Powder quick setting admixture, water stopper material, water stopper, manufacturing method of structure, and cut-off method
The powder quick-setting agent, with a base material and ion-releasing compound, enhances both short-term and long-term water-stopping properties by forming concretions in cracks, addressing the limitations of conventional quick-setting agents.
Patent Information
- Application Number
- JP2024028991
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-02-28
- Publication Date
- 2024-11-06
AI Technical Summary
Conventional water-stopping materials using quick-setting agents effectively stop water in the short term but fail to maintain long-term water-stopping properties, and they struggle to seal minute cracks, leading to new water leaks over time.
A powder quick-setting agent comprising a base material and an ion-releasing compound that forms poorly water-soluble salts, which is applied in a water-stopping material to enhance both short-term and long-term sealing capabilities by forming concretions in cracks.
The powder quick-setting agent improves both short-term and long-term water-stopping properties by forming concretions in cracks and densifying the water-stopping area, effectively preventing new leaks.
Smart Images

Figure 2024156606000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a powder quick-setting admixture. The present invention also relates to a water-stopping material using the powder quick-setting admixture. The present invention also relates to a water-stopping material using the water-stopping material. The present invention also relates to a method for manufacturing a structure using the water-stopping material and a water-stopping method. [Background technology]
[0002] In construction work for tunnels, underground spaces, slopes, etc., water leakage or spring water may occur from walls, ceilings, slopes, etc. Conventionally, sprayed materials such as sprayed concrete have been used to stop water leakage or spring water. The sprayed materials (water-stopping materials) used for water-stopping purposes must withstand water pressure and adhere to the target water-stopping area immediately after being sprayed onto the target water-stopping area. For this reason, the materials for the sprayed materials (water-stopping materials) used for water-stopping purposes usually contain an accelerator.
[0003] As an example of an accelerator, the following Patent Document 1 discloses a cement accelerator having a molar ratio (CaO / Al2O3) of 2.0 to 2.6 between CaO and Al2O3 as chemical components, and a total of 86 to 94 mass% of CaO and Al2O3. The remainder of this cement accelerator contains SiO2 and Fe2O3 as chemical components in a mass ratio (SiO2 / Fe2O3) of 8 to 15, and the content of SiO2 and Fe2O3 in the remainder is 50 mass% or more. This cement accelerator contains a CaO-Al2O3-SiO2-Fe2O3-based amorphous material as an active ingredient. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-071536 A Summary of the Invention [Problem to be solved by the invention]
[0005] Conventional water-stopping materials containing quick-setting agents can effectively stop water in the short term. However, when water is stopped in one place, a new water path may be formed starting from another crack, and new water leaks may occur after a relatively long time has passed since the water-stopping work. In addition, since it is difficult to place water-stopping materials in the fine cracks, new water leaks may occur after a relatively long time has passed since the water-stopping work.
[0006] In this way, when using a water-stopping material containing a conventional quick-setting agent, even if the short-term water-stopping property of the resulting water-stopping material can be improved, it is difficult to improve the long-term water-stopping property.
[0007] An object of the present invention is to provide a powder quick-setting admixture which, when used as a quick-setting admixture in a water-stopping material, can enhance not only short-term water-stopping properties but also long-term water-stopping properties in the resulting water-stopping material. Another object of the present invention is to provide a water-stopping material using the powder quick-setting admixture. Another object of the present invention is to provide a water-stopping material using the water-stopping material. Another object of the present invention is to provide a method for manufacturing a structure using the water-stopping material and a water-stopping method. [Means for solving the problem]
[0008] In this specification, the following powder quick-setting admixture, water-stopping material, water-stopping material, method for manufacturing a structure, and water-stopping method are disclosed.
[0009] Item 1. A powder quick-setting admixture comprising a base material and an ion-releasing compound capable of releasing cations or anions, the ion-releasing compound being present at least on a surface of the base material, and the ion-releasing compound being capable of generating a poorly water-soluble salt.
[0010] Item 2. The powder quick-setting admixture according to Item 1, wherein the poorly water-soluble salt is calcium carbonate.
[0011] Item 3. The powder quick-setting admixture according to Item 1 or 2, wherein the ion-releasing compound is sodium bicarbonate, sodium carbonate, calcium formate, calcium acetate, calcium lactate, or calcium chloride.
[0012] Item 4. The powder quick-setting admixture according to any one of Items 1 to 3, wherein the base material is a resin.
[0013] Item 5. The powder quick-setting admixture according to any one of Items 1 to 4, wherein the base material is a thermoplastic resin.
[0014] Item 6. The powder quick-setting admixture according to any one of Items 1 to 5, wherein the ion-releasing compound is present on the surface of the powder quick-setting admixture and inside the powder quick-setting admixture.
[0015] Item 7. A water-stopping material comprising cement milk or mortar and the powder quick-setting admixture according to any one of items 1 to 6.
[0016] Item 8. The water-stopping material according to item 7, having a pot life of 1 minute or more and 30 minutes or less.
[0017] Item 9. A water-stopping material which is a cured product of the water-stopping material according to item 7 or 8.
[0018] Item 10. Compressive strength at 24 hours is 0.1N / mm 2 More than 5.0N / mm 2 Item 10. The water-stopping material according to item 9, which is as follows:
[0019] Item 11. A method for manufacturing a structure, comprising: a step of placing the water-stopping material according to item 7 or 8 at a waterproofing target portion of a waterproofing target object; and a step of hardening the water-stopping material.
[0020] Item 12. A water-stopping method for sealing a target part of a water-stopping object using the water-stopping material according to item 7 or 8. Effect of the Invention
[0021] The powder quick-setting admixture according to the present invention includes a base material and an ion-releasing compound capable of releasing cations or anions, the ion-releasing compound being present at least on the surface of the base material, and the ion-releasing compound being capable of generating a poorly water-soluble salt. Since the powder quick-setting admixture according to the present invention has the above-mentioned configuration, when used as a quick-setting admixture in a water-stopping material material, the resulting water-stopping material can have improved water-stopping properties not only in the short term but also in the long term. [Brief description of the drawings]
[0022] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a powder quick-setting admixture according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram for explaining a method for evaluating short-term water stoppage ability in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The present invention will be described in detail below.
[0024] (Powder quick-setting agent) The powder quick-setting admixture of the present invention includes a base material and an ion-releasing compound capable of releasing cations or anions, the ion-releasing compound being present on at least the surface of the base material, and the ion-releasing compound being capable of generating a poorly water-soluble salt.
[0025] Hereinafter, in this specification, the "powder quick-setting admixture" may be abbreviated to "quick-setting admixture".
[0026] As used herein, "poorly water-soluble salt" means a salt in which, when 1 g of the poorly water-soluble salt is placed in 100 g of water and kept at 20°C for 10 minutes, the weight of the poorly water-soluble salt that dissolves in water is 0.1 g or less.
[0027] Since the quick-setting admixture according to the present invention has the above-mentioned configuration, when it is used as a quick-setting admixture in a water-stopping material, the resulting water-stopping material can have improved not only short-term water-stopping properties but also long-term water-stopping properties.
[0028] The quick-setting admixture according to the present invention is preferably used by mixing with a component containing cement (e.g., cement milk or mortar). The quick-setting admixture according to the present invention is preferably used by mixing with a component containing cement to obtain a water-stopping material. Since the quick-setting admixture according to the present invention is a powder, it is easily mixed with a component containing cement.
[0029] In the quick-setting admixture according to the present invention, the ion-releasing compound is present on at least the surface of the base material. Therefore, when the quick-setting admixture is mixed with a component containing cement, the component can be hardened in a short period of time by the quick-setting action, and the short-term water-stopping property of the resulting water-stopping material can be improved.
[0030] In addition, since the quick-setting admixture according to the present invention contains the ion-releasing compound, the water-stopping material also contains the ion-releasing compound. When the water-stopping material comes into contact with leaking water, the ion-releasing compound releases ions, generating poorly water-soluble salts and forming concretions. In addition, the ion-releasing compound or the ions released from the ion-releasing compound dissolve in the leaking water and move to fine cracks, so that concretions are also formed in the fine cracks. This makes the water-stopping area and its surroundings more dense, and can also improve long-term water-stopping properties.
[0031] The quick-setting admixture is a powder. The quick-setting admixture may be in a spherical shape, a substantially spherical shape, a pellet shape, or a shape other than these.
[0032] The average particle size of the quick-setting agent is preferably 10 μm or more, more preferably 30 μm or more, preferably 1000 μm or less, more preferably 500 μm or less, and even more preferably 100 μm or less. When the average particle size of the quick-setting agent is equal to or more than the lower limit, the dispersibility in the water-stopping material can be further improved. When the average particle size of the quick-setting agent is equal to or less than the upper limit, the viscosity of the water-stopping material can be easily improved.
[0033] The average particle size of the quick-setting admixture is the number average particle size. The average particle size of the quick-setting admixture is obtained by observing 50 random quick-setting admixtures with an electron microscope or an optical microscope and calculating the average particle size. The particle size of the quick-setting admixture means the circle-equivalent diameter of the cross section of the quick-setting admixture.
[0034] In the quick-setting admixture, the ion-releasing compound is present at least on the surface of the base material. In the quick-setting admixture, the ion-releasing compound is preferably present at least on the surface of the quick-setting admixture. The ion-releasing compound may be present only on the surface of the quick-setting admixture, or may be present on the surface of the quick-setting admixture and inside the quick-setting admixture.
[0035] In the quick-setting agent, it is preferable that the ion-releasing compound is present on the surface of the quick-setting agent and inside the quick-setting agent. In this case, when the water-stopping material comes into contact with water, the ions of the ion-releasing compound present inside the quick-setting agent are gradually released, so that the long-term water-stopping ability can be further improved compared to the case where the ion-releasing compound is present only on the surface of the quick-setting agent.
[0036] Hereinafter, the present invention will be described in detail with reference to the drawings. Note that in the drawings, for convenience of illustration, the size of each component may differ from the actual size.
[0037] FIG. 1 is a cross-sectional view that illustrates a powder quick-setting admixture according to one embodiment of the present invention.
[0038] The quick-setting admixture 1 (powder quick-setting admixture) shown in Fig. 1 includes a base material 2 and an ion-releasing compound. The ion-releasing compound includes an ion-releasing compound 31 present on the surface of the quick-setting admixture 1, and an ion-releasing compound 32 present inside the quick-setting admixture 1. The ion-releasing compound 31 is present on the surface of the base material 2. The ion-releasing compound 32 is present inside the base material 2. The surface of the quick-setting admixture 1 is constituted by the surface of the base material 2 and the surface of the ion-releasing compound 31.
[0039] Hereinafter, the details of each component used in the quick-setting admixture according to the present invention will be described.
[0040] <Base material> The quick-setting agent contains a base material. Examples of the base material include resin. The base material may be used alone or in combination of two or more kinds.
[0041] Examples of the resin include thermoplastic resins, cured products of curable resins, ion exchange resins, etc. The resins may be used alone or in combination of two or more.
[0042] Examples of the thermoplastic resin include fluororesin, polyolefin resin, polyvinyl chloride resin, polyamide resin, polycarbonate resin, polystyrene resin, polyester resin, acrylonitrile-butadiene-styrene resin (ABS resin), polyethylene terephthalate (PET), polymethyl methacrylate (PMMA), etc. The thermoplastic resin may be used alone or in combination of two or more kinds.
[0043] Examples of the polyolefin resin include polyethylene, polypropylene, ethylene-propylene copolymer (EPDM), isobutylene-isoprene copolymer, polystyrene, polybutene, polyisobutylene, polybutadiene, acrylonitrile-butadiene copolymer, ethylene-vinyl acetate copolymer, and ethylene-α-olefin copolymer.
[0044] Examples of the curable resin include modified silicone resin, silicone resin, epoxy resin, acrylic resin, unsaturated polyester resin, polyurea resin, urethane resin, phenol resin, vinyl ester resin, naphthoxazine resin, etc. The curable resin may be used alone or in combination of two or more kinds.
[0045] Examples of the ion exchange resin include strongly acidic cation exchange resins such as cation exchange resins having sulfonic acid groups, and weakly acidic cation exchange resins such as cation exchange resins having methacrylic carboxylic acid groups and cation exchange resins having acrylic carboxylic acid groups.
[0046] The base material is preferably a resin, more preferably a thermoplastic resin, further preferably polyethylene, polypropylene, polystyrene, polyamide resin, ethylene-vinyl acetate copolymer, or polyethylene terephthalate, and particularly preferably ethylene-vinyl acetate copolymer or polyethylene terephthalate. In this case, the affinity between the base material and water can be increased, so that the water absorption rate and the ion release rate can be increased.
[0047] In 100% by weight of the quick-setting admixture, the content of the base material is preferably 33% by weight or more, more preferably 50% by weight or more, preferably 90% by weight or less, and more preferably 82% by weight or less. When the content of the base material is equal to or more than the lower limit and equal to or less than the upper limit, the content of the ion-releasing compound in the quick-setting admixture can be set within a suitable range, and the effects of the present invention can be more effectively exhibited.
[0048] <Ion-releasing compound> The quick-setting agent contains an ion-releasing compound capable of releasing cations or anions, and the ion-releasing compound is capable of generating a poorly water-soluble salt.
[0049] The ion-releasing compound may be a compound capable of releasing a cation, a compound capable of releasing an anion, a compound capable of releasing both a cation and an anion, or a mixture of a compound capable of releasing a cation and a compound capable of releasing an anion. The ion-releasing compound may be in the form of particles. The ion-releasing compound may be used alone or in combination of two or more kinds.
[0050] The ion-releasing compound is preferably a compound capable of generating a poorly water-soluble salt upon contact with moisture. When the ion-releasing compound is a compound capable of releasing cations, it is preferable that the cations released from the ion-releasing compound and the anions dissolved in moisture or the like undergo a chemical reaction to generate a poorly water-soluble salt. When the ion-releasing compound is a compound capable of releasing anions, it is preferable that the anions released from the ion-releasing compound and the cations dissolved in moisture or the like undergo a chemical reaction to generate a poorly water-soluble salt. In addition, when the ion-releasing compound is a compound capable of releasing both cations and anions, or a mixture of a compound capable of releasing cations and a compound capable of releasing anions, it is preferable that the cations and anions released from the ion-releasing compound move through moisture or the like to a medium, and generate a poorly water-soluble salt at the point where they meet.
[0051] Examples of the poorly water-soluble salt include calcium carbonate, barium carbonate, calcium phosphate, calcium sulfate, calcium silicate, and iron hydroxide.
[0052] From the viewpoint of forming concretions more satisfactorily and further enhancing long-term water-stopping properties, the poorly water-soluble salt is preferably calcium carbonate, i.e., the ion-releasing compound is preferably capable of generating calcium carbonate as a poorly water-soluble salt.
[0053] Examples of the ion-releasing compound include calcium sulfate, sodium chloride, calcium chloride, potassium chloride, calcium nitrite, sodium nitrite, potassium nitrite, calcium nitrate, sodium nitrate, potassium nitrate, sodium thiocyanate, sodium hydroxide, potassium hydroxide, lithium carbonate, sodium carbonate, potassium carbonate, ammonium hydrogen carbonate, sodium silicate, aluminum hydroxide, aluminum oxide, sodium aluminum dioxide, calcium aluminate, magnesium silicofluoride, boric acid, dipotassium hydrogen phosphate, zinc oxide, lead oxide, copper oxide, amines, maleic anhydride, oxycarboxylic acid, oxycarboxylate, keto acid, keto acid salt, aminocarboxylic acid, aminocarboxylate, polymeric organic acid, polymeric organic acid salt, water-soluble acrylic acid, water-soluble acrylic acid salt, tricalcium silicate, dicalcium silicate, calcium aluminate, calcium aluminoferrite, calcium hydroxide, calcium oxide, calcium formate, calcium acetate, calcium magnesium acetate, calcium stearate, calcium citrate, calcium malate, calcium benzoate, calcium oxalate, calcium lactate, calcium hydrogen carbonate, potassium hydrogen carbonate, and sodium hydrogen carbonate.
[0054] The ion-releasing compound is preferably a carbonate, an organic acid calcium salt, or calcium chloride, more preferably sodium hydrogen carbonate, sodium carbonate, calcium formate, calcium acetate, calcium lactate, or calcium chloride, and even more preferably sodium carbonate, calcium formate, calcium acetate, calcium lactate, or calcium chloride. In this case, the quick-setting property can be further improved, and the short-term water-stopping property can be further improved. In addition, calcium carbonate can be generated as the poorly water-soluble salt, and the long-term water-stopping property can be further improved.
[0055] The ion-releasing compound may be spherical, may be a shape other than spherical, or may be flat. The ion-releasing compound is preferably spherical.
[0056] The average particle size of the ion-releasing compound is preferably 1.0 μm or more, more preferably 5.0 μm or more, even more preferably 10 μm or more, preferably 200 μm or less, more preferably 150 μm or less, and even more preferably 120 μm or less. When the average particle size of the ion-releasing compound is the above lower limit or more, the dispersibility in the quick-setting admixture can be improved. When the average particle size of the ion-releasing compound is the above lower limit or more, the ion-releasing compound is well coated with a coating agent described below, and the dispersibility in the quick-setting admixture can be improved. When the average particle size of the ion-releasing compound is the above upper limit or less, the viscosity of the water-stopping material can be improved when the water-stopping material is placed at the location to be stopped.
[0057] The average particle size of the ion-releasing compound refers to the number average particle size. The average particle size of the ion-releasing compound is determined by observing 50 random ion-releasing compounds with an electron microscope or optical microscope and calculating the average value. The particle size of the ion-releasing compound refers to the equivalent circle diameter of the cross section of the ion-releasing compound.
[0058] In the quick-setting admixture, the surface of the ion-releasing compound may be coated with a coating agent. In this case, the timing and amount of cations or anions released from the ion-releasing compound can be controlled.
[0059] The ion-releasing compound coated with the coating agent is preferably capable of releasing cations or anions when moisture comes into contact with the quick-setting agent or water-stopping material and diffuses and penetrates into the inside of the coating agent. The ion-releasing compound coated with the coating agent may be capable of releasing cations or anions from voids in the coating agent. The ion-releasing compound coated with the coating agent may be capable of diffusing into the inside of the coating agent and releasing cations or anions. In these cases, the timing and amount of cations or anions released from the ion-releasing compound can be controlled even better.
[0060] Examples of the material of the coating agent include resins. The material of the coating agent preferably contains a resin. In this case, the dispersibility of the ion-releasing compound in the quick-setting agent and the water-stopping material can be improved, and the timing and amount of the release of cations or anions can be well controlled. In addition, the surface of the ion-releasing compound can be uniformly coated with the coating agent.
[0061] The resin that is the material of the coating agent and the resin that is the base material may be the same type of resin (resins with the same resin name) or different types of resin (resins with different resin names).
[0062] Examples of the resin include water-soluble resins, thermoplastic resins, thermosetting resins, photocurable resins, and moisture-curable resins. The resins may be used alone or in combination of two or more.
[0063] Examples of the water-soluble resin include polyvinyl alcohol, polylactic acid resin (PLA resin), poly(meth)acrylic acid, poly(meth)acrylamide, polyvinylpyrrolidone, polyethylene oxide, and methylcellulose.
[0064] Examples of the thermoplastic resin include polyolefin resin, polyvinyl chloride resin, polyamide resin, polycarbonate resin, polystyrene resin, polyester resin, acrylonitrile-butadiene-styrene resin (ABS resin), polyethylene terephthalate (PET), and polymethyl methacrylate (PMMA).
[0065] Examples of the polyolefin resin include polyethylene, polypropylene, polystyrene, polybutene, polyisobutylene, polybutadiene, ethylene-vinyl acetate copolymer, and ethylene-α-olefin copolymer.
[0066] Examples of the thermosetting resin include epoxy resin, phenol resin, (meth)acrylic resin, unsaturated polyester resin, vinyl ester resin, polyimide resin, urethane resin, polyurea resin, etc. The thermosetting resin may be used in combination with a thermosetting agent.
[0067] Examples of the photocurable resin include (meth)acrylic resin, (meth)acrylic urethane resin, epoxy resin, silicone resin, etc. The photocurable resin may be used in combination with a photopolymerization initiator.
[0068] Examples of the moisture-curable resin include moisture-curable urethane resins and hydrolyzable silyl group-containing resins.
[0069] The thickness of the coating agent (the thickness of the coating layer formed by the coating agent) is not particularly limited. From the viewpoint of better controlling the timing and amount of release of cations or anions from the ion-releasing compound, the thickness of the coating agent is preferably 0.5 μm or more, more preferably 1 μm or more, and preferably 25 μm or less, more preferably 20 μm or less.
[0070] In 100% by weight of the quick-setting admixture, the content of the ion-releasing compound is preferably 5% by weight or more, more preferably 15% by weight or more, preferably 99% by weight or less, more preferably 75% by weight or less. When the content of the ion-releasing compound is equal to or more than the lower limit and equal to or less than the upper limit, the quick-setting property can be further improved, and the short-term water-stopping property can be further improved. When the content of the ion-releasing compound is equal to or more than the lower limit and equal to or less than the upper limit, the cations or anions are more effectively released, and the poorly water-soluble salt can be more satisfactorily generated, so that the long-term water-stopping property can be further improved.
[0071] In 100% by weight of the quick-setting admixture, the total content of the base material and the ion-releasing compound is preferably 90% by weight or more, more preferably 95% by weight or more, even more preferably 97.5% by weight or more, particularly preferably 99% by weight or more, and most preferably 100% by weight. When the total content is equal to or more than the lower limit, the effect of the present invention can be more effectively exhibited. In addition, in 100% by weight of the quick-setting admixture, the total content of the base material and the ion-releasing compound may be 100% by weight or less, may be less than 100% by weight, may be 99% by weight or less, or may be 98% by weight or less.
[0072] <Other ingredients> The quick-setting admixture may contain other components different from both the base material and the ion-releasing compound. Examples of the other components include a surface modifier, a thixotropic agent, and an antioxidant. The other components may be used alone or in combination of two or more.
[0073] (Waterstop material) The water-stopping material according to the present invention contains cement milk or mortar and the above-mentioned quick-setting admixture.
[0074] In this specification, "cement milk" refers to a mixture of cement and water (mixing water). In this specification, "cement milk" does not include fine aggregate. In this specification, "mortar" refers to a mixture of cement, fine aggregate, and water (mixing water). In this specification, "cement" refers to a powder whose main raw materials are limestone, clay, silica stone, and iron oxide raw materials, and which can harden by a chemical reaction with water.
[0075] As the cement milk and the mortar, conventionally known cement milk and mortar can be used.
[0076] When the water-stopping material contains cement milk, the injectability of the water-stopping material can be improved. When the water-stopping material contains mortar, shrinkage caused by hardening of cement (autogenous shrinkage) and shrinkage caused by drying after hardening (drying shrinkage) can be suppressed.
[0077] The cement contained in the cement milk and the mortar is not particularly limited. Examples of the cement contained in the cement milk and the mortar include Portland cement, blast furnace cement, silica cement, and fly ash cement.
[0078] Examples of the fine aggregate in the mortar include artificial aggregate and natural aggregate. Examples of the artificial aggregate include blast furnace slag and fly ash. Examples of the natural aggregate include sand. From the viewpoint of reducing material costs, the fine aggregate in the mortar is preferably sand.
[0079] The average particle size of the fine aggregate in the mortar is preferably 5 μm or more, more preferably 10 μm or more, preferably 2000 μm or less, more preferably 1000 μm or less, even more preferably 500 μm or less, and particularly preferably 100 μm or less. When the average particle size of the fine aggregate in the mortar is the above lower limit or more, the strength of the mortar can be improved. When the average particle size of the fine aggregate in the mortar is the above upper limit or less, the fine aggregate can be prevented from settling in the mortar, and the injectability of the water-stopping material can be improved.
[0080] In order to more effectively exert the effects of the present invention, the cement content in 100% by weight of the cement milk is preferably 10% by weight or more, more preferably 20% by weight or more, even more preferably 30% by weight or more, preferably 90% by weight or less, more preferably 80% by weight or less, and even more preferably 70% by weight or less.
[0081] From the viewpoint of exerting the effects of the present invention more effectively, in the above-mentioned cement milk, the content of water (mixing water) per 100 parts by weight of cement is preferably 11 parts by weight or more, more preferably 25 parts by weight or more, even more preferably 35 parts by weight or more, preferably 125 parts by weight or less, more preferably 100 parts by weight or less, and even more preferably 67 parts by weight or less.
[0082] From the viewpoint of exerting the effects of the present invention more effectively, the cement content in 100% by weight of the above mortar is preferably 10% by weight or more, more preferably 15% by weight or more, even more preferably 20% by weight or more, preferably 60% by weight or less, more preferably 50% by weight or less, and even more preferably 40% by weight or less.
[0083] In order to more effectively exert the effects of the present invention, the content of fine aggregate in 100% by weight of the mortar is preferably 10% by weight or more, more preferably 15% by weight or more, even more preferably 20% by weight or more, and preferably 90% by weight or less, more preferably 85% by weight or less, and even more preferably 80% by weight or less.
[0084] From the viewpoint of exerting the effects of the present invention more effectively, in the above mortar, the content of the fine aggregate per 100 parts by weight of cement is preferably 11 parts by weight or more, more preferably 25 parts by weight or more, even more preferably 40 parts by weight or more, and preferably 900 parts by weight or less, more preferably 400 parts by weight or less, and even more preferably 250 parts by weight or less.
[0085] From the viewpoint of exerting the effects of the present invention more effectively, in the above mortar, the content of water (mixing water) per 100 parts by weight of cement is preferably 20 parts by weight or more, more preferably 30 parts by weight or more, even more preferably 40 parts by weight or more, and preferably 200 parts by weight or less, more preferably 100 parts by weight or less, and even more preferably 60 parts by weight or less.
[0086] In order to more effectively exert the effects of the present invention, the content of the cement milk in 100% by weight of the water-stopping material is preferably 80% by weight or more, more preferably 90% by weight or more, even more preferably 95% by weight or more, preferably 99.9% by weight or less, more preferably 99.5% by weight or less, and even more preferably 99% by weight or less.
[0087] From the viewpoint of exerting the effects of the present invention more effectively, the content of the mortar in 100% by weight of the water-stopping material is preferably 80% by weight or more, more preferably 90% by weight or more, even more preferably 95% by weight or more, preferably 99.9% by weight or less, more preferably 99.5% by weight or less, and even more preferably 99% by weight or less.
[0088] From the viewpoint of exerting the effects of the present invention more effectively, in the water-stopping material, the content of the quick-setting admixture per 100 parts by weight of the cement milk is preferably 1 part by weight or more, more preferably 5 parts by weight or more, even more preferably 7 parts by weight or more, preferably 100 parts by weight or less, more preferably 75 parts by weight or less, and even more preferably 50 parts by weight or less.
[0089] From the viewpoint of exerting the effects of the present invention more effectively, in the water-stopping material, the content of the quick-setting admixture relative to 100 parts by weight of the mortar is preferably 1 part by weight or more, more preferably 5 parts by weight or more, even more preferably 7 parts by weight or more, preferably 50 parts by weight or less, more preferably 30 parts by weight or less, and even more preferably 10 parts by weight or less.
[0090] The water-stopping material may contain other components in addition to the three components of the cement milk, the mortar, and the quick-setting agent, if necessary. The other components include foaming agents, reaction catalysts, reaction accelerators, crosslinking agents, water absorbents, foam stabilizers, antioxidants, colorants, and other quick-setting agents different from the quick-setting agent (the quick-setting agent according to the present invention). Only one of the other components may be used, or two or more of them may be used in combination.
[0091] The foaming agent includes animal protein-based surfactants, anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants.
[0092] The pot life of the water-stopping material is preferably 1 minute or more, more preferably 2 minutes or more, preferably 60 minutes or less, more preferably 30 minutes or less, and even more preferably 15 minutes or less. If the pot life is equal to or greater than the lower limit, significant hardening during addition and mixing of the quick-setting agent can be prevented, and workability can be improved. If the pot life is equal to or less than the upper limit, short-term water-stopping properties can be further improved.
[0093] The pot life of the water-stopping material is the pot life of the water-stopping material in an environment of 20°C ± 1°C. The pot life of the water-stopping material is measured in an environment of 20°C ± 1°C as follows. The cement milk or mortar and the above-mentioned quick-setting agent are mixed in a manner conforming to JIS A1138 "How to make concrete in a laboratory" to obtain a water-stopping material (measurement sample). Immediately after the mixing is completed, 400 g of the obtained measurement sample is placed on the surface of a polyethylene sheet (40 cm long x 40 cm wide) attached to the surface of an iron plate. Next, while wearing nitrile rubber gloves, the upper surface of the measurement sample is touched at 1 minute intervals. The time from the end of the preparation of the measurement sample (the end of mixing) to the last time the water-stopping material adheres to the gloves is regarded as the pot life of the water-stopping material. For example, if the waterstop material adheres to the glove when the top surface of the measurement sample is touched 5 minutes after the completion of the preparation of the measurement sample, and if the waterstop material does not adhere to the glove when the top surface of the measurement sample is touched 6 minutes after the completion of the preparation of the measurement sample, the usable life of the waterstop material is 5 minutes.
[0094] The method of preparation of the above-mentioned water-stopping material for actual use does not have to conform to JIS A1138 "Concrete preparation method in a test laboratory."
[0095] (Water-stopping material) The waterproofing material according to the present invention is a cured product of the above-mentioned waterproofing material.
[0096] The compressive strength of the water-stopping material at 24 hours is preferably 0.1 N / mm 2 More preferably, 0.15N / mm 2More than 5.0N / mm 2 Less than or equal to 3.0N / mm 2 Less than 2.0N / mm 2 When the compressive strength is equal to or greater than the lower limit, the strength of the waterstop material can be increased. When the compressive strength is equal to or less than the upper limit, when an external stress such as an earthquake is applied to a structure in which the waterstop material is disposed, the distribution of stress generated at the location where the waterstop material is disposed and its surroundings can be improved.
[0097] The compressive strength of the above water-stopping material at 24 hours of age can be measured in accordance with JIS A1108:2018 "Test method for compressive strength of concrete."
[0098] (Water-stopping method, structure and manufacturing method thereof) The above-mentioned water-stopping material can be used to stop water in a target area. A water-stopping method according to the present invention is a method for stopping water in a target area of a water-stopping object by using the above-mentioned water-stopping material.
[0099] Moreover, a structure can be obtained by using the above-mentioned water-stopping material. The above-mentioned structure preferably includes a water-stopping target object having a water-stopping target portion, and a cured product of the water-stopping material arranged in the water-stopping target portion. The cured product of the water-stopping material is a water-stopping material.
[0100] The method for manufacturing a structure according to the present invention includes a disposing step of disposing the above-mentioned water-stopping material in a waterproofing target portion of a waterproofing target object, and a hardening step of hardening the water-stopping material. The method for manufacturing a structure obtains a structure including a hardened product of the water-stopping material disposed in the waterproofing target portion. The hardened product of the water-stopping material is a water-stopping material.
[0101] In order to effectively exert the effects of the present invention, it is preferable that the water-stopping object includes ground or concrete.
[0102] The method for producing a structure according to the present invention preferably includes a mixing step of mixing the cement milk or mortar with the quick-setting agent to obtain the water-stopping material. The method for producing a structure according to the present invention preferably includes the mixing step, the arrangement step, and the hardening step in this order.
[0103] In the mixing step, the method of mixing the cement milk or mortar with the quick-setting admixture is not particularly limited, and a conventionally known method can be adopted. Examples of the mixing method in the mixing step include the following method. Cement milk or mortar is poured into a mixing bowl and dry-mixed for 15 seconds. Next, the quick-setting admixture is poured into the mixing bowl and dry-mixed for 10 seconds, after which mixing water is poured and mixed quickly and continuously with both hands for 10 to 15 seconds.
[0104] In the disposing step, the method of disposing the water-stopping material on the target area to be waterproofed is not particularly limited, and a conventionally known method can be adopted. The disposing step may be a step of spraying the water-stopping material on the target area to be waterproofed, a step of applying the water-stopping material on the target area to be waterproofed, or a step of injecting the water-stopping material into the target area to be waterproofed.
[0105] The method of spraying the waterproofing material to the target area includes a method of spraying the waterproofing material to the target area by air pressure, etc. The spraying method may be a dry method or a wet method.
[0106] The method of applying the water-stopping material to the target water-stopping area includes a method of V-cutting the target water-stopping area and then applying the water-stopping material to the V-cut target water-stopping area. When the amount of water leakage is small, for example, the following method can be used. The target water-stopping area is V-cut, and the water-stopping material is applied by filling in the periphery of the water-stopping area. The water-stopping material is pressed firmly against the water-stopping area just before it starts to set, and is held down by hand or the like until it hardens. Additional water-stopping material is applied or a waterproofing material is applied on top, so that the surface of the water-stopping material is flush with the surface of the water-stopping object. When the amount of water leakage is large, for example, the following method can be used. The target water-stopping area is V-cut, and the periphery of the water-stopping area is filled in with the water-stopping material. A hose is inserted into the water-stopping area, and the area around the hose is filled in with the water-stopping material while allowing the water to escape. After the water-stopping material around the hose has completely hardened, remove the hose, and before the water-stopping material at the rear of the hose starts to solidify, apply the water-stopping material and hold it down with your hand until it hardens. Apply additional water-stopping material or top coat waterproofing material so that the surface of the water-stopping material is flush with the surface of the object to be waterproofed.
[0107] As a method for injecting the water-stopping material into the target area for water-stopping, a method of injecting the water-stopping material into the target area for water-stopping using an injection gun can be mentioned.
[0108] The present invention will be specifically described below with reference to examples and comparative examples. The present invention is not limited to the following examples. In the following examples, tests were performed in a room temperature (20°C ± 1°C) environment unless otherwise specified.
[0109] Example 1 Preparation of powder accelerator: 1.62 kg of sodium carbonate (average particle size 450 μm, ion-releasing compound) and 1.62 kg of ethylene-vinyl acetate copolymer (Tosoh Corporation's "EVA Ultrathene #636", base material) were melt-mixed in an extruder, extruded into strands, and pelletized. The pelletized product was freeze-pulverized and classified to obtain a powder quick-setting agent with an average particle size of 50 μm. In the obtained powder quick-setting agent, sodium carbonate, which is an ion-releasing compound, is present at least on the surface of the base material. In the obtained powder quick-setting agent, sodium carbonate, which is an ion-releasing compound, is present on the surface and inside of the powder quick-setting agent. In addition, in 100% by weight of the obtained powder quick-setting agent, the content of sodium carbonate, which is an ion-releasing compound, is 50% by weight, and the content of ethylene-vinyl acetate copolymer, which is the base material, is 50% by weight. In addition, as a result of observation with an electron microscope, the average particle size of sodium carbonate, which is an ion-releasing compound, in the obtained powder quick-setting agent was 5 μm.
[0110] Preparation of water-stopping materials and water-stopping materials: The water-stopping material and the water-stopping material were prepared as follows, according to the method compliant with JIS A1138 "How to make concrete in a laboratory". First, a premixed mortar ("M130" manufactured by Yoko Bussan Co., Ltd.) was prepared. This premixed mortar contained 27.80 kg of fine aggregate for 9.27 kg of cement. 37.07 kg of premixed mortar, 5.78 kg of ion-exchanged water (mixing water), and 324 g of powdered quick-setting agent were put into a 5 L bucket, and then mixed for 2 minutes using a mixer ("EARTH MAN KH-500A" manufactured by Takagi Co., Ltd.) to obtain a water-stopping material. In the water-stopping material, the water-cement ratio (W / C), which is the ratio (by weight) of the water (W) content to the cement (C) content, was 0.62.
[0111] The obtained water-sealing material was placed in a Summit can (Φ50 mm×100 mm, manufactured by Sumitomo Cement Co., Ltd.) and cured for one day in an environment of 23° C. and 50% humidity to harden the water-sealing material, thereby obtaining a water-sealing material.
[0112] Example 2 Preparation of powder accelerator: A powder quick-setting admixture having an average particle size of 50 μm was obtained in the same manner as in Example 1, except that sodium hydrogen carbonate (average particle size 450 μm) was used as the ion-releasing compound. In the obtained powder quick-setting admixture, sodium hydrogen carbonate, which is an ion-releasing compound, exists at least on the surface of the base material. In the obtained powder quick-setting admixture, sodium hydrogen carbonate, which is an ion-releasing compound, exists on the surface of the powder quick-setting admixture and inside the powder quick-setting admixture. In addition, in 100% by weight of the obtained powder quick-setting admixture, the content of sodium hydrogen carbonate, which is an ion-releasing compound, is 50% by weight, and the content of ethylene-vinyl acetate copolymer, which is a base material, is 50% by weight. In addition, as a result of observation with an electron microscope, the average particle size of sodium hydrogen carbonate, which is an ion-releasing compound, in the obtained powder quick-setting admixture was 4 μm.
[0113] Preparation of water-stopping materials and water-stopping materials: A water-sealing material and a water-sealing material were obtained in the same manner as in Example 1, except that the obtained powder quick-setting admixture was used.
[0114] Example 3 Preparation of powder accelerator: A powder quick-setting admixture having an average particle size of 50 μm was obtained in the same manner as in Example 1, except that calcium acetate (average particle size 75 μm) was used as the ion-releasing compound. In the obtained powder quick-setting admixture, calcium acetate, which is an ion-releasing compound, is present at least on the surface of the base material. In the obtained powder quick-setting admixture, calcium acetate, which is an ion-releasing compound, is present on the surface of the powder quick-setting admixture and inside the powder quick-setting admixture. In addition, in 100% by weight of the obtained powder quick-setting admixture, the content of calcium acetate, which is an ion-releasing compound, is 50% by weight, and the content of ethylene-vinyl acetate copolymer, which is a base material, is 50% by weight. In addition, as a result of observation with an electron microscope, the average particle size of calcium acetate, which is an ion-releasing compound, in the obtained powder quick-setting admixture was 2 μm.
[0115] Preparation of water-stopping materials and water-stopping materials: A water-sealing material and a water-sealing material were obtained in the same manner as in Example 1, except that the obtained powder quick-setting admixture was used.
[0116] Example 4 Preparation of powder accelerator: A powder quick-setting admixture having an average particle size of 50 μm was obtained in the same manner as in Example 1, except that polyethylene terephthalate ("RAMAPET N1" manufactured by Indorama Ventures) was used as the base material. In the obtained powder quick-setting admixture, sodium carbonate, which is an ion-releasing compound, is present at least on the surface of the base material. In the obtained powder quick-setting admixture, sodium carbonate, which is an ion-releasing compound, is present on the surface of the powder quick-setting admixture and inside the powder quick-setting admixture. In addition, in 100% by weight of the obtained powder quick-setting admixture, the content of sodium carbonate, which is an ion-releasing compound, is 50% by weight, and the content of polyethylene terephthalate, which is the base material, is 50% by weight. In addition, as a result of observation with an electron microscope, the average particle size of sodium carbonate, which is an ion-releasing compound, in the obtained powder quick-setting admixture was 5 μm.
[0117] Preparation of water-stopping materials and water-stopping materials: A water-sealing material and a water-sealing material were obtained in the same manner as in Example 1, except that the obtained powder quick-setting admixture was used.
[0118] Comparative Example 1 Preparation of water-stopping materials and water-stopping materials: A water-sealing material and a water-sealing material were obtained in the same manner as in Example 1, except that no powder quick-setting admixture was used.
[0119] Comparative Example 2 Preparation of water-stopping materials and water-stopping materials: Except for using an ethylene-vinyl acetate copolymer having an average particle size of 50 μm instead of the powder quick-setting admixture, a water-stopping material and a water-stopping material were obtained in the same manner as in Example 1. For convenience of the table, the composition of the ethylene-vinyl acetate copolymer is shown in the column of the powder quick-setting admixture in the following table.
[0120] Comparative Example 3 Preparation of powder accelerator: As the powder quick-setting admixture, sodium carbonate with an average particle size of 50 μm was prepared.
[0121] Preparation of water-stopping materials and water-stopping materials: A water-sealing material and a water-sealing material were obtained in the same manner as in Example 1, except that the prepared powder quick-setting admixture was used.
[0122] Comparative Example 4 Preparation of water-stopping materials and water-stopping materials: Except for using polyethylene terephthalate having an average particle size of 50 μm instead of the powder quick-setting admixture, a water-stopping material and a water-stopping material were obtained in the same manner as in Example 1. For convenience of the table, the composition of the polyethylene terephthalate is described in the column of the powder quick-setting admixture in the following table.
[0123] (evaluation) In the following evaluations, unless otherwise specified, tests were performed in a room temperature environment (20°C ± 1°C).
[0124] (1) Usable life of water-stopping material According to the method described in the above section "Preparation of water-stopping material and water-stopping material", each component was mixed and stirred for 2 minutes to obtain a water-stopping material (measurement sample). Immediately after the stirring was completed, 400 g of the obtained measurement sample was placed on the surface of a polyethylene sheet (Okura Kogyo Co., Ltd. "Poly Sheet", 40 cm long x 40 cm wide) attached to the surface of an iron plate. Next, while wearing nitrile rubber gloves, the upper surface of the measurement sample was touched at 1-minute intervals. The time from the end of the preparation of the measurement sample (the end of stirring) to the last time the water-stopping material was attached to the gloves was defined as the usable time of the water-stopping material.
[0125] (2) Compressive strength of water-stop material after 24 hours The compressive strength of the above water-stopping material at 24 hours of age was measured in accordance with JIS A1108:2018 "Test method for compressive strength of concrete."
[0126] (3) Short-term watertightness FIG. 2 is a diagram for explaining a method for evaluating short-term watertightness. First, mortar was hardened to prepare a mortar specimen 5 measuring 10 cm long x 10 cm wide x 10 cm high. A crack 51 was made in this mortar specimen 5 using Tensilon, and a 1 mm spacer was sandwiched between the cracks 51 and the specimen was attached (FIG. 2(a)). Next, a V-shaped cut of about 2 cm deep was made on one side of the mortar specimen 5 in line with the crack 51. Next, a pipe 6 with a diameter of 5 cm and a height of 20 cm was placed on the upper surface of the mortar specimen 5. Next, the cracks 51 present other than the V-cut portion and the portion where the pipe 6 was placed were sealed with butyl tape 7 (FIG. 2(b)). The prepared watertight material was placed on the V-cut portion, and then left to form a watertight material 10 (FIG. 2(c)). In addition, 20 minutes after the water-stopping material was placed, 196 cc of water (equivalent to a head difference of 10 cm) was added to the pipe 6. One minute after the water was added to the pipe 6, it was visually confirmed whether or not there was a leak. It was determined that there was a leak when both A and B below were met.
[0127] A: The head difference in the pipes has clearly decreased (decreased by more than 2 cm) B: Water is leaking from the joint between the water-stop material and the mortar specimen, or from the water-stop material itself.
[0128] [Criteria for determining short-term watertightness] ○: No leakage ×: Water leakage has occurred
[0129] (4) Long-term water-tightness (generation of poorly water-soluble salts) The water-stopping materials obtained in Examples 1, 2, and 4 and Comparative Examples 1 to 4 were immersed in a 1000 ppm calcium chloride solution for one month. The water-stopping material obtained in Example 3 was immersed in ion-exchanged water for one month. After immersion, the water-stopping materials were taken out and visually observed in detail to see whether particles had precipitated on the surface of the water-stopping materials. When the water-stopping materials on which particles had precipitated were observed using a scanning electron microscope, aggregates of particles with a dense crystal structure (calcite structure of calcium carbonate) were observed. The long-term water-stopping ability (generation of poorly water-soluble salts) was evaluated according to the following criteria.
[0130] [Criteria for determining long-term water-stopping properties (generation of poorly water-soluble salts)] ○○: Of the total surface area of the water-stopping material (100%), the surface area on which particles are deposited is 20% or more. ○: The surface area on which particles are precipitated is 10% or more and less than 20% of the total surface area of the water-stopping material (100%). ×: The surface area on which particles are precipitated is less than 10% of the total surface area of the water-stopping material (100%).
[0131] The configuration and results are shown in Table 1 below.
[0132] [Table 1]
[0133] Table 2 below shows examples of the preparation (examples of blending compositions) of the quick-setting admixture and water-stopping material of the present invention.
[0134] [Table 2] [Explanation of symbols]
[0135] 1...Accelerating agent (powdered accelerator) 2…Base material 31...Ion-releasing compound present on the surface of the accelerator 32...Ion-releasing compound present inside the accelerator
Claims
1. A powder quick-setting admixture, The composition includes a base material and an ion-releasing compound capable of releasing cations or anions, the ion-releasing compound is present on at least a surface of the base material; The powder quick-setting admixture, wherein the ion-releasing compound is capable of generating a poorly water-soluble salt.
2. The powder quick-setting admixture according to claim 1 , wherein the poorly water-soluble salt is calcium carbonate.
3. 3. The powder quick-setting admixture according to claim 1, wherein the ion-releasing compound is sodium bicarbonate, sodium carbonate, calcium formate, calcium acetate, calcium lactate, or calcium chloride.
4. The powder quick-setting admixture according to claim 1 or 2, wherein the base material is a resin.
5. The powder quick-setting admixture according to claim 1 or 2, wherein the base material is a thermoplastic resin.
6. 3. The powder quick-setting admixture according to claim 1, wherein the ion-releasing compound is present on a surface of the powder quick-setting admixture and inside the powder quick-setting admixture.
7. Cement milk or mortar; A water-stopping material comprising the powder quick-setting admixture according to claim 1 or 2.
8. The water-stopping material according to claim 7, which has a pot life of 1 minute or more and 30 minutes or less.
9. A water-stop material which is a cured product of the water-stop material according to claim 7.
10. The compressive strength at 24 hours is 0.1 N / mm 2 5.0N / mm or more 2 The water-stopping material according to claim 9, which is as follows:
11. A placement step of placing the water-stopping material according to claim 7 at a waterproofing target portion of a waterproofing target object; A method for manufacturing a structure, comprising: a curing step of curing the water-stopping material.
12. A waterproofing method, comprising: sealing a target portion of an object to be waterproofed by using the waterproofing material according to claim 7.
Citation Information
Patent Citations
Accelerating agent for cement, ultra rapid hardening power admixture for spray material and spray material
JP2017071536A
Cited By
Granules, cement-based admixture, method for producing granules, and method for producing cement-based admixture
WO2026181906A1