Cosmetic resin composition and cosmetic

The cosmetic resin composition addresses the issue of poor durability in protective equipment environments by using a polymer with specific ethylenically unsaturated monomers and properties, achieving long-lasting makeup retention and resistance to sweat and sebum, with minimal skin irritation.

JP2024156271APending Publication Date: 2024-11-06TOYO INK MFG CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023070597
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-24
Publication Date
2024-11-06

AI Technical Summary

Technical Problem

Conventional cosmetic resins lack durability and performance in environments where protective equipment is worn for extended periods, leading to poor makeup retention due to exposure to sweat and sebum, with existing resin compositions exhibiting poor water, salt water, and oil resistance, and causing skin irritation.

Method used

A cosmetic resin composition with a polymer (A) that includes ethylenically unsaturated monomers, having specific Log Kow values and a storage modulus within a certain range, and a contact angle of water within a specific range, ensuring excellent water, salt water, and oil resistance, while minimizing skin irritation.

Benefits of technology

The resin composition maintains excellent makeup durability under harsh conditions, with improved water, salt water, and oil resistance, and minimal skin irritation, demonstrating good storage stability and long-lasting performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024156271000001
    Figure 2024156271000001
  • Figure 2024156271000002
    Figure 2024156271000002
  • Figure 2024156271000003
    Figure 2024156271000003
Patent Text Reader

Abstract

To provide a cosmetic resin composition that has high storage stability and forms a coating layer with superior water resistance, salt water resistance, oil resistance, and makeup durability.SOLUTION: A cosmetic resin composition, designed for application onto skin, forms a coating layer with a storage modulus of 1×104 Pa or more and 1×109 Pa or less as measured at 37°C in the frequency range of 0.1 Hz or more and 10 Hz or less. When a drop of water lands on the coating layer of the cosmetic resin composition at 25°C, the contact angle of the water measures 5° or more and 90° or less one second after impact.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cosmetic resin composition for application on the skin, and a cosmetic containing the same. [Background technology]

[0002] In recent years, situations in which protective equipment such as masks, face shields, and protective glasses are worn for long periods of time in daily life have been increasing. In an environment in which such protective equipment is worn for long periods of time, the skin is exposed to steam and moisture from exhaled breath, sweat containing salt, sebum containing oil, etc., and this causes problems such as insufficient durability of cosmetics using conventional cosmetic resins, and a significant deterioration in performance such as cosmetic durability.

[0003] Patent Document 1 discloses a cosmetic resin composition using a polymer obtained by emulsion polymerization of a mixture of ethylenically unsaturated monomers containing a carboxyl group-containing ethylenically unsaturated monomer, an ethylenically unsaturated monomer having an alkyl group with 1 to 4 carbon atoms, and an ethylenically unsaturated monomer having an alkyl group with 5 or more carbon atoms in a predetermined amount. Although a certain degree of water resistance can be expected from the coating film of the above-mentioned cosmetic resin composition, it does not assume a situation in which salts from sweat or oils from sebum are abundant. Therefore, in a situation where protective equipment is worn or in an environment where a long time has passed since application, the cosmetic is easily peeled off from the skin, and the cosmetic durability is deteriorated.

[0004] Patent Document 2 discloses a cosmetic resin composition containing a polymer of methyl methacrylate and 2-ethylhexyl acrylate with a coefficient of variation of particle size distribution of 15% or less. This cosmetic resin composition has poor storage stability and does not have a coating film design that is durable against oils such as sebum, making it difficult to maintain excellent cosmetic durability for a long period of time.

[0005] Patent Document 3 discloses a cosmetic resin composition containing an acrylic resin having a glass transition temperature of 20° C. or less, obtained by polymerizing an ethylenically unsaturated monomer containing a (meth)acryloyl group. The performance of the coating film of this cosmetic resin composition also deteriorates significantly in an environment where sweat and sebum components are abundantly present. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2005-002207 A [Patent Document 2] JP 2016-160222 A [Patent Document 3] JP 2020-063300 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention aims to provide a cosmetic resin composition which has excellent storage stability, produces a coating film with good water resistance, salt water resistance and oil resistance, maintains excellent cosmetic durability for a long time even under severe conditions, and is extremely low in skin irritation. [Means for solving the problem]

[0008] The present inventors have conducted extensive research to solve the above problems and have arrived at the present invention. That is, the present invention relates to a cosmetic resin composition for application onto the skin, and a coating film of the cosmetic resin composition has a storage modulus of 1×10 measured at 37° C. in a frequency range of 0.1 Hz to 10 Hz. 4 Pa or more 1×10 9 The present invention relates to a cosmetic resin composition having a viscosity of 100 Pa or less, and when water is dropped onto a coating film of the cosmetic resin composition at 25° C., the contact angle of water 1 second after the drop is 5° or more and 90° or less.

[0009] The present invention also relates to the above-mentioned resin composition for cosmetics, which comprises an aqueous medium and a polymer (A), wherein the polymer (A) is a polymer of an ethylenically unsaturated monomer and contains 90.0 mass % or more and 99.5 mass % or less of a nonionic ethylenically unsaturated monomer (a) having an octanol / water partition coefficient (Log Kow) of 0.4 or more and less than 2.5 at 25°C, based on the total mass of the ethylenically unsaturated monomer, and the acid value of the polymer (A) is 3.0 mgKOH / g or more and 50.0 mgKOH / g or less.

[0010] The present invention also relates to the above-mentioned resin composition for cosmetics, wherein the monomer (a) comprises a nonionic ethylenically unsaturated monomer (a-1) having a logarithm of the octanol / water partition coefficient (Log Kow) at 25°C of 0.4 or more and less than 2.0, and a nonionic ethylenically unsaturated monomer (a-2) having a logarithm of the octanol / water partition coefficient (Log Kow) of 2.0 or more and less than 2.5, and the composition contains 20.0% by mass or more and 79.5% by mass or less of the monomer (a-1) and 20.0% by mass or more and 79.5% by mass or less of the monomer (a-2).

[0011] The present invention also relates to the above-mentioned cosmetic resin composition, wherein the average particle size of the polymer (A) is 30 nm or more and 400 nm or less.

[0012] The present invention also relates to a cosmetic comprising the above-mentioned cosmetic resin composition. Effect of the Invention

[0013] According to the present invention, it is possible to provide a cosmetic resin composition which has excellent storage stability, has good water resistance, salt water resistance, and oil resistance of a coating film, maintains excellent cosmetic durability for a long time even under harsh conditions, and is extremely low in skin irritation. Therefore, it can be used as a cosmetic resin composition which exhibits excellent performance in cosmetics to be applied to the skin, such as foundation, blusher, face powder, eye shadow, eye liner, eyebrow, mascara, concealer, lipstick, lip gloss, and lip pencil.

[0014] Hereinafter, an embodiment of the present invention will be described. In this specification, a numerical range specified using "~" is intended to include the numerical values ​​before and after "~" as the lower and upper limit values ​​of the range. In addition, the nonionic ethylenically unsaturated monomer (a) having an octanol / water partition coefficient (Log Kow) at 25°C of 0.4 or more and less than 2.5, the nonionic ethylenically unsaturated monomer (a-1) having a logarithm of the octanol / water partition coefficient (Log Kow) at 25°C of 0.4 or more and less than 2.0, the nonionic ethylenically unsaturated monomer (a-2) having a logarithm of the octanol / water partition coefficient (Log Kow) of 2.0 or more and less than 2.5, and the other ethylenically unsaturated monomer (a-3) may be abbreviated as monomer (a), monomer (a-1), monomer (a-2), and monomer (a-3), respectively.

[0015] Each component described in this specification is not limited to such examples, and unless otherwise noted, each component may be used independently as a single type or as a combination of two or more types. In addition, a nonionic ethylenically unsaturated monomer is an ethylenically unsaturated monomer that does not have a functionality that dissociates to become an ion when in an aqueous medium (referred to as an "ionic functional group"), and means, for example, an ethylenically unsaturated monomer that does not have an ionic functional group such as a carboxy group.

[0016] <<Cosmetic Resin Composition>> The cosmetic resin composition of the present invention is a cosmetic resin composition for application onto the skin, and a coating film of the cosmetic resin composition has a storage modulus of 1×10 measured at 37° C. in a frequency range of 0.1 Hz to 10 Hz. 4 Pa or more 1×10 9 The cosmetic resin composition has a viscosity of not more than 1 Pa, and when water is dropped onto a coating film of the cosmetic resin composition at 25°C, the contact angle of water 1 second after the drop is 5° or more and 90° or less. Furthermore, the cosmetic resin composition of the present invention contains an aqueous medium and a polymer (A). The polymer (A) is a polymer of an ethylenically unsaturated monomer and contains 90.0% by mass or more and 99.5% by mass or less of a nonionic ethylenically unsaturated monomer (a) having an octanol / water partition coefficient (Log Kow) of 0.4 or more and less than 2.5 at 25°C based on the total mass of the ethylenically unsaturated monomer, and the acid value of the polymer (A) is preferably 3.0 mgKOH / g or more and 50.0 mgKOH / g or less. The cosmetic resin composition of the present invention has excellent storage stability, and the coating film has very good water resistance, salt water resistance, and oil resistance, and can maintain excellent cosmetic durability for a long time even under harsh conditions, while causing very little skin irritation.

[0017] <Aqueous medium> The aqueous medium refers to an aqueous dispersion medium or an aqueous solvent. As the aqueous medium, it is preferable to use water, but if necessary, a water-soluble solvent can also be used. Examples of the water-soluble solvent include alcohols, glycols, cellosolves, amino alcohols, amines, ketones, carboxylic acid amides, phosphoric acid amides, sulfoxides, carboxylic acid esters, phosphoric acid esters, ethers, and nitriles.

[0018] <Polymer (A)> The polymer (A) is preferably a polymer of ethylenically unsaturated monomers having an acid value of 3.0 mgKOH / g or more and 50.0 mgKOH / g or less, and containing 90.0 mass % or more and 99.5 mass % or less of a nonionic ethylenically unsaturated monomer (a) having an octanol / water partition coefficient (log Kow) of 0.4 or more and less than 2.5 at 25°C, based on the total mass of the ethylenically unsaturated monomers.

[0019] The polymer (A) has an acid value in the range of 3.0 mgKOH / g to 50.0 mgKOH / g, preferably 5.0 mgKOH / g to 40.0 mgKOH / g. By having an acid value in the above range, the adhesion between the polymer (A) and the skin is improved. Furthermore, the strength of the coating film of the polymer (A) is improved, and the coating film has good water resistance, salt water resistance, and oil resistance, and maintains excellent cosmetic durability for a long time even under harsh conditions, and has very little skin irritation. In addition, the storage stability of the cosmetic composition is also good.

[0020] [Monomer (a)] Monomer (a) is an ethylenically unsaturated monomer having a logarithm of the octanol / water partition coefficient (Log Kow) at 25° C. of 0.4 or more and less than 2.5, and preferably 1.0 or more and less than 2.3. By having Log Kow in the above range, the coating film of the cosmetic resin composition has excellent water resistance, salt water resistance, and oil resistance, and exhibits excellent cosmetic durability for a long time even under harsh conditions.

[0021] Log Kow is expressed by the following (Formula 1), and is used as an index showing whether a certain compound X is likely to be distributed into the aqueous phase or the oil phase (octanol). The Log Kow of each ethylenically unsaturated monomer can be calculated from experiments such as the shake flask method or HPLC method, and can also be calculated by simulation from the chemical structure such as the YMB method (physical property prediction function) of the Hansen solubility parameter software HSPiP, but the Log Kow in this specification is a value calculated by the YMB method (Version 5.2.05) of the Hansen solubility parameter software HSPiP (manufactured by pirika.com LLC). (Formula 1) Log Kow = Log(concentration of compound X in the octanol phase / concentration of compound X in the aqueous phase)

[0022] The content of monomer (a) is preferably 90.0% by mass or more and 99.5% by mass or less, and more preferably 91.5% by mass or more and 98.5% by mass or less, based on the total mass (100% by mass) of ethylenically unsaturated monomers. By having the content in the above range, the cosmetic resin composition has good storage stability, the coating film has excellent water resistance, salt water resistance, and oil resistance, and exhibits excellent long-lasting cosmetic properties even under harsh conditions. Skin irritation is also extremely low.

[0023] Monomer (a) can be roughly divided into monomer (a-1) and monomer (a-2) according to the difference in the numerical range of Log Kow. Monomer (a) preferably contains monomer (a-1) and monomer (a-2), and preferably contains monomer (a-1) in the range of 20.0% by mass to 79.5% by mass and monomer (a-2) in the range of 20.0% by mass to 79.5% by mass based on the total mass (100% by mass) of monomer (a). By containing monomer (a-1) and monomer (a-2) in the above range, the affinity between the skin surface and the cosmetic resin composition is further improved due to the synergistic effect, and the followability of the coating film on the skin is also improved, so that water resistance, salt water resistance, and oil resistance are further improved. Furthermore, excellent cosmetic durability can be exhibited for a long time even under harsher conditions.

[0024] [Monomer (a-1)] Monomer (a-1) is an ethylenically unsaturated monomer having a logarithm of the octanol / water partition coefficient (Log Kow) at 25° C. of 0.4 or more and less than 2.0, preferably 1.0 or more and less than 2.0. By having Log Kow in the above range, the oil resistance of the coating film of the cosmetic resin composition is further improved, and the cosmetic durability is also further improved. Skin irritation is also reduced.

[0025] Specific examples of the monomer (a-1) include methoxyethyl acrylate (Log Kow=0.45), methyl acrylate (Log Kow=0.65), vinyl acetate (Log Kow=0.65), (methoxyethyl methacrylate (Log Kow=1.15), 2-hydroxyethyl methacrylate (Log Kow=0.7), 4-hydroxybutyl acrylate (Log Kow=0.56), isopropyl acrylamide (Log Kow=0.54), diacetone acrylamide (Log Kow=0.84), 2-acetoacetoxyethyl methacrylate (Log Kow=0.61), glycidyl methacrylate (Log Kow=0.95), 3,4-epoxycyclohexyl acrylate (Log Kow=1.78), methyl methacrylate (Log Kow=1.27), ethyl acrylate (Log Kow=1.16), ethyl methacrylate (Log Examples of the monomer (a-1) include methyl methacrylate (Log Kow=1.78), trifluoroethyl acrylate (Log Kow=1.57), trifluoromethacrylate (Log Kow=1.95), ethylene glycol dimethacrylate (log Kow 1.90), etc. Among these, from the viewpoint of less irritation to the skin surface and exhibiting better oil resistance of the coating film, the monomer (a-1) is preferably methyl methacrylate, ethylene glycol dimethacrylate, or ethyl acrylate, and more preferably methyl methacrylate.

[0026] [Monomer (a-2)] Monomer (a-2) is an ethylenically unsaturated monomer having a logarithm of the octanol / water partition coefficient (Log Kow) at 25° C. of 2.0 or more and less than 2.5, and preferably 2.0 or more and less than 2.3. When the Log Kow is in the above range, the coating film of the cosmetic resin composition has better water resistance and salt water resistance, and the cosmetic durability is also improved.

[0027] Specific examples of the monomer (a-2) include t-butyl acrylate (Log Kow=2.06), isobutyl acrylate (Log Kow 2.09), allyl methacrylate (Log Kow=2.10), n-butyl acrylate (Log Kow=2.23), n-propyl methacrylate (Log Kow=2.28), benzyl acrylate (Log Kow=2.32), phenoxyethyl acrylate (Log Kow=2.44), phenoxydiethylene glycol acrylate (Log Kow=2.33), 3-(methacryloyloxy)propyltrimethoxysilane (Log Kow=2.42), etc. Among them, from the viewpoint of exhibiting better water resistance and salt water resistance, the ethylenically unsaturated monomer (a-2) is preferably n-butyl acrylate, allyl methacrylate, or isobutyl acrylate, and more preferably n-butyl acrylate.

[0028] [Monomer (a-3)] The monomer (a-3) is an ethylenically unsaturated monomer polymerizable with the monomer (a) other than the monomer (a). Examples of the monomer (a-3) include aromatic ethylenically unsaturated monomers such as styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, m-methylstyrene, vinylnaphthalene, benzyl methacrylate, and phenoxyethyl methacrylate; linear or branched alkyl group-containing ethylenically unsaturated monomers, such as hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, and behenyl (meth)acrylate; Alicyclic group-containing ethylenically unsaturated monomers such as cyclohexyl methacrylate and isobornyl (meth)acrylate; Fluorinated alkyl group-containing ethylenically unsaturated monomers such as heptadecafluorodecyl (meth)acrylate; Carboxy group-containing ethylenically unsaturated monomers such as (anhydrous) maleic acid, fumaric acid, itaconic acid, citraconic acid, or alkyl or alkenyl monoesters thereof, β-(meth)acryloxyethyl succinate monoester, acrylic acid, methacrylic acid, crotonic acid, cinnamic acid, and the like; Sulfonic acid group-containing ethylenically unsaturated monomers such as sodium 2-acrylamido 2-methylpropanesulfonate, methallylsulfonic acid, methallylsulfonic acid, sodium methallylsulfonate, allylsulfonic acid, sodium allylsulfonate, ammonium allylsulfonate, and vinylsulfonic acid; (Meth)acrylamide, N-methoxymethyl-(meth)acrylamide, Amide group-containing ethylenically unsaturated monomers such as N-ethoxymethyl-(meth)acrylamide; Hydroxyl-containing ethylenically unsaturated monomers such as 2-hydroxyethyl acrylate; Polyoxyethylene group-containing ethylenically unsaturated monomers such as methoxypolyethylene glycol (meth)acrylate and polyethylene glycol (meth)acrylate; Amino group-containing ethylenically unsaturated monomers, such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, methylethylaminoethyl (meth)acrylate, dimethylaminostyrene, and diethylaminostyrene; etc.

[0029] The monomer (a-3) is contained in an amount of preferably 0.5% by mass or more and 10.0% by mass or less, and more preferably 1.5% by mass or more and 8.5% by mass or less, based on 100% by mass of the total mass of ethylenically unsaturated monomers.

[0030] [Method of synthesizing polymer (A)] Methods for synthesizing the polymer (A) include solution polymerization, emulsion polymerization, bulk polymerization, etc., with emulsion polymerization being preferred from the standpoint of controlling the reaction heat, etc.

[0031] The emulsion polymerization is preferably carried out in the presence of a surfactant. Examples of the surfactant include anionic surfactants, cationic surfactants, nonionic surfactants, and amphoteric surfactants. Among these, anionic surfactants, cationic surfactants, and nonionic surfactants are preferred, and anionic surfactants and nonionic surfactants are more preferred. The surfactant may be a reactive surfactant or a non-reactive surfactant.

[0032] Examples of the anionic surfactant include higher fatty acid salts such as sodium oleate, alkylarylsulfonates such as dodecylbenzenesulfonic acid, alkyl sulfates such as sodium lauryl sulfate, polyoxyethylene alkyl ether sulfates such as sodium polyoxyethylene lauryl ether sulfate, alkyl sulfosuccinates such as sodium monooctyl sulfosuccinate, sodium dioctyl sulfosuccinate, and sodium polyoxyethylene lauryl sulfosuccinate, and derivatives thereof, and polyoxyethylene distyrenated phenyl ether sulfate.

[0033] Examples of non-reactive nonionic surfactants include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether and polyoxyethylene stearyl ether, polyoxyethylene alkyl phenyl ethers such as polyoxyethylene octyl phenyl ether and polyoxyethylene nonyl phenyl ether, sorbitan higher fatty acid esters such as sorbitan monolaurate, sorbitan monostearate, and sorbitan trioleate, polyoxyethylene sorbitan higher fatty acid esters such as polyoxyethylene sorbitan monolaurate and polyoxyethylene sorbitan monostearate, polyoxyethylene higher fatty acid esters such as polyoxyethylene monolaurate and polyoxyethylene monostearate, glycerin higher fatty acid esters such as oleic acid monoglyceride and stearic acid monoglyceride, polyoxyethylene-polyoxypropylene block copolymers, and polyoxyethylene distyrenated phenyl ether.

[0034] The reactive surfactant is an anionic surfactant or a nonionic surfactant having one or more unsaturated double bonds capable of radical polymerization. The reactive anionic surfactant is preferably one whose main skeleton is, for example, a sulfosuccinate ester, an alkyl ether, an alkyl phenyl ether, an alkyl phenyl ester, a (meth)acrylate sulfate ester, a phosphate ester, or the like. The reactive nonionic surfactant is preferably one whose main skeleton is, for example, an alkyl ether, an alkyl phenyl ether, an alkyl phenyl ester, or the like.

[0035] The surfactant is preferably used in an amount of 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, based on 100 parts by mass of the ethylenically unsaturated monomer mixture. By using an appropriate amount of the surfactant, polymerization stability is improved and adverse effects on the skin are reduced.

[0036] In the emulsion polymerization, it is preferable to use a radical polymerization initiator (hereinafter, simply referred to as "polymerization initiator"). As the polymerization initiator, a known oil-soluble polymerization initiator or water-soluble polymerization initiator can be used. Examples of the oil-soluble initiator include organic peroxides such as benzoyl peroxide, tert-butyloxybenzoate, tert-butyl hydroperoxide, tert-butylperoxy-2-ethylhexanoate, tert-butylperoxy-3,5,5-trimethylhexanoate, di-tert-butyl peroxide, cumene hydroperoxide, and p-menthane hydroperoxide; and azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis-2,4-dimethylvaleronitrile, 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), and 1,1'-azobis-cyclohexane-1-carbonitrile. Examples of the water-soluble polymerization initiator include ammonium persulfate, sodium persulfate, potassium persulfate, hydrogen peroxide, and 2,2'-azobis(2-methylpropionamidine) dihydrochloride.

[0037] When carrying out the polymerization, a reducing agent or a transition metal salt can be used in combination with the polymerization initiator, which promotes the decomposition of the polymerization initiator. Examples of reducing agents include organic reducing compounds such as ascorbic acid, erythorbic acid, tartaric acid, citric acid, glucose, and metal salts of formaldehyde sulfoxylate, and inorganic reducing compounds such as sodium sulfite, sodium bisulfite, sodium metabisulfite, and sodium hyposulfite. Examples of transition metal salts include ferrous chloride, ferrous sulfate, and copper sulfate.

[0038] In the emulsion polymerization of the present invention, it is preferable to use a water-soluble polymerization initiator. It is preferable to use 0.03 parts by mass or more and 5 parts by mass or less of the polymerization initiator with respect to 100 parts by mass of the monomer mixture. It is preferable to use 0.01 parts by mass or more and 2.5 parts by mass or less of the reducing agent with respect to 100 parts by mass of the monomer mixture. It is preferable to use 0.0001 parts by mass or more and 0.002 parts by mass or less of the transition metal salt with respect to 100 parts by mass of the monomer mixture. The method of adding the polymerization initiator includes, for example, initial lump-sum charging, divided charging, continuous dropwise addition, etc., but is not particularly limited. In addition, from the viewpoint of hastening the end point of the polymerization reaction, a part of the polymerization initiator may be added to the reaction system before or after the end of the addition of the monomer to the reaction system.

[0039] During the emulsion polymerization, a buffering agent, a chain transfer agent, a basic compound, etc. may be used, if necessary. Buffers include, for example, sodium acetate, sodium citrate, sodium bicarbonate, and the like. Examples of the chain transfer agent include n-octyl mercaptan, n-dodecyl mercaptan, tert-dodecyl mercaptan, lauryl mercaptan, stearyl mercaptan, 3-mercaptopropionic acid, n-octyl 3-mercaptopropionate, 2-ethylhexyl 3-mercaptopropionate, n-octyl thioglycolate, 2-ethylhexyl thioglycolate, etc. Among these, 2-ethylhexyl 3-mercaptopropionate and 2-ethylhexyl thioglycolate are preferred, and 2-ethylhexyl thioglycolate is more preferred. The chain transfer agent is preferably used in an amount of 0.01 part by mass or more and 0.1 part by mass or less based on 100 parts by mass of the monomer mixture. The basic compound is used for neutralization, and examples thereof include alkylamines such as trimethylamine, triethylamine, and n-butylamine, alcoholamines such as 2-dimethylaminoethanol, diethylaminoethanol, diethanolamine, triethanolamine, and aminomethylpropanol, morpholine, ammonia, etc. The basic compound is preferably ammonia in terms of volatility.

[0040] Examples of the emulsion polymerization method include a batch reaction in which an ethylenically unsaturated monomer, a surfactant, and water are all charged in a reaction tank and reacted, and a drop reaction in which a monomer is gradually dropped into a reaction tank and reacted. Among these, a drop reaction is preferred from the viewpoint of controlling heat generation during the polymerization reaction and dibutylene glycol. In addition, in order to further improve the polymerization stability, the drop reaction is preferably performed by mixing and stirring the monomer, water, and surfactant to form a pre-emulsion in an emulsified state and then dropping it.

[0041] The polymer (A) obtained by emulsion polymerization has a particle shape. The average particle size of the particles is preferably 30 nm or more and 400 nm or less, more preferably 35 nm or more and 365 nm or less. When the average particle size is in the above range, the storage stability of the cosmetic resin composition is better. In addition, the generation of defects in the coating film and the segregation of some components are suppressed, and a denser and more uniform coating film can be formed, so that the water resistance, salt resistance, and oil resistance are further improved, and the cosmetic durability is also superior for a long time. In this specification, the average particle size is the median diameter (D 50 As an example of a method for measuring the average particle size, a diluted solution is prepared by diluting the aqueous dispersion of polymer particles 500 times with water, and about 5 mL of the diluted solution is used for measurement with a dynamic light scattering particle size distribution measuring device (NANOTRAC WAVEII EX150 manufactured by Microtrack Bell).

[0042] The content of the polymer (A) is preferably in the range of 5.0% by mass to 50.0% by mass, more preferably in the range of 10.0% by mass to 40.0% by mass, based on the total amount of the cosmetic resin composition. By having the content in the above range, the water resistance, salt resistance, and oil resistance of the coating film are further improved, and the cosmetic durability is also further improved.

[0043] <Optional ingredients> The cosmetic resin composition of the present invention may contain various additives such as pigments, pigment dispersants, thickeners, moisturizers, preservatives, solvents, antifoaming agents, wetting agents, etc. as optional components.

[0044] Examples of pigments include carbon black, iron oxide particles (black iron oxide particles, yellow iron oxide particles, etc.), titanium oxide, Prussian blue, ultramarine, red iron oxide, chromium oxide, chromium hydroxide, zinc oxide, zirconium oxide, cobalt oxide, aluminum oxide, silicon dioxide, calcium carbonate, titanium yellow, fish scale foil, bismuth oxychloride, organic pigments such as Blue No. 1, Blue No. 2, Blue No. 404, Red No. 201, Red No. 202, Red No. 220, Red No. 102, Red No. 104, and Yellow No. 4, aluminum-coated polyester film, laminated film powder, and myric acid. Examples of the luster pigments include at least one type (either alone or as a mixture of two or more types) of luster pigments such as mica titanium, carmine coated mica titanium, chromium oxide coated mica titanium, iron oxide coated mica titanium, iron oxide and carmine coated mica titanium, iron oxide and Prussian blue coated mica titanium, blue coated mica titanium, Prussian blue coated mica titanium, red iron oxide coated mica titanium, red iron oxide and carmine coated mica titanium, red iron oxide and Prussian blue coated mica titanium, red iron oxide and Prussian blue coated mica titanium, and red iron oxide and Prussian blue coated mica titanium.

[0045] Examples of the pigment dispersant include various surfactants exemplified in the synthesis of the above polymer (A), and polymer dispersants such as water-soluble acrylic resins, styrene-acrylic resins, styrene-maleic acid resins, polyurethane resins, polyester resins, and polyamide resins.

[0046] Examples of the thickener include an alkali swelling type thickener, an associative polyurethane, a carboxyvinyl polymer, a thickening polysaccharide, and a clay mineral. Examples of moisturizing agents include sorbitol, xylitol, propylene glycol, dipropylene glycol, 1,3-butylene glycol, glycerin, diglycerin, polyethylene glycol, hyaluronic acid, chondroitin sulfate, pyrrolidone carboxylate, and DL-pyrrolidone carboxylate.

[0047] Examples of the solvent include monohydric alcohols such as ethanol, 1-propanol, 2-propanol, 1-butanol, and 2-butanol; 1,2-ethanediol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,2-pentanediol, 1,5-pentanediol, 1,2-hexanediol, 1,6-hexanediol, 1,2-heptanediol, 2,2-dimethyl-1,3-propanediol, 2-methyl-1,3-propanediol, 2-ethyl-2-methyl-1,3-propanediol, 3-methyl-1,3-butanediol, 3- Dihydric alcohols (glycols) such as methyl-1,5-pentanediol, 2-methyl-2-propyl-1,3-propanediol, 2-methylpentane-2,4-diol, 2-ethyl-1,3-hexanediol, 1,2-octanediol, ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol #200, polyethylene glycol #400, dipropylene glycol, tripropylene glycol, and dibutylene glycol;

[0048] glycol monoalkyl ethers such as ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, diethylene glycol monopentyl ether, diethylene glycol monohexyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol monopropyl ether, triethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, tetraethylene glycol monoethyl ether, tetraethylene glycol monobutyl ether, dipropylene glycol monopropyl ether, tripropylene glycol monomethyl ether, tripropylene glycol monoethyl ether, 1,2-butylene glycol monomethyl ether, and 1,3-butylene glycol monomethyl ether;

[0049] Chain polyol compounds such as glycerin, trimethylolpropane, 1,2,4-butanetriol, 1,2,6-hexanetriol, diglycerin, and polyglycerin; dicarboxylate alkyl esters such as diisopropyl adipate, diisobutyl adipate, dioctyl adipate, diisodecyl adipate, diisopropyl sebacate, dioctyl sebacate, and diisodecyl sebacate; Hydrocarbons such as alkanes, paraffins, and squalene; Long-chain fatty acids such as olive oil and sunflower oil; evaluation of cosmetic resin compositions etc.

[0050] Examples of preservatives include methyl parahydroxybenzoate, ethyl parahydroxybenzoate, propyl parahydroxybenzoate, butyl parahydroxybenzoate, benzoic acid, sodium benzoate, sorbic acid, potassium sorbate, phenoxyethanol, 4-hydroxyacetophenone, dehydroacetic acid, caprylyl glycol, and pentylene glycol. Examples of the defoaming agent include silicone-based defoaming agents and mineral oil-based defoaming agents. Examples of the wetting agent include various surfactants exemplified in the synthesis of the polymer (A).

[0051] <<Formation of coating film of cosmetic resin composition>> The cosmetic resin composition of the present invention forms a coating film by volatilization of the aqueous medium. Examples of a method for applying the cosmetic resin composition to form a coating film include a known coating film forming method, such as a method of applying the cosmetic resin composition directly onto the skin with the hand, a sponge, a brush with a brush tip, a pen core, or the like, and allowing it to dry naturally to form a film, and a method of first applying the cosmetic resin composition to a peelable substrate, drying it to form a coating film, and then transferring it onto the skin.

[0052] The amount of the cosmetic resin composition applied per unit area is not particularly limited, but from the viewpoint of exhibiting excellent adhesiveness, it is preferably 2 g / m2 in terms of dry mass. 2 , 50g / m 2 The range is preferably within the range below, and more preferably within 10 g / m2 More than 40g / m 2 The following is the result.

[0053] The coating film of the cosmetic resin composition of the present invention has a storage modulus of 1×10 4 Pa or more 1×10 9 Pa or less, more preferably 2×10 4 Pa or more 1×10 8 The storage modulus is in the range of 0.1 Pa or less. Since the coating film of the cosmetic resin composition can follow the movement of the skin, the coating film is less likely to have defects and has excellent water resistance, salt water resistance, and oil resistance. In addition, the cosmetic composition can maintain good cosmetic durability for a long time even under harsh conditions. Skin irritation is also very low. The storage modulus can be easily measured by preparing a coating film of the cosmetic resin composition and using a viscoelasticity measuring device.

[0054] When water is dropped onto the coating film of the cosmetic resin composition of the present invention at 25°C, the contact angle of water 1 second after the drop is in the range of 5° to 90°, preferably 5° to 50°. When the contact angle of water to the coating film is in the above range, the hydrophilic and lipophilic components that are dissolved from the coating film or segregated to the surface are small, and the interface properties of the coating film formed by the cosmetic resin composition are unlikely to be adversely affected. Therefore, the coating film exhibits excellent water resistance, salt water resistance, and oil resistance. In addition, good cosmetic durability can be maintained for a long time even under harsh conditions. The contact angle of water can be measured by dropping water onto the coating surface of the substrate coated with the cosmetic resin composition using a contact angle measuring device.

[0055] <Cosmetics> The cosmetic of the present invention comprises the cosmetic resin composition of the present invention. The cosmetic of the present invention can be blended with other components, such as aqueous components, oily components, surfactants, pigments, powders, etc., as desired. EXAMPLES

[0056] The present invention will be described in more detail below with reference to examples, but the following examples are not intended to limit the scope of the invention. In the examples, unless otherwise specified, "parts" means "parts by mass," "%" means "% by mass," the values ​​in the tables are solid content masses, and blanks indicate that no space is used.

[0057] <Acid value> The acid value of polymer (A) is the number of milligrams of potassium hydroxide required to neutralize the acidic components contained in 1 g of dried resin. It was measured by potentiometric titration using an automatic titrator (HIRANUMA "COM" model) and potassium hydroxide-ethanol solution according to the method described in JIS K2501.

[0058] <Average particle size> The aqueous dispersion of polymer (A) produced by the method described below was diluted 500 times with water to prepare a diluted solution, and about 5 mL of the diluted solution was used to measure the particle size distribution at 25°C using a dynamic light scattering particle size distribution measuring device (NANOTRAC WAVEII EX150 manufactured by Microtrack Bell). 50 The particle size (median size) was taken as the average particle size.

[0059] <Preparation of pigment dispersion resin aqueous solution> [Production Example 1] 53.2 parts of n-propanol was charged into a flask (reaction tank) equipped with a reflux condenser, a dropping funnel, a stirrer, a thermometer, a nitrogen gas inlet, and a raw material inlet, and the mixture was stirred while replacing with nitrogen gas, and the internal temperature was raised to 90 ° C. A mixture of 39 parts of butyl acrylate, 23 parts of acrylic acid, 38 parts of styrene, 6 parts of n-propanol, and 3.5 parts of dimethyl 2,2'-azobis(isobutyrate) (manufactured by Wako Pure Chemical Industries, Ltd.) was added dropwise from the dropping funnel over 3 hours while maintaining the internal temperature at 90 ° C. One hour after the completion of the dropping, a solution in which 0.3 parts of dimethyl 2,2'-azobis(isobutyrate) was dissolved in 0.6 parts of n-propanol was added six times at 30 minute intervals, and the reaction was completed by stirring for another 3 hours, to obtain a copolymer for pigment dispersion. The obtained pigment dispersion resin solution was dried to volatilize the solvent and residual monomer, and the pigment dispersion resin was extracted in solid form. Next, 50.0 parts of the solid pigment dispersion resin, 15.0 parts of 25% aqueous ammonia (Kishida Chemical Co., Ltd.), and 132.0 parts of water were added to another flask equipped with a stirrer, and the mixture was heated with stirring to neutralize and dissolve the pigment dispersion resin, thereby preparing an aqueous solution of the pigment dispersion resin. After dissolution, further water was added to adjust the solid content of the aqueous pigment dispersion resin solution to 25.0%.

[0060] <Preparation of concentrated pigment dispersion> [Production Example 2] 30.0 parts of the aqueous solution of the pigment dispersing resin prepared in Production Example 1, 20.0 parts of carbon black (Geotech D&C BLACK No. 2), and 30.0 parts of water were placed in a container and dispersed in a paint conditioner for 2 hours to obtain a concentrated pigment dispersion. [Production Example 3] 30.0 parts of the aqueous solution of the pigment dispersing resin prepared in Production Example 1, 10.0 parts of black iron oxide (BL-100HP manufactured by Titan Kogyo Co., Ltd.), and 20.0 parts of water were placed in a container and dispersed in a paint conditioner for 2 hours to obtain a concentrated pigment dispersion.

[0061] <Production of cosmetic resin composition> [Example 1] In a flask (reaction tank) equipped with a reflux condenser, a dropping funnel, a stirrer, a thermometer, a nitrogen gas inlet, and a raw material inlet, 73.6 parts of water, 0.48 parts of Emal 20C (Kao Corporation, sodium polyoxyethylene lauryl ether sulfate, active ingredient 25% by mass) as an anionic surfactant, 0.12 parts of Emulgen 109P (Kao Corporation, polyoxyethylene lauryl ether, active ingredient 100% by mass) as a non-reactive nonionic surfactant, and 0.12 parts of Rheodol TW-L120 (Kao Corporation, polyoxyethylene sorbitan monolaurate, active ingredient 100% by mass) as a non-reactive nonionic surfactant were charged, and the internal temperature was raised to 78°C while stirring under nitrogen gas introduction. On the other hand, 10.0 parts of methoxyethyl acrylate, 40.0 parts of ethyl methacrylate, 13.0 parts of trifluoroethyl methacrylate, 10.0 parts of isobutyl acrylate, 2.0 parts of benzyl acrylate, 20.0 parts of phenoxyethyl acrylate, 2.0 parts of acrylonitrile, 0.5 parts of acrylamide, 0.5 parts of 2-hydroxyethyl acrylate, 1.0 parts of acrylic acid, 1.0 parts of diallyl phthalate, 4.32 parts of Emal 20C, 0.48 parts of Emulgen 109P, 0.48 parts of Rheodol TW-L120, and 32.0 parts of water were stirred and mixed to prepare a pre-emulsion (emulsion of ethylenically unsaturated monomers), which was then charged into a dropping funnel (dropping tank). Furthermore, 9.6 parts, which is 7% of the pre-emulsion, was added to the reaction tank.

[0062] After the internal temperature stabilized, 2.0 parts of a 10% aqueous solution of ammonium persulfate was added as a polymerization initiator to the flask, and after 20 minutes had passed, the remaining part of the pre-emulsion and 2.0 parts of a 10% aqueous solution of ammonium persulfate were dropped from the dropping funnel over 240 minutes, and the reaction was carried out while raising the temperature and maintaining the internal temperature at 80°C. One and a half hours after the end of the dropping, 1.0 part of a 10% aqueous solution of ammonium persulfate was added, and the reaction was continued for another 3 hours while maintaining the temperature at 80°C, thereby obtaining an aqueous dispersion of polymer (A). After the reaction was completed, 25% ammonia water was added at room temperature of 25°C so as to neutralize the acid value of polymer (A) by 100%, and then further water was added to adjust the solid content of the aqueous dispersion of polymer (A) to 40.0%, thereby obtaining the intended cosmetic resin composition.

[0063] [Examples 2 to 19, Comparative Examples 1 and 2] A cosmetic resin composition was obtained in the same manner as in Example 1, except that the blending composition and blending amount (parts by mass) shown in Tables 1 and 2 were used. In Examples 10 and 11, the amount of EMALE 20C charged in the flask (reaction tank) was changed from 0.6 parts to 1.2 parts and 1.1 parts, respectively. In Examples 12 and 13, the amount of water charged in the flask (reaction tank) was changed from 53.6 parts and 51.6 parts, respectively, and the amount of water for pre-emulsion was changed from 32.0 parts to 22.0 parts and 20.0 parts, respectively, and further water was added after neutralization to adjust the final solid content to 50.0%. In Comparative Example 2, 1.5 parts of 2-ethylhexyl thioglycolate was further added to the mixture of ethylenically unsaturated monomers for pre-emulsion.

[0064] [Example 20] A cosmetic resin composition was obtained by stirring and mixing 18.0 parts of the cosmetic resin composition obtained in Example 7, 50.0 parts of the concentrated pigment dispersion of Production Example 2, 0.5 parts of Rheodol TW-S320V (polyoxyethylene sorbitan monostearate manufactured by Kao Corporation, active ingredient 100% by mass) as a pigment dispersant, 0.3 parts of NTC-CARBOMER 380 (carboxyvinyl polymer manufactured by Nikko Chemicals Corporation, active ingredient 100% by mass), 0.5 parts of ethanol, and 30.7 parts of water using a disperser.

[0065] [Examples 21 to 24, Comparative Examples 3 to 6] A cosmetic resin composition was obtained in the same manner as in Example 20, except that the formulation and amounts (parts by mass) shown in Table 3 were used.

[0066] Evaluation of cosmetic resin compositions Using the cosmetic resin composition prepared above, the viscoelasticity of the coating film and the contact angle of water were measured. Furthermore, as actual property evaluation, storage stability, water resistance, salt water resistance, oil resistance, cosmetic durability test, and skin irritation were evaluated. The results are shown in Tables 1 to 3.

[0067] <Measurement of Viscoelasticity of Coating Film of Cosmetic Resin Composition> The cosmetic resin composition was poured into a peelable silicone mold and dried at 40°C for 3 days to obtain a coating film of the cosmetic resin composition with a thickness of 1 mm. Furthermore, the storage modulus of the coating film was measured in the frequency dispersion mode at 37°C in the frequency range of 0.1 to 10 Hz using a viscoelasticity measuring device (Anton Paar's modular compact rheometer MCR-302). [Evaluation Criteria] A: 2×10 4 Pa or more 1×10 8 Pa or less. Good. B: 2×10 4 Pa or more 1×10 8 Not in the Pa range, but 1×10 4 Pa or more 1×10 9 It is within the range of 100 Pa or less. It can be used practically. C:1×10 4 Less than Pa or 1×10 9 Exceeds Pa. Problematic in practical use.

[0068] <Measurement of the contact angle of water on the coating film of the cosmetic resin composition> A cosmetic resin composition was applied to a glass substrate at a dry weight of 50 g / m 2 The coating was applied with an applicator so that the thickness of the coating was 100 μm, and then dried at 40°C for 24 hours to produce a coating film of the cosmetic resin composition. Water was dropped onto the coating surface of the coating film at 25°C using an automatic contact angle measuring device (Kyowa Interface Co., Ltd. DM-501), and the contact angle of water was measured 1 second after the drop had landed.

[0069] <Storage stability> The viscosity of the cosmetic resin composition was measured before the accelerated aging test. Next, the cosmetic resin composition was placed in a container and left to stand at 70°C for one month to conduct the accelerated aging test. After the accelerated aging test, the viscosity of the cosmetic resin composition was measured again. The viscosity was measured at 25°C using a B-type viscometer. The viscosity change rate before and after the accelerated test was calculated from the obtained viscosity value according to the following formula. Viscosity change rate (%) = |Initial viscosity - Viscosity after aging| x 100 [Evaluation Criteria] S: Viscosity change rate is less than 5%. Very good. A: Viscosity change rate is 5% or more and less than 10%. Good. B: Viscosity change rate is 10% or more and less than 30%. Practical use is possible. C: Viscosity change rate is 30% or more. Problematic for practical use.

[0070] <Water resistance evaluation> The cosmetic resin composition of Example 1 was applied to an artificial skin (Bioskin Plate P001-001 manufactured by Bealux) at a dry weight of 20 g / m 2 The coating was applied with an applicator so that the coating would become even. After coating, the coating was dried at 25°C for 120 minutes, and test pieces measuring 10 mm in length and 20 mm in width were prepared. Water was placed in a glass bottle, and the prepared test pieces were immersed in the bottle, sealed, and shaken in a bioshaker (TAITEC Corporation, BR-43FH) at 37°C and a shaking speed of 100 r / min for 10 hours. After shaking, the test pieces were removed and the degree of peeling of the coating film of the cosmetic resin composition was checked. [Evaluation Criteria] S: The area where the coating has peeled off is less than 1% of the total coating area. Very good. A: The area where the coating has peeled off is between 1% and 5% of the total coating area. Good. B: The peeled area of ​​the coating is 5% or more and less than 10% of the total coating area. Practical use is possible. C: The peeled area of ​​the coating is 10% or more of the total coating area. Problematic for practical use.

[0071] <Saltwater resistance evaluation> A 0.4% aqueous solution of sodium chloride was prepared in a glass bottle to have the same salt concentration as sweat, and the test piece prepared in the same procedure as for the water resistance evaluation was immersed in the solution, sealed, and the glass bottle was shaken in a bioshaker at 37°C and a shaking speed of 100 r / min for 10 hours. After penetration, the test piece was removed and the degree of peeling of the coating film of the cosmetic resin composition was confirmed. [Evaluation Criteria] S: The area where the coating has peeled off is less than 1% of the total coating area. Very good. A: The area where the coating has peeled off is between 1% and 5% of the total coating area. Good. B: The peeled area of ​​the coating is 5% or more and less than 10% of the total coating area. Practical use is possible. C: The peeled area of ​​the coating is 10% or more of the total coating area. Problematic for practical use.

[0072] <Oil resistance evaluation> Jojoba oil was placed in a glass bottle as an oil component similar to sebum, and the test piece prepared in the same manner as in the water resistance evaluation was immersed in the bottle, sealed, and the glass bottle was shaken in a bioshaker at 37°C and a shaking speed of 100 r / min for 10 hours. After shaking, the test piece was removed and the degree of peeling of the coating film of the cosmetic resin composition was confirmed. [Evaluation Criteria] S: The area where the coating has peeled off is less than 1% of the total coating area. Very good. A: The area where the coating has peeled off is between 1% and 5% of the total coating area. Good. B: The peeled area of ​​the coating is 5% or more and less than 10% of the total coating area. Practical use is possible. C: The peeled area of ​​the coating is 10% or more of the total coating area. Problematic for practical use.

[0073] <Cosmetic durability test> The cosmetic resin composition was applied to the eyelids of 10 subjects with a brush and allowed to dry naturally to form a film. Next, the subjects put on protective goggles and evaluated the state of the makeup after 12 hours. [Evaluation Criteria] S: All 10 judged the makeup to last well. Extremely well. A: 8 or 9 people judged the makeup to last well. Good. B: 7 people judged that the makeup lasted well. Practical use is possible. C: Six or fewer judged the makeup to be well-lasting. There is a problem in practical use.

[0074] <Skin irritation> The above cosmetic resin composition was applied to the inside of the arm of 10 subjects, and 24 hours later, the subjects were asked to evaluate whether they felt any abnormality such as itching or pain. [Evaluation Criteria] S: 0 subjects experienced any abnormalities. Very good. A: One subject experienced abnormal symptoms. Good. B: Two subjects experienced abnormalities. Practical use possible. C: Three or more subjects felt abnormal. Practical problem.

[0075] [Table 1]

[0076] [Table 2]

[0077] [Table 3]

[0078] The abbreviations in the table are as follows. Rheodol TW-S320V: Polyoxyethylene sorbitan tristearate (20E.O.) (Kao Corporation) NTC-CARBOMER 380: Carboxyvinyl polymer (manufactured by Nikko Chemicals)

[0079] As can be seen from the results in Tables 1 to 3, the cosmetic resin compositions of the Examples have excellent storage stability, and the coating films have good water resistance, salt water resistance, and oil resistance, and are excellent in cosmetic durability under harsh conditions and have very little skin irritation. On the other hand, the cosmetic resin compositions of the Comparative Examples are significantly inferior in any of the above performances, making it clear that they are problematic in practical use.

Claims

1. A cosmetic resin composition for application onto the skin, wherein a coating of the cosmetic resin composition has a storage modulus of 1×10 measured at 37° C. in a frequency range of 0.1 Hz to 10 Hz. 4 Pa or more 1×10 9 and when water is dropped onto a coating film of the cosmetic resin composition at 25° C., the contact angle of water 1 second after landing is 5° or more and 90° or less.

2. 2. The cosmetic resin composition according to claim 1, comprising an aqueous medium and a polymer (A), the polymer (A) being a polymer of an ethylenically unsaturated monomer and containing 90.0% by mass or more and 99.5% by mass or less of a nonionic ethylenically unsaturated monomer (a) having an octanol / water partition coefficient (Log Kow) of 0.4 or more and less than 2.5 at 25° C. based on the total mass of the ethylenically unsaturated monomer, and the acid value of the polymer (A) is 3.0 mgKOH / g or more and 50.0 mgKOH / g or less.

3. The cosmetic resin composition according to claim 1, wherein the monomer (a) comprises a nonionic ethylenically unsaturated monomer (a-1) having a logarithm of an octanol / water partition coefficient (Log Kow) at 25°C of 0.4 or more and less than 2.0, and a nonionic ethylenically unsaturated monomer (a-2) having a logarithm of an octanol / water partition coefficient (Log Kow) of 2.0 or more and less than 2.5, and the cosmetic resin composition comprises 20.0% by mass or more and 79.5% by mass or less of the monomer (a-1) and 20.0% by mass or more and 79.5% by mass or less of the monomer (a-2).

4. 2. The cosmetic resin composition according to claim 1, wherein the average particle size of the polymer (A) is from 30 nm to 400 nm.

5. A cosmetic comprising the cosmetic resin composition according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Cosmetics

    JP2002284629A

  • Organic-inorganic hybrid copolymer and method for producing the same

    JP2003226706A

  • Skin adhesive sheet, and sheet-like external preparation for skin

    WO2016189697A1

  • Resin for cosmetic use

    JP2005002207A

  • Eye make-up cosmetics

    JP2016160222A