Laminate and sanitary article including laminate

The laminate addresses the balance of waterproofness and breathability in diapers by using a polyurethane resin layer and nonwoven fabric layer, ensuring effective leakage prevention and comfort with reduced material usage and environmental footprint.

JP2024154760AInactive Publication Date: 2024-10-31NITTO DENKO CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023068789
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Disposable diapers face challenges in achieving a balance between waterproofness and breathability, leading to discomfort and potential leakage issues, while also requiring improved tactile sensation and fit for wearers.

Method used

A laminate comprising a polyurethane resin layer with a thickness of 5 μm to 15 μm and a nonwoven fabric layer, with a water vapor permeability of 1500 g/(m²·day) or more, and a stretch recovery rate of 10% or less, enhancing both waterproofness and breathability, and providing excellent elastic recovery properties.

Benefits of technology

The laminate offers improved fit and comfort by reducing leakage and enhancing tactile sensation, while also allowing for reduced material usage and environmental impact through thinner layers and efficient manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154760000001_ABST
    Figure 2024154760000001_ABST
Patent Text Reader

Abstract

To provide a laminate having excellent waterproofness and air permeability while having excellent expansion recoverability.SOLUTION: A laminate includes a nonwoven fabric layer of fibers and a polyurethane resin layer with thickness 5 to 15 μm, inclusive. A sanitary article includes the laminate.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate and to a sanitary article comprising said laminate. [Background technology]

[0002] Disposable diapers are used not only by infants but also by adults, and the demand for them is increasing. Disposable diapers are required to suppress leakage of excrement discharged from the body and to provide a comfortable feel for the wearer. In order to suppress leakage, openings around the legs and waist are required to fit the body. In addition, highly waterproof materials are used as components that make up disposable diapers. On the other hand, if the diaper is only highly waterproof, the inside may become steamy, causing rashes and itching in the wearer, or may produce a foul odor. For this reason, materials that are waterproof and breathable are used for disposable diapers (for example, Patent Document 1). On the other hand, materials that are waterproof and breathable may be unpleasant to the touch, resulting in a disposable diaper that feels like paper. Disposable diapers that are not only waterproof and breathable but also pleasant to the touch and excellent in feel are required. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2023-44181 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention has been made to solve the above-mentioned problems in the conventional art, and an object of the present invention is to provide a laminate having excellent waterproofness and breathability, and also having excellent stretch recovery properties. [Means for solving the problem]

[0005] 1. The laminate of an embodiment of the present invention has a fibrous nonwoven fabric layer and a polyurethane resin layer having a thickness of 5 μm or more and 15 μm or less. 2. The water vapor permeability of the laminate described in 1 above is 1500 g / (m 2 10 days) or more. 3. The laminate described in 1 or 2 above is stretched 100% under conditions of a temperature of 23°C, a chuck distance of 50 mm, and a tensile speed of 300 mm / min, fixed in the stretched state and held for 1 minute, and then released from the stretched state. The rate of variation (%) = [{(B) - (A)} / (A)] × 100 calculated from the initial chuck distance (A) (mm) and the length of the laminate after the test (B) (mm) may be 10% or less. 4. In the laminate according to any one of the above items 1 to 3, the nonwoven fabric layer may be a nonwoven fabric that stretches by 50% or more in the CD direction. 5. The laminate according to any one of the above items 1 to 4 may be a laminate in which the nonwoven fabric layer and the polyurethane resin layer are extrusion laminated. 6. The laminate according to any one of the above items 1 to 4 may be a laminate in which the nonwoven fabric layer and the polyurethane resin layer are laminated via a pressure-sensitive adhesive layer. 7. The laminate according to the above item 6 may be such that the pressure-sensitive adhesive layer is formed on the entire surface of at least one of the nonwoven fabric layer and the polyurethane resin layer. 8. The laminate according to the above item 6 may be such that the pressure-sensitive adhesive layer is intermittently formed on the surface of at least one of the nonwoven fabric layer and the polyurethane resin layer. 9. In the laminate according to any one of the above items 1 to 8, the nonwoven fabric layer may be a nonwoven fabric made of olefin-based fibers. 10. In another aspect of the present invention, a sanitary product is provided. The sanitary product comprises the laminate according to any one of 1 to 9 above. Effect of the Invention

[0006] According to an embodiment of the present invention, a laminate having excellent waterproofness and breathability, as well as excellent stretch recovery properties, can be provided. [Brief description of the drawings]

[0007] [Figure 1] 1 is a schematic cross-sectional view of a laminate according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] A. Overall structure of the laminate FIG. 1 is a schematic cross-sectional view of a laminate according to an embodiment of the present invention. The laminate 100 according to an embodiment of the present invention has a polyurethane resin layer 10 and a fibrous nonwoven fabric layer (hereinafter also referred to as a nonwoven fabric layer) 20. The thickness of the polyurethane resin layer is 5 μm or more and 15 μm or less. In the illustrated example, the nonwoven fabric layer is laminated only on one side of the polyurethane resin layer, but the nonwoven fabric layer may be laminated on both sides of the polyurethane resin layer. Members used in sanitary products such as disposable diapers, particularly members used in backsheets, are required to have waterproofness and breathability. However, laminates with excellent waterproofness and breathability may have a poor feel and may not provide a satisfactory tactile sensation. The laminate according to an embodiment of the present invention has a polyurethane resin layer with a thickness of 5 μm or more and 15 μm or less and a nonwoven fabric layer. A laminate having a thin polyurethane resin layer as described above not only has excellent waterproofness and breathability, but also has excellent stretch recovery. If the laminate of the embodiment of the present invention is applied to a disposable diaper, for example, not only can the laminate have excellent waterproofness and breathability, but also a good fit to the body, and leakage from the leg and waist areas can be suppressed. In addition, the feel of the disposable diaper can be improved. Since disposable diapers are required to fit the body, many sizes are available, and a large space may be required for storage at retail stores, hospitals, nurseries, kindergartens, etc. If the laminate of the embodiment of the present invention is used, the stretchability of the disposable diaper can be improved, and even if only a few sizes are available, the disposable diaper can be appropriately fitted to many body types. In addition, the thickness of the polyurethane resin layer used in the laminate is thin, and the plastic material used in the laminate can be reduced, and the disposable diaper itself using the laminate can be made smaller. As a result, the amount of plastic used can be reduced, which can contribute to reducing the environmental load.

[0009] The polyurethane resin layer 10 and the nonwoven fabric layer 20 may be laminated directly, that is, without any adhesive layer, or may be laminated via any suitable adhesive layer (not shown). The adhesive layer may be an adhesive layer or a pressure-sensitive adhesive layer. The adhesive layer is preferably a pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer may be formed on the entire surface of at least one of the polyurethane resin layer 10 and the nonwoven fabric layer 20, and may be formed intermittently, for example, in a stripe shape, a dot shape, or the like. Preferably, the polyurethane resin layer 10 and the nonwoven fabric layer 20 are directly laminated. If the laminate is directly laminated, the breathability can be further improved.

[0010] The laminate preferably has a water vapor transmission rate of 1500 g / (m 2 ·day) or more, and more preferably 1800g / (m 2 ·day) or more, and more preferably 2000g / (m 2 ·day) or more, and particularly preferably 2500g / (m 2 ·day) or more. If the water vapor permeability is within the above range, a laminate having excellent breathability can be obtained. The higher the water vapor permeability, the more preferable it is. In this specification, the water vapor permeability of the laminate refers to a value measured using a sample of 8 mm × 8 mm at a temperature of 23°C and a humidity of 100% RH in accordance with ISO15106-1.

[0011] The laminate is stretched 100% under the conditions of a temperature of 23°C, a chuck distance of 50 mm, and a tensile speed of 300 mm / min, fixed in the stretched state and held for 1 minute, and then released from the stretched state. The fluctuation rate (%) calculated from the initial chuck distance (A) (mm) and the length (B) (mm) of the laminate after the test = [{(B)-(A)} / (A)] x 100 (hereinafter also referred to as stretch recovery rate) is preferably 10% or less, more preferably 8% or less, even more preferably 6% or less, and particularly preferably 5% or less. If the stretch recovery rate is within the above range, the stretch recovery rate can be excellent. The fluctuation rate is, for example, 2% or more.

[0012] The laminate may be decorated with any suitable decoration. For example, the polyurethane resin layer and / or the nonwoven fabric layer may be colored, or may have any suitable printed portion.

[0013] B. Polyurethane resin layer The polyurethane resin layer is a layer having a thickness of 5 μm or more and 15 μm or less. If the thickness of the polyurethane resin layer is in the above range, a laminate having not only excellent waterproofness and breathability but also excellent stretch recovery can be obtained. Furthermore, even if the thickness of the polyurethane resin layer is in the above range, the polyurethane resin layer has excellent strength, and even if the laminate is stretched, the laminate can be prevented from breaking. If the thickness of the polyurethane resin layer exceeds 15 μm, the breathability can be reduced and the touch can be deteriorated. In addition, this can lead to an increase in material costs, and the environmental load due to the increase in materials used (e.g., plastic materials) can also be increased. The thickness of the polyurethane resin layer is preferably 5 μm to 12 μm, more preferably 5 μm to 10 μm. In one embodiment, the thickness of the polyurethane resin layer is 5 μm or more. In addition, the thickness of the polyurethane resin layer is 15 μm or less, preferably 12 μm or less, more preferably 10 μm or less. The polyurethane resin layer may be a single layer or a laminate of two or more layers.

[0014] B-1.Polyurethane resin Any suitable polyurethane resin may be used as the polyurethane resin. The polyurethane has a soft segment phase and a hard segment phase. The soft segment phase is formed by a high molecular weight polyol compound, and the hard segment phase can be formed by the reaction of a low molecular weight diol compound and an organic diisocyanate compound.

[0015] The high molecular weight polyol compound is, for example, a diol compound having a weight average molecular weight of 500 to 6000. Any appropriate diol can be used as the high molecular weight polyol compound. Examples include polyester diol, polyether diol, polycarbonate diol, and co-condensation products thereof (for example, polyester ether diol). The high molecular weight polyol compound can be obtained, for example, by addition polymerization of alkylene oxides such as propylene oxide and ethylene oxide to low molecular weight compounds having two or more hydroxyl groups in the molecule such as glycol and glycerin, or by condensation of dibasic acids such as adipic acid and polyhydric alcohols such as ethylene glycol. The high molecular weight polyol compound may be one type only or two or more types.

[0016] As the polyester diol, any suitable polyester diol can be used. Preferably, saturated polyester diols obtained from diol compounds of alkane having 2 to 10 carbon atoms, such as propylene glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 2-methylpropanediol, and aliphatic or aromatic dicarboxylic acids having 4 to 12 carbon atoms, such as glutaric acid, adipic acid, pimelic acid, suberic acid, sebacic acid, terephthalic acid, isophthalic acid, and polylactone diols, such as polycaprolactone glycol and polyvalerolactone glycol, are used.

[0017] As the polyether diol, any suitable polyether diol can be used, and preferably, a polyalkylene ether diol such as polyethylene ether glycol, polypropylene ether glycol, polytetramethylene ether glycol, or polyhexamethylene ether glycol is used.

[0018] The low molecular weight diol compound is, for example, a diol compound having a weight average molecular weight of less than 500. Any suitable diol compound can be used as the low molecular weight diol compound. Examples of the diol compound include aliphatic or aromatic diols such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentane glycol, 3-methylpentane glycol, 1,6-hexanediol, and 1,4-bishydroxyethylbenzene. The low molecular weight diol compound may be used alone or in combination of two or more.

[0019] As the organic diisocyanate compound, any appropriate diisocyanate compound can be used. For example, aliphatic or aromatic diisocyanate compounds such as 4,4'-diphenylmethane diisocyanate, tolylene diisocyanate, isophorone diisocyanate, hydrogenated diphenylmethane diisocyanate, xylylene diisocyanate, 2,6-diisocyanate methyl caproate, and hexamethylene diisocyanate can be used. Only one type of organic diisocyanate compound can be used, or two or more types can be used in combination.

[0020] The polymerization of polyurethane resin may contain any suitable additive. For example, hindered phenol and amine antioxidants, benzotriazole and hindered amine UV absorbers, smoothing agents such as amide wax and montanic acid wax, hydrolysis inhibitors such as carbodiimide compounds, pigments such as titanium oxide and red iron oxide, and polymer additives such as gas yellowing inhibitors may be used alone or in combination of two or more.

[0021] The polyurethane resin can be obtained by polymerizing the high molecular weight polyol compound, the low molecular weight diol compound, the organic diisocyanate compound, and, if necessary, any other suitable monomer components and any suitable additives by any suitable method, such as a continuous melt polymerization method, a kneader method, a vat cure method, a belt method, etc.

[0022] As the polyurethane resin, commercially available products may be used, for example, trade names "Elastollan E SP806", "Elastollan E 1170 A", "Elastollan E 1385 A" and the like manufactured by BASF.

[0023] B-2. Filler The polyurethane resin layer may further contain a filler. If the polyurethane resin layer further contains a filler, the breathability of the laminate may be further improved. Any suitable filler may be used as the filler. Specifically, inorganic particles and organic particles may be used. Examples of inorganic particles include talc, titanium oxide, calcium oxide, magnesium oxide, zinc oxide, titanium oxide, calcium carbonate, silica, clay, mica, barium sulfate, whiskers, magnesium hydroxide, and the like. Examples of organic particles include acrylic beads, styrene beads, silicone resin particles, and the like. Only one type of filler may be used, or two or more types may be used in combination.

[0024] The average particle size of the filler may be any appropriate average particle size. The average particle size of the filler is preferably 0.5 μm or more, more preferably 0.6 μm or more, and even more preferably 0.7 μm or more. The average particle size of the filler is preferably 50 μm or less, more preferably 30 μm or less, even more preferably 10 μm or less, and particularly preferably 5 μm or less. In one embodiment, the average particle size of the filler is preferably 0.5 μm to 50 μm, more preferably 0.6 μm to 30 μm, even more preferably 0.7 μm to 10 μm, and particularly preferably 0.7 μm to 5 μm. When the average particle size of the filler is within the above range, the breathability of the laminate can be further improved.

[0025] The filler may be used in any suitable content. The content of the filler is preferably 50 parts by weight or more, more preferably 70 parts by weight or more, and even more preferably 100 parts by weight or more, relative to 100 parts by weight of the polyurethane resin contained in the composition forming the polyurethane resin layer. The content of the filler is preferably 400 parts by weight or less, more preferably 350 parts by weight or less, and even more preferably 300 parts by weight or less. In one embodiment, the content of the filler is preferably 50 parts by weight to 400 parts by weight, more preferably 70 parts by weight to 350 parts by weight, and even more preferably 100 parts by weight to 300 parts by weight, relative to 100 parts by weight of the polyurethane resin. If the content of the filler is within the above range, the breathability of the laminate can be further improved.

[0026] The filler may be coated with a release agent. Any suitable release agent may be used as the release agent. Examples of the release agent include fatty acid amide-based release agents, silicone-based release agents, fluorine-based release agents, and long-chain alkyl-based release agents. The release agent may be used in any suitable amount.

[0027] B-3. ​​Other additives The polyurethane resin layer may further contain any other appropriate additive. Examples of the other additives include ultraviolet absorbers, heat stabilizers, release agents, lubricants, colorants such as dyes, antioxidants, eye plug inhibitors, antiblocking agents, foaming agents, other polymers, tackifiers, plasticizers, deterioration inhibitors, antistatic agents, light stabilizers, etc. The other additives may be used alone or in combination of two or more. The other additives are used in any appropriate content.

[0028] In one embodiment, a commercially available polyurethane film may be used as the polyurethane resin layer. Examples include "SMF-10" manufactured by Seiren Co., Ltd. and "TX2060" manufactured by Argotec Co., Ltd. In addition, examples of commercially available products in which a pressure-sensitive adhesive is laminated on a polyurethane resin layer include "Permiroll Light" manufactured by Nitto Denko Corporation.

[0029] C. A nonwoven layer of fiber Any suitable nonwoven fabric is used as the nonwoven fabric layer of the fibers. The nonwoven fabric layer may be a single layer of nonwoven fabric or a laminate of two or more nonwoven fabrics. The nonwoven fabric is preferably a nonwoven fabric that stretches 50% or more in the CD direction. That is, the flow direction during the production of the nonwoven fabric is the MD direction, and the direction perpendicular to the MD direction is the CD direction. The nonwoven fabric is cut into a length of 50 mm in the longitudinal direction as a sample, and set in a tensile tester (e.g., Shimadzu Corporation, product name "AG-20kNG") with a chuck distance of 50 mm and stretched in the CD direction at a tensile speed of 300 mm / min under the condition of 100% stretching. When the value calculated from the formula (length in the CD direction of the nonwoven fabric after stretching (mm) - length in the CD direction of the nonwoven fabric before stretching (mm)) / length in the CD direction of the nonwoven fabric before stretching (mm) x 100 (%) is 50%, the nonwoven fabric has a strength of 10 N / 50 mm or less. If the strength of the nonwoven fabric when stretched 50% in the CD direction is 10 N / 50 mm or less, the nonwoven fabric layer can follow the elastic recovery of the polyurethane resin layer, and the elastic recovery of the laminate can be improved.

[0030] Examples of fibrous nonwoven fabrics include spunbond nonwoven fabrics, thermal bond nonwoven fabrics, point bond nonwoven fabrics, spunlace nonwoven fabrics, air-through nonwoven fabrics, melt-blown nonwoven fabrics, spunlace nonwoven fabrics, spunbond melt-blown spunbond nonwoven fabrics, spunbond melt-blown spunbond nonwoven fabrics, non-bonded nonwoven fabrics, electrospun nonwoven fabrics, carded nonwoven fabrics, etc. Preferred are nonwoven fabrics that can be stretched in the CD direction, such as spunlace nonwoven fabrics, air-through nonwoven fabrics, melt-blown nonwoven fabrics, and carded nonwoven fabrics.

[0031] Any suitable fibers may be used as the fibers constituting the nonwoven fabric. For example, fibers of olefins such as polypropylene and polyethylene, polyester, polyamide, polyurethane, elastomer, rayon, cellulose, acrylic, copolymers thereof, or mixtures thereof may be used. Olefin-based fibers are preferred, and polypropylene fibers and polyethylene fibers are preferred in terms of cost. Core-sheath fibers of polyester and olefin resin may also be used.

[0032] Examples of the olefin-based fibers include polypropylene fibers, polyethylene fibers, α-olefin copolymer fibers, etc. Preferred examples of the olefin-based fibers include polypropylene fibers and polyethylene fibers.

[0033] The fibers constituting the nonwoven fabric may further contain any appropriate other components. Examples of the other components include other polymers, tackifiers, plasticizers, antidegradants, pigments, dyes, antioxidants, antistatic agents, lubricants, foaming agents, heat stabilizers, light stabilizers, inorganic fillers, and organic fillers. The other components may be used alone or in combination of two or more. The content ratio of the other components in the fibers constituting the nonwoven fabric may be set to any appropriate amount.

[0034] The density of the nonwoven fabric may be set to any suitable value. The density of the nonwoven fabric is preferably 0.90 kg / m 3 ~0.99kg / m 3 and more preferably 0.92 kg / m 3 ~0.98kg / m 3 and more preferably 0.93 kg / m 3 ~0.98kg / m 3 In one embodiment, the density of the nonwoven fabric is preferably 0.90 kg / m 3 More preferably, it is 0.92 kg / m or more. 3 More preferably, it is 0.93 kg / m or more. 3 The density of the nonwoven fabric is preferably 0.99 kg / m 3More preferably, it is 0.98 kg / m or less. 3 More preferably, it is 0.98 kg / m or less. 3 If the density of the nonwoven fabric is within the above range, a laminate having an excellent feel can be provided. In this specification, the density of the nonwoven fabric (kg / m 3 ) is the basis weight of the nonwoven fabric (Xg / m 2 ) and the thickness of the nonwoven fabric (Ymm) measured by the following method. 3 ) is X / Y(kg / m 3 ) <Thickness of nonwoven fabric> Using a digital microscope (for example, Keyence's product name "VHX-1000"), the cross section of the nonwoven fabric is photographed at a magnification of 100x, and the thickness of the nonwoven fabric is measured using the image analysis software of the same machine. In the thickness measurement, the parallel lines at the top and bottom of the nonwoven fabric cross section that intersect with the fibers at 10 points are defined as the upper and lower sides, respectively, and the length between the upper and lower sides is defined as the thickness of the nonwoven fabric.

[0035] The basis weight of the nonwoven fabric is preferably 0.15 g / m 2 ~0.40g / m 2 and more preferably 0.15 g / m 2 ~0.35g / m 2 and more preferably 0.15 g / m 2 ~0.30g / m 2 In one embodiment, the basis weight of the nonwoven fabric is preferably 0.15 g / m 2 The basis weight of the nonwoven fabric is preferably 0.40 g / m 2 More preferably, it is 0.35 g / m or less. 2 More preferably, it is 0.30 g / m or less. 2 When the basis weight of the nonwoven fabric is within the above range, the feel of the laminate can be further improved. The basis weight of the nonwoven fabric can be measured by any appropriate method. For example, it can be measured by the following method. 2 The weight of the cut sample was measured using an electronic balance and the g / m 2The basis weight of a nonwoven fabric can be measured by converting it into units (gsm).

[0036] D. Manufacturing method of laminate The laminate of the embodiment of the present invention can be manufactured by any suitable method. For example, it can be manufactured by preparing a resin film that will be a polyurethane resin layer and laminating it with a fiber nonwoven fabric layer by any suitable method. When laminating a resin film that will be a polyurethane resin layer and a nonwoven fabric, for example, they can be laminated via a pressure-sensitive adhesive layer. Any suitable pressure-sensitive adhesive can be used as the pressure-sensitive adhesive that forms the pressure-sensitive adhesive layer. For example, acrylic pressure-sensitive adhesives and hot melt pressure-sensitive adhesives can be mentioned. The pressure-sensitive adhesive can be formed on the surface (one side surface) of at least one of the resin film and the nonwoven fabric. The pressure-sensitive adhesive layer may be formed on the entire surface of the resin film or nonwoven fabric on which the pressure-sensitive adhesive layer is formed, or may be formed intermittently, for example, in a stripe shape or a dot shape. Preferably, the pressure-sensitive adhesive layer is an intermittent layer. If the pressure-sensitive adhesive layer is an intermittent layer, the breathability of the obtained laminate can be improved.

[0037] The adhesive layer can be formed by applying the adhesive by any suitable method, for example, by applying the adhesive solidly to the resin film or nonwoven fabric, or by intermittently applying the adhesive by spray coating.

[0038] The laminate may be produced by extruding the composition forming the polyurethane resin layer directly onto the fiber nonwoven fabric from the die of the extruder and extrusion lamination. By producing the laminate by extrusion lamination, the breathability of the laminate may be further improved. In addition, the process from the preparation of the composition to the production of the laminate may be performed continuously, and the production efficiency may be improved. More specifically, the composition forming the polyurethane resin layer may be extruded from the T-die of the extruder, and a laminate of the nonwoven fabric and the polyurethane resin layer may be molded to produce the laminate. The extrusion temperature of the composition forming the polyurethane resin layer is preferably 180°C to 250°C, more preferably 180°C to 230°C, and even more preferably 200°C to 230°C. In one embodiment, the extrusion temperature is preferably 180°C or higher, more preferably 200°C or higher. In addition, the extrusion temperature is preferably 250°C or lower, and more preferably 230°C or lower. When performing direct extrusion lamination with the nonwoven fabric, if it is within the above range, the adhesion of the laminate may be further improved.

[0039] The laminate of the embodiment of the present invention can have high breathability without undergoing a pre-stretching process. For example, a laminate including a resin layer formed of an olefin resin can have improved breathability by pre-stretching the resin layer. On the other hand, the strength of the resin layer that has undergone pre-stretching may decrease, and the handleability of the resin layer may decrease in the manufacturing process of the laminate after pre-stretching. In the laminate of the embodiment of the present invention, the polyurethane resin layer exhibits excellent breathability and may also be excellent in strength even without pre-stretching. Therefore, manufacturing processes such as pre-stretching are omitted, and manufacturing efficiency may be improved. In addition, a laminate having excellent waterproofness and breathability may be manufactured without reducing yield. Furthermore, for example, when used in a disposable diaper, the laminate may be prevented from breaking when stretched during wearing or the like.

[0040] E. Applications of laminates The laminate of the embodiment of the present invention can be used for any suitable application. In one embodiment, the laminate of the embodiment of the present invention can be suitably used for sanitary products. Examples of sanitary products include disposable diapers. A disposable diaper typically includes a top sheet that contacts the wearer's body, a back sheet that is the outer side of the disposable diaper, and an absorbent disposed between the top sheet and the back sheet. The laminate of the embodiment of the present invention is preferably used for a back sheet. As described above, the laminate of the embodiment of the present invention has excellent waterproofness and breathability, and can have excellent stretch recovery. If the laminate of the embodiment of the present invention is used as a back sheet, a disposable diaper that suppresses leakage of excrement and the like and fits the wearer better can be provided. In addition, the tactile feel of the disposable diaper can be improved, and a disposable diaper that is more pleasant to the touch can be provided. Furthermore, a disposable diaper that has excellent stretch recovery and can fit a wider range of body types can be provided. As a result, a larger number of body types can be accommodated with a smaller number of sizes, and space saving during storage can be achieved. EXAMPLES

[0041] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples, "parts" and "%" are by weight unless otherwise specified.

[0042] [Example 1] A polyurethane film with an adhesive layer (manufactured by Nitto Denko Corporation, product name "Permiroll Light", urethane film thickness 8 μm, adhesive layer thickness 25 μm) and a carded type nonwoven fabric of propylene (PP) resin fiber (manufactured by Nitto Denko Corporation, product name "Thermostrain 22 HI", basis weight 22 g / m 2 ) was attached to the polyurethane film with the pressure-sensitive adhesive layer via the pressure-sensitive adhesive layer using a hand roller to obtain a laminate.

[0043] [Example 2] Pellets of urethane resin A (manufactured by BASF, product name "Elastran E SP806") were thoroughly dried, and an 8 μm-thick polyurethane resin layer was melt-extruded in an extruder. The extruded PP resin fiber was then made into a carded-type nonwoven fabric (manufactured by Nitto Denko Corporation, product name "Thermostrain 22 HI", basis weight 22 g / m 2 The polyurethane resin layer immediately after extrusion was brought into contact with the laminated sheet 14 and extrusion lamination was carried out to obtain a laminate.

[0044] [Example 3] A laminate was obtained in the same manner as in Example 2, except that the thickness of the polyurethane resin layer was 15 μm.

[0045] [Example 4] A laminate was obtained in the same manner as in Example 2, except that urethane resin A was replaced with polyurethane resin B (manufactured by BASF under the trade name "Elastollan E 1385A").

[0046] [Example 5] Carded type nonwoven fabric made of PP resin fiber (manufactured by Nitto Denko Corporation, product name "Thermostrain 22 HI", basis weight 22g / m 2 ) was coated with a hot melt adhesive (manufactured by Nitto Denko Corporation, product name "Olefin-based hot melt adhesive AC600") at a rate of 8 g / m 2 and a polyurethane resin layer was extruded onto the surface onto which the hot melt adhesive had been sprayed, in the same manner as in Example 4 to obtain a laminate.

[0047] Comparative Example 1 Linear low-density polyethylene (Prime Polymer Co., Ltd., product name "Ultxex 2022L", density 0.919 g / cm 3 A mixture of 63 parts by weight of ethylene-propylene terpolymer (manufactured by Mitsui Chemicals, Inc., product name "K-9720"), 77 parts by weight of ethylene-propylene terpolymer (manufactured by Mitsui Chemicals, Inc., product name "K-9720"), and 210 parts by weight of calcium carbonate was fed into an extruder. The mixture was then melt-extruded from a T-die and stretched in the machine direction (MD) at a stretching temperature of 60°C and a stretching ratio of 2 times by a uniaxial roll stretching method to obtain a porous film with a thickness of 20 μm. Carded type nonwoven fabric made of propylene (PP) resin fiber (manufactured by Nitto Denko Corporation, product name "Thermostrain 22 HI", basis weight 22g / m 2 ) on one side of which a hot melt adhesive (manufactured by Nitto Denko Corporation, product name "olefin-based hot melt adhesive AC600") was applied at a rate of 8 g / m 2 The surface of the nonwoven fabric on which the hot melt adhesive had been spray coated was then spray laminated with the porous film to obtain a laminate.

[0048] Comparative Example 2 Metallocene polypropylene elastomer (ExxonMobil Corporation, product name "Vistamax 7010", density 0.861 g / cm 3 A mixture of 140 parts by weight of cellulose acetate (melt flow rate (MFR) 3g / 10 min), 200 parts by weight of calcium carbonate (average particle size 1.1 μm), 1 part by weight of stearic acid, and 1 part by weight of an antioxidant was fed into an extruder. Next, melt extrusion was performed from a T-die, and the mixture was stretched in the machine direction (MD) at a stretching temperature of 60° C. and a stretching ratio of 2 times by a uniaxial roll stretching method to obtain a porous film with a thickness of 50 μm. A laminate was obtained in the same manner as in Comparative Example 1, except that the obtained porous film was used.

[0049] Comparative Example 3 A laminate was obtained in the same manner as in Comparative Example 2, except that the thickness of the porous film was 15 μm.

[0050] Comparative Example 4 Metallocene polypropylene elastomer (ExxonMobil Corporation, product name "Vistamax 7010", density 0.861 g / cm 3 A mixture of 140 parts by weight of ethylenediaminetetraacetate (MFR 3g / 10 min), 1 part by weight of stearic acid, and 1 part by weight of an antioxidant was fed into an extruder. Next, melt extrusion was performed from a T-die, and the mixture was stretched in the machine direction (MD) at a stretching temperature of 60°C and a stretching ratio of 2 times by a uniaxial roll stretching method to obtain a porous film having a thickness of 50 μm. A laminate was obtained in the same manner as in Comparative Example 1, except that the obtained porous film was used.

[0051] Comparative Example 5 The nonwoven fabric is a spunbond nonwoven fabric made of PP resin fiber (basis weight 19 g / m 2 A laminate was obtained in the same manner as in Example 1, except that the above-mentioned acrylic resin was used instead of the acrylic resin.

[0052] <Evaluation> The laminates obtained in the examples and comparative examples were subjected to the following evaluations. The results are shown in Table 1. 1.Water vapor permeability In accordance with ISO15106-1, the water vapor permeability of the laminate was measured using a water vapor permeability measuring device (manufactured by Lyssy, device name "L80-5000") under measurement conditions of 23°C temperature and 100% RH. Samples of 8mm x 8mm were used for the measurement. Measurements were performed using 10 samples, and the average value was taken as the water vapor permeability of the laminate. The obtained value was measured in m according to the ISO water vapor permeability measuring method. 2 The measured water vapor transmission rate was converted to water vapor transmission rate per unit area.

[0053] 2.Stretch recovery The laminates obtained in the examples and comparative examples were cut to 30 mm in the machine direction, and set in a tensile tester (manufactured by Shimadzu Corporation, product name "AG-20kNG") with a chuck distance of 50 mm in the width direction. The laminates were stretched 100% at a tensile speed of 300 mm / min, and the stretched state was released, and the initial chuck distance of 50 mm (A) and the post-test film length (mm) (B) were measured. The fluctuation rate was calculated from the obtained values ​​using the following formula. A fluctuation rate of more than 10% was marked x, and a fluctuation rate of 10% or less was marked ◯. The rate of change was calculated as follows: Rate of change (%) = [{(B)-(A)} / (A)] x 100.

[0054] 3.Tactile sensation The laminates obtained in the examples and comparative examples were cut into samples of 100 mm x 100 mm. Linear low-density polyethylene (Prime Polymer Co., Ltd., product name "Ultxex 2022L", density 0.919 g / cm 3A resin composition containing 100 parts by weight of propylene (PP) resin fiber and 100 parts by weight of calcium carbonate as a filler was extruded by an extruder to produce a film with a thickness of 30 μm. The obtained film was stretched twice in the machine direction to obtain a breathable backsheet with a thickness of 15 μm. A carded type nonwoven fabric of propylene (PP) resin fiber (manufactured by Nitto Denko Corporation, product name "Thermostrain 22 HI", basis weight 22 g / m) was used. 2 ) was coated with a hot melt adhesive (manufactured by Nitto Denko Corporation, product name "olefin-based hot melt adhesive AC600") at a rate of 8 g / m 2 The sample and the comparative laminate were touched with the hand, and those judged to be soft were rated as ◯ (good), and those judged to be the same or hard were rated as × (room for improvement).

[0055] 4. Productivity The laminate manufacturing process including a pre-stretching step is rated as × (room for improvement), and the laminate manufacturing process not including a pre-stretching step is rated as 1500 g / (m 2 Laminates having a water vapor permeability of 0.4 s or more were rated as ◯ (good).

[0056] 5. Nonwoven fabric stretch The flow direction of the nonwoven fabric during production is defined as the MD direction, and the direction perpendicular to the MD direction is defined as the CD direction. The nonwoven fabric was cut in the MD direction at 50 mm to prepare a sample. The obtained sample was set in a tensile tester (Shimadzu Corporation, product name "AG-20kNG") with a chuck distance of 50 mm, and stretched in the CD direction at a tensile speed of 300 mm / min under the condition of 100% stretching, and the strength (N / 50 mm) was measured when the value calculated by (length in the CD direction of the nonwoven fabric after stretching - length in the CD direction of the nonwoven fabric before stretching) / length in the CD direction of the nonwoven fabric before stretching x 100 (%) was 50%. Nonwoven fabrics with a strength of 10 N / 50 mm or less were rated as ◯ (good), and nonwoven fabrics with a strength exceeding 10 N / 50 mm were rated as × (room for improvement).

[0057] [Table 1]

[0058] The laminates of the examples of the present invention had excellent moisture permeability and excellent stretchability. They also had an excellent feel. Furthermore, they were highly productive and could be produced efficiently. [Industrial Applicability]

[0059] The laminate according to the embodiment of the present invention can be suitably used in sanitary products, in particular as a back sheet for disposable diapers. [Explanation of symbols]

[0060] 10 Polyurethane resin layer 20 Fiber nonwoven layer 100 Laminate

Claims

1. A laminate having a fibrous nonwoven fabric layer and a polyurethane resin layer having a thickness of 5 μm or more and 15 μm or less.

2. The water vapor permeability of the laminate is 1500 g / (m 2 2. The laminate according to claim 1, wherein the average thermal expansion coefficient is 1.0-1.0 days.

3. 2. The laminate according to claim 1, wherein the laminate is stretched to 100% under conditions of a temperature of 23°C, a chuck distance of 50 mm, and a tensile speed of 300 mm / min, fixed in the stretched state and held for 1 minute, and then released from the stretched state, the rate of variation (%) calculated from the initial chuck distance (A) (mm) and the length of the laminate after the test (B) (mm) = [{(B) - (A)} / (A)] x 100 is 10% or less.

4. The laminate according to claim 1 , wherein the nonwoven fabric layer is a nonwoven fabric that stretches in the CD direction by 50% or more.

5. The laminate according to claim 1 , wherein the nonwoven fabric layer and the polyurethane resin layer are extrusion laminated.

6. The laminate according to claim 1 , wherein the nonwoven fabric layer and the polyurethane resin layer are laminated via a pressure-sensitive adhesive layer.

7. The laminate according to claim 6 , wherein the pressure-sensitive adhesive layer is a layer formed on the entire surface of at least one of the nonwoven fabric layer and the polyurethane resin layer.

8. The laminate according to claim 6 , wherein the pressure-sensitive adhesive layer is a layer intermittently formed on a surface of at least one of the nonwoven fabric layer and the polyurethane resin layer.

9. The laminate according to claim 1 , wherein the nonwoven fabric layer is a nonwoven fabric made of olefin-based fibers.

10. A sanitary article comprising a laminate according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Disposable diaper

    JP2023044181A