Thermal transfer sheet
A thermal transfer sheet with a heat-resistant slipping layer of ethylene-vinyl alcohol copolymer and ethylene oxide-propylene copolymer wax addresses migration and adhesion issues, ensuring high-quality prints and blocking resistance without silicone components.
Patent Information
- Application Number
- JP2023066792
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-29
AI Technical Summary
Conventional thermal transfer sheets using silicone-based compounds for heat-resistant slipping layers suffer from issues such as component migration, leading to printing defects, poor adhesion, and mechanical problems due to insufficient film strength, while non-silicone alternatives exhibit poor blocking resistance when using highly sensitive heat-melting thermal transfer ink layers.
A thermal transfer sheet with a heat-resistant slipping layer composed of a long chain alkyl pendant type resin and hydrocarbon-based synthetic wax, specifically an ethylene-vinyl alcohol copolymer and ethylene oxide-propylene copolymer wax, is used to enhance sticking resistance, slipperiness, and blocking resistance without silicone components.
The solution provides a thermal transfer sheet with improved adhesion, reduced printing defects, and enhanced blocking resistance, ensuring high-quality prints even with sensitive ink layers, while preventing component migration and head residue issues.
Smart Images

Figure 2024153138000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermal transfer sheet used for printing (or image printing) by a thermal melt transfer method. [Background technology]
[0002] Conventionally, thermal transfer sheets used in the thermal melt transfer method generally have a thermally meltable thermal transfer ink layer formed on one side of a base film, and a heat-resistant slipping layer formed on the other side. For this heat-resistant slipping layer, it has been proposed to use silicone oil as a lubricant or a silicone-based compound such as a silicone-modified resin, which has excellent heat resistance and releasability, in order to improve sticking resistance when printed with a thermal transfer printer and blocking resistance with the thermal transfer ink layer when the thermal transfer sheet is stored in a rolled form (Patent Documents 1, 2, and 3).
[0003] Although the heat-resistant slipping layer using these silicone compounds has excellent sticking resistance and blocking resistance, the coating strength is insufficient, so that the components of the heat-resistant slipping layer may fall off and adhere to the thermal head due to friction with the thermal head or mechanical stress during continuous printing, generating so-called "head residue." If the accumulation of this head residue becomes excessive, the heat from the thermal head will not be sufficiently transmitted to the thermal transfer sheet, resulting in printing defects.
[0004] In addition, the heat-resistant slipping layer using a silicone compound has a problem of migration of free silicone components. This is because, when a heat-resistant slipping layer is formed on one side of a substrate film and then wound into a roll, and then a heat-transfer ink layer is formed on the other side, if a silicone compound is used for the heat-resistant slipping layer of the thermal transfer sheet, the free silicone components contained in the heat-resistant slipping layer may migrate to the substrate film surface before the formation of the thermal transfer ink layer during winding or during storage in the wound roll, causing ink to be repelled during the formation of the thermal transfer ink layer, or may cause poor adhesion to the substrate film after the formation of the thermal transfer ink layer. In addition, when the produced thermal transfer sheet is stored in a roll, the free silicone components may migrate to the thermal transfer ink layer side, causing poor transfer during printing, or poor adhesion of the transferred ink layer to the transferee.
[0005] On the other hand, Patent Document 4 proposes a heat-resistant slipping layer that does not use a silicone compound, which is a thermal transfer sheet made of heat-resistant fine particles made of a reaction product of a hydroxyl-containing thermoplastic resin and a polyisocyanate, and a polyvinyl butyral or polyvinyl acetoacetal resin as a binder. The heat-resistant slipping layer of this thermal transfer sheet has excellent sticking resistance and does not contain a silicone component, so there is no transfer failure or adhesion failure caused by free silicone components. However, since the release property of the heat-resistant slipping layer is poor, when a resin material with a low softening point is used along with the high sensitivity (low printing energy) of the heat-meltable thermal transfer ink layer, the blocking resistance is poor when the thermal transfer sheet is stored in a rolled form. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent Publication No. 62-82086 [Patent Document 2] JP 4-16390 [Patent Document 3] JP 5-64987 [Patent Document 4] JP 6-135166 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention provides a thermal transfer sheet for a thermal melt transfer system, which has excellent sticking resistance (heat resistance, slipperiness) and can produce good prints (or prints) without print defects caused by head residue adhesion, without using a silicone-based compound containing a free silicone component in the heat-resistant slippery layer, and which also has excellent blocking resistance even when used with a highly sensitive heat-meltable thermal transfer ink layer. [Means for solving the problem]
[0008] The thermal transfer sheet of the present invention has a heat-meltable thermal transfer ink layer on one side of a substrate and a heat-resistant slipping layer on the other side of the substrate, the heat-resistant slipping layer being composed of a long-chain alkyl pendant resin having a long-chain alkyl group on its side chain and a hydrocarbon synthetic wax, the long-chain alkyl pendant resin being a reaction product of an ethylene-vinyl alcohol copolymer and a monofunctional isocyanate having a linear alkyl group having 12 to 22 carbon atoms, the hydrocarbon synthetic wax being an ethylene oxide-propylene oxide copolymer wax and / or a Fischer-Tropsch wax oxide, the hydrocarbon synthetic wax having a melting point in the range of 100 to 130°C and an acid value in the range of 17 to 30 mgKOH / g, and the blending of the long-chain alkyl pendant resin and the hydrocarbon synthetic wax in the heat-resistant slipping layer being such that the mass ratio of the long-chain alkyl pendant resin / hydrocarbon synthetic wax is in the range of 35 / 65 to 75 / 25.
[0009] In one embodiment of the thermal transfer sheet of the present invention, the weight average molecular weight (Mw) of the hydrocarbon synthetic wax can be in the range of 2,500 to 9,500.
[0010] In one embodiment of the thermal transfer sheet of the present invention, the heat-resistant slipping layer may have a thickness in the range of 0.02 to 0.20 μm.
[0011] In one embodiment of the thermal transfer sheet of the present invention, the tape peeling force of the heat-resistant slipping layer can be 2.0 N / 25 mm or less.
[0012] In one embodiment of the thermal transfer sheet of the present invention, the heat-resistant slipping layer can be formed by applying a heat-resistant slipping layer coating liquid to a predetermined thickness, and then heating and drying the heat-resistant slipping layer at a temperature equal to or higher than the melting point of the hydrocarbon-based synthetic wax, to form a coating film in which the long-chain alkyl pendant resin of the heat-resistant slipping layer and the hydrocarbon-based synthetic wax are uniformly dissolved. Effect of the Invention
[0013] The thermal transfer sheet of the present invention does not have any migrating components such as free silicone components that cause poor transfer or poor adhesion in the heat-resistant slipping layer, and does not cause defects during production or quality deterioration during printing. In addition, the heat-resistant slipping layer has excellent sticking resistance (heat resistance, slipperiness), suppresses the generation of head residue, and can obtain good printing (or printing) without printing defects due to adhesion of head residue. Furthermore, even when a highly sensitive heat-meltable thermal transfer ink layer using a resin with a low softening point is used, it is possible to provide a thermal transfer sheet with excellent blocking resistance. [Brief description of the drawings]
[0014] [Figure 1] 1 is a schematic cross-sectional view showing one embodiment of a thermal transfer sheet of the present invention. [Diagram 2] FIG. 2 is a diagram showing a printing pattern A used for evaluating heat resistance and print slippage in an embodiment of the present invention, as well as its printing direction and printing length. [Diagram 3] FIG. 13 is a diagram showing a printing pattern B used for head waste evaluation in an embodiment of the present invention, as well as its printing direction and printing length. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the thermal transfer sheet of the present invention will be described in detail.
[0016] The thermal transfer sheet of the present invention has a layer structure having a heat-fusible thermal transfer ink layer on one surface of a substrate, and a heat-resistant slip layer on the other surface of the substrate.
[0017] (base material) As the substrate of the thermal transfer sheet of the present invention, various plastic films such as polyester films such as polyethylene terephthalate film and polyethylene naphthalate film, polypropylene film, polycarbonate film, polyimide film, aramid film, etc. can be used. Among these, it is preferable to use a polyethylene terephthalate film from the viewpoints of physical properties, processability, cost, etc. The thickness of the substrate is usually about 2 to 12 μm, and in order to improve heat transfer, it is preferably in the range of 2 to 6 μm.
[0018] The surface of the substrate on which the thermal transfer ink layer is formed and the surface on which the heat-resistant slip layer is formed may be subjected to a surface treatment to improve adhesion between each layer, if necessary. Examples of the surface treatment include corona discharge treatment, ultraviolet irradiation treatment, plasma treatment, and primer treatment.
[0019] (Heat-resistant slipping layer) The heat-resistant slipping layer of the thermal transfer sheet of the present invention is made by blending a specific long-chain alkyl pendant resin with excellent release properties with a hydrocarbon-based synthetic wax having a melting point and acid value within a specific range in a specific mass ratio, and by forming a coating film in which the long-chain alkyl pendant resin and the hydrocarbon-based synthetic wax are uniformly compatible when the heat-resistant slipping layer is formed, it is possible to improve the adhesion, film strength, and slipperiness between the heat-resistant slipping layer and the base film without impairing the release properties of the long-chain alkyl pendant resin, and to obtain a heat-resistant slipping layer of a thermal transfer sheet with excellent sticking resistance (heat resistance, slipperiness) and blocking resistance.
[0020] Long-chain alkyl pendant resins are those in which long-chain alkyl groups exist as pendant side chains on a main chain polymer, and examples thereof include homopolymers of vinyl monomers having long-chain alkyl groups and copolymers with other vinyl monomers, and reaction products in which a polymer having active hydrogen, such as vinyl alcohol, ethylene-vinyl alcohol copolymers, polyethyleneimine, and hydroxyl group-containing cellulose derivatives, is reacted with a monofunctional isocyanate having a long-chain alkyl group, etc. These long-chain alkyl pendant resins have excellent releasability and are also widely used as release agents for adhesive tapes.
[0021] The long-chain alkyl pendant resin used in the present invention is a long-chain alkyl pendant resin which is a reaction product of an ethylene-vinyl alcohol copolymer and a monofunctional isocyanate having a long-chain alkyl group, from the viewpoints of heat resistance, film strength, adhesion to substrates, releasability, and the like as a heat-resistant slipping layer of a thermal transfer sheet.
[0022] The ethylene-vinyl alcohol copolymer is a conventionally known copolymer, and has an ethylene content of 10 to 90 mol %, preferably 20 to 70 mol %, and an average degree of polymerization of usually 300 to 3,000, preferably 500 to 2,500.
[0023] The long-chain alkyl group of the monofunctional isocyanate having a long-chain alkyl group is preferably linear, and from the viewpoints of heat resistance, releasability, and solvent solubility of the resin, the carbon number is preferably in the range of 12 to 22, and more preferably in the range of 14 to 18.
[0024] The weight average molecular weight (Mw) of the long-chain alkyl pendant resin used in the present invention is preferably in the range of 100,000 to 300,000, more preferably in the range of 120,000 to 250,000, from the viewpoints of heat resistance, film strength, and solvent solubility of the resin. The weight average molecular weight (Mw) is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).
[0025] The heat-resistant slipping layer of the present invention contains a synthetic hydrocarbon wax to impart slipping properties to the heat-resistant slipping layer. Examples of the synthetic hydrocarbon wax include polyolefin waxes such as polyethylene wax, polypropylene wax, polybutylene wax, ethylene-propylene copolymer wax, and ethylene-butylene copolymer wax, and Fischer-Tropsch wax. From the viewpoint of affinity with the long-chain alkyl pendant resin, the synthetic hydrocarbon wax used in the present invention is preferably an oxidized type synthetic hydrocarbon wax obtained by oxidizing the synthetic hydrocarbon wax. In particular, from the viewpoint of thermal stability and solvent solubility, it is preferable to use an oxidized ethylene-propylene copolymer wax and / or an oxidized Fischer-Tropsch wax having an ethylene skeleton as the main component.
[0026] The oxidation treatment of the hydrocarbon synthetic wax involves introducing functional groups such as hydroxyl groups, aldehyde groups, carboxyl groups, carbonyl groups, ester groups, and hydroperoxide groups into the hydrocarbon skeleton by methods such as oxygen oxidation and chemical oxidation. The presence of these functional groups improves the affinity with the long-chain alkyl pendant resin and also improves solvent solubility.
[0027] The melting point of the hydrocarbon synthetic wax used in the present invention is preferably in the range of 100 to 130°C, more preferably in the range of 100 to 110°C. If the melting point is less than 100°C, the heat resistance of the heat-resistant slipping layer is reduced, and when printing is performed with high energy, the substrate film is likely to break due to heat fusion. On the other hand, if the melting point exceeds 130°C, when the heat-resistant slipping layer is heated and dried at a temperature equal to or higher than the melting point of the hydrocarbon synthetic wax during coating formation, the thin film (2 to 6 μm polyethylene terephthalate film) commonly used in thermal transfer sheets will have a large thermal shrinkage, and thermal wrinkles will cause defects in the coating surface of the thermal transfer ink layer, resulting in reduced productivity. The melting point of the hydrocarbon synthetic wax is the endothermic peak temperature measured by a differential scanning calorimeter (DSC) at a heating rate of 10°C / min.
[0028] The acid value of the hydrocarbon synthetic wax used in the present invention is preferably in the range of 17 to 30 mgKOH / g. If the acid value is less than 17 mgKOH / g, the affinity and adhesion with the long-chain alkyl pendant resin are reduced, and a tough coating film in which the long-chain alkyl pendant resin and the hydrocarbon synthetic wax are uniformly compatible as a heat-resistant slipping layer cannot be formed, so that head residue generation increases. On the other hand, if the acid value exceeds 30 mgKOH / g, the heat resistance is reduced and the slipping property may be further reduced. The acid value of the hydrocarbon synthetic wax is a value measured in accordance with JIS K5902.
[0029] The weight average molecular weight (Mw) of the hydrocarbon synthetic wax used in the present invention is preferably in the range of 900 to 9,500, more preferably in the range of 2,500 to 9,500. Within this range, solubility in a solvent can be ensured, compatibility with long-chain alkyl pendant resins can be easily achieved, and head residue generation can be suppressed. In addition, the hydrocarbon synthetic wax has an appropriate melt viscosity, and when melted by thermal energy from a thermal head, effective lubricity can be imparted. The weight average molecular weight (Mw) is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).
[0030] The blending amount of the long-chain alkyl pendant resin and the hydrocarbon synthetic wax constituting the heat-resistant slipping layer of the present invention is preferably such that the mass ratio of the long-chain alkyl pendant resin / hydrocarbon synthetic wax is in the range of 35 / 65 to 75 / 25, more preferably 40 / 60 to 60 / 40. If the mass ratio of the long-chain alkyl pendant resin is less than 35 / 65, the release property of the heat-resistant slipping layer is deteriorated and the blocking resistance is reduced. On the other hand, if it exceeds 75 / 25, the heat resistance and slipping property are deteriorated and the sticking resistance is reduced.
[0031] The thickness of the heat-resistant slipping layer of the present invention is preferably in the range of 0.02 to 0.20 μm from the viewpoints of film uniformity and productivity. Within this range, a uniform coating film can be easily formed and the effects of the present invention can be sufficiently obtained.
[0032] The heat-resistant slipping layer of the present invention preferably has a tape peeling strength with Nitto Denko 31B tape of 2.0 N / 25 mm or less. If the tape peeling strength is less than the above value, even if a highly sensitive heat-melting thermal transfer sheet is stored in a roll, it will have excellent blocking resistance. The tape peeling strength is a value measured when the heat-resistant slipping layer and Nitto Denko 31B tape are attached to each other and left at 23±2°C for 10 minutes, and then the tape side is peeled off under the conditions of a measurement temperature of 23±2°C, a peeling angle of 180°, and a peeling speed of 1,200 mm / min.
[0033] In the heat-resistant slipping layer of the present invention, inorganic fine particles and the like can be appropriately blended within a range that does not impair the effects of the present invention, for the purpose of removing contaminants such as head residue adhering to the thermal head.
[0034] The method for forming the heat-resistant slipping layer of the present invention can be to dissolve the long-chain alkyl pendant resin and the hydrocarbon synthetic wax in a solvent to prepare a coating liquid, which is then uniformly coated on a substrate film to a predetermined thickness, and then dried by heating to form a coating film. In addition, by setting the heating and drying temperature during coating formation to a temperature equal to or higher than the melting point of the hydrocarbon synthetic wax, the hydrocarbon synthetic wax and the long-chain alkyl pendant resin become more compatible with each other, and a heat-resistant slipping layer can be formed as a more uniform and tough continuous coating film.
[0035] Examples of the method for applying the coating solution for the heat-resistant slipping layer of the present invention include a gravure coater, a bar coater, a comma knife coater, a die coater, and a reverse coater.
[0036] (Thermal transfer ink layer) The thermal transfer ink layer of the thermal transfer sheet of the present invention softens or melts when heated from the heat-resistant slipping layer side by a thermal head, and the softened or melted part is transferred to the transfer target. Such a thermal transfer ink layer is not particularly limited, and can be one that has been used as a heat-melting ink for a thermal transfer sheet in the past. As the constituent materials of this heat-melting ink, conventionally known heat-melting wax, thermoplastic resin and colorant can be used.
[0037] Examples of heat-meltable waxes include vegetable waxes such as candelilla wax, carnauba wax, rice wax, wood wax, and jojoba oil; animal waxes such as beeswax, lanolin, and whale wax; mineral waxes such as montan wax, ozokerite, and ceresin; petroleum waxes such as paraffin wax, microcrystalline wax, and petrolatum; synthetic waxes such as polyethylene wax and Fischer-Tropsch wax; modified waxes such as montan wax derivatives, paraffin wax derivatives, and microcrystalline wax derivatives; hydrogenated waxes such as hydrogenated castor oil and hydrogenated castor oil derivatives; fatty acids such as lauric acid, palmitic acid, myristic acid, stearic acid, and 1,2-hydroxystearic acid; and fatty acid amides.
[0038] Examples of thermoplastic resins include vinyl resins such as polyvinyl chloride, polyvinyl acetate, and ethylene-vinyl acetate copolymers, polyester resins, (meth)acrylic resins, polyurethane resins, cellulose resins, melamine resins, polyamides, polyolefins, and styrene resins.
[0039] The colorant may be a pigment or a dye, and examples of such colorants include carbon black, acetylene black, lamp black, black smoke, iron black, aniline black, silica, calcium carbonate, titanium oxide, cadmium red, cadmium phosphate red, chrome red, vermilion, red iron oxide, azo pigments, alizarin lake, quinacridone, cochineal lake perylene, yellow ocher, aureolin, cadmium yellow, cadmium orange, chrome yellow, zinc yellow, Naples yellow, nickel yellow, azo pigments, greenish yellow, ultramarine, Prussian blue, ultramarine, cobalt, phthalocyanine, and anthraquinone. , indicoid, cinnabar green, cadmium green, chrome green, phthalocyanine, azomethine, perylene and aluminum pigments, and dyes such as diarylmethane dyes, triarylmethane dyes, thiazole dyes, merocyanine dyes, pyrazolone dyes, methine dyes, indoaniline dyes, acetophenone azomethine dyes, pyrazoloazomethine dyes, xanthene dyes, oxazine dyes, thiazine dyes, azine dyes, acridine dyes, azo dyes, spiropyran dyes, indolinospiropyran dyes, fluoran dyes, naphthoquinone dyes, anthraquinone dyes and quinophthalone dyes.
[0040] Furthermore, the hot melt ink may contain various known additives such as dispersants, leveling agents, and fillers, as required.
[0041] The thermal transfer ink layer may be a single layer of a heat-meltable colored ink layer, but if necessary, a release layer having a function of facilitating the release of the colored ink layer from the substrate may be formed between the substrate and the colored ink layer. If necessary, an adhesive layer having a function of improving adhesion to a transfer target may be formed on the heat-meltable colored ink layer. The constituent materials of these release layers and adhesive layers may be conventionally known heat-meltable waxes, thermoplastic resins, and various additives.
[0042] The thickness of the thermal transfer ink layer can be appropriately determined so as to achieve a balance between the required print density and thermal sensitivity, and is usually preferably in the range of 0.5 to 5.0 μm.
[0043] These thermal transfer ink layers can be formed on the substrate by a conventional method. For example, a coating liquid prepared by dispersing or dissolving the constituent materials of the heat-meltable ink in a solvent such as toluene or MEK by a conventional method can be uniformly coated on the surface of the substrate opposite the surface on which the heat-resistant slipping layer is formed, using a conventional coating method such as a gravure coater, so as to achieve a predetermined coating amount, and then the solvent can be dried to form the layer. EXAMPLES
[0044] The thermal transfer sheet of the present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0045] <Preparation of coating solution for heat-resistant slip layer> The following materials were used and mixed in the amounts shown in Table 1. The mixture was heated to 50°C while stirring to dissolve the resin and hydrocarbon-based synthetic wax, and then cooled to room temperature to prepare coating solutions 1 to 17 for the heat-resistant slipping layer. (Coating fluid material for heat-resistant slip layer) [Long-chain alkyl pendant resin A]; Reaction product of ethylene-vinyl alcohol copolymer (ethylene content 45 mol%) and tetradecyl isocyanate (carbon number 14), weight average molecular weight (Mw) 150,000 [Long chain alkyl pendant resin B]; Reaction product of ethylene-vinyl alcohol copolymer (ethylene content 50 mol%) and octadecyl isocyanate (carbon number 18), weight average molecular weight (Mw) 220,000 [Hydrocarbon-based synthetic wax A]; Ethylene oxide-propylene copolymer wax, melting point 102℃, acid value 26mgKOH / g, weight average molecular weight (Mw) 3,100 [Hydrocarbon-based synthetic wax B]; Ethylene oxide-propylene copolymer wax, melting point 100℃, acid value 18mgKOH / g, weight average molecular weight (Mw) 2,600 [Hydrocarbon-based synthetic wax C]; Ethylene oxide-propylene copolymer wax, melting point 103℃, acid value 17mgKOH / g, weight average molecular weight (Mw) 4,200 [Hydrocarbon-based synthetic wax D]; Ethylene oxide-propylene copolymer wax, melting point 129℃, acid value 20mgKOH / g, weight average molecular weight (Mw) 9,500 [Hydrocarbon-based synthetic wax E]; Oxidized Fischer-Tropsch wax, melting point 102°C, acid value 30mgKOH / g, weight average molecular weight (Mw) 2,700 [Hydrocarbon-based synthetic wax F]; Oxidized polyethylene wax, melting point 94℃, acid value 26mgKOH / g, weight average molecular weight (Mw) 2,800 [Hydrocarbon-based synthetic wax G]; Ethylene oxide-propylene copolymer wax, melting point 101℃, acid value 14mgKOH / g, weight average molecular weight (Mw) 2,000 [Hydrocarbon-based synthetic wax H]; Oxidized polyethylene wax, melting point 93℃, acid value 33mgKOH / g, weight average molecular weight (Mw) 2,200
[0046] [Table 1]
[0047] <Preparation of coating solution for release layer> A coating solution for a release layer to be used in a thermal transfer sheet was prepared according to the following formulation. (Release layer coating liquid) Ethylene-vinyl acetate copolymer resin (softening point 70°C) 1.0 part by mass Polyethylene wax (melting point 88°C) 4.0 parts by weight Toluene 95.0 parts by mass
[0048] <Preparation of coating liquid for heat-meltable colored ink layer> A coating solution for a heat-meltable colored ink layer to be used in a thermal transfer sheet was prepared according to the following formulation. (Heat-melting colored ink layer coating liquid) Thermoplastic polyester resin (softening point 60°C) 6.0 parts by mass Carbon black 6.0 parts by weight Pigment dispersant 0.6 parts by weight Methyl ethyl ketone 70.0 parts by mass Toluene 17.4 parts by mass
[0049] Example 1 <Preparation of thermal transfer sheet> [Formation of heat-resistant slip layer] Coating solution 1 for the heat-resistant slipping layer was applied by gravure coating to one side of a 4.5 micron thick PET (polyethylene terephthalate) film so that the coating thickness after drying would be 0.05 μm, and the film was dried by heating with hot air 5°C higher than the melting point of the blended hydrocarbon-based synthetic wax to form a heat-resistant slipping layer. [Formation of peeling layer] A release layer coating liquid was applied by bar coating to the side of the PET film opposite the side on which the heat-resistant slip layer was formed, so that the coating thickness after drying would be 0.6 μm, and the coating was heated and dried with hot air at 60° C. to form a release layer. [Formation of heat-meltable colored ink layer] On the release layer formed, a heat-fusible colored ink layer coating liquid was applied by gravure coating so that the coating thickness after drying would be 1.2 μm, and the coating liquid was heated and dried with hot air at 60° C. to form a heat-fusible colored ink layer, thereby obtaining a thermal transfer sheet having a layer structure of heat-resistant slip layer / substrate / release layer / colored ink layer.
[0050] Example 2 A thermal transfer sheet was obtained in the same manner as in Example 1, except that the coating liquid for the heat-resistant slipping layer in Example 1 was changed to Coating Liquid 2.
[0051] Example 3 A thermal transfer sheet was obtained in the same manner as in Example 1, except that the coating liquid for the heat-resistant slipping layer in Example 1 was changed to Coating Liquid 3.
[0052] Example 4 A thermal transfer sheet was obtained in the same manner as in Example 1, except that the coating liquid for the heat-resistant slipping layer in Example 1 was changed to Coating Liquid 4.
[0053] Example 5 A thermal transfer sheet was obtained in the same manner as in Example 1, except that the coating liquid for the heat-resistant slipping layer in Example 1 was changed to Coating Liquid 5.
[0054] Example 6 A thermal transfer sheet was obtained in the same manner as in Example 1, except that the coating liquid for the heat-resistant slipping layer in Example 1 was changed to Coating Liquid 6.
[0055] Example 7 A thermal transfer sheet was obtained in the same manner as in Example 1, except that the coating liquid for the heat-resistant slipping layer in Example 1 was changed to Coating Liquid 7.
[0056] Example 8 A thermal transfer sheet was obtained in the same manner as in Example 1, except that the coating liquid for the heat-resistant slipping layer in Example 1 was changed to Coating Liquid 8.
[0057] Example 9 A thermal transfer sheet was obtained in the same manner as in Example 1, except that the coating liquid for the heat-resistant slipping layer in Example 1 was changed to Coating Liquid 9.
[0058] Example 10 A thermal transfer sheet was obtained in the same manner as in Example 1, except that the coating liquid for the heat-resistant slipping layer in Example 1 was changed to Coating Liquid 10.
[0059] Example 11 A thermal transfer sheet was obtained in the same manner as in Example 1, except that the coating liquid for the heat-resistant slipping layer in Example 1 was changed to Coating Liquid 11 and the coating thickness of the heat-resistant slipping layer after drying was changed to 0.20 μm.
[0060] Example 12 A thermal transfer sheet was obtained in the same manner as in Example 1, except that the coating liquid for the heat-resistant slipping layer in Example 1 was changed to Coating Liquid 12 and the coating thickness of the heat-resistant slipping layer after drying was changed to 0.02 μm.
[0061] Comparative Example 1 A thermal transfer sheet was obtained in the same manner as in Example 1, except that the coating liquid for the heat-resistant slipping layer in Example 1 was changed to Coating Liquid 13.
[0062] Comparative Example 2 A thermal transfer sheet was obtained in the same manner as in Example 1, except that the coating liquid for the heat-resistant slipping layer in Example 1 was changed to Coating Liquid 14.
[0063] Comparative Example 3 A thermal transfer sheet was obtained in the same manner as in Example 1, except that the coating liquid for the heat-resistant slipping layer in Example 1 was changed to Coating Liquid 15.
[0064] Comparative Example 4 A thermal transfer sheet was obtained in the same manner as in Example 1, except that the coating liquid for the heat-resistant slipping layer in Example 1 was changed to Coating Liquid 16.
[0065] Comparative Example 5 A thermal transfer sheet was obtained in the same manner as in Example 1, except that the coating liquid for the heat-resistant slipping layer in Example 1 was changed to Coating Liquid 17.
[0066] <Heat resistance evaluation> Using the thermal transfer sheets of Examples 1 to 12 and Comparative Examples 1 to 5, printing was performed under the following printing conditions, and the print-free areas on the thermal transfer sheets after printing were visually inspected and evaluated according to the following evaluation criteria. The evaluation results are shown in Table 2. (If it is rated ○ or higher, there is no problem in practical use.) (Printing conditions) Printer: Zebra 110Xi4 Printing speed: 76mm / sec Print energy: 20, 30 (max) Transfer target: Lintec FR1415 (PET film) Printing pattern: Printing pattern A (see Figure 2 for a pattern diagram) (Evaluation Criteria) ◎: No tears in the substrate at printing energy 30 ○: No tears in the substrate at printing energy 20 ×: The substrate is torn at printing energy 20.
[0067] <Print slip evaluation> Using the thermal transfer sheets of Examples 1 to 12 and Comparative Examples 1 to 5, printing was performed under the following printing conditions, the print length and the length of the print gap on the thermal transfer sheet after printing were measured, and the slip rate was calculated using the following calculation formula 1 and evaluated according to the following evaluation criteria. The evaluation results are shown in Table 2. (Printing conditions) Printer: Zebra 110Xi4 Printing speed: 76mm / sec Printing energy: 30 (max) Transfer target: Lintec FR1415 (PET film) Printing pattern: Printing pattern A (see Figure 2 for a pattern diagram) (Formula 1) Slip rate (%) = {[length of print gap on thermal transfer sheet] / [print length]} x 100 (Evaluation Criteria) ◎: Slip rate is 98.5% or more ○: Slip rate is 95.0% or more and less than 98.5% ×: Slip rate is less than 95.0%
[0068] <Head trash evaluation> Using the thermal transfer sheets of Examples 1 to 12 and Comparative Examples 1 to 5, 50 m of printing was performed continuously under the following printing conditions, and the state of head residue attached to the thermal head was observed under a microscope (20 times magnification), and the presence or absence of printing defects (whiteouts, etc.) in the printed matter was visually confirmed, and evaluated according to the following evaluation criteria. The evaluation results are shown in Table 2. (Printing conditions) Printer: Ishida BP-4300 Printing speed: 100mm / sec Printing energy: 95% Transfer target: Lintec FR1415 (PET film) Printing pattern: Printing pattern B (pattern diagram shown in Figure 3) is printed repeatedly (50m continuous) (Evaluation Criteria) ○: No significant adhesion of head residue to the thermal head, no printing defects ×: There is significant head residue adhering to the thermal head, causing printing defects.
[0069] <Evaluation of blocking resistance> The thermal transfer sheets of Examples 1 to 12 and Comparative Examples 1 to 5 were each cut into a 90 mm wide strip, and while a tension of 100 mN / mm width was applied in the longitudinal direction of the thermal transfer sheet, 300 m was wound up on a paper tube with an outer diameter of 35 mm with the thermal transfer ink layer side facing inward to form a roll, and stored at 45°C and 85% RH for 96 hours, then taken out at room temperature and left for at least one day, after which the thermal transfer sheet was unwound and the blocking state (offset) was visually confirmed and evaluated according to the following criteria. The evaluation results are shown in Table 2. (If it is rated ○ or higher, there is no problem in practical use.) (Evaluation Criteria) ◎: The roll could be unwound all the way to the core, and no transfer of the thermal transfer ink to the heat-resistant slipping layer (offset) was observed. ○: The film could be unwound up to the core, but very slight offset was observed within 0.5 m from the core. ×: Set-off was observed 0.5 m or more away from the core.
[0070] <Tape peel strength evaluation> For each of the PET films formed with the heat-resistant slipping layer in Examples 1 to 12 and Comparative Examples 1 to 5, the PET film was fixed to a SUS plate so that the heat-resistant slipping layer side was facing up, Nitto Denko 31B tape (25 mm wide) was attached to the heat-resistant slipping layer side, and the top surface of the tape was pressed with a rubber roller of 2 kg·f back and forth once, and then left at 23±2°C for 10 minutes. After that, the Nitto Denko 31B tape was peeled off at a peel angle of 180° and a peel speed of 1,200 mm / min using a tensile tester, and the peel force was measured and evaluated according to the following evaluation criteria. The evaluation results are shown in Table 2. (Evaluation Criteria) ◎: Peeling force is 1.5N / 25mm or less ○: Peeling force is over 1.5N and 2.0N / 25mm or less ×: Peeling force exceeds 2.0N / 25mm
[0071] [Table 2] [Explanation of symbols]
[0072] 1: Thermal transfer sheet 2: Thermal transfer ink layer 3: Base material 4: Heat-resistant slippery layer
Claims
1. 1. A thermal transfer sheet having a heat-meltable thermal transfer ink layer on one side of a substrate and a heat-resistant slipping layer on the other side of the substrate, wherein the heat-resistant slipping layer is made of a long-chain alkyl pendant resin having a long-chain alkyl group on its side chain and a hydrocarbon synthetic wax, the long-chain alkyl pendant resin being a reaction product of an ethylene-vinyl alcohol copolymer and a monofunctional isocyanate having a linear alkyl group having 12 to 22 carbon atoms, the hydrocarbon synthetic wax being an ethylene oxide-propylene oxide copolymer wax and / or a Fischer-Tropsch wax oxide, the hydrocarbon synthetic wax having a melting point in the range of 100 to 130°C and an acid value in the range of 17 to 30 mgKOH / g, and the blending of the long-chain alkyl pendant resin and the hydrocarbon synthetic wax in the heat-resistant slipping layer is such that the mass ratio of the long-chain alkyl pendant resin to the hydrocarbon synthetic wax is in the range of 35 / 65 to 75 / 25.
2. 2. The thermal transfer sheet according to claim 1, wherein the weight average molecular weight (Mw) of the hydrocarbon synthetic wax is in the range of 2,500 to 9,500.
3. 2. The thermal transfer sheet according to claim 1, wherein the heat-resistant slip layer has a thickness in the range of 0.02 to 0.20 μm.
4. 2. The thermal transfer sheet according to claim 1, wherein the heat-resistant slipping layer has a tape peel strength of 2.0 N / 25 mm or less.
5. The thermal transfer sheet according to claim 1, characterized in that the heat-resistant slipping layer is formed by applying a heat-resistant slipping layer coating liquid to a predetermined thickness, and then heating and drying the heat-resistant slipping layer at a temperature equal to or higher than the melting point of the hydrocarbon-based synthetic wax to form a coating film in which the long-chain alkyl pendant resin of the heat-resistant slipping layer and the hydrocarbon-based synthetic wax are uniformly dissolved.
Citation Information
Patent Citations
Thermal transfer recording medium
JP1987082086A
Thermal transfer ink sheet and heat resistant film to be used therefor
JP1992016390A
Thermal transfer sheet
JP1993064987A
Thermal transfer sheet and coating solution
JP1994135166A