Polycarbonate polyol copolymer

A polycarbonate polyol copolymer with a specific structure addresses the balance of heat, weather, and hydrolysis resistance issues in polyurethane materials, ensuring flexibility and chemical resistance, suitable for applications like synthetic leather and coatings.

JP2024152649APending Publication Date: 2024-10-25ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024059235
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-12
Filing Date
2024-04-01
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing polyurethane materials, such as those using polyether, polyester, and polycarbonate polyols, fail to provide an optimal balance of heat resistance, weather resistance, hydrolysis resistance, flexibility, and chemical resistance, particularly when used in applications requiring high durability and resistance to crystallization at room temperature.

Method used

A polycarbonate polyol copolymer is developed with a specific structure, containing a polycarbonate polyol component and a dimer diol component, which includes a repeating unit represented by a certain formula, ensuring at least 50 mol% of these units are present, and a carbonate group content of 17 to 38% by mass, with a number average molecular weight of 500 to 3000 g/mol, resulting in a transparent, flexible, and chemically resistant material.

Benefits of technology

The polycarbonate polyol copolymer maintains flexibility and resistance to crystallization at room temperature, offering excellent abrasion resistance, low-temperature properties, and hydrolysis resistance, making it suitable for applications like synthetic leather and coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152649000001
    Figure 2024152649000001
  • Figure 2024152649000002
    Figure 2024152649000002
  • Figure 2024152649000003
    Figure 2024152649000003
Patent Text Reader

Abstract

To provide a polycarbonate polyol copolymer which causes neither white turbidity nor solidification even when left at a normal temperature (23°C) and has excellent balance of physical properties such as flexibility (touch feeling), oleic acid resistance (chemical resistance), abrasion resistance, low temperature properties and hydrolysis resistance when formed into a polyurethane.SOLUTION: There is provided a polycarbonate polyol copolymer (A) which comprises a polycarbonate polyol component (a1) containing a repeating unit represented by a formula (1) and a dimer diol component (a2), wherein the repeating unit represented by the formula (1) satisfies a specific condition, a content of the component (a1) is 10 mass% or more and 90 mass% or less and a content of the component (a2) is 10 mass% or more and 90 mass% or less, based on 100 mass% of total mass of the component (a1) and the component (a2).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polycarbonate polyol copolymer. [Background technology]

[0002] Conventionally, polyurethane has been used in a wide range of applications, such as synthetic leather, artificial leather, adhesives, furniture paints, and automotive paints. Among the raw materials for polyurethane, polyether, polyester, and polycarbonate are used as polyol components to react with isocyanates. However, in recent years, there has been an increasing demand for polyurethane resistance, such as heat resistance, weather resistance, hydrolysis resistance, solvent resistance, sunscreen resistance, and scratch resistance.

[0003] In general, polyurethanes using polyether polyols are considered to have excellent flexibility and hydrolysis resistance, but poor heat resistance and weather resistance, while polyurethanes using polyester polyols have improved heat resistance and weather resistance, but poor hydrolysis resistance.

[0004] In contrast, polyurethane using polycarbonate polyol is considered to be the best durable grade in terms of durability such as heat resistance, chemical resistance, and hydrolysis resistance.

[0005] For example, Patent Document 1 discloses an economical and simple method for producing a copolymeric polycarbonate diol. Also, for example, Patent Document 2 discloses a polycarbonate diol / polyether block copolymer.

[0006] For example, Patent Document 3 discloses a method for obtaining a polyester polyol by esterifying a diol with a dicarboxylic acid, in which a dimer acid is hydrogenated to obtain a hydrogenated dimer acid and a diol such as 1,4-cyclohexanedimethanol are used. For example, Patent Documents 4, 5, and 6 disclose polyester polyols having a dimer diol skeleton obtained by reducing a dimer acid with hydrogen to synthesize a dimer diol having 36 carbon atoms, and then reacting the diol with a dibasic acid.

[0007] For example, Patent Document 7 discloses a method for producing a polycarbonate diol from a dimer diol, which comprises transesterifying a dimer diol with a polycarbonate compound in the presence of a transesterification catalyst at a temperature of 110 to 280° C. under normal pressure while distilling off by-produced alcohols or phenols. For example, Patent Document 8 discloses a method for producing a copolymer of a polycarbonate diol and a dimer diol by transesterifying a polycarbonate diol from a dimer diol with an aliphatic polycarbonate diol consisting of an alkyl group or a cycloalkyl group. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 3-252420 [Patent Document 2] JP 2006-124486 A [Patent Document 3] Japanese Patent Application Publication No. 4-145118 [Patent Document 4] Japanese Patent Application Publication No. 3-277680 [Patent Document 5] Japanese Patent Application Publication No. 4-130124 [Patent Document 6] Japanese Patent Application Publication No. 6-128363 [Patent Document 7] Japanese Patent Application Publication No. 10-231360 [Patent Document 8] Japanese Patent Application Publication No. 10-251398 Summary of the Invention [Problem to be solved by the invention]

[0009] However, the polyether copolymerized polycarbonate diols disclosed in Patent Documents 1 and 2 have insufficient heat resistance and weather resistance when used in applications requiring high durability. In addition, the polyether copolymerized polycarbonate diols disclosed in Patent Document 3 have insufficient flexibility and low-temperature properties. In addition, the polyester polyols having a dimer diol skeleton described in Patent Documents 4, 5, and 6 have problems with hydrolysis resistance, and their use is limited in applications requiring high durability.

[0010] The polycarbonate diol of dimer diol disclosed in Patent Document 7 has a problem that the flexibility of the obtained polyurethane is poor because the distance between the hydroxyl group terminals of the dimer diol is short, and the resistance of the obtained polyurethane to oleic acid is poor, so that the use of the polycarbonate diol in paints and coating agents is limited.

[0011] Specifically, Patent Document 8 discloses a method for obtaining a dimer diol copolymer carbonate diol by transesterification using, for example, 1,6-hexanediol type polycarbonate diol and dimer diol. Also, for example, a method for obtaining a dimer diol copolymer carbonate diol using 1,4-butanediol type polycarbonate diol or 1,4-cyclohexanedimethanol type polycarbonate diol instead of 1,6-hexanediol type polycarbonate diol is disclosed. Among these, 1,6-hexanediol type polycarbonate diol and dimer diol copolymer carbonate diol using 1,4-butanediol type polycarbonate diol crystallize due to the crystallinity of the carbonate skeleton when left at room temperature for a long time, causing clouding and solidification, so it is necessary to heat it before use. In addition, dimer diol copolymer carbonate diols using 1,6-hexanediol type polycarbonate diol and 1,4-butanediol type polycarbonate diol have problems in that the polyurethane obtained becomes cloudy and hardens over time due to their crystallinity. On the other hand, dimer diol copolymer carbonate diols using 1,4-cyclohexanedimethanol type polycarbonate diol have a problem in that the polyurethane obtained does not have sufficient flexibility due to its rigid structure.

[0012] In view of the above circumstances, the present invention has an object to provide a polycarbonate polyol copolymer which does not become cloudy or solidify even when left at room temperature (23°C) and which, when made into polyurethane, has an excellent balance of physical properties such as flexibility (touch), oleic acid resistance (chemical resistance), abrasion resistance, low-temperature properties, and hydrolysis resistance. [Means for solving the problem]

[0013] As a result of intensive research, the present inventors have found that by forming a polycarbonate polyol copolymer having a specific structure, the copolymer does not become cloudy or solidify even when left at room temperature (23°C), and when made into a polyurethane, the copolymer has an excellent balance of physical properties such as flexibility (touch), oleic acid resistance (chemical resistance), abrasion resistance, low-temperature properties, and hydrolysis resistance, and have thus completed the present invention.

[0014] That is, the present invention includes the following aspects. [1] A polycarbonate polyol copolymer (A) containing, as copolymerization components, a polycarbonate polyol component (a1) containing a repeating unit represented by the following formula (1) and a dimer diol component (a2), 50 mol % or more of the repeating units represented by the following formula (1) contain at least two kinds of repeating units selected from the group consisting of repeating units represented by the following formula (2), repeating units represented by the following formula (3), and repeating units represented by the following formula (4), or the repeating units represented by the following formula (1) are repeating units represented by the following formula (5): A polycarbonate polyol copolymer (A), in which the content of the polycarbonate polyol component (a1) is 10% by mass or more and 90% by mass or less, and the content of the dimer diol component (a2) is 10% by mass or more and 90% by mass or less, relative to 100% by mass of the total mass of the polycarbonate polyol component (a1) and the dimer diol component (a2). [ka] (In formula (1), R1 is a divalent aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.) [ka] [ka] [ka] [ka] [2] The polycarbonate polyol copolymer (A) according to [1], wherein 50 mol % or more of the repeating units represented by the formula (1) contain at least two kinds of repeating units selected from the group consisting of repeating units represented by the formula (2), repeating units represented by the formula (3), and repeating units represented by the formula (4). [3] The polycarbonate polyol copolymer (A) according to [2], wherein the content of carbonate groups contained in one molecule is 17 to 38 mass % and the number average molecular weight is 500 to 3000 g / mol. [4] The polycarbonate polyol copolymer (A) according to [2] or [3], which has a glass transition temperature of −50° C. or lower as measured by a differential scanning calorimeter. [5] The polycarbonate polyol copolymer (A) according to any one of [2] to [4], which has a water absorption rate of 0.8 mass% or less after 7 days in an atmosphere having a temperature of 85° C. and a relative humidity of 85%. [6] The polycarbonate polyol copolymer (A) according to any one of [2] to [5], which has a biomass degree of 10% or more and 90% or less as measured by accelerator mass spectrometry. [7] The polycarbonate polyol copolymer (A) according to any one of [2] to [6], which is liquid and transparent at 23°C. [8] A polyurethane obtained by using the polycarbonate polyol copolymer (A) according to any one of [2] to [7]. [9] The polyurethane according to [8], having a swelling degree of 5% by mass or more and 35% by mass or less after immersion in oleic acid at 23° C. for 7 days.

[10] [8] or [9]. A water-based polyurethane dispersion, in which the polyurethane according to [8] or [9] is dispersed in water.

[11] [8] or [9]. Synthetic leather comprising the polyurethane.

[12] A method for producing a polycarbonate polyol copolymer (A), comprising a step of polycondensing a dihydroxy compound, a dimer diol, and a carbonate ester as raw material monomers through an ester exchange reaction in the presence of an ester exchange catalyst to obtain a polycarbonate polyol copolymer (A).

[13] In the polycondensation step, With respect to 100% by mass of the total mass of the dihydroxy compound and the dimer diol, The dihydroxy compound is 10% by mass or more and 90% by mass or less, The dimer diol has a mass ratio of 10% by mass to 90% by mass. The present invention is characterized in that the ester exchange reaction is carried out. A method for producing the polycarbonate polyol copolymer (A) according to

[12] .

[14] The method for producing the polycarbonate polyol copolymer (A) according to

[12] or

[13] , wherein the transesterification catalyst comprises a transesterification catalyst A1 containing at least one metal (M1) selected from the group consisting of metals in Group 7 of the long form periodic table, and a transesterification catalyst A2 containing at least one metal (M2) selected from the group consisting of metals in Groups 1 and 2 of the long form periodic table.

[15] The method for producing a polycarbonate polyol copolymer (A) according to

[14] , wherein the metal (M1) is manganese, and the metal (M2) is at least one metal selected from the group consisting of lithium and calcium.

[16] The method for producing a polycarbonate polyol copolymer (A) according to any one of

[12] to

[15] , wherein the dihydroxy compound is 1,3-propanediol.

[17] The polycarbonate polyol copolymer (A) according to [1], wherein the repeating unit represented by the formula (1) is a repeating unit represented by the formula (5). [ka]

[18] The polycarbonate polyol copolymer (A) according to

[17] , wherein the content of carbonate groups contained in one molecule is 20 to 45 mass % and the number average molecular weight is 500 to 3000 g / mol.

[19] The polycarbonate polyol copolymer (A) according to

[17] or

[18] , which has a glass transition temperature of −40° C. or lower as measured by a differential scanning calorimeter.

[20] The polycarbonate polyol copolymer (A) according to any one of

[17] to

[19] , which has a water absorption rate of 1.0 mass% or less after 7 days in an atmosphere having a temperature of 85°C and a relative humidity of 85%. [twenty one] The polycarbonate polyol copolymer (A) according to any one of

[17] to

[20] , having a biomass degree of 70% or more and 95% or less as measured by accelerator mass spectrometry. [twenty two] The polycarbonate polyol copolymer (A) according to any one of

[17] to

[21] , which is liquid and transparent at 23°C. [twenty three] A polyurethane obtained by using the polycarbonate polyol copolymer (A) according to any one of

[17] to

[21] . [twenty four] The polyurethane according to

[23] , having a swelling degree of 5% by mass or more and 30% by mass or less after immersion in oleic acid at 23° C. for 7 days. [twenty five]

[23] or

[24] . An aqueous polyurethane dispersion, in which the polyurethane according to

[23] or

[24] is dispersed in water.

[26]

[23] or

[24] . Synthetic leather comprising the polyurethane according to

[23] or

[24] . Effect of the Invention

[0015] The polycarbonate polyol copolymer (A) of the present invention does not become cloudy or solidify even when left at room temperature (23° C.), and when made into a polyurethane, it can provide a polyurethane having an excellent balance of physical properties such as flexibility (touch), oleic acid resistance (chemical resistance), abrasion resistance, low-temperature properties, and hydrolysis resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an embodiment for carrying out the present invention (hereinafter, abbreviated as "present embodiment") will be described in detail. Note that the present invention is not limited to the following embodiment, and can be carried out in various modifications within the scope of the gist of the present invention.

[0017] The polycarbonate polyol copolymer (A) of the present embodiment contains, as copolymerization components, a polycarbonate polyol component (a1) containing a repeating unit represented by the following formula (1), and a dimer diol component (a2). [ka] (In formula (1), R1 is a divalent aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.)

[0018] In the polycarbonate polyol copolymer (A) of this embodiment, the content of the polycarbonate polyol component (a1) is 10% by mass or more and 90% by mass or less, based on 100% by mass of the total mass of the polycarbonate polyol component (a1) and the dimer diol component (a2), and the content of the dimer diol component (a2) is 10% by mass or more and 90% by mass or less, based on 100% by mass of the total mass of the polycarbonate polyol component (a1) and the dimer diol component (a2).

[0019] The polycarbonate polyol copolymer (A) of the present embodiment can be used as a polyurethane raw material, and by reacting it with an isocyanate, a chain extender, or the like, a polyurethane having an excellent balance of physical properties such as flexibility (touch), oleic acid resistance (chemical resistance), abrasion resistance, low-temperature properties, and hydrolysis resistance can be obtained. The polyurethane can be suitably used, for example, in synthetic leather, adhesives, coating agents, thermoplastic polyurethanes, and the like.

[0020] The polycarbonate polyol copolymer (A) of this embodiment contains a polycarbonate polyol component (a1) containing a repeating unit represented by the above formula (1), and a dimer diol component (a2).

[0021] [Polycarbonate polyol component (a1)] The polycarbonate polyol component (a1) contained in the polycarbonate polyol copolymer (A) of this embodiment contains a repeating unit represented by the following formula (1). [ka] (In formula (1), R1 is a divalent aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.)

[0022] The polycarbonate polyol component (a1) is not particularly limited, but can be synthesized, for example, by using a bifunctional diol compound, and optionally a trifunctional or higher polyhydric alcohol and a carbonate ester as raw materials, for example, by an ester exchange reaction as described in "Polymer Reviews, Vol. 9, pages 9-20" or the like.

[0023] The bifunctional diol compound used in the transesterification reaction is not particularly limited, but examples thereof include diols having a divalent aliphatic or alicyclic hydrocarbon skeleton having 2 to 15 carbon atoms. Specific examples of the bifunctional diol compound include, but are not particularly limited to, ethylene glycol, 1,3-propanediol, 2-methyl-1,3-propanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 2-methyl-1,8-octanediol, 1,11-undecanediol, 1,1 Examples of the diol include 2-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,15-pentadecanediol, 2-isopropyl-1,4-butanediol, 2-ethyl-1,6-hexanediol, 3-methyl-1,5-pentanediol, 2,4-dimethyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, and 1,4-cyclohexanedimethanol.

[0024] These difunctional diol compounds may be used alone or in combination of two or more.

[0025] Among these, from the viewpoint of obtaining a curable composition for synthetic leather excellent in flexibility (touch), chemical resistance, low-temperature properties and heat resistance, alkylene diols having 3 to 9 carbon atoms are preferred, and alkylene diols having 3 to 6 carbon atoms are more preferred.

[0026] The polycarbonate polyol copolymer (A) of the present embodiment contains at least two kinds of repeating units selected from the group consisting of repeating units represented by the following formula (1), repeating units represented by the following formula (2), repeating units represented by the following formula (3), and repeating units represented by the following formula (4), or the repeating units represented by the following formula (1) are repeating units represented by the following formula (5). [ka] (In formula (1), R1 is a divalent aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.) [ka] [ka] [ka] [ka]

[0027] [When 50 mol % or more of the repeating units represented by formula (1) contain at least two kinds of repeating units selected from the group consisting of repeating units represented by formulas (2) to (4)] In the polycarbonate polyol component (a1) contained in the polycarbonate polyol copolymer (A) of the present embodiment, it is preferable that 50 mol % or more of the repeating units represented by the above formula (1) contain at least two kinds of repeating units selected from the group consisting of repeating units represented by the following formula (2), repeating units represented by the following formula (3), and repeating units represented by the following formula (4). [ka] [ka] [ka]

[0028] In this embodiment, the polycarbonate polyol component (a1) is preferably synthesized by using two or more of 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol in combination, and optionally using a trifunctional or higher polyhydric alcohol and a carbonate ester as raw materials, for example, by an ester exchange reaction as described in "Polymer Reviews, Vol. 9, pages 9-20" or the like.

[0029] By using two or more of 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol in combination, the regularity of the structural unit of the polycarbonate component in the polycarbonate polyol copolymer is reduced, and the crystallinity is reduced, so that not only is a polycarbonate polyol copolymer (A) that is liquid at room temperature (23°C) obtained, but the flexibility of the polyurethane tends to be increased. In addition, when an organic solvent is used in the production of polyurethane, the amount of the organic solvent used tends to be reduced.

[0030] In this embodiment, of the repeating units represented by the above formula (1), preferably 50 mol % or more, more preferably 70 mol % or more, and even more preferably 80 mol % or more contain at least two types of repeating units selected from the group consisting of repeating units represented by the above formula (2), repeating units represented by the above formula (3), and repeating units represented by the above formula (4).

[0031] In addition to 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol, other diols that can be used as necessary include, but are not limited to, ethylene glycol, 1,3-propanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nanodiol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,14-tetradecanediol, and other diols having no side chains, 2-methyl-1,8-octanediol, 2-ethyl-1,8-octanediol, and the like. One or more diols can be used from diols having side chains such as 2-methyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2,4-dimethyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, and 2,2-dimethyl-1,3-propanediol, and cyclic diols such as 1,4-cyclohexanedimethanol and 2-bis(4-hydroxycyclohexyl)-propane.

[0032] When at least two types of repeating units selected from the group consisting of repeating units represented by formula (2), repeating units represented by formula (3), and repeating units represented by formula (4) account for 50 mol % or more of the repeating units represented by formula (1), the obtained polyurethane has excellent flexibility (feel), chemical resistance, low-temperature properties, and heat resistance, and when a solvent is used in producing the polyurethane, the amount of solvent used tends to be reduced.

[0033] In this embodiment, when two kinds of repeating units are selected from the group consisting of the repeating unit represented by the above formula (2), the repeating unit represented by the above formula (3), and the repeating unit represented by the above formula (4), the ratio of the two kinds of repeating units is 90:10 to 10:90, preferably 70:30 to 30:70, in terms of molar ratio. When the copolymerization ratio is within the above range, the crystallinity of the polycarbonate polyol copolymer (A) tends to decrease, and a polyurethane having high flexibility, good low-temperature properties, and good touch tends to be obtained. Furthermore, when the copolymerization ratio is within this range, when a solvent is used during polyurethane production, the amount of the solvent used tends to be reduced.

[0034] In this embodiment, when three kinds of repeating units are selected from the group consisting of the repeating unit represented by the formula (2), the repeating unit represented by the formula (3), and the repeating unit represented by the formula (4), the proportions of the repeating unit represented by the formula (2), the repeating unit represented by the formula (3), and the repeating unit represented by the formula (4) are preferably 5 mol% or more, more preferably 10 mol% or more, and even more preferably 20 mol% or more, when the total of these three kinds of repeating units is 100 mol%. When the proportions of each of these three kinds of repeating units in the total of the three kinds of repeating units, the repeating unit represented by the formula (2), the repeating unit represented by the formula (3), and the repeating unit represented by the formula (4), are within the above ranges, the crystallinity of the polycarbonate diol copolymer (A) tends to be reduced, and a polyurethane having high flexibility, good low-temperature properties, and good touch is obtained. Furthermore, when the proportions of the three types of repeating units, i.e., the repeating unit represented by the above formula (2), the repeating unit represented by the above formula (3), and the repeating unit represented by the above formula (4), are within the above ranges, there is a tendency that the amount of solvent used can be reduced when a solvent is used in producing the polyurethane.

[0035] [When the repeating unit represented by formula (1) is a repeating unit represented by formula (5)] In the polycarbonate polyol component (a1) contained in the polycarbonate polyol copolymer (A) of this embodiment, the repeating unit represented by the above formula (1) is preferably a repeating unit represented by the following formula (5). [ka]

[0036] In this embodiment, when the repeating unit represented by formula (1) is a repeating unit represented by formula (5), the polycarbonate polyol component (a1) can be synthesized by using 1,3-propanediol and, if necessary, a trifunctional or higher polyhydric alcohol and a carbonate ester as raw materials, for example, by the transesterification reaction described in "Polymer Reviews, Vol. 9, pages 9 to 20" or the like.

[0037] Surprisingly, by using 1,3-propanediol, the structure of the polycarbonate component in the polycarbonate polyol copolymer becomes amorphous, and a polycarbonate polyol copolymer (A) that is liquid at room temperature (23°C) is obtained. In addition, the flexibility of polyurethane using the polycarbonate polyol copolymer (A) of this embodiment tends to be increased. In addition, when an organic solvent is used during polyurethane production, the amount of the organic solvent used tends to be reduced.

[0038] Other diols that can be used as necessary other than 1,3-propanediol are not particularly limited, but examples thereof include diols having no side chains such as ethylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nanodiol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, and 1,14-tetradecanediol, 2-methyl-1,8-octanediol, and 2-ethyl-1,8-octanediol. One or more diols can be used from diols having side chains such as 2-methyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2,4-dimethyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, and 2,2-dimethyl-1,3-propanediol, and cyclic diols such as 1,4-cyclohexanedimethanol and 2-bis(4-hydroxycyclohexyl)-propane.

[0039] The 1,3-propanediol is not particularly limited, but for example, it is preferable to use plant-derived 1,3-propanediol because it can produce a polycarbonate polyol copolymer (A) with a high biomass content. The commercially available 1,3-propanediol is not particularly limited, but for example, it is available as Susterra (registered trademark) Propandiol manufactured by DuPont Specialty Products Co., Ltd.

[0040] [Dimer diol component (a2)] The component (a2) constituting the polycarbonate polyol copolymer (A) of the present embodiment is not particularly limited as long as it is a dimer diol. In general, dimer diol is a diol obtained by reducing dimer acid and / or its lower alcohol ester in the presence of a catalyst, and the diol is mainly composed of a carboxylic acid moiety of the dimer acid, which is converted to an alcohol. A dimer diol having 36 carbon atoms is well known as a commercially available product. Here, dimer acid is a dibasic acid obtained by intermolecular polymerization reaction of unsaturated fatty acids derived mainly from plants, and is obtained, for example, by dimerizing unsaturated fatty acids having 11 to 22 carbon atoms with a clay catalyst or the like. In addition to dibasic acids having about 36 carbon atoms, industrially obtained dimer acids also contain any amount of trimer acid and monomer acid depending on the degree of purification. Here, the main component means that it is present at 50% by mass or more, and it is known that, in addition to diols having 36 carbon atoms, diols having 22 to 44 carbon atoms but not 36 carbon atoms exist. In this specification, "dimer diol" is defined to include not only diols having 36 carbon atoms, which are made by converting the carboxylic acid moiety of dimer acid into alcohol, but also hydrogenated dimer diols obtained by hydrogenating the carbon-carbon double bonds derived from dimer acid. The dimer diol used in the present embodiment is particularly preferably a hydrogenated dimer diol obtained by hydrogenating the carbon-carbon double bond derived from a dimer acid.

[0041] Non-limiting structural formulae of dimer diol are shown below in formula (6) and formula (7). [ka] (In the formula, R 2 and R 3 are each independently an integer of 1 or more, and R 2 and R 3 The total number of carbon atoms contained in the formula (a) and (b) is 38 or less, and any bond between C and C in the formula may be replaced with a double bond. [ka] (In the formula, R 4 and R 5 are each independently an integer of 1 or more, and R 4 and R 5 The total number of carbon atoms contained in the formula (I) and the numbers of c and d is 42 or less, and any bond between C and C in the formula may be replaced with a double bond.

[0042] Commercially available dimer diols include, but are not limited to, Pripol (registered trademark) 2033 (manufactured by Croda), Pripol (registered trademark) 2030 (manufactured by Croda), Pripol (registered trademark) 2043 (manufactured by Croda), and Sovermol (registered trademark) 908 (manufactured by Cognis).

[0043] The content of the polycarbonate polyol component (a1) containing the structure represented by formula (1) in the polycarbonate polyol copolymer (A) of the present embodiment is, relative to the total mass of the polycarbonate polyol component (a1) containing the structure represented by formula (1) and the dimer diol component (a2), 100% by mass, the content of the polycarbonate polyol component (a1) is 10% by mass or more and 90% by mass or less, preferably 20% by mass or more and 80% by mass or less, and more preferably 30% by mass or more and 70% by mass or less, and the content of the dimer diol component (a2) is 10% by mass or more and 90% by mass or less, preferably 20% by mass or more and 80% by mass or less, and more preferably 30% by mass or more and 70% by mass or less.

[0044] If the content of the polycarbonate polyol component (a1) is 10% by mass or more, the polyurethane obtained from the polycarbonate polyol copolymer tends to have high flexibility, ensure resistance to oleic acid, and have high strength. If the content of the polycarbonate polyol component (a1) is 90% by mass or less, the moisture absorption of the obtained polycarbonate polyol copolymer can be kept low, and the polyurethane obtained from the polycarbonate polyol copolymer (A) tends to have good moist heat resistance.

[0045] In addition, when the content of the dimer diol component (a2) is 10% by mass or more, the moisture absorption of the obtained polycarbonate polyol copolymer (A) can be suppressed to be low, the biomass degree can be increased, and the wet heat resistance of the polyurethane made from the polycarbonate polyol copolymer (A) becomes good. In addition, when the content of the dimer diol component (a2) is 90% by mass or less, the flexibility of the polyurethane made from the polycarbonate polyol copolymer is increased, the resistance to oleic acid is ensured, and the strength tends to be high.

[0046] In the present embodiment, the proportion of each component in the polycarbonate polyol copolymer (A) can be measured by the method described in the examples below.

[0047] In the polycarbonate polyol copolymer (A) of the present embodiment, when 50 mol % or more of the repeating units represented by the above formula (1) contain at least two kinds of repeating units selected from the group consisting of repeating units represented by the following formula (2), repeating units represented by the following formula (3), and repeating units represented by the following formula (4), [ka] [ka] [ka] The polycarbonate polyol copolymer (A) of this embodiment preferably has a carbonate group content in one molecule of 17 to 38 mass%, more preferably 21 to 34 mass%. When the carbonate group content in one molecule is 17 mass% or more, the strength, oleic acid resistance, and abrasion resistance of the resulting polyurethane tend to be excellent. In addition, when the carbonate group content in one molecule is 38 mass% or less, the water absorption rate of the polycarbonate polyol copolymer (A) can be kept low, and the resulting polyurethane tends to be excellent in low-temperature properties, flexibility, and hydrolysis resistance.

[0048] In addition, in the polycarbonate polyol component (a1) contained in the polycarbonate polyol copolymer (A) of the present embodiment, when the repeating unit represented by the above formula (1) is a repeating unit represented by the following formula (5), [ka] The polycarbonate polyol copolymer (A) of this embodiment preferably has a carbonate group content in one molecule of 20 to 45% by mass, more preferably 25 to 40% by mass. When the carbonate group content in one molecule is 20% by mass or more, the strength, oleic acid resistance, and abrasion resistance of the resulting polyurethane tend to be excellent. In addition, when the carbonate group content in one molecule is 45% by mass or less, the water absorption rate of the polycarbonate polyol copolymer (A) can be kept low, and the resulting polyurethane tends to be excellent in low-temperature properties, flexibility, and hydrolysis resistance.

[0049] In the present embodiment, the carbonate group content in the polycarbonate polyol copolymer (A) can be measured by the method described in the examples below.

[0050] The hydroxyl value of the polycarbonate polyol copolymer (A) of the present embodiment is preferably from 37 to 224 mgKOH / g, more preferably from 44 to 160 mgKOH / g, and further preferably from 56 to 113 mgKOH / g.

[0051] When the polycarbonate polyol copolymer (A) has a hydroxyl value of 37 mgKOH / g or more, the viscosity tends to be kept low and the operability tends to be excellent. Also, when the polycarbonate polyol copolymer (A) has a hydroxyl value of 224 mgKOH / g or less, the flexibility (touch) and low-temperature properties of the obtained polyurethane tend to be improved.

[0052] In the present embodiment, the hydroxyl value of the polycarbonate polyol copolymer (A) can be measured by the method described in the examples described below.

[0053] The number average molecular weight of the polycarbonate polyol copolymer (A) of the present embodiment is preferably 500 or more and 3,000 or less, more preferably 700 or more and 2,500 or less, and even more preferably 1,000 or more and 2,000 or less.

[0054] The polycarbonate polyol copolymer (A) of this embodiment has a number average molecular weight of 500 or more, so that the flexibility (touch) and low-temperature properties of the obtained polyurethane tend to be improved. In addition, the polycarbonate polyol copolymer (A) of this embodiment has a number average molecular weight of 3000 or less, so that the viscosity is kept low and the operability tends to be excellent.

[0055] The method for controlling the number average molecular weight of the polycarbonate polyol copolymer (A) within the above range is not particularly limited, but examples thereof include a method of adjusting the amount of each raw material distilled during production and the amount of the reaction product.

[0056] In the present embodiment, the number average molecular weight of the polycarbonate polyol copolymer (A) can be calculated from the hydroxyl value of the polycarbonate polyol copolymer (A) using the method described in the Examples below.

[0057] In the polycarbonate polyol copolymer (A) of the present embodiment, when 50 mol % or more of the repeating units represented by the above formula (1) contain at least two kinds of repeating units selected from the group consisting of repeating units represented by the following formula (2), repeating units represented by the following formula (3), and repeating units represented by the following formula (4), [ka] [ka] [ka] The glass transition temperature (Tg) of the polycarbonate polyol copolymer (A) of this embodiment measured by a differential scanning calorimeter (hereinafter sometimes abbreviated as "DSC") is preferably -50°C or lower, more preferably -52°C or lower, and more preferably -54°C or lower. When the glass transition temperature (Tg) of the polycarbonate polyol copolymer (A) of this embodiment is the above upper limit or lower, the flexibility of the polyurethane under low temperature conditions tends to be improved. The lower limit of the glass transition temperature (Tg) of the polycarbonate diol copolymer (A) of this embodiment is not particularly limited, but is, for example, -70°C.

[0058] The method for controlling the glass transition temperature (Tg) of the polycarbonate polyol copolymer (A) within the above range is not particularly limited, and examples thereof include a method of adjusting the glass transition temperature (Tg) by selecting the types of bifunctional diol raw material and dimer acid used, selecting the ratio of the bifunctional diol and dimer acid, and controlling the amounts of each raw material and the reaction product distilled during production.

[0059] In addition, in the polycarbonate polyol component (a1) contained in the polycarbonate polyol copolymer (A) of the present embodiment, when the repeating unit represented by the above formula (1) is a repeating unit represented by the following formula (5), [ka] The glass transition temperature (Tg) of the polycarbonate polyol copolymer (A) of this embodiment measured by a differential scanning calorimeter (hereinafter sometimes abbreviated as "DSC") is preferably -40°C or lower, more preferably -43°C or lower, and more preferably -45°C or lower. When the glass transition temperature (Tg) of the polycarbonate polyol copolymer (A) of this embodiment is the above upper limit or lower, the flexibility of the polyurethane under low temperature conditions tends to be improved. The lower limit of the glass transition temperature (Tg) of the polycarbonate diol copolymer (A) of this embodiment is not particularly limited, but is, for example, -70°C.

[0060] The method for controlling the glass transition temperature (Tg) of the polycarbonate polyol copolymer (A) within the above range is not particularly limited, and examples thereof include a method of adjusting the glass transition temperature (Tg) by selecting the types of bifunctional diol raw material and dimer acid used, selecting the ratio of the bifunctional diol and dimer acid, and controlling the amounts of each raw material and the reaction product distilled during production.

[0061] In the present embodiment, the glass transition temperature (Tg) of the polycarbonate polyol copolymer (A) can be specifically measured by the method described in the examples described later.

[0062] In the polycarbonate polyol copolymer (A) of the present embodiment, when 50 mol % or more of the repeating units represented by the above formula (1) contain at least two kinds of repeating units selected from the group consisting of repeating units represented by the following formula (2), repeating units represented by the following formula (3), and repeating units represented by the following formula (4), [ka] [ka] [ka] The water absorption rate of the polycarbonate polyol copolymer (A) of this embodiment after being placed in an atmosphere of 85°C and 85% relative humidity for 7 days (hereinafter, also simply referred to as "water absorption rate") is preferably 0.8% by mass or less, more preferably 0.6% by mass or less, and even more preferably 0.5% by mass or less. If the water absorption rate of the polycarbonate polyol copolymer (A) of this embodiment is 0.8% by mass or less, the wet heat resistance tends to be improved when it is made into polyurethane. In addition, since the dielectric constant of the obtained polyurethane can be kept low, it can be suitably used as polyurethane for electronic materials. The lower limit of the water absorption rate of the polycarbonate diol copolymer (A) of this embodiment is not particularly limited, but is, for example, 0.2% by mass.

[0063] The method for controlling the water absorption rate of the polycarbonate polyol copolymer (A) within the above range is not particularly limited, but examples thereof include a method of adjusting the water absorption rate by selecting the types of bifunctional diol raw material and dimer acid used, selecting the ratio of the bifunctional diol and dimer acid, and controlling the amounts of each raw material and the reaction product distilled during production.

[0064] In addition, in the polycarbonate polyol component (a1) contained in the polycarbonate polyol copolymer (A) of the present embodiment, when the repeating unit represented by the above formula (1) is a repeating unit represented by the following formula (5), [ka] The water absorption rate of the polycarbonate polyol copolymer (A) of this embodiment after being placed in an atmosphere of 85°C and 85% relative humidity for 7 days (hereinafter, also simply referred to as "water absorption rate") is preferably 1.0% by mass or less, more preferably 0.9% by mass or less, and even more preferably 0.8% by mass or less. If the water absorption rate of the polycarbonate polyol copolymer (A) of this embodiment is 1.0% by mass or less, the wet heat resistance tends to be improved when it is made into polyurethane. In addition, since the dielectric constant of the obtained polyurethane can be kept low, it can be suitably used as polyurethane for electronic materials. The lower limit of the water absorption rate of the polycarbonate diol copolymer (A) of this embodiment is not particularly limited, but is, for example, 0.2% by mass.

[0065] The method for controlling the water absorption rate of the polycarbonate polyol copolymer (A) within the above range is not particularly limited, but examples thereof include a method of adjusting the water absorption rate by selecting the types of bifunctional diol raw material and dimer acid used, selecting the ratio of the bifunctional diol and dimer acid, and controlling the amounts of each raw material and the reaction product distilled during production.

[0066] In the present embodiment, the water absorption rate of the polycarbonate polyol copolymer (A) can be specifically measured by the method described in the examples described later.

[0067] In the polycarbonate polyol copolymer (A) of the present embodiment, when 50 mol % or more of the repeating units represented by the above formula (1) contain at least two kinds of repeating units selected from the group consisting of repeating units represented by the following formula (2), repeating units represented by the following formula (3), and repeating units represented by the following formula (4), [ka] [ka] [ka] The biomass degree of the polycarbonate polyol copolymer (A) of the present embodiment, as measured by accelerator mass spectrometry, is preferably 10% or more and 90% or less, more preferably 15% or more and 80% or less, and even more preferably 20% or more and 70% or less.

[0068] The "biomass degree" is an index representing the mixture ratio of petroleum-derived raw materials and biological raw materials (biomass), and is determined by measuring the concentration of radioactive carbon (C14) by accelerator mass spectrometry. C14 is contained at a certain concentration in biological raw materials, but is hardly present in petroleum trapped underground. Therefore, the content ratio of biological carbon present in the polycarbonate polyol copolymer (A) of this embodiment can be obtained by measuring the concentration of C14 present in the polycarbonate polyol copolymer (A) of this embodiment by accelerator mass spectrometry. The concentration of C14 in the polycarbonate polyol copolymer (A) of this embodiment is measured as follows. That is, the measurement sample is burned to generate carbon dioxide, and the carbon dioxide purified in a vacuum line is reduced with hydrogen using iron as a catalyst to purify graphite. This graphite is then attached to a tandem accelerator-based C14-AMS dedicated device (manufactured by NEC) to measure the C14 count, C13 concentration (C13 / C12), and C14 concentration (C14 / C12), and the ratio of the C14 concentration of the sample carbon to the standard modern carbon is calculated from these measurements. Oxalic acid (HOXII) provided by the National Institute of Standards (NIST) is used as the standard sample. From the obtained measurements, the biomass degree can be calculated using the δ13C-corrected pMC (percent modern carbon) according to ASTM D6866-21.

[0069] When the biomass degree is 10% or more, the proportion of carbon derived from plants is high, and the effect of suppressing the increase in the total amount of carbon dioxide in the global environment is enhanced. In addition, when the biomass degree is 10% or more, the water absorption rate of the polycarbonate polyol copolymer (A) of this embodiment is low, and the moist heat resistance of the polyurethane using the polycarbonate polyol copolymer (A) of this embodiment tends to be improved. In addition, since the dielectric constant of the obtained polyurethane can be kept low, it can be suitably used as a polyurethane for electronic materials. By making the biomass degree 90% or less, the flexibility of the polyurethane made from the polycarbonate polyol copolymer is increased, oleic acid resistance is ensured, and it tends to have high strength.

[0070] In addition, in the polycarbonate polyol component (a1) contained in the polycarbonate polyol copolymer (A) of the present embodiment, when the repeating unit represented by the above formula (1) is a repeating unit represented by the following formula (5), [ka] The biomass degree of the polycarbonate polyol copolymer (A) of the present embodiment measured by accelerator mass spectrometry is preferably 70% or more and 95% or less, more preferably 75% or more and 93% or less, and even more preferably 80% or more and 90% or less.

[0071] When the biomass degree is 70% or more, the proportion of carbon derived from plants is high, and the effect of suppressing the increase in the total amount of carbon dioxide in the global environment is enhanced. In addition, when the biomass degree is 70% or more, the water absorption rate of the polycarbonate polyol copolymer (A) of this embodiment is low, and the moist heat resistance of the polyurethane using the polycarbonate polyol copolymer (A) of this embodiment tends to be improved. In addition, since the dielectric constant of the obtained polyurethane can be kept low, it can be suitably used as a polyurethane for electronic materials. By making the biomass degree 95% or less, the flexibility of the polyurethane made from the polycarbonate polyol copolymer is increased, oleic acid resistance is ensured, and it tends to have high strength.

[0072] In the polycarbonate polyol copolymer (A) of the present embodiment, when 50 mol % or more of the repeating units represented by the above formula (1) contain at least two kinds of repeating units selected from the group consisting of repeating units represented by the following formula (2), repeating units represented by the following formula (3), and repeating units represented by the following formula (4), [ka] [ka] [ka] The melt viscosity of the polycarbonate polyol copolymer (A) of this embodiment at 50°C is preferably 3000 to 30000 mPa·s, more preferably 4000 to 20000 mPa·s, and even more preferably 5000 to 10000 mPa·s. When the melt viscosity of the polycarbonate polyol copolymer (A) of this embodiment at 50°C is 3000 mPa·s or more, the flexibility and low-temperature properties of the obtained polyurethane tend to be improved. In addition, when the melt viscosity of the polycarbonate polyol copolymer (A) of this embodiment at 50°C is 30000 mPa·s or less, the operability during polyurethane production is excellent, and the amount of organic solvent used during polyurethane production can be reduced.

[0073] The method for controlling the melt viscosity at 50°C of the polycarbonate polyol copolymer (A) within the above range is not particularly limited, and examples thereof include a method of adjusting the melt viscosity by selecting the types of bifunctional diol raw material and dimer acid used, selecting the ratio of the bifunctional diol and dimer acid, and controlling the amounts of each raw material and the reaction product distilled during production.

[0074] In addition, in the polycarbonate polyol component (a1) contained in the polycarbonate polyol copolymer (A) of the present embodiment, when the repeating unit represented by the above formula (1) is a repeating unit represented by the following formula (5), [ka] The melt viscosity of the polycarbonate polyol copolymer (A) of this embodiment at 50°C is preferably 3000 to 40000 mPa·s, more preferably 3500 to 30000 mPa·s, and even more preferably 4000 to 26000 mPa·s. When the melt viscosity of the polycarbonate polyol copolymer (A) of this embodiment at 50°C is 3000 mPa·s or more, the flexibility and low-temperature properties of the obtained polyurethane tend to be improved. In addition, when the melt viscosity of the polycarbonate polyol copolymer (A) of this embodiment at 50°C is 40000 mPa·s or less, the operability during polyurethane production is excellent, and the amount of organic solvent used during polyurethane production can be reduced.

[0075] The method for controlling the melt viscosity at 50°C of the polycarbonate polyol copolymer (A) within the above range is not particularly limited, and examples thereof include a method of adjusting the melt viscosity by selecting the types of bifunctional diol raw material and dimer acid used, selecting the ratio of the bifunctional diol and dimer acid, and controlling the amounts of each raw material and the reaction product distilled during production.

[0076] In the present embodiment, the melt viscosity at 50° C. of the polycarbonate polyol copolymer (A) can be measured by the method described in the examples described later.

[0077] [Method-1 for producing polycarbonate polyol copolymer (A) according to the present embodiment] The method for producing the polycarbonate polyol copolymer (A) of the present embodiment is not particularly limited. For example, the polycarbonate polyol copolymer (A) can be produced by first polymerizing a polycarbonate polyol component (a1) having a structure represented by the following formula (1) as a copolymerization component, and then adding a dimer diol component (a2) to carry out an ester exchange reaction. [ka] (In formula (1), R1 is a divalent aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.)

[0078] The polymerization method of the polycarbonate polyol component (a1) is not particularly limited, but for example, it can be synthesized by using a bifunctional diol compound, and optionally a trifunctional or higher polyhydric alcohol and a carbonate ester as raw materials, for example, by an ester exchange reaction as described in "Polymer Reviews, Vol. 9, pages 9-20" or the like.

[0079] The bifunctional diol compound used in the transesterification reaction is not particularly limited, but examples thereof include diols having a divalent aliphatic or alicyclic hydrocarbon skeleton having 2 to 15 carbon atoms. The bifunctional diol compound is not particularly limited, but specific examples thereof include ethylene glycol, 1,3-propanediol, 2-methyl-1,3-propanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 2-methyl-1,8-octanediol, 1,11-undecanediol, 1,1 Examples of the diol include 2-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,15-pentadecanediol, 2-isopropyl-1,4-butanediol, 2-ethyl-1,6-hexanediol, 3-methyl-1,5-pentanediol, 2,4-dimethyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, and 1,4-cyclohexanedimethanol.

[0080] [When 50 mol % or more of the repeating units represented by formula (1) contain at least two repeating units selected from the group consisting of repeating units represented by formulas (2) to (4)] In the polycarbonate polyol copolymer (A) of the present embodiment, when 50 mol % or more of the repeating units represented by the above formula (1) contain at least two kinds of repeating units selected from the group consisting of repeating units represented by the following formula (2), repeating units represented by the following formula (3), and repeating units represented by the following formula (4), [ka] [ka] [ka] As the bifunctional diol compound used in the transesterification reaction, it is preferable to use two or more of 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol in combination. By using two or more of them in combination, the regularity of the structural unit of the polycarbonate component in the polycarbonate polyol copolymer is reduced, and the crystallinity is reduced, so that not only is a polycarbonate polyol copolymer (A) that is liquid at room temperature (23°C) obtained, but the flexibility of the polyurethane tends to be increased. In addition, when an organic solvent is used during polyurethane production, the amount of the organic solvent used tends to be reduced.

[0081] Among the repeating units represented by the above formula (1), at least two repeating units selected from the group consisting of the repeating units represented by the above formula (2), the repeating units represented by the above formula (3), and the repeating units represented by the above formula (4) are 50 mol% or more, preferably 70 mol% or more, and more preferably 80 mol% or more, so that the polycarbonate polyol copolymer (A) obtained by the transesterification reaction of the polycarbonate polyol component (a1) and the dimer diol component (a2) in the next step is liquid, transparent, and low-viscosity at room temperature (23 ° C.). In addition to the excellent flexibility (touch), chemical resistance, low-temperature properties, and heat resistance of the polyurethane using the polycarbonate polyol copolymer (A) obtained by the transesterification reaction of the polycarbonate polyol component (a1) and the dimer diol component (a2) in the next step, the amount of inert organic solvent used during polyurethane production tends to be reduced. Among the repeating units represented by formula (1), the upper limit of the proportion (mol %) of at least two types of repeating units selected from the group consisting of repeating units represented by formula (2), repeating units represented by formula (3), and repeating units represented by formula (4) is not particularly limited, but is usually 100 mol % or less.

[0082] In order to obtain the polycarbonate polyol component (a1), other diols that can be used as necessary in addition to 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol are not particularly limited, and examples thereof include diols having no side chains such as ethylene glycol, 1,3-propanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nanodiol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, and 1,14-tetradecanediol, 2-methyl-1,8-octanediol, and the like. One or more diols can be used from diols having side chains such as hexanediol, 2-ethyl-1,6-hexanediol, 2-methyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2,4-dimethyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, and 2,2-dimethyl-1,3-propanediol, and cyclic diols such as 1,4-cyclohexanedimethanol and 2-bis(4-hydroxycyclohexyl)-propane.

[0083] In this embodiment, in the synthesis of the polycarbonate polyol component (a1), when two kinds of repeating units are selected from the group consisting of the repeating unit represented by the above formula (2), the repeating unit represented by the above formula (3), and the repeating unit represented by the above formula (4), the ratio of the two kinds of repeating units (hereinafter also referred to as "copolymerization ratio") is 90:10 to 10:90, preferably 70:30 to 30:70, more preferably 60:40 to 40:60, in terms of molar ratio. By having the copolymerization ratio within the above range, the crystallinity of the polycarbonate polyol copolymer (A) obtained by the transesterification reaction of the polycarbonate polyol component (a1) and the dimer diol component (a2) in the next step is reduced, and a polycarbonate polyol copolymer (A) that is liquid, transparent, and low in viscosity at room temperature (23°C) can be obtained. In addition, polyurethane using this polycarbonate polyol copolymer (A) tends to have high flexibility, good low-temperature properties, and feel. Furthermore, when the copolymerization ratio is within this range, there is a tendency that the amount of inert organic solvent used can be reduced when producing a polyurethane using this polycarbonate polyol copolymer (A).

[0084] In this embodiment, when three repeating units are selected from the group consisting of the repeating unit represented by the above formula (2), the repeating unit represented by the above formula (3), and the repeating unit represented by the above formula (4), the ratio of these structural units is preferably 5 mol% or more, more preferably 10 mol% or more, and even more preferably 20 mol% or more, when the total of the three repeating units of the above formulas (2), (3), and (4) is 100 mol%. By each ratio of the three repeating units of the above formulas (2), (3), and (4) to the total of the three repeating units of the above formulas (2), (3), and (4) being within the above range, the crystallinity of the polycarbonate polyol copolymer (A) obtained by the transesterification reaction of the polycarbonate polyol component (a1) and the dimer diol component (a2) in the next step is reduced, and a polycarbonate polyol copolymer (A) that is liquid, transparent, and low viscosity at room temperature (23 ° C.) can be obtained. In addition, polyurethanes using this polycarbonate polyol copolymer (A) tend to have high flexibility, good low-temperature properties, and good touch. Furthermore, by having the proportions of the three repeating units of the above formulae (2), (3), and (4) within the above ranges, the amount of inert organic solvent used during the production of polyurethanes using this polycarbonate polyol copolymer (A) tends to be reduced.

[0085] In this embodiment, in addition to the bifunctional diol, a trifunctional or higher polyhydric alcohol compound can be used as necessary as the raw material of the polycarbonate polyol component (a1).

[0086] The polyhydric alcohol compound is not particularly limited, and examples thereof include trimethylolethane, trimethylolpropane, hexanetriol, pentaerythritol, glycerin, etc. By using a polyhydric alcohol, the average number of hydroxyl groups in one molecule of the polycarbonate polyol component (a1) tends to be easily adjusted to the range of 1.7 to 3.5.

[0087] [When the repeating unit represented by formula (1) is a repeating unit represented by formula (5)] In addition, in the polycarbonate polyol component (a1) contained in the polycarbonate polyol copolymer (A) of the present embodiment, when the repeating unit represented by the above formula (1) is a repeating unit represented by the following formula (5), [ka] As the bifunctional diol compound used in the transesterification reaction, 1,3-propanediol is used.

[0088] In addition, as the bifunctional diol compound, in addition to 1,3-propanediol, a diol other than 1,3-propanediol can be used as necessary. The diol other than 1,3-propanediol is not particularly limited, but for example, ethylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nanodiol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,14-tetradecanediol, and other diols that do not have a side chain, 2-methyl-1,8-octanediol, 2-ethyl-1,6-hexanediol, 2-methyl-1,8-octanediol, 2-ethyl-1,6-hexanediol, 2-methyl-1,8-octanediol, 2-ethyl-1,6-hexanediol, 2-ethyl-1,8-octanedi ... One or more diols may be used from diols having side chains such as 2-methyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2,4-dimethyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, and cyclic diols such as 1,4-cyclohexanedimethanol and 2-bis(4-hydroxycyclohexyl)-propane.

[0089] The ratio of 1,3-propanediol in the bifunctional diol compound is preferably 60% by mass or more, more preferably 80% by mass or more, and further preferably 90% by mass or more. By having the ratio of 1,3-propanediol in the bifunctional diol compound be 60% by mass or more, not only can the biomass degree of the obtained polycarbonate polyol copolymer (A) be increased, but also the oleic acid resistance and abrasion resistance of the polyurethane obtained by using the polycarbonate polyol copolymer (A) of this embodiment tend to be improved.

[0090] In this embodiment, in addition to 1,3-propanediol, a polyhydric alcohol compound having three or more functional groups can be used as necessary as a raw material for the polycarbonate polyol component (a1).

[0091] The polyhydric alcohol compound is not particularly limited, and examples thereof include trimethylolethane, trimethylolpropane, hexanetriol, pentaerythritol, glycerin, etc. By using a polyhydric alcohol, the average number of hydroxyl groups in one molecule of the polycarbonate polyol component (a1) tends to be easily adjusted to the range of 1.7 to 3.5.

[0092] The carbonate ester that can be used in the production of the polycarbonate polyol component (a1) is not particularly limited, and examples thereof include dialkyl carbonates such as dimethyl carbonate, diethyl carbonate, dipropyl carbonate, and dibutyl carbonate; diaryl carbonates such as diphenyl carbonate; alkylene carbonates such as ethylene carbonate, trimethylene carbonate, 1,2-propylene carbonate, 1,2-butylene carbonate, 1,3-butylene carbonate, and 1,2-pentylene carbonate; etc. From the viewpoint of ease of availability and ease of setting the polymerization reaction conditions, it is preferable to use dimethyl carbonate, diethyl carbonate, diphenyl carbonate, and ethylene carbonate as the carbonate ester.

[0093] In the production of the polycarbonate polyol component (a1), a catalyst may or may not be added. When a catalyst is added, it can be freely selected from catalysts used in normal transesterification reactions. The catalyst is not particularly limited, but for example, metals such as lithium, sodium, potassium, rubidium, cesium, magnesium, calcium, strontium, barium, zinc, manganese, aluminum, titanium, molybdenum, nickel, iron, cobalt, germanium, tin, lead, antimony, arsenic, and cerium, as well as metal salts thereof, metal alkoxides thereof, and organic compounds containing the metals are used.

[0094] In addition, the metal catalyst is not particularly limited, but examples thereof include metal salts of formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, enanthic acid, caprylic acid, palmitic acid, margaric acid, stearic acid, and the like, and hydrates thereof. Among these, salts of acetic acid, propionic acid, and butyric acid and hydrates thereof are preferred, and salts of acetic acid and hydrates thereof are particularly preferred. Furthermore, these metal catalysts may be metal complexes, and the ligand for the metal in the metal complex is preferably an acetylacetone analogue.

[0095] Specific examples of preferred metal catalysts include, but are not limited to, lithium methoxide, sodium methoxide, potassium methoxide, lithium t-butoxide calcium (II) acetylacetonate dihydrate, calcium acetate monohydrate, calcium dimethoxide manganese (II) acetylacetonate dihydrate, manganese (III) acetylacetonate, manganese (II) acetate tetrahydrate, 2,2,6,6-tetramethyl-3,5-heptanedionato manganese (II) dihydrate, hexafluoroacetate, Examples of acetylacetonate include manganese(II) acetylacetonate dihydrate, molybdenum(II) acetylacetonate dimer, magnesium(II) acetylacetonate dihydrate, iron(III) acetylacetonate, cobalt(II) acetylacetonate dihydrate, nickel(II) acetylacetonate dihydrate, copper(II) acetylacetonate, titanium(IV) bis(acetylacetonate)diisopropoxide, and magnesium(II) acetylacetonate.

[0096] Among the above catalysts, organic compounds containing titanium, manganese, lithium, and calcium are preferred. These catalysts may be used alone or in combination of two or more.

[0097] These catalysts are also effective in the transesterification reaction between the polycarbonate polyol component (a1) and the dimer diol component (a2) in the next step, so that the polycarbonate polyol component (a1) can be polymerized, and then the dimer diol component (a2) can be added to the polycarbonate polyol component (a1) containing the catalyst to produce the polycarbonate polyol component (a1). The amount of the catalyst used in the transesterification reaction between the polycarbonate polyol component (a1) and the dimer diol component (a2) is 0.0001% by mass to 0.01% by mass, preferably 0.0002% by mass to 0.001% by mass, more preferably 0.0003% by mass to 0.0007% by mass, as the amount of metal contained in the catalyst, of the total mass of the diol compound and the carbonate ester compound used in the production of the polycarbonate polyol component (a1).

[0098] In the present embodiment, the polycarbonate polyol component (a1) can be produced, for example, by a transesterification reaction using a bifunctional diol compound, and optionally a trifunctional or higher polyhydric alcohol and a carbonate ester as raw materials, as described above.

[0099] More specifically, although not particularly limited, the transesterification reaction is carried out, for example, according to the following procedure.

[0100] First, a bifunctional diol compound in a predetermined ratio, one or more trifunctional or higher polyhydric alcohols as needed in a predetermined ratio, and one or more carbonate esters in a predetermined ratio are mixed together, and an ester exchange reaction is carried out at normal or reduced pressure in the absence or presence of an ester exchange catalyst at a temperature of preferably 100 to 200°C, more preferably 140 to 180°C.

[0101] Subsequently, alcohol derived from the carbonate ester produced during the reaction is distilled off to obtain a polycarbonate polyol having a molecular weight of about 300 to 500 g / mol.

[0102] Next, the unreacted carbonate ester and bifunctional diol, and optionally the trifunctional or higher polyhydric alcohol are distilled off under reduced pressure, preferably at 130 to 230°C, more preferably at 150 to 200°C, and a polycarbonate polyol component (a1) having a desired hydroxyl value can be obtained by a condensation reaction.

[0103] The composition of the polycarbonate polyol component (a1) and the average number of hydroxyl groups in one molecule can be adjusted by controlling the initial charging ratio of each component, the amount of each raw material distilled during production, and the amount of the reaction product.

[0104] By designing the average hydroxyl value of the polycarbonate polyol component (a1) in advance, it is possible to adjust the hydroxyl value of the polycarbonate polyol copolymer (A) after the transesterification reaction between the polycarbonate polyol component (a1) and the dimer diol component (a2) in the next step.

[0105] The temperature of the transesterification reaction between the polycarbonate polyol component (a1) and the dimer diol component (a2) in the next step is not particularly limited, but is preferably 120°C or higher and 200°C or lower, more preferably 140°C or higher and 180°C or lower. By setting the reaction temperature to the above lower limit or higher, the transesterification reaction can be carried out in a shorter time, which is economical. By setting the reaction temperature to the above upper limit or lower, coloration of the resulting polycarbonate polyol copolymer can be more effectively prevented.

[0106] The reaction pressure for the transesterification reaction between the polycarbonate polyol component (a1) and the dimer diol component (a2) is not particularly limited, but the reaction is usually carried out under reduced pressure while distilling off the water produced.

[0107] In order to carry out the transesterification reaction more efficiently, it is preferable to use a catalyst. When the transesterification reaction is carried out continuously after the production of the polycarbonate polyol component (a1), the catalyst used in the production of the polycarbonate polyol component (a1) is contained in the polycarbonate polyol component (a1), and therefore acts effectively in the next transesterification reaction between the polycarbonate polyol component (a1) and the dimer diol component (a2). In addition, a catalyst may be added during the transesterification reaction between the polycarbonate polyol component (a1) and the dimer diol component (a2). When a catalyst is added, the type of catalyst to be added can be selected from the catalysts used in the production of the polycarbonate polyol component (a1).

[0108] Among the catalysts used, organic compounds containing titanium, manganese, lithium, and calcium are preferred. These catalysts may be used alone or in combination of two or more.

[0109] When a catalyst is added, the amount of the added catalyst is, in terms of the amount of metal contained in the catalyst, preferably 0.0001 mass% to 0.01 mass%, more preferably 0.0002 mass% to 0.001 mass%, and even more preferably 0.0003 mass% to 0.0007 mass%, relative to 100 mass% of the total mass of the polycarbonate polyol component (a1) and the dimer diol component (a2).

[0110] The reaction time for the transesterification of the polycarbonate polyol component (a1) and the dimer diol component (a2) is preferably 5 to 20 hours, more preferably 10 to 15 hours.

[0111] The progress and completion of the transesterification reaction between the polycarbonate polyol component (a1) and the dimer diol component (a2) can be confirmed by gel permeation chromatography (GPC). As the transesterification reaction proceeds, the peak area derived from the raw material dimer diol component (a2) decreases over time, and the completion of the transesterification reaction can be confirmed when the peak area is 5% or less, preferably 3% or less, and more preferably 1% or less.

[0112] In this embodiment, the polycarbonate polyol component (a1) and the dimer diol component (a2) are used as copolymerization components of the polycarbonate polyol copolymer (A), but polyols other than the polycarbonate polyol component (a1) and the dimer diol component (a2) may be used in combination as necessary. Here, the polyols other than the polycarbonate polyol component (a1) and the dimer diol component (a2) are not particularly limited as long as they are used in the production of ordinary polyurethanes, and examples thereof include polyether polyols, polyester polyols, acrylic polyols, polyolefin polyols, castor oil polyols, polycarbonate polyols other than the polycarbonate polyol component (a1), and the like.

[0113] The mass ratio of the polycarbonate polyol component (a1) and the dimer diol component (a2) to the total mass of the polycarbonate polyol component (a1) and the dimer diol component (a2) and other polyols is preferably 50% by mass or more, more preferably 70% by mass or more. When the mass ratio of the polycarbonate polyol component (a1) and the dimer diol component (a2) is 50% by mass or more, when the polyurethane is made, the balance of flexibility (touch), chemical resistance, low temperature characteristics, and heat resistance tends to be excellent. On the other hand, the addition of other polyols contributes to the effect of reducing the viscosity of the polycarbonate polyol copolymer (A) of this embodiment, and can be used in combination within a range that does not impair performance.

[0114] [Production method 2 of polycarbonate polyol copolymer (A) of the present embodiment] Another method for producing the polycarbonate polyol copolymer (A) of the present embodiment is not particularly limited, but may be, for example, a method in which a bifunctional diol at a predetermined ratio, one or more trifunctional or higher polyhydric alcohols at a predetermined ratio as necessary, a dimer diol component (a2), and a carbonate ester are used as raw materials, and the raw materials are synthesized in one stage by transesterification as described in, for example, "Polymer Reviews, Vol. 9, pages 9-20". The production method in which transesterification is carried out in one stage is more preferable because it has excellent productivity.

[0115] The bifunctional diol compound used in the transesterification reaction is not particularly limited, and examples of the bifunctional diol compound include ethylene glycol, 1,3-propanediol, 2-methyl-1,3-propanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 2-methyl-1,8-octanediol, 1,11 1,12-undecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,15-pentadecanediol, 2-isopropyl-1,4-butanediol, 2-ethyl-1,6-hexanediol, 3-methyl-1,5-pentanediol, 2,4-dimethyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, and 1,4-cyclohexanedimethanol.

[0116] In this embodiment, when 50 mol% or more of the repeating units represented by the above formula (1) contain at least two repeating units selected from the group consisting of the repeating units represented by the above formulas (2) to (4), it is preferable to use two or more of 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol in combination as the bifunctional diol compound used in the transesterification reaction. By using two or more of them in combination, the regularity of the structural unit of the polycarbonate component in the polycarbonate polyol copolymer is reduced, and the crystallinity is reduced, so that not only is a polycarbonate polyol copolymer (A) that is liquid at room temperature (23 ° C.) obtained, but the flexibility of the polyurethane tends to be increased. In addition, when an organic solvent is used during polyurethane production, the amount of the organic solvent used tends to be reduced.

[0117] In this embodiment, when the repeating unit represented by the above formula (1) is a repeating unit represented by the above formula (5), it is preferable to use 1,3-propanediol as the bifunctional diol compound used in the transesterification reaction. By using 1,3-propanediol, the structure of the polycarbonate component in the polycarbonate polyol copolymer (A) becomes amorphous, and a polycarbonate polyol copolymer (A) that is liquid at room temperature (23°C) is obtained. In addition, the flexibility of the polyurethane using the polycarbonate polyol copolymer of this embodiment tends to be increased. In addition, when an organic solvent is used during polyurethane production, the amount of the organic solvent used tends to be reduced.

[0118] In the present embodiment, in addition to the bifunctional diol, a trifunctional or higher polyhydric alcohol compound can be used as necessary as a raw material for the polycarbonate polyol copolymer (A).

[0119] The polyhydric alcohol compound is not particularly limited, and examples thereof include trimethylolethane, trimethylolpropane, hexanetriol, pentaerythritol, glycerin, etc. By using a polyhydric alcohol, the average number of hydroxyl groups in one molecule of the polycarbonate polyol copolymer (A) tends to be easily adjusted to the range of 1.7 to 3.5.

[0120] Next, the carbonate ester that can be used in the production of the polycarbonate polyol copolymer (A) is not particularly limited, but examples thereof include dialkyl carbonates such as dimethyl carbonate, diethyl carbonate, dipropyl carbonate, and dibutyl carbonate; diaryl carbonates such as diphenyl carbonate; alkylene carbonates such as ethylene carbonate, trimethylene carbonate, 1,2-propylene carbonate, 1,2-butylene carbonate, 1,3-butylene carbonate, and 1,2-pentylene carbonate; etc. From the viewpoint of ease of availability and ease of setting the polymerization reaction conditions, it is preferable to use dimethyl carbonate, diethyl carbonate, diphenyl carbonate, and ethylene carbonate as the carbonate ester.

[0121] In the production of the polycarbonate polyol copolymer (A), a catalyst may or may not be added. When a catalyst is added, it can be freely selected from catalysts used in normal transesterification reactions. The catalyst is not particularly limited, but for example, metals such as lithium, sodium, potassium, rubidium, cesium, magnesium, calcium, strontium, barium, zinc, manganese, aluminum, titanium, molybdenum, nickel, iron, cobalt, germanium, tin, lead, antimony, arsenic, and cerium, as well as metal salts thereof, metal alkoxides thereof, and organic compounds containing the metals are used.

[0122] In addition, the metal catalyst is not particularly limited, but examples thereof include metal salts of formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, enanthic acid, caprylic acid, palmitic acid, margaric acid, stearic acid, and the like, and hydrates thereof. Among these, salts of acetic acid, propionic acid, and butyric acid and hydrates thereof are preferred, and salts of acetic acid and hydrates thereof are particularly preferred.

[0123] Furthermore, these metal catalysts may be metal complexes, and the ligand for the metal in the metal complex is preferably an acetylacetone analogue.

[0124] Specific examples of preferred metal catalysts include, but are not limited to, lithium methoxide, sodium methoxide, potassium methoxide, lithium t-butoxide calcium (II) acetylacetonate dihydrate, calcium acetate monohydrate, calcium dimethoxide manganese (II) acetylacetonate dihydrate, manganese (III) acetylacetonate, manganese (II) acetate tetrahydrate, 2,2,6,6-tetramethyl-3,5-heptanedionato manganese (II) dihydrate, hexafluoroacetate, Examples of acetylacetonate include manganese(II) acetylacetonate dihydrate, molybdenum(II) acetylacetonate dimer, magnesium(II) acetylacetonate dihydrate, iron(III) acetylacetonate, cobalt(II) acetylacetonate dihydrate, nickel(II) acetylacetonate dihydrate, copper(II) acetylacetonate, titanium(IV) bis(acetylacetonate)diisopropoxide, and magnesium(II) acetylacetonate.

[0125] Among the above catalysts, organic compounds containing titanium, manganese, lithium, and calcium are preferred. These catalysts may be used alone or in combination of two or more.

[0126] The amount of the catalyst, in terms of the amount of metal contained in the catalyst, is 0.0001% by mass to 0.01% by mass, preferably 0.0002% by mass to 0.001% by mass, and more preferably 0.0003% by mass to 0.0007% by mass relative to 100% by mass of the total mass of the bifunctional diol compound, one or more kinds of trifunctional or higher polyhydric alcohols in a predetermined ratio as necessary, the dimer diol component (a2), and the carbonate ester.

[0127] More specifically, although not particularly limited, the transesterification reaction is carried out, for example, according to the following procedure.

[0128] First, a bifunctional diol compound in a predetermined ratio, one or more trifunctional or higher polyhydric alcohols in a predetermined ratio as required, a dimer diol component (a2), and one or more carbonate esters in a predetermined ratio are mixed together, and an ester exchange reaction is carried out at normal or reduced pressure in the absence or presence of an ester exchange catalyst at a temperature of preferably 100 to 200°C, more preferably 140 to 180°C.

[0129] Subsequently, alcohol derived from the carbonate ester produced during the reaction and water are distilled off to obtain an oligomer of a polycarbonate polyol copolymer having a molecular weight of about 300 to 500 g / mol.

[0130] Next, the unreacted carbonate ester, bifunctional diol, water, and optionally contained trifunctional or higher polyhydric alcohol are distilled off under reduced pressure, preferably at 130 to 230°C, more preferably at 150 to 200°C, and a polycarbonate polyol copolymer (A) having a desired hydroxyl value can be obtained by a condensation reaction.

[0131] The composition of the polycarbonate polyol copolymer (A) and the average number of hydroxyl groups in one molecule can be adjusted by controlling the initial charging ratio of each component, the amount of each raw material distilled during production, and the amount of the reaction product.

[0132] In this embodiment, the polycarbonate polyol component (a1) and the dimer diol component (a2) are used as copolymerization components of the polycarbonate polyol copolymer (A), but polyols other than the polycarbonate polyol component (a1) and the dimer diol component (a2) may be used in combination as necessary. Here, the polyols other than the polycarbonate polyol component (a1) and the dimer diol component (a2) are not particularly limited as long as they are used in the production of ordinary polyurethanes, and examples thereof include polyether polyols, polyester polyols, acrylic polyols, polyolefin polyols, castor oil polyols, polycarbonate polyols other than the polycarbonate polyol component (a1), and the like.

[0133] The mass ratio of the polycarbonate polyol component (a1) and the dimer diol component (a2) to the total mass of the polycarbonate polyol component (a1) and the dimer diol component (a2) and other polyols is preferably 50 mass% or more, more preferably 70 mass% or more. When the mass ratio of the polycarbonate polyol component (a1) and the dimer diol component (a2) is 50 mass% or more, when the polyurethane is made, the balance of flexibility (touch), chemical resistance, low temperature characteristics, and heat resistance tends to be excellent. On the other hand, the addition of other polyols contributes to the effect of reducing the viscosity of the polycarbonate polyol copolymer (A) of this embodiment, and can be used in combination within a range that does not impair performance.

[0134] The polycarbonate polyol copolymer (A) of the present embodiment is preferably liquid and transparent at 23°C.

[0135] [Polyurethane] The polyurethane of the present embodiment is produced using the above-mentioned polycarbonate polyol copolymer (A).

[0136] The polyurethane of this embodiment preferably has a swelling degree (hereinafter also simply referred to as "swelling degree") after immersion in oleic acid at 23°C for 7 days of 5% by mass or more and 35% by mass or less, and more preferably 5% by mass or more and 30% by mass or less.

[0137] The polyurethane of the present embodiment tends to have excellent chemical resistance when the swelling ratio is equal to or less than the upper limit. Also, when the swelling ratio of the polyurethane is equal to or more than the lower limit, the solubility of the polycarbonate polyol, which is the raw material of the polyurethane, in the solvent tends to be good, and the amount of the solvent used during the synthesis of the prepolymer tends to be reduced. From the same viewpoint, the polyurethane of the present embodiment more preferably has a swelling ratio of 7 to 30% by mass, and particularly preferably 10 to 25% by mass.

[0138] In this embodiment, the swelling degree can be measured by the method described in the Examples below.

[0139] The method for producing the polyurethane of the present embodiment is not particularly limited, and known polyurethane-forming reaction conditions for producing ordinary polyurethanes are used.

[0140] Examples of the method include, but are not limited to, a method in which the above-mentioned polycarbonate polyol copolymer (A), other polyol, an isocyanate compound (e.g., polyisocyanate), and a chain extender are mixed together and reacted (hereinafter referred to as the "one-shot method"), and a method in which the above-mentioned polycarbonate polyol copolymer (A), other polyol, and an isocyanate compound (e.g., polyisocyanate) are reacted to prepare a prepolymer having isocyanate groups at both ends, and then the prepolymer is reacted with a chain extender (hereinafter referred to as the "prepolymer method").

[0141] The isocyanate compound used in the production of the polyurethane of this embodiment is not particularly limited as long as it acts as a curing agent, and one having two or more isocyanate groups at its terminals is used.

[0142] Such an isocyanate compound is not particularly limited, but examples thereof include linear aliphatic diisocyanates, cyclic aliphatic diisocyanates, aromatic diisocyanates, and isocyanate compounds having three or more isocyanate groups, as well as isocyanurate-modified products and biuret-modified products of these isocyanate compounds.

[0143] The chain aliphatic diisocyanate is not particularly limited, but examples thereof include hexamethylene diisocyanate and trimethylhexamethylene diisocyanate.

[0144] The cyclic aliphatic diisocyanate is not particularly limited, but examples thereof include isophorone diisocyanate.

[0145] The aromatic diisocyanate is not particularly limited, but examples thereof include tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate (hereinafter sometimes abbreviated as "MDI"), xylylene diisocyanate, and naphthylene diisocyanate.

[0146] The isocyanate compound having three or more isocyanate groups is not particularly limited, and examples thereof include triphenylmethane-4,4'-4''-triisocyanate, 1,3,5-triisocyanatobenzene, 2,4,6-triisocyanatoene, and 4,4'-dimethyldiphenylmethane-2,2',5,5'-tetraisocyanate, as well as diisocyanate derivatives such as biuret, allophanate, uretdione, and isocyanurate, and polyhydric alcohol adducts.

[0147] The isocyanate compound may be a commercially available product or may be synthesized by a known method.

[0148] Furthermore, it is also possible to use so-called blocked isocyanates in which an isocyanate compound is blocked with a known blocking agent, such as a lower alcohol such as butanol or 2-ethylhexanol, methyl ethyl ketone oxime, lactams, phenols, imidazoles, or an active methylene compound.

[0149] Commercially available isocyanate compounds include, but are not limited to, Sumidur 44S, 44V70 (both manufactured by Sumika Bayer Urethane), Dismodur HL (manufactured by Sumika Bayer Urethane), which is a copolymer of TDI and HDI, and various Duranates manufactured by Asahi Kasei Corporation, namely, Duranate 24A-100, Duranate 22A-75PX, Duranate 18H-70B, Duranate 21S-75E, Duranate THA-100, Duranate TPA-100, Duranate MFA-75X, Duranate TSA-100, Duranate TSS-100, and Duranate TSE-100. , Duranate D-101, Duranate D-201, Duranate P-301-75E, Duranate E-402-90T, Duranate E-402-90T, Duranate E-405-80T, Duranate ME20-100, Duranate 17B-60PX, Duranate TPA-B80X, Duranate MF-B60X, Duranate E-402-B80T, Duranate ME20-B80S, Duranate WB40-100, Duranate WB40-80D, Duranate WT20-100, Duranate WT30-100, and the like.

[0150] The content of the isocyanate compound may be appropriately adjusted according to the molar amount of the hydroxyl group of the polycarbonate polyol copolymer (A) of this embodiment. Specifically, the molar ratio (NCO / OH) of the isocyanate group of the isocyanate compound to the hydroxyl group of the polycarbonate polyol copolymer (A) of this embodiment is adjusted to be preferably 0.7 to 1.3, more preferably 0.8 to 1.2, and even more preferably 0.9 to 1.1. By making the molar ratio (NCO / OH) of the isocyanate group of the isocyanate compound 0.7 or more and 1.3 or less, the molecular weight of the obtained polyurethane can be appropriately controlled, and the mechanical properties such as strength, elongation, and abrasion resistance tend to be excellent.

[0151] A chain extender can be used in the polyurethane of this embodiment as necessary. The chain extender is used to increase the abrasion resistance and strength of the resulting polyurethane, but on the other hand, it may also reduce the flexibility of the resulting polyurethane, so it is used appropriately and as necessary. The chain extender is not particularly limited, but examples thereof include short-chain diols such as ethylene glycol and 1,4-butanediol; polyhydric alcohols such as trimethylolethane, trimethylolpropane, hexanetriol, pentaerythritol, and glycerin; and the like. In addition, the chain extender is not particularly limited, but examples thereof include diamines such as ethylenediamine, propylenediamine, hexamethylenediamine, tolylenediamine, xylylenediamine, diphenyldiamine, diaminodiphenylmethane, diaminocyclohexylmethane, piperazine, 2-methylpiperazine, and isophoronediamine, and water.

[0152] The amount of the chain extender added is preferably 30% by mass or less, more preferably 3% by mass or more and 20% by mass or less, and even more preferably 5% by mass or more and 10% by mass or less, based on the polycarbonate polyol copolymer (A) of this embodiment. It is desirable to adjust the amount of isocyanate according to the amount of the chain extender added. For example, the isocyanate equivalent of the isocyanate compound used is preferably adjusted to 0.7 to 1.3 equivalents, more preferably 0.8 to 1.2 equivalents, and even more preferably 0.9 to 1.1 equivalents, based on the total of the hydroxyl group equivalent of the polycarbonate polyol copolymer (A) plus the equivalent of the functional group of the chain extender (adding the amine equivalent when amines are used).

[0153] The chain extender can be used to adjust the physical properties of the cured polyurethane, such as strength, abrasion resistance, flexibility, etc. In addition, by using a polyhydric alcohol as a chain extender, the crosslink density of the resulting polyurethane can be increased, and the strength, abrasion resistance, and chemical resistance can be improved, so that the resulting polyurethane can be suitably used, particularly, for the skin material of synthetic leather.

[0154] In the production of the polyurethane of this embodiment, an inert organic solvent may be included as necessary to adjust workability. The content of the inert organic solvent is preferably 80% by mass or less, more preferably 3% by mass or more and 60% by mass or less, and even more preferably 5% by mass or more and 40% by mass or less, based on the total amount of the polyurethane production raw materials. The inert organic solvent reduces the viscosity of the polyurethane, and improves the workability of application to the base fabric of the polyurethane coating agent, the adhesive phase of the synthetic leather, and the surface layer phase in particular. In addition, the addition of an inert organic solvent is effective in further improving the appearance of the obtained coating and synthetic leather. On the other hand, it is preferable to keep the content of the inert organic solvent to a low amount from the viewpoint of reducing the environmental load.

[0155] The inert organic solvent is not particularly limited as long as it is an organic solvent that is substantially inert to polyisocyanate, and is preferably one that does not have active hydrogen. The inert organic solvent is not particularly limited, but examples thereof include hydrocarbons such as pentane, hexane, heptane, octane, decane, petroleum ether, petroleum benzine, ligroin, petroleum spirit, cyclohexane, and methylcyclohexane; fluorine-based inert liquids such as trichlorofluoroethane, tetrachlorodifluoroethane, and perfluoroether fluorinated oils; perfluorocyclohexane, perfluorobutyltetrahydrofuran, perfluorodecalin, perfluoro-n-butylamine, perfluoropolyether, and dimethylpolysiloxane. These may be used alone or as a mixture. The inert organic solvent may further include methyl ethyl ketone (also referred to as MEK), acetone, ethyl acetate, butyl acetate, N,N-dimethylformamide (DMF), toluene, xylene, and other single or mixed solvents.

[0156] To the polyurethane using the polycarbonate polyol copolymer (A) of the present embodiment, a curing accelerator (catalyst), a filler, a flame retardant, a dye, an organic or inorganic pigment, a release agent, a flowability adjusting agent, a plasticizer, an antioxidant, an ultraviolet absorber, a light stabilizer, an antifoaming agent, a leveling agent, a colorant, a foaming agent, and the like can be added depending on various applications.

[0157] The curing accelerator is not particularly limited, but examples thereof include amines and metal catalysts.

[0158] The amine curing accelerator is not particularly limited, but examples thereof include monoamines such as triethylamine and N,N-dimethylcyclohexylamine, diamines such as tetramethylethylenediamine, other triamines, cyclic amines, alcohol amines such as dimethylethanolamine, and ether amines.

[0159] The metal catalyst is not particularly limited, but examples thereof include potassium acetate, potassium 2-ethylhexanoate, calcium acetate, lead octoate, dibutyltin dilaurate, tin octoate, bismuth neodecanoate, bismuth oxycarbonate, bismuth 2-ethylhexanoate, zinc octoate, zinc neodecanoate, phosphine, and phospholine.

[0160] The fillers and pigments are not particularly limited, but examples thereof include woven fabric, glass fiber, carbon fiber, polyamide fiber, mica, kaolin, bentonite, metal powder, azo pigments, carbon black, clay, silica, talc, gypsum, alumina white, barium carbonate, and the like.

[0161] The release agent, flow control agent, and leveling agent are not particularly limited, but examples thereof include silicone, aerosil, wax, stearates, and polysiloxanes such as BYK-331 (manufactured by BYK Chemicals).

[0162] As additives for the polyurethane using the polycarbonate polyol copolymer (A) of this embodiment, at least an antioxidant, a light stabilizer and a heat stabilizer are preferably used.

[0163] The antioxidant is not particularly limited, but examples thereof include phosphorus compounds such as aliphatic, aromatic, or alkyl group-substituted aromatic esters of phosphoric acid, phosphorous acid, hypophosphorous acid derivatives, phenylphosphonic acid, phenylphosphinic acid, diphenylphosphonic acid, polyphosphonates, dialkyl pentaerythritol diphosphites, and dialkyl bisphenol A diphosphites; phenol derivatives, particularly hindered phenol compounds; sulfur-containing compounds such as thioethers, dithioacid salts, mercaptobenzimidazoles, thiocarbanilides, and thiodipropionates; and tin compounds such as tin maleates and dibutyltin monoxide. These may be used alone or in combination of two or more.

[0164] In recent years, in consideration of environmental considerations, aqueous polyurethane dispersions are used for polyurethane coating agents, adhesive phases of synthetic leathers, surface layers, etc. The polycarbonate polyol copolymer (A) of the present embodiment can be suitably used as a raw material for aqueous polyurethanes.

[0165] The water-based polyurethane dispersion of this embodiment is obtained by dispersing the above-mentioned polyurethane in water.

[0166] The aqueous polyurethane dispersion of the present embodiment is not particularly limited, but can be obtained, for example, by dispersing in water a water-dispersible polyurethane obtained by reacting the above-mentioned polycarbonate polyol copolymer (A) with an organic polyisocyanate compound containing two or more isocyanate groups in one molecule, and a carboxyl group- and / or sulfone group-containing polyol or a salt thereof.

[0167] The organic polyisocyanate compound used in producing the aqueous polyurethane dispersion of this embodiment is not particularly limited as long as it is an organic polyisocyanate compound containing two or more isocyanate groups in one molecule. Examples of organic polyisocyanate compounds include, but are not limited to, aromatic, aliphatic, and alicyclic organic diisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, cyclohexane diisocyanate, tolylene diisocyanate, hexamethylene diisocyanate (HDI), trimethylhexane diisocyanate, 1,5-naphthalene diisocyanate, xylylene diisocyanate, 2,6-diisocyanate methylcaproate, isophorone diisocyanate (IPDI), methylcyclohexane-2,4-(or 2,6-)diisocyanate, and 4,4'-methylenebis(cyclohexylisocyanate), or multimers containing polyfunctional isocyanate groups such as biuret and isocyanurate forms thereof, or these isocyanates used alone or in mixtures.

[0168] Particularly from the viewpoint of weather resistance, aliphatic and alicyclic diisocyanates such as HDI, IPDI, dodecane diisocyanate, cyclohexane diisocyanate and dicyclohexylmethane diisocyanate, or these isocyanates used alone or in mixtures are preferred.

[0169] The carboxyl group- and / or sulfone group-containing polyol or its salt used in the production of the aqueous polyurethane dispersion of this embodiment is a component used for introducing a carboxylate group or a sulfonate group for the purpose of self-emulsifying the water-dispersible polyurethane in water and imparting dispersion stability to the aqueous polyurethane dispersion. The carboxyl group-containing polyol is not particularly limited, but examples thereof include 2,2-dimethylolpropionic acid (DMPA), 2,2-dimethylolbutanoic acid, 2,2-dimethylolheptanoic acid, and 2,2-dimethyloloctanoic acid. The sulfone group-containing polyol is not particularly limited, but examples thereof include sulfonic acid diol {3-(2,3-dihydroxypropoxy)-1-propanesulfonic acid} and sulfamic acid diol {N,N-bis(2-hydroxylalkyl)sulfamic acid} and their alkylene oxide adducts. The salts of these carboxyl group- and / or sulfone group-containing polyols are not particularly limited, but examples thereof include ammonium salts, amine salts [salts of primary amines having 1 to 12 carbon atoms (primary monoamines, for example, methylamine, ethylamine, propylamine, and octylamine), salts of secondary monoamines (dimethylamine, diethylamine, and dibutylamine), salts of tertiary monoamines (aliphatic tertiary monoamines such as trimethylamine, triethylamine, triethanolamine, N-methyldiethanolamine, and N,N-dimethylethanolamine; heterocyclic tertiary monoamines such as N-methylpiperidine and N-methylmorpholine; aromatic ring-containing tertiary monoamines such as benzyldimethylamine, α-methylbenzyldimethylamine, and N-dimethylaniline)], salts of alkali metals (sodium, potassium, and lithium cations), and combinations of two or more of these salts.

[0170] Among the salts, amine salts are preferred, aliphatic tertiary monoamine salts are more preferred, and triethylamine salts are particularly preferred.

[0171] When the polyol is not a salt but is a carboxyl- and / or sulfone-containing polyol, the carboxyl and / or sulfone groups can be neutralized to carboxylate and / or sulfonate groups using a neutralizing agent.

[0172] The neutralizing agent is not particularly limited, but may be, for example, an alkaline compound that forms the cations listed as the counter ions.Specific examples include, but are not particularly limited to, ammonia, amines [primary amines having 1 to 12 carbon atoms (primary monoamines, such as methylamine, ethylamine, propylamine, and octylamine), secondary monoamines (dimethylamine, diethylamine, and dibutylamine), tertiary monoamines (aliphatic tertiary monoamines such as trimethylamine, triethylamine, triethanolamine, N-methyldiethanolamine, and N,N-dimethylethanolamine; heterocyclic tertiary monoamines such as N-methylpiperidine and N-methylmorpholine; aromatic ring-containing tertiary monoamines such as benzyldimethylamine, α-methylbenzyldimethylamine, and N-dimethylaniline)], alkali metals (sodium, potassium, and lithium cations), alkali metal hydroxides, and combinations of two or more of these.

[0173] Among these, preferred are amines, more preferred are aliphatic tertiary monoamines, and particularly preferred is triethylamine.

[0174] The amount of the carboxyl group- and / or sulfone group-containing polyol or its salt used is preferably such that the carboxyl group and / or sulfone group is 0.01 to 10% by weight relative to the weight of the water-dispersible polyurethane. The ratio of the carboxyl group and / or sulfone group to the weight of the water-dispersible polyurethane is more preferably 0.1 to 7% by weight, and even more preferably 0.5 to 5% by weight. When the carboxyl group and / or sulfone group is 0.01% by weight or more, the dispersion stability of the water-based polyurethane dispersion tends to be more excellent. Also, when the content is 10% by weight or less, the water resistance of the obtained film tends to be more excellent.

[0175] Emulsion stability may also be maintained by using in combination with a suitable surfactant, such as an anionic surfactant typified by higher fatty acids, resin acids, acidic fatty alcohols, sulfates, higher alkyl sulfonates, alkylaryl sulfonates, sulfonated castor oil, sulfosuccinates, etc., or a nonionic surfactant typified by a known reaction product of ethylene oxide with a long-chain fatty alcohol or a phenol. Of these, the preferred surfactants are nonionic surfactants.

[0176] The method for producing the aqueous polyurethane dispersion of the present embodiment is not particularly limited, but may be, for example, the following method. In the presence or absence of an organic solvent not containing an active hydrogen-containing group in the molecule (e.g., acetone, methyl ethyl ketone, tetrahydrofuran, N,N-dimethylformamide, etc.), an organic polyisocyanate containing two or more isocyanate groups in one molecule, the above-mentioned polycarbonate polyol copolymer (A), and a carboxyl group- and / or sulfone group-containing polyol or a salt thereof are reacted by a one-shot method or a multi-stage method at an (NCO group / OH group) equivalent ratio of preferably 0.5 to 1.5, more preferably 0.8 to 1.2, and even more preferably 0.9 to 1.1 to synthesize polyurethane, and then neutralize the polyurethane with a neutralizing agent as necessary. Water is dropped into the resulting reaction solution while vigorously stirring, and the solvent is removed as necessary after the dropwise addition to obtain an aqueous polyurethane dispersion.

[0177] It is also possible to add the above-obtained reaction liquid to water with stirring to disperse it, and then remove the solvent as necessary to obtain an aqueous polyurethane dispersion.

[0178] By having an (NCO group / OH group) equivalent ratio of 0.5 or more, the molecular weight of the polyurethane obtained can be increased, and a more stable aqueous dispersion tends to be obtained, and furthermore, the strength and flexibility of the film formed by the aqueous polyurethane dispersion containing the aqueous polyurethane dispersion as a constituent tends to be superior. Similarly, by having an (NCO group / OH group) equivalent ratio of 1.5 or less, the molecular weight of the polyurethane obtained can be increased, and a more stable aqueous dispersion tends to be obtained, and furthermore, the strength and flexibility of the film formed by the aqueous soft-feel coating composition containing the aqueous polyurethane dispersion as a constituent tends to be superior.

[0179] In addition, as a method for producing the aqueous polyurethane dispersion of this embodiment, it is also possible to synthesize a prepolymer in advance from (a) an organic polyisocyanate containing two or more isocyanate groups in one molecule, the above-mentioned polycarbonate polyol copolymer (A), and (c) a carboxyl group- and / or sulfone group-containing polyol or a salt thereof under conditions of excess isocyanate, disperse this prepolymer in water, and then add a chain extender to form an aqueous polyurethane dispersion.

[0180] The chain extender is not particularly limited, but examples thereof include water, short-chain diols such as ethylene glycol, 1,3-propanediol, and 1,4-butanediol, and polyamines such as hydrazine, ethylenediamine, diethyltriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, propylenediamine, hexamethylenediamine, and cyclohexylenediamine. The amount of the chain extender added is usually 0 to 1.2 mol, and preferably 0.1 to 0.6 mol, per mol of isocyanate groups in the urethane prepolymer.

[0181] In the process of producing the aqueous polyurethane dispersion of this embodiment, a known urethanization reaction catalyst can be used as necessary. The urethanization reaction catalyst is not particularly limited, but includes, for example, amine catalysts such as triethylamine, N-ethylmorpholine, triethylenediamine, etc., tin catalysts such as dibutyltin dilaurate, dioctyltin dilaurate, and tin octylate, and titanium catalysts such as tetrabutyl titanate.

[0182] The solids content of the aqueous polyurethane dispersion of this embodiment is preferably from 10 to 70% by mass, and more preferably from 20 to 60% by mass.

[0183] The particle size of the aqueous polyurethane dispersion of this embodiment is preferably 500 nm or less, more preferably 200 nm or less, and even more preferably 150 nm or less. When the particle size of the aqueous polyurethane is 500 nm or less, the appearance, strength, and abrasion resistance of the coating film using the aqueous polyurethane dispersion tend to be more excellent, which is preferable.

[0184] To the aqueous polyurethane dispersion of this embodiment, a filler, a flame retardant, a dye, an organic or inorganic pigment, a release agent, a flowability modifier, a plasticizer, an antioxidant, an ultraviolet absorber, a light stabilizer, an antifoaming agent, a leveling agent, a colorant, a solvent, and the like can be added depending on various applications.

[0185] The filler or pigment is not particularly limited, but examples of commonly used fillers and pigments that can be used include woven fabric, glass fiber, carbon fiber, polyamide fiber, mica, kaolin, bentonite, metal powder, azo pigments, carbon black, clay, silica, talc, gypsum, alumina white, barium carbonate, and resin fine particles.

[0186] The release agent, flow control agent, and leveling agent are not particularly limited, but examples thereof include silicone, aerosil, wax, stearates, and polysiloxanes such as BYK-331 (manufactured by BYK Chemicals).

[0187] The additives used in the aqueous polyurethane dispersion of this embodiment are preferably at least an antioxidant, a light stabilizer, and a heat stabilizer.These antioxidants are not particularly limited, but may be, for example, phosphoric acid, phosphorous acid aliphatic, aromatic, or alkyl-substituted aromatic esters, hypophosphorous acid derivatives, phosphorus compounds such as phenylsulfonic acid, phenylphosphinic acid, diphenylphosphonic acid, polyphosphonates, dialkyl pentaerythritol diphosphite, and dialkyl bisphenol A diphosphite; phenol derivatives, particularly hindered phenol compounds, choethers, and dithioacid salts; sulfur-containing compounds such as mercaptobenzimidazoles, thiocarbanilides, and thiodipropionates; and tin compounds such as tin maleates and dibutyltin monoxide.These may be used alone or in combination of two or more.

[0188] The method for applying the aqueous polyurethane dispersion of the present embodiment is not particularly limited, but examples include a method in which the aqueous polyurethane dispersion is mixed with each additive component and then applied to a substrate with a spray, a roll, a blade, a brush, or the like.

[0189] [Manufacturing method of synthetic leather] The synthetic leather of the present embodiment contains polyurethane.

[0190] The synthetic leather of the present embodiment can be produced, for example, from a polyurethane using the above-mentioned polycarbonate polyol copolymer (A).

[0191] The synthetic leather of the present embodiment is preferably a synthetic leather in which a base fabric, an adhesive layer, an intermediate layer, and a surface layer are laminated in this order. Examples of methods for producing the synthetic leather of the present embodiment include a wet method in which a polyurethane using the above-mentioned polycarbonate polyol copolymer (A) is applied to or impregnated into a substrate (base fabric) and wet-coagulated, and a dry method in which a polyurethane using the above-mentioned polycarbonate polyol copolymer (A) is applied to a release paper or a substrate (base fabric) and dried.

[0192] Furthermore, as a method for producing synthetic leather, a transfer coating method (a type of dry method) can also be used in which a polyurethane using the above-mentioned polycarbonate polyol copolymer (A) is applied to release paper to form a skin material, and then the polyurethane using the above-mentioned polycarbonate polyol copolymer (A) is used as an adhesive layer on top of the skin material, and the base material (base fabric) is bonded to the skin material, and the release paper is then removed.

[0193] The method for producing synthetic leather will be explained below using the dry method as an example.

[0194] Various substrates (base fabrics) can be used, and examples thereof include, but are not limited to, fibrous substrates. Examples of fibrous substrates include, but are not limited to, fiber aggregates in which fibers are shaped into nonwoven fabrics, woven fabrics, net fabrics, etc., or fiber aggregates in which each fiber is bonded with an elastic polymer. Examples of fibers used in the fiber aggregate include, but are not limited to, natural fibers such as cotton, hemp, and wool, regenerated or semi-synthetic fibers such as rayon and acetate, and synthetic fibers such as polyamide, polyester, polyacrylonitrile, polyvinyl alcohol, and polyolefin. These fibers may be either single spun fibers or mixed spun fibers. Examples of other substrates include, but are not limited to, paper, release paper, plastic films of polyester or polyolefin, metal plates such as aluminum, glass plates, etc. The polyurethane using the polycarbonate polyol copolymer (A) of the present embodiment can be applied by a commonly used method. The application method is not particularly limited, but can include, for example, a floating knife coater, a knife over roll coater, a reverse roll coater, a roll doctor coater, a gravure roll coater, a kiss roll coater, etc. The synthetic leather obtained can be used as it is. Alternatively, the synthetic leather can be obtained in a form in which a polymer solution or emulsion of polyurethane resin, vinyl chloride, cellulose resin, or the like is applied to the synthetic leather for the purpose of imparting various properties. The synthetic leather can also be obtained in a form of a laminate obtained by laminating a coating film obtained by drying the above-mentioned polymer solution or emulsion that has been applied separately to a release paper, and then peeling off the release paper.

[0195] [Application] The polycarbonate polyol copolymer (A) of the present embodiment can be used as a raw material for polyurethane to be reacted with polyisocyanate, and the polyurethane has excellent strength, flexibility, oleic acid resistance, abrasion resistance, low temperature properties, and resistance to decomposition, and therefore can be widely used in foams, elastomers, paints, coating agents, pressure sensitive adhesives, adhesives, artificial leather, synthetic leather, water-based polyurethane paints, etc. Furthermore, it can be used as a modifier for polyesters and polyimides, etc. EXAMPLES

[0196] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples as long as it does not depart from the gist of the invention. In the following examples and comparative examples, the methods for analyzing and evaluating the physical properties of each component are as follows.

[0197] [Analysis and Evaluation of Polycarbonate Polyol Copolymer (A)] <Hydroxyl value of polycarbonate polyol copolymer (A)> Measurements were performed in accordance with JIS K1557-1. <Number average molecular weight (Mn) of polycarbonate diol copolymer (A)> The hydroxyl value was determined according to JIS K1557-1, and the number average molecular weight (Mn) of the polycarbonate diol was calculated using the following formula (II). Number average molecular weight (Mn) = 56.1 x 2 x 1000 ÷ hydroxyl value (II)

[0198] <Appearance of polycarbonate polyol copolymer (A)> After synthesis of the polycarbonate polyol copolymer (A), it is left to stand at 23° C. for 10 days and then visually evaluated.

[0199] <Composition of polycarbonate polyol copolymer (A) (copolymerization ratio)> 1 g of a sample of polycarbonate polyol copolymer (A) was taken in a 100 mL eggplant flask, 30 g of ethanol, and 4 g of potassium hydroxide were added, and the mixture was reacted at 100 ° C for 1 hour. After cooling the reaction solution to room temperature, 2 to 3 drops of phenolphthalein were added as an indicator, and the mixture was neutralized with hydrochloric acid. The neutralized reaction solution was cooled in a refrigerator for 1 hour, and the precipitated salt was removed by filtration, and the filtrate was analyzed using gas chromatography (GC). GC analysis was performed using a gas chromatograph GC-14B (Shimadzu Corporation, Japan) equipped with a DB-WAX (J&W, USA) column, diethylene glycol diethyl ester as an internal standard, and a flame ionization detector (FID) as a detector, and quantitative analysis of each component was performed. The column temperature rise profile was a profile in which the temperature was held at 60 ° C for 5 minutes, and then raised to 250 ° C at 10 ° C / min. From the molar ratio of each alcohol component detected from the above analysis results, the composition of the polycarbonate polyol component (a1) constituting the polycarbonate polyol copolymer (A) was obtained. The proportion of the dimer diol component (a2) was calculated on the assumption that the dimer diol component (a2) was not distilled off by polymerization and was entirely incorporated into the polycarbonate polyol copolymer (A) obtained based on the charged weight.

[0200] <Measurement of Melt Viscosity of Polycarbonate Polyol Copolymer (A)> The polycarbonate polyol copolymer (A) was preheated to 50° C., and then the melt viscosity was measured at 50° C. using an E-type viscometer (manufactured by Toki Sangyo Co., Ltd., TVE-22HT, cone: No. 6).

[0201] <Biomass Degree of Polycarbonate Polyol Copolymer (A)> The biomass degree of the polycarbonate polyol copolymer (A) was measured as follows. Specifically, the concentration of C14 present in the polycarbonate polyol copolymer (A) was measured by accelerator mass spectrometry to determine the content ratio of carbon derived from living organisms present in the polycarbonate polyol copolymer (A). The concentration of C14 in the polycarbonate polyol copolymer (A) was measured as follows. That is, the measurement sample was burned to generate carbon dioxide, and the carbon dioxide purified in a vacuum line was reduced with hydrogen using iron as a catalyst to purify graphite. Then, this graphite was attached to a tandem accelerator-based C14-AMS dedicated device (manufactured by NEC Corporation) to measure the counting of C14, the concentration of C13 (C13 / C12), and the concentration of C14 (C14 / C12), and the ratio of the C14 concentration of the sample carbon to the standard modern carbon was calculated from the measured values. The standard sample used was oxalic acid (HOXII) provided by the National Institute of Standards (NIST). From the measured values, the biomass degree was calculated using δ13C-corrected pMC (percent modern carbon) according to ASTM D6866-21.

[0202] <Glass transition temperature of polycarbonate polyol copolymer (A)> The glass transition temperature of the polycarbonate polyol copolymer (A) was measured by a differential scanning calorimeter. Specifically, about 20 mg of the polycarbonate diol copolymer (A) was sealed in an aluminum pan, and a differential scanning calorimeter (DSC7000X, Hitachi High-Techno Science Co., Ltd.) was used to raise and lower the temperature from 30°C to 100°C at a rate of 20°C per minute, from 100°C to -100°C at a rate of 5°C per minute, and from -100°C to 100°C at a rate of 5°C per minute under a nitrogen atmosphere, and the inflection point (peak of the differential curve) at the second temperature rise was determined as the glass transition temperature (Tg). The lower the glass transition temperature (Tg), the better the low-temperature properties are evaluated to be.

[0203] <Water absorption rate of polycarbonate polyol copolymer (A)> The water absorption rate of the polycarbonate polyol copolymer (A) was measured after 7 days under an atmosphere of 85°C and 85% relative humidity. Specifically, 50 g of the polycarbonate polyol copolymer was precisely weighed in a glass petri dish (60 mmφ, 17 mm deep) and left in a thermo-hygrostat under an atmosphere of 85°C and 85% relative humidity for 7 days. After removing the polycarbonate polyol copolymer, the mass was immediately measured, and the rate of increase in mass was calculated from the following formula (II) to be the water absorption rate (%). Water absorption rate (%) = {(mass after test - mass before test) / mass before test} x 100 (II) The lower the water absorption rate, the more excellent the moist heat resistance is evaluated.

[0204] <Carbonate group content in polycarbonate polyol copolymer (A)> The carbonate group content in the polycarbonate polyol copolymer (A) was measured as follows. The carbonate group content is the mass proportion of the carbonate groups contained in the polycarbonate polyol copolymer (A), and specifically, was calculated by the following formula (III). Carbonate group content (%)={(carbonate group molecular weight)×(number of repeating units (n) in polycarbonate polyol component (a1)) / (number average molecular weight of polycarbonate polyol copolymer (A))×100 (III) (Here, the carbonate group molecular weight (-OC=OO-) is 60.01.) The number of repeating units (n) in the polycarbonate polyol component (a1) was calculated using the following formula (IV) based on the structure of the polycarbonate polyol component (a1) represented by the following formula (8). [ka] (Here, m is the average methylene number, n is the number of repeating units of the polycarbonate polyol component (a1), and the underlined parts represent terminal groups.) The average methylene number m of the polycarbonate polyol component (a1) was determined from the composition (copolymerization ratio) of the polycarbonate polyol component (a1). Number of repeating units (n) in polycarbonate polyol component (a1)={(number average molecular weight (M1) of polycarbonate component (a1)-terminal group molecular weight)} / (molecular weight of repeating unit) (IV) (Here, the number average molecular weight (M1) of the polycarbonate polyol component (a1) was calculated by multiplying the number average molecular weight of the polycarbonate polyol copolymer (A) by the mass proportion of the polycarbonate polyol component (a1).)

[0205] [Analysis and evaluation of polyurethane] <Preparation of polyurethane film> The polyurethane solution or aqueous dispersion obtained in the examples and comparative examples described below was preheated to 40°C, and then applied to a polypropylene resin sheet (width 100mm, length 1200mm, thickness 1mm) with an applicator to a width of 80mm, length 100mm, and thickness of 0.8mm, and dried on a hot plate with a surface temperature of 60°C for 2 hours, and then in an oven at 100°C for 12 hours. The polyurethane film was then left to stand at a constant temperature and humidity of 23°C and 55%RH for 12 hours or more to obtain a polyurethane film. The obtained polyurethane film was subjected to evaluation of various physical properties.

[0206] <Evaluation method for tensile breaking strength, breaking elongation, and 100% modulus> A sample with a width of 10 mm and a length of 60 mm was cut out from the polyurethane film. In a thermostatic chamber at 23°C, the tensile breaking strength (MPa), elongation at break (%), and stress at 100% elongation (100% modulus: MPa) of the film were measured using a Universal Testing Machine (Zwick Corp.) with a chuck distance of 20 mm and a pulling speed of 10 mm / min. The lower the stress at 100% elongation, the softer and more flexible the film is. The breaking strength is preferably 31 or more, more preferably 33 or more, and even more preferably 38 or more. The breaking elongation is preferably 450 or more, more preferably 460 or more, and even more preferably 470 or more. The 100% modulus is preferably 8.8 or less, more preferably 8.0 or less, and even more preferably 7.9 or less.

[0207] <Oleic acid swelling rate> A sample with a width of 10 mm and a length of 60 mm was cut out from the polyurethane film. This polyurethane film was immersed in oleic acid at 23°C for one week (7 days) and then the swelling ratio (degree of swelling) was measured. The swelling ratio was calculated using the following formula (III). The lower the swelling ratio (%), the better the chemical resistance is evaluated to be. Swelling ratio (%) = {(mass after test - mass before test) / mass before test} x 100 (III)

[0208] <Abrasion resistance> The abrasion resistance of the prepared polyurethane film was measured using a Taber abrasion tester in accordance with the method of JIS K5600-5-8 (abrasion wheel CS-10, weight 500 g, 500 revolutions). The mass change (mg) between the mass of the coated film plate before the abrasion test and the mass of the coated film plate after the abrasion test was measured and expressed. The smaller the mass change (mg), the better the abrasion resistance is evaluated to be. As a guideline, a mass change of less than 5.0 mg can be judged to have good abrasion resistance. A mass change of 3.5 mg or less is preferable, and a mass change of 3.2 mg or less is more preferable.

[0209] <Measurement of low-temperature properties (glass transition temperature)> A sample with a width of 10 mm and a length of 40 mm was cut out from the polyurethane film. The cut out film piece was used to measure the viscoelasticity using a viscoelasticity measuring device (Hitachi High-Tech Science Corporation, [TA7000 series, DMA7100]), with the test piece set at a chuck distance of 20 mm, and the temperature was raised from -100°C to 100°C at a rate of 5°C / min. The peak temperature of tan δ was read to determine the glass transition temperature (Tg). The lower the glass transition temperature (Tg), the better the low-temperature properties are evaluated to be. Although it depends on the application, if the glass transition temperature of the polyurethane film is -9°C or lower, the low-temperature properties are generally good. The glass transition temperature of the polyurethane film is preferably -11°C or lower, more preferably -12°C or lower.

[0210] <Evaluation of hydrolysis resistance> A sample with a width of 10 mm and a length of 40 mm was cut out from the polyurethane film. It was heated in a thermo-hygrostat at a temperature of 70°C and a relative humidity of 95% for 400 hours. The breaking strength of the heated sample was measured in the same manner as in the above <Evaluation method of tensile breaking strength, breaking elongation, and 100% modulus>, and its retention rate (%) was calculated. From the viewpoint of practical use, it is desirable for the hydrolysis resistance to be higher than 86%, and more desirably higher than 90%.

[0211] <Number average molecular weight (Mn) of polyurethane> The number average molecular weight (Mn) of the polyurethane was measured as follows. The polyurethane concentration was adjusted to 0.1% by mass with an N,N-dimethylformamide (DMF) solution to obtain a sample. The number average molecular weight (Mn) of the polyurethane was measured in terms of standard polystyrene using the following gel permeation chromatography (GPC) device. GPC equipment: Tosoh HLC-8320 Column: HLC-8220 x 3 Eluent: N-dimethylformamide (DMF) Flow rate: 1.0mL / min Column temperature: 40℃ RI detector: RI (built into the device HLC-8320)

[0212] [Example 1] In a 1L separable flask equipped with a stirrer, a thermometer, and a vacuum jacketed Oldershaw flask with a reflux head at the top, 136g of 1,4-butanediol, 204g of 1,6-hexanediol, 175g of dimer diol (CRODA, product name Pripol 2033), and 290g of ethylene carbonate were charged as raw material monomers. 16.3mg of manganese (II) acetate tetrahydrate and 6.7mg of lithium methoxide were added as catalysts, and the reaction was carried out for 5 hours while distilling off the mixture of ethylene glycol and ethylene carbonate produced at a reaction temperature of 140 to 160°C and a pressure of 10 kPa to 2 kPa. Then, the reaction was switched to simple distillation, and the pressure was gradually reduced to 0.5 kPa while the reaction was continued at 180°C for 2 hours to distill off the monomers, thereby obtaining a polycarbonate diol copolymer. The results of the analysis of the obtained polycarbonate diol copolymer are shown in Tables 1-2 and 1-3. The polycarbonate polyol copolymer is referred to as PC1.

[0213] [Examples 2 to 13] Except for the types and amounts of diol, dimer diol and ethylene carbonate added being as shown in Table 1-1, polycondensation was carried out by transesterification in the same manner as in Example 1 to obtain a polycarbonate polyol copolymer. The physical properties of the obtained polycarbonate polyol are shown in Tables 1-2 and 1-3.

[0214] [Table 1-1]

[0215] [Table 1-2]

[0216] [Table 1-3]

[0217] [Comparative Examples 1 to 5] Except for the types and amounts of diol, dimer diol and ethylene carbonate added being as shown in Table 2-1, polycondensation was carried out by transesterification in the same manner as in Example 1 to obtain a polycarbonate polyol copolymer. The physical properties of the obtained polycarbonate polyol are shown in Tables 2-2 and 2-3.

[0218] [Table 2-1]

[0219] [Table 2-2]

[0220] [Table 2-3]

[0221] [Example 14] In a 500 mL separable flask equipped with a stirrer sealed with nitrogen gas, 15.34 g of diphenylmethane-4,4'-diisocyanate (MDI, average number of isocyanate groups in one molecule: 2.0) and 80 g of N,N-dimethylformamide (DMF) were charged and heated to 40 ° C. to obtain a solution. In the flask, 60 g of N,N-dimethylformamide (DMF) and 40.0 g of polycarbonate polyol copolymer PC1 to which 0.0028 g of dibutyltin dilaurate was added as a catalyst were dropped over 30 minutes under stirring. The mixture was reacted at 60 ° C. for 2 hours under stirring to obtain a prepolymer with terminal isocyanate. Next, 3.6 g of 1,4-butanediol was added as a chain extender, and the reaction was carried out at 60 ° C. for 1 hour, after which 0.5 g of ethanol was added as a reaction terminator to obtain a DMF solution of polyurethane (solid content about 30 mass %). A polyurethane film was prepared by the above-mentioned <Preparation of polyurethane film> method and subjected to evaluation of various physical properties. The evaluation results of the polyurethane film are shown in Table 3.

[0222] [Examples 15 to 19] Polyurethane films were obtained using PC2 to PC6 as the polycarbonate polyol copolymers in the same manner as in Example 14, and were subjected to evaluation of various physical properties. The evaluation results are shown in Table 3.

[0223] [Example 20] A polyurethane film was obtained in the same manner as in Example 14, except that PC7 was used as the polycarbonate polyol copolymer and the amount of PC7 used was 80.0 g, and the film was subjected to evaluation of various physical properties. The evaluation results are shown in Table 3.

[0224] [Example 21] A polyurethane film was obtained in the same manner as in Example 14, except that PC8 was used as the polycarbonate polyol copolymer and the amount of PC8 used was 20.0 g, and the film was subjected to evaluation of various physical properties. The evaluation results are shown in Table 4.

[0225] [Examples 22 to 26] Polyurethane films were obtained using PC9 to PC13 as the polycarbonate polyol copolymers in the same manner as in Example 14, and were subjected to evaluation of various physical properties. The evaluation results are shown in Table 4.

[0226] [Comparative Examples 6 to 10] Polyurethane films were obtained using PC14 to PC18 as the polycarbonate polyol copolymers in the same manner as in Example 14, and were subjected to evaluation of various physical properties. The evaluation results are shown in Table 5.

[0227] [Table 3]

[0228] [Table 4]

[0229] [Table 5]

[0230] [Example 27] In a 1000mL four-neck flask equipped with a stirrer, a cooling tube, a nitrogen inlet tube, and a thermometer, 33.3g of isophorone diisocyanate (IPDI, average number of isocyanate groups per molecule: 2.0), 100g of polycarbonate polyol copolymer PC1, 6.7g (0.05 mol) of 2,2-dimethylolpropionic acid (DMPA), 6.1g (0.05 mol) of triethylamine (TEA), and 30mL of methyl ethyl ketone (MEK) were added under a nitrogen atmosphere, and the mixture was reacted at 80°C for 2.5 hours to obtain a prepolymer solution with terminal isocyanate (NCO terminal). Next, 342g of deionized water was added and mixed with the prepolymer solution at 35°C to obtain a prepolymer dispersion. A solution containing 1.5g of ethylenediamine (EDA) as a chain extender in 2.0g of deionized water was added to the prepolymer dispersion, and the mixture was stirred at 30°C for 1 hour to obtain a mixture. The mixture was then heated to 80°C to remove the MEK, yielding an aqueous polyurethane dispersion with a solid content of 30% by mass. A polyurethane film was produced by the above-mentioned <Preparation of polyurethane film> method, and various physical properties were evaluated. The evaluation results of the polyurethane film are shown in Table 6.

[0231] [Examples 28 to 30] Polyurethane films were obtained in the same manner as in Example 27 using PC2, PC3, and PC5 as polycarbonate polyol copolymers and the isocyanate component and chain extender component shown in Table 6, and were subjected to evaluation of various physical properties. The evaluation results are shown in Table 6.

[0232] [Example 31] A polyurethane film was obtained in the same manner as in Example 27, except that PC7 was used as the polycarbonate polyol copolymer and the amount of PC7 used was 200.0 g, and the film was subjected to evaluation of various physical properties. The evaluation results are shown in Table 6.

[0233] [Example 32] A polyurethane film was obtained in the same manner as in Example 27, except that PC8 was used as the polycarbonate polyol copolymer and the amount of PC8 used was 50.0 g, and the film was subjected to evaluation of various physical properties. The evaluation results are shown in Table 7.

[0234] [Examples 33 to 36] Polyurethane films were obtained in the same manner as in Example 27 using PC2, PC9, PC10, and PC13 as polycarbonate polyol copolymers and the isocyanate component and chain extender component shown in Table 7, and were subjected to evaluation of various physical properties. The evaluation results are shown in Table 7.

[0235] [Comparative Examples 11 to 15] Polyurethane films were obtained in the same manner as in Example 27 using PC14 to PC18 as the polycarbonate polyol copolymers, and the isocyanate component and chain extender component shown in Table 8, and were subjected to evaluation of various physical properties. The evaluation results are shown in Table 8.

[0236] [Table 6]

[0237] [Table 7]

[0238] [Table 8]

[0239] [Example 37] In a 1L separable flask equipped with a stirrer, a thermometer, and a vacuum jacketed Oldershaw flask with a reflux head on top, 317g of 1,3-propanediol (manufactured by DuPont Specialty Products Co., Ltd., Susterra (registered trademark) Propandiol), 175g of dimer diol (manufactured by Croda, trade name Pripol 2033), and 369g of ethylene carbonate were charged as raw material monomers. 16.3mg of manganese (II) acetate tetrahydrate and 6.7mg of lithium methoxide were added as catalysts, and the reaction was carried out for 5 hours while distilling off the mixture of ethylene glycol and ethylene carbonate produced at a reaction temperature of 140 to 160°C and a pressure of 10 to 2kPa. Then, the reaction was switched to simple distillation, and the pressure was gradually reduced to 0.5 kPa while the reaction was continued at 180°C for 2 hours to distill off the monomers, thereby obtaining a polycarbonate diol copolymer. The results of the analysis of the obtained polycarbonate diol copolymer are shown in Tables 9-2 and 9-3. The polycarbonate polyol copolymer is called PC19.

[0240] [Examples 38 to 41] A polycarbonate polyol copolymer was obtained by polycondensation through transesterification in the same manner as in Example 37, except that the types and amounts of 1,3-propanediol, dimer diol and ethylene carbonate added were as shown in Table 9-1. The physical properties of the obtained polycarbonate polyol are shown in Tables 9-2 and 9-3.

[0241] [Comparative Examples 16 to 19] A polycarbonate polyol copolymer was obtained by polycondensation through transesterification in the same manner as in Example 37, except that the types and amounts of diol, dimer diol and ethylene carbonate added were as shown in Table 9-1. The physical properties of the obtained polycarbonate polyol copolymer are shown in Tables 9-2 and 9-3.

[0242] [Table 9-1]

[0243] [Table 9-2]

[0244] [Table 9-3]

[0245] [Example 42] In a 500mL separable flask equipped with a stirrer sealed with nitrogen gas, 15.34g of diphenylmethane-4,4'-diisocyanate (MDI, average number of isocyanate groups in one molecule: 2.0) and 80g of N,N-dimethylformamide (DMF) were charged and heated to 40°C to obtain a solution. 60g of N,N-dimethylformamide (DMF) and 40.0g of polycarbonate polyol copolymer PC19 to which 0.0028g of dibutyltin dilaurate was added as a catalyst were added dropwise to the flask over 30 minutes under stirring. The mixture was reacted at 60°C for 2 hours under stirring to obtain a prepolymer with terminal isocyanate. Next, 3.6g of 1,4-butanediol was added as a chain extender, and the reaction was carried out at 60°C for 1 hour, after which 0.5g of ethanol was added as a reaction terminator to obtain a DMF solution of polyurethane (solid content about 30% by mass). A polyurethane film was prepared by the above-mentioned <Preparation of polyurethane film> method and subjected to evaluation of various physical properties. The evaluation results of the polyurethane film are shown in Table 10.

[0246] [Examples 43 and 44] Using PC20 and PC21 as the polycarbonate polyol copolymers, polyurethane films were obtained in the same manner as in Example 42, and the physical properties were evaluated. The evaluation results are shown in Table 10.

[0247] [Example 45] A polyurethane film was obtained in the same manner as in Example 42, except that PC22 was used as the polycarbonate polyol copolymer and the amount of PC22 used was 20.0 g, and the film was subjected to evaluation of various physical properties. The evaluation results are shown in Table 10.

[0248] [Example 46] A polyurethane film was obtained in the same manner as in Example 42, except that PC23 was used as the polycarbonate polyol copolymer and the amount of PC23 used was 80.0 g, and the obtained film was subjected to evaluation of various physical properties. The evaluation results are shown in Table 10.

[0249] [Comparative Examples 20 to 23] Polyurethane films were obtained using PC24 to PC27 as the polycarbonate polyol copolymers, and the physical properties were evaluated in the same manner as in Example 42. The evaluation results are shown in Table 11.

[0250] [Table 10]

[0251] [Table 11]

[0252] [Example 47] In a 1000mL four-neck flask equipped with a stirrer, a cooling tube, a nitrogen inlet tube, and a thermometer, 33.3g of isophorone diisocyanate (IPDI, average number of isocyanate groups per molecule: 2.0), 100g of polycarbonate polyol copolymer PC19, 6.7g (0.05 mol) of 2,2-dimethylolpropionic acid (DMPA), 6.1g (0.05 mol) of triethylamine (TEA), and 30mL of methyl ethyl ketone (MEK) were added under a nitrogen atmosphere, and the mixture was reacted at 80°C for 2.5 hours to obtain a prepolymer solution with terminal isocyanate (NCO terminal). Next, 342g of deionized water was added and mixed with the prepolymer solution at 35°C to obtain a prepolymer dispersion. A solution containing 1.5g of ethylenediamine (EDA) as a chain extender in 2.0g of deionized water was added to the prepolymer dispersion, and the mixture was stirred at 30°C for 1 hour to obtain a mixture. The mixture was then heated to 80°C to remove the MEK, yielding an aqueous polyurethane dispersion with a solid content of 30% by mass. A polyurethane film was produced by the above-mentioned <Preparation of polyurethane film> method, and various physical properties were evaluated. The evaluation results of the polyurethane film are shown in Table 12.

[0253] [Examples 48 and 49] Polyurethane films were obtained in the same manner as in Example 47 using PC20 and PC21 as polycarbonate polyol copolymers, and the isocyanate component and chain extender component shown in Table 12, and were subjected to evaluation of various physical properties. The evaluation results are shown in Table 12.

[0254] [Example 50] A polyurethane film was obtained in the same manner as in Example 47, except that PC22 was used as the polycarbonate polyol copolymer and the amount of PC22 used was 50.0 g, and the film was subjected to evaluation of various physical properties. The evaluation results are shown in Table 12.

[0255] [Example 51] A polyurethane film was obtained in the same manner as in Example 47, except that PC23 was used as the polycarbonate polyol copolymer and the amount of PC23 used was 200.0 g, and the film was subjected to evaluation of various physical properties. The evaluation results are shown in Table 12.

[0256] [Example 52] A polyurethane film was obtained in the same manner as in Example 47, except that PC20 was used as the polycarbonate polyol copolymer, hydrogenated MDI was used as the isocyanate component, and the amount of hydrogenated MDI added was 39.3 g, and the film was subjected to evaluation of various physical properties. The evaluation results are shown in Table 12.

[0257] [Comparative Examples 24 to 27] Polyurethane films were obtained in the same manner as in Example 47 using PC24 to PC27 as the polycarbonate polyol copolymers, and the isocyanate component and chain extender component shown in Table 13, and were subjected to evaluation of various physical properties. The evaluation results are shown in Table 13.

[0258] [Table 12]

[0259] [Table 13]

Claims

1. A polycarbonate polyol copolymer (A) containing, as copolymerization components, a polycarbonate polyol component (a1) containing a repeating unit represented by the following formula (1) and a dimer diol component (a2), 50 mol % or more of the repeating units represented by the following formula (1) contain at least two kinds of repeating units selected from the group consisting of repeating units represented by the following formula (2), repeating units represented by the following formula (3), and repeating units represented by the following formula (4), or the repeating units represented by the following formula (1) are repeating units represented by the following formula (5): A polycarbonate polyol copolymer (A), in which the content of the polycarbonate polyol component (a1) is 10% by mass or more and 90% by mass or less, and the content of the dimer diol component (a2) is 10% by mass or more and 90% by mass or less, relative to 100% by mass of the total mass of the polycarbonate polyol component (a1) and the dimer diol component (a2). 【Chemistry 1】 (In formula (1), R1 is a divalent aliphatic or alicyclic hydrocarbon having 2 to 15 carbon atoms.) 【Chemistry 2】 【Chemistry 3】 【Chemistry 4】 【Chemistry 5】

2. The polycarbonate polyol copolymer (A) according to claim 1, wherein 50 mol % or more of the repeating units represented by the formula (1) contain at least two kinds of repeating units selected from the group consisting of the repeating units represented by the formula (2), the repeating units represented by the formula (3), and the repeating units represented by the formula (4).

3. The polycarbonate polyol copolymer (A) according to claim 2, wherein the carbonate group content in one molecule is 17 to 38 mass% and the number average molecular weight is 500 to 3000 g / mol.

4. The polycarbonate polyol copolymer (A) according to claim 2, which has a glass transition temperature of -50°C or lower as measured by a differential scanning calorimeter.

5. The polycarbonate polyol copolymer (A) according to claim 2, which has a water absorption rate of 0.8 mass% or less after 7 days in an atmosphere having a temperature of 85°C and a relative humidity of 85%.

6. The polycarbonate polyol copolymer (A) according to claim 2, having a biomass degree of 10% or more and 90% or less as measured by accelerator mass spectrometry.

7. The polycarbonate polyol copolymer (A) according to claim 2, which is liquid and transparent at 23°C.

8. A polyurethane obtained by using the polycarbonate polyol copolymer (A) according to any one of claims 2 to 7.

9. The polyurethane according to claim 8, which has a degree of swelling after immersion in oleic acid at 23°C for 7 days of 5% by mass or more and 35% by mass or less.

10. 9. A water-based polyurethane dispersion, comprising the polyurethane according to claim 8 dispersed in water.

11. 9. Synthetic leather comprising the polyurethane of claim 8.

12. A method for producing a polycarbonate polyol copolymer (A), comprising a step of polycondensing a dihydroxy compound, a dimer diol, and a carbonate ester as raw material monomers through an ester exchange reaction in the presence of an ester exchange catalyst to obtain a polycarbonate polyol copolymer (A).

13. In the polycondensation step, With respect to 100% by mass of the total mass of the dihydroxy compound and the dimer diol, The dihydroxy compound is present in an amount of 10% by mass or more and 90% by mass or less, The dimer diol has a mass ratio of 10% by mass to 90% by mass. The present invention is characterized in that the ester exchange reaction is carried out. A method for producing the polycarbonate polyol copolymer (A) according to claim 12.

14. The method for producing the polycarbonate polyol copolymer (A) according to claim 12, wherein the transesterification catalyst comprises a transesterification catalyst A1 containing at least one metal (M1) selected from the group consisting of metals in Group 7 of the long-form periodic table, and a transesterification catalyst A2 containing at least one metal (M2) selected from the group consisting of metals in Groups 1 and 2 of the long-form periodic table.

15. The method for producing a polycarbonate polyol copolymer (A) according to claim 14, wherein the metal (M1) is manganese, and the metal (M2) is at least one metal selected from the group consisting of lithium and calcium.

16. The method for producing a polycarbonate polyol copolymer (A) according to claim 12, wherein the dihydroxy compound is 1,3-propanediol.

17. The polycarbonate polyol copolymer (A) according to claim 1, wherein the repeating unit represented by the formula (1) is a repeating unit represented by the formula (5). 【Chemistry 6】

18. The polycarbonate polyol copolymer (A) according to claim 17, wherein the carbonate group content in one molecule is 20 to 45% by mass and the number average molecular weight is 500 to 3000 g / mol.

19. The polycarbonate polyol copolymer (A) according to claim 17, which has a glass transition temperature of -40°C or lower as measured by a differential scanning calorimeter.

20. The polycarbonate polyol copolymer (A) according to claim 17, which has a water absorption rate of 1.0 mass% or less after 7 days in an atmosphere at a temperature of 85°C and a relative humidity of 85%.

21. The polycarbonate polyol copolymer (A) according to claim 17, having a biomass degree of 70% or more and 95% or less as measured by accelerator mass spectrometry.

22. The polycarbonate polyol copolymer (A) according to claim 17, which is liquid and transparent at 23°C.

23. A polyurethane obtained by using the polycarbonate polyol copolymer (A) according to any one of claims 17 to 22.

24. The polyurethane according to claim 23, having a degree of swelling of 5% by mass or more and 30% by mass or less after immersion in oleic acid at 23° C. for 7 days.

25. 24. A water-based polyurethane dispersion, comprising the polyurethane according to claim 23 dispersed in water.

26. 24. Synthetic leather comprising the polyurethane of claim 23.

Citation Information

Patent Citations

  • Production of copolymerized polycarbonate diol

    JP1991252420A

  • Aqueous emulsion adhesive composition

    JP1991277680A

  • polyisocyanate

    JP1992130124A

  • Polyurethane resin composition for coating and production of thereof

    JP1992145118A

  • Thermoplastic polyester elastomer

    JP1994128363A