Ionic liquid for heavy metal recovery
An ionic liquid composed of imidazolium cation and specific anions enables recyclable and stable heavy metal recovery, addressing the limitations of existing chelating agents by facilitating repeated use.
Patent Information
- Application Number
- JP2023217591
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-20
- Filing Date
- 2023-12-25
- Publication Date
- 2024-10-31
AI Technical Summary
Existing chelating agents used for heavy metal recovery are not recyclable and stable after decomposition, limiting their reuse.
Development of an ionic liquid composed of imidazolium cation and specific anions, such as succinate, acetopyruvate, or citrate, which allows for the recovery and regeneration of heavy metals like cobalt, nickel, and manganese, maintaining chemical stability.
The ionic liquid achieves excellent heavy metal recovery and can be reused multiple times due to its chemical stability, preventing decomposition or polymerization during the recovery process.
Smart Images

Figure 2024155709000001 
Figure 2024155709000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an ionic liquid for recovering heavy metals. [Background technology]
[0002] Although heavy metals are widely used as materials for secondary batteries, their recovery after use is an issue. As a method for recovering heavy metals, the use of a specific chelating agent has been proposed (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2003-079940 A Summary of the Invention [Problem to be solved by the invention]
[0004] Even with the technology of Patent Document 1, the chelating agent used in recovering heavy metals is discarded after a decomposition process, and therefore it cannot be said to be fully satisfactory. An object of the present invention is to provide an ionic liquid for heavy metal recovery that is recyclable and stable even after recovery, and therefore can be reused. [Means for solving the problem]
[0005] The present inventors have conducted extensive research to solve the above problems and have arrived at the present invention. That is, the present invention relates to an ionic liquid for recovering heavy metals, which is composed of an imidazolium cation (CA) and an anion (AN) represented by the following general formula (1). RC(=O)O - (1) [In general formula (1), R is a residue obtained by removing one carboxyl group from a dicarboxylic acid having 2 to 10 carbon atoms, a residue obtained by removing one carboxyl group from a monocarboxylic acid having a β-dicarbonyl structure having 3 to 6 carbon atoms, or a residue obtained by removing one carboxyl group from a tricarboxylic acid having 4 to 6 carbon atoms.] Effect of the Invention
[0006] The ionic liquid for heavy metal recovery of the present invention has the following effects. (1)Excellent recovery of heavy metals. (2) It is renewable and chemically stable even after recovery, so it can be reused. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] <Imidazolium cation (CA)> Examples of the imidazolium cation (CA) in the present invention include 1-methylimidazolium, 1-ethylimidazolium, 1-propylimidazolium, 1-butylimidazolium, 1,3-dimethylimidazolium, 1-ethyl-3-methylimidazolium, 1-propyl-3-methylimidazolium, 1-butyl-3-methylimidazolium, 1-hexyl-3-methylimidazolium, 1,3-diethylimidazolium, and 1-octyl-3-methylimidazolium.
[0008] Of the above imidazolium cations (CA), from the viewpoint of recovery of heavy metals, preferred are 1-ethyl-3-methylimidazolium, 1-butyl-3-methylimidazolium, and 1,3-diethylimidazolium, more preferred are 1-ethyl-3-methylimidazolium and 1-butyl-3-methylimidazolium, and particularly preferred is 1-ethyl-3-methylimidazolium.
[0009] <Anion (AN)> The anion (AN) in the present invention is represented by the following general formula (1). RC(=O)O - (1)
[0010] In the above general formula (1), R is a residue obtained by removing one carboxyl group from a dicarboxylic acid having 2 to 10 carbon atoms, a residue obtained by removing one carboxyl group from a monocarboxylic acid having a β-dicarbonyl structure having 3 to 6 carbon atoms, or a residue obtained by removing one carboxyl group from a tricarboxylic acid having 4 to 6 carbon atoms.
[0011] Examples of the dicarboxylic acid having 2 to 10 carbon atoms include aliphatic dicarboxylic acids (oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, azelaic acid, and sebacic acid) and aromatic ring-containing dicarboxylic acids (phthalic acid, isophthalic acid, and terephthalic acid). Among the above dicarboxylic acids having 2 to 10 carbon atoms, from the viewpoint of heavy metal recovery, aliphatic dicarboxylic acids are preferred, malonic acid and succinic acid are more preferred, and succinic acid is particularly preferred.
[0012] Examples of the monocarboxylic acid having a β-dicarbonyl structure having 3 to 6 carbon atoms include acetopyruvic acid, diacetoacetic acid, and acetoacetic acid. Of the above monocarboxylic acids having a β-dicarbonyl structure having 3 to 6 carbon atoms, from the viewpoint of heavy metal recovery, preferred are acetopyruvic acid and diacetoacetic acid, and more preferred is acetopyruvic acid.
[0013] Examples of the tricarboxylic acid having 4 to 6 carbon atoms include citric acid, isocitric acid, cis-aconitic acid, and trans-aconitic acid. Among the above tricarboxylic acids having 4 to 6 carbon atoms, citric acid is preferred from the viewpoint of heavy metal recovery.
[0014] Of these, succinic acid is most preferred from the viewpoint of both recovery of heavy metals and stability after recovery. When R in general formula (1) is a residue obtained by removing one carboxyl group from succinic acid, the anion (AN) can also be said to be a residue obtained by removing one hydrogen from the carboxyl group of succinic acid (succinate).
[0015] <Ionic liquid for heavy metal recovery> The ionic liquid for heavy metal recovery of the present invention is composed of the imidazolium cation (CA) and the anion (AN). That is, examples of ionic liquids include 1-ethyl-3-methylimidazolium monosuccinate, 1-butyl-3-methylimidazolium monosuccinate, 1-ethyl-3-methylimidazolium acetopyruvate, 1-butyl-3-methylimidazolium acetopyruvate, 1-ethyl-3-methylimidazolium monocitrate, and 1-butyl-3-methylimidazolium monocitrate. The ionic liquid for recovering heavy metals can be applied to recover various compositions containing heavy metals and various heavy metal-containing compounds. The heavy metals to be recovered are preferably cobalt, nickel, and manganese, and more preferably cobalt.
[0016] The ionic liquid for heavy metal recovery of the present invention can be produced by a known method, and optimum conditions can be adopted depending on the raw material. For example, when the ionic liquid is 1-ethyl-3-methylimidazolium monosuccinate, it can be produced by the following production method. (1) 1-Ethylimidazole and dimethyl carbonate are reacted in methanol to obtain a methanol solution of 1-ethyl-3-methylimidazolium monomethyl carbonate. (2) A methanol solution of 1-ethyl-3-methylimidazolium monomethyl carbonate is gradually added to a methanol solution of succinic acid to obtain a solution of 1-ethyl-3-methylimidazolium monosuccinate. (3) The solution of 1-ethyl-3-methylimidazolium monosuccinate is desolvated to obtain 1-ethyl-3-methylimidazolium monosuccinate.
[0017] Furthermore, for example, when the ionic liquid is 1-butyl-3-methylimidazolium acetopyruvate, it can be produced by the following production method. (1) 1-Butylimidazole and dimethyl carbonate are reacted in methanol to obtain a methanol solution of 1-butyl-3-methylimidazolium monomethyl carbonate. (2) A methanol solution of 1-butyl-3-methylimidazolium monomethyl carbonate is gradually added to a methanol solution of acetopyruvic acid to obtain a solution of 1-butyl-3-methylimidazolium acetopyruvate. (3) The solution of 1-butyl-3-methylimidazolium acetopyruvate is desolvated to obtain 1-butyl-3-methylimidazolium acetopyruvate.
[0018] Furthermore, for example, when the ionic liquid is 1-ethyl-3-methylimidazolium monocitrate, it can be produced by the following production method. (1) 1-Ethylimidazole and dimethyl carbonate are reacted in methanol to obtain a methanol solution of 1-ethyl-3-methylimidazolium monomethyl carbonate. (2) Slowly add the methanol solution of 1-ethyl-3-methylimidazolium monomethyl carbonate to a methanol solution of citric acid to obtain a solution of 1-ethyl-3-methylimidazolium monocitrate. (3) The solution of 1-ethyl-3-methylimidazolium monocitrate is desolvated to obtain 1-ethyl-3-methylimidazolium monocitrate.
[0019] The method for recovering heavy metals using the ionic liquid for heavy metal recovery of the present invention is, for example, as follows: In this specification, a heavy metal is deemed to be "recovered" when the heavy metal is transferred to the outside of a heavy metal-containing composition (such as an electrode constituting a lithium ion secondary battery) from which the heavy metal is to be recovered. (1) A heavy metal-containing composition, i.e., a positive electrode material (e.g., lithium cobalt oxide) removed from a used lithium ion secondary battery, is placed in a container. The positive electrode material removed from the lithium ion secondary battery may be subjected to a heat treatment, pulverization, or other treatment as necessary before being placed in the container. (2) Next, an ionic liquid for recovering heavy metals is added, and the cobalt in the positive electrode material is recovered into the ionic liquid while stirring. The temperature in this step is preferably 150 to 230° C., more preferably 180 to 200° C., from the viewpoint of recovery of heavy metals. (3) After the above (2), the positive electrode material after leaching the heavy metal (cobalt) can be separated from the ionic liquid by solid-liquid separation. The liquid component after separation of the solid component is an ionic liquid containing the heavy metal (cobalt) component leached (recovered) from the positive electrode material. Next, the ionic liquid containing a heavy metal (cobalt) component is cooled and an acid (sulfuric acid, hydrochloric acid, oxalic acid, etc.) is added, whereby the recovered cobalt can be isolated in the form of a cobalt salt. When an acid is added to an ionic liquid containing a heavy metal (cobalt) component, the heavy metal (cobalt) component in the ionic liquid reacts with the acid to form a salt, which precipitates. By separating this precipitate from the ionic liquid, the heavy metal (cobalt) can be separated from the ionic liquid containing the heavy metal (cobalt) component. At the same time, the ionic liquid for recovering heavy metals of the present invention is regenerated. The ionic liquid from which the heavy metal components have been separated (regenerated ionic liquid for heavy metal recovery) can be used as is for the next heavy metal recovery process.
[0020] The reason why the ionic liquid for heavy metal recovery of the present invention has excellent heavy metal recovery properties is believed to be, for example, that it solubilizes the positive electrode material (lithium cobalt oxide) and chemically bonds the heavy metal (ion) to the carboxyl group or β-carbonyl group of the ionic liquid for heavy metal recovery. After the recovery, as in (3) above, the heavy metals can be isolated in the form of salts with acids, and the ionic liquid for heavy metal recovery can be regenerated at the same time. Furthermore, the ionic liquid for heavy metal recovery of the present invention is (chemically) stable even after heavy metal recovery and after regeneration, and can therefore be reused as a solvent for heavy metal recovery. The above phrase "(chemically) stable even after heavy metal recovery and after regeneration" means that it is unlikely to undergo reactions such as decomposition or polymerization even after heating in the heavy metal recovery process and addition of acid during regeneration. EXAMPLES
[0021] The present invention will be further described below with reference to examples, but the present invention is not limited to these. In the examples, the parts are parts by weight.
[0022] <Example 1> In a stainless steel vessel equipped with stirring, 30 parts of 1-ethyl-3-methylimidazolium acetopyruvate as an ionic liquid for heavy metal recovery (K-1) and 1 part of lithium cobalt oxide (product name "Cellseed", manufactured by Nippon Chemical Industry Co., Ltd.) were charged. Next, while stirring at 60 rpm, the temperature was raised to 200°C over 10 minutes, stirring was continued at 200°C for a further 10 minutes, and then the mixture was cooled to 40°C over 10 minutes to recover heavy metals. The contents were evaluated for heavy metal recovery and post-recovery stability using the methods described below. The results are shown in Table 1.
[0023] (1) Recovery of heavy metals (Evaluation condition A) Ten parts of the contents of the stainless steel container were mixed with 90 parts of dimethyl sulfoxide, and the remaining solid component (lithium cobalt oxide) was filtered off. The filtrate was subjected to fluorescent X-ray measurement (Axios, manufactured by Spectris) to calculate the cobalt concentration (wt%) in the ionic liquid (K) phase, and evaluated according to the following <Evaluation Criteria>.
[0024] <Evaluation criteria> ◎: Cobalt concentration is 5% by weight or more ○: Cobalt concentration is 2% by weight or more and less than 5% by weight △: Cobalt concentration is 1% by weight or more and less than 2% by weight ×: Cobalt concentration is less than 1% by weight
[0025] (2) Stability after recovery To the filtrate from (1) above, an equal amount of sulfuric acid (reagent grade) to that of cobalt was added over a period of 5 minutes. Next, the produced cobalt sulfate is removed by filtration, and then the dimethyl sulfoxide is distilled off at 150° C. under reduced pressure, and the weight of the ionic liquid for heavy metal recovery (K) in the residue is determined as follows: 1 H-MNR, 13 The properties were calculated from the C-NMR spectrum and evaluated according to the following <evaluation criteria>.
[0026] <Evaluation criteria> ◎: The weight of ionic liquid (K) is 98% by weight or more ○: The weight of the ionic liquid (K) is 95% by weight or more and less than 98% by weight. △: The weight of the ionic liquid (K) is 90% by weight or more and less than 95% by weight. ×: The weight of the ionic liquid (K) is less than 90% by weight
[0027] <Examples 2 to 3, Comparative Example 1> Evaluation was performed in the same manner as in Example 1, except that the ionic liquid for heavy metal recovery (K) or the comparative ionic liquid (comparative K) shown in Table 1 was used in Example 1. The results are shown in Table 1.
[0028] [Table 1]
[0029] <Example 4> In a test tube (1.6 cm, height 20 cm), lithium nickel manganese cobalt oxide [LiNi 0.33 Mn 0.33 Co 0.33 The reactor was charged with 1 part of NMC111 (manufactured by Tokyo Chemical Industry Co., Ltd.) and 30 parts of 1-ethyl-3-methylimidazolium acetopyruvate, an ionic liquid for heavy metal recovery (K-1). Next, using a hot plate and an aluminum heat block, the temperature was raised to 180°C in 10 minutes, and heating was continued at 180°C for a further 48 hours, after which the temperature was cooled to 40°C in 10 minutes to recover the heavy metals. The contents were evaluated for heavy metal recovery and post-recovery stability using the methods described below. The results are shown in Table 2.
[0030] (3) Recovery of heavy metals (evaluation condition B) After heating, 150 parts of acetonitrile was added to the test tube, which was then shaken and mixed, and the solid and liquid components were separated by passing through a syringe filter [manufactured by Cytiva, GD / X Φ25 mm, 0.2 μm]. The liquid components obtained were analyzed by fluorescent X-ray measurement [Rigaku, Supermini 200], and the leaching concentration (metal concentration) (ppm) of each metal (Ni, Co, Mn) was determined by semi-quantitative method, and the metal leaching rate (%) was calculated according to the following formula. The results are shown in Table 2. Metal leaching rate (%) = [metal concentration (ppm) × 10 -4 × weight of liquid component (g)] / [Weight of NMC111 (g) × metal content in NMC111 (%)] × 100
[0031] (4) Stability after recovery To the liquid component (3) above, sulfuric acid (reagent grade 1) in an amount equal to the amount of metal (total amount of Ni, Co, and Mn) determined in (3) was added over a period of 5 minutes to precipitate the metal components. Next, the resulting precipitate (metal sulfate) was removed by filtration, and then the dimethyl sulfoxide was distilled off at 150°C under reduced pressure. The weight of the ionic liquid for heavy metal recovery in the residue was calculated as follows: 1 H-MNR, 13 The properties were calculated from the C-NMR spectrum and evaluated according to the following <evaluation criteria>.
[0032] <Evaluation criteria> ◎: The weight of ionic liquid (K) is 98% by weight or more ○: The weight of the ionic liquid (K) is 95% by weight or more and less than 98% by weight. △: The weight of the ionic liquid (K) is 90% by weight or more and less than 95% by weight. ×: The weight of the ionic liquid (K) is less than 90% by weight
[0033] <Examples 5 to 6, Comparative Example 2> Evaluation was performed in the same manner as in Example 4, except that the ionic liquid for heavy metal recovery (K) or the comparative ionic liquid (comparative K) shown in Table 2 was used in Example 4. The results are shown in Table 2.
[0034] [Table 2]
[0035] The results in Tables 1 and 2 show that the ionic liquid for heavy metal recovery of the present invention is superior in heavy metal recovery to the comparative example. In addition, it is recyclable and has excellent stability after recovery, so it can be used repeatedly to recover heavy metals. [Industrial Applicability]
[0036] The ionic liquid for heavy metal recovery of the present invention can be applied to the recovery of various compositions containing heavy metals and various heavy metal-containing compounds. For example, cobalt can be recovered from a positive electrode material (lithium cobalt oxide) removed from a used lithium ion secondary battery. It may also be isolated as a cobalt salt. In addition, the ionic liquid for heavy metal recovery of the present invention can be recycled and is (chemically) stable even after recovery, and therefore can be reused.
Claims
1. The ionic liquid for heavy metal recovery is composed of an imidazolium cation (CA) and an anion (AN) represented by the following general formula (1): R-C(=O)O - (1) [In general formula (1), R is a residue obtained by removing one carboxyl group from a dicarboxylic acid having 2 to 10 carbon atoms, a residue obtained by removing one carboxyl group from a monocarboxylic acid having a β-dicarbonyl structure having 3 to 6 carbon atoms, or a residue obtained by removing one carboxyl group from a tricarboxylic acid having 4 to 6 carbon atoms.]
2. 2. The ionic liquid for heavy metal recovery according to claim 1, wherein the imidazolium cation (CA) is at least one selected from the group consisting of 1-ethyl-3-methylimidazolium and 1-butyl-3-methylimidazolium.
3. The ionic liquid for heavy metal recovery according to claim 1, wherein the dicarboxylic acid having 2 to 10 carbon atoms, the monocarboxylic acid having a β-dicarbonyl structure having 3 to 6 carbon atoms, or the tricarboxylic acid having 4 to 6 carbon atoms is at least one selected from the group consisting of acetopyruvic acid, diacetoacetic acid, malonic acid, succinic acid, and citric acid.
4. 2. The ionic liquid for heavy metal recovery according to claim 1, wherein the heavy metal is at least one selected from the group consisting of cobalt, nickel and manganese.
Citation Information
Patent Citations
Computer-readable recording medium in which program for video game is recorded, program for video game, and method and device for processing video game