Solid hybrid electrolyte, producing method thereof, and use thereof

The solid hybrid electrolyte with a polymeric layer on inorganic fibers or strands addresses interfacial resistance and dendrite issues, enhancing the performance and safety of lithium metal batteries.

JP2024153777AInactive Publication Date: 2024-10-29UNIV OF MARYLAND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024121911
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2017-03-29
Filing Date
2024-07-29
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Current lithium-ion batteries face challenges such as high interfacial resistance between solid electrolytes and electrodes, leading to increased overvoltage, reduced Coulombic efficiency, and safety concerns due to metal dendrite formation and chemical/physical shorting, which limits their energy density and cycling performance.

Method used

A solid hybrid electrolyte is developed with a polymeric material layer on the surface of a solid electrolyte, forming a continuous ionic conduction path through a 3D network of inorganic fibers or strands, reducing interfacial resistance and preventing dendrite penetration.

Benefits of technology

The hybrid electrolyte design achieves low interfacial resistance, enhances mechanical stability, and prevents dendrite formation, resulting in stable and safe lithium metal batteries with improved energy density and cycling performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153777000001_ABST
    Figure 2024153777000001_ABST
Patent Text Reader

Abstract

To provide a solid hybrid electrolyte having desirable ion conductivity and a solid hybrid electrolyte provided with a non-limiting layer such as a polymer layer (for example, a polymer film) realizing a stably and excellently connected interface between such electrolyte and an electrode.SOLUTION: A solid hybrid electrolyte has a layer of a polymer material that may be a polymer / copolymer layer or a gel polymer / copolymer layer, disposed on at least part or all of the outer surface of the solid electrolyte (SSE), and forms an interface with an electrode of an ion conductive battery exhibiting desirable characteristics. The SSEs include monolithic SSE bodies, mesoporous SSE bodies, inorganic SSEs having fibers or strands, and in the case of solid electrolytes having strands, strands can be formed using a sacrificial template, and the solid hybrid electrolyte can be used for ionic conductive batteries that may be flexible ionic conductive batteries.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Patent Application No. 62 / 478,396, filed March 29, 2017, and U.S. Provisional Patent Application No. 62 / 483,816, filed April 10, 2017, the disclosures of each of which are incorporated herein by reference.

[0002] STATEMENT REGARDING FEDERALLY FUNDED RESEARCH This invention was made with Government support under Contract Nos. DEEE0006860 and DEEE0006860 awarded by the Department of Energy. The Government has certain rights in this invention.

[0003] The present disclosure relates generally to solid hybrid electrolytes and, more particularly, to solid hybrid electrolytes for use in ion-conducting batteries. [Background technology]

[0004] Over the past few decades, lithium-ion battery technology has made significant advances. Pure lithium metal has the highest specific capacity (3860 mAh / g) and lowest electrochemical potential (-3.04 V vs. standard hydrogen electrode) compared to any other lithium-ion anode material. A key challenge associated with lithium metal anodes is the formation of metal dendrites in liquid electrolyte systems that can penetrate the polymer separator and lead to both safety concerns and performance degradation in long-term cycling applications. Solid-state electrolytes (SSEs) have been identified as a solution to prevent the formation of Li dendrites by acting as a strong impenetrable barrier.

[0005] SSEs generally have a wide electrochemical stability potential window, a high rigidity that prevents penetration of Li dendrites, and are usually non-flammable, improving safety. A major challenge for SSEs in Li metal batteries is the high interfacial resistance between the SSE and the cathode or anode. High interfacial resistance leads to large overpotentials and reduced coulombic efficiency during cell cycling.

[0006] Chemical / physical short circuit and volume change of electrodes are the other two major challenges in lithium batteries. In conventional batteries, polymer separators cannot effectively prevent both chemical and physical short circuit. Dissolved active materials inevitably migrate through the pores of the polymer membrane, and highly elastic Li dendrites easily penetrate the membrane, resulting in poor performance and safety concerns. Volume change during lithiation and delithiation raises other concerns, such as desorption of active materials at the interface and structural instability of the whole cell. In the case of sulfur cathodes, the formation of lithium polysulfides and their migration across the liquid organic electrolyte is another major constraint in realizing high energy density batteries. Although there has been extensive research to prevent short circuit and accommodate volume change by developing cathode hosts, improving separators, or protecting Li metal, there are few methods that can simultaneously address these challenges.

[0007] Liquid organic electrolytes are the industry standard ionic conductors for lithium-ion batteries (LIBs). Liquid electrolytes are characterized by high ionic conductivity and good wettability with the electrodes. However, liquid systems are flammable, inevitably cause dissolution and diffusion of active materials, and migration of unwanted species from the cathode to the anode creates "chemical short circuits" that degrade the electrodes and limit the development of new cathode properties, which are typical for high-voltage cathodes, sulfur, and air / O2. In high-voltage LIBs, LiNi 0.5 Mn 1.4 O4(LNMO) Dissolution of transition metals in spinel cathodes and their diffusion to the respective anode surfaces results in continuous electrolyte decomposition leading to rapid capacity fade and Li +In LIBs, as well as in Li metal batteries, diffusion of active materials is more dominant. For example, in Li-S batteries, diffusion of polysulfides corrodes the Li metal anode, and repeated shuttling of polysulfides between the electrodes leads to reduced coulombic efficiency and loss of active materials. Similarly, short-circuit shuttles by mobile redox mediators in Li-air / O2 batteries should be avoided. Therefore, it is important to prevent chemical short-circuits in terms of minimizing or preventing the migration of such soluble components through the battery.

[0008] There is an urgent need for innovative approaches to develop new battery technologies that have higher energy density and at the same time are less prone to catastrophic failure. Solid electrolytes are key to providing high energy density while addressing the challenges of chemical and physical short circuits, as well as flammability and safety issues, by preventing unwanted active material migration and penetration of metal dendrites.

[0009] In the past decades, many prominent solid-state electrolyte materials have been developed for solid-state batteries, including conductive oxides, phosphates, hydrides, halides, sulfides, and polymer-based composites. Solid-state Li-ion conductors have been demonstrated for incorporation into batteries across a broad range of materials ensembles, including 0D nanoparticles, 1D nanofibers, 2D thin films, 3D networks, and bulk components. Among these, the concept of a 3D Li-ion conducting framework represents a creative solution to the deficiencies in the capacity and cycling kinetics of current solid-state batteries, providing continuous Li-ion transport pathways and adequate mechanical reinforcement.

[0010] A strategy to address Li dendrite penetration and SEI formation is the development of solid-state electrolytes (SSEs) that mechanically suppress Li dendrites and essentially eliminate SEI formation. Among the various types of solid electrolytes (inorganic oxides / non-oxides and Li-salt-containing polymers), solid polymer electrolytes have been most extensively studied. In PEO-based composites, powders are incorporated into the host PEO polymer matrix to improve the ionic conductivity of the Li salt / polymer system by influencing the recrystallization kinetics of the PEO polymer chains and promoting local amorphous regions. The addition of powders also improves the electrochemical stability and mechanical strength. The development of nanostructured fillers is one approach to enhance the ionic conductivity of polymer composite electrolytes by increasing the surface area of ​​the amorphous regions and improving the interface between the filler and the polymer. One-dimensional nanowire fillers have been demonstrated to enhance the ionic conductivity of polymer composite electrolytes. This is because nanowire fillers provide extended ion migration paths in the polymer matrix, as opposed to the isolated dispersion of nanoparticle fillers in polymer electrolytes. However, some residual ceramic filler agglomeration may remain, which poses a challenge in large-scale preparation of uniform solid polymer electrolytes by blending with polymers. To address this issue, in situ synthesis of highly monodispersed ceramic filler particles in polymer electrolytes has been reported in recent years. The reported solid polymer electrolyte, which was synthesized in situ from nanosized SiO2 particles in a PEO / Li salt polymer, had a molecular weight of 4.4 × 10 at 30 °C. -5 Although they have demonstrated ionic conductivities of 100 S / cm at room temperature, further improvements are needed to achieve higher ionic conductivities. Therefore, based on our understanding, there is a large unmet need for fabricating continuous SSE networks with interconnected long-range ionic transport in composite hybrid electrolytes. Summary of the Invention [Means for solving the problem]

[0011] The present disclosure provides a solid hybrid electrolyte. The present disclosure also provides methods for making the solid hybrid electrolyte and uses thereof.

[0012] In one aspect, the present disclosure provides a solid hybrid electrolyte. The solid hybrid electrolyte has a layer of a polymeric material disposed on at least a portion or all of an outer surface of a solid electrolyte (SSE). In various examples, the solid hybrid electrolyte is a polymeric material / solid hybrid electrolyte, a polymer / solid hybrid electrolyte, or a gel polymer / solid hybrid electrolyte. In various examples, the SSE is a monolithic or mesoporous SSE body or an SSE including multiple fibers or multiple strands.

[0013] In one aspect, the present disclosure provides methods of making inorganic fibers or strands. The fibers or strands can form inorganic SSEs. In various examples, these methods are templating or electrospinning methods.

[0014] The strands can be formed by a templating method. The template comprises interconnected voids that can be used to form strands of inorganic material that can form inorganic solid electrolytes (e.g., solid hybrid electrolytes). The voids can be engineered or occur naturally in biological materials (e.g., wood, plants, etc.).

[0015] In one aspect, the present disclosure provides the use of the solid hybrid electrolyte of the present disclosure. The solid hybrid electrolyte can be used in various devices. In various examples, the device comprises one or more solid hybrid electrolytes of the present disclosure. Examples of devices include, but are not limited to, electrolytic cells, electrolytic cells, fuel cells, batteries, and other electrochemical devices (e.g., sensors, etc.).

[0016] The device may be a battery. The battery may be an ionically conductive battery. The battery may be configured for applications such as portable applications, transportation applications, stationary energy storage applications, etc. Examples of ionically conductive batteries include, but are not limited to, lithium ion conductive batteries, sodium ion conductive batteries, magnesium ion conductive batteries, etc.

[0017] For a better understanding of the operation and objects of the present disclosure, reference should be made to the following detailed description taken in conjunction with the accompanying drawings. [Brief description of the drawings]

[0018] [Figure 1] Schematic diagram of solid gel polymer battery designs (a) with hybrid polymer / garnet-type SSE electrolyte and (b) without interfacial gel polymer layer and poor interfacial contact between the garnet SSE and the electrodes (gel polymer layer can improve the contact between the electrodes and the SSE). [Diagram 2] FIG. 14 shows impedance analysis of symmetric cells with hybrid electrolyte: (a) EIS of LiFePO4 cathode|polymer|SSE|polymer|cathode symmetric cell, (b) EIS of SS|polymer|SSE|polymer|SS symmetric cell, (c) EIS of cathode|polymer|SSE|polymer|cathode symmetric cell, (d) EIS plot of Li|polymer|Li symmetric cell, (e) EIS plot of Li|polymer|SSE|polymer|Li symmetric cell, (f) comparison of SSE|electrode interface resistance with and without gel polymer interface. [Diagram 3] FIG. 13 shows the impedance of the electrode|SSE|electrode symmetric cell component with and without a gel polymer interfacial layer. [Figure 4]FIG. 2 shows electrochemical performance of polymer|SSE|polymer hybrid electrolyte for symmetric completed cells: (a) voltage profile of Li stripping and plating in Li|polymer|SSE|polymer|Li symmetric cell at constant current over 15 h; (b) EIS plots of the cell before and after cycling; (c) charge-discharge voltage profile of cathode|SSE|Li cell with gel polymer interfacial layer; (d) discharge capacity and coulombic efficiency of the cell over 130 cycles; (e) EIS of the cell before cycling, after 20 cycles, and after 130 cycles. [Diagram 5] FIG. 13 shows the impedance of electrode|SSE|electrode symmetric cells without a gel polymer interface: (a) EIS of cathode|SSE|cathode symmetric cell, (b) EIS of Li|SSE|Li symmetric cell. [Figure 6] FIG. 1 shows a comparison between conventional batteries and solid hybrid electrolytes, focusing on the bilayer solid electrolyte matrix. [Figure 7] Characterization of bilayer garnet solid electrolyte. Schematic diagram of the 3D structure of the bilayer garnet structure, including (a) a photographic image of the bilayer garnet SSE, (b) a top-view SEM image of the porous layer (scale bar is 200 μm), (c) a magnified view of the porous layer (scale bar is 50 μm), (d) an SEM of the connection between the porous layer and the dense layer (scale bar is 10 μm), (e) a magnified SEM image of the granular dense microstructure (the dense structure can block the soluble active material and suppress the penetration of Li dendrites. Scale bar is 10 μm), and (f) a cross-section of the bilayer garnet structure (the two distinct layers of the porous and dense garnet structures can be clearly observed (the dense layer is about 35 μm and the porous layer is 70 μm)). [Figure 8-1]Chemical stability of garnet SSEs in polysulfide solutions, liquid electrolytes, and molten sulfur. (a) (b) S 2p XPS spectra of dense garnet pellets before and after Ar sputtering onto their surfaces (the dense garnet pellets were fully immersed in polysulfide solutions (Li2S8 in DME / DOL) for one week prior to XPS analysis). (c) Zr 3d XPS spectra of dense garnet pellets before and after Ar sputtering onto their surfaces. XPS spectra, (d)(e) XRD patterns and Raman spectra of garnet powder after immersion in liquid electrolyte (LiTFSI in DME / DOL) and polysulfide solution for 1 week (samples were sealed in Kapton bags to avoid oxygen and moisture contamination), (f) TEM image of garnet nanopowder after immersion in polysulfide solution for 1 week, (g) XRD pattern of garnet powder after immersion in molten sulfur at 160 °C for 1 week, (h) calculation of mutual reaction energy ΔED,mutual for garnet, Li2S, and Li2S8. [Figure 8-2] Chemical stability of garnet SSEs in polysulfide solutions, liquid electrolytes, and molten sulfur. (a) (b) S 2p XPS spectra of dense garnet pellets before and after Ar sputtering onto their surfaces (the dense garnet pellets were fully immersed in polysulfide solutions (Li2S8 in DME / DOL) for one week prior to XPS analysis). (c) Zr 3d XPS spectra of dense garnet pellets before and after Ar sputtering onto their surfaces. XPS spectra, (d)(e) XRD patterns and Raman spectra of garnet powder after immersion in liquid electrolyte (LiTFSI in DME / DOL) and polysulfide solution for 1 week (samples were sealed in Kapton bags to avoid oxygen and moisture contamination), (f) TEM image of garnet nanopowder after immersion in polysulfide solution for 1 week, (g) XRD pattern of garnet powder after immersion in molten sulfur at 160 °C for 1 week, (h) calculation of mutual reaction energy ΔED,mutual for garnet, Li2S, and Li2S8. [Figure 9-1]Electrochemical characterization of the liquid-solid hybrid electrolyte: (a)(b) schematic and SEM images of the exposed dense garnet layer surface; (c)(d) schematic and SEM of the polymer-coated dense garnet layer surface; (e) EIS of the symmetric cell with polymer coating; (f) voltage profile of Li plating / stripping cycles at a current density of 0.3 mA / cm2 (red line is the Li / garnet / Li morphology prepared by attaching molten Li directly to the garnet dense layer. Li / garnet / Li shows a high impedance, high voltage curve. The black line is from the symmetric hybrid electrolyte cell. The inset shows the detailed voltage plateaus of Li stripping / plating in the first hours and at 140 hours); (g)(h) voltage profiles of Li plating / stripping cycles at current densities of 0.5 and 1.0 mA / cm2. [Figure 9-2] Electrochemical characterization of the liquid-solid hybrid electrolyte: (a)(b) schematic and SEM images of the exposed dense garnet layer surface; (c)(d) schematic and SEM of the polymer-coated dense garnet layer surface; (e) EIS of the symmetric cell with polymer coating; (f) voltage profile of Li plating / stripping cycles at a current density of 0.3 mA / cm2 (red line is the Li / garnet / Li morphology prepared by attaching molten Li directly to the garnet dense layer. Li / garnet / Li shows a high impedance, high voltage curve. The black line is from the symmetric hybrid electrolyte cell. The inset shows the detailed voltage plateaus of Li stripping / plating in the first hours and at 140 hours); (g)(h) voltage profiles of Li plating / stripping cycles at current densities of 0.5 and 1.0 mA / cm2. [Figure 10-1]Electrochemical characterization of solid-state hybrid Li-S batteries, including (a) schematic diagrams of conventional Li-S and solid-state hybrid Li-S batteries (in conventional Li-S, the polymer porous membrane is unable to block polysulfides or prevent Li dendrite penetration. In solid-state hybrid Li-S batteries, the ceramic dense membrane not only physically blocks the liquid electrolyte and polysulfides, but also suppresses the growth of Li dendrites toward the cathode side); (b) voltage profiles of conventional and hybrid Li-S cells (the extended plateau of charging indicates the shuttle effect of polysulfides in conventional Li-S, whereas the shuttle effect does not occur in hybrid Li-S cells); (c) the voltage profiles of conventional and hybrid Li-S cells at high current density (Fig. 1c). (d) Voltage profile of the hybrid Li-S cell (a dense garnet film and a slurry-cast sulfur electrode with mass loading of about 1.2 mg / cm2 were assembled into a hybrid cell); (d) Rate performance of the hybrid Li-S cell; (e) Schematic of the solid-state hybrid bilayer Li-S battery (sulfur and CNTs were encapsulated in the pores. The mechanically stable bilayer garnet structure can accommodate the volume expansion of sulfur and maintain a stable electrode structure during cycling); (f) Cross-section of the bilayer sulfur cathode (elemental mapping shows the sulfur distribution inside the porous layer); (g)(h) Voltage profile and cycle performance of the hybrid bilayer Li-S cell with 7.5 mg / cm2 loading at 0.2 mA / cm2. [Figure 10-2]Electrochemical characterization of solid-state hybrid Li-S batteries, including (a) schematic diagrams of conventional Li-S and solid-state hybrid Li-S batteries (in conventional Li-S, the polymer porous membrane is unable to block polysulfides or prevent Li dendrite penetration. In solid-state hybrid Li-S batteries, the ceramic dense membrane not only physically blocks the liquid electrolyte and polysulfides, but also suppresses the growth of Li dendrites toward the cathode side); (b) voltage profiles of conventional and hybrid Li-S cells (the extended plateau of charging indicates the shuttle effect of polysulfides in conventional Li-S, whereas the shuttle effect does not occur in hybrid Li-S cells); (c) the voltage profiles of conventional and hybrid Li-S cells at high current density (Fig. 1c). (d) Voltage profile of the hybrid Li-S cell (a dense garnet film and a slurry-cast sulfur electrode with mass loading of about 1.2 mg / cm2 were assembled into a hybrid cell); (d) Rate performance of the hybrid Li-S cell; (e) Schematic of the solid-state hybrid bilayer Li-S battery (sulfur and CNTs were encapsulated in the pores. The mechanically stable bilayer garnet structure can accommodate the volume expansion of sulfur and maintain a stable electrode structure during cycling); (f) Cross-section of the bilayer sulfur cathode (elemental mapping shows the sulfur distribution inside the porous layer); (g)(h) Voltage profile and cycle performance of the hybrid bilayer Li-S cell with 7.5 mg / cm2 loading at 0.2 mA / cm2. [Figure 11] FIG. 1 shows Nyquist plots of high density garnet SSE pellets at different temperatures (25, 30, 40, and 50° C.) (the thickness of the high density garnet pellet is about 250 μm). [Figure 12] FIG. 1 shows an Arrhenius plot of the conductivity of garnet SSE (activation energy is 0.35 eV). [Figure 13]FIG. 1 shows (a) the voltage profile of a conventional Li-S battery (sulfur mass loading is about 1.2 mg / cm2), with a long charging plateau, indicating the shuttle effect of polysulfides; (b) the cycling performance of the conventional Li-S cell (the cell degrades at a high rate after 10 cycles); and (c) the low coulombic efficiency of the conventional Li-S cell. [Figure 14] FIG. 2 shows the cycle performance of solid-state hybrid Li-S battery at a current of 0.1 mA / cm2 (sulfur loading was 1.2 mg / cm2, and the hybrid cell achieved a high capacity of over 1000 mAh / g). [Figure 15] FIG. 14 shows SEM micrographs of the CNT-coated garnet porous structure (CNTs were deposited on the garnet surface to provide an electronic conducting network for the sulfur active material. Scale bars in (a) and (b) are 10 μm and 500 nm). [Figure 16] FIG. 1 shows the calculation of the specific energy density of the tested garnet bilayer Li-S cells. [Figure 17] FIG. 13 shows the estimated energy density of a bilayer garnet solid-state Li-S battery with optimized parameters. [Figure 18] Schematic of multiscale aligned mesoporous garnet Li6.4La3Zr2Al0.2O12 (LLZO) membrane with polymer electrolyte incorporated in a lithium symmetric cell (garnet wood has a multiscale aligned mesostructure derived from natural wood, eliminating the blockage of Li ion transport through the garnet and polymer electrolyte along the garnet-polymer interface). [Figure 19] Characterization of wood templates: preparation of wood templates by compression and slicing; (b) top-down SEM image of original wood; (c) top-down SEM image of compressed wood (diameter of wood microchannels is apparently smaller after compression); cross-sectional SEM images comparing (d) original wood and (e) compressed wood (channels are closed but highly aligned structure is maintained); (f) SEM image of aligned nanofibers with diameters around 10 nm. [Figure 20]FIG. 2 shows the firing of wood-templated aligned garnets: (a) cross-sectional SEM image showing channel alignment at both the microscale and (b) nanoscale; (c) photograph of flexible garnet wood consisting of aligned mesoporous garnets and PEO-based polymer electrolyte; (d) XRD pattern of aligned garnets, which matches JCPDS#90-0457 and confirms the cubic garnet structure. [Figure 21] TEM characterization of the garnet crystal structure: (a) HRTEM image of nanoparticles separated from aligned garnet showing (21 0) and (021) lattice planes (inset shows FFT pattern of HRTEM image); (b) TEM image of the edge of a garnet nanoparticle showing a clear polycrystalline structure; (c) EELS spectrum of the garnet surface showing the ROI, spectral image, and relative composition map of O, C, and La, respectively. [Figure 22-1] Electrochemical characterization of garnet wood with aligned mesoporous structure: (a) SEM and its corresponding EDX images showing complete and uniform infiltration of polymer electrolyte throughout the aligned garnet (scale bar is 100 μm); (b) Nyquist plot showing the decrease in impedance of garnet-wood film with increasing temperature (inset schematic shows structure of test cell); (c) comparison of ionic conductivity between garnet wood and PE-based polymer electrolyte at different temperatures (blue area indicates measurements performed within room temperature (RT) range); (d) schematic of lithium symmetric cell with garnet wood showing low tortuosity and fast lithium transport pathways; (e) galvanostatic cycling of Li / garnet wood / Li at current density of 0.1 mA / cm2 at room temperature. [Figure 22-2]Electrochemical characterization of garnet wood with aligned mesoporous structure: (a) SEM and its corresponding EDX images showing complete and uniform infiltration of polymer electrolyte throughout the aligned garnet (scale bar is 100 μm); (b) Nyquist plot showing the decrease in impedance of garnet-wood film with increasing temperature (inset schematic shows structure of test cell); (c) comparison of ionic conductivity between garnet wood and PE-based polymer electrolyte at different temperatures (blue area indicates measurements performed within room temperature (RT) range); (d) schematic of lithium symmetric cell with garnet wood showing low tortuosity and fast lithium transport pathways; (e) galvanostatic cycling of Li / garnet wood / Li at current density of 0.1 mA / cm2 at room temperature. [Diagram 23] FIG. 1 is a photograph of a portion of sintered aligned mesoporous garnet (the garnet film was white and flat with an area similar to that of the wood template). [Figure 24] FIG. 2 is a cross-sectional SEM image of garnet wood. (The thickness of the garnet wood can be controlled by the thickness of the wood template. The SEM image shows a thin garnet wood sample, approximately 30 μm thick, with low-torque channels that are highly aligned and penetrate the entire garnet film.) [Diagram 25] FIG. 2 is a cross-sectional SEM image of the aligned garnet structure. (The SEM image shows a portion of a 18 μm thick garnet wood sample. The sample was sintered from a template that had been thinned by slicing and grinding.) [Figure 26] 1 is a cross-sectional SEM image of garnet wood (the SEM image shows the cross section and top surface of the garnet wood. The ordered structures are completely filled with PEO-based polymer electrolyte). [Figure 27] FIG. 13 shows the weight change of the wood template upon precursor infiltration (the wood template was immersed in the precursor solution and the weight increased with time. The weight change indicates the high absorbency of the wood template). [Figure 28]Figure 1 shows (a) EIS measurements and (b) ionic conductivity of PEO / SCN / Li-TFSI polymer electrolyte at different temperatures. (The highlighted areas show the measurements performed around room temperature (RT). The inset shows that the PEO / LiTFSI / SCN polymer electrolyte membrane was sandwiched between two stainless steel electrodes. A polyethylene (PE) separator ring was placed around the polymer electrode membrane to fix the thickness at high temperatures and to avoid short circuits.) [Figure 29] Galvanostatic cycling of Li / garnet wood / Li at a current density of 0.1 mA / cm2 at room temperature for over 600 hours (the voltage variations are due to the change in ambient temperature of the cell. The extended cycling indicates the outstanding electrochemical and mechanical stability of the garnet wood composite electrolyte in the Li metal cell). [Diagram 30] Flexible lithium-ion conducting ceramic fibers were flexible and maintained the physical properties of the original template. The unique fiber structure allows for long-distance lithium-ion transport pathways through continuous fibers and yarns, high surface area / volume ratio of solid ion conductors, and multi-level porosity distribution. [Figure 31-1] Characterization of garnet fibers: (a) SEM image of pretreated fiber template, (b) SEM image of precursor solution-impregnated template, (c) SEM image of garnet fiber converted from precursor solution-impregnated template, (d) reconstructed model of flat uniformity of garnet fiber generated by 3D laser scanning, (e) flexibility, processability, and solvent resistance of garnet fiber, (f) powder XRD patterns of milled garnet fibers sintered at different temperatures, (g) elemental distribution mapping of a single garnet fiber sintered at 800°C. [Figure 31-2]Characterization of garnet fibers: (a) SEM image of pretreated fiber template, (b) SEM image of precursor solution-impregnated template, (c) SEM image of garnet fiber converted from precursor solution-impregnated template, (d) reconstructed model of flat uniformity of garnet fiber generated by 3D laser scanning, (e) flexibility, processability, and solvent resistance of garnet fiber, (f) powder XRD patterns of milled garnet fibers sintered at different temperatures, (g) elemental distribution mapping of a single garnet fiber sintered at 800°C. [Figure 32-1] Electrochemical characterization of the flexible composite polymer electrolyte reinforced with garnet fibers: (a) dried CPE exhibiting flexibility and mechanical strength; (b) fibrous garnet dominated lithium ion transport mechanism; (c) impedance spectra of the CPE at different temperatures; (d) Arrhenius plot of lithium ion conductivity of the CPE as a function of temperature; (e) galvanostatic cycling measurements of a Li / CPE / Li symmetric cell at various current densities and at 60°C. [Figure 32-2] Electrochemical characterization of the flexible composite polymer electrolyte reinforced with garnet fibers: (a) dried CPE exhibiting flexibility and mechanical strength; (b) fibrous garnet dominated lithium ion transport mechanism; (c) impedance spectra of the CPE at different temperatures; (d) Arrhenius plot of lithium ion conductivity of the CPE as a function of temperature; (e) galvanostatic cycling measurements of a Li / CPE / Li symmetric cell at various current densities and at 60°C. [Diagram 33] Characterization of garnet fiber 3D electrode configuration for solid-state Li-S batteries with sulfur loading of 10.8 mg / cm2: (a) photograph of garnet fiber sintered on dense supporting electrolyte; (b) SEM image of sulfur cathode infiltrated garnet fiber electrode configuration; (c) EDX elemental mapping of a single garnet fiber loaded with sulfur / carbon mixture; (d) charge-discharge profile of solid-state lithium-sulfur battery. [Diagram 34]FIG. 13 shows characterization of flexible garnet fibers: (a) thermogravimetric analysis of garnet precursor solution-impregnated fiber template; (b) cross-sectional SEM image of pre-treated fiber template; (c) cross-sectional SEM image of precursor solution-impregnated fiber template; (d) cross-sectional SEM image of garnet fiber after pyrolysis of the template and high temperature sintering. [Diagram 35] FIG. 1 shows flexible garnet fibers of large size and different shapes. [Diagram 36] Characterization of Li-ion conducting garnet and insulating Al2O3 fiber reinforced flexible CPEs: (a) cross-sectional SEM image of garnet fiber reinforced flexible CPE, (b) insulating Al2O3 fiber fabricated using the same templating method, (c) impedance plots of control CPE at different temperatures. [Figure 37] Electrochemical characterization of garnet fiber reinforced flexible CPE: (a) impedance plots of Li / CPE / Li symmetric cell before and after 500 h cycling at 60 °C; (b) room temperature galvanostatic cycling results of Li / CPE / Li symmetric cell at 0.05 mA / cm2; (c) galvanostatic cycling results of Li / CPE / Li symmetric cell at 1 mA / cm2 and 60 °C. [Figure 38] Characterization of sulfur-infiltrated 3D electrodes constructed with garnet fiber configuration for solid-state Li-S batteries: (a) EDX elemental linear scan along the direction from exposed yarn area to dense electrolyte surface of 3D sulfur cathode constructed with garnet fiber; (b) high magnification cross-sectional SEM image and elemental mapping of 3D sulfur cathode constructed with garnet fiber. [Figure 39]Characterization of garnet electrolyte supports fabricated by tape casting and high temperature lamination and chemical compatibility of garnet electrolyte with polysulfide catholyte and liquid electrolyte. (a) Cross-sectional SEM image of 500 μm thick dense garnet electrolyte support; (b) XRD pattern of milled garnet electrolyte; (c) Lithium ion conductivity of dense garnet electrolyte in the temperature range of 25°C to 100°C; (d) Photograph of new garnet electrolyte support polished in a glove box; (e) Photograph of garnet electrolyte soaked in polysulfide catholyte and liquid electrolyte for 300 h; (f) Photograph of garnet electrolyte subsequently washed with DME / DOL solvent (no obvious discoloration was observed); (g) XRD pattern of garnet electrolyte before and after soaking experiment (no chemical change was observed). [Diagram 40] FIG. 14 shows the discharge and charge profiles of a solid-state Li-S battery constructed in garnet fiber configuration with sulfur loading of 10.8 mg / cm2 at 0.75 mA / cm2. [Diagram 41] FIG. 14 shows the discharge and charge profiles of a solid-state Li-S battery constructed with garnet fiber configuration with high sulfur loading of 18.6 mg / cm2 at 0.15 mA / cm2. [Diagram 42] Figure 14. Relative weight and energy density of solid-state Li-S battery with sulfur loading of 18.6 mg / cm2 for different electrolyte support structural configurations: (a) relative weight distribution of garnet, cathode, anode, and current collector in solid-state Li-S battery and corresponding energy density; (1) 500 μm thick electrolyte support and 63% electrolyte area utilization; (2) 100 μm thick electrolyte support and 100% electrolyte area utilization; (3) bilayer support structure consisting of thin dense electrolyte (20 μm) and porous substrate (70 μm) and 100% electrolyte area utilization; (b) representative SEM images of low weight bilayer support structure. [Diagram 43] FIG. 1 is a diagram showing the densities of the constituent materials of a solid-state Li-S battery. [Diagram 44] FIG. 13 shows structural parameters of different electrolyte support configurations. [Diagram 45] FIG. 13 shows the parameters of the cathode components. [Figure 46] FIG. 13 shows parameters of the anode components. [Figure 47] Schematic of the solid hybrid composite electrolyte (ceramic garnet nanofibers act as reinforcement and lithium ion conducting polymer acts as the matrix. The interconnected garnet nanofiber network provides continuous ion conducting pathways in the electrolyte membrane). [Figure 48] FIG. 14: Fabrication of flexible solid fiber reinforced composite (FRPC) electrolyte: (a) schematic setup of electrospun garnet / PVP nanofibers, (b) schematic procedure for fabricating FRPC Li-ion conducting membrane, (c) SEM image of spun nanofiber network, (d) diameter distribution of spun nanofibers, (e) SEM image of garnet nanofiber network, (f) diameter distribution of garnet nanofibers, (g) photographic image showing flexible and bendable FRPC Li-ion conducting membrane. [Figure 49] Morphological characterization of garnet nanofiber reinforcement and solid FRPC electrolyte: (a) SEM image showing interconnected garnet nanofibers, (b) TEM image of polycrystalline garnet nanofibers (inset is a magnified image of garnet nanofibers with an average particle size of 20 nm in diameter), (c) high-resolution TEM image of individual garnet nanofibers, (d) SEM image of the FRPC electrolyte membrane surface, (e) cross-sectional SEM image of the membrane, (f) magnified SEM image of the cross-sectional morphology (the vacant space of the garnet 3D porous structure is filled with polymer). [Figure 50] Figure 11. Thermal properties and flammability tests of solid FRPC electrolyte: (a) TGA curves of spun nanofibers, (b) TGA curves of Li-salt / PEO polymer and FRPC electrolyte membrane, (c) flammability test of Li-salt / PEO polymer mixed with garnet nanoparticles, (d) flammability test of FRPC electrolyte membrane. [Figure 51]Phase structure of garnet fibers and electrical properties of solid FRPC electrolyte: (a) XRD pattern of garnet nanoparticles, (b) EIS profile of FRPC electrolyte membrane at different temperatures (25°C, 40°C, and 90°C), (c) Arrhenius plot of FRPC electrolyte membrane at high temperature (recorded from 20°C to 90°C and every 10°C increment), (d) LSV curve of FRPC electrolyte membrane showing electrochemical stability window in the range of 0 to 6 V. [Figure 52] Electrochemical performance of the FRPC electrolyte membrane measured in a Li|FRPC electrolyte|Li symmetric cell, showing (a) schematic diagram of the symmetric cell for lithium plating / stripping experiments, (b) voltage profile of lithium plating / stripping cycles at 15° C. with a current density of 0.2 mA / cm2, (c) voltage profile of subsequent lithium plating / stripping cycles at 25° C. with a current density of 0.2 mA / cm2, (d) impedance spectra of the symmetric cell measured at different cycle times (300 h, 500 h, and 700 h), (e) expanded EIS spectrum in the high frequency region, and (f) voltage profile of subsequent lithium plating / stripping cycles at 25° C. with a current density of 0.5 mA / cm2. [Diagram 53] FIG. 1 shows a magnified TEM image of garnet nanofibers with an average particle size of 20 nm in diameter. [Figure 54] As the test temperature increased to 25 °C, the voltage dropped to 0.3 V due to the improved ionic conductivity at high temperature, as shown in Figure 6c. (In subsequent long-term cycles, the voltage continued to drop to 0.2 V as the cycle time increased to 700 h. The voltage fluctuation was due to the temperature change of the surrounding environment.) [Figure 55] FIG. 11 compares two voltage profiles of a symmetric cell at two different stripping / plating process times. [Figure 56] FIG. 1 is a schematic diagram showing an example of a battery according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Although the claimed subject matter is described in terms of certain embodiments, other embodiments, including embodiments that do not provide all of the benefits and features described herein, are within the scope of this disclosure. Various structural, logical, process step, and electronic changes may be made without departing from the scope of the disclosure.

[0020] All ranges given herein include all values ​​within the range to ten decimal places unless otherwise specified.

[0021] The present disclosure provides a solid hybrid electrolyte. The present disclosure also provides methods for making the solid hybrid electrolyte and uses thereof.

[0022] In one aspect, the present disclosure provides a solid hybrid electrolyte. The solid hybrid electrolyte has a layer of a polymeric material disposed on at least a portion or all of an outer surface of a solid electrolyte (SSE). In various examples, the solid hybrid electrolyte is a polymeric material / solid hybrid electrolyte, a polymer / solid hybrid electrolyte, or a gel polymer / solid hybrid electrolyte. In various examples, the SSE is a monolithic or mesoporous SSE body or an SSE including multiple fibers or multiple strands.

[0023] In various examples, the present disclosure provides solid hybrid electrolytes formed by different methods, for example, with non-limiting layers, such as polymer layers (e.g., polymer membranes), that provide a solid hybrid electrolyte with desirable ionic conductivity and a stable, well-connected interface between such electrolyte and an electrode. The solid hybrid electrolytes of the present disclosure have, for example, a conductivity of 248 Ω×cm at the electrolyte / lithium ion cathode interface. 2 The interface resistance at the electrolyte / lithium metal anode interface is 214 Ω×cm 2The interface resistance may be as follows: The layer can be made of gel polymer (liquid electrolyte inside the polymer), dry polymer (no liquid inside the polymer, e.g. conductive Li ions with salt in the polymer), or various conductive thin films. The solid electrolyte with polymer interface can be constructed with e.g. carbon or Li metal anode and Li metal oxide, sulfur, or air to make a solid Li battery. The present disclosure addresses the issue of interface resistance between the solid electrolyte and the electrodes, which will facilitate further development of solid ionically conductive (e.g. lithium ion conductive) batteries.

[0024] In various examples, the present disclosure provides a solid-state hybrid electrolyte with flexible inorganic SSEs. The flexible inorganic SSEs can be low-cost, thin, flexible ion-conducting membranes that are expected to enable next-generation ion-conducting batteries (e.g., Li-metal batteries) that exhibit desirable safety. For example, flexible ion-conducting SSE membranes are fabricated by infiltration of ion-conducting 3D networks with Li-ion conducting polymers, etc. A schematic example is shown in FIG. 47. In various examples, oxide SSE materials are used to generate 3D ion-conducting networks, including LLZO garnets, LLTO perovskites, and LATP glasses. The 3D structure can enhance the polymer matrix, for example, by providing long-range ion transport pathways and structural reinforcement. The membrane has desirable electrochemical stability against high voltages (e.g., greater than 6 V), high ionic conductivity (e.g., greater than 10 -4 Scm -1 ), and high mechanical stability for effectively arresting, for example, lithium dendrites.

[0025] The solid hybrid electrolyte may include an inorganic SSE (e.g., an inorganic (e.g., ceramic) monolithic or mesoporous structured SSE body or an SSE including a plurality of inorganic fibers or a plurality of inorganic strands (F / S SSE)) and a polymeric material disposed on at least a portion or all of an outer surface of the SSE.

[0026] Inorganic SSEs (e.g., inorganic SSEs of F / S SSEs) may have a three-dimensional network structure with one or more nodes formed by at least two fibers or strands. Inorganic solid electrolytes (e.g., solid hybrid electrolytes) have a continuous ion-conducting pathway from one side of the inorganic solid electrolyte to the other side of the inorganic solid electrolyte. The 3D ion-conducting network of the ionic SSE may act as reinforcement and the ion-conducting (e.g., lithium-ion conducting) polymer may act as a matrix. The 3D network provides a continuous ion-conducting pathway in the electrolyte membrane. In the case of a solid hybrid electrolyte formed by strands or fibers, the inorganic solid material may be exposed on one or more surfaces of the solid hybrid electrolyte. In the case of a solid hybrid electrolyte formed by multiple strands, the inorganic SSE may be a continuous and optionally ordered mesoporous structure.

[0027] In various examples of solid hybrid electrolytes, the polymeric material fills at least some or all of the voids of the inorganic fibers or templating inorganic strands. For solid hybrid electrolytes in which the polymeric material fills some of the voids of the templating inorganic solid electrolyte, at least some of the voids open to the outer surface of the templating inorganic solid electrolyte may be filled with cathode and / or anode materials to form integrated cathodes and / or electrodes.

[0028] The inorganic SSE can be formed from a variety of inorganic materials. The inorganic material may be a ceramic material. The inorganic material is an ionically conductive material (e.g., lithium-ion conductive, sodium-ion conductive, magnesium-ion conductive, etc.). The inorganic SSE may be an ionically conductive electrolyte. Examples of suitable inorganic materials are known in the art. Non-limiting examples of inorganic materials include lithium-ion conductive inorganic materials, sodium-ion conductive inorganic materials, magnesium-ion conductive inorganic materials, etc. Any inorganic SSE electrolyte material known in the art can be used. Methods of making inorganic SSE electrolyte materials are known in the art.

[0029] Inorganic materials can have a variety of structures (e.g., secondary structures). In various examples, inorganic materials are amorphous, crystalline (e.g., monocrystalline and polycrystalline), or have a variety of amorphous and / or crystalline domains.

[0030] The inorganic material may be a lithium-conducting inorganic (e.g., ceramic) material. The lithium-conducting inorganic material may be a lithium-containing material.

[0031] Non-limiting examples of lithium ion conducting SSE materials include lithium perovskite materials, Li3N, Li-β-alumina, lithium superionic conductors (LISICON), Li 2.88 PO 3.86 N 0.14 (LiPON), Li9AlSiO8, Li 10 GeP2S 12 , Lithium garnet SSE material, Doped lithium garnet SSE material, Lithium In various examples, the lithium garnet SSE material is a cation-doped Li5La3M 1 2O 12 (However, M 1 is Nb, Zr, Ta, or a combination of these), cation-doped Li6La2BaTa2O 12 , cation-doped Li7La3Zr2O12 , and cation-doped Li6BaY2M 1 2O 12 and the cation dopant is barium, yttrium, zinc, or a combination thereof. In other examples, the lithium garnet SSE material is Li5La3Nb2O 12 , Li5La3Ta2O 12 , Li7La3Zr2O 12 , Li6La2SrNb2O 12 , Li6La2BaNb2O 12 , Li6La2SrTa2O 12 , Li6La2BaTa2O 12 , Li7Y3Zr2O 12 , Li 6.4 Y3Zr 1.4 Ta 0.6 O 12 , Li 6.5 La 2.5 Ba 0.5 TaZrO 12 , Li6BaY2M 1 2O 12 , Li7Y3Zr2O 12 , Li 6.75 BaLa2Nb 1.75 Zinc 0.25 O 12 , Li 6.75 BaLa2Ta 1.75 Zinc 0.25 O 12 etc.

[0032] The inorganic material may be a sodium ion conducting inorganic (e.g., ceramic) material. The sodium ion conducting inorganic material may be a sodium-containing material. For example, the sodium ion conducting inorganic material may be β″-Al2O3, Na4Zr2Si2PO 12 (NASICON), cation-doped NASICON, etc.

[0033] The inorganic material may be a magnesium ion conductive inorganic (e.g., ceramic) material. The magnesium ion conductive inorganic material may be a magnesium-containing material. In various examples, the magnesium ion conductive inorganic material is selected from doped magnesium oxide materials. In various examples, the magnesium ion-containing material is selected from Mg 1+x (Al,Ti)2(PO4)6 (where x is 4 or 5), NASICON-type magnesium ion conductive material, etc.

[0034] The monolithic or mesoporous SSE body may have a variety of sizes (i.e., dimensions) and / or shapes. Suitable monolithic or mesoporous SSE bodies are known in the art. The monolithic SSE body may be a dense body (e.g., including only a dense layer of inorganic material) or a dense sintered body.

[0035] Non-limiting examples of mesoporous SSEs include planar SSE structures that include an outer layer of porous (e.g., mesoporous) material (e.g., multi-layer SSE structures that include a dense layer and at least one porous (e.g., mesoporous) layer). Non-limiting examples of multi-layer SSE structures include bi-layer structures (including a porous layer disposed on a dense layer) and tri-layer structures (including two porous layers disposed on either side of a dense layer), as are known in the art. Examples of multi-layer structures are disclosed in U.S. Patent Application No. 14 / 222,306, entitled "Ion Conducting Batteries with Solid State Electrolyte Materials," filed March 21, 2014 and published September 25, 2014 as U.S. Patent Application Publication No. 2014 / 0287305, and U.S. Patent Application No. 15 / 364,528, entitled "Ceramic Ion Conducting Structures and Methods of Fabricating Same, and Uses of Same), the disclosures of each of which are incorporated herein by reference.

[0036] The F / S SSE may include fibers or strands of various sizes (i.e., dimensions) and / or shapes. In various examples, the fibers or strands are cylindrical or substantially cylindrical, polyhedral or substantially polyhedral, irregularly shaped, etc. The fibers or strands may have a length that corresponds to a multiple of one or more dimensions of the equipment used. In various examples, the fibers or strands may have lengths ranging from 1 micron to 20 meters. (including all integer micron values ​​and ranges therebetween) and / or a maximum cross-sectional dimension (e.g., diameter) of 1 nm to 10 microns (including all integer nm values ​​and ranges therebetween). In one example, the F / S SSE includes fibers or strands with lengths up to a maximum cross-sectional dimension (e.g., diameter) of 10 or more.

[0037] Fibers or strands of F / S SSEs may be flexible to provide a flexible solid-state hybrid electrolyte for use in flexible devices such as batteries. The F / S SSE and polymeric material may form the electrolyte. The F / S SSEs may be made by the methods described herein.

[0038] A variety of polymeric materials can be used. A mixture of two or more polymeric materials (e.g., two or more polymers) can be used. The polymeric materials can be conductive (e.g., ionically and / or electronically conductive), non-conductive, or a combination thereof. The polymeric materials can be dry polymers or gels.

[0039] In the case of monolithic SSEs or mesoporous bodies, it may be desirable for the polymeric material to be conductive (e.g., ionically and / or electronically conductive). In the case of inorganic SSEs comprising multiple fibers or strands, it may be desirable for the polymeric material, which may be a mixture of multiple polymeric materials, to provide mechanical strength to the SSE.

[0040] In the case of a solid hybrid electrolyte having a monolithic SSE or mesoporous SSE body, it is desirable to have a thin layer of polymer material, for example having a thickness between 5 nm and 10 microns (including all integer nm values ​​and ranges therebetween).

[0041] The polymeric material can be disposed on at least a portion or all of a surface of the SSE (e.g., an inorganic SSE). In the case of dense SSE materials, the polymeric material is a layer (e.g., a conformal layer) disposed on at least a portion (e.g., the portion of the SSE material on which the electrodes (e.g., cathode and / or anode) are disposed). In the case of porous SSEs (which may be a monolithic or mesoporous SSE body or the exterior (e.g., a layer) of an SSE comprising a plurality of fibers or strands), the polymeric material is disposed on the pore surfaces, the non-porous surfaces, or both. It may be desirable for the polymeric material to be disposed on the portion of the porous SSE material on which the electrodes (e.g., cathode and / or anode) are disposed. In one example, the polymer material is present at 1 volume percent or more, 5 volume percent or more, 10 volume percent or more, 20 volume percent or more, 30 volume percent or more, 40 volume percent or more, 50 volume percent or more, or 60 volume percent or more of the solid hybrid electrolyte.

[0042] In the case of a monolithic SSE or a solid hybrid electrolyte with mesoporous bodies, the polymeric material can be a layer. The layer can be formed by various methods known in the art, such as dip coating, slurry casting, spray coating, or spin coating.

[0043] In the case of a solid hybrid electrolyte with a F / S SSE, the polymer material is disposed in the voids formed by the individual fibers or strands of the SSE. The voids may be pores as a result of the use of a template. The polymer material may be incorporated into the F / S SSE by methods known in the art. For example, the polymer material is infiltrated or in-situ synthesized into the voids (e.g., pores) of the F / S SSE.

[0044] A variety of polymeric materials can be used. The polymeric material may include one or more polymers, one or more copolymers, or a combination thereof. The molecular weight of the polymer and / or copolymer is not particularly limited. For example, depending on the performance (e.g., ionic conductivity) requirements of the device (e.g., solid-state ionically conductive battery), the polymer and / or copolymer may have a wide range of molecular weights. It may be desirable for the polymer and / or copolymer to be conductive. The polymeric material may include a mixture of conductive and non-conductive polymers and / or copolymers.

[0045] The polymers and / or copolymers can have a variety of structures (e.g., secondary structures). In various examples, the polymers and / or copolymers are amorphous, crystalline, or a combination thereof. It may be desirable for the polymers and / or copolymers to have low crystallinity.

[0046] Polymeric materials include, but are not limited to, polymers and copolymers. The polymers and copolymers may be conductive or non-conductive. Non-limiting examples of polymers and copolymers include poly(ethylene) (PE), poly(ethylene oxide) (PEO), poly(propylene) (PP), poly(propylene oxide), polymethyl methacrylate (PMMA), polyacrylonitrile (PAN), poly[bis(methoxyethoxyethoxide)-phosphazene], poly(dimethylsiloxane) (PDMS), cellulose, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, polyvinylidene difluoride (PVdF), polyvinylpyrrolidone (PVP), polystyrene, sulfonates (PSS), polyvinyl chloride (PVC) family, poly(vinylidene chloride) polypropylene oxide, polyvinyl acetate, polyvinyl chloride ... Examples of suitable poly(vinylidene fluoride-hexafluoropropylene copolymers include poly(methyl methacrylate-ethyl acrylate copolymers) and poly(vinylidene fluoride-hexafluoropropylene copolymers). Examples of suitable poly(vinylidene fluoride-hexafluoropropylene copolymers include ...

[0047] The polymeric material may be a gel. The gel includes a polymeric material (e.g., one or more polymers and / or one or more copolymers) and a liquid. A combination of liquids can also be used. In various examples, the liquid is an organic liquid (e.g., ethylene carbonate (EC), diethyl carbonate (DEC), dimethoxyethane (DME), dioxolane (DOL), etc.) or an ionic liquid (e.g., N-propyl-N-methylpyrrolidinium bis(trifluoromethanesulfonyl)imide (PYR 13 TFSI, etc.

[0048] The liquid may be a liquid electrolyte. The liquid electrolyte may include a metal salt (e.g., one or more lithium salts, one or more sodium salts, one or more magnesium salts, etc.). A non-limiting example of a liquid electrolyte is an aqueous liquid electrolyte. Non-limiting examples of liquid electrolytes include LiPF6 (e.g., 1M) in ethylene carbonate (EC) / diethyl carbonate (DEC), LiTFSI (e.g., 1M) in dimethoxyethane (DME) / dioxolane (DOL), N-propyl-N-methylpyrrolidinium bis(trifluoromethanesulfonyl)imide (PYRP), and LiCl (LiCl) (e.g., 1M). 13 TFSI) LiTFSI (e.g., 0.5M) in ionic liquids.

[0049] The polymeric material may include a filler. In one example, the polymeric material includes one or a plurality of ceramic fillers (e.g., 2-25 wt% ceramic filler based on the total weight of the polymeric material). Non-limiting examples of ceramic fillers include conductive particles, non-conductive particles (e.g., Al2O3, SiO2, TiO2 nanoparticles, etc.), and ceramic nanomaterials (e.g., ceramic nanoparticles, ceramic nanofibers, etc.). The ceramic nanomaterials may have the composition of the inorganic materials disclosed herein.

[0050] In one aspect, the present disclosure provides methods of making inorganic fibers or strands. The fibers or strands can form inorganic SSEs. In various examples, these methods are templating or electrospinning methods.

[0051] The strands can be formed by a templating method. The template comprises interconnected voids that can be used to form strands of inorganic material that can form inorganic solid electrolytes (e.g., solid hybrid electrolytes). The voids can be engineered or occur naturally in biological materials (e.g., wood, plants, etc.).

[0052] The templating method provides a simple yet effective way to generate the required structures. The fiber template is contacted (e.g., soaked) with one or more inorganic SSE material precursors, followed by an optional heating step to react the precursors and thermal treatment (e.g., pyrolysis) to remove the organic components. The resulting fibrous inorganic material may exhibit desirable properties that allow integration into flexible or rigid battery configurations. For example, inorganic strand or fiber networks have established lithium ion migration pathways within polymeric materials and improved mechanical strength of the polymeric materials. Alternatively, inorganic material (e.g., ceramic) fibers can be combined with electrode materials in interdigitated or concentric configurations to minimize electrolyte volume and maximize electrode utilization, thus increasing active electrolyte area, lithium ion interfacial migration, and electrode volume change resistance during charge / discharge.

[0053] The templating method provides a porous (e.g., nanoporous and / or microporous) inorganic SSE comprising a plurality of strands. The strands may have the general shape (e.g., cylindrical or substantially cylindrical, polyhedral or substantially polyhedral, irregular, etc.) of the template used to construct the individual strands. For example, the strands have lengths in the micrometer to meter range and / or maximum cross-sectional dimensions (e.g., diameters) in the nanometer to micrometer range.

[0054] The pores (e.g., pore size, pore size distribution, pore morphology, etc.) of the inorganic SSE electrolyte may vary depending on the method (e.g., templating or electrospinning used). In the case of templating methods, the pores may be formed by removal of a template material (e.g., may have a size and / or shape corresponding to the templating material). In the case of electrospinning, the pores may be formed by voids formed by the fibers. For example, in the case of inorganic SSEs formed by templating methods, at least some or all of the pores have at least one dimension between 1 and 100 microns. For example, in the case of inorganic SSEs formed by electrospinning, at least some or all of the pores have at least one dimension between 1 nm and 500 microns.

[0055] In various examples, the pores of the solid hybrid electrolyte, the strands (e.g., some or all of the strands) of the solid hybrid electrolyte (if present), and / or the pores of the solid hybrid electrolyte may be aligned or substantially aligned. "Aligned" refers to the longitudinal axis of each strand being parallel to the longitudinal axis of an adjacent strand. It means that the strands and / or pores of the inorganic SSE are aligned such that the strands and / or pores are aligned at an angle of less than 30°, less than 20°, less than 15°, less than 10°, or less than 5°. In one example, the strands and / or pores are not arranged end-to-end. Substantial alignment means that at least 50%, at least 60%, at least 70, 80%, at least 90%, at least 95%, at least 99% of the strands are aligned.

[0056] As an illustrative example, when a solid hybrid electrolyte formed from a biomaterial template (e.g., a wood template, a plant template, etc.) is used in a battery with planar discrete electrodes, the individual strands are aligned generally perpendicular (e.g., vertical) to the plane defined by one or both of the electrodes, and the pores are also aligned generally perpendicular (e.g., vertical) to the plane defined by one or both of the electrodes.

[0057] In various examples, the strands of the inorganic SSE (e.g., some or all of the strands) are arranged as a fabric (e.g., a woven fabric, a braided fabric, etc.). The strands of the inorganic SSE may take on the general structure of the fibrous template used to make the inorganic SSE. The dimensions of the inorganic SSE may be substantially smaller than the dimensions of the fibrous template.

[0058] As an illustrative example, when a solid hybrid electrolyte formed from a carbon template (e.g., a fiber template, etc.) is used in a battery with planar discrete electrodes, the individual strands of the inorganic SSE are aligned generally parallel (e.g., parallel) to the plane defined by one or both of the electrodes, and the pores of the inorganic SSE are aligned perpendicular to the plane defined by one or both of the electrodes.

[0059] In various examples, a templating method for constructing an inorganic solid electrolyte (e.g., a solid hybrid electrolyte) can include: contacting the template with one or more SSE material precursors; Optionally, reacting the SSE material precursor to form a solid inorganic material (e.g., comprising at least a portion or all of the reacted and / or decomposed SSE material precursor); heat treating the template with a solid inorganic material, where the template is removed (e.g., as carbon dioxide) and an inorganic SSE (e.g., a monolithic SSE or a mesoporous or F / S SSE) is formed; contacting the calcined template with a polymeric material to form a layer on the inorganic SSE material, in the case of a monolithic or mesoporous body (and optionally fill at least some or all of the pores exposed on the surface of the inorganic SSE material), or, in the case of a F / S SSE, the polymeric material fills at least some or all of the pores of the F / S SSE (e.g., pores corresponding to the template); Includes.

[0060] In various examples, a templating method for forming an inorganic solid electrolyte (e.g., a solid hybrid electrolyte) includes: contacting (e.g., infiltrating) the biomaterial template with one or more SSE material precursors (e.g., one or more inorganic SSE material sol-gel precursors) such that one, more, or all of the aligned channels of the biomaterial template (e.g., the compressed biomaterial template) are at least partially or completely filled with the SSE material precursor; Optionally, reacting (e.g., by heating) the SSE material precursor filled template to form a solid inorganic material (e.g., including at least a portion or all of the reacted and / or decomposed inorganic SSE material sol-gel precursor); and heat treating the heated template to remove substantially all of the template material. or all of the inorganic SSE material is removed to form the inorganic SSE material; contacting the calcined template with a polymeric material, wherein the polymeric material at least partially fills the nanopores and / or micropores of the inorganic SSE; and Includes.

[0061] In various examples, a templating method for constructing an inorganic solid electrolyte (e.g., a solid hybrid electrolyte) can include: contacting the carbon template with one or more inorganic SSE material precursors (e.g., one or more metal salts); Optionally, reacting (e.g., by heating) the carbon template-contacted carbon template to form a solid inorganic material (e.g., a plurality of nanoparticles of an inorganic material); heat treating the template to remove substantially all or all of the template material and form the inorganic SSE material; contacting (e.g., infiltrating) the inorganic SSE with a polymeric material, wherein the polymeric material at least partially fills the nanopores and / or micropores of the template; Includes.

[0062] A variety of templates can be used. The template can be formed of a polymer (e.g., biologically derived polymers (e.g., cellulose, protein fibers, etc.), artificial polymers (e.g., PET, polyamides such as nylon, regenerated cellulose such as rayon, polyester, etc.). The template can have a hierarchical interconnected structure including interconnected nanoscale and / or microscale voids. For example, the template can be a low-torsion template (e.g., a low-torsion template formed from a wood template). The template can be a biological material (e.g., wood, plants, etc.) or an artificial template, which can be formed by methods such as tape casting, screen printing, extrusion, 3D printing, weaving, braiding, non-woven knitting, etc. In these methods, all or substantially all of the template is removed (i.e., a sacrificial template). For example, the template can be removed by heat treatment.

[0063] A variety of carbon templates can be used. Examples of carbon templates include, but are not limited to, fiber templates, paper templates, foam templates, etc. The carbon template can be a fiber. In various examples, the fiber is a fabric. The fabric can include various weaves, braids, etc., or can be non-woven. In the case of a woven fabric, the woven fabric can be of any weave pattern.

[0064] A variety of biomaterial templates can be used: the biomaterial template may be a wood template, a plant template, etc.

[0065] A variety of wood and plant templates can be used. The wood or plant template includes a plurality of nano- and / or micro-channels. The plurality of nano- and / or micro-channels are interconnected to form a three-dimensional network having at least one node. The wood template can be a compressed wood template. Typically, the wood template is formed by removing at least some or all of the lignin from wood of a size and shape appropriate for the formation of F / S SSEs. The removal of the lignin results in the formation of a template (e.g., a template with aligned porous nanostructures) with a plurality of aligned channels (e.g., channels having a cross-sectional size (e.g., longest dimension such as diameter) of 1 nm to 10 microns (including all integer nm values ​​and ranges therebetween). Compressing the template in a can results in the formation of nano- and micro-channels. The microchannels may be reduced in cross section and / or the cross section may be reduced. Lignin may be removed by chemical treatment. Suitable treatments are known in the art. For example, lignin may be removed by contacting the wood sample with an aqueous base solution. Wood templates may be formed from a variety of woods, such as, for example, basswood, balsa wood, etc.

[0066] Fibers of the inorganic SSE can be formed by electrospinning. Suitable electrospinning methods are known in the art. Electrospinning can be carried out by methods known in the art.

[0067] The inorganic SSE material precursors may be reacted (e.g., at least partially or totally reacted and / or thermally degraded) to form a solid inorganic material, such as one or more of the precursors (which may include a residue, such as a carbon-based residue), and the inorganic material may be thermally treated to provide the inorganic SSE material.

[0068] In various examples, the electrospinning process for forming an inorganic solid electrolyte (e.g., a solid hybrid electrolyte) can include: electrospinning a precursor solution comprising an electrospinning polymer and one or more inorganic SSE precursor materials to provide nanofibers comprising the polymer and one or more inorganic SSE precursor materials; heat treating the nanofibers to remove all or substantially all of the polymer of the nanofibers and form an inorganic SSE material; contacting the inorganic SSE with a polymeric material, wherein the polymeric material at least partially fills voids of the inorganic SSE material; Includes.

[0069] A variety of electrospinning polymers can be used. Suitable electrospinning polymers are known in the art. Non-limiting examples of electrospinning polymers include polyvinylpyrrolidone (PVP), polyacrylonitrile (PAN), poly(ethylene oxide) (PEO), or polyvinyl chloride (PVC).

[0070] A variety of inorganic SSE precursor materials can be used. Non-limiting examples of inorganic SSE precursor materials include sol-gel precursors, metal salts, and the like. The SSE material precursor may be one or more sol-gel precursors or one or more metal salts that upon reaction (e.g., heating) provide an inorganic SSE of a desired composition. Examples of suitable sol-gel precursors and sol-gel precursor combinations are known in the art. Examples of suitable metal salts and metal salt combinations are known in the art. In various examples, the heat treatment includes sintering and / or calcining the inorganic SSE material precursor or the reacted (e.g., at least partially or fully reacted) inorganic SSE material precursor.

[0071] The thermal treatment removes (e.g., pyrolyzes) the template material. The thermal treatment removes at least a portion (e.g., substantially) or all of the template to provide the inorganic SSE. In various examples, the thermal treatment is performed at 700-1000° C. in an air atmosphere or an oxygen-containing atmosphere.

[0072] In one aspect, the present disclosure provides uses of the solid hybrid electrolytes of the present disclosure. The solid hybrid electrolytes can be used in a variety of devices. In various examples, the devices include one or more solid hybrid electrolytes of the present disclosure. Examples of devices include electrolyzers, electrolytic cells, fuel cells, batteries, and other electrochemical devices (e.g., sensors, etc.). These include, but are not limited to:

[0073] The device may be a battery. The battery may be an ionically conductive battery. The battery may be configured for applications such as portable applications, transportation applications, stationary energy storage applications, etc. Examples of ionically conductive batteries include, but are not limited to, lithium ion conductive batteries, sodium ion conductive batteries, magnesium ion conductive batteries, etc.

[0074] In various examples, a battery (e.g., an ionically conductive battery, such as a solid-state ionically conductive battery) comprises the solid hybrid electrolyte of the present disclosure, an anode, and a cathode, with the solid hybrid electrolyte disposed between the anode and the cathode. In one example, the polymer material of the solid hybrid electrolyte is disposed between the inorganic SSE material of the solid hybrid electrolyte and the anode and / or cathode.

[0075] The inorganic SSE material can be used in a conventional ion-conducting battery (e.g., the ion-conducting battery includes an electrolyte as the base electrolyte). The conventional ion-conducting battery includes a non-conducting (e.g., non-ion-conducting) separator. Thus, in one example, the battery includes an inorganic SSE material disclosed herein (e.g., an F / S SSE, which may be a templating inorganic SSE or an electrospun inorganic SSE) or a solid hybrid electrode disclosed herein (e.g., an F / S SSE), and an electrolyte. The electrolyte may be any electrolyte used in a conventional ion-conducting (e.g., lithium-ion-conducting) battery known in the art. Non-limiting examples of electrolytes in a conventional battery include liquids, such as organic liquids, gels, polymers, etc. In various examples, the liquid electrolyte is not part of the solid hybrid electrolyte (e.g., part of the polymeric material, such as the gel polymer, of the solid hybrid electrolyte). In this case, the inorganic SSE material or the solid hybrid electrode is the separator of the conventional battery. In various examples, the inorganic SSE material or solid hybrid electrode replaces the separator of a conventional battery. Unlike the typical separator used in conventional batteries, the inorganic SSE material or solid hybrid electrode both separates the cathode and anode and is ionically conductive. In various examples, the inorganic SSE material or solid hybrid electrode is the ionically conductive separator of a conventional battery. A variety of electrodes (e.g., cathode and anode) can be used. The individual electrodes (e.g., cathode and / or anode) can be independent (e.g., separate) from the solid hybrid electrolyte (e.g., planar electrodes) or can be integrated with the solid hybrid electrolyte. In the case of an integrated electrode, the solid hybrid electrolyte (e.g., a monolithic SSE or mesoporous SSE body) has one or more porous regions exposed at the surface of the solid hybrid electrolyte, and the electrodes are formed by electrode materials (e.g., cathode material and / or anode material) disposed in the pores of the discrete porous regions of the solid hybrid electrolyte.

[0076] The cathode and anode can be formed from a variety of materials (e.g., cathode or anode materials, respectively). Examples of suitable cathode and anode materials are known in the art.

[0077] The cathode includes one or more cathode materials in electrical contact with the solid hybrid electrolyte. A variety of cathode materials can be used. Combinations of cathode materials may be used. For example, the cathode material is an ionically conductive material that stores ions by mechanisms such as intercalation or reacts with ions to form a secondary phase (e.g., air or sulfide electrodes). Examples of suitable cathode materials are known in the art.

[0078] In the case of an integrated cathode, the cathode material is deposited on the surface of the porous region of the solid hybrid electrolyte. (e.g., a pore surface of one of the pores). The cathode material may at least partially fill one or more pores (e.g., a majority of the pores) of the porous region or one of the porous regions of the ion-conducting solid electrolyte material. In one example, the cathode material infiltrates at least some of the pores of the porous region of the ion-conducting solid electrolyte material.

[0079] In one example, the cathode material is disposed on at least a portion of the pore surfaces on the cathode side of the porous region of the porous SSE material, and the cathode side of the porous region of the SSE material faces the anode side of the porous region of the porous SSE material on which the anode material is disposed.

[0080] In various examples, the cathode comprises a conductive carbon material. Non-limiting examples of carbon materials include graphite, hard carbon, porous hollow carbon spheres and tubes, and the like. The cathode material may further comprise an organic or gel ion-conducting electrolyte. Suitable organic or gel ion-conducting electrolytes are known in the art.

[0081] It may be desirable to use a conductive material as part of the ion-conducting cathode material. Also, in one example, the ion-conducting cathode material includes a conductive carbon material (e.g., graphene or carbon black) and, optionally, further includes an organic or gel ion-conducting electrolyte. The conductive material may be separate from the ion-conducting cathode material. For example, the conductive material (e.g., graphene, carbon nanotubes, etc.) is disposed on at least a portion of the surface (e.g., pore surface) of the porous region of the ion-conducting SSE electrolyte material, and the ion-conducting cathode material is disposed on at least a portion of the conductive material (e.g., graphene, carbon nanotubes, etc.).

[0082] In various other examples, the cathode includes a sulfur-containing material. In one example, the cathode material is an organic sulfide or polysulfide. Examples of organic sulfides include carbyne polysulfides and copolymerized sulfur. Non-limiting examples of sulfur-containing materials include sulfur, sulfur composite materials (e.g., carbyne polysulfides, copolymerized sulfur, etc.), and polysulfide materials.

[0083] In one example, the cathode is an air electrode. Examples of materials suitable for the air electrode include materials used in ionically conductive batteries, such as lithium-ion batteries with air cathodes, such as high surface area carbon particles (e.g., Super P, a conductive carbon black) and catalyst particles (e.g., α-MnO2 nanorods) bound to a mesh (e.g., a polymeric binder such as a PVDF binder).

[0084] The cathode material may be a lithium ion conducting material. Non-limiting examples of lithium ion conducting cathode materials include lithium nickel manganese cobalt oxide (e.g., NMC, LiNi x Mn y Co z O2 (where x+y+z=1, e.g. Li(NiMnCo) 1 / 3 O2 etc.)), LiCoO2, LiNi 1 / 3 Co 1 / 3 Mn1 / 3 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, lithium manganese oxides (LMOs) (e.g., LiMn2O4 and LiNi 0.5 Mn 1.5 O4), lithium iron phosphate (LFP) (e.g., LiFePO4), LiMnPO4, LiCoPO4, and Li2MMn3O8 (wherein M is selected from Fe, Co, etc.).

[0085] The cathode material may be a sodium ion conducting material. Non-limiting examples of sodium ion conducting cathode materials include Na2V2O5, P2-Na 2 / 3 Fe 1 / 2 Mn 1 / 2 O2, Na3V2(PO4)3, NaMn 1 / 3 Co 1 / 3 Ni 1 / 3 PO4, and Na 2 / 3 Fe 1 / 2 Mn 1 / 2 and composite materials such as O2@graphene composites (e.g., composites containing carbon black).

[0086] The cathode material may be a magnesium ion conducting material. Non-limiting examples of magnesium ion conducting cathode materials include doped manganese oxides (e.g., Mg x MnO2 y H2O), Mg 1+x (Al,Ti)2(PO4)6 (where x is 4 or 5), NASICON-type magnesium ion conductive material, etc.

[0087] The anode comprises one or more anode materials in electrical contact with the porous region of the solid hybrid electrolyte. For example, the anode material is a metallic form of ions that conduct in the solid electrolyte (e.g., metallic lithium in lithium ion batteries) or a compound that inserts conducting ions (e.g., lithium carbide, Li6C in lithium ion batteries). Examples of suitable anode materials are known in the art.

[0088] In the case of an integrated anode, the anode material is disposed on at least a portion of a surface (e.g., a pore surface of one of the pores) of the porous region of the solid hybrid electrolyte. The anode material may at least partially fill one or more pores (e.g., a majority of the pores) of the porous region of the solid hybrid electrolyte. In one example, the anode material infiltrates at least a portion of the pores of the porous region of the solid hybrid electrolyte.

[0089] In one example, the anode material is disposed on at least a portion of the pore surfaces of the anode-side porous region of the solid hybrid electrolyte, and the anode side of the solid hybrid electrolyte faces the cathode side of the solid hybrid electrolyte on which the cathode material is disposed.

[0090] In various examples, the anode comprises (or consists of) a conductive carbon material. Non-limiting examples of carbon materials include graphite, hard carbon, porous hollow carbon spheres and tubes, and the like. The anode material may further comprise an organic or gel ion-conducting electrolyte. Suitable organic or gel ion-conducting electrolytes are known in the art.

[0091] The anode material may be a conductive material. Non-limiting examples of conductive materials include conductive carbon materials, tin and its alloys, tin / carbon, tin / cobalt alloys, silicon / carbon materials, etc. Non-limiting examples of conductive carbon materials include graphite, hard carbon, porous hollow carbon spheres and tubes (e.g., carbon nanotubes), etc.

[0092] The anode may be a metal, non-limiting examples of which include lithium metal, sodium metal, magnesium metal, and the like.

[0093] The anode material may be a lithium-containing material, non-limiting examples of which include lithium metal, lithium carbide, Li6C, and lithium titanate (LTO) (e.g., Li4Ti5O12 etc.)

[0094] The anode material may be a sodium-containing material. Non-limiting examples of anode materials include sodium metal, Na2C8H4O4, and Na 0.66 Li 0.22 Ti 0.78 Examples include ionically conductive sodium-containing anode materials such as O2.

[0095] The anode material may be a magnesium-containing material, hi one example, the anode material is magnesium metal.

[0096] The battery may include a current collector. For example, the battery may include a cathode (first) current collector disposed on the cathode side of the solid hybrid electrolyte and an anode (second) current collector disposed on the anode side of the solid hybrid electrolyte. and an anode-side (second) current collector disposed on the anode-side. Each current collector is independently made of a metal (e.g., aluminum, copper, or titanium) or a metal alloy (e.g., aluminum alloy, copper alloy, or titanium alloy).

[0097] The battery may include various additional structural elements (e.g., bipolar plates, external packaging, electrical contacts / leads connecting wires, etc.). In one example, the battery further includes a bipolar plate. In various examples, the battery further includes electrical contacts / leads connecting wires, as well as the bipolar plate and external packaging. In one example, the repeating battery cell units are separated by bipolar plates.

[0098] The solid hybrid electrolyte, the cathode, the anode, the cathode side (first) current collector (if present), and the anode side (second) current collector (if present) may form a cell. The battery may comprise multiple cells separated by one or more bipolar plates. The number of cells in a battery is determined by the performance requirements (e.g., voltage output) of the battery and is limited only by fabrication constraints. For example, a solid-state ionically conductive battery may comprise 1 to 500 cells (including all integer cell numbers and ranges therebetween).

[0099] The method steps in the various embodiments and examples disclosed herein are sufficient to carry out the disclosed method, such that in one example, the method consists essentially of a combination of the method steps disclosed herein, and in another example, the method consists of such steps.

[0100] The following statements provide examples of the disclosed solid hybrid electrolytes and their uses. Statement 1. An SSE (e.g., an inorganic (e.g., ceramic) SSE) as disclosed herein (or including an inorganic SSE material as disclosed herein); a polymeric material as disclosed herein disposed on at least a portion or all of an exterior surface of a solid electrolyte (e.g., a solid electrolyte material); A hybrid electrolyte (e.g., a solid hybrid electrolyte). Statement 2. A hybrid electrolyte as described in Statement 1, wherein the SSE material is a monolithic (e.g., porous monolithic, dense monolithic) SSE body or a mesoporous SSE body as disclosed herein (examples of mesoporous SSE body materials include bilayer and trilayer materials comprising one or more layers of porous SSE material disposed on a layer of dense SSE material). Statement 3. The hybrid electrolyte of statement 1 or 2, wherein the SSE material is a disk, sheet, or polyhedron (e.g., has a polyhedral shape). Statement 4. The hybrid electrolyte of any one of statements 1 to 3, wherein the polymer material has a thickness at one or more points of from 10 nm to 10 microns (e.g., from 5 to 10 microns). Statement 5. The hybrid electrolyte of any one of statements 1 to 4, wherein the SSE comprises a plurality of fibers or strands (e.g., a plurality of non-woven strands or a plurality of woven strands). Statement 6. The hybrid electrolyte according to statement 5, wherein the fiber is present as a woven or knitted substrate. Statement 7. The hybrid electrolyte according to statement 5 or 6, wherein the fibers are randomly arranged or aligned. Statement 8. The hybrid electrolyte according to any one of statements 5 to 7, wherein the fibers or strands of polymer material form an interconnected 3D network. Statement 9. The SSE material is a lithium ion conducting (e.g., lithium ion containing) SSE material, a sodium ion conducting (e.g., sodium ion containing) SSE material, A hybrid electrolyte according to any one of statements 1 to 8, comprising a magnesium ion conducting (e.g., magnesium ion containing) SSE material. Statement 10. The lithium ion conducting SSE material is selected from the group consisting of lithium perovskite materials, Li3N, Li-β-alumina, lithium superionic conductors (LISICON), Li 2.88 PO 3.86 N 0.14 (LiPON), Li9AlSiO8, Li 10 GeP2S 12 10. The hybrid electrolyte of claim 9, wherein the lithium garnet material is selected from the group consisting of a lithium garnet material, a doped lithium garnet material, a lithium garnet composite material, and combinations thereof. Statement 11. The lithium garnet material is cation-doped Li5La3M 1 2O 12 (However, M 1is Nb, Zr, Ta, or a combination of these), cation-doped Li6La2BaTa2O 12 , cation-doped Li7La3Zr2O 12 , and cation-doped Li6BaY2M 1 2O 12 (However, M 1 is Nb, Zr, Ta, or a combination thereof; and the cation dopant is barium, yttrium, zinc, or a combination thereof. Statement 12. The lithium garnet material is Li5La3Nb2O 12 , Li5La3Ta2O 12 , Li7La3Zr2O 12 , Li6La2SrNb2O 12 , Li6La2BaNb2O 12 , Li6La2SrTa2O 12 , Li6La2BaTa2O 12 , Li7Y3Zr2O 12 , Li 6.4 Y3Zr 1.4 Ta 0.6 O 12 , Li 6.5 La 2.5 Ba 0.5 TaZrO 12 , Li6BaY2M 1 2O 12 , Li7Y3Zr2O 12 , Li 6.75 BaLa2Nb 1.75 Zinc 0.25 O 12 , Li 6.75 BaLa2Ta 1.75 Zinc 0.25 O 12 and combinations thereof. Statement 13. The sodium ion conducting SSE material is β”-Al2O3, Na4Zr2Si2PO 12 (NASICON), cation-doped NASICON, and combinations thereof. Statement 14. The magnesium ion conducting SSE material is 1+x The hybrid electrolyte according to statement 9, wherein the cations are selected from the group consisting of (Al,Ti)2(PO4)6 (wherein x is 4 or 5), NASICON-type magnesium ion conducting materials, and combinations thereof. Statement 15. The hybrid electrolyte of any one of statements 1-14, wherein the inorganic SSE has pores exposed to an exterior surface of the inorganic SSE, and the hybrid electrolyte further comprises at least one cathode material and / or at least one anode material disposed in at least a portion of the pores, and when the at least one cathode material and the at least one anode material are disposed in at least a portion of the pores, the at least one cathode material and the at least one anode material are disposed in discrete and electrically isolated regions of the inorganic SSE. Statement 16. The polymeric material is poly(ethylene) (PE), poly(ethylene oxide) (PEO), poly(propylene) (PP), poly(propylene oxide), polymethyl methacrylate (PMMA), polyacrylonitrile (PAN), poly[bis(methoxyethoxyethoxide)-phosphazene], poly(dimethylsiloxane) (PDMS), cellulose, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, polyvinylidene difluoride (PVdF), polyvinylpyrrolidone (PVP), polystyrene, polyvinyl chloride, polystyrene sulfonate (PSS), polyvinyl chloride, polystyrene-sulfonate (PSC), ... (PVC) family, poly(vinylidene chloride) polypropylene oxide, polyvinyl acetate, polytetrafluoroethylene (e.g., Teflon), poly(ethylene terephthalate) (PET), polyimides, polyhydroxyalkanoates (PHAs), PEO-containing copolymers (e.g., polystyrene (PS)-PEO copolymers and poly(methyl methacrylate) (PMMA)-PEO copolymers), polyacrylonitrile (PAN), poly(acrylonitrile-methyl acrylate copolymers), PVdF-containing copolymers (e.g., polyvinylidene fluoride-hexafluoropropene copolymers), polyvinyl chloride (PVDF) ... 16. The hybrid electrolyte of any one of statements 1-15, comprising (e.g., is) a polymer selected from the group consisting of poly(propylene glycol-vinyl chloride-propylene copolymer (PVdF-HFP copolymer)), PMMA copolymer (e.g., poly(methyl methacrylate-ethyl acrylate copolymer)), derivatives thereof, and combinations thereof. Statement 17. The hybrid electrolyte of any one of statements 1 to 16, wherein the polymeric material is a gel (e.g., a gel containing 60 to 80 wt % liquid, based on the total weight of the polymeric material). Statement 18. The liquid is a liquid electrolyte (e.g., LiPF6 (e.g., 1M) in ethylene carbonate (EC) / diethyl carbonate (DEC), LiTFSI (e.g., 1M) in dimethoxyethane (DME) / dioxolane (DOL), N-propyl-N-methylpyrrolidinium bis(trifluoromethanesulfonyl)imide (PYR 13 18. The hybrid electrolyte of any one of statements 1 to 17, wherein the electrolyte is a non-aqueous liquid electrolyte such as LiTFSI (e.g., 0.5 M) in a ionic liquid. Statement 19. The hybrid electrolyte of statement 17 or 18, wherein the polymeric material of the gel comprises (e.g., is) a polymer selected from the group consisting of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP copolymer), polyvinylpyrrolidone (PVP), PEO, PMMA, PAN, polystyrene (PS), polyethylene (PE), and combinations thereof. Statement 20. The hybrid electrolyte of any one of statements 1 to 19, wherein the polymeric material comprises a metal salt (e.g., a metal salt selected from the group consisting of lithium salts, sodium salts, magnesium salts, etc.). Statement 21. The hybrid electrolyte of any one of statements 1 to 20, wherein the polymer material comprises a ceramic filler (e.g., 2 to 25 wt %, based on the total weight of the polymer material). Statement 22. The hybrid electrolyte according to statement 21, wherein the ceramic filler is selected from the group consisting of conductive particles, non-conductive particles (e.g., Al2O3, SiO2, TiO2 nanoparticles, etc.), ceramic nanomaterials (e.g., ceramic nanoparticles, ceramic nanofibers). Statement 23. A device comprising one or more hybrid electrolytes of the present disclosure (e.g., a hybrid electrolyte described in any one of statements 1-22). Statement 24. A hybrid electrolyte of the present disclosure (e.g., a hybrid electrolyte described in any one of statements 1 to 22); An anode; A cathode; Equipped with The device of statement 23, wherein the device is a battery (e.g., an ionically conductive battery such as a solid-state ionically conductive battery) in which the hybrid electrolyte is disposed between the cathode and the anode (e.g., the polymeric material of the hybrid electrolyte is disposed between the SSE material of the hybrid electrolyte and the anode and / or cathode (e.g., filling substantially all of the voids between the SSE material of the hybrid electrolyte and the anode and / or cathode)). Statement 25. The device of statement 24, wherein the battery further comprises a current collector disposed on at least a portion of the cathode and / or the anode. Statement 26. The device according to Statement 25, wherein the current collector is an electrically conductive metal or metal alloy. Statement 27. The device of any one of statements 24-26, wherein the battery is a lithium-ion conducting solid-state battery and the hybrid electrolyte is a lithium-ion conducting (e.g., lithium-containing) SSE material (e.g., a lithium conducting (e.g., lithium-containing) SSE material described in any one of statements 11-13). Statement 28. The battery is a sodium ion conductive solid-state battery and a hybrid The device of any one of statements 24 to 26, wherein the electrolyte is a sodium ion conducting (e.g., sodium-containing) SSE material (e.g., a sodium ion conducting (e.g., sodium-containing) SSE material described in statement 14). Statement 29. The device of any one of statements 24-26, wherein the battery is a magnesium ion conducting solid-state battery and the hybrid electrolyte is a magnesium ion conducting (e.g., magnesium-containing) SSE material (e.g., a magnesium ion conducting (e.g., magnesium-containing) SSE material described in statement 15). Statement 30. The device of any one of statements 24 to 29, wherein the cathode and / or anode comprise a conductive carbon material (e.g., graphite, hard carbon, porous hollow carbon spheres and tubes, etc.), and the cathode material optionally further comprises an organic or gel ionically conductive electrolyte. Statement 31. The apparatus of any one of statements 24 to 29, wherein the cathode comprises a material selected from sulfur, sulfur composite materials (e.g., carbyne polysulfides, copolymerized sulfur, etc.), and polysulfide materials, or is air. Statement 32. The device of statement 27, wherein the cathode (e.g., a lithium ion conducting, lithium-containing cathode) comprises a material selected from the group consisting of lithium-containing materials. Statement 33. The lithium-containing cathode material is lithium nickel manganese cobalt oxide (e.g., NMC, LiNi x Mn y Co z O2 (where x+y+z=1, e.g. Li(NiMnCo) 1 / 3 O2 etc.)), LiCoO2, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, lithium manganese oxides (LMOs) (e.g., LiMn2O4 and LiNi 0.5 Mn 1.533. The apparatus of statement 32, wherein the lithium phosphate (LFP) (e.g., LiFePO4), LiMnPO4, LiCoPO4, and Li2MMn3O8 (wherein M is selected from Fe, Co, and combinations thereof). Statement 34. The device of statement 28, wherein the cathode (e.g., a sodium ion conducting, sodium-containing cathode) comprises a material selected from the group consisting of sodium-containing cathode materials. Statement 35. The sodium-containing cathode material is Na2V2O5, P2-Na 2 / 3 Fe 1 / 2 Mn 1 / 2 O2, Na3V2(PO4)3, NaMn 1 / 3 Co 1 / 3 Ni 1 / 3 PO4, and Na 2 / 3 Fe 1 / 2 Mn 1 / 2 35. The apparatus of claim 34, wherein the O2@graphene composite is selected from the group consisting of: Statement 36. The cathode (e.g., magnesium ion conducting, magnesium-containing cathode) is doped with magnesium oxide (e.g., Mg 1+x 30. The device of claim 29, comprising a material selected from the group consisting of (Al,Ti)2(PO4)6 (wherein x is 4 or 5), NASICON-type magnesium ion conducting materials, etc. Statement 37. The device of any one of statements 24-36, wherein the anode comprises a material selected from the group consisting of silicon-containing materials (e.g., silicon, silicon / carbon, etc.), tin and its alloys (e.g., tin / cobalt alloys, etc.), tin / carbon, and phosphorus. Statement 38. The device of any one of statements 24-27 and 31-33, wherein the anode (e.g., lithium ion conducting anode and lithium-containing anode) comprises a material selected from the group consisting of lithium ion conducting anode materials. Statement 39. Lithium ion conductive anode materials include lithium carbide, Li6C, and lithium titanate (LTO) (e.g., Li4Ti 15 O 12 The device of statement 38, wherein the lithium-containing material is selected from the group consisting of: Statement 40. The device of Statement 38, wherein the anode is lithium metal. Statement 41. The anode (e.g., sodium-containing and sodium-ion conducting anodes) is made of a material selected from the group consisting of sodium-ion conducting anode materials. The device according to any one of statements 24 to 26, 28, 34, and 35, comprising: Statement 42. The sodium-containing anode material is Na2C8H4O4 and Na 0.66 Li 0.22 Ti 0.78 The device of statement 41, selected from the group consisting of O4. Statement 43. The apparatus of statement 41, wherein the anode is sodium metal. Statement 44. The device of any one of statements 24-26, 29, and 36, wherein the anode is a magnesium-containing anode material. Statement 45. The apparatus of Statement 44, wherein the anode is magnesium metal. Statement 46. The device of any one of statements 24 to 45, wherein the hybrid electrode, the cathode, the anode, and the optional current collector form a cell, and the battery comprises a plurality of cells, each adjacent pair of cells being separated by a bipolar plate. Statement 47. The device of any one of statements 23-46, which is a conventional ionically conductive battery with a liquid electrolyte (e.g., as a base electrolyte), wherein the battery comprises an inorganic SSE disclosed herein or a solid hybrid electrolyte disclosed herein and a liquid electrolyte (e.g., a liquid electrolyte used in a conventional battery), wherein the liquid electrolyte is not present as a component of the solid hybrid electrolyte, and wherein the inorganic SSE material or the solid hybrid electrolyte is a separator in the conventional battery. Statement 48. The apparatus of statement 47, wherein the inorganic SSE is a F / S SSE disclosed herein (e.g., a templating inorganic SSE or an electrospun inorganic SSE). Statement 49. A method of making a hybrid electrolyte (e.g., a solid hybrid electrolyte) (e.g., a hybrid electrolyte according to any one of statements 1-22), comprising: contacting the template with one or more SSE material precursors; reacting (e.g., by heating) the SSE material precursor to form a solid inorganic material (e.g., including at least a portion or all of the reacted and / or decomposed SSE material precursor); heat treating (e.g., sintering and / or calcining) the template with a solid inorganic material, whereby the template is removed (e.g., by combustion as carbon dioxide) and an inorganic SSE (e.g., a monolithic SSE or a mesoporous or F / S SSE) is formed; contacting (e.g., infiltrating) the calcined template with a polymeric material; Including, A method in which, in the case of a monolithic SSE or mesoporous body, a layer is formed on an inorganic SSE material (and optionally filling at least some or all of the pores exposed on the surface of the inorganic SSE material), or, in the case of a F / S SSE, a polymeric material fills at least some or all of the pores of the F / S SSE (e.g., pores corresponding to the template). Statement 50. The method of statement 49, wherein the SSE material precursor is a sol-gel precursor or a metal salt. Statement 51. The method of statements 49 or 50, wherein the template is a carbon template (e.g., a fiber template) or a biomaterial template (e.g., a wood or plant template).

[0101] The following examples are presented as illustrations of the present disclosure and are not intended to be limiting in any way. EXAMPLES

[0102] This example provides a description of the solid hybrid electrolytes of the present disclosure and provides examples of the fabrication and characterization of such electrolytes.

[0103] Reducing the interfacial resistance of hybrid polymer / garnet-type electrolyte systems for lithium metal batteries Garnet-type solid electrolytes have been developed due to their high ionic conductivity (10 -4 S / cm~10 -3 S / cm) and a wide electrochemical stability window (0–6 V vs Li + / Li) have revealed promising results for Li-metal batteries. One of the major challenges of garnet-type solid electrolytes is the high interfacial resistance between the electrolyte and the electrode. This example shows the formation of a solid Li7La between two gel polymer electrolyte layers that reduces the interfacial resistance and protects against dendrite penetration in lithium-metal symmetric cells. 2.75 Ca 0.25 Zr 1.75 Nb 0.25 O 12 A hybrid electrolyte containing a garnet-type electrolyte (LLCZN) is described. The gel polymer electrolyte layer forms a favorable interface between the garnet solid-state electrolyte (SSE) and the electrode with low interfacial resistance and long-term electrochemical stability. The hybrid gel polymer and LLCZN electrolyte achieves a resistivity of 248 Ω×cm at the SSE / cathode interface. 2 Before and after, 214 Ω×cm at the SSE / Li metal interface 2A low interfacial charge transfer resistance is achieved between the front and rear. As a distinct advantage of this design, the hybrid electrolyte can prevent the formation of lithium dendrites due to the dense LLCZN garnet layer. Our results show that the hybrid symmetric cell can operate with stable stripping and plating profiles over long cycle periods. This hybrid electrolyte can also be used for Li metal batteries with low overpotential and high reliability against dendrite shorting. The hybrid electrolyte design with gel-polymer interfacial layer is an interesting surface engineering solution that is effective against garnet-solid interfacial resistance and demonstrates high performance safe Li metal batteries.

[0104] The proposed hybrid electrolyte with gel polymer electrolyte as an interface layer between LLCZN garnet SSE reduces the interfacial resistance and demonstrates a Li metal complete cell that can operate at room temperature. Figure 1a is a schematic diagram of the solid polymer-Li metal battery design with polymer / garnet SSE hybrid electrolyte. In this battery, the interface resistance is reduced by using gel polymer as an interface layer between the garnet SSE and the electrode. The gel polymer electrolyte can help to reduce the garnet SSE interfacial resistance to the cathode and Li metal by increasing the contact between the garnet SSE and the electrode (Figure 1b). The gel polymer electrolyte used in this work is a combination of a porous PVdF-HFP polymer matrix and a limited amount of liquid electrolyte stored inside the polymer. The gel polymer prepared by known techniques has good ionic conductivity (5 × 10 -4 S / cm) at 0 to 4.5 V vs. Li + / Li, making it suitable for most commercially used cathode materials. Due to the hybrid design with a gel polymer electrolyte at the interface between the garnet-type SSE and the active electrode, the interfacial resistance is 248 Ω × cm for the cathode interface. 2 , 214 Ω×cm for the Li metal anode interface 2Our results show that the hybrid symmetric cell can operate with stable stripping and plating profiles and low overpotentials for up to 15 hours, indicating a stable interface between the garnet-type SSE and the metallic Li anode. Since the gel polymer interlayer stores a minimal amount of liquid electrolyte, the hybrid electrolyte does not leak like conventional liquid electrolyte-based batteries. The hybrid electrolyte design with the gel polymer interfacial layer is considered as an important surface engineering strategy to reduce the overall interfacial resistance to the electrodes, including both the cathode and the Li metal anode in the electrochemical cell, as well as to demonstrate high-performance safe Li metal batteries.

[0105] Results and Discussion Characterization of hybrid electrolytes The characterization of garnet-type SSEs and gel polymer electrolytes is described herein. Cross-sectional scanning electron microscope (SEM) images of the net-type LLCZN pallets were obtained, which shows a total thickness of approximately 450 μm, which is consistent between samples in these trials. The surface of the garnet pallets is not smooth, which results in poor contact to the electrode layer. Enlarged cross-sectional SEM images of the garnet-type LLCZN pallets were examined, which have micrograins as a result of the 12-hour high-temperature sintering during the synthesis process. The dense structure of the garnet-type SSEs prevents lithium metal dendrites from penetrating the electrolyte during cycling. SEM images of the PVdF-HFP polymer matrix were obtained. The porous structure of the matrix adequately absorbs and contains additional liquid electrolyte. X-ray diffraction (XRD) was performed on the garnet-type LLCZN pallets, which shows that the cubic phase garnet-type Li5La3Nb2O 12The results are in good agreement with standard XRD plots of the LLCZN pallets, indicating that the LLCZN pallets have a cubic garnet phase with higher Li-ion conductivity compared to the tetragonal garnet phase. Electrochemical impedance spectroscopy (EIS) was performed on two LLCZN pallets with thicknesses of 1000 μm and 150 μm, tested in symmetric cells with gold deposited on both sides. The semicircles in the high frequency part of the impedance spectroscopy curves represent the bulk and grain boundary resistances of LLCZN. The LLCZN pallets with different thicknesses have a cubic garnet phase with higher Li-ion conductivity compared to the tetragonal garnet phase. -4 They have the same bulk conductivity of around S / cm. The formula is σ=R -1 LS -1 The conductivity was calculated using the formula: where R is the resistance, L is the thickness of the LLCZN pallet, and S is the area of ​​the electrode. The bulk areal resistivity (ASR) of the 450 μm thick LLCZN pallet is 225 Ω×cm 2 , which is within the acceptable range for batteries. This means that the internal resistance of the garnet-type SSE is relatively small, and the interface between the SSE and the electrode mainly contributes to the resistance of the solid-state battery. Therefore, as long as the interface resistance can be reduced to the same level as the internal resistance, the solid electrolyte can have a resistance small enough for battery use. Cyclic voltammetry (CV) was performed by the Li|polymer|Ti system. The steep peaks at -0.3 V and 0.3 V correspond to the plating and stripping of lithium, and there are no peaks in the higher voltage range. The flatness of the CV curve in the voltage range from 0.5 V to 4.5 V indicates that the gel polymer electrolyte is electrochemically stable up to 4.5 V. In addition, the garnet-type LLZO exhibits a low resistance at 0 to 6 V vs. Li + Because the hybrid electrolyte design is electrochemically stable at 0-4.5 V vs. Li + The hybrid electrolyte is stable over a voltage range of 100000000000000001 / Li. This stable voltage range makes the hybrid electrolyte suitable for lithium metal designs with many cathode materials. The area specific resistance and ionic conductivity of the 40 μm thick gel polymer are approximately 8 Ω×cm from the EIS plot of a simple symmetric cell with a stainless steel plate. 2 and 5×10 -4S / cm. This flexible and highly ionically conductive gel polymer can improve the contact between the SSE and the electrode, resulting in low interfacial resistance.

[0106] Analysis of the interfacial impedance of hybrid electrolytes The impedance analysis of the symmetric cell with garnet-polymer hybrid electrolyte is shown in Figure 2. Figure 2a shows the impedance profile of a cathode|polymer|cathode symmetric cell. The bulk resistance of this cell is small because the gel polymer layer is thin and conductive. The mid-frequency semicircle has a resistance of approximately 107 Ω×cm on each side. 2 Charge transfer resistance (R ct ) This value is calculated by equivalent circuit simulation. R ct represents the dynamic hindrance of charge transfer between the cathode material and the gel polymer, and R ct The small R means that the gel polymer and the cathode have good interfacial contact. The long tail in the low frequency part corresponds to the diffusion impedance in the cathode. Figure 2b shows the impedance profile of the stainless steel (SS)|polymer|SSE|polymer|SS symmetric cell, which shows the bulk and grain boundary impedance of the garnet-type SSE at high frequencies, the interfacial R in the mid-frequency range, and the impedance of the SS|polymer|SSE at high frequencies. ct The impedance plot of the gel polymer shows that the R between the gel polymer and the SS is ct is approximately zero since no corresponding semicircle appears in the impedance plot. Therefore, R for the SS|polymer|SSE|polymer|SS symmetric cell ct All of the R at the polymer|SSE interface is c t is approximately 155 Ω × cm for each side, as calculated from the corresponding fitting results in Figure 5b. 2 This resistance is calculated by the R ct, which means that the polymer|SSE interface and the cathode|polymer interface have similar contact performance. Figure 2c is the EIS plot of the cathode|polymer|SSE|polymer|cathode symmetric cell. The impedance curve combines three parts. The high frequency part is the bulk and grain boundary impedance of the garnet-type SSE itself. The mid frequency part is the R of the polymer|SSE interface and the cathode|polymer interface because the resistance of the gel polymer layer itself is relatively much smaller. ct Including the interface R between the garnet-type SSE and the cathode, ct The low frequency part is a straight line, which corresponds to the diffusion impedance of the cathode. The total interface R of the cathode symmetric cell is ct is 248 Ω x cm for each side 2 This value was obtained by equivalent circuit fitting. The interface R of the cathode|polymer|SSE|polymer|cathode symmetric cell ct is the polymer|cathode interface R ct and polymer|SSE interface R ct , and the impedance of all three interfaces appears in the mid-frequency range. This means that the impedance of the cathode|polymer|SSE interface is the sum of the polymer|cathode and polymer|SSE interface impedances. As a comparison of the symmetric cells with and without the gel polymer interfacial layer, Figure 5a is an EIS plot of the cathode|SSE|cathode symmetric cell without any interfacial modification. The symmetric cell was constructed by direct brushing of the cathode slurry on the garnet-type SSE surface and subsequent drying. This is the sum of the R of the cathode|SSE|cathode symmetric cell without the polymer interfacial layer. ct is approximately 1×10 6 Ω×cm 2 This large resistance is evidence of poor contact between the SSE and the LiFePO4 cathode material. This problem can be solved by a hybrid design of gel polymer layer between the garnet-type SSE and the cathode.

[0107] Figure 2d shows the impedance curve of the Li|polymer|Li symmetric cell. The intersection of the impedance curve with the Z' axis is 6.4 Ω×cm 2 , which is the bulk resistance of the gel polymer. The diameter of the semicircle is 180 Ω × cm 2 which is the R of the two polymer|Li interfaces on either side of the symmetric cell. ct Therefore, the interface resistance of one polymer|Li interface is 90 Ω×cm 2 , which is close to the polymer|cathode interface resistance. This means that the contact between the gel polymer and Li metal is as good as that between the gel polymer and the cathode, and the surface of the Li metal electrode is also well wetted by the gel polymer. Figure 2e shows the EIS plot of the Li|polymer|SSE|polymer|Li symmetric cell, which includes four parts. The high frequency part is the bulk resistance and grain boundary resistance of the garnet-type SSE. The mid frequency part is the interface resistance between the garnet-type SSE and Li metal, which mainly comes from the impedance of the polymer|SSE interface and the polymer|Li interface, since the impedance of the gel polymer layer itself is rather small. ct From the corresponding equivalent circuit fitting results herein, the total interfacial area R on one interface of the Li|polymer|SSE|polymer|Li symmetric cell is ct is 214Ω×cm 2 Figure 5b shows that the total resistance of the Li|SSE|Li symmetric cell without interface modification is approximately 1400 Ω×cm 2 Metallic lithium is melted and coats both sides of the garnet-type SSE. The reason for the lower resistance compared to the cathode|SSE|cathode symmetric cell in Figure 5a is that the melted lithium metal provides improved surface contact compared to solid cathode powder and binder. However, the resistance is only 1400 Ω×cm 2 The interfacial resistance of is still too large for battery use. This can be reduced by a gel polymer interfacial layer. In conclusion, the gel interfacial layer can reduce the interfacial resistance R between the LLCZN solid electrolyte and the electrode, including many cathode materials and Li metal anodes. ctcan be significantly reduced. Figure 2f compares the interfacial resistance of the Li|SSE|Li and cathode|SSE|cathode symmetric cells with and without the gel-polymer interface. It clearly shows that the gel interface can reduce the interfacial resistance to an acceptable range. After the application of the gel-polymer interface, the cathode and the garnet-type The interface resistance between the SSE is 6×10 4 Ω×cm 2 to 248 Ω×cm 2 After application of the gel polymer interface, the interfacial resistance between the Li metal anode and the garnet-type SSE was reduced to 1400 Ω×cm 2 to 214Ω×cm 2 It dropped to.

[0108] FIG. 3 analyzes the impedances identified for each interface in a symmetric cell with and without a gel-polymer interface. The impedance analysis of the cathode|polymer|SSE|polymer|cathode symmetric cell comes from FIG. 2a-c, while the impedance analysis of the cathode|SSE|cathode symmetric cell without a gel-polymer interface is shown in FIG. 5a. The corresponding equivalent circuits are described herein. In each equivalent circuit, for one interface impedance, there is one parallel connection between a resistor and a capacitor / constant phase element (CPE). The capacitor / CPE is for the double layer capacitance on the interface, and the resistor is for the charge transfer resistance on the interface. The total interface R of the cathode|polymer|SSE|polymer|cathode symmetric cell is ct is 496Ω×cm 2 and the interface R of the cathode|SSE|cathode symmetric cell without a gel polymer interface ct (1.3×10 5 Ω×cm 2), which is much smaller than the total interfacial resistance R of the Li|polymer|SSE|polymer|Li symmetric cell. This reduction in resistance means that the gel-polymer interface can significantly improve the contact performance between the cathode and the SSE. The impedance analysis of the Li|polymer|SSE|polymer|Li symmetric cell comes from the analysis of Figures 2b, 2d, and 2e, and the impedance analysis of the Li|SSE|Li symmetric cell without the gel-polymer interface comes from Figure 5b, which compares the impedance of the Li|SSE|Li symmetric cell with and without the gel-polymer interface. The corresponding equivalent circuit is described herein. The total interfacial resistance R of the Li|polymer|SSE|polymer|Li symmetric cell ct is 428Ω×cm 2 The interface R of the Li|SSE|Li symmetric cell without interface modification ct (2800Ω×cm 2 ), which is much smaller than that of the gel-polymer interface. This reduction in resistance means that the gel-polymer interface can significantly improve the contact performance between Li and the SSE.

[0109] Electrochemical performance of hybrid solid polymer electrolytes The electrochemical performance of the lithium symmetric cell with the polymer / garnet-type SSE hybrid electrolyte and the completed cell are shown in Figure 4. Figure 4a shows the DC cycling voltage profile of the Li|SSE|Li symmetric cell with the gel polymer interfacial layer under galvanostatic cycling. The total DC ASR of the symmetric cell is 1400 Ω×cm. 2 This means that the voltage value of 180 mV corresponds to a surface current density of 125 μA / cm 2The inset in Fig. 4a shows that the DC resistance remains constant for one cycle. This DC resistance comes from the bulk and grain boundary resistance of the SSE and the resistance of the SSE|polymer|Li interface, so the interfacial resistance remains constant for one cycle. The voltage drops from 180 mV to 160 mV in the first 5 h due to the improved interfacial contact between the lithium and the gel polymer electrolyte caused by lithium stripping and plating. After 5 h, the voltage remains constant, the interfacial resistance also remains constant, and the interface is stable. Figure 4b shows the EIS plots of the cell before and after cycling for 15 h. During cycling, the interfacial ASR remains almost constant, at 1000 Ω×cm. 2 to 1100Ω×cm 2 This means that the gel-polymer interface was stable and maintained a small resistance for a long period of time.

[0110] Figures 4c-e show the cycling performance of a completed cell with a polymer / garnet-type SSE hybrid electrolyte. The cell achieved a current of 65 μA / cm over 130 cycles. 2 and 1C rate (170 mA / g). Figure 4c shows the charge-discharge profiles for the 1st, 10th, 50th, 100th, and 130th cycles. The charge-discharge curves show a stable voltage plateau, and the overpotential of the cycles is consistent, which means that the interfacial resistance is constant during the 130 charge-discharge cycles. Figure 4d shows the discharge capacity and coulombic efficiency for each cycle, and the coulombic efficiency is approximately 95% for each cycle after the second. The low coulombic efficiency for the first cycle is due to the formation of an SEI layer between the electrode and the gel during this first cycle. The discharge capacity is stable at 50-55 mAh / g over 130 cycles. The stable discharge capacity indicates that the interfacial layer is stable over long cycles. The reason for the small specific capacity may be that most of the liquid electrolyte is inside the gel and only a small amount is inside the cathode material, so not all of the cathode material is wetted by the gel and not all of it is active in the reaction. However, the discharge capacity of the battery has good stability over time, as the interfacial layer is chemically stable. Figure 4e shows the EIS plots of the battery before cycling, after 20 cycles, and after 130 cycles. R, shown as the diameter of a semicircle in the mid-frequency range, is ct is approximately 500Ω×cm 2 The impedance of the gel polymer electrolyte is very stable and can maintain a small charge transfer resistance over 130 cycles. In conclusion, the hybrid polymer / garnet electrolyte can be used in Li metal complete cells with small overpotential and good stability.

[0111] This example demonstrates that instead of pure SSE, polymer / garnet hybrid electrolyte can be used in a good solid-state polymer battery design to reduce the interfacial resistance between the garnet-type SSE and the electrodes. The gel polymer electrolyte has high ionic conductivity and a wide electrochemically stable potential window. Therefore, it can be used as an interfacial layer between the LLZCN garnet SSE and the electrodes to provide an electrochemically stable ionically conductive interface. The R between the SSE with gel polymer interfacial layer and the electrodes can be reduced. ct has a resistance of 248 Ω×cm to the cathode as measured by impedance spectroscopy on symmetric and completed cells. 2 , 214 Ω×cm for Li metal anode 2This interfacial resistance is within the acceptable range for commercial lithium metal cell production. A Li metal symmetric cell with a polymer / garnet-type SSE hybrid electrolyte was demonstrated and cycled for over 15 hours with a stable voltage profile. This indicates that the gel polymer interface between the Li metal anode and the garnet-type SSE is electrochemically stable. A battery was realized and cycled 130 times at room temperature with a Li metal anode, LiFePO4 cathode, and polymer / garnet hybrid electrolyte. During cycling, the interfacial R of the completed cell was 1.2 μm. ct was constant, which means that the gel polymer electrolyte can form a stable interface between the LLCZN garnet electrolyte and the lithium iron phosphate electrode. Overall, this study demonstrated a new hybrid garnet polymer electrolyte, a combination of a pure solid electrolyte coated with two gel polymer layers on both sides. The performance without the gel polymer layer and the resistivity of 6 × 10 Ω × cm 2 After application of the gel-polymer interface, the total interfacial resistance at room temperature is lower (approximately 500 Ω×cm) compared to the total interfacial resistance of 2 ).

[0112] experiment LLCZN Palette Synthesis Garnet type Li7La 2.75 Ca 0.25 Zr 1.75 Nb 0.25 O 12 The powders were synthesized by the sol-gel method. The precursors LiNO3 (99%, Alfa Aesar), La(NO3)3·6H2O (99%, Alfa Aesar), Ca(NO3)2·4H2O (99.9%, Sigma Aldrich), NbCl5 (99%, Alfa Aesar), and zirconium(IV) propoxide (70 wt% in 1-propanol, Sigma Aldrich) were dissolved in stoichiometric amounts in ethanol containing 10 wt% excess LiNO3, the solution was stirred until clear, and then pure acetic acid was added in a 1:4 volume ratio to the solution. The ethanol solvent was evaporated at 100 °C to obtain a gel precursor. The gel was heated at 350 °C to obtain a dry precursor powder, which was then heated at 800 °C for 10 h to obtain the garnet powder. The powder was ball milled for 48 h and then pressed into a cylindrical pallet. The pallet had an area of ​​0.5 cm. 2 The pellets were then sintered at 1150°C for 12 hours. The synthesized pellets were polished with sandpaper to thin them to 400-450 μm and washed with isopropyl alcohol (IPA).

[0113] Synthesis of PVDF-HFP-based gel polymer electrolytes A PVDF-HFP-based gel polymer electrolyte was prepared by the following method. First, 0.25 g of PVDF-HFP (Sigma Aldrich) was dissolved in a mixture of 4.5 g of acetone and 0.25 g of ethanol under mechanical stirring for 1 h to obtain a homogeneous solution. Then, the solution was cast onto a flat aluminum foil and the solvent was evaporated in a constant humidity chamber at 80% humidity and 25 °C. The sample was dried under vacuum at 60 °C for 5 h. After that, a homogeneous free-standing membrane was obtained. The thickness of the PVDF-HFP membrane is around 40 μm. Second, the prepared porous PVDF-HFP membrane was placed on a 0.2 cm2 sieve. 2 The films were cut into small circular films of 0.01 mm and immersed in 1 M LiPF6 in 1:1 ethylene carbonate (EC):diethyl carbonate (DEC) liquid electrolyte for 1 min to ensure complete immersion in the electrolyte, and excess liquid on the surface of the films was removed with a wiper.

[0114] Materials characterization The D8 Advanced was used with a CuKα radiation source operating at 40 kV and 40 mA. Phase analysis of the LLCZN garnet pallets was performed by X-ray diffraction (XRD) on a with LynxEye and SolX (Bruker AXS, WI, USA). The microstructural morphology of the fabricated LLCZN garnet pallets and PVDF-HFP membranes was investigated by a field emission scanning electron microscope (FE-SEM, JEOL 2100F).

[0115] Electrochemical testing of battery construction The interfacial impedance was measured for both the Li|SSE interface and the LiFePO4 cathode|SSE interface. 2 The lithium metal electrodes were press-cut into circular disks with a thickness of 0.5 mm. To prepare the cathode, LiFePO4, carbon black, and polyvinylidene difluoride (PVDF) were dissolved in N-methyl-2-pyrrolidone (NMP) in a mass ratio of 3:2:1 and mixed to form a slurry. The slurry was coated onto aluminum foil and then dried in an oven at 100 °C for 12 hours. After drying, the cathode was cut into a 0.2 cm2 area. 2 The electrodes were cut into circular disks of 0.01 mm diameter and immersed in 1M LiPF6 in 1:1 ethylene carbonate (EC):diethyl carbonate (DEC) liquid electrolyte before testing to remove excess liquid electrolyte. The cells were assembled and electrochemically tested in an argon-filled glove box. Cyclic voltammetry (CV) of the Li|gel polymer|Ti cells was tested at a voltage range of -0.3 V to 4.5 V and a scan rate of 1 mV / s. Symmetric cells were also fabricated for EIS testing. The schematic diagram of the cell for each test is shown in the corresponding EIS plot. With one stainless steel pallet placed on each side of the cell, clips pressed the electrodes, gel membrane, and garnet pallet together in sequence. The electrochemical performance of the cells was tested by a Bio-Logic tester. The EIS tests of the symmetric cells were performed at a voltage amplitude of 10 mV and a frequency range of 0.1 Hz to 1 MHz. Galvanostatic cycling of Li|SSE|Li with a gel interface layer was performed at a current density of 0.125 mA / cm using the same assembly method as in the EIS tests. 2Cycling was performed at 4000 V for 10 min. EIS measurements of the cells before and after 15 h cycling were compared. The garnet, gel, and electrolyte layers were pressed together to create a Li|SSE|LiFePO4 complete cell with a gel-polymer interface in a CR2016 coin cell and sealed with epoxy. The cell was cycled at 50 μA / cm over a voltage range of 2 V to 4.5 V. 2 The cells were cycled at a constant current of 0.05 V and the EIS of the cells was measured before and after cycling.

[0116] A lithium metal battery system was investigated. The bulk resistance of the 40 μm thick gel polymer layer was 7 Ω×cm. 2 FIG. 5 shows the impedance of electrode|SSE|electrode symmetric cells without a gel polymer interface, (a) EIS of cathode|SSE|cathode symmetric cell, (b) EIS of Li|SSE|Li symmetric cell. EXAMPLES

[0117] This example provides a description of the solid hybrid electrolytes of the present disclosure and provides examples of the construction and characterization of such electrolytes.

[0118] A solid ionically conductive framework to prevent chemical and physical shorts in Li-metal batteries Chemical and physical short circuits, associated with soluble material migration and Li dendrite penetration, are two key challenges in Li metal batteries that lead to limited battery cycle life and thermal runaway. To address these challenges, this example describes a solid-state hybrid electrolyte system consisting of a structural garnet-type solid electrolyte (SSE) and a liquid electrolyte. The hybrid electrolyte utilizes a regular liquid electrolyte to maintain high ion migration kinetics in the electrode, and employs the SSE to not only separate the electrode and liquid electrolyte, but also to prevent the diffusion of unwanted species and Li dendrites. This example explores the chemical properties of the garnet SSE and its electrochemical stability in sulfur, polysulfide, and liquid electrolytes, and demonstrates the formation of a continuous Li-ion hybrid electrolyte in the porous layer of a high sulfur loading cathode. +The study describes the development of a bilayered garnet SSE framework for hybrid Li-S batteries with an electronic pathway and dense layers that block polysulfide diffusion and dendrite penetration. Based on the completed cell level, the study demonstrates an integrated sulfur loading of 7 mg / cm. 2 It has been shown that the energy density can exceed 280Wh / kg. The initial coulombic efficiency is as high as 99.8%, and no chemical or physical short circuits were observed in the hybrid system. This bilayer hybrid configuration is expected to improve Li-S batteries, and the design is expected to be extended to other cathode materials such as high voltage cathodes (LNMO) and air / O2 cathodes, paving the way for the transition from conventional to all-solid-state batteries.

[0119] The chemical properties of garnet SSEs and their electrochemical stability in sulfur, polysulfide, and liquid electrolytes are investigated, and continuous Li in the porous layer of high sulfur loaded cathodes is investigated. + We developed a bilayer garnet SSE framework for hybrid Li-S batteries with a ZnO / electron pathway and a dense layer that blocks polysulfide diffusion and dendrite formation. Compared with conventional battery configurations, the solid-state hybrid battery can increase the cathode mass loading, trap liquid electrolyte, and release the cathode volume change, as well as prevent chemical and physical short circuits. A schematic diagram of the bilayer hybrid Li-S battery is shown in Figure 6. In the bilayer SSE, the porous garnet layer is thicker, so the supporting dense layer can be thinned to a few micrometers, contributing to a small electrolyte impedance. As the bilayer SSE directly encapsulates the active materials in the pores, these pores can be adjusted to accommodate the volume change of the active materials to keep the battery structure stable during cycling. An integrated sulfur cathode loading of 7 mg / cm 2Over the past few years, the proposed hybrid Li-S battery has shown high initial coulombic efficiency (>99.8%) and high coulombic efficiency (>99%) for each subsequent cycle, and no chemical or physical short circuit was observed in the hybrid system. This bilayer SSE represents a promising approach to revolutionize Li-S batteries. This structural hybrid electrolyte design with high surface reaction sites for the cathode and a blocking layer for the Li anode can also be expected to pave the way for the transition from conventional to all-solid-state batteries using other cathode materials such as high-voltage cathodes (LNMO) and air / O2 cathodes.

[0120] Characterization of garnet solid electrolytes The porous structures were fabricated by tape casting using LLCZN powder slurry containing poly(methyl methacrylate) (PMMA) spheres in the tape as sacrificial pore formers. The bilayer garnet SSE was fabricated by laminating the porous tape to a dense tape and then removing the organic polymer by co-sintering. Details of the fabrication can be found in the present specification. Figure 7a shows a photographic image of the bilayer garnet SSE. It has adequate mechanical strength for manual handling and stacking together in series to obtain high voltage cells. Unlike sulfide type superionic conductors, which are sensitive to air and moisture, the garnet SSE is much more chemically stable in dry air and can be handled in a dry room environment. A schematic diagram of the bilayer garnet SSE structure is shown in Figure 7. The porous structure was placed on the dense layer, so that it is possible to fabricate ultra-thin high-temperature cells. The mechanical strength of the dense layer can be improved. Further encapsulation of the cathode material by these pores results in an integral structure of the cathode and electrolyte. Figure 7b is a top view of a scanning electron microscope (SEM) image of the porous layer. The micro-sized pores are uniformly distributed, and the electrode slurry can easily reach the internal structure. Cross sections of the bilayer garnet SSE are shown in Figures 7c-7e. The garnet powder was sintered into a 3D network with a porosity of about 70%. Figure 7d shows the connection of the porous and dense layers, which are sufficiently sintered that no delamination is observed. The dense garnet layer in Figure 7e shows that the large garnet grains form a dense microstructure, which can prevent soluble active materials and liquid electrolyte from passing through the solid electrolyte. Figure 7f is a cross section of the bilayer garnet with a total thickness of 105 μm, including a dense section of 35 μm and a porous section of 70 μm.

[0121] The phase of the sintered garnet SSE was confirmed by X-ray diffraction (XRD). 2.75 Ca 0.25 Zr 1.75 Nb 0.25 O 12 The synthesized garnet SSE based on (LLCZNO) exhibits a cubic structure. All peaks correspond to those of the standard cubic garnet Li5La3Nb2O 12The Raman spectrum is in good agreement with that of the garnet spectrum reported elsewhere, where broad and partially overlapping bands confirm the cubic phase of LLCZNO garnet. The ionic conductivity was measured by electrochemical impedance spectroscopy (EIS) using a blocking cell setup. A dense garnet pellet was used in a symmetric Au / garnet SSE / Au blocking cell configuration. EIS of the garnet SSE was measured in the temperature range 25°C–50°C (Fig. 11). The intercept of the real axis at high frequencies is assigned to the bulk resistance of the garnet SSE, and the concave semicircles are associated with the grain boundaries of the garnet SSE. The low frequency intercept, which corresponds to the capacitive behavior of the Au electrode, was used to calculate the total resistance, including the bulk and grain boundary contributions. The ionic conductivity was calculated using σ=L / (Z×A), where Z is the impedance of the real axis in the Nyquist plot, L is the garnet ceramic disk length, and A is the surface area. The log ionic conductivity of the garnet SSE versus the inverse temperature is plotted in Figure 12. By using the Arrhenius equation, an activation energy of 0.35 eV was calculated from the conductivity as a function of temperature.

[0122] Chemical stability of liquid-solid hybrid electrolyte systems Experiments were performed to understand the compatibility of garnet SSEs with liquid Li-S chemistry by immersing the garnet SSEs in lithium polysulfide solution (Li2S8 dissolved in DME / DOL) and liquid electrolyte (LiTFSI in DME / DOL) to study their surface composition and phase structure. The surfaces of the garnet pellets were cleaned with sandpaper to remove Li2CO3 and then immersed in the liquid electrolyte or lithium polysulfide solution for one week. After immersion in the solutions, the garnet SSEs were washed with DME / DOL solvent, dried and characterized separately. The transfer of the samples was done in a protective environment to avoid oxygen and moisture contamination. After immersion of the garnet pellets in Li2S8 / DME / DOL for one week, X-ray photoelectron spectroscopy (XPS) analysis revealed that the ion-excited ions on the garnet surface were observed to be 100%.

number

number

number

[0123] Electrochemical characterization of hybrid liquid-solid electrolytes The structure and chemistry of the interface between the SSE and the electrode are the main challenges for solid electrolytes. Recent studies have shown that poor contact at the interface is the main factor leading to the large interfacial resistance of garnet SSEs with Li. Introducing a liquid phase between the solid electrolyte and the electrode using a liquid electrolyte interlayer should be an effective way to suppress the respective interfacial resistance. As part of this study, the interfacial modification of garnet SSEs with Li metal is focused on. Figure 9a is a schematic diagram of the dense surface of garnet SSE. Individual pores are distributed on the garnet surface, and these cavities limit the surface area of ​​garnet with Li metal (Figure 9b). Moreover, the undulating and rigid garnet surface leads to poor conformal contact with Li metal and high interfacial resistance. In Figure 9c, a polymer gel-like layer is designed to conformally coat the garnet SSE surface. Not only can this layer absorb the liquid electrolyte, but the elastic interlayer can ensure the intimate contact between the garnet SSE and lithium metal. Figure 9d shows the cross section of the polymer-coated garnet SSE. Polyethylene oxide (PEO) polymer was deposited on the garnet SSE surface by spin coating. The PEO has a thickness of 2 μm and conformally covers the garnet SSE (Figure 8e). This elastic polymer layer can compensate for the undulations of the garnet and Li metal and ensure a uniform Li-ion flux through the interface. The Nyquist plot of electrochemical impedance spectroscopy (EIS) measurements shows that the total impedance is about 900 Ω cm. 2 This shows that (Figure 9e).

[0124] The stability of the interface was characterized by mimicking the operating conditions of a real lithium metal battery through galvanostatic plating and stripping of Li ions in a symmetric cell by applying a constant current of 0.3 mA / cm. Figure 8f shows the interfacial stability.2 Figure 1 shows the voltage profile as a function of time for a Li / hybrid SSE / Li cell under a current of 1000 Ω cm. Positive voltage indicates Li stripping and negative voltage indicates Li plating. The cells were operated for 0.5 h per cycle. The cells initially showed a voltage of ±0.3 V, but after 10 h of cycling, the voltage gradually decreased to ±0.2 V. As a comparison, a Li / garnet / Li symmetric cell was also fabricated and tested. For the hybrid cell, the stripping / plating voltages remained relatively stable over the 160 h of cycling. The inset shows the initial cycles for the two cells and the 140 h cycle for the hybrid cell. High impedance and large polarization were observed. The non-smooth voltage plateau suggests a large interfacial resistance between Li and garnet. The hybrid cell showed a smooth voltage curve. The symmetric total resistance is calculated according to Ohm's law, where the resistance is calculated by dividing the voltage by the current, so the initial resistance was about 1000 Ω cm. 2 After that, the cell resistance is about 660 Ω cm 2 The voltage profile was maintained at 0.5 and 1.0 mA / cm in Fig. 8g and Fig. 8h, respectively, which is consistent with the EIS in Fig. 9. These direct current (DC) resistances are slightly higher than the alternating current (AC) resistances measured by EIS. The drop in resistance indicates that the resistance between the garnet and Li metal was improved by the gel electrolyte interlayer during repeated Li stripping and plating. The periodic variation of the voltage profile shows the temperature dependence of the solid hybrid electrolyte. 2 The voltage profile of the Li / hybrid SSE / Li cell under currents demonstrates the high current capacity of the hybrid electrolyte.

[0125] Electrochemical evaluation of hybrid Li-S batteries The electrochemical characterization of the solid hybrid electrolyte for Li-S battery is shown in Figure 10. In Figure 10a, the schematic diagrams of Li-S battery with conventional electrolyte and solid hybrid electrolyte are compared. Soluble polysulfides can diffuse through the porous polymer separator and migrate to the Li metal anode, but cannot penetrate the dense ceramic ion conductor, thus avoiding the polysulfide shuttle effect, side reactions on Li, and corrosion of Li metal. As shown in Figure 10b, the polysulfide shuttling behavior occurs in the charging process. The extended charging voltage plateau is a typical polysulfide shuttle effect, which causes a long charging time before reaching the upper cutoff voltage. The rapid capacity fade and low coulombic efficiency in conventional Li-S (Figure 13) make the use of solid hybrid configurations urgent. In the hybrid cell, the charging curve does not show the extended plateau, the capacity value is close to the discharge capacity, and the coulombic efficiency is close to 100%, resulting in stable cycling performance (Figure 14), demonstrating the absence of polysulfide shuttling in the solid hybrid electrolyte system.

[0126] Figure 10c shows the charge-discharge curves of the hybrid cell at different current densities. The hybrid cell was fabricated using dense garnet SSE and a slurry-cast sulfur cathode. The mass loading of sulfur was about 1.2 mg / cm. 2 A conventional liquid electrolyte (LiTFSI in DME / DOL) was used as the liquid electrolyte. No LiNO3 was added to the liquid electrolyte. At a current density of 200 mA / g, the sulfur cathode delivered a specific capacity of about 1000 mAh / g with a coulombic efficiency of about 100%. At a current density of 800 mA / g (1 mA / cm 2 At 1000 s, the specific capacity was 550 mAh / g, and the cell still maintained a high coulombic efficiency close to 100%. The rate performance is shown in Figure 10d. The hybrid cell showed good cycling stability at high current densities as well as good capacity retention at low currents.

[0127] Figure 10e is a schematic diagram of a solid-state hybrid bilayer Li-S battery. Sulfur is encapsulated in a thick porous layer, and the volume change of sulfur and its soluble polysulfides is proportional to the volume change of the solid garnet matrix. The sulfur was supported by directly fusing sulfur powder into the porous matrix at 160 °C. Prior to fusing the sulfur, carbon nanotubes (CNTs) were infiltrated into the porous garnet microstructure to set up an internal electronically conductive network (Figure 15). The cross section and elemental mapping (La in red and S in green) of the bilayer Li-S cathode are shown in Figure 10f. The elemental mapping image clearly shows the sulfur content in the garnet pores. The voids between the sulfur and garnet allow the liquid electrolyte to easily penetrate into the internal channels and wash the sulfur. Figure 10g shows the cross section of the bilayer Li-S cathode at a current density of 0.2 mA / cm. 2 The S mass loading in the 2 Figure 10 shows the charge-discharge voltage profiles of the hybrid bilayer Li-S cell with 1000 mAh / g. The first cycle discharge capacity is about 645 mAh / g with a coulombic efficiency of 99.8%, which is exceptionally high. The long and flat voltage plateau indicates the irreconcilable polarization between the charge-discharge curves. This should be attributed to the porous garnet SSEs, which provide more reaction sites with sulfur due to their large surface area, allowing for lower voltage polarization and better capacity. The cycling performance is shown in Figure 10h. No rapid capacity growth occurs in the first few cycles, indicating that no polysulfides are lost in the hybrid cell with such a high sulfur mass loading. The coulombic efficiency remains above 99%, confirming that the shuttle effect does not occur in the hybrid design. With a mass loading of 7.5 mg / cm, the cell is stable at 1000 mAh / g. 2The hybrid bilayer Li-S cell has an energy density of 280Wh / kg based on the cathode, Li anode, and electrolyte. The cycle performance is slightly degraded, which may be due to the fact that the charging products Li2S and Li2S2 were not reactivated in the subsequent cycles and the high mass loading of sulfur prevented further reactions inside the bulk sulfur loading. An electronic conductive network and increased sulfur distribution are highly desirable. In this example, the hybrid electrolyte and hybrid cell were investigated using solid sulfur as a model material, and it is expected that the use of catholyte with liquid polysulfides could be another approach for the bilayer porous dense design of garnet SSE.

[0128] In conclusion, we have disclosed the chemical properties of garnet SSEs and their electrochemical stability in sulfur, polysulfide, and liquid electrolytes, and have demonstrated the continuous Li-ionization in the porous layer of high sulfur-loaded cathodes. + We have developed a bilayered garnet SSE framework for hybrid Li-S batteries with a high density layer that prevents the diffusion of polysulfides and the penetration of dendrites as well as an electron pathway. Compared with conventional battery configurations, the solid-state hybrid battery not only prevents chemical and physical short circuits, but also allows for increased cathode mass loading, capture of liquid electrolyte, and release of cathode volume changes. As the bilayered SSEs directly encapsulate the active materials in the pores, these pores can adjust to accommodate the volume changes of the active materials to keep the battery structure stable during cycling. Our studies show that an integrated sulfur cathode loading of 7 mg / cm2 can be achieved. 2 Over the years, the proposed hybrid Li-S battery has shown high initial coulombic efficiency (>99.8%) and high coulombic efficiency (>99%) for each subsequent cycle, and no chemical or physical short circuit was observed in the hybrid system. This structural hybrid electrolyte is considered an improvement over Li-S batteries. This design is also expected to be extended to other cathode materials for high-performance batteries, such as high-voltage cathodes (LNMO) and air / O2 cathodes, paving the way for the transition from conventional to all-solid-state batteries.

[0129] LLCZN powder was synthesized by a modified sol-gel method. The starting materials were LiNO3 (99%, Alfa Aesar), La(NO3)3 (99.9%, Alfa Aesar), Ca(NO3)2 (99.9%, Sigma Aldrich), ZrO(NO3)2 (99.9%, Alfa Aesar), and NbCl5 (99.99%, Alfa Aesar). Stoichiometric amounts of these chemicals were dissolved in deionized water, and 10% excess LiNO3 was added to compensate for lithium volatilization during high-temperature pellet preparation. Citric acid and ethylene glycol (1:1 molar ratio) were added to the solution. The solution was evaporated at 120 °C for 12 h to produce a precursor gel, which was then calcined at 400 °C and 800 °C for 5 h to synthesize the garnet powder. The garnet powder was then uniaxially pressed into pellets. Then, it was covered with the same powder and sintered at 1050° C. for 12 hours.

[0130] Materials characterization The D8 Advanced was used with a CuKα radiation source operating at 40 kV and 40 mA. Phase analysis was performed by powder X-ray diffraction (XRD) on a LynxEye and SolX (Bruker AXS, WI, USA). The morphology of the samples was examined by field emission scanning electron microscopy (FE-SEM, JEOL 2100F).

[0131] Electrochemical characterization A Li|solid electrolyte|Li symmetric cell was fabricated and assembled in an argon-filled glove box. To measure the ionic conductivity of the garnet solid electrolyte, a dense ceramic disk was coated on both sides with Au paste to act as blocking electrodes. The gold electrodes were sintered at 700 °C to form good contact with the ceramic pellet. The cell was then assembled as a 2032 coin cell with a highly conductive carbon sponge. The carbon sponge acted as a buffer to prevent damage to the garnet ceramic disk. Battery test clips were used to hold and provide good contact with the coin cell. The edges of the cell were sealed with epoxy resin. EIS was performed over the frequency range of 1 MHz to 100 mHz with a perturbation amplitude of 50 mV. The conductivity was calculated using σ=L / (Z×A), where Z is the impedance on the real axis in the Nyquist plot, L is the garnet ceramic disk length, and A is the surface area. The activation energy was determined from the conductivity as a function of temperature by using the Arrhenius equation.

[0132] First principles calculation Using the same approach as defined in our previous work, the interface is considered as a pseudobinary system of Li2S / Li2S8 and garnet SSE. A phase diagram was constructed to identify possible thermodynamically favorable reactions. The energies of the materials used in our study were obtained from the Materials Project (MP) database, and the compositional phase diagram was constructed using the pymatgen package. The interaction energies of the pseudobinary system were calculated using the same approach as defined in our previous work.

[0133] Fabrication and evaluation of solid-state hybrid batteries All cells were assembled in an argon-filled glove box. The solid-state hybrid cells were assembled as 2032 coin cells. The sulfur electrode was made of 70% elemental sulfur powder (Sigma), 20% carbon black, and 10% polyvinylpyrrolidone in water (PVP, Sigma, M w=360,000) binder. The electrodes were dried in vacuum at 60 °C for 24 h. 1 M bis(trifluoromethane)sulfonimide lithium salt (LiTFSI, Sigma) in a mixture of dimethoxyethane (DME) and 1,3-dioxolane (DOL) (volume ratio 1:1) was used as the electrolyte for the solid-state hybrid Li-S battery. No LiNO3 was added. The electrolyte / sulfur mass ratio is about 10 ml / g on the cathode side. The cells were tested in 2032 coin cells. Galvanostatic charge-discharge tests were measured using a cutoff voltage window of 1-3.5 V. To fabricate the bilayer cathode, elemental sulfur powder was uniformly dispersed on the porous garnet and heated at 160 °C to melt the sulfur. Prior to melting the sulfur, a 10 wt% carbon nanotube (CNT) ink in dimethylformamide (DMF) was prepared and dropped onto the porous layer of the bilayer garnet SSE and dried in vacuum at 100 °C for 12 h.

[0134] 11 to 15 show the characterization of the bilayer garnet structure described in this example. EXAMPLES

[0135] This example provides a description of the solid hybrid electrolytes of the present disclosure and provides examples of the construction and characterization of such electrolytes.

[0136] High energy density lithium metal-sulfur batteries based on three-dimensional bilayer garnet solid electrolyte This example describes a novel design of safe, high-energy density solid-state hybrid batteries using a three-dimensional (3D) solid electrolyte framework and a lithium metal anode that can utilize a wide variety of cathode chemistries. This solid electrolyte framework may open new research directions for next-generation high-energy density Li-metal batteries.

[0137] To simultaneously address the challenges of chemical / physical shorting and electrode volume change, we present a three-dimensional (3D) bilayer garnet solid electrolyte framework for advanced Li metal batteries. The thickness of the dense layer can be reduced to a few microns while maintaining good mechanical stability, enabling the safe use of Li metal anodes. A thick porous layer acts as a mechanical support for the thin dense layer, which acts both as a host for high loading of cathode material and provides a pathway for continuous ion migration. Results show that an integrated sulfur cathode loading of 7 mg / cm2 was achieved. 2 Meanwhile, the proposed hybrid Li-S battery exhibits high initial coulombic efficiency (>99.8%) and high average coulombic efficiency (>99%) in subsequent cycles. This electrolyte framework is expected to improve Li metal batteries by transitioning to all-solid-state batteries and is also extendable to other cathode materials.

[0138] In hybrid batteries, chemical and physical short circuits can be prevented by a dense solid electrolyte that physically blocks the dissolved cathode material and suppresses the penetration of Li dendrites. The volume change of the active material can be accommodated by designing a compatible host structure of the porous solid electrolyte. To achieve this goal, we present a 3D solid electrolyte framework with a dense-porous bilayer structure. The 3D bilayer solid electrolyte framework has several unique advantages: (a) the thin dense bottom layer is a rigid barrier with high modulus that can effectively separate the electrode and liquid electrolyte while preventing the penetration of Li dendrites; (b) the thick top porous layer mechanically supports the thin dense layer; (c) the interface between the dense and porous layers is well sintered with good mechanical integrity and continuous ion transfer; (d) the solid framework can provide electronic and ionic conductive pathways for the encapsulated cathode material; and (e) the solid framework can locally confine the cathode material to accommodate the volume change caused by solid sulfur and polysulfide catholytes, etc. Our results show that the integrated sulfur cathode loading is 7 mg / cm 2While the proposed hybrid Li-S battery exhibits high initial coulombic efficiency (>99.8%) and high average coulombic efficiency (>99%) for each subsequent cycle. This electrolyte framework is expected to improve Li metal batteries by transitioning to all-solid-state batteries, such as high voltage (LNMO) and air / O2 cathodes, and is also extendable to other cathode materials.

[0139] Fabrication of garnet bilayer frameworks A bilayer framework was fabricated by laminating dense porous tapes as bilayer tapes and then removing the organic binder and polymer by co-sintering. The porous garnet structures were fabricated by scalable tape casting using garnet powder slurry-containing poly(methyl methacrylate) (PMMA) spheres as sacrificial pore formers with porosity of 70%. Separate details of the fabrication process are given in the Experimental Section. Unlike sulfide-type superionic conductors, which are sensitive to air and moisture, garnet is chemically stable to processing in dry air and has sufficient mechanical strength for handling. Therefore, the tape casting method can be easily scaled to fabricate low-cost garnet solid electrolyte frameworks. During sintering, the organic filler was decomposed and integrally sintered with the garnet powder to form the porous layer. The thickness of the porous and dense layers is controlled by the tape thickness.

[0140] Characterization of garnet bilayer frameworks A well-sintered porous dense layer interface without observable delamination indicates good contact at the interface. This interface may allow good ion transfer from the porous to the dense solid electrolyte. A dense garnet layer with large garnet grains may prevent chemical and physical short circuits between the active electrodes. A cross section of the bilayer garnet has a total thickness of 105 μm, including a 35 μm dense layer and a 70 μm porous support.

[0141] X-ray diffraction (XRD) revealed that sintered Li7La 2.75 Ca 0.25 Zr 1.75Nb 0.25 O 12 (LLCZNO) The standard cubic phase of garnet was confirmed to be cubic Li5La3Nb2O 12 (PDF80-0457). Also, the broad and partially overlapping bands in the Raman spectra confirm the cubic phase of LLCZNO garnet. The ionic conductivity of the dense garnet pellets was measured by electrochemical impedance spectroscopy (EIS) in a Au / garnet / Au symmetric blocking cell. EIS was performed in the temperature range 25°C to 50°C. The low frequency intercept, which corresponds to the capacitive behavior of the Au electrode, was used to calculate the total resistance, including bulk and grain boundary contributions. The ionic conductivity was calculated using σ=L / (Z×A), where Z is the impedance on the real axis in the Nyquist plot, L is the garnet ceramic disk length, and A is the surface area. This is 2.2×10 at 22°C. -4 S / cm. The logarithmic ionic conductivity of the garnet electrolyte was plotted against the inverse of temperature. By using the Arrhenius equation, an activation energy of 0.35 eV was calculated from the conductivity as a function of temperature.

[0142] Electrochemical characterization of garnet solid electrolyte / Li metal. The structure and chemistry of the interface between garnet and electrode are the main challenges in applying solid electrolytes. Recent studies have shown that poor contact at the interface is the main factor leading to high interfacial impedance of solid electrolyte and electrode. For example, a thin (~5 nm) atomic layer deposition (ALD) interfacial layer can significantly reduce the Li metal / garnet interfacial resistance. Compared with the reported vacuum-based process, gel electrolyte as an artificial interlayer between solid electrolyte and electrode can be more scalable for battery fabrication. In this case, gel electrolyte with good wettability can not only give a uniformly distributed Li ion flux at the interface but also prevent potential reduction of solid electrolyte after contact with Li metal. Individual pores are distributed on the garnet surface, and the cavities reduce the surface area for contact with Li metal, which leads to non-uniform Li ion migration and high interfacial resistance. A polymer gel layer was implemented to conformally cover the garnet surface. The liquid-filled interlayer ensures the intimate contact between garnet and lithium metal. A 2 μm thick polyethylene oxide (PEO) polymer conformally covers the garnet. This polymer layer compensates for the interface undulations and allows for uniform Li-ion flux through the interface.

[0143] The stability of the interface was evaluated by galvanostatic plating and stripping of Li metal in a symmetric hybrid cell (Li / polymer / garnet / polymer / Li) by applying a constant current of 0.3 mA / cm. 2The voltage profile as a function of time of the Li / hybrid electrolyte / Li cell was determined under a current density of 1000 s. The positive voltage indicates Li stripping and the negative voltage is Li plating. The cell was operated for 0.5 h per cycle. The cell initially showed a voltage of ±0.3 V, but after 10 h of cycling, the voltage gradually decreased to ±0.2 V. The hybrid cell was cycled for more than 160 h, and the stripping / plating voltages remained relatively stable. As a comparison, a Li / garnet / Li symmetric cell without a polymer interface was also fabricated and tested. The insets show the initial cycles of the two cells and the 140 h cycle of the hybrid cell. In the case of the Li / garnet / Li cell, high impedance and large polarization are observed, and the non-smooth voltage plateau suggests a large interfacial resistance between Li and garnet. In contrast, the hybrid cell shows a smooth voltage curve. Voltage profile The periodic variation of 0.5 and 1.0 mA / cm indicates the temperature dependence of the solid hybrid electrolyte performance. 2 The voltage profile of the Li / hybrid electrolyte / Li cell under a load of 1000 mA demonstrates the high applied current capability of the hybrid electrolyte.

[0144] Proof-of-concept Li-S battery with bilayer garnet framework The electrochemical performance of Li-S batteries with bilayer solid garnet hybrid electrolyte was determined. CNTs were infiltrated into the microstructure of porous garnet to construct an improved electronic conductive network. Photographs and SEM images of the CNT-infiltrated bilayer garnet framework show that the inside of the porous structure is CNT-coated. The volume expansion of sulfur and its soluble polysulfides can be accommodated by the solid garnet framework. Sulfur was directly loaded by melting sulfur powder into the porous matrix at 160 °C. Cross-sections and elemental mapping of the Li-S cathode were performed. The elemental mapping images clearly show the sulfur distribution in the pores of the bilayer garnet. The additional pores between the sulfur and garnet allow the liquid electrolyte to penetrate into the inner channels and coat the sulfur.

[0145] Sulfur mass loading is about 7.5 mg / cm 2 A hybrid bilayer cell with a high current density of 0.2mA / cm was fabricated. 2 The charge-discharge voltage profile of the hybrid Li-S cell was constructed in . The first cycle discharge capacity is around 645 mAh / g with a coulombic efficiency of 99.8%, which is exceptionally high. The long flat voltage plateau indicates the irreconcilable polarization between the charge-discharge curves. This can be attributed to the thin dense and porous garnet layer, which has a large surface area and increases the number of reaction sites with sulfur, allowing for lower voltage polarization and good capacity. The cycle performance was plotted. No rapid capacity growth occurs in the first few cycles, indicating that no polysulfides are lost in this hybrid cell with such a high sulfur mass loading. In the subsequent cycles, the coulombic efficiency remains above 99%, confirming that the shuttle effect does not occur in the hybrid design. Furthermore, the mass loading of 7.5 mg / cm 2 The hybrid bilayer Li-S cell has a total cell energy density (calculated in FIG. 16) of 248.2 Wh / kg considering the total mass of the cathode, Li anode, and electrolyte, far exceeding any solid-state battery available today. The cycle performance is slightly degraded, which is likely due to the fact that the charging products Li2S and Li2S2 are not reactivated in subsequent cycles. The high mass loading of sulfur prevents further reactions inside the bulk sulfur cathode.

[0146] This work demonstrates for the first time the feasibility of using a bilayer solid electrolyte framework in a hybrid battery. Further developments will focus on increasing the amount and loading of active sulfur by incorporating carbon-sulfur composites into the hybrid cell. If the bilayer framework is further optimized, for example, by thinning the dense layer and increasing the active material in the thick porous layer, an energy density of over 900Wh / kg is estimated (Figure 17).

[0147] This example describes a 3D bilayer solid electrolyte framework that addresses both the chemical and physical short circuit issues in Li metal batteries. To minimize the impedance of the solid electrolyte, the thickness of the dense garnet film was reduced to a few microns while maintaining adequate mechanical strength for battery assembly. A bilayer solid electrolyte framework was designed with a thick porous layer that mechanically supports the thin dense layer while hosting the electrode materials and liquid electrolyte. The thick porous layer acts as a continuous Li + / electron pathway. The thin dense layer also blocks the diffusion of polysulfides and hinders the formation of Li dendrites. The bilayer garnet solid electrolyte framework was applied to Li-S batteries to demonstrate its feasibility as well as high energy density and excellent performance. The demonstrated hybrid Li-S battery had a 7 mg / cm 2 The electrolyte framework exhibits high sulfur loading over 1000 s, high initial coulombic efficiency (>99.8%) and high average coulombic efficiency (>99%) in subsequent cycles. The framework is expected to improve Li-metal batteries, and the battery designs supported by this framework are extendable to other cathode materials for commercially viable and intrinsically safe Li-metal batteries, such as high-voltage (LNMO) and air / O2 cathodes.

[0148] method Preparation of garnet solid electrolyte LLCZN powders were synthesized by a modified sol-gel method. The starting materials were LiNO3 (99%, Alfa Aesar), La(NO3)3 (99.9%, Alfa Aesar), Ca(NO3)2 (99.9%, Sigma Aldrich), ZrO(NO3)2 (99.9%, Alfa Aesar), and NbCl5 (99.99%, Alfa Aesar). Stoichiometric amounts of these chemicals were dissolved in deionized water, and 10% excess LiNO3 was added to compensate for lithium volatilization during high-temperature pellet preparation. Citric acid and ethylene glycol (1:1 molar ratio) were added to the solution. The solution was evaporated at 120 °C for 12 h to produce a precursor gel, which was then calcined at 400 °C and 800 °C for 5 h to synthesize the garnet powders. The garnet powder was then uniaxially pressed into pellets, which were then covered with the same powder and sintered at 1050°C for 12 hours for conductivity and stability experiments.

[0149] A bilayer framework was fabricated by tape casting to fabricate dense and porous layers, respectively, and then laminated as a bilayer tape. The thickness of each individual layer was well controlled. A slurry was made with fully calcined LLZCN in the desired phase. LLZCN powder with fish oil as a dispersant was added to toluene, isopropanol (IPA). After 24 hours of milling, polyvinyl butyral (PVB) and butyl benzyl phthalate (BBP) were added as binders and plasticizers, followed by ball milling for another 24 hours. To remove air bubbles, the slurry was degassed by stirring in a vacuum chamber for 2 hours. Immediately after the degassing process, the slurry was poured into a hanging chamber with slots where the slurry was drawn out as a thin film onto a Mylar sheet. The resulting tape was then dried at 120°C for 1 hour. To fabricate the porous tape, poly(methyl methacrylate) (PMMA) spheres were mixed into the well-mixed slurry 1 hour before degassing. The pore size of the porous layer can be controlled by the size and content of the polymer-based pore former. The tapes were laminated and hot pressed at 80°C for 2 hours to allow the porous and dense layers to melt at their respective interfaces and form a good connection at their respective interfaces. The samples were pre-sintered at 700°C for 4 hours to remove the organic components, and then sintered at 1100°C for the final stage sintering. Good control of the sintering process ensured that the samples remained flat during sintering, which is important for Li / S infiltration and Li-S electrochemical performance tests.

[0150] Materials characterization The D8 Advanced was used with a CuKα radiation source operating at 40 kV and 40 mA. Phase analysis was performed by powder X-ray diffraction (XRD) on a LynxEye and SolX (Bruker AXS, WI, USA). The morphology of the samples was examined by field emission scanning electron microscopy (FE-SEM, JEOL 2100F).

[0151] Electrochemical characterization A Li|solid electrolyte|Li symmetric cell was prepared and assembled in an argon-filled glove box. To measure the ionic conductivity of the garnet solid electrolyte, a dense ceramic disk was coated on both sides with Au paste to act as a blocking electrode. The gold electrodes were sintered at 700 °C to form a good contact with the ceramic pellet. The cell was then assembled as a 2032 coin cell with a highly conductive carbon sponge. The carbon sponge acted as a buffer to prevent damage to the garnet ceramic disk. A battery test clip was used to measure the ionic conductivity of the garnet ceramic disk. A good contact with the coin cell was maintained and provided. The edges of the cell were sealed with epoxy resin. EIS was performed over the frequency range of 1 MHz to 100 mHz with a perturbation amplitude of 50 mV. The conductivity was calculated using σ=L / (Z×A), where Z is the impedance on the real axis in the Nyquist plot, L is the garnet ceramic disk length, and A is the surface area. The activation energy was determined from the conductivity as a function of temperature by using the Arrhenius equation.

[0152] Fabrication and characterization of garnet solid-state-based Li-S batteries All the cells were assembled in an argon-filled glove box. The solid-state hybrid cells were assembled as 2032 coin cells. 1 M bis(trifluoromethane)sulfonimide lithium salt (LiTFSI, Sigma) in a mixture of dimethoxyethane (DME) and 1,3-dioxolane (DOL) (volume ratio 1:1) was used as the electrolyte for the solid-state hybrid Li-S battery. Constant current charge-discharge tests were measured using a cut-off voltage window of 1–3.5 V. In the fabrication of the bilayer cathode, 10 wt% carbon nanotube (CNT) ink in dimethylformamide (DMF) was prepared, and a few drops of the CNT ink were added to the porous layer of the bilayer garnet framework and dried in vacuum at 100 °C for 12 h. After that, elemental sulfur powder was uniformly distributed on the porous garnet and heated at 160 °C to melt the sulfur. The bilayer garnet framework was about 17 mg, which was about 20 mg / cm. 2The actual sulfur infiltrated into the bilayer garnet framework was about 2.5 mg, which corresponds to about 7.5 mg / cm 2 The mass loading corresponds to 1000 s. The completed cell was assembled in an Ar-filled glove box. Liquid electrolyte was added to wash the sulfur cathode. The same amount of liquid electrolyte was used. The Li anode was made by thinning Li grains (Sigma) in a hydraulic press. The cell was packaged as a 2032 coin cell and sealed with epoxy resin to prevent air leakage at the edges. Specific energy density calculations (specific energy density calculations for the tested garnet bilayer Li-S battery) are shown in Figure 16.

[0153] With further optimization of the Li metal and S cathode thickness and mass loading, cell energy densities in excess of 900Wh / kg are achievable.

[0154] FIG. 17 shows the estimated energy density of the bilayer garnet solid-state Li-S battery with optimized parameters. EXAMPLES

[0155] This example provides a description of the solid hybrid electrolytes of the present disclosure and provides examples of the construction and characterization of such electrolytes.

[0156] Nature-inspired aligned garnet nanostructures Solid-state Li batteries (SSLiBs) with solid-state electrolytes (SSEs) can potentially prevent Li dendrite penetration and achieve high energy density with improved safety by applying metallic lithium anodes. The ion transport behavior and ionic conductivity in Li-ion batteries are significantly affected by the tortuosity of the electrode and electrolyte materials. A low-torque structure with straight ion pathways is highly desirable but quite difficult to achieve in solid-state ionic conductors. We have developed a highly conductive garnet framework with a multiscale aligned mesostructure by a scalable top-down approach. Ion-conducting polyethylene oxide (PEO) was incorporated into mesoporous wood-templating aligned garnet nanostructures to obtain a mixed hybrid ionic conductor, termed garnet-wood. The synergistic integration of aligned garnet with a flexible and mechanically robust polymer resulted in high ionic conductivity (1.8 × 10 at room temperature). -4 Both the tensile strength (T / cm) and good mechanical flexibility were obtained. This work provides a new direction for the development of nature-inspired fast-ion conductors with low torsion.

[0157] Inspired by the ordered structure of natural wood, we disclose highly ion-conducting garnet networks with well-ordered mesostructures by templating synthesis. By employing wood as a sacrificial template, we obtained multiscale ordered porosity, low tortuosity, and high specific surface area of ​​the garnet mesostructures. Garnet-type LLZO was selected as a model system to fabricate aligned solid electrolytes with low tortuosity due to its high ionic conductivity, good chemical stability with Li anodes, and wide electrochemical window. A composite electrolyte was developed by incorporating PEO polymer electrolyte into the wood-templated aligned garnet (referred to as garnet-wood). The polymer electrolyte provides an additional transport pathway and supplements the mechanical strength of the composite structure. Li ions can be effectively transported through the garnet, polymer, and along the garnet-polymer interface. As a result, the garnet-wood film exhibits a 1.8 × 10 -4Based on this concept, the design principles and fabrication process of the aligned garnet wood electrolyte can be extended to a wide range of solid electrolytes.

[0158] Due to its high growth rate, low cost, and high porosity, Basswood was selected as a template to develop an aligned garnet solid electrolyte framework. After partial removal of lignin from natural Basswood by chemical treatment, the wood template was obtained by compressing and slicing perpendicular to the longitudinal direction (natural growth direction) of the wood (Figure 19a). The wood was densified by mechanical pressing. The dense structure of the framework is maintained by additional hydrogen bonds formed between adjacent cellulose fibers during densification. The morphological changes due to mechanical compression were investigated by scanning electron microscopy (SEM) measurements of several samples. Before compression, the microchannels in the wood have a proximal cylindrical shape with an average diameter of 10-50 μm (Figures 19b and 19d). After compression, most of the previously observed microchannels were crushed into crack-like gaps, and some of the adjacent channels were connected (Figures 19c and 19e). Although these open channels were severely deformed by compression, their highly aligned multiscale pore structures remained unchanged (Figure 19f) and exhibited excellent absorption when immersed in precursor solutions. For example, after immersion for 48 h and drying in vacuum at 70 °C for 4 h, the mass of the wood template increased by 27.8%, from 2.7 mg to 3.45 mg (Figure 25). The high absorption of the precursor solution, the flexibility of the template pores, and the scalability of the procedure indicate a cost-effective and productive method to fabricate SSEs with aligned mesostructures.

[0159] LLZO films were obtained by calcining the wood infiltrated with the garnet precursor in oxygen at 800 °C for 4 h. The channel-aligned wood template has two unique functions. First, the free channels in the wood template provide a reservoir to feed the precursor solution to the templated combustion reaction. Second, the aligned nanofibers with diameters of 2–10 nm in the wood template act as sacrificial pore formers for additional aligned porosity in the garnet film. The morphology changes after calcination were characterized by SEM. The aligned pore structure from the wood template was also inherited by the resulting garnet framework at both the microscale (Figure 20a) and nanoscale (Figure 20b). The highly aligned garnet film directly inherited from the wood becomes flexible upon infiltration with a PEO-based polymer electrolyte (Figure 20c). The crystalline phases of the garnet film were identified by X-ray diffraction (XRD). The XRD pattern of the ordered mesoporous garnet synthesized using the wood template (Fig. 20d) shows that the cubic phase garnet Li5La3Nb2O 12 (JCPDS#80-0457). As a representative structure of fast lithium ion conducting garnets, Li5La3M2O5 (M=Nb, Ta) is widely used as a standard to distinguish conducting garnet phases from non-conducting garnet phases. The good XRD pattern matching of the ordered mesoporous garnets with JCPDS#80-0457 confirms that the wood templating garnet is a conducting cubic phase.

[0160] High-resolution transmission electron microscopy (HRTEM) of the resulting aligned garnets reveals a well-defined and well-crystallized lattice structure of the garnets (Fig. 22a). The Miller indices were calculated from the corresponding fast Fourier transform (FFT) patterns (inset in Fig. 22a). The lattice constant derived by HRTEM and FFT is 12.982 Å, which is consistent with previously reported values. In the HRTEM image of a larger garnet grain that has broken away from the structure, grains of various orientations can be clearly distinguished (Fig. 21b). The TEM results show that the aligned mesoporous garnets have a highly crystallized and well-connected polycrystalline structure. The composition of the garnet films was analyzed by electron energy loss spectroscopy (EELS). Figure 21 shows the EELS spectrum at the outlined region of interest (ROI). The EELS mapping shows the relative composition and distribution of oxygen, carbon, and lanthanum. The overlapping regions of the oxygen k-edge and lanthanum n-edge signals identify the location of the LLZO. Carbon k-edge signals are uncommon throughout the sample, but small regions of overlap of oxygen k-edge and carbon k-edge signals were identified, indicating minimal Li2CO3 impurities due to calcination in oxygen.

[0161] Garnet wood was fabricated by infiltrating the aligned garnet with PEO polymer electrolyte. Figure 22a characterizes the polymer infiltration by energy dispersive X-ray spectroscopy (EDX). The uniformly distributed carbon signals from above and below into the aligned garnet channels indicate the complete and uniform infiltration of the polymer electrolyte, which is essential for the construction of sufficient Li-ion migration pathways. As suggested herein, three Li-ion migration pathways are possible. The first pathway is the aligned PEO polymer electrolyte, whose bulk ionic conductivity (without filler) is typically 10 at room temperature. -7The second pathway is the aligned garnet-polymer interface. At the interface, the aligned mesoporous garnet behaves like a ceramic filler that can induce changes in the partial dynamics of the polymer to affect the lithium ion migration. Intensive studies on the effect of fillers on the ionic conductivity of polymer electrolytes suggest that ceramic fillers with Lewis acid properties can facilitate lithium ion migration by anion binding and providing favorable conduction pathways. The third pathway is migration through a high volume percentage (~68%) of aligned garnet nanostructures. Recent studies have pointed out that of the three migration pathways in garnet-polymer composite electrolyte systems, the conduction through the garnet phase is the most favorable, as revealed by tracking the migration of isotopically labeled Li ions using nuclear magnetic resonance (NMR). Note that the typical bulk ionic conductivity of high-density LLZO realized in our laboratory with the same composition is up to 2.2 × 10 at room temperature. -4 S / cm. However, this bulk ionic conductivity is difficult to achieve in conventional mesoporous structures due to the highly tortuous transport paths caused by random pores and poor solid-solid interfacial contacts in the numerous inter-pore spaces. In contrast, the low tortuosity of the ordered mesoporous garnet structure does not impede Li-ion transport along the normal direction of the flexible garnet wood, which can effectively promote ionic conductivity.

[0162] The ionic conductivity of garnet wood was characterized by electrochemical impedance spectroscopy (EIS). Garnet wood membranes (area 0.1 cm) were placed in symmetric cells with stainless steel as the blocking electrode. 2 , 0.4 μm thick) were assembled and scanned from 1 MHz to 100 mHz. Figure 22b shows the Nyquist plots of the electrolyte membranes tested from room temperature (25 °C) to the melting temperature of PEO (65 °C). The thickness and area of ​​the electrolyte membrane were used to calculate the experimental ionic conductivity, which is shown in Figure 22c. The garnet wood membrane had a conductivity of 1.8 × 10 at room temperature. -4 The theoretical ionic conductivity of the composite is the total contribution of each phase weighted by the volume fraction: 1.03×10-6 The conductivity of the PEO polymer electrolyte is 2.2×10 -4 Given the conductivity of garnet in S / cm, the theoretical conductivity of garnet wood is 1.5×10 at room temperature. -4 In this low twist structure with continuous conduction paths in each phase, the two-phase interface Without the enhanced conductivity at the interface, the theoretical conductivity should be preserved. Therefore, we believe that the difference between the theoretical and experimental conductivity may be due to the increased interfacial contribution to the total ionic conductivity.

[0163] As the operating temperature increases, the intersection point of the semicircle with the real impedance axis decreases, indicating that the ionic conductivity increases with increasing temperature (Figure 22b). At 95 °C, the ionic conductivity is 1.1 × 10 -3 The temperature dependence of ionic conductivity of garnet wood is given by the Arrhenius equation as follows:

number

[0164] where σ is the total ionic conductivity of garnet wood, A is the frequency factor, T is the absolute temperature, and E A is the activation energy of garnet wood and k is the Boltzmann constant. The calculated activation energy of garnet wood is 0.38 eV, which can be further lowered by adjusting the proportion of polymer electrolyte. This effect is attributed to various enhancement effects, such as the increased volume fraction of the amorphous conducting phase and improved long-range polymer chain mobility.

[0165] As a proof of concept, a Li metal / garnet wood / Li metal symmetric cell was fabricated and Li stripping / plating tests were performed at room temperature (Figure 22d). Figure 22e shows the Li-stripping / plating tests at a current density of 0.1 mA / cm for 30 min in each direction. 2The results show a characteristic 180-hour cycle at 1000 Hz. The voltage response of the symmetric cell was stable at 50 mV with little fluctuation. The symmetric cell cycled well for over 600 hours with small polarization (Figure 27). This long-term cycling performance indicates that the garnet-wood film enhanced by the aligned mesoporous garnet can enable fast and stable ion transfer. The polymer electrolyte also greatly improves the mechanical flexibility of the aligned garnet, making it usable in Li-metal batteries.

[0166] Thus, we have described a garnet-wood composite electrolyte with a multiscale aligned mesoporous structure. The scalable compressed wood template provides a unique low tortuosity and large surface area mesostructure, which is critical for enhanced electrochemical performance and mechanical stability. The ion-conducting polymer acts as a matrix to supplement the mechanical strength of the aligned mesoporous garnet film and provide additional ion migration paths through the amorphous conducting phase and the garnet-polymer interface. Benefiting from these structural advantages combined with the intrinsic high ionic conductivity and low tortuosity of aligned mesoporous garnet, the garnet-wood composite electrolyte exhibits a 1.8 × 10 ionic conductivity at room temperature. -4 S / cm, 1.1 × 10 at 95°C -3 "We achieve high Li-ion conductivity of 1.5 S / cm, which is close to the bulk conductivity of the garnet itself and further shows an enhanced contribution from the garnet / polymer interface. Garnet wood shows excellent potential as a low-torsion structure for highly conductive SSEs and provides a model study for the design and optimization of solid-state CPEs."

[0167] Experimental section Material preparation Stoichiometric amounts of LiNO3 (≥99.0%, Aldrich), La(NO3)3 (≥99.9%, Aldrich), Al(NO3)3·9H2O (≥98.0%, Aldrich), ZrO(NO3)2·xH2O (≥99.9%, Aldrich), and acetic acid (>99.7%, Aldrich) were dissolved in ethanol at room temperature with magnetic stirring. Garnet precursor solutions were prepared by dissolving in 1,2-dichlorophenyl ether (>99.8%, Aldrich). The total cation concentration of the precursor solution was 2 mol / L. An excess of 15% lithium nitrate was added to compensate for lithium loss at high firing temperatures.

[0168] The wood template was immersed in the aforementioned solution for 48 h to impregnate the garnet precursor. Excess solution was removed from the wood template and the sample was dried at 70 °C for 4 h. A subsequent heat treatment was performed in oxygen at 800 °C for 4 h to burn out the wood template and sinter the dispersed precursor. Careful control of the sintering process maintained the microstructure of the wood template. Grinding of the garnet film and sonication in isopropanol (IPA) yielded garnet nanoparticles and nanofibers for TEM investigation.

[0169] In an argon-filled glove box at room temperature, lithium bis(trifluoromethane)sulfonimide (LiTFSI, 99.85% or higher, Aldrich, EO:Li + PEO-based polymer electrolytes were prepared by dissolving PEO (Mv=600,000, Aldrich) containing 100% ethanol (Mv=8:1) in acetonitrile (anhydrous, 99.8%, Aldrich) with magnetic stirring. 15 wt% succinonitrile (SCN, 99%, Aldrich) was added to the solution and the mixture was magnetically stirred until the SCN was completely dissolved. Prior to electrochemical testing, the drop-cast polymer electrolyte in the aligned mesoporous garnet (garnet wood) was thoroughly dried in vacuum at room temperature for 1 h.

[0170] Materials characterization XRD was performed on a Bruker D8 Advance with Cu K radiation. SEM images and their corresponding EDX images were acquired using a Hitachi SU-70 field emission SEM equipped with an energy dispersive X-ray spectrometer. TEM images were acquired using a JEM2100 field emission gun TEM equipped with an electron energy loss spectrometer for EELS investigations. FFT images were calculated from the high-resolution TEM images using a Gatan microscopy set. EIS measurements were performed using a Solartron-1260 impedance gain phase analyzer on symmetric cells consisting of garnet wood between stainless steel plates as blocking electrodes. Before each EIS test, the cells were left in an environmental chamber at a given temperature for 30 min to reach thermal equilibrium, and then impedance curves at different temperatures were acquired, scanning from 1 MHz to 100 mHz. Li stripping / plating tests were performed using a Bio-Logic VMP3 multichannel potentiostatic electrolyzer on symmetric cells consisting of garnet wood between Li metal foils as electrodes. Electrochemical electrolysis was performed at 0.1 mA / cm for 30 min at room temperature in each direction in an argon-filled glove box. 2 The cell was cycled at a current density of 0.01 V.

[0171] 23 to 29 show the preparation of the solid electrolyte of this example and the evaluation of its characteristics. EXAMPLES

[0172] This example provides a description of the solid hybrid electrolytes of the present disclosure and provides examples of the construction and characterization of such electrolytes.

[0173] Lithium-ion conducting ceramic fibers: a new architecture for flexible solid-state lithium metal batteries The design of solid-state lithium metal batteries requires high-rate lithium-ion conductors, good electrochemical stability, and scalable processing approaches for device integration. This example demonstrates the unique design of flexible lithium-ion conducting ceramic fibers with the above characteristics for use in solid-state batteries. The ceramic fibers are made of garnet-type conductor Li7La3Zr2O 12Based on this, solid garnet fibers have demonstrated a variety of desirable chemical and structural properties, including lithium-ion conductive cubic structure, low density, multiscale porosity, high surface area / volume ratio, and good flexibility. This reinforces the solid polymer electrolyte, enabling high lithium ion conductivity and stable long-term Li cycling without failure for over 500 hours. The fibers also provide ultra-high cathode loading (10.8 g / cm) for high-performance Li metal batteries. 2 This study provides an electrolyte framework for designing 3D electrodes that realize the transfer of charged particles (e.g., sulfur).

[0174] To achieve a finely distributed ion-conducting phase, a fibrous structure with a large surface / volume ratio is the ideal configuration for ion conduction and electrochemical reactions occurring in the battery. The templating method offers a simple yet effective way to generate the required structure. The fibrous template is immersed in a ceramic precursor solution, followed by pyrolysis to remove the organic components. The resulting fibrous ceramic features desirable properties that allow integration into flexible or rigid battery configurations. For example, the use of ceramic fiber networks establishes lithium ion migration pathways within the polymer electrolyte and improves the mechanical strength of the polymer. Alternatively, ceramic fibers can be combined with electrode materials in an interdigitated or concentric configuration to minimize electrolyte volume and maximize electrode utilization, thus increasing the active electrolyte area, lithium ion interfacial migration, and electrode volume change resistance during charge / discharge.

[0175] This example demonstrates the fabrication of template-derived garnet-based lithium-ion conducting ceramic fibers, producing fibers with superior properties for integration into solid-state batteries. The use of garnet fibers simultaneously reinforced the polymer electrolyte and 3D electrode structure for stable Li cycling for over 500 hours, achieving a maximum of 10.8 g / cm for high-performance Li metal batteries. 2We provide a solid-state lithium-ion conducting framework that achieves ultrahigh sulfur loading of 1000 times the capacity of lithium-ion batteries. The simplicity of the templating method is useful for the fabrication of ceramics with tuned composition and structure, opening up the possibility of constructing low-cost and durable solid-state batteries.

[0176] Materials and Methods Synthesis of garnet fibers Various heterovalent cations have been proposed to effectively stabilize the cubic phase garnet and obtain high lithium ion conductivity at room temperature. Li was prepared by dissolving stoichiometric amounts of 2.31 g LiNO3 (99%, Alfa Aesar), 0.48 g Al(NO3)3·9H2O (98%, Alfa Aesar), 6.94 g La(NO3)3·6H2O (99.9%, Alfa Aesar), and 5.0 g zirconium propoxide solution (70 wt%, Sigma Aldrich) in 30 ml of ethanol containing 15 vol% acetic acid. 6.28 Al 0.24 La3Zr2O 11.98Al-doped LLZO with the chemical composition of Al was prepared. Excess LiNO3 (15 wt%) was added to compensate for lithium loss in the subsequent calcination procedure. The cellulose fiber template was prepared by annealing in air at 270 °C for 10 h, followed by washing with ethanol (Sigma Aldrich) and drying at 100 °C for 12 h. After pretreatment, the template was immersed in 2.5 mol / L LLZO precursor solution for 24 h. The multiscale porosity present in the porous template allowed for uniform impregnation of the LLZO precursor. The thermal behavior of the LLZO precursor-infiltrated fiber template was analyzed by thermogravimetric analysis (TGA, STAR System). Calcination of the precursor-infiltrated template was performed in oxygen at different temperatures to obtain garnet fibers. The 3D morphology of the garnet fibers was scanned using an LK-H082 semiconductor laser model (Keyence) with a wavelength of 655 nm. The crystalline phase of LLZO was analyzed by powder X-ray diffraction on a D8 Advanced with LynxEye and SolX (XRD, Bruker AXS) using a CuKα radiation source operated at 40 kV and 40 mA. The microstructure and elemental distribution were investigated by an analytical scanning electron microscope (SEM, Hitachi SU-70) equipped with an energy dispersive spectrometer (EDS, Oxford Instruments).

[0177] Preparation of garnet fiber reinforced composite polymer electrolytes The polymer matrix was prepared by dissolving LiTFSI (Sigma Aldrich) and PEO (~600,000, Sigma Aldrich) in acetonitrile as described in our previous work. Garnet fibers mounted on a Teflon block were repeatedly infiltrated with the lithium salt / polymer mixture. The composite polymer electrolyte was first dried in an argon-filled glove box and then in a vacuum oven to remove residual solvent before characterizing its morphological and electrochemical performance. As a comparison, insulating Al2O3 fibers made by the same templating method were prepared and incorporated into the polymer matrix as a control composite electrolyte. The electrochemical impedance of the composite polymer electrolyte was measured in a stainless steel / composite polymer electrolyte / stainless steel sandwich configuration using a Solartron-1260 impedance analyzer. The thickness was fixed with a Teflon spacer. Impedance tests were performed at 20 mV AC amplitude in the frequency range of 1 Hz to 1 MHz from 25 °C to 100 °C. The long-term lithium cycling stability and compatibility of the composite polymer electrolytes were evaluated using Li / composite polymer electrolyte / Li sealed symmetric cells. The charge-discharge cycles of the symmetric cells were monitored by an Arbin BT-2000 in an environmental chamber (Tenney).

[0178] Fabrication of garnet fiber electrode configurations for solid-state Li-S batteries Following the same process as our previous study, Li7La 2.75 Ca 0.25 Zr 1.75 Nb 0.25 O 12Garnet powder with the composition was synthesized. A dense electrolyte support was fabricated by a scalable tape casting and high temperature lamination method. The laminated green tapes were sintered at 1050 °C in a tube furnace under oxygen atmosphere. Garnet fibers were sintered onto the garnet electrolyte support in oxygen to form the framework for cathode infiltration. The cells were assembled in an argon-filled glove box with O2 and H2O levels both below 0.1 ppm. Lithium metal was melted onto the dense garnet electrolyte support coated with an ultrathin amorphous Si layer to achieve proper interfacial contact.

[0179] Sulfur slurry was made by mixing sulfur powder (from Sigma Aldrich), carbon nanotubes (from Carbon Solutions), and PVP (ca. 40,000, from Sigma Aldrich) in a mass ratio of 8:1:1 in N-methylpyrrolidone (from Sigma Aldrich) to achieve a concentration of approximately 10 mg / mL. After 5 h of sonication to obtain a homogeneous suspension with low concentration, droplets of sulfur slurry were repeatedly applied to the garnet fibers to infiltrate the open pores and dry. The final sulfur loading was calculated by subtracting the weight of the unfinished cell before infiltration of the cathode slurry from the total weight of the finished battery, then multiplying by the weight ratio of sulfur in the cathode mixture. 1M in trace DME / DOL LiTFSI was introduced into the cathode to promote sulfur / garnet contact before carbon felt was placed on the cathode side as a spacer and current collector. The battery was sealed as a coin cell with epoxy and connected to an Arbin BT-2000 to perform charge / discharge measurements.

[0180] Results and Discussion Lithium-ion conducting ceramic fibers were fabricated by impregnating the template with a precursor solution followed by pyrolytic conversion. As shown in Figure 30, the flexible ceramic fibers retained the structural properties of the original fiber template, which differs significantly from the rigid network of discrete particles in conventional sintered porous ceramic compacts. The fiber structure consisted of a network of continuous interlacing fibers and crossing yarns with weaving affecting the spatial distribution of lithium-ion conducting material and open pores. Lithium ion migration could occur throughout the fiber pattern, both within and along the surface of the polycrystalline fibers. Small polydisperse interconnected pores existed between individual fibers, while large discrete pores of relatively uniform size and shape were found between adjacent yarns.

[0181] Characterization of flexible garnet fibers. Fibrous ceramic fibers are commercial products in various technical fields. The production of ceramic fibers and fibers can be classified into direct spinning and indirect templating processes. The general procedure of the templating process is illustrated by the representative images in Figures 31a-c: (1) pre-treating the template, (2) impregnating the template with a precursor solution, and (3) converting the precursor into nano-sized ceramic oxides by pyrolysis of the template at high temperature and sintering of the remaining structure (thermogravimetric analysis in Figure 34a). The garnet fibers essentially retained the characteristic physical properties of the original template, which consisted mostly of continuous individual microfibers with a diameter of about 10 μm arranged parallel and twisted to each other. Cross-sectional SEM images can be seen in Figures 34b-d. The fibers were bundled together as threads with a diameter of approximately 200 μm that crossed each other, forming a periodically arranged woven and knitted pattern. Heat treatment formed inter-fiber pores and larger pores between the threads with diameters ranging from 10 to 20 μm.

[0182] For quality control and inspection purposes, large areas of garnet fiber geometry were mapped by applying non-destructive 3D laser scanning. The reconstructed digital structure in Fig. 31d shows a typical one-upper, one-lower plain weave fiber pattern. The height profile of this topology shows the distance between the highest point of the cross-yarn branching in the pattern and the lowest point of the grounding. While the branching areas are typically around 200 μm high, some of the edge areas showed slightly higher values. The edge up-rolling can be eliminated by strict process control to ensure proper sintering. Fig. 31e shows the remarkable physical characteristics of garnet fibers. Unlike the rigid appearance of normal sintered ceramics, garnet fibers were similar to templates in terms of constant bending strength, geometric adjustment, and resistance to organic solvent attack. The simplicity, rapidity, and cost-saving characteristics of the templating method also allow a smooth transition from small-scale fabrication to large-scale manufacturing. Fig. 35 shows how garnet fibers can be tailored to specific shapes of large dimensions.

[0183] In addition to being able to create versatile ceramic structures, the templating method offers chemical flexibility in the synthesis of complex oxides. 12 Garnet-type conductors in exist in two phases: cubic and tetragonal. The cubic structure favors high ionic conductivity but is stable only at high temperatures. As shown in Fig. 31f, the stabilization of the cubic phase can be achieved at a sintering temperature as low as 800 °C by simple composition design through doping with multivalent cations and optimizing the lithium concentration in the precursor solution. Care should be taken to ensure that the sintering process avoids over-sintering, which would cause excessive volatilization of lithium and separation of the lanthanum zirconate (LZO) phase. In Fig. 31g, the uniform distribution of the constituent chemical elements in the garnet fiber was confirmed by EDS. Element aluminum acted as a doping cation to stabilize the cubic phase and promote sintering due to its simplicity and low cost.

[0184] Garnet fiber reinforced flexible composite polymer electrolytes The structural and chemical advantages of garnet fibers make them ideal for reinforcing the mechanical and electrochemical properties of composite polymer electrolytes (CPEs), as shown in Figure 32. Free-standing CPEs were fabricated by vacuum infiltration of garnet fibers with a solution containing PEO and lithium salt. The dry CPE in Figure 32a appears soft and flexible, indicating that efficient wetting and capillary action successfully drew the fluid into the multi-level pores, allowing for strong physical bonding between the garnet fibers and the polymer matrix. Cross-sectional microstructural analysis further confirmed that the CPE appeared to be well densified without noticeable pores in Figure 36a. The cured CPE, although appearing as a homogeneous solid, was composed of physically and chemically unique ceramic and polymer phases separated by distinct interfaces. Thus, both components influenced the lithium ion migration kinetics within the CPE, which is illustrated by the schematic diagram in Figure 32b. Most continuous ceramic fibers have The PEO matrix is ​​bundled into a thread that penetrates the CPE. The thread is generally oriented perpendicular to the vertical direction of lithium ion transport within the CPE (thick arrows). Lithium ions migrate across the CPE by a multi-step process: (1) through the PEO to the "bottom" of the garnet fiber and from the PEO into the highly conductive fiber, and (2) along the length of the fiber until they reach the "top" of the yarn and then back to the PEO. This process minimizes the involvement of resistive garnet / polymer interfaces or diffusion through the polymer bulk (dotted arrows), making lithium ion diffusion independent of solvated lithium content of the polymer matrix.

[0185] Figure 32c shows typical impedance plots of CPEs measured at different temperatures. The lithium ion migration process was divided into ionic conduction in the CPE (high frequency arc) and ionic blocking at the CPE / stainless steel interface (low frequency sloping tail). The resistance of the CPE was obtained by reading the real impedance value at the high frequency intercept of the arc. Figure 32d shows the temperature dependence of lithium ion conductivity analyzed using Arrhenius plot. In general, lithium ion conductivity exhibited nonlinear behavior with increasing temperature. There was a slight decrease in activation energy when the temperature exceeded 60 °C, which corresponds to the phase transition temperature of PEO. When the PEO-LiX system undergoes thermal phase transition, the conductivity is known to undergo a steep change in activation energy. In contrast, the energy barrier for lithium ion conduction in crystalline garnets is expected to remain constant throughout the test temperature range. Therefore, the smooth transition of activation energy observed in the CPEs suggests that the fibrous garnet phase dominates in lithium ion conduction in the CPEs due to the formation of long-range garnet fibrous networks and continuous channels along the fiber surface. To further illustrate the effect of the Li-ion conducting garnet fibers on the electrochemical performance of the CPE, a control sample was constructed using insulating Al2O3 fibers prepared by the same templating method (Fig. 36b). The EIS of this control sample was measured as a function of temperature (Fig. 36c). The resulting high impedance and corresponding low room temperature 2.48 × 10 -6 The conductivity of 1.5 S / cm, which is essentially the room temperature polymer conductivity, indicates that the Al2O3 phase and the ceramic / polymer interface make little contribution to the Li-ion conduction in the CPE, confirming the dominant contribution from the Li-ion conducting garnet fiber phase.

[0186] The measured lithium ion conductivity of the garnet CPE is 2.7×10 at 25°C. -5 S / cm, 1.8 × 10 at 60 °C -4 These are the conductivity values ​​of the PEO-LiX polymer electrolyte system containing 85 vol% CPE (approximately 10 S / cm at 25 °C). -6S / cm, approx. 10 at 60°C -5 This is an order of magnitude higher than the reported ionic conductivity of 4 × 10 at 25 °C. -4 S / cm, while the Al-doped garnet contains only 15 vol% CPE. The corresponding theoretical volume fraction normalized CPE conductivity at 25 °C is 6 × 10 -5 S / cm, which is consistent with the measured CPE conductivity. Therefore, significant improvement in conductivity can be easily achieved by optimizing the densification process of the garnet ceramic fibers to increase the garnet phase volume fraction.

[0187] The long-term lithium cycling stability and compatibility of the CPE was evaluated by galvanostatic stripping (0.5 h) and plating (0.5 h) measurements. Stable DC cycling as a function of current density was achieved over the entire test period at 60 °C in Figure 36e. The current density was 0.05 mA / cm 2 and 0.1mA / cm 2 At a current density of 0.2 mA / cm, the symmetric cells achieved low overpotentials of 15 mV and 27 mV, respectively. 2 As the temperature rises to 100°C, the overpotential increases sharply and reaches a maximum value of 47 mV. During the remainder of the test period, the overpotential decreases gradually and stabilizes at 41 mV. The overall resistance and impedance measurements obtained by voltage vs. current density (Fig. 37a) decrease with increasing current density and operation time, which is attributed to the activated diffusion process in the CPE and the improvement of the lithium / CPE interface. Also, at lower operating temperatures (Fig. 37b) and Stable galvanostatic cycling of the CPE was achieved at low and high current densities (Figure 37c). For practical applications, further reduction in overpotential and extension of operational lifetime require increased garnet phase loading in multilevel pores and the adoption of sulfur-bridged polymers.

[0188] 3D electrode configuration with garnet fiber structure Garnet fibers can also be used to construct 3D electrode configurations by sintering the fibers onto a dense electrolyte support (Fig. 33a) and infiltrating the fiber structure with electrode materials. Here, we demonstrate a Li-S battery as a proof of concept due to the high energy density and low material cost of the sulfur cathode. The well-distributed pores of the fibrous structure allowed the fibers to easily accommodate high sulfur loadings. Fig. 33b shows that the fibers can support high sulfur loadings of 10.8 mg / cm. 2 33c show SEM images of sulfur-loaded garnet fibers of 1000 nm. The garnet fibers were bound together and the open pores were filled with a sulfur / carbon mixture. In FIG. 38a, an EDX linear scan across the region of the yarn / electrolyte interface reveals sulfur / carbon on the exposed surface of the garnet yarn and electrolyte. In FIG. 38b, cross-sectional analysis shows that the sulfur / carbon mixture penetrates the porous fibers, coats the individual fibers, and reaches the dense electrolyte surface. In FIG. 33c, under high magnification, EDX mapping confirms the uniform elemental distribution of sulfur / carbon loaded on the garnet fibers and intimate contact between the successive lithium ion conducting, electronic conducting, and sulfur phases.

[0189] A solid-state Li-S battery was assembled to demonstrate the electrochemical advantages of the garnet fiber 3D electrode configuration. A trace amount of liquid electrolyte was added to activate the sulfur and improve the contact between the garnet and sulfur without creating an undesirable lithium ion barrier. The hybrid configuration was still largely solid despite the addition of trace amounts of liquid electrolyte. In Figure 39, the dense garnet electrolyte support acted as a lithium ion conductor, electronic insulator, and lithium polysulfide shuttle shield.

[0190] 10.8 mg / cm 2 A solid-state Li-S battery with sulfur of 0.15mA / cm 2The charge-discharge profiles of the sulfur cathode cycled at 0.5 V and 1.0 V are shown in Fig. 33d. The sulfur cathode exhibited two discharge plateaus at 2.1 V and 1.8 V, while the charge profile had plateaus corresponding to 2.38 V and 2.43 V. The relatively large polarization overpotential (~0.6 V) during charging and discharging may be attributed to the polarization contributions from the relatively thick garnet electrolyte and impurities on the garnet electrolyte surface, which can be improved by thinning the electrolyte and adding a moisture-proof LiF phase or another liquid electrolyte. The discharge capacity reached a high value of 1,250 mAh / g at the fifth cycle due to the improved sulfur utilization by the successive wetting process by adding a trace amount of liquid electrolyte. The 3D Li-ion conducting electrode structure also provided a high discharge capacity of 0.75 mA / cm. 2 We successfully cycled a solid-state Li-S battery at a current density of 1000 nm (Figure 40). To maximize the volumetric utilization of the fiber electrode configuration, we used a fiber electrode with almost double the sulfur content (~18.6 mg / cm). 2 ) was attempted. Such high sulfur loading resulted in poor utilization and early cycling degradation (Figure 41). However, a stable and reversible high capacity of 800 mAh / g confirmed the energy storage capacity of the electrode framework constructed with garnet fibers.

[0191] The theoretical energy density of a Li-S battery using a dense solid electrolyte to separate the lithium and sulfur has been estimated as high as 500Wh / kg at the cell level. In comparison, Figure 42a shows the energy density of a solid Li-S battery using ceramic fibers for sulfur support and a tunable dense electrolyte structure at the interface with the lithium. With a 500 μm thick electrolyte support and 63% utilization of the electrolyte area, an achievable energy density of 71 Wh / kg is possible. By reducing the electrolyte support thickness to 100 μm and supporting more sulfur by matching the electrolyte / electrode area, an energy density as high as 281 Wh / kg is also possible. Further thinning of the electrolyte support requires a large amount of material to maintain mechanical strength. A complex electrolyte structure needs to be developed to achieve this. Figure 42b shows a representative SEM image of the required bilayer structure consisting of a thin dense electrolyte (20 μm) and a porous substrate (70 μm). Lithium metal can be injected into the pores to generate sufficient lithium / garnet transfer interfaces and further enhance the mechanical strength. By integrating the garnet fibers and bilayer support, an even higher energy density of 352 Wh / kg can be achieved, which is far beyond the capacity of state-of-the-art lithium-ion batteries.

[0192] We have successfully demonstrated flexible lithium-ion conducting garnet fibers fabricated by a simple templating method. The unique compositional advantages of flexible fibrous garnet fibers enable the creation of solid electrolyte frameworks with continuous lithium-ion conducting pathways and high surface-to-volume ratios. Incorporation of the fibers into solid polymer electrolytes enables enhanced lithium-ion conductivity and stable Li cycling for over 500 hours. Additionally, the use of tailored garnet fibers has enabled the fabrication of 3D porous electrodes with high sulfur loading (10.8 mg / cm). 2 ) and the resulting batteries provided capacities as high as 1000 mAh / g. The current laboratory-scale fabrication procedures are transferable to affordable and reliable industrially relevant scale production. Although initial efforts so far have been directed at solid-state lithium metal batteries, the novel structural design strategies utilized in this example are expected to be applicable to other solid-state devices for energy storage and conversion beyond lithium-ion technology.

[0193] 32-42 depict the flexible solid-state electrolytes of this example and the characterization of these electrolytes, showing thermogravimetric analysis, additional SEM images, photographs of large-scale garnet fibers, characterization of the composite polymer electrolyte, SEM images of sulfur-infiltrated garnet fiber electrodes, characterization of the stability of garnet and sulfur, performance of a high sulfur-loaded solid-state battery, and calculation of energy density. EXAMPLES

[0194] This example provides a description of the solid hybrid electrolytes of the present disclosure and provides examples of the construction and characterization of such electrolytes.

[0195] Flexible solid ionically conducting membrane with 3D garnet nanofiber network for lithium batteries Due to the highest specific capacity (3860 mA / g) and lowest negative electrochemical potential (~3.040 V vs. standard hydrogen electrode) of lithium, it is highly desirable to replace traditional ion intercalation anode materials with metallic lithium anodes beyond the state of the art in lithium-ion battery (LIB) technology. In this example, continuous Li + Garnet-type Li providing transport channels 6.4 La3Zr2Al 0.2 O 12 A three-dimensional (3D) Li-ion conducting ceramic network based on (LLZO) lithium ion conductor is described. The composite structure provides additional structural reinforcement that improves the mechanical properties of the polymer matrix. The flexible solid electrolyte composite membrane has a 2.5 × 10 -4 The membrane exhibited an ionic conductivity of 0.2 mA / cm for approximately 500 hours. 2 and a current density of 0.5mA / cm for over 300 hours 2 The dendrites in Li|electrolyte|Li symmetric cells can be effectively inhibited during repeated lithium stripping / plating at room temperature. These results provide an all-solid-state ionically conductive membrane that can be applied to flexible lithium-ion batteries and other electrochemical energy storage systems such as lithium-sulfur batteries.

[0196] This example describes a flexible solid-state lithium-ion conducting membrane based on a three-dimensional (3D) ion-conducting network and polymer electrolyte for lithium batteries. The 3D ion-conducting network is a percolating garnet-type Li2+ that enhances the ionic conductivity of the solid electrolyte membrane at room temperature and the mechanical strength of conventional polymer electrolytes. 6.4 La3Zr2Al 0.2 O 12 (L The membrane is based on a solid electrolyte nanofiber (LZO). The membrane effectively blocks lithium dendrites and therefore exhibits excellent electrochemical stability against high voltages and high mechanical stability. This work represents a major breakthrough in enabling high-performance lithium batteries.

[0197] In this study, we report a continuous Li-ion conducting membrane in a PEO-based composite electrolyte as an all-solid-state ion conducting membrane for lithium batteries. + Garnet-type Li providing transport channels 6.4 La3Zr2Al 0.2 O 12 We have successfully developed a three-dimensional (3D) ceramic network based on (LLZO) nanofibers. (a) By optimizing element substitution, we have achieved a 10 -3 Garnet-type lithium-ion conducting ceramics were selected as the inorganic component due to its multiple desirable physical and chemical properties, including (a) high ionic conductivity approaching 10000 S / cm, (b) good chemical stability to lithium metal, and (c) good chemical stability to air and moisture. Figure 47 shows the schematic structure of the 3D LLZO / polymer composite membrane. The LLZO porous structure consists of randomly distributed and interconnected nanofibers, which constitute a continuous lithium-ion conducting network. Then, Li salt / PEO polymer is filled into the porous 3D ceramic network to form the 3D garnet / polymer composite membrane. Different from the traditional method of fabricating polymer electrolyte, the 3D garnet / polymer composite membrane does not require mechanically mixing the filler with the polymer, instead, we can directly immerse the preformed 3D ceramic structure into the Li salt / polymer solution to obtain the desired polymer composite electrolyte hybrid structure, which simplifies the fabrication process and avoids the agglomeration of the filler.

[0198] Results and Discussion Figure 48 shows a schematic of the procedure for synthesizing flexible solid garnet LLZO nanofiber-reinforced polymer composite electrolyte. Garnet LLZO nanofibers were fabricated by electrospinning polyvinylpyrrolidone (PVP) polymer mixed with relevant garnet LLZO salts, as shown in Figure 48a, and then calcined in air at 800°C for 2 hours. The nanofibers were collected on a drum collector of the electrospinning setup by covering a thin nonwoven fabric.

[0199] A schematic fabrication of FRPC Li-ion conducting membrane with 3D porous garnet nanofiber network is shown in Figure 2b. A PEO polymer mixture with Li salt, such as lithium bis(trifluoromethane)sulfonimide (LiTFSI), is prepared. The Li salt / PEO polymer is then reinforced with 3D nanofibers to construct a composite electrolyte, which can be called fiber-reinforced polymer composite (FRPC) electrolyte membrane. Compared with filler-containing polymer electrolytes, the FRPC electrolyte membrane is believed to have superior mechanical properties due to the continuous nanofiber structure that maintains the framework of the 3D garnet nanofiber network and improves the integrity of the polymer electrolyte.

[0200] The morphology of the spun PVP / garnet salt nanofibers and calcined garnet nanofibers was characterized by scanning electron microscopy (SEM), as shown in Figure 48c and Figure 48e. Before calcination, the PVP / garnet salt nanofibers have a smooth surface and an average diameter of 256 nm. The corresponding diameter distribution is shown in Figure 48d. After calcination in air at 800 °C, the PVP polymer was removed to obtain garnet LLZO nanofibers. The average diameter of the nanofibers was reduced to 138 nm. The respective diameter distributions are shown in Figure 48f. After annealing, the garnet nanofibers were "interconnected" with each other to form a crosslinked 3D garnet nanofiber network. The large space volume between the nanofibers can facilitate Li-salt / polymer infiltration to form a composite membrane. The flexibility of the membrane is shown in Figure 48g. And by employing a flexible electrolyte membrane, a flexible solid-state lithium battery can be constructed. It should be noted that the design of flexible 3D ion-conducting networks mainly relies on ceramic garnet nanofibers, which have been shown to exhibit good ion conductivity and battery fabrication properties. For feasibility, thin and mechanically stable structures are desirable. To achieve thinner polymer composite electrolytes while maintaining good mechanical stability, several important parameters need to be considered, including the electrospinning process (e.g., collection time, drum rotation speed, syringe movement speed, etc.), preparation of the precursor solution (e.g., garnet salt concentration, polymer concentration, polymer molecular weight, solvent selection, etc.), as well as optimization of thermal annealing (e.g., heating rate, temperature, time, cooling rate, etc.).

[0201] Figure 49 shows the morphological characterization of the garnet nanofibers and the resulting FRPC electrolyte. As shown in Figure 49a, the garnet nanofibers were integrally joined at their intersections to form a crosslinked network. These interconnected garnet nanofibers provide continuous ion conduction pathways with extended long-range lithium transport channels, which should be superior to isolated particle fillers dispersed in a typical polymer matrix. Figures 49b and 49c show transmission electron microscopy (TEM) images of the garnet nanofibers. The garnet nanofibers have a polycrystalline structure consisting of interconnected small crystallites that make up long continuous nanofibers (Figure 49b). Figure 53 shows a magnified TEM image of the garnet nanofibers with an average grain size of 20 nm in diameter. Figure 49c shows the highly crystallized structure of the garnet grains.

[0202] The morphology of the FRPC electrolyte was investigated by SEM (Figures 49d-f). The FRPC electrolyte exhibited a smooth surface originating from the PEO-LiTFSI polymer (Figure 49d). Inside the FRPC electrolyte, a 3D porous garnet nanofiber network was observed to support the main structure of the composite, and the PEO-LiTFSI polymer was observed to infiltrate the porous garnet film and fill the spaces between the garnet nanofibers. The cross-sectional image of the FRPC electrolyte showed a thickness of 40-50 μm (Figure 49e). To improve the interphase contact between the garnet nanofibers and the PEO-LiTFSI polymer, the polymer melting temperature (T mThe FRPC electrolyte was heat-treated at 60 °C, slightly above the initial temperature, to allow the molten PEO-LiTFSI polymer to fully infiltrate the 3D porous garnet nanofiber network. As shown in Figure 49f, after heat treatment, sufficient garnet nanofibers were embedded in the PEO-LiTFSI polymer. The garnet nanofibers were enlarged to an average diameter of 500 nm by the PEO-LiTFSI polymer coating. The interconnected pores were filled with polymer to maintain good lithium ion transport. It is proposed that the FRPC electrolyte membrane has three ion-conducting pathways: the interconnected ceramic garnet nanofiber network, the continuous garnet fiber / polymer interface, and the Li-salt-containing polymer matrix. Due to the higher ionic conductivity of the garnet-type electrolyte than the Li-salt-containing polymer electrolyte, we believe that the former two ion-conducting pathways are the dominant factors to improve the ionic conductivity of the electrolyte membrane.

[0203] The formation of garnet nanofibers during the calcination process was investigated by thermogravimetric analysis (TGA). TGA was performed under air flow with a rapid heating rate of 10 °C / min. Figure 50a shows the TGA profile of the spun nanofibers containing PVP polymer and garnet precursor. The results indicate that the weight was stable above 750 °C and stable garnet nanofibers were formed. Figure 50b compares the TGA profiles of PEO / LiTFSI and FRPC electrolytes. Both electrolytes were thermally stable up to around 200 °C. In the rapid heating process, the polymer showed a large mass loss due to the fact that it started to decompose above 200 °C and almost completely decomposed around 400 °C. The slope at 400 °C was the decomposition of LiTFSI. In the case of FRPC electrolyte, the weight was stable at 500 °C, and the others were garnet nanofiber films due to the excellent stability of the garnet material in air. In the case of polymer electrolyte, the weight was stable at 650 °C, and the decomposed LiTFSI salt remained.

[0204] Thermal stability is an important consideration when using solid electrolytes, especially polymer electrolytes. Traditional liquid electrolytes, such as carbonate electrolytes, tend to cause thermal runaway when the battery is subjected to extreme conditions of short circuit, overcharging, and high temperature. Polymer electrolytes, due to their relatively high thermal stability, are a safer option than liquid electrolytes. Traditional polymer electrolytes are built on their own polymer structure and the filler cannot provide sufficient mechanical support for the electrolyte, so at high temperatures, especially above the polymer pyrolysis temperature, they will inevitably melt and shrink, which can lead to direct contact between the cathode and anode, which is a major safety concern. FRPC electrolytes can address this issue because the garnet nanofiber membrane in the polymer electrolyte provides a ceramic barrier that physically blocks contact between the cathode and anode even after the polymer is lost.

[0205] Figure 50c and Figure 50d compare the flammability tests of the conventional polymer electrolyte and the novel FRPC electrolyte developed in this study. The conventional polymer electrolyte was prepared by using garnet nanopowder (vs. 3D garnet network) as filler while PEO-LiTFSI polymer was prepared by the same method. The mass ratio of polymer and filler was controlled to 4·1. In Figure 50c, the polymer electrolyte ignited the moment it approached the ignition device and burned out quickly to ashes. This high flammability indicates the poor thermal stability of the polymer electrolyte. In comparison, the FRPC electrolyte showed outstanding thermal stability even when the polymer component was lost, and the garnet nanofiber membrane still kept its structure (Figure 50d). This low flammability that the FRPC electrolyte can provide enhances the safety of all lithium metal and lithium ion batteries.

[0206] The powder X-ray diffraction (XRD) pattern of the LLZO garnet nanofibers calcined at 800 °C for 2 h is shown in Figure 51a. Almost all the diffraction peaks are from the cubic phase garnet Li5La3Nb2O 12(JCPBS Card 80-0457). Li5La3M2O5 (M=Nb, Ta) is the first example of a fast lithium ion conducting garnet-like structure and is a representative structure that is widely used as a model to examine the garnet structure of LLZO materials. Therefore, we use the standard Li5La3Nb2O 12 XRD profiles were used to identify the synthesized garnet nanofiber structure. Trace amounts of La2Zr2O7 were identified, while other impurities were below the detection limit. TG results showed that the decomposition of the precursors to oxides was complete at about 750 °C. Upon further heating to 800 °C, the oxides reacted to form the cubic phase LLZO garnet structure. However, trace amounts of La2Zr2O7 phase could also be formed due to lithium loss at high temperatures.

[0207] The overall lithium ion conductivity of the FRPC electrolyte was characterized by electrochemical impedance spectroscopy (EIS). Figure 51b shows a typical Nyquist plot of the FRPC electrolyte sandwiched between stainless steel blocking electrodes in the frequency range of 1 Hz to 1 MHz. Each impedance profile shows a real axis intercept at high frequency, a semicircle at mid-frequency, and a sloping straight line at low frequency. The extended semicircle and semicircle intercepts on the real axis in the high-frequency and mid-frequency regions represent the bulk relaxation of the FRPC electrolyte. The low-frequency tail is due to the lithium ion migration and the surface inhomogeneity of the blocking electrodes. Figure 51c shows the Arrhenius plot of the FRPC electrolyte. The lithium ion conductivity was calculated based on the thickness of the FRPC electrolyte and the diameter of the stainless steel electrodes. The lithium ion conductivity of the cubic phase LLZO garnet pellets was calculated to be 10 -3 S / cm at room temperature, whereas lithium salt-filled PEO typically has a dielectric constant of 10 -6 ~10 -9 The conductive cubic LLZO garnet and lithium PEO combined in our FRPC electrolyte have a conductivity of the order of 2.5 × 10 -4 It can exhibit a fairly high ionic conductivity of 100 S / cm.

[0208] Another key factor determining the application of polymer electrolytes in high-voltage lithium batteries is the large electrochemical window. Figure 51d shows the results of the electrochemical window using lithium metal as the reference counter electrode and stainless steel as the working electrode. The linear sweep voltammetry (LSV) profile of the FRPC electrolyte used as the electrode is shown. The FRPC electrolyte exhibits a maximum of 6.0 V vs Li / Li + The results show a stable potential window of 0.1 to 1.0 V, indicating that this conductive film can meet most of the requirements for high-voltage lithium batteries.

[0209] A Li|FRPC electrolyte|Li symmetric cell was used to evaluate the mechanical stability of the FRPC electrolyte membrane against Li dendrites. In the charge-discharge process at constant current, lithium ions mimic the charge-discharge behavior of lithium metal batteries by plating / stripping the lithium metal electrode. Figure 52a shows a schematic diagram of the symmetric cell setup. The FRPC electrolyte membrane was sandwiched between two lithium metal foils and sealed into a coin cell. Figure 52b shows the mechanical stability of the FRPC electrolyte membrane against Li dendrites at 0.2 mA / cm 2 Figure 1 shows the voltage profile as a function of time for a cell with a FRPC electrolyte membrane cycled at a constant current density of 1000 V and a temperature of 15°C for over 230 h. The control cell was cyclically charged and discharged for 0.5 h. The positive voltages are Li-stripping and the negative voltage values ​​represent the Li-plating process. In the first 70 h, the cell voltage increased slightly from 0.3 V to 0.4 V and then stabilized at 0.4 V.

[0210] As shown in Figure 52c, when the test temperature was increased to 25°C, the voltage dropped to 0.3 V due to the improved ionic conductivity at high temperatures. In the subsequent long cycles, the voltage continued to drop to 0.2 V as the cycle time increased to 700 h (Figure 54). The voltage fluctuation was caused by the temperature change of the surrounding environment. As shown in Figure 55, two voltage profiles of the symmetric cell at two different stripping / plating process times were compared. The voltage hysteresis was obviously less with the cycle time. This voltage drop is quite different from the liquid electrolyte system, where the voltage generally increases with time, and is mainly due to the non-uniform Li deposition and violent electrolyte decomposition that results in an increase in impedance. A similar voltage drop has been observed in recent studies of polymer electrolytes, but the reason for the continued voltage drop with cycle time has not been explained. Based on our understanding, the voltage drop is attributed to the improvement of the interface between the electrolyte film and lithium metal upon repeated electrodeposition of Li, which is confirmed by the EIS spectra of the symmetric cell measured at 300, 500, and 700 hours (Figure 52d). The concave semicircle at low frequency indicates the decrease in the interfacial impedance between the electrolyte film and lithium metal during cycling. At high frequency (Figure 52e), the semicircle also becomes smaller with cycling time, indicating the decrease in the bulk impedance of the electrolyte film. At a current density of 0.5 mA / cm 2 52f), indicating good cycling stability with a long cycle life.

[0211] In this paper, we have synthesized a 3D garnet / polymer composite all-solid-state ion-conducting membrane for lithium batteries. A 3D garnet nanofiber network was fabricated by electrospinning and high-temperature annealing. The garnet nanofibers constituted an "interconnected" 3D structure that provided long-distance lithium ion transport pathways and augmented the polymer matrix by providing structural reinforcement. This flexible solid electrolyte composite membrane had a conductivity of 2.5 × 10 at room temperature.-4 The membrane exhibited an ionic conductivity of 0.2 mA / cm for approximately 500 hours. 2 and current densities of 0.5 mA / cm for 300 hours and over 300 hours 2 It is possible to effectively inhibit dendrites in the Li|electrolyte|Li symmetric cell during repeated lithium stripping / plating at room temperature. A voltage drop is observed with cycling time for the symmetric cell, which is attributed to the improvement of the interface upon repeated lithium electrodeposition. This example describes the development of 3D Li-ion conducting ceramic materials in solid electrolytes with anticipated applications in flexible lithium-ion batteries and other electrochemical energy storage systems such as lithium-sulfur batteries.

[0212] Although the present disclosure has been described with respect to one or more particular embodiments and / or examples, it will be understood that other embodiments and / or examples of the present disclosure are possible without departing from the scope of the present disclosure.

Claims

1. an inorganic solid electrolyte (SSE); a polymer material disposed on at least a portion or all of an outer surface of the solid electrolyte material; A solid hybrid electrolyte comprising:

2. 2. The hybrid electrolyte of claim 1 , wherein the SSE material is a monolithic SSE body or a mesoporous SSE body.

3. 10. The hybrid electrolyte of claim 1 , wherein the SSE material is a disk, a sheet, or a polyhedron.

4. The hybrid electrolyte of claim 1, wherein the polymer material has a thickness at one or more points between 10 nm and 10 microns.

5. 10. The hybrid electrolyte of claim 1 , wherein the SSE comprises a plurality of fibers or strands.

6. The hybrid electrolyte of claim 5 wherein the fibers are present as a woven or knitted substrate.

7. The hybrid electrolyte of claim 5 , wherein the fibers are randomly arranged or aligned.

8. 6. The hybrid electrolyte of claim 5 , wherein the fibers or strands of the inorganic SSE material form an interconnected 3D network.

9. 2. The hybrid electrolyte of claim 1 , wherein the SSE material comprises a lithium ion conducting SSE material, a sodium ion conducting SSE material, or a magnesium ion conducting SSE material.

10. The lithium ion conducting SSE material is a lithium perovskite material, Li 3 N, Li-β-alumina, lithium superionic conductor (LISICON), Li 2.88 P.O. 3.86 N 0.14 (LiPON), Li 9 AlSiO 8 , Li 10 GeP 2 S 12 10. The hybrid electrolyte of claim 9, wherein the lithium garnet material is selected from the group consisting of a lithium garnet material, a doped lithium garnet material, a lithium garnet composite material, and combinations thereof.

11. The lithium garnet material is a cation-doped Li 5 La 3 M 1 2 O 12 (However, M 1 is Nb, Zr, Ta, or a combination thereof), cation-doped Li 6 La 2 BaTa 2 O 12 , cation-doped Li 7 La 3 Zr 2 O 12 , and cation-doped Li 6 BaY 2 M 1 2 O 12 (However, M 1 11. The hybrid electrolyte of claim 10, wherein Nb, Zr, Ta, or a combination thereof, and the cation dopant is barium, yttrium, zinc, or a combination thereof.

12. wherein the lithium garnet material is Li 5 La 3 Nb 2 O 12 、Li 5 La 3 Ta 2 O 12 、Li 7 La 3 Zr 2 O 12 、Li 6 La 2 SrNb 2 O 12 、Li 6 La 2 BaNb 2 O 12 、Li 6 La 2 SrTa 2 O 12 、Li 6 La 2 BaTa 2 O 12 、Li 7 Y 3 Zr 2 O 12 、Li 6.4 Y 3 Zr 1.4 Ta 0.6 O 12 、Li 6.5 La 2.5 Ba 0.5 TaZrO 12 、Li 6 BaY 2 M 1 2 O 12 、Li 7 Y 3 Zr 2 O 12 、Li 6.75 BaLa 2 Nb 1.75 Zn 0.25 O 12 、Li 6.75 BaLa 2 Ta 1.7 5 Zinc 0.25 O 12 and combinations thereof.

13. The sodium ion conducting SSE material is β″-Al 2 O 3 , Na 4 Zr 2 S 2 P.O. 12 10. The hybrid electrolyte of claim 9, wherein the electrolyte is selected from the group consisting of NASICON, cation-doped NASICON, and combinations thereof.

14. The magnesium ion conducting SSE material is Mg 1+x (Al, Ti) 2 (P.O. 4 ) 6 10. The hybrid electrolyte of claim 9, wherein x is selected from the group consisting of: NASICON-type magnesium ion conducting materials; NASICON-type magnesium ion conducting materials; and combinations thereof.

15. the inorganic SSE has pores exposed at an outer surface of the inorganic SSE, and the hybrid electrolyte further comprises at least one cathode material and / or at least one anode material disposed in at least a portion of the pores; 2. The hybrid electrolyte of claim 1, wherein when at least one cathode material and at least one anode material are disposed in at least a portion of the pores, the at least one cathode material and at least one anode material are disposed in discrete and electrically isolated regions of the inorganic SSE.

16. The polymeric material may be selected from the group consisting of poly(ethylene) (PE), poly(ethylene oxide) (PEO), poly(propylene) (PP), poly(propylene oxide), polymethyl methacrylate (PMMA), polyacrylonitrile (PAN), poly[bis(methoxyethoxyethoxide)-phosphazene], poly(dimethylsiloxane) (PDMS), cellulose, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, polyvinylidene difluoride (PVdF), polyvinylpyrrolidone (PVP), polystyrene, sulfonates (PSS), polyvinyl chloride (PVC), poly(vinylidene chloride) polypropylene oxide, polyvinyl chloride (PVC) and polyvinyl chloride (PVC) groups.

10. The hybrid electrolyte of claim 1, comprising (e.g., is) a polymer selected from the group consisting of polyvinyl acetate, polytetrafluoroethylene, poly(ethylene terephthalate) (PET), polyimide, polyhydroxyalkanoate (PHA), PEO-containing copolymers (e.g., polystyrene (PS)-PEO copolymers and poly(methyl methacrylate) (PMMA)-PEO copolymers), polyacrylonitrile (PAN), poly(acrylonitrile-methyl acrylate copolymers), PVdF-containing copolymers, PMMA copolymers, derivatives thereof, and combinations thereof.

17. The hybrid electrolyte of claim 1 , wherein the polymeric material is a gel.

18. The gel is made of ethylene carbonate (EC), diethyl carbonate (DEC), dimethoxyethane (DME), dioxolane (DOL), N-propyl-N-methylpyrrolidinium bis(trifluoromethanesulfonyl)imide (PYR 13 TFSI), and combinations thereof, and / or LiPF 6 20. The hybrid electrolyte of claim 17 comprising a salt selected from the group consisting of LiTFSI, LiTFSI, and combinations thereof.

19. 18. The hybrid electrolyte of claim 17, wherein the polymeric material of the gel comprises (e.g. is) a polymer selected from the group consisting of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP copolymer), polyvinylpyrrolidone (PVP), PEO, PMMA, PAN, polystyrene (PS), polyethylene (PE), and combinations thereof.

20. The hybrid electrolyte of claim 1 , wherein the polymeric material comprises a metal salt.

21. The hybrid electrolyte of claim 1 , wherein the polymeric material comprises a ceramic filler.

22. 22. The hybrid electrolyte of claim 21 , wherein the ceramic filler is selected from the group consisting of conductive particles, non-conductive particles, and ceramic nanomaterials.

23. 13. A device comprising the hybrid electrolyte of claim 1.

24. The hybrid electrolyte; An anode; A cathode; Equipped with 24. The device of claim 23, wherein the hybrid electrolyte is disposed between the cathode and the anode.

25. 25. The device of claim 24, wherein the battery further comprises a current collector disposed on at least a portion of the cathode and / or the anode.

26. 26. The device of claim 25, wherein the current collector is a conductive metal or metal alloy.

27. 25. The device of claim 24, wherein the battery is a lithium ion conducting solid-state battery and the hybrid electrolyte is a lithium ion conducting SSE material.

28. 25. The device of claim 24, wherein the battery is a sodium ion conducting solid-state battery and the hybrid electrolyte is a sodium ion conducting SSE material.

29. 25. The device of claim 24, wherein the battery is a magnesium ion conducting solid-state battery and the hybrid electrolyte is a magnesium ion conducting SSE material.

30. 25. The device of claim 24, wherein the cathode and / or the anode comprise a conductive carbon material, the cathode material optionally further comprising an organic or gel ionically conductive electrolyte.

31. 25. The apparatus of claim 24, wherein the cathode comprises a material selected from sulfur, sulfur composites, and polysulfide materials, or is air.

32. 30. The device of claim 27, wherein the cathode comprises a material selected from the group consisting of lithium-containing cathode materials.

33. The lithium-containing cathode material is lithium nickel manganese cobalt oxide, LiCoO 2 , LiNi 1/3 Co 1/3 Mn 1/3 O 2 , LiNi 0.5 Co 0.2 Mn 0.3 O 2 , lithium manganese oxide (LMO), lithium iron phosphate (LFP), LiMnPO 4 , LiCoPO 4 , and Li 2 M.M. 3 O 8 33. The device of claim 32, wherein M is selected from the group consisting of: (wherein M is selected from Fe, Co, and combinations thereof).

34. 30. The device of claim 28, wherein the cathode comprises a material selected from sodium-containing cathode materials.

35. The sodium-containing cathode material is 2 V 2 O 5 , P2-Na 2/3 Fe 1/2 Mn 1/2 O 2 , Na 3 V 2 (P.O. 4 ) 3 , NaMn 1/3 Co 1/3 Ni 1/3 P.O. 4 , and Na 2/3 Fe 1/2 Mn 1/2 O 2 28. The device of claim 27, wherein the material is selected from the group consisting of: @graphene composites.

36. 36. The device of claim 35, wherein the cathode comprises a material selected from the group consisting of doped magnesium oxides.

37. 25. The device of claim 24, wherein the anode comprises a material selected from the group consisting of silicon-containing materials, tin and its alloys, tin / carbon, and phosphorous.

38. 25. The device of claim 24, wherein the anode comprises a material selected from the group consisting of lithium ion conducting anode materials.

39. The lithium ion conducting anode material is lithium carbide, Li 6 40. The device of claim 38, wherein the lithium-containing material is selected from the group consisting of C, and lithium titanate (LTO).

40. 40. The device of claim 38, wherein the anode is lithium metal.

41. 25. The device of claim 24, wherein the anode comprises a material selected from sodium ion conducting anode materials.

42. The sodium-containing anode material is 2 C 8 H 4 O 4 and Na 0.66 Li 0.22 Ti 0.78 O 2 42. The device of claim 41, selected from the group consisting of:

43. 42. The device of claim 41 , wherein the anode is sodium metal.

44. 25. The device of claim 24, wherein the anode is a magnesium-containing anode material.

45. 45. The device of claim 44, wherein the anode is magnesium metal.

46. 25. The device of claim 24, wherein the hybrid electrode, cathode, anode, and optionally the current collector form a cell, and wherein the battery comprises a plurality of the cells, each adjacent pair of the cells separated by a bipolar plate.

47. A conventional ion-conducting battery with a liquid electrolyte, the battery comprising an inorganic SSE or a solid hybrid electrolyte and a liquid electrolyte, the liquid electrolyte not being present as part of the solid hybrid electrolyte; 24. The device of claim 23, wherein the inorganic SSE material or the solid hybrid electrolyte is a separator of the conventional battery.

48. 48. The apparatus of claim 47, wherein the inorganic SSE is a F / S SSE.

49. 1. A method of making a solid hybrid electrolyte comprising the steps of: contacting the template with one or more SSE material precursors; Optionally, reacting the SSE material precursor; and heat treating the template with the solid inorganic material, whereby the template is removed and the inorganic SSE is formed; and contacting the calcined template with a polymeric material; Including, A solid hybrid electrolyte is formed.

50. 48. The method of claim 47, wherein the SSE material is a sol-gel precursor or a metal salt.

51. 49. The method of claim 47 or 48, wherein the template is a carbon template or a biomaterial template.

52. 52. The method of claim 51, wherein the carbon template is a fiber template.

53. 52. The method of claim 51, wherein the biomaterial template is a wood template or a plant template.