Method for manufacturing sample

The method of sputtering and plasma smoothing techniques addresses the issue of physical damage in existing observation methods, enabling precise and detailed observation of inclusions in steel materials, enhancing the reliability and lifespan of bearing products.

JP2024155263AInactive Publication Date: 2024-10-31SANYO SPECIAL STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023069853
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for observing non-metallic inclusions in steel materials cause physical damage and fail to provide precise, wide-range observation of inclusions and their surrounding microstructures, affecting the reliability and lifespan of bearing products.

Method used

A method involving sputtering and plasma smoothing techniques using Ar and O2 gases to expose and smooth the sample surface, followed by optional corrosion treatment, allowing for precise observation of inclusions and their microstructures without physical damage.

Benefits of technology

Enables detailed observation of inclusions and their microstructures, facilitating better understanding of their harmfulness and fatigue behavior, thereby improving the reliability and lifespan of bearing products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155263000001_ABST
    Figure 2024155263000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing a sample capable of precisely grasping the state of inclusions in a steel material or a steel material component.SOLUTION: In a method for manufacturing a sample of a steel material or a steel material component to be used for observation of inclusions, an inclusions revealing step and a first smoothing step are performed. In the inclusions revealing step, Ar gas is converted into plasma by glow discharge, and a processed surface of the sample is sputtered, thereby causing the inclusions in the sample to emerge on a processed surface. After the inclusions revealing step, the first smoothing step is carried out, in which a gas mixture of Ar and O2 is converted into plasma by glow-discharge to further sputter the processed surface, thereby smoothing the processed surface.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This relates to a method for preparing samples to be used for observing nonmetallic inclusions and their surrounding areas present in steel materials and steel products. [Background technology]

[0002] Even if a bearing is used in an appropriate environment, it may break before its lifespan, and non-metallic inclusions (hereafter referred to as "inclusions") present in the bearing steel are thought to be one of the causes of breakage. Inclusions are inevitably generated and mixed into the steel during the refining process, and inclusions that cannot be completely removed during the casting and solidification process after refining end up in the bearing material or bearing product obtained by rolling or forging after the casting and solidification process.

[0003] Inclusions are foreign bodies with properties different from steel, and if such inclusions are present in an area directly below the raceway of a bearing where shear stress is high, stress will concentrate around the inclusion during use, generating cracks that may propagate and lead to spalling. In other words, inclusions are considered to be an influencing factor that has a detrimental effect on the life of the bearing.

[0004] The above-mentioned inclusions include oxides, sulfides, nitrides, etc., and the state (composition, size, shape, etc.) of each inclusion is different from the others, and it is thought that this difference in state will manifest as a difference in the harmfulness to the life.

[0005] Non-Patent Document 1 describes that as the size of inclusions increases, the rolling fatigue life of the bearing decreases. Non-Patent Documents 2 and 3 state that when gaps are formed between inclusions and the parent phase surrounding them, their detrimental effect on the life span increases. It is believed that these gaps are generated because the deformability of the steel and the inclusions contained therein differs when the cast steel is subsequently hot worked to be manufactured into a semi-finished product, and when the steel subsequently undergoes various plastic working processes to be made into a finished product. [Prior art documents] [Non-patent literature]

[0006] [Non-Patent Document 1] M. Nagao, K. Hiraoka, Y. Unigame: Sanyo Special Steel Technical Report, 12 (2005) 1, 38-45 [Non-Patent Document 2] Takeshi Fujimatsu, Kazuhiko Hiraoka, and Atsuyuki Yamamoto, "Crack Initiation Behavior from Internal Defects in Rolling Contact Fatigue of High Carbon Chromium Bearing Steel," Iron and Steel, The Iron and Steel Institute of Japan, Vol. 94, No. 1 (2008), pp. 13-20 [Non-Patent Document 3] K. Hashimoto, T. Fujimatsu, N. Tsunekage, K. Hiraoka, K. Kida, E. Santos, "Effect of inclusion / matrix interface cavities on internal―fracture―type rolling contact fatigue life," Materials & Design, Elsevier BV, (Netherlands), Vol. 32, Issue 10, December 2011, p. 4980-4985 Summary of the Invention [Problem to be solved by the invention]

[0007] As described above, changes in the state of inclusions in steel and the condition of the gaps around the inclusions can change the rolling fatigue behavior of the finished bearing, which can then affect its life. Therefore, it may be possible to improve the life of bearings by appropriately controlling the state of inclusions in steel materials in processes from the steel refining stage to the product manufacturing stage. In addition, some inclusions in steel have no known harmful effects on rolling fatigue, and it is considered necessary to investigate the harmful effects of such inclusions in order to improve the reliability of products such as bearing steel.

[0008] In order to investigate the harmful effects of inclusions, it is essential to observe the inclusions in steel and bearing products, and to understand the relationship with the fatigue behavior of the surrounding microstructure, etc. By gaining a detailed understanding of the state of the inclusions in steel, it is possible to verify their harmful effects in more detail, and it is expected that better improvement measures can be found. Furthermore, when the harmfulness of an inclusion with certain properties and characteristics is unknown, in order to confirm the harmfulness of such an inclusion, it is necessary to conduct a rolling fatigue test or the like and then observe the relationship between the inclusion and its surroundings.

[0009] Here, by directly observing the inclusions, more information about the inclusions can be obtained. Direct observation includes a method of two-dimensionally observing the cross section where the inclusions are present. Specifically, direct observation methods include a method of polishing the cross section and observing it, and a method of polishing a micro area with a focused ion beam (FIB) and then observing it.

[0010] Methods that utilize cross-section polishing include a processing step using rough polishing, which involves a relatively large amount of grinding. From a microscopic perspective, this processing step involves physically scraping off material using abrasive grains attached to grinding paper, and there are cases in which the inclusions to be observed get caught by the abrasive grains and fall off. Furthermore, when a gap exists around an inclusion, the base material around the gap may become thin and burr-like and cover the gap, making it impossible to precisely observe the actual state of the gap around the inclusion.

[0011] One possible processing method that can solve these problems, that is, a processing method that does not involve physical snagging or the formation of burrs, is to use a focused ion beam (FIB). However, the area that can be removed with a focused ion beam (FIB) is generally limited to a range of about several tens of μm, and therefore it is not considered suitable as a means for observing inclusions larger than that size, or the overall behavior of cracks arising from those inclusions.

[0012] An object of the present invention is to provide a method for preparing an observation specimen which causes less physical polishing damage to inclusions than conventional methods and allows for detailed observation of the state of a wide cross section. [Means for solving the problem]

[0013] In order to solve the above problems, the sample preparation method of the present invention is a method for preparing a sample of a steel material or steel part to be subjected to inclusion observation, and is characterized by having: (1) an inclusion revealing step in which Ar gas is turned into plasma by glow discharge and the processed surface of the sample is sputtered to reveal inclusions inside the sample on the processed surface; and after the inclusion revealing step, a first smoothing step in which a mixed gas of Ar and O2 is turned into plasma by glow discharge and the processed surface is further sputtered to smooth the processed surface.

[0014] (2) The method for preparing a sample according to (1) above, characterized in that after the first smoothing step, a second smoothing step is performed on the processed surface by Ar ion milling.

[0015] (3) A method for preparing a sample as described in (1) above, characterized in that after carrying out the first smoothing step, a corrosion treatment is carried out on the processed surface to reveal the microstructure around the inclusions.

[0016] (4) A method for preparing a sample as described in (2) above, characterized in that after the second smoothing step, a corrosion treatment is performed on the processed surface to reveal the microstructure around the inclusions.

[0017] (5) A method for preparing a sample described in any one of (1) to (4) above, characterized in that the inclusions contained in the sample subjected to the inclusion revealing process are inclusions that have been previously subjected to fatigue due to repeated loads.

[0018] (6) A method for preparing a sample according to any one of (1) to (4) above, characterized in that a depth adjustment process is carried out before carrying out the inclusion revealing process, in which the depth from the sample surface to the position where the inclusion is present is adjusted to within 0.1 mm.

[0019] (7) A method for preparing a sample described in any one of (1) to (4) above, characterized in that the presence or absence of inclusions is determined by carrying out the inclusion revealing step while analyzing the elements of the sputtered particles.

[0020] (8) A method for preparing a sample according to (5) above, characterized in that the presence or absence of inclusions is determined by carrying out the inclusion revealing step while analyzing the elements of the sputtered particles.

[0021] (9) A method for preparing a sample according to (6) above, characterized in that the presence or absence of inclusions is determined by carrying out the inclusion revealing step while analyzing the elements of the sputtered particles.

[0022] (10) A method for preparing a sample according to (7) above, characterized in that the presence or absence of inclusions is determined by carrying out the inclusion revealing step while analyzing the elements of the sputtered particles. Effect of the Invention

[0023] By using the specimens prepared according to the present invention for observation, it becomes possible to grasp the state of inclusions in steel or steel parts more precisely than ever before. This makes it possible to investigate, for example, the harmfulness of inclusions in bearing steel in more detail, and can be used to propose more effective improvement measures based on the results and to investigate the fatigue behavior of inclusions whose harmfulness is unknown. [Brief description of the drawings]

[0024] [Figure 1] 1 shows an SEM image of an inclusion and its surroundings immediately after an inclusion revealing process was carried out on a sample of an example. [Diagram 2]This is an SEM image of an inclusion and its surroundings immediately after the first smoothing process was carried out on the sample in Figure 1. [Diagram 3] This is an SEM image of the sample in Figure 2 immediately after the corrosion treatment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] The sample preparation method of this embodiment is a method for preparing a sample of a steel material or a steel part to be subjected to inclusion observation, and includes a preparation step, an inclusion revealing step, and a first smoothing step. If necessary, a second smoothing step and / or an etching treatment may also be carried out.

[0026] (About the preparation process) The specimens to be used for observing inclusions are selected according to the purpose of observation. Here, observing inclusions includes observing the state of the inclusions contained in the specimen (shape, distribution, state of gaps around the inclusions) and observing the microstructure around the inclusions. The sample may be a steel material or a steel part (including "a cut portion cut out from a steel part"; the same applies below). The steel material includes steel material for bearings, etc. The steel part includes bearing products, etc. The sample may also be a steel material or a steel part after it has been subjected to fatigue such as rolling fatigue. The inclusions may be inclusions that are inevitably produced during the steel refining process (hereinafter also referred to as unavoidable inclusions), or inclusions that are artificially embedded (hereinafter also referred to as artificial inclusions).

[0027] (Regarding the inclusion revealing process) Sputtering is performed on the processed surface of the sample, and a process is performed to expose the inclusions inside the sample on the processed surface (sputtered surface). The processed surface of the sample is the surface on which the inclusion revealing process is performed, and any surface of the sample (that is, any surface) can be used as the processed surface. The processed surface may be a cut surface of the sample. In this case, it is preferable to grind the cut surface. At this point, the inclusions have not been revealed, so the grinding method is not particularly specified. However, since there are cases in which the sample is corroded after preparation to observe the microstructure, it is preferable to use a method that does not cause damage to the sample due to heat. For example, wet polishing with emery paper may be used as a grinding method. Next, the Ar gas is turned into plasma by glow discharge, and the processed surface of the sample is gradually removed by colliding Ar ions with it. Sputtering using Ar gas allows for relatively fast sputtering, making it possible to replace a series of conventional grinding and finishing processes, and to perform these processes quickly.

[0028] For example, a radio-frequency glow discharge optical emission surface analyzer can be used as an apparatus for performing sputtering. A radio-frequency glow discharge optical emission surface analyzer is equipped with a sputtering function and a simultaneous elemental analysis function. That is, a radio-frequency voltage is applied to a plasma generating electrode via a sample to generate Ar plasma between the sample and the electrode, thereby sputtering the sample surface, and the sputtered atoms (referred to as sputtered particles) are made to emit atomic light in the plasma, and elemental analysis can be performed simultaneously by analyzing the emission spectrum.

[0029] A high-frequency glow discharge optical emission surface analysis instrument can perform localized processing at a high sputtering rate (i.e., a high processing rate) with minimal damage to the sample using plasma, while sensitively detecting the behavior of changes in elements on the processed surface.

[0030] A high-frequency glow discharge optical emission surface analyzer can detect changes in elements with a minimum detection sensitivity of the order of ppm. This makes it possible to grasp changes in the appearance of inclusions on the processed surface, i.e., the surface being observed (such as a gradual increase in the area in which inclusions appear) from changes in the detection intensity of elements. In other words, by performing an inclusion revealing process while analyzing the elements of the sputtered particles, it is possible to grasp the presence or absence of inclusions. Incidentally, since the size of the inclusions (typically around several tens of μm) is often small compared to the size of the machined surface (typically in the range of a few mm), it is desirable to narrow down the types of elements of interest in advance so that changes in the specific elements of interest can be detected more sensitively.

[0031] As sputtering conditions, it is desirable to appropriately set the electrode diameter, Ar gas pressure, and high-frequency applied voltage. If the electrode diameter is small, the energy density of the generated plasma increases, and the sputtering rate increases, but the detection sensitivity of elements decreases. From this perspective, the electrode diameter is desirably 2 mm or more and 4 mm or less in diameter. In addition, the Ar gas pressure and the high frequency applied voltage are both parameters that affect the sputtering rate and the smoothness of the shape of the sputtered mark. Therefore, from the viewpoint of making the sputtered bottom smoother, the Ar gas pressure is preferably 200 Pa or more and 800 Pa or less, and the high frequency applied voltage is preferably 20 W or more and 45 W or less.

[0032] The position of the sample where sputtering is performed is arbitrary, but for example, when the inclusion to be observed is predetermined, sputtering may be performed for the purpose of observing the inclusion. In this case, the inclusion may be an unavoidable inclusion or an artificial inclusion, as described above. For example, although the frequency of occurrence in actual steel materials or products is rare, if a large inclusion is present in a dangerous portion (such as directly below the raceway of a bearing as described above), there is a risk of the component being damaged in a short lifespan. In this case, in order to perform observation assuming such a large inclusion, a sample containing an artificial inclusion may be selected, and an inclusion revealing process may be performed in which the artificial inclusion is the observation target. Test pieces using such artificial inclusions are convenient for placing the inclusions in advance in the area directly under the raceway surface that is affected by fatigue (rolling fatigue) in the bearing so that they are included in the area to be observed by this method after the fatigue test, and are also convenient for processing them into minute samples for high-resolution observation and for conducting CT observation of fatigue cracks caused by rolling fatigue. The position where the inclusions are artificially placed in this case is not particularly specified because it varies depending on the conditions for performing the rolling fatigue test, but it is possible to place the inclusions in advance within a depth suitable for sputtering (within 0.1 mm as described below).

[0033] When sputtering is performed on a predetermined inclusion, it is first necessary to adjust the sputtering position based on the location of the inclusion. This is because if sputtering processing is continued beyond a depth of about 0.1 mm, the distance from the electrode to the processing surface becomes too far, making it difficult to continue stable generation of plasma, and sputtering cannot be continued any further. Therefore, it is better to adjust the location of the inclusion to a position shallower than 0.1 mm from the sample surface.

[0034] As a method for grasping the position (coordinates) of an inclusion in advance, for example, ultrasonic testing can be used. According to ultrasonic testing, an ultrasonic beam is irradiated onto a sample, and the ultrasonic waves propagating inside the sample hit the inclusion and are reflected. By detecting the reflected waves, information such as the position of the inclusion can be collected nondestructively. For example, based on information such as the time it takes for the reflected waves to return, the depth (position information) from the sample surface to the position of the inclusion can be identified. In addition, by changing the frequency of the ultrasonic waves, the detectable depth range and defect detection resolution can be varied, and by selecting these appropriately, it is possible to collect information on inclusions of a size appropriate for the purpose.

[0035] After collecting the position information of the inclusions, a depth adjustment process is performed to adjust the position of the inclusions to within a depth range where sputtering is possible. In this adjustment process, based on the position information of the inclusions identified by ultrasonic flaw detection, the depth from the sample surface to the position where the inclusions are present is adjusted to within 0.1 mm. The adjustment method may be grinding or the like. At this stage, the inclusions do not appear on the surface, that is, there is no physical damage caused by grinding, so grinding can be used. In other words, in this depth adjustment process, the inclusions themselves are not ground, so it is possible to prevent the inclusions to be observed from falling off the sample. It should be noted that if it is determined based on the collected position information that the depth at which the inclusions are buried is within 0.1 mm from the sample surface, the depth adjustment process can be omitted.

[0036] After the depth adjustment process, the above-mentioned continuous sputtering and simultaneous elemental analysis are performed to determine the state of cross-section appearance of the inclusions. At this time, the quantitative fluctuation of the elements collected from the processed surface each time can be understood from the transition of the detection intensity of the elements with the passage of sputtering time.

[0037] If the type of inclusion is known in advance, it is sufficient to monitor the elements contained therein. Even if the type is unknown, monitoring can be performed by focusing on the main elements contained in the inclusion assumed to be the target (sulfur for sulfides, calcium and aluminum for oxides, elements contained in the deoxidation products during the steelmaking process). When inclusions of a certain size are present, for example, when a 2 mm electrode is used, 15 μm 2 If there is an inclusion with a cross-sectional area of ​​about this size or more, the timing of the "inclusion appearance" can be determined.

[0038] In this way, by collecting information on the sputtered elements that are simultaneously processed by sputtering, it is possible to grasp the timing at which the inclusion to be observed appears on the surface of the processed surface. This solves the problems that can occur when grinding manually. Specifically, it reduces the risk of overlooking the target inclusion due to overcutting. In addition, it is no longer necessary to repeat the time-consuming process of grinding, finish polishing, and observation until the inclusion is found, significantly reducing the workload. In addition, by stopping sputtering near the maximum detected intensity of an element while observing the transition of the detected intensity, it becomes possible to observe the cross section near where the size of the inclusion is maximum. One method for determining whether the detected intensity of an element is near the maximum is to observe the timing when the increase in the detected intensity slows down and becomes constant. When using the above-mentioned device, the sputtering rate can be set to a constant value. Therefore, if the size and shape of the inclusion are known beforehand, for example, as in the case of an artificial inclusion, or if the shape of the inclusion can be roughly grasped by non-destructive testing such as CT based on transmission observation, it is possible to control and observe the appearance state of the inclusion based on that information and the transition of detection intensity focusing on the elements contained therein.

[0039] (Regarding the first smoothing process) The first smoothing step is carried out on the machined surface from which the inclusions have been revealed by the inclusion revealing step, and involves sputtering (glow discharge plasma sputtering) by glow discharge using a mixed gas of Ar gas and O2 gas. This utilizes the effect of mixing O2 to significantly slow down the rapid sputtering rate of Ar plasma, and at the cost of a slower sputtering rate, the surface is smoothed. In other words, extra energy is consumed to turn the impurity O2 into plasma, which slows down the sputtering rate, but at the cost of a smoother surface. In this process, the sputtering rate is significantly reduced, so the state of the inclusions adjusted in the previous inclusion revealing process does not change significantly. Using this technique, minute irregularities on the surface sputtered with Ar alone can be smoothed out, allowing for more detailed observation of the inclusions and their surroundings.

[0040] When the mixed gas is taken as 100 mass %, the concentration of Ar is preferably 94 mass % or more and 98 mass % or less, and the concentration of O2 is preferably 2 mass % or more and 6 mass % or less. The time for sputtering using the mixed gas may be appropriately determined while monitoring the finish state of the sputtered surface. Other conditions may be the same as those in the above-mentioned inclusion revealing process.

[0041] (Regarding the second smoothing process) After the first smoothing step, the processed surface may be subjected to a finishing process using Ar ion milling, which is a process in which the processed surface is irradiated with a low-acceleration Ar ion beam to further smooth the processed surface. When deposits accumulate in the gaps around inclusions during sputtering with a mixed gas of Ar and O2, this can be improved by performing a finishing process using Ar ion milling.

[0042] (About the corrosion process) After the first smoothing step, the sputtered surface may be subjected to an etching treatment. For the etching treatment, etching may be used. For the etching, nital (a nitric acid alcohol solution) or the like may be used. By performing the etching treatment, the relationship between the inclusions and the microstructure around them becomes easier to observe. The etching step may be performed after the second smoothing step.

[0043] As described above, this embodiment makes it possible to precisely observe the state (shape, distribution, gap state) of inclusions in steel material and their relationship with the surrounding microstructure (e.g., relationship with fatigue behavior). Although the embodiment of the present invention has been described above, this embodiment has been described as an example and is not intended to limit the scope of the invention. This new embodiment can be implemented with various other modifications and improvements, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. This embodiment and its modifications are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims.

[0044] (Example) The present invention will be specifically described below with reference to examples. SUJ2 that had been quenched and tempered was used as a sample for observation. Sputtering (inclusion revealing process) was performed on any surface of the sample. A high-frequency glow discharge optical emission surface analyzer having both a sputtering function and a simultaneous elemental analysis function was used to perform the sputtering. From the viewpoint of practicality, a relatively wide range can be covered, and further, from the viewpoint of achieving both a high sputtering rate and high element detection sensitivity, an electrode with a diameter of 2 mm was used. Furthermore, if the shape of the sputtering marks is not smooth but is convex or concave, it becomes difficult to observe the exposed inclusions two-dimensionally, and three-dimensional observation may become necessary. When three-dimensional observation becomes necessary, the time required for observation increases, so from this perspective, sputtering conditions were selected that would make the sputter bottom as smooth as possible. Specifically, the Ar gas pressure was set to 600 Pa and the high-frequency applied voltage was set to 35 W. The purity of the Ar gas was 99.9999%. As a result of carrying out the inclusion revealing process under these conditions, rapid (depth direction processing speed 5 μm / min) and smooth (height difference within 5 μm) local polishing was achieved.

[0045] Figure 1 is a SEM (Scanning Electron Microscope) image of the processed surface immediately after the inclusion revealing process. As shown in the figure, sulfides (inclusions) were observed on the processed surface. At this stage, minute irregularities were formed in the parent phase due to the effect of Ar sputtering, so a first smoothing process must be carried out in order to make a detailed observation.

[0046] In the first smoothing step, smoothing was performed using the high-frequency glow discharge optical emission surface analyzer used in the inclusion revealing step. Sputtering (glow discharge plasma sputtering) was performed by glow discharge using a mixed gas consisting of 95 mass% Ar and 5 mass% O2 (purity of each gas was 99.9999%). The sputtering time was set to 20 minutes. Figure 2 is an SEM image of the inclusion and its surroundings on the processed surface immediately after the first smoothing step. It can be seen from the figure that the minute irregularities in the parent phase had been improved to a state where they were almost unnoticeable.

[0047] After the first smoothing process, the machined surface was subjected to an etching treatment. 5% nital was used for the etching treatment. Figure 3 is an SEM image showing the sulfides (inclusions) and the surrounding microstructure after the etching treatment in the same field of view. Since the sample to be observed was quenched and tempered SUJ2, spherical carbides of about several μm were dispersed in the martensite structure of the parent phase, and this state could be clearly observed. In this way, by observing the microstructure around the inclusions, it is possible to confirm the fatigue behavior around the inclusions after rolling fatigue is applied, for example, and to verify the harmfulness of the inclusions.

Claims

1. A method for preparing a sample of a steel material or a steel part to be subjected to observation of inclusions, comprising the steps of: an inclusion revealing step of making the inclusions inside the sample appear on the processed surface by generating plasma from Ar gas by glow discharge and sputtering the processed surface of the sample; After the inclusion revealing step is performed, Ar and O 2 a first smoothing step of smoothing the processed surface by converting the mixed gas of the above-mentioned step 1 into plasma by glow discharge and further sputtering the processed surface; A method for preparing a sample, comprising:

2. 2. The method for preparing a specimen according to claim 1, further comprising the step of: performing a second smoothing step by Ar ion milling on the processed surface after the first smoothing step.

3. 2. The method for preparing a specimen according to claim 1, further comprising the step of: subjecting the processed surface to an etching treatment after the first smoothing step, thereby revealing the microstructure around the inclusions.

4. 3. The method for preparing a specimen according to claim 2, further comprising the step of: subjecting the processed surface to an etching treatment after the second smoothing step, thereby revealing the microstructure around the inclusions.

5. 5. A method for producing a specimen according to claim 1, wherein the inclusions contained in the specimen subjected to the inclusion revealing step are inclusions to which fatigue has been imparted in advance by repeated loading.

6. A sample preparation method according to any one of claims 1 to 4, characterized in that a depth adjustment process is performed before carrying out the inclusion revealing process, in which the depth from the sample surface to the position where the inclusion is present is adjusted to within 0.1 mm.

7. 5. The method for preparing a specimen according to claim 1, wherein the presence or absence of inclusions is determined by carrying out the inclusion revealing step while analyzing the elements of the sputtered particles.

8. 6. The method for preparing a specimen according to claim 5, wherein the presence or absence of inclusions is determined by carrying out the inclusion revealing step while analyzing the elements of the sputtered particles.

9. 7. The method for preparing a specimen according to claim 6, wherein the presence or absence of inclusions is determined by carrying out the inclusion revealing step while analyzing the elements of the sputtered particles.

10. 8. The method for preparing a specimen according to claim 7, wherein the presence or absence of inclusions is determined by carrying out the inclusion revealing step while analyzing the elements of the sputtered particles.