Sheet for liquid development, and method for manufacturing sheet for liquid development

The liquid spreading sheet with a polyester resin, nonionic surfactant, and conductive resin configuration addresses set-off and layer contact issues, enhancing inspection accuracy and speed while maintaining durability.

JP2024153565APending Publication Date: 2024-10-29TORAY INDUSTRIES INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024058530
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-04-01
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing POCT test sheets face issues with liquid set-off to the backside when using low-viscosity biological fluids, and hydrophilic and water-repellent layers contacting each other during rolling or lamination, affecting inspection accuracy and speed.

Method used

A liquid spreading sheet configuration with a protective base material, a liquid receiving layer containing a polyester resin with a bisphenol A structure, a nonionic surfactant, and a conductive resin, along with specific composition ratios and thermal lamination, prevents set-off and enhances liquid spreadability.

Benefits of technology

The solution provides a sheet with improved inspection accuracy, speed, quality, and durability by preventing liquid receiving layer components from transferring to the backside, ensuring excellent adhesion and liquid spreadability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153565000001_ABST
    Figure 2024153565000001_ABST
Patent Text Reader

Abstract

To provide a sheet for liquid development which exhibits excellent liquid development properties even when the sheet is wound in a roll shape or the sheets are stacked one by one.SOLUTION: A sheet for liquid development has at least a protective base material, a liquid receiving layer, a base material film, and a water-repellent layer in this order, wherein the liquid receiving layer contains a polyester resin having a bisphenol A structure, a nonionic surface active agent, and a conductive resin.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sheet for spreading a liquid and a method for producing the sheet for spreading a liquid. [Background technology]

[0002] In recent years, point-of-care testing (POCT) in clinical medicine has expanded to cover a wide range of testing items. There is a strong demand for these POCT testing devices to provide highly accurate and rapid test results. In particular, the water repellency and hydrophilicity of the test sheet play an important role in dominantly influencing the test accuracy and speed, so various attempts have been made to date.

[0003] For example, Patent Document 1 discloses a technique of using a binder and a surfactant in a liquid-receiving layer as a method for controlling the test speed, while Patent Document 2 discloses a technique of laminating a hydrophilic layer on one side of a chip substrate and a water-repellent layer on the opposite side of the hydrophilic layer as a method for compensating for the test accuracy that is an issue for POCT testing devices. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-349860 A [Patent Document 2] Japanese Patent Application Publication No. 10-246717 Summary of the Invention [Problem to be solved by the invention]

[0005] However, although the technology described in the aforementioned Patent Document 1 has excellent liquid spreadability, when a biological fluid with extremely low viscosity is spread, the liquid will seep through to the back surface, posing a problem in terms of testing accuracy.

[0006] On the other hand, in the technology described in Patent Document 2, when the chip substrate is wound into a roll or stacked sheet by sheet, the hydrophilic layer and the water-repellent layer come into contact with each other, causing the components of the water-repellent layer to be transferred to the hydrophilic layer, resulting in issues with liquid spreadability.

[0007] In order to solve such problems, the present invention aims to provide a liquid-spreading sheet that prevents the components of the liquid-receiving layer from bleeding through to the back side even when wound into a roll or stacked sheet by sheet, and that has excellent liquid-spreading properties. [Means for solving the problem]

[0008] As a result of extensive research aimed at solving the above problems, the inventors have found that the problems can be solved as follows, and have arrived at the present invention. That is, a preferred embodiment of the liquid spreading sheet of the present invention has the following configuration. (1) A liquid spreading sheet having at least a protective substrate, a liquid receiving layer, a substrate film, and a water-repellent layer in this order, the liquid receiving layer containing a polyester resin having a bisphenol A structure, a nonionic surfactant, and a conductive resin. (2) The liquid spreading sheet according to (1), wherein the content of the polyester resin is 80% by mass or more and 99.8% by mass or less, and the total content of the surfactant and the conductive resin is 0.2% by mass or more and 20% by mass or less, based on 100.0% by mass of the liquid receiving layer. (3) The liquid spreading sheet according to (2), wherein the peel strength between the protective substrate and the liquid receiving layer is 0.1 mN / 10 mm or more and 10 mN / 10 mm or less. (4) The liquid spreading sheet according to (3), wherein the thickness of the liquid receiving layer is 0.1 μm or more and 5.0 μm or less. (5) The liquid spreading sheet according to (4), wherein the protective substrate and the substrate film are both polyethylene terephthalate films. (6) The liquid spreading sheet according to (5), wherein the resin constituting the protective substrate has a crystallinity of 0.25 or more and 0.35 or less. (7) The liquid spreading sheet according to (6), wherein the thermal shrinkage rate of the protective substrate in the width direction at 180° C. is 1.0% or less. (8) The liquid spreading sheet according to (7), wherein the water-repellent layer is mainly composed of a silicone resin. (9) The liquid spreading sheet according to any one of (1) to (8), which is used as a biological fluid spreading sheet. (10) A method for producing a liquid spreading sheet according to any one of (1) to (8), comprising a step of applying a coating composition containing the polyester resin, the surfactant and the conductive resin onto the substrate film to form a liquid receiving film, and then thermally laminating the protective substrate and the liquid receiving layer at a temperature of 40°C or higher and 100°C or lower. Effect of the Invention

[0009] According to the present invention, it is possible to provide a liquid spreading sheet which is excellent in liquid spreading properties and in which the components of the liquid receiving layer are prevented from being transferred to the back side even when the sheet is wound into a roll or laminated in sheets. As a result, the test sheet using the liquid spreading sheet of the present invention is excellent in test accuracy, test speed, quality, and durability. In other words, the test sheet using the liquid spreading sheet of the present invention enables inexpensive, rapid and accurate testing. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view of a liquid spreading sheet according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The liquid spreading sheet of the present invention has at least a protective substrate, a liquid receiving layer, a substrate film, and a water-repellent layer in this order, and the liquid receiving layer contains a polyester resin having a bisphenol A structure, a nonionic surfactant, and a conductive resin. By adopting such an embodiment, the liquid spreading sheet of the present invention is excellent in liquid spreading properties, and the components of the liquid receiving layer are prevented from being transferred to the back side even when the liquid spreading sheet of the present invention is wound into a roll or laminated in sheets. And, the inspection sheet using the liquid spreading sheet of the present invention is excellent in inspection accuracy, inspection speed, productivity, quality, and durability. The liquid spreading sheet of the present invention will be specifically described below.

[0012] In addition, since the productivity of the liquid development sheet is excellent, the productivity of the test sheet using this liquid development sheet is also excellent. In addition, since the quality of the liquid development sheet is excellent, the quality of the test sheet using this liquid development sheet is also excellent. In addition, since the durability of the liquid development sheet is excellent, the durability of the test sheet using this liquid development sheet is also excellent.

[0013] 1 is a schematic cross-sectional view of a liquid spreading sheet according to one embodiment of the present invention, which comprises a protective substrate 1, a liquid receiving layer 2, a substrate film 3, and a water-repellent layer 4 in this order.

[0014] (Liquid Receptive Layer) The liquid receiving layer of the liquid spreading sheet of the present invention contains a polyester resin having a bisphenol A structure, a nonionic surfactant, and a conductive resin. By adopting such a form, the liquid spreading sheet has excellent productivity and durability, and an inspection sheet using this liquid spreading sheet has excellent inspection accuracy, inspection speed, productivity, and durability.

[0015] The polyester resin having a bisphenol A structure refers to a polyester resin obtained by copolymerizing a glycol component having a bisphenol A structure with a dibasic acid component. By adopting such a form, the adhesion between the liquid receiving layer containing the polyester resin having a bisphenol A structure and the base film and the protective base material is improved. By improving the adhesion between the liquid receiving layer and the base film, the liquid receiving layer is prevented from peeling off from the base film when used as a liquid spreading sheet, so that the liquid spreading sheet has excellent durability. In addition, by improving the adhesion between the liquid receiving layer and the protective base material, the handling of the protective base material becomes easy when wound into a roll or laminated in sheets, so that the liquid spreading sheet has excellent productivity. In addition, since bisphenol A has a high affinity with a nonionic surfactant and can control the bleeding out of the nonionic surfactant to the protective base material side, the inspection sheet using this liquid spreading sheet has excellent inspection accuracy.

[0016] Examples of glycol components having a bisphenol A structure include hydrogenated bisphenol A, ethylene oxide adducts and propylene oxide adducts of bisphenol A, ethylene oxide adducts and propylene oxide adducts of hydrogenated bisphenol A, and the like.

[0017] Examples of the dibasic acid component include aromatic dibasic acids such as orthophthalic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 2,2'-diphenyldicarboxylic acid, and 4,4'-diphenyletherdicarboxylic acid, and aliphatic or alicyclic dibasic acids such as adipic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, and 4-methyl-1,2-cyclohexanedicarboxylic acid.

[0018] The glass transition temperature of the polyester resin having a bisphenol A structure of the present invention is preferably 40°C or more and 100°C or less from the viewpoint of further improving the adhesion to the base film and the adhesion to the protective substrate. By having a glass transition temperature of 100°C or less, the adhesion to the base film and the adhesion to the protective substrate are sufficient, and the liquid spreading sheet has excellent productivity. From the same viewpoint, it is more preferable to set the glass transition temperature to 90°C or less. In addition, by having a glass transition temperature of 40°C or more of the polyester resin having a bisphenol A structure, the hardness of the liquid receiving layer in the temperature range used as the liquid spreading sheet is improved, and the liquid spreading sheet has excellent durability. From the same viewpoint, it is more preferable to set the glass transition temperature of the polyester resin having a bisphenol A structure to 60°C or more. From the above viewpoint, it is more preferable to set the glass transition temperature to 60°C or more and 100°C or less.

[0019] The polyester resin having a bisphenol A structure of the present invention is preferably solvent-soluble, which means that the polyester resin is soluble in at least 3% by mass at 25° C. in one or more of toluene, methyl ethyl ketone, cyclohexanone, tetrahydrofuran, and ethyl acetate alone or in a mixed solvent of any two or more of these solvents in any mixing ratio.

[0020] The content of the polyester resin having a bisphenol A structure is 80.0% by mass or more in 100.0% by mass of the liquid receiving layer, and the adhesion to the base film and the adhesion to the protective base material are improved, and the surface hardness of the liquid receiving layer is improved, so that the liquid spreading sheet has excellent productivity and durability. From the same viewpoint, it is more preferable to contain 85.0% by mass or more, and even more preferable to contain 90.0% by mass or more. In addition, by making the content of the polyester resin having a bisphenol A structure 99.8% by mass or less, the content ratio of the nonionic surfactant and the conductive resin described later in the liquid receiving layer can be increased, so that the inspection sheet using the liquid spreading sheet can be excellent in inspection accuracy and inspection speed. From the same viewpoint, it is more preferable to contain 99.0% by mass or less, and even more preferable to contain 97.0% by mass or less.

[0021] From the above viewpoints, the polyester resin having a bisphenol A structure in the present invention is preferably contained in an amount of 80.0 mass% or more and 99.8 mass% or less, more preferably 85.0 mass% or more and 99.0 mass% or less, and even more preferably 90.0 mass% or more and 97.0 mass% or less, of 100.0 mass% of the liquid receiving layer.

[0022] The nonionic surfactant used in the present invention refers to a substance that, when it is added alone to pure water at 5 mass %, can reduce the surface tension of the pure water by 30% or more. From the viewpoint of improving the wettability of the liquid-receiving layer and improving the adhesion to the protective substrate, the liquid-receiving layer contains a nonionic surfactant, and an acetylene glycol-based surfactant or an ethylene oxide adduct surfactant of an acetylene glycol is more preferable.

[0023] By making the content of the nonionic surfactant 0.1% by mass or more, the wettability of the liquid receiving layer can be improved, so that the inspection sheet using the liquid spreading sheet has excellent inspection speed. From the same viewpoint, it is more preferable to contain 1.0% by mass or more, and even more preferable to contain 3.0% by mass or more.

[0024] In addition, by making the content of the nonionic surfactant 19.9% ​​by mass or less, when an electrode is formed on the liquid spreading sheet, the nonionic surfactant is prevented from bleeding onto the electrode, which causes poor sensitivity in the test, and the test sheet using this liquid spreading sheet has excellent test accuracy. In addition, since the adhesion to the protective substrate is improved as a liquid spreading sheet, the productivity as a liquid spreading sheet is excellent. From the same viewpoint, it is more preferable to contain 15.0% by mass or less, and even more preferable to contain 10.0% by mass or less.

[0025] From the above viewpoints, the nonionic surfactant in the present invention is preferably contained in an amount of 0.1% by mass or more and 19.9% ​​by mass or less, more preferably 1.0% by mass or more and 15.0% by mass or less, and even more preferably 3.0% by mass or more and 10.0% by mass or less, based on 100.0% by mass of the liquid receiving layer.

[0026] From the viewpoint of improving the wettability of the liquid-receiving layer, the molecular weight of the nonionic surfactant is preferably 1,000 or less.

[0027] The conductive resin of the present invention is a resin having a volume resistivity of 1 × 10 Ω m or less by itself, and from the viewpoint of the antistatic effect, i.e., reducing the surface resistance value, is preferably a cationic conductive resin, more preferably a quaternary ammonium salt polymer, and further preferably polyvinylbenzyltrimethylammonium chloride and / or polydiallyldimethylammonium chloride.

[0028] By making the content of the conductive resin 0.1% by mass or more, the surface resistance value of the liquid receiving layer is lowered, and thus the antistatic effect is further obtained, so that the adhesion of foreign matter when forming electrodes on the liquid spreading sheet is suppressed, and the liquid spreading sheet has excellent productivity. From the same viewpoint, the content of 1.0% by mass or more is more preferable, and the content of 3.0% by mass or more is even more preferable.

[0029] Furthermore, by making the total content of the conductive resin 19.9% ​​by mass or less, it is possible to prevent poor sensitivity of the test due to short circuiting or the like when electrodes are formed on the liquid spreading sheet, and when the liquid spreading sheet is used as a test sheet, the test sheet has excellent test accuracy. From the same viewpoint, it is more preferable to contain 15.0% by mass or less, and even more preferable to contain 10.0% by mass or less. The weight average molecular weight of the conductive resin is preferably 5000 or more.

[0030] From the above viewpoints, the conductive resin in the present invention is preferably contained in an amount of 0.1% by mass or more and 19.9% ​​by mass or less, more preferably 1.0% by mass or more and 15.0% by mass or less, and even more preferably 3.0% by mass or more and 10.0% by mass or less, based on 100.0% by mass of Layer A. Furthermore, by adopting such a form, the surface resistance value of the liquid-receiving layer can be made 1×108 Ω or more and 1×1010 Ω or less.

[0031] From the above viewpoints, it is preferable that the content of the polyester resin is 80% by mass or more and 99.8% by mass or less, and further, the total content of the surfactant and the conductive resin is 0.2% by mass or more and 20% by mass or less, based on 100.0% by mass of the liquid receiving layer.

[0032] In the present invention, the surface resistance of the liquid receiving layer is preferably 1×108 Ω or more and 1×1010 Ω or less. By making the surface resistance 1×108 Ω or more, it is possible to prevent poor sensitivity of the test due to short circuiting when electrodes are formed on the liquid developing sheet, and the test sheet using this liquid developing sheet has excellent test accuracy. From the same viewpoint, it is more preferable to make it 5×108 Ω or more, and even more preferable to make it 7×108 Ω or more.

[0033] In addition, by making the surface resistance value 1×1010Ω or less, an antistatic effect is obtained, which suppresses the adhesion of foreign matter when forming electrodes on the liquid spreading sheet, resulting in a liquid spreading sheet with excellent quality. From the same viewpoint, it is more preferable to make it 7×109Ω or less, and even more preferable to make it 5×109Ω or less. The surface resistance value is determined by the method described in the examples.

[0034] The thickness of the liquid receiving layer of the present invention is preferably 0.1 μm or more and 5.0 μm or less from the viewpoint of making the productivity of the liquid spreading sheet excellent and furthermore, making the inspection sheet using this liquid spreading sheet excellent in inspection accuracy. By making the thickness of the liquid receiving layer 0.1 μm or more, it is possible to prevent the liquid receiving layer from slipping off due to scratches during processing of the liquid spreading sheet and the occurrence of pinholes, so that the liquid spreading sheet has excellent quality and furthermore, the inspection sheet using this liquid spreading sheet has excellent inspection accuracy. From the same viewpoint, it is more preferable to make it 0.5 μm or more.

[0035] Furthermore, by making the thickness of the liquid receiving layer 5.0 μm or less, workability can be improved and blocking can be prevented when the liquid is wound into a roll, resulting in a liquid spreading sheet with excellent productivity. From the same viewpoint, it is more preferable to make the thickness 3.0 μm or less.

[0036] When the composition of the polyester resin having a bisphenol A structure, the nonionic surfactant, and the conductive resin in the liquid-receiving layer of the present invention cannot be determined from the blending of the raw materials, the following LC / MS / MS (liquid chromatography mass spectrometry) and pyrolysis GC / MS can be preferably used as qualitative and quantitative analysis methods.

[0037] <Separation / Extraction> Weigh 0.04 g of the layer into a 25 mL measuring flask. Next, add 1 mL of HFIP (1,1,1,1,3,3,3-hexafluoro-2-propanol) / chloroform (volume ratio 1 / 1) to the measuring flask to dissolve the layer, add 2 mL of chloroform, and then gradually add acetonitrile to insolubilize the polyester resin component.

[0038] Add acetonitrile and adjust the volume to 25 mL. Dilute the adjusted solution 100-fold with acetonitrile, filter it through a PTFE disk filter (0.45 μm), and use the filtrate as the measurement solution.

[0039] <Qualitative analysis> The measurement solution is subjected to LC / MS / MS, and the retention time and peak area at which the peaks derived from the nonionic surfactant and the conductive resin are detected from the chromatogram are confirmed. Then, the peaks derived from the nonionic surfactant and the conductive resin are qualitatively analyzed by mass spectrometry. The formula weights of the positive and negative ions derived from the nonionic surfactant are confirmed to qualitatively analyze the nonionic surfactant.

[0040] The insolubilized polyester resin is subjected to pyrolysis GC / MS, and a qualitative analysis is performed by mass spectrometry on a peak derived from the polyester resin having a bisphenol A structure.

[0041] <Adjusting standard solutions and creating calibration curves> Weigh out 0.01 g of the qualified nonionic surfactant and conductive resin samples into a 10 mL measuring flask, dissolve them in methanol, and make the volume to 10 mL to make a standard solution. Aliquot the standard solution and dilute each with methanol to obtain a total of four standard solutions of arbitrary concentrations, which are then subjected to LC / MS / MS to confirm the peak area of ​​the chromatogram for each concentration. A calibration curve is obtained by linearly approximating the relationship between the solution concentration and the peak area.

[0042] <Quantitative analysis> The peak areas at which the peaks originating from the nonionic surfactant and the conductive resin are detected from the chromatogram confirmed by the qualitative analysis are substituted into the equation for the calibration curve, and the concentrations of the surfactant and the conductive resin contained in the layer are calculated to obtain the contents of the polyester resin having a bisphenol A structure, the nonionic surfactant, and the conductive resin.

[0043] The above LC / MS / MS analysis can be performed using LC20-A (LC system, manufactured by Shimadzu Corporation), API4000 (MS system, manufactured by AB SCIEX Corporation), and ODS-3 (manufactured by GL Sciences Inc., column, "Intersil" (registered trademark)) under the following conditions: APCI (atmospheric pressure chemical ionization) ionization method, positive ion detection and negative ion detection, SRM (selected reAction monitoring) measurement mode, column temperature of 50°C, flow rate of 0.25 mL / min, and injection volume of 1 μL.

[0044] In addition, pyrolysis GC / MS can be performed using a PY3030D (Frontier Labs, Inc.) and a GCMS-QP2010 (Shimadzu Corporation) at a heating temperature of 500°C and a heating rate of 50°C / min.

[0045] (Base film) From the viewpoint of dimensional stability and durability, the base film in the liquid spreading sheet of the present invention is preferably a film made of polyester, such as polyethylene terephthalate, polyethylene 2,6-naphthalate, polyethylene α,β-bis(2-chlorophenoxy)ethane 4,4'-dicarboxylate, polybutylene terephthalate, etc. These may be copolymers. Among these, a film made of polyethylene terephthalate, i.e., a polyethylene terephthalate film, is particularly preferred from the viewpoint of excellent handling properties and durability of the liquid spreading sheet, and from the same viewpoint, a biaxially stretched polyethylene terephthalate film is most preferred.

[0046] The thickness of the base film is preferably 10 μm or more from the viewpoint of excellent dimensional stability and durability. From the same viewpoint, it is more preferable to set it to 20 μm or more, and even more preferable to set it to 30 μm or more. Moreover, the thickness of the base film is preferably 500 μm or less from the viewpoint of excellent handleability as an inspection sheet. From the same viewpoint, it is more preferable to set it to 300 μm or less, and even more preferable to set it to 200 μm or less.

[0047] From the above viewpoints, the thickness of the base film is preferably from 10 μm to 500 μm, more preferably from 20 μm to 300 μm, and even more preferably from 30 μm to 200 μm.

[0048] (protective base material) With conventional liquid spreading sheets, when the sheet is rolled up, the liquid receiving layer and the water-repellent layer come into contact with each other, causing the silicone resin in the water-repellent layer to be transferred to the liquid receiving layer. As a result, there was an issue that the testing speed was slow when using conventional liquid spreading sheets.

[0049] In contrast, the liquid spreading sheet of the present invention is formed by applying a coating composition containing a polyester resin having a bisphenol A structure, a nonionic surfactant, and a conductive resin onto a substrate film to form a liquid receiving film, and then heat laminating the protective substrate and the liquid receiving layer at 40 ° C. or more and 100 ° C. or less, and setting the peel strength between the protective substrate and the liquid receiving layer to 0.1 mN / 10 mm or more and 10 mN / 10 mm or less, so that the liquid spreading sheet does not impair productivity, and since it has a protective substrate, a liquid receiving layer, a substrate film, and a water-repellent layer in this order, the silicone resin of the water-repellent layer is prevented from being transferred to the liquid receiving layer, and the inspection sheet using this liquid spreading sheet has excellent inspection accuracy and inspection speed. From the above viewpoint, it is preferable that the peel strength between the protective substrate and the liquid receiving layer is 0.1 mN / 10 mm or more and 10 mN / 10 mm or less.

[0050] By setting the heating temperature for thermally laminating the protective substrate and the liquid receiving layer at 40°C or higher, the peel strength between the protective substrate and the liquid receiving layer becomes 0.1 mN / 10 mm or higher, and the sheet transport after thermal lamination and the winding property into a roll are improved, resulting in a liquid spreading sheet with excellent productivity. From the same viewpoint, it is preferable to set the heating temperature at 45°C or higher, and more preferably at 50°C or higher.

[0051] In addition, by setting the heating temperature for thermally laminating the protective substrate and the liquid receiving layer at 100° C. or less, wrinkles due to thermal shrinkage of the protective substrate during the lamination process can be reduced, resulting in a liquid spreading sheet of excellent quality. By adopting such a configuration, the peel strength between the protective substrate and the liquid receiving layer can be set to 10 mN / 10 mm or less.

[0052] From the viewpoint of dimensional stability and durability, the protective substrate in the liquid spreading sheet of the present invention is preferably a film made of polyester, such as polyethylene terephthalate, polyethylene 2,6-naphthalate, polyethylene α,β-bis(2-chlorophenoxy)ethane 4,4'-dicarboxylate, polybutylene terephthalate, etc. These may be copolymers. Among these, a film made of polyethylene terephthalate, i.e., a polyethylene terephthalate film, is particularly preferred from the viewpoint of excellent processability of the liquid spreading sheet, and from the same viewpoint, a biaxially stretched polyethylene terephthalate film is most preferred.

[0053] The thickness of the protective substrate is preferably 5 μm or more from the viewpoint of excellent dimensional stability and durability, and efficient heating of the liquid receiving layer during thermal lamination. From the same viewpoint, it is more preferable to set it to 8 μm or more, and even more preferable to set it to 10 μm or more. In addition, the thickness of the substrate film is preferably 100 μm or less from the viewpoint of excellent handleability as an inspection sheet. From the same viewpoint, it is more preferable to set it to 50 μm or less, and even more preferable to set it to 38 μm or less.

[0054] The crystallinity of the resin constituting the protective substrate is preferably 0.25 or more from the viewpoint of suppressing the thermal shrinkage of the protective substrate during thermal lamination, improving the thermal dimensional stability of the liquid spreading sheet, and providing excellent winding properties as a liquid spreading sheet. By increasing the heat setting temperature in the manufacturing process of the polyethylene terephthalate film or by performing heat treatment after manufacturing, the crystal growth of the resin constituting the protective substrate is promoted, so the crystallinity can be increased, and the crystallinity of the resin can be 0.25 or more. From the same viewpoint, it is more preferable to set it to 0.27 or more. In addition, the crystallinity of the resin constituting the protective substrate is preferably 0.35 or less from the viewpoint of suppressing the thermal expansion of the protective substrate during thermal lamination, improving the thermal dimensional stability of the liquid spreading sheet, and providing excellent winding properties as a liquid spreading sheet. From the same viewpoint, it is more preferable to set it to 0.33 or less. By lowering the heat setting temperature in the manufacturing process of the polyethylene terephthalate film, the crystal growth of the resin constituting the protective substrate is suppressed, so the crystallinity can be set to 0.35 or less.

[0055] The thermal shrinkage rate of the protective substrate in the width direction at 180°C is preferably 1.0% or less from the viewpoint of suppressing the occurrence of curls, wrinkles, etc. of the protective substrate during thermal lamination and providing excellent winding properties as a liquid spreading sheet. From the same viewpoint, the thermal shrinkage rate of the protective substrate in the width direction at 180°C is more preferably 0.5% or less. By increasing the heat setting temperature in the manufacturing process of the polyethylene terephthalate film or by subjecting the film to heat treatment after manufacturing, crystal growth of the resin constituting the protective substrate is promoted, and the thermal expansion rate at 180°C can be made 1.0% or less.

[0056] From the above viewpoints, the thickness of the protective substrate is preferably 5 μm or more and 100 μm or less, more preferably 8 μm or more and 50 μm or less, and even more preferably 10 μm or more and 38 μm or less.

[0057] In view of the improved processability of the liquid spreading sheet, it is preferred that both the protective substrate and the substrate film in the liquid spreading sheet of the present invention are polyethylene terephthalate films.

[0058] (Water-repellent layer) The water-repellent layer in the liquid spreading sheet of the present invention is preferably composed mainly of silicone resin. By using silicone resin as the main component, when a liquid is dropped onto the liquid receiving layer side of the liquid spreading sheet, the liquid spreads in the liquid receiving layer, but the liquid is prevented from spreading along the surface of the liquid spreading sheet to the water-repellent layer side, and when the liquid spreading sheet is used as an inspection sheet, the inspection sheet has excellent inspection accuracy. The water-repellent layer being composed mainly of silicone resin means that the content of silicone resin in the water-repellent layer is 80% by mass or more.

[0059] The silicone resin is preferably selected from the group consisting of addition reaction type silicone resin, condensation polymerization type silicone resin, ultraviolet curing type silicone resin, electron beam curing type silicone resin, and solventless type silicone resin, from the viewpoint that the water repellency of the water repellent layer is improved, the wettability of the liquid as a liquid spreading sheet is controlled, and when the liquid spreading sheet is used as an inspection sheet, the inspection sheet has excellent inspection accuracy. From the same viewpoint, it is more preferable to use an addition reaction type silicone resin, and it is even more preferable to use an addition polymerization type silicone resin of polydimethylsiloxane containing a terminal vinyl group and hydrogensiloxane. By adopting such a form, the surface free energy of the water repellent layer can be made 30 mN / m or less. When the surface free energy of the water repellent layer is 30 mN / m or less, good water repellency is obtained, so that the components of the liquid receiving layer are suppressed from being transferred to the back side, and the inspection accuracy of the inspection sheet using the liquid spreading sheet of the present invention is improved.

[0060] By making the thickness of the water-repellent layer 0.02 μm or more, good water-repellency can be obtained and thickness variation can be suppressed, so that when used as a liquid spreading sheet, the quality of the liquid spreading sheet is excellent, and further, the inspection accuracy of the inspection sheet using this liquid spreading sheet is also excellent. From the same viewpoint, it is more preferable to make it 0.05 μm or more. Furthermore, by making the thickness of the water-repellent layer 0.5 μm or less, it is possible to maintain the drying performance and suppress the migration of the silicone resin, so that when the liquid spreading sheet is used as an inspection sheet, this inspection sheet has excellent inspection accuracy. From the same viewpoint, it is more preferable to make it 0.3 μm or less.

[0061] From the above viewpoints, the thickness of the water-repellent layer is preferably 0.02 μm or more and 0.5 μm or less, and more preferably 0.05 μm or more and 0.3 μm or less.

[0062] In addition, from the viewpoint of improving the adhesion between the water-repellent layer and the base film, an anchor layer made of one or more cured compounds selected from the group consisting of γ-methacryloxy group-containing organoalkoxysilanes, epoxy group-containing organoalkoxysilanes, vinyl group-containing organoalkoxysilanes, and vinyl group-containing acetoxysilanes may be provided between the water-repellent layer and the base film.

[0063] (Liquid spreading sheet) The liquid spreading sheet of the present invention has at least a protective substrate, a liquid receiving layer, a substrate film, and a water-repellent layer in this order, and when this liquid spreading sheet is used as a test sheet, this test sheet is excellent in test accuracy, test speed, productivity, and durability. As a result, it can be suitably used as a liquid spreading sheet for testing and quantifying specific components contained in biological samples such as blood and urine, raw materials and products in the food industry, samples such as fruit juice, etc.

[0064] The method for producing the liquid spreading sheet of the present invention can include, for example, the following exemplary materials, amounts used, treatment contents, treatment procedures, etc.

[0065] The liquid spreading sheet of the present invention can be produced, for example, by applying a coating composition for a water-repellent layer to one side of a substrate film, and then performing a heat treatment to obtain a substrate film laminated with a water-repellent layer, and then applying a paint composition containing a polyester resin having a bisphenol A structure, a nonionic surfactant, and a conductive resin to the back side of the water-repellent layer of the substrate film, and performing a heat treatment to form a liquid-receiving layer, and then performing a thermal lamination process on the protective substrate and the liquid-receiving layer at a temperature of 40°C or higher and 100°C or lower.

[0066] In obtaining a coating composition containing a polyester resin having a bisphenol A structure, a nonionic surfactant, and a conductive resin for obtaining a liquid receiving layer, there is no particular limitation on the method of mixing and dispersing each component, and known mixing and dispersing methods such as a magnetic stirrer, a homodisper, ultrasonic irradiation, vibration dispersion, and manual mixing and dispersion can be used. In addition, the coating composition preferably contains an organic solvent from the viewpoint of improving the coatability to the substrate film. Examples of organic solvents include ethyl methyl ketone, methyl isobutyl ketone, butyl acetate, ethyl acetate, methanol, isopropanol, cyclohexanone, toluene, and xylene. In addition, inorganic particles, organic particles, leveling agents, etc. can be blended into the coating composition from the viewpoint of preventing blocking when wound up on a film roll and improving the coatability to the substrate film, as long as the effect of the present invention is not impaired. The coating composition for the water-repellent layer can also be obtained by the same method.

[0067] Preferred methods for laminating the liquid receiving layer and the water repellent layer onto the base film include, for example, the comma coating method, the applicator method, the dip coating method, the roller coating method, the wire bar coating method, the reverse coating method, the kiss coating method, the gravure coating method, and the die coating method (see U.S. Pat. No. 2,681,294), and from the viewpoint of processability, the wire bar coating method, the reverse coating method, and the gravure coating method are more preferred.

[0068] The liquid spreading sheet of the present invention can be suitably used as a biological fluid spreading sheet, where biological fluid means blood, urine, etc. EXAMPLES

[0069] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0070] [Measurement and evaluation methods] (1) Thickness of the liquid-receiving layer The thickness (μm) of the liquid receiving layer was determined by cutting the liquid spreading sheet perpendicular to the thickness using a manual rotary microtome (Leica Microsystems, "HistoCore BIOCUT" (registered trademark) R) to obtain a cross-section of the liquid spreading sheet, and observing the cross-section of the conductive layer using a scanning electron microscope (FEI, XL30 SFEG) at an accelerating voltage of 20 kV and an observation magnification of 100,000 times, and measuring any five points on the cross-sectional photograph to calculate the average value obtained.

[0071] (2) Peel strength between protective substrate and liquid-receiving layer (N / 10 mm) The liquid spreading sheet wound into a roll was cut into 10mm wide x 150mm wide rectangles at 10%, 50%, and 90% of the total length of the film, and the protective substrate and the liquid receiving layer were forcibly peeled off. A 180° peel test was performed using a tensile tester (Orientec Tensilon UCT-100) with an initial tensile chuck distance of 100mm and a tensile speed of 20mm / min. The measurement was continued until the peel length reached 130mm (chuck distance 230mm), and the average load value from 25mm to 125mm of peel length was taken as the peel strength.

[0072] (3) Adhesion between the liquid-receiving layer and the base film The liquid spreading sheet wound into a roll was cut into 100 mm x 100 mm squares at three randomly selected locations, and the adhesion between the liquid receiving layer and the base film was evaluated using a cross-cut guide CCJ-1 (manufactured by Cortex Co., Ltd.) based on JIS K5600-5-6 (1999) and the following criteria, with a score of C or above being considered a pass. A: Classification 0 B: Classification 1 C: Classification 2 D: Classification 3, Classification 4, Classification 5 (4) Liquid spreading property of the liquid receiving layer The liquid spreading sheet wound into a roll was cut into 100mm x 100mm squares at three points, 10%, 50%, and 90% of the total length of the film, to prepare measurement samples. 5μl of glucose injection solution (Otsuka Sugar Solution 50% manufactured by Otsuka Pharmaceutical Co., Ltd.) was dropped onto the surface of the liquid receiving layer of the measurement sample, and the spread of the glucose injection solution was measured 30 seconds after dropping. The spread was measured by measuring the diameter of the liquid, and if the liquid was elliptical, the short diameter was considered to be the diameter. The average value of the three points was calculated, and if the spread of the glucose injection solution was 5mm or more, it was considered to have passed. However, if the spread was 5mm or more but the glucose injection solution flowed to the back side of the liquid receiving layer, it was marked as N and failed.

[0073] (5) Surface resistance of the liquid-receiving layer The liquid spreading sheet was wound into a roll and cut into 100 mm x 100 mm squares at three points on the surface of the roll to prepare test pieces. The surface resistance of the liquid receiving layer surface of the test pieces was measured using a resistivity meter (Hi-rester UX MCP-HT800, manufactured by Nitto Seiko Analytech Co., Ltd.) and the average value of the three points was calculated.

[0074] (6) Surface appearance of the liquid-receiving layer The liquid spreading sheet wound into a roll was cut into 100 mm x 100 mm square pieces at three points on the surface of the roll to prepare test pieces, and the condition of the liquid spreading sheet was observed. The sheet was then evaluated according to the following criteria, with a grade of B or higher being deemed to be acceptable. A: In all three locations, no sliding off of the liquid-receiving layer due to scratches or the like and no pinholes were visually observed. B: Slippage of the liquid-receiving layer due to scratches or pinholes were visually observed in one or two places. C: In all three locations, sliding of the liquid-receiving layer due to scratches or the like and pinholes were visually observed.

[0075] (7) Surface free energy of water-repellent layer The liquid spreading sheet wound into a roll was cut into 100 mm x 100 mm squares at three randomly selected locations, and the squares were conditioned for 24 hours at a room temperature of 23°C and a relative humidity of 65% to prepare measurement samples. The static contact angles of the water-repellent layer of the measurement sample were measured using a contact angle meter (DMs-401, manufactured by Kyowa Interface Science Co., Ltd.) for three types of measurement liquid: water, ethylene glycol, and methylene iodide. Next, the dispersion term, polarity term, and hydrogen bond term of the surface free energy of each liquid described in J. Panzer: J. Colloid Interface Sci., 44, 142 (1973) were introduced into the "Extended Hawks Equation of Hata and Kitazaki" described in Yasuaki Kitazaki and Toshio Hata: Japan Adhesion Association Paper, 8, (3) 131 (1972), and the surface free energy of the water-repellent layer was calculated by solving the simultaneous equations using surface free energy analysis add-in software (FAMAS made by Kyowa Interface Science Co., Ltd.), and the average value of three points was calculated. Then, evaluation was performed according to the following criteria, and C or higher was considered to be a pass. A: Less than 20mN / m B: 20mN / m or more and 25mN / m or less C: 25mN / m or more and 30mN / m or less D: Exceeding 30mN / m (8) Roll-up ability of liquid spreading sheet The condition of the liquid spreading sheet wound into a roll during production was observed and evaluated according to the following criteria, with a score of B or higher being deemed acceptable. A: No wrinkles, dents, convex deformations, or misalignment were visually observed on the roll of the liquid spreading sheet. B: Wrinkles, dents, convex deformations, and misalignment of the wound liquid spreading sheet were visually observed to a degree that did not cause any practical problems in the roll. C: Wrinkles, dents, convex deformations, and misalignment of the roll that are problematic for practical use were visually observed on the roll of the liquid spreading sheet.

[0076] (9) Crystallinity of the resin constituting the protective substrate A test piece was prepared by cutting out 5 mg of the protective substrate from the liquid spreading sheet wound into a roll, and the temperature was raised from 25°C to 300°C at a heating rate of 20°C / min using a differential scanning calorimeter (Seiko Instruments Inc. DSC, RDC220) and a data analyzer (Seiko Instruments Inc. Disk Station, SSC / 5200) in accordance with JIS K7121 (1987). The heat of the peak of the endothermic peak of melting observed at that time was used to calculate the degree of crystallization from the following formula using the heat of crystal fusion (ΔHm) and the heat of cold crystallization (ΔHc). Crystallinity = (ΔHm-ΔHc) / ΔHm0 Here, ΔHm0 (heat of fusion of perfectly crystalline PET) was set to 140.10 J / g.

[0077] (10) Thermal shrinkage rate of protective substrate in the width direction at 180°C Only the protective substrate was removed from the liquid spreading sheet wound into a roll, and test pieces of 150 mm in the width direction and 10 mm in the machine direction were cut out from 5 randomly selected locations on the protective substrate to prepare test pieces. These were heat-treated at 180°C for 30 minutes, and the heat shrinkage rate at 180°C was calculated from the dimensional change before and after the heat treatment, and the average value of the 5 locations was calculated. This average value was taken as the heat shrinkage rate. [Materials] (Polyester Resin A) Polyester resin with bisphenol A structure ("Pesresin" (registered trademark) S140 manufactured by Takamatsu Oil Co., Ltd.) (Polyester resin B) Polyester resin without bisphenol A structure ("Nichigo Polyester" (registered trademark) TP-235 manufactured by Mitsubishi Chemical Corporation) (Surfactant A) Ethylene oxide adduct surfactant of acetylene glycol ("Olfine" (registered trademark) E1004, manufactured by Nissin Chemical Industry Co., Ltd.) (Surfactant B) Alkyltrimethylammonium salt surfactant ("Katinal" (registered trademark) LTC-35A, manufactured by Toho Chemical Industry Co., Ltd.) (Conductive resin) Quaternary ammonium salt polymer ("Anstex" (registered trademark) C-200X, manufactured by Toho Chemical Industry Co., Ltd.) (Silicone resin) Addition reaction type silicone resin (Dow Toray Industries, Inc. "DOWSIL" (registered trademark) LTC750A) (Platinum catalyst) Dow Toray Industries, Inc. "DOWSIL" (registered trademark) SRX212 Catalyst (Acrylic resin) Acrylic resin (8BS-900 manufactured by Taisei Fine Chemical Co., Ltd.) (Base film A) Polyethylene terephthalate film (Toray Industries, Inc.'s "Lumirror" (registered trademark) S10, thickness 75 μm) (Base film B) Polybutylene terephthalate film (ESRM manufactured by Okura Kogyo Co., Ltd., thickness 75 μm) (Protective base material A) Polyethylene terephthalate film (Toray Industries, Inc.'s "Lumirror" (registered trademark) S10, thickness 12 μm) (Protective base material B) Polyethylene terephthalate film (Toyobo "Ester" (registered trademark) ET510, thickness 12 μm) (Protective base material C) Polyethylene terephthalate film (Toray Industries, Inc.'s "Lumirror" (registered trademark) S56, thickness 12 μm) that was heat-treated at 220°C for 10 seconds [Example 1] The raw materials for obtaining the liquid-receiving layer and the water-repellent layer were made to have the compositions shown in Table 1, and each was dissolved in ethyl methyl ketone, and the raw materials were mixed and dispersed using a Homodisper (manufactured by Primix Corporation) to obtain a 10% by mass adjusted solution. Next, the adjusted solution for obtaining the water-repellent layer was applied by gravure coating to one side of a 75 μm-thick substrate film (biaxially oriented polyethylene terephthalate film "Lumirror" (registered trademark) S10 manufactured by Toray Industries, Inc.), and dried at 120° C. to obtain a water-repellent layer laminate film having a thickness of 0.2 μm, which was then wound into a roll. Next, a preparation solution for obtaining a liquid-receiving layer was applied by gravure coating to the back side of the water-repellent layer of the obtained water-repellent layer laminate film, and after drying at 120°C, a liquid-receiving layer having a thickness of 1.0 μm was laminated. Furthermore, a protective substrate A having a thickness of 12 μm (biaxially oriented polyethylene terephthalate film "Lumirror" (registered trademark) S10 manufactured by Toray Industries, Inc.) was thermally laminated at 50°C to the liquid-receiving layer to obtain a liquid-spreading sheet, which was then wound into a roll.

[0078] [Examples 2 to 19, Comparative Examples 1 to 3] The compositions of each layer, excluding the solvent, the base film, and the protective base were as shown in Tables 1 to 5, and liquid spreading sheets were produced in the same manner as in Example 1, except that the formation of the protective base was omitted in Comparative Example 1. The evaluation results are shown in Tables 1 and 2.

[0079] All of the liquid spreading sheets of Examples 1 to 19 had excellent liquid spreading properties in the liquid receiving layer, and furthermore, since the surface free energy of the water-repellent layer was low, the inspection sheets using the above liquid spreading sheets had excellent inspection accuracy; since the liquid spreading properties of the liquid receiving layer was high, the inspection sheets using the above liquid spreading sheets had excellent inspection speed; furthermore, since at least one of the crystallinity of the resin constituting the protective substrate and the thermal shrinkage rate at 180°C in the width direction of the protective substrate was suitable, the thermal dimensional stability of the liquid spreading sheets was good and the winding up ability was excellent, so the inspection sheets using the above liquid spreading sheets had excellent quality; and since the adhesion between the liquid receiving layer and the base film was excellent, the above liquid spreading sheets had excellent durability.

[0080] On the other hand, the liquid spreading sheet of Comparative Example 1 was inferior to the liquid spreading sheets of the Examples in terms of the liquid spreading properties of the liquid receiving layer and the surface free energy of the water-repellent layer, and the test sheet using the liquid spreading sheet of Comparative Example 1 was inferior in liquid spreading properties and test accuracy.

[0081] Furthermore, the liquid spreading sheet of Comparative Example 2 was inferior to the liquid spreading sheets of the Examples in terms of adhesion between the liquid receiving layer and the base film and in terms of roll-up properties, and the liquid spreading sheet of Comparative Example 2 was inferior in durability and quality.

[0082] Furthermore, the liquid spreading sheet of Comparative Example 3 was inferior to the liquid spreading sheets of the Examples in terms of adhesion between the liquid receiving layer and the base film and in terms of roll-up properties, and the liquid spreading sheet of Comparative Example 3 was inferior in durability and quality.

[0083] [Table 1]

[0084] [Table 2]

[0085] [Table 3]

[0086] [Table 4]

[0087] [Table 5] [Explanation of symbols]

[0088] 1: Protective base material 2: Liquid receiving layer 3: Base film 4: Water-repellent layer [Industrial Applicability]

[0089] The liquid spreading sheet of the present invention is preferably used when testing and quantifying liquids, for example, biological fluid components such as blood and urine, and can be suitably used as a biological fluid spreading sheet.

Claims

1. A liquid spreading sheet comprising at least a protective substrate, a liquid receiving layer, a substrate film, and a water-repellent layer in this order, the liquid receiving layer containing a polyester resin having a bisphenol A structure, a nonionic surfactant, and a conductive resin.

2. 2. The liquid spreading sheet according to claim 1, wherein the content of the polyester resin is 80% by mass or more and 99.8% by mass or less, and the total content of the surfactant and the conductive resin is 0.2% by mass or more and 20% by mass or less, relative to 100.0% by mass of the liquid receiving layer.

3. 3. The liquid spreading sheet according to claim 2, wherein a peel strength between the protective substrate and the liquid receiving layer is 0.1 mN / 10 mm or more and 10 mN / 10 mm or less.

4. 4. The liquid spreading sheet according to claim 3, wherein the thickness of the liquid receiving layer is from 0.1 μm to 5.0 μm.

5. 5. The liquid spreading sheet according to claim 4, wherein the protective substrate and the substrate film are both polyethylene terephthalate films.

6. 6. The liquid spreading sheet according to claim 5, wherein the resin constituting the protective substrate has a crystallinity of 0.25 or more and 0.35 or less.

7. 7. The liquid spreading sheet according to claim 6, wherein the thermal shrinkage rate of the protective substrate in the width direction at 180°C is 1.0% or less.

8. 8. The liquid spreading sheet according to claim 7, wherein the water-repellent layer is mainly composed of a silicone resin.

9. 9. The liquid spreading sheet according to claim 1, which is used as a biological fluid spreading sheet.

10. 9. The method for producing a liquid spreading sheet according to any one of claims 1 to 8, comprising a step of applying a coating composition containing the polyester resin, the surfactant and the conductive resin onto the substrate film to form a liquid receiving film, and then thermally laminating the protective substrate and the liquid receiving layer at a temperature of 40°C or higher and 100°C or lower.

Citation Information

Patent Citations

  • Small biosensor and its manufacture