Tri-functional long-chain branched polyolefin
The controlled formation of trifunctional long chain branches in olefin-based polymers using dienes and multi-site catalysts addresses the issue of excessive branching and reactor fouling, improving polymer stability and properties.
Patent Information
- Application Number
- JP2024125715
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-03-29
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2040-03-27
AI Technical Summary
Existing methods for controlling the amount of long chain branching in olefin-based polymers, such as polyethylene and polypropylene, often result in excessive branching leading to gelation and reactor fouling, making it difficult to achieve controlled levels of trifunctional long chain branches.
A process involving the use of dienes with specific structures, such as dimethyldivinylsilane, in polymerization reactors with catalysts having multiple active sites, allowing for the controlled formation of trifunctional long chain branches through concerted addition across proximal polymer chains, thereby avoiding reactor fouling and gel formation.
This method enables the production of polymers with controlled trifunctional long chain branches, enhancing mechanical and thermal properties while preventing reactor fouling and gel formation, resulting in stable polymerization processes.
Smart Images

Figure 2024156836000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application is a continuation of U.S. Provisional Patent Application No. 62 / 826,270, filed March 29, 2019. No. 4, the entire disclosure of which is incorporated herein by reference.
[0002] Embodiments of the present disclosure generally relate to a polymer composition having trifunctional long chain branching, and The present invention relates to a process by which the polymer compositions are synthesized. [Background technology]
[0003] Olefin polymers such as polyethylene are produced through a variety of catalytic systems. The selection of such a catalyst system for use in the polymerization process of the olefin-based polymer is dependent on such It is an important factor that contributes to the characteristics and properties of olefin-based polymers.
[0004] Polyethylene and polypropylene are manufactured for a wide variety of products. The ethylene and polypropylene polymerization process produces a variety of resins suitable for different applications. A wide variety of resulting polyethylene resins with different physical properties make The amount of long chain branching in the polyolefin can be varied in many ways to produce a The effect of branching on the properties of polyethylene depends on the length and amount of branching. Short branches mainly affect the mechanical and thermal properties. As the length of the branches increases, the branches can form layered crystals, which are mechanically and The thermal properties are decreased. Small amounts of long chain branching can significantly alter the processing properties of a polymer. Summary of the Invention [Problem to be solved by the invention]
[0005] To form long chain branches, the vinyl or terminal double bonds of the polymer chain are converted into new polymers. Reincorporation of vinyl terminated polymers and introduction of diene comonomers The insertion occurs when a vinyl group on one polymer strand is incorporated into a second polymer strand. In addition, long chain branching is induced via radicals. All three mechanisms It is difficult to control the amount of branching in the polymer. If branching begins, there will be too much branching, which will lead to gelling and reactor fouling. The reintegration mechanism does not generate many branches, and the branches are can only occur after a land has been generated, thereby further limiting the amount of branching that can occur. will be done.
[0006] An embodiment of the present disclosure is a polymerizable composition comprising the polymerization product of ethylene, at least one diene comonomer, and optionally at least one of C3 to C 14 Includes polymers that contain comonomers. The polymer occurs at a frequency of at least 0.03 per 1000 carbon atoms of the polymer Contains trifunctional long chain branches arising from dienes.
[0007] The diene has a structure according to formula (I). [ka]
[0008] In formula (I), X is CR, SiR, or GeR, and each R is independently C1~C 12 In some embodiments, in formula (I), X is -C(R)-, and each R is -H. In another embodiment, X in formula (I) is -Si(R)2-, where each R is C1 to C 12 It is an alkyl.
[0009] Various embodiments of the process may be carried out in a solution polymerization reactor, or in a slurry reactor or gas phase. Particle formation occurs in polymerization reactors such as reactors, and molecular or solid supported catalysts are delivered to the reaction medium. The reaction medium is reached or developed in the reactor system, which may be a batch, continuous or cell type. The reactor residence time distribution is similar to that of a non-backmixed reactor. Reactors may be narrow, such as backmixed reactors, and series and recycle reactors. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a graphical depiction of polymer molecular weight with the number of branched methines per 1000 carbons. [Figure 2A] FIG. 2A is a plot of molecular weight increase versus diene linkages. [Figure 2B] FIG. 2B is a plot of polydispersity versus diene linkages. [Diagram 3] FIG. 3 is a graphical depiction of the predicted dependence of molecular weight distribution (MWD) curves on trifunctional diene branching level. [Figure 4] FIG. 4 is a graphical depiction of the predicted dependence of relative peak molecular weight (MW) on trifunctional diene branching level. [Diagram 5] FIG. 5 is a graphical depiction of the MWD curve showing how the point of maximum slope is used to define the high MWD tail area metric. [Figure 6] FIG. 6 is a conventional (RI) GPC of dimethyldivinylsilane samples (Examples 1.C and 1.1-1.7) with increasing amounts of diene. [Figure 7]FIG. 7 is a global carbon NMR spectrum of dimethyldivinylsilane branched polyethylene (Example 12.1). [Figure 8] Figure 8 is the Si(Me)2 region of the carbon NMR spectrum of dimethyldivinylsilane branched polyethylene (Example 12.1). Trifunctional LCB carbon = 0.17 Me / 1000C and tetrafunctional LCB carbon = 0.12 Me / 1000C. [Figure 9] Figure 9 shows the methine region of the carbon NMR spectrum of dimethyldivinylsilane branched polyethylene (Example 12.1). Trifunctional LCB = 0.09CH / 1000C, tetrafunctional LCB = 0.16CH / 1000C. [Figure 10] FIG. 10. Conventional (RI) and absolute (LS) GPC of linear PE (Example 12.C) and dimethyldivinylsilane branched PE (Example 12.1). [Figure 11] FIG. 11 shows the extensional viscosity fixture (EVF) of dimethyldivinylsilane branched PE (Example 12.1). [Figure 12] FIG. 12 is a melt strength plot of dimethyldivinylsilane branched polyethylene (Example 12.1). [Figure 13] FIG. 13. DMS of dimethyldivinylsilane branched polyethylene (Example 12.1) at 190° C. [Figure 14A] FIG. 14A is a graph of absolute molecular weight distributions of comparative conventional branched polymer samples with varying amounts of diene. [Figure 14B] FIG. 14B is a graph of conventional molecular weight distributions of comparative conventional branched polymer samples with varying amounts of diene. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Processes for synthesizing polymers and polymers synthesized by the processes of the present disclosure Particular embodiments of the polymers are described herein. The process may be embodied in different forms and is limited to the specific embodiments described in this disclosure. It should be understood that this disclosure is not to be construed as being exhaustive or illustrative. This disclosure is provided so that it is comprehensive and complete, and will fully convey the scope of the subject matter to those skilled in the art.
[0012] definition The term "polymer" refers to any combination of monomers, whether of the same or different types. It refers to a polymeric compound prepared by polymerizing The generic term is usually used to refer to polymers prepared from only one type of monomer The term "homopolymer" refers to a polymer prepared from two or more different monomers. As used herein, the term "interpolymer" includes "copolymers." refers to a polymer prepared by polymerization of at least two different types of monomers. Therefore, the general term interpolymer includes copolymers and polymers with three or more units such as terpolymers. and polymers prepared from different types of monomers.
[0013] "Polyethylene" or "ethylene-based polymer" refers to a polymer made from ethylene monomers. 0 mol % of units. This refers to a polymer containing more than 0 mol % of polyethylene homopoly It includes mers or copolymers (meaning units derived from two or more comonomers). Common forms of polyethylene known in the art include low density polyethylene. (LDPE), Linear Low Density Polyethylene (LLDPE), Ultra Low Density Polyethylene (UL DPE), Very Low Density Polyethylene (VLDPE), Linear and Substantially Linear Low Density Resin containing single-site catalyzed linear low density polyethylene (m-LLDPE), Polyethylenes include polyethylene (MDPE), and high density polyethylene (HDPE). .
[0014] "Ethylene-diene polymer" means a polymer that contains more than 50 mol % of ethylene monomer. It means a polymer containing a small amount of diene. The polymer optionally comprises one or more (C 12 ) Units derived from α-olefins may include.
[0015] An embodiment of the present disclosure is a polymerizable composition comprising the polymerization product of ethylene, at least one diene comonomer, and optionally at least one of C3 to C 14 Includes polymers that contain comonomers. The polymer occurs at a frequency of at least 0.03 per 1000 carbon atoms of the polymer Contains trifunctional long chain branches arising from dienes.
[0016] The diene has a structure according to formula (I). [ka]
[0017] In formula (I), X is CR, SiR, or GeR, and each R is independently C1~C 12 In some embodiments, in formula (I), X is -C(R)-, and each R is -H. In another embodiment, X in formula (I) is -Si(R)2-, where each R is C1 to C 12 One or more embodiments In one embodiment, the diene is dimethyldivinylsilane.
[0018] In some embodiments, R of formula (I) is C1-C 12 If it is alkyl, C1 ~C 12Alkyl is methyl, ethyl, 1-propyl, 2-propyl, 1-butyl, 2- Butyl, 2-methylpropyl, 1,1-dimethylethyl, 1-pentyl, 1-hexyl, 1-heptyl, n-octyl, tert-octyl, nonyl, decyl, undecyl, or is dodecyl. C1~C 12 The term "alkyl" refers to a saturated alkyl group of 1 to 12 carbon atoms. "N" means a linear or branched hydrocarbon radical which is substituted with 1,2,3,4,5,6,7,8,9,10,11,12,13,14,15,16,17,18,19,19,20,21,22,23,
[0019] In various embodiments, the polymer has at least one trifunctional long chain branch per 1000 carbon atoms. In one or more embodiments, the trifunctional long chain of the polymer occurs with a frequency of at least 0.05. The branches occur at a frequency of at least 0.1 per 1000 carbon atoms. In this study, the trifunctional long chain branches of the polymer have a frequency of at least 0.2 per 1000 carbon atoms. This occurs at different degrees.
[0020] The polymers of the present disclosure are produced via a process for synthesizing long chain branched polymers. In one or more embodiments, the process includes one or more of C2 to C 14 Alkene monomers, at least A multi-chain catalyst in the presence of at least one diene, optionally a solvent, and optionally hydrogen. together, the multi-chain catalyst comprising a plurality of polymerization sites, the diene being represented by the formula: I) has a structure conforming to C2~C 14 At least two polymer chains of alkene monomers Each polymer chain is polymerized at one of the polymerization sites. Polymers are synthesized by linking two polymer chains with a diene. The linking or joining of chains is carried out in a concerted manner during polymerization. Long chain branching polymers are It has a ratio of trifunctional to tetrafunctional long chain branches of 5:1 to 100:0. In an embodiment, the ratio of trifunctional to tetrafunctional long chain branches is The ratio is adjusted if it deviates from the target ratio for chain branching. 14 Alkenes By varying the amount of monomer feed, the amount of hydrogen feed, or a combination thereof, The value is adjusted accordingly.
[0021] In various embodiments, the long chain branched polymer has a trifunctionality of 0.05:1 to 100:0. has a ratio of tetrafunctional long chain branches.
[0022] In one or more embodiments, the trifunctional long chain branches are produced from dienes and The branches occur at a frequency of at least 0.03 per 1000 carbon atoms.
[0023] The term "link" in the context of "connecting two polymer chains" is used in a broad sense to mean any polymer chain that is This means that the polymer chains are covalently bonded.
[0024] In one or more embodiments, the ratio of trifunctional to tetrafunctional long chain branches is The ratio is adjusted if the ratio deviates from the target ratio for tetrafunctional long chain branches of C2 ~C 14 Amount of alkene monomer feed, amount of hydrogen feed, C2 to C 14 Alkene Monomers by changing the ratio of feed to hydrogen, or a combination thereof. do.
[0025] In some embodiments, C2 to C 14 Molar Alkene Monomer Feed to Hydrogen The feed ratio is from 100:0 to 1:1. In one or more embodiments, the feed ratio is from 80: In various embodiments, the feed ratio is 70:1 to 30:1, 60:2 ~10:1, or 50:1 to 25.1.
[0026] Processes for synthesizing polymers according to the present disclosure are also disclosed in US Pat. No. PCTUS2019, filed on Oct. 23, 2019, which is incorporated by reference in its entirety. No. / 053524, No. PCTUS2019 / 053527, No. PCTUS2019 / 0 No. 53529 and PCTUS2019 / 053537 It is different from chain branching or the earlier "ladder" branching. The term "long chain branching" refers to "Branch" refers to a branch having more than 1 carbon atom in a polymer extending from a tertiary carbon atom. If a branch extends from a tertiary carbon atom, there are two other branches, may collectively be polymer strands from which branches extend. In the present disclosure, a branch is Defined as trifunctional long chain branching in that the point has three polymer chains emanating from it Conventionally, long chain branching (LCB) is achieved by polymerization processes, as shown in Scheme 1. Naturally occurring LCBs are the result of vinyl termination of the polymer chain and This can occur through vinyl reinsertion to create trifunctional long chain branches. Depending on the degree of branching, Various methods, such as nuclear magnetic resonance (NMR), determine the LCB or L For example, the effect of LCB can be distinguished from that of van Gurp-Palmen. It has been observed in the shear flow of the nucleation, and the increase in shear viscosity at low angular frequencies and the shear The strength of the thinning behavior can be attributed to the LCB. In extensional flow, the effect of the LCB is usually dominated by the strain hardening The degree or melt strength and maximum deformation achieved are distinguished by the degree of melt strength and the maximum deformation achieved. To ensure the formation of LCBs, a limited concentration of mers (maximum one per polymer chain) was used. High levels of natural LCBs in polymers due to the need to achieve high ethylene conversions for To ensure high conversion, the ethylene concentration in the reactor must be low. Therefore, large amounts of the vinyl terminated polymer can be reinserted into a second polymer chain. Scheme 1: Spontaneous long chain branching: Chain transfer events leading to vinyl terminated polymers [ka]
[0027] In Scheme 1, "Cat" is the catalyst and "P" is the polymer chain.
[0028] There is minimal long chain branching formed by naturally occurring branching. One approach to this, whether it is a radical, heterogeneous, or homogeneous process, is to This is due to the addition of α,ω-diene to the polymerization system. Generally, dienes are As shown in Fig. 1, they are added to the polymer chain in a manner similar to that of α-olefins, but they also This leaves pendant vinyl groups that can be inserted once to create an LCB. Generally, the diene length is It is not essential that the polymer chain be bonded together, only that it is possible to bond two polymer chains together. The concentration of pendant vinyl can be controlled by the amount of diene added to the reactor. Thus, the degree of LCB can be controlled by the concentration of the pendant vinyl. Scheme 2: Long-chain branching via diene incorporation [ka] In Scheme 2, "Cat" is the catalyst and "P" is the polymer chain. The diene is 1,5-hexadiene.
[0029] Conventional processes for incorporating dienes into polymer synthesis systems have been subject to the risk of gel formation or reactor fouling. The kinetic modeling discussed in a later section deals with gel formation in a fundamental way. For example, longer polymer chains can provide better prediction results that allow for a better understanding of , the more inserted olefins and therefore the more inserted dienes, but Thus, longer polymer chains with more pendant vinyl are reinserted into the catalyst. This means that the longer polymer chains are more likely to form LCBs. The tetrafunctional branch is then first reinserted to form a larger polymer molecule, which then fills the gap between the gel. As shown in Scheme 2, tetrafunctional LCBs are (the number of carbons between the two double bonds) and it consists of two long chains on either side of a short segment. The weight average molecular weight (M w ) and number average molecular weight (M n )of Simulations were performed for polyethylene in a constant pressure semi-batch reactor as shown in Figure 1. In Figure 1, M n is M w As goes to infinity, there is only a slight increase. w When the number increases to more than 200,000 grams per mole (g / mol), the polymer gel, Gelling occurs or there is reactor fouling.
[0030] The term "gel" or "gelation" refers to a solid that is composed of at least two components. The first refers to a three-dimensional cross-linked polymer, and the second refers to a medium in which the polymer is not completely soluble. If the polymer gels and does not dissolve completely, the reactor will become fouled with polymer gel. It is possible.
[0031] The term "ladder branching" polymer refers to a polymer formed from a "ladder branching mechanism." As shown in Scheme 2, the polymer has a tetrafunctional long chain branch structure. In addition, the terms "ladder branched" polymer and "ladder branching mechanism" refer to the It also refers to the polymerization process that produces polymers and trifunctional long chain branched polymers.
[0032] The process for synthesizing tetrafunctional long-chain branched polymers achieves long-chain branching and prevents gel formation or Without being bound by theory, it is believed that the reaction of two alkenes with a diene Reactor fouling is avoided by reacting in a concerted manner across two proximal polymer chains For example, as shown in Scheme 3, one alkene of a diene can be , reacts before the second alkene, which reacts because too many ethylene molecules are reacts before being added to the polymer strand, thereby providing a second alkene at the reactive site. Remove the adjacent ethylene monomers. to one polymer of an alkene, and to an adjacent polymer of a diene to a second polymer of an alkene. The reaction towards the proximal polymer chain is referred to as the concerted addition of the diene to the proximal polymer chain. Scheme 3: Incorporating dienes in a concerted fashion, also known as the tetrafunctional "ladder branching" mechanism. (P is the polymer chain). [ka]
[0033] Depending on the catalyst or diene, different intermediates can result from the diene reaction. showed the formation of tetrafunctional LCBs by addition of dienes to two-chain catalysts (Scheme 3). ), the formation of trifunctional long-chain branches is also possible (Scheme 4). Scheme 4: Depiction of trifunctional long-chain branch formation from the reaction of dienes. [ka]
[0034] A polymer strand is a linear segment of a polymer, or more specifically, a copolymer. The aryl groups are optionally joined at their termini by branched junctions. For example, This is in contrast to trifunctional branched junctions, which join the ends of three polymer strands, as shown in Alternatively, a tetrafunctional branched junction joins the ends of four polymer strands.
[0035] Without wishing to be bound by theory, it is believed that the mechanisms described in this section How does the double-stranded catalyst produce a unique trifunctional cross-linking molecule when the mer is polymerized under the desired conditions? The term "diene" refers to a compound that has two alkenes. The mechanism is illustrated in Scheme 5, where the catalyst The center produces two polyolefin chains. Scheme 5 shows the diene crosslinking and chain transfer. How does the combination create a diene "ladder-branched" trifunctional polymer structure? The term "ladder branched" polymers of dienes refers to long chain branching, which In a branch, a short chain or rung containing 1 to 12 carbon atoms links two polymer chains together. As shown, a metal-ligand catalyst having at least two polymer chain sites , growing two separate polymer chains. One alkene of the diene sits at one of the catalytic sites. Due to the proximity of the propagation sites, the second alkene of the diene is then incorporated into the second It is believed that they are rapidly incorporated into the polymer chain, thereby forming bridges or rungs. This sequential addition of dienes is called the "concerted" addition of dienes, which results in the formation of two proximal chains. The diene addition is distinct from the catalysts that do not have a vinyl-containing polymer that reacts later in the reactor. The term "lang" refers to the fact that once a diene is split into two separate polymers, Refers to a diene that, when incorporated into a strand, bonds the strands together The first and second polymer strands are formed by either transferring the polymer to another catalyst or The diene continues to grow until it is released from the catalyst, the catalyst dies, or another diene is added. continue. Scheme 5. Diagram of the trifunctional "ladder branching" mechanism including the resulting molecular structure. -Ligand catalyst, LM + It is expressed collectively as: [ka]
[0036] As shown in Scheme 5, trifunctional ladder branching can occur upon introduction of hydrogen gas. The introduction of hydrogen gas terminates the polymer chain at one of the polymerization sites of the multi-chain catalyst. Upon termination, the polymer chain is scission to produce a trifunctional polymer. The mer contains a trifunctional long chain branch arising from the diene of formula (I).
[0037] In one or more embodiments, the ratio of trifunctional to tetrafunctional branches is It is controlled through adjusting the propane / hydrogen ratio or other reactor conditions such as temperature. In some embodiments, the ratio of trifunctional to tetrafunctional long chain branches is from greater than 0.1:1 to about 1. The time is 00:0.
[0038] Without wishing to be bound by theory, the molecular weight distributions associated with these proposed kinetics However, it is essentially stable at high branching levels when diene crosslinking reactions are the only source of branching. The molecular weight distribution (MWD) is defined as the weight average molecular weight divided by the number average molecular weight. (M w / M n The inherent stability of MWD is dependent on the weight average molecular weight (M w ) but with high branching levels This means that the M w and M. w / M n However, the four senses are moderate. This is in contrast to conventional diene comonomer branching technology, where the potential branching levels are infinite.
[0039] The combination of multi-chain catalyst and diene affects the amount and type of branching. The illustrated embodiments are directed to polymer properties such as: 1) the use of multiple diene species; 2) multiple multi-chain polymers; 3) combinations of polymerization environments, including multiple reactor zones or zone gradients. or 4) different types of long chain branching, e.g., controlled and controlled tri- and tetrafunctional long chain branching. and combinations thereof.
[0040] Nevertheless, by using multiple catalysts, including single-chain catalysts, traditional branching The use of multiple diene species also creates no branching or "conventional" Also included are those dienes that tend to result in LCB. The process is different from conventional long-chain branching. The term "long-chain branching" refers to a process in which more than 100 carbon atoms are bonded together. The term "branched" refers to a polymer having a branch that extends from a tertiary carbon atom. If a branch extends from a tertiary carbon atom, two other branches are present and These can collectively be branched polymer chains. Long chain branching (LCB) is represented by the scheme This can occur naturally during the polymerization process, as shown in Figure 1. This can occur by termination and reinsertion of polymeric vinyl to create trifunctional long chain branches.
[0041] In one or more embodiments, the process for polymerizing the long chain branched polymer comprises This includes catalysts with at least two active sites (multi-chain catalysts). Distances of less than 1000 nm (Å), less than 6 Å, or about 5 Å are included.
[0042] Modern computational techniques allow for good comparison of known experimental structures as a method for estimating the distance between catalytic chains. It is well known that the method can be reproduced with high accuracy. or -Ge(R)-, where each R is independently hydrogen or a hydrocarbyl group; The diene structure according to formula (I) makes it possible to estimate the size of the diene. The end-to-end distance of the diene according to formula (I) where X is -Ge(R)2-, the diene is about 7 .5 Å. Therefore, the polymerization site for multiple chains is 8 Å or 2 Å for bimetallic catalysts. The two metals are within 8 Å.
[0043] In the case of heterogeneous systems, the surface concentration of the metal can be estimated, which is often on the order of nanometers. Metal atoms per square (M / nm 2 This surface coating is uniformly distributed. In the case of the accessible surface area, which can be converted to M-M distance, reflecting the distance between polymer chains, For extended surfaces, it provides an estimate of 1 metal / nm 2 is the 10 Å distance between metal atoms. At 8 Å, it gives 1.5 metals / nm 2 The coverage of can be determined.
[0044] Examples of catalysts having at least two active sites in close proximity include bimetallic transition metal catalysts, heterogeneous catalysts, dianionic activators with two related active catalysts, Ligation of growing polymer chains with transition metal catalysts, monoanionic groups, bidentate monoanionic groups anionic groups, tridentate monoanionic groups, or monodentate, bidentate, or tridentate monoanionic groups with external donors These include, but are not limited to, Group IV olefin polymerization catalysts containing non-anionic groups.
[0045] The catalysts in Table 1 are exemplary embodiments of the aforementioned catalyst classes and specific catalysts contemplated. The examples in Table 1 are not intended to be limiting, but rather They are merely illustrative and specific examples of the classes of catalysts mentioned above. [Table 1]
[0046] Without wishing to be bound by theory, it is believed that the mechanisms described in this section How does the double-stranded catalyst produce a unique trifunctional cross-linking molecule when the mer is polymerized under the desired conditions? The term "diene" refers to a compound that has two alkenes. The mechanism is illustrated in Scheme 5, where the catalyst The center produces two polyolefin chains. Scheme 5 shows the diene crosslinking and chain transfer. How does the combination create a diene "ladder-branched" trifunctional polymer structure? The term "ladder branched" polymers of dienes refers to long chain branching, which In a branch, a short chain or rung joins two polymer chains together. Metal-ligand catalysts having at least two polymer chain sites will form two separate polymer chains. The alkene of one of the dienes is incorporated into one of the catalytic sites and is adjacent to the propagation site. Due to the contact, the second alkene of the diene is then rapidly incorporated into the second polymer chain. It is believed that this succession of dienes forms bridges or rungs. Such addition is called a "concerted" diene addition and is distinct from catalysts that do not have two proximal chains. This results in the addition of dienes and the concentration of vinyl-containing polymers which react later in the reactor. The term "diene" refers to the fact that once the diene is incorporated into two separate polymer strands, , thereby referring to the diene that bonds the strands together. Strands form when the polymer migrates to another catalyst, when the polymer is released from the catalyst, or when the polymer is released from the catalyst. Growth continues until the catalyst dies or another diene is added.
[0047] In one or more embodiments, the polymers of the present disclosure contain at least 50 mole % ethylene. In this disclosure, "ethylene-based polymer" refers to an ethylene-based copolymer comprising ethylene. homopolymers, and / or ethylene and optionally one or more α-olefins, Refers to interpolymers (including copolymers) with comonomers, and is a monomer derived from ethylene. The unit may comprise at least 50 mole percent (mol%). All individual values and subranges encompassed by "from one cent" are considered as separate embodiments. Disclosed herein are, for example, ethylene-based polymers, homopolymers of ethylene and / or or an interpolymer of ethylene and optionally one or more comonomers such as α-olefins. The polymer (including copolymer) contains at least 60 mole percent ethylene-derived monomer units. at least 70 mole percent of monomer units derived from ethylene; At least 80 mole percent of monomer units and 50 to 100 mole percent of monomer units derived from ethylene 00 mole percent, or 80 to 100 mole percent of monomer units derived from ethylene may include.
[0048] kinetics A mathematical model has previously been derived for tetrafunctional "ladder" long chain branches, Each was filed on September 27, 2019, application number PCTUS2019 / 05352. No. 4, No. PCTUS2019 / 053527, No. PCTUS2019 / 053529 and PCTUS2019 / 053537, in which trifunctional A model is derived for "ladder branching" long chain branching. The mathematical model is The mathematics of the branching structures described in this disclosure are also used to establish the metrics and ranges of A mathematical model can be derived from the kinetic description of the proposed branching mechanism. Although some assumptions are made to promote simplicity, these assumptions are within the scope of this disclosure. The assumptions are not intended to be limiting in scope. The compounds are subject to the typical industrial uses, as well as additional assumptions specific to the hypothesized diene branching mechanism. The common assumptions made are: (1) propagation is much faster than chain transfer, and therefore the average chain length (2) only a single pure catalytic species is active. (3) the catalytic center makes many chains during its lifetime, and thus the lifetime of a chain is (4) Copolymerization is a process in which composition drift is minimal. In some cases, the polymerization can be approximated by a homopolymerization model.
[0049] Kinetics for the trifunctional "ladder branch" theory of dienes. Model derivation. The first step in deriving a model of the system is to express the kinetics in symbolic form. Describe and indicate the effect of each reaction on the molecular attributes of the target. It is standard practice to use an index to indicate the number of repeat units associated with a polymer chain. Furthermore, if the homopolymer rate constant is considered to be the effective complex copolymerization rate constant, The molecular structure of addition copolymers is accurately described by the kinetics and models of homopolymers. It is also recognized that it is possible to Olmer 1991,32(14),2641).
[0050] P n,m Dual-site catalysts in which the active catalytic center grows two polymer molecules The kinetics of a simple addition polymerization using The molecule on the right has m repeat units. The formation of tetrafunctional branches from diene bridges across the mer molecule was investigated. The following kinetics , a diene bridge across two growing molecules to form trifunctional (b3) branches or bifunctional bonds (b 2) Consider the diene bridge that is assumed to be created. The reaction is considered to be non-productive and is ignored in the kinetic scheme.
[0051] Kinetics of diene trifunctional and difunctional ladder branching theory. [Table 2]
[0052] The kinetics are described for each of the two polymer molecules growing on the catalyst, left and right. The result of growth is identified as the left side (P n+1,m ) or right side (P n,m+1 ) Regardless of the molecular size, the molecular size increases stepwise by one repeat unit. The chain is separated from the catalyst and the left (D n ) or Right (D m ) dead polymer molecules from either Additional simple chain transfer type reactions such as hydrogenation or beta hydride elimination can be Do not add complexity to the model.
[0053] k for diene crosslinking reaction d are written for each catalyst side, and each rate is the rate of A factor of 2 is used due to the two reactive groups. Both (two) sides are described, Since the diene (D) has two reactive groups, the diene crosslinking reaction k g 4 to that speed Thus, the diene consumption kinetics is calculated on a group basis rather than a molecular basis. The rate constant is defined in terms of
[0054] Reinitiation of polymer chains occurs very rapidly and relatively infrequently relative to growth. It is standard practice to assume that by assuming instantaneous restarts, the species P n,0 , P 0,m , and P 0,0is essentially excluded from consideration in the polymer population.
[0055] Population balance and rates. The kinetic scheme shows how each reaction affects the molecular structure. These can be rendered into a set of balanced equations that describe how In describing the balance, it is convenient to use an abbreviated nomenclature to represent the rate of each reaction. These velocity groups are defined below. The transfer terms, e.g., Ω=k tra A+k trh H2+ k b Only by expanding the definition of trh )oh and beta hydride desorption (k b ) other chain transfer reactions can be included.
[0056] The kinetic velocity group is Ω=k tra AΨ=k d DП=k g DΦ=k p It is defined as M.
[0057] Growth polymer (P n,m ) molecule and dead polymer molecule (D n ) discrete population The kinetic balance is calculated using the kinetics group defined above for n ≥ 1 and m ≥ 1 molecular systems. These balances are described below for the rate of change of molecular population versus size. Define and add an additional convection term if the balance applies to a particular reactor environment or type. It can be modified to include δ k The terms are used in these discrete balances so that the term k=0 Specifies that the element is included only if
[0058]
number
number
[0059] Other important population balances are on the left (L n ) and right side (R n ) growth point Distribution of Rimer subspecies and convolution distribution (V n ) can be derived from the above. The symmetry imposed in defining the scheme allows for the separation of left- and right-hand growing polymer subspecies. The fabrics are equal.
[0060]
number
number
[0061] ξ as the total active catalyst concentration 0,0 Using
number
[0062] The first step in rendering a usable model is to determine the speed of the relevant polymer variants. Degree
number
[0063] Method of moments for prediction of MWD mean Models describing the moments of the chain length distribution of polymer species are often based on kinetic theory. Moment-based models can be derived from population balances obtained from the , molecular weight averages and polydispersity indices, but generally bimodality, Smaller nuances in peak MW and MWD such as tailing are not discussed. The method of moments is used to estimate chain length distribution models for various polymer subspecies, such as: The bulk polymer moment (λ i ) reflects bulk polymer properties The solution of the bulk moment model is generally a function of the various living polymer moments. A solution is needed.
[0064] Living Polymer Moment:
number
[0065] Bulk Polymer MWD Moment:
number
[0066] Considering that the rate of change of the live species is assumed to be zero, the bulk moment The rate of change of the polymer is easily derived from the population balance of the dead polymer.
number
[0067] Any experienced polymer reaction engineer can determine from a set of population balances It would be expected that a moment model could be derived. The rates of change of moment (λ0, λ1, λ2) are given below, and the kinetic chain is After imposing the assumption that Φ>>Ω, Φ>>Ψ, and Φ>>П are long, the negligible terms are To be removed.
number
[0068] The evaluation of the rates of change of these bulk moments allows the determination of the bulk moment distributions of a number of living polymer subpopulations. These live polymer moments are due to the "steady state assumption". is an algebraic quantity given below. Higher bulk moments such as λ are predicted. If so, additional live moments are required.
number
[0069] Evaluation of moment velocities After algebraic simplification, the instantaneous number-averaged and weight-averaged chain lengths (DP n , DP w ) are provided below. Of course, the average molecular weight (M n , M w ) is the average chain It is equal to the length multiplied by the apparent monomer repeat unit weight (g / mol).
number
number
[0070] Branch Metric The model expression is the diene-free average linear kinetic chain length DP, which is equal to Φ / Ω. no The model is further simplified by several substitutions such as F, the fraction of ene conjugates b By expressing it in terms of a dimensionless instantaneous branching metric, This can be further simplified as: When the diene level is varied, F b is almost constant can be expected, but certainly varies with catalyst choice and probably with reaction conditions. Therefore, F as a metric b The use of is reasonable.
[0071] Fraction of bifunctional diene conjugates
number
[0072] Additional metrics are needed to describe the relative levels of divergence, and here we use two One preferred option is to use a diene bond to the original polymer molecule. R c The solution is to use R. c One advantage of this is that it is simply a diene bond. R is the scaling factor for the diene. k c The disadvantage of this is that the original kinetic chain length or concentration generally falls within a series containing zero diene branching levels. The problem is that the data are only directly available if they are measured.
[0073] Diene conjugations per original kinetic chain
number
[0074] Metric R n is the branch metric R kc is an alternative to R n is a diene-linked poly The ratio of the mer molecules was calculated using R to analyze the data.n The use of number average molecular weight G This is facilitated by the possibility of measuring chain length or concentration by PC measurements. Since the number of polymer molecules is affected by the junctions, R n is not simply proportional to the diene. Bifunctional Coupling (F b =0), the two metrics R kc and R n teeth, are identical.
[0075] Diene conjugations per polymer molecule
number
[0076] The average chain length and molecular weight are given below along with the polydispersity, and the diene-free polydispersity is given below. The dispersity index is 2 due to the simplicity and ideality assumptions of the kinetics.
number
number
number
[0077] F b , R kc , and R n Rendering as a function of physically meaningful parameters such as Once the model is analyzed, some simple conclusions can be drawn from it. The delta is the weight average chain length (DP w ) or molecular weight (M w ) but up to twice as much when dienes are incorporated Any bifunctional bond can only increase the DP n or M n Low It is expected to bring down the DP w or M w mitigates any increase in. 2 zero diene maybe Starting from the polydispersity, the polydispersity (Z p ) is a maximum of 4 and can be set to any This is mitigated by the appearance of arbitrary bifunctional bonds.
[0078] Figure 2 shows the relationship between the diene-grafted functionality (F) and the molecular weight and polydispersity of the polymer. b ) effect The model demonstrates that pure trifunctional diene bridges exert a restraining effect on molecular weight and polydispersity. It has a limited two-fold potential effect and R kc Incremental effect at higher diene levels such as >3 It is clearly shown that F b = 5% or 10% moderately bifunctional diene If the diene junction level is expected, experimental data indicate that the diene level and M w Even the positive correlation between It may not be possible to prove it.
[0079] Complete MWD curve model Sometimes it is possible to solve the population balance of the molecular weight distribution curve. A practical algebraic solution would be to use the space- or time-variable nature of the reaction rate, as is usually assumed in this case. Of particular interest is the bulk MWD moment The polymer distribution function D that was previously used to render the model equation for n Yes Similarly, the instantaneous bulk polymer chain length distribution, X n can be expressed as follows:
[0080] Instantaneous bulk chain length distribution:
number
[0081] The long chain assumption ensures that the distribution of all species (X n , D n , L n , V n etc.) into discrete functions The population of the steady-state polymer species can be treated as if it were a continuous function rather than a linear function. A ration balance is a function of a differential equation in a continuous variable n when the difference terms are replaced by their derivatives. For example, L n The steady-state population balance of The difference term L can be replaced by its derivative as shown n ~L n-1 Contains:
[0082]
number
[0083] Similar substitutions lead to the following set of ordinary differential equations (ODEs), Integrate to obtain the chain length distributions for various defined live subspecies distributions L(n) and V(n) The model is summarized below as an initial value problem, where the chain length distribution function is The lower bound of n=0 on the distribution function is chosen only for mathematical simplicity. Finally, if high molecular weight polymers are formed, this does not significantly affect the model predictions. stomach.
number
number
[0084] Analytical solutions exist for the continuous distribution functions L(n) and V(n), and these functions are used can be used to render a function of the continuous bulk polymer chain length distribution (X(n)). do.
number
[0085] The solution for X(n) is a bit complicated, but can be easily expressed as follows:
number
number
number
number
[0086] Alternative assignments of X(n) functional terms have been previously applied to instantaneous average chain length and molecular weight models. The branch metric (F b , R kc , R n ) can be rendered using the following X Item (n) is F b and R kc is written as a function of R kc =R n / (1- F b R n ) to obtain R n can be converted to use α=1+R kc +1 / 2F b R kc
number
number
number
[0087] The integral of X(n) can be used to express the number and weight average chain lengths as well as the polydispersity. can.
number
[0088] As expected, by integrating the distribution equation X(n), we obtain the average degree of polymerization and the average molecular weight The results are in exact agreement with the instantaneous moment model presented earlier. The model does not provide additional or contradictory predictions of MWD average and polydispersity. Using this full chain length distribution model, we can determine how the MWD nuances are affected by diene addition. In particular, the model can capture how diene incorporation rates are affected by The modality, steepness, and tail of the MWD as a function of the belt and embedded modes. It is possible to predict the
[0089] Limiting cases for the MWD model There are two limiting cases for the chain length distribution model. The trivial case is F b =1, This occurs when the polymer is completely linear and has the most probable MWD. The average chain length of the most probable MWD decreases with the diene bridge level, which is b =1 Therefore, it is completely bifunctional.
[0090] A more interesting limiting case is when there is no bifunctional bond (F b =0), and branch Trick R kc and R n Each diene bond is a trifunctional branch point. Therefore, a specific nomenclature for branched polymers can be used.
[0091] F b If =0, B n = branch points per polymer molecule = R kc =R n
[0092] F b If =0, B c = Branch points per linear segment = (1 + B n ) / B n
[0093] This pure trifunctional branch chain length distribution is B n and B. c is shown below.
number
number
[0094] By integrating the above distribution function, F b We can obtain the average MWD for =0, and use this as The number average molecular weight of this trifunctional branched system is determined by the number of polymer molecules in the system as the branching reaction proceeds. does not change with increasing diene incorporation.
number
number
number
[0095] Polydispersity (M w / M n The above relationship for the trifunctional branching level of Most surprising is that at high branching levels, The prediction is that the dispersion will plateau at 4. Naturally, this prediction is unreasonable. Ideal copolymerization and symmetric catalyst systems, whereas non-ideal ones lead to increased polydispersity. It is expected that this will happen.
[0096] The chain length distribution function can again be used to construct the predicted MWD curve. Functional branching (B c Or B n A series of simulated SEC tracks with varying levels of The independent variables in Figure 3 are plots that are universal and dependent on the starting molecular weight. The zero fraction in FIG. 3 is scaled by the linear molecular weight or chain length so that the The branched case is the well-known “most probable” MWD, which is a linear attachment carried out under ideal uniform conditions. Figure 4 shows a plot of the relative peak MW of the trifunctional diene branches. , MWD peak is 0.2 n <0.9 or 0.17 c Approximate range of <0.5 We demonstrate that the most sensitive branching level is at mid-branching levels within the nucleus.
[0097] Traditional branching model The purpose of this section is to characterize various conventional diene branched and random polymer couples. The comparison is between the "ladder branch" model and the "ladder branch" model. In contrast, we have realized the inherent instability of traditional diene branching and random polymer coupling. The molecular structure resulting from diene “ladder branching” is (a) a conventional diene continuous stirred tank process. (b) conventional diene semi-batch branching model; (c) poly What are the (a) polymer-CSTR coupling model, and (b) polymer-batch coupling model? different.
[0098] a) Conventional diene CSTR branching model, Ver Strate-1980 (G.V. r Strate, C. Cozewith, WW Graessley, J. App. Polym.Sci.1980,25,59), Guzman-2010(JDGu zman, DJ Arriola, T. Karjala, J. Gaubert, BW .S.Kolthammer,AIChE 2010,56,1325):
number
[0099] b) Traditional diene semi-batch branching model, Cozewith-1979 (C. Coz ewith,WWGraessley,G.Ver Strate,Chem.En g. Sci. 1979, 34, 245), and d) polymer batch coupling model , Cozewith-1979, Flory-1953(PJFlory,Prin ciples of Polymer Chemistry,Cornell Univ. ersity Press,1953), Tobita-1995(H. Tobita, J. Polym. Sci. B 1995, 33, 1191):
number
number
[0100] c) Polymer CSTR coupling model:
number
[0101] Characterization of trifunctional long-chain branched polyolefins. Depending on the degree of branching, various methods, such as nuclear magnetic resonance (NMR), can be used to determine the LCB. or one can distinguish the effect of LCB in the polymer. The effect of is observed in the shear flow of the van Gurp-Palmen analysis and also in the low The increase in shear viscosity at high angular frequencies and the strength of the shear thinning behavior can be attributed to the LCB. In extensional flow, the effect of LCB is usually determined by the degree of strain hardening or the strength of the melt and the Other plots, such as the Mark-Houwink plot, g', broadened molecular weight distribution (MWD), and g' vis The plot provides additional information about the LCB. Provides information on the limited concentration of vinyl terminated polymers (maximum one per polymer chain) and Due to the need to achieve high ethylene conversion to ensure the formation of LCB and It is difficult to achieve high levels of natural LCB in the mer. The ethylene concentration in the reactor is low, and therefore a large amount of vinyl-terminated polymer is produced in the second polymer. It may be reinserted into the mer strand.
[0102] The difference between trifunctional and tetrafunctional long chain branches is best distinguished by NMR analysis. The dienes allow for diagnostic measures of tri- and tetrafunctional long chain branching. Scheme 6 This mechanism shows the difference between the formation of trifunctional and tetrafunctional long chain branches. In this case, the branching ratio The rate can be controlled by the ratio of ethylene to hydrogen in the reactor. In this particular example Dimethyldivinylsilane has a diagnostic methyl group on the silicon atom and can be used to Trifunctional or tetrafunctional long chain branches can be determined (Scheme 6 and Figure 7). 9). The carbon on the silicon of the tetrafunctional branched polymer is The carbon atoms on the nucleus are shifted upfield relative to the carbon atoms on the nucleus (see Figure 8). This shows that it is possible to control the ratio of branching. Scheme 6: Depiction of trifunctional long-chain branch formation from the reaction of dienes. [ka]
[0103] In addition to hydrocracking, termination events such as β-hydride elimination also lead to trifunctional long-chain branches. In cases where β-hydride elimination is the key mechanism, e.g., the vinylene group in Scheme 7 There is unsaturation as shown. Scheme 7: Trifunctional long-chain branch formation from the reaction of dienes followed by β-hydride elimination Description of. [ka]
[0104] Conventional processes for incorporating dienes into polymer synthesis result in high branching levels leading to gel formation or The kinetic modeling discussed in the previous section suffers from the fundamental drawback of reactor fouling. It may provide good predictive results that allow for a better understanding of gel formation. For example, longer The polymer chain has proportionally more pendant vinyls, The polymer chains containing the aryl group are likely to be reinserted into the catalyst to form LCBs. Thus, larger polymer chains are preferentially reinserted to form even larger polymer molecules. If the LCB level reaches a threshold, gel problems or instability may occur. Weight average molecular weight (M) as a function of conventional tetrafunctional branching w ) and number average molecular weight Amount (M n ) was simulated in a constant pressure semi-batch reactor for the production of ethylene-based polymers. The above is shown in FIG. 1. In FIG. n is M w As goes to infinity, it increases slightly. In this example, M w But 200,000 grams per mole (g / mol) When the number increases beyond this, the molecular weight distribution (MWD) of the polymer becomes unstable and gel formation begins. MWD is the weight average molecular weight M w The number average molecular weight M n is defined as dividing by (M w / M n ).
[0105] A polymer gel, for purposes of this disclosure, is defined as a polymeric gel having a high branching level and / or a high molecular weight. A polymer gel is defined in the narrow sense as a polymer fraction that is phase-separated due to the These properties can be observed in the polymer or melt and affect optical clarity, as well as film and fiber performance. Polyethylene interpolymer gels tend to interfere with the properties of the polymers when exposed to hot xylene. The gel content can be measured by the degree of insolubility of the polymer. Gel content is often determined by the GPC polymer The percentage of the polymer gel formed is correlated with, and therefore can be extrapolated from, the recovery percentage of the polymer gel. If the reactor is subjected to excessive heat, they can accumulate in the reactor and cause fouling.
[0106] To describe the high molecular weight tailing effect when dienes are added to the polymerization, the following measures are used: The present application has been disclosed in detail in PCT Application No. PCTUS2012 / 010363 filed on September 27, 2019. No. 019 / 053524, No. PCTUS2019 / 053527, No. PCTUS201 (described in PCTUS Publication Nos. PCTUS2019 / 053529 and PCTUS2019 / 053537) Tetrafunctional "ladder branched" polymers do not exhibit this tailing effect. High MW polymers A series of metrics quantifying the amount of A HIGH , and A TAIL has been previously disclosed (see Figure 5). The terms "high molecular weight tail" or "high molecular weight tail" are used to describe the Depending on the catalyst / diene pairing and experimental conditions, , "ladder branch" system has some conventional branching, whereby the shape metric One might expect values to be higher than would be expected for a pure "ladder branch".
[0107] A HIGH Or A TAIL The value defined by increases as the conventional branching level increases. However, the "ladder branch" model (tetrafunctional or trifunctional ) for the high MW area metric (A HIGH Or A TAIL ) is the "ladder branch" level It is predicted that the impact of the most probable MWD is minimal. HIGH and A TAIL of The values are approximately 0.07 and 0.015, respectively. Linear polymers that do not form due to the non-ideal nature of the polymerization HIGH and A TAI L The exemplary data demonstrate that most probable MWD tends to have slightly higher values of A variety of highly branched "ladder" molecules with essentially no high MW tail beyond what would be expected. The high MW area metric also indicates a "branched" polymer when accompanied by some degree of conventional branching. It is also diagnostic of the slight levels of high MW tail formation that "double-branched" polymers can exhibit. Rick A TAIL A HIGH It is less affected by linear MWD non-idealities than However, theoretically, A HIGH and A TAIL Metrics are high MW tail formation are shown equivalently.
[0108] Trifunctional long chain branched polyolefin As shown in Scheme 4, the polymer generated from the "ladder branch" is Included in the disclosure.
[0109] In some embodiments, the polymers of the present disclosure have a molecular weight of 0.1 per 1000 carbon atoms. In some embodiments, the polymers of the present disclosure have a trifunctional long chain branching level of greater than 1. , greater than 0.2 per 1000 carbon atoms, greater than 0.3 per 1000 carbon atoms , more than 0.4 per 1000 carbon atoms or less than 0.5 per 1000 carbon atoms has a level of trifunctional long chain branching in excess of
[0110] In embodiments, the ethylene-based polymers of the present disclosure have a melting point of at least 10 at 190° C. Melt Viscosity Ratio or Rheology Ratio (V 0.1 / V 100 ), including V 0.1 is 0.1 radians is the viscosity of ethylene-based polymers at 190 °C at an angular frequency of 100 kV / sec, and V is the viscosity of 100 is 100 Viscosity of ethylene-based polymers at 190°C with angular frequency in radians / second. In embodiments, the melt viscosity ratio is at least 14, at least 20, at least 25, or In some embodiments, the melt viscosity ratio is greater than 50 and is at least 6. 0 or greater than 100. In some embodiments, the melt viscosity ratio is from 14 to 200. do.
[0111] "Rheology ratio" and "melt viscosity ratio" are V at 190°C. 0.1 / V 100 By Defined, V 0.1 is the angular frequency of 0.1 rad / sec for an ethylene polymer at 190°C. is the viscosity of 100 is the angular frequency of 100 rad / s for ethylene at 190°C. is the viscosity of the polymer.
[0112] In one or more embodiments, the ethylene-based polymers of the present disclosure have an average g' of less than 0.86. and the average g' is determined by gel permeation chromatography using a triple detector. In some embodiments, the ethylene-based polymers of the present disclosure have an intrinsic viscosity ratio of 0.5 The average g' is between 0.55 and 0.86. All individual The values and subranges are disclosed herein as separate embodiments, for example, ethylene-based polyolefins. The average g' for Rimer was 0.64-0.75, 0.58-0.79, or 0.65-0. In one or more embodiments, the average g' may range from 0.55 to 0.84, 0.83, or 0.85 to 0.86. .59 to .82, or .66 to .80.
[0113] In one or more embodiments, the melt viscosity ratio of the ethylene-based polymers of the present disclosure is 10 times, and the melt viscosity ratio (V 0.1 / V 100 ) is V 0.1 , 0.1 radians / Viscosity of ethylene-based polymers at 190 °C in angular frequency in seconds, and V 100 , 100 radia The elastic modulus is determined by the viscosity of an ethylene polymer at 190°C at an angular frequency of 1000 kcal / sec. m is [((tan(δ 0.1 )-tan(δ 100 ))*1000) / (0.1-10 0))] and tan(δ 0.1 ) is the tangent of the phase angle in 0.1 radians / second, tan(δ 100 ) is the tangent of the phase angle in 100 radians / second.
[0114] In one or more embodiments, the ethylene-based polymer has a viscosity of 19 s / radian or less. The elastic modulus at 0° C. may be m, where m is [((tan(δ 0.1 )-tan(δ 100 )) *1000) / (0.1-100)). In another embodiment, the ethylene-based polymer may have a modulus of elasticity m at 190° C. that is 4 sec / radian or less.
[0115] In various embodiments, the melt strength of the ethylene-based polymers of the present disclosure may be greater than 6 cN. (Rheotens device, 190°C, 2.4 mm / sec) 2 , from the die exit to the wheel 120mm to center, extrusion speed 38.2 seconds -1 , 30mm long, 2mm diameter, and inflow In some embodiments, the ethylene-based polymer melt is The strength may be greater than 10 cN.
[0116] In an embodiment, the ethylene-based polymer has an MWD area metric A TAIL Determined by may have a quantified molecular weight tail, TAIL is less than 0.04. All individual values and subranges encompassed within the above are hereby incorporated by reference as separate embodiments. For example, in some embodiments, the A of the ethylene-based polymer of the present disclosure TAIL is 0 as determined by gel permeation chromatography using a triple detector. Exceeds and is equal to or less than 0.03.
[0117] In one or more embodiments, the polymers of the present disclosure are characterized by gel permeation chromatography using a triple detector. A molecular weight average of less than 800,000 Daltons as determined by chromatography. Amount (M w In various embodiments, the polymer may be subjected to gel immersion using a triple detector. 400,000 Daltons or less, 200,000 Daltons or less, as determined by permeation chromatography ,000 Daltons or less, or 150,000 Daltons or less weight average molecular weight (M w )of It is possible.
[0118] In one or more embodiments, the polymers of the present disclosure are characterized by gel permeation chromatography using a triple detector. M less than or equal to 6, as determined by w / M n (Weight average molecular weight / number In various embodiments, the polymer may be analyzed by gel immersion using a triple detector. M less than 5, or less than 4, as determined by permeation chromatography. w / M n of In some embodiments, the MWD of the long chain branched polymer is from 1 to 3, and the other Embodiments include MWD from 1.5 to 2.5.
[0119] Each M w0 and M. p0 As previously discussed, diene was added to the reactor during polymerization. is not a polymer resin metric. Each subsequent addition of diene increases the metric M w or M p The amount of diene incorporated into the reactor produces a polymer resin from which the amount of the reaction can be determined. The addition of diene is therefore less than the other reactants in the reactor. The total amount of ethylene, ethylene, and solvent is not affected.
[0120] In various embodiments, the ethylene-based polymer has a gpcBR branching index from 0.1 to 3.0. All individual values and subranges within "0.10 to 3.00" are As disclosed herein in certain embodiments, for example, the ethylene-based polymer may have a molecular weight of 0.10 to 2 .00, 0.10-1.00, 0.15-0.65, 0.20-0.75, or 0.1 It may include a gpcBR branching index of 0 to 0.95.
[0121] The long chain branching polymerization process described in the preceding paragraphs is carried out by polymerization of olefins, mainly ethylene and propene. In some embodiments, a single type of olefin is used in the polymerization scheme. Only olefins or α-olefins are present with small amounts of incorporated diene comonomers. However, additional α-olefins can be added to the polymerization procedure to essentially create a homopolymer of the α-olefin. Additional α-olefin comonomers may be incorporated. Typically, the additional α-olefin comonomers are 20 carbons or less. For example, the α-olefin comonomers have 3 to 10 carbon atoms, or 3 Exemplary α-olefin comonomers include propylene and propylene copolymers. , 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene , 1-decene, 4-methyl-l-pentene, and ethylidenenorbornene. For example, but not limited to, the one or more α-olefin comonomers may be propylene. 1-butene, 1-hexene, and 1-octene, or alternatively from the group consisting of 1-butene, 1-hexene, and 1-octene. -hexene and 1-octene.
[0122] Long chain branched polymers, for example homopolymers of ethylene and / or ethylene and optionally Optionally, the interpolymers may be formed with one or more comonomers such as α-olefins (copolymers). The copolymer (including the copolymer) may contain at least 50 weight percent of units derived from ethylene. All individual values and subranges encompassed by "at least 50 weight percent" are expressly incorporated herein by reference. Disclosed herein as an embodiment are, for example, ethylene-based polymers, homopolymers of ethylene. Polymers, and / or ethylene and optionally one or more com pound(s) such as α-olefins. Interpolymers (including copolymers) with monomers are at least 60 weight percent Units derived from ethylene, at least 70 percent by weight of units derived from ethylene, At least 80 percent by weight of units derived from ethylene, or 50 to 100 percent by weight ethylene-derived units, or 80 to 100 percent by weight ethylene-derived units It may include units such as
[0123] In some embodiments of the ethylene-based polymer, the ethylene-based polymer comprises additional α- The amount of additional α-olefin in the ethylene-based polymer is 50 mole percent or less. In other embodiments, the amount of additional α-olefin is at least In a further embodiment, the additional α-olefin comprises 0.01 mol % to 25 mol % of the In some embodiments, the amount of is at least 0.1 mol % to 10 mol %. The α-olefin is 1-octene.
[0124] In some embodiments, the long chain branched polymer has at least 50 mole percent ethylenediaminetetraacetate. At least 90 mole percent of all individual units derived from ethylene. All values and subranges are included herein and disclosed herein as separate embodiments. For example, the ethylene-based polymer may contain at least 93 mole percent units derived from ethylene, At least 96 mole percent of units derived from ethylene, at least 97 mole percent Ethylene-derived units, or alternatively, 90 to 100 mole percent ethylene-derived units 90 to 99.5 mole percent of units derived from ethylene; 97 to 99.5 mole percent It may contain units derived from ethylene.
[0125] In some embodiments of the long chain branched polymer, the amount of additional α-olefin is 50% and other embodiments include at least 1 mole percent (mol %) to 20 mole %. In a further embodiment, the amount of additional α-olefin is at least 5 mol % to 10 mol %. In some embodiments, the additional α-olefin is 1-octene.
[0126] Any conventional polymerization process may be used to produce the long chain branched polymer. Conventional polymerization processes include one or more conventional reactors, e.g., loop reactors, isothermal reactors, , fluidized bed gas phase reactors, stirred tank reactors, batch reactors, etc., in parallel, in series, or in any combination thereof. Solution polymerization process, gas phase polymerization process, slurry phase polymerization process, etc., using any combination. processes, and any combination thereof.
[0127] In one embodiment, the ethylene-based polymer is produced in a dual reactor system, e.g., a single loop reactor system. can be produced via solution polymerization in which ethylene and optionally one or more α-olefins are The olefins are polymerized in the presence of the catalyst system described herein and, optionally, one or more cocatalysts. In another embodiment, the ethylene-based polymer is produced in a dual reactor system, e.g., a dual loop. In the reactor system, ethylene and optionally one or more The α-olefins are produced by the catalytic system and optionally one or more of the catalyst systems described herein. The catalyst systems described herein are optionally polymerized in the presence of one or more other catalysts. It can be used in combination with other catalysts in the first reactor or in the second reactor. In one embodiment, the ethylene-based polymer is produced in a dual reactor system, e.g., a dual loop reactor system. can be produced via solution polymerization in which ethylene and optionally one or more α-olefins are The olefins are polymerized in both reactors in the presence of the catalyst system described herein.
[0128] In another embodiment, the long chain branched polymers can be produced in a single reactor system, e.g., a single loop reactor system. can be produced via solution polymerization in which ethylene and optionally one or more α-olefins are The olefins are prepared by reacting a catalyst system as described herein with one or more of the optional cocatalysts described in the preceding paragraphs. In some embodiments, the long chain branching to produce a long chain branched polymer is carried out in the presence of The chain branching polymerization process comprises the step of reacting ethylene and at least one additional α- It involves polymerizing olefins.
[0129] The long chain branched polymer may further comprise one or more additives. Such additives include are antistatic agents, color enhancers, dyes, lubricants, pigments, primary antioxidants, secondary antioxidants, additives Processing aids, UV stabilizers, and combinations thereof. The ethylene-based polymer may contain any amount of additives. Based on the weight of the ethylene-based polymer and one or more additives, the total weight of such additives The amount of the ethylene-based polymer may be about 0 to about 10 percent. The ethylene-based polymer may further include a filler. The filler may include, but is not limited to, organic or inorganic fillers. Long chain branched polymers are not compatible with ethylene-based polymers and any additives or fillers. Fillings such as calcium carbonate, talc, or Mg(OH)2, based on total weight The ethylene-based polymer may contain from about 0 to about 20 weight percent of a polymerizing agent. The composition may be further blended with a polyether ether ester to form a blend.
[0130] In some embodiments, the long chain polymerization process for producing the long chain branched polymer comprises: In the presence of a catalyst having two polymer forming sites, ethylene and at least one additional Such a polymer having two polymer-forming sites may include polymerizing an α-olefin. Long chain branched polymers resulting from such catalyst systems are prepared according to ASTM D792, the entire contents of which are incorporated herein by reference. (incorporated herein), for example, 0.850 g / cm 3 ~0.960g / cm 3 , 0.880g / cm 3 ~0.920g / cm 3 , 0.880g / cm 3 ~0.910 g / cm 3 , or 0.880 g / cm 3 ~0.900g / cm 3 The density of the sintered body may be 0.01 to 0.01.
[0131] In another embodiment, the long chain branched polymer resulting from the long chain polymerization process has 5 to 100 Melt flow ratio (I 10 / I2), where the melt index I2 is ASTM D1 238, which is incorporated herein by reference in its entirety, Measured with a load of .16 kg, melt index I 10 According to ASTM D1238 The melt flow ratio is measured at 190° C. and a load of 10 kg. (I 10 / I2) is 5 to 50, in others the melt flow ratio is 5 to 25, in others In this case, the melt flow ratio is 5 to 9.
[0132] Gel Permeation Chromatography (GPC) (conventional GPC) The chromatography system was a Polymer equipped with an internal IR5 infrared detector (IR5). rChar GPC-IR (Valencia, Spain) High Temperature GPC Chromatograph , and Precision Detectors (now Agilent Tech A 4-axis laser detector coupled to a 2-angle laser light scattering (LS) detector model 2040 (Nologies) was used. For all absolute light scattering measurements, a 15 degree angle was measured. The autosampler oven compartment was set to 160 degrees Celsius and the column compartment was set to 160 degrees Celsius. The temperature was set at 150°C. The columns used were four Agilent "Mixed A" 3 The column was a 200 cm, 20 micron linear mixed bed column. Chromatography solvents used is 1,2,4-trichlorobenzene and 200 ppm of butylated hydroxytoluene. The solvent source was nitrogen sparged. The injection volume used was 2 The volume was 1.00 microliters and the flow rate was 1.0 milliliters / minute.
[0133] The calibration of the GPC column set has molecular weights ranging from 580 to 8,400,000. Run at least 20 narrow molecular weight distribution polystyrene standards and compare individual molecular weights. The standards were placed in six "cocktail" mixtures with at least 10 intervals between them. , purchased from Agilent Technologies. Over 1,000,000 The molecular weight is 0.025 grams in 50 milliliters of solvent and 1,000,000 Polystyrene standards at 0.05 g in 50 ml solvent for molecular weights less than 0 The polystyrene standards were dissolved at 80 degrees Celsius with gentle agitation for 30 minutes. The peak molecular weights of the polystyrene standards were converted to polyethylene molecular weights using Equation 48. (Williams and Ward, J. Polym. Sci., Pol Ym. Lett., 6, 621 (1968). M ポリエチレン =A×(M ポリスチレン ) B (48) where M is the molecular weight, A has a value of 0.4315, and B is equal to 1.0.
[0134] A polynomial between third and fifth order was used to fit each polyethylene equivalent calibration point. The A was calculated so that the NIST standard NBS1475 is obtained at 52,000 MW. is adjusted slightly (approximately 0.415 to 0.44) to account for column resolution and band broadening effects. Corrected.
[0135] The total plate count for the GPC column set was 100 mL of eicosane (50 mL of T CB and dissolved for 20 min with gentle stirring). The plate count (Equation 49) and symmetry (Equation 50) were calculated according to the following equations: Measurements were performed by injecting 200 microliters.
number
number
[0136] The samples were analyzed using PolymerChar's "Instrument Control" software. The samples were prepared in a semi-automated fashion using the software, with a target sample weight of 2 mg / ml and Poly Septa caps pre-sparged with nitrogen via the merChar high temperature autosampler Solvent (containing 200 ppm BHT) was added to the vial. The sample was shaken at "slow" speed. The mixture was dissolved at 160 degrees Celsius for 2 hours.
[0137] M n(GPC) , M w(GPC) , and M.z(GPC) The calculation is Polymer Char GPCOne™ software, based on each equally spaced data collection point (i). The IR chromatogram with the baseline subtracted and the narrow standard at point (i) from Equation 1. Using the polyethylene equivalent molecular weight obtained from the calibration curve, Po Internal IR5 detector (measurement channel) of the lymerChar GPC-IR chromatograph Based on the GPC results using
number
number
number
[0138] To monitor deviations over time, a PolymerChar GPC-IR system was used. A flow rate marker (decane) was introduced to each sample via a controlled micropump. The quantitative markers (FM) were used to narrow the decane peaks in the sample (RV (FM sample)). The peaks of each sample were matched to the decane peaks in the semi-calibrated (RV (FM calibrated)). The decane marker was then used to linearly calibrate the flow rate (flow rate (apparent)). Any change in the time of the peak is associated with a linear shift in flow rate (effective flow rate). To facilitate the highest accuracy of RV measurements of the flow marker peak, a minimum of A power fitting routine was used to fit the peaks in the flow marker concentration chromatogram to a quadratic Then use the first derivative of the quadratic equation to find the true peak position. After calibrating the system based on the peaks of the flow markers (against narrow standard calibrations), ) The effective flow rate is calculated as in Equation 7. The processing of the flow marker peaks is carried out using Polym This was done via the erChar GPCOne™ software. Positive means that the effective flow rate should be within + / - 2% of the apparent flow rate. Flow (effective) = Flow (apparent) * (RV (FM calibrated) / RV (FM sample)) (54 )
[0139] Triple detector GPC (TDGPC) (Absolute GPC) Chromatography system, run conditions, column set, column calibration, and conventional molecular The calculation and distribution of molecular weight moments are described in Gel Permeation Chromatography (GPC). The procedure was carried out according to the method described.
[0140] Multiplex detection for determining viscometer and light scattering detector offsets from the IR5 detector A systematic approach for determining the instrument offset is described by Balke, Mourey, et. al. Mourey and Balke,Chromatography Polym.Ch pt 12,(1992))(Balke,Thitiratsakul,Lew,Ch eung,Mourey,Chromatography Polym.Chpt 13 ,(1992)) which is based on the Polym Using erChar GPCOne™ software, a wide range of homopolymer and polyester Ethylene standard (M w / M n >3) triple detector log(MW and IV) results Optimize for narrow standard column calibration results from narrow standard calibration curve.
[0141] Absolute molecular weight data was obtained using PolymerChar GPCOne™ software. Using Zimm (Zimm, BH, J. Chem. Phys., 16, 109 9 (1948)) and Kratochvil (Kratochvil, P., Clas sical Light Scattering from Polymer Solu tions, Elsevier, Oxford, NY (1987) The overall injection concentration used in the molecular weight determination is: A suitable linear polyethylene homopolymer or polyethylene standard polymer of known weight average molecular weight is It is obtained from the mass detector area and mass detector constant, which are derived from one of the quasi-quantities. (G Molecular weights calculated using PCOne™ are based on the polyethylene standards set forth below. and a refractive index concentration coefficient, dn / Generally, the mass (determined using GPCOne™) The detector response (IR5) and light scattering constant are approximately 0.1% for molecules with molecular weights above 50,000 g / mol. Viscometer calibration (determined using GPCOne™) The standard is determined using a method described by the manufacturer or, alternatively, Materials (SRM) 1475a (available from the National Institute of Standards and Technology (NIST) This can be achieved using published values of suitable linear standards. The viscosity area (DV) and injected mass are related to the intrinsic viscosity (GPCOne ( The chromatographic concentration is calculated using the second Assume low enough to preclude dealing with viral coefficient effects (concentration effects on molecular weight) will be done.
[0142] Absolute weight average molecular weight (M w(Abs) ) is photochemically analyzed (using GPCOne™) The area integrated chromatogram of scattering (LS) (factored by the light scattering constant) was calculated using the mass constant and The molecular weight and specific molecular weight are calculated by dividing the area of the mass detector (IR5) by the mass recovered. The viscosity response is linearly extrapolated at the chromatographic end where the signal-to-noise is low (GP COne™). Each of the other moments, M n(Abs) and M. z (Abs) is calculated according to equations 55-56 as follows:
number
number
[0143] Dynamic Mechanical Spectroscopy (or Small Angle Oscillatory Shear) The complex viscosity (η*), elastic modulus (G', G''), tan delta, and phase angle (δ) are Dynamic oscillation frequency sweep test at 190°C in the frequency range of 0.1 to 100 rad / s The level of strain is determined by strain sweep testing at 100 rad / sec at 190°C. The test is performed using a TA Instruments A strain-controlled rheometer, ARES-G2, was used with stainless steel parallel plates of 25 mm diameter. Before the actual test, a sample with a thickness of 3.3 mm is drawn and then subjected to two steps. In the first step, the sample is melted for 2.5 min and squeezed to a gap of 3 mm. After a further 2.5 min immersion at 190°C, the sample is then cut into a 2 mm gap and trimmed. This method allows the system to reach thermal equilibrium. An additional 5 minute delay is built in to allow for the determination of the concentration of the ions in the sample. The test is performed under a nitrogen atmosphere.
[0144] gpcBR branching index by triple detector GPC (TDGPC) The gpcBR branching index can be determined by first calibrating the light scattering, viscosity, and concentration detectors mentioned above. The baseline was then determined from light scattering, viscometer, and concentration chromatograms. The refractive index chromatogram was then subtracted to show the presence of detectable polymer. The total integral of the low molecular weight retention volume range in the light scattering and viscometer chromatograms was confirmed. An integration window was then set to ensure that the linear polyethylene standard The Mark-Houwink constants for polyethylene and polystyrene were established using the constants Then, using the two values, we can obtain 2 for polyethylene molecular weight and polyethylene intrinsic viscosity as a function of elution volume Two linear reference conventional calibrations were constructed.
number
number
[0145] The gpcBR branching index is based on Yau, Wallace W., “Examples of Using 3D-GPC-TREF for Poly-olefin Chara cterization,”Macromol.Symp.,2007,257,29- 45, this index is a robust method for characterizing long chain branching. The conventional method used in determining g' and calculating branching frequencies is to use the entire detector area. Avoid the "slice-by-slice" TDGPC calculations that use the peak area The method was used to measure the sample bulk absolute weight average molecular weight (M w , abs) can be obtained using this method, which uses the light scattering detection required for traditional g' determination. Avoid the "slice-by-slice" ratio of the detector signal to the concentration detector signal. The intrinsic viscosity of the sample was also obtained independently using equation (63). The area calculation in this case was As the actual sample area, the baseline and integration are determined by the detector noise and the TDGPC settings. It provides greater accuracy because it is less sensitive to variations caused by the fractional limits. More importantly, the peak area calculation was not affected by the detector volume offset. Similarly, the intrinsic viscosity (IV) of the sample with high accuracy was calculated by the area method in equation (59): Got it.
number
[0146] In equation (59), DPi represents the differential pressure signal monitored directly from the online viscometer. To determine the gpcBR branching index, the light scattering elution area of the sample polymer was used. The molecular weight of the sample was determined. The viscosity detector elution area of the sample polymer was used to determine the intrinsic viscosity of the sample. (IV or [η]) was determined. First, the molecular weight and intrinsic viscosity as a function of elution volume were SRM1475a or equivalent, using conventional calibration ("cc") for both degrees The molecular weights and intrinsic viscosities of linear polyethylene standards such as those described above were determined.
number
number
[0147] All statistics with a "cc or conv" subscript are The elution volume of the compound is determined using the corresponding conventional calibration method described above, and the concentration (Ci). Values without a letter are measurements based on mass detector, LALLS, and viscometer area. .K PE The value of is iteratively adjusted until the linear reference sample has a gpcBR measurement of zero. For example, in this particular case, α and Log K for determining gpcBR The final values for polyethylene were 0.725 and -3.355, respectively, and for polystyrene were are 0.722 and -3.993, respectively. Using the procedure considered, Once the K and α values are determined.
[0148] The procedure was repeated using the previous branched sample. The final "cc" value was chosen as the best calibration value. Branched samples were analyzed using the approximate Mark-Houwink constants.
[0149] The interpretation of gpcBR is simple. For linear polymers, the LS and viscometers give The gpcBR is close to zero because the values measured are close to the traditional calibration standards. If -, the measured polymer molecular weight is calculated M w,cc higher than and calculated IV cc is higher than the measured polymer IV, especially at high levels of long chain branching, g The pcBR is greater than zero. In fact, the gpcBR value increases as a result of polymer branching. represents the fractional IV change due to the molecular size shrinkage effect of 0.5 or 2.0 gpcBR value at levels of 50% and 200%, respectively, for an equivalent weight of linear polymer molecules. In these particular cases, the traditional "g' index" The advantage of using gpcBR compared to branch frequency calculations is the higher accuracy of gpcBR. All parameters used in the gpcBR index determination were determined with good precision. and is adversely affected by the low TDGPC detector response at high molecular weights from the concentration detector. Errors in detector volume alignment also do not affect the accuracy of the gpcBR index determination.
[0150] NMR analysis Sample preparation. Raw polymer samples must be cleaned prior to NMR measurement of unsaturation and branching. The polymer contained residues of solvents and catalysts that had to be removed first. Dissolve in tetrachloroethane (TCE) at 5°C, then add 3-propanol (IPA) The polymer was precipitated using hexanes and cooled to room temperature. The polymer was isolated by centrifugation. This process of washing the polymer was repeated at least three times. Dry in a vacuum oven at 37°C.
[0151] Approximately 70 mg of the washed and dried polymer was placed in a 10 mm N The samples were placed in MR tubes. The samples were then cooled by bubbling house nitrogen through them for 15 min. The purged sample was then placed in an aluminum heating block at 125°C. .
[0152] For bifurcation analysis, a single pulse of the sample 13 C NMR spectra were obtained by 10 mm 13 600MHz Bruker Avan equipped with C / 1H DUL CryoProbe Acquired at 120 °C using a CE III HD spectrometer with 90 pulses and a total of 10 seconds. 1400-5000 scans were collected with relaxation delay (AQ+D1).
[0153] Tetrafunctional and For quantification of trifunctional long chain branches, a single pulse of the sample 13 1C NMR spectrum 600MHz Bruk equipped with a 0mm 13C / 1H DUL CryoProbe Acquired at 120 °C using an Avance III HD spectrometer for 90 pulses and 960-5000 scans were collected with a total relaxation delay (AQ+D1) of 12 seconds. In addition, the QA-RINEPT spectrum (J. Hou, Y. He, X. Qiu, Mac romolecules 2017,50,2407-2414) with a relaxation delay of 7 seconds The parameter QA-RINEPT is the total amount of methyl groups in QA-RINEPT. The ratio to carbon was chosen to match the single pulse data.
[0154] Data processing and assignment methods. All NMR data were Mnova for 0.5Hz line broadening for the NMR spectrum and 3Hz line broadening for the carbon spectrum. Proton data were referenced to the TCE solvent resonance at 5.99 ppm. The carbon spectrum was referenced to the polymer's predominant CH2 at 29.99 ppm.
[0155] Trifunctional LCB (-3.36 ppm) and tetrafunctional LCB silylmethyl (-4.0 A virtual assignment for the 100-nm peak at 6 ppm was obtained using the ACD 100 C NMR predictor and the observed covariances. These assignments were found to be in close agreement with the branched methine resonances (24 0.9ppm for tetrafunctional and 25.7ppm for trifunctional) and CH2 carbon to Y-branch silicon This was confirmed using a quantitative relationship between the alpha resonance (approximately 15.3 ppm).
[0156] Batch Reactor Polymerization Procedure The batch reactor polymerization reaction was carried out in a 2 L Parr™ batch reactor. The reactor is heated by an electric heating mantle and cooled by an internal coiled cooling coil containing cooling water. Both the reactor and the heating / cooling system were equipped with Camile™ TG Pro. The reactor is controlled and monitored by a process computer. At the bottom of the reactor, a It is fitted with a dump valve that transfers the contents to a stainless steel dump pot. Catalyst deactivation solution (typically 5 mL of Irgafos / Irganox / toluene mixture) Both the pot and the tank are purged with nitrogen and the dump pot is The mixture is vented to a 30 gallon blowdown tank. All solvents are passed through a solvent purification column to remove any impurities that may affect the polymerization. 1-Octene and Isopar E are separated in the first column, Q, which contains A2 alumina. The ethylene is passed through two columns, the second column containing A204 alumina and
number
number
[0157] The reactor is loaded with IsoparE solvent and / or 1-octene depending on the reactor load. The shot tank is loaded first, which may contain the Fill to the load set point using the attached lab scale. After adding the liquid feed, Heat the reactor to the polymerization temperature set point. If ethylene is used, maintain the reaction pressure set point. Ethylene is added to the reactor at a reaction temperature to produce the desired ethylene. The amount of ethylene added is The flow rate is monitored by a Micro Motion flow meter. In experiments, the standard conditions at 150°C were 13 g ethylene in 585 g IsoparE, 1 The standard conditions are 5g of 1-octene, 240 psi of hydrogen, and 150°C. 15g ethylene, 45g 1-octene, 200 psi hydrogen in IsoparE. do.
[0158] The procatalyst and activator are mixed with an appropriate amount of purified toluene to obtain a solution of the desired molar concentration. The procatalyst and activator are handled in an inert glove box and syringed to obtain The syringe is then filled with 5 mL of toluene and transferred under pressure into the catalyst shot tank. Rinse 3 times. Immediately after the catalyst is added, the run timer begins. If using ethylene , is added by Camile to maintain the reaction pressure set point in the reactor. The reaction was carried out for 10 minutes, then the agitator was stopped and the bottom dump valve was opened to allow the inside of the reactor to cool. Transfer the contents of the dump pot into a tray and place in the lab hood. The tray containing the remaining polymer is then placed in a vacuum oven where the solvent is allowed to evaporate overnight. The mixture is transferred to a tray and heated to 140° C. under vacuum to remove any remaining solvent. After the tube was cooled to ambient temperature, the polymer yield was measured to measure the efficiency, and the polymer were subjected to the Mar test. Example from a batch reactor [ka]
[0159] In Table 2, the polymer characteristics of the comparative linear polymer sample (1.C) are shown from the batch reactor. The polymerization reaction consisted of 585 g of ISOPAR-E™, 15 g of of octene and 240 psi hydrogen pressure (ΔH2) at a temperature of 150°C. 14 g of ethylene was loaded, and the pressure was adjusted to 0.3 μmol of catalyst 1, 0.36 μmol of cocatalyst Catalyzer A (Methyldi(tetradecyl)ammonium tetrakis(pentafluorophenyl)boron) The cells were maintained in the presence of 10 μM MMAO-3A at 100 μM RT. Benzenedimethyldivinylsilane was added. [Table 3] [Table 4]
[0160] Table 2 collects data for Comparative Example 1.C and other diene Examples 1.1-1.7. NMR data show both tri- and tetrafunctional LCBs, as well as an increase in the number of LCBs with dienes. and demonstrate increased levels of
[0161] FIG. 6 shows conventional molecular weight distributions for examples using different amounts of diene.
[0162] Batch Reactor Example 2 In Table 3, the polymer characteristics of the comparative linear polymer sample (2.C) are shown from the batch reactor. The polymerization reaction consisted of 585 g of ISOPAR-E™, 15 g of of octene and 240 psi hydrogen pressure (ΔH2) at a temperature of 150°C. 15 g of ethylene was loaded, and the pressure was adjusted to 0.3 μmol of catalyst 1, 0.36 μmol of cocatalyst Catalyzer A (Methyldi(tetradecyl)ammonium tetrakis(pentafluorophenyl)boron) The cells were maintained in the presence of 10 μM MMAO-3A at 100 μM RT. Benzenedimethyldivinylsilane was added. [Table 5] [Table 6]
[0163] Table 3 collects data for Comparative Example 2.C and Diene Example 2.1. NMR Data The ratio of trifunctional (0.15LCB / 10) was 1.4:1 (trifunctional:tetrafunctional LCB). Both tetrafunctional (0.10LCB / 1000C) and tetrafunctional (0.10LCB / 1000C) are demonstrated. The dynamic mechanical spectrum of branched Example 2.1 was measured and the results are recorded in Table 3. 0. The viscosity at 1 radian / sec was determined to be 609,361 Pa s and at 100 radians / sec The viscosity of the solution was measured to be 2,453 Pa s, with a rheological ratio (V 0.1 / V1 00 ) was provided.
[0164] Batch Reactor Example 3 In Table 4, the polymer characteristics of the comparative linear polymer sample (3.C) are shown from the batch reactor. The polymerization reaction consisted of 585 g of ISOPAR-E™, 15 g of of octene and 240 psi hydrogen pressure (ΔH2) at a temperature of 140°C. 10 g of ethylene was loaded, and the pressure was adjusted to 0.3 μmol of catalyst 1, 0.36 μmol of cocatalyst Catalyzer A (Methyldi(tetradecyl)ammonium tetrakis(pentafluorophenyl)boron) The cells were maintained in the presence of 10 μM MMAO-3A at 100 μM RT. Benzenedimethyldivinylsilane was added. [Table 7] [Table 8]
[0165] Table 4 collects data for Comparative Example 3.C and Diene Example 1.1. NMR Data The ratio of trifunctional (0.23LCB / 10) was 1.8:1 (trifunctional:tetrafunctional LCB). Both tetrafunctional (0.13LCB / 1000C) and tetrafunctional (0.13LCB / 1000C) are demonstrated.
[0166] The dynamic mechanical spectrum of the branched Example 3.1 was measured and the results are recorded in Table 4. The viscosity at .1 rad / s was determined to be 515,022 Pa s and at 100 rad / s The viscosity at 200°C was measured to be 2,140 Pa s, with a rheological ratio (V 0.1 / V 100 ) was provided.
[0167] Batch Reactor Example 4 In Table 5, the polymer characteristics of the comparative linear polymer sample (4.C) are shown from a batch reactor. The polymerization reaction consisted of 585 g of ISOPAR-E™, 15 g of of octene and 160 psi hydrogen pressure (ΔH2) at a temperature of 150°C. 15 g of ethylene was loaded, and the pressure was adjusted to 0.4 μmol of catalyst 1, 0.48 μmol of cocatalyst Catalyzer A (Methyldi(tetradecyl)ammonium tetrakis(pentafluorophenyl)boron) The cells were maintained in the presence of 10 μM MMAO-3A at 100 rpm for 1 h at 4 °C (Table 3). Dienedimethyldivinylsilane was added. [Table 9] [Table 10]
[0168] Table 5 collects data for Comparative Example 4.C and Diene Example 4.1. NMR Data The ratio of trifunctional (0.31 LCB / 1) was 1.03:1 (trifunctional:tetrafunctional LCB). Both tetrafunctional (0.30LCB / 1000C) and tetrafunctional (0.30LCB / 1000C) are demonstrated.
[0169] The dynamic mechanical spectrum of the branched Example 4.1 was measured and the results are recorded in Table 5. The viscosity at .1 rad / s was determined to be 867,379 Pa s and at 100 rad / s The viscosity at 2818 Pa s was measured, with a rheological ratio (V 0.1 / V 100 ) was provided.
[0170] Batch Reactor Example 5 In Table 6, the polymer characteristics of the comparative linear polymer sample (5.C) are shown from a batch reactor. The polymerization reaction consisted of 585 g of ISOPAR-E™, 15 g of of octene and 80 psi hydrogen pressure (ΔH2) at a temperature of 160°C. 15 g of ethylene was loaded, the pressure was adjusted to 0.4 μmol of catalyst 1, 0.48 μmol of cocatalyst A (methyldi(tetradecyl)ammonium tetrakis(pentafluorophenyl)borate The cells were maintained in the presence of 10 μM of dielate, and 10 μM of MMAO-3A. Dimethyldivinylsilane was added. [Table 11] [Table 12]
[0171] Table 6 collects data for Comparative Example 5.C and Diene Example 5.1. NMR Data The ratio of trifunctional LCBs was 0.8:1 (trifunctional:tetrafunctional LCBs) and trifunctional (0.25LCB / 10 Both tetrafunctional (0.30LCB / 1000C) and tetrafunctional (0.30LCB / 1000C) are demonstrated.
[0172] The dynamic mechanical spectrum of the branched Example 5.1 was measured and the results are recorded in Table 6. The viscosity at .1 rad / s was determined to be 813,746 Pa s and at 100 rad / s The viscosity at 2742 Pa s was measured, with a rheological ratio (V 0.1 / V 100 ) was provided.
[0173] Batch Reactor Example 6 In Table 7, the polymerization reaction of Example 6.1 was carried out using 585 g of ISOPAR-E™, At 15 g of octene and 240 psi hydrogen pressure (ΔH2), at a temperature of 150°C 13 g of ethylene was charged, and the pressure was adjusted to 0.3 μmol of catalyst 1, 0.36 μmol of catalyst 2, and Cocatalyst A (methyldi(tetradecyl)ammonium tetrakis(pentafluorophenyl) The mixture was maintained in the presence of 10 μmol of MMAO-3A, 10 μmol of dimethyl ether (DMSO), and 10 μmol of MMAO-3A. Dienedimethyldivinylsilane was added to the reaction mixture. The mixture was mixed with 600 g of ISOPAR-E™, zero octane, and 240 psi of hydrogen. The reaction took place at a temperature of 160°C under a pressure (ΔH2). 13 g of ethylene was charged and the pressure was , 0.4 μmol of catalyst 1, 0.48 μmol of cocatalyst A (methyldi(tetradecyl)ammonium 10 μmol of MMAO The mixture was maintained in the presence of -3A. Dienedimethyldivinylsilane was added as shown in the table. In Table 7, the polymerization reaction of Example 6.3 was carried out using 600 g of ISOPAR-E™, Zeolite, At 240 psi hydrogen pressure (ΔH2) and a temperature of 160°C, 13 g of ethylene was loaded, and the pressure was adjusted to 0.4 μmol of catalyst 2, 0.48 μmol of cocatalyst Catalyst A (Methyldi(tetradecyl)ammonium tetrakis(pentafluorophenyl) Borate) and 10 μmol of MMAO-3A. Dienedimethyldivinylsilane was added. [Table 13] [Table 14]
[0174] Table 7 collects data for diene Examples 6.1, 6.2, and 6.3. Example 6 6.2 and 6.3 show that different catalysts react with different amounts of trifunctional LCB and different ratios of trifunctional For example, under the same conditions, catalyst 1 ( Example 6.2) and Catalyst 2 (Example 6.3) were 0.26LCB / 1000C and 0. Trifunctional LCB levels of 07LCB / 1000C and trifunctional LCB levels of 2.2:1 and 0.4:1 The amount and trifunctionality of trifunctional LCBs were: The proportion of tetrafunctional LCBs is highly dependent on the catalyst.
[0175] Examples 6.1 and 6.2 show that polymerizations are carried out under comparable conditions, but The main difference is that Example 6.1 contains octene and Example 6.2 does not contain octene. The amount of trifunctional LCB and the ratio of trifunctional:tetrafunctional LCB were determined for the two runs. are very similar in
[0176] The dynamic mechanical spectrum of Example 6.1 was measured and the results are recorded in Table 7. The viscosity in Angstroms / second was determined to be 306,441 Pa s, and the viscosity at 100 radians / second was determined to be 306,441 Pa s. was measured at 1,754 Pa s, with a rheological ratio (V 0.1 / V 100 ) was provided.
[0177] Batch Reactor Example 7 In Table 8, the polymer characteristics of the comparative linear polymer sample (7.C) are shown from a batch reactor. The polymerization reaction consisted of 580 g of ISOPAR-E™, 20 g of of octene, and zero hydrogen, at a temperature of 160°C. 11 g of ethylene The pressure was adjusted to 0.7 μmol of catalyst 1, 0.84 μmol of cocatalyst A (methyldi(tetrahydrofuran) tetrakis(pentafluorophenyl)borate), and 10 The mixture was maintained in the presence of 1 μmol of MMAO-3A. The silane was added. [Table 15] [Table 16]
[0178] Table 8 collects data for Comparative Example 7.C and Diene Example 7.1. NMR Data demonstrated that in this example, where hydrogen is not present, trifunctionality is not present. CB is present (0.14LCB / 1000C) and the trifunctional:tetrafunctional ratio is zero. be.
[0179] The dynamic mechanical spectrum of Example 7.1 was measured and the results are recorded in Table 8. The viscosity in Angstroms / second was determined to be 475,848 Pa s, and the viscosity at 100 radians / second was determined to be 475,848 Pa s. was measured at 1,982 Pa s, with a rheological ratio (V 0.1 / V 100 ) was provided.
[0180] Batch Reactor Example 8 In Table 9, the polymer characteristics of the comparative linear polymer sample (8.C) are shown from a batch reactor. The polymerization reaction consisted of 580 g of ISOPAR-E™, 20 g of of octene and 28 psi hydrogen pressure (ΔH2) at a temperature of 160 °C. 13 g of ethylene was loaded, the pressure was adjusted to 0.7 μmol of catalyst 1, 0.84 μmol of cocatalyst A (methyldi(tetradecyl)ammonium tetrakis(pentafluorophenyl)borate The cells were maintained in the presence of 10 μM of dielate, and 10 μM of MMAO-3A. Dimethyldivinylsilane was added. [Table 17] [Table 18]
[0181] Table 9 collects data for Comparative Example 8.C and Diene Example 8.1. NMR Data The ratio of trifunctional LCBs was 0.8:1 (trifunctional:tetrafunctional LCBs) and trifunctional (0.09LCB / 10 Both tetrafunctional (0.11LCB / 1000C) and tetrafunctional (0.11LCB / 1000C) are demonstrated.
[0182] The dynamic mechanical spectrum of Example 8.1 was measured and the results are recorded in Table 9. The viscosity in Angstroms / second was determined to be 721,022 Pa s, and the viscosity at 100 radians / second was determined to be 721,022 Pa s. was measured to be 2,297 Pa s, with a rheological ratio (V 0.1 / V 100 ) was provided.
[0183] Batch Reactor Example 9 Table 10 shows the polymer characteristics of the comparative linear polymer sample (9.C) from a batch reactor. The polymerization reaction was carried out with 580 g of ISOPAR-E™, 20 g of octene and 46 psi of hydrogen pressure (ΔH2) at a temperature of 160°C. 13 g of ethylene was loaded, and the pressure was adjusted to 0.7 μmol of catalyst 1, 0.84 μmol of cocatalyst Catalyzer A (Methyldi(tetradecyl)ammonium tetrakis(pentafluorophenyl)boron) The cells were maintained in the presence of 10 μM MMAO-3A at 100 μM RT. Benzenedimethyldivinylsilane was added. [Table 19] [Table 20]
[0184] Table 10 collects data for Comparative Example 9.C and diene Example 9.1. NMR Data The LCBs were trifunctional (0.09 LCB / 1) in a ratio of 0.9:1 (trifunctional:tetrafunctional LCB). Both tetrafunctional (0.10LCB / 1000C) and tetrafunctional (0.10LCB / 1000C) are demonstrated.
[0185] The dynamic mechanical spectrum of Example 9.1 was measured and the results are recorded in Table 10. The viscosity at 100 radians / sec was determined to be 697,565 Pa s, and the viscosity at 100 radians / sec was determined to be 697,565 Pa s. The viscosity was measured to be 2,782 Pa s, with a rheological ratio (V 0.1 / V 100 ) was provided.
[0186] Batch Reactor Example 10 In Table 11, the polymer characteristics of the comparative linear polymer sample (10.C) are shown in the batch reactor. The polymerization reaction was carried out using 575 g of ISOPAR-E™, 2 Generated at 160°C with 5g of octene and 83 psi hydrogen pressure (ΔH2) 14 g of ethylene was loaded, and the pressure was adjusted to 0.6 μmol of catalyst 1, 0.72 μmol of cocatalyst Catalyst A (Methyldi(tetradecyl)ammonium tetrakis(pentafluorophenyl) Borate) and 10 μmol of MMAO-3A. Dienedimethyldivinylsilane was added. [Table 21] [Table 22]
[0187] Table 11 collects the data for Comparative Example 10.C and Diene Example 10.1. NMR Data are for trifunctional (0.07 LCB) in a ratio of 0.7:1 (trifunctional:tetrafunctional LCB). Both tetrafunctional (0.10LCB / 1000C) and tetrafunctional (0.10LCB / 1000C) are demonstrated.
[0188] The dynamic mechanical spectrum of Example 10.1 was measured and the results are recorded in Table 11. The viscosity at radians / sec was determined to be 240,894 Pa s, and at 100 radians / sec The viscosity was measured to be 1,642 Pa s, with a rheological ratio (V 0.1 / V 10 0) was provided.
[0189] Batch Reactor Example 11 In Table 12, the polymer characteristics of the comparative linear polymer sample (11.C) are shown for the batch reactor. The polymerization reaction was carried out using 575 g of ISOPAR-E™, 2 At 5 g of octene and 160 psi hydrogen pressure (ΔH2), the 14 g of ethylene was charged, and the pressure was adjusted to 0.4 μmol of catalyst 1, 0.48 μmol of Cocatalyst A (methyldi(tetradecyl)ammonium tetrakis(pentafluorophenyl) ) borate), and 10 μmol of MMAO-3A. As shown in Table Then, diendimethyldivinylsilane was added. [Table 23] [Table 24]
[0190] Table 12 collects the data for Comparative Example 11.C and diene Example 11.1. NMR Data are for a 1.5:1 (trifunctional:tetrafunctional LCB) ratio of trifunctional (0.09 LCB Both tetrafunctional (0.06LCB / 1000C) and tetrafunctional (0.06LCB / 1000C) are demonstrated.
[0191] The dynamic mechanical spectrum of Example 11.1 was measured and the results are recorded in Table 12. The viscosity at radians / sec was determined to be 203,979 Pa s, and at 100 radians / sec The viscosity was measured to be 1,523 Pa s, with a rheological ratio (V 0.1 / V 10 0) was provided.
[0192] The measured melt strength of the polymer of Example 11.1 was 18 cm at an elongation of 32 mm / sec. It was N.
[0193] Batch Reactor Example 12 In Table 13, the polymer characteristics of the comparative linear polymer sample (12.C) are shown for the batch reactor. The polymerization reaction was carried out using 570 g of ISOPAR-E™, 3 At 0 g of octene and 240 psi hydrogen pressure (ΔH2), the 20 g of ethylene was charged, and the pressure was adjusted to 0.3 μmol of catalyst 1, 0.36 μmol of Cocatalyst A (methyldi(tetradecyl)ammonium tetrakis(pentafluorophenyl) ) borate), and 10 μmol of MMAO-3A. As shown in Table Then, diendimethyldivinylsilane was added. [Table 25] [Table 26]
[0194] Table 13 collects the data for Comparative Example 12.C and Diene Example 12.1. NMR Data are for a 1.3:1 (trifunctional:tetrafunctional LCB) ratio of trifunctional (0.08 LCB Both tetrafunctional (0.06LCB / 1000C) and tetrafunctional (0.06LCB / 1000C) are demonstrated (Figure 7 ~See Figure 9).
[0195] The conventional and absolute molecular weights of Examples 12.C and 12.1 are plotted in FIG. to.
[0196] The extensional viscosity fixture (EVF) for Example 12.1 is shown in FIG.
[0197] The measured melt strength of the polymer of Example 12.1 was 19 cm at an elongation of 32 mm / sec. N (see Figure 12).
[0198] The dynamic mechanical spectrum of Example 12.1 was measured and the results are recorded in Table 13. The viscosity at radians / second was determined to be 395,948 Pa s, and at 100 radians / second The viscosity was measured to be 2,075 Pa s, with a rheological ratio (V 0.1 / V 10 0) was provided (see Figure 13).
[0199] Batch Reactor Example 13 In Table 14, the polymer characteristics of the comparative linear polymer sample (13.C) are shown for the batch reactor. The polymerization reaction was carried out using 585 g of ISOPAR-E™, 1 At 5 g of octene and 240 psi hydrogen pressure (ΔH2), the 11 g of ethylene was charged, and the pressure was adjusted to 0.4 μmol of catalyst 1, 0.48 μmol of Cocatalyst A (methyldi(tetradecyl)ammonium tetrakis(pentafluorophenyl) ) borate), and 10 μmol of MMAO-3A. As shown in Table Then, diendimethyldivinylsilane was added. [Table 27] [Table 28]
[0200] Table 14 collects the data for Comparative Example 13.C and Diene Example 13.1. NMR Data are for a 1.7:1 (trifunctional:tetrafunctional LCB) ratio of trifunctional (0.12 LCB Both tetrafunctional (0.07LCB / 1000C) and tetrafunctional (0.07LCB / 1000C) are demonstrated.
[0201] The dynamic mechanical spectrum of Example 13.1 was measured and the results are recorded in Table 14. The viscosity at radians / second was determined to be 53,390 Pa s, and the viscosity at 100 radians / second was The viscosity was measured to be 887 Pa s, with a rheological ratio (V 0.1 / V 100 ) proposed was offered.
[0202] The measured melt strength of the polymer of Example 13.1 was 10 cm at an elongation of 65 mm / sec. It was N.
[0203] Examples 7 (Table 8) to 13 (Table 14) show the results for given catalysts and equivalent conditions. The ratio of trifunctional to tetrafunctional LCBs is controlled to reduce the amount of hydrogen in the reactor to ethylene. It is shown that the ratio can be controlled and the mechanism in Scheme 6 can be supported.
[0204] Examples 7 (Table 8) to 13 (Table 14) show the ratio of trifunctional to tetrafunctional LCBs. As the rate increases, M w / M w0 It was shown that M w is a diene component is the weight average molecular weight of the sample, M w0 is the weight average molecular weight of the unbranched comparative sample The higher the ratio of trifunctional branches, the higher the M w The present specification includes a method for reducing the increase in The trifunctional kinetic model in, and the respective applications were filed on September 28, 2018 U.S. Provisional Patent Applications Nos. 62 / 738,606, 62 / 73,8612, and 62 / 738 ,621, and 62 / 738,633, Support Dell.
[0205] Guzman-2010 is a method for determining the mechanism of diene branching in a steady-state CSTR. The MWD and physical properties of the catalyst were demonstrated and analyzed. In a very well mixed one gallon reactor system, ethylene, 1-octene, and 1 ,9-Decadiene was copolymerized. The specific CG used by Guzman-2010 For the C catalyst, see U.S. Pat. No. 5,965,756 (Structure IX) and U.S. Pat. 553,917 (Example 3). The catalyst was designed to grow a single chain from the catalytic center. The data showed that the CSTR was operated at a pressure of 525 psig and a temperature of 155°C over a range of diene feed concentrations. The data were collected at steady state over a wide operating range. Various steady-state polymer samples collected contained measurable levels of gel or insoluble material. However, at the highest diene feed levels, some internal reaction occurred. Reactor fouling was observed and higher levels of diene feed resulted in gel formation or reactor MWD defects. It was expected to bring stability.
[0206] In Guzman-2010, a selected set of data was used to The reactor conditions were fixed throughout the series. The feed concentrations of 1-octene and 1-octene were set at 13.8 wt% and 3.6 wt%, respectively. The catalyst feed rate was adjusted to maintain a constant ethylene conversion of 79% throughout the series. The temperature was continuously adjusted to give a fixed polymer production rate of 2.2 kg / h. Polymer density, a measure of polymer composition, remained constant at about 0.922 g / cc.
[0207] According to the data from Guzman-2010, I2 and I 10 is reflected by As such, changes in the conventional diene branching level affect the average molecular weight and polydispersity as well as viscosity, etc. It was demonstrated how the branching of conventional dienes versus molecular weight affects properties. The effect of is presented for both absolute and conventional MWD measurement techniques. Absolute MWD measurements are the preferred method for branched polymers, but are not always available. Therefore, the Guzman-2010 was measured using conventional techniques using a refractive index detector. The results in Table 33 show that, by both measurement techniques, the diene feed As the weight average molecular weight (M w ) will increase substantially Demonstrate the following.
[0208] Although not reported in Guzman-2010, absolute GPC measurement techniques and conventional For the GPC measurement technique, the MWD curves are found in Figures 14A and 14B, respectively; The MWD curve data in Figure 14 shows the expected high molecular weight resulting from conventional diene branching. I M w This demonstrated that tail formation occurred. A significant increase in peak MW with increasing diene branching The lack of movement is also evident from the MWD curves.
[0209] The molecular weight distribution data in Figures 14A and 14B show that more diene monomers are present in the CST A simple metric that describes the evolution of the position and shape of the MWD curves as they are fed into R The data are based on the absolute MWD measurements of polymer samples from Guzman-2010 and These MWD metrics are presented for both conventional and absolute MWD measurements. The data shows that the 1,9-decadiene feed ranges from 0 to 923 ppm, resulting in a molecular weight of up to It was shown that the 87% increase in p The peak molecular weight change, as shown by Neither measure of quantity varied significantly, and the results were consistent with those for the "ladder branched" polymers. The shape factors are summarized in Table 34 (Guzman-2010) and Supply levels and M w As increases, G 79 / 29 and A TAIL Both values As increases, their shape factors do not coincide with "ladder branches".
[0210] No modifications to the described embodiments may be made without departing from the spirit and scope of the claimed subject matter. It will be apparent to those skilled in the art that various modifications can be made. The document provides that such modifications and variations are within the scope of the appended claims and their equivalents. It is intended to cover modifications and variations of the described embodiments to the extent that they fall within the scope of the present invention.
Claims
1. ethylene, at least one diene comonomer, and optionally at least one C 3 ~C 14 A polymer comprising the polymerization product of a comonomer, the diene has a structure according to formula (I): 【Chemistry 1】 In the formula, X is CR 2 , SiR 2 , or GeR 2 and each R is independently 1 ~ C 12 is hydrocarbyl or -H; said polymer having at least 0.03 per 1000 carbon atoms of said polymer The polymer comprises trifunctional long chain branches arising from said dienes which occur with frequency.
2. X in formula (I) is -C(R) 2 - and each R is -H. polymer.
3. In formula (I), X is -Si(R) 2 -, each R is C 1 ~C 12 Alkyl The polymer of claim 1 .
4. The polymer of claim 3 wherein the diene is dimethyldivinylsilane.
5. The polymer is an ethylene-based copolymer containing at least 50 mole percent ethylene. The polymer according to any one of claims 1 to 4.
6. The polymer has a molecular weight distribution (MWD) area metric, A TAIL Quantified by The molecular weight tail of the A TAIL However, gel permeation using a triple detector The method according to any one of claims 1 to 5, wherein the chromatographic determination is 0.04 or less. The polymer according to any one of claims 1 to 5.
7. The polymer has an average g' of 0.55 to 0.86, and the average g' is The intrinsic viscosity ratio is determined by gel permeation chromatography using a viscometer.
7. The polymer according to any one of 1 to 6.
8. The polymer has a melt viscosity ratio at 190° C. (V 0.1 / V 100 ), wherein V 0.1 The shear rate of said polyimide at 190° C. is 0.1 rad / sec. is the viscosity of 100 However, the shear rate of 100 rad / s was 190° C. The polymer according to any one of claims 1 to 7, wherein the viscosity of the polymer is a viscosity of the styrene-based polymer.
9. The melt viscosity ratio at 190 ° C. (V 0.1 / V 100 ) is at least 50, The polymer according to claim 8.
10. The trifunctional long chain branches occur at a frequency of at least 0.05 per 1000 carbon atoms. The polymer according to any one of claims 1 to 9.
11. The trifunctional long chain branches occur at a frequency of at least 0.1 per 1000 carbon atoms. The polymer according to any one of claims 1 to 10.
12. Any one of claims 1 to 11, wherein the polymer has a melt strength of more than 6 cN. The polymer according to claim 1.
13. The polymer was determined by gel permeation chromatography using a triple detector. When the polymer is polymerized, the weight average molecular weight (M) is 800,000 Daltons or less. w ) 13. The polymer according to any one of claims 1 to 12.
14. The polymer was determined by gel permeation chromatography using a triple detector. When the polymer is polymerized, the weight average molecular weight (M) is 400,000 Daltons or less. w ) 14. The polymer according to any one of claims 1 to 13.
15. The polymer was determined by gel permeation chromatography using a triple detector. When the polymer is polymerized, the weight average molecular weight (M) is 200,000 Daltons or less. w ) 15. The polymer according to any one of claims 1 to 14.
16. The polymer was determined by gel permeation chromatography using a triple detector. When the polymer is polymerized, the weight average molecular weight (M) is less than 150,000 Daltons. w ) 16. The polymer according to any one of claims 1 to 15.
17. The polymer was determined by gel permeation chromatography using a triple detector. When the polymer is used, the weight average molecular weight / number average molecular weight, M, is less than 4. w / M n Claims 1 to 5 17. The polymer according to any one of claims 16.
Citation Information
Patent Citations
Ethylenic polymer and its production
JP1996059723A
Polymers with long chain branches and their production
JP1998512600A
Olefin polymerization catalyst and polymerization method
JP2004501245A
Polyethylene resin composition and laminate comprising the same
JP2009293014A
Ethylene polymer and method of producing the same
JP2013124262A