Catalyst used for organic hydride generation, production method for catalyst, and organic hydride production method using catalyst
The boron-doped catalyst addresses the limitations of conventional noble metal catalysts by enhancing hydrogenation activity, enabling efficient organic hydride production at lower pressures and temperatures, thus optimizing hydrogen storage and transport systems.
Patent Information
- Application Number
- JP2023071281
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-07
AI Technical Summary
Conventional catalysts for hydrogenation reactions using noble metals are expensive, difficult to control structurally, and challenging to produce in large quantities, necessitating improved hydrogenation activity for compact and efficient hydrogen storage and transport.
A catalyst is developed by adding boron to a metal having hydrogenation activity supported on a metal oxide, comprising platinum or rhodium on aluminum oxide, silicon oxide, or titanium oxide carriers, with a molar ratio of boron to metal between 0.5 to 2.0, enhancing hydrogenation activity through a spillover mechanism.
The boron-doped catalyst exhibits higher hydrogenation activity, allowing for efficient production of organic hydrides at lower pressures and temperatures, reducing equipment size and facilitating heat management, thus improving the efficiency and cost-effectiveness of hydrogen storage and transport.
Smart Images

Figure 2024157131000001
Abstract
Description
[Technical field]
[0001] The present invention relates to organic hydride technology, and more particularly to boron doped catalysts, methods for making the catalysts, and methods for producing organic hydrides using the catalysts. [Background technology]
[0002] Hydrogen energy technology has been attracting attention as one of the technologies to reduce the pollution and global warming caused by the consumption of fossil fuels, and the risk of radiation exposure caused by the use of nuclear energy. Hydrogen can be produced by electrolysis of water, so it can be said that there is an almost limitless supply of hydrogen on Earth. It is also a clean energy source that does not produce carbon dioxide after combustion.
[0003] To utilize hydrogen, it is necessary to store and transport hydrogen gas safely and efficiently. In recent years, the organic hydride method has attracted attention as a technology for storing and transporting hydrogen. Organic hydrides refer to saturated hydrocarbons such as cyclohexane, methylcyclohexane, and decalin, which are produced by adding hydrogen to unsaturated hydrocarbons, including aromatic compounds such as benzene, toluene, and naphthalene. In the organic hydride method, which uses organic hydrides to store and transport hydrogen, hydrogen is added to unsaturated hydrocarbons in the hydrogen production area to produce organic hydrides that are liquid at room temperature, and the organic hydrides are stored or transported in a liquid state, and the organic hydrides are separated into hydrogen and unsaturated hydrocarbons by a dehydrogenation reaction in the demand area. The separated hydrogen is used as an energy source in the demand area, and the unsaturated hydrocarbons are transported back to the hydrogen production area and used in the hydrogen addition reaction. In this way, the hydrogen addition reaction and dehydrogenation reaction of hydrocarbons are used to enable the safe and efficient storage and transportation of hydrogen gas.
[0004] Conventionally, in the hydrogenation reaction to produce organic hydrides, catalysts in which a precious metal such as platinum is supported on a carrier such as aluminum oxide have been used. However, catalysts using precious metals are expensive. In addition, the hydrogenation reaction is an exothermic reaction, and heat management (heat removal) is required. To facilitate heat management, the device for carrying out the hydrogenation reaction needs to be made compact. To make the device compact, it is essential to improve the hydrogenation reaction activity of the catalyst (hereinafter referred to as hydrogenation activity) so that organic hydrides can be produced efficiently with a small amount of catalyst.
[0005] Prior art has been proposed that aims to improve the hydrogenation activity of catalysts in hydrogenation reactions. Patent Document 1 (Japanese Patent No. 6099238) and Patent Document 2 (Japanese Patent No. 6734275) are technologies relating to catalysts having a structure that can improve hydrogenation activity. Patent Document 3 (Japanese Patent Publication No. 2006-130378) proposes a technology relating to a catalyst obtained by coating a catalyst material on a support using a sputtering method, and Patent Document 4 (Japanese Patent Publication No. 2018-103158) proposes a technology relating to a catalyst that uses layered hydroxide as a support that supports a catalytic metal. However, these catalysts have problems such as difficulty in controlling the structure, high manufacturing costs, and difficulty in mass production.
[0006] Regarding the technology related to the dehydrogenation reaction, the inventor of the present invention developed a new catalyst in which phosphorus was added to a catalyst in which rhodium was supported on aluminum oxide (Non-Patent Document 1). This catalyst showed a higher methylcyclohexane dehydrogenation activity than a rhodium catalyst. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 6099238 [Patent Document 2] Patent No. 6734275 [Patent Document 3] JP 2006-130378 A [Patent Document 4] JP 2018-103158 A [Non-patent literature]
[0008] [Non-Patent Document 1] Yasuharu Kanda and 3 others, "Synthesis and Utilization Processes of Organic Hydride and Ammonia" p.85-93, CMC Publishing, 2021 [Non-Patent Document 2] "Remarkable Enhancement in Hydrogenation Ability by Phosphidation of Ruthenium: Specific Surface Structure Having Unique Ru Ensemble", S. Furukawa et al., ACS Catalysis, 8 (2018), 8177-8181 [Non-Patent Document 3] "Efficient hydrogen storage in boron doped graphene decorated by transition metals - A first-principles study", S.Nachimuthu et al., Carbon, 73(2014), 132-140 [Non-Patent Document 4] "The double tuning effect of TiO2 on Pt catalyzed dehydrogenation of methylcyclohexane", X. Yang et al., Mol. Catal., 492(2020), 110971 Summary of the Invention [Problem to be solved by the invention]
[0009] An object of the present invention is to provide a catalyst that can be used in hydrogenation reactions, which has high hydrogenation activity even under low pressure conditions and can be produced relatively easily and at low cost, and a method for producing the same. Another object of the present invention is to provide a method for producing an organic hydride with high efficiency by using the above catalyst. [Means for solving the problem]
[0010] The inventors of the present invention discovered that by adding boron to a catalyst used in the production of organic hydrides (hydrogenation reaction), in which a metal active in a hydrogenation reaction is supported on a metal oxide, a catalyst having higher hydrogenation activity than conventional catalysts can be obtained, and thus completed the present invention.
[0011] One aspect of the present invention provides a catalyst for producing an organic hydride. The catalyst includes a metal having hydrogenation reaction activity, a carrier supporting the metal, and boron added to the metal. The molar ratio of boron to the metal is preferably 0.5 to 2.0. The metal having hydrogenation reaction activity is preferably a platinum group metal, more preferably platinum or rhodium, or both. The carrier supporting the metal is preferably a metal oxide, more preferably aluminum oxide, silicon oxide, titanium oxide, cerium oxide, or a combination thereof.
[0012] Another aspect of the present invention provides a method for producing a catalyst for producing an organic hydride. The method includes the steps of preparing a raw catalyst in which a metal is supported on a carrier, adding boron to the raw catalyst, and reducing the raw catalyst to which boron has been added. The step of adding boron to the raw catalyst preferably includes the steps of impregnating the raw catalyst with an organic solvent solution of a boron compound, and drying the raw catalyst impregnated with the organic solvent solution. The boron compound is preferably any one of triphenylborane, triethylborane, and sodium borohydride, or a combination thereof. The step of reducing the raw catalyst to which boron has been added preferably includes the step of reducing the raw catalyst at 650°C to 850°C under a hydrogen atmosphere.
[0013] Yet another aspect of the present invention provides a method for producing an organic hydride using a catalyst for producing an organic hydride. This method includes a step of reducing the catalyst for producing an organic hydride according to the present invention, a reaction step of contacting the reduced catalyst with a raw material containing an unsaturated hydrocarbon and hydrogen, and a separation step of separating the organic hydride from a product containing the organic hydride and hydrogen produced by the reaction step. In one embodiment, the unsaturated hydrocarbon used can be toluene, and the organic hydride produced can be methylcyclohexane. The step of reducing the catalyst preferably includes a step of reducing the catalyst at 150°C to 400°C under a hydrogen atmosphere. The reaction step is preferably performed at a reaction pressure of 0 MPaG to 10 MPaG, more preferably at a reaction pressure of 0 MPaG to 1 MPaG. Effect of the Invention
[0014] According to the present invention, by adding boron to a catalyst in which a metal having activity in hydrogenation reaction is supported on a metal oxide, a catalyst having higher hydrogenation activity than conventional catalysts can be obtained. By using the catalyst according to the present invention, organic hydrides can be produced more efficiently than with conventional catalysts, making it possible to make the hydrogenation reaction apparatus more compact and facilitating heat management in hydrogenation reactions in which heat removal is essential. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will be described in detail below.
[0016] <Catalyst> The catalyst according to the present invention includes a metal having activity in a hydrogenation reaction (hydrogenation activity), a carrier supporting the metal having hydrogenation activity, and boron added to the metal having hydrogenation activity. Conventionally, catalysts used in hydrogenation reactions to produce organic hydrides generally include metals having hydrogenation activity supported on a carrier. However, conventional catalysts do not have sufficient hydrogenation activity. In contrast, the catalyst according to the present invention has a higher hydrogenation activity than conventional catalysts due to the addition of boron, and can carry out the reaction with high efficiency.
[0017] The metal contained in the catalyst according to the present invention may be a platinum group metal, gold, or silver, which is a metal having hydrogenation activity. Among them, the platinum group metal is more preferable as the metal contained in the catalyst according to the present invention, since it has a higher hydrogenation activity, and platinum and rhodium are even more preferable. These metals may be used alone or in combination.
[0018] The carrier contained in the catalyst according to the present invention can be a material generally used in hydrogenation reactions, if necessary. As the carrier, it is preferable to use a metal oxide, and among the metal oxides, it is more preferable to use aluminum oxide, silicon oxide, titanium oxide and cerium oxide, and it is even more preferable to use aluminum oxide. These metal oxides can be used alone or in combination.
[0019] The shape of the support is not particularly limited, but may be in the form of porous particles, a porous membrane, or may be in the form of a honeycomb or monolith. In the case of a porous particle shape, the particle size of the support is typically, but not limited to, 5 μm to 500 mm. The support may be, but is not limited to, a carrier having a surface area of 1 m 2 / g~200m 2In the catalyst according to the present invention, the metal having hydrogenation activity is preferably supported on the carrier in the form of particles, but is not limited thereto, and may be supported on the carrier in the form of, for example, needles, rods, films, nets, etc.
[0020] The amount of metal supported in the catalyst is not limited, but is preferably 0.1% by mass to 50% by mass with respect to 100% by mass of the support. If the amount of metal supported is less than 0.1% by mass, the desired catalytic performance may not be obtained. If the amount of metal supported is more than 50% by mass, the cost becomes high.
[0021] The catalyst according to the present invention is characterized in that boron is added in addition to a metal having hydrogenation activity and a support. Boron is added to the metal having hydrogenation activity in the form of zero-valent boron. By adding boron, the catalyst according to the present invention can improve the activity of the hydrogenation reaction compared to conventional catalysts.
[0022] In the catalyst according to the present invention, the molar ratio of boron to metal is preferably 0.5 to 2.0, more preferably 0.8 to 1.2, and even more preferably about 1.0. If the molar ratio of boron to metal is lower than 0.5, the desired catalytic performance may not be obtained. If the molar ratio is higher than 2.0, the metal having hydrogenation activity may be covered with boron and not exposed.
[0023] The inventors have found from experiments described below that when the catalyst according to the present invention is used to produce saturated hydrocarbons (specifically, methylcyclohexane) by hydrogenation of unsaturated hydrocarbons (specifically, toluene) as raw materials, the conversion rate of the unsaturated hydrocarbons is equal to or higher than that when a conventional catalyst is used. In addition, when the CO adsorption amount (equivalent to the amount of exposed metal) of the catalyst used in this experiment was measured, it was found that the CO adsorption amount of the catalyst according to the present invention was smaller than that of the conventional catalyst. When the TOF of the catalyst was calculated using these results, it was found that the TOF of the catalyst according to the present invention was about 2.5 to about 3.4 times that of the conventional catalyst, indicating that the hydrogenation activity was high.
[0024] Here, TOF (Turnover frequency) is a value that indicates the amount of reactant that one active site (one metal atom) can process per unit time, and the higher this value, the more active the catalyst is in hydrogenation. TOF can be calculated using the following formula (1). TOF = (F × X / 100) / (W × U) (1) F = feed rate of unsaturated hydrocarbon (mol / h) X = Conversion rate (%) W=catalyst weight (g) U = CO adsorption amount (mol / g)
[0025] The inventors of the present invention speculate that the reason why the hydrogenation activity of the catalyst according to the present invention is higher than that of conventional catalysts by adding boron is as follows. First, the inventors measured the XPS (X-ray photoelectron spectroscopy) spectrum of the catalyst according to the present invention. As a result, it was found that negatively charged (δ-) metals and non-negatively charged metals are present in the catalyst according to the present invention. In addition, unsaturated hydrocarbons, which are raw materials for hydrogenation reactions, are electron-rich and therefore are not easily adsorbed by negatively charged metals. Here, Non-Patent Document 2 reports a catalyst in which phosphorus is added to a catalyst containing ruthenium, and this document states that ruthenium is charged to δ+, and electron-rich toluene is strongly adsorbed thereto, thereby obtaining a higher hydrogenation activity than conventional catalysts. If so, it is considered that the hydrogenation activity of the catalyst according to the present invention is improved by a mechanism different from that of Non-Patent Document 2.
[0026] The present inventors believe that the high hydrogenation activity of the catalyst according to the present invention is due to the fact that the addition of boron makes it easier for atomic hydrogen to move (spillover phenomenon). It is known that the addition of boron to transition metal-supported carbon reduces the activation energy of hydrogen atom movement (Non-Patent Document 3), and that negatively charged metals are more likely to generate spillover hydrogen (Non-Patent Document 4). Therefore, in the catalyst according to the present invention, in addition to unsaturated hydrocarbons being adsorbed and hydrogenated by non-negatively charged metals, the hydrogenation activity is thought to be high due to a dual-functional mechanism in which unsaturated hydrocarbons adsorbed by non-negatively charged metals are hydrogenated by spillover hydrogen generated by negatively charged metals. In general, hydrogen is adsorbed (in atomic form with the HH bond cleaved) to metal atoms that function as catalysts, and it is known that the dissociated and adsorbed hydrogen moves on the support depending on the conditions (catalyst metal, support, reaction temperature, etc.), and this hydrogen that moves on the support is called spillover hydrogen.
[0027] <Catalyst manufacturing method> Next, a method for producing a catalyst according to the present invention will be described. The method includes a step of preparing a raw catalyst in which a metal is supported on a carrier, and a step of adding boron to the raw catalyst. Below, a method for producing the catalyst using an impregnation method will be described, but the method for producing the catalyst is not limited to this, and for example, a coprecipitation method can also be used.
[0028] In the process of preparing a raw catalyst in which a metal is supported on a carrier, first, an aqueous solution of a starting material containing a metal having hydrogenation activity is prepared. As the starting material, a salt of a metal element having hydrogenation activity can be used. When the metal having hydrogenation activity is platinum, the starting material can be, but is not limited to, chloroplatinic acid, tetraammineplatinum chloride, diamminedinitroplatinum nitrate, etc. When the metal having hydrogenation activity is rhodium, the starting material can be, but is not limited to, rhodium chloride, rhodium nitrate, hexaamminerhodium chloride, etc. The same applies to other metals having hydrogenation activity. The aqueous solution of the starting material can be prepared by adding the above starting material to water and stirring.
[0029] Next, the support is impregnated with an aqueous solution of the starting material, and if necessary, allowed to stand. It is preferable to dry the support before impregnating with the aqueous solution. After evaporating the water from the impregnated material impregnated with the aqueous solution and drying it, if necessary, the starting material is decomposed by heat treatment to obtain a raw catalyst.
[0030] The method of evaporating the moisture is not particularly limited, and can be performed, for example, on a hot plate. The drying and heat treatment are preferably performed in an inert gas atmosphere to prevent oxidation. The drying temperature, drying time, and heat treatment temperature are not particularly limited.
[0031] In the step of adding boron to the raw catalyst, the raw catalyst prepared as described above is impregnated with an organic solvent solution containing elemental boron, and if necessary, allowed to stand. The solution containing elemental boron is not limited, but can be prepared by adding, for example, triphenylborane, triethylborane, sodium borohydride, or the like to an organic solvent such as toluene, n-octane, or ethanol. The catalyst according to the present invention is obtained by evaporating the water from the raw catalyst impregnated with the solution and drying it.
[0032] The method of evaporating the water is not limited, and can be performed, for example, on a hot plate. Drying is preferably performed under an inert gas atmosphere to prevent oxidation. The drying temperature and drying time are not particularly limited.
[0033] Next, the raw catalyst to which boron has been added is reduced. The reduction is preferably carried out in a hydrogen atmosphere at a temperature of 650°C to 850°C for a predetermined period of time. By reducing the raw catalyst to which boron has been added (also called a catalyst precursor) within the above temperature range, an active phase (boride) having high hydrogenation activity can be generated. If the reduction temperature is lower than 650°C, the boride is not generated well, and if the reduction temperature is higher than 850°C, sintering occurs, so neither is preferable.
[0034] <Method of generating organic hydrides> Next, a method for producing an organic hydride using the catalyst according to the present invention will be described. The production of an organic hydride can be carried out using an apparatus well known to those skilled in the art, for example, but not limited to, a flow-bed reactor, a fixed-bed reactor, etc. The method for producing an organic hydride includes a reaction step of contacting a raw material containing an unsaturated hydrocarbon and hydrogen with the catalyst according to the present invention, and a separation step of separating the organic hydride from a product containing the organic hydride and hydrogen produced by the reaction step.
[0035] Examples of the unsaturated hydrocarbons used as raw materials include, but are not limited to, benzene, toluene, and naphthalene. One or a combination of these can be used as the raw unsaturated hydrocarbons as necessary. These are petroleums of Class 4 hazardous materials, similar to gasoline, and can be used in existing infrastructure. Among these compounds, toluene is preferable as the raw unsaturated hydrocarbon from the viewpoints of being liquid at room temperature and pressure, being gaseous at reaction temperature, having a strong structure, having a stable benzene ring, and having little adverse effect on the environment and human body.
[0036] Examples of the organic hydride produced include, but are not limited to, cyclohexane, methylcyclohexane, and decalin. When toluene is used as a preferred unsaturated hydrocarbon, methylcyclohexane can be obtained as the organic hydride. Like toluene, methylcyclohexane also has the advantages of being a liquid at room temperature and pressure, being a gas at the reaction temperature, having a strong structure, having a stable benzene ring, and having little adverse effect on the environment and the human body.
[0037] The reaction formula for producing an organic hydride from a raw material containing an unsaturated hydrocarbon and hydrogen is represented, for example, by the following formula. C6H6+3H2→ C6H 12 (Benzene hydrogenation reaction) C7H8+3H2→ C7H 14 (Toluene hydrogenation reaction) C 10 H8+5H2→ C 10 H 18 (Naphthalene hydrogenation reaction)
[0038] In the reaction step, a raw material containing unsaturated hydrocarbons and hydrogen is supplied to the reactor. It is preferable to supply a raw material gas containing unsaturated hydrocarbons and hydrogen as a raw material to the reactor. In this case, the unsaturated hydrocarbons are preheated and mixed with hydrogen gas as a gas before being supplied to the reactor. The method of supplying the raw material to the reactor is not limited thereto. For example, the unsaturated hydrocarbons may be supplied to the reactor in a liquid or gaseous state and hydrogen gas may be added thereto, or hydrogen gas may be supplied to the reactor first and the unsaturated hydrocarbons in a liquid or gaseous state may be added thereto. In any case, it is sufficient that the reaction between the unsaturated hydrocarbons and hydrogen is carried out on the catalyst.
[0039] The reaction temperature in the reaction step is preferably 30°C to 500°C, more preferably 80°C to 250°C, and even more preferably 100°C to 200°C. If the reaction temperature is lower than 30°C, the raw material will liquefy, the reaction field will decrease, and the efficiency of the reaction will decrease. In addition, if the reaction temperature is low, there are problems such as the required reaction rate not being obtained and the product is difficult to separate from the catalyst surface. If the reaction temperature is higher than 500°C, in addition to inducing coking that causes catalyst deterioration, in equilibrium reactions, the equilibrium will shift in the direction of canceling the exothermic reaction (i.e., in the direction of the endothermic reaction) under high temperature conditions, so in the case of the hydrogenation reaction, which is an exothermic reaction, equilibrium will be disadvantageous under high temperature conditions, and the reaction rate will decrease.
[0040] The reaction pressure in the reaction step is preferably 0 MPaG to 10 MPaG, and more preferably 0 MPaG to 1 MPaG. If the reaction pressure is lower than 0 MPaG, the efficiency of the reaction decreases. If the reaction pressure is higher than 10 MPaG, the catalyst may deteriorate, and the durability of the device may decrease. In particular, if the catalyst according to the present invention is used, an efficient hydrogenation reaction can be promoted even at a low reaction pressure of 0 MPaG to 1 MPaG. The reason why the catalyst according to the present invention can increase the hydrogenation activity even at such a low pressure reaction is considered to be that the addition of boron makes the spillover phenomenon more likely to occur, as already explained.
[0041] The inventors of the present invention consider the following regarding the temperature and pressure in the reaction process using the catalyst according to the present invention. From the viewpoints of increasing the conversion rate of the reactants, reducing the energy supplied to the apparatus, and reducing the burden on components such as the reactor, it is preferable that the reaction step is carried out at as low a temperature and pressure as possible. Therefore, the catalyst according to the present invention, which has higher hydrogenation activity at lower temperatures and lower pressures than conventional catalysts, is extremely suitable for producing organic hydrides.
[0042] In order for the reaction to produce organic hydrides to proceed efficiently, it is preferable that the temperature of the reaction step is (1) equal to or higher than the boiling points of the reactants (i.e., unsaturated hydrocarbons) and products (organic hydrides) and lower than (2). Regarding (1), in order to increase the number of reaction sites by diffusing the reactants and products throughout the reactor, the reactants and products need to be gaseous, and for this reason, it is important that the temperature of the reaction step is higher than the boiling points of the reactants and products. Regarding (2), when the temperature of the reaction step increases, the equilibrium shifts from the hydrogenation reaction to the dehydrogenation reaction, so by carrying out the reaction at a lower temperature, a high conversion rate of the reactants can be obtained, and the energy consumed during the reaction can be reduced, reducing the burden on the components.
[0043] Taking toluene as an example of a reactant, the boiling point of toluene is about 110°C at atmospheric pressure (0.1 MPaG) and 200°C or higher at 0.7 MPaG, which is a general reaction pressure. When the catalyst of the present invention, which has high hydrogenation activity even at low pressure, is used, the reaction is possible at 0 MPaG to 0.3 MPaG, and the reaction process can be carried out at about 110 to 160°C, which is the boiling point of toluene at this pressure. In other words, when a conventional catalyst is used, the reaction process is generally carried out at a temperature higher than 200°C, so when the catalyst of the present invention is used, the apparatus can be operated at a lower temperature.
[0044] It is preferable to reduce the catalyst according to the present invention in a hydrogen atmosphere before carrying out the reaction step. The reduction is preferably carried out at a temperature of 150°C to 400°C for a predetermined time. By reducing the catalyst in the above temperature range, the oxide film on the catalyst surface can be removed. It is known that reduction is carried out before use for the same purpose in conventional catalysts as well, but the reduction temperature in the case of conventional catalysts is about 100°C to 200°C. In contrast, the catalyst according to the present invention can be reduced in a higher temperature range than the case of conventional catalysts. The reason why the catalyst according to the present invention can be reduced in a high temperature range has already been explained.
[0045] When the organic hydride is produced in the reaction step, a product containing the produced organic hydride and hydrogen is discharged from the reactor. The discharged product is cooled to become a mixture of liquid organic hydride and hydrogen gas, and the liquid organic hydride is separated by removing the hydrogen gas from the product. The separation step of separating the organic hydride from the product can be performed using a gas-liquid separator well known to those skilled in the art. EXAMPLES
[0046] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.
[0047] <Catalyst Production> Example 1 The manufacturing method of boron-added platinum catalyst (B / Pt / Al2O3) supported on alumina is explained. First, alumina-supported platinum catalyst (Pt / Al2O3) is prepared as the raw catalyst. Chloroplatinic acid hexahydrate (H2PtCl6·6H2O) manufactured by Kanto Chemical Co., Ltd. was used as the starting material containing platinum. Chloroplatinic acid hexahydrate was added to water and stirred to prepare an aqueous solution.
[0048] After drying the alumina carrier at 400°C for 1 hour, the alumina was impregnated with the above aqueous solution and left to stand for 24 hours. The amount of platinum supported was adjusted so that platinum was 5% by mass relative to 95% by mass of alumina. Next, the carrier to which the aqueous solution was added was evaporated to dryness at 90°C to 100°C on a hot plate, dried at 110°C in a nitrogen stream (70mL / min) for 24 hours, and further heated at 450°C in a nitrogen stream (200mL / min) for 1 hour to decompose platinum chloride. As a result, an alumina-supported platinum catalyst was obtained as a raw catalyst.
[0049] Next, triphenylborane (B(C6H5)3) manufactured by Strem Chemicals, Inc. was dissolved in toluene to prepare a toluene solution. The amount of triphenylborane dissolved was adjusted so that the molar ratio of boron to platinum in the alumina-supported platinum catalyst was 1. The alumina-supported platinum catalyst was impregnated with the toluene solution of triphenylborane and allowed to stand for 24 hours. Next, the alumina-supported platinum catalyst to which the toluene solution had been added was evaporated to dryness at 90°C to 100°C on a hot plate, and dried in a nitrogen stream (70 mL / min) at 110°C for 24 hours. This resulted in the production of a boron-added alumina-supported platinum catalyst.
[0050] Example 2 A boron-doped rhodium catalyst supported on alumina (B / Rh / Al2O3) was prepared as Example 2. The method for producing this catalyst was the same as that of Example 1, except that rhodium chloride trihydrate (RhCl3·3H2O) manufactured by Kanto Chemical Co., Ltd. was used as the rhodium-containing starting material.
[0051] <Catalyst performance evaluation> A toluene hydrogenation reaction was carried out using the catalyst of Example 1 (boron-doped alumina-supported platinum catalyst ((B / Pt / Al2O3)) and the catalyst of Example 2 (boron-doped alumina-supported rhodium catalyst (B / Rh / Al2O3)), the catalyst of Comparative Example 1 (alumina-supported platinum catalyst (Pt / Al2O3)), and the catalyst of Comparative Example 2 (alumina-supported rhodium catalyst (Rh / Al2O3)). The catalysts of Comparative Example 1 and Comparative Example 2 were raw material catalysts for producing the catalysts of Example 1 and Example 2, respectively. In the following, the catalyst of Example 1 is referred to as "Pt-B", the catalyst of Example 2 as "Rh-B", the catalyst of Comparative Example 1 as "Pt", and the catalyst of Comparative Example 2 as "Rh". The hydrogenation reaction was carried out using an atmospheric pressure fixed-bed flow type reactor.
[0052] The hydrogenation reaction conditions were as follows: Catalyst amount: 0.02g Catalyst reduction conditions: H2 (30mL / min), 850℃, 1 hour Reaction temperature: 150℃ Raw material gas Toluene:H2:N2=3.8:16.25:81.25 kPa Raw gas flow rate H2+N230mL / min Toluene 1.17mL / min (3.13×10 -3 mol / h) Reaction time: 180 min (analysis of generated gas every 30 min)
[0053] The experiment was carried out according to the following procedure. First, the catalyst was placed in the reactor, and the reactor was then assembled into the device. The air in the device was then replaced with hydrogen gas (at 30 mL / min for 10 minutes). Next, in both the examples and the comparative examples, the catalyst was reduced with hydrogen at 850°C for 1 hour. Next, the raw material gas was passed through the reactor and brought into contact with the catalyst to produce methylcyclohexane.
[0054] The reaction product (a mixture of methylcyclohexane, unreacted toluene and hydrogen) was extracted from the apparatus with a syringe and analyzed by a gas chromatograph equipped with a flame ionization detector under the following analytical conditions: Carrier gas N2 (200kPa) Column DB-1(30m) Column temperature: 60℃-140℃ Analysis time 21min Sample introduction temperature: 280℃ Detector temperature: 280℃ From the area of toluene obtained by analysis, the conversion rate of toluene was calculated according to the following formula (2). Conversion rate [%] = total product area / (total product area + unreacted toluene area) × 100 (2)
[0055] In H2 (30 mL / min), 0.1 g of catalyst was heated to the reduction temperature at 10°C / min and reduced for 1 hour. After cooling to 25°C in He (30 mL / min), CO was passed through the catalyst layer every 3 minutes by the pulse method using He as a carrier gas. The CO after passing through the catalyst layer was analyzed by a gas chromatograph equipped with a thermal conductivity detector. After 10 pulses of CO adsorption, the amount of CO adsorption was calculated from the total difference between the average area at saturated adsorption and the area before saturated adsorption. The TOF of the catalyst was calculated from the above formula (1).
[0056] [Table 1]
[0057] The toluene conversion, CO adsorption amount, and TOF obtained for the catalysts of the Examples and Comparative Examples are shown in Table 1. When the catalyst of Example 1 (Pt-B) was used, the toluene conversion was about 73%. In contrast, with the catalyst of Comparative Example 1 (Pt), the toluene conversion was about 36%, which was about half of that of Example 1. The CO adsorption amount (equivalent to the amount of exposed metal) of the catalyst of Comparative Example 1 was about 59 μmol / g. In contrast, with the catalyst of Example 1, the CO adsorption amount decreased to about 36 μmol / g. The TOF obtained from these toluene conversion and CO adsorption amounts using the above formula (1) was 3.2×10 3 (h -1 ), whereas the catalyst of Comparative Example 1 had a yield of 9.5 × 102 (h -1 ), and the TOF of the catalyst of Example 1 was about 3.4 times that of the catalyst of Comparative Example 1.
[0058] Similarly, in the cases of Example 2 (Rh-B) and Comparative Example 2 (Rh), the TOF was calculated using the toluene conversion rate and the CO adsorption amount. 2 (h -1 ) whereas the catalyst of Comparative Example 2 was 2.6 × 10 2 (h -1 ), and the TOF of the catalyst of Example 2 was about 2.5 times that of the catalyst of Comparative Example 2. When Example 2 and Comparative Example 2 are compared, the toluene conversion rate of Example 2 is equivalent to that of Comparative Example 2 (or slightly lower), but the CO adsorption amount of Example 2 was significantly smaller than that of Comparative Example 2. As a result, the TOF of the catalyst of Example 2 was larger than that of the catalyst of Comparative Example 2.
[0059] These results show that the hydrogenation activity of the catalyst is improved by adding boron. In addition, when comparing the TOF of the catalyst of Example 1 and the catalyst of Example 2, the TOF of Example 1 is higher than that of Example 2. Therefore, the catalyst of Example 1, i.e., the catalyst using platinum as the metal having hydrogenation activity, shows a better hydrogenation activity than the catalyst of Example 2, i.e., the catalyst using rhodium as the metal having hydrogenation activity.
Claims
1. A metal having hydrogenation reaction activity; A support supporting the metal; Boron added to the metal; A catalyst comprising:
2. the molar ratio of said boron to said metal is 0.5 to 2.0; The catalyst according to claim 1.
3. the metal is a platinum group metal; The catalyst according to claim 1.
4. the metal is platinum or rhodium or both; The catalyst according to claim 3.
5. The support is a metal oxide. The catalyst according to claim 1.
6. The support is aluminum oxide, silicon oxide, titanium oxide, cerium oxide, or a combination thereof; The catalyst according to claim 5.
7. A method for producing the catalyst according to any one of claims 1 to 6, comprising the steps of: A step of preparing a raw catalyst having a metal supported on a support; adding boron to the raw catalyst; reducing the raw catalyst to which boron has been added; A method for producing a catalyst comprising the steps of:
8. The step of adding boron to the raw catalyst comprises: impregnating the raw catalyst with an organic solvent solution of a boron compound; The raw catalyst impregnated with the organic solvent solution is dried.
8. A method for producing the catalyst of claim 7, comprising:
9. The boron compound is any one of triphenylborane, triethylborane, and sodium borohydride, or a combination thereof; A method for producing the catalyst according to claim 8.
10. The step of reducing the raw catalyst having boron added thereto includes reducing the raw catalyst in a hydrogen atmosphere at 650° C. to 850° C.; A method for producing the catalyst according to claim 7.
11. 1. A method for producing an organic hydride, comprising: A step of reducing the catalyst according to any one of claims 1 to 6; a reaction step of contacting the reduced catalyst with a raw material containing an unsaturated hydrocarbon and hydrogen; a separation step of separating the organic hydride from a product containing the organic hydride and hydrogen produced by the reaction step; The method includes:
12. The step of reducing the catalyst comprises reducing the catalyst at 150° C. to 400° C. under a hydrogen atmosphere; The method of claim 11.
13. The method according to claim 11, wherein the reaction step is carried out at a reaction pressure of 0 MPaG to 10 MPaG.
14. The method according to claim 13, wherein the reaction step is carried out at a reaction pressure of 0 MPaG to 1 MPaG.
15. The unsaturated hydrocarbon is toluene and the organic hydride is methylcyclohexane. The method of claim 11.
Citation Information
Patent Citations
Endoscopic ultrasonic diagnostic apparatus
JP1985099238A
Catalyst structure for storing and generating hydrogen and storage and generation method for hydrogen using it
JP2006130378A
Hydrogenation catalyst, manufacturing method of hydrogenation catalyst and manufacturing method of hydrogen carrier material
JP2018103158A
Nanocrystalline composite catalyst for storing and supplying hydrogen, nanocrystalline composite catalyst mixture for storing and supplying hydrogen, and method for supplying hydrogen
JP6734275B2