Power storage device

The inclusion of a resin layer with a conductive agent between the current collector foil and active material layers in power storage devices addresses the risk of large current flow during internal short circuits, enhancing resistance and preventing damage.

JP2024154287APending Publication Date: 2024-10-30GS YUASA CORP

Patent Information

Application Number
JP2023068039
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-10-30

AI Technical Summary

Technical Problem

Conventional power storage devices are prone to large current flow during internal short circuits, posing a risk of potential damage.

Method used

A power storage device design that includes a resin layer containing a conductive agent between the current collector foil and the active material layers, increasing resistance and suppressing large current flow.

Benefits of technology

The resin layer effectively reduces large current flow and protects the device from internal short circuits by enhancing resistance and preventing electrolyte penetration through pinholes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154287000001_ABST
    Figure 2024154287000001_ABST
Patent Text Reader

Abstract

To provide a power storage device in which the flow of large current can be suppressed.SOLUTION: A power storage device includes a plurality of electrode units 100 stacked in a stacking direction. Each of the electrode units includes at least a current collecting foil 110, a positive electrode active material layer 111 formed on one surface of the current collecting foil, and a negative electrode active material layer 112 formed on the other surface of the current collecting foil. In at least one electrode unit, a resin layer 150 containing a conductive agent is disposed between the current collecting foil and at least one active material layer of the positive electrode active material layer and the negative electrode active material layer.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electricity storage device. [Background technology]

[0002] Conventionally, there is known an electricity storage device including an electrode unit in which active material layers (positive and negative active material layers) are formed on both sides of a current collector foil. For example, Patent Document 1 discloses an electricity storage device in which a positive active material layer is disposed on the surface of a positive current collector and a negative active material layer is disposed on the surface of a negative current collector. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2022-77634 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the above-mentioned conventional power storage devices, there is a risk that a large current will flow if an internal short circuit occurs. Therefore, a power storage device capable of suppressing the flow of a large current is desired.

[0005] The present invention was made by the inventors of the present application by focusing on the above-mentioned problem, and has an object to provide an electricity storage device capable of suppressing the flow of a large current. [Means for solving the problem]

[0006] An energy storage device according to one embodiment of the present invention includes a plurality of electrode units stacked in a stacking direction, each of the plurality of electrode units having at least a current collecting foil, a positive electrode active material layer formed on one surface of the current collecting foil, and a negative electrode active material layer formed on the other surface of the current collecting foil, and in at least one of the current collecting foil and the positive electrode active material layer, a resin layer containing a conductive agent is disposed between the current collecting foil and at least one of the positive electrode active material layer and the negative electrode active material layer. Effect of the Invention

[0007] According to the electricity storage device of the present invention, it is possible to suppress a large current flow. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a perspective view showing the appearance of a power storage device according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing an internal configuration of the electricity storage device according to the embodiment. [Diagram 3] FIG. 3 is a perspective view and a cross-sectional view showing a configuration of an electrode unit included in the power storage device according to the embodiment. [Figure 4] FIG. 4 is a cross-sectional view showing the configuration of a resin layer of the electrode unit according to the embodiment. [Diagram 5] FIG. 5 is a cross-sectional view showing the configuration of the electricity storage pack. [Figure 6] FIG. 6 is a cross-sectional view showing another configuration of the electricity storage pack. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] (1) An energy storage device according to one embodiment of the present invention includes a plurality of electrode units stacked in a stacking direction, each of the plurality of electrode units having at least a current collecting foil, a positive electrode active material layer formed on one surface of the current collecting foil, and a negative electrode active material layer formed on the other surface of the current collecting foil, and in at least one of the current collecting foil and the positive electrode active material layer, a resin layer containing a conductive agent is disposed between the current collecting foil and at least one of the positive electrode active material layer and the negative electrode active material layer.

[0010] According to this, in the electricity storage device, a resin layer containing a conductive agent is disposed between the current collector foil and at least one of the positive and negative active material layers. This makes it possible to increase the resistance between the current collector foil and the active material layer. Therefore, even if an internal short circuit occurs in the electricity storage device, the resin layer can suppress the flow of a large current.

[0011] (2) In the energy storage device described in (1) above, the current collecting foil may have two metal layers aligned in the stacking direction, and the metal layer of the two metal layers on which the resin layer is arranged may be thinner in the stacking direction than the metal layer on the opposite side to the resin layer.

[0012] When a current collecting foil has two metal layers, pinholes are likely to occur in the thinner metal layer. For this reason, a resin layer is placed on the thinner metal layer. This allows the metal layer to be protected by the resin layer, which makes it possible to prevent pinholes from occurring in the metal layer.

[0013] (3) In the energy storage device described in (1) or (2) above, the current collecting foil may have two metal layers aligned in the stacking direction, and the metal layer on which the resin layer is arranged of the two metal layers may be a plated layer plated on the metal layer opposite the resin layer.

[0014] According to this, when forming a current collecting foil having two metal layers, the current collecting foil can be easily formed by plating the metal layer with a plating layer. In this case, since pinholes are likely to occur in the plating layer, a resin layer is disposed on the plating layer. This makes it possible to protect the plating layer with the resin layer, thereby suppressing the occurrence of pinholes in the plating layer.

[0015] (4) In the energy storage device described in any one of (1) to (3) above, the resin layer may have a first portion located between the current collecting foil and the one of the active material layers, and a second portion protruding from between the current collecting foil and the one of the active material layers, and the second portion may be thicker in the stacking direction than the first portion.

[0016] According to this, the second portion of the resin layer protrudes from between the current collecting foil and the active material layer, so that the effect of the resin layer can be obtained even in the portion of the current collecting foil protruding from the active material layer. In particular, the second portion of the resin layer is thicker than the first portion, so that the effect of the resin layer can be further achieved in the second portion. In other words, the first portion located between the current collecting foil and the active material layer is made thinner by pressing or the like to have a relatively low resistance, and the second portion protruding from between the current collecting foil and the active material layer is made thicker to have a relatively high resistance, so that heat generation due to a foreign object short circuit, a nail short circuit, or the like can be suppressed.

[0017] (5) In the electricity storage device according to any one of (1) to (4) above, the current collecting foil and the one active material layer may be joined by the resin layer.

[0018] According to this, by bonding the current collector foil and the active material layer with the resin layer, it is possible to prevent the active material layer from falling off the current collector foil.

[0019] (6) In the electricity storage device according to any one of (1) to (5) above, the resin layer may have a characteristic that its resistance increases when heated.

[0020] According to this, since the resistance of the resin layer increases when heated, when an internal short circuit or the like occurs in the energy storage device and a large current flows, the resin layer is heated and the resistance of the resin layer increases, thereby making it possible to reduce the current flowing through the energy storage device.

[0021] (7) In the energy storage device described in any one of (1) to (6) above, the one active material layer may be larger in size than the other active material layer when viewed from the stacking direction, and the resin layer may be larger in size than the one active material layer when viewed from the stacking direction.

[0022] According to this, when the size of one active material layer is larger than the size of the other active material layer, the size of the resin layer is made larger than the size of one active material layer, so that the resin layer can cover the entire one active material layer having the larger size, thereby enhancing the effect of the resin layer.

[0023] Hereinafter, a description will be given of a power storage device according to an embodiment (including modified examples) of the present invention with reference to the drawings. Note that the embodiments described below are all comprehensive or specific examples. The numerical values, shapes, materials, components, the arrangement and connection of the components, manufacturing processes, and the order of the manufacturing processes shown in the following embodiments are merely examples and are not intended to limit the present invention. In each drawing, the dimensions are not strictly shown. In each drawing, the same or similar components are given the same reference numerals.

[0024] In the following description and drawings, the longitudinal direction of the power storage device, or the opposing direction of a pair of short side surfaces of the power storage device, is defined as the X-axis direction. The opposing direction of a pair of long side surfaces of the power storage device is defined as the Y-axis direction. The thickness direction of the power storage device, the stacking direction of the multiple electrode units, the stacking direction of the current collecting foils and active material layers, the arrangement direction of a pair of end members, or the up-down direction is defined as the Z-axis direction. These X-axis, Y-axis, and Z-axis directions intersect with each other (orthogonal in this embodiment). Note that, depending on the mode of use, the Z-axis direction may not be the up-down direction, but for convenience of explanation, the following description will be given assuming that the Z-axis direction is the up-down direction.

[0025] In the following description, the positive X-axis direction refers to the direction of the X-axis arrow, and the negative X-axis direction refers to the opposite direction to the positive X-axis direction. When simply referring to the X-axis direction, it refers to both or either of the positive and negative X-axis directions. The same applies to the Y-axis and Z-axis directions. Expressions indicating relative directions or attitudes, such as parallel and perpendicular, also include cases where the directions or attitudes are not strictly speaking the same. For example, two directions being parallel not only means that the two directions are completely parallel, but also means that the directions are substantially parallel, that is, that there is a difference of, for example, about a few percent. In the following description, when the term "insulation" is used, it means "electrical insulation."

[0026] (Embodiment) [1 General Description of Power Storage Device 10] First, the general description of the energy storage device 10 in this embodiment will be given. FIG. 1 is a perspective view showing the appearance of the energy storage device 10 according to this embodiment. FIG. 2 is a cross-sectional view showing the internal configuration of the energy storage device 10 according to this embodiment. Specifically, FIG. 2 is a cross-sectional view of the energy storage device 10 in FIG. 1 cut along the YZ plane passing through the line II-II. FIG. 2 shows each component included in the energy storage device 10. FIG. 3 is a perspective view and a cross-sectional view showing the configuration of the electrode unit 100 included in the energy storage device 10 according to this embodiment. Specifically, FIG. 3(a) is a perspective view showing the appearance of the electrode unit 100. FIG. 3(b) is a cross-sectional view showing the configuration of the electrode unit 100 in FIG. 3(a) cut along the YZ plane passing through the line IIIb-IIIb. In FIG. 3, for convenience of explanation, the seal portion 210 included in the electrode unit 100 is omitted.

[0027] The power storage device 10 is a device that can charge electricity from an external source and discharge electricity to the outside. The power storage device 10 in this embodiment has a substantially rectangular parallelepiped shape. Specifically, the power storage device 10 is a bipolar battery. The power storage device 10 is used as a battery for driving or starting an engine of a moving body such as an automobile, a motorcycle, a watercraft, a ship, a snowmobile, an agricultural machine, a construction machine, an automatic guided vehicle (AGV), or a railway vehicle for an electric railway. Examples of the above-mentioned automobiles include electric vehicles (EVs), hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), and fossil fuel (gasoline, diesel, liquefied natural gas, etc.) vehicles. Examples of the above-mentioned railway vehicles for an electric railway include electric trains, monorails, linear motor cars, and hybrid trains equipped with both a diesel engine and an electric motor. The power storage device 10 can also be used as a stationary battery for home or business use.

[0028] As shown in FIG. 1 and FIG. 2, the energy storage device 10 includes a plurality of electrode units 100, end units 101 and 102, a plurality of separators 140, and a pair of end members 300. Each of the plurality of electrode units 100, the end units 101, and the end units 102 is a rectangular plate-like portion in a plan view, and is stacked in the Z-axis direction. In the present embodiment, the plan view refers to a view from the stacking direction (Z-axis direction). The direction in which the plurality of electrode units 100, the end units 101, and the end units 102 are stacked (Z-axis direction) is also referred to as the stacking direction. The separator 140 is disposed between each of the plurality of electrode units 100 and the end units 101 and 102. The pair of end members 300 are disposed on both sides of the plurality of electrode units 100 and the end units 101 and 102 in the stacking direction (Z-axis direction). In the present embodiment, two electrode units 100 are stacked in the stacking direction between the end unit 101 and the end unit 102, but the number of stacked electrode units 100 is not particularly limited. The shapes of the electrode unit 100, the end unit 101, the end unit 102, etc. in a plan view are also not particularly limited.

[0029] [1.1 Description of the electrode unit 100] The configuration of the electrode unit 100 will be described in detail below with reference to Fig. 3. The electrode unit 100 is a single unit in which active material layers are formed on both sides of a single current collector foil. Each of the multiple electrode units 100 has at least a current collector foil 110, a positive electrode active material layer 120 formed on one side of the current collector foil 110, a negative electrode active material layer 130 formed on the other side of the current collector foil 110, and a seal portion 210. In this embodiment, the thickness of the electrode unit 100 (thickness in the stacking direction) is about 135 µm to 190 µm.

[0030] The current collecting foil 110 is a plate-like member having a rectangular shape in a plan view. The current collecting foil 110 is a metal foil. As shown in FIG. 3, the current collecting foil 110 has two metal layers 111 and 112 arranged in the stacking direction (Z-axis direction). The metal layers 111 and 112 are plate-like parts having the same size and shape in a plan view. Hereinafter, of the metal layers 111 and 112, the metal layer 111 on which the positive electrode active material layer 120 is formed is also referred to as the positive electrode metal layer 111, and the metal layer 112 on which the negative electrode active material layer 130 is formed is also referred to as the negative electrode metal layer 112. The positive electrode metal layer 111 is a metal layer located in the positive direction of the current collecting foil 110 on the Z-axis, and the negative electrode metal layer 112 is a metal layer located in the negative direction of the current collecting foil 110 on the Z-axis. That is, the current collecting foil 110 is formed by laminating the positive electrode metal layer 111 and the negative electrode metal layer 112 in a lamination direction in a state in which the positive electrode metal layer 111 and the negative electrode metal layer 112 are connected (contacted or joined) to each other. One of the positive electrode metal layer 111 and the negative electrode metal layer 112 may be a metal foil, and the other may be a plated layer plated on the metal foil. Alternatively, both the positive electrode metal layer 111 and the negative electrode metal layer 112 may be metal foils. When both the positive electrode metal layer 111 and the negative electrode metal layer 112 are metal foils, the current collecting foil 110 may be a clad material formed by joining two metal foils together, or may have two metal foils in a state in which the two metal foils are connected (contacted) without being joined to each other.

[0031] The material of the positive electrode metal layer 111 may be a metal such as aluminum, titanium, tantalum, or stainless steel, or an alloy thereof. Among these, from the viewpoint of the balance between the electric potential resistance, the high conductivity, and the cost, the material of the positive electrode metal layer 111 is preferably aluminum or an aluminum alloy. The form of the positive electrode metal layer 111 may be a plated layer, but from the viewpoint of workability and cost, a foil is preferable. That is, the positive electrode metal layer 111 is preferably an aluminum foil. The material of the negative electrode metal layer 112 may be a metal such as copper, nickel, stainless steel, or nickel-plated steel, or an alloy thereof, and among these, it is preferable to use copper or a copper alloy. The form of the negative electrode metal layer 112 may be a plated layer or a foil (copper foil), and examples of the copper foil include rolled copper foil and electrolytic copper foil. The thickness (thickness in the lamination direction) of the current collector foil 110 is about 20 μm to 30 μm. The positive electrode metal layer 111 has a thickness (thickness in the stacking direction) of about 5 μm to 20 μm, and the negative electrode metal layer 112 has a thickness (thickness in the stacking direction) of about 5 μm to 15 μm.

[0032] The positive electrode active material layer 120 is a positive electrode active material layer formed on one surface (surface in the positive direction of the Z axis) of the current collector foil 110. Specifically, the positive electrode active material layer 120 is formed on the positive electrode metal layer 111 (the outer surface (surface in the positive direction of the Z axis) of the positive electrode metal layer 111). The positive electrode active material layer 120 is formed in a rectangular shape smaller in size than the positive electrode metal layer 111 in a planar view according to the shape of the positive electrode metal layer 111. Small size in a planar view means that the area in the XY plane is small. The same applies below. The thickness (thickness in the stacking direction) of the positive electrode active material layer 120 is about 70 μm to 100 μm.

[0033] The positive electrode active material layer 120 contains a positive electrode active material, and optionally contains a conductive agent, a binder, a thickener, a filler, etc. 2 (M1 is one or more metal elements selected from Li, Fe, Ni, Mn, Co, etc.), layered lithium transition metal oxides such as LiM2 2 O 4(M2 is one or more metal elements selected from Li, Fe, Ni, Mn, Co, etc.), spinel-type lithium transition metal oxides such as LiM3PO 4 , LiM3SiO 4 , LiM3BO 3 (M3 is one or more metal elements selected from Li, Fe, Ni, Mn, Co, etc.) and other polyanion compounds. As the positive electrode active material, one of these compounds may be used alone, or two or more may be mixed and used. The conductive agent contained in the positive electrode active material layer 120 is not particularly limited as long as it has conductivity. Examples of the conductive agent include carbon black such as furnace black, acetylene black, and Ketjen black, and natural or artificial graphite. Examples of the binder (binding agent) include fluororesin (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), sulfonated EPDM, and styrene butadiene rubber (SBR). Examples of the thickener include polysaccharide polymers such as carboxymethyl cellulose (CMC) and methyl cellulose.

[0034] The negative electrode active material layer 130 is a negative electrode active material layer formed on the other surface (surface in the negative Z-axis direction) of the current collector foil 110. Specifically, the negative electrode active material layer 130 is formed on the negative electrode metal layer 112 (the outer surface (surface in the negative Z-axis direction) of the negative electrode metal layer 112). In this embodiment, the negative electrode active material layer 130 is formed on the negative electrode metal layer 112 via a resin layer 150. That is, the electrode unit 100 further has a resin layer 150 formed on the negative electrode metal layer 112 (the outer surface (surface in the negative Z-axis direction) of the negative electrode metal layer 112), and the negative electrode active material layer 130 is formed on the resin layer 150. The negative electrode active material layer 130 is formed in a rectangular shape smaller in size than the negative electrode metal layer 112 in a planar view according to the shape of the negative electrode metal layer 112. The negative electrode active material layer 130 is formed in a larger size than the positive electrode active material layer 120 in a planar view. A large size in plan view means a large area in the XY plane. The same applies below. That is, the area in the XY plane of the negative electrode active material layer 130 is larger than that of the positive electrode active material layer 120. The thickness of the negative electrode active material layer 130 (thickness in the stacking direction) is about 45 μm to 60 μm.

[0035] The negative electrode active material layer 130 contains a negative electrode active material, and optionally contains optional components such as a conductive agent, a binder, a thickener, and a filler. The optional components such as the conductive agent, the binder, the thickener, and the filler can be the same as those in the positive electrode active material layer 120. As the negative electrode active material, a material capable of absorbing and releasing lithium ions is usually used. As the negative electrode active material, for example, metals or semi-metals such as Si and Sn; metal oxides or semi-metal oxides such as Si oxide and Sn oxide; and carbon materials such as graphite and non-graphitic carbon (easily graphitizable carbon or non-graphitizable carbon) can be used.

[0036] The sealing portion 210 is a portion disposed around the positive electrode active material layer 120 or the negative electrode active material layer 130. In the present embodiment, the sealing portion 210 is an annular portion disposed around the positive electrode active material layer 120 and the negative electrode active material layer 130 over the entire circumference of the positive electrode active material layer 120 and the negative electrode active material layer 130. Specifically, the sealing portion 210 is formed in a quadrangular ring shape along the outer periphery of the current collector foil 110 so as to cover the outer periphery of the current collector foil 110. The sealing portion 210 is formed from an insulating material such as polycarbonate (PC), polypropylene (PP), polyethylene (PE), polystyrene (PS), polyphenylene sulfide resin (PPS), polyphenylene ether (PPE (including modified PPE)), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyether ether ketone (PEEK), tetrafluoroethylene-perfluoroalkyl vinyl ether (PFA), polytetrafluoroethylene (PTFE), polyethersulfone (PES), polyamide (PA), ABS resin, or a composite material thereof.

[0037] The seal parts 210 of two adjacent electrode units 100 are connected to each other. The seal parts 210 may be connected to each other by being integrally and continuously formed, or may be connected to each other by being joined to each other by heat sealing (thermal welding), ultrasonic welding, laser welding, adhesive, or the like. As a result, the seal part 210 is disposed around the positive electrode active material layer 120 of one of the two electrode units 100 and the negative electrode active material layer 130 of the other of the two electrode units 100, and the seal part 210 is provided between the current collector foils 110 of the two electrode units 100. In other words, the seal part 210 is provided continuously between the current collector foils 110 of the two electrode units 100, and the current collector foils 110 are sealed from each other.

[0038] An electrolyte layer (not shown) is formed on the inside of the seal portion 210 of each of the electrode units 100. In this embodiment, the electrolyte layer is a non-aqueous liquid electrolyte (electrolytic solution), but may be a solid electrolyte (solid electrolyte) or a gel electrolyte. Any known electrolyte may be used as the electrolyte. The electrolyte (non-aqueous electrolyte) may be a non-aqueous solvent in which an electrolyte salt is dissolved. Examples of the non-aqueous solvent include cyclic carbonates such as ethylene carbonate (EC) and propylene carbonate (PC), and chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC). The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiPF 6 , LiPO 2 F 2 , LiBF 4 , LiClO 4 , LiN(SO 2 F) 2 , LiN(SO 2 CF 3 ) and other inorganic lithium salts.

[0039] [1.2 Description of end units 101 and 102] Next, the configuration of the end units 101 and 102 will be described in detail. The end unit 101 is disposed at the end of the multiple electrode units 100 in the negative direction of the Z axis. The end unit 102 is disposed at the end of the multiple electrode units 100 in the positive direction of the Z axis. The end units 101 and 102 are portions that sandwich the multiple electrode units 100 in the Z axis direction.

[0040] The end unit 101 has at least a positive electrode metal layer 111, a positive electrode active material layer 120 formed on a surface of the positive electrode metal layer 111 in the Z-axis positive direction, and a seal portion 220. The positive electrode metal layer 111 and the positive electrode active material layer 120 of the end unit 101 have the same configuration as the positive electrode metal layer 111 and the positive electrode active material layer 120 of the current collector foil 110 of the electrode unit 100 described above.

[0041] The sealing portion 220 is a portion disposed around the positive electrode active material layer 120. In the present embodiment, the sealing portion 220 is an annular portion disposed around the positive electrode active material layer 120 over the entire circumference of the positive electrode active material layer 120. Specifically, the sealing portion 220 is formed in a quadrangular ring shape along the outer periphery of the positive electrode metal layer 111 and the end member 300 so as to cover the outer periphery of the positive electrode metal layer 111 and the end member 300. The sealing portion 220 is formed of the same material as the sealing portion 210 of the electrode unit 100.

[0042] The seal portion 220 is connected to the seal portion 210 of the electrode unit 100 adjacent to the end unit 101. The connection between the seal portion 220 and the seal portion 210 is similar to the connection between the seal portions 210 described above, and therefore a detailed description will be omitted. This provides a seal between the positive electrode metal layer 111 of the end unit 101 and the current collecting foil 110 of the electrode unit 100. The above-mentioned electrolyte layer (not shown) is formed inside the seal portion 220.

[0043] The end unit 102 has at least a current collecting foil 110, a negative electrode active material layer 130 arranged on a surface of the current collecting foil 110 in the negative Z-axis direction, and a seal portion 230. The current collecting foil 110 and the negative electrode active material layer 130 of the end unit 102 have the same configuration as the current collecting foil 110 and the negative electrode active material layer 130 of the electrode unit 100 described above. That is, also in the end unit 102, the negative electrode active material layer 130 is formed on the current collecting foil 110 via a resin layer 150. Specifically, the end unit 102 further has a resin layer 150 formed on the negative electrode metal layer 112 of the current collecting foil 110, and the negative electrode active material layer 130 is formed on the resin layer 150.

[0044] The sealing portion 230 is a portion disposed around the negative electrode active material layer 130. In the present embodiment, the sealing portion 230 is an annular portion disposed around the negative electrode active material layer 130 over the entire circumference of the negative electrode active material layer 130. Specifically, the sealing portion 230 is formed in a quadrangular ring shape along the outer periphery of the current collector foil 110 and the end member 300 so as to cover the outer periphery of the current collector foil 110 and the end member 300. The sealing portion 230 is formed of the same material as the sealing portion 210 of the electrode unit 100.

[0045] The seal portion 230 is connected to the seal portion 210 of the electrode unit 100 adjacent to the end unit 102. The connection between the seal portion 230 and the seal portion 210 is similar to the connection between the seal portions 210 described above, and therefore a detailed description will be omitted. This provides a seal between the current collecting foil 110 of the end unit 102 and the current collecting foil 110 of the electrode unit 100. The above-mentioned electrolyte layer (not shown) is formed inside the seal portion 230.

[0046] In this manner, the seal portions 210, 220, and 230 are connected to one another to form the seal member 200. The seal member 200 is a cylindrical (rectangular cylindrical) member that is disposed so as to surround the entire periphery of the positive electrode metal layer 111, the negative electrode metal layer 112, the positive electrode active material layer 120, the negative electrode active material layer 130, the separator 140, and the end member 300, and seals these members from the outside.

[0047] [1.3 Description of the separator 140 and the end member 300] The separator 140 is a microporous sheet made of resin. The separator 140 is disposed between the electrode units 100, between the end unit 101 and the electrode unit 100, and between the end unit 102 and the electrode unit 100. Specifically, the separator 140 is disposed between the positive electrode active material layer 120 and the negative electrode active material layer 130. For example, a woven fabric, a nonwoven fabric, a porous resin film, or the like is used as the material of the separator 140. Among these, a porous resin film is preferable. From the viewpoint of strength, a polyolefin such as polyethylene or polypropylene is preferable as the main component of the porous resin film. The separator 140 may be a multilayer film in which a layer containing a filler is formed on the surface of the porous resin film. The separator 140 is formed in a rectangular shape larger than the negative electrode active material layer 130 in a planar view. In this embodiment, the size of the separator 140 is smaller than that of the current collector foil 110 in a planar view, but may be larger than the current collector foil 110 in a planar view. The thickness of the separator 140 (thickness in the stacking direction) is about 15 μm to 20 μm.

[0048] The end member 300 is a member disposed at an end of the power storage device 10 in the stacking direction (Z-axis direction) relative to the plurality of electrode units 100. In this embodiment, a pair of end members 300 are disposed at the end closest to the negative Z-axis direction and the end closest to the positive Z-axis direction of the power storage device 10. The pair of end members 300 are connected to the end units 101 and 102 (the positive electrode metal layers 111 of the end units 101 and 102). As a result, the pair of end members 300 sandwich the plurality of electrode units 100 and the end units 101 and 102, etc., located therebetween, from both sides in the stacking direction (Z-axis direction). The end member 300 is a flat plate-shaped member (end plate). The end member 300 is electrically connected to another end member 300 of another power storage device 10 via another conductive member (bus bar, cooling plate, etc., not shown).

[0049] The end member 300 is formed of a conductive member made of metal such as aluminum, an aluminum alloy, copper, a copper alloy, or nickel, or a combination thereof, or a conductive member other than a metal. Since the end member 300 is connected to the positive electrode metal layer 111, it is preferable that the end member 300 is formed of the same material as the positive electrode metal layer 111, such as aluminum. The thickness of the end member 300 (thickness in the stacking direction) is about 0.5 mm to 3 mm. The electricity storage device 10 may have another conductive member on the outside of the end member 300 (outside in the Z-axis direction).

[0050] In the above configuration, the separator 140, the positive electrode active material layer 120 and the negative electrode active material layer 130 sandwiching the separator 140 in the Z-axis direction, and the positive electrode metal layer 111 and the negative electrode metal layer 112 sandwiching them in the Z-axis direction may be referred to as one energy storage element. In this case, the energy storage device 10 can also be said to be a group of energy storage elements having a configuration in which a plurality of energy storage elements stacked in the Z-axis direction are sandwiched between a pair of end members 300 in the Z-axis direction and are surrounded by a sealing member 200.

[0051] [2 Explanation of resin layer 150] Next, the configuration of the resin layer 150 will be described in more detail. Fig. 4 is a cross-sectional view showing the configuration of the resin layer 150 of the electrode unit 100 according to this embodiment. Specifically, Fig. 4(a) shows the electrode unit 100 of Fig. 3(b), and Fig. 4(b) shows an enlarged view of a part (a part surrounded by a dashed line) of the electrode unit 100 shown in Fig. 4(a).

[0052] As described above, in the electrode unit 100, the resin layer 150 is disposed between the current collector foil 110 and at least one of the positive electrode active material layer 120 and the negative electrode active material layer 130 (in this embodiment, the negative electrode active material layer 130). As shown in FIG. 4, the one active material layer (negative electrode active material layer 130) is larger in size than the other active material layer (positive electrode active material layer 120) when viewed from the stacking direction (Z-axis direction), and the resin layer 150 is larger in size than the one active material layer (negative electrode active material layer 130) when viewed from the stacking direction (Z-axis direction). In this embodiment, the resin layer 150 is a rectangular portion that covers the entire surface of the current collector foil 110 (negative electrode metal layer 112) when viewed from the Z-axis direction.

[0053] The resin layer 150 has a first portion 151 located between the current collector foil 110 and the one active material layer (negative electrode active material layer 130), and a second portion 152 protruding from between the current collector foil 110 and the one active material layer (negative electrode active material layer 130). The first portion 151 is a portion of the resin layer 150 that is disposed between the negative electrode metal layer 112 and the negative electrode active material layer 130. In other words, the first portion 151 is a rectangular portion of the resin layer 150 that is located in a region that overlaps with the negative electrode active material layer 130 when viewed from the Z-axis direction. The second portion 152 is a portion of the resin layer 150 that protrudes (protrudes) from between the negative electrode metal layer 112 and the negative electrode active material layer 130. That is, the second portion 152 is a ring-shaped (quadratic ring-shaped) portion (a portion other than the first portion 151) of the resin layer 150 located in a region that does not overlap with the negative electrode active material layer 130 when viewed from the Z-axis direction.

[0054] The second part 152 has a thickness in the stacking direction (Z-axis direction) greater than that of the first part 151. When manufacturing the electrode unit 100, the resin layer 150 is applied to the negative electrode metal layer 112, and the negative electrode metal layer 112 is pressed by a press roll. As a result, the first part 151 of the resin layer 150 is compressed, and the thickness of the second part 152 becomes greater than that of the first part 151. Furthermore, the density of the second part 152 (density of the negative electrode active material) becomes lower than the density of the first part 151 (density of the negative electrode active material). Thereafter, the resin layer 150 is cured by heat of about 100° C. (it may be cured by a two-liquid mixed resin). In this embodiment, the second part 152 is thicker than the first part 151 around the entire circumference of the negative electrode active material layer 130, but a part of the entire circumference of the second part 152 may be the same thickness as the first part 151 or thinner than the first part 151.

[0055] From the viewpoint of reducing the thickness of the electricity storage device 10, the thickness of the first part 151 in the stacking direction (Z-axis direction) is preferably 20 μm or less, and more preferably 10 μm or less. From the viewpoint of further enhancing the effect of the resin layer 150 described later, the thickness of the first part 151 is preferably 0.5 μm or more, and more preferably 2 μm or more. For these reasons, the thickness of the first part 151 is preferably 0.5 μm or more and 20 μm or less, and more preferably 2 μm or more and 10 μm or less. The thickness of the second part 152 is preferably 1 μm or more and 25 μm or less, and more preferably 3 μm or more and 13 μm or less. The thickness of the resin layer 150 (the first part 151 and the second part 152) is an average thickness obtained by measuring the thickness of the resin layer 150 at five or more points on a cross section of the electrode unit 100 using a scanning electron microscope (SEM) and averaging the measured values. Cross-sectional SEM is a method in which a cut surface of a sample is prepared and the cut surface is observed using a scanning electron microscope. Similar methods can be used to measure the thickness of other members described above or below.

[0056] In this embodiment, the metal layer 112 (negative metal layer 112) on which the resin layer 150 is arranged, out of the two metal layers 111 and 112 included in the current collecting foil 110, has a thickness in the stacking direction (Z-axis direction) smaller than that of the metal layer 111 (positive metal layer 111) on the opposite side to the resin layer 150. Specifically, the metal layer 112 (negative metal layer 112) on which the resin layer 150 is arranged, out of the two metal layers 111 and 112, is a plated layer plated on the metal layer 111 (positive metal layer 111) on the opposite side to the resin layer 150. That is, the positive metal layer 111 is a metal foil, and the negative metal layer 112 is a plated layer. The positive metal layer 111 may be a metal foil of any material used for the above-mentioned positive metal layer 111, but in this embodiment, it is a metal foil containing aluminum. Specifically, the positive metal layer 111 is an aluminum foil. The negative electrode metal layer 112 is a plating layer formed on the positive electrode metal layer 111 (metal foil). The negative electrode metal layer 112 may be a plating layer made of any of the materials used for the negative electrode metal layer 112 described above, but in this embodiment, the negative electrode metal layer 112 is a plating layer containing copper. Specifically, the negative electrode metal layer 112 is copper plating. The negative electrode metal layer 112 is formed on the positive electrode metal layer 111 by adhesive plating or the like.

[0057] The thickness of the negative electrode metal layer 112 in the stacking direction (Z-axis direction) is 5 μm or more, and preferably 10 μm or more. When the thickness of the negative electrode metal layer 112 is not uniform, the minimum thickness of the negative electrode metal layer 112 is 5 μm or more, and preferably 10 μm or more. Furthermore, in this embodiment, the negative electrode metal layer 112 (plating layer) is thinner in the stacking direction than the positive electrode metal layer 111 (metal foil). As described above, the thickness of the positive electrode metal layer 111 is about 5 μm to 20 μm, and the thickness of the negative electrode metal layer 112 is thinner than the thickness of the positive electrode metal layer 111.

[0058] In the present embodiment, for each of the multiple electrode units 100 included in the electricity storage device 10, a resin layer 150 is disposed between the current collector foil 110 (negative electrode metal layer 112) and the negative electrode active material layer 130. As described above, in the end unit 102 as well, a resin layer 150 is disposed between the current collector foil 110 (negative electrode metal layer 112) and the negative electrode active material layer 130, and the configuration thereof is similar to that in the electrode unit 100. This resin layer 150 will be described in detail below.

[0059] The resin layer 150 is a resin layer containing a conductive agent (a mixture of a resin and a conductive agent). In this embodiment, the resin layer 150 has a characteristic that the resistance increases when heated. Specifically, the resin layer 150 is formed of a resin (PTC resin) having a PTC (Positive Temperature Coefficient) characteristic that the electrical resistance increases as the temperature increases. The resin layer 150 may be of a type in which the resin material melts to break the internal conductive path due to the conductive agent, thereby increasing the electrical resistance, or of a type in which the resin material expands when heated, thereby increasing the electrical resistance.

[0060] Specifically, the resin layer 150 contains a conductive agent, a polyolefin, and a binder.

[0061] (Conductive agent) The conductive agent is not particularly limited as long as it has conductivity. Examples of the conductive agent include carbon black such as furnace black, acetylene black, and ketjen black, natural or artificial graphite, metals, conductive ceramics, and the like. Of these, carbon black is preferred as the conductive agent. The conductive agent is usually in the form of particles. The term "conductive" refers to a material having a volume resistivity of 10 or more as measured in accordance with JIS-H-0505 (1975). 7This means that the particle size is Ω·cm or less. The particle size of the conductive agent is preferably, for example, 20 nm or more and 1 μm or less. By using a conductive agent with such a particle size, the softening of the polyolefin makes it easier to break the electronic conduction path between the conductive agents, and the shutdown function can be further improved. The particle size refers to the value (D50) at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50%.

[0062] The lower limit of the content of the conductive agent in the resin layer 150 may be, for example, 1% by mass, but is preferably 2% by mass, and more preferably 5% by mass. When the content of the conductive agent in the resin layer 150 is equal to or greater than the above lower limit, sufficient conductivity can be exhibited during normal use. The upper limit of the content of the conductive agent in the resin layer 150 may be, for example, 20% by mass, but is preferably 15% by mass, and more preferably 10% by mass. When the upper limit of the content of the conductive agent in the resin layer 150 is within the above range, the electron conduction path between the conductive agents is effectively cut off as the polyolefin softens, and a more excellent shutdown function can be exhibited. When the content of the conductive agent in the resin layer 150 is 15% by mass or less, the magnitude of the short-circuit current is suppressed, and safety can be further improved.

[0063] (Polyolefin) Polyolefin is a polymer synthesized using olefin, an unsaturated hydrocarbon compound, as a monomer. Polyolefin is usually insulating. Examples of polyolefin include low-density polyethylene, high-density polyethylene, polypropylene, etc. Among these, polypropylene is preferred from the viewpoint of its relatively high melting point. One or more types of polyolefin can be used in combination. The lower limit of the melting point of the polyolefin may be 100°C, preferably 140°C, and more preferably 160°C. By setting the melting point of the polyolefin within the above range, sufficient conductivity is ensured under normal circumstances, while the electronic conduction path between the conductive agents is sufficiently cut off during excessive heat generation, and the resistance can be effectively increased. During drying in the manufacturing process, the product is not softened and shape retention is maintained, so that it can be manufactured efficiently.

[0064] It is preferable that the polyolefin is particulate in the resin layer 150 under normal conditions. By setting the melting point of the polyolefin within the above range, sufficient conductivity is ensured under normal conditions, while the polyolefin can soften and cover the conductive agent when excessive heat is generated due to a short circuit, so that the resistance can be effectively increased. The particulate form may mean that some of the particles melt and bond together as long as the particle shape is maintained. When the polyolefin is particulate, it is preferable that the particle diameter of the polyolefin is larger than the particle diameter of the conductive agent. By using polyolefin with such a particle diameter, the polyolefin exists in a state where it is higher than the conductive agent in the thickness direction of the resin layer 150. Therefore, the softened polyolefin can cover the conductive agent when excessive heat is generated due to a short circuit, so that the resistance can be effectively increased and the effect of suppressing the increase in short circuit current can be improved. The particle diameter of the polyolefin is preferably 1 μm or more and 10 μm or less. The particle diameter means a value (D50) at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50%.

[0065] The lower limit of the polyolefin content relative to the conductive agent content in the resin layer 150 is 2 times, preferably 4 times, and more preferably 6 times, in mass ratio. By setting the polyolefin content relative to the conductive agent to the above lower limit or more, the conductive agent is covered with a sufficient amount of polyolefin to cause the above-mentioned separation, so that the electrical resistance can be effectively increased and a sufficient shutdown function can be exhibited. The upper limit of the polyolefin content relative to the conductive agent content in the resin layer 150 is 20 times, preferably 16 times, and more preferably 12 times, in mass ratio. By setting the polyolefin content relative to the conductive agent to the above upper limit or less, a sufficient amount of conductive agent can be present in the resin layer 150, and good conductivity can be ensured under normal conditions.

[0066] The lower limit of the polyolefin content in the resin layer 150 is, for example, preferably 30% by mass, more preferably 50% by mass, and even more preferably 60% by mass. When the polyolefin content in the resin layer 150 is equal to or greater than the lower limit, the conductive agent is covered with a sufficient amount of polyolefin to cause the above-mentioned disconnection, so that the electron conduction path in the resin layer 150 is effectively disconnected, and a better shutdown function can be exhibited. The upper limit of the polyolefin content in the resin layer 150 is, for example, preferably 90% by mass, and more preferably 85% by mass. By setting the polyolefin content in the resin layer 150 to the upper limit or less, a good balance between good conductivity during normal use and good shutdown function during excessive heat generation can be exhibited.

[0067] (binder) Examples of the binder (binding agent) include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyimide, etc.; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, etc.; polysaccharide polymers, etc. Among these, fluororesins are preferred, and PVDF is more preferred. Fluorine-containing fluororesins, which have low intermolecular forces and low surface energy, swell with heat generation and have appropriate binding properties as a binder. As a result, by using fluororesins, the electron conduction path in the resin layer 150 is relatively easily cut off when the polyolefin softens during heat generation, and the shutdown function can be more effectively expressed. The lower limit of the binder content in the resin layer 150 is preferably 5% by mass, and more preferably 10% by mass. The upper limit of this content is preferably 30% by mass, and more preferably 20% by mass. By setting the content of the binder in the resin layer 150 within the above range, it is possible to achieve a good balance between sufficient binding properties and the ability to disrupt the electron conduction pathways in the resin layer 150 when excessive heat is generated.

[0068] In this way, the resin layer 150 contains a binder (binding agent), and thus the resin layer 150 has binding properties. Therefore, the current collector foil 110 (negative electrode metal layer 112) and the one active material layer (negative electrode active material layer 130) are joined (bonded) by the resin layer 150. The resin layer 150 may contain a modified polyolefin having strong binding properties, the raw material of which is the above-mentioned polyolefin (polyethylene, polypropylene, etc.). The modified polyolefin is a polyolefin in which a polar group has been introduced to impart adhesive properties to different materials.

[0069] (Other ingredients) From the viewpoint of improving the effect of suppressing an increase in short-circuit current, the resin layer 150 may further contain other components other than the conductive agent, polyolefin, and binder. However, the upper limit of the content of the other components in the resin layer 150 is preferably, for example, 20% by mass. This upper limit may be 10% by mass, 5% by mass, or 1% by mass. By setting the content of the other components to the above upper limit or less, it is possible to better achieve both good conductivity during normal use and a shutdown function in the event of an abnormality.

[0070] Examples of the other components include carbonate compounds, hydrogen carbonate compounds, hydroxides (excluding hydroxides of alkali metals), other inorganic compounds, or combinations of these compounds. When the resin layer 150 further contains such other components, the shutdown function in the event of excessive heat generation can be improved, and safety can be further improved.

[0071] Examples of the carbonate compound include alkaline earth metal carbonates such as magnesium carbonate and calcium carbonate, and aluminum carbonate. Among these, alkaline earth metal carbonates are preferred, and magnesium carbonate is more preferred. By using such a carbonate compound, the shutdown function during excessive heat generation can be improved, and safety can be further improved. Examples of the hydrogen carbonate compound include alkaline metal hydrogen carbonates such as sodium hydrogen carbonate and potassium hydrogen carbonate, and alkaline earth metal hydrogen carbonates such as calcium hydrogen carbonate. Examples of the hydroxide include alkaline earth metal hydroxides such as magnesium hydroxide and calcium hydroxide, and aluminum hydroxide (excluding hydroxides of alkali metals). By using such hydroxides, the current shutdown function works in response to heat generation due to a short circuit, and further heat generation can be suppressed, so safety can be further improved. Examples of other inorganic compounds include inorganic oxides such as alumina, titanium oxide, magnesium oxide, silicon oxide, and aluminum oxide-silicon oxide composite oxide; titanic acid compounds such as barium titanate; and nitrides such as aluminum nitride and silicon nitride. By using the inorganic compound, the shape of the resin layer 150 can be maintained even when the polyolefin resin is softened.

[0072] The resin layer 150 may contain a gas-generating compound instead of polyolefin. That is, instead of disrupting the electronic conduction path between the conductive agents by softening the polyolefin, the electronic conduction path between the conductive agents may be disrupted by gas generation. In this case, the resin layer 150 contains the above-mentioned conductive agent, gas-generating compound, and binder.

[0073] One embodiment of the gas-generating compound is a compound (a) that decomposes at 100° C. or higher to generate gas. Specific examples of such compounds (a) include carbonate compounds, hydrogen carbonate compounds, hydroxide oxides, hydrates, hydroxides, and other organic compounds, and carbonate compounds, hydrogen carbonate compounds, hydroxide oxides, hydrates, and hydroxides are preferred, carbonate compounds, hydrogen carbonate compounds, and hydroxides are more preferred, carbonate compounds and hydroxides are even more preferred, and hydroxides are even more preferred. Other embodiments of the gas-generating compound include carbonate compounds, hydrogen carbonate compounds, hydroxide oxides, hydrates, and hydroxides (excluding hydroxides of alkali metals). These compounds (b) usually decompose when heated to generate gas. Compound (b) decomposes at, for example, 100° C. or higher. Among the compounds (b), carbonate compounds, hydrogen carbonate compounds, and hydroxides are preferred, carbonate compounds and hydroxides are more preferred, and hydroxides are even more preferred. The gas-generating compounds can be used alone or in combination of two or more.

[0074] Examples of the carbonate compound include alkaline earth metal carbonates such as magnesium carbonate and calcium carbonate, and aluminum carbonate. Among these, alkaline earth metal carbonates are preferred, and magnesium carbonate is more preferred. Magnesium carbonate and the like may be anhydrous or hydrated. Examples of the hydrogen carbonate compound include alkaline metal hydrogen carbonates such as sodium hydrogen carbonate and potassium hydrogen carbonate, and alkaline earth metal hydrogen carbonates such as calcium hydrogen carbonate. Among these, alkaline metal hydrogen carbonates are preferred, and sodium hydrogen carbonate is more preferred. Examples of the hydroxide oxide include aluminum hydroxide oxide (boehmite, etc.) and magnesium hydroxide oxide. Examples of the hydrate include calcium sulfate dihydrate, copper sulfate pentahydrate, magnesium carbonate n-hydrate, etc. Examples of the hydroxide include alkaline earth metal hydroxides such as magnesium hydroxide and calcium hydroxide, and hydroxides of Group 13 elements such as aluminum hydroxide.

[0075] The lower limit of the temperature at which the gas-generating compound decomposes is preferably 130°C, more preferably 160°C, and even more preferably 200°C. This can reduce the risk of the gas-generating compound decomposing in the drying process. The upper limit of the temperature at which the gas-generating substance decomposes is not particularly limited as long as it is equal to or lower than the maximum temperature reached inside the power storage device 10 during an abnormality such as a short circuit, but is preferably equal to or lower than 800°C, more preferably equal to or lower than 600°C, and even more preferably equal to or lower than 450°C. The temperature at which the gas-generating compound decomposes is preferably lower than the temperature at which the power storage device 10 thermally escapes. The gas-generating compound decomposes to generate gas before the power storage device 10 thermally escapes, and thus the disconnection of the electron conduction path in the resin layer 150 progresses, and a sufficient shutdown function can be expressed. The shape of the gas-generating compound is usually particulate in the resin layer 150 under normal conditions. The gas-generating compound is usually insulating.

[0076] When the gas-generating compound is heated from room temperature (20° C.) to 300° C. or 500° C., the lower limit of the mass reduction rate is preferably 3% by mass, more preferably 5% by mass, and sometimes even more preferably 10% by mass, 20% by mass, or 30% by mass. The upper limit of this mass reduction rate is preferably 70% by mass, and sometimes even more preferably 50% by mass, 30% by mass, or 20% by mass. By keeping the mass reduction rate, i.e., the amount of gas generated, within the above range, safety during heat generation can be further improved.

[0077] The gas generated by the gas-generating compound is preferably flame-retardant and non-flammable. By generating a flame-retardant and non-flammable gas, the possibility of ignition due to heat generation can be reduced, and safety is further improved. Examples of flame-retardant and non-flammable gases include carbon dioxide, water (water vapor), and nitrogen, and among these, carbon dioxide is preferred. The gas-generating compound is preferably one that generates a solid insulating inorganic substance such as an oxide upon decomposition. In such a case, the solid insulating inorganic substance itself can also contribute to ensuring insulation.

[0078] The D50 particle size of the gas-generating compound is preferably, for example, 0.1 μm or more and 10 μm or less. The BET specific surface area of ​​the gas-generating compound is, for example, 2 / g or more 10m 2 / g or less is preferable. By using a gas generating compound having such particle size and specific surface area, gas is generated more effectively during heat generation, and the resistance can be effectively increased. The "BET specific surface area" is a value measured by the following method. First, the pore size distribution is measured using a nitrogen adsorption method. This measurement can be performed using an "autosorb iQ" manufactured by Quantachrome. Five points are extracted from the region of P / P0 = 0.06 to 0.3 of the obtained adsorption isotherm, and a BET plot is performed, and the BET specific surface area is calculated from the y-intercept and slope of the straight line.

[0079] The shape of the gas-generating compound is not particularly limited, but is preferably rod-shaped. When the gas-generating compound is rod-shaped, the anchor effect is enhanced, and the melting and outflow of the binder that exhibits the PTC function can be sufficiently suppressed. When the gas-generating compound is rod-shaped, decomposition due to heating is likely to occur. "Rod-shaped" refers to particles with a ratio of the major axis to the minor axis of 2 or more, and it is preferable that the ratio is 5 or more. The upper limit of this ratio may be, for example, 100. The above-mentioned minor axis and major axis are the average values ​​of the top five particles with the largest major axis in one visual field observed by an electron microscope. The lower limit of the minor axis of the rod-shaped gas-generating compound is preferably 0.01 μm, and more preferably 0.1 μm. The upper limit of this minor axis is preferably 10 μm, and more preferably 4 μm.

[0080] The lower limit of the content of the gas-generating compound relative to the content of the conductive agent in the resin layer 150 is 2 times, preferably 4 times, and more preferably 6 times, in mass ratio. By making the content of the gas-generating compound relative to the conductive agent equal to or greater than the above lower limit, gas is generated to a degree sufficient to cause the disconnection of the electron conduction path in the resin layer 150, and a sufficient shutdown function is exhibited. The upper limit of the content of the gas-generating compound relative to the content of the conductive agent in the resin layer 150 is 20 times, preferably 16 times, and more preferably 12 times, in mass ratio. By making the content of the gas-generating compound relative to the conductive agent equal to or less than the above upper limit, a sufficient amount of conductive agent can be present in the resin layer 150, and good conductivity can be ensured under normal conditions.

[0081] The lower limit of the content of the gas-generating compound in the resin layer 150 may be, for example, 10% by mass, preferably 30% by mass, more preferably 50% by mass, and even more preferably 60% by mass. When the content of the gas-generating compound in the resin layer 150 is equal to or more than the above lower limit, the electron conduction path in the resin layer 150 is effectively cut off with the generation of gas, and a more excellent shutdown function can be exhibited. When the content of the gas-generating compound in the resin layer 150 is equal to or more than the above lower limit, the anchor effect is enhanced, and the melting and outflow of the binder exhibiting the PTC function can be sufficiently suppressed. The upper limit of the content of the gas-generating compound in the resin layer 150 may be, for example, 95% by mass, preferably 90% by mass, and more preferably 85% by mass. When the content of the gas-generating compound in the resin layer 150 is equal to or less than the above upper limit, a good balance between good conductivity during normal use and good shutdown function during heat generation can be exhibited.

[0082] In this way, the resin layer 150 has the property of expanding when heated. The resin layer 150 expands 1.1 to 3 times its size when heated.

[0083] [3 Explanation of effects] As described above, according to the electricity storage device 10 of the embodiment of the present invention, the resin layer 150 containing a conductive agent is disposed between the current collector foil 110 and at least one of the positive electrode active material layer 120 and the negative electrode active material layer 130. This makes it possible for the resin layer 150 to increase the resistance between the current collector foil 110 and the active material layer. Therefore, even if an internal short circuit occurs in the electricity storage device 10, the resin layer 150 can suppress the flow of a large current.

[0084] If the current collector foil 110 has a pinhole, the electrolyte may penetrate through the pinhole, causing a short circuit due to the electrolyte. Specifically, when the aluminum foil as the positive electrode metal layer 111 is rolled using a pressure roll, pinholes may occur due to the compression of oil or foreign matter from the lubricant during rolling. The plating layer as the negative electrode metal layer 112 has a small thickness, so pinholes may occur. If a pinhole occurs in the positive electrode metal layer 111 or the negative electrode metal layer 112, the electrolyte may penetrate through the pinhole, causing a short circuit due to the electrolyte (a short circuit between the metal layer and the active material of the opposite electrode). In the pinhole in the positive electrode metal layer 111, the positive electrode active material layer 120 and the negative electrode metal layer 112 (Cu plating, etc.) are short-circuited via the electrolyte, and furthermore, a pinhole is formed in Cu due to the elution of Cu, and finally a short circuit occurs between the positive electrode active material layer 120 and the negative electrode active material layer 130. At the pinholes in the negative electrode metal layer 112, the negative electrode active material layer 130 and the positive electrode metal layer 111 (such as an Al foil) are short-circuited via the electrolyte, and furthermore, Li of the negative electrode permeates into the Al to form a Li / Al alloy, and the alloy portion expands to form cracks, eventually causing a short circuit between the positive electrode active material layer 120 and the negative electrode active material layer 130. For this reason, by disposing a resin layer 150 between the current collector foil 110 and the active material layer, even if the electrolyte permeates through the pinholes, the resin layer 150 can stop the electrolyte from permeating, and a short circuit caused by the electrolyte can be suppressed. The resin layer 150 can protect the current collector foil 110, and therefore it is also possible to suppress the occurrence of pinholes in the current collector foil 110.

[0085] When the current collecting foil 110 has two metal layers 111 and 112, pinholes are likely to occur in the thinner metal layer 112 (negative metal layer 112). For this reason, the resin layer 150 is disposed on the thinner metal layer 112 (negative metal layer 112). This allows the metal layer 112 (negative metal layer 112) to be protected by the resin layer 150, so that pinholes can be prevented from occurring in the metal layer 112 (negative metal layer 112). Even if pinholes occur in the metal layer 112 (negative metal layer 112) (or if there are parts of the plating layer that are not completely plated), the resin layer 150 can prevent the intrusion of the electrolyte that permeates through the pinholes, etc., and therefore, an internal short circuit via the electrolyte can be prevented.

[0086] When forming a current collecting foil 110 having two metal layers 111 and 112, the current collecting foil 110 can be easily formed by plating the metal layer 111 (positive electrode metal layer 111) with a plating layer (negative electrode metal layer 112). In this case, since pinholes are likely to occur in the plating layer (negative electrode metal layer 112), a resin layer 150 is disposed on the plating layer (negative electrode metal layer 112). This allows the plating layer (negative electrode metal layer 112) to be protected by the resin layer 150, making it possible to suppress the occurrence of pinholes in the plating layer (negative electrode metal layer 112).

[0087] The second portion 152 of the resin layer 150 protrudes from between the current collecting foil 110 and the negative electrode active material layer 130, so that the effect of the resin layer 150 can be achieved even in the portion of the current collecting foil 110 protruding from the negative electrode active material layer 130. In particular, the second portion 152 of the resin layer 150 is thicker than the first portion 151, so that the effect of the resin layer 150 can be further achieved in the second portion 152. That is, the first portion 151 located between the current collecting foil 110 and the negative electrode active material layer 130 is made thin by pressing or the like to have a relatively low resistance, and the second portion 152 protruding from between the current collecting foil 110 and the negative electrode active material layer 130 is made thicker to have a relatively high resistance, so that heat generation due to a foreign object short circuit, a nail short circuit, or the like can be suppressed. That is, even if a foreign object short circuit, a nail short circuit, or the like occurs at the position of the first portion 151, the resistance is relatively large due to the resistance of both the negative electrode active material layer 130 and the resin layer 150, so the current that flows is small. However, if a foreign object short circuit, a nail short circuit, or the like occurs at the position of the second portion 152, the resistance is relatively small because the negative electrode active material layer 130 is not disposed, so a large current is likely to flow. Therefore, by increasing the thickness of the resin layer 150 that serves as a resistance layer at the position of the second portion 152, the resistance between the nail, the resin layer 150, and the current collecting foil 110 can be increased and the short circuit current can be restricted, so that heat generation can be suppressed and safety can be improved.

[0088] By bonding the current collector foil 110 and the negative electrode active material layer 130 with the resin layer 150, the negative electrode active material layer 130 can be prevented from falling off the current collector foil 110.

[0089] Since the resistance of the resin layer 150 increases when heated, when an internal short circuit or the like occurs in the energy storage device 10 and a large current flows, the resin layer 150 is heated and the resistance of the resin layer 150 increases. This makes it possible to reduce the current flowing through the energy storage device 10.

[0090] Even if one active material layer (negative electrode active material layer 130) is larger in size than the other active material layer (positive electrode active material layer 120), the resin layer 150 is made larger in size than the one active material layer (negative electrode active material layer 130). This allows the resin layer 150 to cover the entire one active material layer (negative electrode active material layer 130), thereby enhancing the effect of the resin layer 150.

[0091] [4 Explanation of Modifications] Although the power storage device 10 according to the present embodiment has been described above, the present invention is not limited to the above embodiment. The embodiment disclosed herein is illustrative and not restrictive in all respects, and the scope of the present invention includes all modifications within the meaning and scope of the claims.

[0092] In the above embodiment, the current collecting foil 110 is formed of multiple layers (two layers) of the positive electrode metal layer 111 and the negative electrode metal layer 112, but the current collecting foil 110 may be formed of one layer (one metal foil). In other words, the current collecting foil 110 may be formed of a single sheet of stainless steel foil or the like, and the single sheet of stainless steel foil or the like may have the functions of both the positive electrode metal layer and the negative electrode metal layer.

[0093] In the above embodiment, the resin layer 150 is larger in size than the negative electrode active material layer 130 when viewed from the Z-axis direction, but may be the same size as the negative electrode active material layer 130 or smaller in size than the negative electrode active material layer 130. The resin layer 150 is a rectangular portion when viewed from the Z-axis direction, but the shape of the resin layer 150 is not particularly limited.

[0094] In the above embodiment, in resin layer 150, second portion 152 is thicker than first portion 151, but second portion 152 may be the same thickness as first portion 151 or thinner than first portion 151. That is, in the above embodiment, resin layer 150 is not limited to the above-mentioned thickness. Other members are also not limited to the above-mentioned thickness.

[0095] In the above embodiment, the resin layer 150 has a characteristic that the resistance increases when heated, but the resin layer 150 does not have to have this characteristic. Even in this case, the resin layer 150 has an insulating member (resin) and has a higher resistance than when the resin layer 150 does not have an insulating member (resin), so that even if an internal short circuit occurs in the energy storage device 10, the resin layer 150 can suppress a large current from flowing.

[0096] In the above embodiment, the resin layer 150 is disposed between the current collecting foil 110 (negative electrode metal layer 112) and the negative electrode active material layer 130, but it may be disposed between the current collecting foil 110 (positive electrode metal layer 111) and the positive electrode active material layer 120. In this case, the end unit 101 may have the resin layer 150 between the positive electrode metal layer 111 and the positive electrode active material layer 120. Even in these cases, the resin layer 150 has a configuration similar to that of the above embodiment, and can achieve similar effects.

[0097] In the above embodiment, all the electrode units 100 have the resin layer 150, but any of the electrode units 100 may not have the resin layer 150. That is, in at least one electrode unit 100, a resin layer 150 containing a conductive agent may be disposed between the current collecting foil 110 and at least one of the positive electrode active material layer 120 and the negative electrode active material layer 130. Similarly, although the end unit 102 has the resin layer 150, it may not have the resin layer 150.

[0098] The electricity storage device 10 may be used in an electricity storage pack 1 as shown in FIG. 5. FIG. 5 is a cross-sectional view showing the configuration of the electricity storage pack 1. In FIG. 5, the internal configuration of the electricity storage device 10 is omitted. As shown in FIG. 5, the electricity storage pack 1 includes an electricity storage device stack 2 in which a plurality of electricity storage devices 10 are stacked, and a conductive member 3. In this case, the technology of the present invention may be applied to at least one electricity storage device 10 included in the electricity storage pack 1. Two adjacent electricity storage devices 10 in the electricity storage device stack 2 are electrically connected by contact or joining (welding, etc.). The conductive member 3 is made of a metal such as stainless steel, and the electricity storage device 10 located at the end in the stacking direction (Z-axis direction) and the conductive member 3 are electrically connected by contact or joining (welding, etc.). An adhesive may be used for the joining. The plurality of electricity storage devices 10 in the electricity storage device stack 2 are connected in series, and charging and discharging are performed via the conductive member 3. The electricity storage pack 1 may be restrained in the stacking direction (Z-axis direction) by using a restraining member such as a screw, a resin band, or a metal band. The electricity storage device stack 2 and the conductive member 3 may be housed in a metal case or a resin case.

[0099] As another example of the electricity storage pack 1, a configuration in which individual electricity storage devices 10 are housed in an exterior body 4 is shown in FIG. 6. FIG. 6 is a cross-sectional view showing the configuration of an electricity storage pack 1a. As shown in FIG. 6, the electricity storage device 10 of this configuration has a connection portion 5 exposed from the exterior body 4. A laminate film or the like can be used as the exterior body 4. The connection portions 5 of adjacent electricity storage devices 10 are electrically connected to each other by contact or bonding (welding, etc.). The connection portion 5 of the electricity storage device 10 located at the end in the stacking direction (Z-axis direction) and the conductive member 3 are electrically connected to each other by contact or bonding (welding, etc.). The other configuration is similar to that of the above-mentioned electricity storage pack 1, so a description thereof will be omitted.

[0100] Any combination of the components included in the above-described embodiment and its modified examples is also included within the scope of the present invention. [Industrial Applicability]

[0101] The present invention can be applied to electricity storage devices such as bipolar batteries. [Explanation of symbols]

[0102] 1, 1a storage pack 2. Electricity storage device laminate 3 Conductive materials 4 Exterior body 5 Connection part 10. Energy storage device 100 electrode units 101, 102 End unit 110 Current collecting foil 111 Positive electrode metal layer (metal layer) 112 Negative electrode metal layer (metal layer) 120 Cathode active material layer 130 Negative electrode active material layer 140 Separator 150 Resin layer 151 Part 1 152 Part 2 200 Sealing material 210, 220, 230 Seal part 300 End member

Claims

1. A plurality of electrode units are stacked in a stacking direction, each of the plurality of electrode units includes at least a current collecting foil, a positive electrode active material layer formed on one surface of the current collecting foil, and a negative electrode active material layer formed on the other surface of the current collecting foil; In at least one electrode unit, a resin layer containing a conductive agent is disposed between the current collector foil and at least one of the positive electrode active material layer and the negative electrode active material layer. Energy storage device.

2. The current collecting foil has two metal layers aligned in the stacking direction, The metal layer on which the resin layer is disposed of, out of the two metal layers, has a smaller thickness in the stacking direction than the metal layer on the opposite side to the resin layer. The power storage device according to claim 1 .

3. The current collecting foil has two metal layers aligned in the stacking direction, The metal layer on which the resin layer is disposed of among the two metal layers is a plated layer formed by plating the metal layer on the side opposite to the resin layer. The power storage device according to claim 1 or 2.

4. The resin layer is a first portion located between the current collecting foil and the one active material layer; a second portion protruding from between the current collecting foil and the one active material layer, The second portion has a thickness in the stacking direction greater than that of the first portion. The power storage device according to claim 1 or 2.

5. The current collecting foil and the one active material layer are bonded to each other by the resin layer. The power storage device according to claim 1 or 2.

6. The resin layer has a characteristic that its resistance increases when heated. The power storage device according to claim 1 or 2.

7. the one active material layer is larger in size than the other active material layer when viewed in the stacking direction, The resin layer is larger in size than the one of the active material layers when viewed in the stacking direction. The power storage device according to claim 1 or 2.

Citation Information

Patent Citations

  • Power storage device

    JP2022077634A

Cited By

  • Electrode plate, power storage device, and electrode plate production method

    WO2026203712A1