Method for producing ε-caprolactam, and method for producing polyamide 6
The method depolymerizes polyamide 6 composite materials with subcritical water and copper compounds to efficiently produce ε-caprolactam, addressing energy and emission challenges in recycling processes.
Patent Information
- Application Number
- JP2023067101
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for recycling polyamide 6 to produce ε-caprolactam face challenges such as high energy consumption, long reaction times, and catalyst deactivation due to impurities, which hinder efficient recycling and reduction of global warming gas emissions.
A method involving the depolymerization of a composite material containing polyamide 6 and other resins with subcritical water at controlled temperatures and pressures, using a copper compound to enhance efficiency, without prior separation of components, and producing ε-caprolactam with high yield and low energy consumption.
This method achieves high yield and low energy consumption in producing ε-caprolactam, facilitating the cyclical use of fossil resources and reducing global warming gas emissions by optimizing the depolymerization process.
Smart Images

Figure 2024153300000001 
Figure 2024153300000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing ε-caprolactam and a method for producing polyamide 6. [Background technology]
[0002] In recent years, interest in global environmental issues has increased, triggered by the problem of marine plastic pollution, and awareness of the need to build a sustainable society is spreading. Global environmental issues include global warming, resource depletion, and water shortages. Many of these global environmental issues are caused by the rapid increase in resource consumption and greenhouse gas emissions due to human activity since the Industrial Revolution.
[0003] Therefore, in order to build a sustainable society, technologies for recycling fossil resources such as plastics and reducing greenhouse gas emissions will become increasingly important.
[0004] As a method for recycling polyamide 6, which is used in large quantities in various fields as fibers, films, and engineering plastics, a method for obtaining ε-caprolactam by blowing in superheated steam in the presence of a phosphoric acid catalyst has been disclosed (see, for example, Patent Document 1). In addition, a method for recovering ε-caprolactam with high purity and high yield by chemical recycling of a polyamide 6 composite material using a similar method has been disclosed (see, for example, Patent Documents 2 and 3).
[0005] In addition, as a method for depolymerizing polyamide 6 without using a catalyst such as an acid or a base, a method has been disclosed in which polyamide 6 is contacted with superheated water at a temperature of 280°C to 320°C to recover ε-caprolactam (see, for example, Patent Document 4). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 8-217746 [Patent Document 2] JP 2008-31127 A [Patent Document 3] JP 2008-179816 A [Patent Document 4] Japanese Patent Application Publication No. 10-510280 Summary of the Invention [Problem to be solved by the invention]
[0007] The method for recovering ε-caprolactam disclosed in Patent Document 1 is a high-yield reaction with a depolymerization yield of 80% or more for polyamide 6, but the depolymerization reaction takes a long time. Furthermore, since a large amount of superheated steam, about 10 times the amount of polyamide 6 fiber, is required, it is a technology that has problems in achieving both fossil resource recycling and reduction of greenhouse gas emissions. In addition, since this method is a reaction using phosphoric acid as a catalyst, it is a reaction that is easily affected by impurities, such as catalyst deactivation by additives contained in plastics and impurities attached to waste plastics. In fact, when the inventors performed a recovery experiment using polyamide 6 containing potassium salt as a raw material under the same or similar conditions as the method described in Patent Document 1, it was found that the yield was significantly reduced. The inventors speculate that this is due to the deactivation of the phosphoric acid catalytic action by potassium salt.
[0008] In addition, Patent Documents 2 and 3 disclose methods for recovering ε-caprolactam from a composite material mainly composed of polyamide 6. However, in order to recover ε-caprolactam with high purity and high yield, a pretreatment of the composite material using a large amount of an alkaline aqueous solution or an organic solvent such as dimethylformamide to remove components other than polyamide 6 is an essential technique, and a large amount of energy is required to purify and reuse the large amount of solvent used in this pretreatment.
[0009] On the other hand, the method for recovering ε-caprolactam disclosed in Patent Document 4 uses only water in the depolymerization reaction and does not use a catalyst such as phosphoric acid, and therefore has the advantage that the reaction is not deactivated by additives or adhering impurities. However, the disclosed method for recovering ε-caprolactam requires a large amount of water, which has a very high specific heat capacity of 4.2 kJ / kg·K and a heat of vaporization of 2,250 kJ / kg, about 10 times the amount of water used for polyamide 6, and the reaction is carried out for a long time, so a large amount of energy is required for the depolymerization reaction and the recovery of ε-caprolactam from the low-concentration aqueous solution of ε-caprolactam. In addition, simply reducing the amount of water used under the same or similar conditions only reduced the recovery rate of ε-caprolactam. The present inventors speculate that this is because the thermodynamic equilibrium point between ε-caprolactam produced by depolymerization and linear oligomers produced by hydrolytic ring-opening of ε-caprolactam shifts to the linear oligomer side when the amount of water used is simply reduced. Furthermore, Patent Document 4 does not mention at all the simultaneous depolymerization of a composite material consisting of at least two types of resins, the main component of which is polyamide 6. [Means for solving the problem]
[0010] In order to solve the above problems, the present invention has the following configuration. (1) A method for producing epsilon-caprolactam by contacting a composite material (A) consisting of at least two types of resins, the composite material (A) being mainly composed of polyamide 6, with water (B) having a temperature of 290°C or higher and 350°C or lower, the method comprising the steps of: (a) contacting the composite material (A) with water (B) at a temperature of 290°C or higher and 350°C or lower, the mass ratio of water (B) to composite material (A) (water (B):composite material (A)) being X:1, and (b) providing a reaction temperature of Y°C, such that the product of X and Y is 2,000 or lower. (2) A method for producing ε-caprolactam as described in (1) above, in which resin components other than polyamide 6 in the composite material (A) are also obtained as valuable materials. (3) The method for producing ε-caprolactam according to (1) or (2) above, wherein the pressure when the composite material (A) is contacted with the water (B) is 7.5 MPa or more and 30 MPa or less. (4) The method for producing ε-caprolactam according to any one of (1) to (3) above, further comprising a copper compound when the composite material (A) is brought into contact with the water (B). (5) The method for producing ε-caprolactam according to any one of (1) to (4) above, wherein the contact is carried out under conditions such that the product of X, Y and Z is 60,000 or less, where the residence time at a reaction temperature of Y° C. is Z minutes. (6) The method for producing ε-caprolactam according to the above (4) or (5), wherein the copper compound is at least one selected from the group consisting of organic copper salts and inorganic copper salts. (7) The method for producing ε-caprolactam according to any one of (2) to (6) above, wherein the valuable product other than ε-caprolactam is glycol. (8) The method for producing ε-caprolactam according to any one of (1) to (7) above, wherein the composite material (A) contains polyamide 6 and at least one of polyester and polyurethane. (9) A method for producing polyamide 6, comprising the steps of obtaining ε-caprolactam by the method for producing ε-caprolactam according to any one of the above (1) to (8) and polymerizing the obtained ε-caprolactam to obtain polyamide 6. Effect of the Invention
[0011] The present invention provides a method for producing ε-caprolactam with low energy consumption, since it is not necessary to separate components other than polyamide 6 in advance in the depolymerization of a composite material mainly composed of polyamide 6, and furthermore, ε-caprolactam can be produced in high yield even with a small amount of water having a high specific heat capacity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will now be described in further detail.
[0013] The method for producing ε-caprolactam of the present invention comprises contacting a composite material (A) consisting of at least two kinds of resins, the composite material (A) containing polyamide 6 as a main component, with water (B) having a temperature of 290°C or higher and 350°C or lower, and the contact is carried out under the condition that, when the mass ratio of water (B) to composite material (A) (water (B):composite material (A)) is X:1 and the reaction temperature is Y°C, the product of X and Y is 2,000 or less.
[0014] (1) Composite material (A) The method for producing ε-caprolactam of the present invention is a method for producing ε-caprolactam by contacting a composite material (A) containing polyamide 6 as a main component and comprising at least two types of resin with water (B) at a temperature of 290°C or higher and 350°C or lower.
[0015] The polyamide 6 used in the present invention is a polyamide resin whose main raw material is 6-aminocaproic acid and / or ε-caprolactam. Other monomers may be copolymerized within the scope of the present invention. Here, "main raw material" means that the polyamide resin contains 50 mol% or more of units derived from 6-aminocaproic acid or ε-caprolactam in total out of 100 mol% of the total monomer units constituting the polyamide resin. It is more preferable that the polyamide resin contains 70 mol% or more of units derived from 6-aminocaproic acid or ε-caprolactam, and even more preferable that the polyamide resin contains 90 mol% or more of units derived from 6-aminocaproic acid or ε-caprolactam.
[0016] Examples of other monomers to be copolymerized include amino acids such as 11-aminoundecanoic acid, 12-aminododecanoic acid, and para-aminomethylbenzoic acid, lactams such as ω-laurolactam, aliphatic diamines such as tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, 2-methylpentamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, 2,2,4- / 2,4,4-trimethylhexamethylenediamine, and 5-methylnonamethylenediamine, aromatic diamines such as metaxylylenediamine and paraxylylenediamine, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, biphenyls, and the like. Examples of the diamine include alicyclic diamines such as bis(4-aminocyclohexyl)methane, bis(3-methyl-4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, 1,4-bis(3-aminopropyl)piperazine, and 1-(2-aminoethyl)piperazine; aliphatic dicarboxylic acids such as adipic acid, suberic acid, azelaic acid, sebacic acid, and dodecanedioic acid; aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, 5-sodium sulfoisophthalic acid, and 2,6-naphthalenedicarboxylic acid; and alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, and 1,3-cyclopentanedicarboxylic acid. Two or more of these may be copolymerized.
[0017] Moreover, a polymerization degree regulator, a terminal group regulator, etc. may be added to the polyamide 6. Examples of the polymerization degree regulator and the terminal group regulator include acetic acid and benzoic acid.
[0018] In the method for producing ε-caprolactam of the present invention, the degree of polymerization of polyamide 6 is not particularly limited, but it is preferable that the relative viscosity measured in a 98% concentrated sulfuric acid solution having a resin concentration of 0.01 g / mL at 25° C. is in the range of 1.5 to 5.0. When the relative viscosity is in such a preferable range, the reaction efficiency with a small amount of water tends to be high.
[0019] The composite material (A) in the present invention is not particularly limited as long as it is a material composed of at least two kinds of resins, with polyamide 6 as the main component. Here, "polyamide 6 as the main component" means that the content of polyamide 6 in the resin constituting the composite material (A) is 50% by mass or more. The content of polyamide 6 is preferably 60% by mass or more, more preferably 70% by mass or more, and particularly preferably 80% by mass or more. By having the content of polyamide 6 within these ranges, ε-caprolactam can be produced with low environmental impact. As an analysis method for the polyamide 6 content in the composite material (A), for example, if the composite material (A) is clothing and the name of the type of raw material resin and the blending ratio written on the quality label can be confirmed, a method of judging from the quality label can be mentioned. In addition, in the case of a textile product where it is difficult to judge from the quality label, a test method for fiber blending ratio specified by JIS (JIS L 1030-1, 2) can be mentioned. Furthermore, if it is difficult to confirm the polyamide 6 content by any of these, an analysis method using the characteristic wave number of polyamide 6 by the total reflection measurement method (ATR method) can be mentioned.
[0020] Examples of the composite material (A) in the present invention include composite fibers obtained by simultaneously spinning two or more types of resins into a single fiber, blended yarns in which short fibers are mixed together, blended yarns in which long fibers are mixed together, covering yarns in which a core yarn is protected by a sheath yarn, fabrics, strings, and other fiber structures using these in part or in whole, repair materials in which polyamide 6 fiber products are repaired with fibers made of other resins, fiber components such as clothing in which not only polyamide 6 fibers but also other resins are contained as part of the component, multilayer films in which other resins are laminated or coated on a polyamide 6 film, modules such as indoor and outdoor structures and automobile parts containing polyamide 6, and resin compositions obtained by melt-kneading polyamide 6 with at least one or more other resins.
[0021] Specific examples of resins other than polyamide 6 contained in the composite material (A) include polyamides other than polyamide 6, polyesters, polyurethanes, polyolefins, modified polyphenylene ethers, polysulfones, polyketones, polyetherimides, polyarylates, polyethersulfones, polyetherketones, polythioetherketones, polyetheretherketones, polyimides, polyamideimides, polyethylene tetrafluoride, and polyphenylene sulfide. Among these, polyesters and polyurethanes are preferred. That is, in the method for producing ε-caprolactam of the present invention, it is preferred that the composite material (A) contains polyamide 6 and at least one of polyesters and polyurethanes. Note that two or more of these resins may be used.
[0022] Preferred examples of polyester and polyurethane will be described in detail below.
[0023] The polyester in the present invention is obtained by polycondensation of the dicarboxylic acid or its ester-forming derivative, which is a polyester component, and the diol as the main raw materials. Here, the main raw materials refer to the total of the dicarboxylic acid, its ester-forming derivative, and diol in the polymer being 80 mol% or more. The total of these structural units is more preferably 90 mol% or more, even more preferably 95 mol% or more, and most preferably 100 mol%.
[0024] Examples of dicarboxylic acids or ester-forming derivatives thereof include, but are not limited to, aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, diphenyl-4,4'-dicarboxylic acid, diphenyl ether-4,4'-dicarboxylic acid, diphenyl thioether-4,4'-dicarboxylic acid, 5-tetrabutylphosphonium isophthalic acid, and 5-sodium sulfoisophthalic acid; and aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, sebacic acid, azelaic acid, undecanedioic acid, and dodecanedioic acid, or ester-forming derivatives thereof.
[0025] The ester-forming derivatives referred to here are the lower alkyl esters, acid anhydrides, acid halides, etc. of the dicarboxylic acids mentioned above. The lower alkyl esters of dicarboxylic acids referred to here are esters of the dicarboxylic acids and alcohols having 1 to 4 carbon atoms or diols having 2 to 4 carbon atoms. As the lower alkyl esters of dicarboxylic acids, methyl esters, ethyl esters, hydroxyethyl esters, hydroxybutyl esters, etc. are preferably used. As the acid anhydrides of dicarboxylic acids, acid anhydrides of dicarboxylic acids and acid anhydrides of dicarboxylic acids and acetic acid are preferably used. As the halides of dicarboxylic acids, acid chlorides, acid bromides, acid iodides, etc. are preferably used.
[0026] As the dicarboxylic acid or its ester-forming derivative, an aromatic dicarboxylic acid or its ester-forming derivative is preferred because it is used in large amounts as a polyester raw material for fibers, resins, and films. As the aromatic dicarboxylic acid or its ester-forming derivative, terephthalic acid, 2,6-naphthalenedicarboxylic acid, or their dimethyl esters are more preferred.
[0027] Examples of the diol include ethylene glycol, 1,3-propanediol, neopentyl glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, decamethylene glycol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, cyclohexanedimethanol, xylylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, bisphenol A-ethylene oxide adduct, etc. Among these, ethylene glycol, 1,3-propanediol, and 1,4-butanediol are preferred because the resulting polyester has high versatility.
[0028] The dicarboxylic acid, the ester-forming derivative of the dicarboxylic acid, and the diol may each be used alone or in combination of two or more kinds.
[0029] Examples of polyesters in the present invention include polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, polycyclohexane dimethylene terephthalate, polyethylene isophthalate, polypropylene isophthalate, polybutylene isophthalate, polycyclohexane dimethylene isophthalate, polyethylene naphthalate, polypropylene naphthalate, polybutylene naphthalate, polycyclohexane dimethylene terephthalate / polyethylene terephthalate, polyethylene isophthalate / terephthalate, polypropylene isophthalate / terephthalate, polybutylene isophthalate / terephthalate, polyethylene terephthalate / naphthalate, polypropylene terephthalate / naphthalate, polybutylene terephthalate / naphthalate, polyethylene terephthalate / 5-sodium sulfoisophthalate, polypropylene terephthalate / 5-sodium sulfoisophthalate, polybutylene terephthalate / 5-sodium sulfoisophthalate, etc. Here, " / " represents a copolymer. Among these, polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate are preferred. Furthermore, polyethylene terephthalate, polypropylene terephthalate, and polybutylene terephthalate are more preferable because they are highly versatile and can be recovered in large amounts as a recycling resource.
[0030] The intrinsic viscosity of the polyester used in the present invention is preferably 0.4 to 2.0 dl / g. Here, the intrinsic viscosity of the polyester is a value measured at 25°C using o-chlorophenol as a solvent. When the intrinsic viscosity of the polyester is in such a preferred range, the reaction efficiency with a small amount of water increases, and the energy required for depolymerization of the composite material tends to be low. When the polyester used in the present invention is polyethylene terephthalate, the intrinsic viscosity is preferably 0.4 to 1.5 dl / g, more preferably 0.6 to 1.3 dl / g. When the polyester used in the present invention is polypropylene terephthalate, the intrinsic viscosity is more preferably 0.6 to 2.0 dl / g, more preferably 0.7 to 1.6 dl / g. When the polyester used in the present invention is polybutylene terephthalate, the intrinsic viscosity is more preferably 0.6 to 2.0 dl / g, more preferably 0.8 to 1.8 dl / g.
[0031] The polyurethane in the present invention is not particularly limited, and may be any polyurethane that uses polymer diol and diisocyanate, which are polyurethane constituents, as starting materials. In addition, polyurethane urea may be a polyurethane made of polymer diol, diisocyanate, and low molecular weight diamine as a chain extender, polyurethane made of polymer diol, diisocyanate, and low molecular weight diol as a chain extender, or polyurethane urea using a compound having a hydroxyl group and an amino group in the molecule as a chain extender.
[0032] The polymer diol used in the present invention is preferably at least one selected from polyether diols, polyester diols, and polycarbonate diols.
[0033] As the polyether diol, for example, polyethylene oxide, polyethylene glycol, a derivative of polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol (hereinafter abbreviated as PTMG), tetrahydrofuran (hereinafter abbreviated as THF), modified PTMG which is a copolymer of 3-methyltetrahydrofuran, modified PTMG which is a copolymer of THF and 2,3-dimethylTHF, polyols having side chains on both sides, such as a copolymer of neopentyl glycol and THF, random copolymers in which THF and ethylene oxide and / or propylene oxide are irregularly arranged, etc. may be preferably used. These polyether diols may be used alone or in a mixture or copolymer of two or more kinds.
[0034] Also usable are butylene adipate, polycaprolactone diol, polyester-based diols such as polyester polyols having side chains obtained by polycondensing, for example, polypropylene polyol with a dicarboxylic acid such as adipic acid, and polycarbonate diols.
[0035] The above polymer diols may be used alone, or two or more kinds may be mixed or copolymerized for use.
[0036] From the viewpoint of maintaining practical strength, the molecular weight of the polymer diol used in the present invention is preferably a number average molecular weight of 1,000 or more and 8,000 or less, and more preferably 1,800 or more and 6,000 or less.
[0037] Examples of the diisocyanate used in the present invention include aromatic diisocyanates such as diphenylmethane diisocyanate, tolylene diisocyanate, 1,4-diisocyanate benzene, xylylene diisocyanate, and 2,6-naphthalene diisocyanate, and alicyclic diisocyanates such as methylene bis(cyclohexyl isocyanate), isophorone diisocyanate, methylcyclohexane 2,4-diisocyanate, methylcyclohexane 2,6-diisocyanate, cyclohexane 1,4-diisocyanate, hexahydroxylylene diisocyanate, hexahydrotolylene diisocyanate, and octahydro-1,5-naphthalene diisocyanate. In particular, when it is desired to suppress yellowing of polyurethane yarn, it is preferable to use an alicyclic diisocyanate. These diisocyanates may be used alone or in combination of two or more.
[0038] In the present invention, the molecular weight of the polyurethane is preferably in the range of 30,000 to 150,000 in terms of number average molecular weight, from the viewpoint of maintaining practical strength and facilitating reaction with water (B). The molecular weight is measured by GPC (gel permeation chromatography) using tetrahydrofuran (THF) as a solvent, and converted into polymethyl methacrylate.
[0039] In the present invention, the composite material (A) may be waste of composite materials. Examples of waste of composite materials include polyamide 6 products, industrial waste generated during the manufacturing process of polyamide 6 products, and used waste of polyamide 6 products. Examples of polyamide 6 products include textile structures for clothing such as used clothes, uniforms, sportswear, and innerwear, industrial textile structures such as curtains, carpets, ropes, nets, belts, and sheets, molded parts for housing construction materials, electrical and electronic molded parts, aircraft parts, industrial machine parts, film products, extrusion molded products, on-site polymerization molded products, and RIM molded products. In addition, product scraps, pellet scraps, lump scraps, and cutting scraps generated during cutting processing are also subject to waste.
[0040] (2) Method for producing ε-caprolactam In the method for producing ε-caprolactam of the present invention, when a composite material (A) is brought into contact with water (B) having a temperature of 290° C. or more and 350° C. or less, the contact is carried out under the condition that, when the mass ratio of water (B) to composite material (A) (water (B):composite material (A)) is X:1 and the reaction temperature is Y° C., the product of X and Y is 2,000 or less.
[0041] The water (B) used here is not particularly limited, and any type of water may be used, such as tap water, ion-exchanged water, distilled water, well water, etc. From the viewpoint of suppressing side reactions caused by the influence of coexisting salts, it is preferable that the water (B) is ion-exchanged water or distilled water.
[0042] Water (B) is water with a temperature of 290°C or more and 350°C or less. When water is heated to a pressure of 22.1 MPa and a temperature of 374.2°C, it is in a state that is neither liquid nor gas. This point is called the critical point of water, and hot water with a temperature and pressure lower than the critical point is called subcritical water. The temperature of water (B) used in the present invention is 290°C or more and 350°C or less, which corresponds to subcritical water. Although this subcritical water is water, it has the characteristics of (i) a low dielectric constant and (ii) a high ionic product. The dielectric constant and ionic product of subcritical water depend on the temperature and partial pressure of water, and can be controlled. The low dielectric constant makes it an excellent solvent for organic compounds, even though it is water, and the high ionic product makes it have high concentrations of hydrogen ions and hydroxide ions, resulting in excellent hydrolysis action.
[0043] In the method for producing ε-caprolactam of the present invention, the temperature of the water (B) is preferably 300° C. or more and 340° C. or less, and more preferably 320° C. or more and 340° C. or less. When the temperature is in such a preferred range, corrosion of the apparatus during the reaction tends to be suppressed.
[0044] In addition, the pressure of the water (B) is preferably higher than the saturated vapor pressure. Specifically, the pressure when the composite material (A) and the water (B) are contacted is preferably 7.5 MPa or more and 30 MPa or less, more preferably 8.0 MPa or more and 25 MPa or less, and even more preferably 10.0 MPa or more and 22 MPa or less. By being in such a pressure range, the ionic product of the water tends to be high. For example, a method for making the water (B) in such a pressure range is a method of pressurizing the inside of a pressure vessel and sealing it. For example, a method for pressurizing the inside of a pressure vessel is a method of sealing a gas in addition to the water (B). Examples of such a gas include air, argon, and nitrogen. Among them, nitrogen and argon are preferable from the viewpoint of suppressing side reactions such as oxidation reactions. The degree of gas pressurization is not particularly limited because it is set to the desired pressure, but 0.3 MPa or more is preferable.
[0045] The method for producing ε-caprolactam of the present invention is characterized in that, when the mass ratio of water (B) to the composite material (A) (water (B):composite material (A)) is X:1 and the reaction temperature is Y°C, the product of X and Y is 2,000 or less. The product of X and Y is preferably 1,600 or less, more preferably 1,300 or less, and particularly preferably 1,200 or less. There is no particular restriction on the lower limit of the product of X and Y, but it is preferably 300, more preferably 320, and particularly preferably 340. In addition, when the mass ratio of water (B) to polyamide 6 in the composite material (A) is Xa:1 and the reaction temperature is Y°C, the product of Xa and Y is preferably 2,000 or less, more preferably 1,600 or less, more preferably 1,300 or less, and particularly preferably 1,200 or less. Furthermore, the lower limit of the product of Xa and Y is not particularly limited, but is preferably 300, more preferably 320, and particularly preferably 340. As described above, the present invention relates to the energy-saving production of ε-caprolactam from a composite material mainly composed of polyamide 6, which aims to achieve both the cyclical use of fossil resources and the reduction of greenhouse gas emissions. Since the specific heat capacity of water is 4.3 kJ / kg·K and the heat of vaporization is 2,250 kJ / kg, which are very high compared to other organic solvents, it is important to reduce the amount of water used in order to produce it in an energy-saving manner. On the other hand, in addition to the production of ε-caprolactam in the reaction of polyamide 6 with water, a side reaction of the reaction of ε-caprolactam with water to produce linear oligomers proceeds as a side reaction. Therefore, if the amount of water used is simply reduced, a large amount of linear oligomers are produced, and the production efficiency of ε-caprolactam is significantly reduced. Therefore, the present inventors analyzed the thermodynamic equilibrium points of the reaction of producing ε-caprolactam by reacting polyamide with water and the side reaction of producing linear oligomers, and found that in the method for producing ε-caprolactam of the present invention, by setting the product of X and Y, preferably the product of Xa and Y, within these condition ranges, it is possible to suppress the by-production of linear oligomers and significantly improve the production efficiency of ε-caprolactam, thereby achieving both efficient production of ε-caprolactam and energy saving, thereby arriving at the present invention.
[0046] In the method for producing ε-caprolactam of the present invention, when the residence time at a reaction temperature of Y° C. is Z minutes, it is preferable to contact under conditions where the product of X, Y, and Z is 60,000 or less. The product of X, Y, and Z is more preferably 40,000 or less, even more preferably 30,000 or less, and particularly preferably 20,000 or less. There is no particular restriction on the lower limit of the product of X, Y, and Z, but it is preferably 5,000, more preferably 8,000, and particularly preferably 9,000. Furthermore, it is more preferable to contact under conditions where the product of Xa, Y, and Z is 60,000 or less, even more preferably 40,000 or less, and particularly preferably 30,000 or less. There is also no particular restriction on the lower limit of Xa, Y, and Z, but it is more preferably 5,000, even more preferably 8,000, and particularly preferably 9,000. By setting the product of X, Y and Z, or the product of Xa, Y and Z, within such a preferable range of conditions, it is possible to produce ε-caprolactam with greater energy savings.
[0047] In the method for producing ε-caprolactam of the present invention, it is preferable to obtain the resin components other than polyamide 6 in the composite material (A) as valuable materials. The polyamide 6 and resins other than polyamide 6 constituting the composite material (A) can be simultaneously depolymerized without pretreatment using a large amount of an aqueous alkaline solution or an organic solvent. The valuable materials here are not particularly limited as long as they are resin components other than polyamide 6, and preferably include main raw materials for polymerization that can be used in polymerization of recycled resins. Among them, it is preferable that the valuable materials other than ε-caprolactam are glycols. By obtaining the resin components other than polyamide 6 as valuable materials, the amount of waste generated when processing the composite material can be significantly reduced, and it is possible to achieve both the cyclical use of fossil resources and the reduction of greenhouse gas emissions at a higher level.
[0048] In the method for producing ε-caprolactam of the present invention, it is preferable to further include a copper compound when the composite material (A) and water (B) are brought into contact with each other. The presence of the copper compound in the reaction system tends to significantly improve the efficiency of producing ε-caprolactam by the reaction of the composite material (A) and water (B). The copper compound may be added when the composite material (A) and water (B) are brought into contact with each other to react, or the composite material (A) and the copper compound may be mixed in advance by melt kneading or the like and used for the reaction. The copper compound may also be a copper compound contained as a constituent of the composite material (A).
[0049] The copper valence in the copper compound may be either monovalent or divalent. The copper compound may be a hydrate. Two or more kinds of copper compounds may be used in combination.
[0050] In the method for producing ε-caprolactam of the present invention, the copper compound is not particularly limited, but is preferably at least one selected from the group consisting of organic copper salts and inorganic copper salts.
[0051] Examples of organic copper salts include copper formate, copper acetate, copper propionate, copper butyrate, copper valerate, copper caproate, copper enanthate, copper caprylate, copper pelargonate, copper caprate, copper undecylate, copper laurate, copper tridecylate, copper myristate, copper pentadecylate, copper palmitate, copper margarate, copper stearate, copper nonadecylate, copper arachidate, copper henicosylate, copper behenate, copper tridecylate, copper lignocerate, copper cerotic acid, copper montanate, copper melissic acid, copper benzoate, copper oxalate, copper malonate, copper succinate, copper terephthalate, copper isophthalate, copper phthalate, copper salicylate, copper citrate, and copper tartrate.
[0052] Examples of inorganic copper salts include copper sulfate, copper carbonate, copper nitrate, copper halides such as copper iodide, copper bromide and copper chloride, copper hydroxide, and copper oxide.
[0053] Among them, the copper compound is more preferably at least one selected from the group consisting of organic copper salts, copper sulfate, copper carbonate, copper nitrate, copper halides, copper hydroxide, and copper oxide, and even more preferably at least one selected from organic copper salts, copper halides, copper hydroxide, and copper oxide. These copper compounds have excellent miscibility with the composite material (A) and are therefore easily dispersed in the composite material without agglomeration, and the yield of ε-caprolactam can be easily improved by adding a smaller amount.
[0054] The copper valence of these copper salts, i.e., organic copper salts and inorganic copper salts, may be either monovalent or divalent. Two or more kinds of copper salts may be used in combination. These copper salts may be hydrates.
[0055] For the production of ε-caprolactam of the present invention, various known reaction methods such as batch and continuous methods can be adopted. For example, in the case of batch methods, autoclaves equipped with a stirrer and a heating function, vertical and horizontal reactors, and vertical and horizontal reactors equipped with a compression mechanism such as a cylinder in addition to a stirrer and a heating function can be mentioned. In the case of continuous methods, extruders equipped with a heating function, tubular reactors, tubular reactors equipped with a mixing mechanism such as a baffle, line mixers, vertical and horizontal reactors, vertical and horizontal reactors equipped with a stirrer, towers, and the like can be mentioned. In addition, the atmosphere in the production is preferably a non-oxidizing atmosphere, and it is preferable to carry out the production under an inert atmosphere such as nitrogen, helium, and argon, and a nitrogen atmosphere is preferable from the viewpoints of economy and ease of handling.
[0056] (3) Recovery method of ε-caprolactam In the present invention, there is no particular limitation on the method for recovering ε-caprolactam, and any method can be adopted. For example, when the depolymerization reaction is carried out in a batchwise manner, after the depolymerization reaction is completed, the ε-caprolactam aqueous solution is distilled together with water to obtain the ε-caprolactam aqueous solution. When the depolymerization reaction is carried out in a continuous manner, the ε-caprolactam aqueous solution can be obtained as the reaction proceeds. The obtained ε-caprolactam aqueous solution can be separated from water by, for example, distillation to recover ε-caprolactam with high purity. In addition, if the recovered ε-caprolactam aqueous solution contains water-insoluble components, they can be separated in advance by a known method such as solid-liquid separation, and then subjected to distillation separation.
[0057] To obtain even higher purity ε-caprolactam, the recovered ε-caprolactam can be combined with other purification methods, such as precision distillation of the recovered ε-caprolactam, distillation under reduced pressure with the addition of a small amount of sodium hydroxide, treatment with activated carbon, ion exchange treatment, recrystallization, etc. These methods can efficiently remove impurities that are difficult to separate by distillation separation.
[0058] (4) Polyamide 6 and its molded products The method for producing polyamide 6 of the present invention includes a step of obtaining ε-caprolactam by the method for producing ε-caprolactam of the present invention, and a step of obtaining polyamide 6 by polymerizing the obtained ε-caprolactam.
[0059] The process for obtaining ε-caprolactam by the method for producing ε-caprolactam of the present invention is as described above. The method for producing ε-caprolactam of the present invention can obtain ε-caprolactam with high purity. Therefore, the obtained ε-caprolactam can be used as a polymerization raw material for polyamide 6.
[0060] Next, there will be described a step of polymerizing the obtained ε-caprolactam to obtain polyamide 6. Polyamide 6 can be produced, for example, by a commonly known method in which ε-caprolactam is heated and melt-polymerized in the presence of a small amount of water.
[0061] The polyamide 6 thus obtained can be melt-kneaded with a fibrous filler or various additives as necessary to produce a polyamide 6 resin composition, and various molded products such as sheets and films can be obtained by commonly known methods such as injection molding and extrusion molding.
[0062] The polyamide 6 of the present invention and its molded products can be utilized for various applications such as electric and electronic parts, building materials, various containers, daily necessities, household goods and sanitary goods, taking advantage of their excellent properties. In particular, they are preferably used for aircraft parts and electric and electronic parts applications that require toughness and rigidity. Specifically, they are used for aircraft-related parts such as landing gear pods, winglets, spoilers, edges, rudders, elevators, failings and ribs, electric and electronic parts such as generators, electric motors, transformers, current transformers, voltage regulators, rectifiers, resistors, inverters, relays, power contacts, switches, circuit breakers, switches, knife switches, multi-pole rods, motor cases, television housings, notebook computer housings and internal parts, CRT display housings and internal parts, printer housings and internal parts, mobile terminal housings and internal parts such as mobile phones, mobile personal computers and handheld mobiles, housings for ICs and LEDs, capacitor seat plates, fuse holders, various gears, various cases, etc. These include electrical components such as switchgear and cabinets, connectors, SMT-compatible connectors, card connectors, jacks, coils, coil bobbins, sensors, LED lamps, sockets, resistors, relays, relay cases, reflectors, small switches, power supply components, coil bobbins, capacitors, variable capacitor cases, optical pickup chassis, oscillators, various terminal boards, transformers, plugs, printed circuit boards, tuners, speakers, microphones, headphones, small motors, magnetic head bases, power modules, Si power modules and SiC power modules, semiconductors, liquid crystal displays, FDD carriages, FDD chassis, motor brush holders, transformer components, parabolic antennas, and computer-related parts. EXAMPLES
[0063] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.
[0064] Evaluation method (ε-caprolactam yield (HPLC)) The ε-caprolactam yield (HPLC) was calculated by high performance liquid chromatography under the following measurement conditions. Equipment: Shimadzu LC-10Avp series Column: Mightysil RP-18GP150-4.6 Detector: Photodiode array detector (UV=205nm) Flow rate: 0.5mL / min Column temperature: 40℃ Mobile phase: 0.1% acetic acid aqueous solution / acetonitrile (mixture ratio: 90wt% / 10wt%) Sample: 0.1 g of the reaction mixture was weighed out, diluted with approximately 10 g of deionized water, and components insoluble in deionized water were separated and removed by filtration to prepare a sample for high performance liquid chromatography analysis. Quantitative determination of ε-caprolactam: The amount of ε-caprolactam relative to polyamide 6 was quantified using the absolute calibration curve method.
[0065] (Ethylene glycol yield (GC)) The ethylene glycol yield (GC) was calculated by gas chromatography under the following measurement conditions. Equipment: Shimadzu GC-2010 Column: Agilent Technologies DB-5 0.32mm x 30m (0.25μm) Carrier gas: Helium Detector: Flame ionization detector (FID) Sample: Approximately 1.2 g of the reaction mixture was weighed out, diluted with approximately 5 g of methanol, and filtered to separate and remove components insoluble in methanol, to prepare a sample for gas chromatography analysis. Quantitative determination of ethylene glycol: The amount of ethylene glycol relative to polyethylene terephthalate was determined using an absolute calibration curve.
[0066] [Reference example 1] Into a SUS316L autoclave equipped with a stirrer, 20.0 g of polyamide 6 ("Amilan" (registered trademark) CM1017 manufactured by Toray Industries, Inc.) and 60.0 g of deionized water were charged. The mass ratio of water to polyamide 6 was 3:1.
[0067] The reaction vessel was replaced with nitrogen, and then sealed under a nitrogen pressure of 0.5 MPa. The reaction was carried out by holding the temperature at 320°C for 15 minutes while stirring at 200 rpm. The pressure reached during the reaction was 10.5 MPa. After the reaction was completed, the reaction mixture was cooled to room temperature and collected.
[0068] The yield of ε-caprolactam calculated from the recovered reaction mixture by high performance liquid chromatography was 78%.
[0069] [Example 1] A SUS316L autoclave equipped with a stirrer was charged with 23.8 g of a knitted fabric (20.0 g of polyamide 6 fiber, 3.8 g of polyurethane fiber) made by combining polyamide 6 fiber (manufactured by Toray Industries, Inc.) and polyurethane elastic fiber (Lycra manufactured by Toray Opelontex Co., Ltd.) in a mass ratio of 84 / 16 (breakdown: 20.0 g of polyamide 6 fiber, 3.8 g of polyurethane fiber), and 60.0 g of deionized water. The mass ratio of water to the composite material (X:1) was 2.5:1, and the mass ratio of water to polyamide 6 (Xa:1) was 3:1.
[0070] The reaction vessel was replaced with nitrogen, and after sealing under a nitrogen pressure of 0.5 MPa, the reaction was carried out by holding at 320°C for 15 minutes while stirring at 200 rpm. The pressure reached during the reaction was 10.5 MPa. After the reaction was completed, the reaction mixture was cooled to room temperature and collected. Since the reaction temperature Y°C is 320°C, the product of X and Y is 807, the product of Xa and Y is 960, and the residence time at the reaction temperature of 320°C is 15 minutes, the product of X, Y, and Z is 12,100, and the product of Xa, Y, and Z is 14,400.
[0071] The yield of ε-caprolactam calculated by liquid chromatography analysis of the recovered reaction mixture was 78%. Comparison with Reference Example 1 shows that even when a composite material made of polyamide 6 fiber and polyurethane-based elastic fiber is used, ε-caprolactam is obtained in a yield equivalent to that obtained when polyamide 6 alone is used.
[0072] The amount of heat required to produce 1 kg of ε-caprolactam was calculated based on the mass ratio of water to the composite material (X), reaction temperature (Y), ε-caprolactam yield, and the fixed values of the specific heat of water (4.2 kJ / kg K), specific heat of the composite material (0.6 kcal / kg K), heat of dissipation (10 kcal / kg), and heat of decomposition (29 kcal / kg), and on the assumption that 20% of the required heat amount per unit time is dissipated. The amount of heat required to produce 1 kg of ε-caprolactam was 1,646 kcal / kg-Lcm.
[0073] In addition, the energy required to produce 1 kg of ε-caprolactam was calculated to be 1,728 kcal / kg-Lcm using the mass ratio of water to the composite material (X), reaction temperature (Y), ε-caprolactam yield, and residence time (Z) and the above-mentioned fixed values.
[0074] In addition, 0.5 times the weight of cyclohexane was added to the reaction mixture recovered from the above reaction, and the mixture was heated and stirred at 70°C for 1 hour to extract hot cyclohexane-soluble components. After cooling to room temperature, the cyclohexane layer was recovered, cyclohexane was removed using an evaporator, and vacuum dried at 80°C to obtain 1.1 g of a cyclohexane extract. NMR analysis of the extracted component revealed that the extracted component was polytetramethylene glycol, a polyurethane component.
[0075] Furthermore, the aqueous layer from the hot cyclohexane extraction was subjected to distillation separation of water at a reduced pressure of 30 mmHg and a heating temperature of 55°C to obtain a concentrated aqueous solution of ε-caprolactam, which was further distilled at a reduced pressure of 5 mmHg and a heating temperature of 150 to 170°C to obtain distilled ε-caprolactam. The concentration and distillation yield was 92.7%. The HPLC impurity content of the distilled ε-caprolactam was 0.47%, and it was of a quality that could be used as a polymerization raw material for polyamide 6.
[0076] [Examples 2 to 9, Comparative Examples 1 to 4] As in Example 1, a fabric having a mass ratio of polyamide 6 fiber and polyurethane elastic fiber of 84 / 16 was used as the raw material, and depolymerization was carried out to produce ε-caprolactam in the same manner as in Example 1, while changing the amount of water relative to the fabric, the reaction temperature, and the reaction time. The reaction conditions, the ε-caprolactam yield, and the heating heat amount and energy required to produce 1 kg of ε-caprolactam are shown in Table 1.
[0077] [Table 1]
[0078] From Table 1, it is understood that by making the product of X and Y 2,000 or less, and further making the product of X, Y and Z 60,000 or less, it is possible to produce ε-caprolactam in a high yield while greatly reducing the amount of energy required for the production of ε-caprolactam.
[0079] [Example 10] A nylon fiber processed fabric was prepared by sewing 300 g of polyamide 6 fabric with 30 g of polyethylene terephthalate yarn using a sewing machine, and the resulting fabric was cut into 5 cm square pieces to obtain cutting waste.
[0080] 22.0 g of the above-mentioned shredded material (20.0 g of polyamide 6, 2.0 g of polyethylene terephthalate) and 60.0 g of deionized water were charged into a SUS316L autoclave equipped with a stirrer. The mass ratio of water to the shredded material of the composite material (X:1) was 2.7:1, and the mass ratio of water to polyamide 6 (Xa:1) was 3:1.
[0081] The reaction vessel was replaced with nitrogen, and after sealing under a nitrogen pressure of 0.5 MPa, the reaction was carried out by holding at 320°C for 15 minutes while stirring at 200 rpm. The pressure reached during the reaction was 10.5 MPa. After the reaction was completed, the reaction mixture was cooled to room temperature and collected. Since the reaction temperature Y°C is 320°C, the product of X and Y is 873, the product of Xa and Y is 960, and the residence time at the reaction temperature of 320°C is 15 minutes, the product of X, Y, and Z is 13,091, and the product of Xa, Y, and Z is 14,400.
[0082] The yield of ε-caprolactam calculated from the recovered reaction mixture by liquid chromatography analysis was 64%, and the yield of ethylene glycol calculated from the reaction mixture by gas chromatography analysis was 85%.
[0083] The amount of heat required to produce 1 kg of ε-caprolactam was calculated based on the mass ratio of water to the composite material (X), reaction temperature (Y), ε-caprolactam yield, and the fixed values of the specific heat of water (4.2 kJ / kg K), specific heat of the composite material (0.6 kcal / kg K), heat of dissipation (10 kcal / kg), and heat of decomposition (29 kcal / kg), and on the assumption that 20% of the required heat amount per unit time is dissipated. The amount of heat required to produce 1 kg of ε-caprolactam was 1,988 kcal / kg-Lcm.
[0084] In addition, the energy required to produce 1 kg of ε-caprolactam was calculated to be 2,088 kcal / kg-Lcm using the mass ratio of water to the composite material (X), reaction temperature (Y), ε-caprolactam yield, and residence time (Z) and the above-mentioned fixed values.
[0085] The reaction mixture recovered from the above reaction was subjected to distillation separation of water at a reduced pressure of 30 mmHg and a heating temperature of 55°C to obtain a concentrated aqueous solution of ε-caprolactam, which was further distilled at a reduced pressure of 5 mmHg and a heating temperature of 100 to 120°C to obtain distilled ethylene glycol. The distillation was further performed at a reduced pressure of 5 mmHg and a heating temperature of 150 to 170°C to obtain distilled ε-caprolactam. The concentration and distillation yield was 91.55%. The HPLC impurity content of the distilled ε-caprolactam was 0.46%, which was of a quality suitable for use as a raw material for polyamide 6 polymerization.
[0086] [Example 11] A SUS316L autoclave equipped with a stirrer was charged with 22.0 g of the shredded material described in Example 10 (20.0 g of polyamide 6, 2.0 g of polyethylene terephthalate), 60.0 g of deionized water, and 0.08 g of copper oxide (I). The mass ratio (X:1) of water to the shredded material of the composite material was 2.7:1, and the mass ratio Xa:1 of water to polyamide 6 was 3:1.
[0087] The reaction vessel was replaced with nitrogen, and after sealing under a nitrogen pressure of 0.5 MPa, the reaction was carried out by holding at 320°C for 15 minutes while stirring at 200 rpm. The pressure reached during the reaction was 10.5 MPa. After the reaction was completed, the reaction mixture was cooled to room temperature and collected. Since the reaction temperature Y°C is 320°C, the product of X and Y is 873, the product of Xa and Y is 960, and the residence time at the reaction temperature of 320°C is 15 minutes, the product of X, Y, and Z is 13,091, and the product of Xa, Y, and Z is 14,400.
[0088] The yield of ε-caprolactam calculated from the recovered reaction mixture by liquid chromatography analysis was 77%, and the yield of ethylene glycol calculated from the reaction mixture by gas chromatography analysis was 91%.
[0089] The amount of heat required to produce 1 kg of ε-caprolactam, calculated in the same manner as in Example 10, was 1,653 kcal / kg-Lcm, and the energy required to produce 1 kg of ε-caprolactam was 1,736 kcal / kg-Lcm.
[0090] Comparison with Example 10 shows that the presence of a copper compound when the composite material is brought into contact with water and reacted enables ε-caprolactam to be obtained more efficiently and with less energy.
[0091] [Examples 12 to 15] Using the same shredded waste as in Examples 10 and 11 as the raw material, depolymerization was carried out in the same manner as in Examples 10 and 11 by changing the amount of water relative to the shredded waste and the reaction temperature, to produce ε-caprolactam. The reaction conditions, ε-caprolactam yield, and the amount of heating heat and energy required to produce 1 kg of ε-caprolactam are shown in Table 2.
[0092] [Table 2]
[0093] It can be seen from Tables 1 and 2 that by making the product of X and Y 2,000 or less, and further by making the product of X, Y and Z 60,000 or less, it is possible to produce ε-caprolactam in a high yield while significantly reducing the amount of energy required for the production of ε-caprolactam, regardless of the composite material.
[0094] [Example 16] Polymerization of polyamide 6 10 g of ε-caprolactam, 2.16 mg of benzoic acid, and 10.0 g of ion-exchanged water were weighed into a test tube, which was recovered by the method described in Example 1. The test tube was placed in an autoclave, and the inside of the autoclave was replaced with nitrogen. The jacket temperature was set to 250°C, and heating was started. After the internal pressure reached 1.0 MPa, the internal pressure was maintained at 1.0 MPa for 3 hours. The internal pressure was then released to normal pressure over 1.5 hours, and heating was stopped when the internal temperature reached 228°C. After polymerization was completed, the polymer was recovered from the test tube and crushed. The crushed polymer was treated in 95°C hot water for 15 hours, and unreacted monomers and low polymers were extracted and removed. The extracted polymer was subjected to vacuum drying at 80°C for 24 hours to obtain polyamide 6 resin with a melting point of 226°C and ηr = 2.75.
Claims
1. A method for producing ε-caprolactam by contacting a composite material (A) composed of at least two kinds of resins, the composite material (A) containing polyamide 6 as a main component, with water (B) at a temperature of 290° C. or more and 350° C. or less, the contact is carried out under conditions where, when the mass ratio of water (B) to the composite material (A) (water (B):composite material (A)) is X:1 and the reaction temperature is Y° C., the product of X and Y is 2,000 or less.
2. The method for producing ε-caprolactam according to claim 1, wherein resin components other than polyamide 6 in the composite material (A) are also obtained as valuable materials.
3. 3. The method for producing ε-caprolactam according to claim 1, wherein the pressure when the composite material (A) is contacted with the water (B) is 7.5 MPa or more and 30 MPa or less.
4. 3. The method for producing ε-caprolactam according to claim 1, wherein a copper compound is further contained when the composite material (A) is brought into contact with the water (B).
5. The method for producing ε-caprolactam according to claim 1 or 2, wherein the contact is carried out under conditions such that the product of X, Y and Z is 60,000 or less, where the residence time at a reaction temperature of Y° C. is Z minutes.
6. The method for producing ε-caprolactam according to claim 4, wherein the copper compound is at least one selected from the group consisting of organic copper salts and inorganic copper salts.
7. The method for producing ε-caprolactam according to claim 2, wherein the valuable substance other than ε-caprolactam is glycol.
8. 3. The method for producing ε-caprolactam according to claim 1, wherein the composite material (A) contains polyamide 6 and at least one of a polyester and a polyurethane.
9. 3. A method for producing polyamide 6, comprising the steps of obtaining ε-caprolactam by the method for producing ε-caprolactam according to claim 1 or 2, and polymerizing the obtained ε-caprolactam to obtain polyamide 6.
Citation Information
Patent Citations
Urification of epsilon-caprolactam
JP1996217746A
Method for producing caprolactam by hydrocleavage of molten polycaprolactam
JP1998510280A
Method for chemically recycling nylon fibers processed with polyurethane
JP2008031127A
Recycling method for nylon 6 product
JP2008179816A