Adhesive resin composition, adhesive resin molding, adhesive resin laminate, and housing sealing material

The adhesive resin composition with acid-modified polyolefin resin and inorganic fillers addresses the lack of both adhesive and gas barrier properties in resin films, providing enhanced performance.

JP2024155976AInactive Publication Date: 2024-10-31FUJIMORI KOGYO CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024144190
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing resin films lack both adhesive properties and gas barrier properties, as highlighted in Patent Documents 1 and 2.

Method used

An adhesive resin composition comprising acid-modified polyolefin resin and inorganic fillers, such as titanium oxide or calcium carbonate, which provides both adhesive strength and gas barrier properties.

Benefits of technology

The composition achieves both adhesive properties and gas barrier properties, enhancing the performance of resin films and sealing materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155976000003
    Figure 2024155976000003
  • Figure 2024155976000004
    Figure 2024155976000004
  • Figure 2024155976000005
    Figure 2024155976000005
Patent Text Reader

Abstract

To provide an adhesive resin composition, an adhesive resin molding, an adhesive resin laminate, and a housing sealing material which have both adhesiveness and gas barrier properties.SOLUTION: The adhesive resin composition contains, as essential components, an acid-modified polyolefin resin (A) and an inorganic filler (B) as a gas barrier component. The adhesive resin composition contains, in 100 pts.wt. of the total solid content, the acid-modified polyolefin resin (A) in the range of 50-90 pts.wt. and the inorganic filler (B) in the range of 10-30 pts.wt. The inorganic filler (B) is alumina.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive resin composition, an adhesive resin molded product, an adhesive resin laminate, and a housing sealant. [Background technology]

[0002] Compared with inorganic materials such as metals and glass, organic materials such as resins and rubbers have large gaps between polymer molecules and tend to have low gas barrier properties against oxygen and the like. For this reason, gas barrier properties are imparted using gas barrier materials. For example, Patent Document 1 describes applying a coating agent in which inorganic filler particles are dispersed in ethylene vinyl alcohol copolymer (EVOH) to a plastic film. Patent Document 2 describes sequential lamination of an inorganic vapor deposition layer and an inorganic filler-containing layer on a polyethylene naphthalate film via a transparent primer layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2007-211038 A [Patent Document 2] Patent No. 5092421 Summary of the Invention [Problem to be solved by the invention]

[0004] However, Patent Documents 1 and 2 do not suggest anything about a resin film that has both adhesiveness and gas barrier properties.

[0005] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide an adhesive resin composition, an adhesive resin molded product, an adhesive resin laminate, and a housing sealant that combine adhesiveness and gas barrier properties. [Means for solving the problem]

[0006] In order to solve the above problems, the present invention provides an adhesive resin composition comprising, as essential components, an acid-modified polyolefin resin (A) and an inorganic filler (B) as a gas-blocking component, the adhesive resin composition comprising, per 100 parts by weight of total solids, within the ranges of 50 to 90 parts by weight of the acid-modified polyolefin resin (A) and 10 to 30 parts by weight of the inorganic filler (B).

[0007] The inorganic filler (B) may be at least one selected from the group consisting of titanium oxide, calcium hydroxide, calcium carbonate, barium sulfate, zeolite, alumina, silicon dioxide, and magnesium silicate. The adhesive resin composition may contain a thermoplastic elastomer resin (C) in the range of 1 to 15 parts by weight per 100 parts by weight of the total solid content.

[0008] The present invention also provides an adhesive resin molded article comprising an adhesive resin film or adhesive resin sheet formed from the adhesive resin composition. The present invention also provides an adhesive resin laminate comprising an adhesive resin film or adhesive resin sheet having an adhesive resin layer made of the adhesive resin composition on at least one side of a base layer.

[0009] The present invention also provides a housing sealant formed from the adhesive resin molded article. The present invention also provides a housing sealant formed from the adhesive resin laminate. Effect of the Invention

[0010] According to the present invention, it is possible to provide an adhesive resin composition, an adhesive resin molded product, an adhesive resin laminate, and a housing sealant that have both adhesiveness and gas barrier properties. [Brief description of the drawings]

[0011] [Figure 1] 1 is a cross-sectional view showing an example of an adhesive resin molded body of the present invention. [Diagram 2] 1 is a cross-sectional view showing an example of an adhesive resin laminate of the present invention. [Diagram 3] 1 is a cross-sectional view showing an example of a housing sealed with the housing sealing material of the present invention. [Figure 4] FIG. 2 is a perspective view illustrating a method for measuring adhesive strength, where (a) is a method for preparing a test piece, (b) is a test piece, and (c) is a measurement method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the present invention will be described based on preferred embodiments. The adhesive resin composition of the embodiment is an adhesive resin composition containing, as essential components, an acid-modified polyolefin resin (A) and an inorganic filler (B) as a gas blocking component.

[0013] [Acid-modified polyolefin resin (A)] The acid-modified polyolefin resin (A) is a polyolefin resin modified with an unsaturated carboxylic acid or its derivative, and has a carboxyl group or a carboxylic anhydride group in the polyolefin resin. Preferably, the polyolefin resin is modified with an unsaturated carboxylic acid or its derivative. The acid-modified polyolefin resin can be modified by graft modification such as melt-kneading an acid functional group-containing monomer with a polyolefin resin in the presence of a radical polymerization initiator such as an organic peroxide or an aliphatic azo compound, or copolymerization of an acid functional group-containing monomer with an olefin.

[0014] Examples of the polyolefins include polyethylene, polypropylene, poly-1-butene, polyisobutylene, random copolymers of propylene and ethylene or α-olefin, block copolymers of propylene and ethylene or α-olefin, etc. Among them, polypropylene-based resins such as homopolypropylene (homopolypropylene, propylene homopolymer), block copolymers of propylene-ethylene (block PP), and random copolymers of propylene-ethylene (random PP) are preferred. Random PP is particularly preferred. Examples of the olefins to be copolymerized include olefin monomers such as ethylene, propylene, 1-butene, isobutylene, 1-hexene, and α-olefins.

[0015] The acid functional group-containing monomer is a compound having an ethylenic double bond and a carboxylic acid group or a carboxylic acid anhydride group in the same molecule, and is composed of various unsaturated monocarboxylic acids, dicarboxylic acids, or acid anhydrides of dicarboxylic acids. Examples of acid functional group-containing monomers having a carboxylic acid group (carboxylic acid group-containing monomers) include α,β-unsaturated carboxylic acid monomers such as acrylic acid, methacrylic acid, maleic acid, nadic acid, fumaric acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, tetrahydrophthalic acid, and endo-bicyclo[2.2.1]-5-heptene-2,3-dicarboxylic acid (endic acid). Examples of the acid functional group-containing monomer having a carboxylic acid anhydride group (carboxylic acid anhydride group-containing monomer) include unsaturated dicarboxylic acid anhydride monomers such as maleic anhydride, nadic acid anhydride, itaconic acid anhydride, citraconic acid anhydride, and endic acid anhydride. In the acid-modified polyolefin resin (A), these acid functional group-containing monomers may be used alone or in combination of two or more.

[0016] Among the above-mentioned acid functional group-containing monomers, carboxylic acid anhydride group-containing monomers are more preferred, and maleic anhydride is more preferred. When a portion of the acid functional group-containing monomer used for the acid modification remains unreacted, in order to suppress adverse effects on adhesive strength, it is preferable to remove the unreacted acid functional group-containing monomer and use the resulting resin as the acid-modified polyolefin resin (A).

[0017] Regarding the propylene component in the acid-modified polyolefin resin (A), it is preferable that the propylene unit is the majority from the viewpoint of the heat resistance of the resin. The majority here means that the propylene component is 50% by weight or more relative to the acid-modified polyolefin resin (A). Therefore, the acid-modified polyolefin resin (A) is preferably an acid-modified polypropylene-based resin in which the propylene unit is the majority.

[0018] [Inorganic filler (B)] The inorganic filler (B) functions as a gas blocking component that imparts gas barrier properties to the adhesive resin composition. The inorganic filler (B) is not particularly limited as long as it is an inorganic substance, but it is preferable to select it appropriately from the viewpoint of the gas barrier properties of the adhesive resin composition, miscibility with resins such as the acid-modified polyolefin resin (A), and other various suitabilities when used as a product. As the inorganic filler (B), as an appropriate metal compound, for example, a metal oxide, hydroxide, carbonate, sulfate, silicate, or aluminosilicate can be mentioned. As the metal contained in the inorganic filler (B), titanium, alkaline earth metals (calcium, strontium, barium), alkali metals (sodium, potassium, etc.), aluminum, silicon, magnesium, etc. can be mentioned. As a specific example of the inorganic filler (B), at least one selected from the group consisting of titanium oxide, calcium hydroxide, calcium carbonate, barium sulfate, zeolite, alumina, silicon dioxide, and magnesium silicate can be mentioned.

[0019] In order for the inorganic filler (B) to function as a gas barrier component, it is preferable that the inorganic filler (B) is well dispersed in the adhesive resin composition, and the inorganic filler (B) particles are arranged so as to block the movement of gas molecules that are trying to pass through the adhesive resin composition. For example, if the inorganic filler (B) is unevenly dispersed, the gas barrier property may be locally reduced in the area where the distribution ratio of the inorganic filler (B) is low. In addition, if gaps are generated between the molecules of the acid-modified polyolefin resin (A) and the particles of the inorganic filler (B), or between the particles of the inorganic filler (B), due to poor dispersion, the gas barrier property of the adhesive resin composition may be reduced. If the ratio of the inorganic filler (B) is low, it may be difficult to impart sufficient gas barrier property even if the particles of the inorganic filler (B) are well dispersed in the adhesive resin composition.

[0020] The adhesive resin composition preferably contains 10 to 30 parts by weight of inorganic filler (B) per 100 parts by weight of total solid content, and 50 to 90 parts by weight of acid-modified polyolefin resin (A) per 100 parts by weight of total solid content.

[0021] In order to disperse the inorganic filler (B) particles well and more uniformly in the adhesive resin composition, it is preferable to melt-knead the acid-modified polyolefin resin (A) and the inorganic filler (B). As the melt-kneading device, a single-screw extruder, a multi-screw extruder, a Banbury mixer, a plastomill, a heated roll kneader, or the like can be used. The heating temperature during melt-kneading is preferably selected from the range of 130 to 300°C so that the acid-modified polyolefin resin (A) is sufficiently melted and does not thermally decompose. When the acid-modified polyolefin resin (A) is a polypropylene-based resin, the kneading temperature is preferably 180 to 300°C, and more preferably 240 to 300°C to further improve the dispersibility of the inorganic filler (B). The kneading temperature can be measured by a method such as contacting a thermocouple with the adhesive resin composition in a molten state immediately after being extruded from the melt-kneading device.

[0022] In the melt-kneading, it is preferable to remove volatile components such as water in advance outside the apparatus. In addition, when volatile components are generated during the melt-kneading, it is preferable to discharge them from the apparatus as needed by degassing or the like. This makes it possible to suppress foaming when forming an adhesive resin molded body or an adhesive resin layer using the adhesive resin composition.

[0023] [Thermoplastic elastomer resin (C)] The adhesive resin composition may contain a thermoplastic elastomer resin (C). Examples of the thermoplastic elastomer resin (C) include styrene elastomers, styrene-butadiene copolymers, epoxy-modified styrene-butadiene copolymers, olefin elastomers, polyester elastomers, styrene-butadiene-styrene block copolymers, styrene-ethylene-propylene-styrene block copolymers, styrene-isoprene-butadiene-styrene block copolymers, and styrene-isoprene-styrene block copolymers. When the adhesive resin composition contains a thermoplastic elastomer resin (C), it is preferable that the thermoplastic elastomer resin (C) is contained within a range of 1 to 15 parts by weight per 100 parts by weight of the total solid content.

[0024] The thermoplastic elastomer resin (C) can be added before melt-kneading as long as it does not react with the acid-modified polyolefin resin (A) or the inorganic filler (B) under the conditions for melt-kneading the adhesive resin composition. Alternatively, the thermoplastic elastomer resin (C) can be kneaded into the adhesive resin composition after melt-kneading the acid-modified polyolefin resin (A) and the inorganic filler (B).

[0025] [Adhesive resin composition] The adhesive resin composition of the embodiment can be produced by melt-kneading and extruding an adhesive resin composition containing, as essential components, an acid-modified polyolefin resin (A) and an inorganic filler (B) as a gas barrier component, to produce an adhesive resin layer. The presence of the acid functional group in the acid-modified polyolefin resin (A) provides excellent adhesion to various adherends such as metals. The adhesive resin composition contains an inorganic filler (B), so that it can have both adhesion and gas barrier properties. The adhesive resin composition has a simple composition, and the adhesive resin layer can be easily produced.

[0026] The adhesive resin composition may contain other additives such as fillers, colorants, antioxidants, defoamers, leveling agents, and light absorbers. The adhesive resin composition may be configured without containing any resin or polymer component other than the acid-modified polyolefin resin (A) among the essential components and the thermoplastic elastomer resin (C) which is an optional component. The proportion of other solids other than the acid-modified polyolefin resin (A) and inorganic filler (B) which are essential components and the thermoplastic elastomer resin (C) which is an optional component may be 10 parts by weight or less, 5 parts by weight or less, 1 part by weight, etc., per 100 parts by weight of the total solids.

[0027] [Adherend] Adherends that can be bonded using the adhesive resin composition of the embodiment include various adherends such as metals, glass, plastics, etc. The shape of the adherend is not particularly limited, and examples thereof include a film, a sheet, a plate, a panel, a tray, a rod (rod-shaped body), a box, a housing, etc.

[0028] Examples of metals include steel, stainless steel, aluminum, copper, nickel, chromium, and alloys thereof. The present invention can also be applied to composite materials having a metal plating layer on the surface. In this case, the base material for plating is not particularly limited as long as it can be plated, and may be various materials such as metal, glass, and plastic.

[0029] Examples of glass include alkali glass, non-alkali glass, and quartz glass. Examples of plastics include polyolefin resins such as polyethylene and polypropylene; polyamide resins such as nylon; aromatic polyester resins such as polyethylene terephthalate (PET); acrylic resins such as polyacrylonitrile (PAN); and polyvinyl resins such as vinyl acetate (EVA), polyvinyl alcohol (PVA), vinyl alcohol / ethylene copolymer (EVOH), polyvinylidene chloride (PVDC), and polyvinyl chloride (PVC).

[0030] [Adhesive resin molded body] The adhesive resin molded body of the embodiment is a molded body formed from the adhesive resin composition and having a shape such as a film or sheet, and can be used as an adhesive resin film or adhesive resin sheet. As shown in Fig. 1, the adhesive resin molded body 10 can be produced by melt-kneading the adhesive resin composition and molding it into an adhesive resin layer 11 such as a film or sheet by extrusion molding or the like. At least one side of the adhesive resin molded body 10 can be bonded to adherends 21, 22.

[0031] The adhesive resin formed body 10 can be laminated with an adherend and adhered to various adherends by, for example, the following methods (1) to (4) and heating, preferably by heating and pressing. (1) A method of laminating and adhering the adhesive resin formed body 10 to one side of the adherend. (2) A method in which separate adhesive resin molded bodies are laminated on both sides of the adherend and bonded to each other. (3) A method in which separate adherends are laminated and bonded to both sides of an adhesive resin molded article. (4) A method in which a plurality of adhesive resin molded bodies and a plurality of adherends are alternately laminated and bonded to each other.

[0032] [Adhesive Resin Laminate] The adhesive resin laminate of the embodiment is a laminate having an adhesive resin layer made of the adhesive resin composition on at least one side of a substrate layer. As shown in FIG. 2, the adhesive resin laminate 10A has an adhesive resin layer 11 on one or both sides of a substrate layer 12, and can be bonded to adherends 21, 22 using the adhesive resin layer 11. The substrate layer 12 does not need to have adhesiveness in itself, and is preferably one that can be bonded to the adhesive resin layer 11. As with the above-mentioned examples of the adherend, various substrate layers 12 such as metal, glass, and plastic can be used. By using a thin substrate layer 12, the adhesive resin laminate 10A can be used as an adhesive resin film or adhesive resin sheet.

[0033] The adhesive resin laminate can be produced by a method of melt-kneading the adhesive resin composition and forming the adhesive resin layer by extrusion molding or the like. When the substrate layer is made of a thermoplastic resin, the adhesive resin composition can be extruded by a co-extrusion method. The adhesive resin composition can also be extruded by an extrusion lamination method.

[0034] When the adhesive resin laminate has the adhesive resin layer on only one side of the base material layer, it can be laminated with an adherend by, for example, the method described in (1) or (2) above, and bonded to various adherends by heating, preferably by heating and pressurization. Furthermore, when the adhesive resin laminate has the adhesive resin layers on both sides of the base material layer, it can be laminated with an adherend by, for example, the methods listed in (1) to (4) above, and bonded to various adherends by heating, preferably by heating and pressurization.

[0035] [Housing sealing material] The housing sealant of the embodiment can be formed from the adhesive resin molded body or the adhesive resin laminate. Fig. 3 shows an example of a configuration in which an adhesive resin molded body 10 is disposed between adherends 21 and 22 constituting a housing 20, and the adherends 21 and 22 are bonded using the adhesive resin molded body 10, thereby sealing an internal space 23 of the housing 20 from the outside of the housing 20.

[0036] When the pair of adherends 21, 22 constituting the housing 20 are made of metal, glass, or the like, the adhesive resin molded body 10 that seals the gap between the adherends 21, 22 is preferably thin, since the housing 20 itself has high gas barrier properties. The adhesive resin composition can be formed into a film with a thickness of 50 μm, so that it is possible to prevent the gas barrier properties of the housing 20 from decreasing in the cross-sectional direction. As the sealing material for the housing 20, an adhesive resin laminate 10A having adhesive resin layers 11 on both sides of a base layer 12 can also be used. The width of the housing sealing material along the cross-sectional direction of the housing 20 is not particularly limited, but may be, for example, about 1 to 5 mm.

[0037] The present invention has been described above based on a preferred embodiment, but the present invention is not limited to the above-mentioned embodiment, and various modifications are possible without departing from the gist of the present invention. EXAMPLES

[0038] The present invention will be specifically described below with reference to examples.

[0039] (Adhesive resin film) Adhesive resin films of each Example and Comparative Example were manufactured with the composition shown in Table 1. The adhesive resin film was manufactured by melt-kneading the acid-modified polyolefin resin (A), the inorganic filler (B), and the thermoplastic elastomer resin (C) first, and then extrusion-molding the mixture into a film of a predetermined thickness. The melt-kneading conditions for extrusion were 240°C and 2 minutes.

[0040] [Table 1]

[0041] The abbreviations used in Table 1 have the following meanings: "(A)-1": Maleic acid modified polypropylene (acid added 0.1 mass%, melting point 140°C, specific gravity 0.9) "(B)-1": Calcium carbonate "(B)-2": Zeolite "(B)-3": Alumina "(C)-1": Propylene-α-olefin copolymer elastomer (softening point 70°C)

[0042] (Method of evaluating film-forming properties) The appearance of the adhesive resin film obtained by extrusion molding was visually inspected, and if there were no problems with the appearance, it was rated as "○", and if there were defects such as tears or holes due to unevenness, it was rated as "×".

[0043] (Method of measuring adhesive strength) As shown in FIG. 3(a), a sample of the adhesive resin molded body 10 having a length of 20 mm was sandwiched between test adherends 31 and 32 having a length of 50 mm, and heat-pressed as shown in FIG. 3(b) to prepare a test piece 30. The width of the test piece 30 was set to 15 mm. After heat-pressing, the test piece 30 may be cut in the width direction so that the widths of the adhesive resin molded body 10 and the test adherends 31 and 32 are uniform. As shown in FIG. 3(c), the test piece 30 was pulled by T-shaped peeling in which the end of the test adherends 31 and 32 on the side not bonded by the adhesive resin molded body 10 is in the direction of approximately 180°, and the adhesive strength between the adhesive resin molded body 10 and the test adherends 31 and 32 was measured.

[0044] The sample of adhesive resin molded body 10 is an adhesive resin film having a thickness of 100 μm molded from an adhesive resin composition having the composition shown in Table 1. Test adherends 31 and 32 are aluminum foils having a thickness of 40 μm. The conditions for heat-pressing when preparing test piece 30 are a temperature of 150° C., a pressure of 0.1 MPa, and a time of 3 seconds. The conditions for measuring T-peel are a speed of 300 mm / min and a width of 15 mm. Adhesive strengths of 5 N / 15 mm or more were evaluated as "○", and those less than 5 N / 15 mm were evaluated as "×".

[0045] (Method of measuring oxygen permeability) According to JIS K 7126-2 (Plastics - Films and Sheets - Gas Permeability Test Method - Part 2: Isobaric Method), Method A (electrolytic sensor method), temperature 30℃, humidity 70% RH, measurement area 50cm 2 The oxygen permeability of the adhesive resin film was measured under the measurement conditions below. The thickness of the adhesive resin film used for measuring the oxygen permeability was set to 100 μm, the same as that of the adhesive resin film used for measuring the adhesive strength.

[0046] The oxygen permeability of the adhesive resin film is 1200cc / (m 2 ·day·atm) is marked as "○", and 1200cc / (m 2 ·day·atm) or more was evaluated as "×". Note that due to limitations of the measuring device, the measured value was 1800cc / (m 2 If the total volume was greater than 1800 (day atm), the result was displayed as "1800 or more."

[0047] [Table 2]

[0048] The evaluation results of the adhesive resin films are shown in Table 2. The adhesive resin films of Examples 1 to 5 had good film-forming properties and had both sufficient adhesive strength (adhesiveness) and oxygen permeability (gas barrier properties). The adhesive resin film of Comparative Example 1 did not contain inorganic filler (B), and therefore had higher oxygen permeability and lower gas barrier properties than Examples 1 to 5. Comparative Example 2 contained a larger amount of inorganic filler (B), but instead had higher oxygen permeability and lower gas barrier properties. [Explanation of symbols]

[0049] Reference Signs List 10: adhesive resin molded body, 10A: adhesive resin laminate, 11: adhesive resin layer, 12: base material layer, 20: housing, 21, 22: adherend, 23: internal space of housing, 30: test piece, 31, 32: test adherend.

Claims

1. An adhesive resin composition comprising, as essential components, an acid-modified polyolefin resin (A) and an inorganic filler (B) as a gas barrier component, An adhesive resin composition comprising, per 100 parts by weight of a total solid content, 50 to 90 parts by weight of the acid-modified polyolefin resin (A) and 10 to 30 parts by weight of the inorganic filler (B), wherein the inorganic filler (B) is alumina.

2. 2. An adhesive resin molded article comprising an adhesive resin film or adhesive resin sheet formed from the adhesive resin composition according to claim 1.

3. 10. An adhesive resin laminate comprising an adhesive resin film or adhesive resin sheet having an adhesive resin layer made of the adhesive resin composition according to claim 1 on at least one surface of a substrate layer.

4. A housing sealant formed from the adhesive resin molded article according to claim 2.

5. A housing sealant formed from the adhesive resin laminate according to claim 3.

Citation Information

Patent Citations

  • JP1974025029A

  • JP1974025030A

  • Laminate and cover material using it

    JP1997094905A

  • Adhesive sheet for sealing flat electrochemical cell metal terminal

    JP2009087628A

  • Resin film for terminal, tab using the same, and power storage device