Laminate and packaging container

The laminate structure with a polyethylene resin base and olefin elastomer enhances adhesion and gas barrier properties, addressing recyclability issues in packaging containers by preventing delamination and improving recyclability.

JP2024155979AActive Publication Date: 2024-10-31DAI NIPPON PRINTING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024144251
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-10-31
Estimated Expiration
2040-03-31

AI Technical Summary

Technical Problem

Conventional polyester and polyethylene film laminates used in packaging containers are difficult to separate and recycle, leading to poor recyclability due to insufficient adhesion between layers, especially when a vapor-deposited film is applied, which can result in delamination and reduced gas barrier properties.

Method used

A laminate structure is developed using a polyethylene resin base material with controlled stretching and incorporation of an olefin elastomer, enhancing adhesion and gas barrier properties by adjusting the density and composition of the polyethylene resin layers, including a vapor-deposited film.

Benefits of technology

The laminate achieves improved interlayer adhesion and gas barrier properties, enabling the production of monomaterial packaging containers that are suitable for recycling without delamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155979000001_ABST
    Figure 2024155979000001_ABST
Patent Text Reader

Abstract

To provide a laminate which is suitably usable for manufacturing a monomaterial packaging container, has high adhesion to a vapor-deposited film, can effectively prevent delamination when being formed into a packaging container, and has a high gas barrier property.SOLUTION: A laminate according to a first aspect includes at least a first sealant layer, a vapor-deposited film, a base material, a gas barrier layer, and a second sealant layer, wherein the base material includes a first polyethylene resin layer composed of a polyethylene resin having a density of 0.943 g / cm3 or less, the base material is subjected to drawing treatment, the vapor-deposited film is provided on the first polyethylene resin layer of the base material, and the first sealant layer and the second sealant layer are composed of a polyethylene resin.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate and a packaging container.

[0002] Conventionally, resin films made of polyester resins such as polyethylene terephthalate (hereinafter also referred to as polyester films) have been used as substrates constituting laminates used in the manufacture of packaging containers because they are excellent in mechanical properties, chemical stability, heat resistance and transparency, and are inexpensive.

[0003] Such polyester films are usually laminated with a polyethylene film, which is a sealant layer, to form a laminate, which is then formed into a packaging container.

[0004] The packaging containers made from the above-mentioned laminate of different resin films, i.e., a polyester film and a polyethylene film, are difficult to separate into their respective layers, and packaging containers collected after use are not suitable for recycling, and therefore are not actively recycled.

[0005] In order to improve the recyclability of packaging containers, studies are being conducted on the use of stretched polyethylene film (stretched polyethylene film) as the base material instead of polyester film, and the production of packaging containers using laminates made of the same material (mono-material packaging containers). Summary of the Invention [Problem to be solved by the invention]

[0006] Recently, the inventors attempted to form a vapor-deposited film on the surface of the stretched polyethylene film in order to compensate for the reduced gas barrier properties that result from changing from polyester film to stretched polyethylene film and to improve its design and gloss. However, they discovered a new problem in that the adhesion between the stretched polyethylene film and the vapor-deposited film was insufficient, and when a packaging container was produced using the stretched polyethylene film with the vapor-deposited film formed thereon, there was a risk of delamination occurring between the stretched polyethylene film and the vapor-deposited film.

[0007] Surprisingly, the present inventors have found that by adjusting the density of the polyethylene resin in the layer forming the vapor-deposited film of the substrate made of polyethylene resin, the adhesion between the layer and the vapor-deposited film can be significantly improved, thereby solving the above-mentioned problems.

[0008] Furthermore, the present inventors have surprisingly found that the adhesion between the layer and the vapor-deposited film of the substrate made of polyethylene resin can be significantly improved by adding an olefin-based elastomer together with the polyethylene resin to the layer forming the vapor-deposited film, and the above-mentioned problems can be solved. The reason why the adhesion to the vapor-deposited film is improved is not clear, but it is thought to be as follows. Normally, a polyethylene film that has been subjected to a stretching process has a decreased amount of amorphous components and an increased amount of oriented crystals, so that the adhesion between the film and a vapor-deposited film of aluminum or the like tends to decrease. In the present invention, it is believed that the oriented crystallization during stretching can be adjusted by adding an olefin-based elastomer together with the polyethylene resin, and the adhesion to the vapor-deposited film can be maintained.

[0009] The present invention has been made based on such findings, and the problem to be solved by the present invention is to provide a laminate that can be suitably used for producing mono-material packaging containers, has high adhesion to a vapor deposition film, can effectively prevent delamination when used as a packaging container, and has high gas barrier properties.

[0010] Another problem to be solved by the present invention is to provide a packaging container. [Means for solving the problem]

[0011] In a first aspect, the laminate of the present invention is a laminate including at least a first sealant layer, a vapor-deposited film, a substrate, a gas barrier layer, and a second sealant layer, in that order, The substrate has a density of at least 0.943 g / cm 3 The first polyethylene resin layer is made of the following polyethylene resin: The substrate is subjected to a stretching treatment, the vapor-deposited film is provided on a first polyethylene resin layer of the substrate, The first sealant layer and the second sealant layer are characterized in that they are made of a polyethylene resin.

[0012] In a second embodiment, the laminate of the present invention is a laminate including at least a first sealant layer, a vapor-deposited film, a substrate, a gas barrier layer, and a second sealant layer in this order, The substrate includes at least a first polyethylene resin layer composed of a polyethylene resin and an olefin-based elastomer resin, The substrate is subjected to a stretching treatment, the vapor-deposited film is provided on a first polyethylene resin layer of the substrate, The first sealant layer and the second sealant layer are characterized in that they are made of a polyethylene resin.

[0013] In one embodiment, the olefin-based elastomer resin is an ethylene-based elastomer resin.

[0014] In one embodiment, the olefin-based elastomer resin is an olefin-based block copolymer.

[0015] In one embodiment, the olefin-based block copolymer is an ethylene / α-olefin interpolymer.

[0016] In one embodiment, the olefin-based block copolymer comprises a hard block comprised of polyethylene and a soft block comprised of an α-olefin interpolymer.

[0017] In one embodiment, the content of the olefin-based elastomer resin in the first polyethylene resin layer is 1% by mass or more and 40% by mass or less.

[0018] In one embodiment, the gas barrier layer has a five-layer structure consisting of a first polyolefin resin layer, an adhesive resin layer, a layer containing a gas barrier resin, an adhesive resin layer, and a second polyolefin resin layer.

[0019] In one embodiment, the first polyolefin resin layer and the second polyolefin resin layer are composed of a polyethylene resin and a compatibilizer.

[0020] In one embodiment, the laminate of the present invention further comprises a barrier coat layer between the first sealant layer and the vapor-deposited film.

[0021] In one embodiment, the laminate of the present invention is used in a packaging container.

[0022] In one embodiment, the content of the polyethylene resin in the entire laminate is 90% by mass or more.

[0023] The packaging container of the present invention is characterized by comprising the above-mentioned laminate.

[0024] In one embodiment, the packaging container is a laminate tube. Effect of the Invention

[0025] According to the present invention, it is possible to provide a laminate which can be suitably used for producing a mono-material packaging container, can significantly improve the interlayer adhesion with a vapor-deposited film, and can achieve favorable gas barrier properties. Further, according to the present invention, a packaging container can be provided. [Brief description of the drawings]

[0026] [Figure 1] FIG. 1 is a schematic cross-sectional view showing one embodiment of a laminate 10 of the present invention. [Diagram 2] FIG. 1 is a schematic structural diagram illustrating an embodiment of a deposition apparatus. [Diagram 3] FIG. 1 is a front view showing a laminate tube 30, which is one embodiment of a packaging container of the present invention. [Figure 4] FIG. 4 is a cross-sectional view of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] (Laminate) A laminate 10 of the present invention includes at least a first sealant layer 11, a vapor-deposited film 12, a substrate 13, a gas barrier layer 14, and a second sealant layer 15, as shown in FIG. The substrate, the first sealant layer, and the second sealant layer of the laminate are made of the same resin, i.e., polyethylene resin, and a laminate having such a configuration can be suitably used as a laminate for producing a mono-material packaging container. Furthermore, the laminate of the present invention has significantly improved interlayer adhesion between the substrate and the deposited film, and has extremely high gas barrier properties.

[0028] The content of the polyethylene resin in the total amount of solids contained in the laminate is preferably 90% by mass or more, which makes the laminate suitable for use in producing mono-material packaging containers.

[0029] Each layer of the laminate 10 will now be described.

[0030] (base material) The substrate constituting the laminate of the present invention has a polyethylene resin layer, similar to the first and second sealant layers composed of a polyethylene resin described below. In this way, the substrate and the sealant layer are composed of the same resin material, so that the laminate can be used as a material with excellent recyclability for mono-material packaging containers, etc. The substrate may be a single layer or a multilayer as long as it has a polyethylene resin layer. In the case of a multilayer substrate, the substrate can be produced by a coextrusion method in which each polyolefin resin such as a polyethylene resin is heated and melted in a separate extruder, laminated in a molten state by a method such as a coextrusion multilayer die method or a feed block method, and then molded into a film by an inflation method, a T-die method, or the like.

[0031] For example, when the substrate has a multilayer structure formed by coextrusion, it may have, in order from the first polyethylene resin layer on the side in contact with the vapor-deposited film, second, third, fourth, etc. polyethylene resin layers (hereinafter sometimes referred to as "other polyethylene resin layers") The provision of the other polyethylene resin layers can improve the performance of the laminate, such as heat resistance, strength, transparency, and stretchability.

[0032] In the present invention, the substrate is characterized in that it has been subjected to a stretching treatment, which can improve the strength and heat resistance of the substrate, as well as the printability. The stretching process may be uniaxial stretching or biaxial stretching.

[0033] The stretching ratio of the substrate in the machine direction (MD direction) and the transverse direction (TD direction) is preferably 2 times or more and 15 times or less, and more preferably 3 times or more and 10 times or less. By setting the stretching ratio at 2 times or more, the strength and heat resistance of the substrate can be further improved. In addition, the printability of the substrate can be improved. From the viewpoint of the breaking limit of the substrate, the stretching ratio is preferably 15 times or less.

[0034] In the first embodiment, the substrate has a density of 0.943 g / cm as the layer on which the vapor-deposited film is formed. 3 The first polyethylene resin layer is made of the following polyethylene resin:

[0035] The density of the first polyethylene resin layer is 0.943 g / cm 3 The following polyethylene resin may be a biomass-derived polyethylene resin or a polyethylene resin recycled by mechanical recycling or chemical recycling.

[0036] Density of the first polyethylene resin layer: 0.943 g / cm 3 The content of the following polyethylene resin is preferably 50% by mass or more, more preferably 70% by mass or more, further preferably 80% by mass or more, and particularly preferably 90% by mass or more. Density of the first polyethylene resin layer: 0.943 g / cm 3 By making the content of the following polyethylene resin 50% by mass or more, the adhesion to the vapor-deposited film can be further significantly improved.

[0037] Density of the first polyethylene resin layer: 0.943 g / cm 3 The melting point of the following polyethylene resin is preferably 60° C. or higher and 135° C. or lower, and more preferably 65° C. or higher and 130° C. or lower. By making the melting point 60° C. or higher, the printability, strength, and heat resistance of the substrate can be further improved. By making the melting point 135° C. or lower, the difference in appropriate stretching temperature between each layer can be reduced.

[0038] Density of the first polyethylene resin layer: 0.943 g / cm 3 The MFR of the following polyethylene resin is preferably 0.1 g / 10 min to 5 g / 10 min, more preferably 0.2 g / 10 min to 4 g / 10 min. By setting the MFR to 0.1 g / 10 min to 5 g / 10 min, the film formability in the inflation method is stabilized.

[0039] The first polyethylene resin layer has a density of 0.943 g / cm within a range that does not impair the characteristics of the present invention. 3 The first polyethylene resin layer may contain the following resin materials (other resin materials) other than polyethylene resin: From the viewpoint of adhesion to the vapor-deposited film, it is preferable that the first polyethylene resin layer does not contain other resin materials. In addition, the first polyethylene resin layer may contain additives within the range that does not impair the characteristics of the present invention, such as crosslinking agents, antioxidants, antiblocking agents, slip agents, UV absorbers, light stabilizers, fillers, reinforcing agents, antistatic agents, pigments, and modifying resins.

[0040] In a second embodiment, the substrate comprises a first polyethylene resin layer composed of a polyethylene resin and an olefin-based elastomer resin.

[0041] As the polyethylene resin, high density polyethylene resin (HDPE), medium density polyethylene resin (MDPE), low density polyethylene resin (LDPE), linear low density polyethylene resin (LLDPE) and very low density polyethylene resin (VLDPE) can be used. Moreover, as the polyethylene resin, a copolymer of ethylene and another monomer can also be used. Furthermore, as the polyethylene resin, a biomass-derived polyethylene resin or a mechanically recycled or chemically recycled polyethylene resin can also be used.

[0042] The first polyethylene resin layer has a density of 0.970 g / cm 3 The first polyethylene resin layer may include a polyethylene resin having a density of 0.970 g / cm 3 By including the following polyethylene resin, the adhesion to the vapor-deposited film can be further improved significantly.

[0043] The melting point of the polyethylene resin contained in the first polyethylene resin layer is preferably 110° C. or more and 140° C. or less, and more preferably 115° C. or more and 135° C. or less. By setting the melting point to 110° C. or more, the processability during the preparation of the laminate is improved from the viewpoint of heat resistance. By setting the melting point to 140° C. or less, the difference in melting points between the layers in the multilayer structure is small, and stretching at a constant temperature tends to be easy.

[0044] The MFR of the polyethylene resin contained in the first polyethylene resin layer is preferably 0.1 g / 10 min to 5 g / 10 min, more preferably 0.2 g / 10 min to 4 g / 10 min. By setting the MFR to 0.1 g / 10 min to 5 g / 10 min, the film formability in the inflation method is stabilized.

[0045] The content of the polyethylene resin in the first polyethylene resin layer is preferably 60% by mass or more and 99% by mass or less, and more preferably 70% by mass or more and 95% by mass or less. When the content of the polyethylene resin in the first polyethylene resin layer is 60% by mass or more, a laminate that can be suitably used for producing a mono-material packaging container can be obtained. Furthermore, when the content of the polyethylene resin in the first polyethylene resin layer is 99% by mass or less, a sufficient amount of olefin-based elastomer resin can be contained in the first polyethylene resin layer, and adhesion with the vapor deposition film can be improved.

[0046] In one embodiment, the olefin-based elastomer resin is an ethylene-based elastomer resin. By using an ethylene-based elastomer resin as the olefin-based elastomer resin, the laminate of the present invention can be more suitably used for producing a mono-material packaging container.

[0047] In one embodiment, the olefin-based elastomer resin is an olefin-based block copolymer. By including an olefin-based block copolymer as the olefin-based elastomer resin in the first polyethylene resin layer, the adhesion between the vapor-deposited film and the first polyethylene resin layer can be further improved. A block copolymer comprises a sequence (block or segment) of the same monomer unit covalently bonded to a sequence of a different type. Block copolymer forms include, for example, a diblock structure AB and a triblock structure ABA (where A represents one block and B represents a different block or segment). In a multiblock copolymer, A and B can be connected in many different ways and repeated multiple times. They can also contain additional blocks or segments of different types. Multiblock copolymers can be linear multiblock polymers or multiblock star polymers (where all blocks or segments are bonded to the same atom or chemical moiety).

[0048] In one embodiment, the olefin-based block copolymer is an ethylene-based block copolymer, and preferably an ethylene-based multi-block copolymer. By using an ethylene-based block copolymer as the olefin-based block copolymer, the laminate of the present invention can be more suitably used for the production of a mono-material packaging container.

[0049] In one embodiment, the ethylene-based block copolymer is an ethylene / α-olefin interpolymer, and the use of the ethylene / α-olefin interpolymer can further improve the adhesion between the deposition film and the first polyethylene resin layer. The ethylene / α-olefin interpolymer includes ethylene and one or more copolymerizable α-olefin monomers in a polymerized form. The interpolymer means a polymer prepared by polymerization of at least two types of monomers. Thus, the interpolymer includes a copolymer that is a polymer of two types of monomers, a terpolymer that is a polymer of three types of monomers, and a polymer that is a polymer of four or more types of monomers.

[0050] In one embodiment, the ethylene / α-olefin interpolymer, which is an ethylene-based block copolymer, has a hard block (hard segment) composed of polyethylene and a soft block (soft segment) composed of an α-olefin monomer.

[0051] The α-olefin monomers constituting the interpolymer include propylene, 1-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-eicosene, cyclopentene, cycloheptene, norbornene, 5-methyl-2-norbornene, tetracyclododecene, 2-methyl-1,4,5,8-dimethano-1,2,3,4,4a,5,8,8a-octahydronaphthalene, butadiene, isoprene, 4-methyl-1,3-pentadiene, 1,3-pentadiene. , 1,4-pentadiene, 1,5-hexadiene, 1,4-hexadiene, 1,3-hexadiene, 1,3-octadiene, 1,4-octadiene, 1,5-octadiene, 1,6-octadiene, 1,7-octadiene, ethylidenenorbornene, vinylnorbornene, dicyclopentadiene, 7-methyl-1,6-octadiene, 4-ethylidene-8-methyl-1,7-nonadiene, 5,9-dimethyl-1,4,8-decatriene, 3-phenylpropene, 4-phenylpropene, 1,2-difluoroethylene, tetrafluoroethylene, styrene, and 3,3,3-trifluoro-1-propene.

[0052] The olefin-based elastomer resin may be a commercially available product. For example, INFUSE9100 manufactured by Dow Chemical may be used as an olefin-based block copolymer having a hard block composed of polyethylene and a soft block composed of an α-olefin monomer. Furthermore, Toughmer A-4085S manufactured by Mitsui Chemicals can also be used.

[0053] The content of the olefin-based elastomer resin in the first polyethylene resin layer is preferably 1% by mass or more and 40% by mass or less, and more preferably 5% by mass or more and 30% by mass or less. When the content of the olefin-based elastomer resin in the first polyethylene resin layer is 1% by mass or more, the adhesion between the first polyethylene resin layer and the vapor deposition film can be further improved. In addition, when the content of the olefin-based elastomer resin in the first polyethylene resin layer is 40% by mass or less, a laminate that can be suitably used for producing a mono-material packaging container can be obtained.

[0054] The first polyethylene resin layer may contain a resin material other than polyethylene resin (other resin material) within the range that does not impair the characteristics of the present invention. From the viewpoints of adhesion to the vapor deposition film and recyclability, it is preferable that the first polyethylene resin layer does not contain other resin materials. In addition, the first polyethylene resin layer may contain additives within the range that does not impair the characteristics of the present invention, such as crosslinking agents, antioxidants, antiblocking agents, slip agents, UV absorbers, light stabilizers, fillers, reinforcing agents, antistatic agents, pigments, and modifying resins.

[0055] The other polyethylene resin layers are made of polyethylene resin. As the polyethylene resin, high density polyethylene resin (HDPE), medium density polyethylene resin (MDPE), low density polyethylene resin (LDPE), linear low density polyethylene resin (LLDPE) and very low density polyethylene resin (VLDPE) can be used. Moreover, as the polyethylene resin, a copolymer of ethylene and another monomer can also be used. Furthermore, as the polyethylene resin, a biomass-derived polyethylene resin or a mechanically recycled or chemically recycled polyethylene resin can also be used.

[0056] In a substrate having a multilayer structure, the densities of the polyethylene resins constituting adjacent layers may be the same or different, i.e., the polyethylene resin layers constituting the substrate may have a density gradient. In a polyethylene resin layer having a density gradient, if the density difference between the layers is large, delamination may occur at the interface. Therefore, the density difference between the layers is set to 0.05 g / cm 3 It is preferable that the concentration is 0.04 g / cm or less. 3 It is even more preferable that:

[0057] (a) In one embodiment, the substrate having a multilayer structure has a five-layer structure including a first polyolefin resin layer, a second polyethylene resin layer composed of a medium-density polyethylene resin, a third polyethylene resin layer composed of a linear low-density polyethylene resin, a fourth polyethylene resin layer composed of a medium-density polyethylene resin, and a fifth polyolefin resin layer composed of a high-density polyethylene resin. (b) In one embodiment, the substrate having a multilayer structure has a seven-layer structure including a first polyethylene resin layer, a second resin layer composed of a blend resin of high-density polyethylene resin and medium-density polyethylene resin, a third polyethylene resin layer composed of medium-density polyethylene resin, a fourth polyethylene resin layer composed of a linear low-density polyethylene resin, a fifth polyethylene resin layer composed of medium-density polyethylene resin, a sixth resin layer composed of a blend resin of high-density polyethylene resin and medium-density polyethylene resin, and a seventh polyolefin resin layer composed of high-density polyethylene resin. (c) In one embodiment, the substrate having a multilayer structure has a three-layer structure including a first polyethylene resin layer, a second polyethylene resin layer composed of a linear low-density polyethylene resin, and a third polyolefin resin layer composed of a medium-density polyethylene resin. (d) In one embodiment, the substrate having a multilayer structure has a two-layer structure of a first polyethylene resin layer and a second polyolefin resin layer made of a medium-density polyethylene resin. (e) In one embodiment, the substrate having a multilayer structure has a five-layer structure including a first polyethylene resin layer containing an olefin-based elastomer resin, a second polyolefin resin layer composed of a medium-density polyethylene resin, a third polyolefin resin layer composed of a linear low-density polyethylene resin, a fourth polyolefin resin layer composed of a medium-density polyethylene resin, and a fifth polyolefin resin layer composed of an olefin-based elastomer resin and a medium-density polyethylene resin.

[0058] As an embodiment of the multilayered substrate by the co-extrusion method as described above, for example, each resin is heated and melted by an extruder, and a five-layer laminate consisting of the first to fifth polyethylene resin layers is formed by a feed block method, and then the laminate is formed into a tube by an inflation method, and the insides of the tube are pressed together by a rubber roll or the like to form a ten-layered multilayered film. The multilayered film thus obtained has a layer structure that is symmetrical from top to bottom in the cross-sectional thickness direction. That is, for example, when five layers consisting of the first to fifth polyethylene resin layers are laminated by a co-extruder, the obtained laminated film becomes a substrate having a ten-layered structure consisting of the first / second / third / fourth / fifth / fifth / fourth / third / second / first polyethylene resin layers in order from the surface. However, in reality, the two adjacent fifth polyethylene resin layers in the thickness cross-sectional direction can be regarded as one layer, so that the substrate can have a nine-layered multilayer structure consisting of the first / second / third / fourth / fifth / fourth / third / second / first polyethylene resin layers. The multilayer film obtained by such a manufacturing method is sometimes called a “block film.” According to the above-mentioned manufacturing method, the number of defective products in the manufacturing process can be significantly reduced, and ultimately, the production efficiency can be improved.

[0059] The substrate may have a printed layer on its surface. The image formed on the printed layer is not particularly limited, and may represent characters, patterns, symbols, combinations of these, and the like. The printing layer on the substrate can be formed using ink derived from biomass, which reduces the environmental impact. The method for forming the printed layer is not particularly limited, and examples of the method include conventionally known printing methods such as gravure printing, offset printing, and flexographic printing.

[0060] The substrate may be subjected to a surface treatment, which can improve adhesion to adjacent layers. The method of surface treatment is not particularly limited, and examples thereof include physical treatments such as corona discharge treatment, ozone treatment, low-temperature plasma treatment using oxygen gas and / or nitrogen gas, and glow discharge treatment, as well as chemical treatments such as oxidation treatment using chemicals.

[0061] The thickness of the substrate, whether it is a single-layer structure or a multi-layer structure, is preferably 1 μm or more and 60 μm or less, more preferably 9 μm or more and 60 μm or less, and even more preferably 12 μm or more and 50 μm or less. By making the thickness of the substrate 1 μm or more, the heat resistance and strength of the substrate can be improved. By making the thickness of the substrate 60 μm or less, the processability of the substrate can be improved.

[0062] (evaporated film) The laminate has a vapor-deposited film on the first polyethylene resin layer of the substrate, which can improve the gas barrier properties of the laminate, specifically the oxygen barrier properties and water vapor barrier properties.

[0063] The vapor-deposited film may be composed of a metal or an inorganic oxide, but a vapor-deposited film composed of a metal (hereinafter referred to as a metal vapor-deposited film) is preferred because it can impart a glossy appearance to a container produced using the laminate of the present invention and improve its design. Examples of metals that can be used to form the metal vapor deposition film include aluminum, chromium, tin, nickel, copper, silver, gold, and platinum. Examples of the metal oxide include aluminum oxide, silicon oxide, magnesium oxide, calcium oxide, zirconium oxide, titanium oxide, boron oxide, hafnium oxide, and barium oxide.

[0064] Among the above, aluminum is particularly preferred because it has high gas barrier properties and can impart a good glossy feel.

[0065] The surface of the deposited film is preferably subjected to the above-mentioned surface treatment, which can improve adhesion to adjacent layers.

[0066] The thickness of the evaporated film is preferably 1 nm or more and 150 nm or less, more preferably 5 nm or more and 60 nm or less, and even more preferably 10 nm or more and 40 nm or less. By making the thickness of the vapor-deposited film 1 nm or more, the gas barrier properties and gloss of the laminate 20 can be further improved. Moreover, by setting the thickness of the vapor-deposited film to 150 nm or less, a laminate that can be suitably used for producing mono-material packaging containers can be obtained, and further, the occurrence of cracks in the vapor-deposited film can be prevented.

[0067] The method for forming the vapor-deposited film may be a conventional method, for example, a physical vapor deposition method (PVD method) such as a vacuum deposition method, a sputtering method, or an ion plating method, or a chemical vapor deposition method (CVD method) such as a plasma chemical vapor deposition method, a thermal chemical vapor deposition method, or a photochemical vapor deposition method. Hereinafter, one embodiment of the method for forming the evaporated film will be described, but the method for forming the evaporated film is not limited thereto.

[0068] Specifically, the deposition film can be formed by using (1) a vacuum deposition method in which a metal or metal oxide is used as a raw material, heated to vaporize it, and then deposited on the first polyethylene resin layer of the substrate, (2) an oxidation reaction deposition method in which a metal or metal oxide is used as a raw material, oxidized by introducing oxygen, and then deposited on the first polyethylene resin layer of the substrate, and (3) a plasma-assisted oxidation reaction deposition method in which the oxidation reaction is assisted by plasma, etc. In the above, the deposition material can be heated by, for example, a resistance heating method, a high-frequency induction heating method, an electron beam heating method (EB), etc.

[0069] A method for forming a vapor-deposited film of an inorganic substance or an inorganic oxide by physical vapor deposition will be described below. Fig. 2 is a schematic diagram showing an example of a take-up type vacuum deposition apparatus. As shown in Fig. 2, in a vacuum chamber B of a take-up type vacuum deposition apparatus A, a substrate X unwound from a winding roll C is guided to a cooled coating drum F via guide rolls D and E. In one embodiment, the device A has a plasma treatment device G disposed between the guide roll E and a cooled coating drum F. The plasma treatment device G irradiates a plasma gas onto the surface of the first polyethylene resin layer of the substrate X, thereby subjecting the surface of the first polyethylene resin layer of the substrate X to plasma treatment before the deposition film is formed. Next, the deposition source I (e.g., aluminum metal or aluminum oxide) heated and evaporated in the crucible H is deposited on the first polyethylene resin layer of the substrate guided onto the cooled coating drum F to form a deposition film. The deposition of the deposition source I may be performed through masks J, J, and further, if necessary, may be performed while blowing oxygen gas or the like from an oxygen gas blowing port K. Next, the substrate X on which the vapor-deposited film has been formed is sent out via guide rolls L and M, and taken up on a take-up roll N, thereby completing the vapor-deposited film formation by this apparatus. The above steps may be repeated to form a multi-layered deposition film made of different materials. The multi-layered deposition film may be formed by using the above apparatus multiple times, or by using an apparatus in which multiple apparatuses are connected together. The formation of such a vapor-deposited film is disclosed in, for example, Japanese Patent No. 4569982.

[0070] (First and second sealant layers) In one embodiment, the first and second sealant layers can be formed of a resin material that can be fused to each other by heat, and examples of such resins include low-density polyethylene resin (LDPE), medium-density polyethylene resin (MDPE) resin, high-density polyethylene resin (HDPE), linear low-density polyethylene resin (LLDPE), ethylene-α-olefin copolymers polymerized using a metallocene catalyst, random or block copolymers of ethylene and polypropylene, polypropylene resin, ethylene-vinyl acetate copolymer (EVA), ethylene-acrylic acid copolymer (EAA), ethylene-ethyl acrylate copolymer (EEA), ethylene-methacrylic acid copolymer (EMAA), ethylene-methyl methacrylate copolymer (EMMA), ionomer resins, heat-sealable ethylene-vinyl alcohol resins, and acid-modified versions of these polyolefin resins, vinyl resins, and (meth)acrylic resins. Of the above, polyethylene resin is particularly preferred because it can produce a laminate 20 that can be suitably used for producing a mono-material packaging container.

[0071] The content of the polyethylene resin in the sealant layer is preferably 80% by mass or more, and more preferably 90% by mass or more, which makes it possible to obtain a laminate that can be suitably used for producing a mono-material packaging container.

[0072] The sealant layer may contain the above-mentioned additives as long as the characteristics of the present invention are not impaired.

[0073] The sealant layer may have a single-layer structure or a multi-layer structure.

[0074] The thickness of the sealant layer is preferably 20 μm or more and 100 μm or less, and more preferably 30 μm or more and 70 μm or less. By making the thickness of the sealant layer 20 μm or more, the laminate strength of the packaging container can be further improved. Furthermore, by setting the thickness of the sealant layer to 100 μm or less, the moldability of the laminate can be improved, and the packaging container can be produced more easily.

[0075] The first sealant layer and the second sealant layer may have the same configuration or may have different configurations.

[0076] The sealant layer can be produced by extruding the above-mentioned material into a film by a conventionally known method such as a T-die method or an inflation method.

[0077] The sealant layer can be laminated via a conventionally known adhesive or a molten resin layer.

[0078] (Gas barrier layer) The laminate of the present invention includes a gas barrier layer, which can improve the gas barrier properties of the laminate of the present invention.

[0079] The gas barrier layer includes at least a layer containing a gas barrier resin, such as ethylene-vinyl alcohol copolymer (EVOH), polyvinyl alcohol, polyacrylonitrile, polyamides such as nylon 6, nylon 6,6, and polymetaxylylene adipamide (MXD6), polyesters, polyurethanes, and (meth)acrylic resins, and among these, EVOH is preferred from the viewpoints of oxygen barrier properties and water vapor barrier properties.

[0080] The content of the gas barrier resin in the layer containing the gas barrier resin is preferably 50% by mass or more, and more preferably 75% by mass or more. By adjusting the content of the gas barrier resin in the layer containing the gas barrier resin to 50% by mass or more, the oxygen barrier property and water vapor barrier property of the laminate of the present invention can be further improved.

[0081] The layer containing the gas barrier resin may contain the above-mentioned additives to the extent that the characteristics of the present invention are not impaired.

[0082] The thickness of the layer containing a gas barrier resin is preferably 0.5 μm or more and 20 μm or less, and more preferably 1 μm or more and 16 μm or less. By making the thickness of the layer containing the gas barrier resin 0.5 μm or more, the oxygen barrier property and water vapor barrier property of the laminate of the present invention can be improved, and by making the thickness of the layer containing the gas barrier resin 20 μm or less, the laminate can be made suitable for use in the production of mono-material packaging containers.

[0083] In one embodiment, the gas barrier layer has a multi-layer structure. In one embodiment, the gas barrier layer 14 has a five-layer structure including a first polyolefin resin layer 16, an adhesive resin layer 17, a layer 18 containing a gas barrier resin, an adhesive resin layer 19, and a second polyolefin resin layer 20, as shown in FIG.

[0084] (First and second polyolefin resin layers) The first and second polyolefin resin layers are made of polyolefins, such as polyethylene resins, polypropylene resins, polymethylpentene, ethylene-propylene copolymers, and propylene-butene copolymers. Of these, polyethylene resins are preferred from the viewpoint of recyclability.

[0085] In one embodiment, the first and second polyolefin resin layers contain a compatibilizer, which can effectively prevent the gas barrier resin and the polyethylene resin from being mixed uniformly and causing a deterioration in the physical properties and transparency when the packaging container produced using the laminate of the present invention is heated and melted for recycling.

[0086] The compatibilizer may be appropriately selected from conventionally known ones and used. From the viewpoint of recyclability, however, unsaturated carboxylic acid modified polyolefin resins are preferred, and among them, maleic anhydride modified polyethylene resins are more preferred.

[0087] The content of the compatibilizer in the first and second polyolefin resin layers is preferably 5% by mass or more and 30% by mass or less. By setting the content of the compatibilizer in the first and second polyolefin resin layers to 5% by mass or more, the above-mentioned effects can be further improved. By setting the content of the compatibilizer in the first and second polyolefin resin layers to 30% by mass or less, the strength and heat resistance of the substrate can be improved.

[0088] As long as the characteristics of the present invention are not impaired, the first and second polyethylene resin layers may contain a resin material other than a polyolefin resin, such as (meth)acrylic resin, vinyl resin, cellulose resin, polyamide resin, polyester resin, and ionomer resin. From the viewpoint of recyclability, it is particularly preferable that the first and second polyolefin resin layers contain no resin other than polyethylene resin.

[0089] Furthermore, the first and second polyethylene resin layers may contain the above-mentioned additives, provided that the characteristics of the present invention are not impaired.

[0090] The thickness of the first and second polyolefin resin layers is preferably 5 μm or more and 100 μm or less, more preferably 10 μm or more and 50 μm or less. By making the thickness of the polyolefin resin layer 5 μm or more, the strength and heat resistance of the laminate of the present invention can be improved. By making the thickness of the polyolefin resin layer 100 μm or less, the processability of the laminate of the present invention can be improved.

[0091] The first and second polyolefin resin layers may have the same or different configurations.

[0092] (adhesive resin layer) The adhesive resin layer contains at least one resin material, for example, polyolefin resin, modified polyolefin resin, polyester resin, vinyl resin, polyamide resin, etc. Among these, polyolefin resin and modified polyolefin resin are preferred from the viewpoint of adhesion.

[0093] The adhesive resin layer may contain the above-mentioned additives within the range that does not impair the characteristics of the present invention.

[0094] The thickness of the adhesive resin is preferably 0.5 μm or more and 10 μm or less, and more preferably 1 μm or more and 5 μm or less. By making the adhesive resin layer 0.5 μm or more thick, the adhesion between the gas barrier resin layer and the polyolefin resin layer can be improved, and by making the adhesive resin layer 10 μm or less thick, the laminate can be suitably used for producing a mono-material packaging container.

[0095] The gas barrier layer can be produced by extrusion film formation of the above-mentioned materials by a conventionally known method such as a T-die method or an inflation method.

[0096] The gas barrier layer can be laminated via a conventionally known adhesive or a molten resin layer.

[0097] (Barrier coat layer) The laminate of the present invention may further include a barrier coat layer on the vapor-deposited film (between the first sealant layer and the vapor-deposited film, or between the vapor-deposited film and the substrate), thereby improving the gas barrier properties of the laminate.

[0098] In one embodiment, the barrier coat layer is composed of a gas barrier resin such as an ethylene-vinyl alcohol copolymer (EVOH), polyvinyl alcohol, polyacrylonitrile, polyamide resins such as nylon 6, nylon 6,6 and polymetaxylylene adipamide (MXD6), polyester resin, polyurethane resin, and (meth)acrylic resin.

[0099] The thickness of the barrier coat layer is preferably 0.01 μm or more and 10 μm or less, and more preferably 0.1 μm or more and 5 μm or less. By making the thickness of the barrier coat layer 0.01 μm or more, the gas barrier property can be further improved. By making the thickness of the barrier coat layer 10 μm or less, the processability of the laminate can be improved. In addition, the laminate can be suitably used for producing a mono-material packaging container.

[0100] The barrier coat layer can be formed by dissolving or dispersing the above-mentioned material in water or an appropriate solvent, applying the solution or dispersion, and drying the solution.

[0101] In another embodiment, the barrier coat layer is a gas barrier coating film containing at least one resin composition such as a hydrolysate of a metal alkoxide or a hydrolyzed condensate of a metal alkoxide obtained by polycondensing a mixture of a metal alkoxide and a water-soluble polymer by a sol-gel method in the presence of a sol-gel catalyst, water, an organic solvent, etc. By providing such a barrier coat layer on the vapor-deposited film, the occurrence of cracks in the vapor-deposited film can be effectively prevented.

[0102] In one embodiment, the metal alkoxide is represented by the following general formula: R 1 n M(OR 2 ) m (In the formula, R 1 , R 2 each represents an organic group having 1 to 8 carbon atoms, M represents a metal atom, n represents an integer of 0 or more, m represents an integer of 1 or more, and n+m represents the atomic valence of M.

[0103] As the metal atom M, for example, silicon, zirconium, titanium, aluminum, etc. can be used. Also, R 1 and R 2 Examples of the organic group represented by the formula (I) include alkyl groups such as a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, and an i-butyl group.

[0104] Examples of metal alkoxides that satisfy the above general formula include tetramethoxysilane (Si(OCH 3 ) 4 ), tetraethoxysilane (mass%) Si(OC 2 H 5 ) 4 ), tetrapropoxysilane (Si(OC 3 H 7 ) 4 ), tetrabutoxysilane (Si(OC 4 H 9 ) 4 ) etc.

[0105] It is also preferable to use a silane coupling agent together with the metal alkoxide. As the silane coupling agent, a known organoalkoxysilane containing an organic reactive group can be used.

[0106] As the water-soluble polymer, polyvinyl alcohol and an ethylene-vinyl alcohol copolymer are preferred, and from the viewpoints of oxygen barrier properties, water vapor barrier properties, water resistance and weather resistance, it is preferred to use these in combination.

[0107] The thickness of the gas barrier coating film is preferably from 0.01 μm to 10 μm, and more preferably from 0.1 μm to 5 μm, which can further improve the gas barrier properties. By making the thickness of the gas barrier coating film 0.01 μm or more, the oxygen barrier property and water vapor barrier property of the barrier laminate can be improved, and the occurrence of cracks in the vapor-deposited film can be prevented. By setting the thickness of the gas barrier coating film to 10 μm or less, it is possible to obtain a laminate 20 that can be suitably used for producing mono-material packaging containers.

[0108] The gas barrier coating film can be formed by applying a composition containing the above-mentioned materials by a conventionally known means such as roll coating using a gravure roll coater or the like, spray coating, spin coating, dipping, brushing, bar coding, or an applicator, and then polycondensing the composition by a sol-gel method. As the sol-gel catalyst, an acid or an amine compound is preferable.

[0109] The composition may further contain an acid, which is used as a catalyst in the sol-gel process, mainly for the hydrolysis of alkoxides, silane coupling agents, and the like. As the acid, mineral acids such as sulfuric acid, hydrochloric acid, nitric acid, etc., and organic acids such as acetic acid, tartaric acid, etc. can be used.

[0110] The composition may also contain an organic solvent, such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, or n-butanol.

[0111] Hereinafter, one embodiment of the method for forming a gas barrier coating film will be described. First, a composition is prepared by mixing a metal alkoxide, a water-soluble polymer, a sol-gel catalyst, water, an organic solvent, and optionally a silane coupling agent, etc. In the composition, a polycondensation reaction gradually proceeds. Next, the composition is applied onto the deposition film by the above-mentioned conventionally known method and dried. This drying causes the polycondensation reaction of the alkoxide and the water-soluble polymer (and the silane coupling agent if the composition contains a silane coupling agent) to proceed further, forming a layer of a composite polymer. Finally, the gas barrier coating film can be formed by heating.

[0112] (packaging container) The packaging container of the present invention is characterized by comprising the sealant laminate 30 described above.

[0113] Specific examples of the packaging container of the present invention include laminate tubes, packaging bags, and lids.

[0114] (Laminated tube) In one embodiment, the packaging container of the present invention is a laminate tube 30. The laminate tube 30 of the present invention will be described below with reference to the drawings. Fig. 3 is a diagram showing a simplified configuration of the laminate tube 30, and Fig. 4 is a cross-sectional view taken along line aa in Fig. 3. As shown in Fig. 3, the laminate tube 30 is characterized in that it comprises a laminate tube body 31 having a head 32 and a body 33, and the body 33 is formed from the laminated body described above.

[0115] (head) The head portion 32 has a shoulder portion 34 connected to one end of the body portion 33 and a sampling port portion 35 connected to the shoulder portion 34. In one embodiment, the spout portion 35 includes a thread 37 for screwing the cap 36 thereon.

[0116] In one embodiment, the head 32 is made of a polyethylene resin, which can improve the recyclability of the laminate tube. The polyethylene resin may be a high-density polyethylene resin, a medium-density polyethylene resin, a low-density polyethylene resin, a linear low-density polyethylene resin, or an ultra-low-density polyethylene resin. Among these, high density polyethylene resin is preferred from the viewpoint of shape retention. Moreover, as the polyethylene resin, a polyethylene resin derived from biomass or a polyethylene resin recycled by mechanical recycling or chemical recycling can be used. The head 43 may contain the above-mentioned additives as long as the characteristics of the present invention are not impaired.

[0117] The method for producing the head 32 is not particularly limited, and the head 32 may be produced by a conventionally known method. For example, the head 32 may be produced by a compression molding method or an injection molding method, and may be joined to the body portion.

[0118] When the laminated tube 30 is manufactured using the compression molding method, the body 33 is attached to a male mold having a convex portion on the top, the male and female molds are then opposed to each other, and a material such as molten polyethylene resin is supplied into the male and female molds. The head 32 is formed by compression molding, and the head 32 is joined to one opening of the body 33, thereby manufacturing the laminated tube 30 consisting of the head 32 and the body 33. Furthermore, when the laminated tube 30 is manufactured using an injection molding method, the body 33 is attached to a male mold having a convex portion on the top, the male mold and female mold are then opposed to each other, and a material such as molten polyethylene resin is supplied from a gate, and the head 32 is formed by injection molding and joined to one opening of the body 33, thereby producing a laminated tube consisting of the head 32 and the body 33.

[0119] (Torso) In the laminate tube body 31 of the present invention, the trunk portion 33 is connected to a shoulder portion 34 of the head portion 32 . The body 33 can be obtained by rolling the laminate into a cylindrical shape, overlapping the first sealant layer and the second sealant layer, and heat-sealing the polymerized portion to form a welded portion 38. The body 33 also includes a bottom seal 39 formed by heat sealing the opening of the rolled laminate.

[0120] Heat sealing can be performed by a conventional method such as bar sealing, rotary roll sealing, belt sealing, impulse sealing, high frequency sealing, ultrasonic sealing, or flame sealing.

[0121] (cap) The laminate tube 30 may include a cap 36 . The cap is removably attached to the extraction port of the head and serves to close the extraction port. The cap is made of a thermoplastic resin. Examples of the thermoplastic resin include polyolefin resins such as polyethylene and polypropylene, polyester, cellulose resin, and vinyl resin, with polyethylene resin being particularly preferred from the viewpoint of recyclability. Furthermore, the cap 36 may contain the above-mentioned additives as long as the characteristics of the present invention are not impaired.

[0122] The cap may be a screw type having a groove on the inner surface of cap 36 so as to screw into threaded thread 37 of extraction port 35, as shown in FIG. 3, or it may be a plug type which fits into extraction port 37 by plugging it. EXAMPLES

[0123] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. The materials used in the following examples are as follows: Polyethylene resin A: Dow Chemical, ELITE5960G, HDPE, density 0.962g / cm 3 , melting point 134℃, MFR 0.85g / 10min Polyethylene resin B: Dow Chemical, ELITE5538G, MDPE, density 0.941g / cm 3 , melting point 129℃, MFR 1.3g / 10min Polyethylene resin C: Dow Chemical, Affinity PL1880G, m-C8-LLDPE, density 0.902g / cm 3 , Melting point 99℃, MFR 1.0g / 10min Olefin elastomer resin A: Dow Chemical Co., INFUSE9100, olefin block copolymer (with polyethylene as the hard block and α-olefin elastomer resin as the soft block), density 0.877g / cm 3 , Melting point 120℃, MFR 1.0g / 10min

[0124] Example 1-1 Polyethylene resin B was co-extruded by inflation molding to form a two-layer film consisting of a first polyethylene resin layer (10 μm) and a second polyethylene resin layer (115 μm). This film was stretched 5 times in the machine direction (MD) to obtain a stretched substrate having a thickness of 25 μm. After stretching, the first polyethylene resin layer had a thickness of 2 μm, and the second polyethylene resin layer had a thickness of 23 μm.

[0125] On the surface of the first polyethylene resin layer of the stretched substrate prepared as described above, an Al vapor deposition film having a thickness of 30 nm was formed by PVD to obtain a vapor deposition substrate. The optical density (OD value) of the vapor deposition film formed was measured and found to be 3.0.

[0126] As the first sealant layer, Linear low-density polyethylene resin D (Dow Chemical, Dowlex 2098P, density 0.926 g / cm 3 )and, High density polyethylene resin (Hi-Zex 3300F, manufactured by Prime Polymer Co., Ltd., density 0.950 g / cm 3 )and, Linear low-density polyethylene resin D (Dow Chemical, Dowlex 2098P, density 0.926 g / cm 3 )and, The mixture was co-extruded by an inflation method to obtain a first sealant layer having a thickness of 100 μm. In the first sealant layer thus obtained, the layer composed of linear low density polyethylene resin D had a thickness of 20 μm, the layer composed of high density polyethylene resin had a thickness of 60 μm, and the layer composed of linear low density polyethylene resin D had a thickness of 20 μm.

[0127] A urethane adhesive (RU004 / H1, manufactured by Rock Paint) was applied to the vapor deposition surface of the substrate and dried to form an adhesive layer 3 μm thick. The layer composed of linear low-density polyethylene resin D of the first sealant layer was then bonded to the substrate through this adhesive layer.

[0128] Linear low-density polyethylene resin E (Dow Chemical, Dowlex 2045G, density 0.920 g / cm 3 )and, Adhesive resin (Mitsui Chemicals, Admer NF557, density 0.903 g / cm 3 )and, Ethylene-vinyl alcohol copolymer (Kuraray Co., Ltd., EVAL H171B, density 1.17 g / cm 3 , ethylene content 38 mol%); Adhesive resin (Mitsui Chemicals, Admer NF557, density 0.903 g / cm 3 )and, Linear low-density polyethylene resin E (Dow Chemical, Dowlex 2045G, density 0.920 g / cm 3 )and, The gas barrier layer was obtained by co-extrusion of five layers of the mixture using the inflation method. The gas barrier layer obtained as described above had a five-layer structure with a total thickness of 60 μm, including a 17.5 μm-thick layer composed of linear low-density polyethylene resin E, a 5 μm-thick layer composed of adhesive resin, a 15 μm-thick layer composed of ethylene-vinyl alcohol copolymer, a 5 μm-thick layer composed of adhesive resin, and a 17.5 μm-thick layer composed of linear low-density polyethylene resin E.

[0129] A low-density polyethylene film (Novatec LC600A, density 0.918 g / cm, manufactured by Japan Polyethylene Corporation) was applied to the non-deposited film of the substrate. 3 ) was melt-extruded to form a melt-extruded polyethylene layer having a thickness of 20 μm, and the layer side of the gas barrier layer composed of linear low density polyethylene resin E was laminated via this melt-extruded polyethylene layer.

[0130] As a second sealant layer, Linear low-density polyethylene resin D (Dow Chemical, Dowlex 2098P, density 0.926 g / cm 3 )and, High density polyethylene resin (Prime Polymer, Hi-Zex 3300F, density 0.950g / cm 3 )and, Linear low-density polyethylene resin D (Dow Chemical, Dowlex 2098P, density 0.926 g / cm 3 )and, The mixture was co-extruded by an inflation method to obtain a second sealant layer having a thickness of 100 μm. In the second sealant layer thus obtained, the layer composed of linear low density polyethylene resin D had a thickness of 20 μm, the layer composed of high density polyethylene resin had a thickness of 60 μm, and the layer composed of linear low density polyethylene resin D had a thickness of 20 μm.

[0131] A low-density polyethylene resin (Novatec LC600A, density 0.918 g / cm, manufactured by Japan Polyethylene Corporation) was placed on the layer composed of the other linear low-density polyethylene resin E of the gas barrier layer.3 ) was melt-extruded to form a melt-extruded polyethylene layer having a thickness of 20 μm, and the layer composed of linear low density polyethylene resin D of the second sealant layer was bonded to the melt-extruded polyethylene layer through this melt-extruded polyethylene layer to obtain a laminate of the present invention. The polyethylene content in this laminate was 90% by mass.

[0132] Examples 1-2 to 1-5 Except for changing the configuration of the first polyethylene resin layer as shown in Table 1, a laminate was produced in the same manner as in Example 1-1. [Table 1]

[0133] Example 2-1 Polyethylene resin B was coextruded by inflation molding to form a three-layer film consisting of a first polyethylene resin layer (10 μm), a second polyethylene resin layer (105 μm), and a third polyethylene resin layer (10 μm). This film was stretched 5 times in the machine direction (MD) to obtain a stretched substrate having a thickness of 25 μm. After stretching, the first polyethylene resin layer had a thickness of 2 μm, the second polyethylene resin layer had a thickness of 21 μm, and the third polyethylene resin layer had a thickness of 2 μm.

[0134] On the surface of the first polyethylene resin layer of the stretched substrate prepared as described above, an Al vapor deposition film having a thickness of 30 nm was formed by PVD to obtain a vapor deposition substrate. The optical density (OD value) of the vapor deposition film formed was measured and found to be 3.0.

[0135] As the first sealant layer, Linear low-density polyethylene resin D (Dow Chemical, Dowlex 2098P, density 0.926 g / cm 3 )and, High density polyethylene resin (Hi-Zex 3300F, manufactured by Prime Polymer Co., Ltd., density 0.950 g / cm 3 )and, Linear low-density polyethylene resin D (Dow Chemical, Dowlex 2098P, density 0.926 g / cm 3 )and, The mixture was co-extruded by an inflation method to obtain a first sealant layer having a thickness of 100 μm. In the first sealant layer thus obtained, the layer composed of linear low density polyethylene resin D had a thickness of 20 μm, the layer composed of high density polyethylene resin had a thickness of 60 μm, and the layer composed of linear low density polyethylene resin D had a thickness of 20 μm.

[0136] A urethane adhesive (RU004 / H1, manufactured by Rock Paint) was applied to the vapor deposition surface of the substrate and dried to form an adhesive layer 3 μm thick. The layer composed of linear low-density polyethylene resin D of the first sealant layer was then bonded to the substrate through this adhesive layer.

[0137] Linear low-density polyethylene resin E (Dow Chemical, Dowlex 2045G, density 0.920 g / cm 3 )and, Adhesive resin (Mitsui Chemicals, Admer NF557, density 0.903 g / cm 3 )and, Ethylene-vinyl alcohol copolymer (Kuraray Co., Ltd., EVAL H171B, density 1.17 g / cm 3 , ethylene content 38 mol%); Adhesive resin (Mitsui Chemicals, Admer NF557, density 0.903 g / cm 3 )and, Linear low-density polyethylene resin E (Dow Chemical, Dowlex 2045G, density 0.920 g / cm 3 )and, The gas barrier layer was obtained by co-extrusion of five layers of the mixture using the inflation method. The gas barrier layer obtained as described above had a five-layer structure with a total thickness of 60 μm, including a 17.5 μm-thick layer composed of linear low-density polyethylene resin E, a 5 μm-thick layer composed of adhesive resin, a 15 μm-thick layer composed of ethylene-vinyl alcohol copolymer, a 5 μm-thick layer composed of adhesive resin, and a 17.5 μm-thick layer composed of linear low-density polyethylene resin E.

[0138] A low-density polyethylene film (Novatec LC600A, density 0.918 g / cm, manufactured by Japan Polyethylene Corporation) was applied to the non-deposited film of the substrate. 3 ) was melt-extruded to form a melt-extruded polyethylene layer having a thickness of 20 μm, and the layer side of the gas barrier layer composed of linear low density polyethylene resin E was laminated via this melt-extruded polyethylene layer.

[0139] As a second sealant layer, Linear low-density polyethylene resin D (Dow Chemical, Dowlex 2098P, density 0.926 g / cm 3 )and, High density polyethylene resin (Prime Polymer, Hi-Zex 3300F, density 0.950g / cm 3 )and, Linear low-density polyethylene resin D (Dow Chemical, Dowlex 2098P, density 0.926 g / cm 3 )and, The mixture was co-extruded by an inflation method to obtain a second sealant layer having a thickness of 100 μm. In the second sealant layer thus obtained, the layer composed of linear low density polyethylene resin D had a thickness of 20 μm, the layer composed of high density polyethylene resin had a thickness of 60 μm, and the layer composed of linear low density polyethylene resin D had a thickness of 20 μm.

[0140] A low-density polyethylene resin (Novatec LC600A, density 0.918 g / cm, manufactured by Japan Polyethylene Corporation) was placed on the layer composed of the other linear low-density polyethylene resin E of the gas barrier layer.3 ) was melt-extruded to form a melt-extruded polyethylene layer having a thickness of 20 μm, and the layer composed of linear low density polyethylene resin D of the second sealant layer was bonded to the melt-extruded polyethylene layer through this melt-extruded polyethylene layer to obtain a laminate of the present invention. The polyethylene content in this laminate was 90% by mass.

[0141] Examples 2-2 to 2-5 Except for changing the configurations of the first and third polyethylene resin layers as shown in Table 2, a laminate was produced in the same manner as in Example 2-1. [Table 2]

[0142] Example 3-1 Polyethylene resin B was extruded into a single layer by inflation molding to obtain a film consisting of a first polyethylene resin layer (125 μm). This film was stretched 5 times in the machine direction (MD) to obtain a stretched substrate having a thickness of 25 μm.

[0143] On the surface of the first polyethylene resin layer of the stretched substrate prepared as described above, an Al vapor deposition film having a thickness of 30 nm was formed by PVD to obtain a vapor deposition substrate. The optical density (OD value) of the vapor deposition film formed was measured and found to be 3.0.

[0144] As the first sealant layer, Linear low-density polyethylene resin D (Dow Chemical, Dowlex 2098P, density 0.926 g / cm 3 )and, High density polyethylene resin (Hi-Zex 3300F, manufactured by Prime Polymer Co., Ltd., density 0.950 g / cm 3 )and, Linear low-density polyethylene resin D (Dow Chemical, Dowlex 2098P, density 0.926 g / cm 3 )and, The mixture was co-extruded by an inflation method to obtain a first sealant layer having a thickness of 100 μm. In the first sealant layer thus obtained, the layer composed of linear low density polyethylene resin D had a thickness of 20 μm, the layer composed of high density polyethylene resin had a thickness of 60 μm, and the layer composed of linear low density polyethylene resin D had a thickness of 20 μm.

[0145] A urethane adhesive (RU004 / H1, manufactured by Rock Paint) was applied to the vapor deposition surface of the substrate and dried to form an adhesive layer 3 μm thick. The layer composed of linear low-density polyethylene resin D of the first sealant layer was then bonded to the substrate through this adhesive layer.

[0146] Linear low-density polyethylene resin E (Dow Chemical, Dowlex 2045G, density 0.920 g / cm 3 )and, Adhesive resin (Mitsui Chemicals, Admer NF557, density 0.903 g / cm 3 )and, Ethylene-vinyl alcohol copolymer (Kuraray Co., Ltd., EVAL H171B, density 1.17 g / cm 3 , ethylene content 38 mol%); Adhesive resin (Mitsui Chemicals, Admer NF557, density 0.903 g / cm 3 )and, Linear low-density polyethylene resin E (Dow Chemical, Dowlex 2045G, density 0.920 g / cm 3 )and, The gas barrier layer was obtained by co-extrusion of five layers of the mixture using the inflation method. The gas barrier layer obtained as described above had a five-layer structure with a total thickness of 60 μm, including a 17.5 μm-thick layer composed of linear low-density polyethylene resin E, a 5 μm-thick layer composed of adhesive resin, a 15 μm-thick layer composed of ethylene-vinyl alcohol copolymer, a 5 μm-thick layer composed of adhesive resin, and a 17.5 μm-thick layer composed of linear low-density polyethylene resin E.

[0147] A low-density polyethylene film (Novatec LC600A, density 0.918 g / cm, manufactured by Japan Polyethylene Corporation) was applied to the non-deposited film of the substrate. 3 ) was melt-extruded to form a melt-extruded polyethylene layer having a thickness of 20 μm, and the layer side of the gas barrier layer composed of linear low density polyethylene resin E was laminated via this melt-extruded polyethylene layer.

[0148] As a second sealant layer, Linear low-density polyethylene resin D (Dow Chemical, Dowlex 2098P, density 0.926 g / cm 3 )and, High density polyethylene resin (Prime Polymer, Hi-Zex 3300F, density 0.950g / cm 3 )and, Linear low-density polyethylene resin D (Dow Chemical, Dowlex 2098P, density 0.926 g / cm 3 )and, The mixture was co-extruded by an inflation method to obtain a second sealant layer having a thickness of 100 μm. In the second sealant layer thus obtained, the layer composed of linear low density polyethylene resin D had a thickness of 20 μm, the layer composed of high density polyethylene resin had a thickness of 60 μm, and the layer composed of linear low density polyethylene resin D had a thickness of 20 μm.

[0149] A low-density polyethylene resin (Novatec LC600A, density 0.918 g / cm, manufactured by Japan Polyethylene Corporation) was placed on the layer composed of the other linear low-density polyethylene resin E of the gas barrier layer. 3 ) was melt-extruded to form a melt-extruded polyethylene layer having a thickness of 20 μm, and the layer composed of linear low density polyethylene resin D of the second sealant layer was bonded to the melt-extruded polyethylene layer through this melt-extruded polyethylene layer to obtain a laminate of the present invention. The polyethylene content in this laminate was 90% by mass.

[0150] Examples 3-2 to 3-5 Except for changing the configuration of the first polyethylene resin layer as shown in Table 3, a laminate was produced in the same manner as in Example 3-1. [Table 3]

[0151] Example 4-1 Polyethylene resin B is co-extruded by an inflation molding method to form a five-layered tubular film consisting of a first polyethylene resin layer (10 μm), second to fourth polyethylene resin layers (46.5 μm), and a fifth polyethylene resin layer (6 μm). Next, the fifth polyethylene resin layers, which were the inner layers, were pressed together with a rubber roll to obtain a block film. The block film was composed of a first polyethylene resin layer (10 μm), second to fourth polyethylene resin layers (46.5 μm), a fifth polyethylene resin layer (12 μm), second to fourth polyethylene resin layers (46.5 μm), and a first polyethylene resin layer (10 μm).

[0152] This block film was stretched in the machine direction (MD) at a stretch ratio of 5 times to obtain a stretched substrate film having a thickness of 25 μm. The thicknesses after stretching were 2 μm for the first polyethylene resin layer, 9.3 μm for the second to fourth polyethylene resin layers, 2.4 μm for the fifth polyethylene resin layer, 9.3 μm for the second to fourth polyethylene resin layers, and 2 μm for the first polyethylene resin layer. It was.

[0153] On the surface of the first polyethylene resin layer of the stretched substrate prepared as described above, an Al vapor deposition film having a thickness of 30 nm was formed by PVD to obtain a vapor deposition substrate. The optical density (OD value) of the vapor deposition film formed was measured and found to be 3.0.

[0154] As the first sealant layer, Linear low-density polyethylene resin D (Dow Chemical, Dowlex 2098P, density 0.926 g / cm 3 )and, High density polyethylene resin (Hi-Zex 3300F, manufactured by Prime Polymer Co., Ltd., density 0.950 g / cm 3 )and, Linear low-density polyethylene resin D (Dow Chemical, Dowlex 2098P, density 0.926 g / cm 3 )and, The mixture was co-extruded by an inflation method to obtain a first sealant layer having a thickness of 100 μm. In the first sealant layer thus obtained, the layer composed of linear low density polyethylene resin D had a thickness of 20 μm, the layer composed of high density polyethylene resin had a thickness of 60 μm, and the layer composed of linear low density polyethylene resin D had a thickness of 20 μm.

[0155] A urethane adhesive (RU004 / H1, manufactured by Rock Paint) was applied to the vapor deposition surface of the substrate and dried to form an adhesive layer 3 μm thick. The layer composed of linear low-density polyethylene resin D of the first sealant layer was then bonded to the substrate through this adhesive layer.

[0156] Linear low-density polyethylene resin E (Dow Chemical, Dowlex 2045G, density 0.920 g / cm 3 )and, Adhesive resin (Mitsui Chemicals, Admer NF557, density 0.903 g / cm 3 )and, Ethylene-vinyl alcohol copolymer (Kuraray Co., Ltd., EVAL H171B, density 1.17 g / cm 3 , ethylene content 38 mol%); Adhesive resin (Mitsui Chemicals, Admer NF557, density 0.903 g / cm 3 )and, Linear low-density polyethylene resin E (Dow Chemical, Dowlex 2045G, density 0.920 g / cm 3 )and, The gas barrier layer was obtained by co-extrusion of five layers of the mixture using the inflation method. The gas barrier layer obtained as described above had a five-layer structure with a total thickness of 60 μm, including a 17.5 μm-thick layer composed of linear low-density polyethylene resin E, a 5 μm-thick layer composed of adhesive resin, a 15 μm-thick layer composed of ethylene-vinyl alcohol copolymer, a 5 μm-thick layer composed of adhesive resin, and a 17.5 μm-thick layer composed of linear low-density polyethylene resin E.

[0157] A low-density polyethylene film (Novatec LC600A, density 0.918 g / cm, manufactured by Japan Polyethylene Corporation) was applied to the non-deposited film of the substrate. 3 ) was melt-extruded to form a melt-extruded polyethylene layer having a thickness of 20 μm, and the layer side of the gas barrier layer composed of linear low density polyethylene resin E was laminated via this melt-extruded polyethylene layer.

[0158] As a second sealant layer, Linear low-density polyethylene resin D (Dow Chemical, Dowlex 2098P, density 0.926 g / cm 3 )and, High density polyethylene resin (Prime Polymer, Hi-Zex 3300F, density 0.950g / cm 3 )and, Linear low-density polyethylene resin D (Dow Chemical, Dowlex 2098P, density 0.926 g / cm 3 )and, The mixture was co-extruded by an inflation method to obtain a second sealant layer having a thickness of 100 μm. In the second sealant layer thus obtained, the layer composed of linear low density polyethylene resin D had a thickness of 20 μm, the layer composed of high density polyethylene resin had a thickness of 60 μm, and the layer composed of linear low density polyethylene resin D had a thickness of 20 μm.

[0159] A low-density polyethylene resin (Novatec LC600A, density 0.918 g / cm, manufactured by Japan Polyethylene Corporation) was placed on the layer composed of the other linear low-density polyethylene resin E of the gas barrier layer.3 ) was melt-extruded to form a melt-extruded polyethylene layer having a thickness of 20 μm, and the layer composed of linear low density polyethylene resin D of the second sealant layer was bonded to the melt-extruded polyethylene layer through this melt-extruded polyethylene layer to obtain a laminate of the present invention. The polyethylene content in this laminate was 90% by mass.

[0160] Examples 4-2 to 4-5 Except for changing the configuration of the first polyethylene resin layer as shown in Table 4, a laminate was produced in the same manner as in Example 4-1. [Table 4]

[0161] Example 5-1 Linear low-density polyethylene (Dow Chemical, Dowlex 2045G, density 0.920 g / cm 3 ) and a compatibilizer (Dow Chemical, maleic anhydride modified polyethylene, Retain 3000, density 0.870 g / cm 3 ) were blended in a ratio of linear low-density polyethylene:compatibilizer=93% by mass:7% by mass to prepare a blend resin.

[0162] The blend resin prepared above, Adhesive resin (Mitsui Chemicals, Admer NF557, density 0.903 g / cm 3 )and, Ethylene-vinyl alcohol copolymer (Kuraray Co., Ltd., EVAL H171B, density 1.17 g / cm 3 , ethylene content 38 mol%); Adhesive resin (Mitsui Chemicals, Admer NF557, density 0.903 g / cm 3 )and, A blend resin; The gas barrier layer was obtained by co-extrusion of five layers of the mixture using the inflation method.

[0163] The gas barrier layer obtained as described above had a five-layer structure with a total thickness of 60 μm, including a layer composed of the blend resin having a thickness of 17.5 μm, a layer composed of the adhesive resin having a thickness of 5 μm, a layer composed of the ethylene-vinyl alcohol copolymer having a thickness of 15 μm, a layer composed of the adhesive resin having a thickness of 5 μm, and a layer composed of the blend resin having a thickness of 17.5 μm.

[0164] A laminate of the present invention was produced in the same manner as in Example 1-1, except that the gas barrier layer was changed to that produced as described above. The polyethylene content in this laminate was 90% by mass.

[0165] Example 5-2 A laminate of the present invention was produced in the same manner as in Example 1-2, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0166] Example 5-3 A laminate of the present invention was produced in the same manner as in Example 1-3, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0167] Example 5-4 A laminate of the present invention was produced in the same manner as in Example 1-4, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0168] Example 5-5 A laminate of the present invention was produced in the same manner as in Example 1-5, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0169] Example 6-1 A laminate of the present invention was produced in the same manner as in Example 2-1, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0170] Example 6-2 A laminate of the present invention was produced in the same manner as in Example 2-2, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0171] Example 6-3 A laminate of the present invention was produced in the same manner as in Example 2-3, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0172] Example 6-4 A laminate of the present invention was produced in the same manner as in Example 2-4, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0173] Example 6-5 A laminate of the present invention was produced in the same manner as in Example 2-5, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0174] Example 7-1 A laminate of the present invention was produced in the same manner as in Example 3-1, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0175] Example 7-2 A laminate of the present invention was produced in the same manner as in Example 3-2, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0176] Example 7-3 A laminate of the present invention was produced in the same manner as in Example 3-3, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0177] Example 7-4 A laminate of the present invention was produced in the same manner as in Example 3-4, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0178] Example 7-5 A laminate of the present invention was produced in the same manner as in Example 3-5, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0179] Example 8-1 A laminate of the present invention was produced in the same manner as in Example 4-1, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0180] Example 8-2 A laminate of the present invention was produced in the same manner as in Example 4-2, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0181] Example 8-3 A laminate of the present invention was produced in the same manner as in Example 4-3, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0182] Example 8-4 A laminate of the present invention was produced in the same manner as in Example 4-4, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0183] Example 8-5 A laminate of the present invention was produced in the same manner as in Example 4-5, except that the gas barrier layer was changed to that produced in Example 5-1. The polyethylene content in this laminate was 90 mass%.

[0184] Comparative Example 1 A laminate was produced in the same manner as in Example 1-1, except that the substrate was a biaxially oriented polyethylene terephthalate having a thickness of 12 μm (Toyobo Co., Ltd., Ester film E5100). The polyethylene content in this laminate was 85% by mass.

[0185] (Preparation of tube containers) The laminate obtained as described above was cut into a 120 mm wide slit using a bobbin cutter, and both ends in the width direction were overlapped so that the overlap width was about 1.5 mm, and then the overlapped ends were heat-sealed to obtain a cylindrical raw roll with a tube. The obtained raw roll was cut in the length direction to 122 mm to produce a cylindrical body portion that would become the body portion of the tube container.

[0186] The cylindrical body was attached to a mandrel for forming tube containers, and a head consisting of a truncated cone-shaped shoulder and a cylindrical extraction port connected to it was attached to one end of the cylindrical body using high-density polyethylene resin (Novatec HJ360, made by Nippon Polyethylene Co., Ltd., density 0.951 g / cm 3 ) was molded by injection molding to produce a tube container as shown in Figure 3. The spout part at the head of the obtained tube container body had an outer diameter of 13 mm, a height of 1.5 mm, a thread was provided on the side of the spout part, and the outer diameter of the shoulder part was 38 mm.

[0187] Next, the high density polyethylene was injected into a die for forming a cap and molded to prepare a cap, thereby obtaining a tube container of the present invention.

[0188] <<Recyclability evaluation>> The recyclability of the laminates obtained in the above Examples and Comparative Examples was evaluated based on the following evaluation criteria. The evaluation results are summarized in Table 5. (Evaluation Criteria) ◯: The content of the same polyolefin in the laminate was 90% by mass or more. ×: The content of the same polyolefin in the laminate was less than 90% by mass.

[0189] <<Shoulder adhesive strength>> Test pieces were obtained by cutting a strip 15 mm wide from the joining point between the body and shoulder toward the bottom hem. The test piece was pulled at a test speed of 300 mm / min using a tensile tester (Orientec Co., Ltd., RTC-1310A) to measure the peel strength when the body part was peeled off from the shoulder part. The measurement results are summarized in Table 5.

[0190] <<Side seam strength>> The specimen was cut into strips 15 mm wide perpendicular to the side seam (overlapping area) of the body, and pulled at a test speed of 300 mm / min using a tensile tester to measure the strength at break. The measurement results are shown in Table 5.

[0191] <<Leakage evaluation>> A cap was screwed onto the extraction opening of the tube container body, and then 120 g of commercially available toothpaste was poured into the opening of the cylindrical body, which was then heat-sealed. The tightening torque set for capping was 4.7 kg cm. The container was left at room temperature for two weeks, and visually inspected every day to see if there was any leakage of the contents. The evaluation criteria for leakage were as follows: (Evaluation Criteria) 〇: No leakage of contents was observed even after 2 weeks. ×: Leakage of contents was observed within 2 weeks

[0192] [Table 5] [Explanation of symbols]

[0193] 10: laminate, 11: first sealant layer, 12: vapor deposition film, 13: substrate, 14: gas barrier layer, 15: second sealant layer, 16: first polyolefin resin layer, 17: adhesive resin layer, 18: layer containing gas barrier resin, 19: adhesive resin layer, 20: second polyolefin resin layer, 30: laminate tube, 31: laminate tube body, 32: head, 33: body, 34: shoulder, 35: pouring outlet, 36: cap, 37: thread, 38: welded portion, 39: bottom seal portion

Claims

1. A laminate including at least a first sealant layer, a vapor-deposited film, a substrate, and a second sealant layer in this order, The substrate has a density of at least 0.943 g / cm 3 The present invention comprises a first polyethylene resin layer composed of the following polyethylene resin: The substrate is subjected to a stretching treatment, the vapor-deposited film is provided on the first polyethylene resin layer of the substrate, A laminate, wherein the first sealant layer and the second sealant layer are made of a polyethylene resin.

2. A laminate including at least a first sealant layer, a vapor-deposited film, a substrate, and a second sealant layer in this order, the substrate includes at least a first polyethylene resin layer composed of a polyethylene resin and an olefin-based elastomer resin; The substrate is subjected to a stretching treatment, the vapor-deposited film is provided on the first polyethylene resin layer of the substrate, A laminate, wherein the first sealant layer and the second sealant layer are made of a polyethylene resin.

3. The laminate according to claim 2 , wherein the olefin-based elastomer resin is an ethylene-based elastomer resin.

4. The laminate according to claim 2 or 3, wherein the olefin-based elastomer resin is an olefin-based block copolymer.

5. The laminate of claim 4, wherein the olefin-based block copolymer is an ethylene / α-olefin interpolymer.

6. 6. The laminate of claim 5, wherein the ethylene / α-olefin interpolymer comprises hard blocks constituted by polyethylene and soft blocks constituted by α-olefin monomers.

7. The laminate according to any one of claims 2 to 6, wherein the content of the olefin-based elastomer resin in the first polyethylene resin layer of the substrate is 1% by mass or more and 40% by mass or less.

8. The laminate according to any one of claims 1 to 7, wherein the gas barrier layer has a five-layer structure consisting of a first polyolefin resin layer, an adhesive resin layer, a gas barrier resin-containing layer, an adhesive resin layer, and a second polyolefin resin layer.

9. The laminate according to claim 8 , wherein the first polyolefin resin layer and the second polyolefin resin layer of the gas barrier layer are composed of a polyethylene resin and an unsaturated carboxylic acid-modified polyolefin resin.

10. The laminate according to any one of claims 1 to 9, further comprising a barrier coat layer having an oxygen barrier and / or a water vapor barrier between the first sealant layer and the vapor-deposited film.

11. The laminate according to any one of claims 1 to 10, which is used for a packaging container.

12. The laminate according to any one of claims 1 to 11, wherein the content of the polyethylene resin in the entire laminate is 90 mass% or more.

13. A packaging container comprising the laminate according to any one of claims 1 to 12.

14. The packaging container according to claim 13, which is a laminated tube.

Citation Information

Patent Citations

  • Laminate and process for producing the same

    JP2009078566A

  • Laminate for packaging material and packaging material

    JP2020040259A

  • Multilayer structures, processes for manufacturing multilayer structures, and related articles

    JP2020517502A

  • Laminate and packaging container

    JP2021160267A

  • Laminate, and packaging material, packaging bag and stand-up pouch each comprising said laminate, and multi-layer substrate

    WO2019189092A1