Radiation-sensitive composition, cured film and method for producing the same, semiconductor device and display device
A radiation-sensitive composition with tailored structural units and a photoacid generator forms cured films with low dielectric constant and transparency, addressing the limitations of existing compositions in semiconductor and display elements.
Patent Information
- Application Number
- JP2023070383
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-04-21
AI Technical Summary
Existing radiation-sensitive compositions for forming cured films in semiconductor and display elements have high dielectric constants and insufficient transparency, limiting their performance in applications requiring low dielectric materials.
A radiation-sensitive composition containing specific structural units represented by formulas (1) and (2) in a polymer component, along with a photoacid generator, which allows for the formation of a cured film with low dielectric constant and excellent transparency through controlled solubility and crosslinking reactions.
The composition achieves a cured film with a dielectric constant of 3.3 or less and high transparency, enhancing the performance of semiconductor and display elements by improving radiation sensitivity and chemical resistance.
Smart Images

Figure 2024155568000001 
Figure 2024155568000002 
Figure 2024155568000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a radiation-sensitive composition, a cured film and a method for producing the same, a semiconductor device, and a display device. [Background technology]
[0002] Cured films (e.g., interlayer insulating films, spacers, protective films, etc.) of semiconductor elements and display elements are generally formed using a radiation-sensitive composition containing a polymer component and a radiation-sensitive compound (a photoacid generator, a photopolymerization initiator, etc.). For example, a coating film formed from the radiation-sensitive composition is irradiated with radiation, and then developed to form a pattern, and then the resulting film is heat-cured by heating to obtain a cured film having a pattern shape.
[0003] Various radiation-sensitive compositions have been proposed as materials for forming cured films provided on semiconductor elements and display elements (see, for example, Patent Documents 1 to 3). Patent Document 1 discloses a radiation-sensitive resin composition used for forming a cured film, which contains a polymer including a structural unit having a partial structure in which a trialkoxysilyl group is bonded to an alkyl chain, a benzene ring, or a naphthalene ring, an epoxy compound, and a radiation-sensitive compound. Patent Document 1 also describes that the radiation-sensitive composition of Patent Document 1 can provide a cured film having excellent heat resistance, chemical resistance, surface hardness, development adhesion, transparency, and low dielectric properties, and also has satisfactory properties such as storage stability and sensitivity.
[0004] Patent Document 2 discloses a radiation-sensitive composition containing a polymer component having a structural unit derived from maleimide and a structural unit containing an alkoxysilyl group in the same or different polymers, and a radiation-sensitive compound. Patent Document 2 describes that the radiation-sensitive composition of Patent Document 2 has high radiation sensitivity, and that by using the composition, a cured film having high chemical resistance and low corrosiveness to metal wiring can be obtained.
[0005] Patent Document 3 discloses a radiation-sensitive composition containing a polymer component containing, in the same or different polymers, a structural unit having a partial structure in which a trialkylsilyloxy group is bonded to an aromatic ring and a structural unit having a crosslinkable group, and a radiation-sensitive acid generator. Patent Document 3 also describes that the radiation-sensitive composition of Patent Document 3 has good radiation sensitivity, storage stability, outgassing properties, and coatability due to the inclusion of the above structural unit in the polymer component. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2017-107024 A [Patent Document 2] JP 2019-174614 A [Patent Document 3] Patent Publication No. 2021-196577 Summary of the Invention [Problem to be solved by the invention]
[0007] According to the radiation-sensitive composition of Patent Document 3, it is possible to obtain a cured film with reduced outgassing while improving radiation sensitivity. However, the cured film obtained from the radiation-sensitive composition of Patent Document 3 has a relatively high dielectric constant, and there is room for further improvement. In addition, in applications requiring transparency, the film obtained from the radiation-sensitive composition is required to have high transmittance.
[0008] The present invention has been made in consideration of the above problems, and has as its main object to provide a radiation-sensitive composition that has excellent radiation sensitivity, and is capable of forming a cured film that has a low dielectric constant and excellent transparency. [Means for solving the problem]
[0009] According to the present invention, there are provided the following radiation-sensitive composition, cured film and method for producing the same, semiconductor device, and display device.
[0010] [1] A radiation-sensitive composition comprising: [A] a polymer component including, in the same molecule or in different molecules, a first structural unit having a partial structure represented by the following formula (1) and a second structural unit having a partial structure represented by the following formula (2), and [B] a photoacid generator, wherein the first structural unit is contained in an amount of 5 to 50 mass % and the second structural unit is contained in an amount of 0.1 to 20 mass % based on the total structural units of the polymer component: [ka] (In formula (1), Ar 1 is a divalent aromatic ring group. 1 is an acid dissociable group. n is 0 or 1. "*" represents a bond. However, when n is 0, the first structural unit is a structural unit derived from a monomer having a maleimide ring, and Y 1 is bonded to the nitrogen atom of the maleimide ring. [ka] (In formula (2), R 1 , R 2 and R 3 are each independently a hydrogen atom, a halogen atom, a hydroxyl group, an alkoxy group having 1 to 6 carbon atoms, an alkyl group having 1 to 10 carbon atoms, or a phenyl group. 1 , R 2 and R 3 At least one of the groups is an alkoxy group having 1 to 6 carbon atoms. "*" represents a bond bonded to a carbon atom.)
[0011] [2] A cured film formed using the radiation-sensitive composition described in [1] above. [3] A method for producing a cured film, comprising the steps of: forming a coating film using the radiation-sensitive composition described in [1] above; exposing at least a portion of the coating film to light; developing the exposed coating film; and heating the developed coating film. [4] A semiconductor element comprising the cured film described in [2] above. [5] A display element comprising the cured film described in [2] above. Effect of the Invention
[0012] The radiation-sensitive composition of the present invention has excellent radiation sensitivity, and can form a cured film having a low dielectric constant and excellent transparency. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Matters related to the embodiments will be described in detail below. In this specification, a numerical range described using "~" means that the numerical range includes the numerical values before and after "~" as the lower and upper limits. A "structural unit" refers to a unit that mainly constitutes the main chain structure, and at least two or more units are contained in the main chain structure.
[0014] In this specification, the term "hydrocarbon group" includes chain-shaped hydrocarbon groups, alicyclic hydrocarbon groups, and aromatic hydrocarbon groups. The term "chain-shaped hydrocarbon group" means a straight-chain hydrocarbon group and a branched hydrocarbon group that do not include a cyclic structure in the main chain and are composed only of a chain structure. However, the chain-shaped hydrocarbon group may be saturated or unsaturated. The term "alicyclic hydrocarbon group" means a hydrocarbon group that includes only an alicyclic hydrocarbon structure as a ring structure and does not include an aromatic ring structure. However, the alicyclic hydrocarbon group does not need to be composed only of an alicyclic hydrocarbon structure, and also includes those that have a chain structure as a part of it. The term "aromatic hydrocarbon group" means a hydrocarbon group that includes an aromatic ring structure as a ring structure. However, the aromatic hydrocarbon group does not need to be composed only of an aromatic ring structure, and may include a chain structure or an alicyclic hydrocarbon structure as a part of it. The ring structure of the alicyclic hydrocarbon group and the aromatic hydrocarbon group may have a substituent composed of a hydrocarbon structure. The term "cyclic hydrocarbon group" means a hydrocarbon group that includes an alicyclic hydrocarbon group and an aromatic hydrocarbon group. The term "aromatic ring group" refers to a group in which r hydrogen atoms (r is an integer) have been removed from the ring portion of an aromatic ring. The term "aromatic ring" includes aromatic hydrocarbon rings and aromatic heterocycles. The term "(meth)acrylic" includes "acrylic" and "methacrylic".
[0015] 《Radiation sensitive composition》 The radiation-sensitive composition of the present disclosure (hereinafter also referred to as "the composition") contains a polymer component [A] and a photoacid generator [B]. Each component contained in the composition and other components that are blended as necessary will be described below. Note that, unless otherwise specified, each component may be used alone or in combination of two or more.
[0016] <[A] Polymer component> The polymer component [A] contains a first structural unit having a partial structure represented by the following formula (1) and a second structural unit having a partial structure represented by the following formula (2) in the same molecule or in different molecules. The polymer component [A] contains 5 to 50 mass% of the first structural unit and 0.1 to 20 mass% of the second structural unit, based on the total structural units of the polymer component [A]. [ka] (In formula (1), Ar 1 is a divalent aromatic ring group. 1 is an acid dissociable group. n is 0 or 1. "*" represents a bond. However, when n is 0, the first structural unit is a structural unit derived from a monomer having a maleimide ring, and Y 1 is bonded to the nitrogen atom of the maleimide ring. [ka] (In formula (2), R 1 , R 2 and R 3 are each independently a hydrogen atom, a halogen atom, a hydroxyl group, an alkoxy group having 1 to 6 carbon atoms, an alkyl group having 1 to 10 carbon atoms, or a phenyl group. 1 , R 2 and R 3 At least one of the groups is an alkoxy group having 1 to 6 carbon atoms. "*" represents a bond bonded to a carbon atom.)
[0017] (First structural unit) The first structural unit has a partial structure represented by the above formula (1). When the composition is irradiated with radiation, the acid generated from the photoacid generator [B] acts to convert the acid-dissociable group (Y 1 ) is eliminated. As a result, when n in the above formula (1) is 1, a hydroxyl group bonded to the aromatic ring is generated, and when n is 0, -NH- is generated. As a result, the solubility of the polymer component [A] in the developer (more specifically, alkali solubility) can be changed, and a cured film on which a pattern is formed can be obtained. In addition, the generation of a hydroxyl group or -NH- bonded to the aromatic ring can increase the curing reactivity of the polymer component [A]. In order to increase the curing reactivity of the polymer component [A], it is preferable that n in the above formula (1) is 1. In this specification, "alkali soluble" means that it is soluble or swellable in an alkaline aqueous solution such as a 2.38 mass% aqueous solution of tetramethylammonium hydroxide (TMAH).
[0018] In the above formula (1), Ar 1 The divalent aromatic ring group represented by the formula (I) is a group in which two hydrogen atoms have been removed from the ring portion of a substituted or unsubstituted aromatic ring. Examples of the aromatic ring include a benzene ring, a naphthalene ring, and an anthracene ring. 1 In the case where the aromatic ring of Ar has a substituent, examples of the substituent include a halogen atom, an alkyl group, and an alkoxy group. 1 Of these, a substituted or unsubstituted phenylene group, naphthylene group or anthrylene group is preferable, and a substituted or unsubstituted phenylene group or naphthylene group is more preferable.
[0019] Y 1 The acid dissociable group represented by the formula (I) is not particularly limited. In this specification, the term "acid dissociable group" refers to a group that substitutes a polar hydrogen atom of an acid group (e.g., a hydroxyl group, a carboxyl group, an amino group, a sulfo group, etc.) and dissociates under the action of an acid. From the viewpoint of enhancing the effect of improving the sensitivity, storage stability, and pattern shape of the present composition, Y 1The acid-dissociable group represented by the following formula (Y-1), formula (Y-2) or formula (Y-3) is preferable. [ka] (In formula (Y-1), R 4 , R 5 and R 6 are each independently a hydrogen atom, a halogen atom, a hydroxyl group, a monovalent hydrocarbon group having 1 to 20 carbon atoms, or a group in which some or all of the hydrogen atoms in the hydrocarbon group have been substituted with a substituent. "*" represents a bond.) [ka] (In formula (Y-2), R 7 , R 8 and R 9 satisfies the following (1) or (2). 7 R is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms. 8 and R 9 are each independently an alkyl group having 1 to 12 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms. (2) R 7 R is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms. 8 and R 9 are combined with each other. 8 and OR 9 represents a cyclic ether structure formed together with the carbon atom to which it is bonded. "*" represents a bond.) [ka] (In formula (Y-3), R 10 is a tertiary alkyl group. "*" represents a bond.)
[0020] In the above formula (Y-1), R 4 , R 5 or R 6Examples of the monovalent hydrocarbon group represented by the formula (1) include a monovalent chain hydrocarbon group having 1 to 20 carbon atoms, a monovalent alicyclic hydrocarbon group having 4 to 20 carbon atoms, and a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms. Specific examples of these include, as the chain hydrocarbon group having 1 to 20 carbon atoms, alkyl groups such as a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, a tert-butyl group, and an n-pentyl group; and alkenyl groups such as a vinyl group and an allyl group.
[0021] Examples of the alicyclic hydrocarbon group having 4 to 20 carbon atoms include monocyclic alicyclic hydrocarbon groups such as a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a methylcyclohexyl group, and a cyclooctyl group; a bicyclo[2.2.2]octyl group, a tricyclo[5.2.1.0]octyl group, and the like. 2,6 ] decyl group, adamantyl group, norbornyl group and other polycyclic alicyclic hydrocarbon groups.
[0022] Examples of the aromatic hydrocarbon group having 6 to 20 carbon atoms include aryl groups such as a phenyl group, a tolyl group, a xylyl group, and a naphthyl group; and aralkyl groups such as a benzyl group and a phenethyl group. R 4 , R 5 or R 6 When the group represented by the formula (I) is a group in which some or all of the hydrogen atoms of a hydrocarbon group having 1 to 20 carbon atoms have been substituted with a substituent, examples of the substituent include a halogen atom (a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc.) and a hydroxy group.
[0023] R 4 , R 5 or R 6 From the viewpoint of improving the radiation sensitivity and coatability of the composition, and of obtaining a cured film with little outgassing, the group represented by the following formula (1) is preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 5 carbon atoms, and even more preferably an alkyl group having 1 to 3 carbon atoms, among the above groups.
[0024] In the above formula (Y-2), R 7 , R 8 and R9 The alkyl group having 1 to 12 carbon atoms represented by the formula (I) may be linear or branched. The number of carbon atoms in the alkyl group is preferably 1 to 6, and more preferably 1 to 4. 7 , R 8 and R 9 Specific examples of the alkyl group having 1 to 12 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group.
[0025] R 7 , R 8 and R 9 Examples of the monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms represented by the formula (I) include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a norbornyl group, an isobornyl group, and an adamantyl group. 8 and R 9 Examples of the aralkyl group having 7 to 20 carbon atoms represented by the following formula include a benzyl group, a phenethyl group, and a methylbenzyl group.
[0026] R 8 and R 9 The cyclic ether structure formed by combining these rings preferably has a ring member number of 5 or more. Specific examples thereof include a tetrahydrofuran ring structure and a tetrahydropyran ring structure.
[0027] R is easily dissociated by acid. 7 Of these, a hydrogen atom, a methyl group, or an ethyl group is preferable, and a hydrogen atom is more preferable. In the above formula (Y-3), R 10 The tertiary alkyl group represented by the following formula (I) is preferably a tert-butyl group in terms of good releasability.
[0028] Y in the above formula (1) 1 is a group represented by the above formula (Y-1), the group represented by the above formula (1) is preferably represented by the following formula (Y1-1) or formula (Y1-2). [ka] (In formula (Y1-1) and formula (Y1-2), A 1 and A 2 are each independently a halogen atom, a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. n1 is an integer of 0 to 4. n2 is an integer of 0 to 6. However, when n1 is 2 or more, multiple A 1 are the same or different groups. When n2 is 2 or more, a plurality of A 2 are the same or different groups. 4 , R 5 and R 6 has the same meaning as in formula (Y-1). "*" represents a bond.
[0029] In the above formula (Y1-1) or (Y1-2), A 1 Or A 2 Specific examples of the alkyl group having 1 to 6 carbon atoms and the alkoxy group having 1 to 6 carbon atoms represented by the formula (Y-1) are 4 ~R 6 Examples of the alkyl group and alkoxy group include those exemplified above.
[0030] The group "-O-SiR 4 R 5 R 6 " is located at A 1 and A 2 For example, in the case of the above formula (Y1-1), "-O-SiR 4 R 5 R 6 The position of " may be any of ortho, meta, or para, and is preferably the para position. n1 is preferably 0 or 1, and more preferably 0. n2 is preferably 0 to 2, and more preferably 0. When the first structural unit has a group represented by formula (Y-1), it is particularly preferable that the first structural unit is a structural unit having a group represented by formula (Y1-1).
[0031] Y in the above formula (1) 1When is a group represented by the above formula (Y-1), the first structural unit is preferably a structural unit derived from a monomer having a polymerizable carbon-carbon unsaturated bond (hereinafter also referred to as "unsaturated monomer"). Specifically, the first structural unit is preferably at least one selected from the group consisting of a structural unit represented by the following formula (1-1A) and a structural unit represented by the following formula (1-2A), and more preferably a structural unit represented by the following formula (1-1A). [ka] (In formula (1-1A) and formula (1-2A), R A R is a hydrogen atom, a methyl group, a hydroxymethyl group, a cyano group, or a trifluoromethyl group. 4 , R 5 and R 6 has the same meaning as in formula (Y-1). 1 , A 2 , n1 and n2 have the same meanings as in formula (Y1-1) and formula (Y1-2) above.)
[0032] Y in the above formula (1) 1 is a group represented by the above formula (Y-1), specific examples of the monomer that provides the first structural unit include, when n in the above formula (1) is 1, 4-isopropenylphenyloxytrimethylsilane, 4-isopropenylphenyloxytriethylsilane, 4-isopropenylphenyloxymethyldiethylsilane, 4-isopropenylphenyloxydimethylethylsilane, 3-isopropenylphenyloxytrimethylsilane, 4-isopropenylnaphthyloxytrimethylsilane, 4-vinylphenyloxytrimethylsilane, 4-vinylphenyloxytriethylsilane, 4-vinylphenyloxymethyldiethylsilane, 4-vinylphenyloxydimethylethylsilane, 3-vinylphenyloxytrimethylsilane, 4-vinylnaphthyloxytrimethylsilane, 4-trimethylsilyloxy-N-phenylmaleimide, 4-trimethylsilyloxyphenyl(meth)acrylate, and the like. Examples of the compound in which n is 0 in the above formula (1) include N-trimethylsilylmaleimide, N-triethylsilylmaleimide, and N-methyldiethylsilylmaleimide.
[0033] Y in the above formula (1) 1 is a group represented by the above formula (Y-2) or formula (Y-3), the first structural unit is preferably a structural unit derived from an unsaturated monomer. Specifically, the first structural unit is preferably at least one selected from the group consisting of a structural unit represented by the following formula (1-1B) and a structural unit represented by the following formula (1-2B). [ka] (In formula (1-1B) and formula (1-2B), R B R is a hydrogen atom, a methyl group, a hydroxymethyl group, a cyano group, or a trifluoromethyl group. 7 , R 8 and R 9 has the same meaning as in formula (Y-2). 10 has the same meaning as in formula (Y-3). 3 is a halogen atom, a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. n3 is an integer of 0 to 4.
[0034] Y in the above formula (1) 1 When Y is a group represented by the above formula (Y-2), specific examples of the monomer that gives the first structural unit include structural units represented by the following formulas (1-2-1) to (1-2-3). 1 When is a group represented by the above formula (Y-3), a specific example of a monomer that provides the first structural unit is a structural unit represented by the following formula (1-3-1). [ka] (In formulas (1-2-1) to (1-2-3) and (1-3-1), R B is a hydrogen atom, a methyl group, a hydroxymethyl group, a cyano group, or a trifluoromethyl group.
[0035] From the viewpoint of radiation sensitivity and transmittance, the first structural unit is, among the above, Y in the above formula (1). 1 is preferably a group represented by the above formula (Y-1).
[0036] The content of the first structural unit in the polymer component [A] is 5 to 50% by mass based on the total structural units constituting the polymer component [A]. If the content of the first structural unit is less than 5% by mass, the radiation sensitivity of the composition is low, and the resolution is poor. If the content of the first structural unit is more than 50% by mass, the transmittance of the film obtained using the composition is low, and outgassing is likely to occur from the cured film. From the above viewpoints, the content of the first structural unit in the polymer component [A] is preferably 10% by mass or more, more preferably 15% by mass or more. From the viewpoint of achieving both the transmittance and resolution of the film, the content of the first structural unit is preferably 45% by mass or less, more preferably 40% by mass or less, based on the total structural units constituting the polymer component [A].
[0037] (Second structural unit) The second structural unit is a structural unit having a partial structure represented by the above formula (2). The second structural unit differs from the first structural unit in that the second structural unit does not have the partial structure represented by the above formula (1).
[0038] In the above formula (2), R 1 , R 2 or R 3 Examples of the alkoxy group having 1 to 6 carbon atoms represented by the formula (I) include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, and a tert-butoxy group. 1 , R 2 or R 3 The alkoxy group represented by the formula (2) preferably has 1 to 5 carbon atoms, more preferably has 1 to 3 carbon atoms, and is further preferably a methoxy group or an ethoxy group. In particular, when the group represented by the formula (2) is bonded to an aromatic ring group, R 1 , R 2 and R 3At least one of R is preferably a methoxy group. When the group represented by the formula (2) is bonded to a chain hydrocarbon group, R 1 , R 2 and R 3 At least one of these is preferably an ethoxy group.
[0039] R 1 , R 2 or R 3 The alkyl group having 1 to 10 carbon atoms represented by the formula (I) may be linear or branched. 1 , R 2 or R 3 Examples of the alkyl group represented by R include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group. 1 , R 2 or R 3 The alkyl group represented by the formula (I) is preferably a methyl group, an ethyl group or a propyl group.
[0040] R 1 , R 2 or R 3 At least one of the groups represented by the formula (I) is an alkoxy group having 1 to 6 carbon atoms. 1 , R 2 or R 3 When is a group other than an alkoxy group having 1 to 6 carbon atoms, examples of the group include a hydroxy group, an alkoxy group having 1 to 6 carbon atoms, an alkyl group having 1 to 10 carbon atoms, and a phenyl group.
[0041] From the viewpoint of obtaining a cured film with excellent heat resistance by forming a crosslinked structure, R 1 , R 2 and R 3 It is preferable that two or more of R are alkoxy groups having 1 to 6 carbon atoms. 1 , R 2 and R 3 It is more preferable that all of the groups are alkoxy groups having 1 to 6 carbon atoms.
[0042] In the second structural unit, the group represented by the formula (2) may be bonded to a carbon atom. From the viewpoint of improving the transparency and outgassing properties of the film, the group represented by the formula (2) is preferably bonded to an aromatic ring group or a chain hydrocarbon group, or to a carbon atom constituting the main chain of the polymer. When the group represented by the formula (2) is bonded to an aromatic ring group, examples of the aromatic ring to which the group represented by the formula (2) is bonded include a benzene ring, a naphthalene ring, and an anthracene ring. These rings may have a substituent such as an alkyl group. When the group represented by the formula (2) is bonded to a chain hydrocarbon group, examples of the chain hydrocarbon group include an alkanediyl group and an alkenediyl group.
[0043] When the group represented by the above formula (2) is bonded to an aromatic ring group or a chain hydrocarbon group, the group represented by the above formula (2) is preferably bonded to a benzene ring, a naphthalene ring, or an alkyl chain among the above. Specifically, when the group represented by the above formula (2) is bonded to an aromatic ring group or a chain hydrocarbon group, the second structural unit preferably has at least one selected from the group consisting of a group represented by the following formula (2-1), a group represented by the following formula (2-2), and a group represented by the following formula (2-3). [ka] (In formula (2-1), formula (2-2) and formula (2-3), A 4 and A 5 are each independently a halogen atom, a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. m1 is an integer of 0 to 4. m2 is an integer of 0 to 6. However, when m1 is 2 or more, multiple A 4 are the same or different. When m2 is 2 or more, multiple A 5 are the same or different. R 11 is an alkanediyl group. 1 , R 2 and R 3 is defined as the above formula (2). "*" represents a bond.
[0044] In the above formula (2-1) or (2-2), A 4 Or A 5 Examples of the alkoxy group having 1 to 6 carbon atoms and the alkyl group having 1 to 6 carbon atoms represented by the formula (2) are 1 ~R 3 The same groups as those exemplified as the groups for the aromatic ring "-SiR 1 R 2 R 3 The bonding position of " is A 4 and A 5 For example, in the case of the above formula (2-1), "-SiR 1 R 2 R 3 The position of " may be any of the ortho, meta, and para positions relative to the position of the bond represented by "*". The para position is preferred. m1 is preferably 0 or 1, and more preferably 0. m2 is preferably 0 to 2, and more preferably 0. In the above formula (2-3), R 11 From the viewpoint of increasing the heat resistance of the resulting cured film, R 11 Preferably, the group has 1 to 6 carbon atoms, and more preferably has 1 to 4 carbon atoms.
[0045] In terms of increasing the heat resistance, chemical resistance and hardness of the cured film, it is preferable that the second structural unit has at least one selected from the group consisting of the group represented by the above formula (2-1) and the group represented by the above formula (2-2) among the above formulas (2-1) to (2-3). 1 R 2 R 3 When " is directly bonded, it is possible to stabilize the silanol groups generated in the presence of water. This is preferable in that the solubility of the exposed area in an alkaline developer can be increased, and a good pattern can be formed. Among these, it is particularly preferable that the second structural unit is a structural unit having a group represented by the above formula (2-1).
[0046] The second structural unit is preferably a structural unit derived from a monomer having a polymerizable carbon-carbon unsaturated bond as a bond involved in polymerization (hereinafter, also referred to as "unsaturated monomer"). Specifically, the second structural unit is preferably at least one selected from the group consisting of a structural unit represented by the following formula (2A-1) and a structural unit represented by the following formula (2A-2). [ka] (In formula (2A-1) and formula (2A-2), R C R is a hydrogen atom, a methyl group, a hydroxymethyl group, a cyano group, or a trifluoromethyl group. 12 R is a divalent aromatic ring group or a chain hydrocarbon group. 13 R is a single bond, a divalent aromatic ring group, or a chain hydrocarbon group. 1 , R 2 and R 3 is defined as the above formula (1).
[0047] In the above formula (2A-1) and formula (2A-2), R 12 or R 13 The divalent aromatic ring group represented by the formula (I) is preferably a substituted or unsubstituted phenylene group, or a substituted or unsubstituted naphthalenediyl group. In the aromatic ring group, examples of the substituent bonded to the ring include one or more selected from the group consisting of a halogen atom, a hydroxyl group, an alkyl group having 1 to 6 carbon atoms, and an alkoxy group having 1 to 6 carbon atoms. The divalent chain hydrocarbon group is preferably an alkanediyl group having 1 to 6 carbon atoms, and more preferably an alkanediyl group having 1 to 4 carbon atoms.
[0048] R is advantageous in that it can produce a cured film with higher heat resistance, chemical resistance and hardness, and can increase the solubility of the exposed area in an alkaline developer. 12 and R 13 Among the above, is preferably a divalent aromatic ring group, and more preferably a substituted or unsubstituted phenylene group.
[0049] Specific examples of the structural unit represented by the formula (2A-1) include structural units represented by the following formulas (2A-1-1) and (2A-1-2), etc. Specific examples of the structural unit represented by the formula (2A-2) include structural units represented by the following formulas (2A-2-1), (2A-2-2) and (2A-2-3), etc. [ka] (In formula (2A-1-1), formula (2A-1-2), formula (2A-2-1), formula (2A-2-2) and formula (2A-2-3), R 21 and R 22 are each independently an alkyl group having 1 to 4 carbon atoms. 23 is an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a hydroxyl group. n3 is an integer of 1 to 4. A 4 , A 5 , m1 and m2 have the same meanings as in formula (2-1) and formula (2-2) above. C has the same meaning as the above formula (2A-1) and formula (2A-2).
[0050] Specific examples of the monomer constituting the second structural unit include compounds having a group represented by the above formula (2-1), such as styryltrimethoxysilane, styryltriethoxysilane, styrylmethyldimethoxysilane, styrylethyldiethoxysilane, styryldimethoxyhydroxysilane, styryldiethoxyhydroxysilane, 4-vinylphenyltrimethoxysilane, (meth)acryloxyphenyltrimethoxysilane, (meth)acryloxyphenyltriethoxysilane, (meth)acryloxyphenylmethoxydimethoxysilane, and (meth)acryloxyphenylethyldiethoxysilane; Examples of the compound having a group represented by the above formula (2-2) include trimethoxy(4-vinylnaphthyl)silane, triethoxy(4-vinylnaphthyl)silane, methyldimethoxy(4-vinylnaphthyl)silane, ethyldiethoxy(4-vinylnaphthyl)silane, (meth)acryloxynaphthyltrimethoxysilane, etc.; Examples of the compound having a group represented by the above formula (2-3) include 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, 4-(meth)acryloxybutyltrimethoxysilane, etc. Specific examples of the monomer constituting the second structural unit include, in addition to the above, vinyltrimethoxysilane, vinyltriethoxysilane, etc.
[0051] In the polymer component [A], the content of the second structural unit is 0.1 to 20% by mass based on the total structural units constituting the polymer component [A]. If the content of the second structural unit is less than 0.1% by mass, the dielectric constant of the cured film obtained using the composition cannot be sufficiently reduced. If the content of the second structural unit is more than 20% by mass, the radiation sensitivity of the composition is poor. From the viewpoint of increasing the dielectric constant of the cured film, the content of the second structural unit in the polymer component [A] is preferably 0.5% by mass or more, more preferably 1% by mass or more. From the viewpoint of achieving both the sensitivity of the composition and the low dielectric constant and high transmittance of the cured film obtained, the content of the second structural unit is preferably 15% by mass or less, more preferably 10% by mass or less, based on the total structural units constituting the polymer component [A].
[0052] (Other structural units) The polymer component [A] may further contain structural units different from the first structural unit and the second structural unit (hereinafter also referred to as "other structural units"). Examples of the other structural units include the third to fifth structural units shown below.
[0053] Third structural unit It is preferred that the polymer component [A] further contains at least one structural unit selected from the group consisting of structural units derived from maleimide and structural units having an acid group (excluding the first structural unit and the second structural unit; this is referred to as the "third structural unit"). By further containing the third structural unit, the solubility of the polymer component [A] in an alkaline developer (alkali solubility) can be increased, and the curing reactivity can be increased.
[0054] When the third structural unit has an acid group, examples of the acid group include a carboxy group, a sulfonic acid group, a phenolic hydroxyl group, and an alcoholic hydroxyl group. Specifically, the third structural unit is preferably at least one selected from the group consisting of a structural unit having a carboxy group, a structural unit having a sulfonic acid group, a structural unit having a phenolic hydroxyl group, and a maleimide unit. In this specification, the term "phenolic hydroxyl group" refers to a hydroxyl group that is directly bonded to an aromatic ring (e.g., a benzene ring, a naphthalene ring, an anthracene ring, etc.).
[0055] The monomer that gives the third structural unit is not particularly limited, but is preferably an unsaturated monomer from the viewpoint of copolymerizability. Specific examples of the monomer that gives the third structural unit include unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, and 4-vinylbenzoic acid as monomers that give structural units having a carboxyl group; unsaturated dicarboxylic acids such as maleic acid, fumaric acid, citraconic acid, mesaconic acid, and itaconic acid as monomers that give structural units having a sulfonic acid group; and 4-hydroxystyrene, o-isopropenylphenol, m-isopropenylphenol, p-isopropenylphenol, and hydroxyphenyl(meth)acrylate as monomers that give structural units having a phenolic hydroxyl group. Maleimide can also be used as the monomer that gives the third structural unit.
[0056] In the polymer component [A], the content of the third structural unit is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more, based on the total structural units constituting the polymer component [A], from the viewpoint of imparting good solubility in an alkaline developer. Also, from the viewpoint of sufficiently generating a difference in solubility in an alkaline developer between an exposed portion and an unexposed portion and obtaining a pattern with a good shape, the content of the third structural unit is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, based on the total structural units constituting the polymer component [A].
[0057] Fourth structural unit It is preferable that the polymer component [A] further contains a structural unit having a crosslinkable group (excluding the first structural unit, the second structural unit, and the third structural unit; this is referred to as a "fourth structural unit.") The polymer component [A] further contains the fourth structural unit, which is preferable in that the resolution and adhesion of the film obtained by using the present composition can be further improved.
[0058] The fourth structural unit may be a structural unit having one or more selected from the group consisting of oxiranyl group and oxetanyl group.In this specification, oxiranyl group and oxetanyl group are also referred to as "epoxy group".When the fourth structural unit has an epoxy group, it is preferable that the epoxy group acts as a crosslinking group, and thus a cured film having high chemical resistance and suppressed deterioration over a long period of time can be formed.
[0059] The fourth structural unit is preferably a structural unit derived from an unsaturated monomer having an epoxy group, and specifically, is preferably at least one selected from the group consisting of a structural unit represented by the following formula (4-1) and a structural unit represented by the following formula (4-2). [ka] (In formula (4-1) and formula (4-2), R 30 R is a monovalent group having an oxiranyl group or an oxetanyl group. Dis a hydrogen atom, a methyl group, a hydroxymethyl group, a cyano group, or a trifluoromethyl group. 1 is a single bond or a divalent linking group.
[0060] In the above formula (4-1) and formula (4-2), R 30 Examples of the aryl groups include oxiranyl, oxetanyl, 3,4-epoxycyclohexyl, and 3,4-epoxytricyclo[5.2.1.0 2,6 ]decyl group, 3-ethyloxetanyl group, and the like.
[0061] X 1 Preferred divalent linking groups include alkanediyl groups such as a methylene group, an ethylene group, and a 1,3-propanediyl group; and divalent groups in which any methylene group of an alkanediyl group is replaced with an oxygen atom.
[0062] Specific examples of the monomer having an epoxy group include glycidyl (meth)acrylate, 3,4-epoxycyclohexyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 2-(3,4-epoxycyclohexyl)ethyl (meth)acrylate, 3,4-epoxytricyclo[5.2.1.0 2,6 ] Decyl (meth) acrylate, 2-hydroxyethyl methacrylate [3,4-epoxytricyclo (5.2.1.0 2,6 ) decan-9-yl], (3-methyloxetan-3-yl)methyl (meth)acrylate, (3-ethyloxetan-3-yl) (meth)acrylate, (oxetan-3-yl)methyl (meth)acrylate, 3-(meth)acryloyloxymethyl-3-ethyloxetane, o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, p-vinylbenzyl glycidyl ether, and the like.
[0063] When the polymer component [A] contains a fourth structural unit, the content of the fourth structural unit in the polymer component [A] is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more, based on the total structural units constituting the polymer component [A]. The content of the fourth structural unit is preferably 55% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less, based on the total structural units constituting the polymer component [A]. By setting the content of the fourth structural unit within the above range, the film obtained by using the composition exhibits better resolution, and the heat resistance and chemical resistance of the obtained cured film can be sufficiently increased, which is preferable.
[0064] 5th structural unit The polymer component [A] may further contain a structural unit having an acid dissociable group (excluding the first structural unit, the second structural unit, the third structural unit and the fourth structural unit; this will be referred to as the "fifth structural unit"). Unlike the first structural unit, the fifth structural unit does not have the partial structure represented by the above formula (1). The acid dissociable group of the fifth structural unit is preferably a group that substitutes a hydrogen atom of a carboxy group, an alcoholic hydroxyl group or a sulfonic acid group, and is a group that dissociates under the action of an acid. Among them, the fifth structural unit is preferably a structural unit from which the acid dissociable group is eliminated under the action of an acid to generate a carboxy group.
[0065] When the fifth structural unit is a structural unit derived from a protected unsaturated carboxylic acid when an acid dissociable group is eliminated by the action of an acid to generate a carboxyl group, the fifth structural unit may be a structural unit derived from a protected unsaturated carboxylic acid. The unsaturated carboxylic acid is not particularly limited, and examples thereof include unsaturated monocarboxylic acid, unsaturated dicarboxylic acid, unsaturated acid anhydride, and unsaturated polycarboxylic acid.
[0066] Specific examples of these include unsaturated monocarboxylic acids such as (meth)acrylic acid, crotonic acid, α-chloroacrylic acid, cinnamic acid, 2-(meth)acryloyloxyethyl-succinic acid, 2-(meth)acryloyloxyethylhexahydrophthalic acid, 2-(meth)acryloyloxyethyl-phthalic acid, (meth)acrylic acid-2-carboxyethyl ester, and 4-vinylbenzoic acid. Examples of unsaturated dicarboxylic acids include maleic acid, fumaric acid, itaconic acid, and citraconic acid. Examples of unsaturated acid anhydrides include maleic anhydride, itaconic anhydride, and citraconic anhydride. Examples of unsaturated polycarboxylic acids include ω-carboxypolycaprolactone mono(meth)acrylate. Examples of acid-dissociable groups include, for example, acetal functional groups, tertiary alkyl groups, tertiary alkyl carbonate groups, and trialkylsilyl groups. Among these, acetal functional groups are preferred because they are easily dissociated by acid.
[0067] When the fifth structural unit has a carboxy group protected by an acetal functional group, the fifth structural unit preferably has an acetal ester structure of a carboxylic acid, and more specifically, preferably has a group represented by the following formula (5-1). [ka] (In formula (5-1), R 41 , R 42 and R 43 satisfies the following (1) or (2). 41 R is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms. 42 and R 43 are each independently an alkyl group having 1 to 12 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms. (2) R 41 R is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms. 42 and R 43 are combined with each other. 42 and OR 43represents a cyclic ether structure formed together with the carbon atom to which it is bonded. "*" represents a bond.)
[0068] R 41 , R 42 or R 43 Specific and preferred examples of the group represented by the formula (Y-2) are 7 , R 8 or R 9 Examples of the group represented by the formula (I) include the same groups as those explained above.
[0069] Specific examples of the acetal ester structure of a carboxylic acid represented by the above formula (5-1) include a 1-methoxyethoxycarbonyl group, a 1-ethoxyethoxycarbonyl group, a 1-propoxyethoxycarbonyl group, a 1-butoxyethoxycarbonyl group, a 1-cyclohexyloxyethoxycarbonyl group, a 2-tetrahydrofuranyloxycarbonyl group, a 2-tetrahydropyranyloxycarbonyl group, and a 1-phenylmethoxyethoxycarbonyl group.
[0070] Specific examples of the fifth structural unit include structural units represented by the following formulas (5-1-1) to (5-1-6). E is a hydrogen atom, a methyl group, a hydroxymethyl group, a cyano group, or a trifluoromethyl group. [ka]
[0071] When the polymer component [A] contains the fifth structural unit, the content of the fifth structural unit in the polymer component [A] is preferably 30 mass % or less, more preferably 25 mass % or less, and even more preferably 20 mass % or less, based on all structural units constituting the polymer component [A].
[0072] Examples of other structural units include structural units derived from at least one monomer selected from the group consisting of (meth)acrylic acid alkyl esters, (meth)acrylic acid esters having an alicyclic structure, (meth)acrylic acid esters having an aromatic ring structure, aromatic vinyl compounds, N-substituted maleimide compounds, vinyl compounds having a heterocyclic structure, conjugated diene compounds, nitrogen-containing vinyl compounds, and unsaturated dicarboxylic acid dialkyl ester compounds. By introducing these structural units into the polymer component [A], the glass transition temperature of the polymer component [A] can be adjusted, and the pattern shape and chemical resistance of the resulting cured film can be improved.
[0073] Specific examples of monomers which provide other structural units that are different from the third to fifth structural units (hereinafter also referred to as "sixth structural unit") include (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-lauryl (meth)acrylate, and n-stearyl (meth)acrylate; Examples of (meth)acrylic acid esters having an alicyclic structure include cyclohexyl (meth)acrylate, 2-methylcyclohexyl (meth)acrylate, tricyclo[5.2.1.0 (meth)acrylate, 2,6 ]decan-8-yl, (meth)acrylic acid tricyclo[5.2.1.0 2,5 ]decan-8-yloxyethyl, isobornyl (meth)acrylate, etc.; Examples of (meth)acrylic acid esters having an aromatic ring structure include phenyl (meth)acrylate and benzyl (meth)acrylate; Aromatic vinyl compounds include styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, α-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 5-t-butyl-2-methylstyrene, divinylbenzene, trivinylbenzene, t-butoxystyrene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethyl ether, N,N-dimethylaminoethylstyrene, N,N-dimethylaminomethylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2-t-butylstyrene, 3-t-butylstyrene, 4-t-butylstyrene, diphenylethylene, vinylnaphthalene, vinylpyridine, etc.; Examples of N-substituted maleimide compounds include N-cyclohexylmaleimide, N-cyclopentylmaleimide, N-(2-methylcyclohexyl)maleimide, N-(4-methylcyclohexyl)maleimide, N-(4-ethylcyclohexyl)maleimide, N-(2,6-dimethylcyclohexyl)maleimide, N-norbornylmaleimide, N-tricyclodecylmaleimide, N-adamantylmaleimide, N-phenylmaleimide, N-(2-methylphenyl)maleimide, N-(4-methylphenyl)maleimide, N-(4-ethylphenyl)maleimide, N-(2,6-dimethylphenyl)maleimide, N-benzylmaleimide, and N-naphthylmaleimide. Examples of vinyl compounds having a heterocyclic structure include tetrahydrofurfuryl (meth)acrylate, tetrahydropyranyl (meth)acrylate, 5-ethyl-1,3-dioxan-5-ylmethyl (meth)acrylate, 5-methyl-1,3-dioxan-5-ylmethyl (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, 2-(meth)acryloxymethyl-1,4,6-trioxaspiro[4,6]undecane, (γ-butyrolactone-2-yl) (meth)acrylate, (meth)acrylic acid glycerin carbonate, (γ-lactam-2-yl) (meth)acrylate, and N-(meth)acryloxyethylhexahydrophthalimide; Conjugated diene compounds include 1,3-butadiene and isoprene; Nitrogen-containing vinyl compounds include (meth)acrylonitrile and (meth)acrylamide; Examples of the unsaturated dicarboxylic acid dialkyl ester compound include diethyl itaconate, etc. Examples of the monomers that provide other structural units include, in addition to the above, monomers such as vinyl chloride, vinylidene chloride, and vinyl acetate.
[0074] When the polymer component [A] further contains a sixth structural unit, the content of the sixth structural unit is preferably 5% by mass or more, more preferably 10% by mass or more, based on all structural units constituting the polymer component [A], from the viewpoint of appropriately increasing the glass transition temperature of the polymer component [A]. The content of the sixth structural unit is preferably 60% by mass or less, more preferably 55% by mass or less, and even more preferably 45% by mass or less, based on all structural units constituting the polymer component [A].
[0075] The polymer component [A] can be produced, for example, by using an unsaturated monomer capable of introducing each of the structural units described above in a suitable solvent in the presence of a polymerization initiator, etc., according to a known method such as radical polymerization. Examples of the polymerization initiator include azo compounds such as 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(isobutyric acid) dimethyl. The proportion of the polymerization initiator used is preferably 0.01 to 30 parts by mass relative to 100 parts by mass of the total amount of the monomers used in the reaction. Examples of the polymerization solvent include alcohols, ethers, ketones, esters, and hydrocarbons. The amount of the polymerization solvent used is preferably such that the total amount of the monomers used in the reaction is 0.1 to 60% by mass relative to the total amount of the reaction solution.
[0076] In the polymerization, the reaction temperature is usually 30°C to 180°C. The reaction time varies depending on the type of polymerization initiator and monomer and the reaction temperature, but is usually 0.5 to 10 hours. The polymer obtained by the polymerization reaction may be used for the preparation of the radiation-sensitive composition as it is dissolved in the reaction solution, or may be used for the preparation of the radiation-sensitive composition after being isolated from the reaction solution. The isolation of the polymer can be performed by a known isolation method such as a method of pouring the reaction solution into a large amount of poor solvent and drying the precipitate obtained under reduced pressure; a method of distilling the reaction solution under reduced pressure with an evaporator; or the like.
[0077] The weight average molecular weight (Mw) of the polymer component [A] in terms of polystyrene measured by gel permeation chromatography (GPC) is preferably 2,000 or more. Mw of 2,000 or more is preferable in that a cured film having sufficiently high heat resistance and chemical resistance and exhibiting good developability can be obtained. The Mw of the polymer component [A] is more preferably 5,000 or more, even more preferably 6,000 or more, and particularly preferably 7,000 or more. In addition, the Mw of the polymer component [A] is preferably 50,000 or less, more preferably 30,000 or less, even more preferably 20,000 or less, and particularly preferably 15,000 or less, from the viewpoint of improving film formability.
[0078] The molecular weight distribution (Mw / Mn) of the polymer component [A], which is expressed as the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) converted into polystyrene by GPC, is preferably 4.0 or less, more preferably 3.0 or less, and even more preferably 2.5 or less. When the polymer component [A] is composed of two or more polymers, it is preferable that the Mw and Mw / Mn of each polymer satisfy the above ranges.
[0079] <[B] Photoacid generator> The photoacid generator [B] is not particularly limited as long as it is a compound that generates an acid upon irradiation with radiation. Examples of the photoacid generator [B] include oxime sulfonate compounds, onium salts, sulfonimide compounds, halogen-containing compounds, diazomethane compounds, sulfone compounds, sulfonic acid ester compounds, and carboxylate compounds.
[0080] Specific examples of the oxime sulfonate compound, onium salt, N-sulfonyloxyimide compound, halogen-containing compound, diazomethane compound, sulfone compound, sulfonate compound, and carboxylate compound include the compounds described in paragraphs 0078 to 0106 of JP 2014-157252 A and the compounds described in WO 2016 / 124493 A. [B] As the photoacid generator, from the viewpoint of radiation sensitivity, it is preferable to use at least one selected from the group consisting of oxime sulfonate compounds and N-sulfonyloxyimide compounds.
[0081] The oxime sulfonate compound is preferably a compound having a sulfonate group represented by the following formula (6). [ka] (In formula (6), R 50 is a monovalent hydrocarbon group or a monovalent group in which some or all of the hydrogen atoms in the hydrocarbon group have been substituted with a substituent. "*" represents a bond.)
[0082] In the above formula (6), R 50 Examples of the monovalent hydrocarbon group represented by the formula (I) include an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 4 to 12 carbon atoms, and an aryl group having 6 to 20 carbon atoms. Examples of the substituent include an alkoxy group having 1 to 5 carbon atoms, an oxo group, and a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom).
[0083] Examples of the oxime sulfonate compound include (5-propylsulfonyloxyimino-5H-thiophen-2-ylidene)-(2-methylphenyl)acetonitrile, (5-octylsulfonyloxyimino-5H-thiophen-2-ylidene)-(2-methylphenyl)acetonitrile, (camphorsulfonyloxyimino-5H-thiophen-2-ylidene)-(2-methylphenyl)acetonitrile, (5-p-toluenesulfonyloxyimino- Examples of the oxime sulfonate compound include 5H-thiophen-2-ylidene)-(2-methylphenyl)acetonitrile, (2-[2-(4-methylphenylsulfonyloxyimino)]-2,3-dihydrothiophen-3-ylidene]-2-(2-methylphenyl)acetonitrile), 2-(octylsulfonyloxyimino)-2-(4-methoxyphenyl)acetonitrile, compounds described in International Publication No. 2016 / 124493, and compounds described in Japanese Patent No. 5914663. Examples of commercially available oxime sulfonate compounds include Irgacure PAG121 manufactured by BASF.
[0084] Examples of N-sulfonyloxyimide compounds include N-(trifluoromethylsulfonyloxy)succinimide, N-(camphorsulfonyloxy)succinimide, N-(4-methylphenylsulfonyloxy)succinimide, N-(2-trifluoromethylphenylsulfonyloxy)succinimide, N-(4-fluorophenylsulfonyloxy)succinimide, N-(trifluoromethylsulfonyloxy)phthalimide, N-(camphorsulfonyloxy)phthalimide, N-(2-trifluoromethylphenylsulfonyloxy)phthalimide, N-(2-fluorophenylsulfonyloxy)phthalimide, N-(trifluoromethylsulfonyloxy)diphenylmaleimide, N-(camphorsulfonyloxy)diphenylmaleimide, 4-methylphenylsulfonyloxy)diphenylmaleimide, and trifluoromethanesulfonic acid-1,8-naphthalimide (N-hydroxynaphthalimide triflate).
[0085] The content of the photoacid generator [B] in the present composition is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more, relative to 100 parts by mass of the polymer component [A]. The content of the photoacid generator [B] is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, and preferably 5 parts by mass or less, relative to 100 parts by mass of the polymer component [A]. When the content of the photoacid generator [B] is 0.01 parts by mass or more, acid is sufficiently generated by irradiation with radiation, and the difference in solubility between the exposed part and the unexposed part in an alkaline solution can be sufficiently increased. This allows good patterning to be performed. In addition, the amount of acid involved in the reaction with the polymer component [A] can be increased, and heat resistance and solvent resistance can be sufficiently ensured. On the other hand, when the content of the photoacid generator [B] is 20 parts by mass or less, the amount of unreacted photoacid generator [B] after exposure can be sufficiently reduced, which is preferable in that the decrease in developability due to the remaining photoacid generator [B] can be suppressed.
[0086] <Other ingredients> The composition may further contain, in addition to the polymer component [A] and the photoacid generator [B], a component different from the polymer component [A] and the photoacid generator [B] (hereinafter, also referred to as "other component"), such as an antioxidant [C], an acid diffusion controller [D], an orthoester compound [E], a crosslinking agent [F], an adhesion aid [G], and a solvent [F].
[0087] ([C] Antioxidants) The antioxidant [C] is a component that suppresses the cleavage of bonds in polymer molecules by capturing radicals generated by exposure or heating, or by decomposition of peroxides generated by oxidation. When the present composition contains the antioxidant [C], the cleavage and deterioration of polymer molecules in the cured film is suppressed, which is preferable in that light resistance and the like can be improved.
[0088] Examples of the antioxidant [C] include a compound having a hindered phenol structure, a compound having a hindered amine structure, a compound having an alkyl phosphite structure, a compound having a thioether structure, etc. Among these, it is preferable to include a compound having a hindered phenol structure as the antioxidant [C], since it has a high effect of improving light resistance.
[0089] Specific examples of compounds having a hindered phenol structure include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tris-(3,5-di-tert-butyl-4-hydroxybenzyl)-isocyanurate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide), 3,3',3',5',5' -Hexa-tert-butyl-a,a',a'-(mesitylene-2,4,6-triyl)tri-p-cresol, 4,6-bis(octylthiomethyl)-o-cresol, 4,6-bis(dodecylthiomethyl)-o-cresol, ethylene bis(oxyethylene) bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate, hexamethylene bis[3-(3,5- di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris[(4-tert-butyl-3-hydroxy-2,6-xylyl)methyl]-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamine)phenol, and the like.
[0090] Commercially available compounds having a hindered phenol structure include, for example, Adeka STAB AO-20, AO-30, AO-40, AO-50, AO-60, AO-60G, AO-70, AO-80, and AO-330 (all manufactured by ADEKA Corporation); sumilizer GM, GS, MDP-S, BBM-S, WX-R, and GA-80 (all manufactured by Sumitomo Chemical Co., Ltd.); and IRGANOX 1010. , 1035, 1076, 1098, 1135, 1330, 1726, 1425WL, 1520L, 245, 259, 3114, 565, IRGAMOD295 (all manufactured by Chiba Japan); Yoshinox BHT, BB, 2246G, 425, 250, 930, SS, TT, 917, 314 (all manufactured by API Corporation).
[0091] When the composition contains an antioxidant [C], the content of the antioxidant [C] in the composition is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and preferably 0.1 parts by mass or more, relative to 100 parts by mass of the polymer component [A]. The content of the antioxidant [C] is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, and preferably 5 parts by mass or less, relative to 100 parts by mass of the polymer component [A].
[0092] ([D] Acid diffusion control agent) The acid diffusion controller [D] is a component that controls the diffusion length of the acid generated from the photoacid generator [B] upon exposure to light. By incorporating the acid diffusion controller [D] in the present composition, the diffusion length of the acid can be appropriately controlled, which is preferable in that the pattern developability can be improved.
[0093] [D] The acid diffusion control agent can be selected from basic compounds used in chemically amplified resists. Examples of basic compounds include fatty acid amines, aromatic amines, heterocyclic amines, quaternary ammonium hydroxides, and quaternary ammonium carboxylates. Specific examples of basic compounds include the compounds described in paragraphs 0128 to 0147 of JP-A-2011-232632. [D] The acid diffusion control agent can be preferably at least one selected from the group consisting of aromatic amines and heterocyclic amines.
[0094] Examples of aromatic amines and heterocyclic amines include aniline derivatives such as aniline, N-methylaniline, N-ethylaniline, N-propylaniline, N,N-dimethylaniline, 2-methylaniline, 3-methylaniline, 4-methylaniline, ethylaniline, propylaniline, trimethylaniline, 2-nitroaniline, 3-nitroaniline, 4-nitroaniline, 2,4-dinitroaniline, 2,6-dinitroaniline, 3,5-dinitroaniline, and N,N-dimethyltoluidine; imidazole derivatives such as imidazole, 4-methylimidazole, 4-methyl-2-phenylimidazole, benzimidazole, 2-phenylbenzimidazole, triphenylimidazole, and N-(tert-butoxycarbonyl)-2-phenylbenzimidazole; pyrrole, 2H-pyrrole, 1-methylpyrrole, and the like. pyrrole derivatives such as pyridine, 2,4-dimethylpyrrole, 2,5-dimethylpyrrole, and N-methylpyrrole; pyridine derivatives such as pyridine, methylpyridine, ethylpyridine, propylpyridine, butylpyridine, 4-(1-butylpentyl)pyridine, dimethylpyridine, trimethylpyridine, triethylpyridine, phenylpyridine, 3-methyl-2-phenylpyridine, 3-methyl-4-phenylpyridine, 4-tert-butylpyridine, diphenylpyridine, benzylpyridine, methoxypyridine, butoxypyridine, dimethoxypyridine, 1-methyl-2-pyridone, 4-pyrrolidinopyridine, 1-methyl-4-phenylpyridine, 2-(1-ethylpropyl)pyridine, aminopyridine, dimethylaminopyridine, and nicotine, as well as the compounds described in JP2011-232632A.
[0095] When the composition contains an acid diffusion controller [D], the content of the acid diffusion controller [D] is preferably 0.001 parts by mass or more, more preferably 0.005 parts by mass or more, and even more preferably 0.01 parts by mass or more, relative to 100 parts by mass of the polymer component [A], from the viewpoint of obtaining a sufficient effect of improving the pattern developability by the acid diffusion controller [D]. The content of the acid diffusion controller [D] is preferably 10 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 2 parts by mass or less, relative to 100 parts by mass of the polymer component [A].
[0096] ([E] Orthoester compounds) [E] Orthoester compounds are classified as -OR 60 " (wherein R 60 is a monovalent hydrocarbon group) bonded to the same carbon atom, and has the general formula: R 61 -C(OR 60 )3, where R 61 is a hydrogen atom or a monovalent organic group. The orthoester compound [E] exhibits water absorption in the presence of acid and is hydrolyzed to convert to an ester. For this reason, by incorporating the orthoester compound [E] in the present composition, the water absorption action of the orthoester compound [E] is exhibited by the acid generated from the photoacid generator [B] (in other words, by irradiation with radiation), and the water absorption action of the orthoester compound [E] can improve the development adhesion of the coating film. In addition, the orthoester compound [E] is preferred in that it is stable and hydrophobic in an alkaline developer and has little effect on unexposed areas (for example, effect on sensitivity).
[0097] "-OR 60 Examples of the group represented by "-OR" include a methoxy group, an ethoxy group, an n-propoxy group, an i-propoxy group, an n-butoxy group, an i-butoxy group, a tert-butoxy group, an n-pentoxy group, a phenoxy group, and a methylphenyl group. 60 The group represented by "-OR" is preferably an alkoxy group, more preferably an alkoxy group having 1 to 4 carbon atoms. 60" may be the same group or different groups.
[0098] R 61 Examples of R include a hydrogen atom, a monovalent chain hydrocarbon group, a monovalent halogenated chain hydrocarbon group, and a monovalent aromatic ring group. 61 is preferably a hydrogen atom, a monovalent chain hydrocarbon group, or a monovalent aromatic ring group, and specific examples thereof include a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, and an aryl group having 6 to 20 carbon atoms.
[0099] Specific examples of the orthoester compound [E] include triethyl orthochloroacetate, trimethyl orthoformate, triethyl orthoformate, tripropyl orthoformate, triisopropyl orthoformate, tributyl orthoformate, diethylphenyl orthoformate, trimethyl orthoacetate, triethyl orthoacetate, triethyl orthodichloroacetate, trimethyl orthobutyrate, triethyl orthobutyrate, trimethyl orthopropionate, triethyl orthopropionate, trimethyl orthovalerate, triethyl orthovalerate, trimethyl orthoisobutyrate, trimethyl orthobenzoate, and triethyl orthobenzoate.
[0100] [E] As the orthoester compound, among the above, a compound having an aromatic ring group can be preferably used in terms of increasing the development adhesion of the coating film.Specific examples of the orthoester compound having an aromatic ring group include trimethyl orthobenzoate, triethyl orthobenzoate, and diethylphenyl orthoformate.Of these, trimethyl orthobenzoate and triethyl orthobenzoate are preferred in terms of improving the development adhesion of the coating film and maintaining the sensitivity better.
[0101] In addition, as the orthoester compound [E], a compound having a boiling point higher than the pre-bake temperature can be preferably used. By using an orthoester compound having a boiling point sufficiently higher than the pre-bake temperature, the development adhesion of the coating film can be further improved. Specifically, the boiling point of the orthoester compound [E] is preferably 105°C or higher, more preferably 110°C or higher, and even more preferably 115°C or higher.
[0102] Specific examples of orthoester compounds having a boiling point of 105° C. or higher include triethyl orthoformate, tripropyl orthoformate, tributyl orthoformate, trimethyl orthoacetate, triethyl orthoacetate, triethyl orthodichloroacetate, trimethyl orthobutyrate, trimethyl orthopropionate, triethyl orthopropionate, trimethyl orthovalerate, trimethyl orthobenzoate, triethyl orthobenzoate, etc. In this specification, the boiling point is a value at 1 atmospheric pressure.
[0103] In the present composition, the content of the orthoester compound [E] is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 1 part by mass or more, relative to 100 parts by mass of the polymer component [A]. The content of the orthoester compound [E] is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, relative to 100 parts by mass of the polymer component [A]. When the content of the orthoester compound [E] is 0.1 parts by mass or more, it is preferable in that the effect of improving the development adhesion of the coating film by having the orthoester compound [E] present in the film can be sufficiently obtained. When the content of the orthoester compound [E] is 30 parts by mass or less, it is preferable in that the decrease in sensitivity caused by the orthoester compound [E] can be suppressed.
[0104] ([F] Crosslinker) As the crosslinking agent [F], at least one silane compound selected from the group consisting of silanol compounds and alkoxysilane compounds (hereinafter also referred to as "crosslinkable silane compound") can be preferably used. From the viewpoint of obtaining a film having a low dielectric constant and excellent development adhesion, the crosslinkable silane compound is preferably a compound represented by the following formula (7). In addition, the silane compound represented by the following formula (7) is preferred in that it is stable and hydrophobic in an alkaline developer and has little effect on unexposed areas (for example, effect on sensitivity). (R 70 ) k Si(OR 71 ) 4-k …(7) (In formula (7), R 70 is a hydrophobic group. 71 is a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. k is an integer of 1 to 3. R 70 If there are multiple R 70 are the same or different. R 71 If there are multiple R 71 are the same or different.)
[0105] In the above formula (7), R 70 Examples of the hydrophobic group represented by the formula (I) include a monovalent hydrocarbon group and a monovalent fluorinated hydrocarbon group. 70 The hydrophobic group represented by the formula (I) is preferably a monovalent hydrocarbon group, and examples thereof include a monovalent chain hydrocarbon group having 1 to 12 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 12 carbon atoms, and a monovalent aromatic hydrocarbon group having 1 to 12 carbon atoms. 70 is preferably a monovalent chain hydrocarbon group or a monovalent aromatic hydrocarbon group, more preferably an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 12 carbon atoms. R 71 is preferably a hydrogen atom, a methyl group or an ethyl group. In the above formula (7), k is preferably 1 or 2, since this can enhance the effects of improving the development adhesion and lowering the dielectric constant of the cured film.
[0106] Among the crosslinkable silane compounds, specific examples of the silanol compounds include silanol compounds having a hydroxyl group, such as trimethylsilanol, ethyldimethylsilanol, diethylmethylsilanol, triethylsilanol, methylsilanetriol, diphenylsilanediol, phenylsilanetriol, triphenylsilanol, bis(4-tolyl)silanediol, and tris(4-tolyl)silanol.
[0107] Among the crosslinkable silane compounds, examples of trifunctional alkoxysilane compounds include trimethoxy(methyl)silane, triethoxy(methyl)silane, methyltrippropoxysilane, tributoxy(methyl)silane, methyltriphenoxysilane, ethyltrimethoxysilane, triethoxy(ethyl)silane, ethyltrippropoxysilane, tributoxy(ethyl)silane, ethyltriphenoxysilane, trimethoxy(propyl)silane, triethoxy(propyl)silane, tripropoxy(propyl)silane, tributoxy(propyl)silane, and triphenoxy(propyl)silane. Examples of the silane that can be used include butyltrimethoxysilane, butyltriethoxysilane, butyltrippropoxysilane, tributoxy(butyl)silane, butyltriphenoxysilane, trimethoxy(phenyl)silane, triethoxy(phenyl)silane, phenyltrippropoxysilane, tributoxy(phenyl)silane, triphenoxy(phenyl)silane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, cyclohexyltripoxysilane, cyclohexyltributoxysilane, and cyclohexyltriphenoxysilane.
[0108] Among the crosslinkable silane compounds, examples of bifunctional alkoxysilane compounds that can be preferably used include dimethoxydimethylsilane, diethoxydimethylsilane, methylphenyldimethoxysilane, methylphenyldiethoxysilane, diisobutyldimethoxysilane, dicyclopentyldimethoxysilane, cyclohexyl(dimethoxy)methylsilane, cyclohexyldiethoxymethylsilane, dimethoxydiphenylsilane, diethoxydiphenylsilane, methylphenyldiethoxysilane, and dimethoxydiphenylsilane.
[0109] When forming a film using this composition, the coating film made of this composition is usually heated (prebaked) to remove the solvent component contained in this composition. Therefore, in order to suppress the volatilization of the crosslinkable silane compound during prebaking and to leave a large amount of the crosslinkable silane compound in the film after prebaking, a compound with a sufficiently high boiling point can be preferably used as the crosslinkable silane compound. Specifically, the boiling point of the crosslinkable silane compound is preferably 80°C or higher, more preferably 95°C or higher, even more preferably 120°C or higher, even more preferably 150°C or higher, and even more preferably 180°C or higher.
[0110] The crosslinkable silane compound to be added to the composition can also be selected according to the pre-bake temperature. Specifically, the boiling point of the crosslinkable silane compound is preferably 5°C or higher than the pre-bake temperature, more preferably 10°C or higher, even more preferably 20°C or higher, even more preferably 30°C or higher, and even more preferably 50°C or higher.
[0111] Among the above crosslinkable silane compounds, a compound having an aromatic ring can be preferably used, and a compound having two or more aromatic rings in one molecule can be more preferably used, because it has a high boiling point and high hydrophobicity and can enhance the effect of improving the development adhesion and low dielectric constant of the cured film.
[0112] The molecular weight of the crosslinking agent [F] is preferably at least 90, more preferably at least 100, and even more preferably at least 150. The molecular weight of the crosslinking agent [F] is preferably at most 500, more preferably at most 450, and even more preferably at most 400. When the molecular weight of the crosslinking agent [F] is within the above range, it is preferable in that the development adhesion of the cured film can be increased while suppressing a decrease in the sensitivity and development solubility of the composition, and a low dielectric constant can be achieved.
[0113] In the present composition, the content of the [F] crosslinking agent is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 1 part by mass or more, based on 100 parts by mass of the [A] polymer component. The content of the [F] crosslinking agent is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, based on 100 parts by mass of the [A] polymer component. When the content of the [F] crosslinking agent is 0.5 parts by mass or more, it is preferable in that the effect of improving the development adhesion and the dielectric constant of the coating film can be sufficiently obtained. When the content of the [F] crosslinking agent is 30 parts by mass or less, it is preferable in that the decrease in sensitivity caused by the [F] crosslinking agent can be suppressed.
[0114] ([G] Adhesion aid) [G] The adhesion aid is a component that improves the adhesion between the cured film formed by using the composition and the substrate. [G] The adhesion aid is preferably a functional silane coupling agent having a reactive functional group. Examples of the reactive functional group of the functional silane coupling agent include a carboxy group, a (meth)acryloyl group, an epoxy group, a vinyl group, and an isocyanate group.
[0115] Specific examples of functional coupling agents include trimethoxysilylbenzoic acid, 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, vinyltriacetoxysilane, vinyltrimethoxysilane, and 3-isocyanatopropyltriethoxysilane.
[0116] The content of the adhesion assistant (G) in the present composition is preferably no more than 30 parts by mass, and more preferably no more than 20 parts by mass, per 100 parts by mass of the polymer component (A).
[0117] ([H] Solvent) The present composition is a liquid composition in which the polymer component [A], the photoacid generator [B], and other components that are optionally blended are dissolved or dispersed preferably in a solvent [H]. The solvent [H] is preferably an organic solvent that dissolves each of the components blended in the present composition and does not react with each of the components.
[0118] Specific examples of the solvent [H] include alcohols such as methanol, ethanol, isopropanol, butanol, and octanol; esters such as ethyl acetate, butyl acetate, ethyl lactate, γ-butyrolactone, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, methyl 3-methoxypropionate, and ethyl 3-ethoxypropionate; ethers such as ethylene glycol monobutyl ether, propylene glycol monomethyl ether, ethylene diglycol monomethyl ether, ethylene diglycol ethyl methyl ether, dimethylene glycol dimethyl ether, diethylene glycol dimethyl ether, and diethylene glycol ethyl methyl ether; amides such as dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; and aromatic hydrocarbons such as benzene, toluene, xylene, and ethylbenzene. Of these, the solvent preferably contains at least one selected from the group consisting of ethers and esters, and more preferably contains at least one selected from the group consisting of ethylene glycol alkyl ether acetate, diethylene glycols, propylene glycol monoalkyl ether, and propylene glycol monoalkyl ether acetate.
[0119] Examples of other components include, in addition to the above, polyfunctional polymerizable compounds (polyfunctional (meth)acrylates, etc.), quinone diazide compounds, surfactants (fluorine-based surfactants, silicone-based surfactants, nonionic surfactants, etc.), polymerization inhibitors, antioxidants, chain transfer agents, etc. The blending ratio of these components can be appropriately selected according to each component within a range that does not impair the effects of the present disclosure.
[0120] The solid content concentration of the present composition (the ratio of the total mass of the components other than the [H] solvent in the radiation-sensitive composition to the total mass of the radiation-sensitive composition) is appropriately selected in consideration of viscosity, volatility, and the like. The solid content concentration of the present composition is preferably in the range of 5 to 60 mass %. When the solid content concentration is 5 mass % or more, a sufficient thickness of the coating film can be ensured when the present composition is applied onto a substrate. On the other hand, when the solid content concentration is 60 mass % or less, the thickness of the coating film does not become too large, and furthermore, the viscosity of the radiation-sensitive composition can be appropriately increased, and good coatability can be ensured. The solid content concentration of the present composition is more preferably 10 to 55 mass %, and further preferably 12 to 50 mass %.
[0121] <Cured film and manufacturing method thereof> The cured film of the present invention is formed by the radiation-sensitive composition prepared as described above. The radiation-sensitive composition has high radiation sensitivity and excellent storage stability. In addition, by using the radiation-sensitive composition, a pattern film can be formed that exhibits high adhesion to a substrate even after development, has a low dielectric constant, and is excellent in chemical resistance. Therefore, the radiation-sensitive composition can be preferably used as a material for forming, for example, an interlayer insulating film, a planarizing film, a spacer, a protective film, a colored pattern film for a color filter, a partition wall, a bank, etc.
[0122] In producing a cured film, the above-mentioned radiation-sensitive composition can be used to form a positive cured film depending on the type of photosensitizer. The cured film can be produced using the above-mentioned radiation-sensitive composition by a method including, for example, the following steps 1 to 4. (Step 1) A step of forming a coating film using the above-mentioned radiation-sensitive composition. (Step 2) A step of exposing at least a part of the coating film to light. (Step 3) A step of developing the coating film after exposure. (Step 4) Heating the developed coating. Each step will be described in detail below.
[0123] [Process 1: Coating process] In step 1, the radiation-sensitive composition is applied to a surface on which a film is to be formed (hereinafter also referred to as the "film-forming surface"), and the solvent is preferably removed by a heat treatment (pre-bake) to form a coating film on the film-forming surface. The material of the film-forming surface is not particularly limited. For example, when forming an interlayer insulating film, the radiation-sensitive composition is applied to a substrate provided with switching elements such as TFTs to form a coating film. Examples of the substrate include a glass substrate, a silicon substrate, and a resin substrate. The surface of the substrate on which the coating film is to be formed may have a metal thin film formed according to the application, or may have been subjected to various surface treatments such as HMDS (hexamethyldisilazane) treatment.
[0124] Examples of the method for applying the radiation-sensitive composition include spraying, roll coating, spin coating, slit die coating, bar coating, and inkjet. Among these, spin coating, slit die coating, and bar coating are preferred. Pre-baking conditions vary depending on the types and content ratios of each component in the radiation-sensitive composition, but are, for example, 60 to 130° C. and 0.5 to 10 minutes. The thickness of the coating film formed (i.e., the film thickness after pre-baking) is preferably 0.1 to 12 μm. The radiation-sensitive composition applied to the surface to be coated may be dried under reduced pressure (VCD) before pre-baking.
[0125] [Step 2: Exposure step] In step 2, at least a part of the coating film formed in step 1 is irradiated with radiation. At this time, the coating film is irradiated with radiation through a mask having a predetermined pattern, thereby forming a cured film having a pattern. Examples of radiation include ultraviolet rays, far ultraviolet rays, visible light, X-rays, and charged particle beams such as electron beams. Among these, ultraviolet rays are preferred, and examples of such beams include g-rays (wavelength 436 nm) and i-rays (wavelength 365 nm). The radiation exposure is 0.1 to 20,000 J / m 2 is preferred.
[0126] [Process 3: Development process] In step 3, the coating film irradiated in step 2 is developed. Specifically, the coating film irradiated in step 2 is developed with a developer to remove the irradiated portion, thereby performing positive development. Examples of the developer include an aqueous solution of an alkali (basic compound). Examples of the alkali include sodium hydroxide, tetramethylammonium hydroxide, and the alkali compounds described in paragraph 1 of JP 2016-145913 A.
[0127] Examples of the alkali include those exemplified in the above. From the viewpoint of obtaining suitable developability, the alkali concentration in the aqueous alkaline solution is preferably 0.1 to 5% by mass. Examples of the developing method include a puddle method, a dipping method, a swing immersion method, a shower method, and the like. The developing time varies depending on the composition of the composition, but is, for example, 30 to 120 seconds. After the developing step, it is preferable to perform a rinsing treatment by washing with running water on the patterned coating film.
[0127] [Process 4: Heating process] In step 4, the coating film developed in step 3 is heated (post-baked). Post-baking can be performed using a heating device such as an oven or a hot plate. Regarding post-baking conditions, the heating temperature is, for example, 120 to 250° C. The heating time is, for example, 5 to 40 minutes when the heating treatment is performed on a hot plate, and 10 to 80 minutes when the heating treatment is performed in an oven. In this manner, a cured film having a desired pattern can be formed on a substrate. The shape of the pattern of the cured film is not particularly limited, and examples thereof include a line-and-space pattern, a dot pattern, a hole pattern, and a lattice pattern.
[0128] By curing this composition, a cured film with a sufficiently low dielectric constant of 3.3 or less can be obtained. The dielectric constant of the cured film is measured by applying an integrated exposure dose of 9,000 J / m 2 The dielectric constant of the cured film was measured at a frequency of 10 kHz by irradiating the film with ultraviolet light under the conditions of (a) above and heating the film at 220° C. for 1 hour. For details on the method for measuring the dielectric constant of the cured film, follow the method described in the Examples below.
[0129] When the polymer component in the radiation-sensitive composition contains the first structural unit, the acid-dissociable group (Y 1 ) is eliminated, hydroxyl groups are generated in the first structural unit, which is considered to cause the dielectric constant of the cured film to increase. In this regard, it is considered that by introducing a relatively small amount of the second structural unit into the polymer component containing the first structural unit, the hydroxyl groups generated in the first structural unit by exposure and the functional groups in the second structural unit (specifically, the silanol groups generated by exposure) are crosslinked, thereby forming a cured film with a low dielectric constant and high transparency. Note that this is merely a guess and does not limit the present invention in any way.
[0130] <Semiconductor element> The semiconductor element of the present disclosure includes a cured film formed using the present composition. The cured film is preferably an interlayer insulating film that insulates wiring in the semiconductor element. The semiconductor element of the present disclosure can be manufactured using a known method.
[0131] <Display element> The display element of the present disclosure includes a cured film formed using the present composition. The display element of the present disclosure may include a cured film formed using the present composition by including a semiconductor element of the present disclosure. Furthermore, the display element of the present disclosure may include a planarization film formed on a TFT substrate as a cured film formed using the present composition. Examples of the display element include a liquid crystal display element and an organic electroluminescence (EL) display element.
[0132] According to the present disclosure described above in detail, the following means are provided. <Means 1> A radiation-sensitive composition comprising: [A] a polymer component including, in the same molecule or in different molecules, a first structural unit having a partial structure represented by the formula (1) above, and a second structural unit having a partial structure represented by the formula (2) above; and [B] a photoacid generator, the first structural unit being contained in an amount of 5 to 50 mass % and the second structural unit being contained in an amount of 0.1 to 20 mass % based on the total structural units of the polymer component. <Measure 2> The radiation-sensitive composition according to <Measure 1>, wherein the photoacid generator is at least one selected from the group consisting of an oxime sulfonate compound and an N-sulfonyloxyimide compound. <Means 3> The Y 1 The radiation-sensitive composition according to <means 1> or <means 2>, which is represented by the above formula (Y-1), formula (Y-2) or formula (Y-3). <Means 4> The Ar 1 The radiation-sensitive composition according to any one of <Measures 1> to <Measures 3>, wherein is a substituted or unsubstituted phenylene group, naphthylene group, or anthrylene group. <Means 5> The radiation-sensitive composition according to any one of <Means 1> to <Means 4>, wherein the polymer component further contains at least one selected from the group consisting of a structural unit derived from maleimide and a structural unit having an acid group. <Means 6> The radiation-sensitive composition according to any one of <Means 1> to <Means 5>, wherein the polymer component further contains a structural unit having a crosslinkable group (excluding the first structural unit and the second structural unit). <Measures 7> The radiation-sensitive composition according to any one of <Measures 1> to <Measures 6>, further comprising an orthoester compound. <Measures 8> A cured film formed using the radiation-sensitive composition according to any one of <Measures 1> to <Measures 7>. <Means 9> The cured film according to <Means 8>, which has a relative dielectric constant of 3.3 or less at a frequency of 10 kHz. <Means 10> A method for producing a cured film, comprising the steps of: forming a coating film using the radiation-sensitive composition according to any one of <Means 1> to <Means 7>; exposing at least a part of the coating film to light; developing the exposed coating film; and heating the developed coating film. <Means 11> A semiconductor device comprising the cured film according to <Means 8>. <Means 12> A display device comprising the cured film according to <Means 8>. EXAMPLES
[0133] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples and comparative examples, "parts" and "%" are based on mass unless otherwise specified. In the examples, the weight average molecular weight (Mw) and number average molecular weight (Mn) of the polymer were measured by the following method.
[0134] [Weight average molecular weight (Mw) and number average molecular weight (Mn)] The Mw and Mn of the polymer were measured by the following method. Measurement method: Gel permeation chromatography (GPC) method Equipment: Showa Denko GPC-101 GPC column: Shimadzu GLC GPC-KF-801, GPC-KF-802, GPC-KF-803 and GPC-KF-804 combined Mobile phase: Tetrahydrofuran Column temperature: 40℃ ·Flow rate: 1.0mL / min Sample concentration: 1.0% by mass Sample injection volume: 100μL Detector: Differential refractometer Standard material: Monodisperse polystyrene
[0135] [Monomer] The abbreviations of the monomers used in the synthesis of the polymer are as follows. <Monomer that provides the first structural unit> TMSPIPE: 4-isopropenylphenyloxytrimethylsilane TESPIPE: 4-isopropenylphenyloxytriethylsilane TMSPHS: 4-vinylphenyloxytrimethylsilane TMSOPMI: 4-trimethylsilyloxy-N-phenylmaleimide TMSOPMA: 4-trimethylsilyloxyphenyl methacrylate EOEPIPE: 1-(4-isopropenylphenyloxy)-1-ethoxyethane BocPIPE: (4-isopropenylphenyl)-(1,1-dimethylethyl) carbonate
[0136] <<Monomer that provides the second structural unit>> MPTMS: methacryloyloxypropyltrimethoxysilane APTMS: acryloyloxypropyltrimethoxysilane MPTES: Methacryloyloxypropyltriethoxysilane STTMS: 4-vinylphenyltrimethoxysilane VTES: Vinyltriethoxysilane
[0137] <<Monomer that provides the third structural unit>> MA: methacrylic acid MI: Maleimide 4IPP: 4-isopropenylphenol HPMA: Hydroxyphenyl methacrylate
[0138] <<Monomer that provides the fourth structural unit>> GA: Glycidyl acrylate GMA: glycidyl methacrylate ECHMA: 3,4-epoxycyclohexylmethyl methacrylate OXMA: 3-methacryloyloxymethyl-3-ethyloxetane EDCPMA: 2-hydroxyethyl methacrylate [3,4-epoxytricyclo(5.2.1.0^2,6)decan-9-yl]
[0139] <Monomer that provides the fifth structural unit> TMSMA: Trimethylsilyl methacrylate M-THP: Tetrahydro-2H-pyran-2-yl methacrylate M-THF: 2-Tetrahydrofuranyl methacrylate
[0140] Other Monomers MMA: Methyl methacrylate CHMI: N-cyclohexylmaleimide PMI: N-phenylmaleimide ST: styrene CHMA: Cyclohexyl methacrylate
[0141] <Synthesis of polymer component (A)> [Synthesis Example 1] Synthesis of polymer (A-1) In a flask equipped with a cooling tube and a stirrer, 10 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) and 200 parts of diethylene glycol methyl ethyl ether were charged. Subsequently, 15 parts of 4-isopropenylphenyloxytrimethylsilane, 5 parts of methacryloyloxypropyltrimethoxysilane, 15 parts of maleimide, 10 parts of glycidyl acrylate, 45 parts of methyl methacrylate, and 10 parts of N-cyclohexylmaleimide were charged, and after nitrogen replacement, the temperature of the solution was raised to 70°C while gently stirring, and this temperature was maintained for 5 hours to obtain a polymer solution containing polymer (A-1). The solid content concentration of this polymer solution was adjusted to 30% by mass. The Mw of polymer (A-1) was 10,500, and the molecular weight distribution (Mw / Mn) was 2.2.
[0142] [Synthesis Examples 2 to 22, Comparative Synthesis Examples 1 to 5] Synthesis of Polymers (A-2) to (A-22) and (CA-1) to (CA-5) Polymer solutions containing polymers having the same solid content concentration, weight average molecular weight, and molecular weight distribution as polymer (A-1) were obtained in the same manner as in Synthesis Example 1, except that the types and amounts (parts by mass) of each component shown in Table 1 were used.
[0143] [Table 1]
[0144] <Preparation of Radiation-Sensitive Composition (1)> The components used in preparing the radiation-sensitive composition are shown below. {[A] Polymer component} A-1 to A-22: Polymers (A-1) to (A-22) synthesized in Synthesis Examples 1 to 22 CA-1 to CA-5: Polymers (CA-1) to (CA-5) synthesized in Comparative Synthesis Examples 1 to 5
[0145] [B] Photoacid generator B-1: NIT (N-hydroxynaphthalimide triflate) B-2: Irgacure PAG121 (BASF) B-3: OS-17 described in International Publication No. 2016 / 124493 B-4: OS-25 described in International Publication No. 2016 / 124493 B-5: B-9 described in Patent No. 5914663
[0146] [C] Antioxidants C-1: Adeka STAB AO-20 (ADEKA) C-2: Adeka STAB AO-60 (ADEKA) C-3: Adeka STAB AO-330 (ADEKA)
[0147] [D] Acid diffusion control agent D-1: 2-phenylbenzimidazole D-2: N-(tert-butoxycarbonyl)-2-phenylbenzimidazole
[0148] [E] Orthoester compounds E-1: Trimethyl orthoformate E-2: Triethyl orthoacetate E-3: Trimethyl orthobenzoate
[0149] Crosslinking Agent (F) F-1: Cyclohexyltrimethoxysilane F-2: Methylphenyldiethoxysilane F-3: Dimethoxydiphenylsilane F-4: Diphenylsilanediol F-5: Dicyclopentyldimethoxysilane F-6: Diisobutyldimethoxysilane
[0150] [Example 1] To the polymer solution containing the polymer (A-1) obtained in Synthesis Example 1, 3 parts of a photoacid generator (B-1), 1 part of an antioxidant (C-1), 0.01 parts of an acid diffusion controller (D-1), 1 part of an orthoester compound (E-1), and 1 part of a crosslinking agent (F-1) were mixed in an amount equivalent to 100 parts (solid content) of the polymer (A-1), and diethylene glycol ethyl methyl ether and propylene glycol monomethyl ether were added in a mass ratio of 1:1 so that the final solid content concentration was 20 mass%. Then, the mixture was filtered through a membrane filter having a pore size of 0.2 μm to prepare a radiation-sensitive composition (S-1).
[0151] [Examples 2 to 25, Comparative Examples 1 to 5] The radiation-sensitive compositions of Examples 2 to 25 and Comparative Examples 1 to 5 were prepared in the same manner as in Example 1, except that the types and amounts (parts by mass) of each component shown in Table 2 were used.
[0152] [Table 2]
[0153] <Evaluation> The following items were evaluated by the methods described below using the radiation-sensitive compositions of Examples 1 to 25 and Comparative Examples 1 to 5. The evaluation results are shown in Table 3.
[0154] [Radiation sensitivity] Using a spinner, the radiation-sensitive composition was applied onto a silicon substrate that had been treated with HMDS at 60°C for 60 seconds, and then prebaked on a hot plate at 90°C for 2 minutes to form a coating film with an average thickness of 3.0 μm. This coating film was irradiated with a predetermined amount of ultraviolet light from a mercury lamp through a pattern mask having a line-and-space pattern with a width of 10 μm. Next, a development process was carried out at 25°C for 60 seconds using a 2.38 mass% aqueous solution of tetramethylammonium hydroxide as a developer, and then washing was carried out with running ultrapure water for 1 minute. At this time, the minimum exposure dose capable of forming a line-and-space pattern with a width of 10 μm was measured, and the radiation sensitivity was evaluated based on the minimum exposure dose. The evaluation criteria are as follows. ○: The minimum exposure measurement is 300 J / m 2 Less than 1000 nm, and has good radiation sensitivity ×: The measured minimum exposure is 300 J / m 2 or more, and radiation sensitivity is poor
[0155] [Dielectric constant] A radiation-sensitive composition was applied to a SUS304 substrate whose surface had been smoothed by polishing with a sisal buff (hemp buff), and the solvent was removed under vacuum with an ultimate pressure set to 100 Pa. The composition was then prebaked at 90°C for 2 minutes to form a coating film with an average thickness of 3.0 μm. The resulting coating film was exposed to an exposure machine (Canon's "MPA-600FA") with an accumulated exposure dose of 9,000 J / m 2 The substrate with the exposed coating was heated in a clean oven at 220°C for 1 hour to form an insulating film on the substrate. A Pt / Pd electrode pattern was formed on this insulating film by deposition to prepare a sample for measuring dielectric constant. The substrate with this electrode pattern was subjected to measurement of the relative dielectric constant by the CV method at a frequency of 10 kHz using an HP16451B electrode and an HP4284A precision LCR meter manufactured by Yokogawa-Hewlett-Packard. The evaluation criteria are as follows: ○: Measurement value is 3.3 or less ×: Measurement value exceeds 3.3
[0156] [Transmittance (transparency)] The radiation-sensitive composition was applied onto a glass substrate using a spinner, and then prebaked on a hot plate at 90° C. for 2 minutes to form a coating film with a thickness of 3.0 μm. The resulting coating film was irradiated with an integrated dose of 3,000 J / m 2 using a mercury lamp. 2 The glass substrate was then heated on a hot plate at 200°C for 30 minutes to obtain a cured film. The transmittance of the obtained cured film was measured using a UV-visible spectrophotometer ("V-630" manufactured by JASCO Corporation). The evaluation criteria were as follows: ○: The transmittance of light with a wavelength of 400 nm is 97% or more, and the transparency is good. ×: The transmittance of light with a wavelength of 400 nm is less than 97%, and the transparency is poor.
[0157] [Storage stability] The prepared radiation-sensitive composition was sealed in a light-shielding, airtight container. After 7 days at 25°C, the container was opened and the minimum exposure dose required to form a 10 μm-wide line-and-space pattern, as determined in the [Radiation Sensitivity] measurement before storage, was irradiated in the same manner as for the [Radiation Sensitivity] above, and the increase rate of the line width for the same exposure dose before and after storage for 7 days was calculated. The evaluation criteria were as follows: ○: The increase is less than 10% and the storage stability is good. ×: Increase is 10% or more, and storage stability is poor.
[0158] [Outgassing properties] The radiation-sensitive composition was applied onto a silicon substrate using a spinner, and then prebaked on a hot plate at 90°C for 2 minutes to form a coating film with an average thickness of 3.0 μm. The substrate was then baked for 30 minutes using an oven heated to 230°C to form a cured film. The silicon substrate was then cut to a size of 1 cm x 5 cm, and baked for 15 minutes at 230°C using a P&T-GCMS device consisting of a JTD-505 manufactured by Japan Analytical Industry Co., Ltd. and a GC-QP-2010 manufactured by Shimadzu Corporation to obtain a chromatogram. The amount of outgassing was calculated from the following formula (I) using the peak area of C18 in the chromatogram when the cured film was used as the measurement sample and the peak area of the chromatogram of standard sample C18 measured separately using the same device. In the following formula (I), the "amount of standard sample introduced" refers to the amount of standard sample introduced into the device when obtaining the chromatogram of standard sample C18. Amount of outgassing (μg) = (peak area of chromatogram of cured film / peak area of chromatogram of standard sample) × amount of standard sample introduced (μg) ... (I) The calculated outgassing amount was used to evaluate the outgassing characteristics according to the following criteria. ○: Outgassing amount is less than 10 μg and outgassing characteristics are good ×: The amount of outgassing is 10 μg or more, and the outgassing characteristics are poor.
[0159] [Pattern shape (taper shape)] Using a spinner, the radiation-sensitive composition was applied onto a silicon substrate that had been treated with HMDS at 60°C for 60 seconds, and then prebaked on a hot plate at 90°C for 2 minutes to form a coating film with an average thickness of 3.0 μm. A predetermined amount of ultraviolet light was irradiated onto this coating film using a pattern mask having a line-and-space pattern with a width of 10 μm, using a mercury lamp. Next, a development process was carried out at 25°C for 60 seconds using a 2.38% by mass aqueous solution of tetramethylammonium hydroxide as a developer, and then washing was carried out with running ultrapure water for 1 minute. Furthermore, the substrate was baked for 30 minutes using an oven heated to 230°C to form a cured film. After cutting the silicon substrate into a size of 1 cm x 1 cm, the cross-sectional shape of the line-and-space pattern was observed using a scanning electron microscope Regulus8100 manufactured by Hitachi High-Tech Corporation, and the taper angle was determined. The pattern shape was evaluated according to the following criteria based on the taper angle. ○: The taper angle is 50 degrees or more and the taper shape is good. ×: The taper angle is less than 50 degrees and the taper shape is poor.
[0160] [Table 3]
[0161] As shown in Table 3, the radiation-sensitive compositions of Examples 1 to 25 were evaluated as being good in terms of practical properties, such as radiation sensitivity, dielectric constant, transmittance, storage stability, outgassing properties, and pattern shapeability, and were well-balanced in terms of various properties. In contrast, the films of Comparative Examples 1 to 3 had low dielectric constants, and Comparative Example 1 also had poor pattern shapeability. Furthermore, Comparative Example 4 had low film transmittance, and Comparative Example 5 had poor radiation sensitivity and pattern shapeability.
Claims
1. [A] a polymer component including, in the same molecule or in different molecules, a first structural unit having a partial structure represented by the following formula (1) and a second structural unit having a partial structure represented by the following formula (2): [B] a photoacid generator; Contains a radiation-sensitive composition comprising the first structural unit in an amount of 5 to 50% by mass and the second structural unit in an amount of 0.1 to 20% by mass, based on the total structural units of the polymer component; 【Chemistry 1】 (In formula (1), Ar 1 is a divalent aromatic ring group. 1 is an acid dissociable group. n is 0 or 1. "*" represents a bond. However, when n is 0, the first structural unit is a structural unit derived from a monomer having a maleimide ring, and Y 1 is bonded to the nitrogen atom of the maleimide ring. 【Chemistry 2】 (In formula (2), R 1 , R 2 and R 3 are each independently a hydrogen atom, a halogen atom, a hydroxyl group, an alkoxy group having 1 to 6 carbon atoms, an alkyl group having 1 to 10 carbon atoms, or a phenyl group. 1 , R 2 and R 3 At least one of the groups is an alkoxy group having 1 to 6 carbon atoms. "*" represents a bond bonded to a carbon atom.)
2. 2. The radiation-sensitive composition according to claim 1, wherein the photoacid generator is at least one selected from the group consisting of oxime sulfonate compounds and N-sulfonyloxyimide compounds.
3. The Y 1 The radiation-sensitive composition according to claim 1, wherein the compound is represented by the following formula (Y-1), formula (Y-2), or formula (Y-3): 【Chemistry 3】 (In formula (Y-1), R 4 , R 5 and R 6 are each independently a hydrogen atom, a halogen atom, a hydroxyl group, a monovalent hydrocarbon group having 1 to 20 carbon atoms, or a group in which some or all of the hydrogen atoms in the hydrocarbon group have been substituted with a substituent. "*" represents a bond.) 【Chemistry 4】 (In formula (Y-2), R 7 , R 8 and R 9 satisfies the following (1) or (2). 7 R is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms. 8 and R 9 are each independently an alkyl group having 1 to 12 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms. (2) R 7 R is a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms. 8 and R 9 are combined together to form R 8 and OR 9 represents a cyclic ether structure formed together with the carbon atom to which it is bonded. "*" represents a bond.) 【Chemistry 5】 (In formula (Y-3), R 10 is a tertiary alkyl group. "*" represents a bond.)
4. The Ar 1 The radiation-sensitive composition according to claim 1 , wherein is a substituted or unsubstituted phenylene group, naphthylene group, or anthrylene group.
5. 2. The radiation-sensitive composition according to claim 1, wherein the polymer component further comprises at least one selected from the group consisting of a structural unit derived from maleimide and a structural unit having an acid group.
6. The radiation-sensitive composition according to claim 1 , wherein the polymer component further comprises a structural unit having a crosslinkable group (excluding the first structural unit and the second structural unit).
7. The radiation-sensitive composition according to claim 1 , further comprising an orthoester compound.
8. A cured film formed using the radiation-sensitive composition according to any one of claims 1 to 7.
9. The cured film according to claim 8 , which has a dielectric constant of 3.3 or less at a frequency of 10 kHz.
10. A step of forming a coating film using the radiation-sensitive composition according to any one of claims 1 to 7; exposing at least a portion of the coating to light; developing the coating film after exposure; heating the developed coating; The method for producing a cured film comprising the steps of:
11. A semiconductor device comprising the cured film according to claim 8.
12. A display device comprising the cured film according to claim 8.
Citation Information
Patent Citations
Radiation sensitive resin composition, method for forming cured article, cured article, semiconductor element and display element
JP2017107024A
Radiation-sensitive composition and use therefor
JP2019174614A
Radiation-sensitive composition, cured film and method for producing the same, semiconductor element and display element
JP2021196577A
Cited By
Positive photosensitive resin composition, organic el element partition wall, organic el element insulating film, and organic el element
JP2025063843A
Positive-type photosensitive resin composition, organic EL element partition, organic EL element insulating film, and organic EL element