Biaxially oriented polypropylene film
A biaxially oriented polypropylene film with controlled surface features and molecular properties addresses the challenges of film breakage and voltage resistance in capacitors, achieving stability and high yield rates for capacitors in electric and hybrid vehicles.
Patent Information
- Application Number
- JP2023067622
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2043-04-18
AI Technical Summary
Polypropylene films used in capacitors for electric and hybrid vehicles require thinner designs with larger electrode areas and higher capacities, necessitating improved stability, higher voltage resistance, especially at high temperatures, and increased yield rates, while addressing issues of uneven adhesion and surface roughness that lead to film breakage and reduced voltage resistance.
A biaxially oriented polypropylene film with controlled surface features, including average maximum elliptical spot length of 3.0 mm or less, peak height difference of 0.040 μm or less, and slow axis angle variation of 0.3° to 2.8°, along with specific molecular weight and thickness ranges, to ensure uniform plasticity and adhesion during stretching, reducing film breakage and enhancing voltage resistance.
The solution provides a polypropylene film with enhanced stability, higher voltage resistance, particularly at high temperatures, and improved yield rates by minimizing film breakage and electric field concentration, ensuring consistent film formation and capacitor performance.
Smart Images

Figure 2024154033000007 
Figure 2024154033000008 
Figure 2024154033000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a biaxially oriented polypropylene film and the like. [Background technology]
[0002] Polypropylene films have excellent electrical properties such as high voltage resistance and low dielectric loss, and also have high moisture resistance. Therefore, they are widely used in electronic devices and electrical equipment. Specifically, they are used as films for filter capacitors and smoothing capacitors in power conversion circuits such as high-voltage capacitors, converters, and inverters.
[0003] In particular, in recent years, polypropylene films have begun to be widely used as capacitors for inverter power supply devices that control drive motors of electric vehicles, hybrid vehicles, etc. Capacitors for inverter power supply devices used in automobiles, etc. are required to be small, lightweight, high capacity, and highly reliable over a long period of time.
[0004] In Patent Document 1, the protrusion is 0.1 mm 2 The biaxially oriented polypropylene film for capacitors, in which the number of particles per square meter and the 10-point average roughness satisfy a predetermined relationship, is disclosed. Patent Document 1 describes that the biaxially oriented polypropylene film for capacitors having the above-mentioned configuration has the following effects: it has excellent processability even though it is a thin film, and exhibits high voltage resistance under a wide range of ambient temperature conditions from low temperature (-40°C) to high temperature (150°C). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2013 / 146367 Summary of the Invention [Problem to be solved by the invention]
[0006] Polypropylene films used as resin films for capacitors in electric vehicles, hybrid vehicles, etc., are required to be thinner and have a larger electrode area due to the recent trend toward smaller capacitors and higher capacity. In addition, there has been a strong demand for further cost reduction in recent years, and a method of high-speed stretch molding of a resin sheet has been considered as a method for producing the film, and it is also required to be able to manufacture capacitor elements with high voltage resistance (especially high voltage resistance at high temperatures) with a high yield.
[0007] Therefore, an object of the present invention is to provide a polypropylene film which can be stably formed for a longer period of time and has a higher yield rate of a film having higher voltage resistance (particularly, voltage resistance at high temperatures). [Means for solving the problem]
[0008] The present inventors have discovered the following in the course of their research.
[0009] The polypropylene film for the above-mentioned applications is thin and flexible, and thus the cast sheet of the stretched precursor is also thin and flexible. When such a cast sheet is continuously transported, air bubbles are easily generated between the sheet and the transport roll. In such a case, the adhesion to the roll becomes uneven, and the non-adhered portion appears as an elliptical depression on the surface of the sheet.
[0010] In addition, the conveying roll is heated in order to induce β crystals on the cast sheet surface and to impart plasticity to the sheet before stretching. When the above-mentioned elliptical depressions are scattered on the sheet surface, the adhesion state of the corresponding parts to the conveying roll differs from that of the other parts, resulting in a difference in the state of β crystal formation and roughening during stretching. In such a case, elliptical spots appear scattered on the film surface.
[0011] If the difference in surface roughness between the "spots" and other areas becomes large, the film tends to break during transverse stretching. This is thought to be because if there are areas within the sheet surface that have been formed with different thermal histories, the plasticity of the resin during transverse stretching becomes locally non-uniform, inducing stretching breakage of the film.
[0012] In addition, the spots tend to reduce the voltage resistance of the capacitor element in practical use and significantly reduce the yield. It is believed that if there is a local difference in surface roughness within the sheet surface, a local difference in interlayer adhesion occurs inside the rolled metallized polypropylene film, and the film is damaged due to electric field concentration.
[0013] Based on the above findings, the present inventors have conducted further research and found that the above problems can be solved by a biaxially stretched polypropylene film having a first surface and a second surface, in which the average maximum length of the approximately elliptical spots on the first surface is 3.0 mm or less, and the difference between the average protruding peak height Rpk outside the spots and the average protruding peak height Rpk within the spots is 0.040 μm or less. That is, the present invention encompasses the following aspects.
[0014] Item 1. A biaxially oriented polypropylene film having a first surface and a second surface, The average maximum length of the approximately elliptical spots on the first surface is 3.0 mm or less; and The difference between the average protruding peak height Rpk outside the spots and the average protruding peak height Rpk within the spots is 0.040 μm or less. Biaxially oriented polypropylene film.
[0015] Item 2. The biaxially oriented polypropylene film according to item 1, wherein the difference between the average protruding valley depth Rvk outside the spots and the average protruding valley depth Rvk within the spots is 0.020 μm or less.
[0016] Item 3. The biaxially stretched polypropylene film according to Item 1, wherein the change in the slow axis angle is in the range of 0.3° or more and 2.8° or less.
[0017] Item 4. The biaxially oriented polypropylene film according to item 1, wherein the average number of approximately elliptical spots per 11.5 mm × 8.6 mm area of the first surface is 0.6 or less.
[0018] Item 5. The biaxially oriented polypropylene film according to item 1, wherein the polypropylene resin constituting the biaxially oriented polypropylene film has a weight average molecular weight Mw of 250,000 or more and 450,000 or less, a ratio of the weight average molecular weight Mw to the number average molecular weight Mn (Mw / Mn) of 5.0 or more and 12.0 or less, a melt flow rate at 230°C under a load of 2.16 kg of 7.0 g / 10 min or less, and a heptane insoluble content of 96.0% or more and 99.5% or less.
[0019] Item 6. The biaxially oriented polypropylene film according to item 1, having a thickness of 1.7 μm or more and 6.5 μm or less.
[0020] Item 7. The biaxially oriented polypropylene film according to item 1, which is a monolayer film.
[0021] Item 8. The biaxially stretched polypropylene film according to any one of Items 1 to 7, which is for a capacitor.
[0022] Item 9. A metal layer-integrated polypropylene film comprising the biaxially oriented polypropylene film according to any one of items 1 to 7 and a metal layer disposed on one or both sides of the biaxially oriented polypropylene film.
[0023] Item 10. A capacitor comprising the metal layer-integrated polypropylene film according to item 9.
[0024] Item 11. A method for producing a biaxially oriented polypropylene film according to any one of Items 1 to 7, comprising: obtaining a cast sheet using a casting drum having a microcracked surface in which, when a virtual line of 0.1 mm in length is provided at any position on the surface in the width direction, 1 to 15 grooves intersect with the virtual line and the groove width is 1 μm to 10 μm; and subjecting the cast sheet to a biaxial stretching treatment. Effect of the Invention
[0025] According to the present invention, it is possible to provide a polypropylene film which can be stably formed for a longer period of time and has a higher yield rate of a film having a higher voltage resistance (particularly, voltage resistance at high temperatures). [Brief description of the drawings]
[0026] [Figure 1] A photograph of a representative roughly elliptical spot is shown. [Diagram 2] The major and minor axes of representative spots are shown. [Diagram 3] For a representative spot, the measurement points of the protruding peak height Rpk and the protruding valley depth Rvk within the spot are indicated by circles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] In this specification, the expressions "contain" and "comprise" include the concepts of "contain", "include", "consist essentially of" and "consist only of".
[0028] In this specification, based on the ranges consisting of the upper and / or lower limits described for each parameter, ranges in which the upper and / or lower limits are arbitrarily interchanged between multiple ranges are also exemplified.
[0029] 1. Biaxially oriented polypropylene film In one aspect, the present invention relates to a biaxially stretched polypropylene film having a first surface and a second surface, in which the average maximum length of the approximately elliptical spots on the first surface is 3.0 mm or less, and the difference between the average protruding peak height Rpk outside the spots and the average protruding peak height Rpk within the spots is 0.040 μm or less (also referred to as the "polypropylene film of the present invention" in this specification). This will be described below.
[0030] Of the two main surfaces of the polypropylene film of the present invention, one surface is a first surface and the other surface is a second surface. The first surface is a surface onto which a metal layer is laminated when a capacitor is produced.
[0031] The average maximum length of the approximately elliptical spots on the first surface of the polypropylene film of the present invention is 3.0 mm or less (characteristic 1).
[0032] The "speckles" in the characteristic 1 are visible on an image obtained by the measurement method described below, and are regions having a different degree of roughness and / or a different roughened surface shape from the surroundings. The maximum length (major axis) of the speckles can be, for example, 10 mm or less, 8 mm or less, 7 mm or less, 6 mm or less, or 5 mm or less.
[0033] Furthermore, in a preferred embodiment of the present invention, from the viewpoint of further improving the film formation stability and / or the yield rate of products with higher voltage resistance, it is preferable that the average number of approximately elliptical spots per 11.5 mm x 8.6 mm area of the first surface is 0.6 or less.
[0034] The method for measuring the average number of spots and the average maximum length of spots is as follows.
[0035] From the center position in the width direction of each biaxially stretched polypropylene film to be measured, 50 mm x 50 mm measurement samples are cut out at a total of 10 locations every 10 m in the longitudinal direction. Next, using a digital scope (Keyence Corporation Digital Microscope VHX-2000), lens magnification: 30 times, light amount: 50% of full range, measurement method: reflection measurement, field of view: 11.5 mm x 8.6 mm, one side of each measurement sample (the side on which the metal layer is laminated when making the capacitor) is observed in "halation removal + sharpening mode (a process is performed to make the color vivid, emphasize the contour, and remove glare)", and the number of approximately elliptical "spots" (a representative one is shown in Figure 1) observed within the field of view is counted. Note that if a part of the spot does not fit within the field of view, that spot is not counted. The number of spots in the visual field of each measurement sample (10 in total) is added up, and the total value obtained is divided by 10 (= the number of measurement samples) to obtain the average number of elliptical spots per visual field (11.5 mm × 8.6 mm area). In addition, for each spot measured above, the longitudinal diameter and width direction diameter of the biaxially oriented polypropylene film are measured, and the longer one (the major diameter of the spot) is regarded as the maximum length of the spot (in the representative example shown in Figure 2, the lateral diameter is the major diameter). The maximum lengths of each spot are added up, and the total value obtained is divided by the number of spots to obtain the average maximum length of the spots.
[0036] The average number of spots is preferably 0 or more and 0.3 or less, more preferably 0 or more and 0.1 or less, and particularly preferably 0, from the viewpoints of film formation stability, yield rate, and the like.
[0037] From the viewpoints of film formation stability, yield rate, etc., the average maximum length of the spots is preferably 0 mm or more and 1.0 mm or less, more preferably 0 mm or more and 0.5 mm or less, and particularly preferably 0 mm (= the average number of spots is 0).
[0038] In the polypropylene film of the present invention, the difference between the average protruding peak height Rpk outside the spots and the average protruding peak height Rpk inside the spots is 0.040 μm or less (characteristic 2).
[0039] The method for measuring the difference between the average protruding peak height Rpk outside the spots and the average protruding peak height Rpk inside the spots is as follows.
[0040] Using a non-contact optical interference surface shape measuring instrument, "VertScan2.0 (model: R5500GML)" manufactured by Ryoka Systems Co., Ltd., the protruding peak height Rpk of one side (the side on which the metal layer is laminated when manufacturing the capacitor) of the biaxially oriented polypropylene film to be measured is measured. First, using the WAVE mode, a 530 white filter and a 1x BODY lens barrel are applied, and a x10 objective lens is used to measure 470.92 μm x 353.16 μm per field of view.
[0041] Within the spots, for each of the spots counted using the method for measuring the number of spots described above, measurements are taken at each of the five locations shown in Figure 3 (the intersection of the long axis and the short axis, the center of the line connecting one end of the long axis and the intersection, the center of the line connecting the other end of the long axis and the intersection, the center of the line connecting one end of the short axis and the intersection, and the center of the line connecting the other end of the short axis and the intersection).
[0042] For the outside spots, measurements are taken at the center of each measurement sample cut out using the method for measuring the number of spots described above.
[0043] The obtained data is subjected to noise removal processing using a median filter (3 x 3), and then Gaussian filter processing with a cutoff value of 30 μm is performed to remove waviness components. This makes it possible to properly measure the condition of the measurement surface. Next, analysis is performed using the "VS-Viewer" analysis software of "VertScan2.0", and the average value of each value obtained at the above points is calculated for the protruding peak height Rpk, a lubricity evaluation parameter. Specifically, it is as follows.
[0044] The measured values of the protruding peak height Rpk within a spot are summed, and the resulting sum is divided by X (= number of measured spots × 5 (measurement points within one spot)) to determine the average protruding peak height Rpk within the spot.
[0045] The measured values of the protruding peak height Rpk outside the spots for each measurement sample are summed, and the resulting sum is divided by 10 (=number of measurement samples) to obtain the average protruding peak height Rpk outside the spots.
[0046] The average protruding peak height Rpk inside the spot is subtracted from the average protruding peak height Rpk outside the spot to obtain the difference between the two.
[0047] The difference between the average protruding peak height Rpk outside the spots and the average protruding peak height Rpk inside the spots is preferably 0 μm or more and 0.030 μm or less, more preferably 0 μm or more and 0.010 μm or less, and particularly preferably 0 μm, from the viewpoints of film formation stability, yield rate, etc. Note that when the average number of spots is 0, the difference is 0 μm.
[0048] The average protruding peak height Rpk outside the spots (= the average protruding peak height Rpk of the film when the average number of spots is 0) is preferably 0.010 μm or more and 0.095 μm or less, more preferably 0.015 μm or more and 0.090 μm or less, and even more preferably 0.020 μm or more and 0.085 μm or less, from the standpoint of high temperature durability of the capacitor element, etc.
[0049] When the average number of spots exceeds 0, the average protruding peak height Rpk within the spots is preferably 0.003 μm or more and 0.095 μm or less, more preferably 0.005 μm or more and 0.090 μm or less, and even more preferably 0.010 μm or more and 0.085 μm or less, from the standpoint of film formation stability, yield rate, etc.
[0050] The combination of characteristic 1 and characteristic 2 described below can further improve the film formation stability and the yield rate of films with higher voltage resistance. Although a limited interpretation is not desired, the reasons are believed to be as follows. If characteristic 1 and characteristic 2 are satisfied, the thermal history of the cast sheet, which is the stretching precursor, is thought to be moderately uniform in the film manufacturing process, and as a result, the plasticity during transverse stretching is also uniform, and film breakage is thought to be suppressed. In addition, when a capacitor is manufactured using such a film, a capacitor having voltage resistance can be efficiently obtained with a high yield. In a capacitor manufactured using such a film, the gap between the film layers is moderately uniform inside the capacitor, and it is thought that electric field concentration due to local interlayer adhesion is unlikely to occur. As a result, it is thought that damage to the film due to local heat generation inside the capacitor is suppressed, and the above-mentioned effects can be obtained.
[0051] From the viewpoint of further improving the yield rate of the film-forming stability and / or the higher voltage resistance, the difference between the average protruding valley depth Rvk outside the spots and the average protruding valley depth Rvk inside the spots of the polypropylene film of the present invention is preferably 0.020 μm or less. The difference is more preferably 0 μm or more and 0.015 μm or less, even more preferably 0 μm or more and 0.010 μm or less, and particularly preferably 0 μm. Note that, when the average number of spots is 0, the difference is 0 μm. Although it is not intended to be interpreted in a restrictive manner, by setting the difference within the above range, leakage current is unlikely to occur from the locally thin parts, and the plasticity during transverse stretching is also uniform, and as a result, it is considered that the film-forming stability and / or the yield rate of the film-forming stability and / or the higher voltage resistance can be further improved.
[0052] The method for measuring the difference between the average protruding valley depth Rvk outside the spots and the average protruding valley depth Rvk inside the spots is similar to the method for measuring the difference between the average protruding peak height Rpk outside the spots and the average protruding peak height Rpk inside the spots described above.
[0053] The measured values of the protruding valley depth Rvk within the spots are summed up, and the resulting sum is divided by X (= number of measured spots × 5 (measurement points within one spot)) to determine the average protruding valley depth Rvk within the spots.
[0054] The measured values of the protruding valley depth Rvk outside the spots for each measurement sample are summed up, and the resulting sum is divided by 10 (=number of measurement samples) to obtain the average protruding valley depth Rvk outside the spots.
[0055] The average protruding valley depth Rvk inside the spot is subtracted from the average protruding valley depth Rvk outside the spot to obtain the difference between them.
[0056] The average protruding valley depth Rvk outside the spots (=the average protruding valley depth Rvk of the film when the average number of spots is 0) is preferably 0.005 μm or more and 0.060 μm or less, more preferably 0.010 μm or more and 0.050 μm or less, and even more preferably 0.015 μm or more and 0.040 μm or less, from the viewpoint of high temperature durability of the capacitor element, etc.
[0057] When the average number of spots exceeds 0, the average protruding valley depth Rvk within the spots is preferably 0.001 μm or more and 0.045 μm or less, more preferably 0.002 μm or more and 0.040 μm or less, and even more preferably 0.003 μm or more and 0.035 μm or less, from the viewpoints of film formation stability and reducing the number of insulation defects.
[0058] From the viewpoint of further improving the film formation stability and / or the yield rate of a film having higher voltage resistance, the polypropylene film of the present invention has a 10 m insulation defect inspection device having a winding-rewinding mechanism and a direct current voltage of 600 V per 1 μm of thickness. 2 It is preferable that the number of insulation defects per 10 m is 1.0 or less. More preferably, the number is 0 / 10 m. 2 More than 0.5 pieces / 10m 2 Less than or equal to 0 pieces / 10m 2 More than 0.1 pieces / 10m 2 Less than or equal to 0 pieces / 10m is especially preferable. 2Although it is not intended to be a restrictive interpretation, a capacitor made using such a film is unlikely to suffer damage to the film due to short circuit even when used for long periods of time in a high-temperature environment, and can achieve high reliability.
[0059] The method for measuring the number of insulation defects is as follows.
[0060] Using an insulation defect inspection device with an unwinding / winding mechanism, the number of insulation defects (pieces / 10m) of the biaxially oriented polypropylene film to be measured was 2 ) is measured. The polypropylene film to be measured is passed between a high-voltage electrode and an earthed metal roller, while a DC voltage is applied and the number of discharges that occur at the insulation defects is counted by a counter attached to the device. The number of measured values is divided by the measured area to determine the number of insulation defects (pieces / 10m 2 The measurement conditions are as follows: Distance between high voltage electrode and earthed metal roller: 50μm The contact angle between the film and the grounded metal roller: 120° - Shape of high voltage electrode: Metal plate with a thickness of 4 mm and the same width as the metal roller Unwinding speed: 20m / min DC voltage: 600V / μm Measurement area: 472m 2 Test environment temperature: 20℃.
[0061] From the viewpoint of further improving the film formation stability and / or the yield rate of films with higher voltage resistance, the polypropylene film of the present invention preferably has a change range of the slow axis angle in the range of 0.3° to 2.8°, more preferably 0.3° to 2.0°, even more preferably 0.3° to 1.5°, and still more preferably 0.3° to 1.0°.
[0062] The slow axis angle of the biaxially stretched polypropylene film means the acute angle between the width direction of the biaxially stretched polypropylene film and the slow axis. The polypropylene film of the present invention is stretched in two axes, a first direction and a second direction perpendicular to the first direction. The biaxially stretched film has birefringence because the polymer is oriented in-plane by the biaxial stretching. The direction in the film plane where the refractive index is maximum is called the slow axis because it is the direction in which the light travels slowly (the phase is delayed).
[0063] In the sequential biaxial stretching method, first, the cast raw sheet is stretched in the machine direction (MD), and then the sheet is stretched in the transverse direction (TD). In this case, in the slow axis of the biaxially stretched polypropylene film, the refractive index in the transverse direction of the second direction tends to be larger than the refractive index in the machine direction of the first direction. Here, the transverse direction of the second direction becomes the slow axis.
[0064] In the case of transverse (TD) stretching, when the film is completely stretched in the transverse direction (when the film is completely stretched in the direction perpendicular to the flow direction), the slow axis angle defined in this specification is 0°. However, in reality, shrinkage stress, external mechanical force, thermoplasticity of the film, etc. act during stretching, so that the film cannot be completely stretched in the transverse direction (TD), and the slow axis angle tends to be larger than 0°.
[0065] In the area where the change in the slow axis angle in the longitudinal direction is large, the stretching is non-uniform, and the film is likely to be distorted. In practice, the non-uniformity of the stretching tends to reduce the voltage resistance performance of the capacitor and significantly reduce the yield. This is thought to be because, when the stretching in the longitudinal direction is non-uniform, the dimensional change inside the capacitor exposed to high temperatures becomes non-uniform, and electric field concentration occurs due to localized interlayer adhesion, causing damage to the film. It is thought that the above-mentioned troubles in the longitudinal direction can be suppressed by controlling the change in the slow axis angle in the longitudinal direction to a range of 0.3° to 2.8°.
[0066] The method for measuring the change range of the slow axis angle and the average slow axis angle is as follows.
[0067] From the center of the biaxially stretched polypropylene film to be measured, 50 mm x 50 mm measurement samples are cut out at 10 m intervals in the longitudinal direction, totaling 10 positions (0 m, 10 m, 20 m, 30 m, 40 m, 50 m, 60 m, 70 m, 80 m, and 90 m positions). Next, the width direction of the measurement sample is set to 0°, and the acute angle between the width direction of the measurement sample and the slow axis is measured as the slow axis angle. Among the 10 measurement samples, the difference between the maximum and minimum values of the slow axis angle is determined as the "change width", and the average value is determined as the "average slow axis angle". The measurement device and measurement conditions are as follows.
[0068] Measurement equipment: Retardation measurement equipment RE-100 manufactured by Otsuka Electronics Co., Ltd. Light source: Laser light emitting diode (LED) Bandpass filter: 550 nm (measurement wavelength) Measurement interval: 0.1 sec Accumulation times: 10 times Number of measurement points: 15 points Gain: 10dB Measurement environment: temperature 23℃, humidity 60%.
[0069] From the viewpoint of yield rate in film production, the average slow axis angle is preferably from 0° to 20°, more preferably from 0° to 15°, and further preferably from 0° to 13°.
[0070] The thickness of the polypropylene film of the present invention is preferably 6.5 μm or less, more preferably 5.5 μm or less, even more preferably 3.5 μm or less, particularly preferably 3.0 μm or less, and most preferably 2.8 μm or less, from the viewpoint of further improving the miniaturization and high capacity of the capacitor when used in a capacitor. From the viewpoint of production, the lower limit is preferably 0.8 μm or more, more preferably 1.0 μm or more, even more preferably 1.7 μm or more, and particularly preferably 2.0 μm or more. In addition, it is preferable to set the thickness within the above range from the viewpoint of film formation stability and / or the yield rate of a film with higher voltage resistance. The method for measuring the thickness of the biaxially stretched polypropylene film in this specification is the method described in the Examples.
[0071] The layer structure of the polypropylene film of the present invention is not particularly limited. The polypropylene film of the present invention may be a single layer consisting of one layer, or may be a plurality of layers having the same or different compositions. The polypropylene film of the present invention is preferably a film consisting of one or more film-like molded layers, and more preferably a single layer film (a film consisting of one film-like molded layer).
[0072] The polypropylene film of the present invention is not particularly limited in terms of its constituent material, so long as it contains a polypropylene resin. The polypropylene resin is not particularly limited, and examples thereof include propylene homopolymers such as isotactic polypropylene, copolymers of propylene and ethylene, long-chain branched polypropylene, and ultra-high molecular weight polypropylene. Among these, isotactic polypropylene is preferred from the viewpoint of heat resistance.
[0073] The content of the polypropylene resin is preferably 90% by mass or more, more preferably 95% by mass or more, based on the entire polypropylene film of the present invention (when the entire polypropylene film is taken as 100% by mass). The upper limit of the content of the polypropylene resin is, for example, 100% by mass, 98% by mass, etc., based on the entire polypropylene film of the present invention.
[0074] The polypropylene resin may be used alone or in combination of two or more kinds.
[0075] Here, when the polypropylene film of the present invention contains two or more kinds of polypropylene resins, the polypropylene resin with the greater content is referred to herein as the "main polypropylene resin". When the polypropylene film of the present invention contains only one kind of polypropylene resin, the polypropylene resin is referred to herein as the "main polypropylene resin".
[0076] Hereinafter, in this specification, when the term "polypropylene resin" is used without specifying whether it is the main component or not, it means both the polypropylene resin as the main component and the polypropylene resin other than the main component unless otherwise specified. For example, when it is described that "the weight average molecular weight Mw of the polypropylene resin is preferably 250,000 or more and 450,000 or less," it means that the weight average molecular weight Mw of the polypropylene resin as the main component is preferably 250,000 or more and 450,000 or less, and that the weight average molecular weight Mw of the polypropylene resin other than the main component is preferably 250,000 or more and 450,000 or less.
[0077] The weight average molecular weight Mw of the polypropylene resin is preferably 250,000 to 450,000 in terms of the thickness uniformity, mechanical properties, and thermo-mechanical properties of the biaxially oriented polypropylene film, more preferably 250,000 to 420,000, even more preferably 250,000 to 400,000, and even more preferably 260,000 to 390,000. By using such a polypropylene resin, the insulation breakdown of the film is suppressed, and it is easy to obtain an extremely thin biaxially oriented polypropylene film suitable for small and high-capacity capacitors. When using two or more polypropylene resins, it is preferable to use a polypropylene resin (preferably a polypropylene resin as a main component) having an Mw of 250,000 to less than 330,000 (preferably 250,000 to 300,000, more preferably 260,000 to 290,000) in combination with a polypropylene resin (preferably a polypropylene resin other than the main component) having an Mw of 330,000 to 450,000 (preferably 350,000 to 420,000, more preferably 370,000 to 400,000, and even more preferably 370,000 to 390,000).
[0078] The ratio (Mw / Mn) of the weight average molecular weight Mw to the number average molecular weight Mn of the polypropylene resin is preferably 5.0 to 12.0, more preferably 5.0 to 10.0, and even more preferably 5.0 to 9.0, from the viewpoint of obtaining an appropriate resin fluidity during biaxial stretching and facilitating the production of an extremely thin biaxially stretched propylene film without thickness unevenness. When using two or more polypropylene resins, it is preferable to use a polypropylene resin (preferably a polypropylene resin as a main component) having the above ratio of 5.0 to less than 7.0 (preferably 5.0 to 6.5) in combination with a polypropylene resin (preferably a polypropylene resin other than the main component) having the above ratio of 7.0 to 12.0 (preferably 7.5 to 10.0, more preferably 7.5 to 9.0).
[0079] The weight average molecular weight Mw and number average molecular weight Mn of the polypropylene resin are measured by the method described in the Examples.
[0080] The melt flow rate (MFR) of the polypropylene resin at 230° C. and a load of 2.16 kg is not particularly limited, but is preferably 7.0 g / 10 min or less from the viewpoint of stretchability, and more preferably 0.5 g / 10 min to 6.0 g / 10 min from the viewpoint of increasing the thickness accuracy of the polypropylene film of the present invention. When using two or more polypropylene resins, it is preferable to use a polypropylene resin (preferably a polypropylene resin of the main component) having an MFR of 4.0 g / 10 min to less than 7.0 g / 10 min (preferably 4.5 g / 10 min to 6.5 g / 10 min, more preferably 5.0 g / 10 min to 6.0 g / 10 min) in combination with a polypropylene resin (preferably a polypropylene resin other than the main component) having an MFR of 0.5 g / 10 min to less than 4.0 g / 10 min (preferably 1.0 g / 10 min to 3.5 g / 10 min, more preferably 1.5 g / 10 min to 3.0 g / 10 min). The melt flow rate of the polypropylene resin is measured by the method described in the Examples.
[0081] The heptane insoluble content (HI) of the polypropylene resin is preferably 96.0% or more and 99.5% or less, more preferably 97.0% or more and 99.0% or less. Here, the higher the heptane insoluble content, the higher the stereoregularity of the resin. By using such a polypropylene resin, the crystallinity is appropriately improved, and the initial voltage resistance and long-term voltage resistance are improved. The heptane insoluble content (HI) is measured by the method described in the Examples.
[0082] The content of the main component polypropylene resin is preferably more than 50 mass% and 100 mass% or less, more preferably 55 mass% or more and 85 mass% or less, even more preferably 60 mass% or more and 75 mass% or less, and still more preferably 60 mass% or more and 70 mass% or less, relative to 100 mass% of the polypropylene resin.
[0083] The polypropylene resin can be produced by a generally known polymerization method, for example, a gas phase polymerization method, a bulk polymerization method, and a slurry polymerization method.
[0084] The polymerization may be a single-stage polymerization using one polymerization reactor, or a multi-stage polymerization using two or more polymerization reactors. The polymerization may be carried out by adding hydrogen or a comonomer as a molecular weight modifier to the reactor.
[0085] The catalyst used in the polymerization can be a generally known Ziegler-Natta catalyst, and is not particularly limited as long as the polypropylene resin can be obtained. The catalyst may contain a cocatalyst component or a donor. By adjusting the catalyst and polymerization conditions, the molecular weight, molecular weight distribution, stereoregularity, etc. can be controlled.
[0086] The molecular weight distribution of the polypropylene resin can be adjusted by resin mixing (blending). For example, a method of mixing two or more resins having different molecular weights or molecular weight distributions can be mentioned. In general, a two-type polypropylene mixture in which the main resin is 55% by mass or more and 90% by mass or less, assuming that the total resin is 100% by mass, and a resin having a higher or lower average molecular weight than the main resin is mixed is preferable because it is easy to adjust the amount of low molecular weight components.
[0087] When the above-mentioned mixing and adjusting method is adopted, the melt flow rate (MFR) may be used as a guide for the average molecular weight. In this case, it is preferable that the difference in MFR between the main resin and the additive resin is about 1 to 30 g / 10 min from the viewpoint of convenience during adjustment.
[0088] The method for mixing the resins is not particularly limited, and examples thereof include a method in which polymer powders or pellets of the main resin and the additive resin are dry-blended using a mixer or the like, and a method in which polymer powders or pellets of the main resin and the additive resin are fed to a kneader and melt-kneaded to obtain a blended resin.
[0089] The mixer and the kneader are not particularly limited. The kneader may be of a single screw type, a twin screw type, or a multi-screw type having more than one screw. In the case of a twin or more screw type, the kneader may be of either a co-rotating or counter-rotating type.
[0090] In the case of blending by melt kneading, the kneading temperature is not particularly limited as long as a good kneaded product is obtained. In general, it is in the range of 200°C to 300°C, and from the viewpoint of suppressing deterioration of the resin, 230°C to 270°C is preferable. In addition, in order to suppress deterioration during kneading and mixing of the resin, an inert gas such as nitrogen may be purged into the kneader. The melt kneaded resin may be pelletized to an appropriate size using a generally known granulator. In this way, mixed polypropylene raw material resin pellets can be obtained.
[0091] Use of the above-mentioned polypropylene resin makes it easier to adjust the film properties as described above, and is also preferable from the viewpoint of film formation stability and / or yield rate of films with higher voltage resistance.
[0092] The polypropylene film of the present invention may contain an additive. The "additive" is not particularly limited as long as it is an additive generally used in polypropylene resins.
[0093] Examples of the additives include antioxidants, light stabilizers, ultraviolet absorbers, plasticizers, lubricants, crosslinking agents, flame retardants, antistatic agents, heat resistance improvers, antiblocking agents, inorganic particles, resin particles, etc. The polypropylene resin may contain the additives in an amount that does not adversely affect the polypropylene film of the present invention (for example, 10% by mass or less, 5% by mass or less, 1% by mass or less, or 0.1% by mass or less, relative to 100% by mass of the polypropylene film of the present invention).
[0094] 2. Manufacturing method of biaxially oriented polypropylene film The biaxially stretched polypropylene film can be produced by obtaining a cast sheet corresponding to the stretched precursor from the resin pellets, and then subjecting the cast sheet to a biaxial stretching process. As is clear from the results of the examples described later, the biaxially stretched polypropylene film of the present invention can be obtained by controlling the microcracks on the casting drum surface, the air blowing speed of the air knife, the distance between the air knife blowing port and the cast sheet, the stretching nip roll temperature, the stretching nip roll hardness, etc., specifically by producing according to the following method.
[0095] Among the above-mentioned production conditions, microcracks on the casting drum surface are an important condition. From this viewpoint, in one aspect, the present invention relates to a method for producing the biaxially oriented polypropylene film of the present invention, which comprises obtaining a cast sheet using a casting drum having a microcrack surface, in which, when a virtual line having a length of 0.1 mm is provided at any position on the surface in the width direction, 1 to 15 grooves intersect with the virtual line and the groove width is 1 μm to 10 μm, and subjecting the cast sheet to a biaxial stretching treatment.
[0096] The method for producing the biaxially oriented polypropylene film of the present invention will be described in detail below.
[0097] 2-1. Cast sheet manufacturing The cast sheet can be formed by using a known method. For example, polypropylene resin pellets, dry-mixed polypropylene resin pellets, or mixed polypropylene resin pellets previously prepared by melt kneading are fed to an extruder, heated and melted, filtered to remove foreign matter and modified polymers, extruded from a T-die into a sheet, and cooled and solidified on at least one metal drum (casting drum), thereby forming a cast sheet.
[0098] In the extruder, polypropylene resin is degraded by heat and oxidation. From the viewpoint of suppressing such polymer degeneration, the resin temperature during melt extrusion is 170° C. or more and 320° C. or less, preferably 200° C. or more and 300° C. or less. Degradation can be suppressed by nitrogen substitution in the extruder, screw shape, internal shape of the T-die during casting, amount of antioxidant added, and the like.
[0099] The temperature of the casting drum is preferably maintained at 80° C. or higher and 140° C. or lower, and more preferably at 90° C. or higher and 105° C. or lower. The β-crystal fraction of the cast sheet obtained in such a temperature range is about 5% or higher and 20% or lower as measured by an X-ray method. Within the above β-crystal fraction range, the roughness of the film surface is appropriately improved, and both the capacitor characteristics and the element winding processability can be satisfied.
[0100] The surface of the casting drum is not particularly limited, but a roll having an uneven surface such as a sandblast roll or a ceramic roll, or a microcrack roll having an exhaust path for entrained air is preferred, in that the desired physical properties of the present invention can be easily obtained. The manufacturing method of these rolls is known, and for example, a microcrack roll can be manufactured according to or in accordance with the method described in Japanese Patent No. 6974939. The microcracks are generated by the stress of the metal plating layer, and the shape and number of the microcracks can be controlled by the thickness of the metal plating layer, plating conditions, heat treatment, chemical treatment, multi-layering, etc. For example, in the case of chrome plating, the plating thickness is preferably 100 μm to 400 μm, more preferably 120 μm to 350 μm, and even more preferably 150 μm to 300 μm. By setting it in this range, it becomes easier to control the shape and number of the grooves, and cracks are less likely to occur when the roll is heated.
[0101] Regarding the microcrack roll, when a virtual line having a length of 0.1 mm is provided in the width direction at any position on the roll surface, it is preferable that 1 to 15 grooves intersect with the virtual line, more preferably 2 to 10 grooves, and even more preferably 3 to 8 grooves. The groove width is preferably 1 μm to 10 μm, more preferably 2 μm to 9 μm, and even more preferably 3 μm to 8 μm. By using the above-mentioned groove number and groove width range, the air that invades between the casting drum and the cast sheet is appropriately discharged, and even a thin cast sheet can be easily transported in close contact, making it easy to obtain an extremely thin biaxially stretched polypropylene film. In addition, even if the molding speed of the thin cast sheet is increased, the phenomenon in which the thickness of the cast sheet wavy, so-called draw resonance (surging) phenomenon, is unlikely to occur, and an extremely thin biaxially stretched polypropylene film having a uniform thickness in the longitudinal direction can be easily obtained.
[0102] The method for adhering the sheet to the casting drum may be any method such as the air knife method, touch roll method, electrostatic application method, water-cooled casting method, etc., but the air knife method is preferred because it is easy to adjust the sheet adhesion and can be handled simply.
[0103] When an air knife is used, the wind speed of the blown air is preferably 70 m / s to 130 m / s, more preferably 80 m / s to 120 m / s, and even more preferably 90 m / s to 110 m / s. The distance between the air knife outlet and the cast sheet is preferably 2 mm to 5 mm, more preferably 2 mm to 4 mm. When the air knife is used in this range, the thin-film resin extruded into a sheet from the T-die can be appropriately adhered to the casting drum, and the film vibration of the molten resin from the T-die outlet to the casting drum can be suppressed. As a result, the above-mentioned film properties can be easily obtained.
[0104] 2-2. Biaxial stretching process The biaxially oriented polypropylene film of the present invention can be obtained by biaxially stretching the cast sheet in the longitudinal and transverse directions. The stretching method can be simultaneous or sequential biaxial stretching, but from the viewpoint of stably achieving uniform thickness and increasing the mechanical strength of the film, sequential biaxial stretching is preferred.
[0105] In the sequential biaxial stretching method, it is preferable to first preheat the cast sheet by passing it through a conveying roll kept at 70° C. to 135° C., preferably 80° C. to 130° C., and then, immediately before stretching in the longitudinal direction, to heat it to 130° C. to 155° C., preferably 140° C. to 150° C. By heating the cast sheet in this manner, excessive thermal expansion of the cast sheet is suppressed, the flatness of the sheet is easily maintained before the longitudinal stretching described later, and the sheet is easily brought into uniform contact with the conveying roll.
[0106] From the viewpoint of easily obtaining the biaxially oriented polypropylene film of the present invention, a method of simultaneously heating both the front and back sides of the cast sheet immediately before the longitudinal stretching is preferred. The method is not particularly limited, but from the viewpoint of suppressing the difference in thermal history within the surface of the cast sheet, a method of heating the stretching nip rolls or a method of heating by electromagnetic radiation is preferred. From the viewpoint of simultaneously fixing the cast sheet immediately before stretching and adjusting the temperature of the sheet, a method of heating the stretching nip rolls is more preferred.
[0107] When the stretching nip rolls are heated, the temperature of the stretching nip rolls is preferably 95°C or higher and 170°C or lower, more preferably 100°C or higher and 150°C or lower, from the viewpoint of suppressing the difference in thermal history between the front and back surfaces of the cast sheet.
[0108] When the stretching nip roll is heated, the rubber hardness of the roll is preferably 40° or more and 80° or less, more preferably 50° or more and 70° or less, so that the shape of the roll surface follows the shape of the cast sheet surface.
[0109] Thereafter, the film is stretched in the longitudinal direction by 3 to 7 times, preferably 4 to 6 times, and immediately cooled to room temperature.
[0110] After stretching in the longitudinal direction, the stretched film is introduced into a tenter, both ends are held with clips heated to 80°C or more and 140°C or less, and the film is preheated at a temperature of 140°C or more and 185°C or less, preferably 150°C or more and 175°C or less, and then stretched in the width direction at a temperature of 140°C or more and 170°C or less, preferably 150°C or more and 160°C or less, by 6 times or more and 12 times or less, preferably 8 times or more and 11 times or less.
[0111] The film is then relaxed, heat-set, and wound up. The wound film is then aged in an atmosphere of 20°C to 45°C, after which it can be cut to the desired product width.
[0112] 3. Polypropylene film with metal layer In one aspect, the present invention also provides a metal layer-integrated polypropylene film (sometimes referred to as the "metal layer-integrated polypropylene film of the present invention" in this specification) comprising the biaxially oriented polypropylene film of the present invention and a metal layer disposed on one or both sides of the biaxially oriented polypropylene film. The metal layer-integrated polypropylene film of the present invention will be described in detail below. A capacitor obtained by winding the metal layer-integrated polypropylene film of the present invention has excellent initial voltage resistance and long-term durability under high temperature and high voltage conditions.
[0113] The polypropylene film of the present invention can be provided with an electrode on one or both sides in order to process it into a capacitor. Such an electrode is not particularly limited as long as the capacitor targeted by this embodiment can be obtained, and electrodes that are usually used for manufacturing capacitors can be used. Examples of the electrode include metal foil, paper with at least one side metallized, and plastic film.
[0114] Since capacitors are increasingly required to be small and lightweight, it is preferable to form electrodes by directly metallizing one or both sides of the polypropylene film of the present invention. The metals used may be, for example, simple metals such as zinc, lead, silver, chromium, aluminum, copper, and nickel, mixtures of multiple types of these metals, and alloys of these metals. In consideration of the environment, economy, and capacitor performance, zinc and aluminum are preferred.
[0115] Examples of methods for directly metallizing the surface of a polypropylene film include vacuum deposition and sputtering, and are not particularly limited as long as the capacitor of the present embodiment can be obtained. From the viewpoints of productivity and economy, the vacuum deposition method is preferred. Examples of vacuum deposition methods include the crucible method and the wire method, but are not particularly limited as long as the capacitor of the present embodiment can be obtained, and the most suitable method can be selected as appropriate.
[0116] From the viewpoint of the electrical properties of the capacitor, the film resistance of the metal vapor deposition film is preferably 1 Ω / □ or more and 100 Ω / □ or less. A higher value within this range is desirable from the viewpoint of self-healing properties, and from the viewpoint of safety, the film resistance is more preferably 5 Ω / □ or more and 50 Ω / □ or less, and even more preferably 10 Ω / □ or more and 30 Ω / □ or less. The film resistance of the metal vapor deposition film can be measured during metal vapor deposition, for example, by a four-terminal method known to those skilled in the art. The film resistance of the metal vapor deposition film can be adjusted, for example, by adjusting the output of the evaporation source to adjust the amount of evaporation.
[0117] When forming a metal vapor deposition film on one side of the film, a certain width is not vapor deposited from one end of the film to form an insulating margin so that the film will become a capacitor when rolled up. Furthermore, in order to strengthen the bond between the metal layer-integrated polypropylene film of the present invention and the metallikon electrode, it is preferable to form a heavy edge structure on the end opposite the insulating margin, and the film resistance of the heavy edge is usually 1 Ω / □ or more and 8 Ω / □ or less, and preferably 1 Ω / □ or more and 5 Ω / □ or less. The thickness of the metal film is not particularly limited, but is preferably 1 nm or more and 200 nm or less.
[0118] There are no particular limitations on the margin pattern of the metal vapor deposition film to be formed, but from the viewpoint of improving the characteristics of the capacitor, such as safety, it is preferable to use a pattern including a so-called special margin, such as a fishnet pattern, a T-margin pattern, etc. When a metal vapor deposition film is formed on one side of a polypropylene film in a pattern including a special margin, the safety of the resulting capacitor is improved, and it is also effective in preventing destruction and short circuits of the capacitor, and is therefore preferable.
[0119] The margin can be formed by any known method without any restriction, such as a tape method in which masking is performed with tape during deposition, or an oil method in which masking is performed by applying oil.
[0120] The metal layer-integrated polypropylene film of the present invention can be processed into the capacitor of the present invention described below by wrapping the film along the longitudinal direction. That is, two metal layer-integrated polypropylene films of the present invention are stacked and wound as a pair so that the metal layer and the polypropylene film are alternately laminated. Then, a pair of metallikon electrodes is formed on both end faces by metal spraying to produce a film capacitor, thereby obtaining the capacitor.
[0121] 4. Capacitor In one aspect, the present invention provides a capacitor including the metal layer-integrated polypropylene film of the present invention (also referred to as the "capacitor of the present invention" in this specification). The capacitor of the present invention will be described in detail below.
[0122] In the process of producing a capacitor, a film winding process is performed. For example, two metal layer-integrated polypropylene films of the present invention are overlapped and wound so that the metal layers and polypropylene films in the metal layer-integrated polypropylene film of the present invention are alternately stacked, and further, the insulating margins are on opposite sides. In this case, it is preferable to stack the two metal layer-integrated polypropylene films of the present invention with a shift of 1 to 2 mm. The winding machine used is not particularly limited, and for example, an automatic winding machine 3KAW-N2 type manufactured by Kaito Seisakusho Co., Ltd. can be used.
[0123] When manufacturing flat capacitors, the resulting roll is usually pressed after winding. Pressing tightens the capacitor and forms the elements. In order to control and stabilize the interlayer gap, the optimum pressure to be applied varies depending on the thickness of the polypropylene film, etc., but is, for example, 2 to 20 kg / cm2.
[0124] Next, a metal is sprayed onto both end surfaces of the wound body to provide metallikon electrodes, thereby producing a capacitor. The capacitor is then subjected to a predetermined heat treatment. That is, in this embodiment, the process includes a step of subjecting the capacitor to a heat treatment in a vacuum at a temperature of 80 to 125°C for one hour or more (hereinafter, this may be referred to as "thermal aging").
[0125] In the above-mentioned step of subjecting the capacitor to heat treatment, the temperature of the heat treatment is 80°C or higher and 130°C or lower, preferably 90°C or higher and 125°C or lower. By subjecting the capacitor to heat treatment at the above-mentioned temperature, the effect of heat aging can be obtained. Specifically, the gap between the films constituting the capacitor based on the metal layer-integrated polypropylene film of the present invention is reduced, corona discharge is suppressed, and the internal structure of the metal layer-integrated polypropylene film of the present invention is changed and crystallization is promoted. As a result, it is considered that the voltage resistance is improved. If the heat treatment temperature is lower than the predetermined temperature, the above-mentioned effect of heat aging cannot be sufficiently obtained. On the other hand, if the heat treatment temperature is higher than the predetermined temperature, the polypropylene film may undergo thermal decomposition, oxidative deterioration, etc.
[0126] The method for subjecting the capacitor to heat treatment may be appropriately selected from known methods including, for example, a method using a thermostatic bath under a vacuum atmosphere, a method using high-frequency induction heating, etc. Specifically, it is preferable to employ a method using a thermostatic bath.
[0127] The time for the heat treatment is preferably 1 hour or more, more preferably 10 hours or more, from the viewpoint of obtaining mechanical and thermal stability, but more preferably 20 hours or less, from the viewpoint of preventing molding defects such as heat wrinkles and molding. Lead wires are usually welded to the metallikon electrodes of the capacitor that have been subjected to heat aging. In addition, in order to impart weather resistance and in particular to prevent deterioration due to humidity, it is preferable to encapsulate the capacitor in a case and pot it with epoxy resin. The capacitor of the present invention is a small-sized, large-capacity capacitor based on the metal layer-integrated polypropylene film of the present invention, and has initial voltage resistance and long-term durability under high temperature and high voltage.
[0128] The capacitor of the present invention using the polypropylene film of the present invention can be suitably used in a high-temperature environment, and can be a small-sized capacitor with a high capacity (for example, a capacitance of 5 μF or more, preferably 10 μF or more, more preferably 20 μF or more, even more preferably 30 μF or more, and particularly preferably 40 μF or more. The upper limit of the capacitance is not particularly limited, and is, for example, 100 μF, 80 μF, 70 μF, or 60 μF). Therefore, the capacitor of the present invention can be used as a high-voltage capacitor, a filter capacitor and a smoothing capacitor for various switching power supplies, converters, inverters, etc., which are used in electronic devices and electric devices. In addition, the capacitor of the present invention can be suitably used as an inverter capacitor, a converter capacitor, etc., which control the drive motor of electric vehicles and hybrid vehicles, which have become increasingly popular in recent years. EXAMPLES
[0129] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples.
[0130] (1) Resin characteristic measurement (1-1) Measurement of weight average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (Mw / Mn) of polypropylene resin The weight average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (Mw / Mn) of the polypropylene resin used as the raw material in the examples and comparative examples were measured using GPC (gel permeation chromatography) under the following conditions.
[0131] Specifically, a high-temperature GPC device with a built-in differential refractometer (RI), HLC-8121GPC-HT model, manufactured by Tosoh Corporation, was used. Three TSKgel GMHHR-H(20)HT columns manufactured by Tosoh Corporation were used in conjunction. Measurements were performed at a column temperature of 140°C, with trichlorobenzene as the eluent flowing at a flow rate of 1.0 ml / min. A calibration curve was prepared using standard polystyrene manufactured by Tosoh Corporation, and the measured molecular weight values were converted to polystyrene values to obtain the weight average molecular weight (Mw) and number average molecular weight (Mn). The molecular weight distribution (Mw / Mn) was obtained using the values of Mw and Mn.
[0132] (1-2) Measurement of heptane insolubles (HI) The polypropylene resin used as the raw material in the examples and comparative examples was press-molded to 10 mm x 35 mm x 0.3 mm to prepare a measurement sample of about 3 g. Next, about 150 mL of heptane was added and Soxhlet extraction was performed for 8 hours. The heptane insoluble matter was calculated from the sample mass before and after extraction.
[0133] (1-3) Measurement of Melt Flow Rate (MFR) The melt flow rate (MFR) of the polypropylene resin used as a raw material in the examples and comparative examples in the form of raw material resin pellets was measured using a melt indexer manufactured by Toyo Seiki Co., Ltd. in accordance with condition M of JIS K 7210. Specifically, a sample weighed to 4 g was inserted into a cylinder whose test temperature was set to 230° C., and preheated for 3.5 minutes under a load of 2.16 kg. The weight of the sample extruded from the bottom hole in 30 seconds was then measured, and the MFR (g / 10 min) was calculated. The above measurement was repeated three times, and the average value was taken as the measured MFR value.
[0134] (2) Preparing the casting drum Casting drums A to E were prepared as metal drums (casting drums) used when producing sheets (cast sheets) to be subjected to biaxial stretching treatment in the manufacturing process of a biaxially oriented polypropylene film.
[0135] At any position on the surface of the casting drum, a virtual line of 0.1 mm in length was drawn at any position in the width direction, and the number of grooves intersecting the virtual line and the average value of the groove width were measured. Specifically, the measurements were performed as follows. A total of 12 positions were observed, including four positions in the circumferential direction of the casting drum (0 degrees, 90 degrees, 180 degrees, and 270 degrees on a clock) and three positions in the width direction (10 (one end), 50 (center), and 90 (one end) for a face length of 100), and a virtual line of 0.1 mm in the width direction was drawn in the center of the screen, and the number of intersecting grooves and the groove width were measured, and the average value was calculated.
[0136] The number of grooves and groove width are shown in Table 1.
[0137] [Table 1]
[0138] (3) Manufacturing of biaxially oriented polypropylene film A biaxially stretched polypropylene film was produced according to the production conditions in Table 2. The thickness of the biaxially stretched polypropylene film was measured using a micrometer (JIS-B7502) in accordance with JIS-C2330.
[0139] <Example 1> Polypropylene resin A (Mw = 270,000, Mw / Mn = 5.7, heptane insoluble = 97.8%, MFR = 5.6g / 10min, manufactured by Prime Polymer) and polypropylene resin B (Mw = 380,000, Mw / Mn = 8.3, heptane insoluble = 98.8%, MFR = 2.3g / 10min, manufactured by Daehan Oil & Chemical) were fed to an extruder in a mass ratio of A: B = 65: 35 and melted at a resin temperature of 230 ° C. Then, after removing foreign matter and modified polymers with a filter installed in the middle of the polymer tube, it was extruded using a T-die, and solidified by wrapping it around a casting drum whose surface temperature was kept at 92 ° C. A cast sheet with a thickness of 0.1 mm was produced at a speed of 60 m / min. The casting drum used was A in Table 1.
[0140] In addition, an air knife was used to adhere the sheet to the casting drum, with the blown air speed set to 110 m / s and the distance between the air knife outlet and the cast sheet set to 3 mm.
[0141] The obtained cast sheet was preheated to a temperature of 130°C, sandwiched between a conveying roll heated to 145°C and a stretching nip roll with a rubber hardness of 70° heated to 110°C, stretched 5 times in the longitudinal direction, and immediately returned to room temperature.
[0142] The stretched film was then introduced into a tenter, both ends were held with 110°C clips, preheated to 170°C, and stretched 10 times in the width direction at a temperature of 155°C, after which relaxation and heat setting were performed, and a biaxially stretched polypropylene film with a thickness of 2.3 μm was wound into a roll.
[0143] <Example 2> A biaxially oriented polypropylene film was obtained in the same manner as in Example 1, except that in the production of the cast sheet, the distance between the air knife outlet and the sheet was set to 5 mm.
[0144] <Example 3> A biaxially oriented polypropylene film was obtained in the same manner as in Example 2, except that in the production of the cast sheet, the wind speed of the air blown from the air knife was set to 70 m / sec.
[0145] <Example 4> In the production of the cast sheet, a biaxially oriented polypropylene film was obtained in the same manner as in Example 1, except that the casting drum was changed to B in Table 1.
[0146] <Example 5> In the production of the cast sheet, a biaxially oriented polypropylene film was obtained in the same manner as in Example 1, except that the casting drum was changed to C in Table 1.
[0147] <Example 6> In producing the cast sheet, the casting drum was E in Table 1, the wind speed of the air blown out of the air knife was 130 m / sec, the distance between the air knife outlet and the sheet was 2 mm, and in the longitudinal stretching process, the temperature of the stretching nip rolls was 130°C. A biaxially oriented polypropylene film was obtained in the same manner as in Example 1.
[0148] <Example 7> A biaxially oriented polypropylene film was obtained in the same manner as in Example 6, except that in the longitudinal stretching treatment, the rubber hardness of the stretching nip rolls was set to 50°.
[0149] <Example 8> In producing the cast sheet, a biaxially oriented polypropylene film was obtained in the same manner as in Example 1, except that the casting drum was D in Table 1, the air knife blowing speed was 70 m / sec, and the distance between the air knife outlet and the sheet was 5 mm.
[0150] <Example 9> A biaxially oriented polypropylene film was obtained in the same manner as in Example 1, except that the thickness of the finally wound biaxially oriented polypropylene film was 1.8 μm.
[0151] <Example 10> A biaxially oriented polypropylene film was obtained in the same manner as in Example 1, except that the thickness of the finally wound biaxially oriented polypropylene film was 6 μm.
[0152] <Example 11> A biaxially oriented polypropylene film was obtained in the same manner as in Example 1, except that in the production of the cast sheet, the resin A was supplied to the extruder.
[0153] <Comparative Example 1> In the production of the cast sheet, the same procedure as in Example 1 was used except that the wind speed of the air blown from the air knife was set to 140 m / sec. In this case, the wind from the air knife entered between the resin extruded in a sheet form from the T-die and the casting drum, and the film vibration of the molten resin from the T-die outlet to the close contact with the casting drum became significant, so that it was not possible to produce a biaxially stretched film.
[0154] <Comparative Example 2> A biaxially oriented polypropylene film was obtained in the same manner as in Example 4, except that in producing the cast sheet, the air blowing speed of the air knife was 70 m / sec and the distance between the air knife outlet and the sheet was 5 mm.
[0155] <Comparative Example 3> A biaxially oriented polypropylene film was obtained in the same manner as in Example 5, except that in producing the cast sheet, the air blowing speed of the air knife was 70 m / sec and the distance between the air knife outlet and the sheet was 5 mm.
[0156] <Comparative Example 4> A biaxially oriented polypropylene film was obtained in the same manner as in Example 6, except that the temperature of the stretching nip rolls was set to 90° C. in the longitudinal stretching treatment.
[0157] <Comparative Example 5> A biaxially oriented polypropylene film was obtained in the same manner as in Example 1, except that the thickness of the finally wound biaxially oriented polypropylene film was 1.6 μm.
[0158] <Comparative Example 6> A biaxially oriented polypropylene film was obtained in the same manner as in Example 12, except that in the longitudinal stretching treatment, the temperature of the stretching nip rolls was 90° C. and the hardness of the stretching nip rolls was 50°.
[0159] [Table 2]
[0160] (4) Measurement of properties of biaxially oriented polypropylene film (4-1) Measurement of spots From the center position in the width direction of each biaxially stretched polypropylene film of the examples and comparative examples, 50 mm x 50 mm measurement samples were cut out at a total of 10 locations every 10 m in the longitudinal direction. Next, using a digital scope (Keyence Corporation digital microscope VHX-2000), lens magnification: 30 times, light amount: 50% of full range, measurement method: reflection measurement, field of view: 11.5 mm x 8.6 mm, one side of each measurement sample (the surface on which the metal layer is laminated when the capacitor is manufactured) was observed in "halation removal + sharp mode (a process is performed to emphasize the outline with vivid colors and remove glare)", and the number of approximately elliptical "spots" (a representative one is shown in Figure 1) observed within the field of view was counted. If a part of the spot was not within the field of view, the spot was not counted. The number of spots in the visual field of each measurement sample (10 in total) was totaled, and the total value obtained was divided by 10 (= number of measurement samples) to obtain the average number of oval spots per visual field (area of 11.5 mm × 8.6 mm).
[0161] In addition, for each of the spots measured above, the longitudinal and lateral diameters of the biaxially oriented polypropylene film were measured, and the longer one (the major diameter of the spot) was taken as the maximum length of the spot (in the representative example shown in Figure 2, the lateral diameter is the major diameter). The maximum lengths of each spot were totaled, and the total was divided by the number of spots to determine the average maximum length of the spots.
[0162] (4-2) Measurement of peak height Rpk and valley depth Rvk The protruding peak height Rpk and protruding valley depth Rvk of one side (the side on which the metal layer is laminated when the capacitor is manufactured) of the biaxially oriented polypropylene film of the examples and comparative examples were measured using a non-contact optical interference surface shape measuring instrument "VertScan2.0 (model: R5500GML)" manufactured by Ryoka Systems Co., Ltd. First, using the WAVE mode, a 530white filter and a 1×BODY lens barrel were applied, and a ×10 objective lens was used to measure 470.92 μm × 353.16 μm per field of view.
[0163] Within the spots, for each of the spots measured in (4-1) above, measurements were taken at five locations shown in Figure 3 (the intersection of the long axis and the short axis, the center of the line connecting one end of the long axis and the intersection, the center of the line connecting the other end of the long axis and the intersection, the center of the line connecting one end of the short axis and the intersection, and the center of the line connecting the other end of the short axis and the intersection).
[0164] Outside the spot, measurements were taken at the center of each measurement sample.
[0165] The obtained data was subjected to noise removal processing using a median filter (3 x 3), and then Gaussian filter processing with a cutoff value of 30 μm was performed to remove waviness components. This made it possible to properly measure the condition of the measurement surface. Next, analysis was performed using the "VS-Viewer" analysis software of "VertScan2.0", and the average values of the protruding peak height Rpk and protruding valley depth Rvk obtained at the above points were calculated for the lubricity evaluation parameters. Specifically, it is as follows.
[0166] The measured values of the protruding peak height Rpk within the spots were summed, and the resulting sum was divided by X (= number of measured spots × 5 (measurement points within one spot)) to determine the average protruding peak height Rpk within the spots.
[0167] The measured values of the protruding peak height Rpk outside the spots of each measurement sample were summed, and the obtained sum was divided by 10 (= the number of measurement samples) to obtain the average protruding peak height Rpk outside the spots.
[0168] The average protruding peak height Rpk inside the spot was subtracted from the average protruding peak height Rpk outside the spot to determine the difference between the two.
[0169] The average protruding peak height Rpk of the film was determined by adding the average protruding peak height Rpk outside the spots and the average protruding peak height Rpk inside the spots and dividing the result by 2. When the average number of spots was 0, the average measurement value of the center of each measurement sample was determined as the average protruding peak height Rpk of the film.
[0170] The measured values of the protruding valley depth Rvk within the spots were summed, and the obtained sum was divided by X (= number of measured spots × 5 (measurement points within one spot)) to obtain the average protruding valley depth Rvk within the spots.
[0171] The measured values of the protruding valley depth Rvk outside the spots of each measurement sample were summed, and the obtained sum was divided by 10 (= the number of measurement samples) to obtain the average protruding valley depth Rvk outside the spots.
[0172] The average protruding valley depth Rvk inside the spot was subtracted from the average protruding valley depth Rvk outside the spot to obtain the difference between the two.
[0173] The average protruding valley depth Rvk of the film was determined by adding the average protruding valley depth Rvk outside the spots and the average protruding valley depth Rvk inside the spots and dividing the resulting value by 2. When the average number of spots was 0, the average measurement value of the center of each measurement sample was determined as the average protruding valley depth Rvk of the film.
[0174] (4-3) Measurement of the number of insulation defects Using an insulation defect inspection device with an unwinding / winding mechanism, the number of insulation defects (number / 10 m) of the biaxially oriented polypropylene films of the examples and comparative examples was measured. 2) was measured. The polypropylene film to be tested was passed between a high-voltage electrode and an earthed metal roller, and a DC voltage was applied while the film was being run. The number of discharges that occurred at the insulation defects was counted using a counter attached to the device. The number of measured values was divided by the measured area to determine the number of insulation defects (number / 10m 2 The measurement conditions were as follows: Distance between high voltage electrode and earthed metal roller: 50μm The contact angle between the film and the grounded metal roller: 120° - Shape of high voltage electrode: Metal plate with a thickness of 4 mm and the same width as the metal roller Unwinding speed: 20m / min DC voltage: 600V / μm Measurement area: 472m 2 Test environment temperature: 20℃.
[0175] (4-4) Measurement of slow axis angle and variation range of slow axis angle From the center of each of the biaxially stretched polypropylene films of the Examples and Comparative Examples, 50 mm x 50 mm measurement samples were cut out at 10 m intervals in the longitudinal direction, a total of 10 positions (0 m, 10 m, 20 m, 30 m, 40 m, 50 m, 60 m, 70 m, 80 m, and 90 m positions). Next, the width direction of the measurement sample was set to 0°, and the acute angle formed by the width direction of the measurement sample and the slow axis was measured as the slow axis angle. Among the 10 measurement samples, the difference between the maximum and minimum values of the slow axis angle was obtained as the "change width". The measurement device and measurement conditions are as follows.
[0176] Measurement equipment: Retardation measurement equipment RE-100 manufactured by Otsuka Electronics Co., Ltd. Light source: Laser light emitting diode (LED) Bandpass filter: 550 nm (measurement wavelength) Measurement interval: 0.1 sec Accumulation times: 10 times Number of measurement points: 15 points Gain: 10dB Measurement environment: temperature 23℃, humidity 60%.
[0177] (4-5) Measurement results The measurement results of the properties of the biaxially oriented polypropylene film are shown in Table 3.
[0178] [Table 3]
[0179] (5) Evaluation of process passability The production of the biaxially stretched films of the Examples and Comparative Examples was started, and the time from the point when the obtained film thickness reached the target thickness (Table 2) ±2% until the film broke due to stretching (time during which film production could be continued) was measured. The point when the thickness reached the target thickness ±2% was measured and confirmed according to the thickness measurement method described in (3) above. Based on the obtained time, the processability was evaluated according to the following evaluation criteria. The results are shown in Table 4 below. A++: Film formation was possible without breakage even after 48 hours. A+: A film was formed without stretching breakage within more than 32 hours and less than 48 hours. A: A film was formed without stretching breakage in more than 24 hours but less than 32 hours. B: A film was formed without stretching breakage within more than 16 hours and less than 24 hours. C: Stretching failure occurred after more than 8 hours and less than 16 hours. D: Stretching failure occurred within 8 hours. E: Film formation was not possible.
[0180] (6) Voltage resistance evaluation Capacitors were produced using the biaxially stretched films of the examples and comparative examples, and the voltage resistance of the capacitors was evaluated.
[0181] (6-1) Making a capacitor Using a vacuum deposition machine manufactured by ULVAC Corporation, the measurement sample obtained in (4-1) above was subjected to aluminum deposition with a T-margin deposition pattern at a deposition resistance of 20 Ω / □ to obtain a metallized film containing a metal film on one side of a biaxially oriented polypropylene film.
[0182] After slitting to a width of 50 mm, the two metallized films were put together and wound 840 turns at a winding tension of 210 g using an automatic winder, 3KAW-N2, manufactured by Kaito Seisakusho Co., Ltd. The wound element was heat-treated at 120°C for 15 hours while being pressed, after which zinc metal was sprayed onto the element end faces to obtain a flat capacitor. Lead wires were soldered to the end faces of the flat capacitor, and then the capacitor was sealed with epoxy resin. The capacitance of the obtained capacitor was 50 μF.
[0183] (6-2) Evaluation of initial voltage resistance The initial capacitance (C0) of the capacitor before the test was measured using an LCR HiTester 3522-50 manufactured by Hioki E.E. Corporation. Next, a DC voltage of 450 V / μm was applied to the capacitor for 10 seconds. The capacitance (C1) of the capacitor after the voltage application was measured in the same manner, and the rate of change in capacitance before and after the voltage application was calculated using the following formula.
[0184]
number
[0185] The capacitance change rate ΔC was measured for 100 elements and evaluated according to the following criteria. The number of capacitors rated A+ to C was calculated, and the ratio of A+ to A capacitors (initial voltage yield) was calculated. An initial voltage yield of 95% or more was considered to be acceptable. A+: ΔC is less than -0.2%. A: ΔC is less than -0.5% and less than -1%. B: ΔC is less than -1% and less than -2%. C: ΔC is -2% or less.
[0186] (6-3) Evaluation of long-term voltage resistance The initial capacitance (C0) of the capacitor before the test was measured using a Hioki E.E. Corporation LCR HiTester 3522-50. Next, a DC voltage of 320 V / μm was continuously applied to the capacitor for 1000 hours in a high temperature chamber at 115°C. The capacitance (C1000 ) was measured in the same way, and the capacity change rate (ΔC 1000 ) was calculated according to the following formula:
[0187]
number
[0188] The above capacity change rate ΔC 1000 The measurement was performed on 100 elements, and the evaluation was performed according to the following criteria. The number of capacitors rated A+ to C was calculated, and the ratio of A+ and A capacitors (long-term voltage withstand yield) was calculated. A long-term voltage withstand yield of 90% or more was considered to be acceptable. A+:ΔC 1000 But it's less than 0.5%. A: ΔC 1000 But below -0.5%, less than -5%. B: ΔC 1000 But below -5%, less than -10%. C: ΔC 1000 But it's less than -10%.
[0189] (7) Evaluation results The evaluation results of processability and voltage resistance are shown in Table 4.
[0190] [Table 4]
Claims
1. A biaxially oriented polypropylene film having a first surface and a second surface, The average maximum length of the substantially elliptical spots on the first surface is 3.0 mm or less; and The difference between the average protruding peak height Rpk outside the spots and the average protruding peak height Rpk within the spots is 0.040 μm or less. Biaxially oriented polypropylene film.
2. 2. The biaxially oriented polypropylene film according to claim 1, wherein the difference between the average protruding valley depth Rvk outside the spots and the average protruding valley depth Rvk within the spots is 0.020 μm or less.
3. 2. The biaxially oriented polypropylene film according to claim 1, wherein the change range of the slow axis angle is in the range of 0.3° to 2.8°.
4. 2. The biaxially oriented polypropylene film according to claim 1, wherein the average number of approximately elliptical spots per 11.5 mm x 8.6 mm area of the first surface is 0.6 or less.
5. The polypropylene resin constituting the biaxially oriented polypropylene film has a weight average molecular weight Mw of 250,000 or more and 450,000 or less, a ratio of the weight average molecular weight Mw to the number average molecular weight Mn (Mw / Mn) of 5.0 or more and 12.0 or less, a melt flow rate at 230°C and a load of 2.16 kg of 7.0 g / 10 min or less, and a heptane insoluble content of 96.0% or more and 99.5% or less.
6. The biaxially oriented polypropylene film according to claim 1, having a thickness of 1.7 μm or more and 6.5 μm or less.
7. 2. The biaxially oriented polypropylene film of claim 1 which is a monolayer film.
8. The biaxially oriented polypropylene film according to any one of claims 1 to 7, which is for a capacitor.
9. A metal layer-integrated polypropylene film comprising the biaxially oriented polypropylene film according to any one of claims 1 to 7 and a metal layer disposed on one or both sides of the biaxially oriented polypropylene film.
10. A capacitor comprising the metal layer-integrated polypropylene film according to claim 9.
11. A method for producing the biaxially oriented polypropylene film according to any one of claims 1 to 7, comprising: obtaining a cast sheet using a casting drum having a microcracked surface in which, when a virtual line having a length of 0.1 mm is provided at any position on the surface in the width direction, 1 to 15 grooves intersect with the virtual line and the groove width is 1 μm to 10 μm; and subjecting the cast sheet to a biaxial stretching treatment.
Citation Information
Patent Citations
Cooling device for melted polymer sheet
JP1983183220A
Cooling device for molten polymer sheet
JP1987204920A
Polypropylene film, metal layer-integrated polypropylene film, film capacitor and film roll
JP2020100800A
Polypropylene film roll and metalized polypropylene film roll
JP2020200188A
Film capacitor, film for film capacitor, method for manufacturing film for film capacitor, and method for manufacturing film capacitor
WO2019069540A1