Digital printing process

A silicone-based ITM with a hydrophilic release layer and specialized aqueous treatment formulation addresses the challenges of ink transfer, resulting in improved image quality and mechanical integrity during digital printing.

JP2024156784AInactive Publication Date: 2024-11-06LANDA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024123121
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2016-05-30
Filing Date
2024-07-30
Publication Date
2024-11-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing digital printing processes face challenges in achieving high-quality ink transfer and image quality due to issues with hydrophobic surfaces on intermediate transfer members (ITMs), leading to non-uniformity and loss of mechanical integrity during the transfer process.

Method used

The use of a silicone-based release layer with specific hydrophilic properties, combined with an aqueous treatment formulation containing quaternary ammonium salts and water-soluble polymers, to create a thin, cohesive, and continuous dry film on the ITM, allowing for efficient ink deposition and transfer onto substrates.

Benefits of technology

This approach results in improved ink dot quality, uniformity, and mechanical integrity of the transferred image, enhancing the overall printing process by ensuring consistent and high-quality ink transfer at high speeds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024156784000001_ABST
    Figure 2024156784000001_ABST
Patent Text Reader

Abstract

To provide improved printing processes, improved ITM (or portions thereof) and improved compositions used for pre-treating the ITM before deposition of droplets of aqueous ink.SOLUTION: An aqueous treatment composition for an ITM (intermediate transfer member) of a printing system, and a printing method including a step of applying the treatment composition to the surface of the ITM are disclosed. The treatment composition comprises at least 3 wt.% of a quaternary ammonium salt, at least 1 wt.% of a water-soluble polymer, and at least 65 wt.% of water. An ITM, and a treatment station for forming a thin layer of liquid treatment formulation on the ITM surface are also disclosed.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This disclosure claims priority to U.S. Patent Application Serial No. 62 / 343,123, filed May 30, 2016, and U.S. Patent Application Serial No. 62 / 343,108, filed May 30, 2016, which are incorporated by reference in their entireties.

[0002] The present disclosure relates to digital printing processes, aqueous treatment formulations, and related kits and systems. [Background technology]

[0003] The following patent publications provide potentially relevant background material, all of which are incorporated by reference in their entireties: WO / 2017 / 009722 (publication of PCT / IB2016 / 053049 filed on May 25, 2016), WO / 2016 / 166690 (publication of PCT / IB2016 / 052120 filed on April 4, 2016); WO / 2016 / 151462 (publication of PCT / IB2016 / 051560 filed on March 20, 2016), WO / 2016 / 113698 (publication of PCT / IB2016 / 050170 filed on January 14, 2016), WO / 2015 / 110988 (publication of PCT / IB2015 / 050501 filed on January 22, 2015), WO / 2015 / 036812 (publication of PCT / IB2013 / 002571 filed on September 12, 2013), WO / 2015 / 036864 (publication of PCT / IB2014 / 002366 filed on September 11, 2014), WO / 2015 / 036865 (publication of PCT / IB2014 / 002395 filed on September 11, 2014), WO / 2015 / 036906 (publication of PCT / IB2014 / 064277 filed on September 12, 2014), WO / 2013 / 136220 (publication of PCT / IB2013 / 051719 filed March 5, 2013); WO / 2013 / 132419 (publication of PCT / IB2013 / 051717 filed March 5, 2013), WO / 2013 / 132424 (publication of PCT / IB2013 / 051727 filed March 5, 2013), WO / 2013 / 132420 (publication of PCT / IB2013 / 051718 filed March 5, 2013), WO / 2013 / 132439 (publication of PCT / IB2013 / 051755 filed March 5, 2013), WO / 2013 / 132438 (publication of PCT / IB2013 / 051751 filed March 5, 2013), WO / 2013 / 132418 (publication of PCT / IB2013 / 051716 filed on March 5, 2013), WO / 2013 / 132356 (publication of PCT / IB2013 / 050245 filed on January 10, 2013), WO / 2013 / 132345 (publication of PCT / IB2013 / 000840 filed March 5, 2013), WO / 2013 / 132339 (publication of PCT / IB2013 / 000757 filed March 5, 2013), WO / 2013 / 132343 (publication of PCT / IB2013 / 000822 filed on March 5, 2013), WO / 2013 / 132340 (publication of PCT / IB2013 / 000782 filed March 5, 2013), WO / 2013 / 132432 (publication of PCT / IB2013 / 051743 filed on March 5, 2013).

[0004] FIG. 1 is a flow chart of a conventional printing process in which an intermediate transfer member (ITM) is pretreated before an ink image is deposited on the ITM. In step S1, a treatment solution is applied to the surface of a hydrophobic ITM to pretreat the ITM surface. In step S9, droplets of a water-based ink are inkjetted onto the pretreated ITM surface, thereby forming an ink image. In step S13, the ink image is dried on the ITM surface. In step S17, the dried ink image is transferred onto a substrate.

[0005] Various embodiments of the present invention relate to improved printing processes, to improved ITMs (or portions of ITMs), and to improved compositions used to pre-treat ITMs prior to depositing droplets of water-based ink. Summary of the Invention

[0006] Various aspects of the present invention include: a. providing an intermediate transfer member (ITM) comprising a silicone-based release layer surface that exhibits sufficient hydrophilicity to satisfy at least one of the following properties: (i) a receding contact angle of a distilled water droplet deposited on the silicone-based release layer surface of at most 60 degrees; and (ii) a 10 second dynamic contact angle (DCA) of a distilled water droplet deposited on the silicone-based release layer surface of at most 108 degrees; and b. providing an aqueous treatment formulation comprising at least 3% by weight of a quaternary ammonium salt having a water solubility of at least 5% at 25 degrees Celsius; ii. at least 1% by weight of at least one water soluble polymer having a water solubility of at least 5% at 25 degrees Celsius; and iii. a carrier liquid comprising water, the water comprising at least 65% by weight of the aqueous treatment formulation, the carrier liquid comprising: i. a receding contact angle of a distilled water droplet deposited on the silicone-based release layer surface of at most 60 degrees; and ii. a static surface tension in the range of 20-40 dynes / cm; ii. a 25 degree Celsius viscosity coefficient of at least 10 cP; and iii. a 60 degree Celsius evaporation load of up to 8:1 by weight; c. applying the aqueous treatment formulation to a silicone based release layer surface of an ITM to form a wet treatment layer on said silicone based release layer surface having a thickness of up to 0.8 μm; d. subjecting the wet treatment layer to a drying process to form a dry treatment film on the silicone based release layer surface from the wet treatment layer; e. depositing droplets of an aqueous ink on the dry treatment film to form an ink image on the release layer surface of the silicone based release layer surface; f. drying the ink image to leave a residual ink image on the silicone based release layer surface; and g. transferring the residual ink image onto the printing substrate by pressurized contact between the ITM and the printing substrate.

[0007] Various aspects of the present invention include: a. providing an intermediate transfer member (ITM) comprising a silicone-based release layer surface exhibiting sufficient hydrophilicity to satisfy at least one of the following characteristics: (i) a receding contact angle of a distilled water droplet deposited on the silicone-based release layer surface of at most 60 degrees; and (ii) a 10 second dynamic contact angle (DCA) of a distilled water droplet deposited on the silicone-based release layer surface of at most 108 degrees; and b. providing an aqueous treatment formulation comprising: at least 3% by weight of a quaternary ammonium salt having a water solubility of at least 5% at 25 degrees Celsius; ii. at least 1% by weight of at least one water soluble polymer having a water solubility of at least 5% at 25 degrees Celsius; and iii. a carrier liquid comprising water, wherein the water comprises at least 65% by weight of the aqueous treatment formulation; providing an aqueous treatment formulation having a static surface tension at 25 degrees Celsius in the range of 20-40 dynes / cm; ii. a 25 degrees Celsius viscosity coefficient of at least 10 cP; and iii. a 60 degrees Celsius evaporation load of up to 8:1 by weight; c. applying the aqueous treatment formulation to a silicone based release layer surface of an ITM to form a wet treatment layer on the silicone based release layer surface; d. subjecting the wet treatment layer to a drying process to form a dry treatment film on the silicone based release layer surface from the wet treatment layer; e. depositing droplets of an aqueous ink on the dry treatment film to form an ink image on the release layer surface of the silicone based release layer surface; f. allowing the ink image to dry to leave a residual ink image on the silicone based release layer surface; and g. transferring the residual ink image onto the 60 degree substrate by pressurized contact between the ITM and the print substrate.

[0008] In some embodiments, the 60 degree Celsius evaporation loading of provided aqueous treatment formulations is at most 6:1, at most 5:1, at most 4:1, at most 3.5:1, or at most 3:1, and optionally at least 2:1, at least 2.2:1, or at least 2.5:1.

[0009] In some embodiments, the concentration of the quaternary ammonium salt in the provided aqueous treatment formulation is in the range of 3-15%, the concentration of the water soluble polymer is in the range of 2.5-10% or 2.5-8%, the 60° C. evaporation loading is in the range of 2.5:1 to 4:1, and the viscosity is at least 12 cP, optionally at least 14 cP or at least 16 cP.

[0010] In some embodiments, the provided aqueous treatment formulations have a total surfactant concentration in the range of at least 6%, at least 7%, at least 8%, at least 9%, or at least 10%, and optionally 6-40%, 6-30%, 6-20%, 7-30%, 7-20%, 7-15%, 8-25%, 8-20%, 8-15%, or 8-13%.

[0011] In some embodiments, the total concentration of organic solvents in the provided aqueous treatment formulation is at most 3 wt%, at most 2 wt%, at most 1 wt%, or at most 0.5 wt%, or the formulation is free of organic solvents.

[0012] In some embodiments, the concentration of the liquid moisture absorbent in the provided aqueous treatment formulation is at most 1.5 wt%, at most 1 wt%, at most 0.5 wt%, at most 0.3 wt%, or at most 0.1 wt%, or the aqueous treatment formulation is free of any liquid moisture absorbent.

[0013] In some embodiments, the quaternary ammonium salt in the provided aqueous treatment formulation is an organic quaternary ammonium salt.

[0014] In some embodiments, the first carbon chain of the organic quaternary ammonium salt has a length of at least 6 carbon atoms, and optionally a length in the range of 6 to 20, 6 to 18, 8 to 20, or 8 to 18 carbon atoms.

[0015] In some embodiments, the second carbon chain of the organic quaternary ammonium salt has a length of up to 3 carbon atoms, or up to 2 carbon atoms.

[0016] In some embodiments, the third carbon chain of the organic quaternary ammonium salt has a length of up to 3 carbon atoms, up to 2 carbon atoms, or up to 1 carbon atom.

[0017] In some embodiments, the organic quaternary ammonium salt is a cationic organic quaternary ammonium salt, optionally having a sulfate or phosphate anion.

[0018] In some embodiments, the silicone-based release layer surface exhibits sufficient hydrophilicity to satisfy at least one of the following characteristics: a receding contact angle of a distilled water droplet deposited on the silicone-based release layer surface is at most 60 degrees.

[0019] In some embodiments, the silicone-based release layer surface exhibits sufficient hydrophilicity to satisfy at least one of the following characteristics: a 10 second dynamic contact angle (DCA) of a distilled water droplet deposited on the silicone-based release layer surface is at most 108 degrees.

[0020] In some embodiments, an ITM is provided that includes a support layer, a release layer having a silicone-based release layer surface, and a second surface (i) opposite the silicone-based release layer surface and (ii) attached to the support structure, where the release layer is formed of an addition-curable silicone material, and the thickness of the release layer is up to 500 micrometers (μm).

[0021] In some embodiments, the release layer of the provided ITM consists essentially of, or comprises at least 95% by weight, addition cure silicone.

[0022] In some embodiments, the functional groups within the silicone-based release layer surface of a provided ITM comprise up to 3% by weight of the addition-curable silicone material.

[0023] In some embodiments, a polyether glycol functionalized polydimethylsiloxane is loaded into the addition cured silicone material of a provided ITM.

[0024] In some embodiments, the release layer of the provided ITM is adapted such that the polar groups of the ink-receptive surface are oriented away from or against the second surface.

[0025] In some embodiments, the surface hydrophobicity of the silicone-based release layer surface of the provided ITM is less than the bulk hydrophobicity of the cured silicone material in the release layer, where the surface hydrophobicity is characterized by the receding contact angle of a distilled water droplet on the ink-receptive surface and the bulk hydrophobicity is characterized by the receding contact angle of a distilled water droplet deposited on an inner surface formed by exposing an area of ​​the cured silicone material in the release layer to form an exposed area.

[0026] In some embodiments, the aqueous treatment formulation is applied to the surface of the silicone-based release layer to provide a wet treatment layer thickness of up to 0.5 μm, or up to 0.4 μm.

[0027] In some embodiments, the wet treatment layer is formed and / or thinned by forcing a rounded surface towards or away from the ITM, where i. the rounded surface has a radius of curvature of at most 2 mm, or at most 1.5 mm, or at most 1.25 mm, or at most 1 mm, and / or ii. the forcing is performed with a force density in the cross print direction of at least 250 g / cm, or at least 350 g / cm, or at least 400 gm / cm, and / or at most 1 kg / cm, or at most 750 g / cm, or at most 600 g / cm, and / or iii. the forcing is performed by applying pressure between the ITM, the magnitude of the pressure being at least 0.1 bar, or at least 0.25 bar, or at least 0.35 bar, or at least 0.5 bar, and optionally at most 2 bar, or at most 1.5 bar, or at most 1 bar.

[0028] In some embodiments, the wet treatment layer is formed and / or thinned by a stationary applicator and / or rounded surface that directly or indirectly applies a force to the moving ITM, thereby (i) deforming the ITM and creating a depression in the ITM, and (ii) establishing a velocity gradient of the flowing aqueous treatment formulation that is perpendicular to the ITM and formed in the gap region between the ITM and the stationary applicator.

[0029] In some embodiments, the magnitude of the velocity gradient is at least 10 6 / sec or at least 2×10 6 / second.

[0030] In some embodiments, the aqueous treatment formulation is applied to at least a portion or portions of the moving ITM at a speed of at least 1 meter / sec, or at least 1.5 meters / sec, or at least 2 meters / sec to form a wet treatment layer thereon.

[0031] In some embodiments, forming the wetting treatment layer or thinning the wetting treatment layer comprises establishing a velocity gradient perpendicular to the ITM, the magnitude of the velocity gradient being at least 10 6 / sec or at least 2×10 6 The method includes forcing the aqueous treatment formulation to flow for 100 s / sec.

[0032] In some embodiments, the release surface of the ITM has a Shore A hardness of at most 50, or at most 45, or at most 40, or at most 35, or at most 30, or at most 25, or at most 20, or at most 15.

[0033] In some embodiments, the drying process of the wet treatment layer is carried out rapidly enough that the viscosity of the aqueous treatment formulation increases quickly enough that surface tension induced beading is inhibited and the dried treatment film has a smooth upper surface.

[0034] In some embodiments, the smooth upper surface of the dried treated film has an average roughness R of at most 12 nanometers, or at most 10 nanometers, or at most 9 nanometers, or at most 8 nanometers, or at most 7 nanometers, or at most 5 nanometers. a It is characterized by:

[0035] In some embodiments, drying of the treatment solution is rapid enough to prevent beading and leave behind a continuous hydrophilic and cohesive polymer treatment film having a thickness of at most 200 nm, or at most 150 nm, or at most 120 nm, or at most 100 nm, or at most 80 nm, or at most 70 nm, or at most 60 nm, or at most 50 nm, or at most 40 nm, or at most 30 nm.

[0036] In some embodiments, the dried film onto which the aqueous ink droplets are deposited has a thickness of at most 200 nm, or at most 120 nm, or at most 100 nm, or at most 80 nm.

[0037] In some embodiments, the dried film onto which the aqueous ink droplets are deposited has a thickness of at least 15 nm, or at least 20 nm, or at least 30 nm.

[0038] In some embodiments, the dry treatment film is continuous across a rectangle of the release surface of the ITM, the rectangle having a width of at least 10 cm and a length of at least 10 meters.

[0039] In some embodiments, for at least 50%, or at least 75%, or at least 90%, or at least 95%, or at least 95%, or at least 99%, or 100% of the area of ​​the rectangle, the thickness of the dried processed film does not deviate from the average thickness value within the rectangle by more than 50%, or 40%, or 30%.

[0040] In some embodiments, during the drying process of the wet processing layer, the dynamic viscosity of the wet processing layer increases by at least 1000 times within a period of up to 250 milliseconds.

[0041] In some embodiments, the liquid content of the dried process film is up to 10% w / w, or up to 7.5% w / w, or up to 5% w / w, or up to 2.5% w / w, or up to 1.5% w / w, or up to 1% w / w.

[0042] In some embodiments, droplets of the water-based ink are deposited by inkjet onto the dried treated film.

[0043] In some embodiments, the residual ink image, along with the non-printed areas of the dried treatment film, is transferred onto the print substrate.

[0044] In some embodiments, the dried film thickness is up to 120 nm.

[0045] In some embodiments, the dry treatment film has sufficient cohesion such that during transfer of the residual ink image, the dry treatment film completely separates from the ITM in both printed and non-printed areas and is transferred to the printing substrate along with the dry ink image.

[0046] In some embodiments, the transfer of the residual ink image occurs at a transfer temperature of up to 100 degrees Celsius or up to 90 degrees Celsius.

[0047] In some embodiments, the solids of the water-based ink (e.g., nanopigments and / or resins) flow into the bulk of the dried processing film and react (e.g., bond) with quaternary ammonium salts present in the dried processing film (thereby, for example, facilitating droplet spreading).

[0048] In some embodiments, the solids of the water-based ink flow into the bulk of the dried process film and react with the quaternary ammonium salts present in the dried process film, thereby facilitating the spreading of the droplets.

[0049] In some embodiments, the method includes: i. forming an ink dot set IDS of ink dots present on the ink substrate; ii. forming an ink dot set IDS of ink dots present on the ink substrate such that a correspondence exists between A. each given droplet of the droplet plurality DP and B. an ink dot present on a given substrate of each of the ink dot sets, such that a droplet of the aqueous ink droplets deposited on a dried processing film present on the ITM gives rise to and / or evolves into an ink dot present on the given substrate; iii. during deposition, whenever a droplet of the droplet plurality impacts with a dried processing film on the ITM, the kinetic energy of the impacting droplet transforms the droplet; and iv. a maximum impact radius of each of the deformed droplets above a surface of the ITM is greater than or equal to a maximum impact radius value R. MAX_IMPACT and v. after the collision, each ink dot of the ink dot set IDS present on the substrate has a dry dot radius R DRIED_DOT_ON_SUBSTRATE vi. for each droplet of the droplet plurality and corresponding ink dot of the ink dot set IDS, A. a dried dot radius R present on the substrate; DRIED_DOT_ON_SUBSTRATE and B. the deformed droplet maximum impact radius value R MAX_IMPACT The ratio of and is at least 1.1.

[0050] In some embodiments, the method comprises: i. a droplet plurality DP of droplets deposited on a dried processing film present on the ITM generates an ink dot set IDS of ink dots present on a substrate (i.e., fixedly attached to an upper substrate surface), each droplet of the droplet plurality DP corresponding to an ink dot present on a different respective substrate of the ink dot set IDS; ii. each ink droplet of the droplet plurality DP is deposited on the substrate according to jetting parameters; and iii. the jetting parameters together with physicochemical properties of the ink droplets of the droplet plurality DP jointly determine an inkjet paper dot radius R. DIRECT-JETTING-ONTO-INK-JET-PAPER-THEORETICAL where R is the radius of the inkjet paper dot. DIRECT-JETTING-ONTO-INK-JET-PAPER-THEORETICALis the radius of the ink dot obtained if the ink droplets are inkjetted directly onto the inkjet paper, not onto a dried thin film, and iv. (A) the dry dot radius R of the dots in the ink dot set IDS DRIED_DOT_ON_SUBSTRATE and (B) the inkjet paper dot radius R DIRECT-JETTING-ONTO-INK-JET-PAPER-THEORETICAL and is performed so that the ratio between is at least 1.1.

[0051] In some embodiments, the density of the set of ink dots is at least 5, or at least 10, or at least 20, or at least 50, or at least 100, and each ink dot of the set of ink dots is distinct on the substrate.

[0052] In some embodiments, the ink dots of the ink dot set are contained within a square geometric protrusion that protrudes on the printing substrate, and each ink dot of the ink dot set is fixedly attached to the surface of the printing substrate, and all the ink dots within the square geometric protrusion are considered as individual members of the ink dot set IDS.

[0053] In some embodiments, the method includes: i. forming an ink dot set IDS of ink dots present on an ink substrate; ii. a concentration of the ink dot set is at least 5, or at least 10, or at least 20, or at least 50, or at least 100, and each ink dot of the ink dot set is distinct on the substrate; iii. the ink dots of the ink dot set are contained within a square geometric protrusion protruding on the printed substrate, each ink dot of the ink dot set being fixedly attached to a surface of the printed substrate, and all of the ink dots within the square geometric protrusion are considered as individual members of the ink dot set IDS; iv. each ink dot of the ink dots comprises at least one colorant dispersed in an organic polymer resin, each dot of the ink dots having an average thickness of less than 2,000 nm and a diameter of 5 to 300 micrometers; and v. each ink dot of the ink dots has a generally convex shape, and wherein deviations from a convex shape (DC dot ) is DCdot = 1-AA / CSA, where AA is the calculated projected area of ​​the dot, which is approximately parallel to the print substrate, CSA is the surface area of ​​the convex shape that minimally encloses the contour of the projected area, and vi. the average deviation of the set of ink dots from convexity (DC dot mean ) is at most 0.05, at most 0.04, at most 0.03, at most 0.025, at most 0.022, at most 0.02, at most 0.018, at most 0.017, at most 0.016, at most 0.015, or at most 0.014.

[0054] In some embodiments, the aqueous treatment formulation is applied to at least a portion or portions of the moving ITM at a speed of at least 1 meter / sec, or at least 1.5 meters / sec, or at least 2 meters / sec to form a wet treatment layer thereon.

[0055] In some embodiments, the method is carried out such that the water soluble polymer concentration in the aqueous treatment formulation is at most 10% by weight, or at most 8% by weight, or at most 6% by weight, or at most 5% by weight.

[0056] 1. An aqueous treatment formulation for use with an intermediate transfer member of a printing system, the formulation comprising: (a) a first surfactant composition comprising a first surfactant, the first surfactant comprising a quaternary ammonium salt having a water solubility of at least 5% at 25 degrees Celsius; (b) at least 1% by weight of at least one water soluble polymer having a water solubility of at least 5% at 25 degrees Celsius; and (c) a carrier liquid comprising water, the water comprising at least 65% by weight of the treatment formulation, the concentration of the quaternary ammonium salt in the aqueous treatment formulation being at least 3% by weight, the treatment formulation having: (i) a static surface tension at 25 degrees Celsius in the range of 20 to 40 dynes / cm; (ii) a 60 degrees Celsius evaporation loading of up to 8:1 by weight; and (iii) a 25 degrees Celsius viscosity in the range of 10 cP to 100 cP.

[0057] In some embodiments, the solubility of the quaternary ammonium salt is at least 7%, at least 10%, at least 15%, or at least 20%, optionally up to 50%, up to 40%, or up to 35%, or further optionally within the range of 5-40%, 5-30%, 5-25%, 7-35%, 10-35%, 12-35%, or 15-35%.

[0058] In some embodiments, the concentration of the quaternary ammonium salt in the aqueous treatment formulation is at least 4%, at least 5%, at least 6%, or at least 7%, optionally up to 30%, up to 25%, or up to 20%, or further optionally within the range of 2-30%, 3-30%, 4-30%, 4-20%, 5-25%, 6-25%, 6-20%, or 7-20%.

[0059] In some embodiments, the concentration of the water soluble polymer in the aqueous treatment formulation is at least 1.5% by weight, or at least 2% by weight, at least 2.5% by weight, at least 3% by weight, or at least 3.5% by weight, optionally up to 10%, or up to 9%, or up to 8%, or up to 7%, or up to 6%, or further optionally within the range of 1.5-20%, or 2-10%, 2-8%, 2-7%, 2.5-10%, 2.5-8%, 2.5-7%, 2.5-6%, 3-8%, 3-7%, 3-6%, 3-6%, 3.5-10%, 3.5-8%, 3.5-7%, 3.5-6%, or 4-6%.

[0060] In some embodiments, the water solubility of the water soluble polymer is at least 7%, at least 10%, at least 12%, or at least 15%.

[0061] In some embodiments, the water soluble polymer is selected from the group consisting of polyvinyl alcohol, water soluble cellulose, polyvinylpyrrolidone (PVP), polyethylene oxide, polyethyleneimine, and water soluble acrylates.

[0062] In some embodiments, the 60 degree Celsius evaporative loading is at most 6:1, at most 5:1, at most 4:1, at most 3.5:1, or at most 3:1, and optionally at least 2:1, at least 2.2:1, or at least 2.5:1.

[0063] In some embodiments, the composition further comprises a second surfactant selected to reduce the static surface tension of the aqueous treatment formulation, which optionally is a silicone polyether, and which optionally has a concentration in the formulation of at least 1%, at least 1.5%, at least 2%, at least 2.5%, or at least 3%, optionally up to 15%, up to 12%, up to 10%, up to 8%, or up to 7%, or further optionally in the range of 1.5-13%, 1.5-10%, 2-13%, 2-10%, 2.5-13%, 2.5-10%, or 3-10%.

[0064] In some embodiments, the treatment formulation further comprises a water absorbing agent disposed within the carrier liquid at a temperature ranging from at least 25 degrees Celsius to 60 degrees Celsius, whereby the aqueous treatment solution is evaporated to form a solid film. The water absorbing agent functions as a water absorbent.

[0065] Some embodiments further include a water absorbing agent disposed within the carrier liquid, the water absorbing agent being solid in a pure state at least within the range of 25 degrees Celsius to 60 degrees Celsius, and acting as a water absorbent when the aqueous treatment solution evaporates to form a solid film.

[0066] In some embodiments, the water absorbing agent has a concentration of 1-25%, 1-15%, 1-10%, 2.5-20%, 2.5-12%, 3-15%, 3-12%, 3-10%, or 3.5-12%.

[0067] In some embodiments, the concentration of the quaternary ammonium salt is in the range of 3-15%, the concentration of the water soluble polymer is in the range of 2.5-10%, 2.5-8%, or 2.5-7%, or 2.5-6%, the 560 degree Celsius evaporation loading is in the range of 2.5:1 to 4:1, and the viscosity is at least 12 cP, preferably at least 14 cP or at least 16 cP.

[0068] In some embodiments, the static surface tension is in the range of 25 to 36 dynes / cm.

[0069] In some embodiments, the water absorbing agent has a concentration of 2.5-10%.

[0070] In some embodiments, the aqueous treatment formulation has a total surfactant concentration of at least 6%, at least 7%, at least 8%, at least 9%, or at least 10%, and optionally within the range of 6-40%, 6-30%, 6-20%, 7-30%, 7-20%, 7-15%, 8-25%, 8-20%, 8-15%, or 8-13%.

[0071] In some embodiments, all components of the aqueous treatment formulation are completely dissolved.

[0072] In some embodiments, the total concentration of organic solvents in the aqueous treatment formulation is at most 3 wt%, at most 2 wt%, at most 1 wt%, or at most 0.5 wt%, or the formulation is free of organic solvents.

[0073] In some embodiments, the concentration of the liquid moisture absorbent in the aqueous treatment formulation is at most 1.5 wt%, at most 1 wt%, at most 0.5 wt%, at most 0.3 wt%, or at most 0.1 wt%, or the aqueous treatment formulation is free of any liquid moisture absorbent.

[0074] In some embodiments, the quaternary ammonium salt is an organic quaternary ammonium salt.

[0075] In some embodiments, the first carbon chain of the organic quaternary ammonium salt has a length of at least 6 carbon atoms, and optionally a length in the range of 6 to 20, 6 to 18, 8 to 20, or 8 to 18 carbon atoms.

[0076] In some embodiments, the second carbon chain of the organic quaternary ammonium salt has a length of up to 3 carbon atoms, or up to 2 carbon atoms.

[0077] In some embodiments, the third carbon chain of the organic quaternary ammonium salt has a length of up to 3 carbon atoms, up to 2 carbon atoms, or up to 1 carbon atom.

[0078] In some embodiments, the organic quaternary ammonium salt is a cationic organic quaternary ammonium salt, optionally having a sulfate or phosphate anion.

[0079] In some embodiments, the polyethyleneimine comprises up to 0.8%, 0.6%, 0.4%, or 0.3%, or 0.2%, or 0.1% by weight of the formulation, or the polyethyleneimine comprises up to 30%, up to 20%, up to 15%, up to 10%, or up to 5% by weight of the water soluble polymer.

[0080] In some embodiments, the viscosity is at least 12 cP, at least 14 cP, or at least 16 cP, optionally up to 90 cP, up to 80 cP, up to 70 cP, up to 60 cP, up to 55 cP, or up to 50 cP, and further optionally within the range of 10-80 cP, 12-80 cP, 12-60 cP, 12-55 cP, or 14-60 cP.

[0081] In some embodiments, the water soluble polymer concentration in the aqueous treatment formulation is up to 10% by weight, or up to 8% by weight, or up to 6% by weight, or up to 5% by weight.

[0082] In some embodiments, an ITM is provided that includes (a) a support layer and (b) a release layer having an ink-receptive surface for receiving an ink image and a second surface opposite the ink-receptive surface, the second surface being attached to the support layer, the release layer being formed from an addition-curable silicone material, the release layer having a thickness of up to 500 micrometers (μm), and the ITM has the following structural characteristics: (1) a total surface energy of the ink-receptive surface is greater than or equal to the total surface energy of a modified ink-receptive surface produced by subjecting the ink-receptive surface of a corresponding release layer to a standard aging procedure; (2) the total surface energy of the ink-receptive surface is at least 4 mN / m, at least 6 mN / m, at least 8 mN / m, or at least 10 mN / m higher than the total surface energy of a hydrophobic ink-receptive surface of a corresponding release layer prepared by standard air curing of a silicone precursor of the cured silicone material; or at least 16 mN / m higher; (3) the receding contact angle of a distilled water droplet on said ink-receptive surface is at least 7 degrees, at least 8 degrees, at least 10 degrees, at least 12 degrees, at least 14 degrees, at least 16 degrees, at least 18 degrees, or at least 20 degrees lower than the receding contact angle of a distilled water droplet on an ink-receptive surface of a corresponding release layer prepared by standard air curing of a silicone precursor of said cured silicone material; and (4) the receding contact angle of a distilled water droplet on said ink-receptive surface is produced by subjecting said ink-receptive surface to a standard aging procedure. (5) the surface hydrophobicity of the ink-receiving surface is less than the bulk hydrophobicity of the cured silicone material in the release layer, the surface hydrophobicity being characterized by the receding contact angle of a distilled water droplet on the ink-receiving surface, the bulk hydrophobicity being characterized by the receding contact angle of a distilled water droplet disposed on an inner surface formed by exposing an area of ​​the cured silicone material in the release layer to form an exposed area;the receding contact angle measured on the ink-receptive surface is at least 7 degrees, at least 8 degrees, at least 10 degrees, at least 12 degrees, at least 14 degrees, at least 16 degrees, at least 18 degrees, or at least 20 degrees lower than the receding contact angle measured on the exposed area; and (6) the receding contact angle of a distilled water droplet on the ink-receptive surface is at most 60 degrees, at most 58 degrees, at most 56 degrees, at most 54 degrees, at most 52 degrees, at most 50 degrees, at most 48 degrees, at most 46 degrees, at most 44 degrees, at most 42 degrees, at most 40 degrees, at most 38 degrees, or at most 36 degrees.

[0083] In some embodiments, the addition-cured silicone material consists essentially of, or comprises at least 95% by weight, of, the addition-cured silicone.

[0084] In some embodiments, functional groups comprise up to 5%, up to 3%, up to 2%, or up to 1% by weight of the addition-cured silicone material, or the addition-cured silicone material is substantially free of functional groups.

[0085] In some embodiments, the addition-cured silicone material is filled with a polyether glycol functionalized polydimethylsiloxane.

[0086] In some embodiments, the polyether glycol functionalized siloxane is loaded into the addition cured silicone material, but does not form part of the covalent structure of the addition cured silicone material.

[0087] An intermediate transfer member (ITM) for use with a printing system (for example, this can be an ITM that is "the provided ITM") comprising: (a) a support layer; and (b) a release layer having an ink-receiving surface for receiving an ink image, and a second surface opposite the ink-receiving surface, the second surface being attached to the support layer, the release layer being formed from an addition-cured silicone material, the release layer having a thickness of up to 500 micrometers (μm), and the ink-receiving surface has the following structural characteristics: (i) a thickness of the ink-receiving surface that is at least 500 micrometers (μm); and (ii) a 10 second dynamic contact angle (DCA) for a distilled water droplet deposited on the ink receptive surface of at least one of 108 degrees, and wherein the release layer has at least one of the following structural characteristics: (1) the addition curable silicone material consists essentially of or comprises at least 95% by weight of the addition curable silicone; and (2) functional groups comprise at most 3% by weight of the addition curable silicone material.

[0088] In some embodiments, the receding contact angle is at most 58 degrees, at most 56 degrees, at most 54 degrees, at most 52 degrees, at most 50 degrees, at most 48 degrees, at most 46 degrees, at most 44 degrees, at most 42 degrees, at most 40 degrees, at most 38 degrees, or at most 37 degrees.

[0089] In some embodiments, the provided ITM (e.g., the ITM of this printing method) has the following characteristics: the functional groups comprise up to 2 wt%, up to 1 wt%, up to 0.5 wt%, up to 0.2 wt%, or up to 0.1 wt% of the addition-cured silicone material, or the addition-cured silicone material is substantially free of the functional groups. In some embodiments, the addition-cured silicone material is loaded with a polyether glycol functionalized polydimethylsiloxane.

[0090] In some embodiments, the ITM provided (i.e., the ITM of this printing method) has the following characteristics: a polyether glycol functionalized siloxane is loaded into the addition-cured silicone material, but does not form part of the covalent structure of the addition-cured silicone material.

[0091] In some embodiments, the provided ITM (e.g., the ITM of this printing method) has the following characteristics: the release layer has a thickness of at most 500 μm, at most 100 μm, at most 50 μm, at most 25 μm, or at most 15 μm.

[0092] In some embodiments, the provided ITM (e.g., an ITM of this printing method) has the following characteristics: the release layer has a thickness in the range of 1-100 μm, 5-100 μm, 8-100 μm, 10-100 μm, or 10-80 μm.

[0093] In some embodiments, the provided ITM (e.g., an ITM of this printing method) has the following characteristics: the thickness of the support layer is in the range of about 50 to 1000 micrometers (μ), 100 to 1000 μ, 100 to 800 μ, or 100 to 500 μ.

[0094] In some embodiments, the ITMs provided (i.e., the ITMs of this method) have the following characteristic: the total surface energy of the ink-receptive surface is at least 2 J / m lower than the total surface energy of a modified ink-receptive surface produced by subjecting the ink-receptive surface of a corresponding release layer to a standard aging procedure. 2 , at least 3 J / m 2 , at least 4 J / m 2 , at least 5 J / m 2 , at least 6 J / m 2 , at least 8 J / m 2 , or at least 10 J / m 2 expensive.

[0095] In some embodiments, the ITMs provided (i.e., the ITMs of this method) have the following characteristics: the total surface energy of the ink-receptive surface is at least 4 J / m lower than the total surface energy of a hydrophobic ink-receptive surface of a corresponding release layer prepared by standard air curing of a silicone precursor of the cured silicone material. 2 , at least 6 J / m 2 , at least 8 J / m 2 , at least 10 J / m 2 , at least 12 J / m 2 , at least 14 J / m 2 , or at least 16 J / m 2 big.

[0096] In some embodiments, the provided ITM (i.e., the ITM of this printing method) has the following characteristics: the receding contact angle of a distilled water droplet on the ink receptive surface is at least 7 degrees, at least 8 degrees, at least 10 degrees, at least 12 degrees, at least 15 degrees, at least 18 degrees, or at least 20 degrees lower than the receding contact angle of a distilled water droplet on the ink receptive surface of a corresponding release layer prepared by standard air curing of a silicone precursor of the cured silicone material.

[0097] In some embodiments, the receding contact angle of a distilled water droplet on the ink receptive surface is at least 5 degrees, at least 6 degrees, at least 7 degrees, or at least 8 degrees lower than the receding contact angle of a distilled water droplet on an aged surface produced by subjecting the ink receptive surface to a standard aging procedure.

[0098] In some embodiments, the surface hydrophobicity of the ink-receptive surface is less than the bulk hydrophobicity of the cured silicone material in the release layer, where the surface hydrophobicity is characterized by the receding contact angle of a distilled water droplet on the ink-receptive surface and the bulk hydrophobicity is characterized by the receding contact angle of a distilled water droplet deposited on an inner surface formed by exposing areas of the cured silicone material in the release layer to form exposed areas.

[0099] In some embodiments, the ITM provided (i.e., the ITM of this printing method) has the following characteristics: the receding contact angle measured on the ink receptive surface is at least 7 degrees, at least 8 degrees, at least 10 degrees, at least 12 degrees, at least 14 degrees, at least 16 degrees, at least 18 degrees, or at least 20 degrees lower than the receding contact angle measured on the exposed area.

[0100] In some embodiments, the receding contact angle of the distilled water droplet on an ink receptive surface is at least 25 degrees, at least 28 degrees, at least 30 degrees, at least 32 degrees, at least 34 degrees, or at least 36 degrees, and further optionally within the range of 25 degrees to 60 degrees, 28 degrees to 60 degrees, 30 degrees to 60 degrees, 30 degrees to 60 degrees, 30 degrees to 55 degrees, 30 degrees to 50 degrees, 32 degrees to 60 degrees, 32 degrees to 55 degrees, 32 degrees to 44 degrees, 35 degrees to 60 degrees, 35 degrees to 55 degrees, 36 degrees to 44 degrees, or 38 degrees to 50 degrees.

[0101] In some embodiments, the release layer is adapted so that the polar groups of the ink-receiving surface have a direction that is spaced apart or opposite to that of the second surface.

[0102] In some embodiments, the release layer is adapted such that when the ITM is in an operational mode in which the ink receptive surface is exposed to the ambient environment, the polar groups on the ink receptive surface are oriented toward or away from the ambient environment.

[0103] In some embodiments, the ITM provided (eg, the ITM of this printing method) has the following characteristics: the ITM forms a component in a digital printing system.

[0104] In some embodiments, the ITM provided (i.e., the ITM of this printing method) has the following features: the support layer includes a resilient compliant layer attached to the second surface of the release layer, the resilient compliant layer adapted to closely follow the surface contours of a printing substrate onto which the ink image is impressed.

[0105] In some embodiments, the ITM provided (i.e., the ITM of this printing method) has the following features: A support layer includes a stiffening layer attached to the compliant layer.

[0106] In some embodiments, the provided ITMs (e.g., ITMs of this printing method) have the following characteristics: the release layer comprises up to 3 wt%, up to 2 wt%, up to 1 wt%, up to 0.5 wt%, up to 0.2 wt%, or substantially 0 wt% total functional groups within its silicone polymer matrix.

[0107] In some embodiments, the provided ITMs (e.g., ITMs of this printing method) have the following characteristics: the release layer comprises, within its silicone polymer matrix, a total amount of up to 3%, up to 2%, up to 1%, up to 0.5%, up to 0.2%, or substantially 0% by weight of functional groups selected from the group of moieties comprising C=O, S=O, OH, and COO.

[0108] In some embodiments, the provided ITMs (e.g., ITMs of this printing method) have the following feature: the release layer comprises, within its silicone polymer matrix, up to 3%, up to 2%, up to 1%, up to 0.5%, up to 0.2%, or substantially 0% by weight of functional groups selected from the group consisting of silane moieties, alkoxy moieties, amide moieties, and amide-alkoxy moieties.

[0109] In some embodiments, the provided ITMs (e.g., ITMs of this printing method) have the following characteristics: the release layer comprises, within its silicone polymer matrix, functional groups selected from the group consisting of amine, ammonium, aldehyde, SO2, SO3, SO4, PO3, PO4, and COC in a combined amount of up to 3%, up to 2%, up to 1%, up to 0.5%, up to 0.2%, or substantially 0% by weight.

[0110] In some embodiments, the ITM provided (i.e., the ITM of this printing method) has the following characteristics: the addition-curable silicone material has a structure constructed from vinyl-functional silicone.

[0111] In some embodiments, the ITM provided (i.e., the ITM of this printing method) has the following characteristics: the addition-curable silicone material includes a polar group of "MQ" type.

[0112] In some embodiments, the ITM provided (eg, the ITM of this printing method) has the following characteristics: the total surface energy of the ink-receptive surface is estimated using the Owens-Wendt surface energy model.

[0113] In some embodiments, the ITM provided (i.e., the ITM of the printing method) has the following characteristics: the 10 second DCA is at most 108 degrees, at most 106 degrees, at most 103 degrees, at most 100 degrees, at most 96 degrees, at most 92 degrees, or at most 88 degrees, optionally at least 60 degrees, at least 65 degrees, at least 70 degrees, at least 75 degrees, at least 78 degrees, at least 80 degrees, at least 82 degrees, at least 84 degrees, or at least 86 degrees, and further optionally within the range of 60-108 degrees, 65-105 degrees, 70-105 degrees, 70-100 degrees, 70-96 degrees, 70-92 degrees, 75-105 degrees, 75-100 degrees, 80-105 degrees, 80-100 degrees, 85-105 degrees, or 85-100 degrees.

[0114] In some embodiments, the ITM provided (i.e., the ITM of the printing method) has the following characteristics: the ink receptive surface is adapted such that, for the distilled water droplet deposited on the ink receptive surface, the difference between the 70 second dynamic contact angle (DCA) and the 10 second DCA is within the range of at least 7 degrees, at least 8 degrees, at least 10 degrees, or at least 12 degrees, optionally up to 25 degrees, up to 22 degrees, up to 20 degrees, up to 18 degrees, or up to 17 degrees, and further optionally, 6-25 degrees, 6-22 degrees, 6-20 degrees, 6-18 degrees, 6-17 degrees, 7-25 degrees, 7-20 degrees, 7-17 degrees, 8-25 degrees, 8-22 degrees, 18-20 degrees, 8-18 degrees, 8-17 degrees, 10-25 degrees, 10-22 degrees, 10-20 degrees, 10-18 degrees, or 10-17 degrees.

[0115] In some embodiments, the ink receptive surface is adapted such that, for the distilled water droplets deposited on the ink receptive surface, the 70 second DCA is in the range of at most 92 degrees, at most 90 degrees, at most 88 degrees, at most 85 degrees, at most 82 degrees, at most 80 degrees, at most 78 degrees, at most 76 degrees, at most 74 degrees, or at most 72 degrees, optionally at least 55 degrees, at least 60 degrees, at least 65 degrees, or at least 68 degrees, and further optionally, 55-92 degrees, 55-90 degrees, 55-85 degrees, 55-80 degrees, 65-92 degrees, 65-90 degrees, 65-85 degrees, 65-80 degrees, 68-85 degrees, 68-80 degrees, 70-92 degrees, 70-90 degrees, 70-85 degrees, or 70-80 degrees.

[0116] a. an intermediate transfer member (ITM) including an endless flexible belt mounted on a plurality of guide rollers; b. an imaging station configured to form an ink image on a surface of the ITM, where first and second of the guide rollers are disposed upstream and downstream of the imaging station to define an upward stroke and a downward stroke through the imaging station; and c. an impression station through which the downward stroke of the ITM passes, the impression station being disposed downstream of the imaging station and configured to transfer the ink image from the ITM surface to a substrate. d. a processing station arranged downstream of the printing station and upstream of the image forming station for forming a uniform thin layer of a liquid processing formulation on the ITM surface on a downward stroke of the ITM, the processing station including: i. a coater for coating the ITM with the liquid processing formulation; and ii. a coating thickness adjustment assembly for removing excess liquid so that only a desired uniform thin layer of the processing formulation remains, the coating thickness adjustment assembly including a rounded tip that faces the ITM surface on the downward stroke.

[0117] In some embodiments, the rounded tip is the tip of a doctor blade.

[0118] In some embodiments, the doctor blade is oriented perpendicular to the ITM surface.

[0119] In some embodiments, the rounded tip is biased towards the ITM surface and / or the ITM surface is biased towards the rounded tip.

[0120] In some embodiments, the rounded tip is urged towards the ITM surface and / or the ITM surface is urged towards the rounded tip by a backing roller having a soft outer surface.

[0121] In some embodiments, (i) a backing roller is positioned inside the closed loop of the endless belt and is positioned opposite the blade, and / or (ii) a backing roller and a rounded tip are positioned on opposite sides of the downward stroke of the ITM.

[0122] In some embodiments, the outer surface of the backing roller has one or more of the following properties: (i) elasticity, (ii) zero memory, (iii) retains its soft outer surface across a range of temperatures, and (iv) is constructed from polyurethane.

[0123] In some embodiments, the difference between the maximum and minimum of the temperature range is at least 10 degrees Celsius, or at least 20 degrees Celsius, or at least 50 degrees Celsius, and / or the mean value of the temperature range is within the range of 50 degrees Celsius to 120 degrees Celsius.

[0124] In some embodiments, the backing roller has a compressible surface that, when urged toward the rounded tip toward the ITM surface and / or the ITM surface toward the rounded tip, compresses such that the rounded tip penetrates into the ITM at a penetration depth.

[0125] In some embodiments, when the rounded tip is urged toward the ITM surface and / or the ITM surface is urged toward the rounded tip, the rounded tip penetrates the ITM at a penetration depth.

[0126] In some embodiments, the magnitude of the penetration depth is at least 1 m or at least 2 mm, and / or up to 5 mm or up to 4 mm or up to 3 mm.

[0127] In some embodiments, the rounded tip is biased toward the ITM and / or the ITM is biased toward the rounded tip with a balanced force against a liquid solution disposed in the gap between the rounded tip and the portion of the IMT surface opposite the rounded tip, thereby maintaining the gap constant.

[0128] In some embodiments, the size of the gap adjusts the thickness of the desired uniform thin layer of the treatment formulation.

[0129] In some embodiments, the ratio between the gap and the desired uniform thin layer thickness is at least 0.1, or at least 0.25, or at least 0.5, and / or at most 10, or at most 4, or at most 2.

[0130] In some embodiments, (i) the gap size is at most 2 microns, or at most 1 micron, or at most 0.8 microns, or at most 0.6 microns, and / or (ii) the ratio between the gap size and the penetration depth of the rounded tip into the ITM surface is at most 0.01, or at most 0.005, or at most 0.001, or at most 0.0005.

[0131] In some embodiments, the penetration depth is set to a set value and the magnitude of the biasing force is adjusted to maintain the penetration depth at the set value.

[0132] In some embodiments, the radius of curvature of the rounded doctor blade is up to 2 mm, or up to 1.5 mm, or up to 1.25 mm, or up to 1 mm.

[0133] In some embodiments, the coater for coating the ITM is selected from the group consisting of: (i) a spray device; and (ii) a wetting tray positioned below the downward stroke of the ITM, within which the liquid treatment formulation is disposed.

[0134] In some embodiments, the system includes a cleaning station located downstream of the impression station and upstream of the conditioning station for removing residual material remaining on the ITM surface after the ink image is transferred to the substrate.

[0135] In some embodiments, the doctor blade is one of multiple doctor blades mounted on the periphery of a rotatable turret to aid in replacement of the doctor blade that is biased against the surface.

[0136] In some embodiments, the spacing of the blades on the turret periphery is set so that during rotation of the turret to replace a doctor blade, the blade being replaced does not stop functioning until the replacement blade has started functioning.

[0137] In some embodiments, a blade cleaning device is provided adjacent the turret to remove any deposits adhering to the currently defunct doctor blade.

[0138] In some embodiments, a blade cleaning device is provided adjacent the turret to remove any deposits adhering to the currently defunct doctor blade.

[0139] In some embodiments, the cleaning device is a rotating brush.

[0140] The printing method includes: a. providing an intermediate transfer member (ITM) having an aqueous ink, an aqueous treatment formulation, and a release surface; b. applying the aqueous treatment formulation to the release surface of the ITM to form a wet treatment layer on the release surface; c. subjecting the wet treatment layer to a drying process to form a dry treatment film on the ITM from the wet treatment layer; d. depositing droplets of the aqueous ink on the dry treatment film to form an ink image on the dry treatment film; e. drying the ink image to leave a residual ink image on the release surface of the ITM; and f. transferring the residual ink image onto the print substrate by pressurized contact between the ITM and the print substrate.

[0141] In some embodiments, the residual ink image, along with the non-printed areas of the dried treatment film, is transferred onto the print substrate.

[0142] In some embodiments, during and / or immediately after transfer, the drying treatment film mechanically contacts and / or bonds the non-printed areas to the residual ink image.

[0143] In some embodiments, immediately following the residual ink image, the dried treatment film is continuous across the ink dots present on multiple separate substrates.

[0144] In some embodiments, at least the release surface of the ITM has a Shore A hardness of at most 50, or at most 45, or at most 40, or at most 35, or at most 30, or at most 25, or at most 20, or at most 15.

[0145] In some embodiments, the ITM has the form of an endless belt mounted on multiple rollers, and the wet treatment layer is formed by applying pressure (normally) to the surface of the ITM at a roller-to-roller location between the upstream and downstream rollers.

[0146] In some embodiments, to form a wet treatment layer on the ITM, (i) the aqueous treatment formulation is applied to the ITM while it is moving, and (ii) the aqueous treatment formulation is applied to the moving portion(s) of the ITM such that at least the portion(s) is moving at a speed of at least 0.5 meters / sec, or at least 1 meter / sec, or at least 1.5 meters / sec, or at least 2 meters / sec, or at least 2.5 meters / sec, or at least 3 meters / sec.

[0147] In some embodiments, the wet treatment layer is formed by applying a force to the ITM from a highly rounded surface having a radius of curvature of up to 5 mm, or up to 3 mm, or up to 2.5 mm, or up to 2 mm, or up to 1.75 mm, or up to 1.5 mm, or up to 1.25 mm, or up to 1 mm.

[0148] In some embodiments, the highly rounded surface is the surface of a doctor blade.

[0149] In some embodiments, the doctor blade is oriented in the cross-printing direction and is biased against the ITM in the cross-printing direction with a force density of at least 250 g / cm, or at least 350 g / cm, or at least 400 gm / cm, and / or up to 1 kg / cm, or up to 750 g / cm, or up to 600 g / cm.

[0150] In some embodiments, the doctor blade is formed from an abrasion resistant material having a Brinell hardness of greater than 100.

[0151] In some embodiments, the doctor blade has a smooth and / or regular cylindrical surface.

[0152] In some embodiments, the surface roughness RA of the doctor blade is at most a few microns, or at most 1 micron, or at most 0.5 microns.

[0153] In some embodiments, the doctor blade is one of multiple doctor blades mounted on a rotatable turret to allow for quick replacement of the doctor blade interacting with the surface of the ITM.

[0154] In some embodiments, the spacing of the blades on the turret periphery is set so that during rotation of the turret to replace the doctor blade, the blade being replaced does not stop interacting with the ITM until the replacement blade stops interacting with the ITM.

[0155] In some embodiments, a cleaning device, such as a rotating brush, is provided adjacent the turret to a rounded edge of at least one of the doctor blades that does not currently interact with an ITM.

[0156] In some embodiments, prior to applying the aqueous treatment solution to the release surface of the ITM, the release surface of the ITM is cleaned to remove any treatment film remaining on the release surface after completion of the previous printing cycle.

[0157] In some embodiments, cleaning of the release surface of the ITM is performed using an aqueous treatment solution to dissolve any dried treatment film on the release surface.

[0158] In some embodiments, the thickness of the wet processing layer is up to 2μ, or up to 1.5μ, or up to 1μ, or up to 0.9μ, or up to 0.8μ, or up to 0.7μ, or up to 0.6μ, or up to 0.5μ, or up to 0.5μ, or up to 0.4μ, or up to 0.3μ, or up to 0.2μ, or up to 0.15μ.

[0159] In some embodiments, the wet treatment layer has a uniform thickness.

[0160] In some embodiments, on a rectangle having a width of at least w cm and a length of at least l cm, the entire rectangle is covered by the wet process film such that the thickness of the wet process film does not deviate from the average thickness value within the rectangle by more than 50%, or more than 40%, or more than 30%, or more than 20%, or more than 10%, or more than 5%, or more than 2.5%, or more than 1%, where (i) the value of w is at least 10, or at least 20, or at least 30, and / or up to 100, or up to 80, or up to 60, and (ii) the value of l is at least 50, or at least 100, or at least 250, or at least 500, or at least 1000.

[0161] In some embodiments, i. forming a thin wet treatment layer includes creating a velocity gradient of the aqueous treatment solution at an intense velocity gradient (IVG) location (A) that is vertically spaced (e.g., by up to 3 microns, or up to 2 microns, or up to 1 micron) from the release surface of the ITM and / or (B) that is located between the applicator and the release surface of the applicator, and ii. at the IVG location, the magnitude of the velocity gradient is equal to or exceeds a VG value, where the VG value is at least 10 6 / sec, or at least 2×10 6 / sec, or at least 4×10 6 / sec, or at least 5×10 6 / sec, or at least 7.5 × 10 6 / sec, or at least 10 7 / sec, or at least 2×10 7 / sec, or at least 4×10 7 / sec, or at least 5×10 7 / sec, or at least 7.5 × 10 7 / second.

[0162] In some embodiments, the velocity gradient is localized along the printing direction such that: i. at an upstream position, upstream of the IVG position, the maximum velocity gradient is up to x% of the value of the velocity gradient at the IVG position; ii. at a downstream position, downstream of the IVG position, the maximum velocity gradient is up to x% of the value of the velocity gradient at the IVG position; iii. the value of x is up to 50, or up to 30, or up to 20, or up to 10; and / or iv. the upstream and downstream positions are each spaced apart from the IVG position along the printing direction by up to 2 cm, or up to 1.5 cm, or up to 1.25 cm, or up to 1 cm, or up to 9 mm, or up to 8 mm, or up to 7.5 mm, or up to 7 mm, or up to 6 mm, or up to 5 mm.

[0163] In some embodiments, drying of the treatment solution occurs rapidly enough to prevent beading and leave behind a continuous hydrophilic, cohesive polymer treatment film having a thickness (e.g., a substantially uniform thickness) of at most 200 nm, or at most 150 nm, or at most 120 nm, or at most 100 nm, or at most 80 nm, or at most 70 nm, or at most 60 nm, or at most 50 nm, or at most 40 nm, or at most 30 nm.

[0164] Nevertheless, in different embodiments, even when the dry processing film is extremely thin, it is thicker than a monolayer or monolayer-type construct. Thus, in different embodiments, the thickness of the dry processing layer can be at least 20 nanometers, or at least 30 nanometers, or at least 40 nanometers, or at least 50 nanometers. In some embodiments, providing this much "bulk" (i.e., a minimum thickness characteristic - e.g., along with other characteristic(s) described below) aids in the formation of a dry processing film that exhibits cohesion and / or elasticity. This can be useful in step S117, where it is desirable to maintain the structural integrity of the dry processing film as it is transferred from the ITM to the substrate (i.e., in the stage of retaining the dry ink image on the dry processing film).

[0165] In some embodiments, the dried film onto which the aqueous ink droplets are deposited has a thickness of at most 200 nm, or at most 100 nm, or at most 50 nm, or at most 30 nm.

[0166] In some embodiments, the dried film onto which the aqueous ink droplets are deposited has a thickness of at least 15 nm, or at least 20 nm, or at least 30 nm, or at least 50 nm, or at least 75 nm.

[0167] In some embodiments, the dry processing film is continuous across a rectangle of the release surface of the ITM, the rectangle having a width of at least w cm and a length of at least l meters, where (i) w is at least 10, or at least 20, or at least 30, and / or up to 100, or up to 80, or up to 60, and (ii) l is at least 50, or at least 100, or at least 250, or at least 500, or at least 1000.

[0168] In some embodiments, the dried process film is continuous such that for at least 50%, or at least 75%, or at least 90%, or at least 95%, or at least 99%, or 100% of the area of ​​the rectangle, the thickness of the dried process film does not deviate from the average thickness value within the rectangle by more than 50%, or more than 40%, or more than 30%, or more than 20%, or more than 10%, or more than 5%, or more than 2.5%, or more than 1%.

[0169] In some embodiments, during the drying process of the wet processing layer, the dynamic viscosity of the wet processing layer increases by at least 100 times, or at least 500 times, or at least 1000 times, or at least 2500 times, or at least 5000 times, or at least 10,000 times, or at least 25,000 times, within a time period of up to 1 second, or up to 500 milliseconds, or up to 250 milliseconds, or up to 150 milliseconds, or up to 100 milliseconds, or up to 75 milliseconds, or up to 50 milliseconds, or up to 25 milliseconds, or up to 15 milliseconds, or up to 10 milliseconds.

[0170] In some embodiments, the liquid content of the dried process film is up to 10% w / w, or up to 7.5% w / w, or up to 5% w / w, or up to 2.5% w / w, or up to 1.5% w / w, or up to 1% w / w.

[0171] In some embodiments, the drying process removes at least 80% by weight, or at least 90% by weight, or at least 95% by weight of the water in the wet process layer (e.g., within a time period of at least 1 second, or at least 0.5 seconds, or at least 100 milliseconds, or at least 50 milliseconds, or at least 25 milliseconds, or at least 10 milliseconds) to form a dry process thin film.

[0172] In some embodiments, the drying process removes at least 80% w / w, at least at least 90% w / w, at least at least 95% w / w of the 60 degrees Celsius / 1 atm liquid from the wet process layer to form a dry process film.

[0173] In some embodiments, the surface of the dried processed film onto which the aqueous ink droplets are deposited (e.g., the upper surface of the dried processed film) is characterized by an average roughness Ra (a commonly used one-dimensional average roughness parameter) of at most 30 nanometers, or at most 25 nanometers, or at most 20 nanometers, or at most 18 nanometers, or at most 16 nanometers, or at most 15 nanometers, or at most 14 nanometers, or at most 12 nanometers, or at most 10 nanometers, or at most 9 nanometers, or at most 8 nanometers, or at most 7 nanometers, or at most 5 nanometers, and / or at least 3 nanometers, or at least 5 nanometers.

[0174] In some embodiments, the dry treatment film on which the aqueous ink droplets are deposited, and the surface of the dry treatment film (e.g., the upper surface of the dry treatment film) are characterized by a dimensional ratio between (i) the average roughness Ra, and (ii) the thickness of the dry treatment layer, which dimensional ratio is at least 0.02, or at least 0.03, or at least 0.04, or at least 0.05, or at least 0.06, or at least 0.07, or at least 0.08, or at least 0.09, or at least 0.10, or at least 0.11, or at least 0.12, or at least 0.13, or at least 0.14, or at least 0.15, or at least 0.16, or at least 0.17, or at least 0.18, or at least 0.19, or at least 0.2.

[0175] In some embodiments, the dry process film on which the aqueous ink droplets are deposited, and the surface of the dry process film (e.g., the upper surface of the dry process film) are characterized by a dimensionless ratio between (i) the average roughness Ra, and (ii) the thickness of the dry process layer, where the dimensionless ratio is at least 0.5, at least 0.4, at least 0.3, at least 0.25, at least 0.2, at least 0.15, or at least 0.1, and optionally at least 0.02, or at least 0.03, or at least 0.04, or at least 0.05, or at least 0.06, or at least 0.07, or at least 0.08.

[0176] In some embodiments, the dried film is continuous when dried.

[0177] In some embodiments, the aqueous treatment formulation is provided in the form of a solution.

[0178] In some embodiments, the aqueous treatment formulation is provided in the form of a dispersion.

[0179] In some embodiments, the solids of the water-based ink (e.g., nanopigments and / or resins) flow into the bulk of the dried processing film and react (e.g., bond) with quaternary ammonium salts present in the dried processing film (thereby, for example, facilitating droplet spreading).

[0180] In some embodiments, the substrate is selected from the group consisting of uncoated fibrous printing substrates, commercially available coated fibrous printing substrates, and plastic printing substrates.

[0181] In some embodiments, the printing substrate is optionally a paper selected from the group of papers consisting of bond paper, uncoated offset printing paper, coated offset printing paper, copy paper, wood paper, coated wood paper, fine paper, coated fine paper, and laser paper.

[0182] In some embodiments, the transfer is performed at a transfer temperature of up to 120 degrees Celsius, or up to 120 degrees Celsius, or up to 100 degrees Celsius, or up to 90 degrees Celsius, or up to 80 degrees Celsius.

[0183] In some embodiments, the solids of the water-based ink (e.g., nanopigments and / or resins) flow into the bulk of the dried process film and react (e.g., bond) with the quaternary ammonium salts present in the dried process film.

[0184] In some embodiments, the method is performed to form a set of ink dots IDS that reside on an ink substrate.

[0185] In some embodiments, the method is performed such that a droplet plurality DP of aqueous ink droplets deposited on a dried processing thin film present on an ITM forms an ink dot set IDS of ink dots present on an ink substrate such that a given droplet gives rise to and / or evolves into an ink dot present on a given substrate, such that a correspondence exists between (i) each given droplet of the droplet plurality DP and (ii) the ink dots present on a given substrate of each of the ink dot sets.

[0186] In some embodiments, the method is performed such that during deposition, whenever a droplet of the droplet plurality impacts with a dried processing film on the ITM, the kinetic energy of the impacting droplet changes the droplet.

[0187] In some embodiments, the method further comprises: (i) determining whether the maximum impact radius of each droplet among the droplets deformed above the surface of the ITM is a maximum impact radius value R MAX_IMPACT (ii) after the collision and / or during and / or after the transfer, each ink dot of the set of ink dots IDS present on the substrate has a dry dot radius R DRIED_DOT_ON_SUBSTRATE Physicochemical forces cause the deformed droplets, or dots derived from such droplets, to develop so as to have (iii) for each droplet of the droplet plurality and corresponding ink dot of the ink dot set IDS, i. Radius R of the dry dots present on the substrate DRIED_DOT_ON_SUBSTRATE and, ii. Maximum impact radius of deformed droplet R MAX_IMPACT and, is at least 1, or at least 1.01, or at least 1.02, or at least 1.03, or at least 1.04, or at least 1.05, or at least 1.1, or at least 1.15, or at least 1.2, or at least 1.25, or at least 1.3, or at least 1.35, or at least 1.4, or at least 1.45, or at least 1.5, and optionally at most 2, at most 1.8, at most 1.7, at most 1.6, or at most 1.55.

[0188] In some embodiments, the method comprises: i. a droplet plurality DP of droplets deposited on a dried processing film present on the ITM generates ink dots present on a substrate (i.e., fixedly attached to a top substrate surface), each droplet of the droplet plurality DP corresponding to an ink dot present on a different respective substrate of the ink dot set IDS; ii. each ink droplet of the droplet plurality DP is deposited on the substrate according to ejection parameters; and iii. the ejection parameters together with physicochemical properties of the ink droplets of the droplet plurality DP jointly determine an inkjet paper dot radius R. DIRECT-JETTING-ONTO-INK-JET-PAPER-THEORETICAL where R is the radius of the inkjet paper dot. DIRECT-JETTING-ONTO-INK-JET-PAPER-THEORETICAL is the radius of the ink dot obtained if the ink droplets are inkjetted directly onto the inkjet paper, not onto a dried thin film, and iv. (A) the dry dot radius R of the dots in the ink dot set IDS DRIED_DOT_ON_SUBSTRATE and (B) the inkjet paper dot radius R DIRECT-JETTING-ONTO-INK-JET-PAPER-THEORETICAL and is at least 1, or at least 1.01, or at least 1.02, or at least 1.03, or at least 1.04, or at least 1.05, or at least 1.1, or at least 1.15, or at least 1.2, or at least 1.25, or at least 1.3, or at least 1.35, or at least 1.4, or at least 1.45, or at least 1.5, and optionally at most 2, at most 1.8, at most 1.7, at most 1.6, or at most 1.55.

[0189] In some embodiments, the density of the set of ink dots is at least 5, or at least 10, or at least 20, or at least 50, or at least 100, and each ink dot of the set of ink dots is distinct on the substrate.

[0190] In some embodiments, the method is performed such that the ink dots of the ink dot set are contained within a square geometric protrusion protruding on the printing substrate, each ink dot of the ink dot set is fixedly attached to the surface of the printing substrate, and all of the ink dots within the square geometric protrusion are considered as individual members of the ink dot set IDS.

[0191] In some embodiments, the method is performed such that each of the ink dots comprises at least one colorant dispersed in an organic polymer resin, and each of the ink dots has an average thickness of less than 2,000 nm and a diameter of between 5 and 300 micrometers.

[0192] In some embodiments, the method further comprises: each ink dot of the ink dots having a generally convex shape, and wherein the deviation from convex shape (DC dot ) but DC dot = 1-AA / CSA, where AA is the calculated projected area of ​​the dot, which is approximately parallel to the print substrate, CSA is the surface area of ​​the convex shape that minimally encloses the outline of the projected area, and DC is the mean deviation of the set of ink dots from convexity (DC dot mean ) is at most 0.05, at most 0.04, at most 0.03, at most 0.025, at most 0.022, at most 0.02, at most 0.018, at most 0.017, at most 0.016, at most 0.015, or at most 0.014.

[0193] In some embodiments, the method includes forming a substrate having a top surface of a substrate, the substrate having a top surface of the substrate being printed with ink, the ink dots each comprising at least one colorant dispersed in an organic polymer resin, the ink dots each covering a continuous area of ​​a top surface of the substrate, and (i) a projected vertical line extending downwardly toward the top substrate surface first encounters the ink dot at each point in the continuous area before encountering the top substrate surface, and / or (ii) each of the ink dots has a diameter of between 15 and 300 micrometers, and / or (iii) each of the ink dots has an average thickness of at most 1,800 nm, and each of the ink dots has a thickness of at most 1,800 nm. aspect =Ddot / H dot The dimensionless aspect ratio (R aspect ), wherein D dot is the diameter, and H dot is the average thickness, and / or (iv) each of the ink dots is disposed entirely over the continuous area such that the aspect ratio is at least 50, or at least 60, or at least 75, or at least 95, or at least 110, or at least 120, or at least 135, or at least 150, or at least 170, or at least 180, or at least 190, or at least 200, or at least 220, or at least 240, or at least 260, or at least 280, or at least 300.

[0194] In some embodiments, the method is performed such that the aspect ratio is at most 400, at most 350, or at most 325.

[0195] In some embodiments, the method includes forming a substrate having a top surface of a substrate, the substrate having a top surface of the substrate being printed with ink, the ink dots each comprising at least one colorant dispersed in an organic polymer resin, the ink dots each covering a continuous area of ​​a top surface of the substrate, and (i) a projected vertical line extending downwardly toward the top substrate surface first encounters the ink dot at each point in the continuous area before encountering the top substrate surface, and / or (ii) each of the ink dots has a diameter of between 15 and 300 micrometers, and / or (iii) each of the ink dots has an average thickness of at most 1,800 nm, and each of the ink dots has a thickness of at most 1,800 nm. aspect =D dot / H dot The dimensionless aspect ratio (R aspect ), wherein D dot is the diameter, and H dotis the average thickness, and / or (iv) each of the ink dots is disposed over the entire continuous area such that the aspect ratio is within the range of 140 to 400, 150 to 300, 160 to 300, 180 to 300, 200 to 300, 210 to 300, 220 to 300, 230 to 300, or 240 to 300.

[0196] In some embodiments, the method is performed such that at least one (or at least a majority or all) of the ink dots of the ink dot set IDS includes less than 2% of charge directors.

[0197] In some embodiments, the method is performed such that at least one (or at least a majority or all) of the ink dots of the set of ink dots IDS does not include a charge director.

[0198] In some embodiments, the method is performed such that at least one (or at least a majority or all) of the ink dots of the ink dot set IDS has a thickness that is at most 1,500 nm, or at most 1000 nm, or at most 800 nm, or at most 600 nm, or at most 400 nm, or at most 350 nm, or at most 300 nm, or at most 250 nm.

[0199] In some embodiments, the method is carried out such that at least one (or at least a majority or all) of the ink dots of an ink dot set IDS comprises at least 1.2% by weight of the colorant.

[0200] In some embodiments, the method is carried out such that at least one (or at least a majority or all) of the ink dots of an ink dot set IDS comprises at least 5% by weight of the resin.

[0201] In some embodiments, the method is performed such that at least one (or at least a majority or all) of the ink dots of the ink dot set IDS is configured so that the total concentration of the colorant and the resin in the ink dot is at least 40%.

[0202] In some embodiments, the method is performed such that at least one (or at least a majority or all) of the ink dots of the ink dot set IDS are configured so that the weight ratio of the resin to the pigment in the ink dot is at least 1:1.

[0203] In some embodiments, the method is performed such that at least one (or at least a majority or all) of the ink dots of the ink dot set IDS does not have an adhesion failure when subjected to a standard tape test.

[0204] In some embodiments, the method is carried out such that at least one (or at least a majority or all) of the upper thin film surface of each ink dot has a surface concentration of nitrogen that exceeds a bulk concentration of nitrogen in the thin film, the bulk concentration being measured at a depth of at least 30 nanometers below the upper thin film surface, and the ratio of the surface concentration to the bulk concentration is at least 1.1 to 1.

[0205] In some embodiments, the method is carried out such that the upper thin film surface of at least one (or at least a majority or all) of each of said ink dots exhibits an X-ray photoelectron spectroscopy (XPS) peak at 402.0±0.4 eV.

[0206] In some embodiments, the method further comprises: heating the ink dots of at least one (or at least a majority or all) of the ink drop sets for 10 minutes at a temperature in the range of 90 degrees Celsius to 195 degrees Celsius. 6 cP~3×10 8 The viscosity coefficient is then adjusted to have a first viscosity coefficient in the range of cP.

[0207] In some embodiments, the method comprises: 7 It is executed so that cP.

[0208] In some embodiments, the method further comprises: 6 cP~10 8 This is carried out so that it is within the range of cP.

[0209] In some embodiments, the method further comprises: 6 It is executed so that cP.

[0210] In some embodiments, the method is performed such that at least one (or at least a dive or all) of the ink dots are contiguous.

[0211] In some embodiments, the method is carried out such that at least one (or at least most or all) has a thickness of at most 1,200 nm, or at most 1,000 nm, or at most 800 nm, or at most 650 nm, or at most 500 nm, or at most 450 nm, or at most 400 nm.

[0212] In some embodiments, the method is carried out such that the ITM is any ITM described herein and / or the aqueous treatment solution is any aqueous treatment solution described herein.

[0213] In some embodiments, the water-based ink comprises a pigment, a binder, a dispersant, and at least one additive.

[0214] Some embodiments of a printing system will now be described with reference to the accompanying drawings. This description, together with the drawings, will make apparent to those skilled in the art how the teachings of the present disclosure can be implemented, by way of non-limiting examples. These drawings are for illustrative purposes and are not intended to show structural details of the embodiments in more detail than is necessary for a fundamental understanding of the present disclosure. For clarity and simplicity, some objects shown in the drawings are not drawn to scale. [Brief description of the drawings]

[0215] [Figure 1] 1 is a flow chart of a prior art printing process. [Diagram 2] 4 is a flow chart of a printing process according to some embodiments of the present invention. [Figure 3A] FIG. 1 illustrates a printing system or components of a printing system. [Figure 3B] FIG. 1 illustrates a printing system or components of a printing system. [Figure 3C] FIG. 1 illustrates a printing system or components of a printing system. [Figure 3D] FIG. 1 illustrates a printing system or components of a printing system. [Figure 4A] FIG. 1 illustrates a printing system or components of a printing system. [Figure 4B] FIG. 1 illustrates a printing system or components of a printing system. [Diagram 5] FIG. 1 illustrates a printing system or components of a printing system. [Figure 6] FIG. 1 illustrates a printing system or components of a printing system. [Figure 7] FIG. 1 illustrates a printing system or components of a printing system. [Figure 8] FIG. 1 illustrates a printing system or components of a printing system. [Figure 9] FIG. 1 illustrates a printing system or components of a printing system. [Figure 10A]FIG. 1 illustrates a printing system or components of a printing system. [Figure 10B] FIG. 1 illustrates a printing system or components of a printing system. [Figure 11A] FIG. 1 illustrates a printing system or components of a printing system. [Figure 11B] FIG. 1 illustrates a printing system or components of a printing system. [Figure 11C] FIG. 1 illustrates a printing system or components of a printing system. [Figure 11D] FIG. 1 shows shear strength as a function of position. [Figure 12] 4 is a flow chart of a printing process according to some embodiments of the present invention. [Figure 13A] 1A-1C are schematic diagrams illustrating a process by which ink droplets are deposited onto an ITM (eg, a release surface of an ITM). [Figure 13B] 1A-1C are schematic diagrams illustrating a process by which ink droplets are deposited onto an ITM (eg, a release surface of an ITM). [Figure 13C] 1A-1C are schematic diagrams illustrating a process by which ink droplets are deposited onto an ITM (eg, a release surface of an ITM). [Figure 13D] 1A-1C are schematic diagrams illustrating a process by which ink droplets are deposited onto an ITM (eg, a release surface of an ITM). [Figure 13E] 1A-1C are schematic diagrams illustrating a process by which ink droplets are deposited onto an ITM (eg, a release surface of an ITM). [Figure 14A] FIG. 2 shows a mechanically plotted topographical profile of a dry processed thin film produced according to the present invention. [Figure 14B] FIG. 2 shows a mechanically plotted topographical profile of a dry processed thin film produced according to the present invention. [Figure 15A] FIG. 1 shows some examples of ink dots on a paper substrate. [Figure 15B] FIG. 1 shows some examples of ink dots on a paper substrate. [Figure 15C] FIG. 1 shows some examples of ink dots on a paper substrate. [Figure 15D] FIG. 1 shows some examples of ink dots on a paper substrate. [Figure 16] FIG. 2 is a schematic cross-sectional view of a carrier. [Figure 17] 1A-1D are schematic diagrams showing different stages of ITM fabrication according to the present method. [Figure 18] 1A-1D are schematic diagrams showing different stages of ITM fabrication according to the present method. [Figure 19] 1A-1D are schematic diagrams showing different stages of ITM fabrication according to the present method. [Figure 20] 1A-1D are schematic diagrams showing different stages of ITM fabrication according to the present method. [Figure 21] 1A-1D are schematic diagrams showing different stages of ITM fabrication according to the present method. [Figure 22] FIG. 2 is a cross-sectional view of a completed ITM after installation into a printing system. [Figure 23A] 1 is a schematic cross-sectional view of a release layer prepared according to the prior art; [Figure 23B] 1 is a schematic cross-sectional view of a release layer prepared according to the prior art; [Figure 23C] 1 is a schematic cross-sectional view of a release layer prepared according to the present method. [Figure 24A] 1A-1D are schematic diagrams illustrating different stages of manufacture of an apparatus in which some embodiments of the method can be carried out; [Figure 24B] 1A-1D are schematic diagrams illustrating different stages of manufacture of an apparatus in which some embodiments of the method can be carried out; [Figure 24C] 1A-1D are schematic diagrams illustrating different stages of manufacture of an apparatus in which some embodiments of the method can be carried out; [Figure 24D] 1A-1D are schematic diagrams illustrating different stages of manufacture of an apparatus in which some embodiments of the method can be carried out; [Figure 25A] 1 is an image of an ink pattern printed onto the release layer of an ITM of the present invention, where the release layer has been cured to a PET carrier surface. [Figure 25B]1 is an image of an ink pattern printed onto the release layer of an ITM of the present invention, where the release layer has been cured to a PET carrier surface. [Figure 25C] 1 is an image of an ink pattern printed onto the release layer of an ITM of the present invention, where the release layer has been cured to a PET carrier surface. [Figure 26A] 1 is an image of an ink pattern printed onto the release layer of an ITM of the present invention, where the release layer has been air cured. [Figure 26B] 1 is an image of an ink pattern printed onto the release layer of an ITM of the present invention, where the release layer has been air cured. [Figure 26C] 1 is an image of an ink pattern printed onto the release layer of an ITM of the present invention, where the release layer has been air cured. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0216] The present invention will now be described, by way of example only, with reference to the accompanying drawings. With particular reference now to the detailed drawings, it is emphasized that the particulars shown herein are presented by way of example and for illustrative purposes only with respect to preferred embodiments of the present invention, with a view to providing what is believed to be the most useful and easily understood explanation of the principles and conceptual aspects of the present invention. In this regard, it is not at all intended to show structural details of the present invention beyond those required for a fundamental understanding of the present invention. By reading the description in conjunction with the following drawings, it will become apparent to those skilled in the art how several forms of the present invention may be actually implemented. Throughout these drawings, like reference numerals are generally used to refer to like elements.

[0217] definition As used herein, the following terms shall be understood to have the following meanings. a) The term "Receding Contact Angle" or "RCA" refers to a contact angle measured using a Dataphysics OCA15 Pro Contact Angle measuring device or an equivalent Video-Based Optical Contact Angle Measuring System by using the Drop Shape Method. The similar term "Advancing Contact Angle" or "ACA" refers to an advancing contact angle measured by substantially the same method. b) The term "standard aging procedure" refers to an accelerated aging procedure performed on each test release layer in a standard convection oven at 160 degrees Celsius for 2 hours. c) The term "standard air cure" refers to a conventional curing process for curing a release layer, in which the release layer surface (or "ink-receptive surface") is exposed to air during the curing of the release layer. d) The term "bulk hydrophobicity" is characterized by the receding contact angle of a drop of distilled water deposited on the inner surface of the release layer, the inner surface being formed by exposing areas of cured silicone material within the release layer. e) The term "image transfer member" or "intermediate transfer member" or "transfer member" refers to the component of a printing system to which ink is first applied by a print head (e.g. by an inkjet head) and from which the jetted image is then transferred to another substrate or substrates (usually the final print substrate). f) The term "blanket" refers to a flexible transfer member that can be mounted in a printing apparatus to form a belt-like structure over two or more rollers, at least one of which can rotate and move the blanket (e.g., by moving its belt) around the rollers. g) The term "on the release surface" in reference to an object such as an ink image or residual ink means supported by and / or above that release surface. The term "on the release surface" does not necessarily imply direct contact between the ink image or residual ink and the release surface. h) Terms such as "having a static surface tension high enough to increase the static surface tension of the aqueous treatment formulation" with respect to a particular surfactant in the formulation are evaluated by adding additional amounts or portions of that particular surfactant to the formulation and comparing the static surface tension of the formulation achieved with the static surface tension of the formulation prior to adding these amounts. i) The term "liquid moisture absorbent" refers to a moisture absorbent that is liquid at at least one temperature within the range of 25 degrees Celsius to 90 degrees Celsius and that in a pure state has a vapor pressure at 90 degrees Celsius of at most 0.05 ata, more typically at most 0.02 ata, at most 0.01 ata, or at most 0.003 ata. The term "liquid moisture absorbent" is specifically intended to refer to substances such as glycerol. j) "Hydrophobic" and "hydrophilic", among other terms, may be used in a relative sense and not necessarily in an absolute sense. k) The term "(treatment) formulation" refers to a solution or dispersion. l) The evaporation loading at x degrees Celsius (x is a positive integer) is defined herein. If a solution is y% solids (wt / wt) and z% liquid (wt / wt) at x degrees Celsius, then the "evaporation loading at x degrees Celsius" of that solution is the ratio z / y. The units of "evaporation loading" are "weight of solvent / weight of total solute". For the purposes of this disclosure, evaporation loading is always defined at atmospheric pressure. For the purposes of this disclosure, the default value for "x" is 60 degrees Celsius. That is, the term "evaporation loading" without a prefix specifying a temperature refers to the 60 degrees Celsius evaporation loading at atmospheric pressure. m) When a portion of an ITM is in motion with a speed of v meters / sec, this means that the portion of the blanket ITM is moving in a direction parallel to its local position surface / plane, e.g., relative to a stationary applicator, at a speed of at least v meters / sec. n) The term "static surface tension" refers to the static surface tension at 25 degrees Celsius and atmospheric pressure. o) The term "thickness" of a wetting layer is defined as follows: When a substance with volume vol covers the surface area of ​​a surface with area SA with a wetting layer, the thickness of the wetting layer is taken as vol / SA. p) The "thickness" of a dry film is defined as follows: When a material of volume vol, of which x% by weight is liquid, wets or covers a surface of surface area SA, and all the liquid has evaporated to convert the wet layer into a dry film, the thickness of the dry film is considered to be given by the following formula: vol / ρ wet layer (100-x) / ()SA·ρ dry layer ) In the formula, ρ wet layer is the specific gravity of the wet layer, ρ dry layer is the specific gravity of the dry layer. q) The term "continuous wetting layer" refers to a continuous wetting layer that covers a convex region without any small exposed areas within the perimeter of the convex region. r) The term "continuous dry film" refers to a continuous dry film covering a recessed area without any discontinuities within the perimeter of the recessed area. s) The term "Cohesive Film / Tensile Strength" refers to a construct that remains together when peeled from the surface to which it is attached. That is, when peeled from a surface, the "Cohesive Film" retains its structural integrity and peels off as a single film rather than breaking up into small pieces. t) The term "normally applied force" refers to a force that has at least one component in the normal direction. Optionally, a "normally applied" force can have additional components in other directions (e.g., along the surface to which the force is applied). u) Unless otherwise specified, physical properties (e.g., viscosity and surface tension) of liquids (e.g., treatment formulations) refer to properties at 25 degrees Celsius. v) Unless otherwise specified, the term "concentration" refers to weight / weight, i.e. (weight of one component of the formulation) / (total weight of the formulation).

[0218] Explanation of Figure 2 Figure 2 is a flow chart of a method for indirect printing of a water-based ink onto a silicone-based release layer surface of an intermediate transfer member (ITM). In some embodiments, the method of Figure 2 (or any combination of steps of the method of Figure 2) may be performed using the apparatus (or components of such apparatus) disclosed in Figures 3A-3B, 4A-4B, 5-9, 10A-10D, and 11A-11C. In particular, as described below, various embodiments of the present invention relate to methods and apparatus that are useful for producing uniform sub-micron thick wet processing layers over large areas of ITMs and / or at high printing speeds.

[0219] In different embodiments, FIG. 2 can be implemented to produce ink images characterized by any combination of the following features: uniform and controlled dot gain, good and uniform print gloss, and good image quality due to high quality dots with stable dot convexity and / or well-defined boundaries.

[0220] Steps S201-S205 relate to ingredients or components or consumables used in the printing process of FIG. 2, while steps S209-S225 relate to the process itself.

[0221] Briefly, the steps of Figure 2 are as follows: in steps S201 and S205, an ITM (i.e., including a silicone-based release layer surface) and an aqueous treatment formulation (e.g., a solution) are provided, each of which has specific properties as described below. In step S209, the aqueous treatment formulation is applied to the release layer surface of the ITM to form a wet treatment layer on the release layer surface. In step S213, the wet treatment layer is dried to form a dry treatment film on the ITM from the wet treatment layer. In step S217, droplets of aqueous ink are deposited on the dry treatment film to form an ink image on the ITM surface. In step S221, the ink image is dried to leave a residual ink image on the ITM surface, and in step S225, the residual ink image is transferred to a print substrate.

[0222] Various embodiments of the present invention relate to methods, apparatus, and kits for achieving the potentially competing objectives of dot gain, image gloss, and dot quality, preferably in a production environment where high printing speed is paramount. According to some embodiments, the inventors have found it useful to carry out the method of FIG. 2 such that the dried processing film formed in step S213 is very thin (e.g., up to 150 nanometers, or up to 120 nanometers, or up to 100 nanometers, or up to 80 nanometers, or up to 70 nanometers, or up to 60 nanometers, or up to 50 nanometers, and optionally at least 20 nanometers, or at least 30 nanometers), and / or continuous over a large area, and / or characterized by a very smooth upper surface, and / or rich in quaternary ammonium salts (e.g., to promote dot gain), and / or has properties that promote good transfer from the ITM to the substrate (i.e., properties of the film itself, or properties of the film relative to the ITM surface).

[0223] For example, thicker treatment films can have a detrimental effect on the gloss or uniformity of the treatment film because, after transfer, dried residual ink can be present underneath the treatment film and on the substrate surface. Therefore, it can be preferable to produce very thin treatment films.

[0224] For example, discontinuities in the treatment film and / or varying thickness of the treatment film may result in a non-uniform gloss image on the substrate or may produce a residual ink image (in step S113) that loses its mechanical integrity when transferred to the substrate. It may therefore be preferable to produce a treatment film that is continuous over a large area (preferably with sufficient cohesion to maintain structural integrity on the print substrate) and / or has thermo-rheological properties such that the treatment film is tacky at transfer temperatures of 75 degrees Celsius to 150 degrees Celsius.

[0225] For example, the presence of quaternary ammonium salts in the dried processing film can promote ink droplet spreading, but not necessarily uniform ink droplet spreading. However, the combination of (i) a high concentration of quaternary ammonium salts in the dried processing film and (ii) a uniform thickness processing film with a very smooth upper surface can promote uniform ink droplet spreading.

[0226] Various embodiments of the present invention are directed to techniques for achieving these results simultaneously, even though these results entail potentially competing objectives. For example, if the process film is required to be very thin, it can be difficult to form a process film that is continuous over a large area, and / or has sufficient coherence for good transfer to the substrate, and / or has a very smooth and uniform upper surface.

[0227] Explanation regarding step S201 The ITM provided in step S201 has a silicone-based release layer whose release surface may be less hydrophobic or appreciably less hydrophobic than many conventional silicone-based release layers. This structural property may be measured and characterized in a variety of ways.

[0228] For example, as shown in step S201 of FIG. 2, an intermediate transfer member (ITM) includes a silicone-based release layer surface that exhibits sufficient hydrophilicity to satisfy at least one of the following characteristics: (i) a distilled water droplet deposited on the silicone-based release layer surface has a receding contact angle of up to 60 degrees; and (ii) a 10-second dynamic contact angle (DCA) of up to 108 degrees for a distilled water droplet deposited on the silicone-based release layer surface.

[0229] Any one of several techniques for reducing the hydrophobicity of a silicone-based release layer can be used.

[0230] In some embodiments, polar functional groups are introduced into and / or generated in the silicone-based release layer.In one case, functional groups are added to a prepolymer batch (e.g., monomers in solution), and these functional groups can become an integral part of the silicone polymer network when cured.Alternatively or additionally, the silicone-based release layer is pretreated (e.g., by corona discharge or by electron beam), thereby increasing the surface energy of the release layer.

[0231] Alternatively, silicone-based release layers can be fabricated to have low hydrophobicity even when substantially free of functional groups. In one case, the silicone polymer backbone of the release layer can be constructed such that its polar groups (e.g., O-Si-O) are oriented approximately perpendicular to the local plane of the ITM surface and face "upward" toward the release layer surface.

[0232] The inventors presently believe that the technique in the previous paragraph provides superior image transfer (step S225).

[0233] Explanation of step S205 in FIG. 2 One characteristic of the aqueous treatment formulation provided in step S205 is that the aqueous treatment formulation has a static surface tension in the range of 20-40 dynes / cm. For example, the aqueous treatment formulation includes one or more surfactants.

[0234] The aqueous processing formulation of step S205 is therefore less hydrophilic than many conventional processing solutions, and significantly less hydrophilic than water.

[0235] In some embodiments, the combination of (i) a silicone-based release layer (step S201) having low hydrophobicity and (ii) an aqueous treatment formulation having low hydrophilicity reduces (but does not necessarily eliminate) the surface tension effects that promote beading of conventional aqueous treatment solutions.

[0236] In addition to a static surface tension in the range of 20-40 dynes / cm, the aqueous treatment formulation provided in step S205 has the following properties: The aqueous processing formulation includes at least 3% by weight of a quaternary ammonium salt, which is useful in ensuring that the dried processing film (i.e., produced in step S217) is rich in quaternary ammonium salts. The aqueous processing formulation comprises at least 1% by weight (e.g., at least 1.5%, or at least 2%, or at least 3%) of at least 5% of at least one water soluble polymer (having a water solubility of at least 5% at 25 degrees Celsius), which may be useful in promoting the formation of a polymer film or polymer matrix in the dried processing film (produced in step S217) that has sufficient cohesion for good transfer in step 225. c. A 25° C. viscosity coefficient of at least 10 cP. As explained below, high viscosity is useful in counteracting any tendency due to surface tension toward beading. d. A 60 degree Celsius evaporation load by weight of up to 8:1 (e.g., up to 7:1, or up to 6:1, or up to 5:1, or up to 4:1). Thus, the solution has a low specific heat capacity compared to conventional processing formulations that have a higher evaporation load. Furthermore, for a particular required residual thickness for an aqueous processing solution and for a given heat power delivered to the aqueous processing solution, the viscosity of the aqueous processing formulation will increase rapidly as a function of evaporation to achieve a high absolute viscosity that effectively counteracts surface tension forces.

[0237] Physically, it is more difficult to induce flow of a fluid with a high viscosity than a fluid with a lower viscosity. That is, a larger driving force is required to induce flow of a fluid with a higher viscosity. The combination of at least a moderate initial viscosity (i.e., a 25° C. viscosity coefficient of at least 10 cP) and a rapid viscosity increase after evaporation on the ITM surface (e.g., due to a low evaporation load) ensures that the aqueous treatment formulation achieves a relatively "high" (e.g., at least 10,000 cP) viscosity in a relatively short time period (e.g., up to 1 second or up to 0.5 seconds). Thus, even if there is any thermodynamic tendency toward beading, actual beading, which may adversely affect the properties of the dried treatment film (i.e., formed in step S213), is prevented or appreciably mitigated.

[0238] In some embodiments, the 25° C. viscosity of the initial aqueous treatment formulation may be at least 12 cP, or at least 14 cP, such as in the range of 10-100 cP, 12-100 cP, 14-100 cP, 10-60 cP, or 12-40 cP.

[0239] In summary, the combination of (A) a release layer that is sufficiently hydrophilic to satisfy at least one of the following characteristics: (i) a receding contact angle of a distilled water droplet deposited on the silicone-based release layer surface of at most 60 degrees; and (ii) a 10-second dynamic contact angle (DCA) of a distilled water droplet deposited on the silicone-based release layer surface of at most 108 degrees, and (B) a static surface tension of the aqueous treatment formulation in the range of 20-40 dynes / cm, is useful in minimizing the magnitude of the thermodynamic driving force that can cause beading. Additionally, the viscosity-related features discussed above are useful in resisting this driving force.

[0240] Countering this tendency and reducing the magnitude of the thermodynamic forces driving beading ensures that any tendency to cause beading does not prevent the formation of a wet layer of treatment formulation having a uniform thickness in step S209.

[0241] In various embodiments of the present invention, the aqueous treatment formulation comprises a carrier liquid that includes water, the water comprising at least 65% by weight (eg, at least 70% or at least 75%) of the aqueous treatment formulation.

[0242] Explanation regarding step S209 In step S209, an aqueous treatment formulation is applied to the silicone-based release layer surface of the ITM to form a wet treatment layer having a thickness of 0.8 μm (e.g., up to 0.7 μm, or up to 0.6 μm, or up to 0.5 μm) on the release layer surface.

[0243] The "thickness of a wetting layer" is defined as follows: when a material with a volume vol covers the surface area of ​​a surface with area SA with a wetting layer, the thickness of the wetting layer is taken as vol / SA.

[0244] Preferably, step S209 is performed such that the wetting process layer is uniform in thickness and free of defects, preferably over a large area (e.g., the entire area of ​​the release layer), which can be particularly difficult when the wetting process layer is sub-micron thick.

[0245] As mentioned above, to counteract beading, it is useful for the aqueous treatment formulation to have at least a "moderate viscosity" (e.g., a 25° C. viscosity coefficient of at least 10 cP). Nevertheless, at such viscosities, there can be challenges associated with obtaining an aqueous treatment formulation that is both uniform and of sub-micron thickness.

[0246] In step S209, the aqueous treatment formulation is applied onto the silicone-based release layer surface to form a wet treatment layer having a thickness of up to 0.8 μm.

[0247] Various embodiments of the present invention relate to apparatus and methods for applying this wet processing layer, preferably to a uniform thickness over a large area of ​​the ITM.

[0248] In some embodiments, after coating the ITM surface with an initial coating of the aqueous treatment formulation, excess treatment formulation may be removed from the initial coating to obtain a wet treatment layer having a uniform thickness of up to 0.8 μm.

[0249] In some embodiments, this may be accomplished by forcing a highly rounded surface (e.g., of a doctor blade) towards or away from the ITM. For example, the radius of curvature of the highly rounded surface may be up to 1.5 mm, or up to 1.25 mm, or up to 1 mm.

[0250] At high printing speeds (e.g., when the surface velocity of the ITM is relatively high (e.g., at least 1 meter / sec, or at least 1.25 meters / sec, or at least 1.5 meters / sec)), removing excess liquid to form a treatment layer having a sub-micron thickness requires a relatively large velocity gradient (i.e., shear) - e.g., at least 10 - in the gap region between the highly surface and the ITM (i.e., the velocity gradient is normal to the ITM surface). 6 / sec, or at least 2×10 6 This may entail establishing a velocity gradient of 1 / sec.

[0251] As mentioned above, the 25° C. viscosity of the treatment formulation may be at least 10 cP. Even if step S209 is performed at higher pressures, the viscosity at these higher temperatures may be at least 3 cP, or at least 5 cP, or at least 10 cP. Thus, in some embodiments of the invention, a relatively large force (e.g., to urge a very rounded surface towards (or away from) the ITM) is required to achieve the required uniform thickness of less than 0.8 μm (preferably).

[0252] In some embodiments, the rounded surface is forced against the ITM, or the ITM is forced against the rounded surface, with a force density in the cross print direction of at least 250 g / cm, or at least 350 g / cm, or at least 400 gm / cm, and / or up to 1 kg / cm, or up to 750 g / cm, or up to 600 g / cm.

[0253] In some embodiments, the wet treatment layer is formed by applying pressure between the applicator and the ITM, the magnitude of the pressure being at least 0.1 bar, or at least 0.25 bar, or at least 0.35 bar, or at least 0.5 bar, and optionally up to 2 bar, or up to 1.5 bar, or up to 1 bar.

[0254] Explanation regarding step S213 In step S213, the wet processed layer is subjected to a drying process, and a dry processed thin film is formed from the wet processed layer.

[0255] For example, during the drying process of the wet processing layer, the dynamic viscosity of the wet processing layer increases by at least 1000 times within a time period of up to 0.5 seconds, or up to 0.25 seconds.

[0256] In some embodiments, the thickness of the dried treatment film (eg, the coherent polymer treatment film) is at most 150 nanometers, or at most 120 nanometers, or at most 100 nanometers, or at most 80 nanometers, or at most 60 nanometers.

[0257] In some embodiments, the dried treatment film has a smooth upper surface, for example, the drying of the wet treatment layer is carried out quickly enough that the viscosity of the aqueous treatment formulation increases quickly enough such that surface tension induced beading is inhibited and the dried treatment film has a smooth upper surface.

[0258] In some embodiments, the smooth upper surface of the dried treated film has an average roughness R of at most 12 nanometers, or at most 10 nanometers, or at most 9 nanometers, or at most 8 nanometers, or at most 7 nanometers, or at most 5 nanometers. a Those skilled in the art are directed to Figure 13 and the accompanying discussion.

[0259] In some embodiments, the dry treatment film is continuous across a rectangle of the release surface of the ITM, the rectangle having a width of at least 10 cm and a length of at least 10 meters.

[0260] In some embodiments, the treatment film is transparent.

[0261] One purpose of the dry treatment film is to protect the ITM surface from direct contact with aqueous ink droplets deposited on the treatment film. However, the aqueous ink droplets may "erode through" the thickness of the dry treatment film, especially when the dry treatment film is thin (e.g., up to 150, or up to 120, or up to 100, or up to 80 nanometers). Thus, in some embodiments, the water-soluble polymer concentration (by weight) of the water-soluble polymer in the aqueous treatment formulation provided (e.g., in step S205 of FIG. 2 or step S95 of FIG. 12) is up to 10%, or up to 8%, or up to 6%, or up to 5%.

[0262] Explanation of steps S217 to S221 In step S217, droplets of the water-based ink are deposited (e.g., by ink drop deposition) onto the dried treatment film to form an ink image on the ITM surface. In step S221, the ink image is dried to leave a residual ink image on the ITM surface.

[0263] For example, the presence of a quaternary ammonium salt in the dried process film is useful in promoting dot spreading and / or dot gain (e.g., uniform dot spreading and / or dot gain) when the droplets are deposited or shortly thereafter. Those skilled in the art are guided by the following description with reference to Figures 13A-13E. As discussed above, the formation of a dried process film (in step S213) having a uniform thickness and / or being free of defects and / or having a very smooth upper surface may promote uniform flow of the water-based ink over the upper surface of the film.

[0264] Explanation regarding step S225 In step SS25, the residual ink image is transferred to a substrate, for example, the residual ink image is transferred, along with the non-printed areas of the dried processing film, onto a print substrate.

[0265] In some embodiments, the dry treatment film has sufficient cohesion such that during transfer of the residual ink image, the dry treatment film completely separates from the ITM in both printed and non-printed areas and is transferred to the printing substrate along with the dry ink image.

[0266] In some embodiments, the temperature of the ITM during transfer is in the range of 80 degrees Celsius to 120 degrees Celsius. In some embodiments, the ITM temperature is up to 100 degrees Celsius, or up to 90 degrees Celsius. In some embodiments, the ITM temperature is at least 100 degrees Celsius, or at least 110 degrees Celsius, or at least 120 degrees Celsius.

[0267] In some embodiments, the presence of an aqueous processing solution water-soluble polymer in the aqueous processing solution provided in step S205 helps ensure that the dried processing film formed in step S213 has sufficient coherence during transfer (e.g., by forming a polymer film or polymer matrix).

[0268] In some embodiments, the substrate on which the ink image resides is glossy paper (eg, glossy coated paper).

[0269] The transfer may be perfect (i.e., the entire residual ink image and dried processing film is transferred to the substrate). Alternatively, the transfer may be less than perfect. To this end, a cleaning station cleans off any material remaining on the ITM surface after the transfer step of S225.

[0270] Description of Figures 3A to 3B In Figure 3A, a schematic diagram of a system for indirect printing according to some embodiments of the present invention is shown. The system of Figure 3A includes an intermediate transfer member (ITM) 210 that includes a flexible endless belt mounted on a number of guideable rollers 232, 240, 250, 251, 253, 242. In other cases (not shown), the ITM 220 is a drum or a belt wrapped around a drum.

[0271] 3A, the ITM 210 (i.e., the belt of the ITM 210) moves in a clockwise direction. The belt movement direction defines an upstream direction and a downstream direction. Rollers 242, 240 are located upstream and downstream, respectively, of the image-forming station 212. Thus, roller 242 may be referred to as the "upstream roller" and roller 240 as the "downstream roller."

[0272] The system in Figure 3A (a) an image forming station 212 (e.g., including print bars 222A-222D, each including an inkjet head portion(s)) configured to form an ink image (not shown) on a surface of the ITM 210 (e.g., by droplet deposition onto a dried processing film - see, e.g., step S217 of FIG. 2 or step S109 of FIG. 12 ); (b) a drying station 214 for drying the ink image (see, e.g., step S221 of FIG. 2 or step S113 of FIG. 12); (c) the ink image is transferred from the surface of the ITM 210 to a sheet or textile substrate (see, e.g., step S225 of FIG. 2 or step S117 of FIG. 12) or impression station 216; 3A, the impression station 216 includes an impression cylinder 220 and a blanket cylinder 218 that holds a compressible blanket 219. In some embodiments, a heater 231 may be provided just prior to the nip between cylinders 218 and 220 of the image transfer station to help impart tack to the ink film to facilitate transfer to the substrate (e.g., a sheet substrate or a woven substrate). The substrate supply is shown diagrammatically. (d) a cleaning station 258 (i.e., shown diagrammatically as a block in FIG. 3A ) where residual material (e.g., the processed processed film and / or ink image or portions thereof) is cleaned from the surface of the ITM 210 (cleaning step not shown in FIG. 2 ); (e) a layer (e.g., having a uniform thickness) of a liquid treatment formulation (e.g., an aqueous treatment formulation) is formed on the ITM surface (e.g., see step S209 of FIG. 2 or step S101 of FIG. 12) at a treatment station 260 (i.e., shown diagrammatically as a block in FIG. 3A ); Further includes:

[0273] Those skilled in the art will appreciate that not all of the components illustrated in FIG. 3A are required.

[0274] In FIG. 3B, multiple "locations" Loc A ~Loc J is shown. A Located at Rolla 242, Loc B is the "start point" of the image station 212, Loc C LocA is the "end" of image station 212, etc. Thus, an ink image is formed (see, e.g., step S217 of FIG. 2) in the region between location LocA and location LocB in image station 212 on the upper stroke of ITM 210. The ink image is then moved to location LocB to form the residual ink image. C and location Loc E (See, e.g., step S221 of FIG. 2 and step S105 of FIG. 12). This drying occurs as the ink image moves through the drying station 214 (e.g., by clockwise rotation of the ITM). The residual ink image is dried at the location Loc E and location Loc F The material remaining on the surface of the ITM 210 after transfer of the residual ink image is transferred to the substrate at the impression station 216 between the positions Loc G and location Loc H The wet processing layer may be cleaned from the surface of the ITM 210 at a cleaning station 258 between the locations Loc I and location Loc J2 (or step S101 of FIG. 12) on the surface of the ITM 210 in a processing station 260 located between the ITM 210 and the processing station 260 (see, for example, step S209 of FIG. 2 or step S101 of FIG. 12). This wet processing layer is then subjected to a drying process (i.e., to convert the wet processing layer into a dry processing thin film) (see, for example, step S213 of FIG. 2 or step S105 of FIG. 12). The drying process is performed at the right-hand position Loc J and location Loc A After the dry treatment film is transported to the imaging station 212 (e.g., by counterclockwise rotation of the ITM 210), an ink image may subsequently be formed by droplet deposition on the dry treatment film (e.g., see step S217 of FIG. 2 or step S109 of FIG. 2).

[0275] As shown in FIG. 3A-FIG. 3B, the position Loc A and location Loc D The portion of the ITM between is the upward stroke of the ITM 210 (i.e., the belt of the ITM 210). This upward stroke (shown in FIG. 3C) is between (i) the upstream guide roller 242, which is upstream relative to the imaging station 212, and (ii) the downstream guide roller 240, which is downstream relative to the imaging station 212. The upward stroke passes through the imaging station 212.

[0276] The downward stroke of the ITM is at the ITM210 position Loc D and location Loc A 3D. The downward stroke passes through impression station 216, cleaning station 258, and treatment station 260.

[0277] An example of a processing station is shown in FIG. 4A.

[0278] In the particular non-limiting embodiment of Figure 4A, the ITM 210 is moved from right to left, as represented by arrow 2012, above a doctor blade generally designated by reference numeral 2014 and preferably mounted in a tank 2016. In Figure 4A, the doctor blade 2014 is of the doctor rod type and formed from a rigid bar or holder 2020 that extends across the entire width of the ITM 210. On its upper surface opposite the lower surface of the ITM 210, the bar 2020 is formed with a channel or groove 24. Supported within the groove 24 is a bar 2022 made of quartz glass and having a smooth and regular cylindrical surface with a roughness of only a few microns (preferably less than 10 microns, in particular less than 0.5 microns).

[0279] Prior to passing over the doctor blade 2014, the underside of the ITM 210 (or downward stroke) is coated with an excess of processing formulation (e.g., solution) 2030 (e.g., provided in step S205 of FIG. 2 or step S95 of FIG. 12). In this illustrative example, the manner in which the excess processing formulation (e.g., solution) is applied to the ITM 210 (and particularly its underside) is not essential to the invention, as will be described below with reference to FIG. 5. The ITM 210 may, for example, simply be immersed in a tank containing liquid, may be passed over a jet of processing formulation (e.g., solution), or may be sprayed using an upward jet 1128 as shown in FIG. 5.

[0280] In one embodiment of the invention, a liquid-permeable fabric is placed above an upwardly facing spray head so that the liquid penetrates the fabric and forms a layer on the side of the fabric facing the surface to be coated. In this case, the spray head will act to urge the fabric towards the surface, but prevents the liquid penetrating the fabric from contacting the surface, which acts in a similar manner to how it does in a fluid bearing.

[0281] As shown in the figure, as the ITM 210 approaches the doctor blade 2014 , the ITM 210 has a coating 2030 of liquid that is significantly greater than the desired thickness of the film to be applied to the ITM 210 .

[0282] The function of the doctor blade 2014 is to remove excess liquid 2030 from the ITM 210 and ensure that any remaining liquid is spread evenly and uniformly across the surface of the ITM 210. To accomplish this, the ITM 210 is urged towards the doctor blade 2014, for example by air pressure (not shown). Alternatively, the force urging the ITM 210 towards the doctor blade 2014 may in some embodiments be a backing roller 1141, such as a sponge roller, which presses (e.g. by its own weight or by the action of a spring) downward against the upper or opposite side of the web. As a further alternative, the doctor blade 2014 itself may be urged towards the ITM 210, keeping the ITM 210 under tension.

[0283] The tip of the doctor blade 2014, which consists of a cylindrical smooth bar 2022, has a uniform radius across the width of the ITM 210, and its smoothness ensures laminar flow of liquid in the gap between the tip and the underside of the ITM 210. The nature of this flow, which may be similar to that of liquid lubricants in hydrodynamic bearings, reduces a thin film of liquid 2030 that remains attached to the underside of the ITM 210 (i.e., the surface of the "down stroke" of the ITM) to a thickness that depends on the force biasing the ITM against the doctor blade 2014 and the radius of curvature of the bar 2022. Because both the radius and force are constant across the width of the fabric, the resulting thin film is uniform, and its thickness can be set by appropriate selection of the applied force and bar diameter. Excess liquid removed by the doctor blade 2014 creates a small pool 2032 just upstream of the bar 2022 before falling into the tank 2016.

[0284] In an alternative embodiment of the invention, the surface of the ITM 210 to be coated with liquid may face upward instead of downward. In this case, instead of applying an excess of liquid to the ITM 210 (i.e., the "down stroke" surface of the ITM), liquid is metered onto the surface such that a small pool of liquid similarly grows and is maintained at the contact line between the wiper blade and the upper surface of the fabric. An air knife may be provided in this case to prevent the treatment formulation (e.g., solution) from the pool from flowing over the lateral edges of the ITM 210.

[0285] In various embodiments of the invention, pool 2032 provides a constant supply of treatment formulation (e.g., solution) across the entire width of the ITM 210 so that the entire area of ​​the ITM 210 is covered, even if the liquid is, for some reason, repelled from part of the surface of the fabric (e.g., by "beading") before reaching the doctor blade 2014.

[0286] The tank 2016 into which the excess treatment formulation (e.g., solution) falls may be a main storage tank from which the liquid is sucked for coating the underside of the fabric, or the tank 2016 may be a separate tank that drains into the main storage tank and / or is poured into a suitable disposal system.

[0287] The rod 2022 is made of a hard material such as quartz glass to resist wear. Small particles such as grit or dust may be present in the liquid and may damage the rounded edges along which the liquid flows. It may be possible to use materials other than quartz glass, but the material used should preferably have a Brinell hardness of more than 100 (e.g., more than 200, more than 500, or even more than 1000). In various embodiments of the invention, the material used should be capable of being formed into a smooth rod with a uniform diameter and a surface roughness of less than 10 microns (particularly less than 0.5 microns).

[0288] The rod 2022, which may have a radius of 6 mm, but possibly only 0.5 mm, is relatively fragile and may require the bar 2020 for support. To hold the rod 2022 precisely in place, the bar 2020 is provided with a groove 24 in which the rod 2022 rests. The rod 2022 may be held in the groove 24 in any suitable manner. For example, an adhesive may be used to press the rod 2022 against a flat surface, such as a glass plate, using the bar 2020 until the adhesive sets. As a further alternative, the groove 24 may be precisely machined to be slightly narrower than the diameter of the rod 2022, and heat shrink may be used to hold the rod 2022 in place in the groove 24.

[0289] When such doctor blades are used to apply a particular formulation (e.g., solution), a deposit 34 of the solution accumulates downstream of the doctor blade 2014. Without wishing to be bound by theory, it is believed that this phenomenon may be due to the fact that a stationary thin film of the formulation (e.g., solution) adheres to the downstream side of the doctor blade and as such film dries, solutes are left behind. Regardless of the reason for the formation of such deposits and their composition, if allowed to grow excessively, such deposits will eventually interfere with the layer of processing formulation (e.g., solution) being applied to the ITM 210.

[0290] Various embodiments of the present invention relate to an apparatus and method for switching doctor blade 2014 when it becomes soiled. In Figure 4B, an example is shown for easily switching doctor blades without interrupting the fabric coating process or printing system that preferably requires a conditioner to be applied to its ITM.

[0291] In FIG. 4B, twelve doctor blades 1122 are evenly mounted in recesses arranged around the circumference of a cylindrical rotatable turret 1120. The axially extending doctor blades 1122 behave similarly to the doctor rod 1122 of FIG. 4A, and the turret 1120 has the same purpose as the rod holder 2020. Instead of using a rod of circular cross section, the doctor blades 1122 are constructed as strips with smooth, rounded and polished edges. Strips with rounded edges of uniform radius of curvature can be produced, for example, by flattening a rod of circular cross section. The doctor blades 1122 are preferably made of stainless steel, but alternatively, other hard materials resistant to wear can be used.

[0292] The manner in which the turret 1120 and doctor blade 122 interact with the ITM 110 is shown in FIG. 5, which shows an example of a cleaning station 258 and a processing station 260 (e.g., a station for applying a wet layer of a processing formulation, see step S209 of FIG. 2 or step S101 of FIG. 2).

[0293] In the case of Figure 5, two separate tanks 1125, 1127 are shown. A quantity of processing solution (e.g., having the characteristics(s) of step S205 of Figure 2 or step S95 of Figure 12) is stored in tank 1125. For example, the processing solution may be squirted (i.e., by squirting device 774) onto the surface of the ITM 210. Brushes 1126A and 1126B are also shown in Figure 5 for mechanically removing material from the surface of the ITM 210 and cleaning the ITM surface. For example, pressure may be applied between backing roller 772A located opposite brush 1126A and backing roller 772B located opposite brush 1126B.

[0294] In some embodiments, the material removed from the surface of the ITM includes a dry processing film that may be redissolved, for example, in a liquid processing formulation (e.g., having particularity(s) of step S205 of FIG. 2 or step S95 of FIG. 12) stored in tank 1125. This may allow for recycling of the processing formulation.

[0295] Regardless of the mechanical properties of the system, in various embodiments of the present invention, the aqueous treatment formulation provided in step S205 of FIG. 2 or step S95 of FIG. 12 is fully redissolvable (e.g., can be fully dissolved in the aqueous treatment formulation after drying).

[0296] The treatment formulation 1128 can be ejected by an ejection device 1128. In the example of FIG. 5, one of the doctor blades 1122 is enabled, and the enabled doctor blade is 1122. ACTIVE A relatively thick layer of the treatment formulation is applied (e.g., by device 1128) and excess treatment formulation is removed by doctor blade 1122. ACTIVE and Doctor Blade 1122 ACTIVE and a backing roller 1141 urged towards the

[0297] The jetting device 1128 is an example of a "applier" for applying a coating of a treatment formulation to the surface of the ITM 210. Another example of a applicator is a pool 2032 when the liquid content of the pool is held on the ITM surface.

[0298] Doctor Blade 1122 ACTIVE (or Doctor Blade 1122 ACTIVE 10A and 11A , the rounded tip 1123 and the backing roller 1141 (or alternatively a device for providing air pressure towards the rounded tip 1123) collectively form a coating thickness adjustment assembly, in which the “final thickness” of the treatment formulation can be adjusted according to the amount of force urging the tip 1123 towards the opposing portion of the ITM 210 (e.g., towards the backing roller 1141) or vice versa.

[0299] In the case of FIG. 5, only one doctor blade 122 interacts with the ITM 110 at any given time, but if a blade becomes fouled, the turret 120 is rotated to bring the next adjacent doctor blade into an operating position where it can function (i.e., close enough to the surface to remove excess liquid and allow only a thin film of the desired thickness to be deposited on the downstream surface of the apparatus).

[0300] Before returning to the operating position, at some later stage in the turret rotation cycle, the fouled blade 1122 passes through a cleaning device (e.g., brush 1130) which removes any deposits and cleans the blade, after which it is restored to functionality.

[0301] Rotation of the turret 1120 may occur on demand by an operator or may be performed at regular intervals.

[0302] The number of doctor blades on the turret 1120 does not necessarily have to be twelve, but preferably there are enough so that during changeover, there is time for two doctor blades 1122 to function simultaneously and interact with the ITM 110, as shown in Figures 8-9, so that there is sufficient continuous exchange of blades so that there is no interruption in the thin film dispensing operation, and therefore doctor blade changeover is possible without interruption to the printing system.

[0303] 8-9 are more detailed perspective enlarged cross-sectional views of the turret 1120 and doctor blade cleaning brush 1130, respectively. Both are mounted on axles rotatably supported in a metal frame 1140 submerged in the tank 1127. The axles of the turret 1120 and doctor blade cleaning brush 1130 are connected to drive motors 1412 and 1144 mounted outside the tank 1127. As can be seen from FIG. 7, the turret 1120 is made from a hollow cylinder, whose cylindrical surface can be perforated so that its weight and moment of inertia are reduced while still providing sufficient strength to support the doctor blade 1122.

[0304] Although the doctor blade 1122 supported by the turret 1120 is shown as a flat strip, it should be understood that the doctor blade 1122 may alternatively be formed as a circular rod as described with reference to FIG.

[0305] Vigorous agitation of a solution of modifier is known to cause bubbles or foam to form for certain modifiers. Ultrasound can be used to break up the bubbles, and such a foam inhibitor can be incorporated into the tank 1125.

[0306] As shown in FIG. 10A, a doctor blade 1122 ACTIVE When the ITM 210 is urged toward the backing roller 1141 (or vice versa), the doctor blade can move toward the downward stroke of the ITM 210. As shown in FIG. 10A, the ITM 210 (i.e., the downward stroke of the ITM 210) is caused by the roller 1141 and the doctor blade 1122. ACTIVE The roller 1141 is therefore disposed between the doctor blade 1122. ACTIVE When the roller 1141 is biased toward the ITM 210, the roller 1141 presses against the ITM 210 (i.e., the downward stroke of the ITM 210), which in turn presses against the doctor blade 1122. ACTIVE and vice versa.

[0307] In the example of FIGS. 10A-10B, the doctor blade 1122 ACTIVE 10A-10B, the doctor blade 1122 is shown. ACTIVE The rounded tip of is labeled as 1123.

[0308] In the case of FIG. 10A, the tip 1123 faces the surface (i.e., the local normal) of the ITM 210. In the case of FIG. ACTIVE is oriented substantially perpendicular to the local surface of the ITM 210 opposite the rounded tip 1123.

[0309] In the case of Figure 10A, a downward force is applied by roller 1141 (i.e., via the ITM) towards the rounded tip 1123. Alternatively, air pressure can be used to urge the ITM 210 towards the rounded tip 1123. As a result, the doctor blade 122 ACTIVE will remove all but a thin film of liquid (eg, typically less than 1 micrometer) whose thickness is determined by the radius of curvature and the applied pressure.

[0310] The jetting device 1128, or a treatment bath into which the ITM surface may be immersed, or any other device for applying an initial coating, may be considered a "coater" for coating the ITM with a liquid treatment formulation. Additionally, the combination of (i) the rounded surface 1123 (e.g., a rounded tip) and a device for applying an opposing force (e.g., roller 1141) to urge the rounded surface 1112 toward the opposing surface of the ITM 210 forms a thickness control assembly for removing excess liquid so that only a layer of the desired uniform thickness (e.g., sub-micron thick) of the treatment formulation remains.

[0311] In various embodiments of the present invention, even if the rounded tip 1123 does not contact the opposing ITM surface (e.g., to maintain a gap between the tip and the ITM surface), the applicator may still indirectly apply pressure to the ITM via the processing fluid.

[0312] In some embodiments, the rounded tip applies a pressure of at least 0.1 bar, or at least 0.25 bar, or at least 0.35 bar, or at least 0.5 bar, and optionally up to 2 bar, or up to 1.5 bar, or up to 1 bar.

[0313] The pressure can be localized in the print direction. For example, a "strip of pressure" (e.g., the strip can be elongated in the cross-print direction) (e.g., having a length of at least 10 cm, or at least 30 cm, or at least 50 cm) has (i) a maximum pressure applied to the ITM within the strip is P_STRIP_MAX, the value of P_STRIP_MAX being at least 0.1 bar, or at least 0.25 bar, or at least 0.35 bar, or at least 0.5 bar, and optionally up to 2 bar, or up to 1.5 bar, or up to 1 bar; and At all positions within the strip, the local pressure applied by the applicator to the ITM is at least 0.5×P_STRIP_MAX, and (iii) at all positions on opposite sides in the cross-printing direction of the strip (upstream side and downstream side—spaced up to 2 cm, or up to 1 cm, or up to 5 mm, or up to 3 mm, or up to 2 mm, or up to 1 mm, or up to 0.5 mm from the strip), the maximum pressure may be applied by the applicator to the ITM of up to 0.2×P_STRIP_MAX or up to 0.1×P_STRIP_MAX.

[0314] As shown in Figure 11A, the presence of a rounded tip 1123 (e.g., a doctor blade) (e.g., held stationary) can create a shear field or velocity gradient (see, e.g., Figures 11B and 11C). At the ITM surface, the velocity of the processing fluid can be non-zero (e.g., substantially equal to the velocity of the ITM) due to non-sticky boundary conditions, and at the applicator, the velocity of the processing liquid can be zero.

[0315] In some embodiments, i. the formation of the thin wetting treatment layer (e.g., in step S209 of FIG. 2 or step S101 of FIG. 12 ) is performed at a strong velocity gradient IVG position x=x that is (i) vertically spaced (e.g., up to 3 microns, or up to 2 microns, or up to 1 micron) from the stripping surface of the ITM and / or between the applicator and the stripping surface of the applicator. IVG_location ii. at the IVG position, the magnitude of the velocity gradient is equal to or exceeds a VG value, the VG value being at least 10 6 / sec, or at least 2×10 6 / sec, or at least 4×10 6 / sec, or at least 5×10 6 / sec, or at least 7.5 × 10 6 / sec, or at least 10 7 / sec, or at least 2×10 7 / sec, or at least 4×10 7 / sec, or at least 5×10 7 / sec, or at least 7.5 × 10 7 / second.

[0316] In some embodiments, the velocity gradient is: i. at an upstream location that is upstream of the IVG location, the maximum velocity gradient is up to x% of the value of the velocity gradient at the IVG location; ii. at a downstream location downstream of the IVG location, the maximum velocity gradient is up to x% of the value of the velocity gradient at the IVG location; iii.x has a value of at most 50, or at most 30, or at most 20, or at most 10, and / or iv. the upstream and downstream locations are each spaced a maximum of 2 cm, or a maximum of 1.5 cm, or a maximum of 1.25 cm, or a maximum of 1 cm, or a maximum of 9 mm, or a maximum of 8 mm, or a maximum of 7.5 mm, or a maximum of 7 mm, or a maximum of 6 mm, or a maximum of 5 mm from the IVG location; It is localized along the print direction.

[0317] In some embodiments, the rounded surface is forced against the ITM, or the ITM is forced against the rounded surface, with a force density in the cross print direction of at least 250 g / cm, or at least 350 g / cm, or at least 400 gm / cm, and / or up to 1 kg / cm, or up to 750 g / cm, or up to 600 g / cm.

[0318] Explanation of Figure 12 Various aspects of the invention relate to a printing process as illustrated in FIG. 12. In some non-limiting embodiments, the apparatus, systems, and devices illustrated in FIGS. 3-11 may be used to perform the method of FIG. 12. The order of steps in FIG. 12 is not intended to be limiting, and in particular steps S91-S99 may be performed in any order. In some embodiments, steps S101-S117 are performed in the order shown in FIG. 12.

[0319] In some embodiments, step S91 may be performed to provide any feature or combination of features of step S201 of FIG.

[0320] In some embodiments, step S95 may be performed to provide any feature or combination of features of step S205 of FIG.

[0321] In some embodiments, step S101 may be performed to provide any feature or combination of features of step S209 of FIG.

[0322] In some embodiments, step S105 may be performed to provide any feature or combination of features of step S213 of FIG.

[0323] In some embodiments, step S109 may be performed to provide any feature or combination of features of step S217 of FIG.

[0324] In some embodiments, step S113 may be performed to provide any feature or combination of features of step S221 of FIG.

[0325] In some embodiments, step S117 may be performed to provide any feature or combination of features of step S225 of FIG.

[0326] Steps S91-S99 relate to ingredients or components or consumables used in the process of Figure 12, while steps S101-S117 relate to the process itself. In summary, (i) in step S101, a thin treatment layer of a wet treatment formulation is applied to an intermediate transfer member (ITM, having a release layer with hydrophobic properties), (ii) in step S105, this treatment layer is dried (e.g., fast dried) into a thin dry treatment film on the release surface of the ITM, (iii) in step S109, droplets of a water-based ink are deposited (e.g., by jetting) onto the thin dry treatment film, (vi) in step S113, the ink image is dried to leave an ink image on the dry treatment film on the ITM, and (v) in step S117, the ink image is transferred (e.g., together with the dry treatment film) onto a print substrate.

[0327] Details regarding the contents of steps S91-S99, as well as process steps S101-S117, are described below.

[0328] In various embodiments of the present invention, steps S91 to S117 are performed as follows. (A) In step S91, an ITM is provided, which has, for example, at most moderate hydrophobicity, and / or has hydrophobic properties, and / or is silicone-based, and / or has only moderate hydrophobicity, and / or has no functional groups, a release layer. (B) In step S95, an aqueous treatment solution is provided that, for example, (i) has a low evaporation load, and / or (ii) is rich in surfactants, and / or (ii) exhibits only moderate hydrophilicity, and / or (iii) contains a water-soluble polymer, and / or (iv) contains a quaternary ammonium salt, and / or (v) has a viscosity low enough that the solution can be spread in a uniform thin layer, (vi) contains hygroscopic materials, and / or (vii) is substantially free of organic solvents, and / or (viii) has a maximum low concentration of flocculants (including multivalent cations). (C) In step S99, a water-based ink is provided. (D) In ​​step S101, an aqueous treatment formulation is applied to a release surface of an ITM (eg, a moving ITM), thereby forming a thin wet treatment layer (eg, thickness ≦0.8μ) on the release surface. (E) In step S105, the thin wet treatment layer is subjected to a drying process (e.g., fast drying) on ​​the ITM release surface to leave a thin dry treatment film (e.g., thickness ≦0.08μ) of the water soluble polymer on the ITM release surface. For example, the thin dry treatment film may have one or both of the following characteristics: (i) for example, the treatment film is a continuous and / or coherent film, and (ii) the upper surface of the dry treatment film is characterized by very low roughness. (F) In step S109, droplets of the water-based ink are deposited (eg, by ink ejection) onto a thin dry treatment film to form an ink image on the treatment film. (G) In step S119, the ink image leaves residual ink on the drying process film (eg, to achieve good ink dot spreading). (H) In step S119, the dried ink image is transferred (eg, at a relatively low temperature) (eg, with a dry treatment film) from the ITM surface to a print substrate (eg, paper-based or plastic-based).

[0329] 12 is performed such that when the aqueous processing solution is applied to the ITM in step S101, there is little or no beading, such that the resulting thin dried processing film (i.e., obtained in step S105) is continuous and / or has a smooth (e.g., very smooth) upper surface, which can be important in obtaining high quality ink-on-substrate images.

[0330] One feature associated with conventional processing, in which an ITM is pre-treated and an ink image is applied on top of the pre-treated ITM, is that after transfer to the substrate, a dry processing formulation is present on the ink image (e.g., after drying), which may increase the undesirable gloss of the ink image. To overcome or minimize this potentially undesirable effect, a thin dry processing film is obtained in step S105 (e.g., having a thickness of up to 400 nanometers, or up to 200 nanometers, or up to 100 nanometers, or even less). Furthermore, in some embodiments, this thin dry processing film (i.e., obtained in step S105) is continuous, which may be advantageous, as described below.

[0331] 12 is performed such that the image transfer of step S117 is performed at a lower temperature (e.g., for an uncoated substrate), such as at a temperature of up to 90 degrees Celsius, or up to 85 degrees Celsius, or up to 80 degrees Celsius, or up to 75 degrees Celsius, or up to 70 degrees Celsius, or up to 65 degrees Celsius, or up to 60 degrees Celsius, such as about 60 degrees Celsius.

[0332] Explanation of step S91 in FIG. 12 In different embodiments, the ITM (ie, the ITM provided in step S91 of FIG. 12 or step S201 of FIG. 2) may provide one or more of the following features A1-A5. A1: In some embodiments, the release layer is formed from a silicone material (e.g., addition cure type), which gives the ITM hydrophobic properties that are useful in step S117. A2: Prior to use in the method of FIG. 12, the silicone-based release layer is produced so that its hydrophobicity is reduced. For example, instead of relying on the addition of functional reactive groups to impart hydrophilicity to the release layer, the silicone release layer can be cured so that the polar atoms in the polar groups (e.g., oxygen atoms in polar Si-O-Si moieties) are aligned or otherwise oriented outward relative to the release layer surface. In this case, the oxygen atoms in "Si-O-Si" do not have the ability to chemically bond to materials in the processing solution in step S117, to the dried ink image, and / or to the dried processing film under normal processing conditions. However, in steps S101-S105, the hydrophilicity of the outwardly oriented polar "O" can provide an advantage. A3: The release surface of the ITM has moderate hydrophobic properties but does not exhibit excessive hydrophobicity, and thus the release surface may have a surface energy (at 25 degrees Celsius) of at least 23 dynes / cm, more typically at least 25 dynes / cm, at least 28 dynes / cm, at least 30 dynes / cm, at least 32 dynes / cm, at least 34 dynes / cm, or at least 36 dynes / cm, and / or up to 48 dynes / cm, up to 46 dynes / cm, up to 44 dynes / cm, up to 42 dynes / cm, up to 40 dynes / cm, up to 38 dynes / cm, or up to 37 dynes. A4: The receding contact angle of a distilled water droplet on the ink receptive surface or release layer surface is typically at least 30 degrees, and more typically 30 degrees to 75 degrees, 30 degrees to 65 degrees, 30 degrees to 55 degrees, or 35 degrees to 55 degrees. A5: The release layer of the ITM is free or substantially free of functional groups attached within the crosslinked polymer structure, which the inventors believe may increase or promote desirable adhesion.

[0333] Explanation of step S95 in FIG. 12 In step S95, an aqueous treatment formulation is provided, the treatment formulation comprising at least 50% w / w, or at least 55% w / w, or at least 60% w / w, or at least 65% w / w water carrier liquid.

[0334] In different embodiments, the aqueous treatment formulation (i.e. the aqueous treatment formulation in its initial state prior to application of step S101 of FIG. 12 or the aqueous treatment formulation in its initial state prior to application of step S205 of FIG. 1) may provide one or more (i.e. any combination) of the following features: B1. Low Evaporation Load - In some embodiments, the initial aqueous treatment formulation has a low evaporation load and is relatively rich in materials that are solid at 60 degrees Celsius (and atmospheric pressure). As explained below, in some embodiments, this can be useful because the viscosity increases rapidly in a very short time period during the performance of step S105, thereby suppressing any tendency of the aqueous treatment formulation to form beading on the release surface (which has hydrophobic properties) of the ITM. For example, the 60 degrees Celsius evaporation load can be up to 10:1, or up to 9:1, or up to 8:1, or up to 6:1, or up to 5:1, or up to 4:1. In some embodiments, this is favorable for achieving a continuous dry treatment film with no exposed portions. B2. Surfactant Rich - In some embodiments, the initial aqueous treatment formulation comprises at least 2% w / w, or at least 2.5% w / w, or at least 3% w / w, or at least 4% w / w, or at least 5% w / w, or at least 6% w / w, or at least 7% w / w, or at least 8% w / w, or at least 9% w / w, or at least 10% w / w of surfactant(s). In various embodiments of the invention, the surfactant present in the initial aqueous treatment formulation (e.g., at least 50% by weight, or at least 75% by weight, or at least 90% by weight of the surfactant in the treatment formulation) may be solid at 60 degrees Celsius, thereby contributing to a low evaporation load. In some embodiments, the presence of a relatively high concentration of surfactant in the initial aqueous treatment formulation contributes to a reduced hydrophilicity of the aqueous treatment formulation, thereby reducing the tendency of the aqueous treatment formulation to bead up on the release surface of the ITM in step S101 and / or step S105. In some embodiments, because the surfactant is a humectant, a relatively high concentration of the surfactant may be useful for spreading the aqueous ink droplets (or suppressing any tendency of the ink droplets to shrink) on the surface of the dried ink film during steps S109 and / or S113, thereby increasing the coverage of the resulting ink dots and causing them to gradually reside on the substrate. B3. Presence of a quaternary ammonium salt (e.g., at a relatively high concentration) - In some embodiments, the initial aqueous treatment formulation comprises at least 1.5% weight / weight (e.g., at least 2%, at least 2.5%, at least 3%, at least 4%, at least 5%) of a quaternary ammonium salt. In some embodiments, the solubility of the quaternary ammonium salt in water is at least 5% at 25 degrees Celsius. In some embodiments, the ammonium quaternary ammonium salt comprises an aliphatic substituent. B4. Initial aqueous treatment formulation with moderate hydrophilicity - In some embodiments, the initial aqueous treatment formulation is only moderately hydrophilic, e.g., has a static surface tension of at most 32 dynes / cm (e.g., 20-32 dynes / cm) or at most 30 dynes / cm (e.g., 20-32 dynes / cm) or at most 28 dynes / cm (e.g., 20-32 dynes / cm) at 25 degrees Celsius. Because the release surface of the ITM exhibits moderately hydrophobic (or moderately hydrophilic) properties, it may be useful not to use an initial aqueous treatment formulation with high hydrophilicity in step S101 and / or step S105, which may result in beading of the aqueous treatment formulation on the surface of the ITM. This may be particularly important for situations where the thickness of the wet treatment layer is small, and it is desired to prevent exposed areas from becoming continuous with a thin dry treatment film. B5. Presence of a water-soluble polymer that forms a polymer matrix (e.g., upon drying in step S105 of FIG. 21 or step S213 of FIG. 2) - In some embodiments, the initial aqueous formulation comprises at least 1.5% by weight (e.g., at least 2% by weight, at least 2.5% by weight, or at least 3% by weight) of at least one water-soluble polymer, more particularly a matrix-forming polymer, having a water solubility of at least 5% at 25 degrees Celsius. Such polymer(s) include, but are not limited to, water-soluble celluloses including polyvinyl alcohol (PVA), e.g., hydroxypropyl methylcellulose, PVP, polyethylene oxide, and derivatives thereof, such as acrylic resins. In some embodiments, the formation of a polymer matrix aids in the formation of a thin film and / or imparts desired elasticity and / or cohesion, or tensile strength to the dried thin film, even when the dried thin film is quite thin. B6. Relatively Low Viscosity Prior to Application onto the ITM in Step S101 of FIG. 12 (or Application to the ITM in Step S209 of FIG. 2) - As described below, in step S101 of FIG. 12 (or step S209 of FIG. 2), the inventors have found that it is desirable to apply a thin but relatively uniform wet layer of the aqueous treatment formulation. To this end, the 25° C. viscosity of the initial aqueous treatment formulation may be up to 100 cP, or up to 80 cP, or up to 40 cP, or up to 30 cP. Alternatively or additionally, the 25° C. viscosity of the initial aqueous treatment formulation may be at least 8 cP, or at least 10 cP, or at least 12 cP, or at least 14 cP - for example in the range of 8-100 cP, 10-100 cP, 12-100 cP, 14-100 cP, 10-60 cP, or 12-40 cP.

[0335] In some embodiments, this feature may be particularly useful when applying the treatment formulation to an ITM that is moving at high speeds (as it passes an applicator device - for example a stationary applicator device). B7. No organic solvents such as glycerol - in some embodiments, the presence of organic solvents with low vapor pressure may prevent the drying of the treatment formulation on the surface of the ITM in step S105 and / or the treatment film may lose the desired elasticity and / or cohesion or tensile strength desired for the transfer step S117. In some embodiments, the formulation is free of organic solvents regardless of vapor pressure in the pure state and / or contains up to 3 wt%, up to 2 wt%, up to 1 wt%, or up to 0.5 wt%, or up to 0.25 wt%, or up to 0.1 wt% organic solvent. In particular, in some embodiments, the formulation is free of organic solvents and / or contains up to 3 wt%, up to 2 wt%, up to 1 wt%, or up to 0.5 wt%, or up to 0.25 wt%, or up to 0.1 wt% glycerol. In some embodiments, the formulation is completely free of glycerol. B8. Include Water Absorbing Material - In some embodiments, the initial aqueous treatment formulation includes a solid water absorbing agent selected to absorb water from the ink when the water absorbing agent is disposed in the solid dry treatment film. For example, such a solid water absorbing agent may have a melting point (i.e., when in a pure state) of up to 60 degrees Celsius, or up to 50 degrees Celsius, or up to 40 degrees Celsius, or up to 30 degrees Celsius, or up to 25 degrees Celsius - for example, at least 1.5% w / w, or at least 2% w / w, or at least 2.5% w / w, or at least 3% w / w. Examples of such water absorbing agents include, but are not limited to, sucrose, urea, sorbitol, and isomaltose. B9. Presence of multiple surfactants, including at least one surfactant whose surface tension exceeds that of the formulation as a whole. - In some embodiments, the initial aqueous treatment formulation includes a first surfactant and a second surfactant, where the first surfactant has a greater hydrophobicity (and lower surface tension) than the second surfactant (e.g., a quaternary ammonium salt). In one case, the first surfactant includes a silicone polyether and / or the second surfactant is a quaternary ammonium salt. For example, the absolute value of the difference in the respective surface tensions between the first and second surfactants can be at least 5 dynes / cm, or at least 7.5 dynes / cm, or at least 10 dynes / cm. For example, (i) the surface tension of the first surfactant is less than the surface tension of the initial aqueous treatment formulation (the difference being, for example, at least 1 dyne / cm, or at least 2 dynes / cm, or at least 3 dynes / cm, or at least 4 dynes / cm, or at least 5 dynes / cm, or at least 7 dynes / cm), and / or (ii) the surface tension of the second surfactant is greater than the surface tension of the initial aqueous treatment formulation (the difference being, for example, at least 1 dyne / cm, or at least 2 dynes / cm, or at least 3 dynes / cm, or at least 4 dynes / cm, or at least 5 dynes / cm, or at least 7 dynes / cm).

[0336] In some embodiments, the primary purpose of the first surfactant is to reduce the hydrophilicity of the initial aqueous treatment formulation (e.g., to a value as described in "Feature A4" above), e.g., to prevent the treatment formulation from agglomerating into beads in steps S101 and / or S105. Alternatively or additionally, the primary purpose of the second surfactant is to provide any of the features described in B3 above.

[0337] In different embodiments, the initial aqueous treatment formulation comprises at least 2% (w / w), or at least 2.5% (w / w), at least 3% (w / w), or at least 4% (w / w), or at least 5% (w / w) of the first surfactant, and / or at least 2% (w / w), or at least 2.5% (w / w), or at least 3% (w / w), or at least 4% (w / w), or at least 5% (w / w) of the second surfactant. For example, the ratio between the concentration (w / w) of the first surfactant and the concentration (w / w) of the second surfactant is at least 0.1, or at least 0.2, or at 0.25, or at least 0.33, or at least 0.5, or at least 0.75, and / or at most 10, or at most 4, or at most 3 at most 2, or at most 4 / 3. B10. Have a low maximum concentration of flocculants that contain multivalent cations (such as calcium chloride, etc.) - in some embodiments, these compounds are believed to be poor for image quality.

[0338] Explanation of step S99 in FIG. 12 Potential features of water-based inks: Feature C1: In some embodiments (e.g., for the method of FIG. 2 or FIG. 12), the ink provides one or more features (any combination of features) described in PCT / IB13 / 51755, or US2015 / 0025179, PCT / IB14 / 02395, or US14 / 917461, all of which are incorporated herein by reference.

[0339] Explanation of step S105 in FIG. 12 Feature D1: The dried processed layer formed in step S105 is thin but not monolayer (e.g., significantly thicker than a monolayer), e.g., having a thickness of at most 100 nanometers. In some embodiments, the dried processed layer is extremely thin, having a thickness of at most 80 nanometers, or at most 75 nanometers, or at most 70 nanometers, or at most 65 nanometers, or at most 60 nanometers, or at most 55 nanometers, or at most 50 nanometers. Nevertheless, in different embodiments, even when the dried processed film is extremely thin, it is thicker than a monolayer or monolayer-type construct. Thus, in different embodiments, the thickness of the dried processed layer may be at least 20 nanometers, or at least 30 nanometers, or at least 40 nanometers, or at least 50 nanometers. In some embodiments, providing this large "bulk" (i.e., minimum thickness feature), e.g., in conjunction with other feature(s) described below, aids in the formation of a dried processed film that exhibits adhesion and / or elasticity. This can be useful in step S117, where it is desirable to maintain the structural integrity of the dry processing film as it is transferred from the ITM to the substrate (ie, in the stage of retaining the dry ink image on the dry processing film).

[0340] In some embodiments, the dried processing formulation can add undesirable gloss to the resulting ink image after it is transferred to the substrate. Therefore, the ability to form a thin, yet coherent, dried processing layer can be useful. A thin layer also aids in evaporation and the layer dries into a thin film. Feature D2: The dry process film formed on the ITM in step S105 is continuous and has no "exposed portions" on the dry process film, regardless of whether it is thin or ultra-thin. As will be explained below, in some embodiments, to achieve this goal (particularly for thin or very thin layers), it may be required that the initial applied wet layer applied in step S101 be both continuous and free of exposed portions, even if the initial applied wet layer is relatively thin, having a thickness of at most about 1μ (or at most 0.8μ, or at most 0.6μ, or at most 0.4μ, more typically at most 0.3μ, at most 0.25μ, or at most 0.2μ, and / or at least 0.1μ), and (ii) the drying process of step S105 is performed very rapidly, such that the viscosity of the drying process formulation increases very rapidly (e.g., at least 100 times, or at least 1000 times, or at least 10,000 times within at most 100 milliseconds, within at most 50 milliseconds, within at most 40 milliseconds, within at most 30 milliseconds, within at most 25 milliseconds, within at most 20 milliseconds, within at most 15 milliseconds, or within at most 10 milliseconds). When the aqueous treatment formulation is applied to the ITM release layer, the aqueous treatment formulation may cause beading because the ITM release layer has hydrophobic properties and the treatment formulation is aqueous and has greater hydrophilicity. However, if the viscosity increases rapidly after application of the wet treatment layer, a higher viscosity treatment formulation may resist beading better than a lower viscosity formulation. In some embodiments, as discussed in feature "B1" above, the aqueous treatment formulation is rich in solids and / or has a low evaporation load. This may aid in the rapid increase in viscosity.

[0341] Other anti-beading features (i.e., anti-beading of steps S101-S105) that are useful in obtaining a continuous dry processing film may relate to the relative properties of (i) the release surface of the ITM, which in some embodiments has hydrophobic properties but is not excessively hydrophobic (see feature "BA"), and (ii) the aqueous processing formulation, which in some embodiments has hydrophilic properties but is not excessively hydrophilic (see feature "B4"). If the static surface tension between the aqueous processing formulation and the release layer of the ITM is relatively small, the driving force toward beading is small and the viscosity of the aqueous processing formulation (e.g., increases rapidly) may be sufficient to prevent beading.

[0342] As discussed above, even though the ITM release layer is only moderately hydrophobic (see feature "A3"), the ITM release layer may have specific properties that limit adhesion between the ITM release layer and the dry process film (see feature "A5"). Thus, even if the process surface is only moderately hydrophobic to avoid beading of the process formulation on the process surface in steps S101 and / or S105, it may be possible to avoid paying the "price" for this advantage in step S117 when it is later desired to minimize adhesion between the ITM release layer and the dry process film (e.g., at least in part because of feature "B2").

[0343] In some embodiments, this is useful for producing images of the ink present on the substrate that have suitable image quality (see, for example, Figures 15A-15D). Feature D3: The dried thin film formed on the ITM in step S105 is characterized by an extremely low surface roughness. In some embodiments, the surface roughness has a roughness average R of at most 20 nanometers, or at most 18 nanometers, or at most 16 nanometers, or at most 15 nanometers, or at most 14 nanometers, or at most 12 nanometers, or at most 10 nanometers, or at most 9 nanometers, or at most 8 nanometers, or at most 7 nanometers, or at most 6 nanometers. a(a commonly used one-dimensional roughness parameter). The dried films formed on the ITM have an R of at least 3 nm or at least 5 nm. a may have:

[0344] In some embodiments, it may be possible to achieve such low roughness average Ra even for thin or extremely thin dried process films formed in step S105, for example when the ratio between the roughness average Ra and the thickness of the dried process layer is at least 0.02, or at least 0.03, or at least 0.04, or at least 0.05, or at least 0.06, or at least 0.07, or at least 0.08, or at least 0.9, or at least 0.1, or at least 0.11, or at least 0.12, or at least 0.13, or at least 0.14, or at least 0.15, or at least 0.16, or at least 0.17, or at least 0.18, or at least 0.19, or at least 0.2.

[0345] In some embodiments, the dry processed film on which the aqueous ink droplets are deposited and the surface of the dry processed film (e.g., the upper surface of the dry processed film) have (i) an average roughness R a and (ii) the thickness of the drying layer, which is at least 0.5, at least 0.4, at least 0.3, at least 0.25, at least 0.2, at least 0.15, or at least 0.1, and optionally at least 0.02, or at least 0.03, or at least 0.04, or at least 0.05, or at least 0.06, or at least 0.07, or at least 0.08. Feature D4: In some embodiments, it is possible to obtain a continuous dry thin film covering the entirety of a rectangle of at least 10 cm by 1 meter, or an entire 1 m2, 3 m2, or 10 m2. The thin film may have a thickness or average thickness of at most 120 nm, at most 100 nm, at most 80 nm, at most 60 nm, at most 50 nm, or at most 40 nm, and typically at least 20 nm, at least 25 nm, or at least 30 nm.

[0346] Explanation of steps S109 to S117 In different embodiments, when steps S109 and / or S113 and / or S117 are performed, one or more of the following processing-related features may be provided. Feature E1: In some embodiments, even if the image is transferred to an uncoated substrate, step S117 is performed at a low transfer temperature (e.g., up to 90° C., or 80° C., or 75° C., or 70° C., or 65° C., or 60° C.—due to thermoplastic properties and / or tensile strength). In some embodiments, providing a low temperature transfer step may be useful in reducing or avoiding clogging of the inkjet head assembly and / or making the overall printing process more environmentally friendly. In some embodiments, both the dried processing film and the dried ink image are tacky at the transfer temperature and therefore susceptible to being cleanly peeled from the release layer, even at relatively low temperatures. This property may be at least partially attributed to the chemistry of the initial aqueous processing solution. In some embodiments, the chemistry and structure of the release layer (see, e.g., feature "A5") may also be useful in providing a low-temperature transfer process in step S117. Feature E2: Spreading - The manner in which the droplets are deposited on the film (e.g. wetting angle) and the physical and / or chemical properties of the treatment film (A2 and / or A3 and / or A8 - nanoparticles in the ink also contribute) are set such that the radius of the ink dots exceeds the radius of the precursor droplets immediately after impact on the dried treatment film (e.g. the size of each droplet increases beyond the size due to droplet diffusion caused by the impact energy of the droplets). [Dmax=2·Rmax, or Dimpact-max=2·Rimpact-max]

[0347] 13A-13E illustrate a schematic process in which an ink droplet is deposited onto an ITM (e.g., a release surface of an ITM). In FIG. 13A, an ink droplet moves towards the ITM. In FIG. 13B-13C, the ink droplet is illustrated immediately after collision between (i) the droplet and (ii) the ITM (or a dried treatment film of the ITM). The kinetic energy of the droplet causes a deformation of the droplet, which is illustrated in FIG. 13B-13C. In particular, the kinetic energy of the droplet causes the droplet to expand outward. In FIG. 13C, the maximum radius of the droplet upon impact (i.e., the maximum increase in radius due to deformation caused by the kinetic energy of the droplet) is illustrated. After the droplet reaches this maximum radius ("R upon impact" or "R max impact", which are used interchangeably) within 10 milliseconds of impact due to kinetic energy driven droplet deformation, the droplet (or dot that replaces the droplet (because each droplet gradually dries into an ink dot)) initially resides on the ITM as shown in FIG. 13D (e.g., via a drying treatment film), and after transfer, the ink droplet resides on the substrate as shown in FIG. 13E. The droplet or dot that replaces the droplet may further expand due to physicochemical forces or chemical interactions. This is the expansion phenomenon shown diagrammatically by comparison of FIG. 13C or FIG. 13D with FIG. 13B. Again, it should be noted that FIGS. 13A-13E are schematic and there is no requirement that the deformed droplet have the specific shape shown in FIG. 13A-13E.

[0348] 14A-14B provide mechanically plotted topographical profiles of dried processed thin films produced according to various embodiments of the present invention.

[0349] General comments regarding FIG. 2 and FIG. 12 - in some embodiments, performing step S201 of FIG. 2 may provide any feature or combination of features of step S91 of FIG. 12. In some embodiments, performing step S205 of FIG. 2 may provide any feature or combination of features of step S95 of FIG. 12. In some embodiments, performing step S209 of FIG. 2 may provide any feature or combination of features of step S101 of FIG. 12. In some embodiments, performing step S213 of FIG. 2 may provide any feature or combination of features of step S105 of FIG. 12. In some embodiments, performing step S217 of FIG. 2 may provide any feature or combination of features of step S109 of FIG. 12. In some embodiments, performing step S221 of FIG. 2 may provide any feature or combination of features of step S113 of FIG. 12. In some embodiments, performing step S225 of FIG. 2 may provide any feature or combination of features of step S117 of FIG. 12.

[0350] In Figures 14A-B, mechanically plotted topographical profiles of successive dried processed thin films produced according to some embodiments of the present invention are provided. These topographical profiles, produced by a Zygo laser interferometer, display average thin film thicknesses of approximately 40-50 nanometers (Figure 14A) and approximately 100 nanometers (Figure 14B), respectively. The thin film surface is exceptionally smooth, with an average roughness (R) of approximately 7 nanometers in Figure 14A. a ), and in FIG. 14B, the average roughness (R a ) other topographical profiles show an average film thickness of approximately 40 nm and a R of about 5 nm. a has been observed.

[0351] Regardless of the thickness of the thin film (typically up to 120 nm, up to 100 nm, up to 80 nm, up to 70 nm, up to 60 nm, up to 50 nm, or up to 40 nm, and more typically 30-100 nm, 40-100 nm, 40-80 nm, 40-70 nm, or 40-60 nm), the thin film is typically less than 20 cm 2 , 50cm 2 , or 200cm 2 , or even larger areas, have no exposed spots and are free of defects.

[0352] Without wishing to be bound by theory, the inventors believe that the extremely smooth surface of the dried film allows the ink dot spreading to occur in a uniform and controlled manner such that the formation of undesirable rivulet or the like is appreciably mitigated or avoided. The resulting ink dot shape is quite similar in quality to the excellent shape (convexity, roughness, edge sharpness) achieved in Landa's Application No. PCT / IB2013 / 000840, which is incorporated by reference for all purposes as if fully set forth herein. This is particularly striking in light of the spreading mechanism utilized by the present disclosure, as compared to the surface tension controlled drop pinning and contraction disclosed in that application.

[0353] In Figures 15A-15D, several examples of ink dots on a paper substrate are shown. In particular, in Figure 15A, a top view of a magnified image of a single ink dot deposited on a coated paper substrate (130 GSM) after being inkjetted onto and transferred from an ITM in accordance with some embodiments of the present invention is provided, in Figure 15B, a top view of a magnified image of multiple inkjet ink dots disposed within a viewing area on a coated paper substrate (130 GSM) in accordance with some embodiments of the present invention is provided, in Figure 15C, a top view of a magnified image of a single ink dot deposited on an uncoated paper substrate after being inkjetted onto and transferred from an ITM in accordance with some embodiments of the present invention is provided, and in Figure 15D, a top view of a magnified image of multiple inkjet ink dots disposed within a viewing area on an uncoated paper substrate in accordance with some embodiments of the present invention is provided.

[0354] The dot and convexity measurements were performed according to the procedures disclosed in PCT / IB2013 / 000840. In addition, the dot and convexity measurements were performed substantially as described below.

[0355] Image acquisition method Acquisition of dot images was performed using a LEXT (Olympus) OLS3000 microscope. Images were collected with an optical zoom of X100 and X20. Color images were saved in an uncompressed format (Tiff) with a resolution of 640 x 640 pixels.

[0356] In addition, a ZYGO microscope with a X100 lens was used to measure the dot thickness and diameter.

[0357] About the analysis The basic parameters of interest (and their units) included in this application are as follows: ·Diameter-Fits a Circle [Ddot] [mic] ·Outer circumference [P] [mic] ·Measurement area [A] [pix^2] ·Minimum convex shape area [CSA] [pix^2] ·Optical uniformity [STD] [8bit gradation value] Thickness [Hdot] [mic]

[0358] From these parameters the following was calculated: Aspect ratio: Raspect=Ddot / Hdot [dimensionless] Dot roundness: ER=P2 / (4π·A) [dimensionless] ·DRdot:ER-1 [Dimensionless] ·Convexity: CX=AA / CSA [dimensionless] ·Non-convexity: Dcdot=1-CX [dimensionless]

[0359] Analysis was performed using MATLAB® image processing tools, utilising the above analysis procedures applied in WO2013 / 132418 where possible.

[0360] blanket The ITM may be manufactured in the manner of the present invention as illustrated in Figures 17 to 22. Such an ITM is particularly suitable for Landa's Nanographic Printing® technology.

[0361] Reference is now made to Figure 16, which shows a schematic cross section through carrier 10. In all of these figures, carrier 10 is shown as a solid black line to distinguish it from the layers which form part of the finished article. Carrier 10 has a carrier contact surface 12.

[0362] In some embodiments, the support contact surface 12 has a roughness (R a In some embodiments, the support contact surface 12 is 1 to 50 nm, 3 to 25 nm, 3 to 20 nm, or 5 nm to 20 nm.

[0363] The hydrophilic properties of the support contact surface 12 are described below.

[0364] In some embodiments, the carrier 10 is inflexible and may be formed, for example, from a piece of glass or a thick metal sheet.

[0365] In some embodiments, the carrier 10 may be advantageously formed of a flexible foil (e.g., a flexible foil consisting essentially of or including aluminum, nickel, and / or chromium). In one embodiment, the foil is a sheet of aluminized PET (polyethylene terephthalate, polyester), e.g., PET coated with evaporated aluminum metal. The aluminum top coat may be protected by a polymeric coating. The sheet typically has a thickness of 0.05 mm to 1.00 mm to maintain flexibility while being resistant to bending at small radii to avoid wrinkling.

[0366] In some embodiments, the carrier 10 may be advantageously formed of an antistatic polymeric film (such as a polyester film such as PET). The antistatic properties of the antistatic film are achieved by a variety of means known to those skilled in the art, including the addition of various additives (e.g., ammonium salts, etc.) to the polymer composition.

[0367] In the steps of the ITM manufacturing method, the results of which are shown in Figure 17, a fluid first curable composition (shown as 36 in Figure 24B) is provided and a layer 16 is formed from that composition on the carrier contacting surface 12. Layer 16 constitutes an initial release layer having an outer ink-transfer surface 14.

[0368] The fluid first curable composition of layer 16 may include an elastomer, typically comprised of a silicone polymer such as polydimethylsiloxane (eg, vinyl-terminated polydimethylsiloxane, etc.).

[0369] In some embodiments, the fluid first hardenable material comprises a vinyl functional silicone polymer (eg, a vinyl silicone polymer that includes at least one pendant vinyl group in addition to a terminal vinyl group, such as, for example, a vinyl functional polydimethylsiloxane).

[0370] In some exemplary embodiments, the fluid first hardenable material comprises a vinyl-terminated polydimethylsiloxane, a vinyl-functional polydimethylsiloxane that includes at least one pendant vinyl group on the polysiloxane chain in addition to the terminal vinyl groups, a crosslinker, an addition cure type catalyst, and optionally, a cure inhibitor.

[0371] As is well known in the art, the curable adhesive composition can include any suitable amount of addition cure type catalyst on a molar basis (typically up to 0.01% per mole of prepolymer).

[0372] Representative formulations for the fluid first hardenable material are provided in the examples below.

[0373] A layer 16 of a fluid first curable composition is applied to the carrier contact surface 12 and then cured. The layer 16 can be developed to a desired thickness, for example using a doctor blade (a knife mounted on a roll), such that the doctor blade does not contact the surface that will ultimately function as the ink transfer surface 14 of the ITM, so that imperfections in the doctor blade do not affect the quality of the finished product. After curing, the "release" layer 16 can have a thickness of about 2 micrometers to about 200 micrometers. An apparatus in which such steps and methods are implemented is shown diagrammatically in Figures 24A and 24B.

[0374] For example, the release layer formulation detailed above may be uniformly coated onto a PET support, uniformized to a thickness of 5-200 micrometers (μ) and cured at 120° C.-130° C. for approximately 2-10 minutes. Surprisingly, the hydrophobicity of the ink-transfer surface of the release layer so prepared, estimated by its receding contact angle (RCA) for a 0.5-5 microliter (μl) drop of distilled water, may be approximately 60 degrees. Meanwhile, the other side of the same release layer (which acts to approximate the hydrophobicity of a layer conventionally prepared with an air interface) may have a significantly higher RCA (typically approximately 90 degrees). The PET carrier used to produce the ink-transfer surface 14 may typically exhibit an RCA of approximately 40 degrees or less. Contact angle measurements were performed using a contact angle analyzer - Kruss® "Easy Drop" FM40Mk2 and / or Dataphysics OCA15 Pro (Particle and Surface Sciences Pty, Gosford, NSW, Australia).

[0375] In a subsequent step of the method, the result of which is shown in Figure 18, an additional layer 18 (called a compliant layer) is applied to layer 16 on the opposite side to ink transfer surface 14. Compliant layer 18 is an elastomeric layer that enables layer 16 and its outermost surface 14 to closely conform to the surface contours of the substrate onto which the ink image is imprinted. Attaching compliant layer 18 to the opposite side from ink transfer surface 14 may involve application of an adhesive or bonding composition in addition to the material of compliant layer 18. Generally, compliant layer 18 typically has a thickness of from about 100 micrometers to about 300 micrometers or more.

[0376] While compliant layer 18 has the same composition as release layer 16, materials and processing economies may justify the use of less expensive materials. Furthermore, compliant layer 18 is typically selected to have different mechanical properties than release layer 16, such as greater resistance to tension. Such desired differences in properties may be achieved, for example, by utilizing a different composition for release layer 16, by varying the ratio between the components used to prepare the release layer 16 formulation, by adding additional components to such formulation, and / or by selecting different curing conditions. For example, the addition of filler particles may desirably increase the mechanical strength of compliant layer 18 compared to release layer 16.

[0377] In some embodiments, the compliant layer 18 may include a variety of rubbers, preferably those that are stable at temperatures of at least 100 degrees Celsius, and may include rubbers such as alkyl acrylate copolymer rubber (ACM), methyl vinyl silicone rubber (VMQ), ethylene propylene diene monomer rubber (EPDM), fluoroelastomer polymers, nitrile butadiene rubber (NBR), ethylene acrylic elastomer (EAM), and hydrogenated nitrile butadiene rubber (HNBR).

[0378] As a non-limiting example, Silopren® LSR2530 (Momentive Performance Materials, NY), a two-component liquid silicone rubber in which the two components are mixed in a 1:1 ratio, was applied to the aforementioned cured release layer 16. The silicone rubber mixture was metered / homogenized using a knife blade to obtain an initial compliant layer 18 having a thickness of about 250 micrometers, which was then cured at 150° C.-160° C. for approximately 5 minutes.

[0379] In a subsequent step of the method, the result of which is shown in Figure 19, a stiffening or support layer 20 is constructed on the compliant layer 18. The support layer 20 typically includes a fiber reinforcement in the form of a woven fabric or textile to provide the support layer 20 with sufficient structural integrity to withstand stretching when the ITM is held under tension in a printing system. The support layer 20 is formed by coating the fiber reinforcement with a resin that is subsequently cured and that retains flexibility after curing.

[0380] Alternatively, the support layer 20 may include such fibers embedded and / or infused in a separately formed and independently cured resin as a reinforcing layer. In this case, the support layer 20 may be attached to the compliant layer 18 via an adhesive layer, eliminating the need to cure the support layer 20 in situ, if desired. In general, the support layer 20, whether formed in situ on the compliant layer 18 or separately, may have a thickness of about 100 micrometers to about 500 micrometers, some of which may be contributed by the thickness of the fibers or fabric, which typically varies from about 50 micrometers to about 300 micrometers. However, the support layer thickness is not limiting. For heavy duty applications, for example, the support layer may have a thickness of 200 micrometers or more, 500 micrometers or more, or 1 mm or more.

[0381] For example, a support layer 20 comprising a woven glass fiber fabric was applied to the multi-layered ITM structure described herein, including a vinyl-functionalized release coating 16 and a two-component silicone rubber compliant layer 18. The glass fiber fabric, having a thickness of about 100 micrometers, was a plain weave fabric having 16 yarns / cm in the vertical direction. The glass fiber fabric was embedded in a hardenable fluid including liquid silicone rubber Silopren® LSR2530, which corresponds to the compliant layer. Overall, the resulting support layer 20 had a thickness of about 200 micrometers and was cured at 150 degrees Celsius for approximately 2-5 minutes. Preferably, a denser fabric (e.g., having 24×23 yarns / cm) may be used.

[0382] After the support layer 20 is formed in situ or after the support layer 20 is installed, additional layers can be constructed on the opposite side as needed. In FIG. 20, an optional felt blanket 22 is shown secured (e.g., by a cured adhesive or resin) to the opposite side of the support layer 20, and in FIG. 21, a high friction layer 24 is shown coated on the opposite side of the blanket 22. As will be appreciated by those skilled in the art, various relatively soft rubbers can be used to provide layers with high friction properties. Just one example of such a rubber is silicone elastomer. In situations where there is no intervening layer such as the blanket 22, the high friction layer 24 can be attached directly to the support layer 20.

[0383] As mentioned above, all layers added to the release layer of the ITM (e.g., 18, 20, 22, 24, or any intervening adhesive or primer layers, etc.) collectively form the base of the structure, as shown for base 200 in Figure 23C.

[0384] Before the ITM can be used, it is necessary to remove the carrier 10 to expose the ink-transfer surface 14 of the release layer 16, as shown in Figure 22. Usually, the finished product can simply be peeled off the carrier 10.

[0385] If the carrier 10 is a flexible foil, it may be preferred to leave it in place on the ITM until the ITM is installed in a printing system, etc. The foil would act to protect the ink transfer surface 14 of the ITM during storage, shipping, and installation. Additionally, the carrier 10 may be replaced with an alternative foil suitable as a protective membrane after the manufacturing process is complete.

[0386] 24A-24D, an apparatus 90 in which an ITM may be manufactured is shown diagrammatically. In FIG. 24A, a schematic of such an apparatus 90 is provided having an unwind roller 40 and a take-up roller 42 moving a flexible loop conveyor 100. Disposed along the path followed by the conveyor 100 are a discharge station 52 capable of discharging a hardenable fluid composition suitable for the desired ITM, a leveling station 54 capable of controlling the thickness of the hardenable layer as it moves downstream of the station, and a curing station 56 capable of at least partially curing a layer so that it can serve as an initial layer for a subsequent step, if any. Discharge station 52, leveling station 54, and curing station 56 constitute layer forming station 50a. As indicated by 50b, the apparatus 90 may include two or more layer forming stations as desired. Additionally, forming station 50 may include additional substations, indicated by discharge roller 58 at station 50a.

[0387] In some embodiments, the need for loop conveyor 100 is omitted and carrier 10 is tensioned directly between rollers 40 and 42. Untreated carrier 10 is unwound from unwind roller 40 and passes through stations 50a and 50b before being wound onto take-up roller 42.

[0388] Although not shown in the drawings, the apparatus may further include a "surface treatment" station upstream of the dispensing station to assist in the subsequent application of the curable composition, if desired, or in some cases in attaching the curable composition to the carrier contact surface or initial layer. As discussed above with respect to the carrier, the optional surface treatment station (not shown) may be suitable for physical treatment (e.g., corona treatment, plasma treatment, ozone treatment, etc.).

[0389] FIG. 24B shows, in a schematic manner, how a carrier 10 disposed on a conveyor 100 can be coated in a forming station 50 of the apparatus 90. In a dispensing station 52, a hardenable composition 36 of the release layer 16 is applied to the carrier contact surface 12. As the carrier 10 is driven in the direction of the arrow, the hardenable composition 36 is uniformized to a desired thickness in a leveling station 54, for example by using a doctor blade. As the uniformed layer advances downstream, it enters a curing station 56, which is configured to at least partially harden the hardenable composition 36, thereby allowing the initial layer 16 to be formed at the exit side of the curing station. Such representative steps have already been described in relation to FIGS. 16 and 17.

[0390] In Fig. 24C and Fig. 24D, it is shown diagrammatically how additional layers (forming the base) are applied. In Fig. 24C, the hardenable composition 38 is dispensed at a dispensing station 52 (which may be the same or different from the station used to coat the carrier with the release layer 16 shown in Fig. 9B). The hardenable composition 38 is leveled to a desired thickness at a leveling station 54, then enters a curing station 56, from which it exits sufficiently cured to serve as an initial layer 18 for a subsequent step, etc. Representative such steps have already been described in relation to Fig. 18. Now referring to Fig. 24C, in Fig. 24C, it is shown diagrammatically how the hardenable composition 39 is applied at the dispensing station 52. The backbone of the support layer (e.g., fabric) may be provided by a dispensing roller 58. The representative fabric may be submerged under the hardenable composition at station 60 before entering the curing station 56. In that way, the support layer 20 may be formed at the exit side of the curing station.

[0391] In Fig. 23A and Fig. 23B it is shown diagrammatically how defects appear in the cross section of an outer layer 80 (e.g. a release layer) prepared according to the method described above. In Fig. 23A, different phenomena related to air bubbles that can be trapped in any hardenable composition are shown if the curing occurs before the air bubbles can be eliminated (e.g. by venting). As can be seen in the figure, bubbles 82 flow towards the layer 80 towards the air interface above the body 800 during production in the flow direction indicated by the arrows. These bubbles 82 can therefore merge into larger bubbles. The air bubbles, regardless of their size, can remain trapped in the bulk of the layer or on its surface. The upper part of the bubble envelope forms a protrusion 84. If an air bubble adjacent to the surface bursts while the curing of the layer is in progress, a crater 86 can remain even if the area of ​​the air bubble envelope protruding from the surface disappears. These phenomena thus typically provide a "gradient" of air bubbles. The upper regions are generally populated with larger bubbles and / or have a higher density of bubbles per cross-sectional area or stack compared to the lower regions, where lower and upper refer to the layer orientation at the time of its manufacture. The impact of bubble-induced defects on the surface is self-evident, and surface inhomogeneity is usually detrimental to any subsequent interaction, for example with an ink image. Under conditions where such ITMs typically operate under tension and / or pressure, over time the craters will widen and merge to form more pronounced cracks. Such phenomena may therefore affect the structural integrity of the surface and any mechanical properties that such integrity would have imparted to the ITM.

[0392] In FIG. 23B, different phenomena are shown diagrammatically with respect to solid contaminants such as dust. In this illustrative example, the dust is represented as being added to the air bubbles, but this is not necessarily true and such surface or layer defects can occur independently. As can be seen in the figure, the solid contaminants can remain on the surface. If the contaminants settle after the outer layer 80 is cured, such contaminants 92 can be removed by simply cleaning the outer layer appropriately. Nevertheless, such a phenomenon is undesirable, since additional cleaning of the ITM may be required before it can be used. If such contaminants occur when the layer is still in an uncured state, they can be trapped on the surface of the layer 80 (e.g., contaminant 94, which appears to be "floating") or even sink into the isolation layer (e.g., contaminant 96). As can be easily understood, larger / heavier contaminants can sink deeper than smaller contaminants.

[0393] Unlike methods known in the art, the method disclosed herein involves forming a layer of a fluid first hardenable material with one side of the layer in contact with a carrier contact surface, which constitutes an initial release layer. The carrier contact surface functions to protect the initial release layer, thereby imparting the desired properties to the ink-transfer layer, while the carrier acts as a physically robust support structure onto which other layers are added to form the ITM until the ITM is complete. As a result, many potential sources of defects are avoided. Furthermore, the finish of the ink-transfer surface is primarily, if not exclusively, determined by the carrier contact surface.

[0394] In FIG. 23C, a cross section through an outer layer 16 (e.g., a release layer) prepared according to the present method is shown diagrammatically. For comparison with the previous figures, this cross section is shown in the same orientation as in FIG. 23A and FIG. 23B, without showing the carrier, but the manufacturing is carried out in the opposite direction as indicated by the arrows. The base 200 (described in more detail below) is attached to the first outer layer 16 after it has been at least partially cured, and is therefore not equivalent to the body 800, which already serves as a support during the manufacturing process. For illustrative purposes only, the layer 16 is represented as containing a large number of bubbles 82, although this is not necessarily true. However, if present, such bubbles would show a more specific pattern than the bubble pattern previously described. First, since the ink transfer surface 14, now the uppermost of the layer 16, was previously in contact with the carrier, no protrusions are observed, and therefore the release layer is free of the phenomenon previously shown by the bubbles 84 protruding from the surface. Similarly, the craters previously shown as cavities 86 are almost absent. Because such craters imply the use of incompatible hardenable layers and carriers. According to the present method, it is believed that the hardenable material forming the outer layer will wet the carrier well, and that there will be substantially no air bubbles that can be trapped between the carrier and the initial layer formed on the carrier. Thus, even if present, such air bubbles will be located in the bulk of the layer. However, since the production is performed in an inverted direction compared to the conventional method, the gradient of the air bubbles will be inverted for the same reason. Thus, as shown in FIG. 23C, the small air bubbles will be closer to the outer surface than the larger air bubbles, which will be closer to the base.

[0395] The inventive release layer structures produced from addition cured formulations may contain substantially no or only a small number (very few OH groups) of functional groups covalently bonded within the polymer matrix. Such functional groups may include moieties such as C=O, S=O, and OH.

[0396] Since these release layer structures contain, at most, very few such functional groups, it would be expected that the release layer would exhibit high hydrophobicity. However, the inventors have surprisingly found that the release layer surfaces produced by the present method do in fact exhibit some hydrophilicity, and are appreciably more hydrophilic than the corresponding release layers (i.e., release layers having the same composition but produced using conventional curing techniques in which the release layer is exposed to air ("standard air curing"). Without wishing to be bound by theory, the inventors believe that the intimate contact between the carrier-contacting surface and the initial release layer surface causes some of the hydrophilic properties of the carrier-contacting surface to be impregnated into the release layer surface.

[0397] As mentioned above, an ITM release layer having a low surface energy can aid in the transfer of a dried ink image to a print substrate. However, during the ink acceptance stage, aqueous ink droplets jetted onto such a low energy hydrophobic release layer tend to coalesce into beads after initial impact, thereby compromising image quality. A higher energy, less hydrophobic release layer can mitigate this effect, but is detrimental to image transfer quality. The inventors have found that the release layer structure of the present invention typically has a characteristically moderately hydrophobic release surface, represented by a receding contact angle with distilled water of up to 80 degrees, or up to 70 degrees, typically up to 60 degrees, or up to 50 degrees, and more typically 30 degrees to 60 degrees, 35 degrees to 60 degrees, 30 degrees to 55 degrees, 30 degrees to 50 degrees, 30 degrees to 45 degrees, or 35 degrees to 50 degrees. However, surprisingly, both the ink acceptance and ink transfer of the dried, heated ink image can be of good quality. It should be emphasized that even lower values ​​of the receding contact angle (and dynamic contact angle, discussed below) can be achieved by using a support surface that has a higher hydrophilicity (lower contact angle for a drop of distilled water) and / or by corona (or similar) treatment.

[0398] Without wishing to be bound by theory, the inventors believe that the above-mentioned induced surface properties improve the interactions between polar groups (e.g., O-Si-O) on the release layer surface and corresponding polar moieties (e.g., OH groups in water) in the aqueous liquid (e.g., aqueous ink-jet ink) deposited on the release layer surface. After subsequent drying of the ink and heating of the ink film to a transfer temperature, these interactions are weakened, allowing complete transfer of the dried or substantially dried ink image. Thus, the performance of the inventive release layer structure, both in the ink-receiving and ink-film transfer stages, is appreciably better than would be expected for a release layer that has moderate hydrophobicity but does not have the special surface structure and properties induced by the carrier-contacting surface.

[0399] Working Example Reference is now made to the following examples, which together with the above descriptions illustrate the invention in a non-limiting fashion.

[0400] [Table 1]

[0401] Carriers used as substrates in the production of the release layer surfaces include (1) antistatic polyester film (Examples 1-7), (2) untreated polyester film, i.e., not antistatic (Example 11), and (3) aluminum-treated polyester film (Example 10).

[0402] Example 1 The ITM release layer of Example 1 had the following composition (wt / wt): [Table 2]

[0403] The release layer was prepared as essentially described in the blanket preparation procedure provided below.

[0404] Blanket Preparation Procedure (for release layer cured to carrier surface) All components of the release layer formulation were thoroughly mixed. An initial release layer of the desired thickness was coated onto the PET sheet using a rod / knife (other coating methods may be used) and then cured at 150 degrees Celsius for 3 minutes. Subsequently, Siloprene LSR 2530 was coated onto the top of the release layer using a knife to achieve the desired thickness. Curing was then carried out at 150 degrees Celsius for 3 minutes. An additional layer of Siloprene LSR 2530 was coated onto the top of the previous (cured) silicone layer and the glass fiber fabric was incorporated into this moistened fresh layer so that the moistened silicone penetrated the fabric structure. Curing was then carried out at 150 degrees Celsius for 3 minutes. A final layer of Siloprene LSR 2530 was then coated onto the glass fiber fabric and curing was again carried out at 150 degrees Celsius for 3 minutes. The integral blanket structure was then cooled to room temperature and the PET was removed.

[0405] Example 2 The ITM release layer of Example 2 had the following composition: [Table 3]

[0406] The blanket was prepared substantially as described in Example 1.

[0407] Example 3 The ITM release layer of Example 3 had the following composition: [Table 4]

[0408] The blanket was prepared substantially as described in Example 1.

[0409] Example 4 The ITM release layer of Example 4 had the following composition: [Table 5]

[0410] The blanket was prepared substantially as described in Example 1.

[0411] Example 5 The ITM release layer of Example 5 was prepared from Silopren® LSR2530 (Momentive Performance Materials, Inc., Waterford, NY), a two-component liquid silicone rubber in which the two components were mixed in a 1:1 ratio. The blanket was prepared substantially as described in Example 1.

[0412] Example 6 The ITM release layer of Example 6 has substantially the same composition as the ITM release layer of Example 4, but includes SR545 (Momentive Performance Materials, Waterford, NY), a commercially available silicone-based resin containing polar groups. The polar groups are of the "MQ" type, where "M" represents Me3SiO and "Q" represents SiO4. The complete composition is listed below. [Table 6]

[0413] The blanket was prepared substantially as described in Example 1.

[0414] Example 7 The ITM release layer of Example 7 has substantially the same composition as the ITM release layer of Example 6, but includes polymer RV5000, which includes a vinyl-functional polydimethylsiloxane having a high density of vinyl groups as described above. The full composition is listed below. [Table 7]

[0415] The blanket was prepared substantially as described in Example 1.

[0416] Comparative Examples 1A to 1F ITM release layers were prepared as "corresponding release layers" or "reference release layers" for the compositions of Examples 1-6, such that the corresponding release layers (designated Comparative Examples 1A-1F) had the same compositions as Examples 1-6, respectively. However, during cure of the release layer, the release layer surface (or "ink-receiving surface") was exposed to air according to the conventional preparation procedure provided below ("standard air cure").

[0417] Comparative Blanket Preparation Procedure (for release layers exposed to air during curing) A first layer of Siloprene LSR2530 was coated onto the PET sheet using a rod / knife and then cured at 150 degrees Celsius for 3 minutes to achieve the desired thickness. An additional layer of Siloprene LSR2530 was coated on top of the previous (cured) silicone layer and the glass fiber fabric was incorporated into this wetted fresh layer so that the wetted silicone penetrated the fabric structure. Next, Siloprene LSR2530 was coated on top of the glass fiber fabric followed by curing at 150 degrees Celsius for 3 minutes. All components of the release layer formulation were thoroughly mixed together before forming the initial release layer. The release layer was coated on top of the cured Siloprene LSR2530 to achieve the desired thickness and then cured at 150 degrees Celsius for 3 minutes while the release layer surface was exposed to air.

[0418] Example 8 The contact angle of a distilled water drop on the release layer surface was measured using a proprietary Dataphysics OCA15 Pro contact angle measurement device (Particle and Surface Sciences Pty Ltd, Gosford, NSW, Australia). The procedure used to perform the receding contact angle (RCA) and advancing contact angle (ACA) measurements is a conventional technique detailed by Dr. Roger P. Woodward ("Contact Angle Measurements Using the Drop Shape Method", inter alia www.firsttenangstroms.com / pdfdocs / CAPaper.pdf).

[0419] Results for Examples 1-6 are provided below, along with results for release layers prepared according to Comparative Examples 1A-1F.

[0420] In virtually all cases, the release surfaces produced on the carrier surfaces exhibited receding contact angles that were lower than the identical formulations cured in air. More specifically, the release surfaces produced on the carrier surfaces exhibited receding contact angles that were at least 5 degrees, at least 7 degrees, at least 10 degrees, at least 12 degrees, or at least 15 degrees lower, or by differences within the ranges of 5 degrees to 30 degrees, 7 degrees to 30 degrees, 10 degrees to 30 degrees, 5 degrees to 25 degrees, 5 degrees to 22 degrees, 7 degrees to 25 degrees, or 10 degrees to 25 degrees.

[0421] Example 9 The release layers produced in Examples 1-6 and Comparative Examples 1A-1F were each aged at 160 degrees Celsius for 2 hours to simulate aging under long term operating conditions. Receding contact angles were measured and the results are listed below. [Table 8]

[0422] For the comparative examples, it is clear that the receding contact angle was substantially maintained after the aging treatment. However, for Examples 1-6 of the present invention, it is clear that the receding contact angle increased by typically 4 degrees to 15 degrees after the aging treatment. Without wishing to be bound by theory, the inventors believe that the increase in contact angle in the release layer structure of the present invention is due to a loss in hydrophilic behavior (or increased hydrophobic behavior) due to some change in the location of polar groups (e.g., Si-O-Si) at the release layer surface.

[0423] Example 10 A blanket containing a release layer of the composition of Example 2 was prepared substantially as described in Example 1, but against an aluminized PET carrier surface.

[0424] Example 11 A release layer having the release layer composition of Example 2 was prepared substantially as described in Example 1, but on a commercially available PET carrier surface that had not been subjected to an antistatic pretreatment.

[0425] Example 12 Contact angle measurements were performed on the release layers produced in Examples 2, 10, and 11 according to the present invention to determine both the advancing and receding contact angles, and the results are provided below. [Table 9]

[0426] Examples 10 and 11 exhibited receding contact angles that were about 30 degrees less than the receding contact angle of the same composition cured with the release layer exposed to air. The release layer surface of Example 2 prepared against an antistatic PET carrier surface exhibited a receding contact angle that was about 50 degrees less than the receding contact angle of the same composition prepared while exposed to air.

[0427] Example 13 Contact angle measurements were performed on the support surfaces utilized in Examples 2, 10, and 11 to determine both the advancing and receding contact angles, and the results are provided below. [Table 10]

[0428] It can be seen from the receding contact angles obtained that the three support surfaces exhibited hydrophilic behavior, with the antistatic treated PET exhibiting the greatest degree of hydrophilic behavior (20 degrees RCA vs. 40 degrees RCA).

[0429] Importantly, the hydrophilic behavior of the carrier surface is at least partially induced in the respective release surfaces, such that a formulation cured while exposed to air has an RCA of 65 degrees, an identical formulation prepared against an antistatic PET surface has an RCA of 45 degrees, and the antistatic PET carrier used exhibits an RCA of 20 degrees. Thus, the release layer structures of the present invention have release surfaces whose hydrophilic / hydrophobic properties lie between those of an identical formulation cured in air and those of the carrier surface itself.

[0430] Example 14 The peel surface energies were calculated for the ink receptive surfaces of the following examples: Example 1A cured under exposure to air, Example 1 cured against an antistatic PET surface, and Example 1 cured against an antistatic PET surface followed by a standard aging procedure at 160 degrees Celsius for 2 hours. All three examples have the same chemical composition.

[0431] For each of these three examples, the total surface energy was calculated using the traditional "harmonic mean" method (also known as the Owens-Wendt surface energy model; see, e.g., KRUSS Technical Note TN306e). The results are provided below. [Table 11]

[0432] The release layer surface of Example 1A, cured under exposure to air, exhibited extreme hydrophobicity and had a low total surface energy of 20.9 J / m, as expected. 2 This is fairly close to the literature value for surface energy for polydimethylsiloxane (PDMS). Importantly, Example 1 cured against an antistatic PET surface had a surface energy of about 26 J / m 2 This Example 1 shows slightly less hydrophobicity than the "air cured" sample. After this formulation was subjected to the standard aging procedure, the total surface energy was about 26 J / m 2 from 23 J / m 2 This result would be seen to confirm the RCA results obtained for various aged and unaged materials of this representative formulation.

[0433] Example 15 The release layer surface energies were calculated for the ink-receptive surfaces of the following examples: Example 2A cured under exposure to air, Example 2 cured against an anti-static PET surface, and Example 2 cured against an anti-static PET surface followed by a standard aging procedure at 160 degrees Celsius for 2 hours. All three examples have the same chemical composition.

[0434] As in Example 14, the total surface energy was calculated using the traditional "harmonic mean" method, and the results are provided below. [Table 12]

[0435] Example 2A cured under air exposure conditions produced a release layer surface that was less hydrophobic than the release layer of Example 1A, with a total surface energy of about 35 J / m2. Example 2 cured against an antistatic PET surface exhibited a total surface energy of about 49 J / m2, which is significantly less hydrophobic than the "air cured" sample. After this formulation was subjected to the standard aging procedure, the total surface energy decreased from about 49 J / m2 to about 40 J / m2. This result would be seen to support the RCA results obtained for various aged and unaged materials of this representative formulation.

[0436] Example 16 The temperature on the blanket surface is kept at 75 degrees Celsius. An image (usually 10-100% color gradation) is printed on the blanket at a speed of 1.7 m / s with a resolution of 1200 dpi. An uncoated paper (A4 Xerox Premium Copy Paper, 80 gsm) is placed between the pressure roller and the blanket, and the pressure is set at 3 bar and the pressure roller is pressed against the blanket. The pressure roller moves over the paper, applying pressure on the contact line between the blanket and the paper, facilitating the transfer process. In some cases, incomplete transfer (residual ink left on the blanket surface) can be observed. To assess the extent of residual ink, a glossy paper (A4 Burgo glossy paper 130 gsm) is placed on the blanket as well as the uncoated paper and the transfer process is carried out again. Any ink left on the blanket and not transferred to the uncoated paper will be transferred to the glossy paper. Thus, glossy paper can be rated for residual ink according to the following scale (% of image surface area): A - No visible residue B - Visible residue is 1-5% C- Visible residue is greater than 5% The results of the evaluation are provided below. [Table 13]

[0437] Example 17 Example 16 was repeated for the release surfaces of Example 2 and Example 3, except that the printing speed was 3.4 m / sec on the blanket. Both release surfaces retained a transfer rating of A.

[0438] Example 18 The ITM release layer compositions of Examples 2 and 3 were cured against a PET substrate according to the procedure provided in Example 1. The ITM release layer compositions of Examples 2 and 3 were cured against air according to the procedures provided in Comparative Examples 1B and 1C. The samples were then subjected to dynamic contact angle (DCA) measurements at 10 seconds and subsequently at 70 seconds according to the following procedure.

[0439] The drop is placed on a smooth PTFE thin film surface with the smallest possible droplet falling so that kinetic energy does not cause the drop to expand. A pendant drop is then formed. The specimen is then raised until it contacts the base of the drop. If the drop is large enough, adhesion to the surface will pull the drop away from the tip of the needle. The tip of the needle is positioned above the surface at a height such that the growing pendant drop contacts the surface and separates before falling freely under its own weight.

[0440] The dynamic contact angle is then measured at 10 seconds and 70 seconds, and the results are provided below. [Table 14]

[0441] It is observed that an initial measurement of the dynamic contact angle at 10 seconds provides a strong indication of the hydrophilicity of the release layer surface. A subsequent measurement at 70 seconds provides an indication of the extent to which any liquid (e.g., polyether glycol functionalized polydimethylsiloxane, etc.) disposed within the release layer is incorporated into the droplet. Such incorporation may further reduce the measured DCA.

[0442] Thus, the samples cured against PET exhibited substantially lower (more hydrophilic) initial DCA measurements (105°, 87°) compared to the hydrophilic initial DCA measurements (114°, 113°) of the respective samples cured against air. In addition to the displayed hydrophilicity, the samples cured against PET exhibited a drop in DCA of 8 to 17 degrees between the first and second measurements.

[0443] In Figures 25A-C, images of various ink patterns printed on the release layer of an ITM of the present invention are provided, where the release layer of Example 2 was cured against a PET carrier surface. Figures 26A-C are images of the same ink patterns printed on the release layer of Example 2, where the release layer was cured against air. Comparing Figures 25A and 26A, it is clear that the ITM of the present invention exhibits higher optical density and more accurately reflects the ink image pattern. A comparison between Figures 25C and 26C reveals the same conclusion. Now comparing Figures 25B and 26B, it is clear that the ink dots in Figure 25B are perceptibly larger than the ink dots in Figure 26B.

[0444] As used herein and in the appended claims, the term "receding contact angle" or "RCA" refers to a receding contact angle measured at ambient temperature using a Dataphysics OCA15 Pro Contact Angle measuring device, or a similar Video-Based Optical Contact Angle Measuring System, using the Drop Shape Method described above. The similar term "advancing contact angle" or "ACA" refers to an advancing contact angle measured in a substantially identical manner.

[0445] The term "dynamic contact angle" or "DCA" as used herein and in the appended claims refers to dynamic contact angle measured using a Dataphysics OCA15 Pro Contact Angle measuring device or a similar Video-Based Optical Contact Angle Measuring System, using the method detailed by Dr. Roger P. Woodward in "Contact Angle Measurements Using the Drop Shape Method" referenced above, and detailed in Example 17 above.

[0446] As used herein and in the appended claims, the term "standard aging procedure" refers to an accelerated aging procedure performed on each test release layer in a standard convection oven at 160 degrees Celsius for two hours.

[0447] As used herein and in the appended claims, the term "standard air cure" refers to a conventional curing process for curing a release layer as described with respect to Comparative Examples 1A-1F, in which the release layer surface (or "ink-receptive surface") is exposed to air while the release layer is cured.

[0448] The term "bulk hydrophobicity" as used in the specification and the appended claims is characterized by the receding contact angle of a distilled water droplet disposed on the inner surface of the release layer, the inner surface being formed by exposing areas of cured silicone material within the release layer.

[0449] Examples C1 to C12 Representative compositions of ITM aqueous treatment fluids of the present invention are provided in the table below. [Table 15] JPEG2024156784000017.jpg228165JPEG2024156784000018.jpg222166

[0450] Examples C13 to C22 The compositions of the ITM aqueous treatment liquids and various properties thereof are provided in the table below as example compositions C13-C22. [Table 16]

[0451] For Examples C1-C12, the viscosity of each sample measured at room temperature is provided below (all values ​​in cP). C1=19.2 C2=18.15 C3=22.3 C4=36.2 C5=19.8 C6=21.2 C7=28.1 C8=18.0 C9=50.0 C10=48.2 C11=20.2 C12=20.7

[0452] The surface tensions for these treatment formulations were more uniform than those for the 12 representative formulations, generally within the range of 26-29 mN / m or 26-28 mN / m at room temperature.

[0453] Example C23 An additional aqueous treatment formulation is provided in Example C23. This formulation has no surfactants other than a quaternary ammonium salt (Larostate 264) present in a relatively high percentage (8 wt%) to sufficiently reduce the surface tension of the aqueous treatment formulation. Its surface tension and viscosity are 32.3 mN / m and 17.8 cP, respectively, at room temperature. [Table 17]

[0454] Dye preparation The pigments used in the examples described below are generally given an initial particle size of a few micrometers. The pigments were milled to the submicron range in the presence of a dispersing agent. The two substances were fed to the milling apparatus as an aqueous mixture. Unless otherwise stated, 30 g of pigment was mixed with a weight of dispersing agent satisfying the weight ratios shown in the examples below. Deionized water was added to the remainder of 200 g. The liquid slurry was milled in a Union Process HDDM-01 / HD-01 attritor to a particle size of 100 nm or less (D V50 The particles were size reduced in the presence of 4500 g of chrome steel beads (Glen Mills, USA) having a diameter of 0.8 mm for a sufficient period of time and with sufficient energy input to prepare a millbase containing pigment particles having a median diameter (analyzed per particle volume) of ≦100 nm. Typically, the mill was operated at about 3000 rpm for at least 48 hours. The milling period was dependent on the initial particle size.

[0455] The particle size and particle size distribution in the compositions so prepared were determined using DLS method (Malvern Zetasizer Nano ZS). Unless otherwise stated, an aliquot was taken from the composition of interest and, if necessary, diluted with double distilled water (DDW) to obtain a sample with a solid concentration of about 1% by weight. Prior to performing DLS measurements, the liquid sample was briefly sonicated (Sonics Vibracell VCX 750 (750 watts) at 75% of maximum power for about 7 seconds) to ensure that the pigment particles were properly dispersed when estimating particle size and distribution. The results were analyzed based on the volume of the particles.

[0456] Once the pigment-dispersant mixture reached the desired particle size, 50 g of water was added to the milling chamber and the resulting diluted dispersion was extracted from the mixture. The beads were separated by filtering the diluted millbase through a suitable mesh. The pigment concentration at this point was 12% by weight.

[0457] To the pigment / dispersant millbase was added sodium dodecanoate (SDD) and / or at least one of the following additives: potassium dodecanoate, sodium oleate, potassium oleate, sodium myristate, potassium myristate, sodium dodecyl sulfate, sodium dodecylbenzenesulfonate, potassium octanoate, and sodium octanoate, as needed to obtain a composition having a pigment concentration of 10% by weight.

[0458] Example I1 - Ink Composition This example describes the preparation of an ink composition. Heliogen® Blue D7079 was ground using a Disperbyk® 190 in an HDDM-01 / HD-01 grinder as previously described. The materials were mixed in the following proportions: [Table 18] The milled concentrate is currently produced using a D V 50 and further diluted with 50 g water and extracted from the mill at 12 wt% pigment concentration. The mill base concentrate was further processed as described below for the preparation of an ink composition. In a first step, 2.4 g of sodium dodecanoate was added to 200 g of the mill base concentrate, thereby obtaining a mill base. The mixture was stirred (5 min, magnetic stirrer at 50 rpm) until homogeneity was reached and incubated at 60 degrees Celsius for 1 day. The mixture was then left to cool to ambient temperature. In a second step, the ink ingredients were added to the mill base as follows: [Table 19] The mixture was stirred at ambient temperature for 30 minutes, resulting in an ink-jettable ink composition having a viscosity of less than 10 cP.

[0459] Examples I2 to I5 - Ink Compositions The inks of Example I1 were formulated but with the addition of 5, 10, 12, and 15 g of TWEEN® 20, respectively.

[0460] Dot Gain Dot gain refers to the increase in dot size relative to the initial spherical drop size. Dot gain is determined by the ratio of the final dot size to the initial drop size. It would be highly desirable to find a way to increase dot size without having to increase the drop volume.

[0461] Utilizing the inventive techniques described herein, the inventors have achieved dot gains of at least 1.5, or 1.6, and more typically at least 1.7, at least 1.8, at least 1.9, or at least 2.0, or within the ranges of 1.5-2.2, 1.5-2.1, 1.7-2.1, or 1.8-2.1.

[0462] For example, using drops having a volume of 6.3 picoliters (D=22.9 micrometers) and using the aqueous treatment formulation of the present invention, the resulting dried ink dots were in the diameter range of 40 to 48 micrometers.

[0463] As used herein and in the appended claims, "hydrophobic" and "hydrophilic", as well as other terms, may be used in a relative sense and not necessarily in an absolute sense.

[0464] The term "functional group" as used herein and in the appended claims refers to a group or moiety attached to the polymer structure of the release layer that has a higher polarity than the O-Si-O group of conventional addition-cured silicones. Various examples are provided herein. The inventors observe that pure addition-cured polydimethylsiloxane polymers contain O-Si-O, SiO4, Si-CH3, and CC groups, and that most other functional groups have a higher dipole, and therefore such functional groups can be considered "functional". It will be apparent to those skilled in the art that such functional groups may have a tendency or strong tendency to react with components typically present in water-based inks utilized in indirect inkjet printing at processing temperatures up to 120 degrees Celsius.

[0465] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs. In case of conflict, the present specification, including definitions, will control.

[0466] In this specification and the claims of this disclosure, the verbs "comprise," "include," and "have" and their conjugations are used to indicate that the object(s) of the verb are not necessarily an exhaustive list of members, components, elements, steps, or portions of the subject(s) of the verb. These terms encompass the terms "consisting of" and "consisting essentially of."

[0467] As used herein, the singular forms "a," "an," and "the" include plural references and mean "at least one" or "one or more" unless specifically stated otherwise.

[0468] Location or motion-related terms such as "top," "bottom," "right," "left," "bottom," "down," "low," "top," "upper," "high," "vertical," "horizontal," "reverse," "forward," "upstream," and "downstream," and grammatical variations thereof, may be used herein for illustrative purposes to indicate the relative location, position, or movement of particular components, to indicate a first component and a second component in the present example, or both. Such terms do not necessarily indicate that, for example, a "bottom" component is below a "top" component, and such orientations, components, or both may be flipped, rotated, moved in space, positioned in a diagonal direction or position, positioned vertically or horizontally, and similarly altered.

[0469] Unless otherwise stated, the use of the word "and / or" between the last two elements of a list of selection options indicates that one or more of the listed options are possible.

[0470] As used herein and in the appended claims, the term "%" refers to weight percent, unless otherwise specified.

[0471] Similarly, the term "ratio" as used in this specification and the appended claims refers to weight ratio, unless otherwise specified.

[0472] In this disclosure, unless otherwise specified, the adjectives "substantially" and "about" modifying a state or relationship characteristic of a feature or features of an embodiment of the present technology should be understood to mean that the state or characteristic is defined within a range of error that is acceptable for the operation of the embodiment for its intended application.

[0473] While the present disclosure has been described in connection with specific embodiments and generally associated methods, modifications and permutations of the various embodiments and methods of the present invention will become apparent to those skilled in the art. It is to be understood that the present disclosure is not limited to the specific embodiments described herein, but rather is limited only by the scope of the appended claims.

Claims

1. providing an intermediate transfer member (ITM) comprising a silicone-based release layer surface that exhibits sufficient hydrophilicity to satisfy at least one of the following characteristics: (i) a distilled water droplet deposited on said silicone-based release layer surface has a receding contact angle of up to 60 degrees, and (ii) a distilled water droplet deposited on said silicone-based release layer surface has a 10 second dynamic contact angle (DCA) of up to 108 degrees; b. below: i. at least 3% by weight of a quaternary ammonium salt having a water solubility of at least 5% at 25 degrees Celsius; ii. at least 1% by weight of at least one water soluble polymer having a water solubility of at least 5% at 25 degrees Celsius; and iii. a carrier liquid comprising water, said water comprising at least 65% by weight of said aqueous treatment formulation; wherein the aqueous treatment formulation has the following properties: i. a static surface tension in the range of 20-40 dynes / cm at 25 degrees Celsius; ii. a dynamic viscosity at 25 degrees Celsius of at least 10 cP; and iii. 60° Celsius evaporative loading up to 8:1 by weight; providing an aqueous treatment formulation having c. applying the aqueous treatment formulation to the silicone-based release layer surface of the ITM to form a wet treatment layer on the silicone-based release layer surface having a thickness of up to 0.8 μm; d. subjecting the wet treatment layer to a drying treatment to form a dry treatment thin film from the wet treatment layer on the surface of the silicone-based release layer; e. depositing droplets of a water-based ink onto the dried treated film to form an ink image on the silicone based release layer surface; f. drying said ink image to leave a residual ink image on the surface of said silicone based release layer; g. transferring said residual ink image onto said print substrate by pressure contact between said ITM and said print substrate; A printing method comprising:

2. 2. The method of claim 1, wherein the 60 degree Celsius evaporative loading of the provided aqueous treatment formulation is at most 6:1, at most 5:1, at most 4:1, at most 3.5:1, or at most 3:1, and optionally at least 2:1, at least 2.2:1, or at least 2.5:

1.

3. 3. The method of claim 1 or claim 2, wherein the concentration of the quaternary ammonium salt in the provided aqueous treatment formulation is in the range of 3 to 15%, the concentration of the water soluble polymer is in the range of 2.5 to 10% or 2.5 to 8%, the 60 degree Celsius evaporation loading is in the range of 2.5:1 to 4:1, and the viscosity is at least 12 cP, optionally at least 14 cP or at least 16 cP.

4. 4. The method of any one of claims 1 to 3, wherein the provided aqueous treatment formulation has a total surfactant concentration in the range of at least 6%, at least 7%, at least 8%, at least 9%, or at least 10%, and optionally 6-40%, 6-30%, 6-20%, 7-30%, 7-20%, 7-15%, 8-25%, 8-20%, 8-15%, or 8-13%.

5. 5. The method of any one of claims 1 to 4, wherein the total concentration of organic solvents in the provided aqueous treatment formulation is at most 3 wt-%, at most 2 wt-%, at most 1 wt-%, or at most 0.5 wt-%, or the formulation is free of organic solvents.

6. 6. The method of any one of claims 1 to 5, wherein the concentration of liquid moisture absorbent in the provided aqueous treatment formulation is at most 1.5 wt%, at most 1 wt%, at most 0.5 wt%, at most 0.3 wt%, or at most 0.1 wt%, or the aqueous treatment formulation is free of liquid moisture absorbent.

7. The method of any one of claims 1 to 6, wherein the quaternary ammonium salt in the provided aqueous treatment formulation is an organic quaternary ammonium salt.

8. 8. The method of claim 7, wherein the first carbon chain of the organic quaternary ammonium salt has a length of at least 6 carbon atoms, and optionally a length in the range of 6 to 20, 6 to 18, 8 to 20, or 8 to 18 carbon atoms.

9. 9. The method of claim 8, wherein the second carbon chain of the organic quaternary ammonium salt has a length of up to 3 carbon atoms, or up to 2 carbon atoms.

10. 10. The method of claim 9, wherein the tertiary carbon chain of the organic quaternary ammonium salt has a length of up to 3 carbon atoms, up to 2 carbon atoms, or up to 1 carbon atom.

11. A method according to any one of claims 7 to 10, wherein the organic quaternary ammonium salt is a cationic organic quaternary ammonium salt, optionally having a sulfate or phosphate anion.

12. 12. The method of any one of claims 1 to 11, wherein the silicone based release layer surface exhibits sufficient hydrophilicity to satisfy at least one of the following characteristics: a receding contact angle of a distilled water drop deposited on the silicone based release layer surface is at most 60 degrees.

13. 13. The method of any one of claims 1 to 12, wherein the silicone based release layer surface exhibits sufficient hydrophilicity to satisfy at least one of the following characteristics: a 10 second dynamic contact angle (DCA) of a distilled water drop deposited on the silicone based release layer surface is up to 108 degrees.

14. 14. The method of any one of claims 1 to 13, wherein the provided ITM comprises a support layer, a release layer having the silicone-based release layer surface, and a second surface (i) facing the silicone-based release layer surface and (ii) attached to the support layer, the release layer being formed from an addition-cured silicone material, the release layer having a thickness of up to 500 micrometers (μm).

15. 15. The method of claim 14, wherein the release layer of the provided ITM has the following property: the addition-cured silicone material consists essentially of or comprises at least 95% by weight of the addition-cured silicone.

16. 16. The method of claim 14 or claim 15, wherein functional groups within the silicone-based release layer surface of the provided ITM comprise up to 3% by weight of the addition-cured silicone material.

17. The method of any one of claims 14 to 16, wherein a polyether glycol functionalized polydimethylsiloxane is loaded into the addition cured silicone material of the provided ITM.

18. 18. The method of any one of claims 14 to 17, wherein the release layer of the provided ITM is adapted such that the polar groups of the ink-receiving surface have a direction away from or opposite to the second surface.

19. 19. The method of any one of claims 1 to 18, wherein a surface hydrophobicity of a silicone-based release layer surface of the provided ITM is less than a bulk hydrophobicity of the cured silicone material in the release layer, the surface hydrophobicity being characterized by a receding contact angle of a distilled water droplet on the ink-receiving surface, and the bulk hydrophobicity being characterized by a receding contact angle of a distilled water droplet deposited on an inner surface formed by exposing an area of ​​the cured silicone material in the release layer to form an exposed area.

20. 20. The method of any one of claims 1 to 19, wherein the aqueous treatment formulation is applied to the surface of the silicone-based release layer such that the thickness of the wet treatment layer is up to 0.5 μm, or up to 0.4 μm.

21. the wetting treatment layer is formed and / or thinned by forcing a rounded surface towards the ITM or the ITM towards the rounded surface; i. the rounded surface has a radius of curvature of at most 2 mm, or at most 1.5 mm, or at most 1.25 mm, or at most 1 mm; and / or ii. the biasing is performed with a force density in the cross print direction of at least 250 g / cm, or at least 350 g / cm, or at least 400 gm / cm, and / or at most 1 kg / cm, or at most 750 g / cm, or at most 600 g / cm; and / or iii. the biasing is performed by applying pressure between the ITM, the magnitude of the pressure being at least 0.1 bar, or at least 0.25 bar, or at least 0.35 bar, or at least 0.5 bar, and optionally up to 2 bar, or up to 1.5 bar, or up to 1 bar; The method according to any one of claims 1 to 20.

22. The formation of the wetting treatment layer or the thinning of the wetting treatment layer is performed by establishing a velocity gradient perpendicular to the ITM, the magnitude of the velocity gradient being at least 10 6 / sec or at least 2×10 6 A method according to any one of claims 1 to 21, comprising forcing the aqueous treatment formulation to flow for 100-250 s / sec.

23. 23. The method according to any one of claims 1 to 22, wherein the drying of the wet treatment layer is carried out sufficiently rapidly such that the viscosity of the aqueous treatment formulation increases rapidly enough such that surface tension induced beading is inhibited and the dried treatment film has a smooth upper surface.

24. 24. The method of claim 23, wherein the smooth upper surface of the dried processed thin film is characterized by an average roughness Ra of at most 12 nanometers, or at most 10 nanometers, or at most 9 nanometers, or at most 8 nanometers, or at most 7 nanometers, or at most 5 nanometers.

25. 25. A method according to any one of the preceding claims, wherein drying of the treatment solution is carried out sufficiently rapidly to prevent beading and to leave behind a continuous hydrophilic and cohesive polymer treatment film having a thickness of at most 200 nm, or at most 150 nm, or at most 120 nm, or at most 100 nm, or at most 80 nm, or at most 70 nm, or at most 60 nm, or at most 50 nm, or at most 40 nm, or at most 30 nm.

26. The method according to any one of the preceding claims, wherein the dried film onto which the aqueous ink droplets are deposited has a thickness of up to 200 nm, or up to 120 nm, or up to 100 nm, or up to 80 nm.

27. The method of any one of claims 1 to 26, wherein the dried film onto which the aqueous ink droplets are deposited has a thickness of at least 15 nm, or at least 20 nm, or at least 30 nm.

28. 28. The method of any one of claims 1 to 27, wherein the dry treatment film is continuous across a rectangle of the release surface of the ITM, the rectangle having a width of at least 10 cm and a length of at least 10 meters.

29. 26. The method of claim 25, wherein for at least 50%, or at least 75%, or at least 90%, or at least 95%, or at least 95%, or at least 99%, or 100% of the area of ​​the rectangle, the thickness of the dried process film does not deviate from the average thickness value within the rectangle by more than 50%, or 40%, or 30%.

30. 30. The method according to any one of claims 1 to 29, wherein during the drying process of the wet processing layer, the dynamic viscosity of the wet processing layer increases by at least 1000 times within a period of up to 250 milliseconds.

31. The method of any one of claims 1 to 30, wherein the residual ink image is transferred onto the print substrate together with the non-printed areas of the dry treatment film.

32. 32. The method of claim 31 , wherein the dry processed film has a thickness of up to 120 nm.

33. 33. The method of any one of claims 1 to 32, wherein the dry treatment film has sufficient cohesion such that during transfer of the residual ink image, the dry treatment film completely separates from the ITM in both printed and non-printed areas and is transferred to the print substrate along with the dry ink image.

34. 34. The method of any one of claims 1 to 33, wherein the aqueous ink solids flow into the bulk of the dried process film and react with quaternary ammonium salts present in the dried process film, thereby facilitating droplet spreading.

35. i. An ink dot set IDS of ink dots present on an ink substrate is formed; ii. The droplet plurality DP of the aqueous ink droplets deposited on the dried film present on the ITM is such that a given droplet gives rise to and / or evolves into an ink dot present on a given substrate; A. each said given droplet of said droplet plurality DP; B. the ink dots present on the given substrate for each of the sets of ink dots; forming the ink dot set IDS of ink dots present on the ink substrate such that there is a correspondence between iii. during deposition, whenever a droplet of the droplet plurality impacts the dried processing film on the ITM, the kinetic energy of the impacting droplet transforms the droplet; iv. The maximum impact radius of each droplet of the deformed droplet across the surface of the ITM is a maximum impact radius value R MAX_IMPACT having v. After impact, each ink dot of the ink dot set IDS present on the substrate has a dry dot radius R DRIED_DOT_ON_SUBSTRATE physicochemical forces cause the deformed droplet to expand so as to have vi. for each droplet of said droplet plurality and corresponding ink dot of said ink dot set IDS, A. The radius R of the dry dots present on the substrate DRIED_DOT_ON_SUBSTRATE and, B. The deformed droplet maximum collision radius value R MAX_IMPACT and is carried out such that the ratio of A method according to any one of claims 1 to 34.

36. i. a droplet multiplicity DP of the droplets deposited on a dried processing film present on the ITM generates an ink dot set IDS of ink dots present on a substrate (i.e. fixedly attached to an upper substrate surface), each droplet of the droplet multiplicity DP corresponding to an ink dot present on a different respective substrate of the ink dot set IDS; ii. each ink droplet of said droplet plurality DP is deposited on said substrate according to ejection parameters; iii. The ejection parameters together with the physicochemical properties of the ink droplets of the droplet plurality DP jointly determine the inkjet paper dot radius R DIRECT-JETTING-ONTO-INK-JET-PAPER-THEORETICAL and the inkjet paper dot radius R DIRECT-JETTING-ONTO-INK-JET-PAPER-THEORETICAL is the radius of the ink dot obtained if the ink droplet is inkjetted directly onto inkjet paper and not onto the drying process film, iv. A. The dry dot radius R of the dots of the ink dot set IDS DRIED_DOT_ON_SUBSTRATE and, B. The inkjet paper dot radius R DIRECT-JETTING-ONTO-INK-JET-PAPER-THEORETICAL and is carried out such that the ratio between is at least 1:1; A method according to any one of claims 1 to 35.

37. 37. The method of claim 35 or claim 36, wherein a density of the set of ink dots is at least 5, or at least 10, or at least 20, or at least 50, or at least 100, and each ink dot of the set of ink dots is clearly distinct on the substrate.

38. The method according to any one of claims 35 to 37, wherein the ink dots of the ink dot set are contained within a square geometric protrusion protruding on the printing substrate, each ink dot of the ink dot set is fixedly attached to the surface of the printing substrate, and all the ink dots within the square geometric protrusion are considered as individual members of the ink dot set IDS.

39. i. An ink dot set IDS of ink dots present on an ink substrate is formed; ii. the density of the set of ink dots is at least 5, or at least 10, or at least 20, or at least 50, or at least 100, and each ink dot of the set of ink dots is distinct on the substrate; iii. The ink dots of the ink dot set are included within a square geometric protrusion protruding on a printing substrate, each ink dot of the ink dot set is fixedly attached to the surface of the printing substrate, and all the ink dots within the square geometric protrusion are considered as individual members of the ink dot set IDS; iv. each of said ink dots comprises at least one colorant dispersed in an organic polymer resin, each of said ink dots having an average thickness of less than 2,000 nm and a diameter of 5 to 300 micrometers; v. Each of the ink dots has a generally convex shape, and the deviation from the convex shape (DC dot ) is D.C. dot = 1 - AA / CSA, where AA is the calculated projected area of ​​the dot, the projected area being approximately parallel to the print substrate, and CSA is the surface area of ​​the convex shape that smallest encloses the contour of the projected area; vi. The average deviation of the set of ink dots from convexity (DC dot mean ) is at most 0.05, at most 0.04, at most 0.03, at most 0.025, at most 0.022, at most 0.02, at most 0.018, at most 0.017, at most 0.016, at most 0.015, or at most 0.014; A method according to any one of claims 1 to 38.

40. 40. The method of any one of claims 1 to 39, wherein the aqueous treatment formulation is applied to at least a portion or portions of the moving ITM at a speed of at least 1 meter / sec, or at least 1.5 meters / sec, or at least 2 meters / sec to form the wet treatment layer on the ITM.

41. 1. An aqueous treatment formulation for use with an intermediate transfer member of a printing system, comprising: (a) a first surfactant composition comprising a first surfactant, the first surfactant comprising a quaternary ammonium salt having a water solubility of at least 5% at 25 degrees Celsius; and (b) at least 1% by weight of at least one water-soluble polymer having a water solubility of at least 5% at 25 degrees Celsius; (c) a carrier liquid comprising water, said water comprising at least 65% by weight of said treatment formulation; Including, the concentration of said quaternary ammonium salt in said aqueous treatment formulation is at least 3% by weight; The treatment formulation has (i) a static surface tension at 25 degrees Celsius in the range of 20-40 dynes / cm, (ii) a 60 degrees Celsius evaporation loading of up to 8:1 by weight, and (iii) a 25 degrees Celsius viscosity in the range of 10 cP to 100 cP. Aqueous treatment formulations.

42. 42. The aqueous treatment formulation of claim 41, wherein the solubility of the quaternary ammonium salt is at least 7%, at least 10%, at least 15%, or at least 20%, optionally up to 50%, up to 40%, or up to 35%, or further optionally within the range of 5-40%, 5-30%, 5-25%, 7-35%, 10-35%, 12-35%, or 15-35%.

43. 43. The aqueous treatment formulation of claim 41 or claim 42, wherein the concentration of the quaternary ammonium salt within the aqueous treatment formulation is at least 4%, at least 5%, at least 6%, or at least 7%, optionally up to 30%, up to 25%, or up to 20%, or further optionally within the range of 2-30%, 3-30%, 4-30%, 4-20%, 5-25%, 6-25%, 6-20%, or 7-20%.

44. 44. The aqueous treatment formulation of any one of claims 41 to 43, wherein the concentration of the water soluble polymer in the aqueous treatment formulation is in the range of at least 1.5% by weight, or at least 2% by weight, at least 2.5% by weight, at least 3% by weight, or at least 3.5% by weight, optionally up to 10%, or up to 9%, or up to 8%, or up to 7%, or up to 6%, or further optionally 1.5-20%, or 2-10%, 2-8%, 2-7%, 2.5-10%, 2.5-8%, 2.5-7%, 2.5-6%, 3-8%, 3-7%, 3-6%, 3-6%, 3.5-10%, 3.5-8%, 3.5-7%, 3.5-6%, or 4-6%.

45. 45. The aqueous treatment formulation of any one of claims 41 to 44, wherein the water solubility of the water soluble polymer is at least 7%, at least 10%, at least 12%, or at least 15%.

46. 46. ​​The aqueous treatment formulation of any one of claims 41 to 45, wherein the water soluble polymer is selected from the group consisting of polyvinyl alcohol, water soluble cellulose, polyvinylpyrrolidone (PVP), polyethylene oxide, polyethyleneimine, and water soluble acrylates.

47. 47. The aqueous treatment formulation of any one of claims 41 to 46, wherein the 60 degree Celsius evaporative loading is at most 6:1, at most 5:1, at most 4:1, at most 3.5:1, or at most 3:1, and optionally at least 2:1, at least 2.2:1, or at least 2.5:

1.

48. 48. The aqueous treatment formulation of any one of claims 41 to 47, further comprising a second surfactant selected to reduce the static surface tension of the aqueous treatment formulation, optionally a silicone polyether, optionally having a concentration in the formulation of at least 1%, at least 1.5%, at least 2%, at least 2.5%, or at least 3%, optionally up to 15%, up to 12%, up to 10%, up to 8%, or up to 7%, or further optionally within the range of 1.5-13%, 1.5-10%, 2-13%, 2-10%, 2.5-13%, 2.5-10%, or 3-10%.

49. 49. The aqueous treatment formulation of any one of claims 41 to 48, further comprising a water absorbing agent disposed within the carrier liquid at a temperature in the range of at least 25 degrees Celsius to 60 degrees Celsius, whereby the aqueous treatment solution is evaporated to form a solid film and the water absorbing agent functions as a water absorbent.

50. 50. The aqueous treatment formulation of any one of claims 41 to 49, further comprising a water absorbing agent disposed within the carrier liquid, the water absorbing agent being solid in a pure state at least within a range of 25 degrees Celsius to 60 degrees Celsius, and acting as a water absorbent when the aqueous treatment solution evaporates to form a solid film.

51. 51. The aqueous treatment formulation of claim 50, wherein the water absorbing agent has a concentration of 1-25%, 1-15%, 1-10%, 2.5-20%, 2.5-12%, 3-15%, 3-12%, 3-10%, or 3.5-12%.

52. 52. The aqueous treatment formulation of any one of claims 41 to 51, wherein the concentration of the quaternary ammonium salt is in the range of 3 to 15%, the concentration of the water soluble polymer is in the range of 2.5 to 10%, 2.5 to 8%, or 2.5 to 7%, or 2.5 to 6%, the 60 degree Celsius evaporation loading is in the range of 2.5:1 to 4:1, and the viscosity is at least 12 cP, optionally at least 14 cP or at least 16 cP.

53. 53. The aqueous treatment formulation of claim 52, wherein the static surface tension is in the range of 25 to 36 dynes / cm.

54. 54. An aqueous treatment formulation according to claim 52 or claim 53, wherein the water absorbing agent has a concentration of 2.5 to 10%.

55. 55. The aqueous treatment formulation of any one of claims 41 to 54, having a total surfactant concentration of at least 6%, at least 7%, at least 8%, at least 9%, or at least 10%, and optionally in the range of 6-40%, 6-30%, 6-20%, 7-30%, 7-20%, 7-15%, 8-25%, 8-20%, 8-15%, or 8-13%.

56. 56. The aqueous treatment formulation of any one of claims 51 to 55, wherein all components of the aqueous treatment formulation are completely dissolved.

57. 57. The aqueous treatment formulation of any one of claims 51 to 56, wherein the total concentration of organic solvents in the aqueous treatment formulation is at most 3 wt-%, at most 2 wt-%, at most 1 wt-%, or at most 0.5 wt-%, or the formulation is free of organic solvents.

58. 58. A treatment formulation according to any one of claims 51 to 57, wherein the concentration of liquid moisture absorbent in the aqueous treatment formulation is at most 1.5 wt%, at most 1 wt%, at most 0.5 wt%, at most 0.3 wt%, or at most 0.1 wt%, or the aqueous treatment formulation is free of liquid moisture absorbent.

59. A treatment formulation according to any one of claims 27 to 48, wherein the quaternary ammonium salt is an organic quaternary ammonium salt.

60. 60. The aqueous treatment formulation of claim 59, wherein the first carbon chain of the organic quaternary ammonium salt has a length of at least 6 carbon atoms, and optionally a length in the range of 6 to 20, 6 to 18, 8 to 20, or 8 to 18 carbon atoms.

61. 61. The aqueous treatment formulation of claim 60, wherein the second carbon chain of the organic quaternary ammonium salt has a length of up to 3 carbon atoms, or up to 2 carbon atoms.

62. 47. The aqueous treatment formulation of claim 46, wherein the tertiary carbon chain of the organic quaternary ammonium salt has a length of up to 3 carbon atoms, up to 2 carbon atoms, or 1 carbon atom.

63. 63. An aqueous treatment formulation according to any one of claims 59 to 62, wherein the organic quaternary ammonium salt is a cationic organic quaternary ammonium salt, optionally having a sulfate or phosphate anion.

64. 64. A treatment formulation according to any one of claims 41 to 63, wherein the polyethyleneimine comprises up to 0.8%, 0.6%, 0.4%, or 0.3%, or 0.2%, or 0.1% by weight of the formulation, or wherein the polyethyleneimine comprises up to 30%, up to 20%, up to 15%, up to 10%, or up to 5% by weight of the water soluble polymer.

65. 65. The treatment formulation of any one of claims 41 to 64, wherein the viscosity is at least 12 cP, at least 14 cP, or at least 16 cP, optionally up to 90 cP, up to 80 cP, up to 70 cP, up to 60 cP, up to 55 cP, or up to 50 cP, and further optionally in the range of 10-80 cP, 12-80 cP, 12-60 cP, 12-55 cP, or 14-60 cP.

66. 66. A treatment formulation according to any one of claims 41 to 65, wherein the water soluble polymer concentration in the provided aqueous treatment formulation is up to 10% by weight, or up to 8% by weight, or up to 6% by weight, or up to 5% by weight.

67. 41. The method of any one of the preceding claims, wherein the water soluble polymer concentration in the provided aqueous treatment formulation is up to 10 wt%, or up to 8 wt%, or up to 6 wt%, or up to 5 wt%.

68. A method according to any one of claims 1 to 40 or claim 67, wherein the provided aqueous treatment formulation is an aqueous formulation according to any one of claims 61 to 67.

69. The surface of the dry treatment film and the surface of the dry treatment film on which the aqueous ink droplets are deposited have an average roughness R a and (ii) a thickness of the drying treatment layer, said dimensionless ratio being at least 0.5, at least 0.4, at least 0.3, at least 0.25, at least 0.2, at least 0.15, or at least 0.1, and optionally at least 0.02, or at least 0.03, or at least 0.04, or at least 0.05, or at least 0.06, or at least 0.07, or at least 0.

08.

70. a. an intermediate transfer member (ITM) comprising an endless flexible belt mounted on a plurality of guide rollers; b. an imaging station configured to form an ink image on a surface of the ITM, the first and second of the guide rollers being disposed upstream and downstream of the imaging station to define an upward stroke and a downward stroke through the imaging station; c. an impression station through which the downward stroke of the ITM passes, the impression station being disposed downstream of the imaging station and configured to transfer the ink image from the ITM surface to the substrate; d. a processing station disposed downstream of said impression station and upstream of said imaging station for forming a uniform thin layer of a liquid processing formulation on said ITM surface during a downward stroke of said ITM, i. a coater for coating the ITM with the liquid treatment formulation; and ii. a coating thickness control assembly for removing excess liquid so that only a desired uniform thin layer of the treatment formulation remains, the coating thickness control assembly including a rounded tip that opposes the ITM surface on the downward stroke; a processing station including A printing system including:

71. 71. The system of claim 70, wherein the rounded tip is the tip of a doctor blade.

72. 72. The system of claim 71, wherein the doctor blade is oriented perpendicular to the ITM surface.

73. A system as claimed in any one of claims 70 to 72, wherein the rounded tip is biased towards the ITM surface and / or the ITM surface is biased towards the rounded tip.

74. 74. The system of claim 73, wherein the rounded tip is urged toward the ITM surface and / or the ITM surface is urged toward the rounded tip by a backing roller having a soft outer surface.

Citation Information

Patent Citations

  • Liquid coating method, liquid coating apparatus, and image formation device

    JP2010005502A

  • Image recording method

    JP2013199114A

  • Intermediate transfer body manufacturing method and image recording method

    JP2014097615A

  • Treatment of the delamination layer

    JP2015517928A