Member for exposure device, method for manufacturing member for exposure device, and member for composite exposure device

Glassy carbon exposure device members address thermal expansion and contamination issues by offering low thermal expansion, high hardness, and reduced weight, ensuring accurate and clean patterning with high-energy light sources.

JP2024153873AActive Publication Date: 2024-10-29NISSHINBO CHEM
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024126682
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-10-29
Estimated Expiration
2040-12-02

AI Technical Summary

Technical Problem

Existing exposure device members, such as pellicle frames and stage components, experience thermal expansion and deformation due to high-energy light sources, leading to reduced accuracy and potential contamination of silicon wafers, especially when using deep ultraviolet light or extreme ultraviolet light, which also causes impurity desorption and dust generation.

Method used

The use of glassy carbon materials with specific properties, including low density, low thermal expansion coefficient, high hardness, and resistance to impurity desorption, is introduced for exposure device members, manufactured through a process involving thermosetting resin molding and high-temperature firing, followed by polishing and grinding to achieve desired shapes and surfaces.

Benefits of technology

The glassy carbon members provide improved thermal stability, reduced weight, enhanced handling properties, and minimized contamination, maintaining high accuracy and reducing deformation during patterning processes, while being resistant to impurity desorption and dust generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153873000002
    Figure 2024153873000002
  • Figure 2024153873000001
    Figure 2024153873000001
Patent Text Reader

Abstract

To provide a member for an exposure device which is less likely to be thermally expanded while being lightweight, a method for manufacturing a member for an exposure device, and a member for a composite exposure device.SOLUTION: A member for an exposure device contains glassy carbon, wherein the member for the exposure device has a frame shape, and at least one surface of two surfaces positioned in a thickness direction of the member for the exposure device is a polished surface. A method for manufacturing a member for an exposure device includes: a molding step of molding a thermosetting resin material to produce a resin molding; and a sintering step of sintering the resin molding to obtain a glassy carbon body. A member for a composite exposure device includes the member for the exposure device.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a member for an exposure apparatus, a method for manufacturing a member for an exposure apparatus, and a member for a composite type exposure apparatus. [Background technology]

[0002] In the lithography process, which involves patterning semiconductor elements and the like on a silicon wafer, patterning is performed using an exposure device. A photomask, which is an exposure substrate, is used in the exposure device, and the circuit formed on the photomask is formed on the silicon wafer. If foreign matter adheres to the photomask or reticle during this process, it may cause defects such as short circuits in the pattern that is formed. For this reason, materials that do not emit dust or release components that cause foreign matter are selected for the exposure device components used in the exposure device. Similarly, high-purity materials that are highly resistant to exposure light and do not contaminate the silicon wafer itself are required. The main components for exposure apparatuses include (a) a pellicle frame, which is generally a rectangular frame with one end surface serving as a pellicle film installation surface, (b) a plate-shaped stage component on which a silicon wafer is placed, (c) a disk-shaped mirror component for position measurement, (d) an object-holding component such as a transport arm having a U-shaped transport section, and (e) other structural components. The pellicle frame forms a pellicle that has a function of protecting photomasks and reticles from dust by stretching a pellicle film on the pellicle film installation surface. Hereinafter, silicon wafers may be simply referred to as "wafers".

[0003] Conventionally, pellicle frames made of aluminum or aluminum alloys have been widely used, but pellicle frames made of other metals such as stainless steel and pellicle frames made of resins such as polyethylene have also been proposed (see, for example, Patent Documents 1 and 2). Moreover, for the above-mentioned stage parts, mirror parts, and exposure object holding members such as the transport arm, ceramic materials that are easy to purify and can also be used for complex surface shapes are generally used, for example, alumina and silicon carbide are widely used. In addition, a combination with ceramics having negative thermal expansion properties has also been proposed (for example, see Patent Document 3). It is also known that stage components are made of materials with a small linear expansion coefficient in order to improve positional accuracy. It is also known that the mirror surface of the mirror parts is formed by vapor deposition of metal, and that reflection is reduced on the parts other than the mirror surface. It is also known that the contact surface of the exposure object holding member such as the transfer arm that comes into contact with the wafer is tapered to reduce the impact on the wafer.

[0004] In recent years, there has been a demand for reducing the mass of exposure apparatus members in order to increase the moving speed of drive system members in lithography processes (exposure processes) and to improve the handleability of exposure apparatus members. For example, the density of aluminum, a material commonly used for pellicle frames, is 2.7 g / cm 3 However, in order to reduce the mass of the exposure apparatus components, it is effective to construct the pellicle frame from a material with a lower density than aluminum. For example, the above-mentioned resin pellicle frame can be considered as a pellicle frame made of a material with a lower density than aluminum. However, a resin pellicle frame undergoes significant thermal expansion when the temperature of the environment in which it is used rises, due to the fact that the linear expansion coefficient of resin is generally large. Normally, in a patterning process, an exposure light source is installed so that the pellicle frame is not directly exposed to light, but exposure generates stray light, and when this stray light hits the pellicle frame, the temperature of the pellicle frame rises. As described above, when a resin pellicle frame undergoes thermal expansion, there is a risk that the pellicle membrane stretched over the pellicle frame will wrinkle, peel off, tear, or the like.

[0005] Furthermore, in the case of stage parts, mirror parts, transport arms, and other members for holding exposed objects, alumina, which has low thermal expansion (linear expansion coefficient = 7.2 × 10 -6 / K, density=3.9g / cm 3 ), silicon carbide (linear expansion coefficient = 3.7 x 10 -6 / K, density=3.2g / cm 3 ) are used. These ceramics have a smaller linear expansion coefficient and density than metals, but as mentioned above, when the temperature of the component rises due to irradiation with exposure light, thermal expansion can deteriorate the exposure accuracy. Therefore, to further improve handling and exposure accuracy, materials with smaller linear expansion coefficients and densities are required. Also, materials with lower surface hardness than wafers are expected to reduce adverse effects on wafers. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2009-025559 A [Patent Document 2] JP 2018-028659 A [Patent Document 3] JP 2006-009088 A Summary of the Invention [Problem to be solved by the invention]

[0007] In recent years, in order to further improve the resolution of exposure patterns, the wavelength of the exposure light used during patterning has been shortened, and for example, deep ultraviolet light (DUV) and light in the region of wavelengths around 10 nm (EUV) have come to be used. When using these high-energy light sources, the temperature rise inside the exposure tool becomes significant, and it is estimated that depending on the component, the temperature may reach several hundred degrees Celsius. In particular, when irradiating these extremely short wavelength lights in a vacuum atmosphere, there is concern about the detachment of impurities and the like from the components used in the exposure tool due to gas flow, and it is thought that the effects of thermal expansion due to temperature rise will be greater. For example, in the case of a pellicle frame, not only the above-mentioned resin pellicle frame, but also an aluminum pellicle frame may expand when heated, causing wrinkles, peeling, tearing, etc. in the pellicle film stretched over the pellicle frame. In addition, in the case of stage parts, mirror parts, and exposed object holding members, there is a concern that thermal expansion may cause a decrease in positional accuracy. In addition, in any part or member, if it is in contact with the exposed object, there is a concern that it may affect the exposed object, and if it is a part or member facing the space in which the exposed object is placed, there is a concern that it may cause the detachment of impurities, etc.

[0008] Therefore, there is a demand for components for exposure apparatuses that are lightweight yet resistant to thermal expansion, thereby enabling an improvement in the movement speed of drive system components and excellent handling properties, and furthermore, that are resistant to deformation even during patterning using a high-energy light source.

[0009] In view of the above problems, an object of the present invention is to provide a member for an exposure apparatus, which is lightweight yet resistant to thermal expansion, a method for manufacturing a member for an exposure apparatus, and a composite member for an exposure apparatus. [Means for solving the problem]

[0010] As a result of extensive investigations aimed at solving the above problems, the inventors discovered that the above problems could be solved by making the exposure apparatus components contain glass-like carbon, and thus completed the present invention. That is, the present invention provides the following [1] to

[13] . [1] A component for an exposure device containing glassy carbon. [2] The density of the glassy carbon is 1.6 g / cm 3 The exposure apparatus member according to the above item [1], [3] The exposure apparatus member according to [1] or [2] above, wherein the vitreous carbon has a Shore hardness (HS) of 100 or more. [4] The linear expansion coefficient of the glassy carbon is 4.0 × 10 -6 / K or less. [5] A member for an exposure apparatus according to any one of the above [1] to [4], wherein the mass fraction of ash in the glassy carbon is 50 ppm or less. [6] 1,300 to 1,400 cm in the Raman spectrum of the glassy carbon -1 The peak intensity of the D band in the range of I D and 1,550~1,650cm -1 The G-band peak intensity I in the range G Peak intensity ratio I D / I G is 1.0 to 2.5, and the half width of the D band is 50 to 130 cm -1 The member for an exposure apparatus according to any one of the above [1] to [5], [7] A member for an exposure apparatus according to any one of the above [1] to [6], wherein at least one surface of the member for an exposure apparatus is a polished surface. [8] A method for producing an exposure apparatus member according to any one of the above items [1] to [7], A molding step of molding a thermosetting resin material to produce a resin molded body; and a firing step of firing the resin molded body to obtain a glass-like carbon body. [9] The method further includes a step of heating the resin molded body to a temperature of 150° C. or higher to make the resin molded body infusible prior to the firing step; The method for producing an exposure apparatus member according to the above-mentioned [8], wherein in the baking step, the infusible resin molded body is baked at 900 to 3,000°C.

[10] The method for manufacturing an exposure apparatus component described in [8] or [9] above, further comprising at least one of a polishing process step of polishing the glass-like carbon body and a grinding process step of grinding the glass-like carbon body into any desired shape.

[11] A composite member for an exposure apparatus, comprising the member for an exposure apparatus according to any one of the above [1] to [7] and a part made of a material different from that of the member for an exposure apparatus.

[12] A pellicle frame made of a component for an exposure apparatus according to any one of the above [1] to [7].

[13] A composite pellicle frame comprising the pellicle frame described in

[12] above and a component made of a material different from that of the pellicle frame. Effect of the Invention

[0011] According to the present invention, it is possible to provide a member for an exposure apparatus, which is lightweight yet resistant to thermal expansion, a method for manufacturing a member for an exposure apparatus, and a composite member for an exposure apparatus. [Brief description of the drawings]

[0012] [Figure 1] 1A and 1B are schematic external views showing an example of a pellicle frame, which is a component for an exposure apparatus according to an embodiment of the present invention, in which FIG. 1A is a plan view and FIG. 1B is a cross-sectional view taken along line IB-IB in FIG. 1A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The following describes the configuration and manufacturing method of an exposure apparatus member according to an embodiment of the present invention, and a composite exposure apparatus member. The exposure apparatus member is not limited to a pellicle frame, but may be any member used in an exposure apparatus, such as the above-mentioned stage parts, mirror parts, and object holding members such as a transport arm, or other structural parts. In the following description, in order to facilitate understanding, the drawings will be referred to as appropriate, and the various surfaces of the pellicle frame will be described using the symbols shown in the drawings, but the present invention is not limited to the embodiments shown in the drawings. Also, the drawings are shown in a schematic and exaggerated manner in order to facilitate understanding.

[0014] 1. Exposure equipment components An exposure apparatus member according to an embodiment of the present invention includes glassy carbon. The exposure apparatus members include movable parts in the exposure apparatus, parts that come into contact with an object to be exposed such as a wafer, and parts that face the space in which the object to be exposed is placed, etc. Specific parts included in the exposure apparatus members include a pellicle frame, a stage part having, for example, a plate-shaped part, a mirror part having, for example, a disk-shaped part used for position measurement, etc., an object to be exposed holding member such as a transport arm having a U-shaped transport part, and other structural parts, etc.

[0015] The glassy carbon contained in the above-mentioned exposure device member is obtained by forming a resin molded body by molding a thermosetting resin material into a predetermined shape, and then heat-treating (firing) this resin molded body at a high temperature. The process of forming a resin molded body by molding (molding process) and the process of firing the resin molded body to obtain a glassy carbon body (firing process) will be described later.

[0016] The density of glass-like carbon is less than 60% of the density of aluminum. In addition, the linear expansion coefficient of glass-like carbon is smaller than that of resin and aluminum. For example, the linear expansion coefficient of polyethylene constituting the above-mentioned resin pellicle frame is 110 to 130 × 10 -6 / K, the linear expansion coefficient of aluminum is 24×10 -6 / K, whereas the linear expansion coefficient of glassy carbon is, as described below, 4.0×10 -6 / K or less. For this reason, a pellicle frame containing glass-like carbon, which is one of the components for exposure apparatuses that contains glass-like carbon, is lighter than pellicle frames made of metals such as aluminum, which have been widely used in the past, and is less susceptible to thermal expansion (i.e., has a smaller linear expansion coefficient) than pellicle frames made of resin or metal. The pellicle frame containing the above-mentioned glassy carbon is lightweight and resistant to thermal expansion, and therefore when a pellicle film is stretched over the pellicle to form a pellicle, the movement speed of the pellicle can be improved and the handling properties can be improved. In addition, the pellicle film can be made less likely to deform even during patterning using a high-energy light source. In other words, when the exposure apparatus member containing the above-mentioned glassy carbon is a movable part that can move within the exposure apparatus, or a part that comes into contact with the exposed object, such as a part that supports the exposed object, it is possible to achieve both weight reduction and low thermal expansion. This makes it possible to improve the high-speed movement and handling properties of the exposure apparatus member, and to suppress the effects on the exposed object and the decrease in dimensional accuracy when the temperature rises.

[0017] In addition, glassy carbon has a unique cross-linked structure, which gives it a highly uniform structure, and it is harder than general graphite, so it is less likely to generate dust due to particle falling off.

[0018] The glassy carbon constituting the above-mentioned exposure device member is obtained by forming a resin molded body by molding a thermosetting resin material into a predetermined shape, as described above, and then heat-treating (firing) this resin molded body at a high temperature. Since the glassy carbon has already been subjected to a high-temperature thermal history through the above-mentioned heat treatment, even if it is heated by exposure, very few components are desorbed from the glassy carbon. This makes it possible to suppress the occurrence of growing foreign matter (haze) that may cause problems in patterning.

[0019] In addition, glassy carbon is close to an ideal black body and is easy to suppress light reflection. Therefore, for example, it has the advantage that it is easy to inspect for foreign objects attached to exposure device components. It is known that aluminum pellicle frames can be blackened by anodizing coating (alumite treatment) in an acidic solution and dyes. However, such anodized aluminum pellicle frames contain residual sulfate ions and nitrate ions contained in the acidic solution, and when the pellicle frame is used, for example, when it is exposed to a high vacuum, the desorbed nitrate ions react with ammonia to generate growing foreign objects, which may cause problems in patterning. In addition, there is a problem that the surface of the anodized coating is porous and prone to dust generation. In order to prevent these problems, it has been proposed to cover aluminum and its anodized coating with polymers by electrochemical coating, etc., but this creates other problems, such as the electrochemical coating film peeling off due to friction during handling and the film deteriorating due to exposure to light. As described above, the exposure apparatus member containing the glassy carbon does not easily generate dust, generates very little gas even in a high vacuum or high temperature environment, and is itself close to a black body. Therefore, even if the exposure apparatus member is a pellicle frame, no additional treatment is required as in the case of an aluminum pellicle frame, and there is no need to cover it with a polymer film. Furthermore, ceramic wafer holding members, such as transport arms, have a higher surface hardness than the wafer and can be adversely affected by impacts when they come into contact with the wafer; however, exposure object holding members, such as transport arms, which contain glassy carbon, have a lower surface hardness than ceramics and can reduce the impact on the wafer. That is, when the exposure apparatus member containing the above-mentioned glassy carbon is a part facing the space in which the exposure object is placed, dust generation and gas generation are unlikely to occur, and problems such as generation of foreign matter are unlikely to occur.

[0020] Furthermore, as described below, the flatness of the exposure apparatus member containing glassy carbon can be increased by polishing. Therefore, when the exposure apparatus member is a pellicle frame, elastic deformation of the pellicle frame is suppressed when a pellicle film is stretched on the pellicle frame or a photomask is bonded thereto, and thus distortion of the pellicle film and the photomask can be suppressed.

[0021] Furthermore, a pellicle frame containing the above-mentioned glassy carbon is advantageous in terms of rigidity compared to a resin pellicle frame, and the pellicle membrane is less likely to deform or break during manufacture or use of the pellicle. In addition, glassy carbon has high chemical resistance to all acids, bases, and organic solvents, which means that exposure equipment components that contain glassy carbon have the advantage of being less susceptible to corrosion.

[0022] The glass-like carbon may contain components (e.g., ash) that are inevitably contained during production. However, from the viewpoint of enabling the glass-like carbon to exhibit desired physical properties and from the viewpoint of preventing the above-mentioned impurities from eluting at high temperatures and high vacuum, it is preferable that the content of the above-mentioned components is small. Here, the ash content refers to components that are mainly derived from impurity metals that are mixed into the glass-like carbon during the manufacturing process of the glass-like carbon. In this specification, the term "glass-like carbon" also includes glass-like carbon that contains the above-mentioned ash content. The mass fraction of ash in the glassy carbon is preferably 50 ppm or less, more preferably 20 ppm or less, even more preferably 10 ppm or less, and most preferably 5 ppm or less, from the viewpoint of minimizing the inclusion of impurities and preventing their elution. The mass fraction of ash in the glassy carbon can be set within the above range by, for example, appropriately selecting the type of thermosetting resin material or implementing process improvements to reduce the inclusion of metal components when heat-treating a thermosetting resin at high temperature to obtain glassy carbon.

[0023] The density of the glass-like carbon constituting the exposure apparatus member is preferably 1.6 g / cm from the viewpoint of weight reduction. 3 Less than or equal to 1.58 g / cm 3 More preferably, 1.56 g / cm 3 The following is the result. There is no particular lower limit to the density of the glass-like carbon. However, from the viewpoint of ensuring the hardness of the glass-like carbon and a sufficient cross-linking structure between carbon atoms, and from the viewpoint of ease of production, it is preferably 1.45 g / cm. 3 It is. As a method for adjusting the density to the above numerical range, for example, there can be mentioned a method for appropriately setting the temperature reached when heat-treating a thermosetting resin at a high temperature to obtain glass-like carbon.

[0024] The Shore hardness (HS) of the glassy carbon constituting the exposure apparatus member is preferably 100 or more, from the viewpoint of easily suppressing dust generation. Glassy carbon has a high Shore hardness compared to that of general graphite (Shore hardness (HS) of about 50 to 80). This is due to the cross-linked structure that is characteristic of glassy carbon. When the Shore hardness (HS) of glassy carbon is 100 or more, the cross-linked structure develops to increase the uniformity of the structure, making it less likely to generate dust due to particle shedding as occurs with graphite. Therefore, even if an exposure apparatus component containing glassy carbon comes into contact with another component, there is little generation of particles due to friction.

[0025] The Shore hardness (HS) of the glassy carbon constituting the above-mentioned exposure apparatus member is more preferably 100-150, even more preferably 110-140, and even more preferably 115-135.

[0026] In this specification, the Shore hardness (HS) is a value measured using a Shore hardness tester, type D, and is specifically measured by the method described in the Examples. As a method for adjusting the Shore hardness (HS) to the above-mentioned range, for example, the heat treatment temperature when heat-treating a thermosetting resin at a high temperature to obtain glassy carbon can be appropriately set.

[0027] The linear expansion coefficient of the glassy carbon constituting the exposure apparatus member is preferably 4.0×10 at 200° C. from the viewpoints of suppressing dimensional changes in the exposure apparatus member and reducing the influence on members other than the exposure apparatus member. -6 / K or less, more preferably 3.5×10 -6 / K or less, more preferably 3.0×10 -6 / K or less. By setting the linear expansion coefficient of the glassy carbon within the above range, for example, when the exposure apparatus component is a pellicle frame, it becomes easy to suppress dimensional changes in the pellicle and ensure adhesion between the pellicle frame and the pellicle film. Also, for example, when the exposure apparatus component is a stage component, it becomes easy to ensure accuracy when driving the stage component and dimensional accuracy of the entire holding part for holding the exposed object. There is no particular lower limit to the linear expansion coefficient. From the viewpoint of ensuring the hardness of the glassy carbon and a sufficient cross-linked structure between carbons, and from the viewpoint of ease of manufacture, it is, for example, 2.0×10 -6 / K. As a method for adjusting the linear expansion coefficient to the above numerical range, for example, there can be mentioned appropriately setting the temperature reached when heat-treating a thermosetting resin at a high temperature to obtain glass-like carbon.

[0028] The glassy carbon constituting the exposure apparatus member preferably has a Raman spectrum of 1,300 to 1,400 cm, from the viewpoint of easily obtaining properties such as low density and low thermal expansion due to sufficient development of a cross-linked structure between carbon atoms. -1 The peak intensity of the D band in the range of I D and 1,550~1,650cm -1 The G-band peak intensity I in the range G Peak intensity ratio I D / I G is 1.0 to 2.5, and the half-width of the D band is 50 to 130 cm -1 It is. The D band is a peak due to defects in the graphite structure, and the G band is a peak due to the ideal graphite structure of carbon materials. D / I GThe fact that the value of I is 1 or more and the half-width of the D band is within the above range means that the carbon structure has many disordered and cross-linked structures and the crystal growth is not as advanced as that of graphite. D / I G If the half-width of the D band is within the above range, the cross-linked structure between carbon atoms is sufficiently developed, making it easier to obtain properties such as low density and low thermal expansion. More preferably, I D / I G is 1.0 to 2.0, and the half-width of the D band is 70 to 130 cm -1 It is. Above peak intensity ratio I D / I G As a method for setting the value within the above range, for example, the temperature reached when the thermosetting resin is heat-treated at a high temperature to obtain glass-like carbon can be appropriately set.

[0029] At least one of the surfaces of the member for an exposure apparatus is preferably a polished surface. For example, when the exposure apparatus member is a pellicle frame, it is preferable that at least one of the pellicle film installation surface and the mask bonding surface is a polished surface.When the exposure apparatus member is a stage part or an object holding member such as a transport arm, it is preferable that the surface that contacts the object is a polished surface.When the exposure apparatus member is a mirror part, it is preferable that the surface including the area that becomes the mirror surface is a polished surface. The polished surface may be a surface having a predetermined surface roughness or may be a mirror-finished surface. In this specification, the term "mirror-finished surface" refers to a surface that has been subjected to mirror finishing using an abrasive such as abrasive grains for mirror finishing.

[0030] The exposure apparatus member may consist of only the exposure apparatus member made of glass-like carbon, or may be a composite including the exposure apparatus member and a part made of a material different from the exposure apparatus member, as described below. In this specification, the composite is referred to as a "composite type exposure apparatus member." Composite type exposure apparatus members will be described later.

[0031] The exposure apparatus member may be composed of only glass-like carbon, or may contain components other than glass-like carbon for the purpose of increasing the strength and other physical properties of the exposure apparatus member. The other components include carbon fiber, graphite, silicon, and the like. The mass fraction of components other than glassy carbon in the above-mentioned exposure apparatus member is preferably 50 mass % or less, more preferably 20 mass % or less, and even more preferably 5 mass % or less, from the viewpoints of ensuring the hardness of the glassy carbon, a sufficient crosslinked structure between carbon atoms, and the like, and from the viewpoints of ease of production.

[0032] 2. Pellicle frame The pellicle frame according to the embodiment of the present invention is one of the above-mentioned exposure apparatus components. The pellicle frame may consist of only a pellicle frame, or may be a composite including the pellicle frame and a component made of a material different from that of the pellicle frame, as described below. In this specification, the composite is referred to as a "composite pellicle frame." The composite pellicle frame will be described later. Next, an example of a pellicle frame according to an embodiment of the present invention is shown in FIG. As shown in the plan view of Fig. 1(a), the pellicle frame 10 shown in Fig. 1 has a rectangular frame shape in plan view, with an opening 10c provided in the center. Each corner 10d where the long straight portion 10e and the short straight portion 10f intersect is rounded. Although not shown in Fig. 1, the pellicle frame may be provided with a countersunk portion or a through hole, which will be described later. As shown in the cross-sectional view of Figure 1(b), of the two surfaces located in the thickness direction of the pellicle frame 10, one is a pellicle film mounting surface 10a on which the pellicle film is mounted, and the other is a mask bonding surface 10b on which a photomask is bonded. In addition, an adhesive layer or a pressure-sensitive adhesive layer, which will be described later, may be provided on the pellicle film mounting surface 10a and the mask bonding surface 10b of the pellicle frame 10, but these layers are omitted from the illustration in FIG. 1(b).

[0033] A pellicle frame containing glassy carbon is lighter than a metal pellicle frame, and is less susceptible to thermal expansion than a resin pellicle frame or a metal pellicle frame. Therefore, when a pellicle film is stretched to form a pellicle, the movement speed of the pellicle can be improved and the handling properties can be improved. In addition, the pellicle film can be made less likely to deform even in patterning using a high-energy light source. In addition, due to the crosslinking structure unique to glassy carbon, dust generation due to particle drop-off is less likely to occur, and since glassy carbon has a high-temperature thermal history during production, there are very few components that are desorbed even when heated. Furthermore, compared to a resin pellicle frame, it is advantageous in terms of rigidity, and the pellicle film is less likely to deform or break during production or use of the pellicle. In addition, since glassy carbon has high chemical resistance, corrosion and the like are less likely to occur, and since glassy carbon is close to an ideal black body, it is easy to suppress light reflection.

[0034] At least one of the pellicle membrane mounting surface (10a in FIG. 1(b)) and the mask bonding surface (10b in FIG. 1(b)) of the pellicle frame is preferably a polished surface. More preferably, both the pellicle membrane mounting surface and the mask bonding surface are polished surfaces. The polished surfaces may be mirror-finished surfaces. By polishing at least one of the pellicle film installation surface and the mask bonding surface, these surfaces can be smoothed and the flatness can be increased. As a result, the flatness of the pellicle frame is increased, making it easier to suppress distortion during bonding with the pellicle film and the photomask.

[0035] The flatness of the above-mentioned pellicle frame is preferably 50 μm or less, from the viewpoint of suppressing elastic deformation of the frame when the pellicle film is stretched onto the pellicle frame or when the photomask is adhered, and suppressing distortion of the pellicle film and the photomask. In this specification, the flatness of a pellicle frame, when the pellicle frame has a polygonal frame shape, is a value calculated by measuring the height of each corner of the pellicle frame and all straight lines (reference numerals 10e, 10f in Figure 1(a)) between a pair of adjacent corners (reference numeral 10d in Figure 1(a)), and calculating the difference between the highest point and the lowest point among the distances of each measurement point from a virtual plane derived from the measured heights by the least squares method; in more detail, the flatness is measured by the method described in the examples. In order to bring the flatness into the above-mentioned numerical range, for example, the pellicle film mounting surface and the mask bonding surface of the pellicle frame containing glassy carbon may be polished.

[0036] The shape of the pellicle frame when viewed in a planar view is not limited to the rectangular frame shape as shown in Figure 1(a), but can be any shape, for example, a polygonal frame shape such as a square, hexagon, etc.

[0037] There is no particular limit to the size of the pellicle frame when viewed in plan, and it may be an appropriate size depending on the size of the area to be exposed, the configuration of the exposure device, etc., and taking into consideration ease of manufacture, etc. In the case of a rectangular pellicle frame, for example, the outer length (see symbol L1 in FIG. 1(a)) can be 50 to 300 mm, the width (see symbol L2 in FIG. 1(b)) can be 50 to 300 mm, and the width of the frame portion (see symbol W in FIG. 1(b)) can be 1 to 50 mm.

[0038] The thickness of the pellicle frame (see symbol D in FIG. 1(b)) is not particularly limited, and may be appropriately determined depending on the strength and specifications of the device to be introduced, and on ease of manufacture, etc. The thickness of the pellicle frame may be, for example, 0.5 to 6.0 mm.

[0039] The pellicle frame according to one embodiment of the present invention has, for example, a polygonal frame shape and has corners. In general, it has a quadrangular frame shape such as a rectangle as shown in FIG. 1(a). The corner where the straight line portions of the pellicle frame intersect may be rounded as shown in the corner 10d shown in FIG. 1(a), or may be chamfered with a plane extending in the thickness direction (the direction shown by the symbol D in FIG. 1(b)). In addition, the pellicle frame may be provided with, for example, a through hole or a countersunk portion. The through hole can be used, for example, for ventilation. The countersunk portion can be used, for example, as a gripping portion or a positioning portion during transportation.

[0040] 3. Manufacturing method for exposure device components The exposure apparatus member according to the embodiment of the present invention can be manufactured by a manufacturing method including the following steps. A process for molding thermosetting resin materials to produce resin molded bodies (molding process) A step of sintering the resin molded body to obtain a glass-like carbon body (sintering step).

[0041] It is preferable that the manufacturing method for the exposure apparatus component further includes at least one of a step of polishing the glass-like carbon body (polishing step) and a step of grinding the glass-like carbon body into any shape (grinding step). For example, when the exposure apparatus member is a pellicle frame, it is preferable to process at least one of the pellicle film installation surface and the mask bonding surface in the polishing process. When the exposure apparatus member is a stage part, it is preferable to process the surface on which the exposed object is placed in the polishing process. When the exposure apparatus member is a mirror part, it is preferable to process the surface including the area that will become the mirror surface in the polishing process. When the exposure apparatus member is an exposed object holding member such as a transport arm, it is preferable to process the surface that comes into contact with the exposed object in the polishing process. By making each of the above-mentioned surfaces into polished surfaces through a polishing process, the surfaces of these surfaces can be controlled to any roughness, and can be made to have high smoothness or a predetermined surface roughness. For example, when the member for the exposure apparatus is a pellicle frame, by increasing the smoothness of the pellicle film installation surface and the mask bonding surface, it is possible to make it difficult for the reticle film and the photomask to be distorted. In addition, when the member for the exposure apparatus is an object holding member such as a stage part or a transport arm, it is possible to easily suppress the influence on the object by making the contact surface with the object a predetermined surface roughness. In addition, when the member for the exposure apparatus is a mirror part, by increasing the smoothness of the area that becomes the mirror surface and making the other area a predetermined surface roughness, the exposure light is reflected with high precision by the mirror surface, and reflection in the other area is suppressed, making it easier to reflect the exposure light as intended. Furthermore, for example, when the exposure apparatus component is a pellicle frame, the grinding process can include forming the outer shape of the pellicle frame, processing it into a frame shape, forming through holes and countersunk portions, etc. When the exposure apparatus component is a stage part, a mirror part, or an exposure object holding member such as a transport arm, processing for forming the outer shapes of these parts can be performed in the grinding process.

[0042] There is no particular restriction on the order of the polishing step and the grinding step, and for example, (i) the polishing step may be followed by the grinding step, (ii) the grinding step may be followed by the polishing step, or (iii) at least a part of the polishing step and the grinding step may be carried out in parallel. In the case of (i) above, polishing can be performed relatively easily in the polishing process. In the case of (ii) above, the area to be polished in the polishing process can be reduced. In the case of (iii) above, the time required for the entire process can be easily shortened.

[0043] Furthermore, there is no particular restriction on the order of the firing step and the polishing and grinding steps. For example, (iv) the polishing and grinding steps may be performed after the firing step, (v) at least a part of the polishing step may be performed before the firing step, or (vi) at least a part of the grinding step may be performed before the firing step. In the case of (iv) above, the work in the firing step and the setting of the manufacturing conditions are easy, while in the cases of (v) and (vi) above, the steps performed after the firing step can be simplified. In this specification, the glassy carbon body obtained by firing the resin molded body and before being subjected to the polishing and grinding steps may be referred to as a "base body for exposure apparatus members".

[0044] The method for producing an exposure apparatus member preferably further includes, prior to the baking step, a step of infusibility-immobilizing the resin molded body by heating the resin molded body to a temperature of 150° C. or higher. In the baking step, the infusibility-immobilized resin molded body is preferably baked at 900 to 3,000° C. In this case, the order of the infusibilizing step, the polishing step, and the grinding step is not particularly limited.

[0045] [Molding process] In the molding step, a thermosetting resin material that serves as a carbon source for the glassy carbon is molded to produce a resin molded body. The raw material for the glassy carbon is a thermosetting resin material that contains a resin component that becomes non-graphitizable carbon by heat treatment, specifically, phenol-formaldehyde resin, furan-based resin, polycarbodiimide resin, etc. The thermosetting resin materials are generally in a powder or liquid state, and therefore it is desirable to obtain a resin molded product by molding the materials using a molding method, such as molding or cast molding, suited to the properties of the respective resins.

[0046] In order to obtain a dense resin molded body suitable for an exposure device member, it is preferable to use a liquid thermosetting resin material as the thermosetting resin material, pour the liquid thermosetting resin material into a mold, heat it to a predetermined temperature, and perform cast molding to produce a resin molded body. The liquid thermosetting resin material may contain a resin component and a solvent. Examples of liquid thermosetting resin materials include resol-type phenol-formaldehyde resin solutions, polycarbodiimide resin solutions, and furfuryl alcohol polymers. Examples of the solvent used together with the resin component include alcohols such as methanol, chlorine-based organic solvents such as perchloroethylene, toluene, N,N-dimethylformamide (DMF), water, etc. From the viewpoint of moldability, etc., alcohols such as methanol, toluene, DMF, water, etc. are preferred.

[0047] In the molding step, it is preferable to heat the thermosetting resin material while bringing the material into contact with an air-permeable member at least in part. It is more preferable to arrange the thermosetting resin material in a planar shape and heat the thermosetting resin material by contacting a sheet-shaped breathable member with at least one surface of the thermosetting resin material arranged in the planar shape. It is also possible to arrange the thermosetting resin material between a pair of sheet-shaped breathable members and heat the thermosetting resin material. Heating may be performed by using a breathable member having a shape surrounding the thermosetting resin material and contacting the inner edge of the breathable member with the thermosetting resin material. A breathable member having a shape surrounding the thermosetting resin material and a sheet-shaped breathable member may be used in combination. In the molding process, a liquid thermosetting resin material is preferably used as the thermosetting resin material, and this liquid thermosetting resin material is poured into a mold and heated at a predetermined temperature to perform cast molding to form a solid resin molded body. By heating a thermosetting resin material in contact with an air-permeable member, the thermosetting resin material is heated uniformly and degassed uniformly via the air-permeable member. In particular, when a thermosetting resin material is arranged in a planar shape and heated in contact with at least one surface of the material in a sheet-like air-permeable member, the surface in contact with the air-permeable member is heated and degassed uniformly. By uniformly heating and degassing in this way, a homogeneous glass-like carbon body can be easily obtained, and the thermosetting resin material is less likely to crack due to gas remaining inside.

[0048] In the molding process, in order to prevent the generation of bubbles due to the evaporation of the solvent, it is preferable to heat the resin solution while gradually increasing the temperature until the temperature reaches a predetermined level. The temperature can be determined, for example, according to the vapor pressure and boiling point of the solvent contained in the resin solution. The heating time until the temperature reaches the desired level is preferably 10 to 50 hours, for example, according to the size of the molded product. An example of a sheet-like breathable member is a sheet made of water-repellent fibers such as a mesh filter. A breathable member having a shape surrounding a thermosetting resin material can be obtained by cutting out a sheet-like breathable member and processing it into a frame shape, or by combining a plurality of sheet-like breathable members processed into a strip shape.

[0049] In addition, by producing a resin molded body having an arbitrary shape in the molding process, the grinding process described later may be omitted or simplified. For example, when producing a pellicle frame as a member for an exposure apparatus, by producing a resin molded body having a frame shape in the molding process, the grinding process described later may be omitted or simplified. In other words, a member for an exposure apparatus may be manufactured by a method in which a resin molded body having an arbitrary shape such as a frame shape is produced in the molding process and a grinding process is not performed, or a resin molded body having an arbitrary shape such as a frame shape is produced in the molding process, so that the amount of processing in the grinding process is reduced.

[0050] [Infusible process] From the viewpoint of enhancing the chemical stability of the resin molded body, it is preferable to provide an infusible step prior to the baking step, in which the resin molded body is heated to a temperature of 150° C. or higher to make it infusible. The resin molded product obtained by molding the thermosetting resin material undergoes an infusibility process, whereby the resin component is cured to become a cured resin molded product. The heating in the infusible step varies depending on the type of resin, but is preferably carried out so that the temperature reached is more preferably 170° C. or higher, and even more preferably 200° C. or higher. The atmosphere during heating is not particularly limited, and heating can be performed, for example, in the air. Examples of the device used for infusibility include a natural convection dryer, a forced convection dryer, and a hot plate.

[0051] [Coating process] A coating step of coating the infusible resin molded body with an antistatic agent may be provided prior to the baking step. By providing the coating step, it becomes easier to prevent impurities from being mixed in or pores from being formed in the exposure apparatus member due to adhesion of trace amounts of metal components contained in the environment. The antistatic agent includes an ionic surfactant and a nonionic surfactant. Examples of the ionic surfactant include cationic surfactants, anionic surfactants, and amphoteric surfactants.

[0052] [Firing process] In the firing step, the resin molded body, preferably the resin molded body after the infusible treatment, is fired at a high temperature to obtain a glassy carbon body (base material for exposure device members). The firing step is preferably carried out under an inert atmosphere such as nitrogen or argon, or -3 ~10 -1 The process is carried out under a vacuum of about Torr. The firing step preferably includes a first heating step in which heating is performed at 900 to 1,100° C., and a second heating step in which heating is performed at a temperature higher than that in the first heating step. In the second heating step, heating is performed to a temperature higher than 1,100° C. and not higher than 3,000° C., and the crystal properties of the glassy carbon can be controlled by adjusting the heating temperature and holding time.

[0053] In the second heating step, the glassy carbon may be highly purified by heating while passing a purified gas such as chlorine gas through the glassy carbon. Examples of the purified gas include fluorine gas, chlorine gas, dichlorodifluoromethane, dichlorofluoromethane, and carbon tetrachloride. The firing temperature in the first heating step is preferably 900 to 1,100°C, more preferably 930 to 1,050°C, and even more preferably 950 to 1,000°C, from the viewpoints of uniformity of the obtained glass-like carbon body and prevention of breakage and cracking, and in the second heating step, the firing temperature is preferably 1,100 to 3,000°C, more preferably 1,150 to 2,500°C, and even more preferably 1,200 to 2,000°C, from the viewpoints of carbon structure and control of its physical properties. The firing apparatus is not particularly limited as long as it can achieve the above firing temperature in the above atmosphere, and various types can be used, for example, an electric furnace, a lead hammer furnace, a vacuum furnace, etc.

[0054] From the viewpoint of preventing cracks and impurities from being mixed in the resulting glass-like carbon body, it is preferable that after obtaining a resin molded body in the above-mentioned molding step, a baking step is carried out after a non-melting step and a coating step.

[0055] The glass-like carbon body obtained by molding and sintering the above-mentioned thermosetting resin material as a raw material has a cross-linked structure characteristic of glass-like carbon. When this cross-linked structure is developed, the structure becomes more uniform, and dust generation due to particle falling off, as in the case of graphite, is less likely to occur. As a result, it becomes easier to suppress particle generation. Whether or not the material is glassy carbon can be confirmed by the presence or absence of the above-mentioned D band and G band in a Raman spectrum obtained by Raman spectroscopy. Methods for developing the crosslinked structure and enhancing the uniformity of the structure include appropriately setting the heating rate of the heat treatment in the molding step or the infusible step, or using an air-permeable material in the molding step to make the structure of the resin molded body uniform, and appropriately setting the heating rate and ultimate temperature in the baking step.

[0056] [Polishing process] In the polishing process, lapping and polishing are performed to obtain a base material for an exposure device member with good flatness. Furthermore, by adjusting the grain size of the abrasive grains, it is possible to finish the surface to any desired roughness. The polishing process may be carried out in two stages, and may include a primary polishing process in which the surface of the glassy carbon body that will become the pellicle membrane mounting surface or the mask bonding surface is processed to a predetermined thickness, and a secondary polishing process in which it is further processed to have a predetermined surface roughness or less.

[0057] The primary polishing process can be carried out, for example, by polishing to a depth of 0.3 to 3.0 mm using a polishing device such as a lapping machine with SiC abrasive grains or B4C abrasive grains having a grain size of #1000 to #2000. The secondary polishing process can be carried out by performing mirror finishing using, for example, alumina-based mirror finish abrasive grains or diamond-based mirror finish abrasive grains. In the secondary polishing process, the abrasive grains used are for mirror finishing and are very fine, which makes it possible to reduce the depth of damage to the surface of the glass-like carbon body caused by polishing and the thickness (modification depth) of the modified layer formed on the surface of the glass-like carbon body by polishing.

[0058] By undergoing the above-mentioned polishing process, for example, when the component for an exposure apparatus is a pellicle frame, the above-mentioned pellicle film mounting surface and mask bonding surface can be polished to improve the flatness of the pellicle film mounting surface and mask bonding surface.

[0059] [Grinding process] In the grinding process, the glassy carbon body is ground. For example, when the exposure apparatus member is a pellicle frame, the glassy carbon body is ground into a frame shape, or a through hole or a countersunk portion is formed in the glassy carbon body. In the grinding process, a corner may be processed into an R shape, such as the corner 10d of the pellicle frame 10 shown in FIG. 1(a). Any tool can be used for the grinding process, for example, a machining center equipped with a high-hardness grinding tool can be used. In the case of an exposure object holding member such as a transfer arm, the contact surface that comes into contact with the wafer can be tapered.

[0060] 4. Composite exposure equipment components A composite member for an exposure apparatus according to an embodiment of the present invention includes the above-mentioned member for an exposure apparatus and a part made of a material different from that of the member for an exposure apparatus. Moreover, a composite pellicle frame according to an embodiment of the present invention includes the above-mentioned pellicle frame and a part made of a material different from that of the pellicle frame. Examples of materials constituting the above-mentioned components that are different from the members of the exposure apparatus and the materials that are different from the pellicle frame include aluminum, resin, and stainless steel.

[0061] The shape of each of the above components is not particularly limited and any shape can be used, but for example, the shape may be the same as the above-mentioned exposure apparatus member in a plan view. In the case of a composite pellicle frame, for example, the shape of the above components may be the same as the frame shape of the pellicle frame. For example, when the exposure apparatus member is a pellicle frame, the above-mentioned part is provided on at least one of the pellicle film installation surface and the mask bonding surface of the pellicle frame via an adhesive layer or a pressure-sensitive adhesive layer. By providing the above-mentioned parts, it becomes easier to increase the strength and rigidity of the above-mentioned composite exposure apparatus member compared to the above-mentioned exposure apparatus member, and the above-mentioned composite pellicle frame compared to the above-mentioned pellicle frame. EXAMPLES

[0062] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples in any way.

[0063] The physical properties of the glassy carbon material used in the manufacture of the pellicle frames of the following Examples, and the physical properties of the pellicle frames of the following Examples, were measured and evaluated according to the following procedures.

[0064] <density> The mass and volume of the glassy carbon body serving as the base material for the exposure apparatus member were measured, and the former was divided by the latter to calculate the density of the glassy carbon constituting the exposure apparatus member.

[0065] <Shore hardness (HS)> One end face of the glass-like carbon body was measured at five different random locations using a Shore hardness tester, Model D, manufactured by Imai Seiki Co., Ltd., and the average value was taken as the Shore hardness (HS) of the glass-like carbon.

[0066] <Linear expansion coefficient> The linear expansion coefficient was measured using a thermomechanical analyzer TMA8310 (Rigaku). The reference specimen was SiO2 with a diameter of φ5 × 10 mm. The measurement sample was prepared by grinding the original material for exposure equipment components to a diameter of φ5 × 10 mm. The measurement conditions were a temperature increase of 10°C / min up to 200°C under nitrogen flow. The linear expansion coefficient was calculated from the change in the height of the test piece.

[0067] <Ash content> The exposure device component raw material was crushed into a powder to facilitate incineration, then placed in a platinum crucible, and the weight of the sample before treatment was measured. It was incinerated at 800°C in oxygen in a muffle furnace. After confirming that no carbon remained, the weight of the residue was measured as ash, and the amount of ash contained in the exposure device component raw material was calculated.

[0068] <Raman peak intensity ratio> A Raman spectroscopic measurement was performed on the main surface of each sample using a microscopic laser Raman spectrometer (LabRAM manufactured by HORIBA Scientific Co., Ltd.) using a 532 nm Nd:YVO4 laser. -1 The peak intensity of the D band in the range of I D , and 1,550~1,650cm -1 The G-band peak intensity I in the range G From the peak intensity ratio I D / I G was calculated.

[0069] <Accelerated exposure test> Accelerated exposure tests were conducted on the original materials for exposure equipment components using an ArF excimer laser. The tests were conducted with a 193 nm ArF laser and an output of 3 mJ / cm. 3 The test was performed under conditions of a total exposure dose of 1 kJ. The surfaces of the exposure device component master bodies were observed using an optical microscope before the start of the test and after the test was completed to check for any changes in the surfaces before and after the exposure.

[0070] <Ion elution test> The exposure apparatus component master body was immersed in deionized water and left for 2 hours at 90° C. Thereafter, the amount of desorbed ions eluted in the deionized water was quantified using ion chromatography.

[0071] <Flatness of the original material for exposure equipment components> The flatness of the exposure apparatus component original was measured by the following procedure: the height of each corner of the exposure apparatus component original and the straight line between a pair of adjacent corners were measured at 5 mm intervals, a least-squares plane (virtual plane) was calculated, and the flatness of the exposure apparatus component original was calculated as the difference between the farthest point above the least-squares plane (highest point) and the farthest point below the least-squares plane (lowest point) among the distances of each measurement point.

[0072] [Production Example 1] As the thermosetting resin material, a methanol solution of resol-type phenol-formaldehyde resin was used. Two sheets of fluororesin nonwoven fabric, which are sheet-like breathable members, were prepared, and a polytetrafluoroethylene (PTFE)-coated aluminum mold was placed between the upper and lower nonwoven fabrics to form the sides. The thermosetting resin material was placed in the mold and cast-molded to produce a square flat resin molded body with a length of 250 mm, a width of 250 mm, and a thickness of 5 mm. The cast molding was performed in an oven by gradually increasing the temperature from room temperature to 90°C over 20 hours. After removing the upper and lower nonwoven fabrics and the molds, the resin molded body was cured and further infusible in an oven to produce a cured resin molded body. The cured resin molded body was heat-treated in a vacuum furnace in a vacuum atmosphere of 0.01 Torr by gradually increasing the temperature from room temperature to 1,000°C as a first heating step, and further by gradually increasing the temperature from 1,000°C to 1,750°C as a second heating step, to obtain a rectangular plate-shaped glassy carbon body made of glassy carbon and measuring approximately 200 mm in length, approximately 200 mm in width, and approximately 4 mm in thickness.

[0073] The measurement results of the above-mentioned physical properties of the above-mentioned glassy carbon body are shown in Table 1. For reference, Table 1 also shows the density, Shore hardness (HS), and linear expansion coefficient of aluminum (A5052) as Reference Example 1 and polyethylene (HDPE) as Reference Example 2. The Shore hardness of Reference Example 1 was measured in the same manner as in Example 1. The densities and linear expansion coefficients of Reference Examples 1 to 3 were general values ​​found in dictionaries, various documents, and the like.

[0074] [Table 1]

[0075] As shown in Table 1, the glass-like carbon body of Production Example 1 produced through the above-mentioned steps had a Raman peak intensity ratio I D / I GThe value of is 1.86, which is greater than 1, and the Raman D band half width is 75.5 cm -1 So, 50~130cm -1 From the fact that the hardness is in the range, it can be seen that the crystal structure of the carbon is disturbed and the cross-linked structure is developed to provide a high degree of uniformity in the structure. As is clear from the comparison with aluminum, the glassy carbon body of Production Example 1 has a high Shore hardness and a low linear expansion coefficient, and even compared with polyethylene and alumina, the glassy carbon body of Production Example 1 has a low linear expansion coefficient, and it can be seen that the glassy carbon body of Production Example 1 is made of glassy carbon suitable for use as a member for an exposure apparatus. Furthermore, as is clear from a comparison between Production Example 1 and Reference Example 1, the glass-like carbon body of Production Example 1 has a lower density than aluminum, and it can be understood that the weight of exposure apparatus components can be significantly reduced. Furthermore, as is clear from a comparison with Production Example 1 and Reference Example 3, the glassy carbon body of Production Example 1 has a smaller linear expansion coefficient and a lower density than ceramics, and therefore it can be understood that when used as a stage part, a mirror part, or a member for holding an exposed object such as a transport arm, the positional accuracy can be improved.

[0076] Furthermore, as shown in Table 1, the results of the accelerated exposure test showed that no changes were observed on the surface of the exposure apparatus component raw material of Manufacturing Example 1 even after exposure, indicating that the exposure apparatus component raw material containing glassy carbon has high light resistance. Furthermore, as shown in Table 1, the results of the ion elution test showed that SO4 2- is less than 5ppb, NH4 + It is clear that the amount of components eluted from the exposure apparatus member master batch of Production Example 1 is extremely small.

[0077] [Example 1] The glass-like carbon body produced in Production Example 1 was subjected to polishing and grinding in the following procedure to produce a pellicle frame of Example 1. The pellicle film mounting surface and the mask bonding surface of the glassy carbon body were polished to 0.5 mm or more using a lapping machine with #1000 SiC abrasive grains as the primary processing. As the secondary processing, the surfaces of the pellicle film mounting surface and the mask bonding surface were mirror-finished with alumina-based mirror-finishing abrasive grains, and finished to a thickness of 3 mm. The glassy carbon body thus obtained, with its upper and lower surfaces mirror-finished, was ground using a machining center equipped with diamond tools to finish the outer shape (L1 and L2 in Fig. 1(b)) to 150 mm x 110 mm, and the width of the frame part (W in Fig. 1(b)) to 2 mm. In addition, for each straight part of the frame part, a countersunk hole with a diameter of 1.5 mm and a depth of 1 mm was provided from the center of the thickness direction (direction D in Fig. 1(b)) of the outer side toward the width direction of each frame part (direction W in Fig. 1(b)) at a position between the center of the straight part from the center to one end and the opposite end, sandwiching the center when viewed in a plane. In this way, a pellicle frame was produced.

[0078] The pellicle frame containing the glass-like carbon of Example 1 obtained through the above polishing and grinding processes was able to have a flatness of less than 20 μm. In addition, the pellicle frame of the above-mentioned Example 1 has a density of aluminum (2.68 g / cm 3 ) and linear expansion coefficient (24×10 -6 / K), the mass can be reduced by about 40% or more compared to an aluminum pellicle frame having a similar shape, and the linear expansion when heated from room temperature to 200°C can be suppressed to about 10% of the linear expansion of the aluminum pellicle frame. In addition, as a resin pellicle frame, a polyethylene pellicle frame (linear expansion coefficient 110 to 130×10) having a similar shape can be used. -6 / K), it can be suppressed to about 2%. [Explanation of symbols]

[0079] 10: Pellicle frame 10a: Pellicle membrane installation surface 10b: Mask bonding surface 10c: opening

Claims

1. A member for an exposure apparatus comprising glassy carbon, the exposure apparatus member is frame-shaped, A member for an exposure apparatus, wherein at least one of two surfaces positioned in a thickness direction of the member for an exposure apparatus is a polished surface.

2. The density of the glassy carbon is 1.6 g / cm 3 2. The member for an exposure apparatus according to claim 1, wherein:

3. 3. The member for an exposure apparatus according to claim 1, wherein the vitreous carbon has a Shore hardness (HS) of 100 or more.

4. The linear expansion coefficient of the glassy carbon is 4.0×10 -6 The member for an exposure apparatus according to any one of claims 1 to 3, wherein the surface roughness is 1 / K or less.

5. 5. The member for an exposure apparatus according to claim 1, wherein the mass fraction of ash in the glassy carbon is 50 ppm or less.

6. The glassy carbon has a Raman spectrum of 1,300 to 1,400 cm -1 The peak intensity I of the D band in the range D and 1,550 to 1,650 cm -1 The G band peak intensity I in the range G Peak intensity ratio I D / I G is 1.0 to 2.5, and the half width of the D band is 50 to 130 cm -1 The member for an exposure apparatus according to any one of claims 1 to 5,

7. 7. The member for an exposure apparatus according to claim 1, wherein both of two surfaces positioned in a thickness direction of the member for an exposure apparatus are polished surfaces.

8. A method for producing an exposure apparatus member according to any one of claims 1 to 7, comprising the steps of: A molding step of molding a thermosetting resin material to produce a resin molded body; and a firing step of firing the resin molded body to obtain a glass-like carbon body.

9. The method further includes a step of heating the resin molded body to a temperature of 150° C. or higher to make the resin molded body infusible prior to the firing step, 9. The method for manufacturing an exposure apparatus member according to claim 8, wherein the infusible resin molded body is baked at 900 to 3,000° C. in the baking step.

10. 10. The method for manufacturing a member for an exposure apparatus according to claim 8, further comprising at least one of a polishing process step of polishing the glass-like carbon body and a grinding process step of grinding the glass-like carbon body into an arbitrary shape.

11. 8. A composite member for an exposure apparatus, comprising: the member for an exposure apparatus according to claim 1; and a part made of a material different from that of the member for an exposure apparatus.

12. A pellicle frame comprising the member for an exposure apparatus according to any one of claims 1 to 7.

13. A composite pellicle frame comprising the pellicle frame according to claim 12 and a component made of a material different from that of the pellicle frame.

Citation Information

Patent Citations

  • Reflection type mask substrate

    JP1997142996A

  • Electron gun and electron beam exposure device

    JP2004259478A

  • Corrosion-resistant member

    JP2007101523A

  • High efficiency replicated x-ray optics and fabrication method

    US6278764B1

  • Carbon material for positive electrode of lithium air battery and lithium air battery

    WO2014065082A1