Medical rubber composition and medical rubber product
A medical rubber composition with halogenated butyl rubber and a specific acid acceptor addresses pH changes and corrosion issues by absorbing halogen gas, providing excellent non-elution properties.
Patent Information
- Application Number
- JP2023069790
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-31
AI Technical Summary
Medical rubber products made from halogenated butyl rubber elute acid acceptors into drugs, causing pH changes and equipment corrosion during storage.
A medical rubber composition containing halogenated butyl rubber and an acid acceptor with a specific BET surface area of 150-200 m²/g and 1-3 parts by mass, which absorbs halogen gas and suppresses equipment corrosion while maintaining drug pH.
The composition maintains drug pH and prevents equipment corrosion by effectively absorbing halogen gas, ensuring excellent non-elution properties.
Smart Images

Figure 2024155234000003 
Figure 2024155234000004 
Figure 2024155234000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a medical rubber composition and a medical rubber product, and more particularly to a technique for improving the non-elution properties of a medical rubber product. [Background technology]
[0002] Medical rubber products applied to pharmaceutical containers are required to have high quality characteristics and physical properties. For example, the quality characteristics required for medical rubber stoppers that seal or plug the openings of vials that store antibiotics and other preparations should conform to the rubber stopper test for infusions in the 17th revised Japanese Pharmacopoeia, due to their intended use. Furthermore, many items are required for medical rubber stoppers that seal the openings of vials, such as gas permeability resistance, non-elution, high cleanliness, chemical resistance, needle resistance, self-sealing properties, and high sliding properties.
[0003] Halogenated butyl rubber is used for medical rubber products such as medical rubber stoppers because of its excellent gas (air, water vapor) permeability. When halogenated butyl rubber is heated during the kneading and molding process, halogen gas is generated, which can cause corrosion of equipment. It is known to mix an acid acceptor into halogenated butyl rubber to absorb the halogen gas.
[0004] For example, Patent Document 1 discloses a medical rubber composition that contains (a) a base polymer containing a halogenated butyl rubber and (b) a liquid polymer, and further contains hydrotalcite or magnesium oxide as an acid acceptor.
[0005] Patent Document 2 discloses a rubber product containing at least any one of rubber components selected from butyl rubber, halogenated butyl rubber, and chloroprene rubber, a filler, a vulcanizing agent, a vulcanization aid, and an acid acceptor selected from magnesium oxide, zinc oxide, and natural or synthetic hydrotalcite, and a precursor for a slidable rubber material bearing a silicone rubber top coating layer which covers the rubber product and has an interface modifying layer which contains an amino-modified silicone compound and / or has reacted with the surface molecules of the rubber product. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent Publication No. 2021-80370 [Patent Document 2] Patent Publication No. 2021-53988 Summary of the Invention [Problem to be solved by the invention]
[0007] When a medical rubber product made by molding a medical rubber composition using halogenated butyl rubber is stored in contact with a drug (e.g., saline), there is a problem that the pH of the drug (e.g., saline) increases as the storage period becomes longer.
[0008] The present invention has been made in view of the above circumstances, and aims to provide a medical rubber composition comprising a halogenated butyl rubber and an acid acceptor, which is capable of maintaining the pH of a drug while suppressing corrosion of equipment caused by halogen gas. Another aim of the present invention is to provide a medical rubber product having excellent non-elution properties. [Means for solving the problem]
[0009] The medical rubber composition of the present invention contains a base polymer containing a halogenated butyl rubber and an acid acceptor, the amount of the acid acceptor is 1 part by mass to 3 parts by mass per 100 parts by mass of the base polymer, and the BET specific surface area of the acid acceptor is 150 m 2 / g~200m 2 / g.
[0010] The present inventors have investigated the cause of the increase in pH of drugs over the longer storage period in medical rubber products made by molding a conventional medical rubber composition in which an acid acceptor is compounded with halogenated butyl rubber, and have found that the acid acceptor dissolves into the drug and affects the pH. 2 / g~200m 2 / g and in an amount of 1 to 3 parts by mass per 100 parts by mass of base polymer, the obtained medical rubber composition can maintain the pH of the drug while suppressing corrosion of equipment due to halogen gas, and thus the present invention has been completed. Effect of the Invention
[0011] According to the present invention, a medical rubber composition capable of maintaining the pH of a drug while suppressing corrosion of equipment caused by halogen gas can be obtained. Also, according to the present invention, a medical rubber product having excellent non-elution properties can be obtained. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is an explanatory diagram of one embodiment (stopper) of the medical rubber product of the present invention. [Diagram 2] FIG. 1 is an explanatory diagram of one embodiment (rubber stopper) of the medical rubber product of the present invention. [Diagram 3] FIG. 1 is an explanatory diagram of one embodiment of the medical rubber product of the present invention (rubber stopper for vial bottle). [Figure 4] FIG. 1 is an explanatory diagram of one embodiment of the medical rubber product of the present invention (rubber stopper for vacuum blood collection tube). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] <Medical rubber composition> The medical rubber composition of the present invention contains a base polymer containing a halogenated butyl rubber and an acid acceptor, the amount of the acid acceptor is 1 part by mass to 3 parts by mass per 100 parts by mass of the base polymer, and the BET specific surface area of the acid acceptor is 150 m 2 / g~200m 2 / g.
[0014] (Base polymer) First, the base polymer containing halogenated butyl rubber used in the present invention will be described. Examples of halogenated butyl rubber include chlorinated butyl rubber, brominated butyl rubber, and brominated copolymer of isobutylene and p-methylstyrene. The halogenated butyl rubber is preferably chlorinated butyl rubber or brominated butyl rubber. The chlorinated butyl rubber or brominated butyl rubber is, for example, obtained by adding or substituting chlorine or bromine to the isoprene structure portion of butyl rubber, specifically, the double bond and / or the carbon atom adjacent to the double bond. Note that butyl rubber is a copolymer obtained by polymerizing isobutylene and a small amount of isoprene.
[0015] The halogen content in the halogenated butyl rubber is preferably 0.5% by mass or more, preferably 1% by mass or more, more preferably 1.5% by mass or more, and is preferably 5% by mass or less, more preferably 4% by mass or less, and further preferably 3% by mass or less.
[0016] A specific example of the chlorinated butyl rubber is CHLOROBUTYL 1066 (stabilizer: NS, halogen content: 1.26%, Mooney viscosity: 38ML) manufactured by Japan Butyl Co., Ltd. 1+8 (125° C., specific gravity: 0.92); LANXESS X_BUTYL CB1240 manufactured by LANXESS Corporation, and the like.
[0017] A specific example of the brominated butyl rubber is BROMOBUTYL2255 (stabilizer: NS, halogen content: 2.0%, Mooney viscosity: 46ML) manufactured by Japan Butyl Co., Ltd. 1+8 (125° C., specific gravity: 0.93)]; at least one of LANXESS X_BUTYL BBX2 and X_BUTYL BB 2030 manufactured by LANXESS Corporation may be mentioned.
[0018] In the present invention, it is preferable to use a chlorinated butyl rubber or a brominated butyl rubber as the halogenated butyl rubber.
[0019] The base polymer may contain a rubber component other than halogenated butyl rubber. Examples of the other rubber components include butyl rubber, isoprene rubber, butadiene rubber, styrene butadiene rubber, natural rubber, chloroprene rubber, nitrile rubber such as acrylonitrile butadiene rubber, hydrogenated nitrile rubber, norbornene rubber, ethylene propylene rubber, ethylene-propylene-diene rubber, acrylic rubber, ethylene-acrylate rubber, fluororubber, chlorosulfonated polyethylene rubber, epichlorohydrin rubber, silicone rubber, urethane rubber, polysulfide rubber, phosphanzene rubber, and 1,2-polybutadiene. These may be used alone or in combination of two or more.
[0020] When other rubber components are used, the content of the halogenated butyl rubber in the base polymer is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 98% by mass or more. In a preferred embodiment, the base polymer consists of only the halogenated butyl rubber.
[0021] (acid acceptor) Next, the acid acceptor used in the present invention will be described. The acid acceptor is blended to absorb halogen gas (e.g., hydrogen chloride gas or hydrogen bromide gas) generated during crosslinking of halogenated butyl rubber. The acid acceptor is not particularly limited as long as it can be blended in a medical rubber composition, and examples thereof include metal oxides, metal hydroxides, and hydrotalcite.
[0022] Specific examples of the metal oxide include magnesium oxide (MgO), zinc oxide (ZnO), calcium oxide (CaO), and aluminum oxide (Al2O3). Specific examples of the metal hydroxide include magnesium hydroxide (Mg(OH)2), zinc hydroxide (Zn(OH)2), calcium hydroxide (Ca(OH)2), and aluminum hydroxide (Al(OH)3). Specific examples of the hydrotalcite include, for example, Mg 4.5 Al2(OH) 13 CO3 3.5H2O, Mg 4.5 Al2(OH) 13 CO3, Mg4Al2(OH) 12 CO3·3.5H2O, Mg6Al2(OH) 16 CO3·4H2O, Mg5Al2(OH) 14 CO3·4H2O, Mg3Al2(OH) 10 Examples of acid acceptors include Mg-Al hydrotalcites such as CO3·1.7H2O. Either natural or synthetic hydrotalcites can be used. These acid acceptors may be used alone or in combination of two or more.
[0023] In the present invention, the acid acceptor is preferably a metal oxide and / or a metal hydroxide, more preferably at least one selected from the group consisting of MgO, ZnO, Ca(OH)2, and Al(OH)3, and particularly preferably MgO or ZnO.
[0024] Specific examples of magnesium oxide used as the acid acceptor include commercially available products such as "Starmag R" manufactured by Konoshima Chemical Co., Ltd.
[0025] The BET specific surface area of the acid acceptor used in the present invention is 150 m 2 / g or more, and 2 / g or more is more preferable, and 170m 2 More preferably, it is 200m 2 / g or less, and 2 / g or less is more preferable, and 180m 2 / g or less is more preferable. If the BET specific surface area of the acid acceptor is within the above range, the halogen gas generated during processing is appropriately absorbed by the acid acceptor. The BET specific surface area of the acid acceptor is a value measured by a gas phase adsorption method using nitrogen gas as the adsorbent gas. For example, it can be measured according to the measurement method described in JIS Z 8830:2013 "Method for measuring the specific surface area of powder (solid) by gas adsorption."
[0026] The maximum particle size of the acid acceptor used in the present invention is preferably less than 20 μm, more preferably 18 μm or less, and even more preferably 15 μm or less. If the maximum particle size of the acid acceptor is less than 20 μm, the raw material itself can be prevented from becoming a white spot foreign matter, and the appearance of the product can be improved. The maximum particle size of the acid acceptor can be measured, for example, by a laser diffraction / scattering method (ultrasonication method).
[0027] The average particle size of the acid acceptor used in the present invention is preferably 2.0 μm or more, more preferably 3.0 μm or more, and preferably 5.0 μm or less, and more preferably 4.0 μm or less. If the average particle size of the acid acceptor is within the above range, the acid acceptor will not aggregate and cause white spots when dispersed in the base polymer, and can be dispersed more uniformly. The average particle size of the acid acceptor can be measured, for example, by a laser diffraction / scattering method (ultrasonic treatment method). The average particle size is measured by the volume-based D 50 The value was taken as the average particle size (μm).
[0028] The amount of the acid acceptor in the medical rubber composition of the present invention is preferably 1.0 part by mass or more, more preferably 1.2 parts by mass or more, even more preferably 1.5 parts by mass or more, and preferably 3.0 parts by mass or less, more preferably 2.5 parts by mass or less, and even more preferably 2.0 parts by mass or less, based on 100 parts by mass of the base polymer. If the content of the acid acceptor is 1.0 part by mass or more, the acid-accepting effect for halogen gas generated during the kneading and molding process of rubber is increased, and corrosion of the equipment used in these processes due to halogen gas can be suppressed. In addition, if the content of the acid acceptor is 3.0 parts by mass or less, the elution of the acid acceptor from the medical rubber product into the drug is suppressed, and the processability during molding (suitability of Mooney viscosity) is also improved.
[0029] The molar ratio (halogen / acid acceptor) of the halogen and acid acceptor contained in the halogenated butyl rubber is preferably 1.0 or less, more preferably 0.8 or less, even more preferably 0.7 or less, preferably 0.3 or more, more preferably 0.4 or more, and even more preferably 0.5 or more. If the molar ratio (halogen / acid acceptor) is 1.0 or less, the acid-accepting effect for halogen gas generated in the rubber kneading and molding process is higher, and corrosion of the equipment used in these processes by halogen gas can be further suppressed. In addition, if the molar ratio (halogen / acid acceptor) is 0.3 or more, the elution of the acid acceptor from the medical rubber product into the drug is further suppressed, and the processability during molding (suitability of Mooney viscosity) is also improved. The molar ratio (halogen / acid acceptor) can be calculated by the following formula. Molar ratio (halogen / acid acceptor)={(parts by mass of halogenated butyl rubber × halogen content in halogenated butyl rubber) / molecular weight of halogen} / {parts by mass of acid acceptor / molecular weight of acid acceptor}
[0030] (Vulcanizing agent) The medical rubber composition of the present invention preferably further contains a vulcanizing agent. The vulcanizing agent is blended to vulcanize the halogenated butyl rubber component contained in the base polymer. The vulcanizing agent is not particularly limited as long as it is capable of vulcanizing the halogenated butyl rubber. Examples of the vulcanizing agent include sulfur, organic peroxides, and triazine derivatives, which may be used alone or in combination of two or more kinds.
[0031] Examples of the sulfur include powdered sulfur, finely divided sulfur, precipitated sulfur, colloidal sulfur, and sulfur chloride.
[0032] Examples of the organic peroxide include dialkyl peroxide, peroxy ester, peroxy ketal, and hydroperoxide. Examples of the dialkyl peroxide include di(2-t-butylperoxyisopropyl)benzene, dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, t-butylcumyl peroxy, di-t-hexyl peroxy, di-t-butyl peroxy, and 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3. Examples of the peroxy ester include t-butyl peroxy maleate, t-butyl peroxy-3,3,5-trimethylcyclohexanoate, t-butyl peroxy laurate, t-butyl peroxy isopropyl monocarbonate, t-hexyl peroxy benzoate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butyl peroxy acetate, and t-butyl peroxy benzoate. Examples of peroxyketals include 1,1-di(t-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-di(t-hexylperoxy)cyclohexane, 1,1-di(t-butylperoxy)-2-methylcyclohexane, 1,1-di(t-butylperoxy)cyclohexane, 2,2-di(t-butylperoxy)butane, n-butyl-4,4-di(t-butylperoxy)valerate, 2,2-di(4,4-di(t-butylperoxy)cyclohexyl)propane, etc. Examples of hydroperoxides include p-menthane hydroperoxide, diisopropylbenzene hydroperoxide, etc.
[0033] The triazine derivative includes, for example, a compound represented by the general formula (1). [ka] [In the formula, R is -SH, -OR 1 , -SR 2 , -NHR 3 or -NR 4 R 5 (R 1 , R2 , R 3 , R 4 and R 5 R represents an alkyl group, an alkenyl group, an aryl group, an aralkyl group, an alkylaryl group, or a cycloalkyl group. 4 and R 5 may be the same or different. 1 and M. 2 is H, Na, Li, K, 1 / 2Mg, 1 / 2Ba, 1 / 2Ca, an aliphatic primary amine, a secondary amine or a tertiary amine, a quaternary ammonium salt or a phosphonium salt. 1 and M. 2 may be the same or different.]
[0034] In the general formula (1), examples of the alkyl group include alkyl groups having 1 to 12 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, tert-pentyl, n-hexyl, 1,1-dimethylpropyl, octyl, isooctyl, 2-ethylhexyl, decyl, and dodecyl. Examples of the alkenyl group include alkenyl groups having 1 to 12 carbon atoms, such as vinyl, allyl, 1-propenyl, isopropenyl, 2-butenyl, 1,3-butadienyl, and 2-pentenyl. Examples of the aryl group include monocyclic or condensed polycyclic aromatic hydrocarbon groups, such as aryl groups having 6 to 14 carbon atoms, such as phenyl, naphthyl, anthryl, phenanthryl, and acenaphthylenyl. Examples of the aralkyl group include aralkyl groups having 7 to 19 carbon atoms, such as benzyl, phenethyl, diphenylmethyl, 1-naphthylmethyl, 2-naphthylmethyl, 2,2-diphenylethyl, 3-phenylpropyl, 4-phenylbutyl, 5-phenylpentyl, 2-biphenylylmethyl, 3-biphenylylmethyl, and 4-biphenylylmethyl. Examples of the alkylaryl group include alkylaryl groups having 7 to 19 carbon atoms, such as tolyl, xyl, and octylphenyl. Examples of the cycloalkyl group include cycloalkyl groups having 3 to 9 carbon atoms, such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, and cyclononyl.
[0035] Specific examples of the triazine derivative represented by the general formula (1) include 2,4,6-trimercapto-s-triazine, 2-methylamino-4,6-dimercapto-s-triazine, 2-(n-butylamino)-4,6-dimercapto-s-triazine, 2-octylamino-4,6-dimercapto-s-triazine, 2-propylamino-4,6-dimercapto-s-triazine, 2-diallylamino-4,6-dimercapto-s-triazine, 2-dimethylamino-4,6-dimercapto-s-triazine, 2-dibutylamino- Examples thereof include 4,6-dimercapto-s-triazine, 2-di(iso-butylamino)-4,6-dimercapto-s-triazine, 2-dipropylamino-4,6-dimercapto-s-triazine, 2-di(2-ethylhexyl)amino-4,6-dimercapto-s-triazine, 2-dioleylamino-4,6-dimercapto-s-triazine, 2-laurylamino-4,6-dimercapto-s-triazine, and 2-anilino-4,6-dimercapto-s-triazine, or sodium salts or disodium salts thereof.
[0036] In the present invention, it is preferable to use sulfur or a triazine derivative as the vulcanizing agent.
[0037] The content of the vulcanizing agent in the medical rubber composition of the present invention is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and even more preferably 0.3 parts by mass or more, and preferably 5.0 parts by mass or less, more preferably 3.0 parts by mass or less, and even more preferably 1.0 parts by mass or less, relative to 100 parts by mass of the base polymer. If the content of the vulcanizing agent is within the above range, a rubber having good rubber properties (hardness, tensile strength, Cset) and good processability (less fading) can be obtained.
[0038] The medical rubber composition of the present invention preferably does not contain a vulcanization accelerator. This is because the vulcanization accelerator may remain in the final rubber product and dissolve into the drug solution in the syringe or vial. Examples of the vulcanization accelerator include guanidine-based accelerators (e.g., diphenyl guanidine), thiuram-based accelerators (e.g., tetramethylthiuram disulfide, tetramethylthiuram monosulfide), dithiocarbamate-based accelerators (e.g., zinc dimethyldithiocarbamate), thiazole-based accelerators (e.g., 2-mercaptobenzothiazole, dibenzothiazyl disulfide), and sulfenamide-based accelerators (N-cyclohexyl-2-benzothiazole sulfenamide, Nt-butyl-2-benzothiazole sulfenamide).
[0039] (Filler) The medical rubber composition of the present invention may further contain a filler. Examples of the filler include inorganic fillers such as clay and talc, olefin resins, styrene elastomers, and ultra-high molecular weight polyethylene (UHMWPE) resin powders. Among these, inorganic fillers are preferred, and clay or talc are more preferred. The filler functions to adjust the rubber hardness of the medical rubber product and also functions as an extender to reduce the production cost of the medical rubber product.
[0040] Examples of the clay include calcined clay and kaolin clay. Specific examples of the clay include SILLITIN (registered trademark) Z manufactured by HOFFMANN MINERAL, SATINTONE (registered trademark) W manufactured by ENGELHARD, NN kaolin clay manufactured by Tsuchiya Kaolin Kogyo Co., Ltd., and PoleStar 200R manufactured by Imerys Specialties Japan Co., Ltd.
[0041] Specific examples of the talc include Hitron A manufactured by Takehara Chemical Industry Co., Ltd., MICRO ACE (registered trademark) K-1 manufactured by Nippon Talc Co., Ltd., and ImerFlex T20 (registered trademark) manufactured by Imerys Specialties Japan.
[0042] The content of the filler in the medical rubber composition of the present invention is preferably set appropriately depending on the rubber hardness of the intended medical rubber product, etc. The content of the filler in the medical rubber composition of the present invention is, for example, preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 20 parts by mass or more, and preferably 200 parts by mass or less, more preferably 150 parts by mass or less, and even more preferably 100 parts by mass or less, relative to 100 parts by mass of the base polymer.
[0043] (Other Ingredients) In addition to the above-mentioned components, the medical rubber composition of the present invention may further contain colorants such as titanium oxide and carbon black, stearic acid, a low-density polyethylene (LDPE) lubricant, a processing aid, and polyethylene glycol as a crosslinking activator in appropriate proportions.
[0044] The medical rubber composition of the present invention is obtained by kneading the base polymer, the acid acceptor, and other compounding materials added as necessary. Kneading can be performed, for example, using an open roll, an internal kneader, etc. The kneaded product is preferably formed into a ribbon, sheet, pellet, etc., and more preferably formed into a sheet.
[0045] The Mooney viscosity (ML 1+4 (100°C)) is preferably 60 or more, more preferably 62 or more, and is preferably 75 or less, more preferably 70 or less. Mooney viscosity (ML 1+4 If the temperature (100° C.) is within the above range, the kneadability of the medical rubber composition becomes better, and the processability is further improved.
[0046] <Medical rubber products> The present invention includes a medical rubber product obtained by molding the medical rubber composition of the present invention. The medical rubber product of the present invention can be manufactured by a conventional manufacturing method. For example, a medical rubber product having a desired shape can be obtained by press molding the medical rubber composition molded into a ribbon, sheet, pellet, or the like. A crosslinking reaction (vulcanization reaction) of the medical rubber composition proceeds during pressing. The molding temperature is, for example, preferably 130°C or higher, more preferably 140°C or higher, and preferably 200°C or lower, more preferably 190°C or lower. The molding time is preferably 2 minutes or longer, more preferably 3 minutes or longer, preferably 60 minutes or shorter, and more preferably 30 minutes or shorter. The molding pressure is preferably 0.1 MPa or higher, more preferably 0.2 MPa or higher, preferably 10 MPa or lower, and more preferably 8 MPa or lower.
[0047] After press molding, unnecessary parts are cut and removed to give the desired shape. The resulting molded product is then washed, sterilized, dried, and packaged to produce medical rubber products.
[0048] The medical rubber product of the present invention may be laminated and integrated with a resin film in the same manner as in the past. Examples of the resin film include films of inactive resins such as polytetrafluoroethylene (PTFE), tetrafluoroethylene-ethylene copolymer (ETFE), and modified products thereof, and ultra-high density polyethylene (UHMWPE).
[0049] The resin film may be laminated on a sheet-like rubber composition and press-molded to be integrated with the medical rubber product formed after press molding.
[0050] The medical rubber product of the present invention can be suitably used, particularly as a medical rubber product that may come into contact with medicines, blood, etc. Specific examples of the medical rubber product of the present invention include medical rubber stoppers such as rubber stoppers for containers for various medicines such as liquid medicines, powder preparations, freeze-dried preparations, and rubber stoppers for vacuum blood collection tubes, and sliding or sealing parts such as stoppers for syringes.
[0051] Fig. 1 is a diagram showing a medical syringe in which the medical rubber product of the present invention is used, a so-called prefillable syringe, in an exploded state. In Fig. 1, a syringe 11 and a stopper 13 are half-sectionally shown. The prefillable syringe 10 includes a cylindrical syringe 11, a plunger 12 that is combined with the syringe 11 and can reciprocate within the syringe 11, and a stopper 13 that is attached to the tip of the plunger 12. The stopper 13 is molded from the medical rubber composition of the present invention. A laminate film for improving sliding properties may be laminated on the surface of the stopper 13.
[0052] The plunger 12 is formed, for example, of a resin plate having a cross-shaped cross section, and is provided with a head portion 18 at its tip to which the stopper 13 is attached. The head portion 18 is made of resin and formed integrally with the plunger 12, and is machined into a male thread shape. The stopper 13 is a roughly short-axis cylindrical member, and its tip surface is, for example, in the shape of an obtuse angled chevron with the shaft center protruding. A female thread-shaped mating recess 15 is formed by carving it axially from the rear end surface. The head portion 18 of the plunger 12 is screwed into the mating recess 15 of the stopper 13, whereby the stopper 13 is attached to the tip of the plunger 12.
[0053] Fig. 2 is a schematic cross-sectional view of one specific example of a rubber stopper 20 which is a medical rubber product of the present invention. Fig. 3 shows a state in which an opening 24b of a container 24 filled with a medicine is sealed with the rubber stopper 20.
[0054] The rubber stopper 20 is configured with a top plate 21 and a stopper leg 22. The top plate 21 has a puncture portion 23 that can be punctured with the injection needle of a syringe and a flange portion 21b that contacts the upper edge surface 24a of the container mouth of the medical container 24. The stopper leg 22 protrudes from the lower surface of the top plate 21 and is fitted into the medical container mouth. In addition, the stopper leg 22 has a substantially cylindrical shape and is provided with a notch 27. A nylon film layer 26 is provided on the top surface of the top plate 21 of the rubber stopper 20. By providing the nylon film layer 26 on the top surface of the rubber stopper 20, mechanical transportability during pharmaceutical production can be ensured. In addition, by providing the nylon film layer 26 on the top surface of the rubber stopper 20, the surface smoothness of the top surface can be increased, and the generation of needle fragments can be prevented when the injection needle is punctured.
[0055] In the embodiment shown in Fig. 3, a vial for storing a freeze-dried preparation is used as container 24. When the liquid pharmaceutical to be contained in container 24 is an injectable liquid, the needle of a syringe is inserted into puncture portion 23 of top plate 21, and the injectable liquid is drawn into the syringe without opening rubber stopper 20. In this manner, rubber stopper 20 is not opened in order to prevent foreign matter from being mixed into the injectable liquid in container 24.
[0056] A metal or resin cap 25 capable of covering the opening 24b of the container 24 and the rubber stopper 20 is provided on the top plate 21. The rubber stopper 20 is sealed with the cap 25, including the opening 24b, in order to prevent mold from adhering to the puncture part 23 where the needle of the syringe is inserted and mixing the mold into the injection liquid from the needle. The cap 25 may be of any type, such as a flip-off cap, pull-top cap, or clean cap. When a large amount of injection liquid is used, such as in a hospital, it is preferable to use a clean cap that can be opened with one hand and is easy to operate.
[0057] 4 is an explanatory diagram showing an example of a vacuum blood collection tube. The vacuum blood collection tube 50 comprises a bottomed tube 51 and a rubber plug 53 that seals the opening of the bottomed tube 51. Such a rubber plug 53 is formed from the medical rubber composition of the present invention. It is designed so that blood can be automatically collected by reducing the pressure inside the blood collection tube. EXAMPLES
[0058] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the following examples, and all modifications and embodiments that do not deviate from the spirit of the present invention are included within the scope of the present invention.
[0059] [Preparation of medical rubber composition] A medical rubber composition was prepared by kneading the materials shown in Table 1. The kneading was carried out using an internal pressure kneader at 80° C. to 140° C. for 5 minutes to 30 minutes.
[0060] [Table 1]
[0061] The details of the compounding materials used are as follows: Brominated butyl rubber: BROMOBUTYL2255 manufactured by Japan Butyl Co., Ltd. [Bromine content: 2.0%] Acid acceptor 1: Starmag (registered trademark) R (magnesium oxide, BET specific surface area 178 m) manufactured by Konoshima Chemical Co., Ltd. 2 / g, maximum particle size 13μm, average particle size 3.5μm) Acid acceptor 2: Kyowa Chemical Industry Co., Ltd.'s Magsarat (registered trademark) 150ST (magnesium oxide, BET specific surface area 65 m 2 / g, maximum particle size 20μm, average particle size 4.8μm) Acid acceptor 3: Starmag (registered trademark) M (magnesium oxide, BET specific surface area 47 m) manufactured by Konoshima Chemical Co., Ltd. 2 / g, maximum particle size 262μm, average particle size 3.5μm) Sulfur: 5% oil-containing sulfur manufactured by Tsurumi Chemical Industry Co., Ltd. Talc: ImerFlex T20 (registered trademark) manufactured by Imerys Specialties Titanium oxide: Ishihara Sangyo Kaisha, Ltd., Typec (registered trademark) A-100 Carbon black: Thermax MT from Cancarb Limited
[0062] [Evaluation method] (1) Mooney Viscosity The Mooney viscosity of the medical rubber composition was measured in accordance with the measurement method described in JIS K6300-1:2013 "Method of determining viscosity and scorch time using a Mooney viscometer."
[0063] (2) BET specific surface area of the acid acceptor (m 2 / g) The BET specific surface area was measured under the following conditions. Measuring device: Macsorp HM model (manufactured by Mountec Co., Ltd.) Pretreatment conditions: 160℃, 1 hour Measurement method for the amount of adsorbed gas: Carrier gas method Method for analyzing adsorption data: Single point method
[0064] (3) Particle size of acid acceptor (μm) 50 mL of ethanol was placed in a 100 mL beaker, about 0.2 g of the sample powder was added, and ultrasonic treatment (UD-201, manufactured by Tommy Seiko Co., Ltd.) was performed for 3 minutes to prepare a dispersion liquid. This preparation liquid was measured using a laser diffraction method-particle size distribution analyzer (Microtrac HRA Model 9320-X100, manufactured by Nikkiso Co., Ltd.). From the obtained particle size distribution, the volume-based D 50 The value and maximum particle size were determined.
[0065] (4) Visual inspection The prepared medical rubber composition was press molded at 15 to 20 atmospheres and 165°C to 190°C for 7 to 20 minutes to prepare a slab (length 225 mm, width 60 mm, thickness 2 mm). The surface of the slab was visually observed to confirm the presence of white spots due to the acid acceptor, and the appearance was evaluated according to the following evaluation criteria. ◯: No white spots due to the acid acceptor were found. △: Only one white spot caused by the acid acceptor was found. ×: Two or more white spots caused by the acid acceptor were observed.
[0066] (5) Extractables Test The prepared medical rubber composition was press molded at 15 to 20 atmospheres and 165°C to 190°C for 7 to 20 minutes to prepare a measurement sample (φ17 mm, 2 mm thick sample) for the elution test. The prepared measurement sample was washed with water or an alkaline aqueous solution such as an aqueous sodium carbonate solution at 121°C for 30 minutes using an autoclave, and then immersed in water for three times to wash. 200g of physiological saline was placed in a glass bottle, and the washed sample was immersed in the test liquid, which was then stored in an oven at 40°C for a predetermined period (0h, 6h, 24h, 48h, 72h, 96h, 168h, 336h, 504h). A blank test liquid in which only 200g of physiological saline was placed in a glass bottle was also stored in an oven at 40°C for a predetermined period. After a certain period of time, the test liquid and the blank test liquid were removed from the oven and cooled to room temperature, and then their pH was measured using a pH meter (LAQUA D-210P model manufactured by Horiba, Ltd.) and the pH difference between them was calculated. The maximum value (peak value) of the pH difference between the test liquid and the blank test liquid during the certain period of time was used to evaluate the non-elution of the acid acceptor according to the following evaluation criteria. The smaller the pH difference, the less the acid acceptor was eluted. ◯: The maximum pH difference between the test solution and the blank test solution is less than 1.05. ×: The maximum pH difference between the test solution and the blank test solution is 1.05 or more.
[0067] (6) Corrosion of equipment After the medical rubber composition was kneaded at 80° C. to 140° C. for 5 to 30 minutes, the metal surface of the kneading machine was visually inspected and the corrosion of the equipment was evaluated according to the following evaluation criteria. Good: The metal is not corroded and the surface gloss is maintained. △: The metal is slightly corroded and the surface gloss is reduced. ×: The metal corrodes, the surface loses its luster, and with continued use, dirt adheres to it and it turns brown.
[0068] The evaluation results for each item are shown in Table 1.
[0069] As is apparent from the results in Table 1, the composition contains a base polymer containing a halogenated butyl rubber and an acid acceptor, the content of the acid acceptor is 1 part by mass to 3 parts by mass per 100 parts by mass of the base polymer, and the BET specific surface area of the acid acceptor is 150 m 2 / g~200m 2 The medical rubber composition of the present invention, which has a viscosity of 1000 ppm or more and a viscosity of 1000 ppm or more, can reduce the elution of the acid acceptor into the drug (maintain the pH of the drug) while suppressing corrosion of equipment due to halogen gas. [Explanation of symbols]
[0070] 10: injector, 11: syringe, 12: plunger, 13: stopper, 15: fitting recess, 18: head portion, 20: rubber stopper, 21: top plate, 21b: flange portion, 22: stopper leg, 23: puncture portion, 24: medical container, 24a: upper edge surface, 24b: opening, 25: cap, 26: nylon film layer, 27: notch, 50: vacuum blood collection tube, 51: bottomed tube, 53: rubber stopper [Industrial Applicability]
[0071] The present invention is suitably applicable to medical rubber compositions and medical rubber products.
[0072] A preferred embodiment (1) of the present invention is a rubber composition comprising a base polymer containing a halogenated butyl rubber and an acid acceptor, the amount of the acid acceptor being 1 part by mass to 3 parts by mass per 100 parts by mass of the base polymer, and the BET specific surface area of the acid acceptor being 150 m 2 / g~200m 2 / g.
[0073] A preferred embodiment (2) of the present invention is the medical rubber composition according to embodiment (1), wherein the halogenated butyl rubber is a chlorinated butyl rubber or a brominated butyl rubber.
[0074] A preferred embodiment (3) of the present invention is the medical rubber composition according to the embodiment (1) or (2), in which the acid acceptor contains magnesium oxide or zinc oxide.
[0075] A preferred embodiment (4) of the present invention is the medical rubber composition according to any one of the embodiments (1) to (3), in which the maximum particle size of the acid acceptor is less than 20 μm.
[0076] A preferred embodiment (5) of the present invention is the medical rubber composition according to any one of the embodiments (1) to (4), further comprising a vulcanizing agent.
[0077] A preferred embodiment (6) of the present invention is the medical rubber composition according to any one of the embodiments (1) to (5), further comprising a filler.
[0078] In a preferred embodiment (7) of the present invention, the Mooney viscosity (ML 1+4 (100° C.)) is 60 to 75.
[0079] A preferred embodiment (8) of the present invention is a medical rubber product obtained by molding the medical rubber composition according to any one of the embodiments (1) to (7).
[0080] A preferred embodiment (9) of the present invention is the medical rubber product according to embodiment (8), which is a stopper for a syringe.
Claims
1. The present invention comprises a base polymer including a halogenated butyl rubber and an acid acceptor, The amount of the acid acceptor is 1 to 3 parts by mass relative to 100 parts by mass of the base polymer, and the BET specific surface area of the acid acceptor is 150 m 2 / g to 200m 2 / g.
2. 2. The medical rubber composition according to claim 1, wherein the halogenated butyl rubber is a chlorinated butyl rubber or a brominated butyl rubber.
3. The medical rubber composition according to claim 1 , wherein the acid acceptor comprises magnesium oxide or zinc oxide.
4. 2. The medical rubber composition according to claim 1, wherein the maximum particle size of the acid acceptor is less than 20 μm.
5. The medical rubber composition according to claim 1, further comprising a vulcanizing agent.
6. The medical rubber composition according to claim 1 , further comprising a filler.
7. Mooney Viscosity (ML 1+4 2. The medical rubber composition according to claim 1, wherein the viscosity at 100° C. is 60 to 75.
8. A medical rubber product obtained by molding the medical rubber composition according to any one of claims 1 to 7.
9. 9. The medical rubber product according to claim 8, which is a stopper for a syringe.
Citation Information
Patent Citations
Rubber composition for medical implement, and its crosslinked product
JP2003147138A
Thermoplastic elastomeric composition and production process
JP2009102615A
Encapsulant
JP2016186014A
Fluorine-containing copolymer composition, metal-rubber laminate, and method of manufacturing metal-rubber laminate
JP2021063197A
Precursor for slidable rubber material carrying coating layer overcoated with silicone rubber