Substrate processing method and substrate processing apparatus

By applying hydrogen fluoride and ammonia gases to react with and remove silicon oxide, and using metal halide gas to eliminate metal oxide components, the method effectively addresses the oxide film removal challenge, ensuring reduced wiring resistance in semiconductor substrates.

JP2024155049AActive Publication Date: 2024-10-31TOKYO ELECTRON LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023069426
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2024-10-31
Estimated Expiration
2043-04-20

AI Technical Summary

Technical Problem

Existing methods fail to effectively remove the oxide film on the surface of metal silicide layers in semiconductor substrates, leading to increased wiring resistance during the manufacturing process.

Method used

A method involving the application of hydrogen fluoride gas and ammonia gas to react with and remove silicon oxide from the oxide film, followed by the use of metal halide gas to remove metal oxide components, utilizing a substrate processing apparatus with specific modules for each step.

Benefits of technology

The method successfully removes the oxide film, preventing an increase in wiring resistance and ensuring efficient conductor embedding in semiconductor substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155049000001_ABST
    Figure 2024155049000001_ABST
Patent Text Reader

Abstract

To provide a technique for removing oxide films on a surface of metal silicide layers formed in the recesses of a substrate.SOLUTION: A substrate processing method includes the steps of: removing an oxide film on the surface of metal silicide layer provided by laminating an insulating layer with recesses formed in the silicon-containing layer and laminating the silicon-containing layer within the recesses, by supplying hydrogen fluoride gas and ammonia gas to the oxide film and reacting with the silicon oxide content contained in the oxide film; and supplying metal halide gas to the oxide film to react with the metal oxide content in the oxide film and remove it.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for processing a substrate and an apparatus for processing a substrate. [Background technology]

[0002] In the manufacturing process of a semiconductor device, a process is performed in which a recess such as a via hole or a trench is formed in an insulating layer formed on a semiconductor wafer (hereinafter also referred to as a "wafer"), which is a substrate, and a conductor, which is a wiring material, is embedded in the recess. In this case, a natural oxide film may be formed on the surface of the metal exposed in the recess due to contact with the atmosphere. If the conductor is embedded without removing such a natural oxide film, it will cause an increase in the wiring resistance.

[0003] Patent Document 1 describes a technique for exposing a substrate including a metal oxide layer that may include one or more metals selected from alkali metals, alkaline earth metals, transition metals, lanthanides, actinides, and late transition metals, and Si, to a metal halide, thereby etching the substrate. Patent Document 2 describes a technique for exposing an oxide layer including one or more of hafnium, tungsten, molybdenum, and titanium to a fluorinating agent to form a fluoride layer, and then exposing the oxide layer to the halide etchant to remove the fluoride layer. However, these patent documents do not contain any description of a technique for effectively removing an oxide film of a metal silicide. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2021-507509 [Patent Document 2] Patent Publication No. 2022-536475 Summary of the Invention [Problem to be solved by the invention]

[0005] The present disclosure provides a technique for removing an oxide film on the surface of a metal silicide layer formed in a recess of a substrate. [Means for solving the problem]

[0006] The method of processing a substrate of the present disclosure includes: a step of laminating an insulating layer having a recess formed therein on a silicon-containing layer, and supplying hydrogen fluoride gas and ammonia gas to an oxide film on a surface of a metal silicide layer laminated on the silicon-containing layer in the recess, thereby reacting the oxide film with silicon oxide contained in the oxide film and removing the oxide film; and supplying a metal halide gas to the oxide film to react with and remove the metal oxide contained in the oxide film. Effect of the Invention

[0007] According to the present disclosure, it is possible to remove an oxide film on the surface of a metal silicide layer formed in a recess of a substrate. [Brief description of the drawings]

[0008] [Figure 1] 1 is a plan view showing a configuration example of a substrate processing apparatus according to an embodiment of the present disclosure; [Diagram 2] 2 is a vertical sectional side view showing a configuration example of a Ti film formation module provided in the substrate processing apparatus. FIG. [Diagram 3] 1 is an explanatory diagram showing an example of a flow of a wafer process according to an embodiment; [Figure 4A] 2 is a first enlarged vertical cross-sectional side view of a surface of a wafer undergoing processing according to an embodiment; [Figure 4B] FIG. 4 is a second enlarged vertical cross-sectional side view of the front side of the wafer. [Figure 4C] FIG. 4 is a third enlarged vertical cross-sectional side view of the front side of the wafer. [Figure 4D] FIG. 4 is a fourth enlarged vertical cross-sectional side view of the wafer of the front surface of the wafer. [Figure 4E] FIG. 5 is a fifth enlarged vertical cross-sectional side view of the wafer of the surface of the wafer. [Figure 4F] FIG. 6 is a sixth enlarged longitudinal cross-sectional side view of the wafer of the surface of the wafer. [Diagram 5] FIG. 11 is a plan view showing an example of the configuration of a substrate processing apparatus according to a second embodiment. [Figure 6] FIG. 11 is an explanatory diagram showing an example of a flow of a wafer processing according to the second embodiment. [Figure 7] FIG. 11 is a plan view showing an example of the configuration of a substrate processing apparatus according to a third embodiment. [Figure 8] FIG. 11 is an explanatory diagram showing an example of a flow of a wafer processing according to a third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] <Substrate processing device 1> Hereinafter, the oxide film (MoSiO X An embodiment of an apparatus (hereinafter, referred to as "substrate processing apparatus 1") having a function of removing the Ru film 67, which is a conductor, and forming the Ru film 67 will be described.

[0010] Before starting to explain the configuration of the substrate processing apparatus 1, an example of the surface structure of a wafer W to be processed by the substrate processing apparatus 1 will be described. As shown in Fig. 4A, a wafer W to be processed has a SiO layer 62 laminated on a SiGe layer 61, which is a silicon-containing layer, and a recess 60 for embedding ruthenium (Ru), which is a conductor, is formed in the SiO layer 62. A molybdenum (Mo) layer for adjusting the Schottky barrier height is formed at the bottom of the recess 60, and a MoSi layer 64 is formed by diffusion of silicon (Si) from the SiGe layer 61.

[0011] When the wafer W having the above-described configuration is transported in a semiconductor manufacturing factory toward the substrate processing apparatus 1, the surface of the MoSi layer 64 is covered with an oxide film of MoSiO X Therefore, the substrate processing apparatus 1 of the present embodiment uses the MoSiO X The layer 65a is removed before Ru is embedded.

[0012] 1 is a schematic plan view showing an example of the configuration of a substrate processing apparatus 1. This substrate processing apparatus 1 includes an atmospheric transfer chamber 11, a load lock chamber 12, a first substrate transfer chamber 13, a second substrate transfer chamber 14, and a plurality of processing modules 151-154.

[0013] The first substrate transfer chamber 13 and the second substrate transfer chamber 14 are each configured to have a rectangular shape in a plan view, and are connected via, for example, two transfer units 17. The insides of the first and second substrate transfer chambers 13, 14 and the transfer unit 17 are set to a vacuum pressure atmosphere, and the pressures are configured to be the same. In addition, first and second transfer mechanisms 131, 141 are disposed inside the first and second substrate transfer chambers 13, 14, respectively.

[0014] The transfer unit 17 is configured to transfer the wafer between the first transfer mechanism 131 provided in the first substrate transfer chamber 13 and the second transfer mechanism 141 provided in the second substrate transfer chamber 14. The first substrate transfer chamber 13, the second substrate transfer chamber 14 and the transfer unit 17 correspond to the vacuum transfer chamber in this embodiment. The first transfer mechanism 131 and the second transfer mechanism 141 correspond to the substrate transfer mechanism in this embodiment.

[0015] The direction in which the first and second substrate transfer chambers 13, 14 are lined up is the length direction, with the first substrate transfer chamber 13 at the front side and the second substrate transfer chamber 14 at the rear side. In this case, an atmospheric transfer chamber 11 set to an atmospheric pressure atmosphere is connected to the front side of the first substrate transfer chamber 13 via, for example, three load lock chambers 12. Between the first and second substrate transfer chambers 13, 14 and the transfer section 17, between the load lock chamber 12 and the first substrate transfer chamber 13, and between the load lock chamber 12 and the atmospheric transfer chamber 11, there are wafer transfer ports and gate valves for opening and closing the transfer ports, respectively, but these are omitted from the drawings.

[0016] For example, four load ports 101 are connected to the atmospheric transfer chamber 11, and a carrier C accommodating a plurality of wafers W is placed on each load port 101. An atmospheric transfer mechanism 111 is provided in the atmospheric transfer chamber 11, and can transfer the wafers W between the carrier C connected to the atmospheric transfer chamber 11 and the load lock chamber 12.

[0017] As viewed from the front side, one COR (Chemical Oxide Removal) module 151, one PHT (Post Heat Treatment) module 152, and two Ti film formation modules 153 are connected to each of the two walls of the first substrate transfer chamber 13. A first transfer mechanism 131 provided in the first substrate transfer chamber 13 is configured to transfer wafers W between these four modules 151 to 153, the transfer section 17, and the load lock chamber 12. In FIG. 1, symbol GV1 indicates a gate valve.

[0018] The COR treatment performed in the COR module 151 and the PHT treatment performed in the PHT module 152 are performed using the above-mentioned MoSiO X This is a pre-cleaning process to remove silicon oxide contained in the layer 65a. X The layer 65a is composed of a complex oxide containing Si, Mo, and oxygen (O). In the present disclosure, the oxidized portion of Si (SiO X ) is called "silicon oxide", and the oxidized part of Mo (MoO X ) is also called "molybdenum oxide". The oxide film of the metal silicide layer, MoSiO X In the layer 65a, the "molybdenum oxide content" corresponds to the "metal oxide content" of the metal silicide layer.

[0019] The COR module 151 is configured to perform an etching process (COR process) of the native oxide film using hydrogen fluoride (HF) gas and ammonia (NH3) gas. The PHT module 152 is configured to perform a PHT process in which a reaction product generated in the COR process is sublimated and removed by heating the wafer W. An example of the configuration of the COR module 151 and the PHT module 152 will be described later. The COR module 151 corresponds to the first process module in this embodiment.

[0020] Next, the Ti film forming module 153 is configured to form a Ti layer 66 which is a metal layer for contact provided between the MoSi layer 64 and the Ru wiring 67a. Furthermore, the Ti film forming module 153 of this embodiment forms the MoSiO X Layer 65a (already SiO X Since "MoO" has been removed, the following is X The MoO X The layer 65b corresponds to the metal oxide portion of this embodiment. X From the viewpoint of removing the layer 65b, the Ti film forming module 153 corresponds to the second processing module of this embodiment. A specific configuration example of the Ti film forming module 153 will be described later with reference to FIG.

[0021] Further, as viewed from the front side, two Ru film formation modules 154 are connected to each of the two left and right walls of the second substrate transfer chamber 14, totaling four Ru film formation modules 154. The second transfer mechanism 141 is configured to transfer wafers W between these four Ru film formation modules 154 and the transfer unit 17. In Fig. 2, symbol GV2 indicates a gate valve.

[0022] Each Ru film forming module 154 is configured to form a Ru film 67, for example, by a CVD (Chemical Vapor Deposition) method using a source gas of Ru which is a conductor. The Ru film forming module 154 corresponds to the fourth processing module of the present embodiment.

[0023] <Ti film forming module 153> Next, a specific configuration example of the Ti film forming module 153 will be described with reference to FIG. 2. The Ti film forming module 153 is configured to supply a film forming gas to the wafer W and form a Ti layer 66 by a plasma CVD method. Further, the Ti film forming module 153 supplies a metal halide gas to the wafer W on which the silicon oxide component of the MoSiO X layer 65a has been removed, and also has a function of removing the remaining MoO X layer 65b.

[0024] FIG. 2 is a longitudinal side view of the Ti film forming module 153 of the present embodiment. The Ti film forming module 153 has corrosion resistance to chlorine and includes a substantially cylindrical processing container 210 made of a grounded metal. In the central portion of the bottom surface of the processing container 210, for example, a cylindrical exhaust chamber 211 protruding downward is formed, and an exhaust passage 212 is connected to the side surface of the exhaust chamber 211. A vacuum exhaust portion 213 including a pressure regulating valve such as a butterfly valve and a vacuum pump is connected to the exhaust passage 212. The vacuum exhaust portion 213 serves to evacuate the inside of the processing container 210 to a preset vacuum pressure. The processing of the wafer W is performed in the space inside the processing container 210.

[0025] On the side surface of the processing container 210, a loading / unloading port 214 for loading and unloading the wafer W between the processing container 210 and the above-described first substrate transfer chamber 13 is formed. The loading / unloading port 214 is configured to be openable and closable by a gate valve 215 (GV1 in FIG. 1). Further, a heater 216 for adjusting the temperature inside the processing container 210 is embedded in the wall portion constituting the processing container 210.

[0026] A mounting table 22 for holding the wafer W substantially horizontally is provided within the processing vessel 210. The mounting table 22 is supported by a support portion 221 extending from the bottom of the exhaust chamber 211. A heater 220 serving as a heating portion is embedded in the mounting table 22, and the wafer W can be heated to a set temperature. In this example, the heating temperature of the wafer W is set within a range of 350 to 800°C, for example, to 450°C.

[0027] Further, a high frequency power supply 223 that supplies high frequency power for attracting ions is connected to the mounting table 22 via a matching box 222. Furthermore, the mounting table 22 is provided with lift pins (not shown) for holding and lifting the wafer W on the mounting table 22. The wafer W can be transferred between the mounting table 22 and the first transfer mechanism 131 on the first substrate transfer chamber 13 side by lifting and lowering the lift pins.

[0028] A flat, disk-shaped shower head 23 is provided on the ceiling surface of the processing vessel 210 to supply a substrate processing gas toward the wafer W. The shower head 23 is attached to the processing vessel 210 via an insulating member 217. A diffusion chamber 231 for diffusing gas is formed inside the shower head 23. A large number of discharge holes 232 for discharging gas toward the wafer W are provided in a distributed manner on the bottom surface of the shower head 23. A heater 235 is embedded in the upper surface side of the shower head 23.

[0029] A high frequency power supply 234 that supplies high frequency power for plasma generation is connected to the shower head 23 through a matching box 233. That is, the substrate processing apparatus 1 of this embodiment is configured as a parallel plate type plasma processing apparatus by the shower head 23 that constitutes an upper electrode and the mounting table 22 that constitutes a lower electrode. The wafer W is placed in the space between the shower head 23 and the mounting table 22, and a film forming gas is supplied and high frequency power is applied, so that the gas is ionized to form plasma. The high frequency power supply 234 may be configured to supply high frequency power of any of the following frequencies: 450 KHz, 13.56 MHz, 27 MHz, 40 MHz, 60 MHz, 100 MHz, and 2.45 GHz. For example, the high frequency power supply 234 supplies high frequency power in a range of more than 0 W and less than or equal to 2000 W.

[0030] The downstream end of the gas supply path 40 is connected to the diffusion chamber 231 of the shower head 23. A TiCl4 gas supply pipe 41, which is a flow path for supplying TiCl4 gas constituting the film formation gas of the Ti layer 66, an Ar gas supply pipe 42, which is a flow path for supplying Ar gas added for plasma generation, and an H2 gas supply pipe 43, which is a flow path for supplying H2 gas, which is a reactive gas, join at the upstream side of the gas supply path 40.

[0031] A TiCl4 gas supply source 410 is connected to the upstream end of the TiCl4 gas supply pipe 41, and a flow rate regulator M41 and a valve V41 are disposed in this order from the upstream side. An Ar gas supply source 420 is connected to the upstream end of the Ar gas supply pipe 42, and a flow rate regulator M42 and a valve V42 are disposed in this order from the upstream side. An H2 gas supply source 430 is connected to the upstream end of the H2 gas supply pipe 43, and a flow rate regulator M43 and a valve V43 are disposed in this order from the upstream side.

[0032] The mixed gas (film forming gas) of TiCl 4 gas, H 2 gas, and Ar gas flows into the diffusion chamber 231 of the shower head 23 via the gas supply path 40 and is supplied into the processing vessel 210 through the outlet holes 232 .

[0033] Furthermore, a WCl5 gas supply pipe 51 joins the gas supply line 40 on the upstream side. WCl5 gas is MoO X This corresponds to the metal halide gas for removing the layer 65b. A WCl5 gas supply source 510 is connected to the upstream end of the WCl5 gas supply pipe 51, and a flow rate regulator M51 and a valve V51 are provided in this order from the upstream side. The supply source 510 for supplying WCl5 gas and the flow rate regulator M51 constitute the metal halide gas supply unit of this embodiment. The WCl5 gas also flows into the diffusion chamber 231 of the shower head 23 through the gas supply path 40, and is supplied into the processing vessel 210 through the outlet hole 232.

[0034] <Other processing modules 151, 152, 153> Although not shown, the COR module 151, the PHT module 152, and the Ru film formation module 154 are similar to the Ti film formation module 153 described above in that they each include a processing vessel 210 and a mounting table 22. In the COR module 151, a mixed gas of HF gas and NH3 gas used in the COR process is supplied to the processing vessel 210 via a gas supply path 40. The gas supply sources and flow rate regulators that supply the HF gas and NH3 gas respectively constitute the mixed gas supply unit of this embodiment.

[0035] In the PHT module 152, N2 gas forming an inert gas atmosphere in which the PHT process is performed is supplied to the processing chamber 210 via the gas supply line 40. In the PHT module 152, the wafer W is heated by the heater 220 of the mounting table 22 to a temperature within a range of 60 to 250°C, for example, to 200°C. Furthermore, the COR module 151 and the PHT module 152 of this embodiment are not provided with a high frequency power source 234 for generating plasma.

[0036] Furthermore, in the Ru film forming module 154, the raw material gas for the Ru film 67, Ru3(CO), 12 The gas and CO gas as a carrier gas are supplied to the processing chamber 210 via the gas supply line 40. 12The gas supply source and the flow rate regulator for supplying the gas and the CO gas correspond to the raw material gas supply unit of this embodiment. The Ru film formation module 154 of this embodiment is configured to form the Ru film 67 by, for example, a thermal CVD method. Therefore, unlike the Ti film formation module 153 described with reference to FIG. 2, it does not include the matcher 233 and the high frequency power source 234 connected to the shower head 23, and the matcher 222 and the high frequency power source 223 connected to the mounting table 22.

[0037] <Control unit 100> The substrate processing apparatus 1 having the above-mentioned configuration includes a control unit 100 as shown in Fig. 1 and Fig. 2. The control unit 100 is configured with a computer including a storage unit storing a program, a memory, and a CPU. The program includes instructions (steps) for executing substrate processing using various modules 151-154 by outputting control signals from the control unit 100 to each unit of the substrate processing apparatus 1 and controlling the supply and cut-off of each gas and the supply of high-frequency power. The program is stored in a storage unit of the computer, such as a flexible disk, a compact disk, a hard disk, an MO (magneto-optical disk), a non-volatile memory, etc., and is read out from the storage unit and installed in the control unit 100.

[0038] <Substrate processing> The substrate processing carried out by the substrate processing apparatus 1 having the above-described configuration will be described with reference to FIG. 3 and FIGS. 4A to 4F. In the substrate processing apparatus 1, first, the atmospheric transfer mechanism 111 takes out the wafer W accommodated in the carrier C and transfers it to the load lock chamber 12 at atmospheric pressure, and adjusts the inside of the load lock chamber 12 to a vacuum pressure atmosphere. Next, the first transfer mechanism 131 transfers the wafer W in the load lock chamber 12 to the COR module 151, and places it on the mounting table 22 in the processing vessel 210.

[0039] In the COR module 151, the temperature of the wafer W placed on the mounting table 22 is adjusted to 60° C. or lower, for example, 27° C. Then, a mixed gas of HF gas and NH3 gas is supplied from the mixed gas supply unit described above to the wafer W in the processing chamber 210 (FIG. 4A). It is known that at temperatures of 60° C. or lower, the probability of HF gas and NH3 gas molecules being adsorbed to the wafer W is high. For this reason, the molecules of each gas are densely adsorbed on the surface of the wafer W, and the MoSiO X Molecules of these gases also reach and are adsorbed on the layer 65a. As a result, MoSiO X The silicon oxide (SiO X A chemical reaction between the silicon oxide particles 10 and the HF and NH3 molecules proceeds, and a reaction product is formed, whereby the silicon oxide is removed (etched) (process P11 in FIG. 3, a process for removing the silicon oxide).

[0040] The reaction products generated in the COR process include ammonium fluorosilicate ((NH4)2SiF6) and moisture (H2O). The reaction products adhere to the bottom and sidewall surfaces of the recess 60, the upper surface of the SiO layer 62, and the like. In the COR process, ammonium fluoride (NH4F) is also generated by the reaction between hydrogen fluoride gas and ammonia gas. The ammonium fluoride molecules also act as an etchant and react with silicon oxide to form reaction products. In the COR process, ammonium fluoride itself may also be deposited on the surface of the wafer W as a solid component.

[0041] The wafer W from which silicon oxide has been removed by the COR process is transferred from the COR module 151 to the PHT module 152 and placed on the mounting table 22 in the processing chamber 210. In the PHT module 152, the wafer W is heated to sublimate and remove reaction products and solid ammonium fluoride generated in the COR process. Specifically, N2 gas is supplied into the processing chamber 210, and the temperature of the wafer W placed on the mounting table 22 is adjusted to 200°C. As a result, the reaction products and solid ammonium fluoride adhering to the heated wafer W are sublimated, and are discharged to the outside of the processing chamber 210 together with the N2 gas (process P11 in FIG. 3, a process for removing reaction products).

[0042] Next, the wafer W is transferred by the first transfer mechanism 131 to the Ti film forming module 153. As described above, in the Ti film forming module 153, MoSiO X MoO X Two processes are performed: removing the layer 65b (metal oxide portion) and depositing the Ti layer 66.

[0043] First, after the wafer W is placed on the mounting table 22 of the Ti film formation module 153, the inside of the processing container 210 is evacuated to a preset pressure by the vacuum exhaust unit 213. The wafer W is heated to the above-mentioned 450° C. by the heater 220. Thereafter, WCl5 gas is supplied into the processing container 210 from the metal halide gas supply unit (FIG. 4B).

[0044] As shown in FIG. 4B, when the WCl5 gas reaches the wafer W, the reaction shown in the following formula (1) proceeds. 2MoO3(s)+2WCl5(g)→WO2Cl2(g)+2MoO2Cl2(g)+WCl2(s) …(1)

[0045] Solid WCl2 remains on the surface of the wafer W. When residual chlorine is undesirable, H2 gas is supplied from the H2 gas supply source 430 together with WCl5 gas to cause the reaction shown in formula (2) below to proceed. WCl2(s)+H2(g)→W(s)+2HCl(g) …(2) By reacting with H2 gas, chlorine is removed as HCl gas, and only metallic tungsten (W) remains on the surface of the wafer W.

[0046] By proceeding with the above formula (1), MoO remaining in the recess 60 after the COR treatment is X The layer 65b can be removed (step P12 in FIG. 3, a step of removing metal oxide). As a result, as shown in FIG. 4C, the inside of the recess 60 is left with the oxide on the surface of the MoSi layer 64 (MoSiO X Layer 65a) is now removed.

[0047] MoO X After the process of removing the layer 65b is completed, a Ti layer 66, which is a metal layer for contact, is formed. Specifically, the supply of WCl5 gas to the processing vessel 210 of the Ti film forming module 153 is stopped. Then, while continuing the heating of the wafer W and the pressure adjustment in the processing vessel 210, TiCl4 gas, H2 gas, and Ar gas are supplied from the gas supply sources 410, 420, and 430 at preset flow rates. As a result, a film forming gas, which is a mixture of these gases, is introduced into the processing vessel 210. Furthermore, high frequency power is applied from the high frequency power source 234 to turn the film forming gas into plasma, and the film forming of Ti on the wafer W proceeds (process P13 in FIG. 3).

[0048] After the Ti film is formed for a preset time, the supply of the film forming gas and the application of the high frequency power are stopped, resulting in the formation of a Ti layer 66 on the bottom surface of the recess 60, as shown in FIG.

[0049] Next, the wafer W is transferred to the Ru film formation module 154 via the first transfer mechanism 131, the transfer section 17, and the second transfer mechanism 141. An inert gas is supplied to the first substrate transfer chamber 13, the transfer section 17, and the second substrate transfer chamber 14 to prevent gas diffusion from the film formation module. The pressure is controlled to, for example, 100 Pa within a range of 20 to 200 Pa. In addition, in order to prevent oxidation of the surfaces during transfer, the ultimate vacuum of a vacuum exhaust mechanism (not shown) that evacuates these spaces (the first substrate transfer chamber 13, the transfer section 17, and the second substrate transfer chamber 14) is set to 1.33×10 -5 The pressure is set to be equal to or lower than Pa. In the Ru film formation module 154, a Ru film 67 is formed so that Ru is embedded in the upper surface side of the Ti layer 66 formed in the recess 60 (P14 in FIG. 3, a process of embedding a conductor).

[0050] Specifically, the wafer W is carried into the processing chamber 210 of the Ru film forming module 154 and placed on the mounting table 22, and the wafer W is heated by the heater 220 to, for example, 150° C. within a range of 130 to 200° C. Furthermore, the pressure in the processing chamber 210 is adjusted, and Ru3(CO) 12 Gas (including CO gas as a carrier gas) is supplied.

[0051] As a result, the Ru3(CO) supplied into the processing vessel 210 12 Thermal CVD proceeds, in which MoSiO is thermally decomposed on the wafer W. By carrying out thermal CVD for a preset period, MoSiO is formed as shown in FIG. X A Ru film 67 can be embedded in the recess 60 from which the layer 65a has been removed.

[0052] After the formation of the Ru film 67 is completed, the wafer W is transferred to the load lock chamber 12 via the second transfer mechanism 141, the delivery unit 17, and the first transfer mechanism 131. Next, the atmosphere in the load lock chamber 12 is switched to an atmospheric pressure atmosphere, and the processed wafer W is returned to the carrier C by the atmospheric transfer mechanism 111. The transferred wafer W is polished by an external CMP (Chemical Mechanical Polishing) device. By this process, the upper surface side is removed, and the wafer W having Ru wiring 67a embedded in the recesses 60 can be obtained as shown in FIG. 4F.

[0053] According to the above-described embodiment, the oxide film (MoSiO X layer 65a) can be removed. As a result, it is possible to suppress an increase in wiring resistance after the Ru film 67 (Ru wiring 67a) is embedded in the recess 60. In particular, in the substrate processing apparatus 1 in which the wafer W is transferred between the processing modules 151 to 154 via the first and second substrate transfer chambers 13 and 14, it is possible to perform substrate processing while avoiding exposure to the atmosphere, and it is possible to suppress the formation of an unnecessary natural oxide film.

[0054] <Second embodiment> Next, the configuration and operation of the substrate processing apparatus 1a according to the second embodiment will be described with reference to Figures 5 and 6. In the substrate processing apparatuses 1a and 1b shown in Figures 5 and 7, components common to the substrate processing apparatus 1 described with reference to Figure 1 are denoted by the same reference numerals as those shown in those figures.

[0055] The substrate processing apparatus 1a according to the second embodiment uses WCl5 gas, which is a metal halide, to produce MoO X This structure addresses the problem that a reaction other than that of the above-mentioned formula (1) also occurs when removing the layer 65b. As will be described later, this reaction involves MoO XInstead of the layer 65b, an oxide of tungsten (W) (hereinafter, also referred to as the "first metal" in the second embodiment) contained in the WCl5 gas is formed. If this oxide of W remains in the recess 60, it may cause an increase in the wiring resistance after Ru is embedded, and therefore, it may be necessary to remove the oxide of W.

[0056] In response to the need to remove the oxides of W, the substrate processing apparatus 1a of this embodiment forms a film of a metal that is more easily oxidized than W, such as titanium (Ti) (hereinafter, also referred to as the "second metal" in the second embodiment). As a result, the oxides of W are reduced by Ti to MoO X The Ti oxide formed in place of the layer 65b is removed by the etching gas.

[0057] In view of the above, the substrate processing apparatus 1a uses WCl5 gas to X The apparatus is equipped with a pre-cleaning module 156 which only removes the layer 65b, a reducing Ti film-forming module 155 which forms a Ti film to reduce W oxides and removes the oxides, and a Ti film-forming module 153a which forms only the Ti layer 66 for contact.

[0058] Although individual illustrations are omitted, the pre-cleaning module 156, the reducing Ti film formation module 155, and the Ti film formation module 153a are similar to the Ti film formation module 153 described using Figure 2 in that each of them has a processing container 210 and a mounting table 22. 2, but does not have a configuration for supplying TiCl4 gas, Ar gas, or H2 gas for forming the Ti layer 66. In addition, the pre-cleaning module 156 does not have a high frequency power supply 234 for turning the gas supplied to the processing vessel 210 into plasma, or a high frequency power supply 223 for attracting ions. The pre-cleaning module 156 corresponds to the second processing module in the second embodiment.

[0059] The reducing Ti film-forming module 155 is configured almost the same as the Ti film-forming module 153 shown in Fig. 2, and includes a film-forming gas supply unit for supplying a film-forming gas that is a mixed gas of TiCl4 gas, H2 gas, and Ar gas. On the other hand, the reducing Ti film-forming module 155 differs from the Ti film-forming module 153 in that it includes an etching gas supply unit for supplying an etching gas for removing Ti oxides, instead of a supply unit for supplying WCl5 gas. The reducing Ti film-forming module 155 of this example uses chlorine (Cl2) gas as the etching gas. For example, the etching gas supply unit includes a Cl2 gas supply source, a flow rate adjustment unit, and the like (both not shown).

[0060] The Ti film formation module 153a is configured almost the same as the Ti film formation module 153 shown in Fig. 2, and includes a film formation gas supply unit for supplying a film formation gas that is a mixed gas of TiCl4 gas, H2 gas, and Ar gas. On the other hand, the Ti film formation module 153a differs from the Ti film formation module 153 in that it does not include a metal halide gas supply unit for supplying WCl5 gas. The Ti film formation module 153a corresponds to the third process module of this embodiment.

[0061] 5 is similar to the substrate processing apparatus 1 of the first embodiment in that one COR module 151 and one PHT module 152 are connected to the first substrate transfer chamber 13. Meanwhile, the substrate processing apparatus 1a of the second embodiment is different from the substrate processing apparatus 1 of the first embodiment in that one pre-cleaning module 156 and one reducing Ti film formation module 155 are connected to the first substrate transfer chamber 13 instead of the two Ti film formation modules 153. Also, one Ti film formation module 153a is connected to the second substrate transfer chamber 14, and three Ru film formation modules 154 are connected to the second substrate transfer chamber 14.

[0062] Processing of a wafer W using this substrate processing apparatus 1a will be described with reference to Fig. 6. In Fig. 6, differences from the substrate processing according to the first embodiment described with reference to Fig. 3 will be mainly described.

[0063] The wafer W to be processed is subjected to COR processing and PHT processing using the COR module 151 and the PHT module 152 (process P11 in FIG. 6). Thereafter, the wafer W is transferred into the pre-cleaning module 156, where WCl5 gas is supplied and MoO X The layer 65b is removed (process P12A in FIG. 6, a process for removing metal oxide components).

[0064] At this time, as shown in FIG. 4B, when the WCl.sub.5 gas reaches the wafer W, the reaction shown in the following formula (3) also proceeds in parallel with the reaction shown in the above-described formula (1). MoO3(s)+WCl5(g)→WO3(s)+2MoCl5(g) …(3)

[0065] Here, in reaction (1), MoO X The Gibbs free energy of the reaction between layer 65b and WCl5 gas is -241 kJ / mol at an absolute temperature of 673 K. On the other hand, the Gibbs free energy of the reaction in equation (3) is -126 kJ / mol under the same temperature conditions. Therefore, the Gibbs free energy of both equations (1) and (3) is negative, and the reaction proceeds in both cases.

[0066] According to the reaction of equation (3), MoO X While the layer 65b is removed, an oxide of W (WO3) which is the first metal is formed on the surface of the wafer W. In the substrate processing apparatus 1a of the second embodiment, the wafer W is loaded into the reducing Ti film forming module 155, and a film forming gas is supplied to form a film of reducing Ti which is the second metal (process P12B in FIG. 6). When Ti and WO3 come into contact with each other due to the formation of the reducing Ti film, the reaction of the following formula (4) proceeds, and WO3 is reduced to W (process of reducing the oxide of the first metal). WO3(s)+3Ti(s)→ W+3TiO …(4)

[0067] Thereafter, the supply of the film formation gas is stopped, and the gas supplied into the process vessel 210 is switched to Cl2 gas. As a result, the reaction shown in the following formula (5) proceeds, and TiO is removed (process P12C in FIG. 6, a process of removing the oxide of the second metal). TiO(s)+Cl2(g)→TiOCl2(g) …(5)

[0068] The above process leaves metallic tungsten (W) on the surface of the wafer W. Also, Ti that did not come into contact with WO3 remains on the surface of the wafer W without being etched. Of the Ti, the Ti formed in the recess 60 is integrated with Ti formed in the subsequent Ti film forming module 153a to form a Ti layer 66. Also, the Ti formed on the surface of the SiO layer 62 is polished and removed by CMP processing after the Ru film 67 is formed.

[0069] As described above, the reaction of formula (1) proceeds in parallel with the reaction of formula (3) that forms the oxide of W (WO3). As a result, if it is undesirable that solid WCl2 remains on the surface of the wafer W, for example, H2 gas may be supplied before forming a film of reducing Ti to cause the reaction of formula (2) to proceed and remove chlorine, as in the substrate processing apparatus 1 according to the first embodiment.

[0070] When the time comes to complete the removal of TiO, the wafer W is carried into the Ti film forming module 153a, and a film forming gas is supplied to form a Ti layer 66, which is a metal layer for contact (process P13A in FIG. 6). Thereafter, the process of forming a Ru film 67 and the operation of carrying out the wafer W after the process are the same as in the case of using the substrate processing apparatus 1 described above, and therefore will not be described again.

[0071] Here, the second metal is not limited to titanium (Ti). For example, Mo or Ta may be formed as a second metal that is more easily oxidized than tungsten (W), and then the oxide of Mo or Ta may be etched with chlorine gas.

[0072] <Third embodiment> Next, the configuration and operation of a substrate processing apparatus 1b according to a third embodiment will be described with reference to FIGS. The substrate processing apparatus 1b according to the third embodiment is not provided with a PHT module 152 for the PHT process to remove reaction products generated in the COR process. X The heating operation of the wafer W when removing the layer 65b is utilized to simultaneously remove reaction products.

[0073] In the substrate processing apparatus 1b shown in FIG. 7, two COR modules 151 and two pre-cleaning modules 156 are connected to the first substrate transfer chamber 13. Therefore, the PHT module 152 is not provided, and the MoO X The substrate processing apparatus 1 according to the first embodiment differs from the substrate processing apparatus 1 according to the first embodiment in that a pre-cleaning module 156 that only removes the layer 65b is used. Also, one Ti film formation module 153a and three Ru film formation modules 154 are connected to the second substrate transfer chamber 14.

[0074] 7 illustrates a configuration corresponding to the progress of the reaction of the above-mentioned formula (1) in the Ti film formation module 153. In the case of responding to the progress of the reaction of the formula (3) in the Ti film formation module 153, for example, a configuration may be adopted in which the first substrate transfer chamber 13 is connected with each of the COR module 151, the pre-cleaning module 156, and the reducing Ti film formation module 155.

[0075] Processing of a wafer W using this substrate processing apparatus 1b will be described with reference to Fig. 8. In Fig. 8, differences from the substrate processing according to the first embodiment described with reference to Fig. 3 will be mainly described.

[0076] First, the COR process is performed on the wafer W to be processed using the COR module 151 (P11A in FIG. 8). Then, the wafer W is loaded into the pre-cleaning module 156, where WCl gas is supplied and MoO X At this time, the wafer W is heated to a temperature in the range of 400 to 800° C. (for example, 450° C.) to remove the MoO XIn parallel with the removal of layer 65b, reaction products generated in the COR process are sublimated and removed (process P12D in FIG. 8).

[0077] Here, FIG. 8 shows the COR process (silicon oxide (SiO X ) in the pre-cleaning module 156, and X By repeating these processes, the MoSiO X The layer 65a can be reliably removed. The number of times these processes are repeated is, for example, within the range of 2 to 10 times.

[0078] In particular, in the substrate processing apparatus 1b according to the third embodiment shown in FIG. 7, the PHT module 152 is omitted, and the reaction product of the COR process and MoO X The removal of the layer 65b is performed in parallel in the pre-cleaning module 156. Therefore, the processing time per cycle can be shortened compared to the case where the processing is repeated using three processing modules (the COR module 151, the PHT module 152, and the Ti film formation module 153).

[0079] In addition, in the example of the substrate processing apparatus 1b shown in FIG. 7, it is possible to provide two sets of the COR module 151 and the Ti film formation module 153, thereby preventing the total processing time from becoming excessively long due to the repeated processing. However, even if the COR treatment and the treatment using WCl5 gas are repeated multiple times, the implementation of the PHT treatment using the PHT module 152 is not excluded. Treatments using the COR module 151, the PHT module 152, and the Ti film formation module 153 may be repeated.

[0080] In this way, both processes are repeated a predetermined number of times to form MoSiO XAfter the layer 65a is removed, a Ti layer 66 for contact is formed in a Ti film forming module 153a, and a Ru film 67 is formed in a Ru film forming module 154. The operation of unloading the wafer W thereafter is the same as in the case of using the substrate processing apparatus 1 described above, and therefore will not be described again.

[0081] <Variations> In each of the embodiments described above, the metal oxide content (MoO X The metal halide gas used to remove the layer 65b) is not limited to the example of WCl5 gas. For example, WCl6 gas or MoCl5 gas can be used to remove MoO X Removal of layer 65b may also be performed.

[0082] The silicon-containing layer may be a single silicon layer not containing germanium, not limited to the SiGe layer 61 described with reference to Fig. 4A. The metal silicide layer may be a TiSi layer or a WSi layer, in addition to the MoSi layer 64. Even if oxide films are formed on the surfaces of these metal silicides, these oxide films can be removed by combining the COR process with a process using a metal halide gas.

[0083] In addition, in removing silicon oxide by COR treatment (HF gas and NH3 gas) and removing metal oxide by metal halide gas, it is not necessary to perform the COR treatment first. The treatment by metal halide gas may be performed first, and then the COR treatment.

[0084] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims. [Explanation of symbols]

[0085] 1, 1a, 1b Substrate Processing Equipment 151 Oxide Removal (COR) Module 153 Ti deposition module 22 Placement table 23. Shower Head

Claims

1. 1. A method for processing a substrate, comprising: a step of laminating an insulating layer having a recess formed therein on a silicon-containing layer, and supplying hydrogen fluoride gas and ammonia gas to an oxide film on a surface of a metal silicide layer laminated on the silicon-containing layer in the recess, thereby reacting the oxide film with silicon oxide contained in the oxide film and removing the oxide film; and supplying a metal halide gas to the oxide film to react with and remove the metal oxide contained in the oxide film.

2. 2. The method of claim 1, wherein removing the silicon oxide fraction comprises removing a reaction product formed by reaction of the silicon oxide fraction with the hydrogen fluoride gas and the ammonia gas by heating the substrate.

3. 2. The method according to claim 1, further comprising the step of removing the metal oxide component while heating the substrate after the step of removing the silicon oxide component, thereby removing the metal oxide component and a reaction product generated by the reaction of the silicon oxide component with the hydrogen fluoride gas and the ammonia gas in parallel.

4. The method of claim 1 , wherein the steps of removing the silicon oxide fraction and removing the metal oxide fraction are performed repeatedly.

5. 2. The method of claim 1, wherein the silicon-containing layer is a silicon germanium layer, the metal silicide layer is a molybdenum silicide layer, and the metal oxide layer is a molybdenum oxide layer.

6. The metal halide gas is WCl 5 Gas or MoCl 5 The method of claim 1 , wherein the gas is a gas.

7. When a metal contained in the metal halide is referred to as a first metal, in the step of removing the metal oxide component, if an oxide of the first metal remains on the substrate instead of the metal oxide component, a step of reducing the oxide of the first metal by forming a film of a second metal that is more easily oxidized than the first metal on the substrate on which the oxide of the first metal remains; 2. The method according to claim 1, further comprising the step of: removing the oxide of the second metal formed in place of the oxide of the first metal in the step of reducing the oxide of the first metal by an etching gas.

8. 8. The method of claim 7, wherein the first metal is tungsten and the second metal is titanium.

9. The method of claim 8 , wherein the etching gas is chlorine gas.

10. The method according to claim 1 , further comprising the steps of forming a conductor on the substrate and embedding the conductor in the recess after performing the steps of removing the silicon oxide and removing the metal oxide.

11. An apparatus for processing a substrate, comprising: a first processing module including a processing vessel including a mounting table on which the substrate is placed, and a mixed gas supply unit for supplying a mixed gas of hydrogen fluoride gas and ammonia gas to the processing vessel; a second processing module including a processing vessel having a mounting table on which the substrate is placed, and a metal halide gas supply unit for supplying a metal halide gas to the processing vessel; A control unit, the control unit is configured to output a control signal for executing the steps of: supplying the mixed gas to an oxide film on a surface of a metal silicide layer, the metal silicide layer being laminated on the silicon-containing layer in the recess, and reacting the mixed gas with a silicon oxide component contained in the oxide film to remove the oxide film; and supplying the metal halide gas to the oxide film and reacting the metal oxide component contained in the oxide film to remove the oxide film.

12. a vacuum transfer chamber to which the processing container of the first processing module and the processing container of the second processing module are connected, and a substrate transfer mechanism disposed in the vacuum transfer chamber, 12. The apparatus according to claim 11, wherein the control unit is configured to output a control signal for performing a step of transporting the substrate between the mounting stage of the first processing module and the mounting stage of the second processing module via the vacuum transport chamber by the substrate transport mechanism between the step of removing the silicon oxide portion and the step of removing the metal oxide portion.

13. the second processing module includes a heating unit that heats the substrate; 12. The apparatus according to claim 11, wherein the control unit is configured to output a control signal for performing, in parallel, removal of the metal oxide components and removal of reaction products generated by reaction of the silicon oxide components with the hydrogen fluoride gas and the ammonia gas, by performing a step of removing the metal oxide components while heating the substrate after the step of removing the silicon oxide components.

14. 12. The device of claim 11, wherein the silicon-containing layer is a silicon germanium layer, the metal suicide layer is a molybdenum suicide layer, and the metal oxide layer is a molybdenum oxide layer.

15. The metal halide gas is WCl 5 Gas or MoCl 5 The device of claim 11 which is a gas.

16. a third processing module including a processing vessel including a mounting table on which the substrate is mounted, a film-forming gas supply unit for supplying a film-forming gas of a second metal, which is more easily oxidized than the first metal, to the processing vessel when a metal contained in the metal halide is referred to as a first metal, and an etching gas supply unit for supplying an etching gas for etching an oxide of the second metal, 12. The apparatus of claim 11, wherein the control unit is configured to output a control signal for executing a step of reducing the oxide of the first metal by supplying the film forming gas to the substrate on which the oxide of the first metal remains to form a film of the second metal when an oxide of the first metal remains on the substrate instead of the metal oxide in the step of removing the metal oxide, and then a step of removing the oxide of the second metal formed in place of the oxide of the first metal by the etching gas in the step of reducing the oxide of the first metal.

17. 17. The apparatus of claim 16, wherein the first metal is tungsten and the second metal is titanium.

18. 20. The apparatus of claim 17, wherein the etching gas is chlorine gas.

19. a fourth process module including a process vessel including a mounting table on which the substrate is placed, and a source gas supply unit for supplying a source gas of a conductor to the process vessel; 12. The apparatus according to claim 11, wherein the control unit is configured to output a control signal for executing a step of placing the substrate on the mounting table of the fourth processing module, supplying the raw material gas into the processing vessel to deposit a conductor on the substrate, and embedding the conductor in the recess, after performing the step of removing the silicon oxide portion and the step of removing the metal oxide portion.

Citation Information

Patent Citations

  • METHOD FOR ETTING METAL OXIDE WITH LOW RESIDUE LEAVING - Patent application

    JP2021507509A

  • Etching metal oxides using fluorine and metal halides

    JP2022536475A

  • METHOD FOR FORMING Ti FILM AND TiN FILM, CONTACT STRUCTURE, COMPUTER READABLE STORING MEDIUM AND COMPUTER PROGRAM

    WO2005098913A1