Cold rolled steel sheet and method of manufacturing the same

A cold rolled steel sheet with tailored composition and microstructure, combined with a specialized manufacturing process, addresses the challenge of balancing strength and formability in automotive applications, achieving high tensile strength and elongation, and ensuring industrial applicability.

JP2024156942AInactive Publication Date: 2024-11-06ARCELORMITTAL SA
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2024131788
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2017-11-10
Filing Date
2024-08-08
Publication Date
2024-11-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing automotive steel sheets face challenges in balancing high strength, formability, and ease of molding while meeting the requirements for improved fuel efficiency and vehicle durability.

Method used

A cold rolled heat treated steel sheet with specific chemical composition and microstructure, including carbon, manganese, silicon, and controlled proportions of austenite, bainite, and martensite, combined with a manufacturing process involving continuous casting, hot rolling, and two-step annealing, to achieve ultimate tensile strength over 1100 MPa and total elongation over 14.0%, along with good weldability and paintability.

Benefits of technology

The solution provides a steel sheet with enhanced mechanical properties, achieving high strength and formability, suitable for automotive applications, while maintaining industrial compatibility and reducing material usage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024156942000001
    Figure 2024156942000001
  • Figure 2024156942000002
    Figure 2024156942000002
  • Figure 2024156942000003
    Figure 2024156942000003
Patent Text Reader

Abstract

To provide a cold rolled steel sheet with both an ultimate tensile strength greater than or equal to 1100 MPa and a total elongation greater than or equal to 14.0%, and a method of manufacturing the same.SOLUTION: A cold rolled heat treated steel sheet has a composition that comprises the following elements, expressed in percentage by weight, 0.1%≤carbon≤0.5%, 1%≤manganese≤3.4%, 0.5%≤silicon≤2.5%, 0.03%≤aluminum≤1.5%, 0%≤sulfur≤0.003%, 0.002%≤phosphorus≤0.02%, and 0%≤nitrogen≤0.01%, and can contain one or more specified optional elements, with the remainder composition being composed of iron and unavoidable impurities resulting from processing. The microstructure of the steel sheet comprises, in area fraction, 10 to 30% Residual Austenite, 50 to 85% Bainite, 1 to 20% Quenched Martensite, and less than 30% Tempered Martensite.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cold-rolled, heat-treated steel sheet suitable for use as an automotive steel sheet. [Background technology]

[0002] Automotive parts must meet two contradictory requirements: ease of formability and strength, but in recent years, due to considerations of the global environment, automobiles have also been given a third requirement: improved fuel efficiency. Therefore, automotive parts must be made of highly formable materials to meet the standards of ease of fit for complex automobile assemblies, while at the same time reducing vehicle weight and improving fuel efficiency while improving the strength of the vehicle's crashworthiness and durability.

[0003] Therefore, intensive research and development efforts are being made to reduce the amount of material used in automobiles by increasing the strength of the materials. Conversely, since increasing the strength of steel sheets reduces their formability, there is a demand for the development of materials that combine high strength and high formability.

[0004] Previous research and development in the field of high strength and highly formable steel plates has led to several methods for producing high strength and highly formable steel plates, some of which are listed here for the final evaluation of the present invention.

[0005] EP3144406 claims a high strength cold rolled steel sheet with excellent ductility, the steel sheet containing, by weight, 0.1% to 0.3% carbon (C), 0.1% to 2.0% silicon (Si), 0.005% to 1.5% aluminum (Al), 1.5% to 3.0% manganese (Mn), 0.04% or less phosphorus (P) (except 0%), 0.015% or less sulfur (S) (except 0%), 0.02% or less nitrogen (N) (except 0%). The balance is iron (Fe) and unavoidable impurities, the sum of silicon and aluminum (Si+Al) (wt%) is 1.0% or more, and the microstructure contains, in area fraction, 5% or less of polygonal ferrite having a minor axis to major axis ratio of 0.4 or more, 70% or less (excluding 0%) of acicular ferrite having a minor axis to major axis ratio of 0.4 or less, 25% or less (excluding 0%) of acicular retained austenite, and the balance is martensite. Furthermore, EP3144406 envisions a high strength steel having a tensile strength of 780 MPa or more.

[0006] EP3128023 describes a high-strength cold-rolled steel sheet having excellent elongation, hole expandability, delayed fracture resistance, and a high yield ratio, and a manufacturing method thereof. The high-strength cold-rolled steel sheet having a high yield ratio has a composition, in mass%, containing 0.13% to 0.25% C, 1.2% to 2.2% Si, 2.0% to 3.2% Mn, 0.08% or less P, 0.005% or less S, 0.01% to 0.08% Al, 0.008% or less N, 0.055% to 0.130% Ti, with the balance being Fe and unavoidable impurities. The steel plate has a microstructure containing 2% to 15% ferrite by volume having an average crystal grain size of 2 μm or less, 5 to 20% retained austenite by volume having an average crystal grain size of 0.3 to 2.0 μm, 10% or less (including 0%) martensite by volume having an average grain size of 2 μm or less, and the remainder being bainite and tempered martensite, where the average crystal grain size of the bainite and tempered martensite is 5 μm or less.

[0007] EP3009527 provides a high-strength cold-rolled steel sheet having excellent elongation, stretch flangeability, and a high yield ratio, and a manufacturing method thereof. The high-strength cold-rolled steel sheet has a certain composition and a certain microstructure. The composition contains, on a mass basis, 0.15% to 0.27% C, 0.8% to 2.4% Si, 2.3% to 3.5% Mn, 0.08% or less P, 0.005% or less S, 0.01% to 0.08% Al, and 0.010% or less N, with the balance being Fe and unavoidable impurities. The microstructure contains ferrite with an average grain size of 5 μm or less and a volume fraction of 3% to 20%, retained austenite with a volume fraction of 5% to 20%, and martensite with a volume fraction of 5% to 20%, with the balance being bainite and / or tempered martensite. The total number of retained austenite with a grain size of 2 μm or less, martensite with a grain size of 2 μm or less, or a mixture of these phases is 150 or more per 2,000 μm2 of the plate thickness cross section parallel to the rolling direction of the steel plate.

[0008] Another patent application WO2015 / 177615 also describes a double annealed steel sheet, the composition of which, in terms of the contents in weight percent, is 0.20%≦C≦0.40%, 0.8%≦Mn≦1.4%, 1.60%≦Si≦3.00%, 0.015%≦Nb≦0.150%, Al≦0.1%, Cr≦1.0%, S≦0.006%, P≦0.030%, Ti≦ 0.05%, V≦0.05%, B≦0.003%, N≦0.01%, the remainder of the composition being iron and inevitable impurities resulting from manufacturing, and the microstructure is, in terms of surface area, 10%-30% retained austenite, 30%-60% annealed martensite, 5%-30% bainite, 10%-30% hardened martensite, and less than 10% ferrite. Furthermore, WO2015 / 177615 assumes a strength of 980 MPa or more. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] European Patent No. 3144406 [Patent Document 2] European Patent No. 3128023 [Patent Document 3] European Patent No. 3009527 [Patent Document 4] International Publication No. 2015 / 177615 Summary of the Invention [Problem to be solved by the invention]

[0010] The object of the present invention is to - an ultimate tensile strength of at least 1100 MPa, preferably greater than 1180 MPa; - a total elongation of at least 14.0%, preferably more than 15%; The object of the present invention is to solve these problems by making available a cold rolled steel sheet having the above properties at the same time. [Means for solving the problem]

[0011] In a preferred embodiment, the steel sheet according to the invention may also exhibit a yield strength to tensile strength ratio of 0.65 or more.

[0012] Preferably, such steels are also weldable and paintable and well suited to forming, especially rolling.

[0013] Another object of the invention is also to make available a manufacturing process for these steel sheets that is robust to variations in manufacturing parameters, while being compatible with conventional industrial applications.

[0014] The above objects and other advantages of the present invention will become more apparent from the detailed description of preferred embodiments of the present invention taken in conjunction with the accompanying drawings.

[0015] The cold rolled, heat treated steel sheet of the present invention may be optionally coated with zinc or a zinc alloy, or aluminum or an aluminum alloy, to improve its corrosion resistance.

[0016] Carbon is present in steel at between 0.10% and 0.5%. Carbon is an element necessary for generating low-temperature transformation phases such as martensite to increase the strength of steel plates, and is also an element necessary for securing retained austenite, since it plays a central role in stabilizing austenite.

[0017] The manganese content of the steel of the present invention is between 1% and 3.4%. This element is of the gamma type. The purpose of adding manganese is to essentially obtain a structure containing austenite and to give strength to the steel. Manganese is an element that stabilizes the austenite to obtain retained austenite. Manganese has been found in amounts of at least about 1% by weight to provide strength and hardenability of the steel sheet as well as to stabilize the austenite. Therefore, in the presented invention, a higher percentage of manganese is preferred, such as 3.4%. However, a manganese content above 3.4% has adverse effects such as retarding the transformation of austenite to bainite during the isothermal hold of the bainite transformation. Furthermore, a manganese content above 3.4% reduces the weldability of the steel and therefore may not achieve the ductility goal. The preferred range of manganese is between 1.2% and 2.3%, and more preferably between 1.2% and 2.2%.

[0018] The silicon content of the steel of the invention is between 0.5% and 2.5%. Silicon is an element that retards the precipitation of carbides during overaging, so that the presence of silicon stabilizes the carbon-rich austenite at room temperature. Moreover, due to the low solubility of silicon in carbides, it effectively inhibits or retards the formation of carbides, thus promoting the formation of low-density carbides in the bainite structure that is sought to give the steel its essential characteristics according to the invention. However, a disproportionate content of silicon does not enhance the mentioned effects and causes problems such as hot rolling embrittlement. The concentration is therefore limited within the upper limit of 2.5%.

[0019] The content of aluminum in the present invention is 0.03-1.5%, since aluminum removes the oxygen present in the molten steel, preventing it from forming a gas phase and boiling during the solidification process. Aluminum also fixes the nitrogen in the steel to form aluminum nitride, reducing the size of the particles. If the aluminum content exceeds 1.5%, the Ac3 point will be higher, which will increase the energy input required for the production of the steel. When adding a high manganese content, an aluminum content between 1.0% and 1.5% can be used to offset the effect of manganese on the transformation point and the progression of austenite formation with temperature.

[0020] The chromium content of the steel of the present invention is between 0.05% and 1%. Chromium is an essential element that gives the steel strength and hardness, but if used in excess of 1%, it impairs the surface finish of the steel. Furthermore, at chromium contents below 1%, the carbide distribution pattern of the bainite structure becomes coarse, and therefore the carbide density of the bainite remains low.

[0021] The phosphorus content of the steel of the invention is between 0.002% and 0.02%. Phosphorus has a tendency to segregate or co-segregate with manganese, especially at grain boundaries, which reduces spot weldability and hot ductility. For these reasons, its content is limited to less than 0.02%, preferably less than 0.013%.

[0022] Sulfur is not an essential element, but may be contained in steel as an impurity, and from the viewpoint of the present invention, the sulfur content is preferably as small as possible, but is 0.003% or less from the viewpoint of production costs. Furthermore, if more sulfur is present in steel, sulfur will combine to form sulfides, especially with manganese and titanium, reducing the beneficial effects of manganese and titanium in the present invention, which may be detrimental to formability.

[0023] Niobium is present in the steel in an amount between 0.001% and 0.1% and is suitable for forming carbonitrides and imparting strength to the steel of the invention by precipitation hardening. Niobium also influences the size of the components of the microstructure through its precipitation as carbonitrides and by retarding recrystallization during the heating process. Thus, a finer microstructure is formed at the end of the temperature hold, as a result after the completion of the annealing which leads to hardening of the product. However, when the niobium content exceeds 0.1%, a saturation effect of its influence is observed, meaning that the addition of niobium does not increase the strength of the product and is not of economic interest.

[0024] Titanium is an optional element that may be added to the steel of the present invention between 0.001% and 0.1%. Like niobium, titanium also forms carbonitride precipitates and therefore plays a role in strengthening the steel. However, titanium also forms titanium nitrides that appear during solidification of the casting. The amount of titanium is limited to 0.1% to avoid coarse titanium nitrides that are detrimental to formability. If the titanium content is less than 0.001%, it does not have any effect on the steel of the present invention.

[0025] The steel of the present invention is added with calcium between 0.0001% and 0.005%. The steel of the present invention is added with calcium as an optional element, especially during inclusion treatment. Calcium contributes to the refining of the steel by trapping the harmful sulphur content in globular form and retarding the harmful effects of sulphur.

[0026] Molybdenum is an optional element constituting 0.001% to 0.5% of the steel of the present invention, and it plays an effective role in determining the hardenability and hardness, delaying the appearance of bainite and avoiding the precipitation of carbides in bainite, but since the addition of molybdenum excessively increases the cost of adding alloying elements, its content is limited to 0.5% for economic reasons.

[0027] Copper may be added as an optional element in amounts between 0.01% and 2% to increase the strength of the steel and improve its corrosion resistance. A minimum of 0.01% is required to achieve this effect. However, if the copper content exceeds 2%, the surface properties may deteriorate.

[0028] Nickel may be added as an optional element in amounts between 0.01% and 3% to increase the strength and toughness of the steel. A minimum of 0.01% is required to obtain this effect. However, if its content exceeds 3%, nickel causes a decrease in ductility.

[0029] Nitrogen is limited to 0.01% to avoid aging of the material, which is detrimental to the mechanical properties of the steel, and to minimize the precipitation of aluminum nitride during solidification.

[0030] Vanadium has the effect of increasing the strength of the steel by forming carbides or carbonitrides, and from an economical point of view, its upper limit is 0.1%. Other elements such as cerium, boron, magnesium or zirconium can be added individually or in combination up to the maximum content levels indicated in the following proportions: cerium ≦0.1%, boron ≦0.003%, magnesium ≦0.01% and zirconium ≦0.01%, and these elements make it possible to refine the grains during solidification.

[0031] The balance of the steel composition consists of iron and inevitable impurities resulting from processing.

[0032] The microstructure of the steel plate claimed in the present invention is composed of bainite, which constitutes 50% to 85% of the microstructure of the steel of the present invention in terms of area fraction. In the present invention, bainite is cumulatively composed of lath bainite and granular bainite, and the granular bainite has very low density carbides, and the low density carbides referred to here are those having a number of carbides per unit area of ​​100 μm 2It has a high dislocation density, meaning less than 100 carbides per lath, which gives the steel of the present invention high strength and elongation. Lath bainite is in the form of thin ferrite laths with austenite or carbides formed between the laths. The lath bainite of the steel of the present invention gives the steel good formability. It is advantageous to have 50% bainite to ensure a total elongation of 14% and preferably 15% or more.

[0033] The retained austenite content of the steel according to the invention is between 10% and 30% of the microstructure in area fraction. Retained austenite is known to have a higher solubility of carbon than bainite and therefore acts as an effective carbon trap, retarding the formation of carbides in bainite. The carbon percentage in the retained austenite according to the invention is preferably higher than 0.9% and preferably lower than 1.1%. The retained austenite of the steel according to the invention confers enhanced ductility.

[0034] Quenched martensite constitutes 1% to 20% of the microstructure by area fraction. Quenched martensite provides strength to the invention. Quenched martensite is formed during the final cooling of the second anneal. Although no minimum is required, more than 20% quenched martensite provides excessive strength but degrades other mechanical properties beyond acceptable limits.

[0035] Tempered martensite constitutes 0% to 30% of the microstructure by area. Martensite occurs when the steel is at Tc min ~Tc max Tempered martensite can be formed when the steel is cooled between 0.25 and 1.05° C. and tempered during the overaging hold. Tempered martensite provides ductility and strength to the present invention. More than 30% tempered martensite provides excessive strength but reduces elongation beyond acceptable limits. Additionally, tempered martensite reduces the hardness gap between soft phases such as retained austenite and hard phases such as hardened martensite.

[0036] In addition to the above microstructure, the steel sheet may have less than 5% by area, preferably less than 3% ferrite, and the microstructure is free of microstructural components such as pearlite or cementite without impairing the mechanical properties of the steel sheet.

[0037] The steel sheet according to the invention can be produced by any suitable method. A preferred method consists in providing a semi-finished casting of steel having a chemical composition according to the invention. Casting can be carried out in ingots or continuously in the form of thin slabs or thin strip, i.e. with thicknesses ranging from about 220 mm for slabs to up to several tens of millimeters for thin strip.

[0038] For example, slabs having the above chemical composition are produced by continuous casting, and the slabs are optionally soft-reduced directly during the continuous casting process to avoid central segregation and to keep the local carbon to nominal carbon ratio below 1.10. The slabs resulting from the continuous casting process can be used directly at high temperature after continuous casting, or they may first be cooled to room temperature and then reheated for hot rolling.

[0039] The temperature of the slab subjected to hot rolling should preferably be at least 1200°C and less than 1280°C. If the temperature of the slab is less than 1200°C, excessive load is applied to the rolling mill, and furthermore, the temperature of the steel is lowered to the ferrite transformation temperature during the finish rolling, so that the steel is rolled in a state in which the structure contains transformed ferrite. Therefore, the temperature of the slab is preferably high enough so that the hot rolling can be completed in the temperature range of Ac3 to Ac3 + 100°C, and the final rolling temperature exceeds Ac3. Reheating at temperatures above 1280°C is industrially expensive and should be avoided.

[0040] A final rolling temperature range between Ac3 and Ac3+100°C is preferred in order to have a structure favourable for recrystallization and rolling. It is necessary to carry out the final rolling pass at a temperature above Ac3, since below this temperature the rollability of the steel sheet is significantly reduced. The steel sheet thus obtained is then cooled at a cooling rate of more than 30°C / s to the coiling temperature, which must be less than 600°C. Preferably, the cooling rate is less than or equal to 200°C / s.

[0041] The hot rolled steel sheet is coiled at a coiling temperature below 600° C. to avoid ovalization of the hot rolled steel sheet, and preferably below 570° C. to avoid scale formation. A preferred range of coiling temperatures is between 350 and 570° C. The coiled hot rolled steel sheet is then cooled to room temperature before being subjected to an optional hot strip anneal.

[0042] The hot rolled steel sheet may be subjected to an optional descaling step to remove the scale formed during hot rolling. The hot rolled steel sheet may then be subjected to an optional hot strip annealing at a temperature between 400°C and 750°C for at least 12 hours and up to 96 hours, while the temperature is kept below 750°C to avoid partial hot rolled microstructural transformation and thus loss of microstructural homogeneity. An optional descaling step of this hot rolled steel sheet may then be carried out, such as pickling of such steel sheet. This hot rolled steel sheet is cold rolled with a thickness reduction between 35 and 90%. The cold rolled steel sheet obtained from the cold rolling step is then subjected to a two-step annealing to impart the microstructural and mechanical properties to the steel of the invention.

[0043] In the first annealing, the cold-rolled steel sheet is heated to a soaking temperature between Ac3 and Ac3+100°C at a heating rate of more than 3°C / s, and Ac3 of the steel is calculated according to the following formula: Ac3=901-262*C-29*Mn+31*Si-12*Cr-155*Nb+86*Al where the elemental contents are expressed as weight percent.

[0044] The steel sheet is then held at the soaking temperature for 10 to 500 seconds to fully recrystallize and transform to the strongly work-hardened initial austenite structure. The steel sheet is then cooled at a cooling rate of more than 20°C / s to below 500°C, preferably below 400°C. Furthermore, to ensure a single phase martensite structure, the cooling rate is preferably more than 30°C / s.

[0045] Next, the temperature of the cold-rolled steel sheet is brought to room temperature. The cold-rolled annealed steel sheet may be optionally tempered at a temperature between 120°C and 250°C.

[0046] The second anneal of the cold rolled annealed steel sheet is performed by heating the annealed cold rolled steel sheet to a soaking temperature range between Ac3 and Ac3+100°C at a heating rate of greater than 3°C / s for 10 to 500 seconds to ensure 100% transformation to an austenitic microstructure. Ac3 is calculated using the following formula: Ac3=901-262*C-29*Mn+31*Si-12*Cr-155*Nb+86*Al. The sheet is then cooled to Tc at a cooling rate of greater than 20°C / s for 1 to 10 seconds. min ~Tc max These temperatures are determined according to the formula proposed herein: -Tc max =565-601*(1-Exp(-0.868*C))-34*Mn-13*Si-10*Cr+13*Al-361*Nb -Tc min =565-601*(1-Exp(-1.736*C))-34*Mn-13*Si-10*Cr+13*Al-361*Nb where the element contents are expressed as weight percent.

[0047] The cold rolled annealed steel sheet is then brought to a temperature range of 350°C to 550°C and held for 5 to 500 seconds to ensure the formation of an adequate amount of bainite and temper the martensite to impart the steel of the present invention with the targeted mechanical properties. The cold rolled annealed steel sheet is then cooled to room temperature at a cooling rate of at least 1°C / sec to obtain a cold rolled heat treated steel sheet.

[0048] The cold rolled heat treated steel sheet may optionally be subjected to an additional heat treatment step to facilitate the coating process, said optional heat treatment step having no effect on the mechanical properties of the steel of the invention. The cold rolled steel sheet may then be optionally coated by any of the known industrial methods such as electrogalvanizing, JVD, PVD, hot dip galvanizing (GI / GA). The electrogalvanizing does not change or modify the mechanical properties or the microstructure of the claimed steel sheet. The electrogalvanizing may be performed by conventional industrial methods, e.g. electroplating. EXAMPLES

[0049] The following tests, examples, figurative illustrations and tables presented herein are to be considered as non-limiting in nature and for illustrative purposes only, illustrating advantageous features of the present invention.

[0050] The steel plates made with different steel compositions are summarized in Table 1, each produced according to the process parameters specified in Table 2. Table 3 summarizes the microstructures of the steel plates obtained during the tests, and Table 4 summarizes the evaluation results of the properties obtained.

[0051]

[0052] [Table 1]

[0053] Table 2 summarizes the annealing process parameters carried out on the steels of Table 1. Steel compositions I1 to I3 serve for the manufacture of steel sheets according to the invention. The table also specifies the compositions of reference steels designated in the table as R1 to R3. Table 2 also shows the Tc values ​​of the inventive and reference steels. min and Tc max A table of temperatures is also shown. min and Tc max is the following formula: -Tc max=565-601*(1-Exp(-0.868*C))-34*Mn-13*Si-10*Cr+13*Al-361*Nb -Tc min =565-601*(1-Exp(-1.736*C))-34*Mn-13*Si-10*Cr+13*Al-361*Nb It is calculated using

[0054] Furthermore, before the annealing treatment was performed on the steels of the invention and the reference steels, the steels were heated to temperatures between 1000°C and 1280°C, then subjected to hot rolling at a finishing temperature above 850°C and coiled at a temperature below 600°C. The hot rolled coils were then processed as claimed and then cold rolled to a thickness reduction between 30 and 95%. These cold rolled steel sheets were subjected to the heat treatments listed in Table 2 herein.

[0055] [Table 2]

[0056] Table 3 illustrates the results of tests carried out according to various microscopic standards, such as scanning electron microscopy, to determine the microstructural composition of both the steel of the invention and the reference steel.

[0057] The results are presented here.

[0058] [Table 3]

[0059] Table 4 illustrates the mechanical properties of both the steels of the invention and the reference steels. The tests of tensile strength, yield strength and total elongation are carried out according to the JIS Z2241 standard.

[0060] The results of the various mechanical tests carried out in accordance with the standard are tabulated below.

[0061]

Table 4

Claims

1. 2. A cold rolled heat treated steel sheet comprising the following elements expressed in weight percent: 0.1%≦Carbon≦0.5% 1%≦Manganese≦3.4% 0.5%≦Silicon≦2.5% 0.03%≦Aluminum≦1.5% 0%≦sulfur≦0.003% 0.002%≦Phosphorus≦0.02% 0%≦Nitrogen≦0.01% and any of the following elements: 0.05%≦Chromium≦1% 0.001%≦Molybdenum≦0.5% 0.001%≦Niobium≦0.1% 0.001%≦Titanium≦0.1% 0.01%≦Copper≦2% 0.01%≦Nickel≦3% 0.0001%≦Calcium≦0.005% 0%≦Vanadium≦0.1% 0%≦Boron≦0.003% 0%≦Cerium≦0.1% 0%≦Magnesium≦0.010% 0%≦Zirconium≦0.010% a residual composition consisting of iron and unavoidable impurities resulting from processing, and a microstructure of the steel sheet containing, in area fractions, 10 to 30% retained austenite, 50 to 85% bainite, 1 to 20% hardened martensite, and less than 30% tempered martensite.

2. 2. The cold rolled heat treated steel of claim 1, wherein said composition comprises 0.7% to 2.4% silicon.

3. 3. Cold rolled heat treated steel according to claim 1 or 2, wherein said composition comprises 0.03% to 0.9% aluminium.

4. 4. The cold rolled heat treated steel of claim 3, wherein the composition comprises 0.03% to 0.6% aluminum.

5. 5. Cold rolled heat treated steel according to any one of claims 1 to 4, wherein the composition comprises from 1.2% to 2.3% manganese.

6. A cold rolled heat treated steel according to any one of the preceding claims, wherein the composition comprises between 0.03% and 0.5% chromium.

7. The cold rolled heat treated steel according to any one of claims 1 to 6, wherein a cumulative amount of bainite and retained austenite is 70% or more.

8. The cold rolled heat treated steel according to any one of claims 1 to 7, wherein the cumulative amount of tempered martensite and quenched martensite is 20% or more, and the proportion of quenched martensite is more than 10%.

9. 9. The cold rolled heat treated steel according to any one of claims 1 to 8, wherein the steel sheet has an ultimate tensile strength of 1100 MPa and a total elongation of 14.0% or more.

10. 10. The cold rolled heat treated steel of claim 9, wherein the steel sheet has an ultimate tensile strength of 1100 MPa or more and a ratio of yield strength to ultimate tensile strength of 0.65 or more.

11. A method for producing a cold rolled heat treated steel sheet, comprising the following successive steps: - Providing a steel composition according to any one of claims 1 to 6, - reheating the semi-finished product to a temperature between 1200°C and 1280°C, - rolling said semi-finished product in the austenitic range so that the hot rolling finishing temperature is above Ac3 to obtain a hot rolled steel sheet; - cooling the steel sheet at a cooling rate of more than 30°C / s to a coiling temperature of less than 600°C and coiling the hot-rolled sheet; - cooling the hot rolled sheet to room temperature; - optionally subjecting the hot rolled steel sheet to a descaling process, Optionally, the hot-rolled steel sheet may be subjected to an annealing treatment at a temperature between 400° C. and 750° C., - optionally subjecting the hot rolled steel sheet to a descaling process, - cold rolling the hot rolled steel sheet with a reduction ratio of between 35% and 90% to obtain a cold rolled steel sheet; - then heating said cold rolled steel sheet at a rate of more than 3°C / s to a soaking temperature between Ac3 and Ac3+100°C and holding it for 10 to 500 seconds; - then cooling the steel plate at a rate of more than 20°C / s to a temperature of less than 500°C; - then cooling the annealed cold rolled steel sheet to room temperature; - optionally carrying out a tempering step of said annealed steel sheet between 120°C and 250°C, - then heating the annealed cold rolled steel sheet at a rate of more than 3°C / s to a soaking temperature between Ac3 and Ac3+100°C and holding it for 10 to 500 seconds; - The steel sheet is then heated to Tc at a rate of more than 20 ° C / sec. max ~Tc min and cooling to a temperature range between Tc max =565-601*(1-Exp(-0.868*C))-34*Mn-13*Si-10*Cr+13*Al-361*Nb Tc min =565-601*(1-Exp(-1.736*C))-34*Mn-13*Si-10*Cr+13*Al-361*Nb Step, - then subjecting said annealed cold rolled steel sheet to a holding temperature range between 350 ° C. and 550 ° C. for a time between 5 and 500 seconds, and then cooling said annealed cold rolled steel sheet to room temperature at a cooling rate of 1 ° C. / s to obtain a cold rolled heat treated steel sheet; - the cold rolled heat treated steel sheet may be optionally coated Manufacturing method.

12. 12. The method of claim 11, wherein the coiling temperature is less than 570°C.

13. The method according to claim 11 or 12, wherein the soaking temperature of the first or second anneal is between Ac3 and Ac3+50°C.

14. The method according to claims 11 to 13, wherein the cooling rate after the first or second anneal is greater than 30°C / s to a temperature below 500°C.

15. Use of a steel sheet according to any one of claims 1 to 10 or produced according to the method according to claims 11 to 14 for the manufacture of structural or safety parts of a vehicle.

16. A part obtainable according to claim 15 by flexible rolling of said steel sheet.

17. A vehicle comprising a part obtained according to any one of claims 11 to 16.

Citation Information

Patent Citations

  • High-strength steel sheet and process for production of the same

    JP2008038247A

  • High-strength steel plate and manufacturing method thereof

    JP2010090475A

  • High-strength cold-rolled steel sheet having elongation, stretch-flange formability and weldability

    JP2010285636A

  • High strength pressed member and method for producing the same

    JP2011184758A

  • High-strength steel sheet, and method of producing the same

    JP2013072101A