Long-fiber nonwoven fabric, separation membrane support and separation membrane

A long-fiber nonwoven fabric with controlled porosity and thermal bonding addresses uneven peel strength and defects in separation membrane supports, improving mechanical stability and uniformity for applications like seawater desalination and water treatment.

JP2024154855APending Publication Date: 2024-10-31TORAY INDUSTRIES INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023069010
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing separation membrane supports made of nonwoven fabrics exhibit density differences leading to uneven membrane peel strength and increased defects during membrane formation, particularly under varying operating pressures.

Method used

A long-fiber nonwoven fabric with controlled cross-sectional porosity and fiber composition, using thermoplastic resins like polyester, is produced through specific thermal compression bonding and laminating processes to ensure uniformity and stability.

Benefits of technology

The solution reduces membrane peel strength variations and defects, enhancing the mechanical strength and uniformity of separation membranes, particularly in applications like seawater desalination and water treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154855000001
    Figure 2024154855000001
Patent Text Reader

Abstract

To provide a long-fiber nonwoven fabric from which a separation membrane having uniform peel strength of membrane can be produced with a reduced number of defects in membrane production, a separation membrane support, and a separation membrane.SOLUTION: A long-fiber nonwoven fabric includes fiber mainly composed of a thermoplastic resin. The long-fiber nonwoven fabric has a cross-section void fraction of 1% or more and 10% or less, with a CV value of 1% or more and 60% or less, and an average single fiber diameter of 10.0 μm or more and 20.0 μm or less. A separation membrane support is composed of the long-fiber nonwoven fabric. A separation membrane includes the separation membrane support.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a long-fiber nonwoven fabric, a separation membrane support, and a separation membrane. [Background technology]

[0002] In recent years, membrane technology has been applied in many water treatment processes. For example, microfiltration membranes and ultrafiltration membranes are used for water treatment at water purification plants, and reverse osmosis membranes are used for desalinizing seawater. In addition, reverse osmosis membranes and nanofiltration membranes are used for treating water for semiconductor manufacturing, boiler water, medical water, pure water for laboratories, and the like. Furthermore, the membrane separation activated sludge process using microfiltration membranes and ultrafiltration membranes is also applied to the treatment of sewage wastewater.

[0003] These separation membranes are roughly classified into flat membranes and hollow fiber membranes based on their shape. Among these separation membranes, flat membranes, which are mainly made of synthetic polymers, are generally used in combination with a support such as a nonwoven fabric or woven fabric because they have poor mechanical strength when used alone with separation function.

[0004] In general, a membrane having a separation function and a support are integrated by a method of casting and fixing a solution of a polymer, which is a raw material of the membrane having a separation function, on a support such as a nonwoven fabric or a woven fabric. In addition, in the case of a semipermeable membrane such as a reverse osmosis membrane, the integration is performed by a method of casting a solution of a polymer on a support such as a nonwoven fabric or a woven fabric to form a support layer, and then forming a semipermeable membrane on the support layer.

[0005] Therefore, the nonwoven fabric, woven fabric, or other support is required to have excellent film-forming properties so that when a solution of a high molecular weight polymer is cast, it does not cause strike-through due to excessive penetration, the membrane material does not peel off, and further the membrane becomes non-uniform or there are defects in the membrane due to fluffing of the support, etc.

[0006] In the case of a reverse osmosis composite membrane used for seawater desalination, the seawater desalination apparatus incorporating the reverse osmosis composite membrane may be operated continuously at a certain operating pressure, or may be operated by changing the operating pressure each time in response to changes in the quality and temperature of the supplied seawater, fluctuations in the management value of the target amount of water produced, etc. In practice, the latter type of operation is common, but in this case, the reverse osmosis composite membrane repeats expansion and contraction in its thickness direction due to fluctuations in the operating pressure applied in the thickness direction of the reverse osmosis composite membrane, and the support membrane and support of the reverse osmosis composite membrane may peel off. In addition, when the apparatus is stopped, forward osmosis works from the permeate side to the supply water side, and the support membrane and support may peel off. For this reason, the separation membrane support is also required to have high peel strength when the separation membrane is formed.

[0007] Conventionally, as such a separation membrane support, a separation membrane has been proposed which is made of a separation membrane support using a non-hydrophilic nonwoven fabric and is characterized by having a membrane peel strength within a specific range (see Patent Document 1).

[0008] In addition, a separation membrane has been proposed in which a membrane having a separation function is formed on a separation membrane support made of a long-fiber nonwoven fabric, and the proportion of macrovoids generated at the interface between the separation membrane support and the membrane is within a specific range, thereby resulting in excellent membrane peel strength (see Patent Document 2). [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2013-71106 A [Patent Document 2] JP 2019-93366 A Summary of the Invention [Problem to be solved by the invention]

[0010] The techniques proposed in Patent Documents 1 and 2 use a nonwoven fabric with excellent mechanical strength as a separation membrane support, and are characterized by producing a separation membrane with a certain degree of membrane peel strength. However, the techniques proposed in Patent Documents 1 and 2 have the problem that there is a high possibility that density differences will occur in the nonwoven fabric that will serve as the separation membrane support, resulting in the occurrence of areas with strong and weak membrane peel strength. In addition, there is a problem that there is a high possibility that membrane production defects will occur due to density differences in the nonwoven fabric that will serve as the separation membrane support when the membrane is produced.

[0011] Therefore, an object of the present invention is to provide a long-fiber nonwoven fabric, a separation membrane support, and a separation membrane which, when made into a separation membrane, can reduce the difference in membrane peel strength and are excellent in reducing the number of membrane production defects during membrane production. [Means for solving the problem]

[0012] As a result of intensive research to achieve the above object, the present inventors have found that a long-fiber nonwoven fabric having a uniform cross-sectional porosity can be obtained by preparing several single-layer long-fiber nonwoven fabrics by forming a fiber web and then subjecting them to preliminary thermocompression bonding, and laminating the resulting fabrics through a flat roll that is an appropriate combination of a metal roll and an elastic roll. Furthermore, the inventors have found that a long-fiber nonwoven fabric having a cross-sectional porosity within a specific range can be obtained, thereby making the long-fiber nonwoven fabric suitable for use as a support for a separation membrane.

[0013] The present invention has been completed based on this finding, and provides the following inventions.

[0014] [1] A long-fiber nonwoven fabric made of fibers whose main component is a thermoplastic resin, the long-fiber nonwoven fabric having a cross-sectional porosity of 1% or more and 10% or less, a CV value of the cross-sectional porosity of 1% or more and 60% or less, and an average single fiber diameter of 10 μm or more and 20 μm or less.

[0015] [2] The long-fiber nonwoven fabric according to [1] above, wherein the fibers are composite fibers in which a low-melting point polymer having a melting point lower than that of a high-melting point polymer is disposed around the high-melting point polymer.

[0016] [3] The basis weight of the long fiber nonwoven fabric is 20 g / m 2 More than 120g / m 2 The long-fiber nonwoven fabric according to the above [1] or [2], which is as follows:

[0017] [4] The long-fiber nonwoven fabric according to any one of [1] to [3] above, wherein the difference R between the maximum and minimum values ​​of the Oken smoothness on one side of the long-fiber nonwoven fabric is 5 seconds or more and 20 seconds or less, and the difference R between the maximum and minimum values ​​of the Oken smoothness on the other side of the long-fiber nonwoven fabric is 1 second or more and 10 seconds or less.

[0018] [5] A separation membrane support comprising the long-fiber nonwoven fabric according to any one of [1] to [4] above.

[0019] [6] A separation membrane comprising the separation membrane support described in [5] above. Effect of the Invention

[0020] According to the present invention, it has become possible to obtain a long-fiber nonwoven fabric, a separation membrane support, and a separation membrane which, when made into a separation membrane, can reduce the difference in membrane peel strength and are excellent in reducing the number of membrane production defects during membrane production. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The long-fiber nonwoven fabric of the present invention is a long-fiber nonwoven fabric made of fibers whose main component is a thermoplastic resin, and the long-fiber nonwoven fabric has a cross-sectional porosity of 1% or more and 10% or less, a CV value of the cross-sectional porosity of 1% or more and 60% or less, and an average single fiber diameter of 10 μm or more and 20 μm or less.

[0022] The components are described in detail below, but the present invention is not limited to the scope described below as long as it does not exceed the gist of the present invention, and various modifications are possible without departing from the gist of the present invention.

[0023] [Fibers made primarily of thermoplastic resin] First, the long-fiber nonwoven fabric of the present invention is made of fibers mainly composed of a thermoplastic resin. Here, in the fibers according to the present invention, "mainly composed of a thermoplastic resin" means that the ratio of the mass of the thermoplastic resin to the mass of the entire fiber is more than 50 mass%. Examples of the thermoplastic resin include polyester, polyamide, polyolefin, and mixtures or copolymers thereof. Among them, polyester is preferably used because of its excellent durability such as mechanical strength, heat resistance, water resistance, and chemical resistance.

[0024] The polyester is a polymer having an acid component and a diol component as monomers, or a hydroxycarboxylic acid component as monomers. In the present invention, the acid component may be an aromatic carboxylic acid such as phthalic acid (ortho form), isophthalic acid, or terephthalic acid, an aliphatic dicarboxylic acid such as succinic acid, adipic acid, or sebacic acid, or an alicyclic dicarboxylic acid such as cyclohexane carboxylic acid. The diol component may be ethylene glycol, diethylene glycol, polyethylene glycol, or 1,4-butanediol. The polyester may also be a polyester having a hydroxycarboxylic acid such as L-lactic acid as a monomer.

[0025] Specific examples of the polyester include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polyethylene naphthalate (PEN), polylactic acid (PLA), polybutylene succinate (PBS), etc. As the polyester used as the high melting point polymer described later, polyethylene terephthalate (PET) is most preferably used because it has a higher melting point, excellent heat resistance, and excellent rigidity.

[0026] Additives such as crystal nucleating agents, matting agents, pigments, mildewproofing agents, antibacterial agents, flame retardants, metal oxides, aliphatic bisamides and / or alkyl-substituted aliphatic monoamides, and hydrophilic agents can be added to these polyester raw materials within the scope of the present invention. Among them, metal oxides such as titanium oxide reduce the surface friction of fibers and prevent fusion between fibers, thereby improving spinnability, and also have the effect of improving the fusion property of long-fiber nonwoven fabrics by increasing thermal conductivity during fusion molding of long-fiber nonwoven fabrics with a heated roll. In addition, aliphatic bisamides such as ethylene bisstearic acid amide and / or alkyl-substituted aliphatic monoamides have the effect of increasing the releasability between the heated roll and the nonwoven fabric web, thereby improving transportability. Note that these additives can also be used when other thermoplastic resins are used.

[0027] The fibers used in the present invention are preferably composite fibers in which a low melting point polymer having a melting point lower than that of a high melting point polymer is arranged around a high melting point polymer. By using such a composite fiber, the fibers are easily fused firmly within the long-fiber nonwoven fabric, and as a result, fluffing on the surface of the long-fiber nonwoven fabric can be suppressed and a smooth surface can be easily obtained. Furthermore, in addition to the fibers constituting the long-fiber nonwoven fabric being fused firmly to each other, the number of fusion points between the fibers in the long-fiber nonwoven fabric can be increased compared to a long-fiber nonwoven fabric in which fibers with different melting points are mixed, and therefore the mechanical strength can also be improved.

[0028] The difference between the melting point of the high melting point polymer and the melting point of the low melting point polymer (hereinafter, sometimes simply referred to as "melting point difference") is preferably 10°C or more and 140°C or less. In other words, it is preferable that the low melting point polymer has a melting point in the range of 10°C or more and 140°C or less lower than the melting point of the high melting point polymer. When the melting point difference is preferably 10°C or more, more preferably 20°C or more, and even more preferably 30°C or more, the fusion property between the fibers can be improved. In addition, when the melting point difference is preferably 140°C or less, more preferably 120°C or less, and even more preferably 100°C or less, the low melting point polymer component is prevented from being fused to the heat roll when the fibers are fused to each other, so that fluffing on the surface of the long fiber nonwoven fabric can be reduced, and further defects occurring on the surface of the long fiber nonwoven fabric can be reduced.

[0029] In the present invention, the melting point of the high melting point polymer in the composite fiber is preferably in the range of 160° C. or more and 320° C. or less. By having the melting point of the high melting point polymer in the composite fiber be preferably 160° C. or more, more preferably 170° C. or more, and even more preferably 180° C. or more, it is possible to obtain a long-fiber nonwoven fabric having excellent shape stability, which can maintain its shape even when subjected to processing that involves the application of heat, when used as a separation membrane support. In addition, by having the melting point of the high melting point polymer in the composite fiber be 320° C. or less, more preferably 300° C. or less, and even more preferably 280° C. or less, it is possible to suppress a large consumption of thermal energy for melting during the production of the long-fiber nonwoven fabric, which leads to a decrease in productivity.

[0030] On the other hand, the melting point of the low melting point polymer in the composite fiber is preferably in the range of 150°C to 310°C while ensuring the above-mentioned difference in melting points. By having the melting point of the low melting point polymer in the composite fiber be preferably 150°C or higher, more preferably 160°C or higher, and even more preferably 170°C or higher, it is possible to obtain a long-fiber nonwoven fabric having excellent shape stability, such that the shape of the long-fiber nonwoven fabric can be maintained even if it is subjected to processing in which heat is applied, when the long-fiber nonwoven fabric is used as a separation membrane support. In addition, by having the melting point of the low melting point polymer in the composite fiber be preferably 310°C or lower, more preferably 290°C or lower, and even more preferably 270°C or lower, it is possible to easily obtain a long-fiber nonwoven fabric having excellent fusibility and excellent mechanical strength when producing the long-fiber nonwoven fabric.

[0031] In the present invention, the melting point of a thermoplastic resin is measured using a differential scanning calorimeter (e.g., PerkinElmer's "DSC-2" model) at a heating rate of 20° C. / min and a measurement temperature range of 30° C. to 350° C., and the temperature at which the obtained melting endothermic curve gives an extreme value is defined as the melting point of the thermoplastic resin. For resins whose melting endothermic curve does not show an extreme value in the differential scanning calorimeter, the resin is heated on a hot plate, and the temperature at which the resin melts under a microscope is defined as the melting point.

[0032] When the thermoplastic resin is polyester, examples of the combination of a high melting point polymer and a low melting point polymer (hereinafter, the order may be high melting point polymer / low melting point polymer) include combinations such as PET / PBT, PET / PTT, PET / polylactic acid, and PET / copolymerized PET, among which the combination of PET / copolymerized PET is preferably used because of its excellent spinnability. As the copolymerization component of the copolymerized PET, isophthalic acid copolymerized PET is preferably used because of its excellent spinnability.

[0033] Examples of the composite form of the composite fiber include a concentric core-sheath type, an eccentric core-sheath type, and an island-in-the-sea type, among which the concentric core-sheath type is preferred because it allows the fibers to be fused uniformly and firmly. Furthermore, the cross-sectional shape of the composite fiber may be a circular cross-section, a flat cross-section, a polygonal cross-section, a multi-lobal cross-section, a hollow cross-section, and the like. Among these, a circular cross-sectional shape is a preferred embodiment of the composite fiber.

[0034] The content ratio of the high melting point polymer and the low melting point polymer in the fiber mainly composed of a thermoplastic resin is preferably in the range of 90:10 to 60:40 in terms of the mass ratio of the high melting point polymer:low melting point polymer, and more preferably in the range of 85:15 to 70:30. By making the high melting point polymer 60% by mass or more and 90% by mass or less with respect to 100% by mass of the total of the two, the durability of the long-fiber nonwoven fabric can be made excellent. On the other hand, by making the low melting point polymer 10% by mass or more and 40% by mass or less with respect to 100% by mass of the total of the two, the fibers constituting the long-fiber nonwoven fabric are firmly fused to each other, and a long-fiber nonwoven fabric with excellent mechanical strength can be obtained.

[0035] The average single fiber diameter of the fiber according to the present invention is 10.0 μm or more and 20.0 μm or less. When the lower limit of the average single fiber diameter range is 10.0 μm or more, a long-fiber nonwoven fabric having excellent mechanical strength can be obtained. On the other hand, when the upper limit of the average single fiber diameter range is 20.0 μm or less, preferably 19.0 μm or less, more preferably 18.0 μm or less, the uniformity of the long-fiber nonwoven fabric can be improved, and a long-fiber nonwoven fabric having a dense surface can be obtained. For example, when a resin coating process such as a membrane forming process is added to the long-fiber nonwoven fabric for a separation membrane support, coating unevenness of the resin agent can be reduced.

[0036] In the present invention, the average single fiber diameter (μm) of the long fiber nonwoven fabric is determined by the following method. (i) Ten small sample pieces are randomly taken from the long fiber nonwoven fabric. (ii) The surface of the collected small sample is photographed using a scanning electron microscope (e.g., Keyence Corporation's "VHX-D500") at magnifications of 500 to 2000 times, enabling the thickness of the fibers to be measured. (iii) From the photographs of each small sample, 10 fibers are randomly selected (100 fibers in total) and their diameters are measured. The fibers are assumed to have a circular cross section, and the diameter is taken as the single fiber diameter. (iv) The average single fiber diameter is calculated by rounding off the arithmetic mean value to one decimal place.

[0037] [Long fiber nonwoven fabric] The long-fiber nonwoven fabric of the present invention is made of fibers mainly composed of the thermoplastic resin. Here, the "long-fiber nonwoven fabric" in the present invention refers to nonwoven fabrics such as spunbonded nonwoven fabrics and meltblown nonwoven fabrics manufactured by the manufacturing methods described below, and does not include nonwoven fabrics (short-fiber nonwoven fabrics) consisting only of fibers cut to a certain length (e.g., 100 mm).

[0038] In the present invention, the "MD direction of the long-fiber nonwoven fabric" refers to the sheet conveying direction when the long-fiber nonwoven fabric is produced, i.e., the winding direction of the nonwoven fabric roll, and the "CD direction of the long-fiber nonwoven fabric" refers to the sheet conveying direction when the long-fiber nonwoven fabric is produced, i.e., the direction perpendicular to the winding direction of the nonwoven fabric roll. In other words, when the MD direction can be determined from the appearance of the long-fiber nonwoven fabric, i.e., when the winding direction of the nonwoven fabric roll can be uniquely determined, this method is determined as the MD direction. On the other hand, when the MD direction cannot be determined from the appearance, such as when the long-fiber nonwoven fabric is cut and not in a rolled state, the MD direction and CD direction are determined by the following procedure. (a) Within the plane of the long-fiber nonwoven fabric, select one arbitrary direction and take five test pieces, each 30 cm long and 5.0 cm wide, at equal intervals along that direction. (b) Similarly, five test pieces, each 30 cm long and 5.0 cm wide, are taken at equal intervals in directions rotated 30 degrees, 60 degrees, and 90 degrees from the direction in which the test pieces were taken. (c) For the test pieces in each direction, measure the tensile strength of each test piece based on the measurement method for the tensile strength of long-fiber nonwoven fabric shown in (c-1) to (c-2) below. Note that this tensile strength (N / 5cm) is to be the value measured as follows in accordance with JIS L1913:2010 "Test methods for general long-fiber nonwoven fabrics" 6.3 "Tensile strength and elongation." (c-1) Apply load until the sample breaks, with a gripping distance of 20 cm and a tensile speed of 100±10 mm / min. (c-2) The strength of the sample at the maximum load is the tensile strength (N / 5cm), the average of the five points is calculated, and the value rounded off to the first decimal place is the tensile strength of the long-fiber nonwoven fabric. (d) The direction in which the measured value is the highest is defined as the MD direction of the long-fiber nonwoven fabric, and the direction perpendicular to this is defined as the CD direction. If there are two or more directions in which the tensile strength is highest, the direction perpendicular to these directions in which the tensile strength is lower is defined as the MD direction of the long-fiber nonwoven fabric, and if there are two or more directions in which the tensile strength is highest and the tensile strengths in the directions perpendicular to these directions are also equal, for example, if the tensile strengths in all four directions are equal, then any of the four directions is defined as the MD direction, and the direction perpendicular to this is defined as the CD direction.

[0039] The long-fiber nonwoven fabric of the present invention has a cross-sectional porosity of 1% or more and 10% or less in the cross section of the long-fiber nonwoven fabric. When the lower limit of the cross-sectional porosity range is 1% or more, preferably 3% or more, and more preferably 5% or more, the fiber surface is prevented from becoming a film-like sheet form, and the long-fiber nonwoven fabric can be sufficiently impregnated with membrane components as a separation membrane support. On the other hand, when the upper limit of the cross-sectional porosity range is 10% or less, preferably 9% or less, the fibers constituting the long-fiber nonwoven fabric are firmly fused to each other, resulting in a long-fiber nonwoven fabric with excellent mechanical strength.

[0040] Here, the cross-sectional porosity (%) in the present invention is determined as follows. (i) Ten small sample pieces whose cross sections can be observed are taken from the long-fiber nonwoven fabric at equal intervals in the CD direction of the long-fiber nonwoven fabric. (ii) A cross section of the collected small sample is photographed at 500x magnification using a scanning electron microscope (SEM, for example, "VHX-D500" manufactured by Keyence Corporation). (iii) Crop the photographs of each sample piece to a size of 140 pixels x 140 pixels. (iv) Each cut-out photograph is converted into a grayscale image (8-bit image), and a threshold is set so that pixel values ​​of 0 to 127 are black and 128 to 255 are white, and the image is binarized. (v) Using image analysis software (such as ImageJ), the ratio of the black area to the entire photograph (white areas, black areas) (the entire area observed in the photograph is considered to be the sample cross-section) is taken as the cross-sectional porosity. (vi) Similarly, the cross-sectional porosity (%) of each of the 10 small sample pieces is calculated, and the arithmetic mean value (%) of the cross-sectional porosity of the 10 small sample pieces is calculated. (vii) The arithmetic mean value (%) of the cross-sectional porosity of the 10 small sample pieces obtained in (vi) is rounded off to one decimal place, and this value is the cross-sectional porosity (%) of the long-fiber nonwoven fabric.

[0041] In addition, means for adjusting the cross-sectional porosity of this long-fiber nonwoven fabric to the above-mentioned range include adjusting the thermocompression conditions in the lamination and thermocompression bonding step, and adjusting the average single fiber diameter of the fibers constituting the long-fiber nonwoven fabric, as will be described later.

[0042] The CV value of the cross-sectional porosity of the long-fiber nonwoven fabric in the present invention is 1% or more and 60% or less. The lower limit of the range of the cross-sectional porosity CV value is ideally 0% (no variation), but in reality, the lower limit is about 1%. On the other hand, by setting the upper limit of the range of the cross-sectional porosity CV value to 60% or less, preferably 55% or less, and more preferably 45% or less, a long-fiber nonwoven fabric with uniform density can be obtained, and the film peel strength difference described later can be reduced, and further the number of film formation defects can be suppressed.

[0043] Here, the cross-sectional porosity CV value (%) in the present invention is a value determined as follows. (i) Ten small sample pieces whose cross sections can be observed are taken from the long-fiber nonwoven fabric at equal intervals in the CD direction of the long-fiber nonwoven fabric. (ii) The cross-sectional porosity (%) of each small sample is measured. (iii) From the values ​​obtained in (ii), the average value (A ave ) and standard deviation (A sdv ) is required. (iv) Based on the results of (i) to (iii), calculate the cross-sectional porosity CV value (%) using the following formula and round off to the first decimal place. Cross-sectional porosity CV value (%) = [(A sdv ) / (A ave )] × 100.

[0044] In the measurement of the cross-sectional porosity and the cross-sectional porosity CV value, the steps for measuring the cross-sectional porosity (%) of each small sample are the same, so they may be measured simultaneously.

[0045] The CV value of the cross-sectional porosity of the long-fiber nonwoven fabric can be adjusted to the above range by, for example, the method described below, specifically, the use of an elastic roll such as a crown roll.

[0046] The basis weight of the long fiber nonwoven fabric in the present invention is 20 g / m 2 More than 120g / m 2 The lower limit of the range of the basis weight of the long fiber nonwoven fabric is preferably 20 g / m 2 More preferably, 30 g / m 2 More preferably, 40 g / m 2 By setting the weight per unit area of ​​the long-fiber nonwoven fabric to 120 g / m or more, the long-fiber nonwoven fabric has excellent mechanical strength. 2 Less than 110 g / m 2 Less than 100 g / m 2 By satisfying this condition, the thickness of the separation membrane can be reduced and the separation membrane area per fluid separation element unit can be increased.

[0047] In the present invention, the basis weight of the long-fiber nonwoven fabric is determined in accordance with "6.2 Mass per unit area" of JIS L1913:2010 "Testing methods for general nonwoven fabrics" and is measured by the following procedure. (i) Three 25cm x 25cm test pieces are taken per meter at equal intervals in the CD direction of the sample. If it is not possible to take a single row in the width direction of the long fiber nonwoven fabric, multiple rows are taken in the width direction, and the extensions of the center lines parallel to the MD direction of the test pieces are arranged at equal intervals in the CD direction. (ii) Weigh the mass (g) of each at standard conditions. (iii) The average value is 1 m 2 Mass per unit (g / m 2 )

[0048] The thickness of the long fiber nonwoven fabric in the present invention is preferably 0.03 mm or more and 0.20 mm or less. By setting the thickness within the above range, for example, when used as a nonwoven fabric for a separation membrane support, good membrane formability can be obtained with little over-penetration during polymer solution casting, and a separation membrane with high membrane peel strength, mechanical strength, and excellent durability can be obtained. In addition, the thickness of the separation membrane can be reduced, and the separation membrane area per fluid separation element unit can be increased.

[0049] In the present invention, the thickness of the long-fiber nonwoven fabric is measured by the following procedure. (i) Using a thickness meter (for example, TECLOCK (registered trademark) SM-114 manufactured by TECLOCK Corporation), set the diameter of the gauge head to 10 mm and the measuring force to 2.5 N, and measure the thickness of the long-fiber nonwoven fabric at 10 cm intervals in the CD direction. (ii) The above arithmetic average value is rounded off to two decimal places to obtain the thickness (mm) of the long-fiber nonwoven fabric.

[0050] The air permeability of the long fiber nonwoven fabric in the present invention is 0.5 cm 3 / cm 2 / second or more 2.5cm 3 / cm 2By setting the air permeability in the above range, for example, when the nonwoven fabric is used as a separation membrane support, the resin can be uniformly formed into a membrane with little breakthrough during polymer solution casting.

[0051] In the present invention, the air permeability of the long-fiber nonwoven fabric is determined based on JIS L1913:2010 "Testing methods for general nonwoven fabrics", 6.8 "Air permeability (JIS method)", 6.8.1 "Fragile type method", as measured as follows. (i) Ten test pieces measuring 150 mm length x 150 mm width are taken at equal intervals in the CD direction of the long-fiber nonwoven fabric. If it is not possible to take 10 pieces in a single row in the width direction of the long-fiber nonwoven fabric, five or more pieces should be taken as many as possible. If it is not possible to take five pieces in a single row, multiple rows should be taken in the width direction, and five pieces should be taken in such an arrangement that the extensions of the center lines parallel to the MD direction of the test pieces are equally spaced in the CD direction. (ii) After attaching a test specimen to one end of the cylinder of the testing machine, adjust the suction fan and air hole so that the inclined barometer indicates a pressure of 125 Pa using the lower limit resistor, and measure the pressure indicated by the vertical barometer at that time. (iii) From the measured pressure and the type of air hole used, calculate the volume of air (cm3) passing through the test piece using the conversion table attached to the tester. 3 / cm 2 / seconds). (iv) The average value of the air permeability of each test piece is rounded to one decimal place to obtain the air permeability of the long fiber nonwoven fabric (cm 3 / cm 2 / second).

[0052] The long-fiber nonwoven fabric of the present invention preferably has different smoothness between its one surface and the other surface. In the long-fiber nonwoven fabric, the side with higher smoothness is called side A, and the side with lower smoothness is called side B. When the long-fiber nonwoven fabric of the present invention is used as a support for a separation membrane, it is preferable that side A is the membrane-forming side and side B is the non-membrane-forming side.

[0053] The smoothness of side A of the long-fiber nonwoven fabric in the present invention is preferably 20 seconds or more and 70 seconds or less. By setting the lower limit of the smoothness range of side A of the long-fiber nonwoven fabric to preferably 20 seconds or more, more preferably 22 seconds or more, and even more preferably 25 seconds or more, and the upper limit to preferably 70 seconds or less, more preferably 68 seconds or less, and even more preferably 65 seconds or less, the polymer solution cast on the support can be solidified after sufficiently penetrating into the support, and the membrane peel strength of the formed separation membrane can be improved.

[0054] The smoothness of side B of the long-fiber nonwoven fabric in the present invention is preferably 5 seconds or more and 30 seconds or less. By setting the lower limit of the smoothness range of side B of the long-fiber nonwoven fabric to preferably 5 seconds or more, more preferably 6 seconds or more, and even more preferably 7 seconds or more, and the upper limit to preferably 30 seconds or less, more preferably 28 seconds or less, and even more preferably 25 seconds or less, air inside the separation membrane support can be quickly discharged during separation membrane production, and partial reduction in membrane peel strength can be suppressed, and the occurrence of membrane production defects such as pinholes can be suppressed.

[0055] In the present invention, the smoothness of the long-fiber nonwoven fabric is measured using an Oken type smoothness tester in accordance with JIS P8155:2010 as follows. (i) Ten test pieces measuring 150 mm length x 150 mm width are taken at equal intervals in the CD direction of the long-fiber nonwoven fabric. If it is not possible to take 10 pieces in a single row in the width direction of the long-fiber nonwoven fabric, five or more pieces should be taken as many as possible. If it is not possible to take five pieces in a single row, multiple rows should be taken in the width direction, and five pieces should be taken in such an arrangement that the extensions of the center lines parallel to the MD direction of the test pieces are equally spaced in the CD direction. (ii) Place the measurement surface of the test piece downwards, place the measurement head on it, and then place a rubber pressure plate, pressure plate and weight on top of it, and measure the smoothness under conditions of a measurement pressure of 4.91±0.02 kPa. (iii) The smoothness (seconds) of the measurement surface of the long-fiber nonwoven fabric shall be determined by rounding off the average value of the smoothness of each test piece to the nearest whole number. (iv) The other surface is similarly measured to determine the smoothness (sec).

[0056] It is preferable that the difference R between the maximum and minimum smoothness values ​​on one side of the long-fiber nonwoven fabric of the present invention is 5 seconds or more and 20 seconds or less, and the difference R between the maximum and minimum smoothness values ​​on the other side is 1 second or more and 10 seconds or less. The difference between the maximum and minimum smoothness values ​​is measured by the method described below. That is, according to the method described below, samples are taken at specific intervals in the CD direction and measured, so it means the difference between the maximum and minimum smoothness values ​​in the CD direction. And a small value of this means that the smoothness is uniform in the CD direction. Hereinafter, the difference between the maximum and minimum smoothness values ​​is abbreviated to "CD direction smoothness difference".

[0057] In particular, the CD smoothness difference of the A-side of the long-fiber nonwoven fabric is preferably 5 seconds or more and 20 seconds or less. More preferably, it is 6 seconds or more and 19 seconds or less. By setting the CD smoothness difference of the A-side in the above range, the surface condition of the long-fiber nonwoven fabric becomes uniform, and when used as a separation membrane support, a resin can be uniformly formed into a membrane. In addition, the CD smoothness difference of the B-side of the long-fiber nonwoven fabric is preferably 1 second or more and 10 seconds or less. More preferably, it is 1 second or more and 9 seconds or less. By setting the smoothness difference of the B-side in the above range, the surface condition of the long-fiber nonwoven fabric becomes uniform, and air inside the separation membrane support is quickly discharged during separation membrane production, allowing a resin to be uniformly formed into a membrane.

[0058] Here, the value of the CD direction smoothness difference (sec) of the long-fiber nonwoven fabric in the present invention is a value determined as follows. (i) Ten test pieces measuring 100 mm length x 100 mm width are taken at equal intervals in the CD direction of the long-fiber nonwoven fabric. If it is not possible to take 10 pieces in a single row in the width direction of the long-fiber nonwoven fabric, five or more pieces should be taken as many as possible. If it is not possible to take five pieces in a single row, multiple rows should be taken in the width direction, and five pieces should be taken in such an arrangement that the extensions of the center lines parallel to the MD direction of the test pieces are equally spaced in the CD direction. (ii) The smoothness (seconds) is measured for one surface of the obtained test piece. (iii) The difference between the maximum and minimum smoothness values ​​(seconds) obtained in (ii) is calculated, and the difference is rounded off to one decimal place to determine the smoothness difference (seconds) on one side of the long-fiber nonwoven fabric. (iv) For the other side of the long-fiber nonwoven fabric, the smoothness difference (seconds) is determined by following steps (ii) to (iii).

[0059] In the measurement of the smoothness and the CD smoothness difference, the process for measuring the smoothness of each surface is the same, so these may be measured simultaneously.

[0060] [Manufacturing method of long fiber nonwoven fabric] Next, a method for producing the long-fiber nonwoven fabric of the present invention will be described. The long-fiber nonwoven fabric of the present invention is preferably produced by a spunbond method by sequentially carrying out the following steps (a) to (d). (a) A step of melt-extruding a thermoplastic resin from a spinneret, and pulling and stretching the spun thermoplastic resin by an ejector to form fibers. (b) A process of regulating the arrangement of the fibers with a fiber-spreading plate and depositing the fibers on a moving net conveyor to form a fiber web. (c) A step of preliminarily thermocompressing the obtained fiber web to form a single-layer long-fiber nonwoven fabric. (d) A step of laminating and thermocompressing the obtained single-layer long-fiber nonwoven fabric to form a long-fiber nonwoven fabric.

[0061] Each of the above steps will now be described in further detail.

[0062] (a) forming a fiber First, in this step, the thermoplastic resin is melt-extruded from a spinneret. In particular, when the fibers constituting the long-fiber nonwoven fabric are composite fibers in which a low-melting point polymer having a melting point lower than that of a high-melting point polymer is arranged around the high-melting point polymer, it is preferable to melt the high-melting point polymer and the low-melting point polymer at a temperature higher than their melting points (melting point + 70°C) and melt-extrude them from a spinneret having a temperature higher than the melting point and lower than (melting point + 70°C) so as to obtain composite fibers in which a low-melting point polymer having a melting point lower than that of the high-melting point polymer is arranged around the high-melting point polymer by 10°C to 140°C. In addition, the shape of the discharge hole of the spinneret through which the molten thermoplastic resin is extruded can be a circle, an ellipse, a polygon, a multi-lobe, or a combination of these shapes according to the cross-sectional shape of the fibers. Among these, the use of a circular cross-sectional shape is a more preferred embodiment, since it allows efficient bonding of the fibers to each other and allows the fibers to be firmly bonded to each other by thermocompression bonding.

[0063] The thermoplastic resin that has been melt-extruded and spun as described above is then drawn and stretched by an ejector to form fibers. At this time, the spinning speed is preferably 3000 m / min or more and 6000 m / min or less.

[0064] (b) forming a fibrous web In this process, the arrangement of the fibers formed by the above process is regulated by a fiber-spreading plate. Specifically, it is preferable that the fibers sucked by the ejector are ejected from a fiber-spreading plate having a slit shape provided at the lower part of the ejector. Then, it is preferable that the fibers are deposited on a moving net conveyor to form a fiber web.

[0065] (c) A step of pre-thermocompressing the fiber web to form a single-layer filament nonwoven fabric. In this step, a method is preferably used in which the fiber web obtained in the previous step is preliminarily thermocompressed by a pair of upper and lower flat rolls to form a single-layer long-fiber nonwoven fabric.

[0066] The "flat roll" used in this method refers to a metal roll or an elastic roll that has no irregularities on the surface of the roll, and further, a pair of upper and lower flat rolls refers to a pair of a metal roll and a metal roll, or a pair of a metal roll and an elastic roll. Here, the elastic roll refers to a roll made of a material that has elasticity compared to a metal roll. Examples of the elastic roll include so-called paper rolls made of paper, cotton, aramid paper, etc., and resin rolls made of urethane resin, epoxy resin, silicon resin, polyester resin, hard rubber, etc., or mixtures of these.

[0067] The temperature of the pair of upper and lower flat rolls during preliminary thermocompression bonding is preferably 20° C. to 120° C. lower than the melting point of the thermoplastic resin (in the case of a composite fiber in which a low-melting point polymer having a melting point lower than that of a high-melting point polymer is disposed around the high-melting point polymer, the melting point of the low-melting point polymer). By setting the temperature at such a level, the fibers are not excessively fused to each other, and transportability during the production of a single-layer long-fiber nonwoven fabric can be improved.

[0068] The linear pressure during preliminary thermocompression bonding is preferably 49 N / cm to 656 N / cm, in which case the mechanical strength required for transporting the fiber web can be imparted and excessive fusion between the fibers can be prevented.

[0069] (d) A process of laminating and thermocompressing the single-layer long-fiber nonwoven fabric to form a long-fiber nonwoven fabric. In the method for producing a long-fiber nonwoven fabric of the present invention, it is preferable to heat-press the single-layer long-fiber nonwoven fabric obtained in the above-mentioned step as it is, or to laminate and heat-press 2 to 5 layers to integrate them. If the number of layers of the single-layer long-fiber nonwoven fabric is 2 or more, the texture is improved compared to when it is a single layer, and sufficient uniformity can be obtained. Furthermore, if the number of layers is 5 or less, it is possible to suppress wrinkling during laminate heat-press bonding and to suppress peeling between layers.

[0070] Here, as a method of thermocompression bonding to form a long-fiber nonwoven fabric by laminating 2 to 5 layers of the single-layer long-fiber nonwoven fabric, for example, when used as a separation membrane support, in order to obtain a separation membrane having good film formability, excellent mechanical strength and durability, and excellent membrane peel strength, a method of laminating and thermocompressing the single-layer long-fiber nonwoven fabric by a pair of upper and lower flat rolls to integrate the fabric can be preferably used, since the surface is smooth and the mechanical strength is excellent. The flat roll is a metal roll or an elastic roll having no unevenness on the roll surface, and a metal roll and a metal roll can be paired, or a metal roll and an elastic roll can be paired. In particular, a method of laminating and thermocompressing the single-layer long-fiber nonwoven fabric by a heated metal roll and an elastic roll is preferably used, since the fusion of the fibers on the surface of the nonwoven fabric is suppressed and the shape is maintained, thereby improving the membrane peel strength of the separation membrane when used as a separation membrane support. Furthermore, since this improves the membrane peel strength of the separation membrane and suppresses excessive penetration of the polymer solution cast onto the support during separation membrane production, it is preferable to use the surface of the long fiber nonwoven fabric in contact with the metal roll as the membrane-forming surface of the separation membrane support and the surface in contact with the elastic roll as the non-membrane-forming surface of the separation membrane support.

[0071] Here, the elastic roll refers to a roll made of a material having elasticity compared to a metal roll, and examples of the material for the elastic roll include so-called paper rolls such as paper, cotton, and aramid paper, and resin rolls such as urethane resin, epoxy resin, silicon resin, polyester resin, and hard rubber.

[0072] The hardness (Shore D) of the elastic roll is preferably 60 to 99. By setting the hardness (Shore D) of the elastic roll to preferably 60 or more, more preferably 62 or more, and even more preferably 64 or more, when the surface of the long-fiber nonwoven fabric in contact with the elastic roll is used as a non-membrane-forming surface, the smoothness of the non-membrane-forming surface of the separation membrane support can be improved, excessive penetration of a coagulation solution mainly composed of water from the non-membrane-forming surface of the separation membrane support into the inside during separation membrane production can be suppressed, and the polymer solution cast on the support can be coagulated after sufficiently penetrating into the support, thereby improving the membrane peel strength of the separation membrane formed. On the other hand, by setting the hardness (Shore D) of the elastic roll to preferably 99 or less, more preferably 97 or less, and even more preferably 95 or less, when the surface of the long-fiber nonwoven fabric in contact with the elastic roll is used as a non-membrane-forming surface, excessive improvement in the smoothness of the non-membrane-forming surface of the separation membrane support is suppressed, which makes it possible for the coagulation liquid, whose main component is water, to penetrate into the separation membrane support during separation membrane production, and prevents excessive penetration of the high molecular weight polymer cast on the membrane-forming surface, i.e., strike-through.

[0073] As a configuration of two or more flat rolls, a two-roll x two-set system or a two-roll x three-set system in which two or more sets of metal / elastic roll combinations are used continuously or discontinuously during the manufacturing process, or a three-roll system such as elastic / metal / elastic, elastic / metal / metal, or metal / elastic / metal can be preferably used.

[0074] With the 2 rolls x 2 sets method, heat and pressure can be applied twice to the long-fiber nonwoven fabric, making it easier to control the properties of the long-fiber nonwoven fabric and enabling production speeds to be increased. In addition, because the adhesive surfaces of the first and second sets of elastic rolls can be easily reversed, it is also easier to control the surface properties of the front and back sides of the long-fiber nonwoven fabric.

[0075] On the other hand, in the case of the 3-roll method, for example, the long-fiber nonwoven fabric that has been thermocompressed between the elastic 1 / metal rolls (elastic 1 / metal / elastic 2) is folded back and further thermocompressed between the metal / elastic 2 rolls, making it possible to apply heat and pressure twice to the long-fiber nonwoven fabric in the same way as the above-mentioned 2-roll x 2 set method, and it is also possible to reduce equipment costs and save space compared to the continuous 2-roll x 2 set method.

[0076] In a manufacturing method using two or more of these elastic rolls, the hardness (Shore D) of the elastic roll in contact with the long-fiber nonwoven fabric in the first stage and the elastic roll in contact with the long-fiber nonwoven fabric in the second stage may be changed.

[0077] The shape of the elastic roll conventionally used in the production of long-fiber nonwoven fabrics is generally a straight roll. However, when the long-fiber nonwoven fabric is produced using only such straight rolls, the cross-sectional voids near the center in the width direction of the long-fiber nonwoven fabric tend to be in a different state compared to other parts, resulting in variations in the cross-sectional void ratio.

[0078] In the present invention, there are no limitations on the manufacturing method as long as the long-fiber nonwoven fabric defined in the present invention is obtained, but by ensuring that the treatment with the elastic roll is uniform in the width direction of the long-fiber nonwoven fabric, the variation in cross-sectional porosity can be easily reduced.

[0079] Specifically, it is preferable that at least one of the elastic rolls used is a crown roll. This allows the long-fiber nonwoven fabric to be treated more uniformly in the width direction, resulting in a uniform cross-sectional void ratio within the long-fiber nonwoven fabric. In a production method using two or more elastic rolls, it is preferable that the shape of the elastic roll that contacts the long-fiber nonwoven fabric in the first stage and the elastic roll that contacts the long-fiber nonwoven fabric in the second stage are a combination of ordinary straight rolls and crown rolls.

[0080] In the above, the straight roll is a roll in which the diameter dimension at the axial center is the same as the diameter dimension at the roll end, and in terms of the crown value described below, it is a roll with a crown value of 0 mm. The crown roll is a roll in which the diameter dimension at the axial center is the largest in the roll axial direction. A radial crown roll, which has a shape that draws a gentle arc from the center to the end, is preferable.

[0081] When using an elastic roll of the crown roll, the crown value is preferably more than 0 mm and not more than 1.0 mm. By setting the crown value to preferably more than 0 mm, more preferably 0.1 mm or more, the uniformity of the density in the CD direction of the long-fiber nonwoven fabric is improved, and the film peel strength is made uniform. On the other hand, by setting the crown value of the elastic roll to preferably 1.0 mm or less, more preferably 0.9 mm or less, excessive fusion of the surface fibers of the long-fiber nonwoven fabric can be suppressed. The crown value of the elastic roll is calculated by the following procedure. (i) A pressure-sensitive film is sandwiched between the target elastic roll and a mating roll, and linear pressure is applied to the film. The linear pressure is not specified. (ii) The nip width transferred to the pressure-sensitive film is measured at two locations on both ends and one location in the center. The average of the measurements at both ends is the end nip width. (iii) Calculate the crown value using the following formula: (Formula) ΔC=(n 2 -N 2 )×(D1+D2) / (2×D1×D2) In the formula, ΔC is the crown value, n is the end nip width, N is the central nip width, D1 is the outer diameter of the elastic roll, and D2 is the outer diameter of the roll opposite the nip.

[0082] The surface temperature of the metal roll is preferably 20°C to 90°C lower than the melting point of the polymer constituting at least the surface of the fibers constituting the long-fiber nonwoven fabric, and more preferably 30°C to 70°C lower. If the surface temperature of the metal roll is 20°C or more lower than the melting point of the polymer constituting at least the surface of the fibers constituting the long-fiber nonwoven fabric, excessive fusion of the surface fibers of the long-fiber nonwoven fabric can be suppressed, the polymer solution can easily penetrate, and a separation membrane support with excellent membrane peel strength can be obtained. On the other hand, if the difference between the surface temperature of the metal roll and the melting point of the polymer constituting at least the surface of the fibers constituting the long-fiber nonwoven fabric is 90°C or less, the fibers constituting the long-fiber nonwoven fabric can be firmly bonded to each other, and the long-fiber nonwoven fabric can be densified to obtain a separation membrane support with excellent mechanical strength. In addition, there is little over-penetration during casting of the polymer solution, and good membrane formability can be obtained.

[0083] Furthermore, it is also a preferred embodiment to provide a temperature difference between the metal roll and the elastic roll, and set the surface temperature of the elastic roll to a temperature 10° C. to 120° C. lower than the surface temperature of the metal roll.

[0084] The linear pressure of the flat roll is preferably 196 N / cm or more and 4900 N / cm or less. The linear pressure of the flat roll is more preferably 490 N / cm or more, and further preferably 980 N / cm or more. If the linear pressure of the flat roll is 196 N / cm or more, the fibers constituting the long-fiber nonwoven fabric can be firmly bonded to each other, and the long-fiber nonwoven fabric can be densified to obtain a separation membrane support having excellent mechanical strength. On the other hand, if the linear pressure of the flat roll is 4900 N / cm or less, excessive fusion of the surface fibers of the long-fiber nonwoven fabric can be suppressed, and the penetration of the polymer solution into the inside of the nonwoven fabric is not hindered, and a separation membrane support having excellent membrane peel strength can be obtained.

[0085] In the method for producing the long-fiber nonwoven fabric of the present invention, the preliminary thermo-compression bonding and the lamination thermo-compression bonding for forming the above-mentioned single-layer long-fiber nonwoven fabric may be carried out continuously on one production line, or the fabric may be wound up once after the preliminary thermo-compression bonding and then unwound again for lamination thermo-bonding.

[0086] The long-fiber nonwoven fabric thus obtained can reduce the variation in cross-sectional porosity, and is therefore preferably effective in the CD size, i.e., in the long-fiber nonwoven fabric having a width of 50 cm or more. In particular, the variation in cross-sectional porosity in the CD direction can be reduced even in the long-fiber nonwoven fabric having a width of 80 cm or more, particularly 100 cm or more. Furthermore, it is possible to make the long-fiber nonwoven fabric have a width of 200 cm or more. There is no upper limit as long as the range specified in the present invention is satisfied, but in reality it is about 400 cm or less. Usually, the wider the width, the greater the variation in the CD direction, but it is worth noting that in the present invention, the variation in cross-sectional porosity in the CD direction can be reduced even in the above range.

[0087] [Separation membrane support] The long-fiber nonwoven fabric of the present invention can reduce the difference in membrane peel strength when used as a separation membrane, and can also reduce the number of membrane defects during membrane production, so it can be preferably used as a separation membrane support. That is, the separation membrane support of the present invention is a separation membrane support made of the long-fiber nonwoven fabric. As will be described later in detail, for example, a separation membrane is formed by providing a separation membrane layer on one side of the long-fiber nonwoven fabric, and the long-fiber nonwoven fabric of the present invention can be used as a separation membrane support that supports this separation membrane. The separation membrane support of the present invention may be a long-fiber nonwoven fabric that has been subjected to a functional treatment such as hydrophilic treatment, or may include other members.

[0088] In particular, as mentioned above, it is preferable to use side A, which has high smoothness (usually the side that comes into contact with the metal roll of the long fiber nonwoven fabric), as the membrane-forming side of the separation membrane support, and side B, which has low smoothness (usually the side that comes into contact with the elastic roll), as the non-membrane-forming side of the separation membrane support.

[0089] As a method for providing a separation membrane layer on the long-fiber nonwoven fabric of the present invention, a method for forming the separation membrane layer by a gravure method, a gravure offset method, a flexography method, a roll coating method, a comma coating method, a knife coating method or the like is preferable.

[0090] [Separation membrane] The separation membrane of the present invention is a separation membrane comprising a separation membrane support, and is usually a separation membrane formed by forming a membrane (separation membrane layer) having a separation function on the above-mentioned separation membrane support. Examples of such separation membranes include microfiltration membranes and ultrafiltration membranes used in water treatment at water purification plants and production of water for industrial processes, and nanofiltration membranes and semipermeable membranes such as reverse osmosis membranes used in the treatment of water for semiconductor manufacturing, boiler water, medical water, and pure water for laboratories, and in seawater desalination treatment.

[0091] As a method for producing a separation membrane, a method is preferably used in which a polymer solution is cast onto at least one surface of the above-mentioned separation membrane support to form a membrane having a separation function. In addition, when the separation membrane is a semipermeable membrane, it is also preferable to form the membrane having a separation function as a composite membrane including a support layer and a semipermeable membrane layer, and to laminate this composite membrane on at least one surface of the separation membrane support.

[0092] The polymer solution to be cast on the separation membrane support of the present invention has a separation function when it is formed into a membrane, and for example, a solution of polyarylethersulfone such as polysulfone or polyethersulfone, polyimide, polyvinylidene fluoride, cellulose acetate, etc. is preferably used. Among them, a solution of polysulfone and polyarylethersulfone is preferably used in terms of chemical, mechanical and thermal stability. The solvent can be appropriately selected depending on the membrane-forming material. In addition, when the separation membrane is a composite membrane including a support layer and a semipermeable membrane layer, a crosslinked polyamide membrane obtained by polycondensation of a polyfunctional acid halide and a polyfunctional amine is preferably used as the semipermeable membrane.

[0093] The separation membrane of the present invention preferably has a membrane peel strength of 15 cN / 15 mm or more and 80 cN / 15 mm or less. By setting the membrane peel strength to 15 cN / 15 mm or more, it is possible to prevent the separation membrane from peeling off from the support due to fluctuations in operating pressure when used as a fluid separation element or the so-called backwashing operation for cleaning the separation membrane. On the other hand, by setting the membrane peel strength to preferably 80 cN / 15 mm or less, it is possible to suppress excessive consumption of the polymer solution during the production of the separation membrane. Note that, when the separation membrane is a composite membrane including a support layer and a semipermeable membrane layer, the membrane peel strength refers to the peel strength between the support layer that is directly bonded to the separation membrane support and the separation membrane support. EXAMPLES

[0094] Next, the long-fiber nonwoven fabric of the present invention will be described in detail based on examples. However, the present invention is not limited to these examples. In addition, in the measurement of each physical property, unless otherwise specified, the measurement was performed based on the above-mentioned method.

[0095] [Measurement method] (1) Melting point of polyester (℃) The measurement was performed using a PerkinElmer differential scanning calorimeter "DSC-2" at a temperature increase rate of 20°C / min as described above, and the temperature giving the extreme value in the obtained melting endothermic curve was taken as the melting point.

[0096] (2) Intrinsic viscosity of polyester (IV) The intrinsic viscosity (IV) of polyester was measured by dissolving 8 g of sample in 100 mL of orthochlorophenol and measuring the relative viscosity η at 25°C using an Ostwald viscometer. r was calculated by the following formula. η r =η / η0=(t×d) / (t0×d0) (Here, η is the viscosity of the polymer solution, η0 is the viscosity of orthochlorophenol, t is the drop time of the solution (sec), and d is the density of the solution (g / cm 3 ), t0 is the fall time of orthochlorophenol (sec), and d0 is the density of orthochlorophenol (g / cm 3) Next, the relative viscosity η r The intrinsic viscosity (IV) was calculated from the following formula: Intrinsic viscosity (IV)=0.0242η r +0.2634.

[0097] (3) Average single fiber diameter (μm) The average single fiber diameter of the fibers according to the present invention was measured and calculated by the above-mentioned method using a scanning electron microscope "VHX-D500" manufactured by Keyence Corporation.

[0098] (4) Weight of long fiber nonwoven fabric (g / m 2 ) The basis weight of the long-fiber nonwoven fabric was measured and calculated by the method described above. The basis weight of the single-layer long-fiber nonwoven fabric was also calculated by the same method, except that the measurement subject was the single-layer long-fiber nonwoven fabric.

[0099] (5) Thickness of long fiber nonwoven fabric (mm) The thickness of the long-fiber nonwoven fabric was measured and calculated by the above-mentioned method using a thickness gauge "TECLOCK" (registered trademark) SM-114 manufactured by Teclock Corporation.

[0100] (6) Air permeability of long fiber nonwoven fabric (cm 3 / cm 2 / sec) The air permeability of the long fiber nonwoven fabric was measured and calculated by the above-mentioned method.

[0101] (7) Cross-sectional porosity of long fiber nonwoven fabric (%) The cross-sectional porosity of the long-fiber nonwoven fabric was measured and calculated by the method described above.

[0102] (8) Cross-sectional porosity CV value (%) of long fiber nonwoven fabric The cross-sectional porosity CV value of the long-fiber nonwoven fabric was measured and calculated by the above-mentioned method.

[0103] (9) Smoothness of long fiber nonwoven fabric (sec) The smoothness of the long fiber nonwoven fabric was measured and calculated by the above-mentioned method.

[0104] (10) Smoothness difference of long fiber nonwoven fabric (sec) The smoothness difference of the long fiber nonwoven fabric was measured and calculated by the above-mentioned method.

[0105] (11) Peel strength of separation membrane (cN / 15mm) Twenty test pieces measuring 130 mm in length x 50 mm in width were taken from the separation membrane formed with the prepared polysulfone membrane at equal intervals in the CD direction, Kikusui Kikraft tape was attached to the polysulfone membrane surface, and 8 cm of the polysulfone layer at one end was peeled off in the vertical direction from the separation membrane support. The polysulfone layer was fixed to one gripping part of a constant-rate extension-type tensile tester, and the separation membrane support was fixed to the other gripping part. The strength was measured under conditions of a gripping distance of 50 mm and a tensile speed of 50 mm / min, and the average strength from the gripping distance of 15 mm, where the strength became stable, to 75 mm was calculated, converted to 15 mm width units, and rounded to the first decimal place to obtain the membrane peel strength.

[0106] (12) Difference between maximum and minimum peel strength of separation membrane (cN / 15mm) The difference between the maximum and minimum values ​​of the 20 film peel strength measurements measured in (11) above was calculated, and the difference was rounded off to one decimal place to determine the difference between the maximum and minimum film peel strength values.

[0107] (13) Number of defects in membrane production The separation membrane with the polysulfone membrane formed was irradiated from the non-membrane-forming side with a 110W LED fluorescent lamp, and the parts that were penetrated were considered defects. The number of defects was counted and divided by the length of the separation membrane with the inspected polysulfone membrane to calculate the number of membrane defects (pieces / m) to one decimal place. Note that the inspection was performed within a range of 500 to 10,000 m, with the start of membrane production being set as 0 m. In other words, if the number of defects was 0.0 pieces / m after inspecting 500 m of the fabric, further inspection was performed up to a maximum of 1,000 m.

[0108] [Resin used] Next, the resins used in the examples and comparative examples will be described in detail. High melting point polymer: Polyethylene terephthalate (referred to as PET in Table 1) that has been dried to a moisture content of 50 mass ppm or less, has an intrinsic viscosity (IV) of 0.65, and a melting point of 260°C. Low melting point polymer: Copolymerized polyethylene terephthalate (referred to as cо-PET in Table 1) that has been dried to a moisture content of 50 ppm by mass or less, has an intrinsic viscosity (IV) of 0.64, has an isophthalic acid copolymerization rate of 11 mol%, and has a melting point of 230°C.

[0109] [Example 1] (The process of forming fibers) The high melting point polymer and the low melting point polymer were melted at temperatures of 295° C. and 280° C., respectively. Thereafter, the high melting point polymer was used as a core component and the low melting point polymer was used as a sheath component, and the core:sheath was spun from a discharge hole of a circular spinneret at a mass ratio of 80:20 at a spinneret temperature of 295° C., and then pulled by an ejector at a spinning speed of 4,900 m / min to spin a composite fiber having a circular cross section in which the low melting point polymer was disposed around the high melting point polymer.

[0110] (Step of forming a fiber web) The arrangement of the composite fibers spun in the above process was regulated by a fiber spreader, and then the fibers were deposited on a moving net conveyor, and a fiber web consisting of fibers with an average single fiber diameter of 11.4 μm was collected.

[0111] (Process for pre-thermocompression of fiber web) The fiber web repaired as described above is passed between a pair of upper and lower metal flat rolls, and pre-heat-pressed under the conditions of a surface temperature of 135°C and a linear pressure of 588N / cm for each flat roll, resulting in a basis weight of 36g / m 2 Thus, a single-layer long-fiber nonwoven fabric (a) in a temporarily bonded state was obtained.

[0112] (Laminated thermocompression process) Two sheets of the single-layer long-fiber nonwoven fabric (a) in the temporarily bonded state obtained above were overlapped, and the laminated nonwoven fabric was passed between the middle and bottom of a set of three flat rolls consisting of an upper resin elastic roll with a hardness (Shore D) of 94 and a crown value of 0 mm, a middle metal roll, and a lower resin elastic roll with a hardness (Shore D) of 66 and a crown value of 0.1 mm. The laminated nonwoven fabric was then folded back and passed through the top and middle parts for thermal compression bonding. The back side of the thermally compressed laminated nonwoven fabric that had been in contact with the elastic roll was then brought into contact with a metal cooling roll with a surface temperature of 45°C for 1 second, and the laminated nonwoven fabric was then cooled to a width of 100 cm and a basis weight of 72 g / m. 2 , thickness 0.09 mm, average single fiber diameter 11.4 μm, cross-sectional porosity 5%, cross-sectional porosity CV value 50%, air permeability 1.1 cm 3 / cm 2 A long-fiber nonwoven fabric was obtained with a smoothness of 34 seconds on side A, 9 seconds on side B, a smoothness difference in the width direction of side A of 11 seconds, and a smoothness difference in the width direction of side B of 3 seconds. At this time, the surface temperatures of the three flat rolls were 130°C on the top, 195°C in the middle, and 140°C on the bottom, and the linear pressure was 1314 N / cm.

[0113] (Process for forming separation membrane) The obtained long-fiber nonwoven fabric was used as a long-fiber nonwoven fabric for a separation membrane support and was used to form a separation membrane.

[0114] That is, the obtained long fiber nonwoven fabric for separation membrane support was unwound at a speed of 12 m / min, and a 16 mass% dimethylformamide solution (casting liquid) of polysulfone ("Udel" (registered trademark)-P3500 manufactured by Solvay Advanced Polymers) was cast on it to a thickness of 50 μm at room temperature (20 ° C.), and immediately immersed in pure water at room temperature (20 ° C.) for 10 seconds, then immersed in pure water at a temperature of 75 ° C. for 120 seconds, and then immersed in pure water at a temperature of 90 ° C. for 120 seconds, and wound up with a tension of 100 N / total width to form a polysulfone membrane and produce a separation membrane. At this time, no strike-through of the casting liquid was observed at all, and the width of the produced separation membrane was 100 cm, the membrane peel strength was 33 cN / 15 mm, the difference between the maximum and minimum values ​​of the membrane peel strength was 30 cN / 15 mm, and the number of membrane defects was 0.1 / m. The results are shown in Table 1.

[0115] [Example 2] In the step of forming fibers, the amount of molten polymer spun out from the nozzle of the circular spinneret was changed to change the average single fiber diameter from 11.4 μm to 10.5 μm, and in the step of forming a fiber web, the speed of the moving net conveyor was changed to change the basis weight of the single-layer long-fiber nonwoven fabric (a) to 36 g / m 2 From 38 g / m 2 A long-fiber nonwoven fabric for a separation membrane support was obtained in the same manner as in Example 1, except that in the (step of pre-thermocompression bonding of the fiber web), the temperature of the metal flat roll during pre-thermocompression bonding was changed from 135°C to 130°C, and in the (step of lamination and thermocompression bonding), the surface temperatures of the three flat rolls during thermocompression bonding were changed from 130°C to 135°C on the top and from 195°C to 190°C on the middle, and the linear pressure was changed from 1314 N / cm to 1196 N / cm. This long-fiber nonwoven fabric had a width of 100 cm and a basis weight of 76 g / m 2 , thickness 0.09 mm, average single fiber diameter 10.5 μm, cross-sectional porosity 8%, cross-sectional porosity CV value 37%, air permeability 0.8 cm 3 / cm 2 The smoothness of the A side was 35 seconds, the smoothness of the B side was 9 seconds, the difference in the width direction of the A side was 9 seconds, and the difference in the width direction of the B side was 5 seconds. The width of the produced separation membrane was 100 cm, the membrane peel strength was 56 cN / 15 mm, the difference between the maximum and minimum membrane peel strengths was 36 cN / 15 mm, and the number of membrane defects was 0.0 / m. The results are shown in Table 1.

[0116] [Example 3] A long-fiber nonwoven fabric for a separation membrane support was obtained in the same manner as in Example 2, except that in (the step of preliminarily thermocompression bonding the fiber web), the temperatures of the metal flat rolls during preliminarily thermocompression bonding were changed from 130°C for both the top and bottom to 140°C for the top and 130°C for the bottom, and in (the step of laminating and thermocompression bonding), the surface temperatures of the three flat rolls during thermocompression bonding were changed from 135°C for the top to 110°C and from 140°C for the bottom to 130°C, and the linear pressure was changed from 1196 N / cm to 1294 N / cm. This long-fiber nonwoven fabric had a width of 100 cm and a basis weight of 76 g / m 2 , thickness 0.10 mm, cross-sectional porosity 8%, cross-sectional porosity CV value 58%, ventilation volume 0.9 cm 3 / cm 2The smoothness of the A side was 40 seconds, the smoothness of the B side was 10 seconds, the difference in the smoothness of the A side in the width direction was 13 seconds, and the difference in the smoothness of the B side in the width direction was 8 seconds. The width of the produced separation membrane was 100 cm, the membrane peel strength was 68 cN / 15 mm, the difference between the maximum and minimum membrane peel strengths was 35 cN / 15 mm, and the number of membrane defects was 0.0 / m. The results are shown in Table 1.

[0117] [Example 4] A long-fiber nonwoven fabric for a separation membrane support was obtained in the same manner as in Example 2, except that in the (step of forming fibers), the amount of molten polymer spun out from the nozzle holes of the circular spinneret was changed to change the average single fiber diameter of the fibers from 10.5 μm to 9.5 μm, and in the (step of lamination and thermocompression bonding), the surface temperature of the inside of the three flat rolls during thermocompression bonding was changed from 190° C. to 180° C. This long-fiber nonwoven fabric had a width of 100 cm and a basis weight of 76 g / m 2 , thickness 0.09 mm, average single fiber diameter 9.5 μm, cross-sectional porosity 4%, cross-sectional porosity CV value 30%, air permeability 0.9 cm 3 / cm 2 / sec, the smoothness of side A was 32 seconds, the smoothness of side B was 7 seconds, the difference in smoothness in the width direction of side A was 10 seconds, and the difference in smoothness in the width direction of side B was 4 seconds. The width of the produced separation membrane was 100 cm, the membrane peel strength was 50cN / 15mm, the difference between the maximum and minimum membrane peel strengths was 32cN / 15mm, and the number of membrane defects was 0.0 / m. The results are shown in Table 1.

[0118] [Comparative Example 1] A long-fiber nonwoven fabric for a separation membrane support was obtained in the same manner as in Example 1, except that in the step of laminating and thermocompression bonding, the hardness (Shore D) of the upper resin elastic roll was changed from 94 to 91, the hardness (Shore D) of the lower resin elastic roll was changed from 66 to 75, the crown value was changed from 0.1 mm to 0 mm, and the linear pressure during thermocompression bonding was changed from 1314 N / cm to 1726 N / cm. This long-fiber nonwoven fabric had a width of 100 cm and a basis weight of 72 g / m 2 , thickness 0.09 mm, cross-sectional porosity 20%, cross-sectional porosity CV value 68%, ventilation volume 1.5 cm 3 / cm 2The smoothness of the A side was 48 seconds, the smoothness of the B side was 17 seconds, the difference in the smoothness of the A side in the width direction was 16 seconds, and the difference in the smoothness of the B side in the width direction was 11 seconds. The width of the produced separation membrane was 100 cm, the membrane peel strength was 35 cN / 15 mm, the difference between the maximum and minimum membrane peel strength was 49 cN / 15 mm, and the number of membrane defects was 0.5 / m. The results are shown in Table 1.

[0119] [Comparative Example 2] (Paper-made non-woven fabric) Made of polyethylene terephthalate resin with a melting point of 260°C, the average single fiber diameter is 11.0μm and the basis weight is 35g / m 2 A nonwoven paper fabric (x) having a thickness of 0.2 mm and a polyethylene terephthalate resin having a melting point of 260°C, an average single fiber diameter of 10 μm, and a basis weight of 35 g / m 2 A papermaking nonwoven fabric (y) having a thickness of 0.2 mm was prepared.

[0120] (Laminated thermocompression process) The prepared papermaking nonwoven fabric (x) and papermaking nonwoven fabric (y) are stacked one by one with the papermaking nonwoven fabric (x) on top, and the stack is passed between a pair of flat rolls, the upper one being a metal roll and the lower one being an elastic roll made of cotton paper with a hardness (Shore D) of 85, to heat and press the fabric into a sheet having a width of 100 cm and a basis weight of 70 g / m. 2 , thickness 0.09 mm, average single fiber diameter 10.5 μm, cross-sectional porosity 30%, cross-sectional porosity CV value 62%, air permeability 2.1 cm 3 / cm 2 A long-fiber nonwoven fabric for separation membrane support was obtained with a smoothness of 26 seconds on side A, 18 seconds on side B, a smoothness difference in the width direction of side A of 8 seconds, and a smoothness difference in the width direction of side B of 6 seconds. At this time, the surface temperatures of the two flat rolls were 230°C on the top and 130°C on the bottom, and the linear pressure was 1176 N / cm.

[0121] (Process for forming separation membrane) A separation membrane was obtained in the same manner as in Example 1. The width of the produced separation membrane was 100 cm, the membrane peel strength was 74 cN / 15 mm, the difference between the maximum and minimum membrane peel strengths was 42 cN / 15 mm, and the number of membrane defects was 0.1 / m. The results are shown in Table 1.

[0122] [Table 1]

[0123] The properties of the obtained nonwoven fabric are as shown in Table 1. All of the long-fiber nonwoven fabrics of Examples 1 to 4 had an average single fiber diameter of 10.0 μm to 20.0 μm, a cross-sectional porosity of 1% to 10%, and a cross-sectional porosity CV value of 1% to 60%, and showed good membrane peel strength and a difference between the maximum and minimum membrane peel strength when used as a separation membrane. The long-fiber nonwoven fabrics also showed good membrane formability with few membrane formation defects. On the other hand, Comparative Example 1 showed a large density difference within the long-fiber nonwoven fabric, so the difference between the maximum and minimum membrane peel strength was large and the number of membrane formation defects was large, which was inferior. Comparative Example 2 showed a large cross-sectional porosity CV value, so the difference between the maximum and minimum membrane peel strength was large and inferior.

Claims

1. A long-fiber nonwoven fabric made of fibers containing a thermoplastic resin as a main component, the long-fiber nonwoven fabric having a cross-sectional porosity of 1% or more and 10% or less, a CV value of the cross-sectional porosity of 1% or more and 60% or less, and an average single fiber diameter of 10.0 μm or more and 20.0 μm or less.

2. 2. The long-fiber nonwoven fabric according to claim 1, wherein the fibers are composite fibers in which a low-melting-point polymer having a melting point lower than that of a high-melting-point polymer is disposed around the high-melting-point polymer.

3. The weight of the long fiber nonwoven fabric is 20 g / m 2 120g / m or more 2 3. The long-fiber nonwoven fabric according to claim 1 or 2, wherein:

4. 3. The long-fiber nonwoven fabric according to claim 1, wherein the difference R between the maximum and minimum values ​​of the Oken smoothness on one side of the long-fiber nonwoven fabric is 5 seconds or more and 20 seconds or less, and the difference R between the maximum and minimum values ​​of the Oken smoothness on the other side of the long-fiber nonwoven fabric is 1 second or more and 10 seconds or less.

5. A separation membrane support comprising the long-fiber nonwoven fabric according to claim 1 or 2.

6. A separation membrane comprising the separation membrane support according to claim 5 .

Citation Information

Patent Citations

  • Separation membrane-supporting body, separation membrane using the same, and fluid-separating element

    JP2013071106A

  • Separation membrane

    JP2019093366A