Method for producing resin particle

By controlling the cooling rate ratio during release agent precipitation in toner production, the method achieves uniform distribution and increased crystallinity, enhancing high-temperature fixability and image quality by reducing dispersion diameter, addressing uneven gloss issues in printed images.

JP2024155163APending Publication Date: 2024-10-31RICOH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023069622
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing methods for producing toner particles fail to achieve uniform distribution of the release agent, leading to uneven gloss and insufficient high-temperature fixability, which affects the quality of printed images.

Method used

Control the cooling temperature during the precipitation of the release agent in the toner production process by setting a specific cooling rate ratio (A≦2B) to increase the crystallinity of the release agent, thereby reducing its dispersion diameter and enhancing uniformity within the particles.

Benefits of technology

The method results in resin particles with excellent high-temperature fixability and improved image quality by minimizing gloss unevenness during fixing, ensuring consistent image quality across various temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155163000004
    Figure 2024155163000004
  • Figure 2024155163000001
    Figure 2024155163000001
  • Figure 2024155163000002
    Figure 2024155163000002
Patent Text Reader

Abstract

To provide a method for producing resin particles which can obtain an image that is excellent in high temperature fixability and has high quality.SOLUTION: A method for producing resin particles containing a binder resin and a release agent includes a step a) of preparing an oil phase in which the binder resin containing a polyester resin is dissolved or dispersed in an organic solvent; a step b) of mixing the release agent and the organic solvent, heating the mixture, and then precipitating the mixture by cooling and preparing a dispersion liquid; and a step c) of aggregating resin particles containing the binder resin and the release agent, wherein when a temperature-lowering rate until the release agent starts to precipitate in the cooling process of the step b) is represented by A, and a temperature-lowering rate until the release agent completely finishes to precipitate is represented by B, A and B satisfy A≤2B.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing resin particles. [Background technology]

[0002] In recent years, there has been an increasing demand for high-quality printing that approaches that of offset printing. Among the requirements for high-quality printing, the uniformity of the release agent inside the toner is important for achieving a wide range of fixing properties and suppressing uneven gloss.

[0003] Patent Document 1 discloses a method for maintaining fixability at high temperatures by adding a prepolymer during production and polymerizing it after toner particle formation. However, the toner produced by this method is insufficient in reducing gloss unevenness. Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a method for producing resin particles which have excellent high-temperature fixability and can provide high-quality images. [Means for solving the problem]

[0005] As a result of investigating the uniformity of the release agent inside the toner, it was found that by controlling the cooling temperature when precipitating the release agent, it is possible to increase the crystallinity of the release agent, reduce the dispersion diameter, and control the uniformity of the release agent inside the particle.

[0006] The present invention relates to a method for producing resin particles containing a binder resin and a release agent, a) preparing an oil phase by dissolving or dispersing the binder resin containing a polyester resin in an organic solvent; b) mixing the release agent with an organic solvent, heating the mixture, and then cooling the mixture to cause precipitation, thereby preparing a dispersion; c) aggregating resin particles containing the binder resin and the release agent, In the cooling process of b), the temperature reduction rate until the release agent starts to precipitate is A, and the temperature reduction rate until the release agent completely precipitates is B, and A≦2B. A method for producing resin particles.

[0007] In the step b), since an exothermic reaction occurs when the release agent precipitates, the temperature drop rate B is smaller than the temperature drop rate A (A>B), but by controlling the temperature drop rate B so that A≦2B, the crystallinity of the release agent increases and it becomes possible to reduce the dispersed diameter of the release agent after precipitation. By reducing the dispersed diameter of the release agent particles, the dispersed diameter of the release agent in the resin particles can also be reduced, and uneven gloss during fixing can be reduced. Effect of the Invention

[0008] According to the present invention, there can be provided a method for producing resin particles which have excellent high-temperature fixing property and enable the formation of high-quality images. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic diagram illustrating an example of an image forming apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The method for producing resin particles according to the present invention will be described in detail below. The present invention is not limited to the following embodiments, and can be modified as appropriate without departing from the gist of the present invention. In addition, in this specification, "to" indicating a numerical range means that the numerical values ​​before and after it are included as the lower and upper limits, unless otherwise specified. Although the present invention relates to a method for producing resin particles, the present invention will be described below by taking toner as an example of resin particles, and therefore, hereinafter, resin particles will be referred to as toner.

[0011] In the toner manufacturing method according to the present embodiment, first, an oil phase is prepared by dissolving or dispersing a binder resin, a colorant, a release agent, etc. in an organic solvent. Hereinafter, materials used in the oil phase preparation step will be described.

[0012] <Binding resin> The binder resin used in the production of the toner according to this embodiment is not particularly limited, but preferably contains an amorphous resin, a crystalline resin, or both. [Amorphous resin] The amorphous resin preferably contains an amorphous polyester resin.

[0013] (Amorphous polyester resin) In the present embodiment, the amorphous polyester resin is preferably a linear polyester resin, and more preferably an unmodified polyester resin.

[0014] The unmodified polyester resin is a polyester resin obtained using a polyhydric alcohol and a polycarboxylic acid or a derivative thereof, such as a polycarboxylic acid, a polycarboxylic anhydride, or a polycarboxylic ester, and is not modified with an isocyanate compound or the like.

[0015] In view of excellent heat resistance storage stability, the amorphous polyester resin preferably contains a dicarboxylic acid component as a constituent component, and the dicarboxylic acid component preferably contains 50 mol % or more of terephthalic acid.

[0016] Examples of the polyhydric alcohol include diols.

[0017] Examples of the diol include alkylene (carbon number 2-3) oxide (average number of added moles 1-10) adducts of bisphenol A such as polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane and polyoxyethylene(2.2)-2,2-bis(4-hydroxyphenyl)propane; ethylene glycol; propylene glycol; hydrogenated bisphenol A; and alkylene (carbon number 2-3) oxide (average number of added moles 1-10) adducts of hydrogenated bisphenol A. These may be used alone or in combination of two or more.

[0018] Examples of the polycarboxylic acid include dicarboxylic acids.

[0019] Examples of the dicarboxylic acid include adipic acid, phthalic acid, isophthalic acid, terephthalic acid, fumaric acid, maleic acid, and succinic acids substituted with an alkyl group having 1 to 20 carbon atoms or an alkenyl group having 2 to 20 carbon atoms, such as dodecenylsuccinic acid and octylsuccinic acid. These may be used alone or in combination of two or more.

[0020] For the purpose of adjusting the acid value and hydroxyl value, the amorphous polyester resin may contain at least one of a trivalent or higher carboxylic acid and a trivalent or higher alcohol at the end of the resin chain.

[0021] Examples of the trivalent or higher carboxylic acid include trimellitic acid, pyromellitic acid, and acid anhydrides thereof.

[0022] Examples of the trihydric or higher alcohol include glycerin, pentaerythritol, and trimethylolpropane.

[0023] The molecular weight of the amorphous polyester resin is not particularly limited and can be appropriately selected depending on the purpose. In the measurement by GPC (gel permeation chromatography), the weight average molecular weight (Mw) is preferably 3,000 to 10,000, more preferably 4,000 to 7,000. The number average molecular weight (Mn) is preferably 1,000 to 4,000, more preferably 1,500 to 3,000. The Mw / Mn is preferably 1.0 to 4.0, more preferably 1.0 to 3.5.

[0024] When the molecular weight is equal to or more than the lower limit of 3,000, it is possible to prevent the toner from decreasing in heat-resistant storage stability and durability against stress such as stirring in a developing machine, etc. When the molecular weight is equal to or less than the upper limit of 10,000, it is possible to prevent the toner from increasing in viscoelasticity when melted, and to prevent the low-temperature fixability from decreasing.

[0025] The acid value of the amorphous polyester resin is not particularly limited and can be appropriately selected according to the purpose. It is preferably 1 mgKOH / g to 50 mgKOH / g, more preferably 5 mgKOH / g to 30 mgKOH / g. When the acid value is 1 mgKOH / g or more, the toner tends to be negatively charged, and further, when fixed to paper, the affinity between the paper and the toner is improved, and low-temperature fixability can be improved. When the acid value is 50 mgKOH / g or less, it is possible to suppress a decrease in charging stability, particularly charging stability against environmental changes.

[0026] The hydroxyl value of the amorphous polyester resin is not particularly limited and may be appropriately selected depending on the purpose, but is preferably 5 mgKOH / g or more.

[0027] The glass transition temperature (Tg) of the amorphous polyester resin is preferably 40° C. to 80° C., more preferably 50° C. to 70° C. When the glass transition temperature is 40° C. or higher, the toner has sufficient heat-resistant storage stability and durability against stress such as stirring in a developing machine, and also has good filming resistance. When the glass transition temperature is 80° C. or lower, the toner is sufficiently resistant to deformation due to heating and pressure during fixing, and has good low-temperature fixing properties.

[0028] The molecular structure of the amorphous polyester resin can be confirmed by nuclear magnetic resonance (NMR) measurement using a solution or solid, as well as X-ray diffraction, gas chromatography / mass spectrometry (GC / MS), liquid chromatography / mass spectrometry (LC / MS), infrared absorption (IR) measurement, etc. A simple method is to detect an amorphous polyester resin as one that does not have absorption due to olefin δCH (out-of-plane bending vibration) at 965±10 cm-1 and 990±10 cm-1 in an infrared absorption spectrum.

[0029] The content of the amorphous polyester resin is not particularly limited and can be appropriately selected according to the purpose, but is preferably 50 parts by mass to 90 parts by mass, more preferably 60 parts by mass to 80 parts by mass, relative to 100 parts by mass of the toner. When the content is 50 parts by mass or more, the dispersibility of the pigment and the release agent in the toner can be suppressed from deteriorating, and the occurrence of fogging and disturbance of the image can be suppressed. When the content is 90 parts by mass or less, the decrease in low-temperature fixability can be suppressed. When the content is in the above-mentioned more preferred range, it is advantageous in that both high image quality and low-temperature fixability are excellent.

[0030] <Crystalline resin> In order to improve low-temperature fixing ability, it is preferable to add a crystalline resin to the toner according to the present embodiment. The crystalline resin is not particularly limited as long as it has crystallinity, and can be appropriately selected according to the purpose. For example, polyester resin, polyurethane resin, polyurea resin, polyamide resin, polyether resin, vinyl resin, modified crystalline resin, etc. can be mentioned. These may be used alone or in combination of two or more kinds.

[0031] [Crystalline polyester resin] The crystalline polyester resin (hereinafter, sometimes referred to as "crystalline polyester resin C") has high crystallinity and therefore exhibits thermal melting characteristics that show a sudden change in viscosity near the fixing start temperature. By using the crystalline polyester resin C having such characteristics together with the amorphous polyester resin, a toner having both good heat-resistant storage stability and low-temperature fixing ability can be obtained.

[0032] For example, by using the crystalline polyester resin C and the amorphous polyester resin together, the heat-resistant storage stability is good due to the crystallinity until just before the melting start temperature, and at the melting start temperature, the viscosity drops sharply due to the melting of the crystalline polyester resin C (sharp melt property). Accordingly, the crystalline polyester resin and the amorphous polyester resin are compatible with each other, and the viscosity of both drops sharply, allowing for good fixation.

[0033] The crystalline polyester resin is obtained from a polyhydric alcohol and a polycarboxylic acid such as a polycarboxylic acid, a polycarboxylic anhydride, or a polycarboxylic ester, or a derivative thereof. Note that, in the present invention, the crystalline polyester resin refers to a resin obtained by using a polyhydric alcohol and a polycarboxylic acid such as a polycarboxylic acid, a polycarboxylic anhydride, or a polycarboxylic ester, or a derivative thereof, as described above, and a modified polyester resin, for example, a prepolymer, and a resin obtained by subjecting the prepolymer to a crosslinking and / or elongation reaction, do not belong to the crystalline polyester resin.

[0034] The polyhydric alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polyhydric alcohol include diols and trihydric or higher alcohols.

[0035] Examples of the diol include saturated aliphatic diols. Examples of the saturated aliphatic diol include linear saturated aliphatic diols and branched saturated aliphatic diols. Among these, linear saturated aliphatic diols are preferred, and linear saturated aliphatic diols having 2 to 12 carbon atoms are more preferred. If the saturated aliphatic diol is a branched type, the crystallinity of the crystalline polyester resin may decrease, resulting in a decrease in melting point. In addition, if the carbon number of the saturated aliphatic diol exceeds 12, it becomes difficult to obtain a practical material.

[0036] Examples of the saturated aliphatic diol include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,14-eicosanedecanediol, etc. Among these, ethylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol are preferred in terms of the high crystallinity of the crystalline polyester resin and excellent sharp melt properties.

[0037] Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, etc. These may be used alone or in combination of two or more.

[0038] The polyvalent carboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include divalent carboxylic acids and trivalent or higher carboxylic acids.

[0039] Examples of the divalent carboxylic acid include saturated aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid; and aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, and naphthalene-2,6-dicarboxylic acid. Further examples include anhydrides of these and lower (1 to 3 carbon atoms) alkyl esters of these. Among these, from the viewpoint of carbon neutrality, saturated aliphatic acids having 12 or less carbon atoms derived from plants are preferred.

[0040] Examples of the trivalent or higher carboxylic acid include 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, and the like, as well as their anhydrides and lower (carbon number 1 to 3) alkyl esters, etc. These may be used alone or in combination of two or more.

[0041] The crystalline polyester resin is preferably composed of a linear saturated aliphatic dicarboxylic acid having 4 to 12 carbon atoms and a linear saturated aliphatic diol having 2 to 12 carbon atoms, which provides a crystalline polyester resin having high crystallinity and excellent sharp melting properties, thereby enabling the resin to exhibit excellent low-temperature fixing properties.

[0042] In addition, as a method for controlling the crystallinity and softening point of a crystalline polyester resin, there can be mentioned a method for designing and using a non-linear polyester which is subjected to condensation polymerization by adding a polyhydric alcohol having a valence of three or more, such as glycerin, as an alcohol component, or a polycarboxylic acid having a valence of three or more, such as trimellitic anhydride, as an acid component during polyester synthesis.

[0043] The molecular structure of crystalline polyester resin can be confirmed by NMR measurement of solution or solid, as well as X-ray diffraction, GC / MS, LC / MS, IR measurement, etc. -1 Or 990±10cm -1 Examples include those that have absorption due to the δCH (out-of-plane bending vibration) of olefins.

[0044] Regarding the molecular weight of the crystalline polyester, those with a sharp molecular weight distribution and low molecular weight have excellent low-temperature fixability, while those with a large amount of low molecular weight components have poor heat-resistant storage stability. As a result of extensive investigation, it has been found that the molecular weight distribution of the soluble portion in o-dichlorobenzene by GPC, in which the horizontal axis is log(M) and the vertical axis is weight%, has a peak position in the range of 3.5 to 4.0, the half-width of the peak is 1.5 or less, the weight average molecular weight (Mw) is 3,000 to 30,000, the number average molecular weight (Mn) is 1,000 to 10,000, and Mw / Mn is 1 to 10. It is further preferable that the weight average molecular weight (Mw) is 5,000 to 15,000, the number average molecular weight (Mn) is 2,000 to 10,000, and Mw / Mn is 1 to 5.

[0045] From the viewpoint of affinity between paper and resin, the acid value of the crystalline polyester resin is preferably 5 mgKOH / g or more to achieve the desired low-temperature fixability, and more preferably 7 mgKOH / g or more to prepare fine particles by phase inversion emulsification, while the acid value is preferably 45 mgKOH / g or less to improve hot offset resistance.

[0046] The hydroxyl value of the crystalline polyester resin is preferably 0 to 50 mgKOH / g, more preferably 5 to 50 mgKOH / g, in order to achieve a desired low-temperature fixability and good charging characteristics.

[0047] <Coloring agent> As the colorant in the present invention, known dyes and pigments can be used, for example, carbon black, nigrosine dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ochre, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Balkan fast yellow (5G, R), tartrazine lake, quinoline yellow lake, anthrazan yellow BGL, isoi Andrinone Yellow, Bengala, Red Lead, Cinnabar, Cadmium Red, Cadmium Mercury Red, Antimony Vermilion, Permanent Red 4R, Para Red, Phaysee Red, Parachlor Orthonitroaniline Red, Lithol Fast Scarlet G, Brilliant Fast Scarlet, Brilliant Kanmin BS, Permanent Red (F2R, F4R, FRL, FRLL, F4RH), Fast Scarlet VD, Belkan Fast Rubin B, Brilliant Scarlet G, Lithol Rubin GX, Permanent Red F5R, Brilliant Tocarmine 6B, Pogment Scarlet 3B, Bordeaux 5B, Toluidine Maroon, Permanent Bordeaux F2K, Helio Bordeaux BL, Bordeaux 10B, Bon Maroon Light, Bon Maroon Medium, Eosin Lake, Rhodamine Lake B, Rhodamine Lake Y, Alizarin Lake, Thioindigo Red B, Thioindigo Maroon, Oil Red, Quinacridone Red, Pyrazolone Red, Polyazo Red, Chrome Vermilion, Benzidine Orange, Perinone Orange, Oil Orange, Cobalt Blue, Cerulean Blue, Alkaline Blue Lake, Peacock Blue Lake, Victoria Blue Lake, Metal-free Phthalocyanine Blue, Phthalocyanine Blue, Fast Sky Blue, Indanthrene Blue (RS, BC), Indigo, Ultramarine Blue, Prussian Blue, Anthraquinone Blue, Fast Violet B, Methyl Violet Lake, Cobalt Purple, Manganese Purple, Dioxane Violet, Anthraquinone Violet, Chrome Green, Zinc Green, Chromium Oxide, Pyridian, Emerald Green, Pigment Green B, Naphthol Green B, Green Gold, Acid Green Lake,Malachite green lake, phthalocyanine green, anthraquinone green, titanium oxide, zinc oxide, lithopone and mixtures thereof can be used.

[0048] <Organic solvent> The organic solvent is not particularly limited and can be appropriately selected according to the purpose, but a volatile solvent with a boiling point of less than 100°C is preferable because it facilitates subsequent removal of the organic solvent. As such an organic solvent, for example, toluene, xylene, benzene, carbon tetrachloride, methylene chloride, 1,2-dichloroethane, 1,1,2-trichloroethane, trichloroethylene, chloroform, monochlorobenzene, dichloroethylidene, methyl acetate, ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, methanol, ethanol, isopropyl alcohol, etc. can be used alone or in combination of two or more. When the resin to be dissolved or dispersed in the organic solvent is a resin having a polyester skeleton, it is preferable to use an ester-based solvent such as methyl acetate, ethyl acetate, or butyl acetate, or a ketone-based solvent such as methyl ethyl ketone or methyl isobutyl ketone, because they have high solubility. Among these, methyl acetate, ethyl acetate, and methyl ethyl ketone, which have high solvent removal properties, are particularly preferable.

[0049] <Prepolymer> The present invention may include a prepolymer. The reactive precursor may be a polyester having a group capable of reacting with an active hydrogen group. The group capable of reacting with the active hydrogen group may be, for example, an isocyanate group, an epoxy group, a carboxylic acid, or an acid chloride group. Among these, an isocyanate group is preferred because it can introduce a urethane bond or a urea bond into the amorphous polyester resin.

[0050] The reactive precursor may have a branched structure imparted by at least one of a trivalent or higher alcohol and a trivalent or higher carboxylic acid.

[0051] The polyester resin containing an isocyanate group may be, for example, a reaction product of a polyester resin having an active hydrogen group and a polyisocyanate. The polyester resin having an active hydrogen group may be obtained by polycondensation of a diol, a dicarboxylic acid, and at least one of a trivalent or higher alcohol and a trivalent or higher carboxylic acid. The trivalent or higher alcohol and the trivalent or higher carboxylic acid impart a branched structure to the polyester resin containing an isocyanate group.

[0052] Examples of the diol include aliphatic diols such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, and 1,12-dodecanediol; diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylol. Examples of the diol include diols having an oxyalkylene group such as ethylene glycol; alicyclic diols such as 1,4-cyclohexanedimethanol and hydrogenated bisphenol A; alicyclic diols to which alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide have been added; bisphenols such as bisphenol A, bisphenol F, and bisphenol S; and alkylene oxide adducts of bisphenols such as those to which alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide have been added. Among these, from the viewpoint of controlling the glass transition point of the polyester resin to 20° C. or less, it is preferable to use aliphatic diols having a carbon number of 3 to 10, such as 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, and 3-methyl-1,5-pentanediol, and it is more preferable to use 50 mol% or more of the alcohol component in the resin. These diols may be used alone or in combination of two or more.

[0053] The polyester resin is preferably an amorphous polyester resin, and the melt viscosity during fixing is reduced by providing steric hindrance to the resin chain, which makes it easier to achieve low-temperature fixing properties. For this reason, the main chain of the aliphatic diol preferably has a structure represented by the following general formula (1). [ka] [In the formula, R1 and R2 each independently represent a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and n represents an odd number from 3 to 9. However, in the n repeating units, R1 and R2 may be the same or different.]

[0054] Here, the main chain of the aliphatic diol in the present invention refers to a carbon chain that connects two hydroxyl groups of the aliphatic diol with the shortest number of carbon atoms. When the carbon number of the main chain is odd, the crystallinity decreases due to the odd-even nature, which is preferable. In addition, when the main chain has at least one alkyl group having 1 to 3 carbon atoms in the side chain, the interaction energy between the main chain molecules decreases due to the steric nature, which is more preferable.

[0055] Examples of the dicarboxylic acid include aliphatic dicarboxylic acids such as succinic acid, adipic acid, sebacic acid, dodecanedioic acid, maleic acid, and fumaric acid; and aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, and naphthalenedicarboxylic acid. In addition, anhydrides, lower (1 to 3 carbon atoms) alkyl esters, and halides of these may be used. Among these, from the viewpoint of controlling the Tg of the polyester resin to 20° C. or less, aliphatic dicarboxylic acids having 4 to 12 carbon atoms are preferred, and it is more preferred to use them in an amount of 50% by mass or more of the carboxylic acid component in the resin. These dicarboxylic acids may be used alone or in combination of two or more.

[0056] Examples of the trihydric or higher alcohol include trihydric or higher aliphatic alcohols such as glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, and sorbitol; trihydric or higher polyphenols such as trisphenol PA, phenol novolac, and cresol novolac; and alkylene oxide adducts of trihydric or higher polyphenols, such as those obtained by adding alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide to trihydric or higher polyphenols.

[0057] Examples of the trivalent or higher carboxylic acid include trivalent or higher aromatic carboxylic acids, and particularly preferred are trivalent or higher aromatic carboxylic acids having 9 to 20 carbon atoms, such as trimellitic acid and pyromellitic acid. In addition, anhydrides, lower (carbon number 1 to 3) alkyl esters, and halides of these may also be used.

[0058] Examples of the polyisocyanate include diisocyanates and tri- or higher valent isocyanates.

[0059] The polyisocyanate is not particularly limited and can be appropriately selected depending on the purpose. For example, 1,3- and / or 1,4-phenylene diisocyanate, 2,4- and / or 2,6-tolylene diisocyanate (TDI), crude TDI, 2,4'- and / or 4,4'-diphenylmethane diisocyanate (MDI), crude MDI [crude diaminophenylmethane [condensation product of formaldehyde and aromatic amine (aniline) or a mixture thereof; diaminodiphenylmethane and a small amount (for example, 5 to 20% by mass) of a trifunctional or more functional compound, Phosgenates of the above polyamines and mixtures thereof: aromatic diisocyanates such as polyallyl polyisocyanate (PAPI), 1,5-naphthylene diisocyanate, 4,4',4"-triphenylmethane triisocyanate, m- and p-isocyanatophenylsulfonyl isocyanate; ethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), dodecamethylene diisocyanate, 1,6,11-undecane triisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, etc. Aliphatic diisocyanates such as isocyanate, lysine diisocyanate, 2,6-diisocyanatomethyl caproate, bis(2-isocyanatoethyl) fumarate, bis(2-isocyanatoethyl) carbonate, and 2-isocyanatoethyl-2,6-diisocyanatohexanoate; isophorone diisocyanate (IPDI), dicyclohexylmethane-4,4'-diisocyanate (hydrogenated MDI), cyclohexylene diisocyanate, methylcyclohexylene diisocyanate (hydrogenated TDI), bis(2-isocyanato alicyclic diisocyanates such as 2,5- and 2,6-norbornane diisocyanate, m- and p-xylylene diisocyanate (XDI), α,α,α',α'-tetramethylxylylene diisocyanate (TMXDI), and other aromatic aliphatic diisocyanates; trivalent or higher polyisocyanates such as lysine triisocyanate and diisocyanate modified products of trivalent or higher alcohols; and modified products of these isocyanates, and mixtures of two or more of these may also be used.Examples of the modified isocyanate include modified products containing a urethane group, a carbodiimide group, an allophanate group, a urea group, a biuret group, a uretdione group, a uretoimine group, an isocyanurate group, and an oxazolidone group.

[0060] In the production of the toner according to this embodiment, a charge control agent, a release agent, and the like may be added.

[0061] <Charge control agent> Any of the known charge control agents can be used, such as nigrosine dyes, triphenylmethane dyes, chromium-containing metal complex dyes, molybdic acid chelate pigments, rhodamine dyes, alkoxy amines, quaternary ammonium salts (including fluorine-modified quaternary ammonium salts), alkylamides, phosphorus simple substance or compounds, tungsten simple substance or compounds, fluorine-based activators, metal salicylic acid salts, and metal salts of salicylic acid derivatives.

[0062] Specifically, these include the nigrosine dye Bontron 03, the quaternary ammonium salt Bontron P-51, the metal-containing azo dye Bontron S-34, the oxynaphthoic acid metal complex E-82, the salicylic acid metal complex E-84, the phenol condensate E-89 (all manufactured by Orient Chemical Industry Co., Ltd.), the quaternary ammonium salt molybdenum complexes TP-302 and TP-415 (all manufactured by Hodogaya Chemical Co., Ltd.), the quaternary ammonium salt Copy Charge PSY VP2038, the triphenylmethane derivative Copy Blue PR, the quaternary ammonium salt Copy Charge NEG VP2036, and Copy Charge NX. Examples of the pigments include VP434 (manufactured by Hoechst), LRA-901, boron complex LR-147 (manufactured by Nippon Carlit), copper phthalocyanine, perylene, quinacridone, azo pigments, and other polymeric compounds having functional groups such as sulfonic acid groups, carboxyl groups, and quaternary ammonium salts. These pigments may be used alone or in combination of two or more.

[0063] The charge control agent may be used in an amount within a range in which it exhibits its performance without interfering with fixability, etc., and is contained in the toner in an amount of 0.5 to 5% by mass, preferably 0.8 to 3% by mass.

[0064] <Release agent> The release agent is not particularly limited and can be appropriately selected depending on the purpose, but a release agent with a low melting point of 50° C. to 120° C. is preferable. The release agent with a low melting point effectively acts between the fixing roller and the toner interface by being dispersed in the resin, and this results in good hot offset resistance even in an oil-less system (no release agent such as oil is applied to the fixing roller).

[0065] Suitable examples of the release agent include waxes. Examples of the waxes include natural waxes such as vegetable waxes such as carnauba wax, cotton wax, wood wax, and rice wax; animal waxes such as beeswax and lanolin; mineral waxes such as ozokerite and cerusine; and petroleum waxes such as paraffin, microcrystalline, and petrolatum. In addition to these natural waxes, synthetic hydrocarbon waxes such as Fischer-Tropsch wax and polyethylene wax; synthetic waxes such as esters, ketones, and ethers; and the like. Furthermore, fatty acid amides such as 12-hydroxystearic acid amide, stearic acid amide, phthalic anhydride, and chlorinated hydrocarbons; homopolymers or copolymers of polyacrylates such as poly-n-stearyl methacrylate and poly-n-lauryl methacrylate, which are low molecular weight crystalline polymer resins (for example, copolymers of n-stearyl acrylate and ethyl methacrylate); and crystalline polymers having long alkyl groups on the side chains may be used. These may be used alone or in combination of two or more.

[0066] The melt viscosity of the wax, as measured at a temperature 20° C. higher than the melting point of the wax, is preferably 5 cps to 1,000 cps, and more preferably 10 cps to 100 cps. If the melt viscosity is 5 cps or more, the release property can be prevented from decreasing, and if it is 1,000 cps or less, the effects of hot offset resistance and low temperature fixability can be sufficiently exhibited. The content of the wax in the toner is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0% by mass to 40% by mass, and more preferably 3% by mass to 30% by mass.

[0067] <Toner manufacturing method> The toner production method according to the present embodiment will be described in detail. The toner production method according to the present embodiment includes an oil phase preparation step, an aqueous phase preparation step, a phase inversion emulsification step, a solvent removal step, an aggregation step, and a fusion step, and may further include other steps such as a shell formation step, a washing step, a drying step, an annealing step, and an external addition step, as necessary.

[0068] [Oil phase preparation process] In the oil phase preparation step, the raw materials of the toner, ie, the binder resin (amorphous polyester resin, crystalline polyester resin, etc.), and, if necessary, materials such as a colorant, a prepolymer, a charge control agent, and a release agent, are dissolved or dispersed in an organic solvent to prepare the oil phase. Note that a part of the materials may be added in the aggregation step described later.

[0069] The method for preparing the oil phase is not particularly limited and can be appropriately selected depending on the purpose, and can be exemplified by a method in which raw materials such as a resin are gradually added to an organic solvent while stirring, and dissolved or dispersed. For dispersion, a known method can be used, and for example, a dispersing machine such as a bead mill or a disk mill can be used.

[0070] The organic solvent is not particularly limited and can be appropriately selected according to the purpose, but a volatile solvent with a boiling point of less than 100° C. is preferred from the viewpoint of easy subsequent removal of the organic solvent. Examples of such organic solvents include toluene, xylene, benzene, carbon tetrachloride, methylene chloride, 1,2-dichloroethane, 1,1,2-trichloroethane, trichloroethylene, chloroform, monochlorobenzene, dichloroethylidene, methyl acetate, ethyl acetate, butyl acetate, methyl ethyl ketone, methyl isobutyl ketone, methanol, ethanol, and isopropyl alcohol. These may be used alone or in combination of two or more. When the resin to be dissolved or dispersed in the organic solvent is a resin having a polyester skeleton, the organic solvent is preferably an ester-based solvent such as methyl acetate, ethyl acetate, or butyl acetate, or a ketone-based solvent such as methyl ethyl ketone or methyl isobutyl ketone, in terms of high solubility. Among these, the organic solvent is preferably methyl acetate, ethyl acetate, or methyl ethyl ketone, which has high solvent removal properties.

[0071] The amount of organic solvent used is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 40 parts by mass or more and 300 parts by mass or less, more preferably 60 parts by mass or more and 140 parts by mass or less, and even more preferably 80 parts by mass or more and 120 parts by mass or less, relative to 100 parts by mass of the raw material for the resin particles.

[0072] [Aqueous phase preparation process] In the aqueous phase preparation step, an aqueous phase (aqueous medium) is prepared.

[0073] The aqueous medium is not particularly limited and may be appropriately selected from known ones, for example, water, a solvent miscible with water, or a mixture thereof. From the viewpoint of granulation, the organic solvent concentration is preferably equal to or lower than the saturation concentration in ion-exchanged water.

[0074] The water-miscible solvent is not particularly limited and can be appropriately selected from known solvents, such as alcohol, dimethylformamide, tetrahydrofuran, cellosolves, lower ketones, and esters.

[0075] Examples of the alcohol include methanol, isopropanol, and ethylene glycol.

[0076] Examples of lower ketones include acetone and methyl ethyl ketone.

[0077] An example of the esters is ethyl acetate.

[0078] These may be used alone or in combination of two or more.

[0079] [Phase inversion emulsification process] In the phase inversion emulsification step, the oil phase obtained in the oil phase preparation step is atomized.

[0080] After neutralizing the oil phase, ion-exchanged water is added to the neutralized oil phase, and a colored fine particle dispersion is obtained by phase inversion emulsification, in which the water-in-oil dispersion is inverted into an oil-in-water dispersion.

[0081] The phase inversion emulsification is carried out while uniformly mixing and dispersing using a conventional stirrer or dispersing device.

[0082] The impeller is not particularly limited and can be appropriately selected according to the viscosity of the solution. Examples include low-viscosity impellers such as paddles and propellers, medium-viscosity impellers such as anchors and Maxblends, and high-viscosity impellers such as helical ribbons. Among these, paddles and anchors are preferred because they can control the volume average particle size of the dispersion (oil droplets) to the preferred range.

[0083] The dispersing device is not particularly limited, and examples thereof include an ultrasonic disperser, a bead mill, a ball mill, a roll mill, a homomixer, an ultra mixer, a dispersing mixer, a penetrating type high pressure dispersing device, a collision type high pressure dispersing device, a multi-hole type high pressure dispersing device, an ultra high pressure homogenizer, an ultrasonic homogenizer, etc. A normal stirrer and a dispersing device may be used in combination.

[0084] The base for neutralizing the oil phase may be either a basic inorganic compound or a basic organic compound. Examples of the basic inorganic compound include sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, sodium carbonate, sodium hydrogen carbonate, potassium carbonate, potassium hydrogen carbonate, and ammonia. Examples of the basic organic compound include N,N-dimethylethanolamine, N,N-diethylethanolamine, triethanolamine, tripropanolamine, tributanolamine, triethylamine, n-propylamine, n-butylamine, isopropylamine, monomethanolamine, morpholine, methoxypropylamine, pyridine, vinylpyridine, and isophoronediamine.

[0085] When a stirring blade is used, the conditions such as the rotation speed, stirring time, and stirring temperature are not particularly limited and can be appropriately selected depending on the purpose.

[0086] The rotation speed is not particularly limited, but is preferably 100 rpm to 1,000 rpm, and more preferably 200 rpm to 600 rpm.

[0087] The stirring time and the stirring temperature are not particularly limited and may be appropriately selected depending on the purpose.

[0088] Also, a dispersant may be used if necessary. The dispersant is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include surfactants, poorly water-soluble inorganic compound dispersants, polymer-based protective colloids, etc. These may be used alone or in combination of two or more. Among these, surfactants are preferred.

[0089] The surfactant is not particularly limited and can be appropriately selected depending on the purpose. For example, anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants, etc. can be used.

[0090] The anionic surfactant is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include alkylbenzene sulfonate, α-olefin sulfonate, phosphate, etc. Among these, those having a fluoroalkyl group are preferred.

[0091] [Solvent removal process] In the solvent removal step, the organic solvent is removed from the obtained colored fine particle dispersion.

[0092] In order to remove the organic solvent from the obtained colored fine particle dispersion, a method can be adopted in which the temperature of the entire system is gradually raised while being stirred, and the organic solvent in the droplets is completely evaporated and removed.

[0093] Alternatively, the obtained colored fine particle dispersion liquid may be sprayed into a dry atmosphere while being stirred to completely remove the organic solvent from the droplets, or the colored fine particle dispersion liquid may be reduced in pressure while being stirred to evaporate and remove the organic solvent.

[0094] These means may be used alone or in combination.

[0095] The drying atmosphere in which the colored fine particle dispersion is sprayed is generally air, nitrogen, carbon dioxide, a gas obtained by heating combustion gas, etc., and in particular, various air streams heated to a temperature equal to or higher than the boiling point of the highest boiling point solvent used. The desired quality can be obtained sufficiently by short-time treatment using a spray dryer, belt dryer, rotary kiln, etc.

[0096] By the above method, a colored particle dispersion liquid from which the organic solvent has been removed can be obtained.

[0097] [Agglutination process] The resulting colored fine particle dispersion is agglomerated with stirring until the particles reach a desired particle size, thereby obtaining aggregated particles.

[0098] To achieve flocculation, existing methods such as adding a flocculant or adjusting the pH can be used. When adding a flocculant, it may be added as is, but it is preferable to add the flocculant in an aqueous solution, since this can avoid localized high concentrations. It is also preferable to add the flocculant salt gradually while monitoring the particle size of the colored particles.

[0099] The temperature of the dispersion during aggregation is preferably near the glass transition temperature Tg of the resin used. If the liquid temperature of the colored particle dispersion is too low, aggregation does not proceed very well, resulting in poor efficiency. If the liquid temperature of the colored particle dispersion is too high, the aggregation speed increases, resulting in the generation of coarse particles and a deterioration in particle size distribution.

[0100] When the target particle size is reached, aggregation is stopped by adding a salt with a low ionic valence or a chelating agent, adjusting the pH, lowering the temperature of the dispersion, adding a large amount of an aqueous medium to dilute the concentration, or the like.

[0101] By the above method, a dispersion of colored aggregated particles can be obtained.

[0102] In the aggregation step, a release agent or a crystalline polyester resin may be added. In this case, the material to be added is mixed with a dispersion liquid in which the material is dispersed in an aqueous medium or with the colored fine particle dispersion liquid, and then the material is aggregated to obtain aggregated particles in which the release agent or the crystalline resin is uniformly dispersed.

[0103] As the flocculant, known flocculants can be used, for example, metal salts of monovalent metals such as sodium and potassium, metal salts of divalent metals such as calcium and magnesium, and metal salts of trivalent metals such as iron and aluminum.

[0104] [Fusing process] Next, the obtained aggregated particles are fused by heat treatment to reduce unevenness and to make them spherical. Fusion can be performed by heating the dispersion of the colored aggregated particles while stirring. The temperature of the liquid is preferably near a temperature above the glass transition temperature Tg of the resin used.

[0105] [Shelling process] If necessary, a shelling process may be carried out in which a shell layer is formed on the spheronized particles obtained in the fusion process.

[0106] The method for forming the shell layer is not particularly limited and can be appropriately selected depending on the purpose. For example, the method for forming the shell layer includes a method in which spherical particles having a desired particle size are produced in a fusion step, and then an amorphous resin is added, and the aggregating step and the fusion step are repeated to form the shell layer.

[0107] By the above method, a toner dispersion can be obtained.

[0108] [Cleaning and drying process] The toner dispersion obtained by the above method contains sub-materials such as coagulating salts in addition to the toner, so washing is carried out in order to extract only the toner from the dispersion.

[0109] The toner washing method includes a centrifugation method, a vacuum filtration method, a filter press method, and the like, but is not particularly limited in the present invention. Any of the methods can obtain a toner cake, but if the toner cannot be sufficiently washed in one operation, the obtained cake may be dispersed again in an aqueous solvent to form a slurry, and the toner may be extracted by any of the above methods, and the process may be repeated. In addition, if washing is performed by the vacuum filtration method or the filter press method, a method may be adopted in which the aqueous solvent is passed through the cake to wash away the secondary materials absorbed by the toner.

[0110] The aqueous solvent used for washing is water or a mixed solvent of water and an alcohol such as methanol or ethanol. Considering the cost and the environmental load due to wastewater treatment, it is preferable to use water.

[0111] Since the washed toner contains a large amount of the aqueous medium, the toner alone can be obtained by drying the toner to remove the aqueous medium.

[0112] For the drying method, a dryer such as a spray dryer, a vacuum freeze dryer, a reduced pressure dryer, a stationary shelf dryer, a movable shelf dryer, a fluidized bed dryer, a rotary dryer, or an agitator dryer can be used.

[0113] The dried toner is preferably dried until the moisture content is finally reduced to less than 1%. If the dried toner is in a state of soft aggregation and causes inconvenience in use, the toner may be disintegrated using a device such as a jet mill, a Henschel mixer, a super mixer, a coffee mill, an Oster blender, or a food processor to break up the soft aggregation.

[0114] [Annealing process] When a crystalline resin is added, annealing after drying causes phase separation between the amorphous resin and the crystalline resin, improving fixability. Specifically, this can be done by storing the toner at a temperature near the Tg for 10 hours or more.

[0115] [External addition process] In order to impart fluidity, chargeability, cleaning properties, and the like to the toner obtained in this embodiment, inorganic fine particles, polymeric fine particles, cleaning aids, and the like may be added or mixed.

[0116] Specific mixing means include a method in which an impact force is applied to the mixture by blades rotating at high speed, and a method in which the mixture is introduced into a high-speed air current, accelerated, and the particles collide with each other or the composite particles with an appropriate collision plate.

[0117] Examples of equipment include an Angmill (manufactured by Hosokawa Micron Corporation), a modified I-type mill (manufactured by Japan Pneumatic Co., Ltd.) with reduced grinding air pressure, a hybridization system (manufactured by Nara Machinery Works, Ltd.), a Cryptron system (manufactured by Kawasaki Heavy Industries, Ltd.), and an automatic mortar.

[0118] (External additives) The primary particle diameter of the inorganic fine particles is preferably 5 nm to 2 μm, and more preferably 5 nm to 500 nm. The specific surface area as measured by the BET method is preferably 20 to 500 m. 2 / g. The proportion of the inorganic fine particles used is preferably 0.01 to 5 mass % of the toner. Specific examples of the inorganic fine particles include silica, alumina, titanium oxide, barium titanate, magnesium titanate, calcium titanate, strontium titanate, zinc oxide, tin oxide, silica sand, clay, mica, wollastonite, diatomaceous earth, chromium oxide, cerium oxide, pengalla, antimony trioxide, magnesium oxide, zirconium oxide, barium sulfate, barium carbonate, calcium carbonate, silicon carbide, and silicon nitride.

[0119] Examples of polymeric fine particles include polymer particles made of polystyrene, methacrylate or acrylate copolymers obtained by soap-free emulsion polymerization, suspension polymerization, or dispersion polymerization, polycondensation systems such as silicone, benzoguanamine, and nylon, and thermosetting resins.

[0120] Such fluidizing agents are surface-treated to increase hydrophobicity and prevent deterioration of flow properties and charging properties even under high humidity. Examples of preferred surface treatment agents include silane coupling agents, silylating agents, silane coupling agents having a fluorinated alkyl group, organic titanate coupling agents, aluminum coupling agents, silicone oils, and modified silicone oils. Examples of cleaning improvers for removing the developer remaining on the photoconductor or primary transfer medium after transfer include fatty acid metal salts such as zinc stearate, calcium stearate, and stearic acid, and polymer fine particles produced by soap-free emulsion polymerization of, for example, polymethyl methacrylate fine particles, polystyrene fine particles, etc. The polymer fine particles preferably have a relatively narrow particle size distribution and a volume average particle size of 0.01 to 1 μm.

[0121] The toner according to the present embodiment can be effectively used as a material for image formation in a developer, a toner set, a toner storage unit, an image forming apparatus, and the like.

[0122] By using the toner according to this embodiment, the environmental impact is reduced, and even if a plant-derived resin is used, it is possible to provide an image having excellent low-temperature fixing property and charging property, and excellent image quality.

[0123] <Developer> The developer according to the present embodiment contains the toner according to one embodiment, and may contain other components, such as a carrier, that are appropriately selected as necessary. This allows the developer to have excellent transferability, chargeability, and the like, and to stably form high-quality images.

[0124] The developer may be a one-component developer or a two-component developer. However, when used in high-speed printers that correspond to the recent improvements in information processing speed, a two-component developer is preferable from the viewpoint of improving the developer life.

[0125] When the toner according to this embodiment is used in a one-component developer, even if the toner is balanced, there is little variation in the particle size of the toner, and toner filming on the developing roller and toner adhesion to components such as blades that thin the toner layer are reduced, resulting in high-quality images being obtained in the developing device.

[0126] When the developer according to the present embodiment is used as a two-component developer, it can be mixed with a carrier and used as a developer. When the toner according to the embodiment is used as a two-component developer, the particle size of the toner is small even if the toner is balanced over a long period of time, and good and stable developability and images can be obtained even when the toner is stirred for a long period of time in a developing device.

[0127] The content of the carrier in the two-component developer can be appropriately selected depending on the purpose, but is preferably 90 parts by mass to 98 parts by mass, and more preferably 93 parts by mass to 97 parts by mass, relative to 100 parts by mass of the two-component developer.

[0128] The developer according to the present embodiment can be suitably used for image formation by various known electrophotographic methods such as a magnetic one-component development method, a non-magnetic one-component development method, and a two-component development method.

[0129] [Career] The carrier is not particularly limited and can be appropriately selected depending on the purpose, but it is preferable that the carrier has a core material and a resin layer (coating layer) that coats the core material.

[0130] (Core material) The material of the core material is not particularly limited and can be appropriately selected according to the purpose. For example, manganese-strontium-based material of 50 emu / g to 90 emu / g, manganese-magnesium-based material of 50 emu / g to 90 emu / g, etc. can be mentioned. In order to ensure image density, it is preferable to use high magnetization materials such as iron powder of 100 emu / g or more, magnetite of 75 emu / g to 120 emu / g. In addition, it is preferable to use low magnetization materials such as copper-zinc-based materials of 30 emu / g to 80 emu / g, because it can reduce the impact of the developer in a standing state on the photoconductor and is advantageous for high image quality. These materials may be used alone or in combination of two or more.

[0131] The volume average particle diameter of the core material is not particularly limited and can be appropriately selected according to the purpose, but is preferably 10 μm to 150 μm, more preferably 40 μm to 100 μm. If the volume average particle diameter is 10 μm or more, the amount of fine powder in the carrier increases, and the magnetization per particle decreases, which can effectively prevent the problem of carrier scattering. On the other hand, if it is 150 μm or less, the specific surface area decreases, which can cause toner scattering, and in full color with many solid parts, the problem of poor reproduction of the solid parts can be effectively prevented.

[0132] (Resin layer) The resin layer can contain a resin and other components as necessary. The resin used in the resin layer can be a known material that can impart the necessary electrostatic property. Specifically, it is preferable to use a silicone resin, an acrylic resin, or a combination of these. In addition, the composition for forming the resin layer preferably contains a silane coupling agent.

[0133] The average thickness of the resin layer is preferably 0.05 to 0.50 μm.

[0134] <Measurement method> [Uneven distribution of release agent] The toner thus prepared is embedded in an epoxy resin and hardened. Ultrathin sections (approximately 100 nm thick) of the toner are prepared using an ultramicrotome (Leica ULTRACUT UCT, diamond knife used).

[0135] The sample is exposed to ruthenium tetroxide, osmium tetroxide, or another staining agent, and the release agent and other parts are differentiated. The exposure time is adjusted appropriately depending on the contrast during observation. The crystalline polyester resin phase is often observed as a lamellar structure. The sample is then observed with a transmission electron microscope (JEM-2100, JEOL) at an accelerating voltage of 100 kV. Depending on the composition of the release agent and amorphous polyester resin, it may be possible to differentiate them without staining, in which case they are evaluated unstained. It is also possible to impart compositional contrast by other means such as selective etching, and observation with a transmission microscope may be performed after such pretreatment.

[0136] If it is possible to distinguish between the release agent and the amorphous polyester resin, it is possible to observe using equipment other than TEM, such as a scanning electron microscope (SU-8230, Hitachi).

[0137] [Dispersion diameter of release agent] The observed cross-sectional images are binarized using commercially available image processing software (e.g., Image-Pro Plus, ImageJ, etc.) to calculate the maximum length and projected area of ​​the release agent. The cross sections of 20 or more toner particles with a toner particle size of Dv±20% are observed to determine the average of the maximum length of each release agent particle. The average of each release agent particle is calculated excluding the upper 10% and lower 10% of the maximum length of the release agent particles. The dispersion diameter of the release agent is preferably less than 3 μm, more preferably less than 2 μm, and even more preferably less than 1 μm.

[0138] <Image forming device> Next, one embodiment of a method for forming an image by the image forming apparatus of the present invention will be described with reference to Fig. 1. Although a printer is shown as an example of the image forming apparatus of this embodiment, the image forming apparatus is not particularly limited as long as it is capable of forming an image using toner, such as a copier, facsimile, or multifunction machine.

[0139] The image forming apparatus includes a paper feed section 210, a conveying section 220, an image creating section 230, a transfer section 240, and a fixing unit 250.

[0140] The paper feed section 210 includes a paper feed cassette 211 in which the paper P to be fed is stacked, and a paper feed roller 212 that feeds the paper P stacked in the paper feed cassette 211 one sheet at a time.

[0141] The conveying section 220 includes a roller 221 that conveys the paper P fed by the paper feed roller 212 toward the transfer section 240, a pair of timing rollers 222 that hold the leading end of the paper P conveyed by the roller 221 and wait to send the paper to the transfer section 240 at a predetermined timing, and a paper discharge roller 223 that discharges the paper P with the color toner image fixed thereto onto a paper discharge tray 224.

[0142] The image creating section 230 includes, spaced at a predetermined interval from left to right in the figure, an image forming unit Y that forms an image using a developer containing yellow toner, an image forming unit C that uses a developer containing cyan toner, an image forming unit M that uses a developer containing magenta toner, an image forming unit K that uses a developer containing black toner, and an exposure device 233.

[0143] Incidentally, when referring to any one of the image forming units (Y, C, M, K), it is referred to as an image forming unit.

[0144] The developer contains toner and carrier. Four image forming units (Y, C, M, K) are essentially identical in mechanical construction, except for the developer used.

[0145] The transfer unit 240 includes a drive roller 241 and a driven roller 242, an intermediate transfer belt 243 that can rotate counterclockwise in the figure as the drive roller 241 is driven, primary transfer rollers (244Y, 244C, 244M, 244K) arranged opposite the photosensitive drum 231 across the intermediate transfer belt 243, and secondary opposing roller 245 and secondary transfer roller 246 arranged opposite each other across the intermediate transfer belt 243 at the transfer position of the toner image to paper.

[0146] The fixing unit 250 includes a fixing belt 251 with an internal heater for heating the paper P, and a pressure roller 252 that forms a nip by applying pressure to the fixing belt 251 so as to be rotatable. This applies heat and pressure to the color toner image on the paper P, fixing the color toner image. The paper P with the fixed color toner image is discharged to a paper discharge tray 224 by a paper discharge roller 223, completing a series of image formation processes.

[0147] Although the embodiment has been described above, the above embodiment is presented as an example, and the present invention is not limited to the above embodiment. The above embodiment can be implemented in various other forms, and various combinations, omissions, substitutions, modifications, etc. can be made without departing from the gist of the invention. These embodiments and their modifications are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. EXAMPLES

[0148] The present invention will be described in more detail below based on examples, but the technical scope of the present invention is not limited to the following examples. In the following description, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".

[0149] <Preparation of amorphous polyester resin 1> In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 2 mol ethylene oxide adduct of bisphenol A / 3 mol propylene oxide adduct of bisphenol A (molar ratio 50 / 50) as a diol component, terephthalic acid / adipic acid (molar ratio 80 / 20) as a dicarboxylic acid component, and 3.5 mol% trimethylolpropane based on the total monomer amount were added so that the molar ratio of hydroxyl group to carboxylic acid (OH / COOH) was 1.1. Furthermore, 1,000 ppm of tetrabutyl orthotitanate based on the total monomer amount was added as a condensation catalyst, and the temperature was raised to 230°C over 2 hours under a nitrogen stream, and the reaction was carried out for 5 hours while distilling off the generated water. Then, the mixture was reacted for 4 hours under reduced pressure of 5mmHg to 15mmHg, and cooled to 180°C. Then, 1.0 mol% of trimellitic anhydride based on the total monomer amount and 200 ppm of tetrabutyl orthotitanate based on the total monomer amount were added, and the mixture was reacted for 1 hour at normal pressure and 180°C. Then, the mixture was reacted for 3 hours under reduced pressure of 5mmHg to 20mmHg, to obtain amorphous polyester resin 1 having a glass transition point of 55°C and a weight average molecular weight of 10,000, as determined from the DSC curve of the first heating cycle by DSC.

[0150] <Synthesis of crystalline polyester resin C-1> In a reaction vessel equipped with a cooling tube, a stirrer, a dehydration tube, a thermocouple, and a nitrogen inlet tube, 1,12-dodecanedioic acid and 1,6-hexanediol were charged so that the molar ratio of hydroxyl groups to carboxyl groups, OH / COOH, was 1.1, and trimellitic anhydride was added in a molar ratio of 0.047. The mixture was reacted together with titanium tetraisopropoxide (500 ppm relative to the resin component) at 180°C for 10 hours, then heated to 200°C and reacted for 3 hours, and further reacted at a pressure of 8.3 kPa for 2 hours to obtain a crystalline polyester resin C-1.

[0151] <Preparation of styrene acrylic resin> In an autoclave reaction tank equipped with a thermometer and a stirrer, 620 parts of xylene and 100 parts of low molecular weight polypropylene (Viscol 660P, manufactured by Sanyo Chemical Industries, Ltd.) were placed and thoroughly dissolved, and after replacing with nitrogen, a mixed solution of 755 parts of styrene, 100 parts of acrylonitrile, 45 parts of butyl acrylate, 21 parts of acrylic acid, 36 parts of di-t-butylperoxyhexahydroterephthalate, and 100 parts of xylene was added dropwise over 3 hours at 170°C to polymerize, and the mixture was maintained at this temperature for a further 0.5 hours. Next, the solvent was removed, and the number average molecular weight was 3,300, the weight average molecular weight was 18,000, the glass transition point was 65.0°C, and the SP value of the vinyl resin was 11.0 (cal / cm 3 ) 1 / 2 As a result, a styrene-acrylic resin of

[0152] <Preparation of release agent dispersion W-1> A container equipped with a stirring rod and a thermometer was charged with 300 parts of HNP-9 (manufactured by Nippon Seiro) and 1,200 parts of ethyl acetate, heated to 80°C while stirring, and held at 80°C for 5 hours, then cooled to 30°C, and dispersed using a bead mill (Ultraviscomill, manufactured by Imex) under the conditions of a liquid delivery rate of 1 kg / hr, a disk peripheral speed of 6 m / sec, 80% by volume of zirconia beads with a diameter of 0.5 mm, and 3 passes. Here, the temperature drop rate until the release agent started to precipitate during cooling (hereinafter referred to as temperature drop rate A) was controlled to 1.8°C / min, and the temperature drop rate until the release agent completely finished precipitating (hereinafter referred to as temperature drop rate B) was controlled to 1.0°C / min. Then, 180 parts of the release agent obtained by removing the ethyl acetate and 720 parts of ion-exchanged water were added with 17 parts of an anionic surfactant (Neogen SC, sodium dodecylbenzenesulfonate, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) as a surfactant. The mixture was dispersed with a homogenizer while being heated to 90°C, to obtain a release agent dispersion liquid W-1. The solid content concentration of the obtained wax dispersion liquid was adjusted to 20%.

[0153] <Preparation of release agent dispersion W-2> A container equipped with a stirring rod and a thermometer was charged with 300 parts of HNP-9 (manufactured by Nippon Seiro), 300 parts of amorphous polyester resin 1, and 900 parts of ethyl acetate, and the mixture was heated to 80°C under stirring, and then held at 80°C for 5 hours. The mixture was then cooled to 30°C, and dispersed using a bead mill (Ultraviscomill, manufactured by Imex) under conditions of a liquid delivery rate of 1 kg / hr, a disk peripheral speed of 6 m / sec, 80% by volume of zirconia beads with a diameter of 0.5 mm, and 3 passes to obtain a release agent dispersion W-2. Here, the cooling rate A was controlled to 1.8°C / min, and the cooling rate B was controlled to 1.0°C / min during cooling.

[0154] <Preparation of release agent dispersion W-3> A container equipped with a stirring rod and a thermometer was charged with 400 parts of HNP-9 (manufactured by Nippon Seiro), 200 parts of styrene acrylic resin, and 900 parts of ethyl acetate, and the mixture was heated to 80°C under stirring, and then held at 80°C for 5 hours. The mixture was then cooled to 30°C, and dispersed using a bead mill (Ultraviscomill, manufactured by Imex) under conditions of a liquid delivery rate of 1 kg / hr, a disk peripheral speed of 6 m / sec, 80% by volume of zirconia beads with a diameter of 0.5 mm, and 3 passes to obtain a release agent dispersion W-3. Here, the cooling rate A was controlled to 1.8°C / min, and the cooling rate B was controlled to 1.0°C / min during cooling.

[0155] <Preparation of release agent dispersion W-4> A container equipped with a stirring rod and a thermometer was charged with 240 parts of HNP-9 (manufactured by Nippon Seiro), amorphous polyester resin 1 (240 parts), 120 parts of styrene acrylic resin, and 900 parts of ethyl acetate, and the mixture was heated to 80°C under stirring, and then held at 80°C for 5 hours. The mixture was then cooled to 30°C, and dispersed using a bead mill (Ultraviscomill, manufactured by Imex) under conditions of a liquid delivery rate of 1 kg / hr, a disk peripheral speed of 6 m / sec, 80% by volume of zirconia beads with a diameter of 0.5 mm, and 3 passes to obtain a release agent dispersion W-4. Here, the cooling rate A during cooling was controlled to 1.8°C / min, and the cooling rate B was controlled to 1.0°C / min.

[0156] <Preparation of release agent dispersion W-5> A container equipped with a stirring rod and a thermometer was charged with 300 parts of HNP-9 (manufactured by Nippon Seiro) and 1,200 parts of ethyl acetate, heated to 80°C while stirring, and held at 80°C for 5 hours, then cooled to 30°C. Dispersion was performed using a bead mill (Ultraviscomill, manufactured by Imex) under conditions of a liquid delivery rate of 1 kg / hr, a disk peripheral speed of 6 m / sec, 80% by volume of zirconia beads with a diameter of 0.5 mm, and 3 passes to obtain a release agent dispersion W-5. Here, the cooling rate A was controlled to 1.8°C / min, and the cooling rate B was controlled to 1.0°C / min during cooling.

[0157] <Preparation of release agent dispersion W-6> Release agent dispersion W-6 was prepared in the same manner as in <Preparation of release agent dispersion W-1>, except that the temperature decreasing rate B during cooling was changed to 0.8° C. / min.

[0158] <Preparation of release agent dispersion W-7> Release agent dispersion W-7 was prepared in the same manner as in <Preparation of release agent dispersion W-5>, except that the temperature decreasing rate B during cooling was changed to 0.8° C. / min.

[0159] <Preparation of colorant master batch MB-1> Amorphous polyester resin 1 and carbon black (Printex35, Dexa) [DBP oil absorption = 42mL / 100mg, pH = 9.5] were premixed in a 1:1 ratio using a Henschel mixer (Mitsui Miike Chemical Engineering Co., Ltd., FM20B), and then melted and kneaded at a temperature of 150°C using a twin-screw kneader (Ikegai Co., Ltd., PCM-30). The resulting kneaded product was rolled to a thickness of 2.7mm with a roller, cooled to room temperature with a belt cooler, and coarsely pulverized to 200μm to 300μm with a hammer mill to obtain colorant master batch MB-1.

[0160] The amounts of each raw material used and the method of preparing the release agent dispersion in the examples described below are shown in Table 1. The adding step: "aggregation" indicates that the release agent dispersion is added in the aggregation step, and the adding step: "oil phase" indicates that the release agent dispersion is added in the oil phase preparation step. The number of parts added (parts) indicates the solid content.

[0161] [Table 1]

[0162] [Example 1] <Oil phase preparation process> Amorphous polyester resin 1 (650 parts), colorant master batch MB-1 (200 parts), and crystalline polyester resin C-1 (50 parts) were placed in a container and mixed with a TK homomixer (manufactured by Primix Corporation) at 5,000 rpm for 60 minutes to obtain oil phase 1. The above blend amounts indicate the blend amounts of solids in each raw material.

[0163] <Aqueous phase preparation process> 990 parts of water, 20 parts of sodium dodecyl sulfate, and 90 parts of ethyl acetate were mixed and stirred to obtain a milky white liquid. This was designated as aqueous phase 1.

[0164] <Emulsification process> Oil phase 1 (700 parts) was added with 20 parts of 28% aqueous ammonia while stirring at 8,000 rpm using a TK homomixer, and mixed for 10 minutes. Then, aqueous phase 1 (1,200 parts) was gradually added dropwise to obtain emulsified slurry 1.

[0165] <Solvent removal process> The emulsified slurry 1 was placed in a vessel equipped with a stirrer and a thermometer, and the solvent was removed at 30° C. for 180 minutes, whereby a solvent-free slurry 1 was obtained.

[0166] <Agglomeration process> The solvent-removed slurry 1 and the release agent dispersion W-1 (100 parts) were mixed, 100 parts of 3% magnesium chloride solution was dropped, and the mixture was stirred for another 5 minutes. The temperature was then raised to 60°C, and when the particle size reached 5.0 μm, 50 parts of a sodium sulfate aqueous solution was added to terminate the aggregation process, and aggregated slurry 1 was obtained.

[0167] <Fusing process> The aggregated slurry 1 was heated to 70° C. with stirring, and cooled when the desired average circularity of 0.96 was reached, to obtain a dispersed slurry 1.

[0168] <Cleaning and drying process> Dispersion slurry 1 (100 parts) was filtered under reduced pressure, (1) 100 parts of ion-exchanged water was added to the filter cake, mixed with a TK homomixer (at 12,000 rpm for 10 minutes), and then filtered. (2) 100 parts of a 10% aqueous sodium hydroxide solution was added to the filter cake of (1), and the mixture was mixed with a TK homomixer (at 12,000 rpm for 30 minutes), followed by filtration under reduced pressure. (3) 100 parts of 10% hydrochloric acid was added to the filter cake of (2), and the mixture was mixed in a TK homomixer (at 12,000 rpm for 10 minutes) and then filtered. (4) Add 300 parts of ion-exchanged water to the filter cake of (3), mix with a TK homomixer (at 12,000 rpm for 10 minutes), and then filter. The above steps (1) to (4) were repeated twice to obtain a filter cake 1. The filter cake 1 was dried in a circulating air dryer at 45° C. for 48 hours and sieved through a mesh having an opening of 75 μm to obtain a resin particle base body 1.

[0169] <External additive processing process> Resin particle base 1 (100 parts) was mixed with 2.0 parts of hydrophobic silica (HDK-2000, manufactured by Clariant) as an external additive in a Henschel mixer, and passed through a sieve with 500 mesh openings to obtain resin particles 1.

[0170] [Examples 2 to 5, Comparative Example 2] Resin particles 2 to 5 and 7 were obtained in the same manner as in Example 1, except that the release agent dispersion was added in the oil phase preparation process rather than in the aggregation process, and that the materials and the addition parts (solid content) shown in Table 1 were added.

[0171] [Comparative Example 1] Resin particles 6 are obtained in the same manner as in Example 1, except that the release agent dispersion W-1 is changed to the release agent dispersion W-6.

[0172] The uneven distribution of the release agent in these resin particles, the dispersion diameter of the release agent, and the upper limit of fixation were evaluated. The results are shown in Table 2.

[0173] [Table 2]

[0174] (Evaluation method) <Uneven distribution of release agent> Evaluate whether or not there is uneven distribution of the release agent in the resin particles. [Evaluation Criteria] ◎: Uniform throughout 〇: Some areas are unevenly distributed △: Distributed between 10% and 30% ×: More than 50% of the release agent is unevenly distributed, or release agent is separated during manufacturing.

[0175] <Dispersion diameter of release agent in resin particles> The dispersion diameter of the release agent in the resin particles is evaluated. [Evaluation Criteria] ◎: Less than 1μm ○: 1μm or more and less than 2μm △: 2μm or more and less than 3μm ×: 3μm or more

[0176] <Hot offset fixing> The carrier used in imageo MP C5503 (manufactured by Ricoh Company, Ltd.) and the resin particles obtained above were mixed so that the concentration of the resin particles was 5% by mass, to obtain a developer. After putting the developer into the unit of Imageo MP C5503 (manufactured by Ricoh Co., Ltd.), a rectangular solid image of 2 cm x 15 cm was printed on PPC paper type 6000<70W>A4 T (manufactured by Ricoh Co., Ltd.) with a resin particle adhesion amount of 0.40 mg / cm 2 At this time, the surface temperature of the fixing roller was changed, and it was observed whether hot offset occurred, in which the development residual image of the solid image was fixed in a place other than the desired place, and the upper limit of fixing was evaluated. [Evaluation Criteria] ◎: Hot offset occurs at 160℃ or higher ○: Hot offset occurs at temperatures between 150℃ and 160℃ △: Hot offset occurs between 140℃ and 150℃ ×: Hot offset occurs at temperatures below 140℃ [Prior art documents] [Patent documents]

[0177] [Patent Document 1] JP 2022-134262 A

Claims

1. A method for producing resin particles containing a binder resin and a release agent, comprising the steps of: a) preparing an oil phase by dissolving or dispersing the binder resin containing a polyester resin in an organic solvent; b) mixing the release agent with an organic solvent, heating the mixture, and then cooling the mixture to cause precipitation, thereby preparing a dispersion; c) aggregating the resin particles containing the binder resin and the release agent, b) In the cooling process, the temperature decreasing rate until the release agent starts to precipitate is A, and the temperature decreasing rate until the release agent completely precipitates is B, where A≦2B. A method for producing resin particles.

2. The method according to claim 1, wherein in the step b), a material of a second component containing at least a styrene-acrylic resin is mixed together with a release agent.

3. 3. The method according to claim 1, further comprising the steps of mixing the dispersion prepared in step b) with the oil phase prepared in step a), and adding water to invert the phase from the water-in-oil dispersion to an oil-in-water dispersion.

4. The method according to claim 1 or 2, wherein the dispersion liquid prepared in step b) is added to the aggregation step c).

Citation Information