Electrophotographic belt and electrophotographic image formation device
The electrophotographic belt with a PEEK base layer containing 18 to 30% carbon black and controlled moisture content and crystallization temperature addresses conductivity and crack issues, ensuring stable high-quality image formation.
Patent Information
- Application Number
- JP2024033578
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2024-03-06
- Publication Date
- 2024-10-25
AI Technical Summary
Existing electrophotographic belts face issues with increased conductivity and crack formation over time due to thermal deterioration and uneven carbon black distribution, leading to instability in forming high-quality images.
The electrophotographic belt incorporates a base layer composed of polyetheretherketone (PEEK) with 18 to 30% carbon black, controlled moisture content of 0.50% or more, and a cooling crystallization temperature of 288.0°C or less, which stabilizes conductivity and prevents cracks by managing carbon black dispersion and crystallization.
The solution enhances long-term conductivity stability and prevents cracks, enabling the formation of high-quality electrophotographic images over an extended period.
Smart Images

Figure 2024152622000001_ABST
Abstract
Description
[Technical field]
[0001] FIELD This disclosure relates to an electrophotographic belt and an electrophotographic image forming apparatus having the electrophotographic belt. [Background technology]
[0002] In electrophotographic image forming apparatuses (hereinafter sometimes referred to as "electrophotographic apparatuses") such as copying machines and laser beam printers, some intermediate transfer belts having an endless shape are used. The endless electrophotographic belts used as intermediate transfer belts include those having a single-layer structure consisting of only a base layer, and those having a laminated structure consisting of two or three layers. The two-layer structure includes, for example, one consisting of a base layer and an elastic layer on the outer peripheral surface of the base layer, and the three-layer structure includes, for example, one having a base layer, an elastic layer on the outer peripheral surface of the base layer, and a surface layer on the outer peripheral surface of the elastic layer.
[0003] It has been proposed to use polyetheretherketone and polyphenylsulfide, which are super engineering plastics with excellent strength, as a binder for the thermoplastic resin that is inexpensive and easy to recycle, in the base layer of such an electrophotographic belt. Polyetheretherketone may be referred to as "PEEK" hereinafter. Polyphenylsulfide may be referred to as "PPS" hereinafter. Since crystalline thermoplastic resins such as PEEK and PPS have high melting points, a conductive filler such as carbon black is used as a conductivity imparting agent for making the base layer conductive, as described in Patent Document 1.
[0004] Here, Patent Document 1 discloses an invention aimed at providing a sheet member for an image-forming apparatus that has excellent roller habit resistance and excellent crack resistance. The sheet member for an image-forming apparatus contains PEEK and less than 19 mass % of a conductive filler, and has a temperature-reducing crystallization peak temperature Tc of less than 299.0°C. Paragraph
[0038] of Patent Document 1 describes that if Tc is low, heat resistance is low, but there is a large amount of high molecular weight components, which is advantageous for crack resistance, and that if Tc is high, low molecular weight components tend to become crystal nuclei and the degree of crystallization tends to be high, resulting in high heat resistance and low crack resistance.
[0005] In addition, Patent Document 1 describes that by selecting PEEK with a low Tc, i.e., PEEK with excellent crack resistance, and slowly cooling and crystallizing it during the film formation process, the roller habit resistance is improved, thereby achieving both crack resistance and roller habit resistance. Furthermore, paragraph
[0050] of Patent Document 1 describes that if the content of the conductive filler in the sheet member for image-forming apparatus according to the invention described in Patent Document 1 exceeds 19% by weight, the crack resistance decreases, which is not preferable. From the viewpoint of stably expressing conductivity, it is preferable to use as much carbon black as possible. However, the sheet member for image-forming apparatus according to Patent Document 1 is premised on the content of carbon black being less than 19% by mass, and in the examples, the content ratio of carbon black based on the mass of the sheet member of carbon black was at most 16% by mass.
[0006] On the other hand, Patent Document 2 discloses that when an electrophotographic belt in which electrical conductivity is imparted by using a conductive filler is used for forming electrophotographic images for a long period of time as, for example, an intermediate transfer belt, the electrical resistance of the electrophotographic belt may decrease. Patent Document 2 describes that such a decrease in electrical resistance occurs due to the following mechanism.
[0007] That is, discharge occurs at the portion where the intermediate transfer belt is separated from the primary transfer roller and the secondary transfer roller, and an excessive current flows inside the intermediate transfer belt at once. A high voltage is applied between the carbon black particles, which are electric points, and the binder resin interposed between the carbon black particles is heated and carbonized. As a result, the carbon black particles, which are originally electrically insulating, become conductive, and the conductivity increases. Patent Document 2 discloses that the above-mentioned decrease in electrical resistance can be solved by improving the dispersibility of carbon black in the binder resin. To achieve this, it is described that carbon black and PEEK are melt-kneaded repeatedly (2 to 6 times). [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Patent Publication No. 2021-009400 [Patent Document 2] JP 2012-177811 A Summary of the Invention [Problem to be solved by the invention]
[0009] The repeated melt-kneading of the binder resin and carbon black disclosed in Patent Document 2 can be a factor in increasing the manufacturing cost of the electrophotographic belt. In addition, repeated kneading at high temperatures may cause thermal degradation of the binder resin (crosslinking due to thermal decomposition or oxidation), which may lead to a decrease in the strength of the electrophotographic belt. Furthermore, even if the dispersibility of the carbon black is highly improved, it is difficult to make the interparticle distances of all the carbon black particles equal. Therefore, when an excessive current flows through the intermediate transfer belt, a high voltage is applied between the carbon black particles that are relatively close to each other. Therefore, it is difficult to completely prevent carbonization of the binder resin interposed between the carbon black particles.
[0010] Therefore, at least one aspect of the present disclosure is directed to providing an electrophotographic belt capable of suppressing an increase in electrical conductivity of the electrophotographic belt over time due to long-term use and preventing the occurrence of cracks at a higher level, and at least one aspect of the present disclosure is directed to providing an electrophotographic image forming apparatus capable of stably forming high-quality electrophotographic images over a long period of time. [Means for solving the problem]
[0011] According to at least one aspect of the present disclosure, there is provided an electrophotographic belt comprising: The electrophotographic belt has at least a base layer, The base layer contains polyether ether ketone, which is a thermoplastic resin, and carbon black, The content of the carbon black is 18 to 30% by mass based on the mass of the base layer, A sample cut out from the base layer is heated in a nitrogen atmosphere from 30°C to 100°C at a rate of 20°C per minute and held at 100°C for 30 minutes; the mass of the sample is defined as X1; the sample is then cooled from 100°C to 30°C at a rate of 20°C per minute and placed in an air environment at a temperature of 23°C and a relative humidity of 50% for 48 hours; the mass of the sample is defined as X2. The moisture content of the base layer calculated by the moisture content of the base layer = ((X2-X1) / X2) × 100 is 0.50 mass% or more, An electrophotographic belt is provided, wherein the base layer has a crystallization temperature at low temperature of 288.0° C. or less as measured by differential scanning calorimetry.
[0012] According to at least one aspect of the present disclosure, there is provided an electrophotographic image forming apparatus including the above-described electrophotographic belt. Effect of the Invention
[0013] According to at least one aspect of the present disclosure, the electrical conductivity of an electrophotographic belt due to long-term use is It is possible to obtain an electrophotographic belt capable of suppressing the change (increase) in the electrical conductivity with time and preventing the occurrence of cracks at a higher level. Furthermore, according to at least one embodiment of the present disclosure, it is possible to obtain an electrophotographic image forming apparatus capable of stably forming high-quality electrophotographic images for a long period of time. [Brief description of the drawings]
[0014] [Figure 1] FIG. 2 is a schematic cross-sectional view of an image forming apparatus used for image evaluation. [Diagram 2] FIG. 2 is an explanatory diagram of a configuration example of an electrophotographic belt. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] In this disclosure, the description of "XX or more and YY or less" or "XX to YY" representing a numerical range means a numerical range including the lower and upper limits, which are the endpoints, unless otherwise specified. In addition, when a numerical range is described in stages, the upper and lower limits of each numerical range can be arbitrarily combined. In addition, in this disclosure, "Ω / □" means "Ω / square".
[0016] An electrophotographic belt according to the present disclosure will now be described. FIG. 2A shows a perspective view of an electrophotographic belt 200 according to an embodiment of the present disclosure. The electrophotographic belt may have an endless shape. An example of the layer structure is a monolayer structure in which the cross section of the line AA in FIG. 2A is composed of only a base layer 201 as shown in FIG. 2B. In this case, the outer surface 200-1 of the base layer becomes the toner carrying surface (outer surface) of the electrophotographic belt. The electrophotographic belt 200 has at least a base layer. As described above, the electrophotographic belt 200 may have an elastic layer on the outer peripheral surface of the base layer 201, and may further have a surface layer on the outer peripheral surface of the elastic layer. In addition, a back layer that covers the inner peripheral surface of the base layer 201 may be provided.
[0017] The base layer contains polyether ether ketone (hereinafter, sometimes referred to as "PEEK"), which is a thermoplastic resin, and carbon black. PEEK can be a binder resin for the base layer. Carbon black can be a conductivity imparting agent. The carbon black content is 18 to 30 mass% based on the mass of the base layer.
[0018] The sample cut out from the base layer is heated in a nitrogen atmosphere from 30°C to 100°C at a rate of 20°C per minute and held at 100°C for 30 minutes; the mass of the sample is designated as X1. The sample is then cooled from 100°C to 30°C at a rate of 20°C per minute, and placed in an air environment at a temperature of 23°C and a relative humidity of 50% for 48 hours; the mass of the sample is designated as X2. The value (moisture content) calculated by the formula Moisture content of the base layer = ((X2-X1) / X2) x 100 is 0.50 mass% or more.
[0019] Here, X1 is the mass of a sample cut out from the base layer when the temperature of the sample is raised from 30° C. to 100° C. at a rate of 20° C. per minute in a nitrogen atmosphere and maintained at 100° C. for 30 minutes. X1 is regarded as the mass of the sample in a state in which water has been removed (hereinafter, also referred to as the “dry state”). X2 is the mass of the sample when the dried sample is cooled from 100°C to 30°C at a rate of 20°C per minute and then placed in an air environment at 23°C and 50% relative humidity for 48 hours. X2 is regarded as the mass of the sample in a state where the sample once dried absorbs water (hereinafter also referred to as the "water-absorbed state").
[0020] Therefore, in the present disclosure, the value calculated by ((X2-X1) / X2) x 100 is referred to as the "water content of the base layer." The present inventors have found that an electrophotographic belt having a base layer with a water content of 0.50% by mass or more is unlikely to suffer from a change in electrical conductivity even after repeated use over a long period of time.
[0021] As described above, the increase in electrical conductivity over time of a conventional electrophotographic belt having a base layer containing PEEK as a binder resin and having carbon black dispersed in the binder resin as conductive particles is believed to be due to the carbonization of the binder resin present between the carbon black particles when a high voltage is applied between the carbon black particles.
[0022] On the other hand, the base layer according to the present disclosure, whose moisture content measured by the above method is 0.50% by mass or more, stably contains a certain amount of moisture in a normal office environment, such as a temperature of 23°C and a relative humidity of 50% under atmospheric conditions. In a base layer that stably contains moisture, even if a high voltage is applied between the carbon black particles due to the above-mentioned discharge phenomenon, the energy is consumed in the evaporation or electrolysis of moisture. Therefore, it is considered that carbonization of the binder resin present between the carbon black particles is suppressed, and the insulation between the carbon black particles is better maintained. As a result, it is considered that the conductivity of the base layer is less likely to change (increase) even with repeated use over a long period of time.
[0023] As described above, even if the base layer becomes dry once, it can again contain a certain amount of water by placing it in an atmosphere at a temperature of 23° C. and a relative humidity of 50% for 48 hours. Therefore, in the electrophotographic belt according to the present disclosure, even if the moisture in the base layer is once consumed by evaporation or decomposition due to application of a high voltage, the base layer can absorb moisture again. Therefore, even if it is used for a long period of time, carbonization of PEEK can be continuously suppressed. As a result, it is considered that the change in conductivity can be suppressed even with long-term use.
[0024] The glass transition point of the PEEK contained in the base layer is, for example, about 143° C. The heat absorption effect of moisture appears at a temperature sufficiently lower than the glass transition point of PEEK, so it is expected to have the effect of suppressing changes in electrical resistance caused by the shrinkage of the resin due to heat generation.
[0025] X1 and X2 are measured using a thermogravimetric measuring device under the following conditions: A plurality of samples cut into 4 mm x 4 mm from the electrophotographic belt are loaded into a platinum sample pan with a capacity of 50 μL or 100 μL so that the total mass is 15 mg ± 4 mg.
[0026] The mass of the sample when it is heated from 30°C to 100°C at a rate of 20°C per minute in a nitrogen atmosphere and held at 100°C for 30 minutes is defined as X1. The sample is then cooled from 100°C to 30°C at a rate of 20°C per minute, and then placed in an air environment at a temperature of 23°C and a relative humidity of 50% for 48 hours, and its mass is defined as X2. The moisture content of the base layer is calculated by the mass change rate calculated by the moisture content of the base layer = ((X2-X1) / X2) x 100. In the electrophotographic belt according to the present disclosure, the moisture content of the base layer is 0.50 mass% or more. When a similar evaluation is performed on PEEK alone that does not contain any carbon black, the moisture content is less than 0.04%.
[0027] The moisture content of the base layer is preferably 0.70 to 1.00% by mass, and more preferably 0.70 to 0.90% by mass. Within this range, the effect of suppressing the change in electrical conductivity of the base layer over time is more easily exhibited.
[0028] As a method for obtaining a base layer having a moisture content in the above range, for example, a method using carbon black, which easily adsorbs moisture, as a conductive filler in the base layer can be mentioned. From the viewpoint of achieving a desired moisture content and further a desired electrical resistivity, the content of carbon black is 18 to 30 mass% based on the mass of the base layer, as described above.
[0029] In this way, the base layer contains 18% by mass or more of carbon black based on the mass of the base layer. By increasing the carbon black content in the base layer, the desired electrical conductivity can be easily imparted to the base layer. However, an increase in the carbon black content in the base layer may lead to the occurrence of cracks in the base layer. As a result of further studies by the present inventors, it was found that even when the carbon black content in the base layer is set to 18 to 30 mass % as described above, the crack resistance can be improved by controlling the cooling crystallization temperature of the base layer to a specific range.
[0030] Specifically, the cooling crystallization temperature of the base layer measured by differential scanning calorimetry (DSC) must be 288.0°C or lower. The peak temperature detected in the process of cooling from a molten state in DSC is the cooling crystallization temperature. The cooling crystallization temperature is the peak temperature that appears when a sample is cut out from the base layer, set in the DSC, heated to 400°C at 10°C / min, and then cooled to room temperature (25°C) at 10°C / min.
[0031] The present inventors consider the reason why the crack resistance improves when the crystallization temperature is 288.0°C or less as follows. The crystallization temperature of 288.0°C is lower than the crystallization temperature of PEEK (292.8°C) achieved in Example 5 of Patent Document 2. The base layer containing PEEK and carbon black is formed, for example, by extrusion molding a melt of a resin composition for forming the base layer containing PEEK. At this time, PEEK is cooled from a molten state and solidifies, and in the process, the carbon black acts as a nucleus to promote crystallization. By delaying the crystallization at this time, that is, by lowering the crystallization temperature of the base layer, the crystallization degree of PEEK in the base layer can be reduced and a large amount of amorphous parts can be present. As a result, it is considered that the crack resistance improves.
[0032] The cooling-down crystallization temperature is preferably 280.0 to 288.0° C., and more preferably 285.0 to 287.8° C. There are no particular limitations on the means for setting the cooling-down crystallization temperature to 288.0° C. or lower, but examples thereof include the use of furnace black that has been subjected to a surface treatment described below.
[0033] Therefore, the carbon black preferably contains furnace black. Compared with acetylene black, which is highly graphitized, furnace black is less likely to interact with PEEK molecules and is relatively less likely to become a crystal nucleus of PEEK. Furthermore, furnace black that has been treated (at least one of surface treatment and nitrogen treatment) described below is less likely to become a crystal nucleus of PEEK and can lower the temperature-reducing crystallization temperature of the base layer. The reason why surface-treated carbon black is less likely to become a crystal nucleus is believed to be that fine irregularities are formed on the surface of the surface-treated carbon black, making its surface area very large.
[0034] The above-mentioned method for producing the electrophotographic belt will now be described in detail. <Binder resin> The electrophotographic belt is required to have a strength that does not stretch even when it is continuously subjected to a tensile load for a long period of time in an electrophotographic image forming apparatus. Therefore, it is preferable that the thermoplastic resin used as the binder resin in the base layer is classified as a super engineering plastic. The base layer according to the present disclosure contains PEEK as the binder resin.
[0035] Various grades of PEEK are commercially available, and in the present disclosure, a single grade may be used, or two or more grades may be used in combination. Commercially available PEEK products include the Victrex PEEK series manufactured by Victrex, Inc. Grades of PEEK include PEEK 450G, 381G, and 151G.
[0036] <Carbon black> The base layer contains carbon black. The carbon black may be a conductivity imparting agent. The carbon black is preferably a commercially available carbon black that has been subjected to a treatment described below to form fine convex portions derived from an organic compound on the surface. In other words, the carbon black preferably has convex portions derived from an organic compound on the surface.
[0037] In this specification, carbon black before treatment may be referred to as "raw carbon black." Furthermore, carbon black having fine protrusions on its surface after treatment may be referred to as "treated carbon black" or simply as "carbon black."
[0038] The melting point of PEEK used as the binder resin is, for example, about 330°C. Therefore, when manufacturing an endless conductive base layer using these resins, it is difficult to use an ion-conductive agent, and carbon black is used. In order to achieve the above-mentioned surface resistivity using carbon black, the content of carbon black in the base layer is 18 to 30 mass% based on the mass of the base layer. The content of carbon black in the base layer is preferably 19 to 30 mass%, more preferably 19 to 25 mass%, and even more preferably 20 to 24 mass%. The content of PEEK in the base layer is preferably 70 to 81 mass%, more preferably 75 to 81 mass%, and even more preferably 76 to 80 mass%.
[0039] In this case, the carbon black preferably has a moisture absorption rate (hereinafter also referred to as CB moisture absorption rate) of 0.70% by mass or more, calculated by the following calculation formula (1). By using such carbon black, it becomes easier to make the moisture content of the base layer 0.50% by mass or more.
[0040] After storing the carbon black for 48 hours under conditions of 23°C and 50% relative humidity, measure its mass using a thermogravimetric analyzer (TGA) and call it W0. After measuring W0, the carbon black is heated from 30°C to 120°C at a rate of 20°C per minute in a nitrogen atmosphere and held at 120°C for 15 minutes; its mass is then measured using a thermogravimetric analyzer (TGA) in the same manner and called W1. CB moisture absorption rate = [(W0 - W1) / W0] × 100 (1).
[0041] The CB water absorption rate is more preferably 1.00 to 2.00% by mass, and further preferably 1.10 to 1.50% by mass. The CB water absorption rate can be controlled by increasing the specific surface area of the carbon black used to increase the amount of water per unit mass. As described above, from the viewpoint of suppressing crystallization during molding, the carbon black is preferably furnace black, and the crystallization temperature can be further lowered by increasing the BET specific surface area by the treatment method described below.
[0042] <Carbon black surface treatment method> The surface treatment method for forming fine convex portions on the surface of raw carbon black to obtain treated carbon black will be described below. The treatment for forming fine convex portions on the surface of raw carbon black includes a first step of adhering an organic substance to the surface of the raw carbon black, and a second step of firing the adhering organic substance. The formation of such fine protrusions makes it easy to increase the BET specific surface area.
[0043] First, the first step of adhering an organic substance to the surface of the raw carbon black will be described. . In the step of adhering an organic substance to the surface of raw carbon black, the raw carbon black may be mixed with the organic substance while still in a solid powder state. From the viewpoint of evenly adhering the organic substance to the surface, it is preferable to mix the raw carbon black with the organic substance in a liquid. Here, the step of adhering an organic substance to the surface of raw carbon black in a liquid will be described.
[0044] The first step is to dissolve an organic substance in a solvent to prepare an organic substance solution, and then to add and stir raw carbon black to the organic substance solution to prepare a raw carbon black dispersion. The solvent that can be used is water or an organic solvent, but water is preferred in consideration of ease of handling and environmental impact. A general dispersant may be used to improve the dispersion state of the raw material carbon black.
[0045] The organic matter to be attached to the raw carbon black preferably has a high affinity for the surface of the raw carbon black and also has a high affinity for the solvent. Specific examples include organic compounds called cationic surfactants, anionic surfactants, and nonionic surfactants. Among these, nonionic surfactants are preferred because they tend to suppress coarsening due to aggregation when the carbon black with the attached organic matter is removed in a later process.
[0046] Nonionic surfactants include, for example, ester type and ether type, and examples of the ester type include glycerin fatty acid esters, sorbitan fatty acid esters, and sucrose fatty acid esters, which have a structure in which polyhydric alcohols such as glycerin and sorbitan, and sucrose are ester-bonded to fatty acids. Examples of the ether type include polyoxyethylene alkyl ethers, polyoxyethylene alkyl allyl ethers, and polyoxyethylene propylene glycol, which are mainly obtained by addition polymerization of higher alcohols, alkylphenols, propylene glycol, and the like, to ethylene oxide. Among these, polyoxyethylene alkyl ethers are preferred because they have good affinity with the solvent and the surface of the conductive carbon. The dispersant used may be one type, or a plurality of dispersants may be used in combination.
[0047] The amount of the organic substance added to and dissolved in the solvent is preferably adjusted to a ratio of the saturated solubility or less relative to 100 parts by mass of the solvent, and the mass ratio "A / B" where A is the part by mass of the raw carbon black and B is the part by mass of the organic substance relative to 100 parts by mass of the solvent, is preferably adjusted to 0.1 or more and 20.0 or less. A / B is more preferably 0.5 or more and 3.0 or less. By setting the amount of the organic substance to be added at or below the saturation solubility, precipitation of the organic substance can be suppressed, and the raw carbon black can be more easily treated.
[0048] In addition, by setting the mass ratio A / B of carbon black to organic matter to 0.1 or more, the amount of organic matter relative to carbon black becomes appropriate, thereby suppressing the amount of organic matter that cannot adhere to the surface of the raw carbon black and floats away. In addition, by setting the mass ratio A / B to 20 or less, the raw carbon black can be treated more efficiently.
[0049] The dissolution of the organic matter in the solvent can be promoted by appropriately selecting a means for promoting dissolution of the organic matter, such as agitation with an agitating blade, or a combination of means such as ultrasonic vibration, a homogenizer, or heat treatment. In addition, since there is a risk of foaming during agitation, an antifoaming agent can also be appropriately selected. The amount of raw carbon black added to the organic matter solution is preferably 1 part by mass or more and 50 parts by mass or less, and more preferably 5 parts by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the solvent.
[0050] It is preferable to add the raw carbon black to the organic matter solution in small amounts. The raw carbon black can be dispersed in the organic matter solution by, for example, screw stirring or shear flow ( This can be achieved by means of a homogenizer, a nanomizer, high pressure liquid collision, or media dispersion (ball mill, bead mill).
[0051] Next, the second step of calcining the organic matter attached to the surface of the raw carbon black will be described. The second step is a step of removing the solvent from the raw carbon black dispersion obtained in the first step, in which organic matter is adhered to the surface of the raw carbon black, and calcining the resulting solid content.
[0052] Any known method can be used to remove the solvent from the raw carbon black dispersion and extract the solid content. Examples of such methods include heat drying, vacuum drying, centrifugation, and reduced pressure filtration. Heat drying is preferred in consideration of the amount of processing required at one time. Examples of heat drying include static drying in which the raw carbon black dispersion is left stationary in a heated atmosphere, stirring drying, air flow drying in which the raw carbon black dispersion is exposed to a heated air flow to promote drying, and spray drying in which the raw carbon black dispersion is sprayed in a mist form in a heated atmosphere to promote drying. Spray drying is preferred in consideration of the amount of processing and the efficiency of removing the solvent.
[0053] A known method can be used as a method for firing the extracted solid content. There are direct heating and indirect heating types for firing devices, but in the method of directly heating the object with a flame such as a burner, it is difficult to control the temperature and the object may be burned, so the indirect heating type is preferred. Specifically, there are electric furnaces, hot air circulation furnaces, high-frequency induction heating furnaces, etc., and hot air circulation furnaces with excellent uniformity of heating temperature are preferred. In addition, there are batch-type heating furnaces and continuous-type heating furnaces, and although continuous-type heating furnaces have a mechanism for charging and discharging, they are not suitable for long-term heating, so batch-type heating furnaces are preferred. In this case, the atmosphere in the heating furnace may be replaced with, for example, nitrogen, in order to suppress excessive firing.
[0054] The baking temperature is preferably equal to or higher than the thermal decomposition start temperature of the organic matter and lower than the decomposition temperature of the raw carbon black. By setting the baking temperature to equal to or higher than the thermal decomposition start temperature of the organic matter, the organic matter attached to the surface of the raw carbon black is decomposed, and treated carbon black having a convex shape on the surface is easily formed. Furthermore, by setting the baking temperature to lower than the decomposition temperature of the raw carbon black, the loss of the raw carbon black during the treatment process can be suppressed. Specifically, the baking temperature is preferably, for example, 300°C or higher and 600°C or lower, and particularly preferably 350°C or higher and 500°C or lower.
[0055] The BET specific surface area of the obtained carbon black (treated carbon black) is preferably 240 m 2 / g or more. Further, it is preferably 240 to 300 m 2 / g, more preferably 250 to 300 m 2 / g, and even more preferably 250 to 270 m 2 / g. When it is in the above range, the temperature-lowering crystallization temperature can be more easily controlled within the aforementioned range. The BET specific surface area can be determined from the amount of nitrogen adsorbed on the particle surface of the carbon black when it reaches equilibrium after immersing the degassed carbon black in liquid nitrogen (Japanese Industrial Standard (JIS) K6217-2:2017). Also, the DBP (dibutyl phthalate) absorption amount of the carbon black is preferably 100 to 200 mL / 100 g, and more preferably 130 to 160 mL / 100 g.
[0056] <CB water absorption rate> As described above, it is considered that the carbonization of the binder resin mainly occurs when a high voltage is applied between the particles of the carbon black. Therefore, by using a carbon black with a large water adsorption amount, it is preferable to make the water content of the base layer 0.50 mass% or more. Here, the base layer containing PEEK as the binder resin needs to undergo kneading at about 300 to 400 °C in the manufacturing process. Therefore, the carbon black contained in the base layer preferably has the ability to maintain a certain amount of water adsorption even after passing through such a temperature. Specifically, the treated carbon black is preferably a carbon black that satisfies the above-described CB water absorption rate.
[0057] Incidentally, the adsorption of water by carbon black is due to functional groups present on the surface of carbon black and the structure of carbon black. Here, it is considered that the functional groups on the surface of carbon black disappear during the process of kneading carbon black at a temperature above the melting point of PEEK. Therefore, the water adsorption ability due to such functional groups is lost after kneading PEEK. On the other hand, the structure of carbon black is hardly lost even after the kneading process of PEEK. Therefore, the water adsorption due to the structure is reversible.
[0058] Because if carbon black with a developed structure exists in the base layer, even if a high voltage is applied between the carbon black particles and the water adsorbed by the carbon black is lost by evaporation or electrolysis, the moisture in the surrounding environment is absorbed into the structure of the carbon black. As a result, it is considered that the base layer can stably contain a certain amount of water.
[0059] <CB water content> Here, regardless of the presence or absence of the above surface treatment, the amount of water contained in carbon black (hereinafter also referred to as "CB water content") can be measured and calculated by the following steps (iv) to (v). Step (iv): Measure the mass (W2) of the carbon black to be judged after leaving it for 48 hours under the conditions of a temperature of 23°C and a relative humidity of 50% using TGA. Step (v): Measure the mass (W3) of the carbon black whose mass (W2) has been measured when the temperature is raised from 30°C to 120°C at a rate of 20°C per minute and held at 120°C for 15 minutes in a nitrogen atmosphere using TGA.
[0060] Calculate the CB water content (mass%) by the following calculation formula (2). CB water content = ((W2 - W3) / W2) × 100 ···(2) The CB water content is preferably 1.00 to 4.00 mass%, more preferably 2.00 to 3.00 mass%, and even more preferably 2.50 to 2.80 mass%.
[0061] For the commercially available carbon blacks "#3230B" and "PrintexL" shown below, the CB moisture content (%) calculated using formula (2) above and the CB moisture absorption rate calculated using formula (1) above are shown in Table 1 below. "#3230B" (product name, manufactured by Mitsubishi Chemical Corporation) "PrintexL" (product name, manufactured by Orion Engineered Carbons Co., Ltd.) [Table 1]
[0062] Although "PrintexL" has a relatively high CB moisture content, the CB moisture absorption rate is extremely low. From this, it can be inferred that the moisture content of "PrintexL" is largely due to its effect on the functional groups on the surface of the carbon black. On the other hand, compared to "PrintexL," "#3230B" is able to adsorb a large amount of moisture even after being baked at high temperatures. From this, it can be inferred that "#3230B" has a developed structure and is able to adsorb moisture reversibly.
[0063] Therefore, "#3230B" can be suitably used as the carbon black to be contained in the base layer. In addition to "#3230B", examples of commercially available carbon black having a CB moisture absorption rate of 0.70 mass% or more include "#44B" (product name, manufactured by Mitsubishi Chemical Corporation; moisture absorption rate = 0.95%). However, carbon black that can be used to obtain the base layer is not limited to these.
[0064] The CB moisture absorption rate can also be measured and calculated by the above-mentioned procedure using carbon black extracted from the base layer. Specifically, for example, when the binder resin is PEEK, a sample taken from the base layer is heated at 600°C for 1 hour in a nitrogen gas atmosphere, whereby the PEEK in the sample is decomposed and the carbon black in the base layer can be extracted. The carbon black content in the base layer can also be calculated using the carbon black extracted in this manner.
[0065] The number-average particle size of the primary particles of the carbon black is preferably 15 nm or more and less than 35 nm, and more preferably 20 to 30 nm. By setting the particle size within the above range, the carbon black can be more reliably prevented from being deteriorated by heat applied in the manufacturing process of the base layer. Also, the carbon black can be more easily and uniformly dispersed in the PEEK.
[0066] <Electrophotographic Belt Manufacturing Method> The electrophotographic belt can be manufactured by a process including the following steps. A step of melt-kneading PEEK, which is a thermoplastic resin, and carbon black to prepare a conductive resin composition in a pellet shape; This process involves melting the pellet-shaped conductive resin composition in a single-screw extruder, extruding the molten material from a cylindrical slit located at the tip of the extruder, and cooling the extruded resin composition using a cylindrical cooling mandrel and cutting it to a specified length.
[0067] The process of melt-kneading a conductive filler and a thermoplastic resin to prepare a pellet-shaped conductive resin composition will be described. The conductive filler and the thermoplastic resin can be melt-kneaded by a known method. For example, a single-screw extruder, a twin-screw kneading extruder, a Banbury mixer, a roll, a Brabender, a plastograph, a kneader, etc. can be used. Among these, a single-screw extruder and a twin-screw kneading extruder are preferred in view of the fact that the materials can be continuously supplied and melt-kneaded, and that the melt-kneaded resin composition is molded into a pellet shape. In addition, at this time, necessary additives may be blended for the purpose of improving the dispersion of the carbon black in the thermoplastic resin and for the purpose of imparting a specific function. When the carbon black contains a large amount of moisture, it is preferable to knead the carbon black while degassing it under reduced pressure during heating.
[0068] The temperature during melt kneading with the thermoplastic resin is equal to or higher than the glass transition temperature of the thermoplastic resin, and is within a temperature range in which the thermoplastic resin does not decompose. For example, when PEEK is used, the melt kneading temperature is preferably 250°C to 400°C, more preferably 300°C to 400°C. When the melt kneading temperature is equal to or higher than the glass transition temperature, the viscosity of the resin is low, and large shear is not applied during melt kneading, making it difficult for the molecular structure of the resin to be broken. In addition, the melt kneading temperature If the temperature is below 400° C., the oxidation and crosslinking of the resin do not proceed easily, making it difficult to form a strong structure.
[0069] The process of molding the conductive resin composition in pellet form into an electrophotographic belt will be described. The obtained conductive resin composition in pellet form is melted in a single-screw extruder and extruded into a tube from a cylindrical slit at the tip of the extruder. The resin composition extruded into a tube is then cut to a predetermined length while controlling the temperature of the resin composition by a cylindrical cooling mandrel, thereby obtaining a base layer for an electrophotographic belt. The temperature during extrusion is preferably from the melting point of the resin to 400°C.
[0070] The conductivity of the base layer is not particularly limited, but considering the primary transferability and secondary transferability when used as an intermediate transfer belt, the surface resistivity is preferably, for example, 1.0×10 3 Ω / □ or more, 1.0×10 14 The range is Ω / □ or less. More preferably, it is 1.0×10 5 Ω / □ or more, 1.0×10 13 Ω / □ or less, and more preferably 1.0×10 9 Ω / □ or more, 1.0×10 13 The range is Ω / □ or less. The thickness of the base layer is, for example, preferably from 25 to 100 μm, and more preferably from 40 to 80 μm.
[0071] The obtained base layer may be further subjected to a heating and cooling treatment. The mechanical strength of PEEK varies greatly depending on its crystallinity. Therefore, by performing heating and cooling treatment according to the usage conditions, the crystallinity can be adjusted to obtain an electrophotographic belt with the desired mechanical strength.
[0072] In addition, the base layer obtained through the above process may have a temporary low moisture content immediately after production because it has been subjected to a heating process. However, the moisture content of the base layer can be controlled to within the above range by storing it in an environment of 23°C and 50% relative humidity for 48 hours or more.
[0073] The base layer obtained as described above can then be provided with a surface layer for covering its outer peripheral surface and a back surface layer for covering its inner peripheral surface, if necessary. Examples of the surface layer include a layer having excellent abrasion resistance, which contains a cured product of an active energy ray curable resin such as an acrylic resin. In this case, the surface layer can be provided, for example, by applying a composition containing an active energy ray curable resin such as a photocurable resin onto the outer peripheral surface of the base layer and curing it. The thickness of the surface layer is not particularly limited, but is preferably, for example, 1 to 5 μm. Examples of the back surface layer include, for example, a resin layer for reinforcing the base layer and a conductive layer for making the inner peripheral surface of the electrophotographic belt conductive. The thickness of the back surface layer is not particularly limited, but is preferably, for example, 0.05 to 10 μm.
[0074] [Electrophotographic Image Forming Apparatus] An embodiment of an image forming apparatus including an electrophotographic belt according to the present disclosure as an intermediate transfer belt will be described. Fig. 1 is a schematic cross-sectional view of an image forming apparatus 100 according to this embodiment. The image forming apparatus 100 according to this embodiment is a tandem-type color laser printer that employs an intermediate transfer method and is capable of forming a full-color image using an electrophotographic method.
[0075] The image forming apparatus 100 has a first, second, third and fourth image forming units Py, Pm, Pc and Pk as a plurality of image forming units. The first, second, third and fourth image forming units Py, Pm, Pc and Pk are arranged in this order along the moving direction of a flat portion (image transfer surface) of an intermediate transfer belt 7 described later. Elements having the same or corresponding functions or configurations in the first, second, third and fourth image forming units Py, Pm, Pc and Pk may be generally described by omitting the suffixes Y, M, C and K indicating that the element is for one of the colors. In this embodiment, the image forming unit P includes a photosensitive drum 1, a charging roller 2, an exposure roller 3, and a photosensitive drum 4, which will be described later. It comprises an optical device 3, a developing device 4, and a primary transfer roller 5.
[0076] The image forming section P has a photosensitive drum 1, which is a drum-type (cylindrical) photosensitive body (electrophotographic photosensitive body) serving as an image carrier. The photosensitive drum 1 is formed, for example, by laminating a charge generating layer, a charge transport layer, and a surface protection layer in this order on an aluminum cylinder serving as a base. The photosensitive drum 1 is driven to rotate in the direction of the arrow R1 in the figure (counterclockwise). The surface of the rotating photosensitive drum 1 is uniformly charged to a predetermined potential of a predetermined polarity (negative polarity in this embodiment) by a charging roller 2, which is a roller-shaped charging member serving as a charging means. During the charging process, a predetermined charging bias (charging voltage) containing a negative DC component is applied to the charging roller 2. The surface of the charged photosensitive drum 1 is scanned and exposed according to image information by an exposure device (laser scanner) 3 serving as an exposure means, and an electrostatic image (electrostatic latent image) is formed on the photosensitive drum 1.
[0077] The electrostatic image formed on the photosensitive drum 1 is developed (visualized) by supplying toner as a developer by a developing device 4 as a developing means, and a toner image (developer image) is formed on the photosensitive drum 1. During the development process, a predetermined development bias (developing voltage) including a negative DC component is applied to a developing roller 4a as a developer carrier provided in the developing device 4. In this embodiment, toner charged with the same polarity as the charging polarity of the photosensitive drum 1 (negative polarity in this embodiment) adheres to an exposed portion (image portion) on the photosensitive drum 1 where the absolute value of the potential has been reduced by exposure after being uniformly charged.
[0078] An intermediate transfer belt 7, which is an endless belt serving as an intermediate transfer body, is disposed so as to face the four photosensitive drums 1. The intermediate transfer belt 7 is stretched around a drive roller 71, a tension roller 72, and a secondary transfer opposing roller 73 serving as multiple tension rollers, and is stretched with a predetermined tension. When the drive roller 71 is driven to rotate, the intermediate transfer belt 7 comes into contact with the photosensitive drums 1 and rotates (moves in a circular motion) in the direction of arrow R2 in the figure (clockwise). On the inner circumferential surface side of the intermediate transfer belt 7, primary transfer rollers 5, which are roller-shaped primary transfer members serving as primary transfer means, are disposed corresponding to the respective photosensitive drums 1.
[0079] The primary transfer roller 5 is pressed against the photosensitive drum 1 via the intermediate transfer belt 7 to form a primary transfer portion (primary transfer nip) T1 where the photosensitive drum 1 and the intermediate transfer belt 7 come into contact with each other. The toner image formed on the photosensitive drum 1 as described above is primarily transferred onto the rotating intermediate transfer belt 7 at the primary transfer portion T1 by the action of the primary transfer roller 5.
[0080] During the primary transfer process, a primary transfer bias (primary transfer voltage), which is a DC voltage of the opposite polarity (positive polarity in this embodiment) to the normal charging polarity of the toner (charging polarity during the development process), is applied to the primary transfer roller 5. The primary transfer roller 5 is composed of a metallic rotating shaft and an elastic layer formed on the outer circumferential surface of the rotating shaft, and is often adjusted to a desired resistance value. However, in recent years, with the miniaturization and cost reduction of devices, an increasing number of devices are composed of a metal roller that is made of material such as SUM (sulfur and sulfur composite free-cutting steel) or SUS (stainless steel) and has a straight shape in the thrust direction.
[0081] In such primary transfer, a transfer voltage of several kV is usually applied to ensure a sufficient transfer rate, and at that time, discharge may occur near the transfer nip. This discharge is one of the causes of deterioration of the surface characteristics of the intermediate transfer body. When the primary transfer roller is made of a metal roller, the transfer nip is narrower than in a primary transfer roller having an elastic layer, and discharge is more likely to occur. Therefore, the effect of the electrophotographic belt according to the present disclosure is more pronounced in an apparatus in which the primary transfer roller 5 is made of a metal roller.
[0082] On the outer peripheral surface side of the intermediate transfer belt 7, at a position facing the secondary transfer opposing roller 73 A secondary transfer roller 8, which is a roller-shaped secondary transfer member serving as a secondary transfer means, is disposed on the intermediate transfer belt 7. The secondary transfer roller 8 is pressed against the secondary transfer opposing roller 73 via the intermediate transfer belt 7, forming a secondary transfer portion (secondary transfer nip) T2 where the intermediate transfer belt 7 and the secondary transfer roller 8 come into contact with each other. The toner image formed on the intermediate transfer belt 7 as described above is secondarily transferred, by the action of the secondary transfer roller 8, at the secondary transfer portion T2 onto a recording material (sheet, transfer material) S such as paper (paper) being conveyed while being sandwiched between the intermediate transfer belt 7 and the secondary transfer roller 8.
[0083] During the secondary transfer process, a secondary transfer bias (secondary transfer voltage), which is a DC voltage of the opposite polarity to the normal charging polarity of the toner, is applied to the secondary transfer roller 8. In the secondary transfer, a transfer voltage of several kV is usually applied to ensure sufficient transfer efficiency. Similarly, the above image forming operation is performed in each of the units Pm, Pc, and Pk of magenta (M), cyan (C), and black (K) as the intermediate transfer belt 7 moves, and four toner images of yellow, magenta, cyan, and black are layered on the intermediate transfer belt 7.
[0084] The four color toner layers are transported by the movement of the intermediate transfer belt 7, and at the secondary transfer section T2, they are transferred collectively by a secondary transfer roller 8 as a secondary transfer means onto a recording medium S (hereinafter also referred to as a "second image carrier") that is transported at a predetermined timing. In such secondary transfer, a transfer voltage of several kV is usually applied to ensure a sufficient transfer rate, and at that time, discharge may occur near the transfer nip. This discharge is one of the causes of the decrease in the electrical resistance value of the intermediate transfer belt.
[0085] The recording material S is supplied from a cassette 12 storing the recording material S to a conveying path by a pickup roller 13. The recording material S supplied to the conveying path is conveyed to a secondary transfer portion T2 by a conveying roller pair 14 and a registration roller pair 15 in synchronization with the toner image on the intermediate transfer belt 7.
[0086] The recording material S onto which the toner image has been transferred is transported to a fixing device 9 as a fixing means. The fixing device 9 heats and presses the recording material S carrying the unfixed toner image with fixing members 91 and 92, thereby fixing (melting and bonding) the toner image onto the recording material S. The recording material S onto which the toner image has been fixed is discharged (output) to the outside of the main body of the image forming apparatus 100 by a pair of transport rollers 16, a pair of discharge rollers 17, etc.
[0087] Toner (primary transfer residual toner) remaining on the surface of the photosensitive drum 1 without being transferred to the intermediate transfer belt 7 in the primary transfer process is developed and collected by the developing device 4, which also serves as a photosensitive body cleaning means. Toner (secondary transfer residual toner) remaining on the surface of the intermediate transfer belt 7 without being transferred to the recording material S in the secondary transfer process is removed from the surface of the intermediate transfer belt 7 and collected by a belt cleaning device 11 serving as an intermediate transfer belt cleaning means. The belt cleaning device 11 is disposed downstream of the secondary transfer portion T2 and upstream of the most upstream primary transfer portion T1y in the rotation direction of the intermediate transfer belt 7 (at a position facing the drive roller 71 in this embodiment). The belt cleaning device 11 scrapes off the secondary transfer residual toner from the surface of the rotating intermediate transfer belt 7 by a cleaning blade serving as a cleaning member disposed so as to come into contact with the surface of the intermediate transfer belt 7, and stores it in a collection container 11b.
[0088] In this manner, in the image forming operation, the process of electrically transferring the toner image from the photosensitive drum 1 to the intermediate transfer belt 7 and from the intermediate transfer belt 7 to the recording material S is repeated. Furthermore, by repeating image formation on a large number of recording materials S, the electrical transfer process is further repeated.
[0089] By using the electrophotographic belt as an intermediate transfer belt in the electrophotographic image forming apparatus, it becomes possible to repeatedly form high-quality electrophotographic images for a long period of time.
[0090] Examples of the electrophotographic belt according to this embodiment are shown below. Note that, although the steps for producing the electrophotographic belt in this embodiment were all carried out using a common device, this embodiment is not limited to the following examples. EXAMPLES
[0091] The present disclosure will be specifically described below using examples. In the examples and comparative examples, the number of parts is based on mass unless otherwise specified.
[0092] As the conductive filler used in producing the intermediate transfer belts according to the examples and comparative examples, commercially available carbon black shown in Table 2 below was prepared, and the carbon black was subjected to the above-mentioned surface treatment or nitrogen treatment. The nitrogen treatment was carried out as follows: The carbon black to be treated was calcined (heat treated) in a nitrogen atmosphere at a temperature of 430° C. for 6 hours.
[0093] The surface treatment was carried out as follows. 10 parts by mass of a nonionic surfactant (polyoxyethylene alkyl ether) (manufactured by Sanyo Chemical Industries, Ltd., product name: "Naroacty") was added to 100 parts by mass of water, and after dissolving, 15 parts by mass of raw carbon black (manufactured by Mitsubishi Chemical Corporation, product name: "#3230B") was added. At this time, the ratio "A / B" was 1.5, where A is the part by mass of the raw carbon black and B is the part by mass of the surfactant, relative to 100 parts by mass of water. The mixture was stirred in a bead mill (product name: "Alpha Mill", manufactured by Imex Co., Ltd.) to obtain a raw carbon black dispersion. The raw carbon black dispersion was dehydrated using a spray dryer (product name: "Spray Dryer L-8i", manufactured by Yamato Scientific Co., Ltd.) to obtain a solid content. The obtained solid content was baked at a temperature of 400°C for 5 hours in a high-temperature furnace (product name: "Constant Temperature Dryer DR200", manufactured by Yamato Scientific Co., Ltd.).
[0094] The physical properties of the treated carbon black (DBP absorption amount, number average particle size of primary particles, BET specific surface area, CB water content, and CB water absorption amount) are shown in Table 2.
[0095] DBP absorption: DBP (dibutyl phthalate) is dropped onto 100g of carbon black while stirring, and the amount of dibutyl phthalate added at the point where the torque reaches its maximum can be calculated (Japanese Industrial Standards (JIS) K6217-4:2017). The measurement device used was an absorption meter (S-500, Asahi Research Institute).
[0096] Primary particle size: Carbon black usually exists as multiple primary particles that are connected three-dimensionally like a bunch of grapes. The number-average particle size of the primary particles (hereinafter also referred to as primary particle size) refers to the number-average particle size of the smallest unit of carbon black (primary particle) that forms one pigment particle. The primary particle size of the carbon black was determined by observing the cross section of the base layer. The measurement was performed using a transmission electron microscope (TEM). Although an ion beam, a diamond knife, or the like can be used to prepare a thin section sample prior to observation, in this disclosure, an "ULTRACUT-S" (trade name, manufactured by Leica) was used to obtain a cut specimen sample for observation with a thickness of 40 nm, which shows the cross section of the base layer in the full thickness direction. Then, a TEM image was obtained using a transmission electron microscope (TEM) (product name: H-7100FA, manufactured by Hitachi, Ltd.) under measurement conditions of TE mode and an accelerating voltage of 100 kV. For the analysis, known image analysis software such as "WinROOF" (product name, manufactured by Mitani Shoji Co., Ltd.) and "ImagePro" (product name, manufactured by Nippon Roper Co., Ltd.) can be used. In the present disclosure, "WinROOF" was used. Then, the area equivalent diameter of 50 primary particles of carbon black was measured, and the average value was taken as the number average particle diameter of the primary particles.
[0097] BET specific surface area: Degassed carbon black is immersed in liquid nitrogen, and the amount of nitrogen adsorbed on the particle surface of the carbon black when equilibrium is reached can be calculated (Japanese Industrial Standard (JIS) K6217-2:2017). Specifically, the measurement was performed using a fully automatic specific surface area measuring device (Macsorb, Mountec Co., Ltd.). The measurement was performed under pre-degassing conditions of 150°C x 3 minutes. [Table 2]
[0098] Example 1 <Production of Electrophotographic Belt> <Pre-mix> PEEK (product name: 381G, manufactured by Victrex) and the treated carbon black shown in Table 2 were weighed out to the blending ratio shown in Table 3, and mixed using a Henschel mixer (Nippon Coke and Engineering Co., Ltd., FM-150L / I). The operating conditions and treatment conditions of the Henschel mixer were as follows: blade rotation speed 1500 rpm, treatment amount 30 kg, treatment time 5 minutes, and treatment temperature 50°C.
[0099] <Melt mixing> The mixture obtained by the above premixing was fed into a twin-screw kneader (Ikegai Corp., PCM43) and melt-kneaded under conditions of an extrusion rate of 6 kg / h, a screw rotation speed of 100 rpm, and a barrel control temperature of 360° C. to obtain a resin composition. During kneading, degassing was performed under reduced pressure from a vent hole on the upstream side to remove vaporized materials.
[0100] <Melt extrusion> The resin composition obtained through the above melt-kneading process was pelletized, and the pellets were then extruded using a single-screw extruder (Plastic Engineering Research Institute Co., Ltd.) equipped with a spiral cylindrical die at the tip at an extrusion rate of 6 kg / h and a die temperature of 380° C. to obtain an endless electrophotographic belt made of a cylindrical film base layer having a thickness of 60 μm.
[0101] <Evaluation of electrophotographic belts> The electrophotographic belt thus produced was left for 48 hours in an environment of a temperature of 23° C. and a relative humidity of 50%, and then various evaluations were carried out.
[0102] (Evaluation 1: Measurement of crystallization temperature under cooling) The peak temperature detected in the process of cooling from a molten state in a differential scanning calorimeter (DSC) is the cooling crystallization temperature. The peak temperature is the temperature that appears when the temperature is set at 400°C, raised to 400°C at 10°C / min, and then lowered to room temperature (25°C) at 10°C / min. The measurement was performed using a differential scanning calorimeter (DSC Q2000, TA Instruments, Inc.) The samples were cut out at three points from the center of the base layer in the direction perpendicular to the circumferential direction of the electrophotographic belt, and the arithmetic average of the measured values was used.
[0103] (Evaluation 2: Calculation of the moisture content of the base layer) A sample was cut out from the base layer of the electrophotographic belt thus produced, and the moisture content of the base layer was measured. In this example, the measurement was carried out using a thermogravimetric analyzer (Q500 manufactured by TA Instruments). A plurality of samples of 4 mm×4 mm cut out from the base layer of the electrophotographic belt were loaded into a platinum sample pan having a capacity of 100 μL so that the total mass was 15 mg±4 mg. The mass of the sample was determined as X1 when the sample was heated from 30° C. to 100° C. at a rate of 20° C. per minute in a nitrogen atmosphere and held at 100° C. for 30 minutes. The sample was then cooled from 100° C. to 30° C. at a rate of 20° C. per minute and then placed in an air environment at a temperature of 23° C. and a relative humidity of 50% for 48 hours. The mass of the sample was determined as X2. Then, the moisture content of the base layer was calculated using the formula: Moisture content of base layer = ((X2 - X1) / X2) x 100. As a result, the moisture content of the base layer according to this example was 0.72 mass%.
[0104] (Rating 3: Mechanical strength, bending resistance) A part of the electrophotographic belt was cut out, and a bending resistance test was performed to measure mechanical strength. In the present disclosure, the MIT test specified in the Japanese Industrial Standards (JIS) P8115:2001 was applied as a folding endurance test (flexural fatigue test), and the bending radius R was changed to 2.5 mm, and the number of times until breakage was evaluated as the bending strength as follows. Rank "A": No breakage even after more than 1 million cycles Rank "B": Broken after 100,000 to less than 1,000,000 cycles Rank "C": Broken after 10,000 to 100,000 cycles Rank "D": Broken in less than 10,000 times The electrophotographic belt evaluated in this example did not break even after 1,000,000 cycles or more, and was given a mechanical strength rank of "A."
[0105] (Evaluation 4: Measurement of surface resistivity) The electrical resistance value of the electrophotographic belt was measured. The electrical resistance was measured using a Hiresta manufactured by Mitsubishi Chemical Corporation at 40 points in total, 5 points in the width direction and 8 points in the circumferential direction, under the condition that the surface resistivity was measured after 10 seconds with an applied voltage of 100 V. The surface resistivity of the obtained electrophotographic belt was 3.00×10 10 It was Ω / □.
[0106] (Rating 5: Image rating) The prepared electrophotographic belt was attached as an intermediate transfer belt to an intermediate transfer unit of a copying machine (manufactured by Canon Inc., product name: "IR-ADVANCE C5051"), and an image quality test was carried out. The printing test was carried out in an environment of a temperature of 15°C and a relative humidity of 10%, using A4 size paper (manufactured by Canon Inc., product name: "GF-600" (basis weight 60 g / m 2 )) was used to print 600,000 full-color images and conduct a paper feed durability test. After the paper feed durability test, 20 magenta solid images were output to check the printed images on the entire peripheral surface of the intermediate transfer belt. The 20 output images were visually checked for the presence or absence of density unevenness, which is a defect in image quality, and were evaluated according to the following criteria. Rank "A": No image defects were observed in any printed images. Rank "B": Image defects are observed in 1 to 3 printed images. Rank "C": Image defects are observed in four or more printed images. In this embodiment, no image defects were observed in the printed images after the paper feed durability test, and the image quality was therefore rated as "A."
[0107] (resistance decrease) In addition, after printing 600,000 sheets, the surface resistivity of the electrophotographic belt was measured under the same conditions as before the paper feed durability test. The amount of resistance change before and after the durability test was calculated from the initial resistance value (electrical resistance value before the paper feed durability test) and the electrical resistance value after the paper feed durability test. The Δ digits were calculated using the following formula. Here, the initial resistance value is ρ0, and the resistance after durability is ρ. Δdigit=Log(ρ0)-Log(ρ) ···(3) The surface resistivity of the electrophotographic belt of Example 1 after the paper feed durability test was 2.74×10 10 The resistivity before and after the durability test was in the order of 0.03.
[0108] [Examples 2 to 3, Comparative Examples 1 to 4] Using the material configurations and compounding ratios shown in Table 3 below, electrophotographic belts of Examples 2 to 3 and Comparative Examples 1 to 4 were produced by the same production method as in Example 1. The obtained electrophotographic belts were subjected to various evaluations by the same methods as in Example 1.
[0109] Example 2 An electrophotographic belt was produced in the same manner as in Example 1, except that the compounding ratio of PEEK and carbon black (CB) was adjusted as shown in Table 3.
[0110] Example 3 An electrophotographic belt was produced in the same manner as in Example 1, except that the compounding ratio of PEEK and carbon black (CB) was adjusted as shown in Table 3.
[0111] Comparative Example 1 An electrophotographic belt was produced in the same manner as in Example 1, except that the type of carbon black was selected and the compounding ratio was adjusted as shown in Table 3.
[0112] Comparative Example 2 An electrophotographic belt was produced in the same manner as in Example 1, except that the type of carbon black was selected and the compounding ratio was adjusted as shown in Table 3.
[0113] Comparative Example 3 An electrophotographic belt was produced in the same manner as in Example 1, except that the type of carbon black was selected and the compounding ratio was adjusted as shown in Table 3.
[0114] Comparative Example 4 An electrophotographic belt was produced in the same manner as in Example 1, except that the type of carbon black was selected and the compounding ratio was adjusted as shown in Table 3. Table 3 shows the evaluation results of the electrophotographic belts produced in Examples 1 and 2 and Comparative Examples 1 to 4.
[0115] In Example 1, the image evaluation after the paper feed durability test gave good results. The change in resistance value before and after the paper feed durability test was also small, and it is believed that the change in resistance value was unlikely to occur due to discharge occurring in the gap between the inner circumferential surface of the intermediate transfer body and the primary transfer roller in the primary transfer section, or between the outer circumferential surface of the intermediate transfer body and the paper in the secondary transfer section. As a result, it is believed that no image defects occurred even after the paper feed durability test. Furthermore, even when the amount of carbon black was increased in Example 2, no decrease in crack resistance was observed. In Example 3, even though the amount of carbon black was small, no decrease in resistance due to the moisture content of the belt was observed.
[0116] In the electrophotographic belt according to Comparative Example 1, a decrease in crack resistance was confirmed due to a high crystallization temperature upon cooling. It is considered that the carbon black used in Comparative Example 1 has a small BET specific surface area due to a small number of fine protrusions on the surface, which resulted in a high crystallization temperature upon cooling. Also in the electrophotographic belt according to Comparative Example 2, the temperature-reducing crystallization temperature was high, and therefore the crack resistance was confirmed to be reduced.
[0117] The electrophotographic belt according to Comparative Example 3 also had a high crystallization temperature under reduced temperature, and thus the crack resistance was reduced. In Comparative Example 3, the moisture content of the base layer was low, and therefore the electrical conductivity changed over time, causing image defects. In the electrophotographic belt according to Comparative Example 4, the moisture content of the base layer was low, so that the conductivity changed significantly over time, and image defects occurred. The electrophotographic belt according to Comparative Example 4 had a high crystallization temperature on cooling of the base layer, but was excellent in mechanical strength. This is believed to be because the content of carbon black in the base layer was low. The high crystallization temperature on cooling of the base layer of the electrophotographic belt according to Comparative Example 4 is believed to be due to the use of acetylene black, which is likely to become a crystal nucleus of PEEK, as the carbon black.
[0118] [Table 3] The number of flexes indicates the number of flexes at which the electrophotographic belt breaks. "1 million or more flexes" indicates that the belt did not break even after flexing 1 million times.
[0119] As described above, by increasing the moisture content of the base layer of the electrophotographic belt, the decrease in resistance can be suppressed, and by lowering the crystallization temperature during cooling, the crack resistance can be improved. This makes it possible to obtain an electrophotographic belt that can achieve both suppression of the decrease in electrical resistance and crack resistance even after long-term use.
[0120] The present disclosure relates to the following configurations. (Configuration 1) 1. An electrophotographic belt, comprising: The electrophotographic belt has at least a base layer, The base layer contains polyether ether ketone, which is a thermoplastic resin, and carbon black, The content of the carbon black is 18 to 30% by mass based on the mass of the base layer, A sample cut out from the base layer is heated in a nitrogen atmosphere from 30°C to 100°C at a rate of 20°C per minute and held at 100°C for 30 minutes; the mass of the sample is defined as X1; the sample is then cooled from 100°C to 30°C at a rate of 20°C per minute and placed in an air environment at a temperature of 23°C and a relative humidity of 50% for 48 hours; the mass of the sample is defined as X2. The moisture content of the base layer calculated by the moisture content of the base layer = ((X2-X1) / X2) × 100 is 0.50 mass% or more, 1 is a schematic diagram showing a crystallization temperature of the base layer measured by differential scanning calorimetry; (Configuration 2) 2. The electrophotographic belt according to claim 1, wherein the content of the carbon black is 19 to 30% by mass based on the mass of the base layer. (Configuration 3) 3. The electrophotographic belt according to claim 1, wherein the carbon black has a number-average particle size of primary particles of 15 nm or more and less than 35 nm. (Configuration 4) The electrophotographic belt according to any one of configurations 1 to 3, wherein the carbon black has a moisture absorption rate of 0.70% by mass or more, calculated by the following formula (1): The carbon black is left for 48 hours under conditions of a temperature of 23°C and a relative humidity of 50%, and its mass is measured using a thermogravimetric analyzer and designated as W0. The carbon black after W0 measurement is then heated from 30°C to 120°C at a rate of 20°C per minute in a nitrogen atmosphere and held at 120°C for 15 minutes, and its mass is similarly measured using a thermogravimetric analyzer and designated as W1. Water absorption rate = [(W0 - W1) / W0] × 100 (1). (Configuration 5) The BET specific surface area of the carbon black is 240 m 2 5. The electrophotographic belt according to any one of configurations 1 to 4, wherein the surface area of the electrophotographic belt is 0.1 μm or more. (Configuration 6) 6. The electrophotographic belt according to any one of configurations 1 to 5, wherein the carbon black comprises furnace black. (Configuration 7) 7. The electrophotographic belt according to any one of configurations 1 to 6, wherein the carbon black has protrusions on the surface thereof derived from an organic compound. (Configuration 8) 8. The electrophotographic belt according to any one of claims 1 to 7, wherein the moisture content of the base layer is 0.70 to 1.00% by mass. (Configuration 9) The surface resistivity of the base layer is 1.0×10 3 Ω / □ or more, 1.0×10 14 9. The electrophotographic belt according to any one of configurations 1 to 8, having a surface roughness of Ω / □ or less. (Configuration 10) 10. The electrophotographic belt according to any one of claims 1 to 9, wherein the thickness of the base layer is 25 to 100 μm. (Configuration 11) 11. The electrophotographic belt according to any one of configurations 1 to 10, wherein the electrophotographic belt is an intermediate transfer belt. (Configuration 12) 12. An electrophotographic image forming apparatus comprising the electrophotographic belt according to any one of configurations 1 to 11. (Configuration 13) 13. The electrophotographic image forming apparatus according to claim 12, further comprising the electrophotographic belt as an intermediate transfer belt. [Explanation of symbols]
[0121] 1 photosensitive drum, 2 primary charging device, 3 exposure device, 4 developing device, 5 primary transfer roller, 7 intermediate transfer belt, 8 secondary transfer roller (secondary transfer outer roller), 9 fixing device, 12 cassette, 13 pickup roller, 15 registration roller, 71 intermediate transfer belt tension roller (drive roller), 72 intermediate transfer belt tension roller (tension roller), 73 intermediate transfer belt tension roller (secondary transfer opposing roller)
Claims
1. 1. An electrophotographic belt, comprising: The electrophotographic belt has at least a base layer, The base layer contains polyether ether ketone, which is a thermoplastic resin, and carbon black, The content of the carbon black is 18 to 30% by mass based on the mass of the base layer, A sample cut out from the base layer is heated in a nitrogen atmosphere from 30° C. to 100° C. at a rate of 20° C. per minute and held at 100° C. for 30 minutes; the mass of the sample is defined as X1; the sample is then cooled from 100° C. to 30° C. at a rate of 20° C. per minute and then placed in an air environment at a temperature of 23° C. and a relative humidity of 50% for 48 hours; the mass of the sample is defined as X2. The moisture content of the base layer, calculated by the formula: moisture content of the base layer = ((X2 - X1) / X2) x 100, is 0.50 mass% or more, The electrophotographic belt according to claim 1, wherein the base layer has a crystallization temperature upon cooling measured by differential scanning calorimetry of 288.0° C. or less.
2. 2. The electrophotographic belt according to claim 1, wherein the content of said carbon black is 19 to 30% by weight based on the weight of said base layer.
3. 2. The electrophotographic belt according to claim 1, wherein the number average particle size of the primary particles of said carbon black is 15 nm or more and less than 35 nm.
4. 2. The electrophotographic belt according to claim 1, wherein the carbon black has a moisture absorption rate of 0.70% by mass or more, calculated by the following formula (1): The carbon black is left for 48 hours under conditions of a temperature of 23° C. and a relative humidity of 50%, and the mass thereof is measured using a thermogravimetric analyzer and designated as W0. The carbon black after W0 measurement is then heated from 30° C. to 120° C. at a rate of 20° C. per minute in a nitrogen atmosphere and held at 120° C. for 15 minutes, and the mass thereof is similarly measured using a thermogravimetric analyzer and designated as W1. Moisture absorption rate = [(W0 - W1) / W0] x 100 ... (1).
5. The BET specific surface area of the carbon black is 240 m 2 2. The electrophotographic belt of claim 1, wherein the surface roughness is 1 / g or more.
6. 2. An electrophotographic belt as in claim 1 wherein said carbon black comprises furnace black.
7. 2. An electrophotographic belt according to claim 1, wherein said carbon black has protrusions on the surface thereof derived from an organic compound.
8. 2. The electrophotographic belt according to claim 1, wherein the moisture content of the base layer is from 0.70 to 1.00% by weight.
9. The surface resistivity of the base layer is 1.0×10 3 Ω / □ or more, 1.0×10 14 2. The electrophotographic belt of claim 1, wherein the surface roughness is Ω / □ or less.
10. 2. The electrophotographic belt according to claim 1, wherein the thickness of said base layer is from 25 to 100 μm.
11. 2. The electrophotographic belt of claim 1, wherein the electrophotographic belt is an intermediate transfer belt.
12. 12. An electrophotographic image forming apparatus comprising the electrophotographic belt according to claim 1.
13. 13. The electrophotographic image forming apparatus of claim 12, wherein the electrophotographic belt is provided as an intermediate transfer belt.
Citation Information
Patent Citations
Method for evaluating temporal stability of electric resistance of electrophotographic belt
JP2012177811A
Sheet-like member for image forming apparatus
JP2021009400A