Method and system for producing refined hydrocarbon from waste plastics

The method addresses the impurity issues in waste plastic pyrolysis oil by employing a multi-step process with a high-temperature filter and demulsification to produce high-value, refined hydrocarbons with improved yield and reduced impurities, suitable for petroleum refining.

JP2024155735APending Publication Date: 2024-10-31SK INNOVATION CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024029054
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-09-21
Filing Date
2024-02-28
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Waste plastic pyrolysis oil contains high levels of impurities such as chlorine, nitrogen, and metals, leading to equipment corrosion, process inefficiencies, and limited use in high-value fuels due to the formation of ammonium salts and impurity particles, which complicates hydrodesulfurization and hydrogenation processes.

Method used

A method and system involving pretreatment, pyrolysis, lightening, dehydration, and distillation steps, using a high-temperature filter filled with beads and a temperature gradient, along with demulsification and hydrogenation, to produce refined hydrocarbons with reduced impurities and improved yield.

Benefits of technology

The process effectively reduces impurities, enhances the yield of light hydrocarbons, and maintains catalyst activity, allowing the production of high-value pyrolysis oil suitable for blending with petroleum products and use in petroleum refining processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155735000001_ABST
    Figure 2024155735000001_ABST
Patent Text Reader

Abstract

To provide a method and a system for producing a refined hydrocarbon from waste plastics.SOLUTION: There is provided a method for producing a refined hydrocarbon from waste plastics which comprises: a pretreatment step of pretreating waste plastics; a pyrolysis step of feeding the waste plastics pretreated in the pretreatment step into a pyrolysis reactor to produce pyrolysis gas; a lightening step of feeding the pyrolysis gas into a hot filter to produce a pyrolysis oil; a dehydration step of applying voltage to a first mixture obtained by mixing the produced pyrolysis oil with washing water and a demulsifier for dehudration; a hydrogenation step of hydrogenating a second mixture obtained by mixing the dehydrated first mixture and a sulfur source to produce a refined pyrolysis oil from which impurities are removed; and a distillation step of distilling the refined pyrolysis oil to obtain a refined hydrocarbon, wherein a liquid condensed by the hot filter is re-fed into the pyrolysis reactor.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method and system for producing refined hydrocarbons from waste plastics. [Background technology]

[0002] Pyrolysis oil produced through the cracking and thermal decomposition of waste materials such as waste plastic pyrolysis oil contains a large amount of impurities originating from the waste materials, and when used as fuel, it may emit air pollutants such as SOx and NOx. In particular, there is a problem that chlorine components are converted into hydrogen chloride during the high-temperature treatment process, which may cause corrosion of equipment, and then emitted. In addition, compared to oil produced from crude oil using conventional methods, waste plastic pyrolysis oil contains a high amount of impurities such as chlorine, nitrogen, and metals, so it can only be blended in limited amounts with high-value-added fuels such as gasoline and diesel, and must go through a refining process in order to use it in large quantities.

[0003] In the past, impurities such as chlorine, nitrogen, and metals were removed through post-treatment processes such as hydrodesulfurization and hydrogen chloride treatment using oil refining technology. However, since pyrolysis oil such as waste plastic pyrolysis oil contains a high content of chlorine, problems such as equipment corrosion, abnormal reactions, and deterioration of product properties have been reported due to the generation of excess hydrogen chloride in the hydrodesulfurization process, making it difficult to introduce untreated pyrolysis oil into the hydrodesulfurization process.

[0004] In addition, when oil and hydrogen are reacted in the presence of a hydrotreating catalyst as in the conventional technology, chlorine compounds such as hydrogen chloride, which are produced together with the refined oil, react with nitrogen compounds to produce ammonium salts (NH4Cl), which cause various process problems. Specifically, the ammonium salts produced inside the reactor when oil reacts with hydrogen not only cause corrosion of the reactor and reduce its durability, but also cause various process problems such as the generation of differential pressure, which in turn reduces process efficiency. In addition, if the process is operated for a long period of time, impurity particles in the waste plastic pyrolysis oil stick to the inside of the reactor, which also causes various process problems.

[0005] Therefore, there is a demand for technology that can prevent or minimize the production of ammonium salts (NH4Cl) during the refining process of waste plastic pyrolysis oil, which contains impurities such as chlorine and nitrogen, and prevent the phenomenon of impurity particles adhering inside the reactor.

[0006] In addition to removing impurities, there is a need to increase the yield of waste plastic pyrolysis oil and to add value to it by making it lighter in order to ensure economic viability.

[0007] In addition, there is a demand for technological development that can obtain refined hydrocarbons with a high ratio of light hydrocarbons from the waste plastic pyrolysis oil. Summary of the Invention [Problem to be solved by the invention]

[0008] According to one embodiment of the present disclosure, high value-added pyrolysis oil with a high proportion of light hydrocarbons can be produced from waste plastics containing a large amount of impurities, and refined hydrocarbons with a high proportion of light hydrocarbons can be obtained from the oil.

[0009] According to another aspect of the present disclosure, the yield of pyrolysis oil obtained from waste plastics can be improved.

[0010] According to another aspect of the present disclosure, high value-added pyrolysis oil with reduced impurities can be produced from waste plastics containing a large amount of impurities, and refined hydrocarbons with reduced impurities can be obtained therefrom.

[0011] According to another aspect of the present disclosure, a method and apparatus can be provided that simplifies the process of producing refined hydrocarbons from waste plastics.

[0012] According to one aspect of the present disclosure, it is possible to produce a high-value-added pyrolysis oil that is of excellent quality and can be blended with existing petroleum products or used as a feedstock in an oil refining process, from which refined hydrocarbons can be obtained.

[0013] According to another aspect of the present disclosure, there can be provided a method and system for producing refined hydrocarbons from waste plastics that minimizes the generation of ammonium salts (NH4Cl) from waste plastic pyrolysis oil containing impurities such as chlorine and nitrogen.

[0014] According to one aspect of the present disclosure, it is possible to provide a method and system for producing refined hydrocarbons from waste plastics, in which catalyst activity is maintained for a long period of time, purification efficiency is excellent, and operation for a long period of time is possible.

[0015] According to another aspect of the present disclosure, it is possible to provide a method and a system for producing refined hydrocarbons from waste plastics, which can prevent the adhesion phenomenon of impurity particles.

[0016] According to another aspect of the present disclosure, there can be provided a method and system for producing refined hydrocarbons from waste plastics, which have extremely low impurity contents such as chlorine, nitrogen, oxygen, metals, and the like, and olefin contents, are of excellent quality, and can be used as a blend with existing petroleum products or as a raw material for petroleum refining and petrochemical processes. [Means for solving the problem]

[0017] The present disclosure can provide a method for producing refined hydrocarbons from waste plastics, the method including: a pretreatment step for pretreating waste plastics; a pyrolysis step for feeding the waste plastics pretreated in the pretreatment step into a pyrolysis reactor to produce a pyrolysis gas; a lightening step for feeding the pyrolysis gas into a hot filter to produce a pyrolysis oil; a dehydration step for applying a voltage to a first mixed liquid obtained by mixing the produced pyrolysis oil with wash water and a demulsifier to dehydrate it; a hydrotreatment step for hydrotreating a second mixed liquid obtained by mixing the dehydrated first mixed liquid with a sulfur source to produce a refined pyrolysis oil from which impurities have been removed; and a distillation step for distilling the refined pyrolysis oil to obtain refined hydrocarbons, the liquid condensed in the hot filter being re-introduced into the pyrolysis reactor.

[0018] In one embodiment according to the present disclosure, the high temperature filter can be packed with beads.

[0019] In one embodiment according to the present disclosure, the beads may include at least one selected from the group consisting of silica sand (SiO2) and aluminum oxide (Al2O3).

[0020] In one aspect of the present disclosure, the method for producing refined hydrocarbons from waste plastics may include forming a temperature gradient in the high-temperature filter.

[0021] In one embodiment of the present disclosure, the temperature gradient may be created by providing at least two heaters on the outside of the hot filter.

[0022] In one embodiment according to the present disclosure, the pyrolysis reactor may include at least two batch reactors.

[0023] In one embodiment according to the present disclosure, the pyrolysis step may be carried out by switching between the at least two batch reactors.

[0024] In one embodiment according to the present disclosure, the refined pyrolysis oil may be blended with petroleum hydrocarbons and distilled into a blended oil.

[0025] In one embodiment of the present disclosure, the refined pyrolysis oil may be contained in an amount of 50% by weight or less based on the total weight of the mixed oil.

[0026] In one embodiment according to the present disclosure, the waste plastic may include at least one selected from the group consisting of polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyvinyl chloride (PVC), and polystyrene (PS).

[0027] In one aspect of the present disclosure, in the method for producing refined hydrocarbons from waste plastics, the pyrolysis oil may be mixed in a larger amount than the wash water in the dehydration step.

[0028] In one aspect of the present disclosure, in the method for producing refined hydrocarbons from waste plastics, in the dehydration step, the first mixed liquid may be a mixture of the pyrolysis oil and the wash water in a volume ratio of 1:0.001 to 0.5.

[0029] In one aspect of the present disclosure, in the method for producing refined hydrocarbons from waste plastics, in the dehydration step, the first mixed liquid may be a mixture of the pyrolysis oil and the demulsifier in a volume ratio of 1:0.000001 to 0.001.

[0030] In one embodiment according to the present disclosure, the demulsifier may be one or a mixture of two or more selected from the group consisting of polyethylene glycol, tert-butanol, acetone, alkyl naphthalene sulfonate, alkyl benzene sulfonate, non-ionic alkoxylated alkyl phenol resin, polyalkylene oxide, and polyoxyethylene sorbitan ester.

[0031] The present disclosure also provides a system for producing refined hydrocarbons from waste plastics, the system including: a pretreatment device for pretreating waste plastics; a pyrolysis reactor for producing pyrolysis gas by inputting the waste plastics pretreated in the pretreatment device; a hot filter for producing pyrolysis oil by inputting the pyrolysis gas; a connection pipe for connecting the high-temperature filter and the pyrolysis reactor so that the liquid condensed in the high-temperature filter is re-introduced into the pyrolysis reactor; a dehydration device for applying a voltage to a first mixed liquid obtained by mixing the produced pyrolysis oil with wash water and a demulsifier to dehydrate the first mixed liquid; a hydrotreatment device for hydrotreating a second mixed liquid obtained by mixing the dehydrated first mixed liquid with a sulfur source to produce refined pyrolysis oil from which impurities have been removed; and a distillation device for distilling the refined pyrolysis oil to obtain refined hydrocarbons.

[0032] In one embodiment according to the present disclosure, the high temperature filter may be filled with beads.

[0033] In one embodiment according to the present disclosure, the beads may include at least one selected from the group consisting of silica sand (SiO2) and aluminum oxide (Al2O3).

[0034] In one embodiment according to the present disclosure, the production system may include at least two heaters external to the high temperature filter. Effect of the Invention

[0035] A method and system for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure can produce high value-added pyrolysis oil with a high proportion of light hydrocarbons from waste plastics containing a large amount of impurities, from which refined hydrocarbons with a high proportion of light hydrocarbons can be obtained.

[0036] The method and system for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure can improve the yield of pyrolysis oil obtained from waste plastics.

[0037] A method and system for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure can produce high-value-added pyrolysis oil with reduced impurities from waste plastics containing a large amount of impurities, from which refined hydrocarbons with reduced impurities can be obtained.

[0038] A method and system for producing refined hydrocarbons from waste plastics according to another aspect of the present disclosure can simplify the process of producing refined hydrocarbons from waste plastics.

[0039] The method and system for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure can produce high-value-added pyrolysis oil that is of excellent quality and has a high proportion of light hydrocarbons that can be blended with existing petroleum products or used as a feedstock for petroleum refining processes, from which refined hydrocarbons with a high proportion of light hydrocarbons can be obtained.

[0040] The method and system for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure can prevent or minimize the production of ammonium salts (NH4Cl) during the purification of waste plastic pyrolysis oil containing impurities such as chlorine and nitrogen, thereby preventing the adhesion of impurity particles.

[0041] The method and system for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure has the advantage of being excellent in purification efficiency and enabling long-term operation of the process because it prevents catalyst deactivation due to moisture.

[0042] The method and system for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure can provide waste plastic pyrolysis oil that has very low impurity contents such as chlorine, nitrogen, oxygen, metals, and the like, and olefin contents, is of excellent quality, and can be used as a blend with existing petroleum products or as a raw material for petroleum refining and petrochemical steps.

[0043] The process and system for producing refined hydrocarbons from waste plastics according to embodiments of the present disclosure can be used to produce eco-friendly petrochemical products using waste plastics. [Brief description of the drawings]

[0044] [Figure 1] FIG. 1 is a process diagram for producing waste plastic pyrolysis oil according to one embodiment of the present disclosure. [Diagram 2] 1 is a diagram of a high temperature filter according to one embodiment of the present disclosure. [Diagram 3] FIG. 2 is a flow diagram of the dehydration and hydrotreating steps according to one embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0045] The advantages and features of the present disclosure, as well as the methods for achieving them, will become apparent from the following detailed examples. However, the present disclosure is not limited to the following examples, and may be implemented in various different forms. The following examples are provided solely for the purpose of making the disclosure complete and fully conveying the category of the present invention to those skilled in the art to which the disclosure pertains, and the present disclosure is only defined by the category of claims.

[0046] Unless otherwise defined, all terms (including technical and scientific terms) used herein can be used with the meaning commonly understood by one of ordinary skill in the art to which this disclosure belongs.

[0047] As used herein, the singular forms of the terms "a," "an," and "the" can be construed as including the plural forms as well, unless otherwise indicated.

[0048] Numerical ranges used herein include lower and upper limits and all values ​​within that range, increments that are logically derived from the shape and width of the ranges defined, all doubly limited values, and all possible combinations of upper and lower limits of differently limited numerical ranges. Unless otherwise specified in the specification of this disclosure, values ​​outside the numerical ranges that may occur due to experimental error or rounding of values ​​are also included in the defined numerical ranges.

[0049] As referred to in this specification, "comprising" is an open-ended term having the same meaning as terms such as "comprising," "containing," "having," "characterized," and the like, and does not exclude further unrecited elements, materials, or steps.

[0050] Unless otherwise specified in this specification, the unit of % means % by weight unless otherwise defined.

[0051] In this specification, "A to B" means "A or more and B or less" unless otherwise specified.

[0052] As used herein, the term "pyrolysis oil yield" refers to the weight ratio of oil to the total weight of oil, aqueous by-products, pyrolysis residue (Char) and by-product gas among the products of the pyrolysis step.

[0053] As used herein, the term "vertical electrode" can mean an electrode that is erected vertically relative to the ground, and "horizontal electrode" can mean an electrode that is placed horizontally relative to the ground.

[0054] The method and system for producing refined hydrocarbons from waste plastics according to the present disclosure will be described in detail below, but this is merely an example and is not limited to the specific embodiment described by way of example in the present disclosure.

[0055] The present disclosure provides a method for producing refined hydrocarbons from waste plastics, the method including: a pretreatment step of pretreating waste plastics; a pyrolysis step of feeding the waste plastics pretreated in the pretreatment step into a pyrolysis reactor to produce a pyrolysis gas; a lightening step of feeding the pyrolysis gas into a hot filter to produce a pyrolysis oil; a dehydration step of applying a voltage to a first mixed liquid obtained by mixing the produced pyrolysis oil with wash water and a demulsifier to dehydrate it; a hydrotreatment step of hydrotreating a second mixed liquid obtained by mixing the dehydrated first mixed liquid with a sulfur source to produce a refined pyrolysis oil from which impurities have been removed; and a distillation step of distilling the refined pyrolysis oil to obtain refined hydrocarbons, in which the liquid condensed in the hot filter is re-introduced into the pyrolysis reactor.

[0056] Therefore, the method for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure can produce high value-added pyrolysis oil with a high ratio of light hydrocarbons from waste plastics containing a large amount of impurities, thereby obtaining refined hydrocarbons with a high ratio of light hydrocarbons. Also, the yield of the obtained pyrolysis oil can be significantly improved.

[0057] In addition, the method for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure can produce high value-added pyrolysis oil with reduced impurities from waste plastics containing a large amount of impurities, and refined hydrocarbons with reduced impurities can be obtained therefrom.

[0058] In the method for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure, the liquid condensed in the high-temperature filter is reintroduced into the pyrolysis reactor, thereby improving the cracking of heavy hydrocarbons in the pyrolysis oil, and thus a pyrolysis oil having a high ratio of light hydrocarbons can be produced, from which refined hydrocarbons having a high ratio of light hydrocarbons can be obtained.

[0059] According to another aspect of the present disclosure, the high-temperature filter may be filled with beads. When the high-temperature filter is filled with beads, the inert effect and heat transfer effect in the high-temperature filter are maximized, and pyrolysis oil having a high proportion of light hydrocarbons can be produced. In addition, the yield of the pyrolysis oil can be improved.

[0060] According to one embodiment of the present disclosure, the beads may be filled in the high-temperature filter at 50 vol% or more, 60 vol% or more, 70 vol% or more, 80 vol% or more, 85 vol% or more, 90 vol% or more, 95 vol% or less, 93 vol% or less, 91 vol% or less, 90 vol% or less, 89 vol% or less, 87 vol% or less, 85 vol% or less, 80 vol% or less, or a value between the above values, based on the internal volume of the high-temperature filter. Specifically, the beads may be filled in the high-temperature filter at 70 to 95 vol%, 80 to 90 vol%, or 85 to 90 vol% based on the internal volume of the high-temperature filter, but are not limited thereto.

[0061] According to one embodiment of the present disclosure, a temperature gradient may be formed in the high-temperature filter. When a temperature gradient is formed in the high-temperature filter, pyrolysis gas moving to the upper stage in the high-temperature filter and liquid condensing in the lower stage are efficiently circulated, and pyrolysis oil with a high ratio of light hydrocarbons can be produced. This also allows refined hydrocarbons with a high ratio of light hydrocarbons to be produced. In addition, the yield of the pyrolysis oil can be improved.

[0062] According to one aspect of the present disclosure, the temperature gradient may be such that the temperature of the lower stage of the high-temperature filter is higher than the temperature of the upper stage of the high-temperature filter. According to another aspect of the present disclosure, the temperature gradient may be such that the temperature of the lower stage of the high-temperature filter is higher than the temperature of the middle stage of the high-temperature filter, and the temperature of the middle stage of the high-temperature filter is higher than the temperature of the upper stage of the high-temperature filter. This can improve the circulation efficiency and heat transfer efficiency within the high-temperature filter.

[0063] According to one embodiment of the present disclosure, the temperature gradient can be formed by providing at least two heaters outside the high-temperature filter. According to another embodiment of the present disclosure, the temperature gradient can be formed by providing at least three heaters outside the high-temperature filter. When at least two heaters are provided outside the high-temperature filter, the temperature gradient of the high-temperature filter can be easily formed, and the temperatures of the upper, middle, and lower stages can be flexibly adjusted according to the operating conditions of the high-temperature filter, allowing for flexible process operation.

[0064] According to one embodiment of the present disclosure, the temperature of the lower stage of the high temperature filter may be 400°C or more, 420°C or more, 440°C or more, 460°C or more, 480°C or more, 500°C or more, 550°C or more, or 600°C or more.

[0065] According to one embodiment of the present disclosure, the temperature of the upper stage of the high temperature filter may be 600°C or less, 550°C or less, 500°C or less, 480°C or less, 460°C or less, 440°C or less, 420°C or less, or 400°C or less.

[0066] According to one embodiment of the present disclosure, the temperature of the middle stage of the high-temperature filter may be 300°C or more and 600°C or less, 400°C or more and 600°C or less, 400°C or more and 500°C or less, 420°C or more and 480°C or less, or 440°C or more and 460°C or less.

[0067] According to one embodiment of the present disclosure, the pretreatment step may include a) reacting the waste plastic with a neutralizing agent, and b) reacting the product of step a) with a copper compound. This allows the pretreatment step to treat the waste plastic raw material to reduce the Cl content to a level that can be introduced into the purification step.

[0068] According to one embodiment of the present disclosure, in addition to the copper compound, additives or neutralizing agents such as metal oxides and zeolites may be used in step b. The metal oxides may be in the form of oxides of divalent metals, but are not limited thereto.

[0069] The waste plastic may include at least one selected from the group consisting of polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyvinyl chloride (PVC) and polystyrene (PS). The waste plastic may include organic chlorine (organic Cl), inorganic chlorine (inorganic Cl) and aromatic chlorine (aromatic Cl), and the chlorine content of the waste plastic may be 10 ppm or more, 50 ppm or more, 100 ppm or more, or 100 to 1,000 ppm, but the present disclosure is not limited thereto. A large amount of impurities resulting from the waste plastic are contained in pyrolysis oil generated through cracking and pyrolysis reaction of waste plastic, such as waste plastic pyrolysis oil. In particular, it is necessary to remove chlorine components such as organic / inorganic chlorine by pretreating the pyrolysis oil. The waste plastic may be classified into household waste plastic and industrial waste plastic. Domestic waste plastic is a plastic in which PVC, PS, PET, PBT, etc. other than PE and PP are mixed, and in the present disclosure, it may mean a mixed waste plastic containing 3% by weight or more of PVC together with PE and PP. Chlorine derived from PVC has a high ratio of organic Cl and inorganic Cl, and Cl in household waste plastics can be removed with high efficiency even with inexpensive neutralizing agents (Ca-, Zn-, Al-based). Industrial waste plastics are mostly PE / PP, but they contain a high amount of organic Cl due to adhesives or dye components, and the ratio of Cl (aromatic chlorine) contained in aromatic rings is particularly high, which makes them difficult to remove with the aforementioned general inexpensive neutralizing agents.

[0070] The present disclosure is characterized in that it removes 95% by weight or more, 97% by weight or more, 98% by weight or more, or 99% by weight or more of chlorine based on the total weight of chlorine contained in waste plastics derived from waste plastics. For this purpose, it is preferable to remove chlorine contained in aromatic rings.

[0071] The step a) is a step in which waste plastic is reacted with a neutralizing agent, and a large amount of hydrogen chloride generated during the melting and thermal decomposition process of PVC, etc. can be removed in the form of neutralized salt.

[0072] The neutralizing agent may include a metal oxide, hydroxide, carbonate, or a combination thereof, and the metal may be calcium, aluminum, magnesium, zinc, copper, iron, or a combination thereof. Specifically, the neutralizing agent may be copper oxide, aluminum oxide, calcium oxide, magnesium oxide, zinc oxide, or iron oxide. The neutralizing agent may include a zeolite component. Specifically, the neutralizing agent may include a spent FCC catalyst (E-cat) containing a zeolite component, and the metal oxide may further include a spent FCC catalyst. Specifically, the neutralizing agent may be calcium oxide, spent FCC catalyst, copper metal, or copper oxide, or may be calcium oxide.

[0073] In one aspect according to the present disclosure, the neutralizing agent may be added during the pyrolysis step.

[0074] The neutralizing agent may be mixed in an amount of 0.5 to 20% by weight, 1 to 10% by weight, or 1 to 5% by weight based on the total weight of the waste plastic. In addition, the ... M / N Cl ) 1 to 25, specifically 0.7 to 15, and more specifically 0.5 to 5.

[0075] Meanwhile, the total moles of chlorine (Cl) in the waste plastics may refer to the total moles of chlorine in the waste plastics solid raw material before pretreatment and pyrolysis.

[0076] In the a) chlorine removal step, the weight ratio (A1 / A) of the chlorine in the product of the a) step to the chlorine content (A) of the waste plastic (100% by weight) may be 50% or less, 40% or less, or 20-30%. Chlorine remaining in the waste plastic after the a) step can be effectively removed in the b) step.

[0077] Step b) is a step in which the product of step a) is reacted with a copper compound, and a small amount of organic chlorine and aromatic chlorine that was not removed in step a) can be removed by the copper compound (catalyst). When the copper compound is used together with the neutralizing agent in step a) or is used to replace the neutralizing agent, the copper compound reacts first with chlorine located at the end of the hydrocarbon chain among organic chlorine and inorganic chlorine (hydrogen chloride), and it may be difficult to contact aromatic chlorine, which is difficult to remove with the neutralizing agent. In addition, at the time of initial pyrolysis when the temperature inside the reactor is raised for pretreatment or pyrolysis, hydrogen chloride begins to be generated at a relatively low temperature (250 to 300 ° C), so it is desirable to remove chlorine preferentially with a neutralizing agent. After that, when the full-scale pyrolysis step proceeds, the temperature is relatively high and the reaction of removing aromatic chlorine is activated. For this reason, it is effective to first remove organic Cl and inorganic Cl with hydrogen chloride using a neutralizing agent, and then remove aromatic chlorine with a copper compound.

[0078] The copper compound may include at least one selected from the group consisting of copper metal (Cu), copper oxide (CuO), copper hydroxide (Cu(OH)2) and copper carbonate (CuCO3), and may specifically include copper metal (Cu) and / or copper oxide (CuO).

[0079] The copper compound may be mixed in an amount of 0.1 to 20% by weight, 0.5 to 10% by weight, or 1 to 5% by weight based on the total weight of the product of step a). ... molar ratio (N Cu / N Cl ) 1 to 10, specifically 0.7 to 5, and more specifically 0.5 to 3.

[0080] Meanwhile, the total moles of chlorine (Cl) in the waste plastics may refer to the total moles of chlorine in the waste plastics solid raw material before pretreatment and pyrolysis.

[0081] In the b) chlorine removal step, the chlorine content ratio (A2 / A) of the product of the b) step to the chlorine content of the waste plastic (100% by weight) (A) may be 10% or less, 5% or less, or 0.5 to 3%.

[0082] According to one embodiment of the present disclosure, the step a) can be carried out at a temperature of 200 to 320° C., and the step b) can be carried out at a temperature of 400 to 550° C. When steps a) and b) are carried out in the respective temperature ranges, chlorine in the waste plastic can be effectively removed.

[0083] According to one embodiment of the present disclosure, the pyrolysis step may include a) reacting waste plastic with a neutralizing agent, and b) reacting the product of step a) with a copper compound.

[0084] In the present disclosure, the pretreatment step may further include a pulverization step of feeding waste plastics into a screw reactor and pulverizing the waste plastics. The pulverization of the waste plastics may be performed by applying a pulverization step known in the art, for example, feeding the waste plastics into a pretreatment reactor and heating it to about 300° C. to produce a pellet-shaped hydrocarbon flow precursor, but the present disclosure is not limited thereto.

[0085] According to one aspect of the present disclosure, the grinding step may be carried out at room temperature.

[0086] For example, the pulverization step may involve mixing the waste plastic with a neutralizing agent and feeding the mixture into the pre-treatment reactor. When the waste plastic is mixed with calcium oxide or the like as the neutralizing agent and pulverized at room temperature, a mechanochemical reaction occurs to generate hydrocarbons and CaOHCl, which has the effect of stably fixing chlorine in the waste plastic raw material with CaOHCl.

[0087] The pretreatment step may then involve feeding the pulverized waste plastic into a pretreatment reactor, heating the pulverized waste plastic, and physically and chemically treating the solid waste plastic raw material to remove chlorine, thereby producing a hydrocarbon flow precursor (pyrolysis raw material). The hydrocarbon flow precursor refers to a waste plastic melt, and the waste plastic melt may refer to a material in which all or a part of pulverized or unpulverized solid waste plastic is converted into liquid waste plastic.

[0088] For example, the pretreatment step may include heating the crushed or uncrushed waste plastic and the neutralizing agent in a pretreatment reactor. Also, the pretreatment step may include heating the crushed or uncrushed waste plastic and the neutralizing agent in a pretreatment reactor, and then heating the first pretreatment step (heating), followed by adding a copper compound to the pretreatment reactor.

[0089] The heating may be performed at a temperature of 200 to 320° C. under normal pressure conditions. Specifically, the heating may be performed at a temperature of 250 to 320° C. or 280 to 300° C. In general, the pretreatment temperature for waste plastics is at least 250° C., but the dechlorinated hydrocarbons can be easily pretreated at a lower temperature of 200° C. to generate hydrogen or methane gas.

[0090] The pretreatment reactor may be an extruder, an autoclave reactor, a batch reactor, or the like, and may be an auger reactor, for example, but the present disclosure is not limited thereto.

[0091] The pyrolysis step involves feeding pyrolysis raw materials, which are classified into three phases, namely, gas phase, liquid phase (oil + wax + water), and solid phase, into a pyrolysis reactor. Specifically, this is a step of feeding the non-pretreated or pretreated waste plastic into a pyrolysis reactor and heating it.

[0092] For example, the pyrolysis step may be a step of mixing pretreated waste plastic and a copper compound, feeding the mixture into a pyrolysis reactor, and heating the mixture. The pyrolysis step may be a step of carrying out at least two pyrolysis steps, either continuously or discontinuously, by carrying out a first pyrolysis step of mixing waste plastic and a neutralizing agent, feeding the mixture into a pyrolysis reactor, and heating the mixture, and then carrying out a second pyrolysis step of feeding a copper compound into the pyrolysis reactor and heating the mixture.

[0093] The heating may be performed in a non-oxidizing atmosphere at a temperature of 320 to 900° C., specifically 350 to 700° C., more specifically 400 to 550° C. The heating may be performed at normal pressure. The non-oxidizing atmosphere is an atmosphere in which the waste plastic is not oxidized (burned), and may be, for example, an atmosphere in which the oxygen concentration is adjusted to 1% by volume or less, or an atmosphere of an inert gas such as nitrogen, water vapor, carbon dioxide, or argon.

[0094] If the heating temperature is 400°C or higher, it is possible to prevent chlorine-containing plastics from fusing; conversely, if the heating temperature is 550°C or lower, the chlorine in the waste plastic can remain in the pyrolysis residue (Char) in the form of CaCl2, CuCl2, etc.

[0095] The pyrolysis reactor may be an autoclave reactor, a batch stirred reactor, a fluidized-bed reactor, a packed-bed reactor, or the like. Specifically, the pyrolysis reactor may be any reactor capable of stirring and temperature control. According to one embodiment of the present disclosure, the pyrolysis reactor may be a batch reactor.

[0096] According to one embodiment of the present disclosure, the pyrolysis reactor may include at least two batch reactors.

[0097] According to one embodiment of the present disclosure, the pyrolysis step may be performed by switching between the at least two batch reactors, thereby ensuring the continuity of the pyrolysis step even at high temperatures.

[0098] In the method for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure, the pyrolysis step or the lightening step may further include at least one step selected from the group consisting of a pyrolysis gas recovery step of recovering the pyrolysis gas phase and the pyrolysis liquid phase as gas, and a separation step of separating the pyrolysis solid phase (solid content) into fine particles and granulated material.

[0099] In the gas recovery step, pyrolysis gas containing low boiling point hydrocarbon compounds such as methane, ethane, and propane is recovered from the gas phase generated in the pyrolysis step or the lightening step. The pyrolysis gas can generally contain combustible substances such as hydrogen, carbon monoxide, and low molecular weight hydrocarbon compounds. Examples of the hydrocarbon compounds include methane, ethane, ethylene, propane, propene, butane, and butene. These pyrolysis gases contain combustible substances and can be used as fuel.

[0100] In the separation step, the solid matter in the solid phase generated in the pyrolysis step or the lightening step, for example, the carbide and the neutralizing agent and / or the copper compound, can be separated into fine particles and granules. Specifically, the solid matter generated in the pyrolysis reaction can be separated into fine particles and granules by classifying using a sieve that is smaller than the average particle size of the chlorine-containing plastic and larger than the average particle size of the neutralizing agent and the copper compound. In the separation step, it is preferable to separate the solid matter into fine particles containing a relatively large amount of the chlorine-containing neutralizing agent and the copper compound, and granules containing a relatively large amount of the carbide. The fine particles and the carbide can be reprocessed as necessary and reused in the pyrolysis step, used as fuel, or disposed of, and the present disclosure is not limited thereto.

[0101] According to one embodiment of the present disclosure, the high-temperature filter may be filled with at least one selected from the group consisting of beads and a neutralizing agent.

[0102] According to another embodiment of the present disclosure, the high-temperature filter may be filled with beads. When the high-temperature filter is filled with beads, the inert effect and heat exchange effect in the high-temperature filter are maximized, and pyrolysis oil having a high proportion of light hydrocarbons can be produced.

[0103] According to one embodiment of the present disclosure, the beads may contain at least one selected from the group consisting of silica sand (SiO2) and aluminum oxide (Al2O3). Specifically, when the beads contain silica sand (SiO2), the inert effect and heat exchange effect in the high-temperature filter are maximized, and stable process operation is possible without wear even during long-term high-temperature operation.

[0104] According to one aspect of the present disclosure, the beads may be, but are not limited to, glass beads.

[0105] According to one embodiment of the present disclosure, the diameter of the beads can be 0.1 mm or more, 1 mm or more, 1.5 mm or more, 2 mm or more, 2.5 mm or more, 3 mm or more, 10 mm or less, 8 mm or less, 6 mm or less, 4 mm or less, 3.5 mm or less, 3 mm or less, 2.5 mm or less, 2 mm or less, or a value between the above values, specifically, 1 mm to 5 mm, 2 mm to 4 mm, 2.5 mm to 3.5 mm, but is not limited thereto. By filling the high-temperature filter with beads having the above particle diameter in the lightening step of the present disclosure, not only can the residence time (GHSV) of the pyrolysis gas be adjusted to achieve lightening of the oil content, but also the generation of a differential pressure in the high-temperature filter can be suppressed to improve the process operation efficiency.

[0106] According to one embodiment of the present disclosure, in the lightening step, the pyrolysis gas may be fed into a hot filter filled with the neutralizing agent to produce a pyrolysis oil.

[0107] The lightening step is carried out in an oxygen-free atmosphere at a temperature of 400 to 550°C and a pressure of normal pressure to 0.5 bar, and the oxygen-free atmosphere can be an inert gas atmosphere or an oxygen-free closed system atmosphere. In the temperature range of the lightening step, the lightening of the pyrolysis gas proceeds well, and the clogging phenomenon caused by wax and the generation of differential pressure can be improved.

[0108] Meanwhile, the lightening step may be a GHSV (gas volumetric flow rate) of 0.3 to 1.2 / hr or 0.5 to 0.8 / hr. This allows the waste plastic pyrolysis product to be lightened and impurities (such as Cl) to be reduced without a separate post-treatment step, and the residence time of the pyrolysis gas (GHSV) can be adjusted to produce pyrolysis oil with a high proportion of light hydrocarbons and refined hydrocarbons with a high proportion of light hydrocarbons as intended in the present disclosure.

[0109] The neutralizing agent filled in the high-temperature filter may have a particle size of 400 to 900 μm, or may have a particle size of 500 to 800 μm. In the operating conditions of the lightening step of the present disclosure, by filling the high-temperature filter with a neutralizing agent having the above particle size, it is possible to adjust the residence time (GHSV) of the pyrolysis gas to achieve lightening of the oil content, and also to suppress the generation of a differential pressure in the high-temperature filter, thereby improving the process operating efficiency.

[0110] Meanwhile, the particle size refers to D50, which means the particle size at which the cumulative volume is 50% from the smallest particle size in particle size distribution measurement by laser scattering method. Here, D50 can be measured by taking a sample of the produced carbonaceous material according to KS A ISO13320-1 standard and measuring the particle size distribution using Malvern's Mastersizer3000. Specifically, the volume density may be measured after dispersing the sample using ethanol as a solvent and an ultrasonic disperser as necessary.

[0111] According to one aspect of the present disclosure, the high temperature filter may be filled with the beads and the neutralizing agent.

[0112] In the art, a high-temperature filter generally serves to separate gas and residue (Char) from the products of the thermal cracking step. In the present disclosure, a high-temperature filter filled with at least one selected from the group consisting of beads and a neutralizing agent is used to remove impurities such as chlorine while lightening the fuel, and the operating conditions such as the temperature of the high-temperature filter and the particle size of the neutralizing agent are adjusted to a specific range as described above.

[0113] The lightening step may satisfy the following Relational Formula 1 and Relational Formula 2.

[0114] [Equation 1] 50<(A2-A1) / A1(%)<100

[0115] [Equation 2] 80<(B2-B1 / B1)(%)<-50

[0116] In the above-mentioned relational formula 1, A1 is the total amount (wt%) of naphtha (boiling point to 150°C) and kerosene (boiling point 150 to 265°C) in the pyrolysis gas, and A2 is the total amount (wt%) of naphtha (bp to 150°C) and kerosene (bp 150 to 265°C) in the pyrolysis oil. In the above-mentioned relational formula 2, B1 is the chlorine content (ppm) of the pyrolysis gas, and B2 is the chlorine content (ppm) of the pyrolysis oil.

[0117] Specifically, the above-mentioned relations 1 and 2 may be 60<(A2-A1) / A1(%)<90, 65<(A2-A1) / A1(%)<85, or 70<(A2-A1) / A1(%)<80, and may be -75<(B2-B1 / B1)(%)<-55, -70<(B2-B1 / B1)(%)<-55, or -65<(B2-B1 / B1)(%)<-55.

[0118] The above-mentioned Relational Equations 1 and 2 numerically show the degree of lightening and heaviening of waste plastic pyrolysis products by using a high-temperature filter filled with at least one selected from the group consisting of beads and neutralizing agents of the present disclosure. The present disclosure has a technical feature in that pyrolysis oil with a high ratio of light hydrocarbons is produced by adjusting the oil composition and chlorine content of the pyrolysis gas fed into the high-temperature filter and the chlorine-containing oil / inorganic substance.

[0119] The pyrolysis oil produced in the lightening step may contain 30-50 wt% naphtha (bp~150°C), 30-50 wt% kerosene (bp150~265°C), 10-30 wt% LGO (Light gas oil, bp265~380°C), and 0-10 wt% UCO-2 / AR (bp380°C~) based on the total weight. Specifically, naphtha (bp~150°C) 35-50 wt%, kerosene (bp150~265°C), 10-30 wt% LGO (Light gas oil, bp265~380°C), and 0-8 wt% UCO-2 / AR (bp380°C~) may be used. The pyrolysis gas may contain 10 to 20% by weight of UCO-2 / AR (bp 265 to 380°C) and 0 to 6% by weight of UCO-2 / AR (bp 380°C or higher). The weight ratio of the light oil content (total of naphtha and kerosene) to the heavy oil content (total of LGO and UCO-2 / AR) in the pyrolysis gas may be 2.5 to 5, 2.5 to 4, or 3 to 3.8.

[0120] The pyrolysis oil produced in the lightening step may have a total chlorine content of less than 100 ppm, 80 ppm or less, 60 ppm or less, 5 to 50 ppm, or 10 to 50 ppm, and an organic chlorine content of less than 90 ppm, 70 ppm or less, 50 ppm or less, 5 to 50 ppm, or 5 to 40 ppm, based on the total weight.

[0121] According to one embodiment of the present disclosure, the pyrolysis step and the lightening step can satisfy the following relational expression 3.

[0122] [Equation 3] 0.7 <T2 / T1<1.3

[0123] In the above Relational Formula 3, T1 and T2 are the temperatures at which the pyrolysis step and the lightening step proceed, respectively.

[0124] When the pyrolysis step and the lightening step are carried out so that the T2 / T1 value is 0.7 or less, the temperature of the pyrolysis step may be relatively high or the temperature of the lightening step may be relatively low. In this case, the proportion of the pyrolysis oil condensed in the high-temperature filter and circulated to the pyrolysis reactor may increase, and the final boiling point of the pyrolysis oil may be excessively low. On the other hand, when the steps are carried out so that the T2 / T1 value is 1.3 or more, the loss rate in the gas phase may be excessively high, and the yield of the pyrolysis oil may be low.

[0125] Specifically, the T2 / T1 may be 0.7 to 1.2, 0.8 to 1.2, 0.8 to 1.1, 0.9 to 1.1, or, for example, 1. This can further improve the above-mentioned effects.

[0126] The dehydration step according to one embodiment of the present disclosure may be a step of applying a voltage to a first mixture of pyrolysis oil, wash water, and a demulsifier to dehydrate the first mixture.

[0127] The pyrolysis oil contains water, which can cause problems such as inactivation of hydrotreating catalysts and corrosion of reactors, and water-soluble impurities are contained in the water, so it is necessary to remove the water. By undergoing the dehydration step, water that exists in the form of an emulsion in the waste plastic pyrolysis oil can be easily removed.

[0128] The pyrolysis oil according to one embodiment of the present disclosure may be a hydrocarbon oil mixture produced by pyrolyzing waste plastic, and in this case, the waste plastic may include solid or liquid waste related to synthetic polymer compounds such as waste synthetic resin, waste synthetic fiber, waste synthetic rubber, and waste vinyl.

[0129] The hydrocarbon oil mixture according to one embodiment of the present disclosure may contain impurities such as chlorine compounds, nitrogen compounds, oxygen compounds, metal compounds, and char-derived particles in addition to the hydrocarbon oil, and may contain impurities in the form of compounds in which chlorine, nitrogen, oxygen, or metals are bonded to the hydrocarbon, and may contain hydrocarbons in the form of paraffins, olefins, lead compounds, or aromatics.

[0130] The washing water according to one embodiment of the present disclosure can increase the contact probability between the water in the form of an emulsion present in the pyrolysis oil. In addition, a basic compound can be added to the washing water to remove water-soluble acidic substances contained in the water, and the basic compound may be, but is not limited to, sodium hydroxide (NaOH).

[0131] The pyrolysis oil according to one embodiment of the present disclosure may be mixed in a larger volume than the washing water, and specifically, the first mixture may be a mixture of waste plastic pyrolysis oil and washing water in a volume ratio of 1:0.001 to 0.5, more specifically, a volume ratio of 1:0.005 to 0.4, and most specifically, a volume ratio of 1:0.01 to 0.3. When the above range is satisfied, water washing is performed sufficiently, impurities in the pyrolysis oil can be significantly reduced, and the cost of removing the mixed washing water can be minimized.

[0132] The demulsifier according to one aspect of the present disclosure may be, but is not limited to, one or a mixture of two or more selected from the group consisting of polyethylene glycol, tert-butanol, acetone, alkyl naphthalene sulfonate, alkyl benzene sulfonate, non-ionic alkoxylated alkylphenol resin, polyalkylene oxide, and polyoxyethylene sorbitan ester.

[0133] The first mixture according to one embodiment of the present disclosure may be a mixture of the pyrolysis oil and the demulsifier in a volume ratio of 1:0.000001 to 0.001, specifically, a volume ratio of 1:0.000002 to 0.0005, and more specifically, a volume ratio of 1:0.000003 to 0.0001. When the above range is satisfied, the emulsion can be broken down while minimizing the impact on the quality of the pyrolysis oil.

[0134] The demulsifier according to one embodiment of the present disclosure may have a weight average molecular weight in the range of 200 to 2,000, specifically, a weight average molecular weight in the range of 300 to 1,000, and more specifically, a weight average molecular weight in the range of 400 to 800. When the demulsifier satisfies the above range, it is easily mixed with the pyrolysis oil and wash water under the conditions in which the dehydration step is performed, and the efficiency of decomposing the water emulsion is increased.

[0135] The emulsion-like water contained in the first mixture of the pyrolysis oil, the cleaning water, and the demulsifier is stable and difficult to remove, so the water can be easily removed by applying a voltage to the first mixture.

[0136] The voltage according to one embodiment of the present disclosure may be applied as an AC or a combination of an AC and a DC. Some impurity particles contained in the pyrolysis oil exhibit polarity, and when a DC voltage is applied, polarized impurity particles may accumulate on a specific electrode, and if the process proceeds for a long period of time, the phenomenon of impurities adhering to the electrode may occur. However, when an AC voltage is applied, the polarity of the electrode changes periodically, so that the adhering phenomenon of impurity particles can be prevented. In addition, the frequency of the AC according to one embodiment of the present disclosure may be a single frequency or a combination of two or more frequencies. As a specific example, when it is a single frequency, an AC having a frequency of 60 Hz may be applied, and when it is a combination of two or more frequencies, an AC having a frequency of 50 Hz and an AC having a frequency of 60 Hz may be applied alternately, but is not limited thereto.

[0137] According to an embodiment of the present disclosure, the voltage may be applied via a vertical electrode. If impurity particles accumulate on the electrode during the preparation of the mixture or during the application of the voltage, the impurity particles may adhere to the electrode after a long period of time unless they are manually cleaned. However, if the vertical electrode is used, the impurity particles do not accumulate on the electrode and fall to the lower part of the reactor due to gravity without the need for a separate cleaning operation, so that the adhesion of the impurity particles can be prevented in advance.

[0138] The magnitude of the voltage according to one embodiment of the present disclosure may be, but is not limited to, 0.1 to 50 kV, specifically 1 to 30 kV, and more specifically 5 to 20 kV.

[0139] The dehydration according to one embodiment of the present disclosure may be performed by any method known in the art. As a non-limiting example, water may be removed by pumping the water layer after the oil-water separation after the application of a voltage. Water may be removed in a gas-liquid separator.

[0140] Metal impurities in the pyrolysis oil stabilize the emulsion and hinder oil-water separation, helping to form a stable emulsion layer, often called a rag layer. This rag layer forms between the upper desalted oil layer and the lower water layer of the first mixture and can thicken gradually with successive dewatering processes. An excessively thick rag layer can be discharged together with the desalted oil into the hydrotreating step equipment. This reduces the desalting effect of the desalted oil and reduces the efficiency of the process. The rag layer is also discharged together with the water, which can cause problems in the wastewater treatment process. Therefore, it is advisable to remove the rag layer that forms between the desalted oil layer and the water layer.

[0141] Therefore, the method for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure may further include a step of removing a rag layer from the first mixed liquid after applying a voltage in the dehydration step. The removal of the rag layer may be performed through a pipe that penetrates the wall of the dehydrator and connects to the outside after measuring the density change of the mixed liquid using a density meter in the dehydrator to determine the formation position and thickness of the rag layer, but is not necessarily limited to this.

[0142] The dehydration step according to one aspect of the present disclosure may include dehydrating the first mixed liquid, and then condensing the water in the dehydrated first mixed liquid to further dehydrate it.

[0143] According to an embodiment of the present disclosure, the additional dehydration may be performed by supplying the dehydrated first mixed liquid to a coalescer. Specifically, the remaining water contained in the dehydrated first mixed liquid may be coalesced and removed by a collection filter in the coalescer, but this is a specific example and is not necessarily limited thereto. The water content in the waste plastic pyrolysis oil is further reduced through the additional dehydration, thereby preventing catalyst inactivation due to water, and improving process stability and the quality of the refined pyrolysis oil.

[0144] According to one embodiment of the present disclosure, the ratio of the water content of the pyrolysis oil to the water content of the dehydrated first mixed liquid may be 1:0.0001 to 0.9, specifically 1:0.0005 to 0.5, and more specifically 1:0.001 to 0.1. When the above range is satisfied, the risk of trouble occurring in subsequent processes including hydrotreatment is significantly reduced, and high-quality refined pyrolysis oil that meets the standards for blending or as a raw material for oil refining and petrochemical processes can be produced, but is not necessarily limited thereto.

[0145] The dehydration step according to one embodiment of the present disclosure may be carried out at a pressure of 50 bar or less. When the dehydration step is carried out at a pressure of 50 bar or less, the water in the pyrolysis oil can be easily removed and the process stability can be ensured. Specifically, the dehydration step may be carried out at a pressure of 30 bar or less, more specifically, at a pressure of 20 bar or less, and may be carried out at a pressure of 5 bar or more, but not limited to this.

[0146] The dehydration step according to one embodiment of the present disclosure may be carried out at a temperature of 20°C to 300°C. When the above range is satisfied, emulsion decomposition and water condensation occur well, and dehydration efficiency can be improved. Specifically, the dehydration step may be carried out at a temperature of 50°C to 250°C, more specifically, 80°C to 200°C.

[0147] In order to improve the dehydration efficiency in the dehydration step according to one embodiment of the present disclosure, any one or more additional steps selected from the group consisting of centrifugation and distillation may be performed before and / or after the dehydration. The additional steps may be performed by any method known in the art and are not particularly limited.

[0148] The hydrotreating step according to one embodiment of the present disclosure may be a step of hydrotreating a second mixed liquid obtained by mixing the first mixed liquid dehydrated in the dehydration step with a sulfur source to produce a refined pyrolysis oil from which impurities have been removed.

[0149] The second mixed liquid according to one embodiment of the present disclosure may have a chlorine (Cl) concentration of 10 ppm or more, specifically 100 ppm or more, more specifically 200 ppm or more, and may have an upper limit of, but is not limited to, 3000 ppm or less.

[0150] The second mixed liquid according to one embodiment of the present disclosure may have a weight ratio of nitrogen to chlorine of 1:0.1-10, specifically 1:0.5-5, and more specifically 1:1-2, but the weight ratios are specific examples of what may be contained in the pyrolysis oil, and the composition of the pyrolysis oil is not limited thereto.

[0151] In the hydrogenation process according to one embodiment of the present disclosure, the ratio of hydrogen to the second mixture is 100 Nm 3 / Sm 3 ~5000Nm 3 / Sm 3 , specifically 500Nm 3 / Sm 3 ~3000Nm / Sm 33 , more specifically 1000Nm 3 / Sm 3 ~1500Nm 3 / Sm 3 When this condition is satisfied, impurities can be effectively removed, the activity of the hydrogenation catalyst can be maintained at a high level for a long period of time, and the process efficiency can be improved.

[0152] The sulfur source refers to a sulfur source that can continuously supply sulfur components during the refining process.

[0153] The hydrotreating step produces a second mixed solution containing the sulfur source, thereby suppressing inactivation of a molybdenum-based hydrotreating catalyst caused by a shortage of the sulfur source during the refining process and high-temperature operation, and maintaining catalytic activity.

[0154] The sulfur source according to one embodiment of the present disclosure may include a sulfur-containing oil. The sulfur-containing oil refers to an oil composed of sulfur-containing hydrocarbons obtained from crude oil. There is no particular limitation as long as the oil contains sulfur, and for example, it may be light gas oil, direct current naphtha, vacuum naphtha, pyrolysis naphtha, direct current kerosene, vacuum kerosene, pyrolysis kerosene, direct current diesel, vacuum diesel, pyrolysis diesel, sulfur-containing waste tire oil, or any mixture thereof.

[0155] By including waste tire oil as the sulfur-containing oil according to one embodiment of the present disclosure, the high content of sulfur contained in the waste tires is converted into oil together with hydrocarbons, and can preferably act as a sulfur source for the waste plastic pyrolysis oil. In addition, by exclusively using the waste tire oil as a sulfur source for the waste plastic pyrolysis oil, it is advantageous in terms of reducing the environmental load due to the recycling of the waste tires and maintaining the catalytic activity for a long period of time.

[0156] Specifically, the sulfur-containing oil may be a light gas oil (LGO) having a specific gravity of 0.7 to 1. When this is used, it can be uniformly mixed with the dehydrated first mixed liquid, and has the advantage of high hydrotreating efficiency. Specifically, the specific gravity may be 0.75 to 0.95, more specifically 0.8 to 0.9. The sulfur-containing oil may contain 100 ppm or more of sulfur. If the sulfur component is contained at 100 ppm or less, the content of the sulfur component supplied is low, and the effect of preventing the inactivation of the molybdenum-based hydrogenation catalyst may be insignificant. Specifically, the sulfur component may be contained at 800 ppm or more, more specifically 8,000 ppm or more, and may be contained at 200,000 ppm or less, but not limited to this.

[0157] The second mixed liquid according to one embodiment of the present disclosure may contain 100 ppm or more of sulfur. As in the case of the sulfur-containing oil, if the sulfur component in the second mixed liquid is contained at 100 ppm or less, the content of the sulfur component supplied is small, and the effect of preventing the inactivation of the molybdenum-based hydrogenation catalyst may be insignificant. Specifically, the sulfur component may be contained at 800 ppm or more, more specifically, at 8,000 ppm or more, or, without limitation, at 200,000 ppm or less.

[0158] According to one embodiment of the present disclosure, the sulfur-containing oil may be contained in an amount of less than 0.5 parts by weight based on 100 parts by weight of the first mixed liquid dehydrated in the dehydration step. Specifically, the sulfur-containing oil may be contained in an amount of less than 0.1 parts by weight, more specifically, less than 0.05 parts by weight, or, without limitation, more than 0.01 parts by weight. By containing less than 0.5 parts by weight of the sulfur-containing oil, the chlorine (Cl) or nitrogen (N) concentration contained in the waste plastic pyrolysis oil is diluted, the ammonium salt (NH4Cl) generation rate can be controlled, and the step and stability can be improved.

[0159] The sulfur source according to one embodiment of the present disclosure may include one or more sulfur-containing organic compounds selected from disulfide-based compounds, sulfide-based compounds, sulfonate-based compounds, and sulfate-based compounds. Specifically, the compound may include one or a mixture of two or more selected from dimethyl disulfide, dimethyl sulfide, polysulfide, dimethyl sulfoxide (DMSO), methyl methanesulfonate, ethyl methanesulfonate, propyl sulfonate, propenyl propenesulfonate, propenyl cyanoethansulfonate, ethylene sulfate, bicycloglyoxalsulfate, and methyl sulfate, which are presented by way of example only and are not intended to limit the present disclosure.

[0160] The sulfur-containing organic compound according to one embodiment of the present disclosure may be contained in an amount of 0.01 to 0.1 parts by weight based on 100 parts by weight of the first mixture dehydrated in the dehydration step. Specifically, the sulfur-containing organic compound may be contained in an amount of 0.02 to 0.08 parts by weight, and more specifically, the sulfur-containing organic compound may be contained in an amount of 0.03 to 0.06 parts by weight. If the sulfur-containing organic compound is contained in an amount of less than 0.01 parts by weight, the content of the sulfur component supplied is small, and the effect of preventing the deactivation of the molybdenum-based hydrogenation catalyst may be insignificant.

[0161] The hydrotreating refers to a hydrogenation reaction that occurs when a reaction gas containing hydrogen gas (H2) is added to a second mixed liquid obtained by mixing the first mixed liquid dehydrated in the dehydration step and a sulfur source under a molybdenum-based hydrogenation catalyst. Specifically, the hydrotreating may refer to a conventionally known hydrotreating reaction including hydrodesulfurization, hydrocracking, hydrodechlorination, hydrodenitrogenation, hydrodeoxygenation, and hydrodemetallization. Through the hydrotreating, impurities including chlorine (Cl), nitrogen (N), and oxygen (O) and some of the olefins are removed, and other metal impurities can also be removed, and by-products containing the impurities are generated.

[0162] The by-products are generated by the reaction of hydrogen gas (H2) with chlorine (Cl), nitrogen (N), sulfur (S) or oxygen (O), which are impurities contained in the waste plastic pyrolysis oil. Specifically, they may include hydrogen sulfide gas (H2S), hydrogen chloride (HCl), ammonia (NH3) or water vapor (H2O), as well as unreacted hydrogen gas (H2), and very small amounts of methane (CH4), ethane (C2H6), propane (C3H8) or butane (C4H 10 ) etc.

[0163] The molybdenum-based hydrogenation catalyst according to one embodiment of the present disclosure may be a catalyst in which a molybdenum-based metal or a metal including at least one selected from nickel, cobalt, and tungsten and a molybdenum-based metal are supported on a carrier. The molybdenum-based hydrogenation catalyst has high catalytic activity during hydrotreating, and may be used alone or, if necessary, in the form of a binary catalyst combined with a metal such as nickel, cobalt, or tungsten.

[0164] The support according to one embodiment of the present disclosure may be, but is not limited to, alumina, silica, silica-alumina, titanium oxide, molecular sieves, zirconia, aluminum phosphate, carbon, niobium, or mixtures thereof.

[0165] The molybdenum-based hydrogenation catalyst according to one embodiment of the present disclosure may include a molybdenum-based sulfide hydrogenation catalyst, such as, but not limited to, molybdenum sulfide (MoS) or molybdenum disulfide (MoS2), and may include any known molybdenum-based sulfide hydrogenation catalyst.

[0166] The reaction gas according to one embodiment of the present disclosure may further include hydrogen sulfide gas (H2S). The hydrogen sulfide gas (H2S) contained in the reaction gas acts as a sulfur source and can regenerate the activity of the molybdenum-based hydrogenation catalyst that is deactivated during the purification step, as the sulfur source mixed with the waste plastic pyrolysis oil.

[0167] The hydrotreating process according to one embodiment of the present disclosure may be carried out at a pressure of 150 bar or less. Specifically, the hydrotreating process may be carried out at a pressure of 120 bar or less, more specifically, at a pressure of 100 bar or less, and may be carried out at a pressure of 50 bar or more, but not limited to this. When the hydrotreating process is carried out under a pressure condition exceeding 150 bar, ammonia and hydrogen chloride are excessively generated during the hydrotreating process, so that the ammonium salt formation temperature increases, and the pressure difference in the reactor or other process may be easily induced, which may significantly reduce the stability of the process. Although the increase in the ammonium salt formation temperature can be partially suppressed even under a pressure condition exceeding 150 bar by adjusting the nitrogen and chlorine content in the waste plastic pyrolysis oil, in this case, the waste plastic pyrolysis oil to be subjected to the refining process according to the present disclosure may be extremely limited, which is not appropriate.

[0168] The hydrogenation treatment according to one embodiment of the present disclosure may be carried out at a temperature of 150° C. to 500° C. When the above range is satisfied, the efficiency of the hydrogenation treatment can be improved. Specifically, the hydrogenation treatment may be carried out at a temperature of 200° C. to 400° C.

[0169] The hydrogenation process according to one embodiment of the present disclosure may be carried out in multiple steps, and as a specific example, may be carried out in two steps. When the hydrogenation process is carried out in two steps, the first step may be carried out at a lower temperature than the second step. In this case, the first step may be carried out at a temperature of 150°C to 300°C, specifically 200°C to 250°C, and the second step may be carried out at a temperature of 300°C to 500°C, specifically 350°C to 400°C, but is not limited thereto.

[0170] The method for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure may further include, after the hydrotreating step, subjecting the stream containing the refined pyrolysis oil from which the impurities have been removed to gas-liquid separation, followed by washing with water.

[0171] The stream containing the refined pyrolysis oil from which the impurities have been removed according to one embodiment of the present disclosure may contain hydrogen chloride, ammonia, unreacted hydrogen gas, etc., including the refined pyrolysis oil from which the impurities have been removed, which is discharged from the rear end of the reactor where the hydrotreatment step is performed.

[0172] By the gas-liquid separation according to one embodiment of the present disclosure, ammonia and hydrogen chloride generated by hydrotreating may be removed from a stream containing refined pyrolysis oil from which impurities have been removed, and unreacted hydrogen gas may be recovered.

[0173] The gas-liquid separation according to one embodiment of the present disclosure may be performed by a method known in the art through a separator, and is not particularly limited.

[0174] The gas-liquid separation according to one embodiment of the present disclosure may be performed 2 to 4 times, specifically 3 to 4 times, more specifically 4 times. When the above range is satisfied, the refined pyrolysis oil contains trace amounts of NH3 and hydrogen chloride, so that the generation of ammonium salts can be minimized even under low temperature conditions for oil-water separation. In addition, in the future, oil refining and petrochemical processes using the refined pyrolysis oil as a raw material can be stably performed without adding a separate salt remover to the refined pyrolysis oil.

[0175] The gas stream produced as a result of the gas-liquid separation according to one embodiment of the present disclosure may include off-gas, which may include light hydrocarbons, hydrogen sulfide, ammonia, or hydrogen chloride, and unreacted hydrogen gas. The off-gas and unreacted hydrogen gas are separated by methods known in the art, and the unreacted hydrogen gas is recycled within the process, while the off-gas is treated through steps described below and may be used as a fuel or discharged to the atmosphere.

[0176] The water washing according to one embodiment of the present disclosure may dissolve and remove salts contained in the gas stream or may dissolve gases that may form salts to suppress salt formation. The water washing may be performed by any method known in the art and is not particularly limited.

[0177] According to one embodiment of the present disclosure, the water washing may be performed 2 to 4 times, specifically 2 to 3 times. When the above range is satisfied, the salt removal and salt formation inhibition effects are sufficiently exhibited, a high-quality refined pyrolysis oil can be obtained, and stability with the steps can be ensured.

[0178] The method for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure may further include, after the step of gas-liquid separation of the stream containing the refined pyrolysis oil from which the impurities have been removed and washing with water, a step of combusting the separated off-gas and a step of treating the unburned off-gas.

[0179] The waste gas according to one embodiment of the present disclosure may contain C1-C4 light hydrocarbons, hydrogen sulfide (H2S), ammonia (NH3), etc. Therefore, in order to use the waste gas as fuel, it is necessary to combust the waste gas to remove hydrogen sulfide (H2S), ammonia (NH3), etc. The exhaust gas generated by the combustion of the waste gas, including sulfur dioxide (SO2), nitrogen dioxide (NO2), etc., may be subjected to caustic scrubbing to meet emission standards and then discharged into the atmosphere.

[0180] In addition, after the step of burning the waste gas, the unburned waste gas may be treated by sour water stripping, adsorption, biological treatment, oxidation, amine scrubbing or caustic scrubbing before being discharged into wastewater.

[0181] According to one aspect of the present disclosure, the method for producing refined hydrocarbons from waste plastics of the present disclosure may include, but is not limited to, a distillation step, and may include, but is not limited to, steps applicable in oil refining or petrochemical processes.

[0182] In one embodiment of the present disclosure, the refined pyrolysis oil may be mixed with petroleum-based hydrocarbons and distilled as a mixed oil.

[0183] The petroleum-based hydrocarbons are a general term for naturally occurring mixtures of hydrocarbons or compounds separated from the mixtures, and specifically may be at least one selected from the group consisting of crude oil and hydrocarbons derived from crude oil, but are not limited thereto.

[0184] According to one embodiment of the present disclosure, the distillation may be carried out in at least one process selected from the group consisting of a crude distillation unit (CDU) and a vacuum distillation unit (VDU).

[0185] According to one embodiment of the present disclosure, in the distillation step, refined hydrocarbons can be obtained from naphtha when the boiling point is in the range of 150°C or less, from kerosene when the boiling point is in the range of 150 to 265°C, from LGO (light gas oil) when the boiling point is in the range of 265 to 340°C, and from VGO (vacuum gas oil) when the boiling point is in the range of 340°C or more.

[0186] In one embodiment of the present disclosure, the refined pyrolysis oil may comprise 60% by weight or less, 50% by weight or less, or 40% by weight or less of the total weight of the mixed oil.

[0187] The present disclosure also provides a system for producing refined hydrocarbons from waste plastics.

[0188] The contents described for the method for producing refined hydrocarbons from waste plastics may be similarly applied to the description of the system for producing refined hydrocarbons from waste plastics, to the extent that they overlap.

[0189] The present disclosure provides a system for producing refined hydrocarbons from waste plastics, the system including: a pretreatment device for pretreating waste plastics; a pyrolysis reactor for producing pyrolysis gas by inputting the waste plastics pretreated in the pretreatment device; a hot filter for producing pyrolysis oil by inputting the pyrolysis gas; a connection pipe for connecting the high-temperature filter and the pyrolysis reactor so that liquid condensed in the high-temperature filter is re-introduced into the pyrolysis reactor; a dehydration device for applying a voltage to a first mixed liquid obtained by mixing the produced pyrolysis oil with wash water and a demulsifier to dehydrate the first mixed liquid; a hydrotreatment device for hydrotreating a second mixed liquid obtained by mixing the dehydrated first mixed liquid with a sulfur source to produce refined pyrolysis oil from which impurities have been removed; and a distillation device for distilling the refined pyrolysis oil to obtain refined hydrocarbons.

[0190] The production system of the present disclosure can produce high value-added pyrolysis oil with a high ratio of light hydrocarbons from waste plastics containing a large amount of impurities, and can produce refined hydrocarbons with a high ratio of light hydrocarbons from the pyrolysis oil. The production system of the present disclosure can also improve the yield of pyrolysis oil obtained from waste plastics.

[0191] According to one embodiment of the present disclosure, the high-temperature filter may be filled with beads. When the high-temperature filter is filled with beads, the inert effect and heat transfer effect in the high-temperature filter are maximized, and pyrolysis oil having a high proportion of light hydrocarbons can be produced. In addition, the yield of the pyrolysis oil can be improved.

[0192] According to one embodiment of the present disclosure, the beads may include at least one selected from the group consisting of silica sand (SiO2) and aluminum oxide (Al2O3).

[0193] According to one embodiment of the present disclosure, the manufacturing system may include at least two heaters outside the high-temperature filter. Also, the manufacturing system may include at least three heaters outside the high-temperature filter. When at least two heaters are provided outside the high-temperature filter, it is easy to form a temperature gradient in the high-temperature filter, and the temperatures of the upper, middle, and lower stages can be flexibly adjusted according to the operating conditions of the high-temperature filter, allowing for flexible process operation.

[0194] The dehydrator according to an embodiment of the present disclosure may include vertical electrodes. The number of vertical electrodes included in the dehydrator according to an embodiment of the present disclosure may be at least 2, specifically 4 or more, more specifically 6 or more, and may be up to 20, but is not necessarily limited thereto.

[0195] The dehydration device according to one embodiment of the present disclosure may include a coalescer therein. The coalescer is a device that captures fine droplets to form larger droplets, and may be a device commonly used in the industry, and is not particularly limited.

[0196] According to one embodiment of the present disclosure, the first mixed liquid dehydrated from the dehydrator flows into the agglomerator to produce a further dehydrated first mixed liquid. When a dehydrator including the agglomerator is used, the additionally dehydrated first mixed liquid flows into a hydrotreating reactor together with hydrogen gas.

[0197] The system for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure may further include a separator that separates the refined pyrolysis oil from which impurities have been removed and produced from the hydrotreatment treatment device into gas and liquid.

[0198] The separator according to one embodiment of the present disclosure may be 2 to 4, specifically 3 to 4, and more specifically 4. When the above range is satisfied, the refined pyrolysis oil contains trace amounts of NH3 and hydrogen chloride, so that the generation of ammonium salts can be minimized even under low temperature conditions for oil-water separation. In addition, even if a separate salt remover is not added to the refined pyrolysis oil, petroleum refining and petrochemical processes using the refined pyrolysis oil as a raw material can be stably performed in the future.

[0199] The system for producing refined hydrocarbons from waste plastics according to one embodiment of the present disclosure may further include a recycle gas compressor that recovers unreacted hydrogen gas from the gas stream separated from the separator and inputs it to the hydrotreater.

[0200] Hereinafter, the embodiments of the present disclosure will be further described with reference to specific experimental examples. The embodiments and comparative examples included in the experimental examples are merely illustrative of the present disclosure and do not limit the scope of the appended claims. It is obvious to those skilled in the art that various changes and modifications to the embodiments are possible within the scope of the category and technical idea of ​​the present disclosure, and it is natural that such changes and modifications belong to the scope of the appended claims.

[0201] As used herein, the term "pyrolysis oil yield" refers to the weight ratio of oil to the total weight of oil, aqueous by-products, pyrolysis residue (Char) and by-product gas among the products of the pyrolysis step.

[0202] [Example 1] The domestic waste plastic for use as feed contains 78.8% by weight of PE, 11.6% by weight of PP, 3.1% by weight of PVC, 2.4% by weight of PET, 2.1% by weight of nylon and 2.0% by weight of PU.

[0203] 1020g of the domestic waste plastic feed was fed into the feed injection section and mixed with the screw. 200g / hr of crushed waste plastic and 10g / hr of CaO were fed into the auger reactor, and pretreatment was carried out under the conditions of a screw speed of 10 rpm, a nitrogen flow rate of 3cc / min, 300°C, and a residence time of 1 hr.

[0204] The pretreated waste plastic was fed into a rotary kiln batch pyrolysis reactor, where pyrolysis was carried out at a rotary kiln rotation speed of 4 rpm and a temperature of 430°C to produce pyrolysis gas.

[0205] The pyrolysis gas produced was fed into a 1.3 L hot filter not filled with glass beads to lighten it, and pyrolysis oil was obtained from the recovery section. The liquid condensed in the hot filter was fed back into the pyrolysis reactor.

[0206] The pyrolysis oil obtained above, washing water, and polyethylene glycol having a weight average molecular weight of 500 were fed into a dehydrator in a volume ratio of 1:0.25:0.001 under conditions of 150°C and 10 bar, and stirred to produce a first mixed solution. The first mixed solution was subjected to oil-water separation by applying an AC voltage of 15 kV through vertical electrodes, and then the water layer was removed and dehydrated.

[0207] At this time, the dehydrator can treat high concentration impurities such as water content of about 5,000 ppm or more, nitrogen (N) of 500 ppm or more, chlorine (Cl) of 200 ppm or more, and olefin of 20 vol% or more from pyrolysis oil.

[0208] 100 parts by weight of the first mixed liquid dehydrated in the dehydrator was mixed with 0.04 parts by weight of dimethyl disulfide to produce a second mixed liquid, which was then hydrogenated at 300°C and 70 bar to produce a refined pyrolysis oil from which impurities had been removed.

[0209] The refined pyrolysis oil was fed to a Crude Distillation Unit (CDU) for distillation, and refined hydrocarbons were obtained as naphtha if the boiling point was below 150° C., kerosene if the boiling point was between 150 and 265° C., LGO (Light gas oil) if the boiling point was between 265 and 340° C., and VGO (Vacuum gas oil) if the boiling point was above 340° C. Table 1 shows the yield of the pyrolysis oil, Table 2 shows the weight ratio of the refined hydrocarbons, and Table 3 shows the measurement results regarding the impurity content in the refined pyrolysis oil.

[0210] [Example 2] The same procedure as in Example 1 was carried out except that glass beads having a diameter of 3 mm were packed into a 1.3 L high-temperature filter at an internal volume ratio of 88 vol % of the high-temperature filter, and the upper, middle and lower temperature stages of the high-temperature filter were maintained at 430°C.

[0211] [Example 3] The same procedure as in Example 1 was carried out except that glass beads having a diameter of 3 mm were packed into a 1.3 L high-temperature filter at an internal volume ratio of 88 vol% and the upper stage temperature of the high-temperature filter was maintained at 430°C, and the middle and lower stage temperatures were maintained at 500°C.

[0212] [Example 4] The same procedure as in Example 1 was carried out except that glass beads having a diameter of 3 mm were packed into a 1.3 L high-temperature filter at an internal volume ratio of 88 vol% of the high-temperature filter, and the upper stage temperature of the high-temperature filter was maintained at 430°C, the middle stage temperature at 450°C, and the lower stage temperature at 500°C.

[0213] [Examples 5 and 6] The same conditions as in Example 1 were followed, except that the waste plastic pyrolysis oil, wash water, and polyethylene glycol were fed into the dehydrator in the volume ratios shown in Table 1 below, to produce refined pyrolysis oil from which impurities had been removed.

[0214] [Example 7] The same procedures as in Example 1 were carried out except that a DC voltage was applied through the horizontal electrodes, and a refined pyrolysis oil from which impurities had been removed was produced.

[0215] [Example 8] The same conditions as in Example 1 were used, except that the dehydration of the first mixed liquid was carried out at a temperature of 120° C., to produce a refined pyrolysis oil from which impurities had been removed.

[0216] [Example 9] In Example 8, the waste plastic pyrolysis oil and polyethylene glycol were added in a volume ratio of 1:0.0001, and the hydrotreating was carried out under the same conditions as in Example 1, except that the pressure was 180 bar, and a refined pyrolysis oil from which impurities had been removed was produced.

[0217] [Example 10] The same procedure as in Example 1 was carried out, except that the first mixed liquid was dehydrated and then further dehydrated in a coagulator, to produce a refined pyrolysis oil from which impurities were removed.

[0218] [Example 11] The same procedure as in Example 1 was carried out, except that the refined pyrolysis oil and crude oil were mixed in a weight ratio of 5:5 and the resulting mixed oil was fed into a crude distillation unit (CDU).

[0219] [Comparative Example 1] The same procedure was followed as in Example 1, except that the liquid condensed in the high temperature filter was not reintroduced into the pyrolysis reactor.

[0220] [Comparative Example 2] The same procedures as in Example 1 were carried out except that no washing water was added, and refined pyrolysis oil from which impurities had been removed was produced.

[0221] [Comparative Example 3] The same conditions as in Example 1 were followed except that no polyethylene glycol was added, and a refined pyrolysis oil from which impurities had been removed was produced.

[0222] [Comparative Example 4] The same conditions as in Example 1 were followed except that no voltage was applied, and refined pyrolysis oil from which impurities had been removed was produced.

[0223] [Comparative Example 5] The same procedure as in Example 1 was carried out, except that dimethyl disulfide was not mixed into the dehydrated first mixed liquid, to produce a refined pyrolysis oil from which impurities had been removed.

[0224] Evaluation example

[0225] [Measurement method] The waste plastic feed composition was analyzed using a Flake analyzer from Germany's RTT, an NIR analyzer.

[0226] GC-Simdis analysis (HT750) was performed to confirm the composition of pyrolysates related to pyrolysis oil yield measurement.

[0227] After the dehydration process was completed, ICP, TNS, EA-O, and XRF analyses were performed to analyze the moisture and impurity Cl, S, N, and O contents in the resulting mixed liquid and the impurity Cl, S, N, and O contents in the final refined pyrolysis oil. The total Cl content was measured according to ASTM D5808, the N content was measured according to ASTM D4629, and the S content was measured according to ASTM D5453.

[0228] The catalyst activity maintenance time was measured in hours based on the time point when the nitrogen content in the refined pyrolysis oil exceeded 10 ppm by performing a Total Nitrogen & Sulfur (TNS element) analysis on the refined pyrolysis oil.

[0229] The steps of the above-mentioned Examples and Comparative Examples were operated for three months, and the particle adhesion rate was measured according to the following formula 1.

[0230] [Formula 1] Particle adhesion rate (%) = (amount of impurity particles adhered to the electrode / amount of impurity particles in the pyrolysis oil) x 100

[0231] The yields of pyrolysis oil in the above examples and comparative examples are shown in Table 1, and the weight ratios of refined hydrocarbons are shown in Table 2. [Table 1] [Table 2] Comparative Example 1, in which the high-temperature filter was not packed with beads and the liquid condensed in the high-temperature filter was not reintroduced into the thermal cracking reactor, was confirmed to have the lowest yield of thermal cracking oil and the lowest proportion of light oils, including naphtha and kerosene.

[0232] It was confirmed that Example 1, in which the liquid condensed in the high-temperature filter is reintroduced into the thermal cracking reactor, can achieve a superior yield of thermal cracking oil and a superior proportion of light hydrocarbons including naphtha and kerosene compared to Comparative Example 1.

[0233] It was confirmed that Example 2, in which the liquid condensed in the high-temperature filter was reintroduced into the thermal cracking reactor and the high-temperature filter was packed with beads, showed a superior thermal cracking oil yield and proportion of light hydrocarbons including naphtha and kerosene to Example 1.

[0234] Examples 3 and 4, in which the liquid condensed in the high temperature filter was re-introduced into the pyrolysis reactor, the high temperature filter was packed with beads, and a temperature gradient was formed in the high temperature filter, showed better pyrolysis oil yield and percentage of light hydrocarbons including naphtha and kerosene compared to Examples 1 and 2.

[0235] In particular, it was confirmed that Example 4, in which the upper stage temperature of the high-temperature filter was maintained at 430°C, the middle stage temperature at 450°C, and the lower stage temperature at 500°C, showed the best pyrolysis oil yield and the proportion of light hydrocarbons including naphtha and kerosene.

[0236] Moreover, the measurement results regarding the impurity contents in the refined pyrolysis oils in the above-mentioned Examples and Comparative Examples are shown in Table 3. [Table 3] As can be seen from Table 3, Comparative Examples 2 to 4, which differ from the examples in terms of whether or not washing water was added, whether or not a demulsifier was added, and whether or not a voltage was applied, showed poor moisture and Cl removal results. This adversely affected the catalyst in the hydrotreating step, and the Cl content in the finally obtained refined pyrolysis oil was high. In Comparative Example 5, it was confirmed that although moisture and some impurities in the pyrolysis oil were sufficiently removed in the dehydration step, the hydrogenation catalyst was inactivated in a short time due to insufficient sulfur content, making it difficult to maintain the refining process for a long period of time.

[0237] However, in Examples 1 and 5 to 10 of the present disclosure, a significant amount of water contained in the pyrolysis oil was removed through the dehydration step, and a sulfur source was added, which significantly prolonged the activity of the hydrotreating catalyst. In addition, some water-soluble impurities were preemptively removed in the dehydration step, and the excellent activity of the catalyst was maintained for a long period of time, allowing the production of high-quality refined pyrolysis oil with an extremely low impurity content.

[0238] Meanwhile, when AC voltage was applied using vertical electrodes, it was confirmed that the adhesion rate of impurity particles derived from char in the pyrolysis oil to the electrode surface was very low even after the process had been running for more than three months. This shows that applying AC voltage or using vertical electrodes eliminates the need to interrupt the process to clean the inside of the reactor, and allows for better process efficiency.

[0239] In addition, in the case of Example 9, the dehydration results were poorer than in the other Examples, but the content of the impurity Cl in the refined pyrolysis oil was very low because the hydrotreating was performed under high pressure conditions. However, it was confirmed that a relatively large amount of ammonium salt was generated even at the temperature at which the hydrotreating was performed because ammonia and hydrogen chloride were generated in excess due to the high pressure.

[0240] In Example 10, by performing additional dehydration using a coagulator, the moisture and chlorine contents after dehydration were lower than those in other Examples, which confirms that the catalyst activity time, process stability, and quality of the refined pyrolysis oil are relatively superior to those in other Examples.

[0241] The above description is merely an example of application of the principles of the present disclosure, and other configurations may be included without departing from the scope of the present disclosure.

Claims

1. A pretreatment step of pretreating waste plastic; A pyrolysis step of feeding the waste plastic pretreated in the pretreatment step into a pyrolysis reactor to produce a pyrolysis gas; A lightening step of producing a pyrolysis oil by feeding the pyrolysis gas into a hot filter; A dehydration step of applying a voltage to a first mixture obtained by mixing the prepared pyrolysis oil with wash water and a demulsifier to dehydrate the first mixture; a hydrotreating step of hydrotreating a second mixed liquid obtained by mixing the dehydrated first mixed liquid with a sulfur source to produce a refined pyrolysis oil from which impurities have been removed; distilling the refined pyrolysis oil to obtain refined hydrocarbons; Including, The liquid condensed in the high temperature filter is reinjected into the pyrolysis reactor. A method for producing refined hydrocarbons from waste plastics.

2. 2. The method for producing refined hydrocarbons from waste plastics according to claim 1, wherein the high temperature filter is filled with beads.

3. The beads are made of silica sand (SiO 2 ) and aluminum oxide (Al 2 O 3 The method for producing refined hydrocarbons from waste plastics according to claim 2, wherein the catalyst comprises at least one selected from the group consisting of:

4. The method for producing refined hydrocarbons from waste plastics according to claim 1, wherein a temperature gradient is formed in the high-temperature filter.

5. 5. The method for producing refined hydrocarbons from waste plastics according to claim 4, wherein the temperature gradient is formed by providing at least two heaters on the outside of the high-temperature filter.

6. 2. The method for producing refined hydrocarbons from waste plastics according to claim 1, wherein the pyrolysis reactor comprises at least two batch reactors.

7. 7. The method for producing refined hydrocarbons from waste plastics according to claim 6, wherein the thermal cracking step is carried out by switching operation of the at least two batch reactors.

8. The method for producing refined hydrocarbons from waste plastics according to claim 1, wherein the refined pyrolysis oil is mixed with petroleum-based hydrocarbons and distilled as a mixed oil.

9. The method for producing refined hydrocarbons from waste plastics according to claim 8, wherein the refined pyrolysis oil is contained in an amount of 50% by weight or less based on the total weight of the mixed oil.

10. 2. The method for producing refined hydrocarbons from waste plastics according to claim 1, wherein the waste plastics include at least one selected from the group consisting of polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyvinyl chloride (PVC) and polystyrene (PS).

11. In the dehydration step, The method for producing refined hydrocarbons from waste plastics according to claim 1 , wherein the pyrolysis oil is mixed in an amount greater than that of the wash water.

12. The dehydration step, 2. The method for producing refined hydrocarbons from waste plastics according to claim 1, wherein the first mixture is a mixture of the pyrolysis oil and the wash water in a volume ratio of 1:0.001 to 0.

5.

13. In the dehydration step, 2. The method for producing refined hydrocarbons from waste plastics according to claim 1, wherein the first mixture is a mixture of the pyrolysis oil and the demulsifier in a volume ratio of 1:0.000001 to 0.

001.

14. 2. The method for producing refined hydrocarbons from waste plastics according to claim 1, wherein the demulsifier is one or a mixture of two or more selected from the group consisting of polyethylene glycol, tert-butanol, acetone, alkylnaphthalene sulfonate, alkylbenzene sulfonate, nonionic alkoxylated alkylphenol resin, polyalkylene oxide, and polyoxyethylene sorbitan ester.

15. A pre-treatment device for pre-treating waste plastics; a pyrolysis reactor into which the waste plastic pretreated in the pretreatment device is input to produce a pyrolysis gas; a hot filter for producing pyrolysis oil by inputting the pyrolysis gas; a connecting pipe connecting the high temperature filter and the pyrolysis reactor so that liquid condensed from the high temperature filter is reintroduced into the pyrolysis reactor; a dehydration device for applying a voltage to a first mixture of the pyrolysis oil, the first mixture being mixed with washing water and a demulsifier, to dehydrate the first mixture; a hydrotreating device for hydrotreating a second mixed liquid obtained by mixing the dehydrated first mixed liquid and a sulfur source to produce a refined pyrolysis oil from which impurities have been removed; a distillation apparatus for distilling the refined pyrolysis oil to obtain refined hydrocarbons; A system for producing refined hydrocarbons from waste plastics, comprising:

16. The system for producing refined hydrocarbons from waste plastics according to claim 15, wherein the high-temperature filter is filled with beads.

17. The beads are made of silica sand (SiO 2 ) and aluminum oxide (Al 2 O 3 The system for producing refined hydrocarbons from waste plastics according to claim 16, comprising at least one selected from the group consisting of: