Heat dissipation resin composition

The resin composition addresses the issue of increased viscosity by incorporating an organic phosphonic acid ester, ensuring reduced viscosity and enhanced heat dissipation through the use of specific components.

JP2024154259AInactive Publication Date: 2024-10-30PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023068001
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-10-30
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The viscosity of heat dissipating resin compositions increases when the content of inorganic fillers is increased, leading to a decrease in fluidity and compromising heat dissipation properties.

Method used

A heat dissipating resin composition comprising an epoxy compound, a curing agent, an inorganic filler, a dispersant, and an organic phosphonic acid ester with a molecular weight of 1000 or less, which reduces viscosity while maintaining good heat dissipation properties.

Benefits of technology

The composition achieves reduced viscosity and maintains effective heat dissipation, facilitating easier application and improved thermal conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154259000001
    Figure 2024154259000001
  • Figure 2024154259000002
    Figure 2024154259000002
  • Figure 2024154259000003
    Figure 2024154259000003
Patent Text Reader

Abstract

To provide a heat dissipation resin composition which can reduce viscosity while maintaining good heat dissipation property.SOLUTION: A heat dissipation resin composition contains an epoxy compound (A), a curing agent (B), an inorganic filler (C), a dispersion agent (D), and organic phosphonic acid ester (E) having a molecular weight of 1,000 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates generally to heat dissipating resin compositions, and more particularly to heat dissipating resin compositions containing inorganic fillers. [Background technology]

[0002] Patent Document 1 discloses a curable composition used as a heat dissipation material for heat generating parts or components. This curable composition contains an epoxy compound (A), an inorganic filler (B) made of an inorganic powder having at least two frequency maximum peaks within the range of 0.5 to 100 μm in particle size distribution, and a dispersant (C) having an acidic phosphate group. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-133454 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, in the curable composition of Patent Document 1, when the content of the inorganic filler (B) is increased in order to further enhance the heat dissipation property, the viscosity increases and the flowability is likely to decrease.

[0005] An object of the present disclosure is to provide a heat-dissipating resin composition that can reduce the viscosity while maintaining good heat dissipation properties. [Means for solving the problem]

[0006] A heat dissipating resin composition according to one embodiment of the present disclosure contains an epoxy compound (A), a curing agent (B), an inorganic filler (C), a dispersant (D), and an organic phosphonic acid ester (E) having a molecular weight of 1,000 or less. Effect of the Invention

[0007] According to the present disclosure, it is possible to reduce viscosity while maintaining good heat dissipation properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] 1. Overview Conventionally, the viscosity of a heat dissipating resin composition has been reduced by dispersing an inorganic filler with a dispersant. The present inventor has found that there is an optimal range for the content of the dispersant in order to reduce the viscosity of the heat dissipating resin composition. The present inventor has continued research and development and found that the viscosity of the heat dissipating resin composition can be further reduced by allowing an organic phosphonic acid ester to coexist with a dispersant, and has completed the heat dissipating resin composition according to this embodiment.

[0009] That is, the heat dissipating resin composition according to this embodiment contains an epoxy compound (A), a curing agent (B), an inorganic filler (C), a dispersant (D), and an organic phosphonic acid ester (E) having a molecular weight of 1,000 or less.

[0010] In this way, the heat dissipating resin composition can obtain good heat dissipation properties by containing the inorganic filler (C). Furthermore, in the heat dissipating resin composition, the dispersant (D) and the organic phosphonic acid ester (E) are coexisted, so that the viscosity can be reduced while maintaining good heat dissipation properties.

[0011] 2.Details (1) Composition of heat dissipating resin composition The heat dissipating resin composition according to this embodiment contains an epoxy compound (A), a curing agent (B), an inorganic filler (C), a dispersant (D), and an organic phosphonic acid ester (E). It is preferable that the heat dissipating resin composition does not substantially contain an organic solvent. That is, it is preferable that the heat dissipating resin composition does not contain an organic solvent except for those that are inevitably contained. That is, it is preferable that the heat dissipating resin composition is solvent-free.

[0012] Each component of the heat dissipating resin composition will be described below in order.

[0013] <Epoxy compound (A)> The epoxy compound (A) can function as a binder in the heat-dissipating resin composition, that is, the epoxy compound (A) can become a bond between particles of the inorganic filler (C) and can make the heat-dissipating resin composition into a paste.

[0014] The epoxy compound (A) is a compound containing one, preferably two or more epoxy groups in one molecule. The epoxy compound (A) is not particularly limited, but examples thereof include glycidylamine type epoxy resin, bisphenol type epoxy resin, hydrogenated bisphenol type epoxy resin, biphenyl type epoxy resin, naphthalene ring-containing epoxy resin, alicyclic epoxy resin, dicyclopentadiene type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, triphenylmethane type epoxy resin, aliphatic epoxy resin, triglycidyl isocyanurate, and glycidyl group-containing silicone resin.

[0015] The epoxy equivalent of the epoxy compound (A) is preferably 50 g / eq or more, more preferably 80 g / eq or more, and even more preferably 90 g / eq or more. On the other hand, the epoxy equivalent of the epoxy compound (A) is preferably 500 g / eq or less, more preferably 400 g / eq or less, and even more preferably 180 g / eq or less.

[0016] The viscosity of the epoxy compound (A) at 25° C. is preferably 0.5 mPa·s or more, more preferably 1 mPa·s or more, and even more preferably 1.5 mPa·s or more. On the other hand, the viscosity of the epoxy compound (A) at 25° C. is preferably 5000 mPa·s or less, more preferably 4500 mPa·s or less, and even more preferably 4000 mPa·s or less.

[0017] <Hardening agent (B)> The curing agent (B) may be either a substance that accelerates the curing reaction of the epoxy compound (A) or a substance that reacts with the epoxy compound (A) to become part of the cured product. The curing agent (B) is not particularly limited, but examples thereof include imidazole curing agents, acid anhydride curing agents, phenolic curing agents, amine curing agents, polymercaptan curing agents, polyaminoamide curing agents, isocyanate curing agents, and blocked isocyanate curing agents.

[0018] Examples of the imidazole curing agent include 2-ethyl-4-methylimidazole, 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, and 2-heptadecylimidazole.

[0019] The curing agent (B) preferably contains an imidazole curing agent. In this case, the viscosity of the heat-dissipating resin composition can be further reduced. Furthermore, the storage stability of the heat-dissipating resin composition can be improved.

[0020] The curing agent (B) is preferably in a liquid state, in which case the viscosity of the heat-dissipating resin composition can be further reduced.

[0021] The content of the curing agent (B) is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and even more preferably 1% by mass or more, based on the total mass of the heat dissipating resin composition. On the other hand, the content of the curing agent (B) is preferably 10% by mass or less, more preferably 7% by mass or less, and even more preferably 5% by mass or less, based on the total mass of the heat dissipating resin composition.

[0022] <Inorganic filler (C)> The inorganic filler (C) is a component that imparts heat dissipation properties such as thermal conductivity to the heat dissipation resin composition.

[0023] Preferably, the inorganic filler (C) contains at least one compound selected from the group consisting of aluminum nitride, aluminum oxide, crystalline silica, aluminum, silicon nitride, silicon carbide, zinc oxide, magnesium oxide, silver, copper, boron nitride, aluminum hydroxide, magnesium carbonate, anhydrous magnesium carbonate, and carbonaceous materials, which can further enhance the heat dissipation properties of the heat dissipation resin composition.

[0024] Here, the carbon-based material means a material whose main component is carbon. The main component refers to the component with the highest content, and the content is preferably 50% by mass or more, more preferably 90% by mass or more. The carbon-based material is not particularly limited, but examples thereof include graphite, graphene, carbon nanotubes, carbon fibers, fullerenes, and carbon black.

[0025] The thermal conductivity of the inorganic filler (C) is preferably 10 W / m·K or more, more preferably 25 W / m·K or more, and even more preferably 35 W / m·K or more. When the thermal conductivity of the inorganic filler (C) is 10 W / m·K or more, the heat dissipation property of the heat dissipation resin composition can be further improved. On the other hand, the upper limit of the thermal conductivity of the inorganic filler (C) is not particularly limited, but is, for example, 1500 W / m·K. However, from the viewpoint of heat dissipation, it is desirable that the thermal conductivity of the inorganic filler (C) is as high as possible.

[0026] The content of the inorganic filler (C) is preferably 40% by volume or more, more preferably 50% by volume or more, and even more preferably 60% by volume or more, based on the total volume of the heat-dissipating resin composition. When the content of the inorganic filler (C) is 40% by volume or more, the heat dissipation property of the heat-dissipating resin composition can be further improved. On the other hand, the content of the inorganic filler (C) is preferably 95% by volume or less, more preferably 90% by volume or less, and even more preferably 85% by volume or less, based on the total volume of the heat-dissipating resin composition. When the content of the inorganic filler (C) is 95% by volume or less, an increase in the viscosity of the heat-dissipating resin composition can be suppressed.

[0027] The content of the inorganic filler (C) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, based on the total mass of the heat-dissipating resin composition. When the content of the inorganic filler (C) is 70% by mass or more, the heat dissipation property of the heat-dissipating resin composition can be further improved. On the other hand, the content of the inorganic filler (C) is preferably 99% by mass or less, more preferably 98% by mass or less, and even more preferably 97% by mass or less, based on the total mass of the heat-dissipating resin composition. When the content of the inorganic filler (C) is 99% by mass or less, an increase in the viscosity of the heat-dissipating resin composition can be suppressed.

[0028] At least a part of the inorganic filler (C) has an average particle size of preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more. When the average particle size of the inorganic filler (C) is 10 μm or more, an increase in the viscosity of the heat dissipating resin composition can be suppressed. The average particle size means the particle size (D50) when the cumulative amount from the small diameter side is 50% in the volume-based particle size distribution measured by a laser diffraction scattering type particle size distribution measuring device.

[0029] On the other hand, the average particle size of the inorganic filler (C) is preferably 80 μm or less, more preferably 70 μm or less, and further preferably 60 μm or less. By making the average particle size of the inorganic filler (C) 80 μm or less, sedimentation of the inorganic filler (C) can be suppressed in the heat dissipating resin composition.

[0030] <Dispersant (D)> The dispersant (D) is a component that disperses the inorganic filler (C) in the heat-dissipating resin composition by blending the epoxy compound (A) with the inorganic filler (C).

[0031] The dispersant (D) preferably has a phosphate group or a phosphate group as an adsorptive group (hydrophilic group) and a polyester chain as a hydrophobic group. That is, the dispersant (D) preferably has a structure in which a phosphate group or a phosphate group is bonded to a polyester chain. A specific example is polyester phosphate.

[0032] The weight average molecular weight of the dispersant (D) is preferably 1000 or more, more preferably 2000 or more, and even more preferably 3000 or more. When the weight average molecular weight of the dispersant (D) is 1000 or more, it is possible to suppress a decrease in the heat resistance of the cured product of the heat dissipating resin composition. On the other hand, the weight average molecular weight of the dispersant (D) is preferably 100,000 or less, more preferably 90,000 or less, and even more preferably 80,000 or less. When the weight average molecular weight of the dispersant (D) is 100,000 or less, it is possible to suppress an increase in the viscosity of the heat dissipating resin composition.

[0033] The content of the dispersant (D) is preferably 2% by mass or more, more preferably 2.5% by mass or more, and even more preferably 3% by mass or more, based on the total mass of the heat-dissipating resin composition. When the content of the dispersant (D) is 2% by mass or more, the viscosity of the heat-dissipating resin composition can be reduced. Furthermore, the adhesive strength of the heat-dissipating resin composition to a metal can be increased. The metal is not particularly limited, but for example, aluminum and the like can be mentioned. On the other hand, the content of the dispersant (D) is preferably 10% by mass or less, more preferably 8% by mass or less, and even more preferably 7% by mass or less, based on the total mass of the heat-dissipating resin composition. When the content of the dispersant (D) is 10% by mass or less, the viscosity of the heat-dissipating resin composition can be reduced. Furthermore, the adhesive strength of the heat-dissipating resin composition to a metal can be increased.

[0034] <Organic phosphonate (E)> The organic phosphonic acid ester (E) is a component that reduces the viscosity of the heat-dissipating resin composition by coexisting with the dispersant (D). That is, the viscosity of the heat-dissipating resin composition containing both the dispersant (D) and the organic phosphonic acid ester (E) is lower than the viscosity of the heat-dissipating resin composition containing the dispersant (D) but not the organic phosphonic acid ester (E). This is particularly effective when the inorganic filler (C) contains aluminum nitride and / or aluminum oxide.

[0035] The organic phosphonate ester (E) is a compound obtained by dehydration condensation of an organic phosphonic acid and a compound containing a hydroxyl group (such as an alcohol). The organic phosphonate ester (E) preferably includes a compound represented by the general formula (1).

[0036] [ka]

[0037] In general formula (1), R 1 and R 2 are the same or different and each represents a hydrocarbon group; R 3 represents an organic group. The organic group means a monovalent group containing at least one carbon atom. When the organic phosphonic acid ester (E) contains a compound represented by general formula (1), the viscosity of the heat dissipating resin composition can be reduced while the adhesive strength to metals can be increased.

[0038] Preferably, R in general formula (1) 3 The (organic group) contains at least one group selected from the group consisting of a hydroxy group, an epoxy group, a phenyl group, an ester bond, an ether bond, an amino group, and a carboxy group, which can further reduce the viscosity and further increase the adhesive strength to metals.

[0039] Specifically, the organic phosphonate ester (E) preferably contains at least one compound selected from the group consisting of a compound represented by formula (E1), a compound represented by formula (E2), a compound represented by formula (E3), a compound represented by formula (E4), and a compound represented by formula (E5).

[0040] [ka]

[0041] The compound represented by formula (E1) is diethyl glycidyl phosphonate.

[0042] [ka]

[0043] The compound represented by formula (E2) is diethyl hydroxymethylphosphonate.

[0044] [ka]

[0045] The compound represented by formula (E3) is ethyl diethylphosphonoacetate.

[0046] [ka]

[0047] The compound represented by formula (E4) is diethyl benzyl phosphonate.

[0048] [ka]

[0049] The compound represented by formula (E5) is diethyl (3,5-di-t-butyl-4-hydroxybenzyl)phosphonate.

[0050] The molecular weight of the organic phosphonate (E) is not more than 1000, preferably not more than 900, and more preferably not more than 800. On the other hand, the lower limit of the molecular weight of the organic phosphonate (E) is not particularly limited, but is, for example, 100.

[0051] The content of the organic phosphonic acid ester (E) is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1.0% by mass or more, based on the total mass of the heat-dissipating resin composition. By having the content of the organic phosphonic acid ester (E) be 0.1% by mass or more, the viscosity of the heat-dissipating resin composition can be reduced while the adhesive strength to metal can be increased. On the other hand, the content of the organic phosphonic acid ester (E) is preferably 20% by mass or less, more preferably 18% by mass or less, and even more preferably 15% by mass or less, based on the total mass of the heat-dissipating resin composition. By having the content of the organic phosphonic acid ester (E) be 20% by mass or less, the decrease in the glass transition temperature (Tg) of the cured product of the heat-dissipating resin composition can be suppressed. In other words, the decrease in the heat resistance of the cured product of the heat-dissipating resin composition can be suppressed.

[0052] (2) Method for producing heat-dissipating resin composition and its uses The heat dissipating resin composition according to this embodiment is obtained by mixing the epoxy compound (A), the curing agent (B), the inorganic filler (C), the dispersant (D) and the organic phosphonic acid ester (E). In this way, the heat dissipating resin composition according to this embodiment can obtain good heat dissipation properties by containing the inorganic filler (C). Furthermore, in the heat dissipating resin composition according to this embodiment, the viscosity can be reduced while maintaining good heat dissipation properties by coexisting the dispersant (D) and the organic phosphonic acid ester (E).

[0053] The heat-dissipating resin composition is preferably in a paste form at room temperature. The room temperature is, for example, from 10° C. to 30° C. In this way, if the heat-dissipating resin composition is in a paste form at room temperature, the heat-dissipating resin composition can be easily applied.

[0054] The heat dissipating resin composition according to the present embodiment is preferably used as a TIM (Thermal Interface Material). For example, when a substrate on which a component that is a heat generating body is mounted is housed in a housing, the heat dissipating resin composition can be interposed between the component and the housing to directly dissipate heat from the component to the housing. In addition, the heat dissipating resin composition can be interposed between the substrate and the housing to dissipate heat from the component to the housing via the substrate.

[0055] As described above, the heat dissipating resin composition according to the present embodiment can reduce the viscosity while maintaining good heat dissipation properties, so that, for example, even if the gap between a component and a housing is narrow, the heat dissipating resin composition can penetrate and fill the gap. The same applies to the gap between a substrate and a housing.

[0056] 3. Aspects As is apparent from the above embodiment, the present disclosure includes the following aspects.

[0057] The first aspect is a heat dissipating resin composition, which contains an epoxy compound (A), a curing agent (B), an inorganic filler (C), a dispersant (D), and an organic phosphonic acid ester (E) having a molecular weight of 1000 or less.

[0058] According to this aspect, it is possible to reduce the viscosity while maintaining good heat dissipation properties.

[0059] A second aspect is the heat-dissipating resin composition according to the first aspect, wherein the inorganic filler (C) has a thermal conductivity of 10 W / m·K or more.

[0060] According to this embodiment, the heat dissipation performance can be further improved.

[0061] A third aspect is a heat dissipating resin composition based on the first or second aspect, wherein the inorganic filler (C) contains at least one compound selected from the group consisting of aluminum nitride, aluminum oxide, crystalline silica, aluminum, silicon nitride, silicon carbide, zinc oxide, magnesium oxide, silver, copper, boron nitride, aluminum hydroxide, magnesium carbonate, anhydrous magnesium carbonate, and carbonaceous materials.

[0062] According to this embodiment, the heat dissipation performance can be further improved.

[0063] A fourth aspect is a heat-dissipating resin composition based on any one of the first to third aspects. In the fourth aspect, the organic phosphonic acid ester (E) includes a compound represented by general formula (1).

[0064] [ka] (In the formula, R 1 and R 2 are the same or different and each represents a hydrocarbon group; R 3 represents an organic group).

[0065] According to this aspect, it is possible to increase the adhesive strength to metal while reducing the viscosity.

[0066] A fifth aspect is a heat dissipating resin composition based on any one of the first to fourth aspects, wherein the organic group includes at least one group selected from the group consisting of a hydroxy group, an epoxy group, a phenyl group, an ester bond, an ether bond, an amino group, and a carboxy group.

[0067] According to this aspect, it is possible to increase the adhesive strength to metal while reducing the viscosity.

[0068] A sixth aspect is a heat-dissipating resin composition based on any one of the first to fifth aspects. In the sixth aspect, the content of the organic phosphonic acid ester (E) is 0.1 mass % or more and 20 mass % or less with respect to the total mass of the heat-dissipating resin composition.

[0069] According to this aspect, it is possible to increase the adhesive strength to metal while reducing the viscosity.

[0070] A seventh aspect is the heat-dissipating resin composition based on any one of the first to sixth aspects. In the seventh aspect, the weight-average molecular weight of the dispersant (D) is 1,000 or more and 100,000 or less.

[0071] According to this embodiment, the inorganic filler (C) can be easily dispersed.

[0072] An eighth aspect is a heat-dissipating resin composition based on any one of the first to seventh aspects. In the eighth aspect, the content of the dispersant (D) is 2 mass % or more and 10 mass % or less with respect to the total mass of the heat-dissipating resin composition.

[0073] According to this aspect, it is possible to increase the adhesive strength to metal while reducing the viscosity.

[0074] A ninth aspect is a heat-dissipating resin composition based on any one of the first to eighth aspects. In the ninth aspect, the content of the inorganic filler (C) is 40 volume % or more and 95 volume % or less with respect to the total volume of the heat-dissipating resin composition.

[0075] According to this embodiment, the heat dissipation performance can be further improved.

[0076] A tenth aspect is a heat-dissipating resin composition based on any one of aspects 1 to 9. In the tenth aspect, the heat-dissipating resin composition is in a paste form at room temperature.

[0077] According to this embodiment, the heat dissipating resin composition can be easily applied. EXAMPLES

[0078] The present disclosure will be specifically described below with reference to examples, but the present disclosure is not limited to the following examples.

[0079] 1. Heat dissipating resin composition The raw materials shown in Tables 1 and 2 were blended and uniformly mixed and dispersed in a mixer to obtain a heat dissipating resin composition in a paste form at room temperature. Details of the raw materials are as follows.

[0080] <Epoxy compound (A)> Epoxy compound 1: glycidylamine type epoxy compound (manufactured by ADEKA Corporation, product name "EP-3950S", epoxy equivalent: 95 g / eq, viscosity: 650 mPa·s / 25°C).

[0081] <Hardening agent (B)> Hardener 1: 2-ethyl-4-methylimidazole (manufactured by Shikoku Chemicals Corporation, product name "2E4MZ").

[0082] <Inorganic filler (C)> Inorganic filler 1: AlN (Aluminum nitride powder, manufactured by Combustion Synthesis Co., Ltd., product name "AN-HF30LGLHTZ", thermal conductivity: 150-200 W / m K, average particle size: 30 μm) Inorganic filler 2: Al2O3 (manufactured by Sumitomo Chemical Co., Ltd., product name "AA2", thermal conductivity: 20 to 35 W / m·K, average particle size: 2.2 μm) Inorganic filler 3: Al2O3 (manufactured by Sumitomo Chemical Co., Ltd., product name "AA03", thermal conductivity: 20 to 35 W / m·K, average particle size: 0.40 μm).

[0083] <Dispersant (D)> Dispersant 1: Polyester phosphate (manufactured by BYK Japan KK, product name "BYK-W9010", weight average molecular weight: 5000 to 10000).

[0084] <Organic phosphonate (E)> Organic phosphonic acid ester 1: diethyl glycidyl phosphonate (manufactured by Katayama Chemical Industry Co., Ltd., trade name "E-100", compound represented by formula (E1), molecular weight: 194) Organic phosphonic acid ester 2: diethyl hydroxymethylphosphonate (manufactured by Johoku Chemical Industry Co., Ltd., trade name "JC-168", compound represented by formula (E2), molecular weight: 166) Organic phosphonic acid ester 3: ethyl diethyl phosphonoacetate (manufactured by Johoku Chemical Industry Co., Ltd., trade name "JC-224", compound represented by formula (E3), molecular weight: 224) Organic phosphonic acid ester 4: diethyl benzyl phosphonate (manufactured by Johoku Chemical Industry Co., Ltd., trade name "JC-228", compound represented by formula (E4), molecular weight: 228).

[0085] <Additives (F)> Additive 1: 3-glycidoxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM-403") Additive 2: o-cresyl glycidyl ether (manufactured by Yokkaichi Chemical Co., Ltd., product name "OCR-EP") Additive 3: 1,6-Hexanediol diglycidyl ether (manufactured by Yokkaichi Chemical Co., Ltd., product name "Epogose HD(D)").

[0086] 2. Evaluation (1) Viscosity The viscosity of the heat-dissipating resin composition was measured using an E-type viscometer (manufactured by Toki Sangyo Co., Ltd., model number: RC-215) under conditions of 25° C., a rotation speed of 0.3 rpm, and 200 seconds.

[0087] (2) Adhesive strength The adhesive strength was evaluated by measuring the tensile shear adhesive strength, which was measured in accordance with JIS K6850:1999 (Test method for tensile shear adhesive strength between adhesive and rigid adherend).

[0088] Two aluminum plates measuring 100 mm in length, 25 mm in width, and 1.6 mm in thickness were prepared as metal adherends. The tips of the two metal adherends were bonded together with a heat-dissipating resin composition to create a test piece. The overlapping portion (bonded portion) of the two metal adherends was in an area of ​​12.5 mm in length and 25 mm in width. The heat-dissipating resin composition was placed between the two metal adherends and thermally cured at 120°C for three hours.

[0089] A tensile test was performed on the above test pieces using a tensile testing machine (Shimadzu Corporation, Autograph, Model "AG-5kNX") at room temperature of 25°C and a tensile speed of 3920 N / min to measure the tensile shear strength. The point at which the tensile shear strength was maximum was taken as the tensile shear adhesive strength.

[0090] (3) Heat dissipation (3.1) Thermal resistance The heat dissipating resin composition was set on the probe of a thermal property measuring instrument (manufactured by Mentor Graphics, model "DynTIM Tester") conforming to ASTM-D5470, and the thermal property (thermal resistance) was measured.

[0091] Specifically, the uncured heat-dissipating resin composition was sandwiched between two aluminum plates and pressed with a thermal property measuring instrument so that the thickness of the heat-dissipating resin composition became 100 to 400 μm. Then, the thermal resistance was measured at a thickness of 100 to 400 μm with the pressure of the thermal property measuring instrument set to 0 (no pressure). In addition, a heat dissipating oil compound (manufactured by Shin-Etsu Chemical Co., Ltd., product name "G-779") was used to reduce the interfacial thermal resistance between the plate and the probe of the thermal property measuring instrument. The temperature gradient during the measurement was 60°C in the heating section and 25°C in the cooling section.

[0092] (3.2) Thermal conductivity The thermal resistance was measured at four points, and the thermal conductivity was calculated from these values.

[0093] The above results are shown in Tables 1 and 2.

[0094] [Table 1]

[0095] [Table 2]

Claims

1. The composition contains an epoxy compound (A), a curing agent (B), an inorganic filler (C), a dispersant (D), and an organic phosphonic acid ester (E) having a molecular weight of 1000 or less. Heat dissipating resin composition.

2. The thermal conductivity of the inorganic filler (C) is 10 W / m K or more. The heat dissipating resin composition according to claim 1 .

3. The inorganic filler (C) contains at least one compound selected from the group consisting of aluminum nitride, aluminum oxide, crystalline silica, aluminum, silicon nitride, silicon carbide, zinc oxide, magnesium oxide, silver, copper, boron nitride, aluminum hydroxide, magnesium carbonate, anhydrous magnesium carbonate, and carbon-based materials. The heat dissipating resin composition according to claim 1 .

4. The organic phosphonic acid ester (E) contains a compound represented by general formula (1), The heat dissipating resin composition according to claim 1 . (In the formula, R 1 and R 2 are the same or different and each represents a hydrocarbon group; R 3 represents an organic group)

5. the organic group contains at least one group selected from the group consisting of a hydroxy group, an epoxy group, a phenyl group, an ester bond, an ether bond, an amino group, and a carboxy group; The heat dissipating resin composition according to claim 4.

6. The content of the organic phosphonic acid ester (E) is 0.1 mass% or more and 20 mass% or less based on the total mass of the heat dissipating resin composition. The heat dissipating resin composition according to claim 1 .

7. The weight average molecular weight of the dispersant (D) is 1,000 or more and 100,000 or less. The heat dissipating resin composition according to claim 1 .

8. The content of the dispersant (D) is 2% by mass or more and 10% by mass or less based on the total mass of the heat dissipating resin composition. The heat dissipating resin composition according to claim 1 .

9. The content of the inorganic filler (C) is 40% by volume or more and 95% by volume or less based on the total volume of the heat dissipating resin composition; The heat dissipating resin composition according to claim 1 .

10. It is paste-like at room temperature. The heat dissipating resin composition according to claim 1 .

Citation Information

Patent Citations

  • Curable composition and cured product of the same

    JP2013133454A