Manufacturing method of electrode

By uniformly dispersing binders and conductive additives through a two-step compounding process followed by a dry film forming method, the method addresses the issue of increased resistance in electrodes, resulting in improved conductivity and battery performance.

JP2024154502AInactive Publication Date: 2024-10-31TOYOTA JIDOSHA KK

Patent Information

Application Number
JP2023068325
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for manufacturing electrodes in batteries often result in increased electrode resistance due to uneven dispersion of binders and conductive additives, leading to decreased electronic conductivity.

Method used

A method involving a first compounding step to combine a binder and a conductive aid, followed by a second compounding step with an active material, using a dry film forming process to form an active material layer, ensuring uniform dispersion of the additives on the active material surface.

Benefits of technology

This approach results in electrodes with suppressed resistance and improved electronic conductivity by ensuring uniform distribution of the binder and conductive aid, thereby enhancing battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154502000001_ABST
    Figure 2024154502000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of an electrode capable of reducing resistance.SOLUTION: A disclosed manufacturing method of an electrode includes: a first compositing step of obtaining a first composite by combining a binder and conductive additive; a second composite step of obtaining a second composite by combining the first composite and an active material; and an active material layer forming step of forming an active material layer including the second composite by dry deposition method.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing an electrode. [Background technology]

[0002] As a method for producing an electrode for a battery, a method in which an active material layer is formed on a substrate using a composite electrode material is known. Also, a dry film formation method is known as a method for forming an active material layer.

[0003] For example, Patent Document 1 discloses a dry film formation method in which an electrostatic film is formed using electrode particles that are composites of electrode materials. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2022-142813 A Summary of the Invention [Problem to be solved by the invention]

[0005] From the viewpoint of improving the performance of a battery, it is preferable that the electrode resistance is suppressed. The present disclosure has been made in view of the above-mentioned circumstances, and has a main object to provide a method for manufacturing an electrode having suppressed resistance. [Means for solving the problem]

[0006] [1] The method for manufacturing an electrode includes a first combining step of combining a binder and a conductive assistant to obtain a first composite, a second combining step of combining the first composite with an active material to obtain a second composite, and an active material layer forming step of forming an active material layer containing the second composite on a substrate by a dry film formation method. Effect of the Invention

[0007] The present disclosure provides an advantage in that an electrode with reduced resistance can be manufactured. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a flow diagram illustrating a method for manufacturing an electrode in the present disclosure. [Diagram 2] 1 is a graph showing SEM images and coverage results of evaluation samples obtained in Examples. [Diagram 3] 1 is a graph showing the volume resistivity of evaluation samples obtained in Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The method for producing an electrode according to the present disclosure will be described in detail below.

[0010] Fig. 1 is a flow diagram illustrating a method for producing an electrode according to the present disclosure. As shown in Fig. 1, in the method for producing an electrode according to the present disclosure, first, a binder and a conductive assistant are compounded to obtain a first composite (first compounding step). Next, the first composite and an active material are compounded to obtain a second composite (second compounding step). Then, an active material layer containing the second composite is formed on a substrate by a dry film formation method (active material layer forming step).

[0011] According to the present disclosure, a binder and a conductive assistant are first compounded, and then an active material is compounded to produce a second composite, and an active material layer is then formed using the second composite, thereby making it possible to manufacture an electrode with reduced resistance.

[0012] In the electrode, it is assumed that a binder and a conductive assistant having a smaller average particle size than the active material are used. In such a case, if each material is compounded at once, it is difficult to uniformly disperse the binder and the conductive assistant on the surface of the active material. In particular, if each material is compounded in a powder state, it is even more difficult to uniformly disperse them. In that case, the conductive assistant and the binder may be unevenly arranged on the surface of the active material, and as a result, the electronic conductivity may decrease and the resistance of the electrode may increase. In contrast, according to the present disclosure, the conductive assistant and the binder are compounded in advance, that is, after the conductive assistant and the binder are crushed in advance, they are compounded with the active material, so that a second composite in which the conductive assistant and the binder are uniformly dispersed on the surface of the active material can be obtained. By using such a second composite, it is possible to suppress the decrease in electronic conductivity and suppress the resistance of the electrode.

[0013] 1.First composite process The first composite step in the present disclosure is a step of compositely combining the binder and the conductive assistant to obtain a first composite.

[0014] Examples of the binder include rubber-based binders such as butylene rubber (BR) and styrene butadiene rubber (SBR), and fluoride-based binders such as polyvinylidene fluoride (PVDF).

[0015] The conductive assistant may be, for example, a carbon material, such as acetylene black (AB) or ketjen black (KB).

[0016] As a method for compounding the binder and the conductive assistant, for example, a method of applying mechanical energy such as compressive force, shear force, and friction force to the binder and the conductive assistant using a mixing device can be mentioned. As the mixing device, for example, a mixer such as a planetary mixer can be used. In this way, a first composite in which the binder and the conductive assistant are physically bonded can be obtained.

[0017] In addition, in the first complexing step, when the binder is 100 parts by weight, the proportion (weight ratio) of the conductive aid is, for example, 90 parts by weight or more and 160 parts by weight or less.

[0018] The shape of the first complex is not particularly limited, and for example, a particulate shape can be mentioned.

[0019] 2. Second complexing step The second complexing step in the present disclosure is a step of complexing the above-described first complex and the active material to obtain a second complex. The first complex is as described above.

[0020] The active material may be a positive electrode active material or a negative electrode active material. Examples of the positive electrode active material include an oxide active material and a sulfur-based active material. Examples of the oxide active material include LiCoO 2 , LiMnO 2 , LiNiO 2 , LiVO 2 , LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 and other rock salt layer-type active materials such as LiMn 2 O 4 , Li 4 Ti 5 O 12 , Li(Ni 0.5 Mn 1.5 )O 4 and other spinel-type active materials such as LiFePO 4 , LiMnPO 4 , LiNiPO 4 , LiCoPO 4 and other olivine-type active materials. Further, as the oxide active material, Li 1+x Mn 2-x-y MyO 4 (M is at least one of Al, Mg, Co, Fe, Ni, Zn, 0 < x + y < 2) represented by the LiMn spinel active material, lithium titanate, etc. may also be used.

[0021] Examples of the negative electrode active material include carbon active material, oxide active material, and metal active material. Examples of the carbon active material include mesocarbon microbeads (MCMB), highly oriented graphite (HOPG), hard carbon, and soft carbon. Examples of the oxide active material include NB 2 O 5 , Li 4 Ti 5 O 12 and SiO. Metal active materials include, for example, In, Al, Si, and Sn.

[0022] The active material is, for example, in the form of particles. The average particle diameter (D 50 ) is, for example, 1 nm or more and 10 μm or less. 50 ) refers to the cumulative 50% particle size in the volume-based particle size distribution measured by a laser diffraction particle size distribution analyzer. Here, the active material may be either primary particles or secondary particles formed by aggregation of primary particles. In other words, the above-mentioned average particle size (D 50 ) may be the average particle size of primary particles or the average particle size of secondary particles.

[0023] In addition, the active material may be particles having a single crystal orientation (single crystal particles) or particles having two or more types of crystal orientations within one particle (twin crystal particles), with the former being preferred.

[0024] The method for compounding the first composite and the active material is the same as that in the first compounding step described above, and therefore the description thereof will be omitted here. In the second compounding step, the ratio (weight ratio) of the active material when the total of the first composite and the active material is 100 parts by weight is, for example, 70 parts by weight or more and 99 parts by weight or less.

[0025] In the second composite, the first composite (binder and conductive additive) is present (bound) on the surface of the active material. In other words, the second composite can be considered as a coated active material in which at least a part of the surface of the active material is coated with the first composite.

[0026] The coverage in the second composite (coated active material) may be, for example, 100%, or less than 100%. In the latter case, the coverage is, for example, 78% or more, 80% or more, or 85% or less. On the other hand, the coverage is, for example, 99% or less, 95% or less, or 90% or less. The coverage can be determined by microscopic observation using, for example, a scanning electron microscope (SEM) or the like.

[0027] The thickness of the coating in the second composite (coated active material) is, for example, 1 nm or more and 500 nm or less. The thickness of the coating can be determined, for example, by the above-mentioned microscope observation.

[0028] The shape of the second complex is not particularly limited, but may be, for example, particulate. The average particle size (D 50 ) is, for example, 5 nm or more and 20 μm or less. Furthermore, the average particle size of the second composite may be the average particle size of the primary particles, or may be the average particle size of the secondary particles.

[0029] 3. Active material layer formation process The active material layer forming step in the present disclosure is a step of forming an active material layer containing the second composite on a substrate by a dry film forming method. The second composite is as described above.

[0030] Examples of the dry film forming method include conventionally known methods. Specifically, a method of forming an active material layer by depositing a powder composition containing the second complex on a substrate can be mentioned. The powder composition may contain only the second complex, or may contain other materials. Examples of other materials include solid electrolytes. Examples of solid electrolytes include inorganic solid electrolytes such as sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and halide solid electrolytes.

[0031] The substrate may be, for example, a member used as a current collector of a battery, or a member used as a transfer substrate for transferring an active material layer. Examples of the substrate include metal foils such as Al, SUS, Cu, and Ni.

[0032] The active material layer may be a positive electrode active material layer or a negative electrode active material layer, and the thickness of the active material layer is, for example, 0.1 μm or more and 1000 μm or less.

[0033] 4. Electrode The electrodes in the present disclosure are generally used in batteries. The battery has a positive electrode having a positive electrode current collector and a positive electrode active material layer, a negative electrode having a negative electrode current collector and a negative electrode active material layer, and an electrolyte layer disposed between the positive electrode active material layer and the negative electrode active material layer, and either the positive electrode or the negative electrode is an electrode manufactured by the above-mentioned method. The type of battery is preferably a lithium ion battery. The battery is preferably a solid battery containing a solid electrolyte as an electrolyte. Examples of applications of the battery include power sources for vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), electric vehicles (BEVs), gasoline vehicles, and diesel vehicles. In particular, it is preferable to use the battery as a driving power source for hybrid electric vehicles, plug-in hybrid electric vehicles, or electric vehicles. The battery in the present disclosure may also be used as a power source for moving objects other than vehicles (for example, railways, ships, and aircraft), and may also be used as a power source for electrical products such as information processing devices.

[0034] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES

[0035] [Example] The positive electrode active material was nickel cobalt manganese oxide lithium (NCM) manufactured by Hunan Ruixiang Co., Ltd., the conductive additive was acetylene black (Li-435) manufactured by Denka Co., Ltd., and the binder was PVdF (LBG8200) manufactured by Arkema Co., Ltd. These were weighed at a weight ratio (weight%) of positive electrode active material: conductive additive: binder = 97.5: 1.5: 1. The weighed binder and conductive additive were introduced into an MP mixer (spherical tank) manufactured by Nippon Coke & Engineering Co., Ltd., and compounded at 10,000 rpm for 10 minutes. This resulted in a first composite (first compounding step). Thereafter, the positive electrode active material was introduced into the MP mixer, and further compounded at 10,000 rpm for 10 minutes (second compounding step). This resulted in an evaluation sample (second composite).

[0036] [Comparative Example] The positive electrode active material, the conductive assistant, and the binder, weighed in the same proportions as in the examples, were introduced into an MP mixer and subjected to a composite treatment at 10,000 rpm for 10 minutes, thereby obtaining an evaluation sample.

[0037] [evaluation] (Coverage rate) Each evaluation sample of the examples and comparative examples was observed with a scanning electron microscope (SEM) to calculate the coverage of the positive electrode active material. The SEM image of the example is shown in Figure 2(a), and the coverage is shown in Figure 2(b).

[0038] (Volume resistivity) The volume resistivity of each evaluation sample of the examples and comparative examples was measured. For the measurement, an automatic powder resistivity measuring system (MCP-PD600) manufactured by Nitto Seiko Anateric Co., Ltd. was used. The weight of each evaluation sample was 2 g, and the pressure during measurement was 20 kN. The results are shown in FIG. 3.

[0039] 2(a) and (b), in the evaluation sample of the example, the first composite (composite of the binder and the conductive additive) was well arranged on the surface of the positive electrode active material, and the coverage was also better than that of the evaluation sample of the comparative example. In this way, by previously combining the binder and the conductive additive, the conductive additive can be well attached to the active material surface, and re-agglomeration is prevented, and as a result, it was confirmed that the dispersibility of the conductive additive on the active material surface is improved.

[0040] In addition, as shown in Figure 3, the evaluation sample of the Example had a significantly lower volume resistivity than the evaluation sample of the Comparative Example. This is presumably because, as shown in Figures 2(a) and (b), in the Example, the conductive additive was able to adhere well to the active material surface, and the coverage rate by the first complex was improved, resulting in a good electron conduction path. In this way, it was confirmed that the resistance of the electrode manufactured by the method of the present disclosure was suppressed.

Claims

[Claim 1] a first composite step of compositely combining the binder and the conductive assistant to obtain a first composite; a second composite step of compositely forming a second composite by compositely forming the first composite and an active material; and forming an active material layer comprising the second composite on a substrate by a dry film-forming method.

Citation Information

Patent Citations

  • Electrostatic film forming apparatus and electrostatic film forming method

    JP2022142813A

Cited By

  • Game machine

    JP2024166283A

  • Game machine

    JP2024166284A

  • Game machine

    JP2024169547A

  • Game machine

    JP2024169551A