Rubber composition and use of rubber composition

A rubber composition with specific silane coupling agents and basic compounds enhances silica-rubber interaction, addressing viscosity issues and improving tire fuel efficiency and grip.

JP2024153078AInactive Publication Date: 2024-10-29OSAKA SODA CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2021122114
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-07-27
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Silane coupling agents used in silica-containing rubber compositions increase viscosity and reduce the interaction between silicas, leading to compromised fuel efficiency and grip in tires.

Method used

A rubber composition containing specific silane coupling agents and basic compounds, such as (R1O3Si-R2-S-C(=O)-C17H35, combined with inorganic fillers like wet silica, to enhance the interaction between silica and rubber, improving fuel efficiency and grip.

Benefits of technology

The composition results in tires with improved fuel efficiency and grip by optimizing the interaction between silica and rubber, reducing hysteresis loss and enhancing dynamic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153078000001
    Figure 2024153078000001
  • Figure 2024153078000002
    Figure 2024153078000002
  • Figure 2024153078000003
    Figure 2024153078000003
Patent Text Reader

Abstract

To provide a rubber composition capable of obtaining a tire having better fuel economy and excellent gripping property when using a known silane coupling agent in a rubber composition.SOLUTION: There is provided a rubber composition comprising rubber (A), an inorganic filler (B), a silane coupling agent (C) represented by the formula (1) and a basic compound (D), wherein the rubber is one selected from a natural rubber (NR), a polyisoprene rubber (IR), a styrene-butadiene copolymer rubber (SBR), a polybutadiene rubber (BR), an acrylonitrile-butadiene copolymer rubber (NBR), a chloroprene rubber (CR), an ethylene-propylene copolymer rubber (EPDM) and a butyl rubber (IIR). (R1O)3Si-R2-S-C(=O)-C17H35 (1) [R1 is independently preferably methyl or ethyl, R2 is methyl, ethyl, propyl or the like, C17H35 is a branched chain or linear chain.]SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition and uses of the rubber composition. [Background technology]

[0002] In recent years, various silica-containing rubber products, such as silica-containing tires with excellent fuel efficiency and braking performance, anti-vibration rubber, and various rubber rolls, are becoming more and more popular. However, silica-containing rubber compositions have a significant increase in compound viscosity, so a method of alleviating the increase in viscosity by compounding a silane coupling agent is generally used. In addition, it is known that the silane coupling agent reacts with the silanol on the silica surface to reduce the interaction between silica particles, thereby lowering the loss tangent and dynamic modulus of rubber.

[0003] Currently, among silane coupling agents, polysulfide-based coupling agents are widely used in fuel-efficient tires (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2000-103794 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a rubber composition which, when a known silane coupling agent is used in the rubber composition, enables the production of a tire having better fuel economy and gripping properties. [Means for solving the problem]

[0006] As a result of intensive research aimed at solving the above problems, the present inventors have found that a rubber composition containing a rubber (A), an inorganic filler (B), a silane coupling agent (C) represented by formula (1), and a basic compound (D) can solve the above problems. (R 1 O) 3 Si-R 2 -SC(=O)-C 17 H 35 …(1) [In formula (1), R 1 are independently H or (C 1 ~C 8 ) alkyl, R 2 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bond hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) double bonded hydrocarbon, alkyl group C 17 H 35 is branched or linear]

[0007] The present invention can also be described as follows. Item 1. A rubber composition comprising a rubber (A), an inorganic filler (B), a silane coupling agent (C) represented by formula (1), and a basic compound (D), (R 1 O) 3 Si-R 2 -SC(=O)-C 17 H 35 …(1) [In formula (1), R 1 are independently H or (C 1 ~C 8 ) alkyl, R 2 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bond hydrocarbons, saturated (C 1 ~C 8) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) double bonded hydrocarbon, alkyl group C 17 H 35 is branched or linear] Term 2. In formula (1), R 1 is ethyl, and R 2 CH 2 CH 2 CH 2 and the alkyl group C 17 H 35 Item 2. The rubber composition according to item 1, wherein the is a linear silane coupling agent. Item 3. The rubber (A) is one or more selected from natural rubber (NR), polyisoprene rubber (IR), styrene-butadiene copolymer rubber (SBR), polybutadiene rubber (BR), acrylonitrile-butadiene copolymer rubber (NBR), chloroprene rubber (CR), ethylene-propylene copolymer rubber (EPDM), and butyl rubber (IIR). The rubber composition according to item 1 or 2. Item 4. The rubber composition according to any one of Items 1 to 3, further comprising 10 to 150 parts by weight of an inorganic filler (B) based on 100 parts by weight of the rubber (A). Item 5. The rubber composition according to any one of Items 1 to 4, further comprising a vulcanizing agent. Item 6. A crosslinked product obtained by crosslinking the rubber composition according to item 5. Item 7. A tire obtained by crosslinking the rubber composition according to item 5. Effect of the Invention

[0008] The present inventors have found that a tire having excellent fuel economy and grip performance can be obtained by using a combination of a specific silane coupling agent (C) and a basic compound (D) in a rubber composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Rubber composition The rubber composition of the present invention is a rubber composition comprising a rubber (A), an inorganic filler (B), a silane coupling agent (C) represented by formula (1), and a basic compound (D), (R 1 O) 3 Si-R 2 -SC(=O)-C 17 H 35 …(1) [In formula (1), R 1 are independently H or (C 1 ~C 8 ) alkyl, R 2 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bond hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) double bonded hydrocarbon, alkyl group C 17 H 35 is branched or linear]

[0010] Rubber (A) The rubber (A) contained in the rubber composition according to the present invention is not particularly limited, and may be natural rubber or synthetic rubber. The synthetic rubber is also not particularly limited, and examples thereof include diene rubbers such as styrene-butadiene rubber (SBR), butadiene rubber (BR), isoprene rubber (IR), nitrile rubber (NBR), acrylonitrile-butadiene rubber (NBR), and chloroprene rubber (CR); olefin rubbers such as butyl rubber (IIR), ethylene-propylene rubber (EPDM), acrylic rubber (ACM), chlorosulfonated polyethylene rubber (CSM), and fluororubber (FKM); silicone rubber (Q); and urethane rubber (AU).

[0011] The rubber (A) may be produced by any polymerization method, and may be a rubber produced by emulsion polymerization or a rubber produced by solution polymerization. The rubber may also be a so-called terminal-modified rubber, in which the molecular terminals are modified.

[0012] The above rubbers (A) can be used alone or in combination of two or more kinds.

[0013] Among them, from the viewpoint of the reactivity of the silane coupling agent represented by formula (1), the rubber (A) is more preferably a diene rubber. In particular, the rubber is particularly preferably at least one selected from the group consisting of styrene-butadiene rubber (SBR), butadiene rubber (BR), natural rubber (NR), butyl rubber (IIR), and ethylene-propylene rubber (EPDM).

[0014] The content of the rubber (A) in the rubber composition of the present invention is not particularly limited, but may be, for example, 20 to 80% by mass based on the entire rubber composition.

[0015] Inorganic filler (B) The rubber composition according to the present invention contains an inorganic filler (B).

[0016] The inorganic filler (B) is not particularly limited as long as it is one that is usually added during the kneading of a rubber composition, but for example, at least one selected from the group consisting of wet silica, dry silica, and aluminum hydroxide can be suitably used. By using these inorganic fillers (B), it is possible to obtain an effect of further improving the reinforcing properties of the rubber. Among them, it is particularly preferable to use wet silica as the inorganic filler (B) from the viewpoint of reactivity with the silane coupling agent. In addition, the BET specific surface area of ​​the above-mentioned wet silica, dry silica, and aluminum hydroxide is 20 to 300 m 2 / g, and 50 to 250m 2 / g is more preferable, and 100 to 250m 2It is more preferable that the BET specific surface area of ​​the inorganic filler (B) is 20 m 2 / g, when the inorganic filler (B) is mixed with the rubber (A), the rubber has excellent reinforcement properties and improves the abrasion resistance of the rubber. 2 / g or less, an increase in the viscosity of the rubber when the inorganic filler (B) and the rubber (A) are mixed can be suppressed, and the inorganic filler (B) and the rubber can be kneaded more uniformly.

[0017] The content of the inorganic filler (B) contained in the rubber composition according to the present invention is not limited thereto, but is preferably 10 to 150 parts by weight, more preferably 20 to 120 parts by weight, and even more preferably 60 to 120 parts by weight, per 100 parts by weight of the rubber (A).

[0018] Silane coupling agent (C) represented by formula (1) The rubber composition according to the present invention contains a silane coupling agent (C) represented by formula (1). (R 1 O) 3 Si-R 2 -SC(=O)-C 17 H 35 …(1) [In formula (1), R 1 are independently H or (C 1 ~C 8 ) alkyl, preferably methyl or ethyl; R 2 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bond hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) double bonded hydrocarbons, preferably CH 2 , C.H. 2 CH 2 , C.H. 2 CH 2 CH 2 , C.H. 2 CH 2CH 2 CH 2 , CH(CH 3 ), C.H. 2 CH(CH 3 ), C(CH 3 ) 2 , CH(C 2 H 5 ), C.H. 2 CH 2 CH(CH 3 ), C.H. 2 CH(CH 3 )CH 2 means an alkyl group C 17 H 35 is branched or linear]

[0019] In the silane coupling agent (C) represented by formula (1) used in the present invention, 1 may be ethyl, R 2 CH 2 CH 2 CH 2 and the alkyl group C 17 H 35 is a straight chain ((CH 2 ) 16 CH 3 ) may be.

[0020] Examples of the silane coupling agent (C) represented by formula (1) include the silane coupling agents exemplified below.

[0021] (CH 3 O) 3 Si-CH 2 -SC(=O)-C 17 H 35 , (CH 3 O) 3 Si-CH 2 CH 2 -SC(=O)-C 17 H 35 , (CH 3 O) 3 Si-CH 2 CH 2 CH 2-SC(=O)-C 17 H 35 、 (CH 3 ABOUT) 3 Si-CH 2 CH 2 CH 2 CH 2 -SC(=O)-C 17 H 35 、 (CH 3 ABOUT) 3 Si-CH 2 CH 2 CH 2 CH 2 CH 2 -SC(=O)-C 17 H 35 、 (CH 3 CH 2 ABOUT) 3 Si-CH 2 -SC(=O)-C 17 H 35 、 (CH 3 CH 2 ABOUT) 3 Si-CH 2 CH 2 -SC(=O)-C 17 H 35 、 (CH 3 CH 2 ABOUT) 3 Si-CH 2 CH 2 CH 2 -SC(=O)-C 17 H 35 、 (CH 3 CH 2 ABOUT) 3 Si-CH 2 CH 2 CH 2 CH 2 -SC(=O)-C 17 H 35 、または、 (CH 3 CH 2 ABOUT) 3 Si-CH 2 CH 2 CH2 CH 2 CH 2 -SC(=O)-C 17 H 35 .

[0022] The silane coupling agent (C) represented by formula (1) is reacted with a silane coupling agent (R 1 O) 3 Si-R 2 The mercaptosilane corresponding to --SH can be prepared by reacting it with stearic acid chloride, filtering off the resulting solid residue and distilling off the solvent.

[0023] The silane coupling agent (C) represented by formula (1) is produced by the reaction of a silane coupling agent represented by formula (2) (R 1 O) 3 Si-R 2 Examples of the -SH mercaptosilane include the following compounds.

[0024] (CH 3 O) 3 Si-CH 2 -SH, (CH 3 O) 3 Si-CH 2 CH 2 -SH, (CH 3 O) 3 Si-CH 2 CH 2 CH 2 -SH, (CH 3 O) 3 Si-CH 2 CH 2 CH 2 CH 2 -SH, (CH 3 O) 3 Si-CH 2 CH 2 CH 2 CH 2 CH 2 -SH, (CH 3 CH 2 O) 3Si-CH 2 -SH、 (CH 3 CH 2 ABOUT) 3 Si-CH 2 CH 2 -SH、 (CH 3 CH 2 ABOUT) 3 Si-CH 2 CH 2 CH 2 -SH、 (CH 3 CH 2 ABOUT) 3 Si-CH 2 CH 2 CH 2 CH 2 -SH、または、 (CH 3 CH 2 ABOUT) 3 Si-CH 2 CH 2 CH 2 CH 2 CH 2 -SH。

[0025] Triethylamine or another amine may be used as the auxiliary base in the preparation of the silane coupling agent (C) represented by formula (1). Examples of the solvent include aliphatic hydrocarbons such as pentane, hexane, heptane, and octane, alicyclic hydrocarbons such as cyclopentane and cyclohexane, aromatic hydrocarbons such as benzene, toluene, and xylene, chlorinated hydrocarbons such as dichloromethane, 1,2-dichloroethane, chloroform, monochlorobenzene, and dichlorobenzene, ether solvents such as diethyl ether, tetrahydrofuran (THF), dioxane, and 1,2-dimethoxyethane, amide solvents such as N,N-dimethylformamide (DMF), N,N-dimethylacetamide, and N-methylpyrrolidone, ester solvents such as methyl formate, ethyl formate, methyl acetate, ethyl acetate, isopropyl acetate, and butyl acetate, ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, nitrile solvents such as acetonitrile and benzonitrile, and sulfone solvents such as dimethyl sulfoxide and sulfolane. The solvent may be one or more of these.

[0026] Basic Compounds (D) The rubber composition according to the present invention contains a basic compound (D).

[0027] The basic compound (D) is not particularly limited, and examples thereof include primary amine compounds (d-1), secondary amine compounds (d-2), and tertiary amine compounds (d-3), etc. The basic compound (D) of the present invention does not include the silane coupling agent described below.

[0028] Examples of the primary amine compound (d-1) include ethylamine, n-propylamine, isopropylamine, 1,2-dimethylpropylamine, n-butylamine, isobutylamine, sec-butylamine, tert-butylamine, isoamylamine, tert-amylamine, 3-pentylamine, n-amylamine, n-hexylamine, n-heptylamine, n-octylamine, 2-octylamine, tert-octylamine, 2-ethylhexylamine, n-nonylamine, n-aminodecane, n-aminoundecane, n-dodecylamine, and n- Examples of the alkylamines include alkylamines having a straight-chain or branched hydrocarbon group, such as tridecylamine, 2-tridecylamine, n-tetradecylamine, n-pentadecylamine, n-hexadecylamine, n-heptadecylamine, n-octadecylamine, n-oleylamine, benzylamine, 2-phenylethylamine, 3-phenylpropylamine, ethanolamine, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, and 3-aminopropylmethyldiethoxysilane.

[0029] Other examples include alicyclic amines such as cyclopropylamine, cyclobutylamine, cyclopropylamine, cyclohexylamine, cycloheptylamine, and cyclooctylamine, and aromatic amines such as aniline, etc. Furthermore, other examples include ether amines such as 3-isopropoxypropylamine, isobutoxypropylamine, and morpholine.

[0030] Examples of the secondary amine compound (d-2) include N,N-dipropylamine, N,N-dibutylamine, N,N-dipentylamine, N,N-dihexylamine, N,N-dipeptylamine, N,N-dioctylamine, N,N-dinonylamine, N,N-didecylamine, N,N-diundecylamine, N,N-didodecylamine, N,N-distearylamine, N-methyl-N-propylamine, N-ethyl-N-propylamine, N-propyl-N-butylamine, bis(2-ethylhexyl)amine, N-methylaminopropyltrimethoxysilane, (3-(butylamino)propyl)trimethoxysilane, 3-(N-phenyl)aminopropyltrimethoxysilane, bis(3-(trimethoxysilyl)propyl)amine, and cyclic amines such as piperidine.

[0031] Examples of the tertiary amine compound (d-3) include triethylamine, tributylamine, trihexylamine, dimethyloctylamine, dimethyldecylamine, dimethyllaurylamine, dimethylmyristylamine, dimethylpalmitylamine, dimethylstearylamine, dilaurylmonomethylamine, quinuclidine, dimethylaminoethanol, pyridine, (3-(dimethylamino)propyl)trimethoxysilane, (3-(diethylamino)propyl)trimethoxysilane, and the like.

[0032] Furthermore, in the present invention, a diamine compound (d-4) having two amino groups in one compound can also be used. Examples of the diamine compound (d-4) include ethylenediamine, N,N-dimethylethylenediamine, N,N'-dimethylethylenediamine, N-ethylethylenediamine, N,N-diethylethylenediamine, N,N'-diethylethylenediamine, 1,3-propanediamine, 2,2-dimethyl-1,3-propanediamine, N,N-dimethyl-1,3-propanediamine, and N,N'-dimethyl-1,3-propanediamine. diamine, N,N-diethyl-1,3-propanediamine, N,N'-diethyl-1,3-propanediamine, 1,4-butanediamine, N,N-dimethyl-1,4-butanediamine, N,N'-dimethyl-1,4-butanediamine, N,N-diethyl-1,4-butanediamine, N,N'-diethyl-1,4-butanediamine, 1,5-pentanediamine, 1,5-diamino-2-methylpentane, 1,6 -hexanediamine, N,N-dimethyl-1,6-hexanediamine, N,N'-dimethyl-1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 2-(2-aminoethylamino)ethanol, imidazole, N,N-dimethylaminopyridine (DMAP), diazabicyclononene (DBN), diazabicycloundecene (DBU), 1,4-diazabicyclo[2.2.2]octane (DABCO), 1,8-bis(dimethylamino)naphthalene (proton sponge), N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(6-aminohexyl)-3-aminopropyltrimethoxysilane, and the like can be exemplified.

[0033] In addition to the above, examples of the basic compound (D) of the present invention include diethylenetriamine, 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, 1,2,3-triphenylguanidine, triethylenetetramine, and hexamethylenetetramine.

[0034] In the rubber composition of the present invention, the basic compound (D) may be used alone or in combination of two or more of the above-mentioned compounds.

[0035] Among these, as the basic compound (D), 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, quinuclidine, diazabicycloundecene (DBU), 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, 1,2,3-triphenylguanidine, and hexamethylenetetramine are preferred, and 1,3-diphenylguanidine is more preferred.

[0036] The amount of the basic compound in the rubber composition of the present invention may be 0.1 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, particularly preferably 0.5 to 5 parts by mass, even more preferably 0.5 to 3 parts by mass, and most preferably 0.5 to 1.5 parts by mass, per 100 parts by mass of rubber.

[0037] Silane coupling agents other than the silane coupling agent (C) represented by formula (1) The rubber composition of the present invention may be compounded with a combination of silane coupling agents that are usually compounded in rubbers, in addition to the silane coupling agent (C) represented by formula (1). As the silane coupling agent other than the silane coupling agent (C) represented by formula (1), for example, at least one of vinyl-based organosilicon compounds, alkyl-based organosilicon compounds, epoxy-based organosilicon compounds, methacrylic-based organosilicon compounds, (protected) mercapto-based organosilicon compounds, (poly)sulfide-based organosilicon compounds, and condensates thereof may be contained (hereinafter, these organosilicon compounds may be collectively referred to as "other organosilicon compounds").

[0038] In the rubber composition of the present invention, when other organosilicon compounds, i.e., at least one selected from vinyl-based organosilicon compounds, alkyl-based organosilicon compounds, epoxy-based organosilicon compounds, methacrylic-based organosilicon compounds, (protected)mercapto-based organosilicon compounds, (poly)sulfide-based organosilicon compounds, and condensates thereof, are contained, it is preferable to compound 0.1 to 20 parts by mass, more preferably 0.5 to 15 parts by mass, even more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 5.0 parts by mass, relative to 100 parts by mass of the inorganic filler.

[0039] Examples of the vinyl-based organosilicon compound of the present invention include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(2-methoxyethoxy)silane, allyltrichlorosilane, allyltriethoxysilane, diethoxymethylvinylsilane, trichlorovinylsilane, trichlorovinylsilane, and the like.

[0040] Examples of the alkyl-based organosilicon compound of the present invention include methyltrimethoxysilane, dimethyldiethoxysilane, propyltriethoxysilane, hexyltrimethoxysilane, octyltriethoxysilane, and hexamethyldisilazane.

[0041] Examples of the epoxy-based organosilicon compound of the present invention include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, and the like.

[0042] Examples of the methacrylic organosilicon compound of the present invention include 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, and the like.

[0043] The (poly)sulfide-based organosilicon compound of the present invention is exemplified by a polysulfide-based silane coupling agent represented by formula (3), with bis(3-triethoxysilylpropyl) disulfide and bis(3-triethoxysilylpropyl) tetrasulfide being particularly preferred. (R 3 -O) 3-m (R 3 ) m -Si-R 4 -S l -R 4 -Si-(R 3 ) m (OR 3 ) 3-m··· (3) (In formula (3), R 3 are independently alkyl groups having 1 to 18 carbon atoms, C a H 2a+1 O-((CH 2 ) b O) c where a is 1 to 18, b is 1 to 6, and c is 1 to 18; R 4 is an alkylene group having 1 to 9 carbon atoms or a divalent phenyl group, l is an integer of 1 to 9, and m is an integer of 0, 1, or 2.

[0044] Examples of the (protected) mercapto-based organosilicon compound of the present invention include mercapto-based organosilicon compounds having a mercapto group as a compound, such as 3-mercaptopropyltrimethoxysilane and 3-mercaptopropyltriethoxysilane, and protected mercapto-based organosilicon compounds which are organosilicon compounds having no mercapto group (wherein the mercapto group is protected), such as 3-octanoylthio-1-propyltriethoxysilane and 3-propionylthiopropyltrimethoxysilane, and which subsequently come to have a mercapto group by the application of heat, chemicals, etc.

[0045] The (protected) mercapto-based organosilicon compound of the present invention is preferably a compound represented by the following formula (4). R 5 n (R 6 ) 3-n -Si-R 7 -SH···(4) R 5are each independently a hydrocarbon group, preferably an alkyl group having 1 to 6 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms. R 6 are each independently an alkoxy group, preferably an alkoxy group having 1 to 8 carbon atoms, and more preferably an alkoxy group having 1 to 3 carbon atoms. R 7 is a divalent hydrocarbon group, preferably a divalent hydrocarbon group having 1 to 18 carbon atoms, and preferably an alkylene group having 1 to 4 carbon atoms. n is 0, 1 or 2.

[0046] Specific examples of other organic silicon compounds that can be used in combination include, but are not limited to, Kabras 2 and Kabras 4 manufactured by Osaka Soda Co., Ltd., which correspond to the compound represented by the formula (3), Si-75, which corresponds to the Kabras-2 type, Si-69, which corresponds to the Kabras-4 type, manufactured by Degussa Co., Ltd., Si-363 represented by the following formula (5), A-1289, which corresponds to the Kabras-4 type, manufactured by Momentive Co., Ltd., A-189 which is 3-mercaptopropyltrimethoxysilane, NXT, which is 3-octanoylthio-propyltriethoxysilane, NXT-LowV, which is represented by the formula (6), and KBE-846, which corresponds to the Kabras-4 type, manufactured by Shin-Etsu Chemical Co., Ltd., and the like. These compounds can also be used alone or in combination.

[0047] [ka]

[0048] [ka]

[0049] In addition, it is preferred that the total mass of at least one of the organosilicon compounds of the present invention, vinyl organosilicon compounds, alkyl organosilicon compounds, epoxy organosilicon compounds, methacrylic organosilicon compounds, (protected) mercapto organosilicon compounds, (poly)sulfide organosilicon compounds, and condensates thereof does not exceed 30 parts by mass per 100 parts by mass of the silica-based filler.

[0050] In addition to the above, the rubber composition of the present invention may contain compounding agents that are generally used in the rubber industry, as long as they do not deviate from the spirit of the present invention. For example, vulcanizing agents, processing aids such as stearic acid, titanate-based coupling agents, antioxidants such as phenyl-α-naphthylamine and N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, fillers such as carbon black and calcium carbonate, crosslinking accelerators (auxiliaries) such as sulfenamide-based crosslinking accelerators and zinc oxide (zinc oxide), reinforcing agents, softeners, plasticizers, tackifiers, scorch inhibitors, etc. may be used.

[0051] Such a vulcanizing agent is not particularly limited as long as it is one that is usually added during the kneading operation of a rubber composition, but it is more preferable that the vulcanizing agent is at least one selected from sulfur, selenium, an organic peroxide, morpholine disulfide, a thiuram compound, and an oxime compound.

[0052] The content of the vulcanizing agent contained in the rubber composition according to the present invention is not particularly limited, but is preferably 0.1 to 20 parts by weight, more preferably 0.2 to 15 parts by weight, and even more preferably 0.5 to 10 parts by weight, per 100 parts by weight of rubber.

[0053] The content of the vulcanizing agent is preferably 0.1 parts by weight or more per 100 parts by weight of rubber, since the rubber can be crosslinked appropriately, and the content of the vulcanizing agent is preferably 20 parts by weight or less per 100 parts by weight of rubber, since rubber-like elasticity can be maintained.

[0054] Examples of sulfenamide crosslinking accelerators include N-cyclohexyl-2-benzothiazyl sulfenamide, N,N-dicyclohexyl-2-benzothiazyl sulfenamide, N-oxydiethylene-2-benzothiazyl sulfenamide, N-tert-butyl-2-benzothiazyl sulfenamide, and N-tert-butyl-di(2-benzothiazole)sulfenimide.

[0055] The amount of the crosslinking accelerator (auxiliary agent) in the rubber composition of the present invention is, relative to 100 parts by mass of rubber, It is preferably 0.1 to 15 parts by mass, more preferably 1 to 10 parts by mass, and particularly preferably 3 to 9 parts by mass. The blending amount of the crosslinking accelerator (auxiliary) is the total blending amount of the crosslinking accelerator and the crosslinking accelerator auxiliary, and when both the crosslinking accelerator and the crosslinking accelerator auxiliary are used, it represents the total blending amount thereof.

[0056] Examples of processing aids include higher fatty acids such as stearic acid, oleic acid, palmitic acid, and lauric acid; higher fatty acid amides such as stearic acid amide and oleic acid amide; higher fatty acid esters such as ethyl oleate; and higher aliphatic amines such as stearylamine and oleylamine.

[0057] The amount of the processing aid in the rubber composition of the present invention is, for example, 300 parts by mass or less, preferably 100 parts by mass or less, more preferably 50 parts by mass or less, and particularly preferably 10 parts by mass or less, per 100 parts by mass of rubber.

[0058] Examples of the softening agent include petroleum waxes such as carnauba wax and ceresin wax; polyglycols such as ethylene glycol, glycerin and diethylene glycol; aliphatic hydrocarbons such as vaseline, paraffin and naphthene; and silicone oils.

[0059] The amount of softener in the rubber composition of the present invention is, for example, 300 parts by mass or less, preferably 100 parts by mass or less, more preferably 50 parts by mass or less, and particularly preferably 30 parts by mass or less, per 100 parts by mass of rubber.

[0060] The amount of the antioxidant mixed in the rubber composition of the present invention is, for example, 30 parts by mass or less, preferably 10 parts by mass or less, and more preferably 5 parts by mass or less, per 100 parts by mass of rubber.

[0061] The rubber composition of the present invention may further contain carbon black. Examples of carbon black include, but are not limited to, carbon blacks of various classes such as SRF, FEF, HAF, ISAF, and SAF.

[0062] The amount of carbon black contained is preferably 0.5 to 100 parts by mass, more preferably 1 to 90 parts by mass, and particularly preferably 2 to 80 parts by mass, based on 100 parts by mass of rubber.

[0063] Method for producing rubber composition The method for producing the rubber composition according to the present invention will be described below.

[0064] The method for producing a rubber composition according to the present invention may include a first kneading step of kneading the inorganic filler into the rubber. The method for producing a rubber composition according to the present invention may further include at least one step selected from a second kneading step of kneading a vulcanizing agent into the kneaded product obtained in the first kneading step, a molding step, and a crosslinking step.

[0065] First kneading process In the first kneading step, the inorganic filler and the silane coupling agent (C) represented by the above formula (1) are kneaded with the above rubber to obtain the rubber composition of the present invention.

[0066] The first kneading step is preferably carried out before the second kneading step in which the vulcanizing agent is kneaded in. That is, in the first kneading step, the inorganic filler and the silane coupling agent (C) represented by the above formula (1) are kneaded into the rubber in a step before the vulcanizing agent is kneaded in.

[0067] In the first kneading step, the inorganic filler and the silane coupling agent (C) represented by the above formula (1) are preferably kneaded at 80 to 250°C, more preferably at 80 to 200°C. By kneading the above components in this temperature range, the inorganic filler and the like can be uniformly dispersed without gelling or scorching the kneaded product, and each component can be kneaded suitably. In addition, since no vulcanizing agent is added in the first kneading step, kneading can be performed at a relatively high temperature without worrying about the formation of crosslinks. The kneading time in the first kneading step is not particularly limited, but is, for example, 1 minute to 1 hour.

[0068] For the kneading in the first kneading step, various mixing machines usually used in the rubber industry, such as a roll, a pressure kneader, an intermixer, or a Banbury mixer, can be used.

[0069] Second kneading process In the second kneading step, the basic compound (D) and the vulcanizing agent are kneaded into the kneaded product obtained in the first kneading step to obtain a composition after adding the vulcanizing agent, i.e., a rubber composition for crosslinking. In this second kneading step, it is preferable to knead the vulcanizing agent into the kneaded product obtained in the first kneading step at 100°C or less. This makes it possible to prevent crosslinking by the vulcanizing agent. The kneading time in this second kneading step is not particularly limited, but is, for example, 1 minute to 1 hour.

[0070] For the kneading in the second kneading step, various mixing machines usually used in the rubber industry, such as a roll, a pressure kneader, an intermixer, or a Banbury mixer, can be used.

[0071] Molding process In the molding step, the rubber composition for crosslinking prepared in the second kneading step is molded into an intended shape by a calendar roll, a press, or the like.

[0072] Crosslinking process In the crosslinking step, the molded product obtained in the molding step is heated for 1 minute to 3 hours at preferably 120 to 230° C. In addition, a mold may be used during crosslinking.

[0073] The molding step and the cross-linking step may be separate steps, or may be one step carried out simultaneously.

[0074] Use of rubber composition As described above, the crosslinked product obtained by crosslinking the rubber composition of the present invention can be used for various applications as a rubber product. Therefore, the crosslinked product obtained by crosslinking the rubber composition is also included in the present invention.

[0075] The shape of such crosslinked products is not particularly limited, and they can be used as tires, tubes, belts, hoses, industrial products, etc.

[0076] As described above, the crosslinked product obtained by crosslinking the rubber composition of the present invention has a small hysteresis loss, and therefore, when used as a tire, for example, the energy loss during tire running can be reduced and the rolling resistance can be reduced. Therefore, the crosslinked product can be suitably used in rubber parts that are used dynamically, such as tires (especially tread parts).

[0077] EXAMPLES

[0078] (Synthesis Example) Preparation of a silane coupling agent represented by formula (1) ((EtO) 3 Si-(CH 2 ) 3 -SC(=O)-C 17 H 35 (Production) To a solution of 98.66 g of 3-mercaptopropyltriethoxysilane in 1300 ml of petroleum ether (boiling range 50-70°C) was added 48.15 g of triethylamine at 5°C, followed by dropwise addition of 125.35 g of stearic acid chloride using a heatable dropping funnel. After heating at reflux for 90 min, the cooled suspension was filtered, the filter cake was rewashed twice with petroleum ether, the resulting filtrates were combined and the solvent was removed. 1 The silane coupling agent represented by formula (1), identified by H-NMR analysis, was obtained in an amount of 186.71 g. The physical properties of the agent are shown below. 1 H NMR (400 MHz, CDCl 3 )δ3.8(q, J=6.8Hz, 6H), 2.9(t, J=7.2Hz, 2H), 2.5(t, J=8.0Hz, 2H), 1.7-1.6(m, 4 H), 1.4-1.2(m, 28H), 1.2(t, J=6.8Hz, 9H), 0.9(t, J=6.8Hz, 3H), 0.8-0.6(m, 2H)

[0079] [Production of rubber composition] The kneading test was carried out using a Labo Plastomill 10C100 (manufactured by Toyo Seiki Co., Ltd.) equipped with a 250cc Banbury mixer type attachment BR-250. The temperature of the device was 100°C with oil circulation heating, and the rotor rotation speed of the mixer was constant at 80 rpm. The compounding test was carried out based on 100 g of rubber. The procedure was to masticate the rubber component for 30 seconds, add the chemicals shown in the formula (I) in Table 1, and knead for 30 seconds. Next, the chemicals shown in the formula (II) in Table 1 were added and kneaded for 3 minutes, and then the kneaded product was discharged. The amount of the organosilicon compound in the examples and comparative examples was adjusted so that the amount of silicon in the organosilicon compound in the examples and comparative examples was the same. The amount of sulfur added in the examples and comparative examples was adjusted so that the amount of sulfur in the system was the same. The discharged kneaded product was cooled on a 6-inch roll at room temperature, and then the crosslinking agent components shown in the formula (III) in Table 1 were added and kneaded for 6 minutes to obtain a sheet (uncrosslinked sheet) with a thickness of about 2 mm. The next day, the remaining compound was crosslinked by heat press at 160° C. for 20 minutes to obtain a test sample (crosslinked sheet).

[0080] <Dynamic viscoelasticity test> A test piece with a width of 4 mm, length of 25 mm, and thickness of 2 mm was punched out from the test sample (crosslinked sheet), and tan δ was measured using Rheogel-4000 manufactured by UBM Co., Ltd. under the conditions of chuck distance of 20 mm, initial strain of 10%, dynamic amplitude of 1%, and vibration of 10 Hz. The measurement temperature range was kept constant at 60°C.

[0081] <Processability test> The uncrosslinked sheet was set in a Mooney viscometer AM-3 manufactured by Toyo Seiki Seisakusho, and ML 1+4 and scorch time (t5) were measured.

[0082] The compounding agents used in the examples and comparative examples are shown below. *1 JSR Corporation SL552 *2 Nipsil AQ (BET specific surface area 215m) manufactured by Tosoh Silica Corporation 2 / g) *3 Sunthene 415 manufactured by Nippon Oil Corporation *4 Sakura Stearic Acid, manufactured by NOF Corporation *5 Nocrac 6C manufactured by Ouchi Shinko Chemical Industry Co., Ltd. *6 CABRUS-2 ((poly)sulfide-based organosilicon compound) manufactured by Osaka Soda Co., Ltd. *7 Zinc oxide type 2 manufactured by Sakai Chemical Industry Co., Ltd. *8 1,3-diphenylguanidine manufactured by Ouchi Shinko Chemical Industry Co., Ltd. *9 Noccela CZ manufactured by Ouchi Shinko Chemical Industry Co., Ltd. *10 Colloidal sulfur manufactured by Hosoi Chemical Industry Co., Ltd.

[0083] TIFF2024153078000003.tif4367

[0084] The test samples (crosslinked sheets) obtained in Examples 1 and 2 and Comparative Example 1 were subjected to a dynamic viscoelasticity test. The results are shown in Table 2.

[0085] JPEG2024153078000004.jpg1342

[0086] The test samples (uncrosslinked sheets) obtained in Example 1, Example 2, and Comparative Example 2 were subjected to a processability test. The results are shown in Table 3.

[0087] As shown in Table 2, Examples 1 and 2 using the organosilicon compound of the present invention have a large tan δ at 0° C., suggesting excellent grip, and a small tan δ at 60° C., suggesting excellent fuel economy, compared with Comparative Example 1 using the most widely used polysulfide-based organosilicon compound. Usually, as the tan δ value at 60° C. decreases, the tan δ value at 0° C. also tends to decrease, but Examples 1 and 2 using the organosilicon compound of the present invention are also preferable in that they are excellent in both grip and fuel economy. [Industrial Applicability]

[0088] The use of the organosilicon compound of the present invention makes it possible to provide a rubber composition and a rubber material having excellent gripping properties and fuel economy, and therefore, is particularly suitable for the manufacture of rubber parts that are used dynamically, such as tire treads, anti-vibration rubbers, and belts.

Claims

1. A rubber composition comprising a rubber (A), an inorganic filler (B), a silane coupling agent (C) represented by formula (1), and a basic compound (D), (R) 1 O) 3 Si-R 2 -S-C(=O)-C 17 H 35 …(1) [In formula (1), R 1 are each independently H or (C 1 ~C 8 ) alkyl, R 2 is a straight chain (C 1 ~C 8 ) double bonded hydrocarbon or branched chain (C 1 ~C 8 ) double bonded hydrocarbons, saturated (C 1 ~C 8 ) double bond hydrocarbon or unsaturated (C 1 ~C 8 ) means a double bonded hydrocarbon, and the alkyl group C 17 H 35 is branched or linear.

2. In formula (1), R 1 is ethyl, R 2 CH 2 CH 2 CH 2 and the alkyl group C 17 H 35 The rubber composition according to claim 1 , wherein the is a linear silane coupling agent.

3. The rubber (A) is one or more selected from natural rubber (NR), polyisoprene rubber (IR), styrene butadiene copolymer rubber (SBR), polybutadiene rubber (BR), acrylonitrile butadiene copolymer rubber (NBR), chloroprene rubber (CR), ethylene propylene copolymer rubber (EPDM), and butyl rubber (IIR). The rubber composition according to claim 1 or 2.

4. 4. The rubber composition according to claim 1, further comprising 10 to 150 parts by weight of an inorganic filler (B) based on 100 parts by weight of the rubber (A).

5. The rubber composition according to any one of claims 1 to 4, further comprising a vulcanizing agent.

6. A crosslinked product obtained by crosslinking the rubber composition according to claim 5.

7. A tire obtained by crosslinking the rubber composition according to claim 5.

Citation Information

Patent Citations

  • Production of sulfur-containing organosilicon compound and production of its synthetic intermediate

    JP2000103794A