Method for producing terephthalic acid on industrial scale
An enzymatic process controls pH in a stirred reactor to depolymerize polyesters, addressing the inefficiencies of traditional methods and achieving high terephthalic acid concentrations for industrial-scale recycling.
Patent Information
- Application Number
- JP2024115464
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2018-11-06
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The production of terephthalic acid from plastic waste on an industrial scale is hindered by the complexity and cost of separating monomers, particularly terephthalic acid, from solid waste and undepolymerized polyester, due to the inefficiencies of traditional mechanical recycling processes.
An enzymatic process is developed to depolymerize polyesters containing terephthalic acid units, maintaining a high concentration of soluble terephthalic acid by controlling pH between 6.5 and 9 in a stirred reactor, allowing for efficient recovery and reuse of terephthalic acid in a solubilized form.
The method achieves high depolymerization rates of over 90% in 24 hours, producing terephthalic acid concentrations of more than 40 kg/t in the liquid phase, simplifying recovery and reducing production costs, and enabling industrial-scale recycling of plastics.
Smart Images

Figure 2024156716000001 
Figure 2024156716000002 
Figure 2024156716000003
Abstract
Description
[Technical field]
[0001] TECHNICAL FIELD OF THEINVENTION The present invention relates to a process for producing terephthalic acid by enzymatic means from the desired polyester on an industrial or semi-industrial scale.
[0002] Background technology Plastic products are durable, inexpensive materials that can be used to manufacture a wide variety of products for various applications (food packaging, clothing textiles, etc.). As a result, the production of plastics has increased dramatically in recent decades. Most are used for short-term applications, which leads to the accumulation of plastic waste and the need for its disposal. The various polymers that make up these plastics include polyethylene terephthalate (PET), aromatic polyesters made from terephthalic acid and ethylene glycol. They are used for many applications, e.g., food packaging (bottles, flasks, jars, trays, pouches), but also in the manufacture of textiles for clothing, decoration (carpets), household linen, etc.
[0003] To address the environmental and economic problems of waste accumulation, recycling or energy recovery technologies have been developed. Mechanical recycling processes are still the most commonly used today, but they have many drawbacks. Indeed, they require complex and expensive sorting, leading to the production of reduced quality recycled plastics (lower molecular weight, uncontrolled presence of additives) intended for lower value applications. Moreover, these recycled plastics do not compete with virgin plastics derived from petroleum.
[0004] In recent years, innovative methods for the enzymatic recycling of plastic products have been developed and are described in particular in patent applications WO 2014 / 079844, 2015 / 097104, 2015 / 173265 and 2017 / 198786. Unlike conventional mechanical recycling processes, these enzymatic processes allow the enzymatic depolymerization of the polymers contained in the plastics back to their main components (monomers). The monomers obtained can then be purified and used to repolymerize new polymers. In these enzymatic processes, the specificity of the enzymes not only makes it possible to avoid the costly sorting of plastics, but also makes it possible to propose an infinite recycling that results in regenerated polymers of the same quality as those derived from petroleum. In particular, these processes make it possible to produce terephthalic acid and ethylene glycol from PET.
[0005] One of the problems associated with the preparation of monomers obtained by depolymerization is the process of recovering said monomers.Indeed, it is difficult to separate monomers in solid form, such as terephthalic acid, from the remainder of the solid waste present in the reactor and in particular from the polyesters that have not yet been depolymerized.Such recovery processes are complex, expensive and poorly suited for use on an industrial scale.
[0006] By addressing these problems, the applicant has developed an enzymatic process optimized to enable the industrial-scale production of terephthalic acid, in particular from plastics and / or textiles containing polyesters, including PET.
[0007] Summary of the Invention The inventors have developed a process for producing terephthalic acid from at least one polyester containing terephthalic acid, which results in a high concentration production of terephthalic acid, thereby addressing the technical and economic constraints of industrial-scale production. More precisely, the inventors have developed a process for introducing a high concentration of polyester into a reactor while maintaining a depolymerization rate of said polyester compatible with industrial feasibility. In particular, the inventors have determined that by controlling the pH between 6.5 and 9 in a stirred reactor, it is possible to maintain a significant portion of the produced terephthalic acid in soluble form. A high concentration of soluble terephthalic acid is particularly advantageous, since it simplifies the recovery process of these monomers, thus lowering the production costs.
[0008] Moreover, the method developed by the inventors makes it possible to maintain a depolymerization rate inside the reactor that is compatible with implementation on an industrial scale. By way of example, the inventors have succeeded in depolymerizing more than 90% of a target polyester containing terephthalic acid in just 24 hours, resulting in a recovery of more than 90% of the terephthalic acid present in the target polyester. The method that is the object of the present invention can be carried out on any plastic waste containing a polyester with terephthalic acid. The plastic waste can be fed directly to the reactor without complex sorting or complex pretreatment. Advantageously, the method of the present invention can be carried out for the depolymerization and / or recycling of plastics. The method of the present invention can be carried out for the recycling of polyesters containing at least one terephthalic acid unit, mainly semi-aromatic polyesters selected in particular from polyethylene terephthalate (PET), polyethylene terephthalate glycol (PETG), polyethylene coisosorbide terephthalate (PEIT), polytrimethylene terephthalate (PTT), polybutylene adipate terephthalate (PBAT), polycyclohexylene dimethylene terephthalate (PCT) and polybutylene terephthalate (PBT).
[0009] The present invention therefore provides a method for producing terephthalic acid (TA) from at least one target polyester comprising at least one TA unit, comprising the steps of enzymatic depolymerization of the polyester, contacting said polyester in a stirred reactor with at least one enzyme capable of depolymerizing said polyester, and recovering the TA salt in solubilized form. It has as its object a process characterized in that the amount of polyester introduced into the reactor is greater than 10% by weight, based on the total weight of the initial reaction medium, the pH is controlled during the depolymerization step between 6.5 and 9, and the TA concentration in the liquid phase of the final reaction medium is greater than 40 kg / t.
[0010] Preferably, the step of recovering the solubilized TA salt comprises separating the liquid phase containing the TA salt from the remainder of the final reaction medium.
[0011] Preferably, the polyester of interest is selected from PTT, PBAT, PBT, PET, PETG, PEIT, PCT, more preferably, the polyester of interest is PET.
[0012] Advantageously, the polyester in question is introduced into the reactor in powder and / or granular form, in particular in powder and / or granular form having a particle size of less than 2 mm, preferably less than 1 mm.
[0013] Advantageously, the depolymerization step of the process of the invention lasts for at most 150 hours, more preferably at most 48 hours. Moreover, the process of the invention can be carried out in industrial size reactors, in particular reactors having useful volumes of several liters, tens of liters or hundreds of liters.
[0014] Preferably, the pH is controlled during the depolymerization step by adding to the reaction medium a basic solution concentrated to at least 10%±1%.
[0015] The present invention also relates to a method for recycling a target polyester, in particular PET, containing at least one TA unit, comprising the steps of enzymatically depolymerizing said polyester by contacting said target polyester with at least one enzyme capable of depolymerizing said polyester, said depolymerization step being carried out in a stirred reactor, the reactor containing an amount of polyester containing more than 10% by weight, based on the total weight of the initial reaction medium, and controlling the pH during the depolymerization step between 6.5 and 9, and recovering the terephthalate in a solubilized form.
[0016] The present invention also has as its object a method for recycling a target polyester comprising at least one TA unit, comprising the step of enzymatically depolymerizing said polyester by contacting said target polyester with at least one enzyme capable of depolymerizing said polyester, said depolymerization step being carried out in a reactor under stirring, the reactor containing the polyester in an amount comprised between 15% and 25% by weight, based on the total weight of the initial reaction medium, the pH being controlled during the depolymerization step between 7.5 and 8.5 by adding to the reaction medium a basic solution concentrated to at least 15%±1%, and the TA concentration in the liquid phase of the final reaction medium is greater than 100 kg / t.
[0017] Advantageously, the recovered TA salts can be reused in the form of TA, in particular for the production of new polyesters.
[0018] Another object of the present invention is the use of a reactor having a volume of more than 1 L, preferably more than 10 L, more than 100 L, more than 1000 L, for carrying out the process as defined above.
[0019] Detailed Description of the Invention definition In the context of the present invention, the expression "plastic material" refers to plastic products (e.g. sheets, trays, films, tubes, blocks, fibers, fabrics, etc.) and to plastic compositions used to manufacture plastic products. Preferably, the plastic material is composed of amorphous and / or semicrystalline polymers. In addition to the polymer, the plastic material may contain additional substances or additives, such as plasticizers, inorganic or organic fillers, dyes, etc. Thus, in the context of the present invention, plastic material refers to any plastic product and / or plastic composition comprising at least one polymer in semicrystalline and / or amorphous form, in particular at least one polyester.
[0020] Plastic products refer to manufactured plastic products such as rigid or flexible packaging (films, bottles, trays), agricultural films, bags, disposable articles, textiles, fabrics, non-wovens, floor coverings, plastic waste or textile waste, etc.
[0021] The term "polymer" refers to a compound whose structure consists of multiple repeating units (i.e., "monomers") linked by covalent chemical bonds. In the context of the present invention, the term "polymer" refers more specifically to such compounds used in the composition of plastic materials.
[0022] The term "polyester" refers to a polymer that contains an ester functional group in the backbone of its structure. An ester functional group is characterized by bonds between a carbon and three other atoms: a single bond to another carbon atom, a double bond to an oxygen, and a single bond to another oxygen atom. The oxygen that is attached to the carbon by a single bond is itself attached to another carbon by a single bond. Polyesters can be formed from only one type of monomer (i.e., homopolymers) or from at least two types of monomers (i.e., copolymers). Polyesters can be aromatic, aliphatic, or semi-aromatic. As an example, polyethylene terephthalate is a semi-aromatic copolymer composed of two monomers, terephthalic acid and ethylene glycol. In the context of the present invention, "polyesters of interest" refer to polyesters that contain at least one terephthalic acid unit as a monomer.
[0023] In the context of the present invention, the term "semicrystalline polymer" refers to a partially crystalline polymer in which crystalline and amorphous regions coexist. The crystallinity of a semicrystalline polymer can be estimated by various analytical methods and is generally comprised between 10% and 90%. A polymer with a crystallinity of less than 10% can be considered amorphous. In the present application, the crystallinity is measured by differential scanning calorimetry (DSC). X-ray diffraction can also be used to measure the crystallinity.
[0024] The term "depolymerization" in reference to a polymer or a plastic material containing a polymer refers to a process in which at least one polymer of the polymer or said plastic material is depolymerized into smaller molecules, e.g. monomers and / or oligomers.
[0025] As used herein, the terms "solubilized" or "in solubilized form" refer to a compound that is dissolved in a liquid, as opposed to an undissolved solid form.
[0026] The term "terephthalic acid" or "TA" refers to the terephthalic acid molecule alone, i.e., C8H6O4, which corresponds to terephthalic acid in its acid form. The terms "terephthalic acid salts", "terephthalate salts" or "TA salts" refer to compounds that include a terephthalic acid molecule associated with a cation, e.g., sodium, potassium, ammonium. In the context of the present invention, TA salts include disodium terephthalate, C8H4Na2O4, dipotassium terephthalate, C8H4K2O4, diammonium terephthalate, C8H4Na2O4, diammonium ... 12 N2O4, monosodium terephthalate C8H5NaO4, monopotassium terephthalate C8H5KO4 and / or monoammonium terephthalate C8H 10 It may contain NO4.
[0027] According to the invention, the concentration of terephthalic acid in the liquid phase of the final reaction medium corresponds to the amount of TA measured at the end of the depolymerization step, regardless of its form, i.e., solubilized or non-solubilized form of TA, including solubilized or salt form. The concentration of terephthalic acid can be determined by any means known to the person skilled in the art, in particular by HPLC.
[0028] In the context of the present invention, "content" refers to the amount of compound, e.g., the amount of polyester of interest or the amount of enzyme, fed to the reactor at the start of the polyester depolymerization process (time t=0). The content of polyester, in particular PET, refers to the amount of that polyester, regardless of other compounds that may be present in the plastic material. Thus, when polyester is contained in plastic waste, the content of said polyester is different from the content of plastic waste, since said plastic waste may contain other compounds in addition to said polyester.
[0029] "Reaction medium" means all materials present in the reactor during the depolymerization step, including in particular the liquid, the enzyme, the polyester of interest and / or the monomers resulting from the depolymerization of said polyester, i.e. the contents of the reactor. "Initial reaction medium" and "final reaction medium" mean the reaction medium at the beginning and end of the depolymerization step, respectively. In the context of the present invention, the total volume of the reactor is advantageously at least 10% greater than the volume of the final reaction medium.
[0030] "Liquid phase of the final reaction medium" means the reaction medium obtained at the end of the depolymerization step and free from solid and / or suspended particles. Said liquid phase comprises the liquid and all compounds dissolved in this liquid, including enzymes, monomers, salts, etc. This liquid phase can be obtained by separation from the solid phase of the reaction medium using conventional techniques known to the skilled person, for example filtration, centrifugation, etc. In the context of the present invention, the liquid phase is in particular free from residual polyester, i.e. not decomposed at the end of the depolymerization step.
[0031] Depolymerization Process The method for producing terephthalic acid according to the invention is based on the enzymatic depolymerization of at least one polyester of interest, which contains at least one terephthalic acid unit in its constituents, by contacting said polyester with at least one enzyme capable of depolymerizing said polyester. In particular, the inventors have developed a method for producing large amounts of terephthalic acid in an easily purifiable form in a relatively short reaction time. In fact, the inventors have unexpectedly discovered that it is possible to feed a large amount of the polyester of interest and at least one enzyme capable of depolymerizing it to a reactor, under stirring and maintaining a pH between 6.5 and 9, and to obtain particularly fast depolymerization rates leading to terephthalic acid concentrations of more than 40 kg / t in the liquid phase of the reaction medium in a time that is perfectly acceptable on an industrial and semi-industrial scale. The method of the invention also makes it possible to obtain terephthalic acid in a solubilized form, i.e. in the form of an easily purifiable TA salt. This makes the method of the invention particularly advantageous on an industrial scale.
[0032] Therefore, the process for producing terephthalic acid (TA) of the present invention comprises: - enzymatically depolymerizing the polyester of interest by contacting the polyester in an agitated reactor with at least one enzyme capable of depolymerizing the polyester; and recovering the TA salt in solubilized form. At the start of the depolymerization step, the reactor contains an amount of polyester of more than 10 wt. % based on the total weight of the initial reaction medium, the pH is controlled to 6.5-9 during the depolymerization step, and at the end of the depolymerization step, the TA concentration in the reactor is more than 40 kg / t in the liquid phase of the final reaction medium.
[0033] Advantageously, the type of terephthalate salt obtained is related to the base used to control the pH. Preferably, the terephthalate salt produced during the depolymerization step is in the form of sodium terephthalate, potassium terephthalate and / or ammonium terephthalate.
[0034] According to the invention, with the pH controlled at or above 6.5, at the end of the depolymerization step, the TA salts are recovered in solubilized form in the liquid phase of the reaction medium.
[0035] The process of the present invention can be carried out in reactors having a volume of more than 500 milliliters (mL), more than 1 liter (L), preferably more than 2 L, more than 5 L, more than 10 L. In certain embodiments, the process of the present invention can be carried out on an industrial and semi-industrial scale. Thus, reactors having a volume of more than 100 L, more than 150 L, more than 1000 L, more than 10000 L, more than 100000 L, more than 400000 L can be used. Preferably, the process is carried out in a reactor having a volume of more than 1000 L.
[0036] Reactor contents The initial reaction medium in the reactor contains at least the polyester of interest, optionally contained in a plastic material, in particular a plastic product or plastic waste, an enzyme for degrading said polyester, and a liquid. As the depolymerization process progresses, the reaction medium becomes enriched in monomers, in particular TA salts, and less of the polyester of interest.
[0037] Preferably, the liquid in the reactor comprises an aqueous solvent, preferably water. In a preferred case, the liquid in the reactor does not comprise a non-aqueous solvent, in particular does not comprise an organic solvent. In an embodiment, the liquid in the reactor comprises only water.
[0038] According to the present invention, the polyester of interest comprises at least one terephthalic acid unit as a monomer. Advantageously, the polyester of interest is selected from polytrimethylene terephthalate (PTT), polybutylene adipate terephthalate (PBAT), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), poly(ethylene coisosorbide terephthalate) PEIT, polycyclohexylene dimethylene terephthalate (PCT) and / or their copolymers. Preferably, the polyester of interest is PET. In a particular case, the polyester of interest is selected from modified polyesters, preferably the polyester of interest is modified PET, for example PET glycol (PETG).
[0039] Advantageously, the content of the polyester of interest in the reactor is 11% by weight or more, preferably 15% by weight or more, preferably 20% by weight or more, based on the total weight of the initial reaction medium. In particular, the content of the polyester of interest in the reactor is less than 60% by weight, preferably less than 50% by weight, based on the total weight of the initial reaction medium. In another particular case, the content of the polyester in the reactor is comprised between 15% by weight and 25% by weight, preferably between 20% ± 2%, based on the total weight of the initial reaction medium. In another particular case, the content of the polyester in the reactor is comprised between 11% by weight and 20% by weight, preferably between 15% ± 2%, based on the total weight of the initial reaction medium. In an embodiment, the content of the polyester of interest in the reactor is comprised between 11% by weight and 60% by weight, preferably between 15% to 50%, more preferably between 15% to 40%, 15% to 30%, 15% to 25%, 20% to 30%, 20% to 25%, based on the total weight of the initial reaction medium. When multiple polyesters containing at least one terephthalic acid unit are used in the reactor, the amount of polyester used refers to the cumulative amount of each polyester.
[0040] According to the present invention, the polyester of interest is an amorphous and / or semi-crystalline polyester. Preferably, the polyester of interest has a crystallinity of less than 30%, preferably less than 25%, more preferably less than 20%. In particular, the polyester of interest has a crystallinity of less than 30%±10%, preferably less than 25%±10%, more preferably less than 20%±10%. In another preferred case, the polyester of interest is an amorphous polyester. According to the present invention, it is possible to carry out an amorphization step of the polyester of interest before the depolymerization step by any means known to the skilled person. Such an amorphization step is described in particular in WO 2017 / 198786. In a particular embodiment, the polyester of interest or the plastic material containing the polyester of interest contained in the reactor is in the form of granules or microgranules with a size of less than 5 mm, preferably with a particle size of less than 3 mm, more preferably with a particle size of less than 2 mm. According to the invention, the polyester depolymerization step can be preceded by a pretreatment step of the target polyester, in particular a step of pulverizing the target polyester or the plastic material containing the target polyester. In a preferred embodiment, the target polyester or the plastic material containing the target polyester is brought into powder form by any suitable means known to the person skilled in the art. In this particular case, the target polyester or the plastic material containing the target polyester is advantageously pulverized so as to be converted into powder form.
[0041] In a particular embodiment, the process comprises a step of amorphizing the target polyester, followed by a step of grinding and / or pulverizing the target polyester or a plastic material containing the target polyester, prior to a polyester depolymerization step.
[0042] In a particular embodiment, the target polyester or the plastic material containing the target polyester contained in the reactor is in the form of a powder and / or granules having an average particle size (d50) of less than 2 mm, preferably less than 1 mm. In another embodiment, the target polyester or the plastic material containing the target polyester contained in the reactor is in the form of a powder having an average particle size (d50) of less than 500 μm.
[0043] Preferably, the target polyester is contained in the reactor in the form of a powder and / or granules having a crystallinity of less than 25%±10% and a size of less than 2 mm, preferably less than 1 mm. According to the invention, it is possible to directly charge the target polyester or a plastic material at least containing the target polyester into the reactor.
[0044] According to the invention, the plastic material contained in the reactor can contain a mixture of several polymers, in particular several polyesters. In a particular embodiment, the depolymerization method of the invention is carried out with a plastic material that contains at least PET. In a preferred embodiment, PET represents at least 80% by weight, preferably at least 85%, 90%, 95%, based on the total weight of said plastic material. In a particular embodiment, the plastic material comprises a mixture of PET and polylactic acid (PLA), a mixture of PET and polyethylene (PE), a mixture of PET and polytrimethylene terephthalate (PTT), a mixture of PET and polyamide (PA) or a mixture of PET and cotton. Advantageously, the plastic material used in the reactor is plastic waste or textile waste. These waste materials can come from collection channels intended for recycling, but can also be waste materials from production or recycling channels, which may therefore contain compounds other than waste plastics. This means that the polyester of interest may be contained in the reactor in combination with other elements present in these streams (for example paper, cardboard, aluminum, glue, etc.). In a particular embodiment, the reactor is filled with a plurality of plastic materials containing at least the polyester of interest, preferably at least PET, more preferably at least 80% PET. In another particular embodiment, the plastic materials are selected from one or more fiber and / or textile wastes, with PET representing at least 60% by weight, preferably at least 65%, 70%, 75%, 80%, 85%, 90%, 95%, based on the total weight of said plastic materials.
[0045] Advantageously, the enzyme that degrades the polyester of interest is selected from cutinases, lipases and esterases that degrade said polyester. In particular, said enzyme is selected from esterases that degrade said polyester of interest. In a particular embodiment, said polyester is PET and the enzyme is a PET-degrading cutinase. In particular, the enzyme is preferably a cutinase from Thermobifida cellulosityca, Thermobifida halotolerans, Thermobifida fusca, Thermobifida alba, Bacillus subtilis, Fusarium solani pisi, Humicola insolens (e.g., those having the accession number A0A075B5G4 in the UniProt database), Sirococcus conigenus, Pseudomonas mendocina and Thielavia terrestris or a variant thereof. In another case, the cutinase is selected from a metagenomic library-derived cutinase, such as the LC-cutinase described in Sulaiman et al., 2012, or a variant thereof. In another case, the enzyme is preferably a lipase from Ideonella sakaiensis. Alternatively, the enzyme is selected from commercially available enzymes, such as Novozym 51032 or a variant thereof. Of course, it is possible to load the reactor with multiple enzymes, in particular at least two of the enzymes mentioned above.
[0046] In certain cases, the one or more enzymes are selected from enzymes having an amino acid sequence having at least 75% identity with SEQ ID NO:1 and / or SEQ ID NO:2 and / or SEQ ID NO:3 and / or SEQ ID NO:4 and / or SEQ ID NO:5 and having activity to depolymerize a polyester comprising at least one terephthalic acid unit. In certain cases, the enzymes are selected from enzymes having an amino acid sequence having at least 75% identity with SEQ ID NO:1 and having PET depolymerization activity.
[0047] In a particular embodiment, the enzyme is capable of depolymerizing a polymer into an oligomer, in which case the enzyme is advantageously associated with an enzyme capable of depolymerizing said oligomer into a monomer, thus in a particular example the two enzymes are selected from enzymes having an amino acid sequence having at least 75% identity with SEQ ID NO:4 and / or SEQ ID NO:5.
[0048] The inventors have determined that the method of the invention is particularly suitable in the specific case where the selected enzyme has an amino acid sequence with at least 90% identity to SEQ ID NO: 1 and the polyester of interest is preferably selected from PET and / or PBAT. This is in particular the case for enzymes having the amino acid sequence of SEQ ID NO: 1 or SEQ ID NO: 2. Unlike other enzymes known to depolymerize polyesters, these enzymes experience limited inhibition of their activity by the monomers produced under the conditions of the method of the invention.
[0049] The object of the present invention is therefore to propose a method for producing terephthalic acid as defined above, characterized in that the enzyme capable of depolymerizing polyesters is chosen from enzymes having an amino acid sequence with at least 90% identity to SEQ ID NO:1 and an activity to depolymerize polyesters comprising at least one terephthalic acid unit, in particular a PET depolymerization activity.
[0050] Preferably, the method for producing terephthalic acid of the present invention is carried out using PET and at least one enzyme capable of depolymerizing said PET selected from cutinases, as described above.
[0051] According to the invention, the amount of enzyme degrading the polyester of interest contained in the reactor is advantageously sufficient to allow total or quasi-total depolymerization of said polyester (i.e. up to at least 80% by weight, based on the weight of said polyester) in a reaction time compatible with implementation on an industrial scale. In an embodiment, the weight ratio of the amount of enzyme contained to the amount of polyester contained is comprised between 0.01:1000 and 3:1000. Preferably, the ratio of the amount of enzyme contained to the amount of polyester contained is comprised between 0.5:1000 and 2.5:1000, more preferably between 1:1000 and 2:1000. In a particular case, the amount of enzyme contained is equal to or greater than the amount of enzyme required to reach the saturation enzyme concentration, i.e. the concentration above which the reaction rate is no longer improved by the addition of the enzyme. In a particular case, the enzyme can be contained in the form of a composition comprising, in addition to the enzyme excipient, a buffer commonly used in biochemistry, a preservative and / or a stabilizer, which can be selected. The amount of enzyme then advantageously refers to the amount of enzyme without any excipients.
[0052] According to the invention, the contents of the reactor are maintained under stirring during the depolymerization step. The stirring speed is controlled by the skilled person to be sufficient to allow suspension of the plastic / polyester material contained in the reactor, temperature uniformity and accuracy of pH control. In particular, the stirring is maintained at a speed comprised between 50 and 500 rpm, for example 80 rpm, 100 rpm, 150 rpm, 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm, 450 rpm, 500 rpm. In a particular embodiment, for reactors with a volume of more than 1000 L, the stirring is equal to or greater than 300 rpm. In a particular embodiment, for reactors with a volume of more than 1000 L, the stirring is equal to or greater than 100 rpm.
[0053] The depolymerization of the polyester of interest produces acidic monomers that may cause a decrease in the pH of the reactor contents. To neutralize the acid produced and control the pH, the addition of a base can be used. In the present case, the pH can be controlled in particular by the addition of any base known to the person skilled in the art. In particular, the pH is controlled by the addition of a base selected from sodium hydroxide (NaOH), potassium hydroxide (KOH) and / or ammonia (NH4OH). In the case of pH control by the addition of a base, the TA produced will associate with the base used to form a TA salt, the solubility of which will be improved relative to the TA. Advantageously, the pH is controlled during the depolymerization step by adding to the reaction medium a basic solution concentrated to at least 10% by weight ±1% by weight of base, based on the total weight of the basic solution (essentially including the base and water). Preferably, the basic solution is concentrated to at least 15% ±1%, up to 50% ±1%, more preferably at least 20% ±1%. In certain cases, the basic solution is concentrated to 20% to 50% ± 1%, more preferably to 20% to 30% ± 1%, even more preferably to 20% to 25% ± 1%. Preferably, the base is selected from sodium hydroxide (NaOH) and potassium hydroxide (KOH) and the basic solution is concentrated to at least 15% and up to 50%.
[0054] For this purpose, the pH is controlled to be maintained at 6.5-9, so that the terephthalic acid produced is mainly in the form of solubilized TA salt and / or at the optimum pH for the enzyme. In a particular embodiment, the pH is controlled to 6.5-8.5, preferably 7-8, during the depolymerization step. In another particular case, the pH is controlled to 7.5-8.5. Preferably, the pH is controlled to 8±0.2.
[0055] Advantageously, the temperature in the reactor, and therefore in the reaction medium, is controlled during the depolymerization step between 35° C. and 90° C., preferably between 45° C. and 80° C. In a preferred embodiment of the invention, the temperature is controlled between 55° C. and 80° C., more preferably between 60° C. and 80° C. In a particular embodiment, the temperature is controlled between 60° C. and 66° C.
[0056] In certain cases, the polyester of interest has a glass transition temperature (Tg) above 30°C, and the temperature in the reactor is controlled to a temperature below the Tg of the polyester of interest. Alternatively or additionally, the temperature is controlled to the optimum temperature of the enzyme used. In certain embodiments, the polyester of interest is PET, which has a Tg of about 70°C ± 5°C, and the temperature in the reactor is maintained at 60°C ± 5°C.
[0057] According to the invention, the depolymerization step is carried out for a reaction time of up to 150 hours. The reaction time depends, inter alia, on the polyester / depolymerase pair of interest and on the desired depolymerization rate of the polyester. The skilled person will know how to adapt the reaction time of the depolymerization step as a function of the above mentioned criteria. Advantageously, the depolymerization step lasts for 1 hour to 120 hours, 1 hour to 100 hours, 1 hour to 72 hours, 1 hour to 48 hours, 1 hour to 36 hours, 1 hour to 24 hours, 1 hour to 12 hours, 1 hour to 10 hours, 1 hour to 6 hours. In a preferred embodiment, the duration of the depolymerization step is not more than 24 hours.
[0058] In a preferred embodiment, the reaction time achieves at least 80%, preferably at least 85%, 90%, 95% depolymerization of the desired polyester. Preferably, depolymerization is carried out down to monomer, i.e., 80% depolymerization results in the production of 80% of the monomer (and no or almost no oligomers).
[0059] In a particular embodiment, a method for producing TA is carried out from a plastic material comprising PET and an enzyme whose amino acid sequence comprises at least SEQ ID NO: 1, said method allows for at least 80% depolymerization of PET in a time period of 72 hours or less, preferably for at least 90% depolymerization of PET in a time period of 72 hours or less. In another preferred embodiment, said method allows for at least 80% depolymerization of PET in a time period of less than 48 hours.
[0060] According to the invention, the depolymerization step can be carried out in any reactor usually used in the chemical industry or in biological production, for example a fermenter. Generally, according to the invention, the depolymerization step can be carried out in any tank or reactor in which the temperature and pH can be controlled and which can be equipped with stirring means for homogenizing the medium.
[0061] Terephthalic acid production The process of the present invention makes it possible to produce highly concentrated terephthalic acid with reaction times that are perfectly compatible with industrial constraints.
[0062] In particular, the method of the present invention makes it possible to obtain, at the end of the depolymerization step, a terephthalic acid concentration of at least 40 kg / t, based on the total weight of the liquid phase of the final reaction medium. Advantageously, the depolymerization step is considered to be complete when the depolymerization rate of the desired polyester reaches at least 80%, preferably at least 90%. In a particular embodiment, the skilled person can stop the depolymerization step when the achieved yield meets the industrial constraints, i.e. when the depolymerization rate of the desired polyester reaches 80%±10%, preferably 90%±5%. Thus, in the context of the present invention, the end of the depolymerization step corresponds to the moment when the depolymerization of the polyester stops and / or the moment when the depolymerization rate of the desired polyester reaches at least 80%, preferably at least 90%, and / or the moment when the step of recovering the TA salt begins.
[0063] Preferably, the concentration of terephthalic acid obtained from the target polyester after the depolymerization step is more than 50 kg / t, more than 60 kg / t, more than 70 kg / t, more than 80 kg / t, more than 90 kg / t, more than 100 kg / t, more than 110 kg / t, more than 120 kg / t based on the total weight of the liquid phase of the final reaction medium. In a preferred case, the concentration of terephthalic acid obtained from the target polyester after the depolymerization step is comprised between 100 kg / t and 115 kg / t ± 10%.
[0064] In certain cases, the concentration of total terephthalic acid (soluble and insoluble) obtained from the target polyester at the end of the depolymerization step is greater than 50 kg / t, greater than 60 kg / t, greater than 70 kg / t, greater than 80 kg / t, greater than 90 kg / t, greater than 100 kg / t, greater than 110 kg / t, greater than 120 kg / t, greater than 130 kg / t, greater than 140 kg / t, greater than 150 kg / t, based on the total weight of the final reaction medium (liquid and solid phase).
[0065] In other particular cases, the concentration of total terephthalic acid (soluble and insoluble) obtained from the target polyester at the end of the depolymerization step is greater than 50 kg / t, greater than 60 kg / t, greater than 70 kg / t, greater than 80 kg / t, greater than 90 kg / t, greater than 100 kg / t, greater than 110 kg / t, greater than 120 kg / t, greater than 130 kg / t, greater than 140 kg / t, greater than 150 kg / t, based on the total weight of the liquid phase + insoluble TA of the final reaction medium.
[0066] Advantageously, according to the invention, at least 80% by weight of the TA salt produced during the depolymerization step is in solubilized form, preferably at least 85%, 90%, 95%.
[0067] In a particular case, the amount of the desired polyester contained in the reactor is 15% by weight or more, based on the total weight of the initial reaction medium, and during the depolymerization step, the pH is controlled at 7-8 and the temperature is controlled at 60° C.±5° C. The TA concentration in the liquid phase of the final reaction medium after 24 hours is advantageously higher than 54 kg / t. In another particular case, the amount of the desired polyester contained in the reactor is 15% by weight or more, based on the total weight of the initial reaction medium, and during the depolymerization step, the pH is controlled at 7.5-8.5 and the temperature is controlled at 60° C.±5° C., and the TA concentration in the liquid phase of the final reaction medium after 24 hours is advantageously higher than 77 kg / t and after 48 hours is advantageously higher than 84 kg / t.
[0068] In another particular case, the amount of the polyester of interest contained in the reactor is 20% by weight or more, based on the total weight of the initial reaction medium, and during the depolymerization step, the pH is controlled at 7-8 and the temperature is controlled at 60° C.±5° C. The TA concentration in the liquid phase of the final reaction medium is advantageously greater than 90 kg / t after 24 hours. In another particular case, the amount of the polyester of interest contained in the reactor is 20% by weight or more, based on the total weight of the initial reaction medium, and during the depolymerization step, the pH is controlled at 7.5-8.5 and the temperature is controlled at 60° C.±5° C. The TA concentration in the liquid phase of the final reaction medium is advantageously greater than 95 kg / t after 24 hours, advantageously greater than 100 kg / t after 48 hours.
[0069] In another particular case, the amount of polyester of interest contained in the reactor is 20% by weight or more, based on the total weight of the initial reaction medium, and during the depolymerization step, the pH is controlled at 7-8 and the temperature is controlled at 50° C.-60° C. The TA concentration in the liquid phase of the corresponding final reaction medium after 48 hours is advantageously greater than 90 kg / t. In a preferred case, the temperature is controlled at 60° C. and the TA concentration in the liquid phase of the final reaction medium after 48 hours is greater than 100 kg / t.
[0070] In another particular case, the amount of the polyester of interest used in the reactor is 20% by weight or more, based on the total weight of the initial reaction medium, the pH is controlled at 7-8 during the depolymerization step, the temperature is controlled at 60° C., the reactor used has a volume of more than 150 L, and the TA concentration in the liquid phase of the final reaction medium after 48 hours is more than 75 kg / t.
[0071] In another particular case, the amount of the polyester of interest used in the reactor is 25% by weight or more, based on the total weight of the initial reaction medium, the pH is controlled at 7-8 during the depolymerization step, the temperature is controlled at 60° C., the reactor used has a volume of more than 1000 L, and the TA concentration in the liquid phase of the final reaction medium after 48 hours is more than 120 kg / t.
[0072] In another particular case, the method for producing terephthalic acid (TA) from at least one PET of the present invention comprises a PET depolymerization step lasting less than 48 hours, in which a plastic material containing PET is contacted with at least one cutinase capable of depolymerizing said PET in a stirred reactor, the reactor containing at the start of the depolymerization step an amount of PET contained in the reactor of 20% by weight or more, based on the total weight of the initial reaction medium, during the depolymerization step, the pH is controlled between 7 and 8.5, the temperature is controlled between 60°C and 80°C, and the TA concentration in the reactor at the end of the depolymerization step is more than 100 kg / t in the liquid phase of the final reaction medium.
[0073] In another particular case, the method for producing terephthalic acid (TA) from at least one plastic material containing PET of the present invention comprises a PET depolymerization step lasting less than 48 hours, in which the plastic material containing PET is contacted with at least one cutinase capable of depolymerizing said PET in a stirred reactor, the reactor containing at the start of the depolymerization step an amount of PET comprised between 15% and 25% by weight, based on the total weight of the initial reaction medium, during the depolymerization step the pH is controlled between 7.5 and 8.5 and the temperature is controlled between 60°C and 80°C, and at the end of the depolymerization step the TA concentration in the liquid phase of the final reaction medium in the reactor is greater than 100 kg / t.
[0074] In another particular case, the amount of the target polyester contained in the reactor is 5% to 25% by weight based on the total weight of the initial reaction medium, the basic solution used is concentrated to 15% ± 1%, and the TA concentration in the liquid phase of the final reaction medium after 48 hours is more than 80 kg / t, preferably more than 100 kg / t. Preferably, the amount of the target polyester contained in the reactor is more than 20% by weight ± 2% based on the total weight of the initial reaction medium, and the TA concentration in the liquid phase of the final reaction medium after 48 hours is more than 110 kg / t. Preferably, the pH is controlled at 7.5 to 8.5.
[0075] In another particular case, the amount of the polyester of interest contained in the reactor is comprised between 15% and 25% by weight, based on the total weight of the initial reaction medium, the basic solution used is concentrated to 20%±1%, and the TA concentration in the liquid phase of the final reaction medium after 48 hours is greater than 85 kg / t, preferably greater than 110 kg / t. Preferably, the amount of the polyester of interest contained in the reactor is greater than 20%±2%, and the TA concentration in the liquid phase of the final reaction medium after 48 hours is greater than 110 kg / t. Advantageously, the pH is controlled between 7.5 and 8.5.
[0076] In another particular case, the amount of polyester of interest contained in the reactor is comprised between 15% and 25% by weight, based on the total weight of the initial reaction medium, the basic solution used is concentrated to 25% ± 1%, and the TA concentration in the liquid phase of the final reaction medium after 48 hours is greater than 90 kg / t, preferably greater than 110 kg / t. Preferably, the amount of polyester of interest contained in the reactor is greater than 20% ± 2%, and the TA concentration in the liquid phase of the final reaction medium after 48 hours is greater than 110 kg / t. Advantageously, the pH is controlled between 7.5 and 8.5. In another particular case, the plastic material is selected from fibers and / or textile waste and / or textiles, the amount of polyester of interest contained in the reactor is comprised between 15% and 25% by weight, based on the total weight of the initial reaction medium, the basic solution used is concentrated to 20% ± 1%, and the TA concentration in the liquid phase of the final reaction medium after 48 hours is greater than 80 kg / t, preferably greater than 90 kg / t. Advantageously, the pH is controlled at 7.5 to 8.5.
[0077] According to the invention, the solubilized terephthalate salts (and / or terephthalic acid) in the liquid phase of the final reaction medium can be easily recovered from the contents of the reactor. In a particular embodiment, the step of recovering the solubilized TA salts comprises in particular separating the liquid phase containing the TA salts from the remainder of the reaction medium. In a particular case, this step of separating the solubilized terephthalate salts in the liquid phase is carried out by filtration of the reaction medium, which allows the recovery in solution of the terephthalate salts in solubilized form. The filtration cut-off can be adapted by the skilled person. The separation step can also be carried out by centrifugation or any other technique known to the skilled person.
[0078] The separated residue ("residue", i.e. the solid phase comprising in particular the residual non-degraded polyester and / or other polymers contained in the plastic material and / or the non-solubilized TA and TA salts) can be recycled to the reactor to undergo a new depolymerization step. It can also be washed with water to allow dissolution of the non-solubilized TA salts in the liquid phase and thus their recovery in solubilized form in the wash water.
[0079] Advantageously, the recovered TA salts can be reused in the form of TA, in particular for the production of new polyesters. According to the invention, the process comprises an additional step of TA recovery by precipitation of the TA contained in said salts.
[0080] In certain embodiments, this precipitation of the TA is achieved by acidification of the medium. For example, the filtrate (i.e., the liquid phase of the final reaction medium) containing the solubilized terephthalate salts can be subjected to some or all of the following steps (this sequence of steps is also suitable for the wash water mentioned above): 1. Purification of the filtrate (and / or wash water) by subjecting the solution to one or more steps selected from ultrafiltration, decolorization on carbon, passage on an ion exchanger, and chromatography; and / or 2. Precipitation of the terephthalic acid contained in the filtrate, wash water or purified solution by acidifying the solution with a mineral acid (which may be chosen, for example, from the following acids: sulfuric acid, hydrochloric acid, phosphoric acid or nitric acid) or with an organic acid (acetic acid type), either alone or in mixture. The solution can also be acidified with a CO2 overpressure. This step also induces the solubilization of the salts formed, at the same time as the precipitation of the TA; and / or 3. filtering the solution containing the precipitated terephthalic acid to recover the terephthalic acid in solid form; and / or 4. Wash the terephthalic acid with purified water (preferably multiple successive washes) and dry to obtain purified TA ("CTA").
[0081] The resulting CTA can then be crystallized and optionally further purified by any technique known to one of skill in the art to obtain purified and crystallized TA ("PTA").
[0082] The CTA and / or PTA obtained by the process of the present invention can be reused, either alone or in a mixture, in particular they can be repolymerized, either alone or in a mixture, for the synthesis of a polyester containing at least one terephthalic acid unit, which may be the same or different from the target polyester contained in the reactor.
[0083] The salts and other monomers obtained in the filtrate from step 3 can be extracted and purified by techniques known to those skilled in the art in order to reuse and / or recover them.
[0084] In another embodiment, the filtrate (i.e. the liquid phase of the final reaction medium) containing the solubilized terephthalate salt is subjected to a concentration step. The concentration step can be carried out by any method (e.g. evaporation) that allows the removal of the water contained in the solution, thus resulting in the precipitation of the terephthalate salt in solid form. The TA salt in solid form is recovered by filtration and then returned to the solution, which is then acidified with an acid (mineral or organic) to precipitate the terephthalic acid. This concentration step can be carried out at any time during the purification process and will be followed by a step of acidification of the medium. The above mentioned step 4 can then be carried out to obtain the CTA.
[0085] According to the present invention, it is possible to recover at least one other monomer by depolymerization of the target polyester. For this reason, the method of the present invention includes an additional step of recovering at least one other monomer constituting the target polyester. In an embodiment, the target polyester is PET, and ethylene glycol monomer is added to terephthalic acid and recovered at the end of the depolymerization step. In another embodiment, the target polyester is PTT, and propanediol (or propylene glycol) monomer is added to terephthalic acid and recovered by the depolymerization step. In another embodiment, the target polyester is PBT, and butanediol monomer is added to terephthalic acid and recovered by the depolymerization step. In another embodiment, the target polyester is PBAT, and butanediol and / or adipic acid monomer is added to terephthalic acid and recovered by the depolymerization step. In another embodiment, the target polyester is PCT, and cyclohexanedimethanol monomer is added to terephthalic acid and recovered by the depolymerization step. In another embodiment, the polyester of interest is PEIT, and ethylene glycol and / or isosorbide monomers are added to terephthalic acid and recovered through a depolymerization process.
[0086] According to the invention, in addition to terephthalic acid, it is also possible to recover oligomers, i.e. molecules containing 2 to 20 monomers including at least one terephthalic acid unit. In a particular case, the polyester of interest is PET and oligomers, such as methyl-2-hydroxyethyl terephthalate (MHET), bis(2-hydroxyethyl) terephthalate (BHET) and dimethyl terephthalate (DMT), are added to the terephthalic acid and recovered at the end of the depolymerization step.
[0087] The invention also relates to the use of a reactor having a volume of more than 1 L for carrying out a process for the production of terephthalic acid (TA), comprising the steps of depolymerizing the polyester of interest, carried out in said reactor, by contacting said polyester with at least one enzyme capable of depolymerizing said polyester, and recovering the TA salts in solubilized form.
[0088] Preferably, it is an object of the present invention to use a reactor having a volume of more than 2 L, more than 5 L, more than 10 L, more than 100 L, more than 1000 L, more than 10000 L, more than 100000 L, more than 400000 L for carrying out the above-mentioned process for producing terephthalic acid (TA).
[0089] The invention also has as its object a reactor containing at least one target polyester comprising at least one TA unit and at least one enzyme capable of depolymerizing said target polyester, the reactor having a volume of at least 1000 liters, in which at least one step of enzymatic depolymerization of said target polyester is carried out, the amount of polyester contained in the reactor being greater than 10% by weight, based on the total weight of the initial reaction medium, and the TA concentration in the liquid phase of the final reaction medium being greater than 40 kg / t. Advantageously, the amount of polyester contained in the reactor is comprised between 15% and 25% by weight, based on the total weight of the initial reaction medium, the TA concentration in the liquid phase of the final reaction medium being greater than 100 kg / t, and the pH is controlled between 7.5 and 8.5 during the depolymerization step by adding a basic solution concentrated to 15% to 50% by weight, preferably to 15% to 25%, based on the total weight of the basic solution.
[0090] According to the invention, the process is carried out discontinuously in the form of a batch process. Thus, in general, the process comprises a depolymerization step carried out for a given time from a given volume of initial reaction medium, followed by a step of recovering the TA salts produced. At the end of the depolymerization step, the reactor can be discharged so as to recover the entire reaction medium, which can then be subjected to the various steps described above so as to separate the solubilized terephthalate salts from the remainder of the reaction medium, purify them and recover the TA.
[0091] All the features of the process for producing terephthalic acid according to the present invention described above can also be applied to a process for producing a monomer similar to terephthalic acid, in particular a process for producing 2,5-furandicarboxylic acid (FDCA) from polyethylene furanoate (PEF).
[0092] Working Example Example 1: Production of terephthalic acid in a reactor containing an amount of PET greater than 10% by weight based on the total weight of the initial reaction medium For this experimental design, terephthalic acid production was carried out in flat-bottom stirred reactors (MiniBioreactors, Global Process Concept) with a total volume of 500 mL. Each reactor was equipped with a temperature probe and a pH probe (Hamilton, EasyFerm HB BioArc 120). The control of these two parameters at the set point was ensured by an internal PID controller in the C-bio software (Global Process Concept). Agitation of the reaction medium was provided by a 3 cm diameter marine paddle attached to a central shaft rotating at 300, 400 or 450 rpm. Several basic solutions were used to control the pH: 6 M NaOH (i.e. concentrated to 19.4%) or 6 M NH4OH (concentrated to 17.4%) or 6 M KOH (concentrated to 25%).
[0093] For experiments A-C, terephthalic acid (TA) production was carried out from colorless bottle preforms composed of 100% amorphous PET, which was cryogenically ground (D50=850 μm) to a fine powder.
[0094] For experiments D-K, terephthalic acid production was carried out using colored washed plastic flakes from a PET waste recycling stream, kindly donated. These plastic materials, consisting of 98% m / m PET, were subjected to an extrusion process followed by rapid cooling to amorphize the PET contained in the waste. The extruder used for amorphization was a Leistritz ZSE 18 MAXX twin screw extruder. The heating zone temperatures were set at 260 °C for the first four zones and 250 °C for the following six zones, and the screw rotation speed was set at 200 rpm. The rods that reached the extruder head were then immediately immersed in a water bath at 10 °C. The crystallinity of the PET after this amorphization process was evaluated at about 19% (by DSC). The obtained rods were granulated and then reduced to a fine powder using a micronizer (1 mm grid). The powder was then sieved through a 500 μm sieve to collect only the powders smaller than this size.
[0095] The enzyme used was LC-cutinase (SEQ ID NO: 1, corresponding to amino acids 36-293 of the sequence described in Sulaiman et al., Appl Environ Microbiol. 2012 Mar.), an enzyme known to depolymerize PET. LC-cutinase was produced by fermentation of recombinant microorganisms in liquid medium. The PET degrading enzyme was added at a weight ratio of 1:1000 or 2:1000 per amount of PET contained.
[0096] These plastic materials or waste plastics were fed into a reactor in which the amount of PET contained at the start of the depolymerization process was 5% to 40% based on the total weight of the initial reaction medium. Phosphate buffer was added to the plastic materials and enzymes to reach the total weight of the initial reaction medium.
[0097] All parameters related to the depolymerization step of the various methods tested are shown in Tables 1A and 1B below.
[0098] [Table 1]
[0099] [Table 2]
[0100] Periodic sampling was used to monitor the reaction kinetics of terephthalic acid production. The solid phase (containing the undegraded plastic material) was first separated from the liquid phase, which contains the terephthalate salts in soluble form, by centrifugation (D100-DragonLab).
[0101] The concentration of TA was measured by chromatography (UHPLC). For this purpose, 1 mL of methanol and 100 μL of 6 M HCl were added to the diluted samples to decomplex the TA salts. If necessary, the samples were diluted with RO water. The prepared samples were filtered through a 0.22 μm cellulose filter and 20 μL was injected into the chromatography column. The HPLC system used was a model 3000 UHPLC system (Thermo Fisher Scientific, Inc., Waltham, MA, USA) including a pump, an automatic sampling system, a column thermostated at 25 °C and a UV detector at 240 nm. Three eluents were used: 10 mM H2SO4 (eluent A); ultrapure water (eluent B) and methanol (eluent C). Terephthalic acid was separated from other molecules by a gradient between these three solvents. Terephthalic acid is measured according to a standard prepared from commercial terephthalic acid (Acros Organics).
[0102] The concentrations of terephthalic acid produced after 24 hours for the various tests are shown below in Tables 2A and 2B.
[0103] [Table 3]
[0104] In this way, the process for producing terephthalic acid of the invention makes it possible to reach TA concentrations of more than 54 kg / t and 69 kg / t after 24 hours in reactors containing polyester in amounts equal to 15% and 20% by weight, respectively, based on the total weight of the initial reaction medium at the start of the depolymerization step, the pH being controlled at 7 during the depolymerization step.
[0105] [Table 4]
[0106] In this way, the process for producing terephthalic acid of the invention makes it possible to reach TA concentrations of more than 57 kg / t, more than 77 kg / t, more than 106 kg / t, more than 95 kg / t and more than 118 kg / t after 24 hours in reactors containing, at the start of the depolymerization step, amounts of polyester contained equal to 10%, 20%, 25%, 30% and 40% by weight, respectively, based on the total weight of the initial reaction medium, with the pH being controlled at 8 during the depolymerization step.
[0107] Example 2: Production of terephthalic acid in a reactor containing PET in an amount equal to 20% by weight based on the total weight of the initial reaction medium, the pH and temperature being controlled at fixed values of 7-8 and 40°C-60°C, respectively, during the depolymerization step. For this second experimental design, all tests were carried out in the same stirred reactor described in Example 1, with stirring at 300 rpm during the depolymerization step. The basic solution used for pH control was 19.4% NaOH (6M).
[0108] The production of terephthalic acid (TA) was carried out using colored and washed plastic flakes from a PET waste recycling stream identical to those used in experiments D-H in Example 1, except for the final sieving. The resulting powder therefore has a particle size of less than 1 mm. The PET portion of this waste plastic constituted 20% of the mass contained at the start of the PET depolymerization process, based on the total weight of the initial reaction medium.
[0109] The enzyme used is the same as that used in Example 1. It was added in a weight ratio of 2:1000 per amount of PET used.
[0110] Phosphate buffer (100 mM, pH 8) is added to the plastic material and enzyme to reach the total weight of the initial reaction medium.
[0111] Three set temperatures and three pH values were tested, the main information is summarized in Table 3 below.
[0112] [Table 5]
[0113] Periodic sampling was used to monitor the reaction kinetics of terephthalic acid production. TA concentration was measured in a manner similar to that in Example 1.
[0114] For the conditions described above, the following results were obtained at 48 or 72 hours.
[0115] [Table 6]
[0116] The process for producing terephthalic acid according to the invention, carried out in a reactor containing, at the start of the depolymerization step, an amount of polyester present equal to 20%, respectively, makes it possible to reach TA concentrations of more than 40 kg / t after 48 hours and 72 hours. At 60° C., the process makes it possible to reach concentrations of more than 90 kg / t after 48 hours for a pH of 7-8. At 50° C., the process makes it possible to reach concentrations of more than 90 kg / t after 72 hours for a pH of 7-8.
[0117] Example 3: Production of terephthalic acid in a reactor containing PET in an amount equal to 20% by weight, contained in a plastic material in granular form For this third experimental design, all tests were carried out in the same stirred reactor as described in Example 1. The temperature set point was fixed at 60° C. and the pH was controlled at 8.0 using 19.4% NaOH (6M) as the basic solution.
[0118] The production of terephthalic acid (TA) was carried out using a PET Lighter C93 from Resinex. PET was amorphized by extrusion followed by rapid cooling. The extruder used for amorphization was a Leistritz ZSE 18 MAXX twin screw extruder with heating zones set at 285°C-304°C. The crystallinity of the PET obtained in granular form after this amorphization step was estimated to be about 13% (by DSC).
[0119] The granules were fed into the reactor at 20% by weight based on the weight of the initial reaction medium. The enzyme used was the same as that used in Example 1. The enzyme was added to the contained PET at a weight ratio of 1:1000. 10 mM potassium phosphate buffer pH 8 was added to the plastic material and enzyme to reach the total weight of the initial reaction medium.
[0120] To monitor the reaction rate of terephthalic acid production, periodic sampling was used as described in Example 1. The produced terephthalic acid was measured by HPLC according to the protocol described in Example 1. After 88 hours, 62 kg / t TA is obtained, based on the total weight of the liquid phase of the final reaction medium. The results show that it is also possible to achieve the performance claimed in this application when the plastic material containing the target polyester is introduced in granular form.
[0121] Example 4: Terephthalic acid production at different reactor scales In this example, different stirred reactors were used to produce terephthalic acid. The large size of these reactors was used to verify the scale-up of the process and its use on an industrial or semi-industrial scale.
[0122] For these tests, two types of plastic materials were used. For tests A, B, C, E and F, the plastic material was the washed and colored flakes described in Example 1 (98% amorphous PET, micronization <500 μm), while for Example D, the plastic material was the bottle preform (100% PET, micronization <1 mm), also described in Example 1. These plastic materials were included in such a way as to obtain an amount of PET included of 20% by weight, based on the weight of the initial reaction medium. The temperature set point was set at 60° C. and the pH was controlled at 8.0 or 7.0 using 19.4% NaOH (tests A to D) or 25% m / m NaOH (tests E and F). For tests A, B, C, D and E, the enzymes used were the same as those used in Example 1. For test F, the enzyme is a variant of the enzyme of Example 1 obtained by fermentation of a recombinant microorganism (having the following mutations SEQ ID NO: 1+F208I+D203C+S248C+V170I+Y92G), which was added in a weight ratio of 1:1000 per weight of PET involved for tests A to D and in a weight ratio of 2:1000 for tests E and F.
[0123] For Test A, a 500 mL flat-bottom reactor as described in Example 1 was used. Agitation was provided by a 3 cm diameter marine paddle attached to the central shaft. The stirring speed was set at 300 rpm. 56.3 g plastic material was included.
[0124] For test B, a dish-bottom reactor (Global Process Concept) with a total volume of 5 L was used. The reactor was equipped with a temperature probe and a pH probe (Hamilton, EasyFerm HB BioArc 325). Control of these two parameters at the set point was ensured by an internal PID controller in the C-bio software (Global Process Concept). Agitation of the reaction medium was provided by a marine paddle with a diameter of 5.5 cm attached to a central shaft rotating at 200 rpm. 375 g plastic material was included.
[0125] For Test C, a dish-bottom reactor with a total volume of 40 L was used. The reactor was equipped with temperature and pH probes (Rosemount analytical HX338-05). The reaction medium was stirred using a 14 cm diameter marine paddle attached to a central shaft rotating at 150 rpm. 4 kg plastic material was used.
[0126] For Test D, a dish-bottom reactor with a total volume of 150 L was used. The reactor was equipped with temperature and pH probes (EasyFerm BioArc 120, Hamilton). The reaction medium was stirred using a 25 cm diameter marine paddle attached to a central shaft rotating at 80 rpm. 14 kg plastic material was used.
[0127] For tests E and F, a flat-bottom reactor with a total volume of 1000 L was used. The reactor was equipped with temperature and pH probes (In Pro3100 / SG / 325, Mettler Toledo). A variable radius marine paddle was used to stir the reaction medium. 75 kg plastic material was used.
[0128] It is understood that the curved or flat shape of the reactor bottom does not affect the process and the shape of the bottom is interchangeable.
[0129] The main information is summarized in Table 5 below.
[0130] [Table 7]
[0131] To monitor the kinetics of terephthalic acid production, periodic sampling was used as described in Example 1. TA concentrations were measured by UHPLC (as described in Example 1).
[0132] For this reason, the results obtained for the different reactions are detailed in Table 6.
[0133] [Table 8]
[0134] In this way, a concentration of terephthalic acid of more than 78 kg / t, based on the total weight of the liquid phase of the final reaction medium, is obtained under each of the conditions described. In particular, a concentration of terephthalic acid of more than 110 kg / t, based on the total weight of the liquid phase of the final reaction medium, is obtained in a 1000 L reactor.
[0135] Example 5: Production of terephthalic acid in a reactor containing PET from textile waste For these experiments, terephthalic acid production was carried out in a dish-bottom reactor (Global Process Concept) with a total volume of 5 L (described in Example 4).
[0136] For experiment A, terephthalic acid production was performed from post-consumer, shredded, fabric free of metal and hard points (buttons, zippers, etc.). The shredded fabric pieces had a size of 5×5 cm and contained approximately 83% PET.
[0137] For experiment B, the TA was made from production scrap from a waterjet weaving process. This material was in the form of a continuous yarn assembly and contained approximately 100% PET.
[0138] These textile materials were subjected to a drying process at 60°C for 16 hours, then subjected to an extrusion process, followed by rapid cooling to amorphize the PET contained in the waste. The same extruder as in Example 1 was used. The temperature of the heating zone was adjusted according to the following profile: 265℃-265℃-265℃-255℃-255℃-250℃-250℃-245℃-245℃-245℃
[0139] The screw speed was set at 150 rpm. The material was introduced into the extruder manually. The cooling and refining steps were the same as those used in Example 1. The crystallinity of the samples was estimated to be about 18% for the samples in experiment A and less than 10% for the samples in experiment B.
[0140] The enzymes used are the same as those used in Example 4 for Test F. The plastic products or waste plastics were fed into the reactor so that the amount of PET contained at the start of the depolymerization process was comprised between 16.6% and 20% based on the total weight of the initial reaction medium. Phosphate buffer was added to the plastic materials and enzymes to reach the total weight of the initial reaction medium.
[0141] The set of parameters associated with the depolymerization process for Experiments A and B are shown in Table 7.
[0142] [Table 9]
[0143] To monitor the reaction kinetics of terephthalic acid production, periodic sampling was used as described in Example 1. The terephthalic acid produced was measured by HPLC according to the protocol described in Example 1.
[0144] The concentrations of terephthalic acid produced after 24 and 48 hours for the different tests are shown in Table 8 below.
[0145] [Table 10]
[0146] In this way, at each of the conditions described, concentrations of terephthalic acid of more than 75 kg / t, based on the total weight of the liquid phase of the final reaction medium, are obtained.
Claims
1. 1. A process for producing terephthalic acid (TA) from at least one target polyester comprising at least one TA unit, comprising: enzymatically depolymerizing the polyester by contacting the polyester in a stirred reactor with at least one enzyme capable of depolymerizing the polyester; and recovering the TA salt in solubilized form. characterized in that the amount of polyester contained in the reactor is greater than 10% by weight, based on the total weight of the initial reaction medium, the pH is controlled at 6.5-9 during the depolymerization step, and the TA concentration in the liquid phase of the final reaction medium is greater than 40 kg / t; method.
2. 2. A process according to claim 1, characterised in that the weight ratio of the amount of enzyme contained to the amount of target polyester contained is comprised between 0.01:1000 and 3:1000, preferably between 1:1000 and 2:1000.
3. 3. A process according to claim 1 or 2, characterized in that the target polyester is selected from PTT, PBAT, PBT, PCT, PETG, PEIT, PET, most preferably PET.
4. 4. The process according to any one of claims 1 to 3, characterized in that the amount of target polyester contained in the reactor is 11% by weight or more, preferably 15% by weight or more, preferably 20% by weight or more, based on the total weight of the initial reaction medium, and / or the TA concentration in the liquid phase of the final reaction medium is more than 50 kg / t, more than 60 kg / t, more than 70 kg / t, more than 80 kg / t, more than 100 kg / t, more than 120 kg / t.
5. A process according to any one of claims 1 to 4, characterised in that the polyester of interest is in powder form, preferably with a particle size of less than 2 mm, more preferably less than 1 mm.
6. A process according to any one of claims 1 to 5, characterized in that during the depolymerisation step the pH is controlled at between 6.5 and 8.5, preferably between 7.5 and 8.
5.
7. 7. A process according to any one of claims 1 to 6, characterized in that the depolymerization step lasts for at most 150 hours, preferably between 1 hour and 120 hours, between 1 hour and 100 hours, between 1 hour and 72 hours, between 1 hour and 48 hours.
8. 8. The method according to claim 1, characterized in that the step of recovering the solubilized TA salt comprises a step of separating a liquid phase containing the TA salt from the remainder of the reaction medium and / or the method comprises the further step of recovering the TA by precipitating the TA contained in the TA salt.
9. 9. The method according to any one of claims 1 to 8, characterized in that the polyester of interest is PET and the enzyme is a cutinase capable of depolymerizing PET, preferably selected from enzymes having an amino acid sequence with at least 75% identity with SEQ ID NO:
1.
10. 10. A process according to any one of claims 1 to 9, characterized in that the pH is controlled during the depolymerization step by adding to the reaction medium a basic solution concentrated to at least 10% by weight ±1%, preferably at least 15% ±1%, more preferably at least 20% ±1% base, based on the total weight of the basic solution.
11. A process according to any one of claims 1 to 10, characterized in that the amount of polyester of interest contained in the reactor is comprised between 15% and 25%, preferably between 20% ± 2%, the pH is controlled between 7.5 and 8.5 during the depolymerization step by adding to the reaction medium a basic solution concentrated to at least 15% ± 1%, and the TA concentration in the liquid phase of the final reaction medium is greater than 100 kg / t.
12. The process according to any one of claims 1 to 11, characterized in that the temperature is controlled at 60 to 80°C.
13. A process according to any one of claims 1 to 12, characterized in that it is carried out in a reactor having a volume of more than 1000 L.
14. A reactor having a volume of at least 1000 liters, carrying out at least one step of enzymatic depolymerization of the target polyester comprising at least one TA unit in a reactor; The amount of polyester contained in the reactor is greater than 10% by weight, based on the total weight of the initial reaction medium, and the TA concentration in the liquid phase of the final reaction medium is greater than 40 kg / t. Reactor.
15. The reactor according to claim 14, characterized in that the amount of the target polyester contained in the reactor is contained in the range of 15% to 25%, preferably 20%±2%, the pH and temperature in the reactor are controlled at 7.5 to 8.5 and 60° C. to 80° C. during the depolymerization step, and the TA concentration in the liquid phase of the final reaction medium is more than 100 kg / t.