nonaqueous gel electrolyte described in [1] above can be produced without going through a hydrogel, and gelation is also possible in the container of the nonaqueous electrolyte storage element, and the production process is relatively simple. In addition, a nonaqueous solvent mainly composed of at least one component selected from the group consisting of sulfones and carbonates including propylene carbonate is difficult to react with a base catalyst, and the crosslinking reaction of the monomer can proceed in such a nonaqueous solvent and under a base catalyst. In addition, by using at least one component selected from the group consisting of sulfones and carbonates including propylene carbonate as the main component of the non-aqueous solvent, the oxidation resistance is also improved. Furthermore, each component constituting the main component of the non-aqueous solvent has a solubility parameter of 10.0 (cal / cm 3 ) 1 / 2 For these reasons, the nonaqueous gel electrolyte has a high affinity with crosslinked polymers having a polyethylene oxide skeleton. Therefore, the nonaqueous solvent is less likely to seep out over time, and the stability of the gel state is high. For these reasons, the nonaqueous gel electrolyte described in [1] above can be produced by a relatively simple process, and is presumed to have high oxidation resistance and high stability of the gel state.
[0016] The "solubility parameter" (SP value) is a numerical value indicating dissolution behavior, and components having similar solubility parameter values have high solubility (compatibility, affinity). In this specification, the "solubility parameter" is the Hildebrand solubility parameter, which is a value obtained by a calculation procedure described in detail later. The term "main component" refers to a component whose content exceeds 50% by volume on a volume basis. The "main component" may be composed of two or more components. That is, in the nonaqueous gel electrolyte described in [1] above, "a main component selected from the group consisting of sulfones and carbonates including propylene carbonate, and having a solubility parameter of 10.0 (cal / cm 3 ) 1 / 2 It is sufficient that "at least one component having a solubility parameter of 10.0 (cal / cm3 or more)" accounts for more than 50% by volume of the non-aqueous solvent. When the main component is composed of two or more components, the total content of the two or more components is more than 50% by volume, and the solubility parameter of each component is 10.0 (cal / cm3 or more). 3 ) 1 / 2 That's all.
[0017] [Method for measuring the type and content of non-aqueous solvent and base catalyst] The type and content of the non-aqueous solvent and base catalyst are measured by liquid chromatography mass spectrometry (LC-MS) and gas chromatography mass spectrometry (GC-MS). Specifically, the measurement is performed as follows. The LC-MS and GC-MS measurements are performed consecutively under the same conditions. 1. Collection of non-aqueous solvent and base catalyst First, the nonaqueous electrolyte storage element is disassembled to remove the nonaqueous gel electrolyte. The removed nonaqueous gel electrolyte is immersed in a suitable extraction solvent (e.g., acetonitrile, etc.), and the nonaqueous solvent diluted with the extraction solvent and the base catalyst are removed. If the nonaqueous gel electrolyte cannot be removed, a suitable extraction solvent (e.g., acetonitrile, etc.) is poured into the nonaqueous electrolyte storage element, and the nonaqueous solvent diluted with the extraction solvent and the base catalyst are removed. 2.LC-MS The collected non-aqueous solvent and base catalyst components are analyzed by LC-MS. The LC-MS analysis is performed in the following order of qualitative and quantitative analysis. The LC-MS analysis is performed using Waters' "ACQUITY UPLC H-Class" and "Xevo G2-SQTof" instruments. Water is used as the eluent. (qualitative analysis) The measurement sample (non-aqueous solvent and base catalyst) is subjected to LC-MS analysis. If the peaks in the obtained liquid chromatogram cannot be separated, GC-MS analysis, described below, is performed instead of LC-MS analysis. If the peaks can be separated, the components contained in the measurement sample are predicted from the MS spectrum of each peak. A known sample of the predicted components (hereinafter referred to as "predicted components") is subjected to LC-MS analysis. The retention times and MS spectrum of the peaks corresponding to each predicted component in the measurement sample are compared with the retention times and MS spectrum of the peaks of known samples of each predicted component, and if they match, the above prediction is presumed to be correct. (Quantitative analysis) Quantitative analysis is performed using the calibration curve method. First, a known sample of the predicted component with a known concentration is measured by LC-MS, and a calibration curve is created by calculating the peak area. The calibration curve is calculated using the coefficient of determination (r 2 ) is created so that it is between 0.99 and 1. The amount of the predicted component in the measurement sample is calculated from the calibration curve and the area of the peak of the predicted component in the measurement sample. The above process is performed for all peaks detected in the LC-MS analysis of the measurement sample, and the amount of each predicted component is calculated. 3.GC-MS The GC-MS analysis is performed in the following order of qualitative and quantitative analysis. The GC-MS analysis equipment used is the Agilent Technologies "7890A" and "5975C". Helium is used as the carrier gas. (qualitative analysis) The measurement sample (non-aqueous solvent and base catalyst) is subjected to GC-MS analysis. The components contained in the sample are predicted from the MS spectrum of each peak in the obtained gas chromatogram. A known sample of the predicted components is subjected to GC-MS analysis. The retention time and MS spectrum of the peak corresponding to each predicted component in the measurement sample are compared with the retention time and MS spectrum of the peak of a known sample of each predicted component, and if they match, the above prediction is presumed to be correct. (Quantitative analysis) The quantitative analysis is performed by the calibration curve method. The quantitative analysis by GC-MS is performed in the same manner as the quantitative analysis by LC-MS described above, and the content of each predicted component is determined. 4. Calculation of the content of each component For each component of the non-aqueous solvent, the total content of each predicted component (i.e., each component) measured by LC-MS or GC-MS is taken as the content of the non-aqueous solvent, and the content of each component in the non-aqueous solvent is calculated. Note that, when calculating the content (volume %) of each component in the non-aqueous solvent, the mass-based content of each component measured by LC-MS or GC-MS is converted to a volume at 20°C, and the total of the volume-converted contents of each component is taken as the content of the non-aqueous solvent. In addition, the extraction solvent is excluded from consideration.
[0018] [Method for measuring cross-linked polymer structure] The structure of the crosslinked polymer is identified using one or more of known analytical methods such as infrared absorption spectroscopy (IR), Raman spectroscopy, and nuclear magnetic resonance spectroscopy (NMR). Measurements of the crosslinked polymer are performed on samples taken according to the following procedure. First, the nonaqueous electrolyte storage element is disassembled to extract the nonaqueous gel electrolyte. The extracted nonaqueous gel electrolyte is washed, dried, etc. to remove the base catalyst, electrolyte salt, nonaqueous solvent, etc., and the crosslinked polymer is isolated. If the nonaqueous gel electrolyte cannot be extracted, the electrode body taken out by disassembling the nonaqueous electrolyte storage element is washed, dried, etc. to remove the base catalyst, electrolyte salt, nonaqueous solvent, etc., and the crosslinked polymer attached to the outermost part of the electrode body can be subjected to IR and Raman spectroscopy measurements.
[0019] [2] In the nonaqueous gel electrolyte according to the above [1], the crosslinked polymer may have a crosslinked site including a structure represented by the following formula (1): [ka] In the above formula (1), R 1 -S-, -NR 3 -(R 3 is a hydrogen atom or an alkyl group. R is a divalent group represented by -O-. 2 is a divalent electron-withdrawing group. * indicates the bonding site with another group or atom.
[0020] The crosslinking moiety containing the structure represented by the above formula (1) is a typical example of a crosslinking moiety formed by a Michael addition reaction using a base catalyst. Specifically, the crosslinking moiety is a nucleophilic group (formally -R 1- ) is an electron-withdrawing group (R 2 ) to the carbon atom constituting the carbon-carbon double bond that is electron-deficient, thereby forming a crosslinking moiety (-R 1 -CCR 2 -) is formed. That is, the nonaqueous gel electrolyte described in [2] above can be efficiently produced by utilizing the Michael addition reaction. The Michael addition reaction using a base catalyst has a higher reaction rate and is less likely to cause reaction unevenness, compared to, for example, a radical reaction caused by heating. Therefore, the nonaqueous gel electrolyte described in [2] above has a small amount of residual monomers and is highly homogeneous. Therefore, a nonaqueous electrolyte storage element using such a nonaqueous gel electrolyte can exhibit particularly good charge / discharge performance.
[0021] [3] In the nonaqueous gel electrolyte according to the above [1] or [2], the crosslinked polymer may be a crosslinked reaction product between a first compound represented by the following formula (2) and a second compound represented by the following formula (3): [ka] In the above formula (2), R 4 is n2 R is a 4-valent hydrocarbon group. 5 Each X is independently a divalent linking group. Each X is independently -SH, -NHR 8 (R 8 is a hydrogen atom or an alkyl group. 9 (R 9 is a hydrogen atom or a metal atom. 1 are each independently an integer of 0 to 250. 2 is an integer between 2 and 8 inclusive. In the above formula (3), R 6 is n 4 R is a 4-valent hydrocarbon group. 7 Each of Y is independently a divalent linking group. Each of Y is independently a group having a double bond between an electron-withdrawing group and the carbon atoms at the α-position and the β-position to the electron-withdrawing group. 3 are each independently an integer of 0 to 250. 4 is an integer between 2 and 8 inclusive. However, n 1 and n 3 At least one of n is an integer between 25 and 250. 2 and n 4 At least one of the above is an integer between 3 and 8.
[0022] The first compound represented by the above formula (2) and the second compound represented by the above formula (3) are a combination of compounds (monomers) that can be crosslinked into a crosslinked polymer by a Michael addition reaction using a base catalyst. Specifically, the first compound represented by the above formula (2) and the second compound represented by the above formula (3) are a combination of compounds (monomers) that can be crosslinked into a crosslinked polymer by a Michael addition reaction using a base catalyst. -) undergoes nucleophilic addition to the carbon atom constituting the carbon-carbon double bond in the group (Y) that is electron-deficient due to the electron-withdrawing group, thereby forming a crosslinked site. That is, the nonaqueous gel electrolyte described in the above [3] can be efficiently produced by utilizing the Michael addition reaction. Also, as described above, the Michael addition reaction using a base catalyst has a high reaction rate and is less likely to cause reaction unevenness. Therefore, the nonaqueous gel electrolyte described in the above [3] has a small amount of residual monomer and is highly homogeneous. Therefore, a nonaqueous electrolyte storage element using such a nonaqueous gel electrolyte can exhibit particularly good charge / discharge performance.
[0023] [4] A nonaqueous electrolyte storage element according to another aspect of the present invention includes the nonaqueous gel electrolyte according to any one of [1] to [3] above.
[0024] The nonaqueous electrolyte storage element described in [4] above can be produced by a relatively simple process and includes a nonaqueous gel electrolyte having high oxidation resistance and gel state stability. Therefore, the nonaqueous electrolyte storage element described in [4] above itself can be produced by a relatively simple process, and the nonaqueous electrolyte storage element can exhibit good charge / discharge performance.
[0025] [5] A method for producing a nonaqueous electrolyte storage element according to another aspect of the present invention includes crosslinking a first compound with a second compound in a container in the presence of a base catalyst and a nonaqueous solvent, wherein at least one of the first compound and the second compound has a polyethylene oxide skeleton, and the first compound and the second compound have functional groups that crosslink with each other in the presence of the base catalyst, and the nonaqueous solvent is selected from the group consisting of sulfones and carbonates including propylene carbonate, and has a solubility parameter of 10.0 (cal / cm 3 ) 1 / 2 The main component is at least one of the above components.
[0026] According to the method for producing a nonaqueous electrolyte storage element described in [5] above, a nonaqueous gel electrolyte can be produced by a relatively simple process, and the produced nonaqueous gel electrolyte has high oxidation resistance and stability in the gel state. Therefore, according to the method for producing a nonaqueous electrolyte storage element described in [5] above, a nonaqueous electrolyte storage element itself can be produced by a relatively simple process, and the obtained nonaqueous electrolyte storage element can exhibit good charge / discharge performance. In particular, in the method for producing a nonaqueous electrolyte storage element described in [5] above, a nonaqueous gel electrolyte is obtained by performing a crosslinking reaction in a container for the nonaqueous electrolyte storage element, so that there is no need to replace the solvent, and the nonaqueous gel electrolyte can be sufficiently permeated between the electrodes and into the electrodes.
[0027] (Solubility parameter calculation procedure) The procedure for calculating the solubility parameters of the components constituting the non-aqueous solvent is explained below. The solubility parameters are calculated based on the solubility of 1 cm 3 The square root of the heat of vaporization required for the liquid phase component to evaporate ((cal / cm 3 ) 1 / 2 The energies of the target components in the liquid and gas phases are calculated using classical molecular dynamics calculations, and the solubility parameters are calculated using the results.
[0028] The calculation software and the force field used in the calculation are as follows. Note that other calculation software may be used as long as the same results are obtained. Pre-post software: CrossAbility Co., Ltd. Winmostar V11 Calculation software: Gromacs ver.5.0.7 Force field: GAFF2 (General Amber Force Field 2)
[0029] (A) Calculation of the energy of the liquid phase The molecules of the components to be calculated are modeled, and charge is assigned to the molecules using the AM1-BCC method (Acpype). The total charge is set to 0. To construct the liquid phase model, the molecules are randomly placed in the simulation cell. The cell shape is a cube, and the initial density is 0.6 g / cm. 3 The number of molecules (particles) placed in the cell is adjusted so that the number of atoms in the cell is about 2000. Then, the GAFF2 force field is assigned to the liquid phase model.
[0030] Under the following calculation conditions, equilibration calculation 1, equilibration calculation 2, equilibration calculation 3 and this calculation are performed consecutively, inheriting the calculation results of the previous procedure.
[0031] Equilibrium calculation 1 (Minimize) nsteps = 10000 integrator =steep pbc=xyz emtol =100.0 emstep =0.01 constraints =hbonds nstlist =10 ns_type =grid cutoff-scheme=Verlet vdwtype =cut-off coulombtype = PME
[0032] Equilibration calculation 2 (NVT: number of particles N, volume V, temperature T constant) dt =0.001 nsteps = 25000 integrator=md gen-vel =yes tcoupl=berendsen tc-grps=System ref-t =300.0 tau-t = 1.0 pcoupl =no pbc=xyz constraints =hbonds nstlist =10 ns_type =grid cutoff-scheme =Verlet vdwtype =cut-off coulombtype =PME
[0033] Equilibrium calculation 3 (NPT: number of particles N, pressure P, temperature T are constant) dt = 0.001 nsteps = 25000 integrator =md gen-vel =no tcoupl =berendsen tc-grps =System ref-t =300.0 tau-t =1.0 pcoupl =Parrinello-Rahma pcouptype =isotropic ref-p = 1.0 tau-p = 1.0 pbc =xyz constraints =hbonds nstlist =10 ns_type =grid cutoff-scheme =Verlet vdwtype =cut-off coulombtype =PME
[0034] This calculation (NPT: number of particles N, pressure P, temperature T are constant) dt = 0.001 nsteps = 25000 integrator =md gen-vel =no tcoupl =berendsen tc-grps =System ref-t =300.0 tau-t = 1.0 pcoupl = Parrinello-Rahma pcouptype =isotropic ref-p =1.0 tau-p = 1.0 pbc=xyz constraints =hbonds nstlist =10 ns_type =grid cutoff-scheme=Verlet vdwtype =cut-off coulombtype = PME
[0035] (B) Calculation of the energy of the gas phase The molecules of the components to be calculated are modeled, and charge is assigned to the molecules using the AM1-BCC method (Acpype). The total charge is set to 0. To construct the gas-phase model, one molecule is placed in the simulation cell. The cell shape is a cube, and the distance between the molecule and the cell boundary is set to 12 Å. The GAFF2 force field is then assigned to the gas-phase model.
[0036] Under the following calculation conditions, equilibration calculation 1, equilibration calculation 2, and this calculation are performed consecutively, inheriting the calculation results of the previous procedure.
[0037] Equilibration calculation 1 (Minimize) nsteps =5000 integrator =steep pbc=no emtol =100.0 emstep =0.01 constraints =hbonds nstlist =1 ns_type =simple cutoff-scheme =group vdwtype =cut-off coulombtype =cut-off
[0038] Equilibrium calculation 2 (NVT: number of particles N, volume V, temperature T are constant) dt = 0.002 nsteps = 5000 integrator =md gen-vel =yes tcoupl =berendsen tc-grps =System ref-t =300.0 tau-t =1.0 pcoupl =no pbc =xyz constraints =all-bonds nstlist = 1 ns_type =simple cutoff-scheme =group vdwtype =cut-off coulombtype =cut-off
[0039] This calculation (NPT: number of particles N, pressure P, temperature T are constant) dt = 0.002 nsteps = 5000 integrator =md gen-vel =no tcoupl =berendsen tc-grps =System ref-t =300.0 tau-t =1.0 pcoupl =no pbc =xyz constraints =all-bonds nstlist = 1 ns_type =simple cutoff-scheme =group vdwtype =cut-off coulombtype =cut-off
[0040] (C) Calculation of solubility parameter The solubility parameters are calculated using the "χ / DPD parameter" function in the result analysis implemented in Winmostar V11. At this time, the solubility parameters are obtained by inputting (A) the edr file and gro file obtained by the "main calculation" in the calculation of the energy of the liquid phase, and (B) the edr file obtained by the "main calculation" in the calculation of the energy of the gas phase.
[0041] A nonaqueous gel electrolyte according to one embodiment of the present invention, a method for producing a nonaqueous gel electrolyte, a nonaqueous electrolyte storage element, an electricity storage device, a method for producing a nonaqueous electrolyte storage element, and other embodiments will be described in detail. Note that the names of the components (elementary components) used in each embodiment may differ from the names of the components (elementary components) used in the background art.
[0042] <Non-aqueous gel electrolyte> The non-aqueous gel electrolyte according to one embodiment of the present invention contains a crosslinked polymer having a polyethylene oxide skeleton, a base catalyst, and a non-aqueous solvent. The non-aqueous gel electrolyte usually further contains an electrolyte salt. The base catalyst and the electrolyte salt may be dissolved in the non-aqueous solvent.
[0043] (Crosslinked polymer) The cross-linked polymer has a polyethylene oxide backbone ((-CH 2 CH 2 O-) n : n is a natural number.) The crosslinked polymer may be a polymer having a three-dimensional network structure. The crosslinked polymer may be a polymer obtained by a crosslinking reaction of one or more monomers including a monomer having three or more crosslinkable groups (polymerizable groups). In one embodiment of the present invention, the crosslinked polymer is a polymer obtained by a crosslinking reaction in the presence of a base catalyst. The crosslinked polymer is preferably a polymer obtained by a crosslinking reaction by Michael addition reaction in the presence of a base catalyst.
[0044] The crosslinked polymer preferably has a crosslinked site containing a structure represented by the following formula (1).
[0045] [ka]
[0046] In the above formula (1), R 1 -S-, -NR 3 -(R 3 is a hydrogen atom or an alkyl group. R is a divalent group represented by -O-. 2 is a divalent electron-withdrawing group. * indicates the bonding site with another group or atom.
[0047] R 2 The divalent electron-withdrawing group represented by the formula (I) includes a carbonyl group (-C(=O)-), a sulfonyl group (-S(=O) 2 -), etc., and a carbonyl group is preferred. The carbonyl group may be a part of an ester group, an imide group, etc.
[0048] R 3 Examples of the alkyl group represented by R include a methyl group, an ethyl group, an n-propyl group, and an isopropyl group. 3 The number of carbon atoms in the alkyl group represented by the following formula is preferably 1 or more and 6 or less, and more preferably 1 or more and 3 or less.
[0049] In the above formula (1), R 1 and R 2 The two carbon atoms between R and R are preferably bonded to at least two hydrogen atoms in total, and more preferably bonded to at least three hydrogen atoms in total. 1 It is also preferred that the carbon atom on the R 1 The carbon atom on the R 2 It is more preferable that the carbon atom on the R 1Preferably, the carbon atom at the side is further bonded to a carbonyl group. Such a structure is particularly likely to be formed by a Michael addition reaction using a base catalyst.
[0050] [ka]
[0051] As described above, the crosslinking moiety containing the structure represented by (1) above is a typical example of a crosslinking moiety formed by a Michael addition reaction using a base catalyst. For example, in the case of a compound having an amino group and a compound having an acryloyl group, a Michael addition reaction of the following formula (I) occurs. The part surrounded by a chain line in the following formula (I) corresponds to the structure represented by the above formula (1). In the following formula (I), R is any group.
[0052] [ka]
[0053] Furthermore, in the case of a compound having a thiol group and a compound having a maleimide group, a Michael addition reaction of the following formula (II) occurs. The part surrounded by the chain line in the following formula (II) corresponds to the structure represented by the above formula (1). In the following formula (II), R is any group.
[0054] [ka]
[0055] The crosslinked polymer is also preferably a crosslinked reaction product between a first compound represented by the following formula (2) and a second compound represented by the following formula (3).
[0056] [ka]
[0057] In the above formula (2), R 4 is n 2R is a 4-valent hydrocarbon group. 5 Each X is independently a divalent linking group. Each X is independently -SH, -NHR 8 (R 8 is a hydrogen atom or an alkyl group. 9 (R 9 is a hydrogen atom or a metal atom. 1 are each independently an integer of 0 to 250. 2 is an integer between 2 and 8 inclusive. In the above formula (3), R 6 is n 4 R is a 4-valent hydrocarbon group. 7 Each of Y is independently a divalent linking group. Each of Y is independently a group having a double bond between an electron-withdrawing group and the carbon atoms at the α-position and the β-position to the electron-withdrawing group. 3 are each independently an integer of 0 to 250. 4 is an integer between 2 and 8 inclusive. However, n 1 and n 3 At least one of n is an integer between 25 and 250. 2 and n 4 At least one of the above is an integer between 3 and 8.
[0058] As described above, the first compound represented by the formula (2) and the second compound represented by the formula (3) are a combination of compounds (monomers) that can become crosslinked polymers by Michael addition reaction using a base catalyst. The first compound and the second compound may each be used alone or in combination of two or more.
[0059] R 4 n represented by 2 valent hydrocarbon radical and R 6 n represented by 4Examples of the n-valent hydrocarbon group include an aliphatic hydrocarbon group and an aromatic hydrocarbon group, with an aliphatic hydrocarbon group being preferred. Examples of the aliphatic hydrocarbon group include an aliphatic chain hydrocarbon group and an aliphatic cyclic hydrocarbon group, with an aliphatic chain hydrocarbon group being preferred. Examples of the aliphatic hydrocarbon group include an aliphatic saturated hydrocarbon group and an aliphatic unsaturated hydrocarbon group, with an aliphatic saturated hydrocarbon group being preferred, with an aliphatic chain saturated hydrocarbon group being more preferred. That is, 2 Hydrocarbon radicals and n 4 As the n-valent hydrocarbon group, from an alkane, 2 Pieces or n 4 It is preferable that n is a group in which n hydrogen atoms have been removed. 2 Hydrocarbon radicals and n 4 The valent hydrocarbon group is a hydrocarbon group having n atoms bonded to different carbon atoms. 2 Pieces or n 4 It is preferable that n is a group in which n hydrogen atoms have been removed. 2 Hydrocarbon radicals and n 4 The number of carbon atoms in each of the valence hydrocarbon groups is preferably 1 to 20, more preferably 2 to 12, even more preferably 3 to 10, still more preferably 4 to 8, and particularly preferably 5 to 6. For example, R 4 and R 6 The tetravalent hydrocarbon group represented by the formula: C(-CH 2 -) 4 A group represented by the following formula is preferred.
[0060] R 5 and R 7 Examples of the divalent linking group represented by the formula (I) include -COO-, -CONH-, -O-, -CO-, -NH-, -S-, an alkanediyl group having 1 to 6 carbon atoms, and groups consisting of combinations thereof. In -COO-, -CONH-, etc., the orientation is not limited. The divalent linking group may contain a plurality of groups of the same structure (e.g., -COO-). An alkanediyl group having 1 to 6 carbon atoms is -(CH 2 ) m - (where m is an integer from 1 to 6) is preferred. 5 and R 7The number of carbon atoms in the divalent linking group represented by the following formula is preferably 0 or more and 10 or less, more preferably 1 or more and 6 or less, and even more preferably 2 or more and 4 or less.
[0061] R 8 Examples of the alkyl group represented by R include a methyl group, an ethyl group, an n-propyl group, and an isopropyl group. 8 The number of carbon atoms in the alkyl group represented by the following formula is preferably 1 or more and 6 or less, and more preferably 1 or more and 3 or less.
[0062] R 9 Examples of the metal atom represented by the formula (I) include an alkali metal atom such as a sodium atom or a potassium atom.
[0063] The group represented by X is preferably --SH.
[0064] Examples of the electron-withdrawing group contained in the group represented by Y include a carbonyl group, a sulfonyl group, etc., and a carbonyl group is preferred. The carbonyl group may be a part of an ester group, an imide group, etc. A typical example of the group represented by Y includes a group having an enone structure. Examples of the group represented by Y include an acryloyl group, a methacryloyl group, a maleimide group, a vinylsulfone group, etc., and a maleimide group is preferred.
[0065] n 1 is preferably 0. n 2 is preferably 4. n 3 is preferably an integer of 25 or more and 250 or less, and more preferably an integer of 40 or more and 200 or less. n 4 is preferably 4.
[0066] The crosslinked polymer may be used alone or in combination of two or more.
[0067] The lower limit of the content of the crosslinked polymer in the nonaqueous gel electrolyte is preferably 1% by mass, more preferably 2%, 3%, 4% by mass, or 5% by mass. On the other hand, the upper limit of the content of the crosslinked polymer is preferably 20% by mass, more preferably 15%, 10%, 8%, 6% by mass, or 5% by mass. The content of the crosslinked polymer may be equal to or greater than any of the lower limits and equal to or less than any of the upper limits. In the nonaqueous gel electrolyte, a crosslinked polymer having a polyethylene oxide skeleton is used, so that the stability of the gel state is high even if the content of the crosslinked polymer is relatively small. Therefore, by setting the content of the crosslinked polymer in the nonaqueous gel electrolyte to a relatively small range, the amount of the nonaqueous solvent and the electrolyte salt contained in the nonaqueous gel electrolyte can be increased, and the ion conductivity can be increased.
[0068] (Base Catalyst) The base catalyst is a catalytic component for causing a crosslinking reaction of monomers. That is, in the nonaqueous gel electrolyte according to one embodiment of the present invention, the base catalyst used for forming the crosslinked polymer remains.
[0069] The base catalyst is not particularly limited as long as it functions as a catalyst for the crosslinking reaction, and is appropriately selected according to the type of monomer for obtaining a crosslinked polymer. Examples of the base catalyst include amidine compounds such as 1,5-diazabicyclo[4.3.0]-5-nonene and 1,8-diazabicyclo[5.4.0]-7-undecene, guanidine compounds such as 1,3-diphenylguanidine and 1,3-dimethylguanidine, imidazole compounds such as imidazole and 1-ethylimidazole, primary amines such as aniline, secondary amines such as piperidine and cyclohexylamine, tertiary amines such as triethylenediamine, tertiary phosphines such as dimethylphenylphosphine and triphenylphosphine, alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, and alkali metal alkoxy compounds such as sodium methoxide and potassium ethoxide. quaternary ammonium hydroxides such as tetrabutylammonium hydroxide and benzyltrimethylammonium hydroxide; quaternary ammonium carbonates such as tetrabutylammonium alkylcarbonate and benzyltrimethylammonium alkylcarbonate; quaternary ammonium fluorides such as tetrabutylammonium fluoride and benzyltrimethylammonium fluoride; quaternary ammonium tetrahydroborates such as tetrabutylammonium tetrahydroborate and benzyltrimethylammonium tetrahydroborate; and metal amides such as lithium diisopropylamide and potassium hexamethyldisilazide.
[0070] The base catalyst is preferably a nonionic nitrogen-containing compound such as an amidine compound, a guanidine compound, an imidazole compound, or a tertiary amine, and more preferably an imidazole compound. One or more types of base catalysts can be used.
[0071] The content of the base catalyst in the nonaqueous gel electrolyte is preferably 0.005% by mass to 4% by mass, more preferably 0.02% by mass to 1.5% by mass, and even more preferably 0.05% by mass to 0.8% by mass. By having the content of the base catalyst in the above range, a sufficient crosslinking reaction occurs, and the stability of the gel state can be further improved.
[0072] (Non-aqueous solvent) The non-aqueous solvent is selected from the group consisting of sulfones and carbonates including propylene carbonate (PC) and has a solubility parameter of 10.0 (cal / cm 3 ) 1 / 2 The main component is at least one of the above components.
[0073] That is, the main component of the non-aqueous solvent may be one or more sulfones, one or more PCs, one or more PCs, one or more sulfones and PC, or one or more sulfones, PC, and one or more carbonates other than PC. The main component of the non-aqueous solvent is preferably one or more sulfones, one or more PCs, or one or more PCs, or one or more PCs.
[0074] At least one of the components (solvents) constituting the main component of the non-aqueous solvent has a solubility parameter of 10.0 (cal / cm 3 ) 1 / 2 The solubility parameter is 10.4 (cal / cm 3 ) 1 / 2 Above, 11.0(cal / cm 3 ) 1 / 2 or more than 12.0 (cal / cm 3 ) 1 / 2 The solubility parameter may be 16.0 (cal / cm 3 ) 1 / 2 It may be less than or equal to 15.0 (cal / cm 3 ) 1 / 2 Less than or equal to 14.5(cal / cm 3 ) 1 / 2 The solubility parameter of at least one component (solvent) constituting the main component of the non-aqueous solvent may be equal to or higher than any of the above-mentioned lower limits and equal to or lower than any of the above-mentioned upper limits.
[0075] Sulfones are compounds that contain a sulfonyl group (-S(=O) 2 -), and refers to an organic compound having a structure in which the two bonds of the sulfonyl group are each bonded to a carbon atom. The sulfones may be cyclic sulfones having a ring structure in which the two bonds of the sulfonyl group are bonded to one divalent hydrocarbon group. The sulfones may be chain sulfones having a chain structure in which the two bonds of the sulfonyl group are each bonded to different monovalent hydrocarbon groups. One or more hydrogen atoms in the hydrocarbon group of the sulfones may be substituted with other atoms or groups. One or more hydrogen atoms in the hydrocarbon group of the sulfones are preferably not substituted with a fluorine atom or a group containing a fluorine atom, and more preferably not substituted with other atoms or groups.
[0076] Solubility parameter is 10.0 (cal / cm 3 ) 1 / 2 As sulfones with a solubility parameter of 12.0 (cal / cm 3 ) 1 / 2 ), 3-methylsulfolane (MSL: solubility parameter 11.4 (cal / cm 3 ) 1 / 2 ), dimethyl sulfone (DMS: solubility parameter 13.4 (cal / cm 3 ) 1 / 2 ), methyl isopropyl sulfone (MiPS: solubility parameter 11.7 (cal / cm 3 ) 1 / 2 ), ethyl methyl sulfone (EMS: solubility parameter 12.4 (cal / cm 3 ) 1 / 2 ), ethyl isopropyl sulfone (EiPS: solubility parameter 10.7 (cal / cm 3 ) 1 / 2 ), ethyl isobutyl sulfone (EiBS: solubility parameter 11.0 (cal / cm 3 ) 1 / 2 ), Ethyl sec-butyl sulfone (EsBS): solubility parameter 10.6 (cal / cm 3 ) 1 / 2), isopropyl sec-butyl sulfone (iPsBS): solubility parameter 10.2 (cal / cm 3 ) 1 / 2 ), isopropyl isobutyl sulfone (iPiBS: solubility parameter 10.3 (cal / cm 3 ) 1 / 2 ), dipropyl sulfone (DPS: solubility parameter 11.0 (cal / cm 3 ) 1 / 2 ), butyl isobutyl sulfone (BiBS): solubility parameter 10.3 (cal / cm 3 ) 1 / 2 ) and the like, with sulfolane being preferred.
[0077] The carbonates refer to organic compounds having a carbonate group (-OC(=O)-O-) and a structure in which the two bonds of the carbonate group are each bonded to a carbon atom. The carbonates may be cyclic carbonates having a cyclic structure in which the two bonds of the carbonate group are bonded to one divalent hydrocarbon group. The carbonates may be chain carbonates having a chain structure in which the two bonds of the carbonate group are each bonded to a different monovalent hydrocarbon group. One or more hydrogen atoms in the hydrocarbon group of the carbonates may be substituted with other atoms or groups. One or more hydrogen atoms in the hydrocarbon group of the carbonates are preferably not substituted with a fluorine atom or a group containing a fluorine atom, and more preferably not substituted with other atoms or groups other than a hydrocarbon group.
[0078] The solubility parameter of PC is 12.7 (cal / cm 3 ) 1 / 2 The solubility parameter is 10.0 (cal / cm 3 ) 1 / 2 Other carbonates besides PC with a solubility parameter of 14.1 (cal / cm 3 ) 1 / 2 ), 1,2-butylene carbonate (1,2-BC: solubility parameter 11.9 (cal / cm 3 ) 1 / 2), 2,3-butylene carbonate (2,3-BC: solubility parameter 11.9 (cal / cm 3 ) 1 / 2 ), isobutylene carbonate (iBC: solubility parameter 11.6 (cal / cm 3 ) 1 / 2 ), vinylene carbonate (VC: solubility parameter 13.4 (cal / cm 3 ) 1 / 2 ), dimethyl carbonate (DMC: solubility parameter 10.4 (cal / cm 3 ) 1 / 2 ) and the like, with DMC being preferred.
[0079] As the non-aqueous solvent, a cyclic carbonate and a chain carbonate may be used in combination. For example, a cyclic carbonate such as PC may be used in combination with a chain carbonate such as DMC as another carbonate. When a cyclic carbonate and a chain carbonate are used in combination, the volume ratio of the cyclic carbonate to the chain carbonate (cyclic carbonate:chain carbonate) is preferably in the range of 5:95 to 50:50, and more preferably in the range of 20:80 to 40:60.
[0080] The main component of the non-aqueous solvent is preferably composed of only a cyclic solvent, or a combination of a cyclic solvent and a chain solvent. By using a cyclic solvent, the dissociation of the electrolyte salt can be promoted to increase the ionic conductivity of the non-aqueous gel electrolyte. Examples of the cyclic solvent include cyclic sulfones and cyclic carbonates. Examples of the chain solvent include chain sulfones and chain carbonates.
[0081] The content of the main component in the non-aqueous solvent, i.e., "a compound selected from the group consisting of sulfones and carbonates including PC, and having a solubility parameter of 10.0 (cal / cm 3 ) 1 / 2The content of the "component which is at least 60% by volume" is preferably at least 60% by volume, more preferably at least 70% by volume, even more preferably at least 90% by volume, even more preferably at least 95% by volume, and even more preferably at least 99% by volume. The content of the main component in the non-aqueous solvent may be 100% by volume. When the content of the main component in the non-aqueous solvent is within the above range, production can be performed by a relatively simple process, and the effects of high oxidation resistance and high stability of the gel state are particularly enhanced.
[0082] The content of the cyclic solvent in the non-aqueous solvent is preferably 20% by volume or more and 100% by volume or less, more preferably 50% by volume or more and 100% by volume or less, and more preferably 70% by volume or more and 100% by volume or less, 80% by volume or more and 100% by volume or less, 90% by volume or more and 100% by volume or less, or 95% by volume or more and 100% by volume or less. When the content of the cyclic solvent in the non-aqueous solvent is above the lower limit, the oxidation resistance tends to be further improved. As the cyclic solvent, at least one selected from the group consisting of cyclic sulfones and cyclic carbonates is preferred, and at least one selected from the group consisting of sulfolane and propylene carbonate is more preferred.
[0083] The non-aqueous solvent may further contain other components (other solvents) in addition to the above-mentioned main components. Examples of the other solvents include carboxylate esters, phosphate esters, sulfonate esters, ethers, amides, nitriles, and solvents having a solubility parameter of 10.0 (cal / cm 3 ) 1 / 2 Sulfones with a solubility parameter of less than 10.0 (cal / cm 3 ) 1 / 2 Examples of suitable carbonates include carbonates having a molecular weight of less than 1000.
[0084] In the non-aqueous solvent, the content of the fluorinated cyclic carbonate is preferably 30% by volume or less, more preferably 10% by volume or less, even more preferably 1% by volume or less, and even more preferably 0% by volume. When the content of the fluorinated cyclic carbonate in the non-aqueous solvent is equal to or less than the upper limit, gelation occurs particularly well together with the formation of a crosslinkable polymer. The fluorinated cyclic carbonate refers to a compound in which one or more hydrogen atoms in a hydrocarbon group of a cyclic carbonate are substituted with a fluorine atom or a group containing a fluorine atom.
[0085] The content of the nonaqueous solvent in the nonaqueous gel electrolyte is preferably 60% by mass to 99% by mass, more preferably 70% by mass to 97% by mass, and even more preferably 80% by mass to 95% by mass. By having the content of the nonaqueous solvent in the nonaqueous gel electrolyte within the above range, it is possible to achieve both ion conductivity and stability of the gel state.
[0086] (Electrolyte salt) The electrolyte salt can be appropriately selected from known electrolyte salts. Examples of the electrolyte salt include lithium salts, sodium salts, potassium salts, magnesium salts, onium salts, etc. Among these, lithium salts are preferred.
[0087] The lithium salt is LiPF 6 , LiPO 2 F 2 , LiBF 4 , LiClO 4 , LiN(SO 2 F) 2 inorganic lithium salts such as lithium oxalate (LiBOB), lithium difluorooxalate (LiFOB), lithium bis(oxalate) difluorophosphate (LiFOP), and other lithium oxalates; LiSO 3 CF 3 , LiN(SO 2 CF 3 ) 2 , LiN(SO 2 C 2 F 5 )2 , LiN(SO 2 CF 3 )(SO 2 C 4 F 9 ), LiC(SO 2 CF 3 ) 3 , LiC(SO 2 C 2 F 5 ) 3 Among these, inorganic lithium salts are preferred, and LiPF 6 is more preferred.
[0088] The content of the electrolyte salt in the nonaqueous gel electrolyte is 0.1 mol / dm at 20°C and 1 atmosphere. 3 More than 2.5mol / dm 3 It is preferable that the value is 0.3 mol / dm or less. 3 More than 2.0mol / dm 3 More preferably, it is 0.5 mol / dm or less. 3 More than 1.7mol / dm 3 More preferably, it is 0.7 mol / dm or less. 3 More than 1.5mol / dm 3 By setting the content of the electrolyte salt within the above range, the ionic conductivity of the nonaqueous gel electrolyte can be increased.
[0089] The non-aqueous gel electrolyte may contain additives in addition to the crosslinked polymer, base catalyst, non-aqueous solvent, and electrolyte salt. Examples of additives include oxalates such as lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP); imide salts such as lithium bis(fluorosulfonyl)imide (LiFSI); aromatic compounds such as biphenyl, alkylbiphenyl, terphenyl, partially hydrogenated terphenyl, cyclohexylbenzene, t-butylbenzene, t-amylbenzene, diphenyl ether, and dibenzofuran; partial halides of the aromatic compounds such as 2-fluorobiphenyl, o-cyclohexylfluorobenzene, and p-cyclohexylfluorobenzene; halogenated anisole compounds such as 2,4-difluoroanisole, 2,5-difluoroanisole, 2,6-difluoroanisole, and 3,5-difluoroanisole; methylvinylene carbonate, ethylvinylene carbonate, succinic anhydride, glutaric anhydride, Maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, cyclohexanedicarboxylic anhydride; ethylene sulfite, propylene sulfite, dimethyl sulfite, methyl methanesulfonate, busulfan, methyl toluenesulfonate, dimethyl sulfate, ethylene sulfate, dimethyl sulfoxide, diethyl sulfoxide, tetramethylene sulfoxide, diphenyl sulfide, 4,4'-bis(2,2-dioxo-1,3,2-dioxathiolane), 4-methyl sulfonate Examples of the additives include nyloxymethyl-2,2-dioxo-1,3,2-dioxathiolane, thioanisole, diphenyl disulfide, dipyridinium disulfide, 1,3-propene sultone, 1,3-propane sultone, 1,4-butane sultone, 1,4-butene sultone, perfluorooctane, tristrimethylsilyl borate, tristrimethylsilyl phosphate, tetrakistrimethylsilyl titanate, lithium monofluorophosphate, lithium difluorophosphate, etc. These additives may be used alone or in combination of two or more.
[0090] The content of the additive contained in the nonaqueous gel electrolyte is preferably 0.01% by mass to 10% by mass, more preferably 0.1% by mass to 7% by mass, even more preferably 0.2% by mass to 5% by mass, and particularly preferably 0.3% by mass to 3% by mass. By setting the content of the additive within the above range, it is possible to improve the capacity retention performance or cycle performance after high-temperature storage, and to further improve safety.
[0091] The nonaqueous gel electrolyte can be suitably used as an electrolyte for nonaqueous electrolyte storage elements such as lithium ion secondary batteries.
[0092] <Method of manufacturing nonaqueous gel electrolyte> The method for producing the nonaqueous gel electrolyte according to one embodiment of the present invention is not particularly limited, and can be carried out, for example, by crosslinking one or more compounds (monomers) that undergo crosslinking reaction in a nonaqueous solvent in the presence of a base catalyst. At this time, an electrolyte salt or the like may be further dissolved in the nonaqueous solvent. In addition, the one or more compounds that undergo crosslinking reaction may be a combination of the first compound and the second compound described above. In addition, the method for producing a nonaqueous electrolyte storage element described later includes a method for producing a nonaqueous gel electrolyte.
[0093] <Non-aqueous electrolyte electricity storage element> A nonaqueous electrolyte storage element (hereinafter, also simply referred to as "storage element") according to one embodiment of the present invention includes an electrode assembly having a positive electrode, a negative electrode, and a separator, a nonaqueous gel electrolyte, and a container that contains the electrode assembly and the nonaqueous gel electrolyte. The electrode assembly is usually a laminated type in which a plurality of positive electrodes and a plurality of negative electrodes are laminated with a separator interposed therebetween, or a wound type in which a positive electrode and a negative electrode are laminated with a separator interposed therebetween and wound. The nonaqueous gel electrolyte is usually present in a state in which it is impregnated in the positive electrode, the negative electrode, and the separator. As an example of a nonaqueous electrolyte storage element, a nonaqueous electrolyte secondary battery (hereinafter, also simply referred to as "secondary battery") will be described.
[0094] (positive electrode) The positive electrode has a positive electrode substrate and a positive electrode active material layer disposed on the positive electrode substrate directly or via an intermediate layer.
[0095] The positive electrode substrate is conductive. Whether or not it has "conductivity" is determined by whether the volume resistivity measured in accordance with JIS-H-0505 (1975) is 10 -2 The threshold value is Ω·cm. The material of the positive electrode substrate is a metal such as aluminum, titanium, tantalum, stainless steel, or an alloy thereof. Among these, aluminum or an aluminum alloy is preferred from the viewpoints of potential resistance, high conductivity, and cost. The positive electrode substrate may be a foil, a vapor deposition film, a mesh, a porous material, etc., and a foil is preferred from the viewpoint of cost. Therefore, aluminum foil or an aluminum alloy foil is preferred as the positive electrode substrate. Examples of aluminum or an aluminum alloy include A1085, A3003, A1N30, etc., as specified in JIS-H-4000 (2014) or JIS-H-4160 (2006).
[0096] The average thickness of the positive electrode substrate is preferably 3 μm to 50 μm, more preferably 5 μm to 40 μm, further preferably 8 μm to 30 μm, and particularly preferably 10 μm to 25 μm. By setting the average thickness of the positive electrode substrate within the above range, it is possible to increase the strength of the positive electrode substrate and to increase the energy density per volume of the nonaqueous electrolyte storage element.
[0097] The intermediate layer is a layer disposed between the positive electrode substrate and the positive electrode active material layer. The intermediate layer contains a conductive agent such as carbon particles to reduce the contact resistance between the positive electrode substrate and the positive electrode active material layer. The configuration of the intermediate layer is not particularly limited, and may contain, for example, a binder and a conductive agent.
[0098] The positive electrode active material layer contains a positive electrode active material and, as necessary, optional components such as a conductive agent, a binder, a thickener, and a filler.
[0099] The positive electrode active material can be appropriately selected from known positive electrode active materials. As the positive electrode active material for a lithium ion secondary battery, a material capable of absorbing and releasing lithium ions is usually used. As the positive electrode active material, for example, α-NaFeO 2 Lithium transition metal composite oxides having a crystalline structure, lithium transition metal composite oxides having a spinel crystalline structure, polyanion compounds, chalcogen compounds, sulfur, etc. 2 As an example of a lithium transition metal composite oxide having a crystalline structure, Li[Li x Ni (1-x) ]O 2 (0≦x<0.5), Li[Li x Ni γ Co (1-x-γ) ]O 2 (0≦x<0.5, 0<γ<1, 0<1-x-γ), Li[Li x Co (1-x) ]O 2 (0≦x<0.5), Li[Li x Ni γ Mn (1-x-γ) ]O 2 (0≦x<0.5, 0<γ<1, 0<1-x-γ), Li[Li x Ni γ Mn β Co (1-x-γ-β) ]O 2 (0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1, 0<1-x-γ-β), Li[Li x Ni γ Co β Al (1-x-γ-β) ]O 2 (0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1, 0<1-x-γ-β). Lithium transition metal composite oxides with spinel crystal structure include Li x Mn 2 O 4 , Li x Ni γ Mn (2-γ) O 4 Examples of polyanion compounds include LiFePO 4 , LiMnPO 4 , LiNiPO 4 , LiCoPO4 , Li 3 V 2 (PO 4 ) 3 , Li 2 MnSiO 4 , Li 2 CoPO 4 Examples of the chalcogen compound include titanium disulfide, molybdenum disulfide, and molybdenum dioxide. The atoms or polyanions in these materials may be partially substituted with atoms or anion species of other elements. The surfaces of these materials may be coated with other materials. In the positive electrode active material layer, one of these materials may be used alone, or two or more of them may be used in combination.
[0100] The positive electrode active material is α-NaFeO 2 Lithium transition metal composite oxides having a crystalline structure or a spinel crystalline structure, and polyanion compounds containing nickel, cobalt or manganese (LiMnPO 4 , LiNiPO 4 , LiCoPO 4 , Li 2 MnSiO 4 , Li 2 CoPO 4 F, etc.) is preferred, and α-NaFeO 2 Lithium transition metal composite oxides having a type crystal structure are more preferred. 2 Among the lithium transition metal composite oxides having a crystalline structure, those containing one or more of nickel, cobalt and manganese as the transition metal element are more preferred, and those containing cobalt are even more preferred. These positive electrode active materials have particularly high redox potentials, and the use of such positive electrode active materials can increase the energy density of the nonaqueous electrolyte storage element. On the other hand, the nonaqueous electrolyte storage element according to one embodiment of the present invention uses the nonaqueous gel electrolyte having high oxidation resistance according to one embodiment of the present invention, so that good charge / discharge performance can be maintained even when these positive electrode active materials having high redox potentials are used.
[0101] The positive electrode active material is usually a particle (powder). The average particle size of the positive electrode active material is preferably, for example, 0.1 μm or more and 20 μm or less. By setting the average particle size of the positive electrode active material to the above lower limit or more, the positive electrode active material can be easily manufactured or handled. By setting the average particle size of the positive electrode active material to the above upper limit or less, the electronic conductivity of the positive electrode active material layer is improved. In addition, when a composite of the positive electrode active material and another material is used, the average particle size of the composite is taken as the average particle size of the positive electrode active material. The "average particle size" means a value at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50% based on the particle size distribution measured by a laser diffraction / scattering method for a diluted solution obtained by diluting particles with a solvent in accordance with JIS-Z-8825 (2013).
[0102] In order to obtain powder with a predetermined particle size, a pulverizer, a classifier, etc. are used. Examples of the pulverization method include a method using a mortar, a ball mill, a sand mill, a vibration ball mill, a planetary ball mill, a jet mill, a counter jet mill, a swirling airflow type jet mill, or a sieve. During pulverization, wet pulverization in the presence of water or an organic solvent such as hexane can also be used. As a classification method, a sieve, an air classifier, etc. are used as necessary for both dry and wet methods.
[0103] The content of the positive electrode active material in the positive electrode active material layer is preferably 50% by mass to 99% by mass, more preferably 70% by mass to 98% by mass, and even more preferably 80% by mass to 95% by mass. By setting the content of the positive electrode active material in the above range, both high energy density and manufacturability of the positive electrode active material layer can be achieved.
[0104] The conductive agent is not particularly limited as long as it is a material having electrical conductivity. Examples of such conductive agents include carbonaceous materials, metals, conductive ceramics, and the like. Examples of carbonaceous materials include graphite, non-graphitic carbon, graphene-based carbon, and the like. Examples of non-graphitic carbon include carbon nanofibers, pitch-based carbon fibers, carbon black, and the like. Examples of carbon black include furnace black, acetylene black, ketjen black, and the like. Examples of graphene-based carbon include graphene, carbon nanotubes (CNT), fullerene, and the like. Examples of the conductive agent include powder and fiber. As the conductive agent, one of these materials may be used alone, or two or more of them may be mixed and used. These materials may also be used in combination. For example, a material in which carbon black and CNT are combined may be used. Among these, carbon black is preferable from the viewpoint of electronic conductivity and coatability, and acetylene black is preferable among them.
[0105] The content of the conductive agent in the positive electrode active material layer is preferably from 1 mass % to 10 mass %, more preferably from 3 mass % to 9 mass %. By setting the content of the conductive agent in the above range, the energy density of the nonaqueous electrolyte storage element can be increased.
[0106] Examples of binders include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic, polyimide, etc.; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, etc.; polysaccharide polymers, etc.
[0107] The content of the binder in the positive electrode active material layer is preferably from 1% by mass to 10% by mass, and more preferably from 3% by mass to 9% by mass. By setting the content of the binder in the above range, the positive electrode active material can be stably maintained.
[0108] Examples of the thickener include polysaccharide polymers such as carboxymethyl cellulose (CMC), methyl cellulose, etc. When the thickener has a functional group that reacts with lithium or the like, this functional group may be deactivated in advance by methylation or the like.
[0109] The filler is not particularly limited. Examples of the filler include polyolefins such as polypropylene and polyethylene, inorganic oxides such as silicon dioxide, alumina, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicates, hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, carbonates such as calcium carbonate, poorly soluble ion crystals such as calcium fluoride, barium fluoride, and barium sulfate, nitrides such as aluminum nitride and silicon nitride, and mineral resource-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, or artificial products thereof.
[0110] The positive electrode active material layer may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than the positive electrode active material, conductive agent, binder, thickener, and filler.
[0111] The positive electrode active material layer may be porous. The porosity of the positive electrode active material layer is preferably 10% or more and 50% or less, more preferably 20% or more and 40% or less. When the porosity of the positive electrode active material layer is within the above range, the charge / discharge performance can be further improved. The porous positive electrode active material layer may be impregnated with the nonaqueous gel electrolyte according to one embodiment of the present invention.
[0112] The porosity of the positive electrode active material layer refers to a value calculated by the following formula from the true density of the positive electrode active material layer calculated from the true density of each component constituting the positive electrode active material layer and the apparent density of the positive electrode active material layer. Porosity (%) = 100 - (apparent density / true density) x 100
[0113] The apparent density of the positive electrode active material layer is the value obtained by dividing the mass of the positive electrode active material layer by the apparent volume of the positive electrode active material layer. The apparent volume refers to the volume including the void portion, and can be calculated as the product of the average thickness and the area of the positive electrode active material layer. The average thickness of the positive electrode active material layer is the average value of the thicknesses measured at any five positions. The porosity of the negative electrode active material layer described later is also a value calculated by the same method.
[0114] (Negative electrode) The negative electrode has a negative electrode substrate and a negative electrode active material layer disposed on the negative electrode substrate directly or via an intermediate layer. The configuration of the intermediate layer is not particularly limited and can be selected from the configurations exemplified for the positive electrode.
[0115] The negative electrode substrate has electrical conductivity. Metals such as copper, nickel, stainless steel, nickel-plated steel, and aluminum, or alloys thereof, carbonaceous materials, etc. are used as the material of the negative electrode substrate. Among these, copper or copper alloys are preferred. Aluminum or aluminum alloys may also be preferred. Examples of the negative electrode substrate include foils, vapor deposition films, meshes, and porous materials, and foils are preferred from the viewpoint of cost. Therefore, copper foil or copper alloy foil is preferred as the negative electrode substrate. Examples of copper foil include rolled copper foil and electrolytic copper foil. Aluminum foil or aluminum alloy foil may also be preferred as the negative electrode substrate.
[0116] The average thickness of the negative electrode substrate is preferably 2 μm to 35 μm, more preferably 3 μm to 30 μm, further preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm. By setting the average thickness of the negative electrode substrate within the above range, it is possible to increase the strength of the negative electrode substrate and to increase the energy density per volume of the nonaqueous electrolyte storage element.
[0117] The negative electrode active material layer contains a negative electrode active material. The negative electrode active material layer contains optional components such as a conductive agent, a binder, a thickener, a filler, etc., as necessary. The optional components such as a conductive agent, a binder, a thickener, a filler, etc. can be selected from the materials exemplified for the positive electrode above.
[0118] The negative electrode active material layer may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, and W as components other than the negative electrode active material, conductive agent, binder, thickener, and filler.
[0119] The negative electrode active material can be appropriately selected from known negative electrode active materials. A material capable of absorbing and releasing lithium ions is usually used as the negative electrode active material for lithium ion secondary batteries. Examples of the negative electrode active material include metal Li; metals or semimetals such as Si and Sn; metal oxides or semimetal oxides such as Si oxide, Ti oxide, and Sn oxide; Li 4 Ti 5 O 12 , LiTiO 2、 TiNb 2 O 7 Examples of the material include titanium-containing oxides such as titanium oxide, polyphosphate compounds, silicon carbide, and carbon materials such as graphite and non-graphitic carbon (easily graphitized carbon or non-graphitizable carbon). Among these materials, graphite and non-graphitic carbon are preferred. Titanium-containing oxides are also preferred. In the negative electrode active material layer, one of these materials may be used alone, or two or more of them may be used in combination.
[0120] "Graphite" refers to graphite that has an average lattice spacing (d 002 ) is 0.33 nm or more and less than 0.34 nm. Examples of graphite include natural graphite and artificial graphite. Artificial graphite is preferred from the viewpoint of availability of materials with stable physical properties.
[0121] "Non-graphitic carbon" refers to carbon that has an average lattice spacing (d 002 ) is 0.34 nm or more and 0.42 nm or less. Examples of non-graphitizable carbon include non-graphitizable carbon and graphitizable carbon. Examples of non-graphitizable carbon include resin-derived materials, petroleum pitch or petroleum pitch-derived materials, petroleum coke or petroleum coke-derived materials, plant-derived materials, and alcohol-derived materials.
[0122] Here, the "discharged state" refers to a state in which the negative electrode active material carbon material is discharged so that lithium ions that can be absorbed and released during charging and discharging are sufficiently released. For example, in a half cell using a negative electrode containing a carbon material as a negative electrode active material as a working electrode and metallic Li as a counter electrode, the open circuit voltage is 0.7 V or more.
[0123] "Non-graphitizable carbon" means the above d 002 This refers to carbon materials with a particle size of 0.36 nm or more and 0.42 nm or less.
[0124] "Graphitizable carbon" means the above d 002 This refers to carbon materials with a particle size of 0.34 nm or more and less than 0.36 nm.
[0125] The negative electrode active material is usually a particle (powder). The average particle size of the negative electrode active material can be, for example, 1 nm or more and 100 μm or less. When the negative electrode active material is a carbon material, a titanium-containing oxide, or a polyphosphate compound, the average particle size may be 1 μm or more and 100 μm or less. When the negative electrode active material is Si, Sn, Si oxide, Sn oxide, or the like, the average particle size may be 1 nm or more and 1 μm or less. By setting the average particle size of the negative electrode active material to the above lower limit or more, the negative electrode active material can be easily manufactured or handled. By setting the average particle size of the negative electrode active material to the above upper limit or less, the electronic conductivity of the negative electrode active material layer is improved. In order to obtain powder with a predetermined particle size, a pulverizer, a classifier, or the like is used. The pulverizing method and the classifying method can be selected from, for example, the methods exemplified for the positive electrode. When the negative electrode active material is a metal such as metallic Li, the negative electrode active material layer may be in the form of a foil.
[0126] The content of the negative electrode active material in the negative electrode active material layer is preferably 60% by mass to 99% by mass, more preferably 90% by mass to 98% by mass. By setting the content of the negative electrode active material in the above range, both high energy density and manufacturability of the negative electrode active material layer can be achieved.
[0127] The negative electrode active material layer may be porous. The porosity of the negative electrode active material layer is preferably 20% or more and 60% or less, more preferably 30% or more and 50% or less. When the porosity of the negative electrode active material layer is within the above range, the charge / discharge performance can be further improved. The porous negative electrode active material layer may be impregnated with the nonaqueous gel electrolyte according to one embodiment of the present invention.
[0128] (Separator) The separator can be appropriately selected from known separators. For example, a separator consisting of only a substrate layer, a separator in which a heat-resistant layer containing heat-resistant particles and a binder is formed on one or both sides of the substrate layer, etc. can be used as the separator. Examples of the shape of the substrate layer of the separator include woven fabric, nonwoven fabric, and porous resin film. Among these shapes, a porous resin film is preferred from the viewpoint of strength, and a nonwoven fabric is preferred from the viewpoint of retention of the nonaqueous gel electrolyte. As the material of the substrate layer of the separator, polyolefins such as polyethylene and polypropylene are preferred from the viewpoint of shutdown function, and polyimide and aramid are preferred from the viewpoint of oxidation decomposition resistance. A material in which these resins are combined may be used as the substrate layer of the separator.
[0129] The heat-resistant particles contained in the heat-resistant layer preferably have a mass loss of 5% or less when heated from room temperature to 500°C under an air atmosphere at 1 atmosphere, and more preferably have a mass loss of 5% or less when heated from room temperature to 800°C. Examples of materials with a mass loss of a predetermined amount or less include inorganic compounds. Examples of inorganic compounds include oxides such as iron oxide, silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicate; nitrides such as aluminum nitride and silicon nitride; carbonates such as calcium carbonate; sulfates such as barium sulfate; sparingly soluble ion crystals such as calcium fluoride, barium fluoride, and barium titanate; covalent crystals such as silicon and diamond; mineral resource-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, or artificial products thereof. As the inorganic compound, these substances may be used alone or in the form of a complex, or two or more of them may be mixed and used. Among these inorganic compounds, silicon oxide, aluminum oxide, or aluminosilicate is preferred from the viewpoint of the safety of the nonaqueous electrolyte storage element.
[0130] The porosity of the separator is preferably 80% by volume or less from the viewpoint of strength, and is preferably 20% by volume or more from the viewpoint of discharge performance. Here, "porosity" refers to a volume-based value measured with a mercury porosimeter.
[0131] The separator may be a nonaqueous gel electrolyte according to one embodiment of the present invention. When the separator is a porous resin film or nonwoven fabric as described above, the pores may be impregnated with the nonaqueous gel electrolyte.
[0132] (Non-aqueous gel electrolyte) The nonaqueous gel electrolyte used in the nonaqueous electrolyte storage element is the nonaqueous gel electrolyte according to one embodiment of the present invention described above. As the nonaqueous gel electrolyte, the nonaqueous gel electrolyte according to one embodiment of the present invention may be used in combination with another nonaqueous gel electrolyte.
[0133] (shape, etc.) The shape of the nonaqueous electrolyte storage element of this embodiment is not particularly limited, and examples thereof include a cylindrical battery, a prismatic battery, a flat battery, a coin battery, and a button battery.
[0134] Fig. 1 shows a nonaqueous electrolyte storage element 1 as an example of a prismatic battery. The figure is a see-through view of the inside of the container. An electrode body 2 having a positive electrode and a negative electrode wound with a separator sandwiched therebetween is housed in a prismatic container 3. The positive electrode is electrically connected to a positive electrode terminal 4 via a positive electrode lead 41. The negative electrode is electrically connected to a negative electrode terminal 5 via a negative electrode lead 51.
[0135] In the non-aqueous electrolyte storage element, the positive electrode potential at the end of charge voltage during normal use is 4.0 V vs. Li / Li + It is preferable that the value is 4.2V vs. Li / Li or more. + More preferably, it is 4.4V vs. Li / Li + More preferably, it is equal to or higher. When the positive electrode potential at the end-of-charge voltage during normal use is equal to or higher than the lower limit, the energy density of the nonaqueous electrolyte storage element can be increased. On the other hand, since the nonaqueous electrolyte storage element includes a nonaqueous gel electrolyte having excellent oxidation resistance, good charge / discharge performance can be maintained even when the positive electrode potential reaches a high potential. "Normal use" refers to a case where the nonaqueous electrolyte storage element is used by adopting charge and discharge conditions recommended or specified for the nonaqueous electrolyte storage element. Regarding the charge conditions, for example, when a charger for the nonaqueous electrolyte storage element is prepared, the charger is used to use the nonaqueous electrolyte storage element. The positive electrode potential at the end-of-charge voltage during normal use of the nonaqueous electrolyte storage element is, for example, 5.0 V vs. Li / Li + It may be less than 4.8V vs.Li / Li + It may be less than 4.7V vs.Li / Li + The positive electrode potential may be equal to or higher than any of the above-mentioned lower limits and equal to or lower than any of the above-mentioned upper limits.
[0136] <Electricity storage device> The nonaqueous electrolyte storage element of the present embodiment can be mounted as an electricity storage unit (battery module) comprising a plurality of nonaqueous electrolyte storage elements assembled together in automobile power sources such as electric vehicles (EVs), hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), etc., power sources for electronic devices such as personal computers and communication terminals, or power storage power sources, etc. In this case, the technology of the present invention may be applied to at least one of the nonaqueous electrolyte storage elements included in the electricity storage unit.
[0137] 2 shows an example of an electricity storage device 30 in which electricity storage units 20, each of which is an assembly of two or more electrically connected nonaqueous electrolyte electricity storage elements 1, are further assembled. The electricity storage device 30 may include a bus bar (not shown) that electrically connects two or more nonaqueous electrolyte electricity storage elements 1, a bus bar (not shown) that electrically connects two or more electricity storage units 20, and the like. The electricity storage unit 20 or the electricity storage device 30 may include a status monitoring device (not shown) that monitors the status of one or more nonaqueous electrolyte electricity storage elements.
[0138] <Method of Manufacturing Nonaqueous Electrolyte Storage Element> Although the method for producing a nonaqueous electrolyte storage element according to one embodiment of the present invention is not particularly limited, the following method is preferable. That is, the method for producing a nonaqueous electrolyte storage element according to one embodiment of the present invention comprises crosslinking a first compound with a second compound in a container in the presence of a base catalyst and a nonaqueous solvent, at least one of the first compound and the second compound has a polyethylene oxide skeleton, the first compound and the second compound have functional groups that crosslink with each other in the presence of the base catalyst, the nonaqueous solvent is selected from the group consisting of sulfones and carbonates including propylene carbonate, and the solubility parameter is 10.0 (cal / cm 3 ) 1 / 2 The main component is at least one of the above components.
[0139] Specific and preferred forms of the first compound and the second compound used in the manufacturing method of the nonaqueous electrolyte storage element include the first compound represented by the above formula (2) and the second compound represented by the above formula (3). That is, examples of the functional groups that undergo a crosslinking reaction in the presence of the base catalyst include the group represented by X in the above formula (2) and the group represented by Y in the above formula (3). Specific and preferred forms of the base catalyst and the nonaqueous solvent used in the manufacturing method are the same as the examples of the base catalyst and the nonaqueous solvent contained in the nonaqueous gel electrolyte according to one embodiment of the present invention.
[0140] The crosslinking reaction in the manufacturing method can be carried out by pouring a precursor solution of a nonaqueous gel electrolyte, which is prepared by dissolving the first compound, the second compound and a base catalyst in a nonaqueous solvent, into a container and leaving it to stand. This precursor solution may further contain other components contained in the nonaqueous gel electrolyte, such as an electrolyte salt. In addition, in the case of a Michael addition reaction, the crosslinking reaction proceeds sufficiently at room temperature. The crosslinking reaction may be carried out by leaving it to stand while heating or the like.
[0141] The method for producing a nonaqueous electrolyte storage element may further include, prior to the crosslinking reaction, preparing an electrode body, housing the electrode body in a container, preparing a precursor solution, and housing the precursor solution in the container.
[0142] <Other embodiments> The nonaqueous gel electrolyte, the nonaqueous electrolyte storage element, and the method for manufacturing the nonaqueous electrolyte storage element of the present invention are not limited to the above-mentioned embodiments, and various modifications may be made without departing from the scope of the present invention. For example, the configuration of one embodiment may be added to the configuration of another embodiment, and part of the configuration of one embodiment may be replaced with the configuration of another embodiment or a well-known technique. Furthermore, part of the configuration of one embodiment may be deleted. Also, a well-known technique may be added to the configuration of one embodiment.
[0143] In the above embodiment, the nonaqueous electrolyte storage element is used as a chargeable and dischargeable nonaqueous electrolyte secondary battery (e.g., a lithium ion secondary battery), but the type, shape, size, capacity, etc. of the nonaqueous electrolyte storage element are arbitrary. The present invention can also be applied to various secondary batteries, electric double layer capacitors, lithium ion capacitors, and other capacitors.
[0144] In the above embodiment, the electrode assembly in which the positive electrode and the negative electrode are stacked with a separator interposed therebetween has been described, but the electrode assembly may not include a separator. For example, the positive electrode and the negative electrode may be in direct contact with each other in a state in which a non-conductive layer is formed on the active material layer of the positive electrode or the negative electrode.
[0145] In the above embodiment, the crosslinked polymer is mainly obtained by the Michael addition reaction, but the crosslinked polymer may be obtained by other crosslinking reactions. Similarly, in the method for producing a nonaqueous electrolyte storage element of the present invention, a crosslinking reaction other than the Michael addition reaction may be used as long as it is a crosslinking reaction caused by a base catalyst.
[0146] <Example> The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. The main compounds used in the Examples, Comparative Examples and Reference Examples are shown below.
[0147] Monomer A Pentaerythritol tetra(3-mercaptopropionate) represented by the following formula (R 4 is C(-CH 2 -) 4 , R 5 -C(=O)-CH 2 -CH 2 -, X is -SH, n 1 The first compound represented by 0: manufactured by Tokyo Chemical Industry Co., Ltd.
[0148] [ka]
[0149] Monomer B A 4-branched polyethylene glycol having a maleimide group at the end, represented by the following formula (R 6 is C(-CH 2 -) 4 , R 7 Ga-CH 2 -NH-C(=O)-CH 2 -CH 2 -, and the second compound having a number average molecular weight of 20,000, in which Y is a maleimide group: manufactured by Aldrich
[0150] [ka]
[0151] Base catalyst 1-Ethylimidazole represented by the following formula
[0152] [ka]
[0153] ETPTA (monomer used in Reference Example 1) Trimethylolpropane EO adduct triacrylate represented by the following formula
[0154] [ka]
[0155] Non-aqueous solvents Hereinafter, the solubility parameter is also referred to as the SP value. The SP value of each non-aqueous solvent below is a value calculated by the above-mentioned calculation procedure. The unit of the SP value (cal / cm 3 ) 1 / 2 ) is omitted. Sulfolane (SL:SP value 12.0) Propylene carbonate (PC: SP value 12.7) Dimethyl carbonate (DMC: SP value 10.4) Diethyl carbonate (DEC: SP value 9.6) 2,2,2-Trifluoroethyl methyl carbonate (TFEMC: SP value 9.8) Ethylene carbonate (EC:SP value 14.1) Fluoroethylene carbonate (FEC)
[0156] [Example 1] (1) Preparation of non-aqueous gel electrolyte In the non-aqueous solvent sulfolane (SL), 1.0 mol / dm 3 LiPF at a concentration of 6 A non-aqueous electrolyte solution was obtained by dissolving monomer A and a base catalyst in the non-aqueous electrolyte solution. Separately, monomer B was dissolved in the non-aqueous electrolyte solution to obtain solution B. Note that solutions A and B were prepared so that the content of the crosslinked polymer, which is the reaction product of monomer A and monomer B, in the non-aqueous gel electrolyte obtained by mixing and reacting solution A and solution B was 5 mass % and the content of the base catalyst was 0.38 mass %. The above-mentioned solutions A and B were mixed to prepare a precursor solution of the nonaqueous gel electrolyte, and the precursor solution was allowed to stand at a temperature of 25° C. for 24 hours. As a result, the nonaqueous gel electrolyte of Example 1 containing a crosslinked polymer was obtained. All of the above operations were carried out under an argon atmosphere.
[0157] (2) Fabrication of non-aqueous electrolyte storage element (Preparation of positive electrode) Positive electrode active material LiCoO 2 The positive electrode mixture paste was prepared by mixing the positive electrode active material, acetylene black (AB) as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and a dispersion medium. The mass ratio of the positive electrode active material, AB, and PVDF was 90:5:5 (solid content conversion). The positive electrode mixture paste was applied to the surface of aluminum foil (average thickness 15 μm) as the positive electrode substrate with a mass of 7.6 mg / cm. 2 (based on solid content) was applied. Thereafter, drying and roll pressing were performed to obtain a positive electrode in which a positive electrode active material layer with a porosity of 30% was formed on the positive electrode substrate.
[0158] (Preparation of negative electrode) Li, the negative electrode active material 4 Ti 5 O 12 The negative electrode mixture paste was prepared by mixing the negative electrode active material, acetylene black (AB) as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and a dispersion medium. The mass ratio of the negative electrode active material, AB, and PVDF was 87:5:8 (solid content conversion). The negative electrode mixture paste was applied to the surface of aluminum foil (average thickness 15 μm) as the negative electrode substrate at a mass of 10 mg / cm. 2 (based on solid content) was applied. Thereafter, drying and roll pressing were performed to obtain a negative electrode in which a negative electrode active material layer with a porosity of 40% was formed on the negative electrode substrate.
[0159] (Preparation of solutions for producing non-aqueous gel electrolytes (solution A and solution B)) In the non-aqueous solvent sulfolane (SL), 1.0 mol / dm 3 LiPF at a concentration of 6 A non-aqueous electrolyte solution was obtained by dissolving monomer A and a base catalyst in the non-aqueous electrolyte solution. Separately, monomer B was dissolved in the non-aqueous electrolyte solution to obtain solution B. Note that solutions A and B were prepared so that the content of the crosslinked polymer, which is the reaction product of monomer A and monomer B, in the non-aqueous gel electrolyte obtained by mixing and reacting solution A and solution B was 5 mass % and the content of the base catalyst was 0.068 mass %.
[0160] (Preparation of non-aqueous electrolyte storage element) A polyolefin microporous film was used as the separator. The positive electrode and the negative electrode were laminated through this separator to prepare an electrode body. The electrode body was housed in a container, and a positive electrode terminal and a negative electrode terminal were attached. The above-mentioned solution A and solution B were mixed to prepare a precursor solution of a nonaqueous gel electrolyte, and the precursor solution was poured into the container, sealed, and left at a temperature of 25°C for 7 days. As a result, a nonaqueous electrolyte storage element of Example 1 having a nonaqueous gel electrolyte containing a crosslinked polymer was obtained. All of the above operations were carried out under an argon atmosphere.
[0161] [Examples 2 and 3, Comparative Examples 1 to 4] Each of the nonaqueous gel electrolytes of Examples 2 and 3 and Comparative Examples 1 to 4 was obtained in the same manner as Example 1, except that each of the nonaqueous solvents shown in Table 1 was used as the nonaqueous solvent. Furthermore, each of the nonaqueous electrolyte storage elements of Examples 2, 3 and Comparative Example 3 was obtained in the same manner as Example 1, except that each of the nonaqueous solvents shown in Table 1 was used as the nonaqueous solvent.
[0162] [Reference example 1] (1) Preparation of non-aqueous gel electrolyte In a non-aqueous solvent, fluoroethylene carbonate (FEC), 1.0 mol / dm 3 LiPF at a concentration of 6 The nonaqueous electrolyte was obtained by dissolving ETPTA at a content of 10% by mass and a radical polymerization initiator (2,2'-azobisisobutyronitrile) at a content of 1% by mass in the nonaqueous electrolyte, and the solution was allowed to stand at a temperature of 60°C for 24 hours. As a result, a nonaqueous gel electrolyte of Reference Example 1 containing a crosslinked polymer was obtained. All of the above operations were carried out under an argon atmosphere.
[0163] [evaluation] (1) Evaluation of gelation and stability of gel state In "(1) Preparation of non-aqueous gel electrolyte", it was confirmed whether gelation occurred after standing for 24 hours and whether a non-aqueous gel electrolyte was obtained. The results are shown in Table 1. If gelation occurred and a non-aqueous gel electrolyte was obtained, it is indicated as "Yes", and if gelation did not occur and a non-aqueous gel electrolyte was not obtained, it is indicated as "No". Next, each of the nonaqueous gel electrolytes of Examples 1 to 3 and Comparative Examples 1 to 3 obtained in "(1) Preparation of nonaqueous gel electrolyte" was allowed to stand for one week at a temperature of 25°C. The appearance of the nonaqueous gel electrolyte after standing for one week was observed to confirm whether or not liquid had seeped out from the nonaqueous gel electrolyte. The results are shown in Table 1. Those in which seepage was confirmed are indicated as "present", and those in which seepage was not confirmed are indicated as "absent". Those in which seepage of liquid was not confirmed can be judged to have a high stability of the gel state.
[0164] (2) Oxidation resistance evaluation Using each of the nonaqueous electrolyte storage elements of Examples 1 to 3 and Comparative Example 3 obtained in "(2) Preparation of nonaqueous electrolyte storage element", the oxidation resistance of the nonaqueous gel electrolyte was evaluated by measuring the oxidative decomposition current according to the following procedure.
[0165] (Initial charge / discharge) Each nonaqueous electrolyte storage element was subjected to constant current / constant voltage charging at a temperature of 25°C with a charging current of 0.1C and a charge cut-off voltage of 2.95V. The charge was terminated until the charging current reached 0.05C. A rest period of 10 minutes was then provided. A constant current discharge was then performed with a discharge current of 0.1C and a discharge cut-off voltage of 1.15V. A rest period of 10 minutes was then provided. This charge / discharge cycle was repeated for two cycles. 1C is 1.3mA / cm 2 The charge cut-off voltage of the positive electrode was 4.50 V vs. Li / Li. + It was set to be.
[0166] (Oxidation decomposition current measurement) Next, constant current / constant voltage charging was performed at a temperature of 25°C with a charging current of 0.1C and a charge cut-off voltage of 2.95V. The charge was terminated when the charging current reached 0.05C. The nonaqueous electrolyte storage element in the charged state was then set in a high-performance electrochemical measurement system ("VMP-300" manufactured by Biologic) and chronoamperometry measurement was performed for 100 hours at a voltage of 2.95V. The specific measurement conditions were as follows: Apply: Ei=2.950V vs.Ref. Ti=100h Record: every dt=30s E Range: 2.93-2.97V I Range: 100μA Bandwidth:8 In the above measurement, the current measured during the measurement time from 80 hours to 100 hours, when the current became approximately constant, was regarded as the current caused by the oxidative decomposition of the nonaqueous gel electrolyte, and the average current was calculated by averaging the current. The average current was divided by the mass of the positive electrode active material layer to obtain the oxidative decomposition current. The results are shown in Table 1. In the measurement of the oxidative decomposition current, in order to reduce the effect of the reductive decomposition of the nonaqueous gel electrolyte, Li, which has a relatively high reaction potential, was used as the negative electrode active material of the nonaqueous electrolyte storage element as described above. 4 Ti 5 O 12 Therefore, the current measured during the measurement time period from 80 hours to 100 hours can be considered to be a current caused by the oxidative decomposition of the nonaqueous gel electrolyte.
[0167] [Table 1]
[0168] DEC(SP value 9.6(cal / cm 3 ) 1 / 2 ) or TFEMC (SP value 9.8 (cal / cm 3 ) 1 / 2 The nonaqueous gel electrolytes of Comparative Examples 1 and 2, in which a nonaqueous solvent containing ethylenediaminetetraacetate (EDA) as one of the main components was used, exhibited poor stability in the gel state due to seepage of the liquid. 3 ) 1 / 2 ) and DMC (SP value 10.4 (cal / cm 3 ) 1 / 2 The nonaqueous electrolyte of Comparative Example 3, in which a nonaqueous solvent containing ) as a main component was used, did not seep out, but had a large oxidative decomposition current value and low oxidation resistance. In Comparative Example 4, in which FEC was used as the nonaqueous solvent, gelation did not occur sufficiently under the base catalyst, and a nonaqueous gel electrolyte was not obtained. This is believed to be due to the reaction of FEC with the base catalyst. In contrast, a compound selected from the group consisting of sulfones and carbonates including PC and having a solubility parameter of 10.0 (cal / cm 3 ) 1 / 2 Each of the nonaqueous gel electrolytes of Examples 1 to 3, in which a nonaqueous solvent containing at least one of the above components as a main component was used, had high stability in the gel state since no liquid seeped out, and had high oxidation resistance since the value of the oxidative decomposition current was small. Note that gelation due to a radical polymerization reaction occurred even when FEC was used as the non-aqueous solvent as in Reference Example 1. The phenomenon in which gelation does not occur when FEC is used as the non-aqueous solvent is considered to be a phenomenon specific to reactions using a base catalyst. [Industrial Applicability]
[0169] The nonaqueous gel electrolyte according to the present invention is suitably used as a nonaqueous electrolyte for a nonaqueous electrolyte storage element. [Explanation of symbols]
[0170] 1. Non-aqueous electrolyte storage element 2 Electrode body 3 containers 4 Positive terminal 41 Positive lead 5 Negative terminal 51 Negative lead 20 Energy Storage Unit 30 Energy storage device
Claims
1. The present invention comprises a crosslinked polymer having a polyethylene oxide skeleton, a base catalyst, and a non-aqueous solvent, The non-aqueous solvent is selected from the group consisting of sulfones and carbonates including propylene carbonate, and has a solubility parameter of 10.0 (cal / cm 3 ) 1/2 A non-aqueous gel electrolyte comprising at least one of the above components as a main component.
2. The nonaqueous gel electrolyte according to claim 1 , wherein the crosslinked polymer has a crosslinked site including a structure represented by the following formula (1): 【Chemistry 1】 In the above formula (1), R 1 is -S-, -NR 3 - (R 3 is a hydrogen atom or an alkyl group. R is a divalent group represented by —O—. 2 is a divalent electron-withdrawing group. * indicates a bonding site with another group or atom.
3. The nonaqueous gel electrolyte according to claim 1 , wherein the crosslinked polymer is a crosslinked reaction product of a first compound represented by the following formula (2) and a second compound represented by the following formula (3): 【Chemistry 2】 In the above formula (2), R 4 is n 2 R is a 4-valent hydrocarbon group. 5 Each X is independently a divalent linking group. 8 (R 8 is a hydrogen atom or an alkyl group. 9 (R 9 is a hydrogen atom or a metal atom. 1 are each independently an integer of 0 to 250. 2 is an integer between 2 and 8 inclusive. In the above formula (3), R 6 is n 4 R is a 4-valent hydrocarbon group. 7 Each of Y is independently a divalent linking group. Each of Y is independently a group having a double bond between an electron-withdrawing group and the carbon atoms at the α-position and the β-position to the electron-withdrawing group. 3 are each independently an integer of 0 to 250. 4 is an integer between 2 and 8 inclusive. However, n 1 and n 3 At least one of n is an integer between 25 and 250. 2 and n 4 At least one of the above is an integer of 3 or more and 8 or less.
4. A nonaqueous electrolyte storage element comprising the nonaqueous gel electrolyte according to claim 1 .
5. A method for crosslinking a first compound with a second compound in a container in the presence of a base catalyst and a non-aqueous solvent, At least one of the first compound and the second compound has a polyethylene oxide skeleton, the first compound and the second compound each have a functional group capable of undergoing a crosslinking reaction with the other in the presence of the base catalyst, The non-aqueous solvent is selected from the group consisting of sulfones and carbonates including propylene carbonate, and has a solubility parameter of 10.0 (cal / cm 3 ) 1/2 A method for producing a nonaqueous electrolyte electricity storage element comprising at least one of the above components as a main component.
Citation Information
Patent Citations
Nonaqueous gel electrolyte, and nonaqueous gel electrolyte secondary battery arranged by use thereof