Tire tread, and side wall reinforcement rubber composition of run flat tire
A rubber composition with a phenolic resin and diene rubber blend addresses the lack of handling stability and fuel efficiency in tire treads, and prevents tire collapse in run-flat tires at 0 kPa air pressure.
Patent Information
- Application Number
- JP2023067596
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2043-04-18
AI Technical Summary
Existing tire tread rubber compositions fail to achieve both excellent handling stability and low fuel consumption, and sidewall reinforcing rubber compositions for run-flat tires do not prevent tire collapse at 0 kPa air pressure.
A rubber composition containing 0.5 to 30 parts by mass of a phenolic resin with a dodecanediamine-derived structural unit, blended with diene rubber, silica, carbon black, and other additives, enhances tire tread and sidewall reinforcement.
The composition produces tires with improved handling stability and low fuel consumption, and run-flat tires that can travel a certain distance at 0 kPa air pressure.
Smart Images

Figure 2024154020000001 
Figure 2024154020000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a tire tread rubber composition that can be used to produce tires that have excellent driving stability and low fuel consumption, and to a sidewall reinforcing rubber composition for run-flat tires that can run a certain distance even when the tire air pressure is 0 kPa. [Background technology]
[0002] A tire tread is the rubber part of a car tire that comes into contact with the road surface. Various tread patterns have been devised to achieve the desired performance. Separately, the rubber portion of the tire tread is a composition, which is a blend of various materials to obtain desired performance properties.
[0003] Run-flat tires are tires that can be driven a certain distance even if the air pressure of the tire becomes 0kPa due to a puncture, etc., and allow the vehicle to be driven to the nearest workshop without changing into a spare tire. According to ISO, run-flat tires are stipulated to be able to be driven 80km at 0kPa air pressure and a speed of 80km / h. The structure of run-flat tires can be roughly divided into those in which the sidewalls of the tire are reinforced with reinforcing rubber and those in which a ring-shaped core is inserted inside. The rubber composition of the present application is for use as a sidewall reinforcing rubber in the former type of tire. The sidewall reinforcement rubber needs to have a certain degree of rigidity so that the tire does not collapse even when the air pressure is 0 kPa. In addition, tire tread rubber and sidewall reinforcing rubber of run-flat tires can be used in common due to their physical properties.
[0004] One of the performance requirements for tire tread rubber is driving stability. In addition, with the recent rise in energy prices, there is a demand for tires with low fuel consumption. Although low fuel consumption is a cost issue, it is an essential theme for continuing sustainable development. There has been a demand for a tire tread rubber composition that can achieve both steering stability and low fuel consumption, but such a tire tread rubber composition has not existed until now. Furthermore, there has not been a sidewall reinforcing rubber composition for run-flat tires that, when used as a sidewall reinforcing rubber for run-flat tires, can prevent the tire from collapsing even when the air pressure is 0 kPa.
[0005] Patent Document 1 aims to provide a tire that is excellent in durability, can suppress the decrease in complex modulus due to temperature rise, can improve steering stability over a wide speed range, and is inexpensive, but there is room for improvement in fuel efficiency and as a sidewall reinforcing rubber composition for run-flat tires. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent Publication No. 2008-050431 [Patent Document 2] Patent Publication No. 2000-080205 [Patent Document 3] Special table 2021-004270
[0007] Patent Document 2 aims to provide a rubber composition for tire treads that can reduce rolling resistance (RR) and improve fuel economy without impairing the braking and cornering performance of automobiles on wet road surfaces, and a pneumatic tire using the rubber composition, but there is room for improvement in steering stability and as a sidewall reinforcing rubber composition for run-flat tires. Patent Document 3 relates to a phenolic resin that has an excellent elastic modulus when compounded with rubber, but it is difficult to achieve both steering stability and low fuel consumption. In addition, there is room for improvement as a sidewall reinforcing rubber composition for run-flat tires. Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention provides a tire tread rubber composition capable of producing a tire having excellent driving stability and low fuel consumption, and a sidewall reinforcing rubber composition for a run-flat tire capable of running a certain distance even when the tire air pressure is 0 kPa. [Means for solving the problem]
[0009] Per 100 parts by mass of diene rubber, A rubber composition comprising 0.5 to 30 parts by mass of a phenolic resin having at least one structural unit derived from dodecanediamine, the structural unit having a linear or branched carbon chain and optionally an unsaturated bond in the molecule. Effect of the Invention
[0010] The rubber composition can be used for a tire tread rubber composition that can be used to produce tires that have excellent driving stability and low fuel consumption, and for a sidewall reinforcing rubber composition for run-flat tires that can run a certain distance even when the tire air pressure is 0 kPa. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The following shows an example of a tire tread rubber according to the present invention that can be used to produce a tire that has excellent driving stability and low fuel consumption, and a sidewall reinforcing rubber composition for a run-flat tire that can run a certain distance even when the tire air pressure is 0 kPa.
[0012] Examples of the phenols (P) used in the present invention include phenol, cresol, xylenol, nonylphenol, para-tertiary-butylphenol, para-secondary-butylphenol, naphthol, catechol, resorcinol, hydroquinone, methylhydroquinone, dimethylhydroquinone, etc. Phenol is more preferred.
[0013] The raw material from which the phenolic resin having at least one structural unit derived from dodecanediamine is made is dodecanediamine (D). The two amino groups of dodecanediamine may be any positional isomer, and the dodecane skeleton may be linear or branched. It may also have an unsaturated bond. A more preferred dodecanediamine (D) is a linear dodecanediamine that does not have an unsaturated bond. An even more preferred dodecanediamine (D) is 1,12-dodecanediamine.
[0014] The amount of dodecanediamine (D) used when obtaining a phenolic resin having at least one structural unit derived from dodecanediamine is 20 to 80 parts by mass, more preferably 30 to 70 parts by mass, per 100 parts by mass of the phenols (P).
[0015] As the aldehyde (F) used in obtaining a phenolic resin having at least one structural unit derived from dodecanediamine, any aldehyde (F) that is usable in the production of a phenolic resin can be used. For example, formaldehyde, paraformaldehyde, trioxane (metaformaldehyde), etc. can be used alone or in combination of two or more. In addition, aldehydes (F) previously dissolved in water can also be used. The amount of the aldehydes (F) added is 1 to 20 parts by mass, more preferably 5 to 15 parts by mass, as an active ingredient, per 100 parts by mass of the phenols (P).
[0016] When obtaining a phenolic resin having at least one structural unit derived from dodecanediamine, pure water can be added for dilution. The amount of pure water added is 25 to 125 parts by mass, more preferably 50 to 100 parts by mass, per 100 parts by mass of the phenol (P).
[0017] In a method for obtaining a phenolic resin having at least one structural unit derived from dodecanediamine, a predetermined amount of phenol (P), dodecanediamine (D) and pure water are added, and the mixture is heated to 100° C. with stirring. A predetermined amount of aldehyde (F) is added dropwise thereto over 0.5 to 3.5 hours, more preferably over 1 to 3 hours, and the mixture is allowed to react for 2 to 6 hours, more preferably over 3 to 5 hours. The temperature of the heater is set to 200° C., and the reaction is carried out for 0.5 to 3.5 hours, more preferably 1 to 3 hours. Then, the heater temperature is set to 180°C, and the unreacted monomer is removed by distillation under vacuum to obtain the product.
[0018] Although the detailed mechanism of the above reaction is unclear, it is thought to be a three-component reaction involving dodecanediamine (D), aldehydes (F), and phenols (P) leading to resinification.
[0019] Examples of diene rubbers used as tire tread rubber and sidewall reinforcing rubber for run-flat tires include styrene-butadiene rubber (SBR), butadiene rubber (BR), isoprene rubber (IR), butyl rubber, and natural rubber (NR). These components can be used alone or in combination of two or more kinds.
[0020] The amount of the phenol resin having at least one structural unit derived from dodecanediamine in the rubber composition of the present application is 0.5 to 30 parts by mass, and more preferably 5 to 20 parts by mass, per 100 parts by mass of the total diene rubber.
[0021] The rubber composition of the present application may contain silica, which is called white carbon in the tire industry. The amount of silica to be added is 1 to 200 parts by mass, more preferably 20 to 120 parts by mass, per 100 parts by mass of the total diene rubber.
[0022] The rubber composition of the present invention may contain carbon black in addition to silica. The amount of carbon black is 0.5 to 200 parts by mass, and more preferably 1 to 120 parts by mass, per 100 parts by mass of the total diene rubber. The total amount of silica and carbon black is preferably 1 to 200 parts by mass, and more preferably 20 to 120 parts by mass, per 100 parts by mass of the diene rubber in total.
[0023] The rubber composition of the present application may contain a coupling agent. In particular, when silica is used, it is preferable to contain a coupling agent. The amount of the coupling agent is 0.5 to 20 parts by mass, more preferably 2 to 10 parts by mass, per 100 parts by mass of the diene rubber in total. An antioxidant can also be blended in. The blending amount of the antioxidant is 0.1 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the total diene rubber.
[0024] The rubber composition of the present application may contain zinc white. The amount of zinc white to be compounded is 0.1 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the total diene rubber. The rubber composition of the present application may further contain stearic acid in an amount of 0.1 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the total diene rubber.
[0025] The rubber composition of the present application may contain an extender oil, the amount of which is 1 to 50 parts by mass, and more preferably 5 to 30 parts by mass, per 100 parts by mass of the total diene rubber. Oil sulfur can also be blended in. The blending amount of oil sulfur is 0.1 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the total diene rubber.
[0026] The rubber composition of the present application may contain a vulcanization accelerator. The amount of the vulcanization accelerator is 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the diene rubber in total. A plurality of types of vulcanization accelerators may be used in combination.
[0027] The present invention will be described in more detail below with reference to examples, comparative examples, test examples, etc., but the present invention is not limited to these examples. EXAMPLES
[0028] <Synthesis of phenolic resin A (phenolic resin having at least one structural unit derived from dodecanediamine)> A reactor equipped with a stirrer, a reflux condenser, and a thermometer was charged with 100 g of phenol, 42 g of dodecanediamine, and 75 g of pure water. The temperature was raised to 100°C, and then 32 g of 37% aqueous formaldehyde solution was added dropwise over 2 hours. The mixture was then reacted under reflux for 4 hours, heated to 200°C, and reacted for 2 hours. The temperature was then lowered to 180°C, and the mixture was distilled under vacuum to remove unreacted monomers, and then discharged to obtain phenolic resin A (phenolic resin of Example 1).
[0029] <Synthesis of phenolic resin B (phenolic resin having at least one structural unit derived from dodecanediamine)> A reactor equipped with a stirrer, a reflux condenser, and a thermometer was charged with 100 g of phenol, 48.2 g of dodecanediamine, and 75 g of pure water. The temperature was raised to 100°C, and then 36 g of 37% aqueous formaldehyde solution was added dropwise over 2 hours. The mixture was then reacted under reflux for 4 hours, heated to 200°C, and reacted for 2 hours. The temperature was then lowered to 180°C, and the mixture was distilled under vacuum to remove unreacted monomers, and then discharged to obtain phenolic resin B (phenolic resin of Example 2).
[0030] <Synthesis of phenolic resin C (not a phenolic resin having at least one structural unit derived from dodecanediamine)> A reactor equipped with a stirrer, a reflux condenser, and a thermometer was charged with 100 g of phenol, 31 g of triethylenetetramine, and 75 g of pure water. The temperature was raised to 100°C, and then 43.3 g of 37% aqueous formaldehyde solution was added dropwise over 2 hours. The mixture was then reacted under reflux for 4 hours, heated to 200°C and reacted for 2 hours. The temperature was then lowered to 180°C, and the mixture was distilled under vacuum to remove unreacted monomers, and then discharged to obtain phenolic resin C (phenolic resin of Comparative Example 1).
[0031] <Method of measuring softening point> The softening points of phenolic resin A, phenolic resin B, phenolic resin C, and phenolic resin D and phenolic resin E described below were measured using an Elex Scientific vapor phase softening point measuring device EX-719PD. The heating rate was 2.5°C / min. The evaluation criteria are that the softening point is in the range of 70°C or higher and 150°C or lower, which is pass, and anything else is fail. If the softening point is less than 70°C, the reinforcing effect will be insufficient, and if the softening point is more than 150°C, workability will be poor.
[0032] <Method of preparing tire tread composition> The components other than the vulcanization accelerators 1 and 2 and the oil sulfur were mixed in the mixing ratios (parts by mass) shown in Table 1 in an internal Banbury mixer for 10 minutes, and then the vulcanization accelerator and the oil sulfur were added and mixed for another 2 minutes to obtain tire tread compositions of Examples 1 and 2 and Comparative Examples 1, 2 and 3. The resulting rubber composition was press-vulcanized in a specified mold at 170° C. for 10 minutes to obtain a vulcanized rubber test piece. The materials shown in Table 1 are as follows: *1 SBR rubber: ENEOS Materials, SBR-1502 *2BR rubber: ENEOS Materials, BR01 *3 Silica: Tosoh Silica, Nipsil AQ *4 Carbon black: Tokai Carbon Co., Ltd., Seast 6 *5 Phenolic resin D: Aica Kogyo Co., Ltd., BRM-845 (cashew-modified phenolic resin) *6 Phenolic resin E: BASF KORESIN resin (sold as a tackifier) *7 Stearic acid: NOF Corporation, Tsubaki *8 Anti-aging agent: Seiko Chemical Co., Ltd., Ozonone 6C *9 Zinc oxide: 3 types of zinc oxide manufactured by Seido Chemical Industry Co., Ltd. *10 Coupling agent: Evonik, Si69 (bis[3-(triethoxysilyl)propyl]tetrasulfide) *11 Extending oil: Aromax 3, manufactured by ENEOS *12 Oil sulfur: Dispersible powder sulfur manufactured by Yabu Shoten *13 Vulcanization accelerator 1: Sancerer CM-G, manufactured by Sanshin Chemical Industry Co., Ltd. *14 Vulcanization accelerator 2: Sancerer D, manufactured by Sanshin Chemical Industry Co., Ltd.
[0033] <Type A hardness measurement method> The test piece obtained in the <Method of preparing a tire tread composition> was subjected to a type A hardness measurement. The measurement temperature was 23±2° C., and the value was measured for 0.5 seconds. The judging criteria are: Type A hardness of 68 or more is pass, and anything below 68 is fail.
[0034] <Method for measuring storage modulus E' at 20℃> The test specimen obtained in the <Method of preparing tire tread composition> was measured with a fully automatic viscoelastic analyzer VR-7130 manufactured by Ueshima Seisakusho under the conditions of an initial strain of 10%, an amplitude of ±2%, a frequency of 10 Hz, and a temperature of 20° C. The results are shown in Table 2. The evaluation criteria are as follows: a storage modulus E' at 20°C of 6.5 GPa or more is pass, and a value less than 6.5 GPa is fail. This value is an index of hardness, and if it passes, it means that the steering stability is excellent.
[0035] <Tan δ at 60℃> The test specimen obtained in <Method of producing tire tread composition> was measured for tan δ under conditions of initial strain of 10%, amplitude of ±2%, frequency of 10 Hz, and temperature of 60° C. The results are shown in Table 2. The criterion for the judgment is that a Tan δ value at 60° C. of less than 0.1 is pass, and a value of 0.1 or more is fail. Tan δ at 60°C is an index of rolling resistance, and if it passes, it means that the tire has excellent "fuel efficiency."
[0036] <Handling stability> A pneumatic tire (trial tire: size 195 / 65 R15) was manufactured using the composition obtained in the <Method of manufacturing a tire tread composition>. Four of the pneumatic tires were mounted on an automobile, and a running sensory test was carried out by a test driver. A test driver drove at 120km / h and, when changing lanes, rated the controllability on a scale of 1 to 5. The higher the score, the better the controllability, with 5 to 3 being a pass and 2 to 1 being a fail.
[0037] The rubber compositions of Examples 1 and 2, which contain 0.5 to 30 parts by mass of a phenolic resin having at least one structural unit derived from dodecanediamine, in which the carbon chain is linear or branched and optionally has an unsaturated bond, in the molecule, per 100 parts by mass of diene rubber, passed all tests for softening point, type A hardness, storage modulus E' at 20°C, Tan δ at 60°C, and handling stability. They are judged to be excellent in handling stability and "low fuel consumption."
[0038] Comparative Example 1, which is not a rubber composition containing 0.5 to 30 parts by mass of a phenol resin having at least one structural unit derived from dodecanediamine, the carbon chain of which is linear or branched and optionally having an unsaturated bond in the molecule, per 100 parts by mass of diene rubber, passed the softening point, storage modulus E' at 20°C, and handling stability tests, but failed the Type A hardness and Tan δ at 60°C. In Comparative Example 2 using a cashew-modified phenolic resin, like Comparative Example 1, the softening point at 20° C., storage modulus E′, and handling stability were acceptable, but the type A hardness and Tan δ at 60° C. were unacceptable. These materials are considered to be inferior in "fuel economy" and lack rigidity when used as sidewall reinforcing rubber for run-flat tires. In Comparative Example 3, which used KORESIN, a tackifier, the softening point was acceptable, but the type A hardness, storage modulus E' at 20°C, Tan δ at 60°C, and handling stability were unacceptable.
[0039] [Table 1]
[0040] [Table 2]
Claims
1. Relative to 100 parts by mass of diene rubber, A rubber composition comprising 0.5 to 30 parts by mass of a phenolic resin having at least one structural unit derived from dodecanediamine, the structural unit having a linear or branched carbon chain and optionally an unsaturated bond in the molecule.
2. The rubber composition according to claim 1, wherein the dodecanediamine-derived structural unit of the phenolic resin is derived from 1,12-dodecanediamine, and the softening point of the phenolic resin is 70° C. or higher and 150° C. or lower.
3. Relative to 100 parts by mass of diene rubber, In addition to 0.5 to 20 parts by mass of a phenolic resin having at least one structural unit derived from dodecanediamine, the carbon chain of which is linear or branched and which optionally has an unsaturated bond in the molecule, The tread rubber or run-flat tire sidewall reinforcing rubber composition according to claim 1 or 2, comprising 1 to 200 parts by mass of silica, 0.5 to 20 parts by mass of a coupling agent, 0.1 to 10 parts by mass of an antioxidant, and 0.1 to 10 parts by mass of a vulcanization accelerator.
Citation Information
Patent Citations
Resin composition comprising benzoxadine ring-containing thermosetting resin
JP2010053324A
Thermosetting resin comprising copolymer having benzoxazine ring
JP2010053325A
Rubber composition containing main chain benzoxazine and method for producing the same
JP2018524438A
Rubber composition for tires and pneumatic tire using the same
JP2021063184A
Rubber composition for tire tread and pneumatic tire using the same
JP2000080205A