Asphalt paving mixture
Patent Information
- Application Number
- JP2023067602
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-30
AI Technical Summary
【0010】 本発明によれば、カーボンニュートラル又はカーボンネガティブに寄与し得るアスファルト混合物を提供することができる。
Smart Images

Figure 2024154024000001 
Figure 2024154024000002 
Figure 2024154024000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an asphalt mixture. [Background technology]
[0002] Asphalt mixture is a composite material mainly used for asphalt pavement of roads, and is obtained by mixing aggregates made of minerals such as stones, sand, and stone powder with asphalt (a residue of fossil fuels). During mixing, the aggregates are heated to about 200°C with a dedicated burner, and the asphalt is heated electrically to about 160°C to 180°C to soften the asphalt and mix it with the aggregate.
[0003] As described above, asphalt mixtures are made from aggregates (minerals) and asphalt, and emit carbon dioxide, a greenhouse gas, when transporting the materials, and also emit carbon dioxide when heated during production. Therefore, it can be said that asphalt mixtures are not suitable for the carbon neutral era, and countermeasures are required. Patent Document 1 describes a method for producing asphalt mixtures that can reduce the carbon dioxide emissions generated during the production of asphalt mixtures. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2021-075907 Summary of the Invention [Problem to be solved by the invention]
[0005] The method for producing an asphalt mixture described in Patent Document 1 involves a process for separating and capturing carbon dioxide generated during drying of aggregate and fixing the captured carbon dioxide in the aggregate, which requires large-scale equipment and leads to increased costs.
[0006] The present invention has been made in consideration of the above-mentioned conventional problems, and an object of the present invention is to provide an asphalt mixture that can contribute to carbon neutrality or carbon negativeness. [Means for solving the problem]
[0007] One aspect of the present invention that solves the above problems is as follows. (1) An asphalt mixture comprising at least asphalt, aggregate, a filler, and biochar.
[0008] (2) The asphalt mixture described in (1) above, wherein the biochar is in granular form.
[0009] (3) The asphalt mixture according to (1) or (2), containing more than 0% by mass and not more than 10% by mass of the biochar. Effect of the Invention
[0010] According to the present invention, it is possible to provide an asphalt mixture that can contribute to carbon neutrality or carbon negativeness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The asphalt mixture of this embodiment contains at least asphalt, aggregate, filler, and biochar. In the asphalt mixture of this embodiment, by replacing a part of the components of aggregates such as stones and sand, or in addition to the components of aggregates, with biochar in which carbon is immobilized, it can contribute to carbon neutral or carbon negative. Here, biochar includes charcoal, bamboo charcoal, etc., and is defined as "a solid material made by heating biomass at a temperature of over 350°C under an oxygen concentration controlled to a level where it does not burn." If left as is, the carbon contained in wood, bamboo, etc., which are the raw materials for biochar, will be decomposed by microbial activity and released into the atmosphere as carbon dioxide. However, if wood, bamboo, etc. are carbonized and carbon is immobilized as biochar, it is possible to suppress the emission of carbon dioxide. In this embodiment, such biochar can be added to replace components of aggregates, etc. in the asphalt mixture, or in addition to the components of aggregates, to contribute to carbon neutral or carbon negative. The asphalt mixture of this embodiment will be described below.
[0012] [asphalt] Asphalt is a polymeric material produced from petroleum. It is liquid at high temperatures, but its viscosity increases as the temperature drops. Various types of asphalt can be used. For example, in addition to straight asphalt, which is petroleum asphalt for paving, modified asphalt can be used. Modified asphalt can be blown asphalt, which is modified with polymers (polymeric materials) such as thermoplastic elastomers and thermoplastic resins. Straight asphalt is the residual bitumen material obtained by subjecting crude oil to atmospheric distillation equipment, reduced pressure distillation equipment, etc. Blown asphalt refers to asphalt obtained by heating straight asphalt and then blowing air into it to oxidize it.
[0013] [aggregate] Aggregates include coarse aggregates with a particle size of 2.36 mm or more and fine aggregates with a particle size of less than 2.36 mm. Coarse aggregates are those that pass through a 2.36 mm sieve and are retained on a 0.075 mm sieve. Examples of coarse aggregate include No. 7 crushed stone with a particle size of 2.36 mm or more and less than 4.75 mm, No. 6 crushed stone with a particle size of 4.75 mm or more and less than 13.2 mm, No. 5 crushed stone with a particle size of 13.2 mm or more and less than 19 mm, and No. 4 crushed stone with a particle size range of 19 mm or more and less than 31.5 mm. The fine aggregate has a particle size of 0.075 mm or more and less than 2.36 mm. Examples of the fine aggregate include river sand, dune sand, mountain sand, sea sand, coarse sand, crushed sand, fine sand, screenings, crushed stone dust, silica sand, artificial sand, glass cullet, foundry sand, and recycled crushed aggregate sand.
[0014] [Filler] In this embodiment, the filler may be stone powder, slaked lime, cement, recycled dust, fly ash, etc. Here, in this embodiment, the filler does not include biochar.
[0015] The content of aggregate and filler in the asphalt mixture is preferably 90 to 97 mass%, more preferably 93 to 97 mass% in general regions, and even more preferably 90 to 95 mass% in snowy and cold regions.
[0016] [Biochar] The asphalt mixture of this embodiment contains biochar, and as described above, since the carbon is fixed, it is possible to prevent it from being emitted as carbon dioxide, which contributes to carbon neutrality or carbon negative.
[0017] It is preferable that biochar replaces a part of aggregate or is added to aggregate. Therefore, it is preferable that the shape of biochar is granular. Table 1 below shows an example of the cumulative particle size distribution of biochar, crushed sand, and fine sand. Specifically, the mass percentages of biochar, crushed sand, and fine sand that pass through sieves with mesh sizes of 2.36 mm, 0.6 mm, 0.3 mm, 0.15 mm, and 0.075 mm, respectively, are shown.
[0018] [Table 1]
[0019] It is preferable to use biochar that is certified as J-Credit. The J-Credit Scheme is a system in which the government certifies the amount of carbon dioxide and other emissions reduced through the introduction of energy-saving equipment and the use of renewable energy, and the amount of carbon dioxide and other emissions absorbed through appropriate forest management as "credits."
[0020] In this embodiment, there is a form in which a portion of the components with a particle size of 2.36 mm or less in a specific mixture specified in Table 6.3.1 "Types and Gradation Ranges of Asphalt Mixtures" in the Pavement Construction Handbook (published in 2006) etc. are replaced with biochar (hereinafter referred to as the "first form"), and a form in which biochar is further added to a specific mixture specified in the same "Types and Gradation Ranges of Asphalt Mixtures" (hereinafter referred to as the "second form").
[0021] In the first form, in a specific mixture specified in Table 6.3.1 "Types and Gradation Ranges of Asphalt Mixtures" in the Pavement Construction Handbook (published in 2006), some of the components with particle sizes of 2.36 mm or less are replaced with biochar. Table 6.3.1 "Types and Gradation Ranges of Asphalt Mixtures" in the Pavement Construction Handbook (published in 2006) is shown in Table 2 below.
[0022] [Table 2]
[0023] For example, in the "dense-graded asphalt mixture (13)" in the above table, some or all of the components with a particle size of 600 μm can be replaced with powdered biochar with an equivalent particle size. In other words, the particle size range and content of biochar are the particle size range and content of fine sand and coarse sand specified in the above pavement construction handbook. An example is shown in Table 1 below. In Table 1, the component composition specified in the standard mix includes No. 6 crushed stone, No. 7 crushed stone, crushed sand, fine sand, and stone powder. In the first form, 4.0% by mass of fine sand in the standard mix is replaced with 4.0% by mass of biochar.
[0024] [Table 3]
[0025] On the other hand, in the second form, biochar is further added to the specific mixture specified in the above "Type and Gradation Range of Asphalt Mixtures." For example, the mixture has the components listed in Table 2 above as is, and biochar is further added.
[0026] The more biochar is used, the more it can contribute to carbon neutrality or carbon negativeness. However, taking into account the strength of the asphalt mixture, it is preferable for the biochar to be contained in an amount of more than 0 mass% and not more than 10 mass%, more preferably 2 to 10 mass%, and even more preferably 3 to 10 mass%, relative to the entire asphalt mixture.
[0027] Here, we will show the actual amount of carbon dioxide (CO2) fixed when using biochar, taking into account the amount of carbon dioxide emitted from the collection of raw materials to the production process. The actual amount of CO2 fixed by biochar is expressed by the following formula (1). Net CO2 fixation by biochar (A) = CO2 fixation by biochar (B) - CO2 emissions during raw material collection and production (C) Equation (1) In the above formula, the amount of CO2 fixed by biochar (B) is expressed as carbon content x carbon remaining rate after 100 years x molecular weight of CO2 (= 44) / atomic weight of carbon (= 12). The above carbon content is given by fixed carbon (0.89) x moisture correction (1-0.15), and the carbon remaining rate after 100 years is set to 0.89 according to the J-Credit methodology. Therefore, The amount of CO2 fixed by biochar (B) = 0.89 x (1 - 0.15) x 0.89 x 44 / 12 = 2.469 kg-CO2 / kg. The CO2 emissions during raw material collection and manufacturing (C) are expressed as the sum of the CO2 emissions from raw material collection and the CO2 emissions during manufacturing. According to the actual values from Nara Tanka Kogyo Co., Ltd., the CO2 emissions from raw material collection are 0.057kg-CO2 / kg, and the CO2 emissions during manufacturing are 0.176kg-CO2 / kg, resulting in a total of 0.233kg-CO2 / kg. Therefore, the actual amount of CO2 fixed by biochar (A) = 2.469 kg-CO2 / kg - 0.233 kg-CO2 / kg = 2.23 kg-CO2 / kg. In other words, 2.23 g of carbon dioxide can be fixed per 1 kg of biochar.
[0028] Based on the above calculations, the carbon dioxide emissions from an asphalt mixture that uses biochar and a regular asphalt mixture that does not use biochar are estimated as shown in Table 3 below. In Table 3, the asphalt mixture that uses biochar is listed as "biochar used," and the regular asphalt mixture that does not use biochar is listed as "regular."
[0029] [Table 4]
[0030] From Table 3, it can be seen that the asphalt mixture using biochar can significantly reduce carbon dioxide compared to a normal asphalt mixture using biochar. In other words, the asphalt mixture of this embodiment contributes to carbon neutral or carbon negative.
[0031] The asphalt mixture of this embodiment can be produced in the same manner as the production of a normal asphalt mixture. For example, it can be obtained by mixing heated aggregate, filler, asphalt, and biochar by a conventional method. The heated aggregate, filler, asphalt, and biochar can be mixed simultaneously or in any order.
Claims
1. An asphalt mixture comprising at least asphalt, aggregate, a filler, and biochar.
2. 2. The asphalt mixture of claim 1, wherein the biochar is in granular form.
3. The asphalt mixture according to claim 1 or 2, comprising more than 0% by mass and no more than 10% by mass of the biochar.
Citation Information
Patent Citations
Asphalt mixture manufacturing method and asphalt plant
JP2021075907A