Monoalkylated diamines for epoxy formulations:novel curing agents for epoxy systems
Monoalkylated cycloaliphatic diamines address the short pot life and viscosity issues of cycloaliphatic amines in epoxy resin systems, enhancing processing and mechanical properties of composite parts by extending pot life and reducing viscosity.
Patent Information
- Application Number
- JP2024121128
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-01-11
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2040-01-10
AI Technical Summary
Existing epoxy resin systems face challenges with short pot life, high viscosity during processing, and compromised mechanical properties due to the use of cycloaliphatic amines, which affect fiber wetting and lead to issues like delamination and stress in composite parts.
The use of monoalkylated cycloaliphatic diamines as primary hardeners in epoxy resin compositions, which extend pot life, maintain mechanical and thermal properties, and reduce viscosity, allowing for improved fiber wetting and processing of large composite parts.
Monoalkylated cycloaliphatic diamines provide a balanced pot life and viscosity, ensuring effective fiber wetting and maintaining mechanical, thermal, and chemical performance in cured epoxy compositions, reducing stress and delamination in composite parts.
Smart Images

Figure 2024156767000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an epoxy resin system comprising an epoxy resin and a monoalkylated diamine. The epoxy resin system may further comprise a second amine. The present invention also relates to a method of making the epoxy resin system comprising combining an epoxy resin with a monoalkylated diamine. The monoalkylated diamine of the present invention enhances desirable processing and cured material properties of the epoxy resin composition without adversely affecting the mechanical properties of the cured material, which is typically observed with cycloaliphatic amine-based hardeners. [Background technology]
[0002] Araliphatic and cycloaliphatic amines are commonly used as epoxy curing agents for thermosetting structural composite applications. The type of amine used as the curing agent is essential to achieve the final performance of the cured product. Each reactive amine of the type, primary or secondary amine, is cured at a specific temperature to achieve full cure. The cure temperature defines the end use temperature and the T g Typically, compounding an epoxy resin with a high-functionality hardener leads to short pot life, high compound viscosity, and weak parts after curing. All these adverse effects are caused by the high functionality of the hardener. In step-growth polymerization, the degree of polymerization X n , and the critical degree of reaction (gel point - p c ) is directly linked to the functionality of the polymerization system: X n =2 / (2-pf ave ) is well known, where p is the progress of the reaction, and f ave is the average functionality, and p c =2 / f ave Thus, systems with higher average functionality will reach higher molecular weights and gels at a lower degree of polymerization than those with lower average functionality. U.S. Pat. No. 4,293,682 discloses the use of tetra- and penta-functional amines as curing agents.
[0003] While low functionality hardeners provide longer pot life, they lead to a final cured network with low crosslink density and poor thermal and mechanical properties. This inverse relationship between high functionality monomers required for final part properties and low functionality monomers for enhanced pot life requires compromises in epoxy resin formulations. Some materials with low functionality do not build robust polymer networks for use in structural applications. Anything that can be done to increase pot life without adversely affecting final part properties would be advantageous. Some materials with low functionality do not build robust polymer networks for use in structural applications.
[0004] Epoxy resin systems are used in the manufacture of a variety of structural parts, including composites. Examples of articles that have been evaluated for manufacture from epoxy resin systems include composite pipes, pressure vessels, automotive parts, and wind turbine blades. Fabrication of such parts involves many requirements for efficient manufacture, especially when complex manufacturing processes are used. These processes include, but are not limited to, resin infusion, resin transfer molding, filament winding, and large scale casting. One need in the art is a relatively long pot life of the epoxy resin system to wet the fibers in relatively thick sections of the article, where the fabric layer is very dense under vacuum or pressure, and the resin cannot easily penetrate the fabric layer. If the temperature increases during the processing of the article, the viscosity of the cycloaliphatic amine increases under this condition, fiber wetting becomes difficult, and results in loss of mechanical properties in the fabricated parts.
[0005] Additionally, the early increase in viscosity during processing can lead to higher shrinkage after curing of the molded parts. The shrinkage of the cured epoxy resin creates stresses that build up in the composite due to the increase in viscosity during processing. The stresses sometimes lead to cracking in the article, with the resultant loss of mechanical properties. The relatively short pot life of the formulation leads to a relatively fast increase in viscosity during processing of longer parts, and a relatively large amount of stress that builds up in the article during processing.
[0006] For advanced composites to achieve higher performance, multifunctional resins and hardeners are often used. The multifunctional materials usually have a very high starting viscosity. Heat is commonly used to reduce the compounding viscosity. This approach increases the reactivity and therefore can cause handling problems. As the composite parts are getting larger and thicker, the compounding viscosity needs to be lower to have optimal wetting of the reinforcing materials (e.g., glass, carbon, Kevlar, natural fibers, etc.).
[0007] Systems for composite processing require a sufficiently low initial mix viscosity and a sufficiently low rate of viscosity increase at the impregnation temperature so that the resin can completely wet the reinforcing fiber preform before the resin system becomes too viscous to flow satisfactorily through the substrate fibers and fabrics. The requirements for low initial viscosity and long pot life become more stringent as the size of the composite parts increases.
[0008] In view of the above, there is a need in the art for improved curing agents to produce epoxy resin systems that have a longer pot life "work time" of the formulation, thereby reducing the amount of material added during processing, and when combined with improved fiber wetting, enhance mechanical properties compared to prior art resin compositions.
[0009] The dialkylation of isophorone diamine (IPD) is known in the literature (US Pat. No. 7,074,963 B2). The monoalkylated structure of IPD is an intermediate for the dialkylated IPD product. The final composition of dialkylated IPD reported in US Pat. No. 6,403,752 B1 and US Pat. No. 7,074,963 does not have any monoalkylated IPD present. In the present invention, monoalkylated IPD and other monoalkylated cycloaliphatic diamines are used as epoxy curing agents to extend the pot life of IPD, which is not found in any prior art. In addition, the isomer type of the monoalkylated IPD product in the present invention is different from the monoalkylated IPD proposed to produce dialkylated products in US Pat. No. 7,074,963 B2. The unalkylated (unmodified) IPD exhibits a higher Tg and a shorter pot life. The dialkylated IPD products do not proceed to full cure with the epoxy resin. The present approach of using monoalkylated IPD and other monoalkylated cycloaliphatic diamines provides an excellent balance of pot life while maintaining the high Tg. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] U.S. Pat. No. 4,293,682 [Patent Document 2] U.S. Pat. No. 7,074,963 [Patent Document 3] U.S. Patent No. 6,403,752 [Patent Document 4] International Publication No. 2009 / 089145 [Patent Document 5] U.S. Patent No. 2,890,194 [Non-patent literature]
[0011] [Non-Patent Document 1] Y. Tanaka, “Synthesis and Characteristics of Epoxides”, CA May, ed., Epoxy Resins Chemistry and Technology (Marcel Dekker, 1988). Summary of the Invention [Problem to be solved by the invention]
[0012] The object of the present invention was to provide an epoxy resin system and a hardener which overcome the above-mentioned disadvantages of the prior art, as well as a method for producing the same. [Means for solving the problem]
[0013] The above object is achieved by the epoxy resin system and hardener as well as the process for the preparation thereof according to the claims.
[0014] Summary of the Invention It has been found that monoalkylated araliphatic and cycloaliphatic diamines can be used as primary curing agents for epoxy resin compositions that provide sufficient pot life during processing (in resin bath and fiber wetting) to improve the overall mechanical properties of the cured composite product compared to typical cycloaliphatic amine-based curing agents. The main drawback of using cycloaliphatic amines is that they have a short pot life. Another way to measure the pot life industrially is the time for the compound viscosity to double. This gives a good measure of the pot life of the system. By using monoalkylated cycloaliphatic diamines as primary curing agents, it is possible to achieve twice the pot life of the cycloaliphatic diamines and to fully cure at a significantly lower temperature than current cycloaliphatic amine curing agents. Test results show that using monoalkylated cycloaliphatic diamines as primary curing agents maintains good mechanical, thermal and chemical performance in the cured epoxy composition and exceeds the mechanical properties of other cycloaliphatic amines. In addition, formulations containing monoalkylated cycloaliphatic diamines exhibit lower viscosity, longer pot life, and lower temperature T compared to epoxy compositions cured with current cycloaliphatic amine curing agents. g They exhibit lower exotherms during development and curing. Monoalkylated cycloaliphatic diamines can also be used in combination with primary and secondary amines as co-curing agents to further enhance desired properties. The lower viscosity of monoalkylated cycloaliphatic diamines aids in fiber wetting. Preliminary results with monoalkylated cycloaliphatic diamines in composite applications (filament wound tubing and fittings, wind blades, high pressure vessels, structural laminates, automotive body parts, aerospace, etc.) are quite promising.
[0015] An embodiment of the present invention is a method for producing a polymerizable composition comprising an epoxy resin and a polymerizable compound represented by formula (I) [ka] [Wherein, Z is cyclohexyl, C 1 ~C 10 Alkyl-substituted cyclohexyl, phenyl, C 1 ~C 10Alkyl-substituted phenyl, methylenebis(cyclohexyl), and C 1 ~C 10 alkyl-substituted methylene bis(cyclohexyl), a and b are independently 0 or 1, and A is selected from the group consisting of C 1 ~C 10 and a monoalkylated diamine, the monoalkylated diamine being selected from monoalkylated IPD, monoalkylated PACM, monoalkylated DMPACM, monoalkylated MXDA, monoalkylated cyclohexyldiamine, and monoalkylated methylcyclohexyldiamine.
[0016] FIG. 1 shows the viscosity profiles at 40° C. for an epoxy resin composition containing isophorone diamine (IPD) and an epoxy resin composition containing monoalkylated isophorone diamine (AIPD). [Brief description of the drawings]
[0017] [Figure 1] FIG. 2 shows the viscosity profiles at 40° C. for an epoxy resin composition containing non-alkylated IPD and an epoxy resin composition containing mono-alkylated IPD. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] definition The following definitions and abbreviations are provided to aid those skilled in the art in understanding the detailed description of the present invention. IPD - Isophoronediamine PACM - 4,4'-methylenebis(cyclohexylamine) MXDA - m-Xylylenediamine DMPACM - 2,2'-dimethyl-4,4'-methylenebis(cyclohexylamine) Hydrogenated TDA - Methylcyclohexyldiamine CHONE - Cyclohexanone MEK - Methyl Ethyl Ketone ISO - Isophorone.
[0019] Detailed Description of the Invention The epoxy resin system of the present invention comprises an epoxy resin and a copolymer of formula (I) [ka] [Wherein, Z is cyclohexyl, C 1 ~C 10 Alkyl-substituted cyclohexyl, phenyl, C 1 ~C 10 Alkyl-substituted phenyl, methylenebis(cyclohexyl), and C 1 ~C 10 alkyl-substituted methylenebis(cyclohexyl), a and b are independently 0 or 1, and Y is selected from the group consisting of C 1 ~C 10 and monoalkylated diamines in which the alkyl group is alkyl.
[0020] The monoalkylated diamines can preferably be obtained by reacting the corresponding diamines with acetone, methyl ethyl ketone, cyclohexanone, isophorone or aliphatic aldehydes, such as acetaldehyde, followed by hydrogenation, or by reacting the diamines with alkyl halides.Y can thus preferably be a cyclohexyl, secondary butyl, trimethylcyclohexyl or isopropyl group, derived from the respective ketone, aldehyde and alkyl halide.
[0021] In a preferred embodiment of the present invention, the monoalkylated diamine has the structure: [ka] [In the formula, R 1 , R 2 , R 3 , R 4 , R 5 , and R 6 Each of these is H, CH 3, or C 2 ~C 4 is an alkyl group, n is 0 or 1, A is H, and B is C 1 ~C 10 or B is H and A is C 1 ~C 10 The monoalkylated diamines are preferably obtained by reacting the diamines with acetone, methyl ethyl ketone, cyclohexanone, isophorone or aliphatic aldehydes, such as acetaldehyde, followed by hydrogenation, or by reacting the diamines with alkyl halides. Thus, A or B may preferably be a cyclohexyl group, a secondary butyl group, a trimethylcyclohexyl group, or an isopropyl group, derived from the respective ketone, aldehyde and alkyl halide.
[0022] In a preferred embodiment of structure (II), the monoalkylated diamine has the structure: [ka] [Wherein, A is C 1 ~C 10 monoalkylated isophorone diamines represented by the formula: structure: [ka] [In the formula, B is C 1 ~C 10 monoalkylated isophorone diamines represented by the formula: structure: [ka] [Wherein, A is C 1 ~C 10 monoalkylated methylcyclohexyldiamine represented by the formula: structure: [ka] [In the formula, B is C 1 ~C 10 wherein R is an alkyl group; and structure: [ka] [Wherein, A is C 1 ~C 10 The monoalkylated cyclohexyldiamine represented by the formula: is selected from the group consisting of:
[0023] In another preferred embodiment of the present invention, the monoalkylated diamine has the structure: [ka] [In the formula, R 1 and R 2 Each of 3 and A is C 1 ~C 10 The monoalkylated diamines are preferably obtained by reacting the diamines with acetone, methyl ethyl ketone, cyclohexanone, isophorone or aliphatic aldehydes, such as acetaldehyde, followed by hydrogenation, or by reacting the diamines with alkyl halides. Thus, A is preferably a cyclohexyl, secondary butyl, trimethylcyclohexyl or isopropyl group, derived from the respective ketone, aldehyde and alkyl halide.
[0024] In a further preferred embodiment of structure (VIII), the monoalkylated diamine has the structure: [ka] [Wherein, A is C 1 ~C 10 monoalkylated 4,4'-methylenebis(cyclohexylamine), structure: [ka] [Wherein, A is C 1 ~C 10 Monoalkylated 2,2'-dimethyl-4,4'-methylenebis(cyclohexylamine) represented by the formula: is selected from the group consisting of:
[0025] In another preferred embodiment of the present invention, the monoalkylated diamine has the structure: [ka] [wherein X is a phenyl group or a cyclohexyl group, and A is C 1 ~C 10 The monoalkylated diamines are preferably obtained by reacting the diamines with acetone, methyl ethyl ketone, cyclohexanone, isophorone or aliphatic aldehydes, such as acetaldehyde, followed by hydrogenation, or by reacting the diamines with alkyl halides. Thus, A may preferably be a cyclohexyl, secondary butyl, trimethylcyclohexyl or isopropyl group, derived from the respective ketone, aldehyde and alkyl halide.
[0026] In a preferred embodiment of structure (XI), the monoalkylated diamine has the structure: [ka] [Wherein, A is C 1 ~C 10 wherein m-xylylenediamine is an alkyl group; and structure: [ka] [Wherein, A is C 1 ~C 10Monoalkylated 1,3-bisaminomethylcyclohexane represented by the formula: is selected from the group consisting of:
[0027] The epoxy resin system may comprise one or more epoxy resins. Preferably, the epoxy resin system comprises only one epoxy resin. Similarly, the epoxy resin system may comprise one or more compounds of formula (I). Preferably, the epoxy resin system comprises only one compound of formula (I).
[0028] In one embodiment, the epoxy resin system comprises 1% to 99% by weight of the monoalkylated diamine, based on the total weight of the curing agent. Preferably, the epoxy resin system comprises at least 20% by weight, more preferably at least 40% by weight, even more preferably at least 60% by weight, and particularly preferably at least 80% by weight of the monoalkylated diamine, based on the total weight of the curing agent.
[0029] Preferably, the epoxy resin system comprises 20-100% by weight of the monoalkylated diamine, 0-50% by weight of the non-alkylated diamine, and 0-30% by weight of the dialkylated diamine, based on the total weight of the curing agent.
[0030] Another aspect of the present invention is a method for producing an epoxy resin system, the method comprising: [ka] [Wherein, Z is cyclohexyl, C 1 ~C 4 Alkyl-substituted cyclohexyl, phenyl, C 1 ~C 4 Alkyl-substituted phenyl, methylenebis(cyclohexyl), and C 1 ~C 4 alkyl-substituted methylenebis(cyclohexyl), a and b are independently 0 or 1, and Y is selected from the group consisting of C 1 ~C 10The method includes combining a monoalkylated diamine of the formula (I) with an alkyl group, and optionally other ingredients.
[0031] The mass ratio of the epoxy resin to the monoalkylated diamine is preferably 1:0.05 to 1:0.95. In a more preferred embodiment, the mass ratio is 1:0.3 to 1:0.6.
[0032] The epoxy resin system may preferably further comprise a second amine, which is selected from the group consisting of primary amines and secondary amines. The second amine preferably comprises one or more amine compounds selected from the group consisting of polyetheramines, polyetherpolyamines, saturated aliphatic cyclic diamines, linear aliphatic amines, cyclic aliphatic amines, polycyclic aliphatic amines, and aromatic amines.
[0033] Preferably, the polyetheramine has the formula: 2 NCH(CH 3 )CH 2 -[OCH 2 CH(CH 3 )] x NH 2 and x is 2 to 70. Preferably, the second amine is selected from the group consisting of 4,4'-methylenebiscyclohexylamine, isophoronediamine, 1,2-diaminocyclohexane, 4,4'-methylenebis(2-methylcyclohexylamine), 1,3-bisaminomethylcyclohexane, and polyetheramine:H 2 NCH(CH 3 )CH 2 [OCH 2 CH(CH 3 )] 2.5 NH 2 The mixture may include:
[0034] Preferably, modified amine compounds, such as Mannich bases, polyamide compounds, amine-epoxy adducts, and combinations thereof, can be used as co-curing agents for use with monoalkylated diamine compounds as described herein.
[0035] Preferably, the epoxy resin may comprise a polyglycidyl ether of a compound selected from the group consisting of an aliphatic glycol, a cycloaliphatic glycol, a triol, a polyol, a polyglycol, and combinations thereof. The epoxy resin system may further comprise a polyacrylate or polymethacrylate ester of a polyol.
[0036] Referring to Figure 1, the viscosity profile at 40°C for an epoxy resin composition containing a non-alkylated product (IPD) is compared to the viscosity profile for an epoxy resin composition containing a mono-alkylated product. The reactivity time (min) of the composition increases significantly with alkylation chemistry.
[0037] The epoxy resin may consist of a single resin or may be a mixture of mutually compatible epoxy resins. The epoxy resin may include, but is not limited to, difunctional epoxy resins, such as bisphenol-A and bisphenol-F resins. As used herein, multifunctional epoxy resins refer to compounds having two or more 1,2-epoxy groups per molecule. Epoxide compounds of this type are well known to those skilled in the art and are described in Y. Tanaka, "Synthesis and Characteristics of Epoxides", CA May, ed., Epoxy Resins Chemistry and Technology (Marcel Dekker, 1988), which is incorporated herein by reference in its entirety.
[0038] One class of epoxy resins suitable for use are the glycidyl ethers of polyhydric phenols, including glycidyl ethers of dihydric phenols. Preferred are the glycidyl ethers of: resorcinol, hydroquinone, bis-(4-hydroxy-3,5-difluorophenyl)-methane, 1,1-bis-(4-hydroxyphenyl)-ethane, 2,2-bis-(4-hydroxy-3-methylphenyl)-propane, 2,2-bis-(4-hydroxy-3,5-dichlorophenyl)propane, 2,2-bis-(4-hydroxyphenyl)-propane (commercially known as bisphenol-A), bis-(4-hydroxyphenyl)-methane (commercially known as bisphenol-F and may contain various amounts of 2-hydroxyphenyl isomers), and the like, or any combination thereof. Additionally, the advanced process dihydric phenol of the structure of formula (XIV) is also preferred in the present disclosure: [ka] [wherein m is 0 to 25, and R is a divalent hydrocarbon group of a dihydric phenol, for example, a divalent hydrocarbon group of a dihydric phenol listed above].
[0039] The material according to formula (1) can be prepared by polymerizing a mixture of a dihydric phenol and epichlorohydrin, or by advancing a mixture of the diglycidyl ether of the dihydric phenol and the dihydric phenol. While in any particular molecule, the value of m is an integer, the material is always a mixture that can be characterized by an average value of m, which is not necessarily an integer. Polymeric materials having an average value of m between 0 and about 7 can be used in one embodiment of the present disclosure. In other embodiments, the epoxy resin can be a polyglycidylamine from one or more of 2,2'-methylenedianiline, 4,4'-methylenedianiline, m-xylylenedianiline, hydantoin, and isocyanate.
[0040] The epoxy resin may preferably be a cycloaliphatic (alicyclic) epoxide. Particularly preferred cycloaliphatic epoxides are diepoxides of cycloaliphatic esters of dicarboxylic acids, in particular bis(3,4-epoxycyclohexylmethyl)oxalate, bis(3,4-epoxycyclohexylmethyl)adipate, bis(3,4-epoxy-6-methylcyclohexylmethyl)adipate, vinylcyclohexene diepoxide; limonene diepoxide; bis(3,4-epoxycyclohexylmethyl)pimelate; dicyclopentadiene diepoxide; and other suitable cycloaliphatic epoxides. Other suitable diepoxides of cycloaliphatic esters of dicarboxylic acids are described, for example, in WO 2009 / 089145 A1, which is hereby incorporated by reference in its entirety.
[0041] Other particularly preferred cycloaliphatic epoxides are 3,3-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate; 3,3-epoxy-1-methylcyclohexyl-methyl-3,4-epoxy-1-methylcyclohexanecarboxylate; 6-methyl-3,4-epoxycyclohexylmethyl-6-methyl-3,4-epoxycyclohexanecarboxylate; and 3,4-epoxy-2-methylcyclohexyl-methyl-3,4-epoxy-3-methylcyclohexanecarboxylate.Other suitable 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylates are described, for example, in U.S. Pat. No. 2,890,194, which is hereby incorporated by reference in its entirety.In other embodiments, the epoxy resin may comprise a polyol polyglycidyl ether from polyethylene glycol, polypropylene glycol or polytetrahydrofuran or a combination thereof.
[0042] In another embodiment, epoxy novolac resins, which are glycidyl ethers of novolac resins, can be used as multifunctional epoxy resins according to the present disclosure. In yet another embodiment, the at least one multifunctional epoxy resin is a diglycidyl ether of bisphenol-A (DGEBA), an advance process variant or higher molecular weight variant of DGEBA, a diglycidyl ether of bisphenol-F, an epoxy novolac resin, or any combination thereof. Higher molecular weight variants or derivatives of DGEBA are produced by the advance process, in which excess DGEBA is reacted with bisphenol-A to produce epoxy-terminated products. The epoxy equivalent weight (EEW) of such products ranges from about 450 to 3000 or more. Because these products are solid at room temperature, they are often referred to as solid epoxy resins.
[0043] DGEBA or advanced process DGEBA resins are often used in structural formulations due to their combination of low cost and high performance properties. Commercial grades of DGEBA with EEWs ranging from about 174 to about 250, and more commonly from about 185 to about 195, are readily available. At these low molecular weights, the epoxy resins are liquid and are often referred to as liquid epoxy resins. It is understood by those skilled in the art that most grades of liquid epoxy resins are slightly polymeric, since pure DGEBA has an EEW of 174. Resins with EEWs of 250 to 450, also typically produced by the advanced process, are referred to as semi-solid epoxy resins, since they are a mixture of solids and liquids at room temperature. Multifunctional resins with an EEW of about 160 to about 750 based on solids are useful in the present disclosure. In another embodiment, the multifunctional epoxy resins have an EEW in the range of about 170 to about 250.
[0044] Depending on its end use application, it may be beneficial to reduce the viscosity of the composition of the present disclosure by modifying the epoxy resin. The epoxy resin, including at least one multifunctional epoxy resin, may further include a monofunctional epoxide. Preferred examples of monoepoxides are styrene oxide, cyclohexene oxide, and phenol, cresols, tert-butylphenol, other alkylphenols, butanol, 2-ethylhexanol, C 4 ~C 14 glycidyl ethers of alcohols, etc., or combinations thereof. The multifunctional epoxy resin may be in a solution or emulsion, where the diluent is water, an organic solvent, or a mixture thereof.
[0045] Hardener As described above, the curing agent is a monoalkylated diamine of formula (I). The curing agent may further include a second amine. The second amine may consist of a single amine or a mixture of amines. The amine in the second amine is a primary or secondary amine.
[0046] In some applications, the following are suitable as the second amine: polyether diamines, saturated aliphatic cyclic diamines, linear aliphatic amines, cycloaliphatic diamines, polycyclic aliphatic amines, aromatic amines, and combinations thereof. The weight ratio of the epoxy resin to the monoalkylated diamine and the second amine is preferably 1:0.95:0.05. In another embodiment, the weight ratio is preferably 1:0.05:0.95. The polyamine is preferably an aliphatic polyamine, such as diethylenetriamine (DETA), triethylenetetramine (TETA), tetraethylenepentamine (TEPA), pentaethylenehexamine (PEHA), hexamethylenediamine (HMDA), N-(2-aminoethyl)-1,3-propanediamine (N 3 -amine), N,N′-1,2-ethanediylbis-1,3-propanediamine (N 4-amine), or dipropylenetriamine; arylaliphatic polyamines, such as m-xylylenediamine (mXDA), or p-xylylenediamine; cycloaliphatic polyamines, such as 1,3-bisaminomethylcyclohexane (1,3-BAC), isophoronediamine (IPDA), 4,4′-methylenebiscyclohexylamine (PACM), 1,2-diaminocyclohexane, or 4,4′-methylenebis-(2-methyl-cyclohexyl-amine); aromatic polyamines, such as m-phenylenediamine, diaminodiphenylmethane (DDM), or diaminodiphenylsulfone (DDS); heterocyclic polyamines such as N-aminoethylpiperazine (NAEP), or 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro(5,5)undecane; polyalkoxypolyamines in which the alkoxy groups may be oxyethylene, oxypropylene, oxy-1,2-butylene, oxy-1,4-butylene or copolymers thereof, such as 4,7-dioxadecane-1,10-diamine, 1-propanamine, 3,3′-(oxybis(2,1-ethanediyloxy))bis- (diaminopropylated diethylene glycol ANCAMINE® 1922A), poly(oxy(methyl-1,2-ethanediyl)), α-(2-aminomethylethyl)-ω-(2-aminomethylethoxy) (JEFFAMINE® D 230, D-400), triethylene glycol diamine and oligomers (JEFFAMINE® XTJ-504, JEFFAMINE® XTJ-512), poly(oxy(methyl-1,2-ethanediyl)), α,α'-(oxydi-2,1-ethanediyl)bis(ω-(aminomethylethoxy)) (JEFFAMINE® XTJ-511), bis(3-aminopropyl)polytetrahydrofuran 350, bis(3-aminopropyl)polytetrahydrofuran 750, poly(oxy(methyl-1,2-ethanediyl)), α-hydro-ω-(2-aminomethylethoxy)ether and 2-ethyl-2-(hydroxymethyl)-1,3-propanediol (3:1) (JEFFAMINE® T-403), and diaminopropyl dipropylene glycol.JEFFAMINE® is a registered trademark of Huntsman Petrochemical LLC.
[0047] Particularly suitable polyamines are isophorone diamine (IPD), 4,4'-methylenebiscyclohexylamine (PACM), 3,3'-dimethyl PACM (ANCAMINE® 2049), N-aminoethylpiperazine (NAEP), 4,7-dioxadecane-1,10-diamine, 1-propanamine, 3,3'-(oxybis(2,1-ethanediyloxy))bis- (ANCAMINE® 1922A), poly(oxy(methyl-1,2-ethanediyl)), α-(2-aminomethylethyl)-ω-(2-aminomethylethoxy) (JEFFAMINE® D 230, D-400), poly(propylene glycol) bis(2-aminopropyl ether), triethylene glycol diamine (JEFFAMINE® XTJ-504), and poly(oxy(methyl-1,2-ethanediyl)), α,α'-(oxy(di-2,1-ethanediyl))bis(ω-(aminomethylethoxy)) (JEFFAMINE® XTJ-511) or mixtures thereof. ANCAMINE® is a registered trademark of Evonik Degussa GmbH.
[0048] Additional amines suitable for forming the second amine include those having the structure (XV): [ka] [In the formula, R 1 is CH 2 CH 2 CH 2 NH 2 ;R 2 , R 3 and R 4 are independently H or CH 2 CH 2 CH 2 NH 2 and X is CH 2 CH 2 or CH 2 CH2 CH 2 In one embodiment, R 2 and R 3 At the same time, it is not H.
[0049] Optional Additives The epoxy-based formulation for the composite may optionally contain additives such as, but not limited to, non-reactive plasticizer(s), filler(s), processing aid(s), stabilizers, defoamers, viscosity modifier(s), UV absorbers, flame retardants, and / or impact modifiers.
[0050] Any of the acrylate or methacrylate esters of polyols are blended with the epoxy resin in a weight ratio of from 0 to about 100 parts ester for every 100 parts epoxy resin. In another embodiment, the acrylate or methacrylate esters of polyols are blended with the epoxy resin in a weight ratio of from about 5 to about 100 parts ester for every 100 parts epoxy resin.
[0051] Nanomaterials / fillers may be included. The term "nanomaterial" includes, but is not limited to, multi-wall carbon nanotubes or boron nitride nanotubes, single-wall carbon, carbon or boron nitride nanoparticles, carbon or boron nitride nanofibers, carbon or boron nitride nanoropes, carbon or boron nitride nanoribbons, nanoclays; nanoclays with tubules; layered inorganic clay materials; talc; carbon black; cellulose fibers; silica; and alumina.
[0052] The epoxy resin system of the present invention can be preferably prepared by a method for preparing an epoxy resin system, wherein the epoxy resin is a carboxylic acid ester having the formula (I): [ka] [Wherein, Z is cyclohexyl, C 1 ~C4 Alkyl-substituted cyclohexyl, phenyl, C 1 ~C 4 Alkyl-substituted phenyl, methylenebis(cyclohexyl), and C 1 ~C 4 alkyl-substituted methylenebis(cyclohexyl), a and b are independently 0 or 1, and Y is selected from the group consisting of C 1 ~C 10 The diamine is then combined with a monoalkylated diamine, wherein the diamine is a monoalkyl group, and optionally other ingredients.
[0053] The curable epoxy resin compositions and cured products described herein may be useful as structural and electrical laminates, coatings, castings, structural members (especially for the aerospace industry), and circuit boards for the electronics industry, among other applications. The curable epoxy resin compositions disclosed herein may be used in electrical varnishes, encapsulants, semiconductors, general purpose molding powders, filament wound pipe and fittings, filament wound pressure vessels, low and high pressure pipe and fittings, low and high pressure vessels, storage tanks, wind turbine blades, automotive structural components, aerospace structural components, oil and gas buoyancy modules, rigs, well plugs, cured in place pipe (CIPP), structural adhesives and laminates, composite liners, pump liners, corrosion resistant coatings, and other suitable epoxy-containing products.
[0054] The curable epoxy resin composition may be used to form a composite material based on a reinforcing fiber substrate. The reinforcing fiber substrate may preferably be one or more layers of a fiberglass material. Contacting the reinforcing fiber substrate with the epoxy resin system may preferably include a coating process selected from the group consisting of hand lamination, infusion process, filament winding, pultrusion, resin transfer molding, fiber pre-impregnation process, and combinations thereof.
[0055] Preferred fibrous substrates include organic or inorganic fibers, natural or synthetic fibers, and may be in the form of woven or non-crimp fabrics, nonwovens, webs or mats, as well as fiber strands (rovings), or staple fibers, which are formed from continuous or discontinuous fibers, such as fiberglass, carbon fibers, carbon nanotubes, nanocomposite fibers, polyaramid fibers, such as those sold under the trade name KEVLAR®, poly(p-phenylene benzobisoxazole) fibers, such as those sold under the trade name ZYLON®, ultra-high molecular weight polyethylene fibers, such as those sold under the trade name SPECTRA®, high and low density polyethylene fibers, polypropylene fibers, nylon fibers, cellulose fibers, natural fibers, biodegradable fibers, and combinations thereof.
[0056] Preferably, these fibers (woven or non-woven) may be coated with said epoxy resin mixtures in solvent or solvent-free form by standard impregnation methods, in particular filament winding (FW), pultrusion, sheet molding compound, bulk molding compound, autoclave molding, resin infusion, vacuum assisted resin transfer molding (VARTM), resin transfer molding (RTM), wet / hand lay-up, vacuum bag molding, resin impregnation, prepreg, fiber impregnation, compression molding (CM), brushing, spraying, or dipping, casting, injection molding or combinations thereof.
[0057] The present disclosure also includes articles of manufacture comprising the amine-epoxy compositions as described above. Such articles may include, but are not limited to, adhesives, coatings, primers, sealants, curing agents, construction products, flooring products, composite products, laminates, potting compounds, grouts, fillers, cementitious grouts, or self-leveling flooring. Additional ingredients or additives can be used together with the compositions of the present disclosure to produce articles of manufacture. Furthermore, such coatings, primers, sealants, curing agents, or grouts can be applied to metal or cementitious substrates.
[0058] The present invention relates to a compound represented by formula (I) [ka] wherein Z is selected from the group consisting of cyclohexyl, phenyl, and methylenebis(cyclohexyl); a and b are independently 0 or 1; and Y is C 1 ~C 10 The present invention also relates to the use of a monoalkylated diamine of the formula (I) wherein R is an alkyl group, R is an alkyl group, or a preferred embodiment thereof as described above, as a hardener for epoxy resins. EXAMPLES
[0059] Examples 1 to 9 are methods for synthesizing the curing agent of the present invention.
[0060] Example 1. Synthesis of sec-butylated isophorone diamine, molar ratio 0.5 / 1.0 (MEK:IPD) The synthesis of N-sec-butylisophoronediamine is a one-batch process. 990.3 g (5.815 mol) of isophoronediamine and 209.7 g (2.908 mol) of 2-butanone were charged to a 2 L autoclave batch reactor with 7.43 g of 5% sulfided platinum on carbon catalyst. The reactor was sealed and subsequently purged with nitrogen and then hydrogen to remove all air from the reactor. The reactor was pressurized to 27.2 atm (400 psig) with hydrogen and the reactor was heated to 120-140°C. The pressure had increased to 54.4 atm (800 psig) when the rate of hydrogen uptake slowed. The hydrogenation process was continued until the rate of hydrogen uptake dropped below 0.0007 MPa / min (0.1 psi / min). The reactor was cooled to ambient temperature and depressurized, and the reaction product was filtered to remove the catalyst. A rotary evaporator was used to remove water, operating under 30 mmHg vacuum and up to 100°C. The resulting reaction product was sec-butylated isophoronediamine, the composition determined by gas chromatography is shown in the table below, and represented by the structure below. Alternatively, the same product was obtained by the same procedure as above using 5% palladium on carbon catalyst, with slightly different conversion rates.
[0061] Example 2. Synthesis of sec-butylated isophorone diamine, molar ratio 1.0 / 1.0 (MEK:IPD) The synthesis of N-sec-butylisophoronediamine is a one-batch process. 843.0 g (4.950 mol) of isophoronediamine and 357.0 g (4.950 mol) of 2-butanone were charged to a 2 L autoclave batch reactor with 6.32 g of 5% sulfided platinum on carbon catalyst. The reactor was sealed and subsequently purged with nitrogen and then hydrogen to remove all air from the reactor. The reactor was pressurized to 27.2 atm (400 psig) with hydrogen and the reactor was heated to 120-140°C. The pressure had increased to 54.4 atm (800 psig) when the rate of hydrogen uptake slowed. The hydrogenation process was continued until the rate of hydrogen uptake dropped below 0.0007 MPa / min (0.1 psi / min). The reactor is cooled to ambient temperature and depressurized, and the reaction product is filtered to remove the catalyst. A rotary evaporator is operated under 30 mmHg vacuum and up to 100°C to remove water. The resulting reaction product is sec-butylated isophorone diamine, and the composition determined by gas chromatography is shown in the table below and represented by the following structure. Alternatively, the same product can be obtained by the same procedure as above using 5% palladium on carbon catalyst, with slightly different conversion rates. In this case, the NMR spectrum of the product is carried out, and the ratio of main monoalkylated IPD to minor monoalkylated IPD is 80:20, while the selectivity of total monoalkylated IPD is about 90%. [ka] Product composition: [Table 1]
[0062] Example 3. Synthesis of cyclohexylated isophorone diamine, molar ratio 0.5 / 1.0 (CHONE:IPD) The synthesis of N-cyclohexylisophoronediamine is a one-batch process. 465.8g (2.74mol) of isophoronediamine and 134.2g (1.37mol) of cyclohexanone were charged into a 1L autoclave batch reactor with 7.0g of 5% sulfided platinum on carbon catalyst. The reactor was sealed and then purged with nitrogen and then hydrogen to remove all air from the reactor. The reactor was pressurized to 27.2atm (400psig) with hydrogen and heated to 120°C. The pressure had increased to 54.4atm (800psig) when the rate of hydrogen uptake slowed. This hydrogenation process was continued until the rate of hydrogen uptake dropped below 0.0007MPa / min (0.1psi / min). The reactor was cooled to ambient temperature and depressurized, and the reaction product was filtered to remove the catalyst. Water was removed using a rotary evaporator operating under 30 mm Hg vacuum and temperatures up to 100° C. The resulting reaction product was cyclohexylated isophorone diamine, the composition of which, as determined by gas chromatography, is shown in the table below.
[0063] Example 4. Synthesis of cyclohexylated isophorone diamine, molar ratio 1.0 / 1.0 (CHONE:IPD) The synthesis of N-cyclohexylisophoronediamine is a one-batch process. 348.9g (2.05mol) of isophoronediamine and 201.1g (2.05mol) of cyclohexanone were charged into a 1L autoclave batch reactor with 5.2g of 5% palladium on carbon catalyst. The reactor was sealed and then purged with nitrogen and then hydrogen to remove all air from the reactor. The reactor was pressurized to 27.2atm (400psig) with hydrogen and heated to 120°C. The pressure had increased to 54.4atm (800psig) when the rate of hydrogen uptake slowed. This hydrogenation process was continued until the rate of hydrogen uptake dropped below 0.0007MPa / min (0.1psi / min). The reactor was cooled to ambient temperature and depressurized, and the reaction product was filtered to remove the catalyst. Water was removed using a rotary evaporator operating under 30 mm Hg vacuum and temperatures up to 100° C. The resulting reaction product was cyclohexylated isophorone diamine, the composition of which, as determined by gas chromatography, is shown in the table below. Product composition: [Table 2]
[0064] Example 5. Synthesis of trimethylcyclohexylated isophorone diamine, molar ratio 0.5 / 1.0 (isophorone:IPD) The synthesis of N-trimethylcyclohexylisophoronediamine is a one-batch process. 170.8g (1.00mol) of isophoronediamine and 69.2g (0.50mol) of isophorone were combined with 240g of tetrahydrofuran and charged into a 1L autoclave batch reactor with 7.2g of 5% palladium on carbon catalyst. The reactor was sealed and then purged with nitrogen and then hydrogen to remove all air from the reactor. The reactor was pressurized to 27.2atm (400psig) with hydrogen and the reactor was heated to 160°C. The pressure had increased to 54.4atm (800psig) when the rate of hydrogen uptake slowed. This hydrogenation process was continued until the rate of hydrogen uptake dropped below 0.0007MPa / min (0.1psi / min). The reactor was cooled to ambient temperature and depressurized, and the reaction product was filtered to remove the catalyst. A rotary evaporator was used to remove water and tetrahydrofuran, operating at 30 mm Hg vacuum and up to 100° C. The resulting reaction product was trimethylcyclohexylated isophorone diamine, the composition of which, as determined by gas chromatography, is shown in the table below.
[0065] Example 6. Synthesis of trimethylcyclohexylated isophorone diamine, molar ratio 1.0 / 1.0 (isophorone:IPD) The synthesis of N-trimethylcyclohexylisophoronediamine is a one-batch process. 132.5g (0.78mol) of isophoronediamine and 107.5g (0.78mol) of isophorone were combined with 240g of tetrahydrofuran and charged into a 1L autoclave batch reactor with 3.6g of 5% palladium on carbon catalyst. The reactor was sealed and then purged with nitrogen and then hydrogen to remove all air from the reactor. The reactor was pressurized to 27.2atm (400psig) with hydrogen and heated to 160°C. The pressure had increased to 54.4atm (800psig) when the rate of hydrogen uptake slowed. This hydrogenation process was continued until the rate of hydrogen uptake dropped below 0.0007MPa / min (0.1psi / min). The reactor was cooled to ambient temperature and depressurized, and the reaction product was filtered to remove the catalyst. A rotary evaporator was used to remove water and tetrahydrofuran, operating at 30 mm Hg vacuum and up to 100° C. The resulting reaction product was trimethylcyclohexylated isophorone diamine, the composition of which, as determined by gas chromatography, is shown in the table below. Product composition: [Table 3]
[0066] Example 7. Synthesis of sec-butylated 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, molar ratio 1.0 / 1.0 (MEK:DMPACM) The synthesis of N-sec-butyl-3,3'-dimethyl-4,4'-diaminodicyclohexylmethane is a one-batch process. 460.7 g (1.93 mol) of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane and 139.3 g (1.93 mol) of 2-butanone were charged to a 1 L autoclave batch reactor with 3.46 g of 5% sulfided platinum on carbon catalyst. The reactor was sealed and subsequently purged with nitrogen and then hydrogen to remove all air from the reactor. The reactor was pressurized to 34.0 atm (500 psig) with hydrogen and the reactor was heated to 160°C. The pressure had increased to 54.4 atm (800 psig) when the rate of hydrogen uptake slowed. The hydrogenation process was continued until the rate of hydrogen uptake dropped below 0.0007 MPa / min (0.1 psi / min). The reactor was cooled to ambient temperature and depressurized, and the reaction product was filtered to remove the catalyst. A rotary evaporator was used to operate under 40 mm Hg vacuum and temperatures up to 100° C. to remove water. The resulting reaction product was sec-butylated 3,3′-dimethyl-4,4′-diaminodicyclohexylmethane, with a composition determined by gas chromatography shown in the table below and represented by the structure below. [ka]
[0067] Product composition: [Table 4]
[0068] Example 8. Synthesis of sec-butylated m-xylylenediamine, molar ratio 1.0 / 1.0 (MEK:MXDA) The synthesis of N-sec-butyl-m-xylylenediamine is a one-batch process. 392.3 g (2.88 mol) of m-xylylenediamine and 207.7 g (2.88 mol) of 2-butanone were charged into a 1 L autoclave batch reactor with 2.94 g of 5% sulfided platinum on carbon catalyst. The reactor was sealed and then purged with nitrogen and then hydrogen to remove all air from the reactor. The reactor was pressurized to 34.0 atm (500 psig) with hydrogen and the reactor was heated to 120° C. The pressure had increased to 54.4 atm (800 psig) when the rate of hydrogen uptake slowed. This hydrogenation process was continued until the rate of hydrogen uptake dropped below 0.0007 MPa / min (0.1 psi / min). The reactor was cooled to ambient temperature and depressurized, and the reaction product was filtered to remove the catalyst. Water was removed using a rotary evaporator operating under 40 mm Hg vacuum and temperatures up to 100° C. The resulting reaction product was sec-butylated m-xylylenediamine, the composition as determined by gas chromatography is shown in the table below and is represented by the structure below. [ka]
[0069] Product composition: [Table 5]
[0070] Example 9. Synthesis of sec-butylated 4,4'-diaminodicyclohexylmethane, molar ratio 1.0 / 1.0 (MEK:PACM) The synthesis of N-sec-butyl-4,4'-diaminodicyclohexylmethane is a one-batch process. 446.6 g (2.13 mol) of 4,4'-diaminodicyclohexylmethane and 153.4 g (2.13 mol) of 2-butanone were charged into a 1 L autoclave batch reactor with 3.40 g of 5% sulfided platinum on carbon catalyst. The reactor was sealed and then purged with nitrogen and then hydrogen to remove all air from the reactor. The reactor was pressurized to 27.2 atm (400 psig) with hydrogen and the reactor was heated to 140°C. The pressure had increased to 54.4 atm (800 psig) when the rate of hydrogen uptake slowed. The hydrogenation process was continued until the rate of hydrogen uptake dropped below 0.0007 MPa / min (0.1 psi / min). The reactor was cooled to ambient temperature and depressurized, and the reaction product was filtered to remove the catalyst. Water was removed using a rotary evaporator operating under 40 mm Hg vacuum and temperatures up to 100° C. The resulting reaction product was sec-butylated 4,4′-diaminodicyclohexylmethane, the composition of which, as determined by gas chromatography, is shown in the table below and is represented by the structure below. [ka]
[0071] Product composition: [Table 6]
[0072] These examples are provided to demonstrate certain aspects of the invention and are not intended to limit the scope of the claims appended hereto.
[0073] Example 10. This example describes the preparation and testing of an alkylated IPD hardener with an epoxy resin.
[0074] Table 1 [Table 7]
[0075] A comparison of commercial cycloaliphatic amines, such as IPD (formulation 1), with the mono- and di-alkylated products of the present invention (formulations 2-4) is reported in Table 1. The neat viscosity of the alkylated isophorone diamine (AIPD) products remains extremely low. It is desirable for the curing agent to have a low viscosity that helps to reduce the total epoxy formulation viscosity for composite applications. The gel time of the alkylated isophorone diamine (AIPD) products with IPD:MEK ratio (1:0.5) doubled, and the IPD:MEK ratio (1:1) increased by almost 5 times at 25°C. This is sufficient time and viscosity to uniformly process relatively large and relatively thick composite parts.
[0076] The reactivity of the alkylated isophorone diamine (AIPD) products with epoxy resins maintained desirable physical, thermal and chemical properties for composite applications.
[0077] The hardener was used to mix with epoxy resin (epoxy equivalent weight (EEW) 180) in various stoichiometric ratios as shown in Table 1. The liquid epoxy resin (LER) (EEW 180) was EPON (登録商標) The number is 826. (登録商標) is a registered trademark of Hexion Specialty Chemicals, Inc.
[0078] The viscosity of all the formulations shown in Table 1 was measured at 25° C. and 40° C. using a Brookfield Viscometer RV with spindle number 27. 12 g of the epoxy resin composition was used to measure the viscosity.
[0079] TECHNE (登録商標) A gel timer was used to measure the gel time of all the formulations shown in Table 1. In the industry, gel time is sometimes also equivalent to pot life. One end of the metal rod was attached to the TECHNE (登録商標)It is connected to a gel timer and the other end has a 1" diameter disk. The epoxy resin and hardener were preheated separately at 25°C. A total of 150g of mixture (epoxy resin and hardener) was mixed for 3-5 minutes. The 1" diameter disk was immersed into the mixture of beaker contents and the gel timer was switched on, giving an immediate accurate reading.
[0080] The results of Formulations 1-4 are reported in Table 1. Formulation 1 is used as a control sample according to the present disclosure and provides an initial mix viscosity of about 319 cP. Formulations 2 and 3 show initial mix viscosities of about 313 cP and 206 cP, respectively. The lower mix viscosity enhances fiber wetting in thick composite sections under pressure due to improved resin penetration between the fabric layers. Formulation 1 provides a Tg in the range of 140°C to 155°C, and Formulations 2 and 3 provide a Tg in the range of 130°C to 150°C. The alkylated isophorone diamine (AIPD) maintains the Tg range relative to non-alkylated IPD while improving the gel time by 2-5 times over the control formulation (IPD).
[0081] Table 2 [Table 8]
[0082] The handling properties results of the alkylated IPD with CHONE and isophorone at two different ratios are reported in Table 2 (formulations 5-8). The neat viscosity of the alkylated product remains extremely low. It is desirable for the curing agent to have a low viscosity that helps to reduce the total epoxy formulation viscosity for composite applications. The reactivity of both alkylated products is significantly slowed. This feature provides sufficient time and viscosity to uniformly process relatively large and relatively thick composite parts.
[0083] Example 11 This example describes the testing of a cured epoxy resin formulation.
[0084] Table 3 [Table 9]
[0085] The epoxy resins and amine hardeners shown in Table 3 were mixed by hand at 40°C for 3-5 minutes. Entrapped air was removed by placing the mixture in a centrifuge for 5 minutes or until the mixture was clear. The mixture was then poured into 1 / 8" aluminum molds. The system in the mold was cured at 60°C for 1 hour and at 150°C for 2 hours. The mold was cooled to room temperature before removing the cured samples. Test specimens were prepared from the cast samples according to ASTM methods for mechanical testing; tensile (ASTM D638), flexural (ASTM D790), and compression (ASTM D695). Additional 1" x 3" x 1 / 8" specimens were prepared for chemical resistance testing in different reagents (Table 4).
[0086] Example 12 This example describes the testing of a cured epoxy resin formulation after chemical soaking.
[0087] Table 4 [Table 10]
[0088] Neat cast panels of Formulations 1-3 were manufactured using the process described in Example 11. Flexural specimens (1 / 2" x 3" x 1 / 8") were machined according to ASTM D790. The specimens were immersed in different reagents at 40°C for 30 days to understand the flexural modulus retention before and after immersion. The reagents used were: deionized water, methanol, 10% ammonium hydroxide, and 10% nitric acid. The flexural modulus of Formulations 2 and 3 was retained in most of the reagents.
[0089] Example 13 This example describes the processing and thermal properties of the alkylation products of different cycloaliphatic amines.
[0090] Table 5 [Table 11]
[0091] A comparison of commercial amines such as IPD, MXDA, PACM and DMPACM (formulations 1, 9, 11, 13) with the monoalkylated products of these amines of the present invention (formulations 3, 10, 12, 14) is reported in Table 5. The neat viscosity of the alkylated products remains extremely low. It is desirable for the curing agent to have a low viscosity that helps to reduce the total epoxy formulation viscosity for composite applications. The gel time of the alkylated products (formulations 3, 10, 12 and 14) increased by almost 5 times at 25°C. This is sufficient time and viscosity to uniformly process relatively large and relatively thick composite parts.
[0092] Preferred embodiments of the present invention are as follows: 1. An epoxy resin and a copolymer of formula (I) [ka] [Wherein, Z is cyclohexyl, C 1 ~C 10 Alkyl-substituted cyclohexyl, phenyl, C 1 ~C 10 Alkyl-substituted phenyl, methylenebis(cyclohexyl) and C 1 ~C 10 alkyl-substituted methylenebis(cyclohexyl), a and b are independently 0 or 1, and Y is selected from the group consisting of C 1 ~C 10 and a monoalkylated diamine of the formula [alkyl]. 2. The monoalkylated diamine has the structure: [ka] [In the formula, R 1 , R 2 , R3 , R 4 , R 5 , and R 6 Each of these is H, CH 3 , or C 2 ~C 4 is an alkyl group; n is 0 or 1; and A is H and B is C 1 ~C 10 or B is H and A is C 1 ~C 10 Epoxy resin system according to claim 1, represented by the formula: 3. The monoalkylated diamine is i) Structure: [ka] [Wherein, A is C 1 ~C 10 monoalkylated isophorone diamines represented by the formula: ii) Structure: [ka] [In the formula, B is C 1 ~C 10 monoalkylated isophorone diamines represented by the formula: iii) Structure: [ka] [Wherein, A is C 1 ~C 10 monoalkylated methylcyclohexyldiamine represented by the formula: iv) Structure: [ka] [In the formula, B is C 1 ~C 10 wherein R is an alkyl group; and v) Structure: [ka] [Wherein, A is C 1 ~C 10 The monoalkylated cyclohexyldiamine represented by the formula: Epoxy resin system according to claim 2, selected from the group consisting of: 4. The monoalkylated diamine has the structure: [ka] [In the formula, R 1 and R 2 Each of 3 and A is C 1 ~C 10 Epoxy resin system according to claim 1, represented by the formula: 5. The monoalkylated diamine is i) Structure: [ka] [Wherein, A is C 1 ~C 10 monoalkylated 4,4'-methylenebis(cyclohexylamine), ii) Structure: [ka] [Wherein, A is C 1 ~C 10 Monoalkylated 2,2'-dimethyl-4,4'-methylenebis(cyclohexylamine) represented by the formula: 5. The epoxy resin system according to claim 4, selected from the group consisting of: 6. The monoalkylated diamine has the structure: [ka] [wherein X is a phenyl group or a cyclohexyl group; and A is C 1 ~C 10 Epoxy resin system according to claim 1, represented by the formula: 7. The monoalkylated diamine is i) Structure: [ka] [Wherein, A is C 1 ~C 10 wherein m-xylylenediamine is an alkyl group; and ii) Structure: [ka] [Wherein, A is C 1 ~C 10 Monoalkylated 1,3-bisaminomethylcyclohexane represented by the formula: 7. The epoxy resin system according to claim 6, selected from the group consisting of: 8. The epoxy resin system according to claim 1, wherein the epoxy resin system comprises at least 20% by weight of the monoalkylated diamine, based on the total weight of the curing agent. 9. The epoxy resin system of claim 1, further comprising a second amine selected from the group consisting of primary amines and secondary amines. 10. The epoxy resin system according to claim 9, wherein the second amine component comprises one or more amine compounds selected from the group consisting of polyetheramines, polyetherpolyamines, saturated aliphatic cyclic diamines, linear aliphatic amines, cyclic aliphatic amines, polycyclic aliphatic amines and aromatic amines. 11. The epoxy resin system of claim 1, wherein the epoxy resin component comprises at least one glycidyl ether selected from the group of glycidyl ethers of resorcinol, hydroquinone, bis-(4-hydroxy-3,5-difluorophenyl)-methane, 1,1-bis-(4-hydroxyphenyl)-ethane, 2,2-bis-(4-hydroxy-3-methylphenyl)-propane, 2,2-bis-(4-hydroxy-3,5-dichlorophenyl)propane, 2,2-bis-(4-hydroxyphenyl)-propane, bis-(4-hydroxyphenyl)-methane, and any combination thereof. 12. The epoxy resin component has the following structure: [ka] Epoxy resin system according to 1 above, comprising at least one dihydric phenol of the formula: [wherein m is 0 to 25 and R is a divalent hydrocarbon group]. 13. The epoxy resin component is selected from the group consisting of bis(3,4-epoxycyclohexylmethyl)oxalate, bis(3,4-epoxycyclohexylmethyl)adipate, bis(3,4-epoxy-6-methylcyclohexylmethyl)adipate, vinylcyclohexene diepoxide; limonene diepoxide; bis(3,4-epoxycyclohexylmethyl)pimelate; dicyclopentadiene diepoxide; 3,3-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, 3,4-epoxycyclohexylmethyl-3,4- 2. The epoxy resin system of claim 1, comprising at least one selected from the group consisting of epoxy cyclohexane carboxylate; 3,3-epoxy-1-methylcyclohexyl-methyl-3,4-epoxy-1-methylcyclohexane carboxylate; 6-methyl-3,4-epoxycyclohexylmethyl-6-methyl-3,4-epoxycyclohexane carboxylate; 3,4-epoxy-2-methylcyclohexyl-methyl-3,4-epoxy-3-methylcyclohexane carboxylate, and combinations thereof. 14. A method for producing an epoxy resin system according to any one of 1 to 13 above, comprising: [ka] [Wherein, Z is cyclohexyl, C 1 ~C 4 Alkyl-substituted cyclohexyl, phenyl, C 1 ~C 4 Alkyl-substituted phenyl, methylenebis(cyclohexyl), and C 1 ~C 4 alkyl-substituted methylenebis(cyclohexyl), a and b are independently 0 or 1, and Y is selected from the group consisting of C 1 ~C 10and optionally other ingredients. 15. Use of an epoxy resin system according to any of 1 to 14 above for producing structural or electrical laminates, coatings, castings, structural components, circuit boards, electrical varnishes, encapsulants, semiconductors, general purpose molding powders, filament wound pipe and fittings, filament wound pressure vessels, low and high pressure pipe and fittings, low and high pressure vessels, storage tanks, wind turbine blades, automotive structural parts, aerospace structural parts, oil and gas buoyancy modules, rigs, well plugs, cured in place pipe (CIPP), structural adhesives and laminates, composite liners, pump liners, corrosion resistant coatings or composites based on reinforced fibre substrates. 16. Compounds of formula (I) as hardeners for epoxy resins [ka] [Wherein, Z is cyclohexyl, C 1 ~C 4 Alkyl-substituted cyclohexyl, phenyl, C 1 ~C 4 Alkyl-substituted phenyl, methylenebis(cyclohexyl), and C 1 ~C 4 alkyl-substituted methylenebis(cyclohexyl), a and b are independently 0 or 1, and Y is selected from the group consisting of C 1 ~C 10 The use of monoalkylated diamines in which the diamine is alkyl.
Claims
1. An epoxy resin and a copolymer of formula (I) 【Chemistry 1】 [Wherein Z is cyclohexyl, C 1 ~C 10 Alkyl-substituted cyclohexyl, phenyl, C 1 ~C 10 Alkyl-substituted phenyl, methylenebis(cyclohexyl) and C 1 ~C 10 alkyl-substituted methylenebis(cyclohexyl), a and b are independently 0 or 1, and Y is selected from the group consisting of C 1 ~C 10 and a monoalkylated diamine of the formula [alkyl].
2. The monoalkylated diamine has the structure: 【Chemistry 2】 [In the formula, R 1 , R 2 , R 3 , R 4 , R 5 , and R 6 are H, CH 3 , or C 2 ~C 4 n is 0 or 1; and A is H and B is C 1 ~C 10 alkyl or B is H and A is C 1 ~C 10 2. The epoxy resin system of claim 1, wherein:
3. The monoalkylated diamine is i) Structure: 【Chemistry 3】 [Wherein A is C 1 ~C 10 a monoalkylated isophorone diamine represented by the formula: ii) Structure: 【Chemistry 4】 [In the formula, B is C 1 ~C 10 a monoalkylated isophorone diamine represented by the formula: iii) Structure: 【Chemistry 5】 [Wherein A is C 1 ~C 10 a monoalkylated methylcyclohexyldiamine represented by the formula: iv) Structure: 【Chemistry 6】 [In the formula, B is C 1 ~C 10 wherein R is an alkyl group; and v) Structure: 【Chemistry 7】 [Wherein A is C 1 ~C 10 wherein the alkyl is an alkyl group.
3. The epoxy resin system of claim 2, selected from the group consisting of:
4. The monoalkylated diamine has the structure: 【Chemistry 8】 [In the formula, R 1 and R 2 Each of 3 and A is C 1 ~C 10 2. The epoxy resin system of claim 1, wherein:
5. The monoalkylated diamine is i) Structure: 【Chemistry 9】 [Wherein A is C 1 ~C 10 wherein R is an alkyl group; and ii) Structure: 【Chemistry 10】 [Wherein A is C 1 ~C 10 monoalkylated 2,2'-dimethyl-4,4'-methylenebis(cyclohexylamine) represented by the formula:
5. The epoxy resin system of claim 4, selected from the group consisting of:
6. The monoalkylated diamine has the structure: 【Chemistry 11】 wherein X is a phenyl group or a cyclohexyl group; and A is C 1 ~C 10 2. The epoxy resin system of claim 1, wherein:
7. The monoalkylated diamine is i) Structure: 【Chemistry 12】 [Wherein A is C 1 ~C 10 and a monoalkylated m-xylylenediamine represented by the formula: ii) Structure: 【Chemistry 13】 [Wherein A is C 1 ~C 10 The monoalkylated 1,3-bisaminomethylcyclohexane represented by the formula:
7. The epoxy resin system of claim 6, selected from the group consisting of:
8. 2. The epoxy resin system of claim 1, wherein the epoxy resin system comprises at least 20 weight percent of the monoalkylated diamine, based on the total weight of the curing agent.
9. 2. The epoxy resin system of claim 1, wherein the epoxy resin system further comprises a second amine selected from the group consisting of primary amines and secondary amines.
10. 10. The epoxy resin system of claim 9, wherein the second amine component comprises one or more amine compounds selected from the group consisting of polyetheramines, polyetherpolyamines, saturated aliphatic cyclic diamines, linear aliphatic amines, cycloaliphatic amines, polycyclic aliphatic amines, and aromatic amines.
11. 2. The epoxy resin system of claim 1, wherein the epoxy resin component comprises at least one glycidyl ether selected from the group of glycidyl ethers of resorcinol, hydroquinone, bis-(4-hydroxy-3,5-difluorophenyl)-methane, 1,1-bis-(4-hydroxyphenyl)-ethane, 2,2-bis-(4-hydroxy-3-methylphenyl)-propane, 2,2-bis-(4-hydroxy-3,5-dichlorophenyl)propane, 2,2-bis-(4-hydroxyphenyl)-propane, bis-(4-hydroxyphenyl)-methane, and any combination thereof.
12. The epoxy resin component has the following structure: 【Chemistry 14】 2. The epoxy resin system of claim 1, comprising at least one dihydric phenol of the formula: wherein m is 0 to 25 and R is a divalent hydrocarbon group.
13. The epoxy resin component is selected from the group consisting of bis(3,4-epoxycyclohexylmethyl)oxalate, bis(3,4-epoxycyclohexylmethyl)adipate, bis(3,4-epoxy-6-methylcyclohexylmethyl)adipate, vinylcyclohexene diepoxide; limonene diepoxide; bis(3,4-epoxycyclohexylmethyl)pimelate; dicyclopentadiene diepoxide; 3,3-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, 3,4-epoxycyclohexylmethyl-3,4-ethylenediaminetetraacetate ...
2. The epoxy resin system of claim 1, comprising at least one selected from the group consisting of: 3,3-epoxy-1-methylcyclohexyl-methyl-3,4-epoxy-1-methylcyclohexanecarboxylate; 6-methyl-3,4-epoxycyclohexylmethyl-6-methyl-3,4-epoxycyclohexanecarboxylate; 3,4-epoxy-2-methylcyclohexyl-methyl-3,4-epoxy-3-methylcyclohexanecarboxylate, and combinations thereof.
14. A method for producing an epoxy resin system according to any one of claims 1 to 13, comprising the step of: 【Chemistry 15】 [Wherein Z is cyclohexyl, C 1 ~C 4 Alkyl-substituted cyclohexyl, phenyl, C 1 ~C 4 Alkyl-substituted phenyl, methylenebis(cyclohexyl), and C 1 ~C 4 alkyl-substituted methylenebis(cyclohexyl), a and b are independently 0 or 1, and Y is selected from the group consisting of C 1 ~C 10 and optionally other ingredients.
15. 15. Use of the epoxy resin system according to any of claims 1 to 13 or obtained by the method according to claim 14 for producing structural or electrical laminates, coatings, castings, structural components, circuit boards, electrical varnishes, encapsulants, semiconductors, general purpose molding powders, filament wound pipes and fittings, filament wound pressure vessels, low and high pressure pipes and fittings, low and high pressure vessels, storage tanks, wind turbine blades, automotive structural parts, aerospace structural parts, oil and gas buoyancy modules, rigs, well plugs, cured in place pipes (CIPP), structural adhesives and laminates, composite liners, pump liners, corrosion resistant coatings or composites based on reinforcing fibre substrates.
16. As hardeners for epoxy resins, 【Chemistry 16】 [Wherein Z is cyclohexyl, C 1 ~C 4 Alkyl-substituted cyclohexyl, phenyl, C 1 ~C 4 Alkyl-substituted phenyl, methylenebis(cyclohexyl), and C 1 ~C 4 alkyl-substituted methylenebis(cyclohexyl), a and b are independently 0 or 1, and Y is selected from the group consisting of C 1 ~C 10 The use of monoalkylated diamines in which the diamine is an alkyl group.
Citation Information
Patent Citations
New cyclohexylamine compounds useful for the preparation of a hardened product, preferably epoxide resin, which is useful e.g. in electrical equipments and for manufacturing rotor blades for wind turbines
DE102011113395A1
Modified cycloaliphatic polyamine
JP2004115427A
Compositions of epoxides and polycarboxylic acid compounds
US2890194A
Nitrogen containing compounds and compositions
US4293682A
Secondary aliphatic diamines as curing agents for polyurethanes and polyureas prepared using high-pressure impingement mixing
US6403752B1