Method of manufacturing water-dispersible Anti-static coating composition, water-dispersible Anti-static coating composition and Anti-static coating film

A water-dispersible antistatic coating composition, formed by reacting isocyanate compounds with hydroxyl group-containing (meth)acrylates and emulsifying with water, combined with a crosslinked conductive polymer, addresses the issues of antistatic coatings by ensuring durability and transparency.

JP2024154323AActive Publication Date: 2024-10-30KYOEISHA CHEM CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023068122
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-10-30
Estimated Expiration
2043-04-18

AI Technical Summary

Technical Problem

Existing antistatic coatings for plastic materials face issues with antistatic properties under high humidity, reduced scratch resistance, and loss of properties when exposed to water, while coatings with conductive fillers or water-soluble polymers suffer from poor transparency and durability.

Method used

A water-dispersible antistatic coating composition is produced by reacting an isocyanate compound with a hydroxyl group-containing (meth)acrylate compound to form a urethane (meth)acrylate oligomer, which is then emulsified with water and combined with a crosslinked conductive coating containing a π-conjugated conductive polymer, binder, and crosslinking agent to create a film with antistatic, water-resistant, and transparent properties.

Benefits of technology

The resulting coating achieves excellent plastic adhesion, transparency, and scratch resistance, providing effective antistatic properties even under humid conditions and after water exposure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154323000001
    Figure 2024154323000001
  • Figure 2024154323000002
    Figure 2024154323000002
  • Figure 2024154323000003
    Figure 2024154323000003
Patent Text Reader

Abstract

To provide a method of manufacturing a specific composition capable of achieving both anti-static and water-resistant anti-static properties.SOLUTION: There is provided a method of manufacturing a water-dispersible anti-static coating composition comprising: reacting a hydroxy group-containing (meth)acrylate compound at an n molar ratio to one molar ratio of a compound having (m+n) isocyanate groups, subsequently reacting a polyalkylene glycol containing a hydroxy group at one terminal and the like at an m molar ratio thereto to obtain an oligomer of the formula (1): (R1O-CONH)m-R2-(NHCO-OR3)n, wherein R1O- is a dehydrogenated residue of polyalkylene glycol compound containing a hydroxy group at one terminal and the like, R2 is a deisocyanated isocyanate group residue, R3O- is a dehydrogenated residue of the hydroxy group-containing (meth)acrylate compound, m and n represent integers of 1 to 50, and m≤n; stirring and emulsifying an interface of the oligomer and water gently to prepare an oligomer composition (A) while adding water to the oligomer; and a π-conjugated conductive polymer-containing crosslinkable conductive coating composition (B) to the composition (A).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a water-dispersible antistatic coating composition, a water-dispersible antistatic coating composition, and an antistatic coating film. [Background technology]

[0002] Plastic substrates are widely used as raw materials for home appliance parts, automobile parts, optical members, organic sheet glass, etc., but plastic substrates are easily scratched and easily charged. For this reason, it has been proposed to cover the plastic substrate with a coating layer containing an antistatic agent or metal fine particles of a conductive filler (Patent Documents 1 to 3 and Non-Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 10-244618 [Patent Document 2] JP 2000-281736 A [Patent Document 3] JP 2022-134106 A [Non-patent literature]

[0004] [Non-Patent Document 1] Journal of Materials Life, 16[4]p120-123 (October 2004) Special feature: Progress in conductive polymers Poly(3,4-ethylenedioxythiophene) Summary of the Invention [Problem to be solved by the invention]

[0005] However, when the coating layer contains a large amount of cationic, anionic, or nonionic surfactants, alkali metal salts, alkaline earth metal salts, ammonium salts, etc. as antistatic agents, bleeding of these substances is caused, and the antistatic properties under high humidity conditions and scratch resistance are deteriorated, and further, when the coating layer comes into contact with water, the antistatic properties are lost due to the solubilization of the antistatic agent. In addition, when the coating layer contains a conductive filler or is a coating layer obtained by thermally curing a water-soluble or water-dispersible conductive polymer, the antistatic properties are excellent, but the transparency and / or scratch resistance may be impaired. The present invention aims to provide a method for producing a water-dispersible antistatic coating composition that can form a cured coating film that has both antistatic properties and water-resistant antistatic properties and is excellent in adhesion to plastics, transparency and abrasion resistance, a water-dispersible antistatic coating composition, and an antistatic coating film. [Means for solving the problem]

[0006] This application includes the following inventions: [1] A water-soluble urethane (meth)acrylate oligomer composition (A) is prepared by reacting 1 mole ratio of an isocyanate compound having (m+n) isocyanate groups with n mole ratios of a hydroxyl group-containing (meth)acrylate compound, and then reacting the resulting reaction product with m mole ratios of an alkylene oxide (meth)acrylate adduct or a polyalkylene glycol compound having a hydroxyl group at one end to obtain a urethane (meth)acrylate oligomer represented by formula (1). Water is added to the urethane (meth)acrylate oligomer while gently stirring the interface between the urethane (meth)acrylate oligomer and water to emulsify the urethane (meth)acrylate oligomer, A method for producing a water-dispersible antistatic coating composition, comprising adding a crosslinked conductive coating composition (B) containing a π-conjugated conductive polymer to the water-soluble urethane (meth)acrylate oligomer composition (A). (R 1 O-CONH) m -R 2 -(NHCO-OR 3 ) n (1) (In the formula, R 1 O- is a dehydrogenation residue of a polyalkylene glycol compound having a hydroxyl group at one end or a (meth)acrylic acid alkylene oxide adduct; R 2 represents a residue of a deisocyanated group of an isocyanate compound, R 3 O- is a dehydrogenation residue of a hydroxyl group-containing (meth)acrylate compound, m and n represent an integer between 1 and 50, provided that m≦n. [2] The method according to [1], wherein the stirring is carried out using a paddle blade at a rotation speed of 10 rpm to 100 rpm. [3] The method for producing the mixture according to [1], further comprising adding water until the solid content becomes 50% by weight or less, and continuing gentle stirring for a predetermined period of time after the addition of water is completed. [4] The method according to [3], wherein after the addition of the water is completed, stirring is continued for 10 minutes or more at a rotation speed of 10 rpm to 100 rpm. [5] The process according to any one of [1] to [4], wherein the isocyanate compound (A) is a diisocyanate or a polyisocyanate of a diisocyanate monomer. [6] The method according to any one of [1] to [5], wherein the polyalkylene glycol compound (A) containing a hydroxyl group at one terminal is an alkoxy polyalkylene glycol. [7] The method according to any one of [1] to [6], wherein the (meth)acrylic acid alkylene oxide adduct compound (A) is a compound obtained by adding (meth)acrylic acid to an alkylene oxide, or a compound obtained by mono(meth)acrylate of a polyalkylene glycol. [8] The method according to any one of [1] to [8], wherein the hydroxyl group-containing (meth)acrylate compound (A) is a hydroxyalkyl (meth)acrylate, a polyol (meth)acrylate or an alkylene oxide-added polyol (meth)acrylate. [9] A water-dispersible antistatic coating composition obtained by the manufacturing method according to any one of [1] to [8], wherein the crosslinked conductive paint composition (B) comprises a π-conjugated conductive polymer (b-1), a binder (b-2) and a crosslinking agent (b-3).

[10] The water-dispersible antistatic coating composition according to [9], further comprising a polymerization initiator (C).

[11] An antistatic coating film which is a heat-cured product of the water-dispersible antistatic coating composition according to [9] or

[10] .

[12] An antistatic coating film which is a cured product of the water-dispersible antistatic coating composition according to [9] or

[10] above, which is irradiated with active energy rays. Effect of the Invention

[0007] According to the present invention, it is possible to provide a method for producing a water-dispersible antistatic coating composition capable of forming a cured coating film which has both antistatic properties and water-resistant antistatic properties and is excellent in adhesion to plastics, transparency and abrasion resistance, a water-dispersible antistatic coating composition and an antistatic coating film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] In this specification, "(meth)acrylate" and "(meth)acrylic acid" respectively mean "at least one selected from the group consisting of acrylate and methacrylate" and "at least one selected from the group consisting of acrylic acid and methacrylic acid". Unless otherwise specified, % means % by mass.

[0009] Method for producing water-dispersible antistatic coating composition The method for producing the water-dispersible antistatic coating composition of the present invention is a method in which a crosslinked conductive coating composition (B) containing a π-conjugated conductive polymer is added to a specific water-soluble urethane (meth)acrylate oligomer composition (A).

[0010] (Preparation of Water-Soluble Urethane (Meth)acrylate Oligomer Composition (A)) It is preferable that the (A) water-soluble urethane (meth)acrylate oligomer composition in the present application is prepared, for example, by the manufacturing method disclosed in JP 2021-050310 A. Specifically, first, a urethane (meth)acrylate oligomer represented by formula (1) is synthesized. The urethane (meth)acrylate oligomer represented by formula (1) is reacting 1 mole ratio of an isocyanate compound having (m+n) isocyanate groups with n mole ratios of a hydroxyl group-containing (meth)acrylate compound; Next, a (meth)acrylic acid alkylene oxide adduct or a polyalkylene glycol compound having a hydroxyl group at one end is reacted in an m molar ratio to obtain the polyalkylene glycol. (R 1 O-CONH) m -R 2 -(NHCO-OR 3 ) n (1) (In the formula, R 1 O- is a dehydrogenation residue of a polyalkylene glycol compound having a hydroxyl group at one end or a (meth)acrylic acid alkylene oxide adduct; R 2 represents a residue of a deisocyanated group of an isocyanate compound, R 3 O- is a dehydrogenation residue of a hydroxyl group-containing (meth)acrylate compound, m and n represent an integer between 1 and 50, provided that m≦n. Then, while adding water to the obtained urethane (meth)acrylate oligomer, the interface between the urethane (meth)acrylate oligomer and the water is gently stirred, whereby a water-soluble urethane (meth)acrylate oligomer composition can be produced.

[0011] The emulsion obtained by the above-mentioned method for producing a water-soluble urethane (meth)acrylate oligomer composition has an extremely small average particle size and is stable over a long period of time (no secondary aggregation occurs), and a coating film obtained from a composition containing this can be a coating composition that has excellent hard coat properties and durability such as water resistance and solvent resistance.

[0012] Examples of the isocyanate compound having (m+n) isocyanate groups include diisocyanates and polyisocyanates of diisocyanate monomers. Examples of diisocyanates include 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, diphenylmethane diisocyanate, (o-, m-, or p-)xylene diisocyanate, methylene bis(cyclohexyl isocyanate), trimethylhexamethylene diisocyanate, cyclohexane-1,3-dimethylene diisocyanate, cyclohexane-1,4-dimethylene isocyanate, 1,5-naphthalene diisocyanate, norbornane diisocyanate, etc. Examples of polyisocyanates of diisocyanate monomers include nurates of hexamethylene diisocyanate, nurates of isophorone diisocyanate, nurates of tolylene diisocyanate, and biuretized products of these diisocyanates. Among these, nurates of hexamethylene diisocyanate, nurates of isophorone diisocyanate, and nurates of tolylene diisocyanate, each of which has three or more isocyanate groups in one molecule, are more preferred. The isocyanate compound may have a urethane structure in which an alcohol compound is added to one or more isocyanate groups contained therein, or a urea structure in which an amine compound is added. When an alcohol compound and an amine compound are added to an isocyanate group, the number of functional groups per molecule of the isocyanate compound can be increased. Examples of alcohol compounds that can be added to an isocyanate group include ethylene glycol, propylene glycol, tetramethylene glycol, glycerin, trimethylolpropane, and pentaerythritol. Examples of amine compounds include diaminoethane, diaminopropane, and tetramethylenediamine. It is preferable to use these alcohol compounds and amine compounds with a small molecular weight per functional group from the viewpoint of increasing the scratch resistance of the cured polymer.

[0013] Examples of the hydroxyl group-containing (meth)acrylate compound include hydroxyalkyl (meth)acrylates, polyol (meth)acrylates, and alkylene oxide-added polyol (meth)acrylates. Examples of the hydroxyalkyl (meth)acrylates include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and hydroxyphenoxypropyl (meth)acrylate. Examples of the polyol (meth)acrylates include glycerin di(meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol penta(meth)acrylate. Examples of the alkylene oxide-added polyol (meth)acrylates include alkylene oxide-added trimethylolpropane di(meth)acrylate, alkylene oxide-added pentaerythritol tri(meth)acrylate, and alkylene oxide-added dipentaerythritol penta(meth)acrylate.

[0014] When reacting an isocyanate compound with a hydroxyl group-containing (meth)acrylate compound, in order to promote the reaction, it is preferable to stir the mixture in the presence of a metal catalyst such as dibutyltin dilaurate or an amine catalyst such as 1,8-diazabicyclo[5.4.0]undecene-7 at a temperature range of 50°C to 80°C, more preferably at a temperature range of 60°C to 70°C.

[0015] Subsequently, the reaction product obtained above is reacted with an alkylene oxide (meth)acrylate adduct or a polyalkylene glycol compound containing a hydroxyl group at one end. The (meth)acrylic acid alkylene oxide adduct is preferably an alkylene oxide adduct of (meth)acrylic acid or a mono(meth)acrylate of polyalkylene glycol. The alkylene oxide adduct of (meth)acrylic acid is obtained by adding an alkylene oxide, such as ethylene oxide, propylene oxide, butylene oxide, to (meth)acrylic acid. It can also be synthesized from a polyalkylene glycol, such as polyethylene glycol, polypropylene glycol, polytetramethylene glycol, etc. The molecular weight of the (meth)acrylic acid alkylene oxide adduct can be selected arbitrarily, but is preferably 900 or more, more preferably 900 to 2000. From another viewpoint, the number of moles of the alkylene oxide added is preferably 20 or more, more preferably 20 to 35. The polyalkylene glycol compound containing a hydroxyl group at one end is preferably an alkoxypolyethylene glycol. Examples of the alkoxypolyethylene glycol include methoxypolyethylene glycol, ethoxypolyethylene glycol, butoxypolyethylene glycol, polyethylene glycol monoallyl ether, polyethylene glycol monododecyl ether, polyethylene glycol monolaurate, and polyethylene glycol monooctyl ether. The molecular weight of the alkoxypolyethylene glycol can be selected arbitrarily, but is preferably 900 or more, and more preferably 900 to 2000. By using such a compound, the water-soluble urethane (meth)acrylate oligomer composition obtained can be a nonionic emulsion, and even when various additives are added to the coating composition, etc., the inhibition of the properties of the emulsion, such as aggregation, precipitation, and separation, can be prevented.

[0016] When the reaction product obtained above is reacted with an alkylene oxide (meth)acrylate adduct or a polyalkylene glycol compound having a hydroxyl group at one end, the reaction is preferably carried out in the presence of a metal catalyst such as dibutyltin dilaurate at a temperature range of 50°C to 80°C, more preferably at a temperature range of 60°C to 70°C. The resin concentration of the obtained urethane (meth)acrylate oligomer can be 100%. The weight average molecular weight of the urethane (meth)acrylate oligomer can be, for example, 5000 to 100000, preferably 7000 to 20000. By using such a weight average molecular weight, a composition with an appropriate viscosity can be obtained, self-emulsification is easily caused, and the water-soluble composition can be easily adjusted using this, and when a coating film containing such a water-soluble composition is formed, a coating film with high hardness can be obtained. The weight-average molecular weight means the weight-average molecular weight calculated based on the molecular weight of standard polystyrene. The weight-average molecular weight was measured by a high-performance liquid chromatography (Shodex GPC system-11 type, manufactured by Showa Denko K.K.) using a column: Shodex GPC KF-806L (exclusion limit molecular weight: 2×10 7, Separation range: 100~2×10 7 The measurement can be performed by using three columns in series (theoretical plate number: 10,000 plates / column, filler material: styrene-divinylbenzene copolymer, filler particle size: 10 μm).

[0017] For example, when an isocyanate compound having (m+n) isocyanate groups is reacted with an alkylene oxide (meth)acrylate adduct or a polyalkylene glycol compound having a hydroxyl group at one end first, the polyalkylene glycol compound has a molecular weight distribution and contains polyalkylene glycols having hydroxyl groups at both ends as well as at one end, so gelation often occurs. When gelation occurs, not only is the reaction unable to proceed stably, but the resulting reaction product is also difficult to dissolve in water. On the other hand, as described above, by first reacting an isocyanate compound having (m+n) isocyanate groups with n molar ratio of a hydroxyl group-containing (meth)acrylate compound and then reacting it with a (meth)acrylic acid alkylene oxide adduct compound or a polyalkylene glycol compound containing a hydroxyl group at one end, the polyalkylene glycol compound is bonded in a pendant-like manner to form a pendant-type urethane acrylate structure, which enables self-emulsification.

[0018] Next, water is added to the urethane (meth)acrylate oligomer represented by formula (1) to produce a water-soluble urethane (meth)acrylate oligomer composition in the form of an emulsion liquid. For this purpose, water is gradually added to the urethane (meth)acrylate oligomer obtained above. At this time, the obtained urethane (meth)acrylate oligomer is preferably maintained at a temperature in the range of, for example, 30°C to 80°C, and the temperature of the water to be added is also preferably adjusted to the same range, more preferably to a temperature range of 40°C to 70°C or 40°C to 60°C. The water to be added may be tap water, deionized water, ion-exchanged water, distilled water, or other various waters. The water is preferably added by, for example, dropping or divided. In the case of divided addition, the amount of water added at one time is, for example, 50% by weight to 200% by weight, preferably 100% by weight to 200% by weight of the mass of the urethane (meth)acrylate oligomer. The amount of water added is preferably an amount that results in a resin concentration of 50% by weight or less, more preferably 10% by weight to 45% by weight, and even more preferably 15% by weight to 40% by weight or 20% by weight to 40% by weight. For example, the time required for adding water may be 5 minutes or more from the start to the end of the addition of water, and is preferably 5 minutes to 2 hours, and more preferably 10 minutes to 30 minutes or 15 minutes to 30 minutes.

[0019] Also, at the same time as the addition of water, it is preferable to place a stirring blade near the interface between the oligomer and water or slightly on the water side of the interface and stir. It is preferable to stir gently here. In addition, since stirring with a stirrer sinks to the bottom of the container and cannot be placed at the interface between the oligomer and water, that is, the W / O interface, it is preferable to stir using a stirrer that can place a stirring blade near the interface between the oligomer and water. As the stirring blade, for example, a paddle blade can be used. The paddle blade can be placed near the interface between the oligomer and water or slightly on the water side of the interface, and may have only one blade or may have two or more blades in multiple stages. For gentle stirring, a rotation speed of 500 rpm or less can be mentioned, preferably 300 rpm or less, more preferably 200 rpm or less, and particularly preferably 100 rpm to 300 rpm, 100 rpm to 150 rpm, or 10 rpm to 100 rpm. Furthermore, it is preferable to continue stirring even after the addition of water is completed. The stirring in this case may be different from the stirring during the addition, but it is preferable to continue stirring at the same rate. After the addition of water is completed, stirring may be continued for, for example, 10 minutes or more, preferably 20 minutes or more, and more preferably 30 minutes or more. The rotation speed in this case may be in the same range as above.

[0020] By emulsifying by such an emulsification method (phase inversion emulsification), the obtained emulsion has an extremely small average particle size and high storage stability. In addition, when the emulsion is used as a coating composition, for example, after coating and drying to form a radiation-cured coating film, the obtained coating film has good leveling properties and extremely high water resistance, and a coating composition having contradictory properties can be obtained in which the oligomer before curing is water-soluble, while the coating film after curing has high water resistance. It has been confirmed that this is due to the fact that the particle size of the urethane (meth)acrylate oligomer in the obtained water-soluble urethane (meth)acrylate oligomer composition is made into uniform fine particles. For example, in the particle size distribution of the emulsion particles, the particle size of 50% of the particles is 100 nm or less. In addition, the 50% particle size is preferably 60 nm or less, more preferably 50 nm or less, and even more preferably 10 nm to 45 nm. In addition, the particle size of 95% of the particles is 150 nm or less. Also, 95% of the particle size is preferably 140 nm or less, more preferably 120 nm or less, and even more preferably 30 nm to 115 nm. From another viewpoint, the arithmetic mean diameter may be 110 nm or less. Also, it is preferably 100 nm or less, more preferably 70 nm or less, and even more preferably 10 nm to 60 nm. These values ​​were obtained by measuring the particle size distribution of the emulsion using a dynamic light scattering particle size distribution measuring device (LB-500) manufactured by Horiba, Ltd. In addition, such a coating film also has antistatic properties, so it can protect the surface of a substrate such as plastic, prevent dust absorption, and even impart antibacterial properties. In addition, such a coating film has excellent antifogging properties because it has a hydrophilic group, so it can be used to prevent fogging not only for plastics but also for glasses, mirrors, etc., and can also provide good dispersibility in water-based pigments. Furthermore, since the molecular weight of the urethane (meth)acrylate oligomer itself is relatively small, it can also be used as a component of water-soluble UV inkjet ink.

[0021] (Addition of crosslinked conductive coating composition (B)) The crosslinked conductive coating composition (B) contains at least a π-conjugated conductive polymer (b-1). By containing the π-conjugated conductive polymer (b-1), the above-mentioned effects, particularly excellent antistatic properties, can be obtained compared to other antistatic agents. The crosslinked conductive coating composition (B) preferably contains a binder (b-2) and a crosslinking agent (b-3) in addition to the π-conjugated conductive polymer (b-1).

[0022] (π-conjugated conductive polymer (b-1)) Examples of the π-conjugated conductive polymer include polythiophenes, polyanilines, polythiophene vinylenes, polypyrroles, and polyfurans. Examples of polythiophenes include polythiophene, poly(alkylthiophenes), poly(monoalkoxythiophenes), poly(dialkoxythiophenes), and poly(alkylenedioxythiophenes). The polythiophenes are preferably alkylenedioxypoly(thiophenes) doped with polystyrenesulfonic acid (PSS), and more preferably a complex of poly3,4-ethylenedioxythiophene (PEDOT) and PSS (hereinafter also referred to as "PEDOT / PSS"). PEDOT / PSS can be obtained, for example, by polymerizing 3,4-ethylenedioxythiophene (EDOT) as a monomer in an aqueous phase in the presence of polystyrenesulfonic acid (PSS) as a dopant using an oxidizing agent. Examples of commercially available PEDOT / PSS include the product name "Clevios P" (manufactured by Heraeus Co., Ltd.) and the product name "Orgacon ICP1010" (manufactured by Agfa Materials Japan, Inc.). Examples of polyanilines include polyaniline, poly(2-methylaniline), poly(3-isobutylaniline), poly(2- or 3-anilinesulfonic acid), and the like. Examples of polythiophene vinylenes include poly(thiophene vinylene), alkylenedioxy group-substituted poly(thiophene vinylene), alkoxy group-substituted poly(thiophene vinylene), alkyl group-substituted poly(thiophene vinylene), carboxyl group-substituted poly(thiophene vinylene), hydroxy group-substituted poly(thiophene vinylene), phenyl group-substituted poly(thiophene vinylene), cyano group-substituted poly(thiophene vinylene), halogen-substituted poly(thiophene vinylene), etc. Examples of alkylenedioxy group-substituted poly(thiophene vinylene)s include poly(3,4-ethylenedioxythiophene vinylene), poly(3,4-propylenedioxythiophene vinylene), poly(3,4-butenedioxythiophene vinylene), etc. Examples of alkoxy-substituted poly(thiophene vinylene)s include poly(3-methoxythiophene vinylene), poly(3-ethoxythiophene vinylene), poly(3-butoxythiophene vinylene), poly(3,4-dimethoxythiophene vinylene), poly(3,4-diethoxythiophene vinylene), poly(3,4-dipropoxythiophene vinylene), poly(3,4-dibutoxythiophene vinylene), poly(3-methyl-4-methoxythiophene vinylene), poly(3-methyl-4-ethoxythiophene vinylene), etc. Examples of alkyl-substituted poly(thiophene vinylene)s include poly(3-methylthiophene vinylene), poly(3-ethylthiophene vinylene), poly(3-propylthiophene vinylene), poly(3,4-dimethylthiophene vinylene), poly(3,4-dibutylthiophene vinylene), etc. Examples of carboxyl group-substituted poly(thiophene vinylene)s include poly(3-carboxythiophene vinylene), poly(3-methyl-4-carboxythiophene vinylene), poly(3-methyl-4-carboxyethylthiophene vinylene), and poly(3-methyl-4-carboxybutylthiophene vinylene). Examples of hydroxyl group-substituted poly(thiophene vinylene)s include poly(3-hydroxythiophene vinylene), poly(3,4-dihydroxythiophene vinylene). Examples of phenyl group-substituted poly(thiophene vinylene)s include poly(3-phenylthiophene vinylene).Cyano-substituted poly(thiophene vinylene)s include poly(3-cyanothiophene vinylene), etc. Halogen-substituted poly(thiophene vinylene)s include poly(3-bromothiophene vinylene), poly(3-chlorothiophene vinylene), poly(3-iodothiophene vinylene), etc. Examples of polypyrroles include poly(pyrrole), alkoxy group-substituted poly(pyrrole), alkyl group-substituted poly(pyrrole), carboxyl group-substituted poly(pyrrole), hydroxy group-substituted poly(pyrrole), etc. Examples of alkoxy group-substituted poly(pyrrole)s include poly(3-methoxypyrrole), poly(3-ethoxypyrrole), poly(3-butoxypyrrole), poly(3-hexyloxypyrrole), poly(3-methyl-4-hexyloxypyrrole), etc. Examples of alkyl group-substituted poly(pyrrole)s include poly(3-methylpyrrole), poly(3-ethylpyrrole), poly(3-n-propylpyrrole), poly(3-butylpyrrole), poly(3,4-dimethylpyrrole), poly(3,4-dibutylpyrrole), etc. Examples of the carboxyl group-substituted poly(pyrrole)s include poly(3-carboxypyrrole), poly(3-methyl-4-carboxypyrrole), poly(3-methyl-4-carboxyethylpyrrole), poly(3-methyl-4-carboxybutylpyrrole), etc. Examples of the hydroxyl group-substituted poly(pyrrole)s include poly(3-hydroxypyrrole). Examples of polyfurans include polyfuran, alkoxy group-substituted polyfurans, alkyl group-substituted polyfurans, carboxyl group-substituted polyfurans, and hydroxy group-substituted polyfurans. Examples of alkoxy group-substituted polyfurans include poly(3-methoxyfuran), poly(3-ethoxyfuran), poly(3-butoxyfuran), poly(3-hexyloxyfuran), and poly(3-methyl-4-hexyloxyfuran). Examples of alkyl group-substituted polyfurans include poly(3-methylfuran), poly(3-ethylfuran), poly(3-n-propylfuran), poly(3-butylfuran), poly(3,4-dimethylfuran), and poly(3,4-dibutylfuran). Examples of carboxyl group-substituted polyfurans include poly(3-carboxyfuran), poly(3-methyl-4-carboxyfuran), poly(3-methyl-4-carboxyethylfuran), and poly(3-methyl-4-carboxybutylfuran). Examples of hydroxy-substituted polyfurans include poly(3-hydroxyfuran). These may be used alone or in combination of two or more. From the viewpoints of the antistatic properties and transparency of the cured product, the component (b-1) is preferably a polythiophene and / or a polyaniline, more preferably a polythiophene, and further preferably PEDOT / PSS.

[0023] (Binder (b-2)) The binder is used for the purpose of improving the adhesion between the substrate and the coating film and the strength of the coating film. Examples of binders include homopolymers such as polyester, polyacrylate, polymethacrylate, polyurethane, polyvinyl acetate, polyvinylidene chloride, polyamide, and polyimide; copolymers obtained by copolymerizing monomers such as styrene, vinylidene chloride, vinyl chloride, alkyl acrylate, and alkyl methacrylate; and alkoxysilane compounds such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. These binders may be used alone or in combination of two or more.

[0024] (Crosslinking agent (b-3)) The crosslinking agent is used for the purpose of further improving the strength of the coating film and for the purpose of improving water resistance (antistatic properties). The crosslinking agent may be used in combination with a binder for the purpose of crosslinking the binder, or may be used to form a self-crosslinking film of the crosslinking agent without using a binder. As a catalyst for crosslinking, an acidic group possessed by the dopant may be used, and further, an organic acid or an inorganic acid may be added. Also, a heat-sensitive acid generator, a radiation-sensitive acid generator, and an electromagnetic wave-sensitive acid generator may be added. Examples of the crosslinking agent include melamine-based, polycarbodiimide-based, polyoxazoline-based, polyepoxy-based and polyisocyanate-based crosslinking agents. These crosslinking agents may be used alone or in combination of two or more.

[0025] The crosslinkable conductive coating composition (B) may contain solvents, dispersion media, additives, etc. that are generally used in conductive coating compositions, as long as the effects of the present invention are not impaired. The solvent or dispersion medium may be any that dissolves or disperses each component contained in the conductive coating composition, and examples thereof include water, organic solvents, and mixtures thereof. Among these, water is preferably contained, and when an organic solvent is further contained, methanol, ethanol, 2-propanol, and the like are preferable. In the present invention, when each component other than the solvent or dispersion medium contained in the conductive coating composition is dissolved, it is called a solvent, and when at least one component constituting the composition is uniformly dispersed, it is called a dispersion medium. The additives include a leveling agent, a conductivity improver, and the like. The leveling agent is used for the purpose of improving the leveling property. Examples of the leveling agent include surfactants such as nonionic surfactants (polyoxyethylene alkylphenyl ether, propylene oxide polymer, ethylene oxide polymer, sorbitan fatty acid ester, coconut oil fatty acid ethanolamide, etc.), anionic surfactants (sulfonic acid ester, phosphoric acid ester, succinic acid ester, etc.). These leveling agents may be used alone or in combination of two or more kinds. The conductive improver is used for the purpose of improving the conductivity. Examples of the conductive improver include ethylene glycol, diethylene glycol, propylene glycol, trimethylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, catechol, cyclohexanediol, cyclohexanedimethanol, glycerin, dimethyl sulfoxide, N-methylpyrrolidone, N-methylformamide, N-dimethylformamide, isophorone, propylene carbonate, cyclohexanone, γ-butyrolactone, and diethylene glycol monoethyl ether. Among them, ethylene glycol, dimethyl sulfoxide, N-methylformamide, and N-methylpyrrolidone are preferred. These conductive improvers may be used alone or in combination of two or more.

[0026] The crosslinked conductive coating composition (B) contains the π-conjugated conductive polymer (b-1) in an amount of preferably 0.05 to 2 parts by mass, more preferably 0.1 to 1 part by mass, per 100 parts by mass of the crosslinked conductive coating composition (B) in terms of solid content. When the binder (b-2) is contained, the binder (b-2) is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, based on 100 parts by mass of the crosslinked conductive coating composition (B) in terms of solid content. When the crosslinking agent (b-3) is contained, the amount of the crosslinking agent (b-3) is preferably 0.05 to 30 parts by mass, more preferably 0.1 to 25 parts by mass, based on 100 parts by mass of the crosslinkable conductive coating composition (B) in terms of solid content. The amount of water contained in the crosslinked conductive coating composition (B) is preferably 20 to 50 parts by mass, more preferably 30 to 40 parts by mass, per 100 parts by mass of the crosslinked conductive coating composition (B). When a solvent or dispersion medium is contained, the solvent or dispersion medium is preferably methanol, ethanol, or 2-propanol. The content of the solvent or dispersion medium is not particularly limited, and is preferably 55 to 75 parts by mass, more preferably 60 to 70 parts by mass, relative to 100 parts by mass of the crosslinked conductive coating composition (B). The ratio (mass ratio) of water to the organic solvent is preferably 100:0 to 5:95, more preferably 100:0 to 30:70. When a leveling agent is contained, the amount of the leveling agent is preferably 0.01 to 0.5 parts by mass, more preferably 0.02 to 0.2 parts by mass, calculated as solid content, per 100 parts by mass of the crosslinked conductive coating composition (B). When a conductivity enhancer is contained, the amount of the conductivity enhancer is preferably 0.1 to 2 parts by mass, more preferably 0.5 to 1.5 parts by mass, per 100 parts by mass of the crosslinked conductive coating composition (B).

[0027] In addition, the "crosslinked" type of crosslinked conductive coating composition is preferably supplied as a two-liquid type due to the short pot life of the coating. In contrast, a "one-liquid" conductive coating composition is a coating composition that contains a conductive polymer (b-1) and a binder (b-2) but does not contain a crosslinking agent (b-3). The "crosslinked" conductive coating composition has superior water resistance (antistatic properties) compared to the "one-liquid" conductive coating composition. The "one-component" conductive coating composition contains the π-conjugated conductive polymer (b-1) in an amount of preferably 0.05 to 2 parts by mass, more preferably 0.1 to 1.5 parts by mass, calculated as solid content, per 100 parts by mass of the conductive coating composition (B). The binder (b-2) is preferably contained in an amount of 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, based on 100 parts by mass of the conductive coating composition (B) in terms of solid content. In this case, the amount of water contained in the conductive coating composition (B) is preferably 50 to 95 parts by mass, more preferably 60 to 90 parts by mass, per 100 parts by mass of the crosslinked conductive coating composition (B). When a solvent or dispersion medium is contained, the solvent or dispersion medium is preferably methanol, ethanol, or 2-propanol. The content of the solvent or dispersion medium is not particularly limited, and is preferably 1 to 15 parts by mass, more preferably 5 to 10 parts by mass, relative to 100 parts by mass of the conductive coating composition (B). When a leveling agent is contained, the amount of the leveling agent is preferably 0.01 to 0.5 parts by mass, more preferably 0.05 to 1 part by mass, calculated as solid content, relative to 100 parts by mass of the conductive coating composition (B). When a conductivity enhancer is contained, the amount of the conductivity enhancer is preferably 0.1 to 5 parts by mass, more preferably 1 to 3 parts by mass, per 100 parts by mass of the conductive coating composition (B). Commercially available products include those under the product names "Denatron TX-401" (manufactured by Nagase ChemteX Corporation) and "Sepulgida AS-G1" (manufactured by Shin-Etsu Polymer Co., Ltd.), and these may be used with the addition of a crosslinking agent (b-3). The content of the crosslinking agent is not particularly limited, but is preferably 0.05 to 30 parts by mass, more preferably 0.1 to 25 parts by mass, based on 100 parts by mass of the "one-liquid type" conductive coating composition, calculated as solid content.

[0028] Water-dispersible antistatic coating composition The water-dispersible antistatic coating composition obtained as described above may contain 100 parts by mass of the water-soluble urethane (meth)acrylate oligomer composition (A) (based on a resin concentration of 30% by mass) and 10 to 60 parts by mass of the crosslinked conductive coating composition (B) (based on a solids concentration of 7% by mass), preferably 20 to 50 parts by mass.

[0029] Such a water-dispersible antistatic coating composition preferably further contains a polymerization initiator (C). By adding a polymerization initiator to the water-dispersible antistatic coating composition, the urethane (meth)acrylate oligomer can be more easily crosslinked and / or polymerized by heat or active energy rays (e.g., ultraviolet rays) to form a cured polymer, and the water-dispersible antistatic coating composition can exhibit its functions (anti-fogging properties, substrate adhesion, transparency, solvent resistance, abrasion resistance, etc.). The polymerization initiator (C) may be a radical polymerization initiator that undergoes radical decomposition by heat or a reducing substance, etc., to cause addition polymerization of vinyl monomers. Examples of the radical polymerization initiator include water-soluble persulfates, peroxides, azobis compounds, etc. Specific examples include potassium persulfate, sodium persulfate, ammonium persulfate, hydrogen peroxide, t-butyl hydroperoxide, t-butyl peroxybenzoate, 2,2-azobisisobutyronitrile, 2,2-azobis(2-diaminopropane) hydrochloride, and 2,2-azobis(2,4-dimethylvaleronitrile). Among these, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]tetrahydrate (trade name: VA-057, Fujifilm Wako Pure Chemical Industries, Ltd.), N,N'-bis(2-hydroxyethyl)-2,2'-dimethyl-2,2'-diazenediyldipropanamide (trade name: VA-086, Fujifilm Wako Pure Chemical Industries, Ltd.), bis[2-(4,5-dihydro-1H-imidazol-2-yl)propan-2-yl]diazene (trade name: VA-061, Fujifilm Wako Pure Chemical Industries, Ltd.), azobisisobutyric acid amidine hydrochloride (trade name: V-50, Fujifilm Wako Preferred are water-soluble azo polymerization initiators such as (E)-1,2-bis[2-(4,5-dihydro-1H-imidazol-2-yl)propan-2-yl]diazene-dihydrochloride (trade name: VA-044, manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) and azobiscyanovaleric acid (trade name: V-501, manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.), and water-soluble organic peroxides such as tert-butyl hydroperoxide (trade name: Perbutyl H, manufactured by NOF Corporation). The polymerization initiator (C) may be contained in an amount of 0.001 to 10 parts by mass relative to 100 parts by mass of the solid content of the water-soluble urethane (meth)acrylate oligomer composition (A) (based on a resin content concentration of 30% by mass), and is preferably contained in an amount of 0.01 to 10 parts by mass, more preferably 0.05 to 8 parts by mass, and further preferably 0.6 to 5 parts by mass. When it is desired to accelerate the polymerization rate and carry out polymerization at a low temperature such as 70°C or lower, it is preferable to use a reducing agent such as sodium bisulfite, ferrous chloride, ascorbate, or Rongalit in combination with a radical polymerization initiator.

[0030] The water-dispersible antistatic coating composition may further contain a photopolymerization initiator, an ethylenically unsaturated monomer, an antistatic agent, a filler, a dye pigment, an oil, a plasticizer, a wax, a drying agent, a dispersant, a wetting agent, an emulsifier, a gelling agent, a stabilizer, an antifoaming agent, a general additive for aqueous emulsion paints, such as a surface conditioner containing nanoparticle colloidal silica to improve surface hardness and abrasion resistance, a surfactant containing a polyglycerin derivative, a pigment, a colorant, a thickener, a thixotropic agent, a flame retardant, an antiseptic, an antifungal agent, an anti-algae agent, a plasticizer, a filler, a reinforcing agent, a matting agent, etc. In addition, a silane coupling agent may be added for the purpose of adhesion to glass, and an antioxidant or an ultraviolet absorbing agent may be added to increase the light resistance of the coating film. Any of these may be used that are commonly used in the field. If necessary, the solvent may contain an organic solvent such as ethyl acetate, butyl acetate, toluene, xylene, methanol, ethanol, propanol, butanol, acetone, methyl isobutyl ketone, methyl ethyl ketone, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cellosolves, and diacetone alcohol. These components may be added simultaneously or sequentially to the water-soluble urethane (meth)acrylate oligomer composition or the water-dispersible antistatic coating composition and mixed.

[0031] The photopolymerization initiator can cure the water-dispersible antistatic coating composition by active energy rays. As the photopolymerization initiator, it is preferable to use a photopolymerization initiator having water-solubility or water-dispersibility. Examples of such photopolymerization initiators include 2-(3-dimethylamino-2-hydroxypropoxy)-3,4-dimethyl-9H-thioxanthone-9-one methchloride (manufactured by Octel Chemicals, "Quantacure QTX"), 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one (manufactured by Ciba Specialty Chemicals, "Irgacure 2959"), and the like. Of these, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one ("Irgacure 2959" manufactured by Ciba Specialty Chemicals, and "Omnirad 2959" manufactured by IGM Resins BV) is preferred. The photopolymerization initiator can be added in an amount of 0.002 to 10 parts by mass, preferably 0.01 to 10 parts by mass, more preferably 0.05 to 8 parts by mass, and even more preferably 0.6 to 5 parts by mass, relative to 100 parts by mass of the solid content of the water-soluble urethane (meth)acrylate oligomer composition (A) (based on a resin concentration of 30% by mass).

[0032] Examples of the photopolymerization initiator aid include triethanolamine, triisopropanolamine, 4,4'-dimethylaminobenzophenone (Michler's ketone), 4,4'-diethylaminobenzophenone, 2-dimethylaminoethylbenzoic acid, ethyl 4-dimethylaminobenzoate, (n-butoxy)ethyl 4-dimethylaminobenzoate, isoamyl 4-dimethylaminobenzoate, 2-ethylhexyl 4-dimethylaminobenzoate, 2,4-diethylthioxanthone, and 2,4-diisopropylthioxanthone. The photopolymerization initiation aid may be added in an amount of 0.1 to 100 parts by mass relative to 100 parts by mass of the photopolymerization initiator.

[0033] Examples of the ethylenically unsaturated monomer include (meth)acrylic acid compounds and vinyl group-containing compounds. Examples of the (meth)acrylic acid compounds include (meth)acrylic acid amides, alkyl (meth)acrylates, aminoalkyl (meth)acrylates, quaternary salts of aminoalkyl (meth)acrylates, alkoxy polyalkylene glycol (meth)acrylates, hydroxyalkyl (meth)acrylates, acid anhydride adducts of hydroxyalkyl (meth)acrylates, polyalkylene glycol di(meth)acrylates, alkyl diol di(meth)acrylates, polyol poly(meth)acrylates, and alkylene oxide-added polyol poly(meth)acrylates. Examples of the vinyl group-containing compounds include vinyl acetate, N-vinyl acetamide, vinyl pyrrolidone, vinyl alkyl ethers, vinyl sulfonic acid, and salts of vinyl sulfonic acid. These may be used alone or in combination of two or more. Examples of acrylic acid amides include acryloyl morpholine and dimethylaminoalkyl (meth)acrylamide. Examples of aminoalkyl (meth)acrylates include diethylaminoethyl (meth)acrylate. Examples of quaternary salts of aminoalkyl (meth)acrylates include alkyloylaminopropyldimethyl-2-hydroxyethylammonium salt. Examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, and propyl (meth)acrylate. Examples of alkoxy polyalkylene glycol (meth)acrylates include methoxy polyethylene glycol (meth)acrylate and methoxy polypropylene glycol (meth)acrylate. Examples of hydroxyalkyl (meth)acrylates include hydroxyethyl (meth)acrylate and hydroxypropyl (meth)acrylate. Examples of the acid anhydride adduct of hydroxyalkyl (meth)acrylate include hydroxyethyl (meth)acrylate phthalic anhydride adduct, hydroxyethyl (meth)acrylate succinic anhydride adduct, hydroxyethyl (meth)acrylate tetrahydrophthalic anhydride adduct, hydroxyethyl (meth)acrylate hexahydrophthalic anhydride adduct, hydroxypropyl (meth)acrylate phthalic anhydride adduct, hydroxypropyl (meth)acrylate succinic anhydride adduct, hydroxypropyl (meth)acrylate tetrahydrophthalic anhydride adduct, and hydroxypropyl (meth)acrylate hexahydrophthalic anhydride adduct. Examples of polyalkylene glycol di(meth)acrylates include polyethylene glycol di(meth)acrylate and polypropylene glycol di(meth)acrylate. Examples of alkyl diol di(meth)acrylates include butane diol di(meth)acrylate and hexane diol di(meth)acrylate. Examples of the polyol poly(meth)acrylates include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.Examples of the alkylene oxide-added polyol poly(meth)acrylates include alkylene oxide-added trimethylolpropane tri(meth)acrylate, alkylene oxide-added pentaerythritol tri(meth)acrylate, alkylene oxide-added pentaerythritol tetra(meth)acrylate, alkylene oxide-added pentaerythritol hexa(meth)acrylate, etc. Examples of the vinyl alkyl ethers include methyl vinyl ether, ethyl vinyl ether, propyl vinyl ether, amyl vinyl ether, 2-ethylhexyl vinyl ether, etc. Among these, the (meth)acrylic acid compound or vinyl group-containing compound is more preferably (meth)acryloylmorpholine, vinylpyrrolidone, dimethylaminoalkyl (meth)acrylate, a quaternary salt of dimethylaminoalkyl (meth)acrylate, dimethylaminoalkyl (meth)acrylamide, N-vinylacetamide, vinylsulfonic acid, or a vinylsulfonate salt, all of which are water-dispersible. The ethylenically unsaturated monomer may be added in an amount of 0 to 100 parts by mass, preferably 0.02 to 80 parts by mass, per 100 parts by mass of the water-soluble urethane (meth)acrylate oligomer composition (A) (based on a resin concentration of 20% by mass).

[0034] The water-dispersible antistatic coating composition can be applied to various substrates and used as an antistatic coating. Substrates include plastics (e.g., polyolefin resins such as polyethylene, polypropylene, and polycyclopentadiene, particularly polyester resins such as polycarbonate and polyethylene terephthalate, ABS resins, acrylic resins, etc.), glass, metal, paper, wood, cement, and other substrates. When the water-dispersible antistatic coating composition is applied to the surface of a substrate (e.g., an easily adhesive PET film), the dry thickness is set to 0.01 to 100 μm, preferably 0.5 to 20 μm. In this way, by applying the water-dispersible antistatic coating composition to a substrate, an antistatic coating film having good substrate adhesion, transparency, initial antistatic property, water resistance (antistatic property), and abrasion resistance can be obtained.

[0035] Examples of a method for coating (applying) the water-dispersible antistatic coating composition on any surface of a substrate include a method using a coater such as a gravure coater, a roll coater, a curtain flow coater, a spin coater, a bar coater, a reverse coater, a kiss coater, a fountain coater, a rod coater, an air doctor coater, a knife coater, a blade coater, a cast coater, or a screen coater; a method using a sprayer such as an air spray, an airless spray, or a rotor dampening; and an immersion method such as dipping. After the water-dispersible antistatic coating composition is applied to a substrate, the coating film is cured by irradiating it with active energy rays, heat treatment, or a combination of these. Examples of active energy rays include far ultraviolet rays, ultraviolet rays, near ultraviolet rays, infrared rays, X-rays, γ-rays, etc. The irradiation dose of active energy rays is, for example, 100 to 2000 mJ / cm. 2 The range is 500 to 1000 mJ / cm 2The range is preferable. The heat treatment may be performed in a temperature range of 80 to 200°C, specifically, in a temperature range of 100 to 200°C or less, for 1 to 30 minutes, including hot air drying and heat treatment, more preferably 5 to 15 minutes at 100°C, 3 to 10 minutes at 120°C, and 1 to 5 minutes at 130°C or 150°C. It is also preferable to irradiate active energy rays after such hot air drying. This prevents moisture from remaining in the coating film, prevents the coating film from whitening in appearance, and improves adhesion to the substrate. In addition, the leveling of the surface of the cured product by the coating film is improved, and the steel wool resistance and water resistance can also be improved. In particular, crosslinking under high-temperature heat treatment improves water resistance and water-resistant antistatic properties.

[0036] The water-dispersible antistatic coating composition of the present invention is crosslinked / polymerized to form a coating film, and has excellent scratch resistance and antistatic properties, so that it can protect the surface of a substrate such as plastic and prevent dust absorption. In addition, it has excellent antifogging properties and can be used to prevent fogging not only of plastics but also of glasses, mirrors, etc. In addition, the water-dispersible antistatic coating composition of the present invention is useful in the fields of optical films for various displays, various electronic components, carrier tapes and cover tapes for packaging electronic components, antistatic agents for trays, etc., transparent electrodes and electromagnetic shields for various displays, etc. In addition, the optical film having such a configuration is suitable as an optical film having an antistatic layer for use in liquid crystal displays, polarizing plates, electroluminescent displays, plasma displays, electrochromic displays, solar cells, etc. EXAMPLES

[0037] Hereinafter, examples of the present invention will be described in detail. A water-dispersible antistatic coating composition of the present invention was prepared as follows. (Production of Urethane (Meth)acrylate Oligomer Composition) In a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a dry air inlet, 159 g (0.29 mol) of hexamethylene diisocyanate trimer (isocyanate group content 23%), 0.6 g of 2,6-di-tert-butylcresol, and 0.02 g of dibutyltin dilaurate were charged. Dipentaerythritol pentaacrylate (0.58 mol) (545 g of a mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate (hydroxyl value 59.8 mgKOH / g)) was added dropwise to the flask at 70°C over about 1 hour, and the mixture was allowed to react at 70°C for 4 hours. The mixture was cooled to 60°C when the remaining isocyanate group reached 1.7%. To this was added dropwise 643.9 g (0.30 mol) of polyethylene glycol monomethyl ether (weight average molecular weight 989.59, hydroxyl value 56.7 mgKOH / g) at 55° C. over approximately 1 hour. When the reaction started, heat was generated intensely, so cooling was performed as necessary. When the heat generation had almost subsided, the mixture was heated to 70° C. and reacted for 3 hours. The infrared absorption spectrum of the oligomer was measured, and the absorption spectrum of the isocyanate group (2280 cm -1 The reaction was terminated when the disappearance of the urethane acrylate oligomer (resin concentration: 100% by mass) was obtained. The weight average molecular weight of the obtained urethane acrylate oligomer was 12,000.

[0038] (emulsification) 300g of the urethane acrylate oligomer obtained above was kept at 60°C, and 700g of ion-exchanged water at room temperature (25°C) was added dropwise or divided into five times (initial 400g, 100g added every 30 minutes) (phase inversion emulsification method) while stirring with a paddle blade near the interface between the oligomer and the ion-exchanged water (W / O interface). The stirring was performed at 10 to 50 rpm. The dropwise addition was stopped when the resin concentration reached 30% by mass, and an emulsion was obtained. Stirring was then maintained for 30 minutes to obtain a water-soluble urethane (meth)acrylate oligomer composition (A). The resulting water-soluble urethane (meth)acrylate oligomer composition (A) had a pH of 4 to 5, a heating residue (hereinafter also referred to as "resin concentration") of 30 mass%, and a viscosity at 25°C of 10 mPa·S.

[0039] (Preparation of crosslinked conductive coating composition (B) containing π-conjugated conductive polymer) The following ingredients were prepared: (B) Crosslinked conductive coating composition containing a π-conjugated conductive polymer π-conjugated conductive polymer (b-1) solution: PEDOT / PSS 0.1-1%, ethanol 1-10%, propanol 1-10%, water 80-95%, pH: 6.9, viscosity: 23.7 mPa·s / 25°C, solid content: 3.6%, Mixture of binder (b-2) and crosslinker (b-3): 2-40% resin mixture of 1-15 parts by mass of acrylic resin copolymer and 1-25 parts by mass of melamine resin derivative, 5-25% ethanol, 0.1-1% methanol, 30-70% water, pH: 7.4, viscosity: 7.6 mPa·s / 25°C, solid content: 20.2%, (B'-1) One-liquid conductive coating composition containing a π-conjugated conductive polymer: product name "Denatron TX-401" (manufactured by Nagase ChemteX Corporation), appearance: dark blue, viscosity: 26.1 mPa s, pH: 7.5, solid content: 3.9 mass%, containing 1 to 1.5 mass% PEDOT / PSS, (B'-2) One-liquid type conductive coating composition containing a π-conjugated conductive polymer: product name "Sepulgida AS-G1" (manufactured by Shin-Etsu Polymer Co., Ltd.), appearance: deep blue liquid, pH: 1.5-2.5, solid content: 1.2 to 1.3 mass%, (B'-3) SW-CNT (containing 3.4% single-wall carbon nanotubes) conductive paint composition: product name "Denatron C-100A" (manufactured by Nagase ChemteX Corporation), appearance: black, viscosity: 7-10 mPa s, pH: 7-10, solid content: 3.4% by mass, (B'-4) Quaternary ammonium salt-based conductive coating composition: Product name "ASA-197" (manufactured by Takamatsu Oil Co., Ltd.), main components: acrylic and quaternary ammonium salt, viscosity: about 500 mPa s, pH: 3-5, (B'-5) Synthetic mineral (anionic) conductive paint composition: Product name "ASA-2050" (manufactured by Takamatsu Oil Co., Ltd.), main components: polyester + synthetic clay mineral, viscosity: 100 mPa·s or less, pH: 8-10, (B'-6) Li-ion electrolyte (LiFSI: lithium bisfluorosulfonylimide): product name "IONEL (registered trademark) LF-101" (manufactured by Nippon Shokubai Co., Ltd.), appearance: white powder, purity: 99.9% or more, solubility: soluble in DMC and EMC at 50 wt% or more.

[0040] Example 1 In a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a dry air inlet, 100 g of the water-soluble urethane (meth)acrylate oligomer composition (A) (30 mass% solid content: 30 g solid content) and 20 g of the π-conjugated conductive polymer liquid (b-1) (containing 0.1 to 1% PEDOT / PSS, 3.6% solid content: 0.72 g solid content) were mixed at room temperature and uniformly dispersed, and then 10 g of a resin mixture of (b-2) and a crosslinking agent (b-3) (Nikarak MW-30LF (20.2% solid content: 2.02 g solid content) manufactured by Nippon Carbide Industries Co., Ltd.) was mixed at room temperature and uniformly dispersed. Then, 1.2 g of a polymerization initiator (C-1) 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one (manufactured by Ciba Specialty Chemicals, "Irgacure 2959") was added and dispersed at room temperature to obtain a water-dispersible antistatic coating composition (solid content 26%).

[0041] Example 2 Instead of 1.2 g of the polymerization initiator (C-1) 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one (manufactured by Ciba Specialty Chemicals, "Irgacure 2959") in Example 1, 1.5 g of ammonium sulfate (C-2) was charged and dispersed at room temperature to obtain a water-dispersible antistatic coating composition (solid content 26%).

[0042] Examples 3 to 4 and Comparative Examples 1 to 11 The components shown in Table 1 below were mixed to prepare water-dispersible antistatic coating compositions of Examples and Comparative Examples in the same manner as in Example 1. The components in Table 1 are as shown in Table 2. [Table 1] TIFF2024154323000002.tif55170 [Table 2]

[0043] Test Example 1 Each of the water-dispersible antistatic coating compositions obtained in the Examples and Comparative Examples was applied to an easily adhesive polyester film (hereinafter, referred to as the substrate PET) using a bar coater #14 so that the film thickness after drying would be 2 μm to 4 μm. After coating the water-dispersible antistatic coating composition, it was cured under the following conditions [a-1] or [a-2]. [a-1] Drying and heat treatment were performed at 130°C for 2 minutes, using an electrodeless lamp H bulb, line speed: 5.4m / min, irradiation amount: 600mJ / cm 2 , Peak illuminance: 1,500mW / cm 2 UV irradiation was performed. [a-2] Drying and heat curing were carried out at 150°C for 5 minutes. Each water-dispersible antistatic coating composition was coated on a highly adhesive polyester film and cured. The polyester film having the antistatic coating film thus obtained was used for the following evaluations.

[0044] (Coating appearance and leveling) The appearance and leveling of the coating of the polyester film with anti-fog coating were visually confirmed based on the presence or absence of whitening, unevenness (non-uniformity) of the coating, and repelling. Those without transparency or repelling were evaluated as good, being uniform and transparent coatings. The results are shown in Table 3. [Table 3]

[0045] Test Example 2 The following tests were carried out on the polyester film with the antistatic coating prepared in Test Example 1. The results are shown in Table 4. (Initial antistatic properties) Hirestar UX Applied voltage: 250V The surface resistivity (Ω / sq.) was measured under a measurement environment of 20°C and 45% RH. Surface resistivity: 1×10 5 ~1×10 11 The value of Ω / sq. was judged to be "○" for antistatic properties. Surface resistivity: 1×10 12 Ω / sq. or more was rated as no antistatic property x. (Water-resistant and anti-static) The polyester film with the antistatic coating was immersed in running water for 10 minutes, the water droplets were wiped off with a cloth, and the film was left to stand for 1 hour in a measurement environment of 20°C and 45% RH. Hirestar UX Surface resistivity (Ω / sq.) was measured at an applied voltage of 250 V under a measurement environment of 20°C and 45% RH. It has initial antistatic properties, Those that showed no increase in surface resistivity after the water resistance test were marked with an O. The increase in surface resistivity after water resistance test is 1×10 1 △, If the increase in surface resistivity after the water resistance test is less than 1×10, it is rated as ×. If the coating film peeled off or ran off from the substrate or turned white after the water resistance test, it was marked as XX. (Abrasion resistance) The abrasion resistance of the polyester film with the anti-fog coating was evaluated by rubbing it back and forth 10 times with steel wool (#0000) under a load of 50 to 500 g. The state of scratches was visually observed. Those without scratches under a load of 300 g or more were rated as ◯. (Coating film hardness) The pencil hardness of the antistatic coated polyester film was measured in accordance with JIS K5400. (Adhesion to substrate) The adhesion to each substrate was evaluated. According to JIS K5400, 100 2 mm squares were made on the polyester film with antistatic coating film obtained by curing each water-dispersible antistatic coating composition obtained in the Examples and Comparative Examples, and an adhesion test was performed using cellophane tape. The peeling state of the squares was observed, and the number of remaining squares was counted. (Optical properties) The total light transmittance of the polyester film with the antistatic coating was measured using a Konica Minolta spectrophotometer CM-3600A. A total light transmittance of 89% or more was considered to be acceptable (substrate A: 89.6% or more). [Table 4]

[0046] Test Example 3 The polyester films with antistatic coatings, which were evaluated in Test Example 2 for initial antistatic property as good (◯) and water-resistant antistatic property as good (◯), were evaluated for optical properties before and after the water resistance test. The results are shown in Table 5. (Optical properties) The haze and total light transmittance of the polyester film with the anti-fog coating were measured using a spectrophotometer CM-3600A manufactured by Konica Minolta. A sample with no change in haze and a total light transmittance of 88% or more was deemed to pass (substrate: 89.4% or more). [Table 5] [Industrial Applicability]

[0047] The water-dispersible antistatic coating composition obtained by the method for producing the water-dispersible antistatic coating composition of the present invention is very useful as various coating material such as paint, adhesive, adhesive, tackifier, release agent, ink, protective coating agent, anchor coating agent, magnetic powder coating binder, sandblasting coating, printing plate material, etc. In addition, the coated article of the present invention has excellent scratch resistance and antistatic properties, so that it can protect the surface of substrates such as plastics and prevent dust attraction. In addition, it has excellent antifogging properties and can be used for antifogging not only plastics but also glasses, mirrors, etc.

Claims

1. A water-soluble urethane (meth)acrylate oligomer composition (A) is prepared by reacting n mole ratios of a hydroxyl group-containing (meth)acrylate compound with 1 mole ratio of an isocyanate compound having (m+n) isocyanate groups, and then reacting m mole ratios of an alkylene oxide (meth)acrylate adduct or a polyalkylene glycol compound having a hydroxyl group at one end with the resulting reaction product to obtain a urethane (meth)acrylate oligomer represented by formula (1). Water is added to the urethane (meth)acrylate oligomer while gently stirring the interface between the urethane (meth)acrylate oligomer and water to emulsify the mixture, A method for producing a water-dispersible antistatic coating composition, comprising adding a crosslinked conductive coating composition (B) containing a π-conjugated conductive polymer to the water-soluble urethane (meth)acrylate oligomer composition (A). (R 1 O-CONH) m -R 2 -(NHCO-OR 3 ) n (1) (In the formula, R 1 O- represents a dehydrogenation residue of a polyalkylene glycol compound having a hydroxyl group at one end or a (meth)acrylic acid alkylene oxide adduct; R 2 represents a residue of a deisocyanated group of an isocyanate compound, R 3 O- represents a dehydrogenation residue of a hydroxyl group-containing (meth)acrylate compound, m and n each represent an integer between 1 and 50, provided that m≦n.

2. The method according to claim 1, wherein the stirring is carried out using a paddle blade at a rotation speed of 10 rpm to 100 rpm.

3. 2. The method according to claim 1, wherein the water is added until the solid content becomes 50% by weight or less, and after the addition of the water is completed, gentle stirring is continued for a predetermined period of time.

4. The method according to claim 3, wherein after the addition of the water is completed, stirring is continued for 10 minutes or more at a rotation speed of 10 rpm to 100 rpm.

5. 2. The method according to claim 1, wherein the isocyanate compound (A) is a diisocyanate or a polyisocyanate of a diisocyanate monomer.

6. 2. The method according to claim 1, wherein the polyalkylene glycol compound (A) containing a hydroxyl group at one end is an alkoxy polyalkylene glycol.

7. 2. The method according to claim 1, wherein the (meth)acrylic acid alkylene oxide adduct (A) is a compound obtained by adding (meth)acrylic acid to an alkylene oxide or by mono(meth)acrylate of a polyalkylene glycol.

8. 2. The method according to claim 1, wherein the hydroxyl group-containing (meth)acrylate compound (A) is a hydroxyalkyl (meth)acrylate, a polyol (meth)acrylate or an alkylene oxide-added polyol (meth)acrylate.

9. A water-dispersible antistatic coating composition obtained by the process according to any one of claims 1 to 8, The crosslinked conductive coating composition (B) is a water-dispersible antistatic coating composition comprising a π-conjugated conductive polymer (b-1), a binder (b-2) and a crosslinking agent (b-3).

10. The water-dispersible antistatic coating composition according to claim 9, further comprising a polymerization initiator (C).

11. An antistatic coating film which is a heat-cured product of the water-dispersible antistatic coating composition according to claim 9.

12. An antistatic coating film which is a cured product of the water-dispersible antistatic coating composition according to claim 9 by irradiation with active energy rays.

Citation Information

Patent Citations

  • Toner composition and its manufacturing method

    JP2005182041A

  • Active energy ray-curable oil in water-type emulsion composition

    JP2007191530A

  • Aqueous emulsion and coating film, cured product and laminate

    JP2020122166A

  • Manufacturing method of aqueous urethane(METH)acrylate oligomer composition, coating composition, coated article and manufacturing method thereof

    JP2021050310A

  • Method for producing active energy ray-curable water-soluble resin composition containing photochromic dye and coating composition, and cured article

    JP2022037865A