Curable composition and cured product

A curable composition using a titanium compound and ammonium fluoride catalyst with colloidal calcium carbonate enhances curing and adhesion in sealants and adhesives, overcoming curability reductions in compositions with reactive silicon groups and fatty acid-treated fillers.

JP2024157200APending Publication Date: 2024-11-07KANEKA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023071400
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Curable compositions containing organic polymers with reactive silicon groups and colloidal calcium carbonate surface-treated with fatty acids experience reduced curability when used as sealants or adhesives.

Method used

A curable composition comprising an organic polymer with reactive silicon groups, a titanium compound, and an ammonium fluoride compound as a curing catalyst, along with colloidal calcium carbonate surface-treated with a fatty acid, to enhance curing properties.

Benefits of technology

The composition exhibits rapid curing and improved adhesion, mechanical properties, and waterproofness, addressing the curability issues of previous formulations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157200000001
    Figure 2024157200000001
  • Figure 2024157200000002
    Figure 2024157200000002
  • Figure 2024157200000003
    Figure 2024157200000003
Patent Text Reader

Abstract

To provide a curable composition that contains an organic polymer with a reactive silicon group (A), a non-tin-based curing catalyst (B), and colloidal calcium carbonate surface-treated with fatty acid (C) and exhibits sufficient quick curability.SOLUTION: A curable composition contains an organic polymer with a reactive silicon group (A), a non-tin-based curing catalyst, and colloidal calcium carbonate surface-treated with fatty acid (C). As the curing catalyst (B), a titanium compound with a specific structure and an ammonium fluoride compound with a specific structure are used in combination.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable composition comprising an organic polymer having a reactive silicon group, a curing catalyst containing a specific compound, and colloidal calcium carbonate that has been surface-treated with a fatty acid, and a cured product of the curable composition. [Background technology]

[0002] Organic polymers having at least one reactive silicon group in the molecule can be crosslinked even at room temperature by the formation of siloxane bonds accompanied by hydrolysis of the silyl group due to moisture, etc. It is known that organic polymers having reactive silicon groups have the property of giving rubber-like cured products through such crosslinking reactions.

[0003] When an organic polymer having a reactive silicon group is used as a curable composition such as a sealing material, adhesive, paint, or waterproofing material, the curable composition is required to have various properties such as curability, adhesiveness, workability, mechanical properties of the cured product, and waterproofness.

[0004] A curable composition containing an organic polymer having a reactive silicon group is usually cured using a silanol condensation catalyst such as an organotin compound having a carbon-tin bond, such as dibutyltin bis(acetylacetonate). The silanol condensation catalyst is also called a curing catalyst. However, in recent years, the toxicity of organotin compounds has been pointed out. For this reason, a curing catalyst other than an organotin compound is required as a curing catalyst contained in a curable composition containing an organic polymer having a reactive silicon group. The use of a fluoride salt compound such as ammonium hydrofluoride (hydrofluoride of ammonia) has been proposed as a curing catalyst other than an organotin compound (Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2013-028819 A Summary of the Invention [Problem to be solved by the invention]

[0006] Colloidal calcium carbonate that has been surface-treated with a fatty acid is often blended as a filler in a curable composition that contains an organic polymer having a reactive silicon group. However, when colloidal calcium carbonate surface-treated with a fatty acid is blended as a filler in the hardenable composition described in Patent Document 1, the hardenability of the hardenable composition may be significantly reduced in some cases.

[0007] Therefore, an object of the present invention is to provide a curable composition which contains an organic polymer (A) having a reactive silicon group, a non-tin curing catalyst (B), and colloidal calcium carbonate (C) which has been surface-treated with a fatty acid, and which exhibits good rapid curing properties. [Means for solving the problem]

[0008] In order to solve the above problems, the present inventors have discovered that the above problems can be solved by using a combination of a titanium compound having a specific structure and an ammonium fluoride compound having a specific structure as the curing catalyst (B) in a curable composition containing an organic polymer (A) having a reactive silicon group, a non-tin-based curing catalyst, and colloidal calcium carbonate (C) that has been surface-treated with a fatty acid, and have thus completed the present invention.

[0009] That is, the present invention provides: A curable composition comprising an organic polymer (A), a curing catalyst (B), and a colloidal calcium carbonate (C) surface-treated with a fatty acid, The organic polymer (A) is represented by the following formula (1): -SiX3(1) (In formula (1), X is a hydroxyl group or a hydrolyzable group, and the three Xs may be the same or different.) and having a reactive silicon group represented by the formula: The curing catalyst (B) contains a titanium compound (b1) and an ammonium fluoride compound (b2); The titanium compound (b1) is represented by the following formula (2): Ti(OR 1 ) d Y 4-d (2) (In formula (2), R 1 represents a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, Y represents a chelate coordination compound, and d represents an integer of 0 to 4. A compound represented by the formula: The ammonium fluoride compound (b2) is represented by the following formula (3): [ka] (In formula (3), R 2 , R 3 , R 4 , and R 5 is a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, R 2 , R 3 , R 4 , and R 5 may be the same or different.) The present invention provides a curable composition comprising a compound represented by the formula: Effect of the Invention

[0010] According to the present invention, it is possible to provide a curable composition which contains an organic polymer (A) having a reactive silicon group, a non-tin curing catalyst (B), and a colloidal calcium carbonate (C) which has been surface-treated with a fatty acid, and which exhibits good rapid curing properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below.

[0012] ≪Curable composition≫ The curable composition contains an organic polymer (A), a curing catalyst (B), and colloidal calcium carbonate (C) that has been surface-treated with a fatty acid. The organic polymer (A) is represented by the following formula (1): -SiX3(1) (In formula (1), X is a hydroxyl group or a hydrolyzable group, and the three Xs may be the same or different.) The compound has a reactive silicon group represented by the formula:

[0013] The curing catalyst (B) includes a titanium compound (b1) and an ammonium fluoride compound (b2). The titanium compound (b1) is represented by the following formula (2): Ti(OR 1 ) d Y 4-d (2) (In formula (2), R 1 represents a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, Y represents a chelate coordination compound, and d represents an integer of 0 to 4. It is a compound represented by the formula: The ammonium fluoride compound (b2) is represented by the following formula (3): [ka] (In formula (3), R 2 , R 3 , R 4 , and R 5 is a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, R 2 , R 3 , R 4 , and R 5 may be the same or different.) It is a compound represented by the formula: The curable composition also optionally contains various other additives.

[0014] The essential and optional components that the curable composition may contain are described below.

[0015] <Organic polymer (A)> The organic polymer (A) has a reactive silicon group represented by the above formula (1). The organic polymer (A) has a polymer backbone and a polymer chain end bonded to the polymer backbone. In the specification and claims of this application, the polymer backbone is also referred to as a "main chain structure". The polymer backbone is a structure in which a plurality of constituent units derived from monomers are bonded in succession. The monomer may be one type or multiple types.

[0016] The polymer chain end is a portion located at the end of the organic polymer (A). The number of polymer chain ends of the organic polymer (A) is 2 when the main chain structure is linear, and is 3 or more when the polymer backbone is branched. When the organic polymer (A) is a mixture of a polymer having a linear main chain structure and a polymer having a branched main chain structure, the number of polymer chain ends is a value between 2 and 3 on average.

[0017] The reactive silicon group may be present in the polymer backbone and at the polymer chain end. In addition, two or more reactive silicon groups may be present at the polymer chain end. When the curable composition is used for adhesives, sealing materials, elastic coating agents, pressure sensitive adhesives, etc., it is preferable that the reactive silicon group is present at the polymer chain end in the organic polymer (A).

[0018] (Reactive silicon group) The reactive silicon group is a group that can generate a silanol group by hydrolysis. When the reactive silicon group generates a silanol group, the organic polymer (A) is crosslinked by a condensation reaction between the silanol groups. As described above, the reactive silicon group is a group represented by the following formula (1). -SiX3(1)

[0019] In formula (1), X is a hydroxyl group or a hydrolyzable group. The three X's may be the same or different.

[0020] X in formula (1) is a hydroxyl group or a hydrolyzable group. The hydrolyzable group is not particularly limited and may be a known hydrolyzable group. Specific examples of the hydrolyzable group include a hydrogen atom, a halogen atom, an alkoxy group, an acyloxy group, a ketoximate group, an amino group, an amide group, an acid amide group, an aminooxy group, a mercapto group, and an alkenyloxy group. Among these, an alkoxy group, an acyloxy group, a ketoximate group, and an alkenyloxy group are preferred, and an alkoxy group such as a methoxy group and an ethoxy group is more preferred because of its mild hydrolysis and easy handling.

[0021] The reactive silicon group represented by formula (1) is not particularly limited. Specific examples of the reactive silicon group represented by formula (1) include trimethoxysilyl group, triethoxysilyl group, methoxymethyldimethoxysilyl group, methoxymethyldiethoxysilyl group, triisopropenyloxysilyl group, and triacetoxysilyl group. Among these, dimethoxymethylsilyl group and trimethoxysilyl group are preferred because the synthesis of polymer (A) is easy. Trimethoxysilyl group and methoxymethyldimethoxysilyl group are preferred because they have excellent curing properties.

[0022] (Main chain structure of organic polymer (A)) The main chain structure of the organic polymer (A) is not particularly limited, and may be any of various known main chain structures. Specific examples of the main chain structure include polyoxyalkylene polymers such as polyoxyethylene polymers, polyoxypropylene polymers, polyoxybutylene polymers, polyoxytetramethylene polymers, polyoxyethylene-polyoxypropylene copolymers, and polyoxypropylene-polyoxybutylene copolymers; hydrocarbon polymers such as ethylene-propylene copolymers, polyisobutylene, isobutylene-isoprene copolymers, polybutadiene, and hydrogenated polyolefin polymers obtained by hydrogenating these polyolefin polymers; polycondensates of dibasic acids such as adipic acid and glycols; and ring-opening polymers of lactones; (meth)acrylic acid ester-based polymers obtained by radical polymerization of (meth)acrylic acid ester-based monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and stearyl (meth)acrylate; vinyl copolymers obtained by radical polymerization of two or more monomers selected from (meth)acrylic acid ester-based monomers, vinyl acetate, acrylonitrile, and styrene; polysulfide-based polymers; and diallyl phthalate-based polymers. Note that (meth)acrylic acid ester means both acrylic acid ester and methacrylic acid ester.

[0023] As the main chain structure, polyoxyalkylene polymers and (meth)acrylic acid ester polymers are particularly preferred, since they have excellent deep curing properties as a one-component composition due to their high moisture permeability, and also have excellent adhesive properties. As the main chain structure, polyoxyalkylene polymers are more preferred, and polyoxypropylene is even more preferred.

[0024] The polyoxyalkylene polymer is -R 6 It is a polymer having a repeating unit represented by -O-. 6 R is a linear or branched alkylene group having 1 to 14 carbon atoms. 6 is preferably a linear or branched alkylene group having 2 to 4 carbon atoms. 6 Specific examples of the repeating unit represented by -O- include -CHO-, -CHCHO-, -CHCH(CH)O-, -CHCH(CH)O-, -CHC(CH)(CH)O-, and -CHCHCHCHO-. The main chain structure of the polyoxyalkylene polymer may be composed of only one type of repeating unit, or may be composed of two or more types of repeating units. In particular, when the curable composition is used as a sealant, adhesive, or the like, a polyoxypropylene polymer having oxypropylene repeating units in an amount of 50% by weight or more, preferably 80% by weight or more of the polymer main chain structure is preferred as the polyoxyalkylene polymer. This is because such a polyoxyalkylene polymer is amorphous and has a relatively low viscosity.

[0025] The main chain structure of the polyoxyalkylene polymer may be either linear or branched.

[0026] The polyoxyalkylene polymer is preferably a polymer obtained by ring-opening polymerization reaction of a cyclic ether compound using a polymerization catalyst in the presence of an initiator.

[0027] Examples of the cyclic ether compound include ethylene oxide, propylene oxide, butylene oxide, tetramethylene oxide, tetrahydrofuran, etc. These cyclic ether compounds may be used alone or in combination of two or more. Among these cyclic ether compounds, propylene oxide is particularly preferred since it is capable of producing an amorphous polyether polymer having a relatively low viscosity.

[0028] Specific examples of the initiator include alcohols such as butanol, ethylene glycol, propylene glycol, propylene glycol monoalkyl ether, butanediol, hexamethylene glycol, neopentyl glycol, diethylene glycol, dipropylene glycol, triethylene glycol, glycerin, trimethylolmethane, trimethylolpropane, pentaerythritol, and sorbitol; and polyoxyalkylene polymers such as polyoxypropylene diol, polyoxypropylene triol, polyoxyethylene diol, and polyoxyethylene triol.

[0029] The method for synthesizing the polyoxyalkylene polymer is not particularly limited. Examples of methods for synthesizing polyoxyalkylene polymers include a polymerization method using an alkali catalyst such as KOH, a polymerization method using a transition metal compound-porphyrin complex catalyst such as a complex obtained by reacting an organoaluminum compound with porphyrin as disclosed in JP-A-61-215623, a polymerization method using a composite metal cyanide complex catalyst as disclosed in JP-B-46-27250, JP-B-59-15336, U.S. Pat. No. 3,278,457, U.S. Pat. No. 3,278,458, U.S. Pat. No. 3,278,459, U.S. Pat. No. 3,427,256, U.S. Pat. No. 3,427,334, and U.S. Pat. No. 3,427,335, and the like, a polymerization method using a catalyst made of a polyphosphazene salt as exemplified in JP-A-10-273512, and a polymerization method using a catalyst made of a phosphazene compound as exemplified in JP-A-11-060722. A polymerization method using a double metal cyanide complex catalyst is more preferred because of its low production cost and the fact that it can produce a polymer with a narrow molecular weight distribution.

[0030] The main chain structure of the organic polymer (A) may be a polyoxyalkylene polymer containing bonds other than ether bonds such as urethane bonds and urea bonds, within the range that does not significantly impair the desired effects. Specific examples of polymers having such a main chain structure include polyurethane prepolymers and polyurea prepolymers.

[0031] The polyurethane prepolymer can be obtained by a known method such as a method of reacting a polyol compound with a polyisocyanate compound, and the polyurea prepolymer can be obtained by a known method such as a method of reacting a polyamine compound with a polyisocyanate compound. The main chain structure may be a prepolymer having a combination of urethane bonds and urea bonds, which is obtained by reacting a polyol compound and a polyamine compound with a polyisocyanate compound.

[0032] Specific examples of the polyol compound include polyether polyol, polyester polyol, polycarbonate polyol, and polyether polyester polyol.

[0033] Specific examples of the polyisocyanate compound include diphenylmethane diisocyanate, tolylene diisocyanate, xylylene diisocyanate, methylene-bis(cyclohexyl isocyanate), isophorone diisocyanate, and hexamethylene diisocyanate.

[0034] The polyurethane prepolymer may have a terminal group of either a hydroxyl group or an isocyanate group, and the polyurea prepolymer may have a terminal group of either an amino group or an isocyanate group.

[0035] In a cured product of a curable composition containing, as the organic polymer (A), a polymer having one or more bonds selected from a urethane bond, a urea bond, and an ester bond in the main chain structure, the strength of the cured product may decrease due to cleavage of the urethane bond, the urea bond, or the ester bond in the main chain structure due to heat or the like.

[0036] When a polymer containing an amide bond in the main chain structure is used as the organic polymer, the curability of the curable composition may be improved. 7 It is represented by -C(=O)-. 7 is a hydrogen atom or an organic group which may have a substituent. When the amount of amide bonds in the main chain structure is within an appropriate range, the viscosity of the polymer is low, and a decrease in strength of the cured product due to cleavage of the amide bonds caused by heat or the like and an increase in viscosity of the curable composition due to storage are unlikely to occur, and the workability of the curable composition is good.

[0037] When the organic polymer (A) contains an amide bond in the main chain structure, the average number of amide bonds per molecule is preferably 1 to 10, more preferably 1.5 to 5, and even more preferably 2 to 3. When the average number of amide bonds per molecule is within this range, the curable composition has good curability, the organic polymer (A) has a low viscosity, and the organic polymer (A) and the curable composition are easy to handle.

[0038] As the polymer (A) described above, from the viewpoint of obtaining a curable composition excellent in storage stability and workability, a polyoxyalkylene polymer that does not contain a urethane bond, a urea bond, an ester bond, or an amide bond in the main chain structure is most preferable.

[0039] The organic polymer (A) is preferably a polymer obtained by introducing a reactive silicon group into a polymer by any one of the following methods (a) to (d). (a) A method in which the terminal hydroxyl groups of a hydroxyl-terminated organic polymer are converted to carbon-carbon unsaturated groups, and then the carbon-carbon unsaturated groups are hydrosilylated with a hydrosilane represented by HSiX3, where X is the same as those in formula (1). (b) A method of reacting a terminal hydroxyl group of a hydroxyl-terminated organic polymer with an isocyanate alkylsilane compound represented by OCN-W-SiX3. W is a divalent organic group. X is the same as those in formula (1). (c) A method in which the terminal hydroxyl groups of a hydroxyl-terminated organic polymer are converted to carbon-carbon unsaturated groups, and then the carbon-carbon unsaturated groups are subjected to an ene-thiol reaction with a mercaptoalkylsilane compound represented by HS-W-SiX3. W is a divalent organic group. X is the same as those in formula (1). (d) A hydroxyl-terminated organic polymer is reacted with a polyisocyanate compound to synthesize an NCO-terminated organic polymer, and then the terminal NCO groups are converted to an NCO-terminated organic polymer by the reaction of HNR 8 A method of reacting with a silane compound represented by the formula: -W-SiX3 or HS-W-SiX3, where W is a divalent organic group. 8 is a hydrogen atom or an alkyl group. X is the same as those in formula (1).

[0040] In the above methods (a) and (c), examples of the terminal carbon-carbon unsaturated group include a vinyl group, an allyl group, a methallyl group, an allenyl group, and a propargyl group.

[0041] In any of the above methods (b) to (d), the polymer (A) obtained by using a silane compound in which W is methylene exhibits extremely high curability.

[0042] The method (a) is preferred because it is easy to obtain an organic polymer (A) having good storage stability, whereas the methods (b), (c), and (d) are preferred because they can obtain a high conversion rate in a relatively short reaction time.

[0043] Methods for introducing reactive silicon groups by method (a) have been proposed in JP-B-45-36319, JP-B-46-12154, JP-A-50-156599, JP-A-54-6096, JP-A-55-13767, JP-A-55-13468, JP-A-57-164123, JP-B-3-2450, U.S. Pat. No. 3,632,557, U.S. Pat. No. 4,345,053, U.S. Pat. No. 4,366,307, and U.S. Pat. No. 4,960,844, etc. Examples of such methods include the method proposed in JP-A-61-197631, JP-A-61-215622, JP-A-61-215623, and JP-A-61-218632, in which reactive silicon groups are introduced by hydrosilylation or the like into a polyoxypropylene polymer having a high molecular weight and narrow molecular weight distribution, that is, a number average molecular weight of 6,000 or more and a Mw / Mn ratio of 1.6 or less, and the method proposed in JP-A-3-72527.

[0044] The number average molecular weight of the organic polymer (A) is not particularly limited. The number average molecular weight of the organic polymer (A) is preferably 3,000 to 100,000, more preferably 3,000 to 50,000, and particularly preferably 3,000 to 30,000, as a polystyrene-equivalent molecular weight in GPC. When the number average molecular weight is within the above range, the amount of reactive silicon group introduced is appropriate, and therefore, it is easy to obtain an organic polymer (A) that has a viscosity that is easy to handle and has excellent workability while keeping production costs within an appropriate range.

[0045] The molecular weight of the organic polymer (A) can also be shown as the end group-converted molecular weight calculated by directly measuring the end group concentration of the polymer precursor before the introduction of reactive silicon groups by titration analysis based on the principles of the hydroxyl value measurement method of JIS K 1557 and the iodine value measurement method specified in JIS K 0070, and taking into consideration the structure of the polymer (the degree of branching determined by the polymerization initiator used). The end group-converted molecular weight of the organic polymer (A) can also be calculated by preparing a calibration curve of the number average molecular weight determined by general GPC measurement of the polymer precursor and the above end group-converted molecular weight, and converting the number average molecular weight determined by GPC of the organic polymer (A) into the end group-converted molecular weight.

[0046] The molecular weight distribution (Mw / Mn) of the organic polymer (A) is not particularly limited. It is preferable that the molecular weight distribution of the organic polymer (A) is narrow. Specifically, the molecular weight distribution is preferably 1.6 or less, more preferably 1.4 or less, even more preferably 1.3 or less, and particularly preferably 1.2 or less. The molecular weight distribution of the organic polymer (A) can be determined from the number average molecular weight and weight average molecular weight obtained by GPC measurement.

[0047] In order to obtain a good rubber-like cured product, the reactive silicon group of the organic polymer (A) is preferably present at the polymer chain end. The number of reactive silicon groups is preferably 0.5 or more on average per polymer chain end, more preferably 0.6 or more, even more preferably 0.7 or more, and particularly preferably 0.8 or more. When the number of reactive silicon groups is 0.5 or more, the curability of the organic polymer (A) and the curable composition is good, and the cured product of the curable composition has good rubber elasticity.

[0048] The number of reactive silicon groups in one molecule is preferably 1 to 7 on average, more preferably 1 to 4, and particularly preferably 1 to 3.

[0049] In addition, as described in WO2013 / 180203, an organic polymer having two or more reactive silicon groups at the polymer chain end can also be used as the organic polymer (A). Such an organic polymer (A) exhibits high curability, and the resulting cured product is expected to have high strength and high recovery.

[0050] Specific examples of commercially available organic polymers (A) include various reactive silicon group-containing polyoxypropylene products such as Kaneka MS Polymer (registered trademark) and Kaneka Silyl (registered trademark), reactive silicon group-containing poly(meth)acrylic acid ester products such as Kaneka TA Polymer (registered trademark) and KANEKA XMAP (registered trademark), reactive silicon group-containing polyisobutylene products such as EPION (registered trademark), etc. All of these commercially available organic polymers (A) are products of Kaneka Corporation.

[0051] <Curing catalyst (B)> The curable composition contains a curing catalyst (B) that cures the organic polymer (A) by hydrolysis and condensation. The curing catalyst (B) contains a titanium compound (b1) and an ammonium fluoride compound (b2). The weight ratio (b1 / b2) of the component derived from the titanium compound (b1) to the component derived from the ammonium fluoride compound (b2) is preferably 5 to 0.1, more preferably 4 to 0.5.

[0052] (Titanium compounds (b1)) The titanium compound (b1) is a compound represented by the following formula (2). Ti(OR 1 ) d Y 4-d (2)

[0053] In formula (2), R 1 represents a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent; Y represents a chelate coordination compound; and d represents an integer of 0 to 4. R 1 The hydrocarbon group as R may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group. 1 When the hydrocarbon group represented by R is an aliphatic hydrocarbon group, the aliphatic hydrocarbon group may have one or more unsaturated bonds. 1 When the hydrocarbon group as the alkyl group is an aliphatic hydrocarbon group, the structure of the aliphatic hydrocarbon group may be linear, branched, or cyclic, or may be a combination of these structures. R 1 The hydrocarbon group represented by R may have a substituent. 1 The hydrocarbon group as R preferably has no substituent. 1 Examples of the substituent that the hydrocarbon group may have include a halogen atom, an amino group, an alkylamino group having 1 to 4 carbon atoms, a dialkylamino group having 2 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, and a hydroxyl group. R 1The hydrocarbon group as the radical preferably has 1 to 12 carbon atoms, more preferably has 1 to 6 carbon atoms, and further preferably has 1 to 4 carbon atoms. R 1 As the hydrocarbon group for , a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, and a phenyl group are preferred.

[0054] The chelating coordination compound Y is preferably a bidentate organic ligand. Examples of the chelating coordination compound include β-diketones and β-ketoesters. Specific examples of β-diketones include acetylacetone (ACAC), trifluoroacetylacetone, hexafluoroacetylacetone, benzoylacetone, thenoyltrifluoroacetone, dipivaloylmethane, dibenzoylmethane, and ascorbic acid.Specific examples of β-ketoesters include methyl acetoacetate, ethyl acetoacetate, allyl acetoacetate, benzyl acetoacetate, n-propyl acetoacetate, isopropyl acetoacetate, n-butyl acetoacetate, isobutyl acetoacetate, tert-butyl acetoacetate, 2-methoxyethyl acetoacetate, and methyl 3-oxopentanoate.

[0055] Specific examples of titanium compound (b1) include tetramethoxytitanium, trimethoxyethoxytitanium, trimethoxyisopropoxytitanium, trimethoxybutoxytitanium, dimethoxydiethoxytitanium, dimethoxydiisopropoxytitanium, dimethoxydibutoxytitanium, methoxytriethoxytitanium, methoxytriisopropoxytitanium, methoxytributoxytitanium, tetraethoxytitanium, triethoxyisopropoxytitanium, triethoxybutoxytitanium, diethoxydiisopropoxytitanium, diethoxydibutoxytitanium, ethoxytriisopropoxytitanium, ethoxytributoxytitanium, tetraisopropoxytitanium, triisopropoxybutoxytitanium, diisopropoxydibutoxytitanium, tetrabutoxytitanium, tetratert-butoxytitanium, bis(acetylacetonato)diisopropoxytitanium, bis(ethylacetoacetate)diisopropoxytitanium, and bis(ethylacetoacetate)diisobutoxytitanium. From the viewpoint of obtaining good curability, tetraalkoxytitanium is preferred, and tetraisopropoxytitanium is particularly preferred.

[0056] From the viewpoints of availability, compatibility with the organic polymer (A) and curability, tetraisopropoxytitanium, tetratert-butoxytitanium, bis(acetylacetonato)diisopropoxytitanium, bis(ethylacetoacetate)diisobutoxytitanium and bis(ethylacetoacetate)diisopropoxytitanium are more preferred, and tetraisopropoxytitanium, bis(ethylacetoacetate)diisobutoxytitanium and bis(ethylacetoacetate)diisopropoxytitanium are particularly preferred. The titanium compound (b2) may be a single component or a combination of multiple components. The titanium compound (b2) may be used alone or in combination of two or more components.

[0057] In terms of rapid curing, the amount of the titanium compound (b2) used is preferably 0.1 to 5.0 parts by weight, more preferably 0.5 to 4.5 parts by weight, and even more preferably 0.5 to 4.0 parts by weight, based on 100 parts by weight of the organic polymer (A).

[0058] (Ammonium fluoride compound (b2)) The ammonium fluoride compound (b2) is a compound represented by the following formula (3). [ka]

[0059] In formula (3), R 2 , R 3 , R 4 , and R 5 R is a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent. 2 , R 3 , R 4 , and R 5 may be the same or different.

[0060] R in Equation (3) 2 , R 3 , R 4 , and R 5 Specific examples of the hydrocarbon group which may have a substituent as R include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-hexyl, 2-ethylhexyl, and n-dodecyl; unsaturated hydrocarbon groups such as vinyl, isopropenyl, and allyl; alkoxymethyl groups such as methoxymethyl; halogenated methyl groups such as chloromethyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl, toluyl, and 1-naphthyl; and aralkyl groups such as benzyl. 2 , R 3 , R 4 , and R 5 Two or more of may be bonded to form a ring. Among these groups, the alkyl group is preferred due to its high curing catalytic activity.

[0061] Specific examples of the ammonium fluoride compound (b2) include tetramethylammonium fluoride, tetraethylammonium fluoride, tetra-n-propylammonium fluoride, tetraisopropylammonium fluoride, tetra-n-butylammonium fluoride, methyltri-n-propylammonium fluoride, methyltri-n-octylammonium fluoride, and benzyltrimethylammonium fluoride, etc. Among these, tetra-n-butylammonium fluoride is preferred because of its high curing catalyst activity and easy availability.

[0062] The amount of the ammonium fluoride compound (b2) used is preferably 0.1 to 4.0 parts by weight, more preferably 0.2 to 3.0 parts by weight, and even more preferably 0.3 to 2.0 parts by weight, based on 100 parts by weight of the organic polymer (A).

[0063] (Reaction product of titanium compound (b1) and ammonium fluoride compound (b2)) The reaction product of the titanium compound (b1) and the ammonium fluoride compound (b2) can be obtained by mixing and reacting the above-mentioned titanium compound (b1) and the above-mentioned ammonium fluoride compound (b2).

[0064] The amount of the reaction product of the titanium compound (b1) and the ammonium fluoride compound (b2) used is preferably 0.1 to 7.0 parts by weight, more preferably 0.2 to 5.0 parts by weight, still more preferably 0.3 to 4.0 parts by weight, and particularly preferably 0.5 to 3.0 parts by weight, relative to 100 parts by weight of the organic polymer (A).

[0065] <Colloidal calcium carbonate (C) surface-treated with fatty acid> In the colloidal calcium carbonate (C) surface-treated with a fatty acid (hereinafter also referred to as "surface-treated calcium carbonate (C)"), the fatty acid is attached to at least a part of the surface of the colloidal calcium carbonate. The surface treatment agent used when attaching the fatty acid to at least a part of the surface of the colloidal calcium carbonate is not particularly limited, and suitable examples thereof include one or more selected from the group consisting of fatty acids, salts of fatty acids, derivatives of fatty acids, and salts of derivatives of fatty acids.

[0066] The fatty acid is not particularly limited, but saturated fatty acids, unsaturated fatty acids, aliphatic carboxylic acids, etc. can be preferably used. Specific examples of fatty acids include caproic acid, caprylic acid, pelargonic acid, capric acid, undecanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, arachis acid, behenic acid, lignoceric acid, cerotic acid, montanic acid, melissic acid, lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, obsucile acid, caroleic acid, undecylenic acid, Linderic acid, tsuzuic acid, physeteric acid, moristoleic acid, palmitoleic acid, petroselinic acid, oleic acid, elaidic acid, asclevic acid, vaccenic acid, gadoleic acid, gondoic acid, cetoleic acid, erucic acid, brassidic acid, selacoleic acid, ximenic acid, lumecic acid, sorbic acid, and linoleic acid. The fatty acids may be used alone or in combination of two or more. Of the above fatty acids, palmitic acid, stearic acid, and oleic acid are particularly preferred.

[0067] The shape of the surface-treated calcium carbonate (C) is not particularly limited, and examples thereof include a spherical shape, a hollow spherical shape, and an amorphous shape. For the purpose of reducing the weight (specific gravity) of the cured product of the curable composition, it is preferable to use a hollow fatty acid surface-treated colloidal calcium carbonate (C).

[0068] The particle size of the surface-treated calcium carbonate (C) is preferably from 0.10 μm to 0.02 μm, and more preferably from 0.09 μm to 0.03 μm.

[0069] The amount of the surface-treated calcium carbonate (C) used is preferably 10 to 400 parts by weight, more preferably 30 to 300 parts by weight, and even more preferably 50 to 200 parts by weight, based on 100 parts by weight of the organic polymer (A).

[0070] As described later, the curable composition may contain, as a filler, other fillers than the surface-treated calcium carbonate (C) together with the surface-treated calcium carbonate (C). As the other filler, calcium carbonate other than the surface-treated calcium carbonate (C) can be used. The total amount of the surface-treated calcium carbonate (C) and the other fillers used in the curable composition is preferably 10 to 500 parts by weight, more preferably 30 to 400 parts by weight, further preferably 50 to 300 parts by weight, and particularly preferably 80 to 250 parts by weight, based on 100 parts by weight of the organic polymer (A).

[0071] <Other additives> The curable composition may contain additives other than the organic polymer (A), the curing catalyst (B), and the surface-treated calcium carbonate (C) within the range in which the desired effect is not impaired. Examples of the additives include silanol condensation catalysts other than the curing catalyst (B), fillers other than the surface-treated calcium carbonate (C), adhesion promoters, plasticizers, solvents, diluents, thixotropy-imparting agents, antioxidants, light stabilizers, ultraviolet absorbers, physical property regulators, tackifier resins, compounds containing epoxy groups, photocurable substances, oxygen-curable substances, epoxy resins, other resins, surface property improvers, foaming agents, curability regulators, flame retardants, silicates, radical inhibitors, metal deactivators, phosphorus-based peroxide decomposers, lubricants, pigments, and fungicides.

[0072] (Silanol condensation catalyst) The curable composition may contain a silanol condensation catalyst other than the above-mentioned curing catalyst (B) for the purpose of promoting a hydrolysis condensation reaction between reactive silicon groups in the organic polymer (A) and chain-extending or crosslinking the polymer. Examples of the silanol condensation catalyst include organotin compounds, metal carboxylates, amine compounds, carboxylic acids, metal alkoxides, and inorganic acids. The silanol condensation catalyst may be used in combination of two or more different catalysts. The amount of the silanol condensation catalyst used is preferably from 0.001 to 20 parts by weight, more preferably from 0.01 to 15 parts by weight, and particularly preferably from 0.01 to 10 parts by weight, based on 100 parts by weight of the organic polymer (A).

[0073] Specific examples of the metal carboxylate include bismuth carboxylate, titanium carboxylate, zirconium carboxylate, iron carboxylate, etc. As the metal carboxylate, salts of the following carboxylic acids combined with various metals can be used.

[0074] Specific examples of the amine compound include amines such as octylamine, 2-ethylhexylamine, laurylamine, and stearylamine; nitrogen-containing heterocyclic compounds such as pyridine, 1,8-diazabicyclo[5,4,0]undecene-7 (DBU), and 1,5-diazabicyclo[4,3,0]nonene-5 (DBN); guanidines such as guanidine, phenylguanidine, and diphenylguanidine; biguanides such as butylbiguanide, 1-o-tolylbiguanide, and 1-phenylbiguanide; amino group-containing silane coupling agents; and ketimine compounds.

[0075] Specific examples of carboxylic acids include acetic acid, propionic acid, butyric acid, 2-ethylhexanoic acid, lauric acid, stearic acid, oleic acid, linoleic acid, neodecanoic acid, and versatic acid.

[0076] Specific examples of alkoxy metals include titanium compounds such as tetrabutyl titanate, titanium tetrakis(acetylacetonate), and diisopropoxytitanium bis(ethylacetoacetate); aluminum compounds such as aluminum tris(acetylacetonate) and diisopropoxyaluminum ethylacetoacetate; and zirconium compounds such as zirconium tetrakis(acetylacetonate). Other silanol condensation catalysts that can be used include fluorine anion-containing compounds, photoacid generators, and photobase generators. The silanol condensation catalyst may be used in combination of two or more different catalysts. The amount of the silanol condensation catalyst used is preferably from 0.001 to 20 parts by weight, more preferably from 0.01 to 15 parts by weight, and particularly preferably from 0.01 to 10 parts by weight, based on 100 parts by weight of the organic polymer (A).

[0077] (Fillers other than surface-treated calcium carbonate (C)) The curable composition may contain fillers other than the surface-treated calcium carbonate (C). Various fillers can be used as the other fillers. Examples of the other fillers include reinforcing fillers such as fumed silica, precipitated silica, crystalline silica, fused silica, dolomite, anhydrous silicic acid, hydrous silicic acid, and carbon black; colloidal calcium carbonate surface-treated with a compound other than fatty acid, colloidal calcium carbonate not surface-treated, ground calcium carbonate, magnesium carbonate, diatomaceous earth, calcined clay, clay, talc, titanium oxide, bentonite, organic bentonite, ferric oxide, aluminum fine powder, flint powder, zinc oxide, activated zinc oxide, and resin powder; and fibrous fillers such as asbestos, glass fiber, and filaments. Examples of the resin powder include PVC powder and PMMA powder. As described above, the total amount of the surface-treated calcium carbonate (C) and the other fillers used in the curable composition is preferably 10 to 500 parts by weight, more preferably 30 to 400 parts by weight, further preferably 50 to 300 parts by weight, and particularly preferably 80 to 250 parts by weight, relative to 100 parts by weight of the organic polymer (A).

[0078] When it is desired to obtain a cured product having high strength by using another filler, a filler selected from mainly fumed silica, precipitated silica, crystalline silica, fused silica, dolomite, silicic anhydride, hydrated silicic acid, carbon black, surface-treated fine calcium carbonate, calcined clay, clay, active zinc oxide, and the like can be preferably used as the other filler. The amount of these other fillers, which is preferable in terms of the strength of the cured product, is preferably 1 to 200 parts by weight per 100 parts by weight of the organic polymer (A). In addition, when it is desired to obtain a cured product with low strength and high breaking elongation, fillers selected from mainly titanium oxide, calcium carbonate other than the surface-treated calcium carbonate (C), magnesium carbonate, talc, ferric oxide, zinc oxide, and shirasu balloons can be preferably used as the other fillers. In general, the larger the specific surface area of ​​these other fillers, the greater the effect of improving the breaking strength, breaking elongation, and adhesiveness of the cured product. The amount of these other fillers used, which is preferable in terms of the breaking elongation of the cured product, is preferably 5 to 200 parts by weight per 100 parts by weight of the organic polymer (A).

[0079] The other fillers may be used alone or in combination of two or more. For example, a colloidal calcium carbonate other than the surface-treated calcium carbonate (C) may be used in combination with calcium carbonate having a particle size of 1 μm or more, such as ground calcium carbonate that has not been surface-treated, as the other fillers.

[0080] The curable composition may contain spherical hollow bodies such as balloons for the purpose of reducing the weight (specific gravity) of the cured product. A balloon is a spherical filler with a hollow interior. Examples of materials for the balloon include inorganic materials such as glass, silase, and silica, and organic materials such as phenolic resin, urea resin, polystyrene, saran, and acrylonitrile. The materials for the balloon are not limited to these materials. The materials for the balloon may be composite materials made of inorganic materials and organic materials. In addition, the materials for the balloon may be laminated with multiple layers. In addition, the balloon may be used alone or in combination with two or more types. The surface of the balloon may be surface-treated, coated, or treated with various surface treatment agents. For example, organic balloons coated with calcium carbonate, talc, titanium oxide, etc., and inorganic balloons surface-treated with a silane coupling agent can be used.

[0081] The particle size of the balloons is preferably 3 to 200 μm, and particularly preferably 10 to 110 μm. When the particle size of the balloons is within the above range, the weight of the cured product can be reduced to a desired extent by using an appropriate amount of balloons, and the cured product can be formed while suppressing the occurrence of surface irregularities and reduction in elongation.

[0082] When using balloons, anti-slip agents such as those described in JP-A-2000-154368 and amine compounds for making the surface of the cured product uneven and matte such as those described in JP-A-2001-164237 can be added to the curable composition. As the amine compounds, primary and / or secondary amines having a melting point of 35° C. or higher are particularly preferred.

[0083] Specific examples of balloons are described in JP-A-2-129262, JP-A-4-8788, JP-A-4-173867, JP-A-5-1225, JP-A-7-113073, JP-A-9-53063, JP-A-10-251618, JP-A-2000-154368, JP-A-2001-164237, WO97 / 05201, and the like.

[0084] The amount of the spherical hollow bodies (balloons) used is preferably 0.01 to 30 parts by weight based on 100 parts by weight of the organic polymer (A). The lower limit is more preferably 0.1 parts by weight, and the upper limit is more preferably 20 parts by weight. By using the spherical hollow bodies in an amount within the above range, the elongation and breaking strength of the cured product can be maintained while improving the workability.

[0085] (Adhesion promoter) The curable composition may contain an adhesion promoter. Examples of the adhesion promoter include a silane coupling agent. Silane coupling agents are compounds having a hydrolyzable silicon group and a functional group other than the hydrolyzable silicon group in the molecule. By using the silane coupling agent, when the curable composition is applied to various adherends, such as inorganic substrates such as glass, aluminum, stainless steel, zinc, copper, and mortar, and organic substrates such as vinyl chloride, acrylic, polyester, polyethylene, polypropylene, and polycarbonate, the agent shows a remarkable adhesiveness improving effect under non-primer conditions or primer treatment conditions. When the curable composition is used under non-primer conditions, the effect of improving the adhesiveness to various adherends is particularly remarkable. In addition to the above functions, the silane coupling agent can also function as a dehydrating agent, a physical property adjuster, and a dispersibility improver for inorganic fillers.

[0086] The hydrolyzable group in the hydrolyzable silicon group of the silane coupling agent is not particularly limited. Examples of the hydrolyzable group include a hydrogen atom, a halogen atom, an alkoxy group, an aryloxy group, an alkenyloxy group, an acyloxy group, a ketoximate group, an amino group, an amide group, an acid amide group, an aminooxy group, and a mercapto group. Among these, a halogen atom, an alkoxy group, an alkenyloxy group, and an aryloxy group are preferred in terms of high activity. A chlorine atom and an alkoxy group are preferred because they are easily introduced into a silane coupling agent. Since they are mildly hydrolyzed and easy to handle, alkoxy groups such as a methoxy group and an ethoxy group are more preferred, and a methoxy group and an ethoxy group are particularly preferred. In addition, the compounds that are eliminated by reaction in the ethoxy group and the isopropenyloxy group are ethanol and acetone, respectively, and are preferred in terms of safety. In some cases, the number of hydrolyzable groups bonded to a silicon atom in a silane coupling agent is preferably 3 in order to ensure good adhesion. In some cases, 2 is better in order to ensure the storage stability of a curable composition.

[0087] When using a silane coupling agent as an adhesion promoter, an aminosilane coupling agent having a hydrolyzable silicon group and a substituted or unsubstituted amino group is preferred because it has a large adhesion improving effect. The substituent in the substituted amino group is not particularly limited. Examples of the substituent include an alkyl group, an aralkyl group, and an aryl group.

[0088] Specific examples of aminosilane coupling agents include γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropyltriisopropoxysilane, γ-aminopropylmethyldimethoxysilane, γ-aminopropylmethyldiethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl)aminopropyltriethoxysilane, γ-(2-aminoethyl)aminopropylmethyldiethoxysilane, γ-(2-aminoethyl)aminopropyltriisopropoxysilane, γ-(2-(2-aminoethyl)aminoethyl)aminopropyltrimethoxysilane, γ-(6-aminohexyl)aminopropyltrimethoxysilane, and 3-(N-ethylamino)-2-methylpropyltrimethoxysilane. , amino group-containing silanes such as γ-ureidopropyltrimethoxysilane, γ-ureidopropyltriethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, N-benzyl-γ-aminopropyltrimethoxysilane, N-vinylbenzyl-γ-aminopropyltriethoxysilane, N-cyclohexylaminomethyltriethoxysilane, N-cyclohexylaminomethyldiethoxymethylsilane, N-phenylaminomethyltrimethoxysilane, N-butylaminopropyltrimethoxysilane, (2-aminoethyl)aminomethyltrimethoxysilane, N,N'-bis[3-(trimethoxysilyl)propyl]ethylenediamine, and bis(trimethoxysilylpropyl)amine; and ketimine-type silanes such as N-(1,3-dimethylbutylidene)-3-(triethoxysilyl)-1-propanamine.

[0089] Among these, γ-aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, and γ-(2-aminoethyl)aminopropylmethyldimethoxysilane are preferred in terms of good adhesion of the cured product. Only one type of aminosilane coupling agent may be used, or two or more types may be used in combination. It has been pointed out that γ-(2-aminoethyl)aminopropyltrimethoxysilane is more irritating than other aminosilanes. Instead of reducing the amount of γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane can be used in combination to reduce irritation. In addition, a silane coupling agent obtained by partially condensing a hydrolyzable silicon group to form an oligomer can also be used preferably in terms of safety and stability. The silane coupling agent to be condensed may be a single type or multiple types. Examples of oligomerized silane coupling agents include Dynasylan 1146 from Evonik. In terms of good storage stability of the curable composition, γ-aminopropyltrimethoxysilane and γ-(2-aminoethyl)aminopropylmethyldimethoxysilane are preferred.

[0090] Specific examples of silane coupling agents other than aminosilane coupling agents include epoxy group-containing silane coupling agents such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltriethoxysilane; isocyanate group-containing silane coupling agents such as γ-isocyanatepropyltrimethoxysilane, γ-isocyanatepropyltriethoxysilane, γ-isocyanatepropylmethyldiethoxysilane, γ-isocyanatepropylmethyldimethoxysilane, (isocyanatemethyl)trimethoxysilane, and (isocyanatemethyl)dimethoxymethylsilane; and γ-mercaptopropyltrimethoxysilane and γ-mercaptopropyltriethoxysilane. mercapto group-containing silane coupling agents such as γ-mercaptopropylmethyldimethoxysilane, γ-mercaptopropylmethyldiethoxysilane, and mercaptomethyltriethoxysilane; carboxy silane coupling agents such as β-carboxyethyltriethoxysilane, β-carboxyethylphenylbis(2-methoxyethoxy)silane, and N-β-(carboxymethyl)aminoethyl-γ-aminopropyltrimethoxysilane; vinyl type unsaturated group-containing silane coupling agents such as vinyltrimethoxysilane, vinyltriethoxysilane, γ-methacryloyloxypropylmethyldimethoxysilane, and γ-acryloyloxypropylmethyltriethoxysilane; halogen-containing silane coupling agents such as γ-chloropropyltrimethoxysilane; isocyanurate silane coupling agents such as tris(trimethoxysilyl)isocyanurate, etc. can also be used. In addition, condensates obtained by partially condensing the above silane coupling agents can also be used. Examples of such condensates include Dynasylan 6490 and Dynasylan 6498 manufactured by Evonik.Furthermore, modified derivatives of these, such as amino-modified silyl polymers, silylated amino polymers, unsaturated aminosilane complexes, phenylamino long-chain alkylsilanes, aminosilylated silicones, and silylated polyesters, can also be used as silane coupling agents.

[0091] Of these, in terms of good adhesiveness of the cured product, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, and γ-glycidoxypropylmethyldimethoxysilane are preferred.

[0092] The above silane coupling agents may be used alone or in combination of two or more. The amount of the silane coupling agent used is preferably from 0.1 to 20 parts by weight, more preferably from 0.5 to 10 parts by weight, based on 100 parts by weight of the organic polymer (A).

[0093] (Plasticizer) The curable composition may contain a plasticizer. The addition of a plasticizer makes it possible to adjust the viscosity and slump of the curable composition, and the mechanical properties, such as the tensile strength and elongation, of the cured product.

[0094] Specific examples of plasticizers include phthalate compounds other than phthalate ester (B), such as dibutyl phthalate, diisononyl phthalate (DINP), diheptyl phthalate, di(2-ethylhexyl) phthalate, diisodecyl phthalate (DIDP), and butyl benzyl phthalate; terephthalate compounds such as bis(2-ethylhexyl)-1,4-benzenedicarboxylate; non-phthalate compounds such as 1,2-cyclohexanedicarboxylic acid diisononyl ester; dioctyl adipate, dioctyl sebacate, and dibutyl sebacate. Examples of suitable oils include aliphatic polycarboxylic acid ester compounds such as diisodecyl succinate and tributyl acetyl citrate; unsaturated fatty acid ester compounds such as butyl oleate and methyl acetylricinoleate; alkylsulfonic acid phenyl esters; phosphate ester compounds such as tricresyl phosphate and tributyl phosphate; trimellitic acid ester compounds; chlorinated paraffins; hydrocarbon oils such as alkyl diphenyls and partially hydrogenated terphenyls; process oils; epoxidized soybean oil, and epoxy plasticizers such as epoxy benzyl stearate. A specific example of the terephthalic acid ester compound is EASTMAN168 (trade name, manufactured by EASTMAN CHEMICAL). A specific example of the non-phthalic acid ester compound is Hexamoll DINCH (trade name, manufactured by BASF). A specific example of the alkylsulfonic acid phenyl ester is Mesamoll (trade name, manufactured by LANXESS).

[0095] Polymeric plasticizers can also be used. The use of polymeric plasticizers allows the initial physical properties of the cured product to be maintained for a long period of time compared to the use of low molecular weight plasticizers. Furthermore, the drying properties (paintability) of the cured product when coated with an alkyd paint are improved.

[0096] Specific examples of polymer plasticizers include vinyl polymers, which are polymers of vinyl monomers; esters of polyalkylene glycols and polyols, such as diethylene glycol dibenzoate, triethylene glycol dibenzoate, and pentaerythritol ester; polyester plasticizers obtained from dibasic acids, such as sebacic acid, adipic acid, azelaic acid, and phthalic acid, and dihydric alcohols, such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, and dipropylene glycol; polyether polyols, such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol, having a number average molecular weight of 500 or more, or even 1,000 or more; derivatives of these polyether polyols in which the hydroxyl groups are converted to ester groups, ether groups, and the like; polystyrenes, such as polystyrene and poly-α-methylstyrene; polybutadiene, polybutene, polyisobutylene, butadiene-acrylonitrile, and polychloroprene. Polymer plasticizers are not limited to these.

[0097] The polymer plasticizer is preferably compatible with the organic polymer (A). From this point of view, polyethers and vinyl polymers are preferred. When polyethers are used as plasticizers, the surface curability and deep curability are improved, and curing delay after storage does not occur. Among polyethers, polypropylene glycol is more preferred. Also, vinyl polymers are preferred from the viewpoint of compatibility with the polymer (A) and the viewpoint of weather resistance and heat resistance of the cured product. Among vinyl polymers, acrylic polymers and / or methacrylic polymers are preferred, and acrylic polymers such as polyacrylic acid alkyl esters are more preferred. As a method for synthesizing vinyl polymers, living radical polymerization is preferred, and atom transfer radical polymerization is more preferred, since it provides a polymer with a narrow molecular weight distribution and low viscosity. Also, the so-called SGO process described in JP-A-2001-207157, in which acrylic acid alkyl ester monomers are continuously bulk polymerized at high temperature and high pressure, is also preferred as a method for producing vinyl polymers.

[0098] The number average molecular weight of the polymer plasticizer is preferably from 500 to 15,000, more preferably from 800 to 10,000, further preferably from 1,000 to 8,000, particularly preferably from 1,000 to 5,000, and most preferably from 1,000 to 3,000. When the number average molecular weight of the polymer plasticizer is within the above range, the outflow of the plasticizer from the cured product over time due to heat, rainfall, etc. can be suppressed, while the initial physical properties of the cured product can be maintained for a long period of time, the curable composition has an appropriate viscosity, and the workability of the curable composition is good. The molecular weight distribution of the polymer plasticizer is not particularly limited, but is preferably narrow. Specifically, the molecular weight distribution is preferably less than 1.80, more preferably 1.70 or less, even more preferably 1.60 or less, even more preferably 1.50 or less, particularly preferably 1.40 or less, and most preferably 1.30 or less.

[0099] The number average molecular weight of vinyl polymers is measured by the GPC method. The number average molecular weight of polyether polymers is measured by the end group analysis method. The molecular weight distribution (Mw / Mn) is measured by the GPC method (polystyrene equivalent).

[0100] The polymer plasticizer may or may not have a reactive silicon group. When the polymer plasticizer has a reactive silicon group, the polymer plasticizer acts as a reactive plasticizer and can prevent the plasticizer from migrating from the cured product. When the polymer plasticizer has a reactive silicon group, the number of reactive silicon groups is preferably 1 or less on average per molecule, more preferably 0.8 or less. When using a plasticizer having a reactive silicon group, particularly a polyether polymer having a reactive silicon group, it is necessary that the number average molecular weight is lower than that of the organic polymer (A).

[0101] The amount of the plasticizer used is preferably 5 to 150 parts by weight, more preferably 10 to 120 parts by weight, and even more preferably 20 to 100 parts by weight, based on 100 parts by weight of the organic polymer (A). When the amount of the plasticizer used is within the above range, a cured product excellent in mechanical strength can be formed while fully obtaining the desired effect of using the plasticizer. The plasticizer may be used alone or in combination of two or more kinds. A low molecular weight plasticizer and a polymeric plasticizer may be used in combination. These plasticizers may be blended with the organic polymer (A) when producing the polymer (A).

[0102] (Solvent, diluent) The curable composition may contain a solvent or a diluent. The solvent and the diluent are not particularly limited. As the solvent and the diluent, aliphatic hydrocarbons, aromatic hydrocarbons, alicyclic hydrocarbons, halogenated hydrocarbons, alcohols, esters, ketones, ethers, etc. can be used. When using a solvent or a diluent, the boiling point of the solvent is preferably 150°C or higher, more preferably 200°C or higher, and particularly preferably 250°C or higher, in view of the problem of air pollution when the curable composition is used indoors. The above-mentioned solvents or diluents may be used alone or in combination of two or more kinds.

[0103] (Thixotropic agent) The curable composition may contain a thixotropy-imparting agent as necessary to prevent sagging and improve workability. The thixotropy-imparting agent is not particularly limited. Examples of the thixotropy-imparting agent include polyamide waxes; hydrogenated castor oil derivatives; and metal soaps such as calcium stearate, aluminum stearate, and barium stearate. Trade names include Disparlon 6500, Disparlon 308, Disparlon 6300, Crayvallac SL, and Crayvallac SLT. These thixotropy-imparting agents may be used alone or in combination of two or more. The amount of the thixotropy imparting agent used is preferably 0.1 to 20 parts by weight based on 100 parts by weight of the polymer (A).

[0104] (Antioxidants) The curable composition may contain an antioxidant (antiaging agent). The use of an antioxidant can improve the weather resistance of the cured product. Examples of the antioxidant include hindered phenol compounds, monophenol compounds, bisphenol compounds, and polyphenol compounds, and hindered phenol compounds are particularly preferred. Examples of the antioxidant include Irganox 245, Irganox 1010, Irganox 1035, Irganox 1076, Irganox 1135, Irganox 1330, Irganox 1520 (all manufactured by BASF); SONGNOX 1076 (manufactured by SONGWON), and BHT. Hindered amine light stabilizers such as TINUVIN 622LD, TINUVIN 144, TINUVIN 292, CHIMASSORB944LD, CHIMASSORB119FL (all manufactured by BASF); ADK STAB LA-57, ADK STAB LA-62, ADK STAB LA-67, ADK STAB LA-63, ADK STAB LA-68 (all manufactured by ADEKA Corporation); SANOL LS-2626, SANOL LS-1114, SANOL LS-744 (all manufactured by Sankyo Lifetech Co., Ltd.); and NOCRAC CD (manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) can also be used. Other antioxidants that can be used include SONGNOX4120, Naugard 445, and OKABEST CLX050. Specific examples of antioxidants are also described in JP-A-4-283259 and JP-A-9-194731. The amount of the antioxidant used is preferably from 0.1 to 10 parts by weight, and more preferably from 0.2 to 5 parts by weight, based on 100 parts by weight of the polymer (A).

[0105] (Light stabilizer) The curable composition may contain a light stabilizer. The use of a light stabilizer can prevent photo-oxidative deterioration of the cured product. Examples of the light stabilizer include benzotriazole-based compounds, hindered amine-based compounds, and benzoate-based compounds. As the light stabilizer, a hindered amine-based compound is particularly preferred. The amount of the light stabilizer used is preferably from 0.1 to 10 parts by weight, and more preferably from 0.2 to 5 parts by weight, based on 100 parts by weight of the polymer (A). Specific examples of light stabilizers are described in, for example, JP-A-9-194731.

[0106] When a photocurable substance is blended in the curable composition, particularly when an unsaturated acrylic compound is used, it is preferable to use a tertiary amine-containing hindered amine light stabilizer as the hindered amine light stabilizer in order to improve the storage stability of the curable composition, as described in JP-A-5-70531. Tertiary amine-containing hindered amine light stabilizers include TINUVIN 123, TINUVIN 144, TINUVIN 249, TINUVIN 292, TINUVIN 312, TINUVIN 622LD, TINUVIN 765, TINUVIN 770, TINUVIN 880, TINUVIN 5866, TINUVIN B97, CHIMASSORB119FL, and CHIMASSORB944LD (all manufactured by BASF); ADK STAB LA-57, LA-62, LA-63, LA-67, and LA-68 (all manufactured by ADEKA Corporation); SANOL LS-292, LS-2626, LS-765, LS-744, and LS-1114 (all manufactured by Sankyo Lifetech Co., Ltd.), SABOSTAB UV91, SABOSTAB UV119, SONGSORB CS5100, SONGSORB CS622, and SONGSORB Examples include CS944 (all manufactured by SONGWON), Nocrac CD (manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), etc.

[0107] (UV absorber) The curable composition may contain an ultraviolet absorber. Use of an ultraviolet absorber can improve the surface weather resistance of the cured product. Examples of ultraviolet absorbers include benzophenone compounds, benzotriazole compounds, salicylate compounds, triazine compounds, substituted tolyl compounds, and metal chelate compounds. Among these, benzotriazole compounds are particularly preferred. Specific examples of benzotriazole compounds include Tinuvin 234, Tinuvin 326, Tinuvin 327, Tinuvin 328, Tinuvin 329, Tinuvin 350, Tinuvin 571, Tinuvin 900, Tinuvin 928, Tinuvin 1130, and Tinuvin 1600 (all manufactured by BASF); and SONGSORB 3290 (manufactured by SONGWON). Specific examples of triazine compounds include TINUVIN 400, TINUVIN 405, TINUVIN 477, and TINUVIN 1577ED (all manufactured by BASF); SONGSORB CS400 and SONGSORB 1577 (manufactured by SONGWON). Specific examples of benzophenone compounds include SONGSORB 8100 (manufactured by SONGWON). The amount of the ultraviolet absorber used is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, based on 100 parts by weight of the polymer (A). It is preferable to use a phenol-based antioxidant or a hindered phenol-based antioxidant in combination with a hindered amine-based light stabilizer and a benzotriazole-based ultraviolet absorber. Addworks IBC760 (Clariant) can be used as a product containing a mixture of antioxidants, light stabilizers, and UV absorbers.

[0108] (Physical property adjuster) The curable composition may contain a physical property adjuster to adjust the tensile properties of the cured product as necessary. The physical property adjuster is not particularly limited. Examples of the physical property adjuster include alkyl alkoxysilanes such as methyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, and n-propyltrimethoxysilane; alkyl isopropenoxysilanes such as dimethyldiisopropenoxysilane, methyltriisopropenoxysilane, and γ-glycidoxypropylmethyldiisopropenoxysilane; alkoxysilanes having functional groups such as γ-glycidoxypropylmethyldimethoxysilane, γ-glycidoxypropyltrimethoxysilane, vinyltrimethoxysilane, vinyldimethylmethoxysilane, γ-aminopropyltrimethoxysilane, N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane, γ-mercaptopropyltrimethoxysilane, and γ-mercaptopropylmethyldimethoxysilane; silicone varnishes; and polysiloxanes. The physical property modifier can be used to increase the hardness of the cured product, or conversely, to decrease the hardness of the cured product and provide breaking elongation. The physical property modifiers may be used alone or in combination of two or more kinds.

[0109] In particular, compounds that generate a compound having a monovalent silanol group in the molecule by hydrolysis have the effect of reducing the modulus of the cured product without worsening the stickiness of the surface of the cured product. Compounds that generate a compound having a monovalent silanol group in the molecule by hydrolysis are particularly preferred, and compounds that generate trimethylsilanol are particularly preferred. Compounds that generate a compound having a monovalent silanol group in the molecule by hydrolysis include compounds described in JP-A-5-117521. In addition, derivatives of alkyl alcohols such as hexanol, octanol, and decanol that generate trialkylsilanols such as trimethylsilanol by hydrolysis, and derivatives of polyhydric alcohols having three or more hydroxyl groups such as trimethylolpropane, glycerin, pentaerythritol, or sorbitol that generate trialkylsilanols such as trimethylsilanol by hydrolysis, as described in JP-A-11-241029, can be mentioned. Examples of the derivatives include those of oxyalkylene polymers that produce silicon compounds that produce trialkylsilanols such as trimethylsilanol by hydrolysis, as described in JP-A-7-258534.Furthermore, polymers having crosslinkable hydrolyzable silicon-containing groups and silicon-containing groups that can become monosilanol-containing compounds by hydrolysis, as described in JP-A-6-279693, can also be used. The physical property adjusting agent is used in an amount of 0.1 to 20 parts by weight, preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the polymer (A).

[0110] (tackifier resin) The curable composition may contain a tackifier resin for the purpose of increasing the adhesiveness or adhesion of the cured product to a substrate, etc. The tackifier resin is not particularly limited, and any tackifier resin that is commonly used in various curable compositions can be used. Specific examples of tackifier resins include terpene resins, aromatic modified terpene resins, hydrogenated terpene resins, terpene-phenol resins, phenol resins, modified phenol resins, xylene-phenol resins, cyclopentadiene-phenol resins, coumarone-indene resins, rosin resins, rosin ester resins, hydrogenated rosin ester resins, xylene resins, low molecular weight polystyrene resins, styrene copolymer resins, styrene block copolymers, hydrogenated styrene block copolymers, petroleum resins, hydrogenated petroleum resins, and DCPD resins. Examples of petroleum resins include C5 hydrocarbon resins, C9 hydrocarbon resins, and C5C9 hydrocarbon copolymer resins. These may be used alone or in combination of two or more. The amount of the tackifier resin used is preferably 2 to 100 parts by weight, more preferably 5 to 50 parts by weight, and even more preferably 5 to 30 parts by weight, based on 100 parts by weight of the polymer (A). By using the tackifier resin in an amount within this range, a cured product having good adhesion and adhesion to the substrate can be formed. The curable composition has an appropriate viscosity, and the handleability of the curable composition is good.

[0111] (Compounds containing epoxy groups) The curable composition may contain a compound containing an epoxy group. The use of a compound having an epoxy group can improve the restorability of the cured product. Examples of the compound having an epoxy group include epoxidized unsaturated fats and oils, epoxidized unsaturated fatty acid esters, alicyclic epoxy compounds, epichlorohydrin derivatives, and mixtures thereof. Specific examples of the compound having an epoxy group include epoxidized soybean oil, epoxidized linseed oil, bis(2-ethylhexyl)-4,5-epoxycyclohexane-1,2-dicarboxylate (E-PS), epoxy octyl stearate, and epoxy butyl stearate. The amount of the compound containing an epoxy group used is preferably 0.5 to 50 parts by weight based on 100 parts by weight of the polymer (A).

[0112] (Epoxy resin) The curable composition may contain an epoxy resin. The curable composition containing an epoxy resin is preferably used as an adhesive, particularly as an adhesive for exterior wall tiles. Examples of the epoxy resin include bisphenol A type epoxy resins and novolac type epoxy resins. The ratio of the weight of the polymer (A) to the weight of the epoxy resin is preferably in the range of 100 / 1 to 1 / 100, expressed as the weight ratio of (weight of the polymer (A)) / (weight of the epoxy resin). When the polymer (A) and the epoxy resin are used in the above ratio, a high-strength cured product having excellent impact strength and toughness is easily formed. When an epoxy resin is used, the curable composition may contain a curing agent together with the epoxy resin. The type of the curing agent is not particularly limited, and a commonly used curing agent may be used. The amount of the curing agent used is preferably 0.1 to 300 parts by weight based on 100 parts by weight of the epoxy resin.

[0113] (light curing substance) The curable composition may contain a photocurable substance. When a photocurable substance is used, a film of the photocurable substance is formed on the surface of the cured product, which improves the stickiness and weather resistance of the cured product. As photocurable substances, various compounds such as organic monomers, oligomers, and resins are known. In addition, many compositions containing photocurable substances are known. Representative photocurable substances include unsaturated acrylic compounds, polyvinyl cinnamates, and azido resins. As unsaturated acrylic compounds, monomers, oligomers, or mixtures thereof having one or more acrylic unsaturated groups or methacrylic unsaturated groups can be mentioned. The amount of the photocurable substance used is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the polymer (A). When the amount of the photocurable substance used falls within this range, it is easy to form a flexible cured product that has excellent weather resistance and is less susceptible to cracking.

[0114] (oxygen curing substance) The curable composition may contain an oxygen curing substance. Examples of the oxygen curing substance include unsaturated compounds that can react with oxygen in the air. When the curable substance contains an oxygen curing substance, the oxygen curing substance reacts with oxygen in the air to form a cured film near the surface of the cured product. By forming a cured film on the surface of the cured product, stickiness and adhesion of dirt and dust to the surface of the cured product can be prevented. Specific examples of the oxygen curing substance include drying oils such as tung oil and linseed oil; various alkyd resins obtained by modifying drying oils; acrylic polymers, epoxy resins, and silicone resins modified with drying oils; liquid polymers such as 1,2-polybutadiene, 1,4-polybutadiene, or C5-C8 diene polymers obtained by polymerizing or copolymerizing diene compounds such as butadiene, chloroprene, isoprene, or 1,3-pentadiene. These may be used alone or in combination of two or more. The amount of the oxygen curing substance used is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the polymer (A). When the oxygen curing substance is used in an amount within this range, the surface is less likely to be contaminated by dirt or dust, and a cured product having excellent mechanical properties such as tensile properties is easily formed. As described in JP-A-3-160053, the oxygen curing substance is preferably used in combination with a photocuring substance.

[0115] <Preparation of Curable Composition> The curable composition can be prepared as a one-component type in which all ingredients are mixed in advance, sealed, and stored, and then cured by moisture in the air after application. The hardener composition can also be prepared as a two-component type in which a hardener compounding material containing a curing catalyst (B), a collagenous calcium carbonate (C) surface-treated with a fatty acid, a filler, a plasticizer, water, and other ingredients is mixed with a composition containing a separately prepared organic polymer (A) before use. From the viewpoint of workability, the one-component type is preferred. When the curable composition is a one-component type, all the ingredients are mixed in advance, so that the ingredients containing water are preferably dehydrated and dried before use, or dehydrated by reducing pressure during mixing and kneading. In addition to the dehydration and drying method, the storage stability can be further improved by adding an alkoxysilane compound such as methyltrimethoxysilane, phenyltrimethoxysilane, n-propyltrimethoxysilane, vinyltrimethoxysilane, vinylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, γ-mercaptopropylmethyldiethoxysilane, and γ-glycidoxypropyltrimethoxysilane. As the dehydrating agent, a partially condensed silane compound such as Dynasylan 6490 from Evonik can also be used preferably from the viewpoint of safety and stability. The amount of the dehydrating agent, particularly the silicon compound capable of reacting with water such as vinyltrimethoxysilane, is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the polymer (A).

[0116] The curable composition can be used as a building sealant, industrial adhesive, waterproof coating film forming composition, adhesive raw material, etc. The curable composition can also be used as a sealant for buildings, ships, automobiles, roads, etc. Furthermore, the curable composition can adhere to a wide range of substrates such as glass, porcelain, wood, metal, and resin moldings, either alone or with the aid of a primer. Therefore, the curable composition can also be used as various types of sealing compositions and adhesive compositions. The curable composition can also be used as a contact adhesive in addition to ordinary adhesives. Furthermore, the curable composition is also useful as a food packaging material, a cast rubber material, a material for molding, and a paint. The cured product of the above curable composition exhibits low water absorption. Therefore, the above curable composition and its cured product are particularly suitable for use as waterproof materials such as sealing materials, waterproof adhesives, and waterproof coating films.

[0117] <Method of manufacturing the cured product> Prior to curing, the curable composition is formed into a desired shape by a method such as coating, casting, or filling.

[0118] The curable composition that has been applied, cast, or filled and shaped is cured under a desired environment, such as room temperature and room humidity.

[0119] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.

[0120] That is, one aspect of the present invention includes the following. <1> A curable composition comprising an organic polymer (A), a curing catalyst (B), and a colloidal calcium carbonate (C) surface-treated with a fatty acid, The organic polymer (A) is represented by the following formula (1): -SiX3(1) (In formula (1), X is a hydroxyl group or a hydrolyzable group, and the three Xs may be the same or different.) and having a reactive silicon group represented by the formula: The curing catalyst (B) contains a titanium compound (b1) and an ammonium fluoride compound (b2); The titanium compound (b1) is represented by the following formula (2): Ti(OR 1 ) d Y 4-d (2) (In formula (2), R 1 represents a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, Y represents a chelate coordination compound, and d represents an integer of 0 to 4. A compound represented by the formula: The ammonium fluoride compound (b2) is represented by the following formula (3): [ka] (In formula (3), R 2 , R 3 , R 4 , and R 5 is a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, R 2 , R 3 , R 4 , and R 5 may be the same or different.) and a curable composition comprising a compound represented by the formula: <2> A reaction product of a titanium compound (b1) and an ammonium fluoride compound (b2) is included. <1> The curable composition according to claim 1. <3> a weight ratio (b1 / b2) of the component derived from the titanium compound (b1) to the component derived from the ammonium fluoride compound (b2) is 5 to 0.1; <1> or <2> The curable composition according to claim 1. <4> The main chain structure of the organic polymer (A) contains a polyoxyalkylene polymer. <3> The curable composition according to claim 1. <5> <1> ~ <4> 2. A cured product obtained by curing the curable composition according to claim 1. EXAMPLES

[0121] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0122] <Preparation Example of Organic Polymer (A)> Hereinafter, the number average molecular weight is a GPC molecular weight measured under the following conditions. Liquid delivery system: Tosoh HLC-8120GPC Column: Tosoh TSK-GEL H type Solvent: THF (tetrahydrofuran) Molecular weight: Polystyrene equivalent Measurement temperature: 40℃

[0123] The end group calculated molecular weight in the examples is a molecular weight calculated by taking into consideration the structure of the organic polymer, determining the hydroxyl value according to the measurement method of JIS K 1557 and the iodine value according to the measurement method of JIS K 0070. The organic polymer structure was considered to be the degree of branching determined by the polymerization initiator used.

[0124] The average number of reactive silicon groups per terminal of the organic polymer shown in the examples is 1 Calculation was performed by H-NMR (measured in CDCl3 solvent using AVANCE III HD-500 manufactured by Bruker).

[0125] (Preparation example 1: Organic polymer (A-1)) Using polyoxypropylene diol with a molecular weight of about 2,000 as an initiator, propylene oxide was polymerized in the presence of zinc hexacyanocobaltate glyme complex catalyst to obtain hydroxyl-terminated polyoxypropylene with a number average molecular weight of 28,500.

[0126] A methanol solution of 1.2 molar equivalents of NaOMe was added to the hydroxyl groups of the obtained hydroxyl-terminated polyoxypropylene. After distilling off the methanol from the reaction solution, allyl chloride was further added to the reaction solution to convert the terminal hydroxyl groups to allyl groups. Unreacted allyl chloride was removed by volatilization under reduced pressure. 100 parts by weight of the obtained unpurified allyl-terminated polyoxypropylene were mixed with 300 parts by weight of n-hexane and 300 parts by weight of water, and then stirred. Next, the mixture was separated into an aqueous phase and a hexane phase by centrifugation, and the aqueous phase was removed. 300 parts by weight of water was mixed again with the obtained hexane phase, and then stirred. Next, the mixture was separated into an aqueous phase and a hexane phase by centrifugation, and the aqueous phase was removed. Then, hexane was removed from the recovered hexane phase by devolatilization under reduced pressure. As a result of the above, a bifunctional polyoxypropylene was obtained, which has an allyl group at the end and a number average molecular weight of about 28,500 in terms of polystyrene measured by GPC.

[0127] To 100 parts by weight of the obtained allyl-terminated polyoxypropylene, 150 ppm of an isopropanol solution of platinum vinyldisiloxane complex with a platinum content of 3 wt% was added as a catalyst. Next, 0.8 molar equivalents of trimethoxysilane were added to the allyl group of the allyl-terminated polyoxypropylene, and the allyl end and trimethoxysilane were reacted at 90°C for 5 hours to obtain a trimethoxysilyl-terminated polyoxypropylene polymer (A-1). The number of trimethoxysilyl groups per polymer chain end was about 0.8.

[0128] (Preparation example 2: Organic polymer (A-2)) Using polyoxypropylene glycol with a molecular weight of about 4,500 as an initiator, propylene oxide was polymerized in the presence of zinc hexacyanocobaltate glyme complex catalyst to obtain polyoxypropylene with a number average molecular weight of 27,900 and hydroxyl groups at both ends.

[0129] To 100 parts by weight of the obtained polyoxypropylene having hydroxyl groups at both ends, 30 ppm of bismuth (III) 2-ethylhexanoate (Bi: 25%) solution was added. Next, 0.95 molar equivalents of (3-isocyanatopropyl)trimethoxysilane was added to the hydroxyl groups of the polyoxypropylene having hydroxyl groups at both ends, and a urethane reaction was carried out on the hydroxyl groups. As a result, a linear silyl-containing polyoxypropylene (A-2) without branch points was obtained. The number of trimethoxysilyl groups was about 0.9 per polymer chain end.

[0130] (Preparation example 3: Organic polymer (A-3)) A 1 / 1 (weight ratio) mixture of polyoxypropylene diol with a molecular weight of approximately 2,000 and polyoxypropylene triol with a molecular weight of 3,000 was used as an initiator, and propylene oxide was polymerized using a zinc hexacyanocobaltate glyme complex catalyst to obtain hydroxyl-terminated polyoxypropylene with a number average molecular weight of approximately 19,000.

[0131] A methanol solution of 1.2 molar equivalents of NaOMe was added to the hydroxyl groups of the obtained hydroxyl-terminated polyoxypropylene. After distilling off the methanol from the reaction solution, allyl chloride was further added to the reaction solution to convert the terminal hydroxyl groups to allyl groups. As a result, allyl-terminated polyoxypropylene with a number average molecular weight of about 19,000 and allyl groups at the terminals was obtained.

[0132] 100 parts by weight of the obtained unpurified allyl-terminated polyoxypropylene were mixed with 300 parts by weight of n-hexane and 300 parts by weight of water, and then stirred. Next, the mixture was separated into an aqueous phase and a hexane phase by centrifugation, and the aqueous phase was removed. 300 parts by weight of water was mixed again with the obtained hexane phase, and then stirred. Next, the mixture was separated into an aqueous phase and a hexane phase by centrifugation, and the aqueous phase was removed. Then, hexane was removed from the recovered hexane phase by devolatilization under reduced pressure. Thus, a purified allyl-terminated polyoxypropylene was obtained. 150 ppm of an isopropanol solution of a platinum vinyldisiloxane complex with a platinum content of 3 wt% was added as a catalyst to 100 parts by weight of the obtained allyl-terminated polyoxypropylene. Next, 0.7 molar equivalents of methyldimethoxysilane was added to the allyl group of the allyl-terminated polyoxypropylene, and the allyl end was reacted with methyldimethoxysilane at 90°C for 5 hours to obtain methyldimethoxysilyl-terminated polyoxypropylene (A-3). The number of methyldimethoxysilyl groups per polymer chain end was about 0.7.

[0133] <Synthesis example of curing catalyst (B)> (Synthesis Example 1: Complex 1) In a 200 mL eggplant flask, 10 g of TC-750 (bis(ethylacetoacetate)diisopropoxytitanium), manufactured by Matsumoto Fine Chemical Co., Ltd.) was added. While stirring the contents of the flask, 10 g of TBAF (tetrabutylammonium fluoride-tetrahydrofuran solution (approximately 1.0 M), manufactured by Fuji Film Wako Pure Chemical Co., Ltd.) was slowly dripped into the flask. After the dripping was completed, the contents of the flask were stirred at room temperature for 2 hours. Then, the mixture was concentrated under reduced pressure to distill off the tetrahydrofuran, and a red concentrated liquid complex 1 was obtained.

[0134] (Synthesis Example 2: Complex 2) A red concentrate complex 2 was obtained in the same manner as in Synthesis Example 1, except that 20 g of TBAF was used.

[0135] (Synthesis Example 3: Complex 3) A red concentrate complex 3 was obtained in the same manner as in Synthesis Example 1, except that 25 g of TBAF was used.

[0136] (Synthesis Example 4: Complex 4) A red concentrate complex 4 was obtained in the same manner as in Synthesis Example 1, except that 30 g of TBAF was used.

[0137] (Synthesis Example 5: Complex 5) A red concentrate complex 5 was obtained in the same manner as in Synthesis Example 1, except that 40 g of TBAF was used.

[0138] (Synthesis Example 6: Complex 6) A red concentrate complex 6 was obtained in the same manner as in Synthesis Example 1, except that 50 g of TBAF was used.

[0139] (Synthesis Example 7: Complex 7) In a 200 mL eggplant flask, 10 g of Tyzor KE-6 (bis(ethylacetoacetate)diisobutoxytitanium), manufactured by Dorff-Ketal) was added. While stirring the contents of the flask, 25 g of TBAF (tetrabutylammonium fluoride-tetrahydrofuran solution (approximately 1.0 M), manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was slowly dripped into the flask. After the dripping was completed, the contents of the flask were stirred at room temperature for 2 hours. The mixture was then concentrated under reduced pressure to distill off the tetrahydrofuran, yielding a red concentrated liquid complex 7.

[0140] (Method of producing curable composition) (Examples 1 to 5 and Comparative Examples 1 to 9) According to the composition (weight ratio) shown in Table 1, colloidal calcium carbonate, heavy calcium carbonate, plasticizer, pigment, thixotropy imparting agent, antioxidant, UV absorber, and light stabilizer were added to the organic polymer (A) and mixed with a spatula. The resulting mixture was dispersed by passing it through a triple paint roll (manufactured by Kodaira Seisakusho Co., Ltd.) three times, and then dehydrated under reduced pressure using a planetary mixer. The dehydrated material was filled into a cartridge, which is a moisture-proof container, to obtain the base material.

[0141] Under an atmosphere of 23°C and 50% relative humidity, an adhesion promoter and a dehydrating agent were added to and mixed with the base resin extruded from the obtained cartridge according to the composition (weight ratio) shown in Table 1. Then, the curing catalyst (B) was added and mixed to obtain a curable composition.

[0142] The components in Table 1 are as follows: Organic polymer (A) ((A-1) (organic polymer (A-1) obtained in Preparation Example 1), (A-2) (organic polymer (A-2) obtained in Preparation Example 2), (A-3) (organic polymer (A-3) obtained in Preparation Example 3)) Colloidal calcium carbonate (product name: Hakuenka CCR (colloidal calcium carbonate surface-treated with fatty acid), manufactured by Shiraishi Kogyo Co., Ltd.) Heavy calcium carbonate (product name: Whiten SB, manufactured by Bihoku Funka Kogyo Co., Ltd.) Plasticizer (product name: Hexamoll DINCH, manufactured by BASF) Pigment (product name: Typak R820, manufactured by Ishihara Sangyo Kaisha, Ltd.) Thixotropic agent (product name: Crayvallc SLT, manufactured by ARKEMA) Antioxidant (product name: Irganox1010, manufactured by BASF) UV absorber (product name: Tinuvin 326, manufactured by BASF) Light stabilizer (product name: Tinuvin 770, manufactured by BASF) Adhesion promoter (product name: Dynasylan AMMO (γ-aminopropyltrimethoxysilane), manufactured by Evonik) Dehydrating agent (product name: DynasylanVTMO (vinyltrimethoxysilane), manufactured by Evonik) Titanium compounds (b1) ((Ti(O i Pr)4 (tetraisopropoxytitanium), manufactured by Tokyo Chemical Industry Co., Ltd.), (trade name: Tyzor 9000 (tetra tert-butoxytitanium), manufactured by Dorff-Ketal), (trade name: Tyzor KE-6 (bis(ethylacetoacetate)diisobutoxytitanium), manufactured by Dorff-Ketal), (trade name: TC-750 (bis(ethylacetoacetate)diisopropoxytitanium), manufactured by Matsumoto Fine Chemical Co., Ltd.) Other metal compounds (b1') ((Al(O S Bu)3 (aluminum sec-butoxide), manufactured by Tokyo Chemical Industry Co., Ltd.), Trade name: ZC-580 (zirconium dibutoxybis(ethylacetoacetate), manufactured by Matsumoto Finechem Co., Ltd.), B(OEt)3 (triethyl borate), manufactured by Tokyo Chemical Industry Co., Ltd.) Ammonium fluoride compound (b2) (TBAF (tetrabutylammonium fluoride-tetrahydrofuran solution (approximately 1.0 M), Fujifilm Wako Pure Chemical Industries, Ltd.) Other ammonium fluoride compounds (b2') (TBAC (tetrabutylammonium chloride, manufactured by Tokyo Chemical Industry Co., Ltd.), TBAB (tetrabutylammonium bromide, manufactured by Tokyo Chemical Industry Co., Ltd.), TBAI (tetrabutylammonium iodide, manufactured by Tokyo Chemical Industry Co., Ltd.))

[0143] (Skinning time (hardening evaluation)) The curable composition was filled into a mold about 5 mm thick in an atmosphere of 23°C and 50% relative humidity, and the surface of the curable composition was smoothed to a flat surface. The time when the surface was smoothed to a flat surface was determined as the curing start time. The curable composition in the mold was touched with a spatula, and the time when the mixture no longer adhered to the spatula was determined as the skinning time, and the curing time (curability) was measured. The measurement results are shown in Table 1.

[0144] [Table 1]

[0145] From the measurement results in Table 1, a comparison between Examples 1 to 4 and Comparative Examples 1 to 8 shows that a curable composition containing a titanium compound (b1) and an ammonium fluoride compound (b2) cures faster than a curable composition not containing either one of the titanium compound (b1) and the ammonium fluoride compound (b2). Also, a comparison between Examples 1 and 5 and Comparative Example 1 shows that a curable composition containing an organic polymer (A-1) or (A-2) having a reactive silicon group represented by the above formula (1) cures faster than a curable composition containing an organic polymer (A-3) not having a reactive silicon group represented by the above formula (1).

[0146] (Examples 6 to 12) Colloidal calcium carbonate, heavy calcium carbonate, plasticizer, pigment, thixotropy imparting agent, antioxidant, UV absorber, and light stabilizer were added to the organic polymer (A) and mixed with a spatula according to the composition (weight ratio) shown in Table 2. The resulting mixture was dispersed by passing it through a triple paint roll (manufactured by Kodaira Seisakusho Co., Ltd.) three times, and then dehydrated under reduced pressure using a planetary mixer to obtain the base resin. After the base material was cooled to 50°C or less, the adhesion promoter and the dehydrating agent were added and mixed to the base material according to the composition (weight ratio) shown in Table 2. Next, the curing catalyst (B) was added and mixed to obtain a curable composition.

[0147] The components in Table 2 are as follows: Organic Polymer (A) ((A-1) (Organic Polymer (A-1) Obtained in Preparation Example 1) Colloidal calcium carbonate (product name: Hakuenka CCR (colloidal calcium carbonate surface-treated with fatty acid), manufactured by Shiraishi Kogyo Co., Ltd.) Heavy calcium carbonate (product name: Whiten SB, manufactured by Bihoku Funka Kogyo Co., Ltd.) Plasticizer (product name: Hexamoll DINCH, manufactured by BASF) Pigment (product name: Typak R820, manufactured by Ishihara Sangyo Kaisha, Ltd.) Thixotropic agent (product name: Crayvallc SLT, manufactured by ARKEMA) Antioxidant (product name: Irganox1010, manufactured by BASF) UV absorber (product name: Tinuvin 326, manufactured by BASF) Light stabilizer (product name: Tinuvin 770, manufactured by BASF) Adhesion promoter (product name: Dynasylan AMMO (γ-aminopropyltrimethoxysilane), manufactured by Evonik) Dehydrating agent (product name: DynasylanVTMO (vinyltrimethoxysilane), manufactured by Evonik) Complex 1 (Complex 1 obtained in Synthesis Example 1) Complex 2 (Complex 2 obtained in Synthesis Example 2) Complex 3 (Complex 3 obtained in Synthesis Example 3) Complex 4 (Complex 4 obtained in Synthesis Example 4) Complex 5 (Complex 5 obtained in Synthesis Example 5) Complex 6 (Complex 6 obtained in Synthesis Example 6) Complex 7 (Complex 7 obtained in Synthesis Example 7)

[0148] (Skinning time (hardening evaluation)) The curing time (curability) was measured in the same manner as in Examples 1 to 5 and Comparative Examples 1 to 9. The measurement results are shown in Table 2.

[0149] [Table 2]

[0150] The measurement results in Table 2 show that all of the curable compositions containing the complex obtained from the titanium compound (b1) and the ammonium fluoride compound (b2) as the curing catalyst (B) exhibit good curability.

Claims

1. A curable composition comprising an organic polymer (A), a curing catalyst (B), and a colloidal calcium carbonate (C) surface-treated with a fatty acid, The organic polymer (A) is represented by the following formula (1): -SiX 3 (1) (In formula (1), X is a hydroxyl group or a hydrolyzable group, and the three Xs may be the same or different.) and having a reactive silicon group represented by the formula: The curing catalyst (B) contains a titanium compound (b1) and an ammonium fluoride compound (b2), The titanium compound (b1) is represented by the following formula (2): Ti(OR 1 ) d Y 4-d (2) (In formula (2), R 1 is a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, Y is a chelate coordination compound, and d is an integer of 0 to 4. and a compound represented by the formula: The ammonium fluoride compound (b2) is represented by the following formula (3): [Formula 1] (In formula (3), R 2 , R 3 , R 4 , and R 5 is a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, R 2 , R 3 , R 4 , and R 5 may be the same or different.) and a curable composition comprising a compound represented by the formula:

2. The curable composition according to claim 1, comprising a reaction product of the titanium compound (b1) and the ammonium fluoride compound (b2).

3. The curable composition according to claim 1 or 2, wherein the weight ratio (b1 / b2) of the component derived from the titanium compound (b1) to the component derived from the ammonium fluoride compound (b2) is 5 to 0.

1.

4. The curable composition according to claim 3 , wherein the main chain structure of the organic polymer (A) contains a polyoxyalkylene polymer.

5. A cured product obtained by curing the curable composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Curable composition and catalyst composition

    JP2013028819A