Method for producing cerium oxide, cerium oxide and dispersion of the same

By preparing reduced cerium oxide particles and acid-treating their surfaces, the method addresses the issue of poor dispersibility in nonpolar solvents, achieving transparent dispersions of cerium oxide.

JP2024157220APending Publication Date: 2024-11-07M TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023071448
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Existing methods for producing cerium oxide nanoparticles in nonpolar solvents require complex surface treatment agents or operations, leading to impurities and poor dispersibility.

Method used

The method involves preparing reduced cerium oxide particles with an average oxidation number of 3 or more and less than 4, followed by acid-treating the surface to improve dispersibility, using hydrazine as a reducing agent and carboxylic or nitric acid for the acid treatment.

Benefits of technology

This approach enables the production of cerium oxide particles with good dispersibility in solvents and resins without complex surface treatments, resulting in transparent dispersions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157220000004
    Figure 2024157220000004
  • Figure 2024157220000005
    Figure 2024157220000005
  • Figure 2024157220000006
    Figure 2024157220000006
Patent Text Reader

Abstract

To provide a method for producing cerium oxide particles having good dispersibility to a solvent, a dispersant or a resin by a simple surface treatment without using a complicated surface treatment agent or treatment operation.SOLUTION: A method for producing acid-treated cerium oxide particles comprises a step of preparing reduced cerium oxide particles having an average value of oxidation number of cerium element of 3 or greater and less than 4, and a step of acid-treating the surface of the reduced cerium oxide particles.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing cerium oxide, cerium oxide, and a dispersion thereof. [Background technology]

[0002] Cerium oxide (IV) is a type of oxide with the chemical composition CeO2, and has long been used widely as a CMP (Chemical Mechanical Polishing) slurry for polishing glass and semiconductors. In terms of physical properties, it has ultraviolet absorption capabilities and high oxygen storage and release capabilities, and due to its unique properties, in recent years it has been used not only as an abrasive, but also in new applications such as ultraviolet absorbers for cosmetics, high refractive index materials, solid electrolytes for fuel cells, and catalyst carriers for decomposing automobile exhaust gases.

[0003] However, little is known about the dispersion of cerium oxide nanoparticles in non-polar solvents, and the dispersions that have been reported have had problems such as requiring complicated treatment or containing impurities.

[0004] Patent Document 1 discloses a method for producing cerium (IV) oxide nanoparticles that have excellent dispersibility in a wide range of solvents and monomers. Specifically, cerium (IV) oxide containing a carboxylic acid is obtained by hydrothermal synthesis using a basic aqueous solution containing cerium (IV) ions and a carboxylic acid. In this case, the particles contain a large amount of carboxylic acid, 20 to 30% by weight, and a long-chain carboxylic acid is required.

[0005] Patent Document 2 discloses a surface-modified core-shell nanoparticle in which a spherical monodisperse core-shell cerium oxide polymer hybrid nanoparticle, in which a core portion is made of secondary particles formed by spherically assembling primary particles of cerium oxide, and a polymer layer is present on the surface of the secondary particles as a shell portion, is surface-modified with a silane coupling agent or the like. Specifically, particles obtained by heating cerium (III) ions and polyvinylpyrrolidone in ethylene glycol are treated with acetic acid and then treated with silane. In this case, the dispersion naturally contains polyvinylhydridone, which is an additive, and silane, which is a surface treatment agent, as impurities. In addition, the surface-modified core-shell nanoparticle in Patent Document 2 is a multi-component composite, and is different from cerium oxide particles.

[0006] As described above, in the conventional techniques, various complicated surface treatment agents or treatment procedures are required to obtain a dispersion of cerium oxide particles. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2018-145057 A [Patent Document 2] JP 2017-20020 A Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a method for producing cerium oxide particles having good dispersibility in solvents, dispersants, resins, etc., by a simple surface treatment without using various complicated surface treatment agents or treatment operations required in the prior art, and further to provide cerium oxide particles and a dispersion of well-dispersed cerium oxide particles. [Means for solving the problem]

[0009] The inventors believed that the reason why the above problems occur in dispersions of cerium oxide nanoparticles is because the surface of metal oxides containing cerium (IV) oxide is covered with hydroxyl groups, and thought that dispersibility could be improved by appropriately treating or modifying the surface. As a result of intensive research aimed at solving the above problems, the present inventors unexpectedly found that cerium oxide particles having good dispersibility in solvents, dispersants, resins, etc. could be obtained by a simple surface treatment of simply subjecting reduced cerium oxide particles, in which the average oxidation number of cerium element is 3 or more and less than 4, to an acid treatment, and thus completed the present invention. That is, the present invention is as follows.

[0010] [1] preparing reduced cerium oxide particles having an average oxidation number of cerium element of 3 or more and less than 4; and A step of treating the surface of the reduced cerium oxide particles with an acid. A method for producing acid-treated cerium oxide particles, comprising: [2] The method according to [1], wherein in the step of preparing reduced cerium oxide particles, the reduced cerium oxide particles are prepared by reducing a raw material cerium oxide. [3] The method according to [1], wherein in the step of preparing reduced cerium oxide particles, the reduced cerium oxide particles are prepared by reducing raw material cerium oxide with a reducing agent. [4] The method of claim 3, wherein the reducing agent is hydrazine. [5] The method according to any one of [1] to [4], wherein the acid used in the acid treatment step is a carboxylic acid or nitric acid. [6] The method according to any one of [1] to [5], wherein the acid-treated cerium oxide particles have a particle size of 1 nm to 100 nm. [7] Producing acid-treated cerium oxide particles by the method described in [1] to [6]; The method for producing a dispersion of acid-treated cerium oxide particles includes dispersing the obtained acid-treated cerium oxide particles in a dispersion medium containing at least one of a solvent, a dispersant, and a resin.

[0011] [8] In the infrared absorption spectrum converted to absorbance, -1 ~500cm -1 When the maximum absorbance of is 1, the -1 Cerium oxide particles having an absorbance of less than 0.490. [9] In the infrared absorption spectrum converted to absorbance, -1 ~500cm -1 When the maximum absorbance of -1 The absorbance at 610 cm is greater than 0.191. -1 Cerium oxide particles having an absorbance of greater than 0.264.

[10] In the infrared absorption spectrum converted to absorbance, the peak at 320 cm -1 The sum of the peak areas with centers on the lower wavenumber side is 1000 cm -1 ~50cm -1 Cerium oxide particles, wherein the ratio of the sum of all peak areas in the range is less than 23.0%.

[11] In the infrared absorption spectrum converted to absorbance, the peak at 700 cm -1 ~600cm -1 The sum of the peak areas centered at 1000 cm -1 ~50cm -1 Cerium oxide particles, the proportion of which in the range of the sum of all peak areas is higher than 4.7%.

[0012]

[12] Cerium oxide particles that have an absorbance at 650 nm of greater than 0.055 when the absorbance at 200 nm is set to 1 in an absorbance-converted ultraviolet-visible-near infrared reflectance spectrum.

[13] Cerium oxide particles in which the sum of the peak areas centered on the wavelength side longer than 550 nm in an ultraviolet-visible-near-infrared reflectance spectrum converted into absorbance is greater than 4.3% of the sum of all peak areas in the range of 190 nm to 1,200 nm.

[14] Cerium oxide particles according to any one of [8] to

[13] , having an average particle diameter of 1 nm to 100 nm.

[15] A dispersion of cerium oxide particles, comprising the cerium oxide particles according to any one of [8] to

[14] in a dispersion medium containing at least one of a solvent, a dispersant, and a resin. Effect of the Invention

[0013] According to the present invention, cerium oxide particles having good dispersibility in solvents, dispersants, resins, etc. can be produced by simple surface treatment without using various complicated surface treatment agents or treatment operations required in the prior art. Furthermore, cerium oxide particles and a dispersion of well-dispersed cerium oxide particles are provided. [Brief description of the drawings]

[0014] [Figure 1] 1 is a TEM photograph of the acid-treated cerium oxide particles of Example 1. [Diagram 2] 1 shows absorbance conversion results of IR measurement of the cerium (IV) oxide particles (untreated) of Reference Example 1 and the acid-treated cerium oxide particles of Example 1. [Diagram 3] FIG. 3 is an enlarged view of 1800 to 1200 cm −1 of the IR measurement results shown in FIG. [Figure 4] FIG. 3 is an enlarged view of the IR measurement results shown in FIG. 2 from 3800 to 2400 cm −1 . [Diagram 5] 1 shows absorbance conversion results of IR measurement of a commercially available reagent, the cerium (IV) oxide particles (untreated) of Reference Example 1, the acid-treated cerium oxide particles of Example 1, and the cerium oxide particles of Comparative Example 1. [Figure 6] 1 shows the absorbance conversion and waveform separation results of the IR measurement results of the acid-treated cerium oxide particles of Example 1. [Figure 7] 1 shows absorbance conversion and waveform separation results of IR measurement results of the cerium oxide particles of Comparative Example 1. [Figure 8] 1 shows the results of UV-vis-NIR measurement of the cerium (IV) oxide particles (untreated) of Reference Example 1, the acid-treated cerium oxide particles of Example 1, and the cerium oxide particles of Comparative Example 1. [Figure 9]1 shows the results of UV-vis-NIR measurement and waveform separation of the acid-treated cerium oxide particles of Example 1. [Figure 10] 1 shows the results of UV-vis-NIR measurement and waveform separation of the cerium oxide particles of Comparative Example 1. [Figure 11] 1 shows absorbance conversion results of diffuse reflectance measurement of the purple wet cake, the pale yellow wet cake, and the wet cake containing reduced cerium oxide particles in Reference Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] An embodiment of the present invention will be described below. 1. Manufacturing method of acid-treated cerium oxide particles The manufacturing method of the present invention is a method for producing acid-treated cerium oxide particles, which includes the steps of preparing reduced cerium oxide particles in which the average oxidation number of cerium element is 3 or more and less than 4, and treating the surfaces of the reduced cerium oxide particles with an acid.

[0016] (Acid-treated cerium oxide particles) The acid-treated cerium oxide particles (hereinafter, sometimes simply referred to as cerium oxide particles) produced by the production method of the present invention are not particularly limited in shape and size. For example, nanoparticles and microparticles are exemplified, but ceramic materials carrying acid-treated cerium oxide particles may also be used. When the purpose is to obtain a dispersion liquid, it is preferable to use nanoparticles. The average particle size of the acid-treated cerium oxide particles produced by the production method of the present invention is preferably 1 nm to 100 nm, more preferably 1 nm to 50 nm, even more preferably 1 nm to 20 nm, and even more preferably 1 nm to 10 nm, in order to ensure the transparency of the dispersion liquid of acid-treated cerium oxide. In the present invention, the particle size refers to the arithmetic mean value of the shortest diameter and the longest diameter of the particles obtained by TEM observation.

[0017] The acid-treated cerium oxide is preferably cerium (IV) oxide, and examples of the acid-treated cerium oxide include cerium (IV) oxide that has been oxidized in air. Furthermore, the cerium oxide in the present invention may be a complex with a substance other than cerium oxide. Examples include cerium oxide carrying a metal such as gold, platinum, or palladium, and a complex with an oxide such as zinc oxide, titanium oxide, zirconium oxide, or silicon oxide. It may also be a mixture with other cerium compounds such as cerium hydroxide or cerium carbonate.

[0018] The acid-treated cerium oxide particles produced by the production method of the present invention preferably have an absorbance-converted infrared absorption spectrum of 400 cm -1 ~500cm -1 When the maximum absorbance of is 1, the -1 Preferably, the absorbance at 400 cm in the infrared absorption spectrum converted into absorbance is less than 0.490. -1 ~500cm -1 When the maximum absorbance of -1 The absorbance at 610 cm is greater than 0.191. -1 Preferably, the absorbance at 320 cm is greater than 0.264 when peak separation is performed in the infrared absorption spectrum converted into absorbance. -1 The sum of the peak areas with centers on the lower wavenumber side is 1000 cm -1 ~50cm -1 In addition, preferably, the ratio of the sum of the peak areas in the range of 700 cm to the sum of the total peak areas in the range of 700 cm to the sum of the total peak areas in the infrared absorption spectrum converted into absorbance is lower than 23.0%. -1 ~600cm -1 The sum of the peak areas centered at 1000 cm -1 ~50cm -1 The proportion of the sum of all peak areas in this range is higher than 4.7%.

[0019] The acid-treated cerium oxide particles produced by the production method of the present invention preferably have, in an absorbance-converted ultraviolet-visible-near-infrared reflectance spectrum, an absorbance at 650 nm of greater than 0.055 when the absorbance at 200 nm is taken as 1. Also preferably, in an absorbance-converted ultraviolet-visible-near-infrared reflectance spectrum, the proportion of the sum of peak areas having centers on the longer wavelength side than 550 nm to the sum of all peak areas in the range of 190 nm to 1200 nm is greater than 4.3%.

[0020] <Step of Preparing Reduced Cerium Oxide Particles> (reduced cerium oxide particles) The reduced cerium oxide used in the production method of the present invention refers to reduced cerium oxide particles in which the average oxidation number of cerium element is 3 or more and less than 4, for example, CeO 2-n [wherein n is more than 0 and 0.5 or less]. n is preferably 0.01 to 0.5, more preferably 0.05 to 0.5, even more preferably 0.1 to 0.5, and even more preferably 0.2 to 0.5.

[0021] The reduced cerium oxide particles and the raw cerium oxide particles can be prepared by any known method. Specifically, naturally occurring cerium oxide may be used, or the cerium oxide may be chemically synthesized. In the case of chemical synthesis, examples include calcination of cerium hydroxide and hydrothermal synthesis. In the case of hydrothermal synthesis, it is desirable from the viewpoint of mass production to carry out the synthesis using a fluid treatment device (the device described in JP 2011-189348 A). Commercially available cerium oxide particles may also be used.

[0022] The reduced cerium oxide particles are preferably prepared by reducing raw cerium oxide. The raw material cerium oxide is not limited to cerium (IV) oxide, but may be any cerium oxide having an average oxidation number of the cerium element higher than the average oxidation number of the cerium element in the reduced cerium oxide particles. The reduced cerium oxide particles are preferably prepared by reducing raw cerium oxide with a reducing agent.

[0023] (reducing agent) In the present invention, the type of reducing agent is not particularly limited, and for example, known reducing agents can be widely used. Examples include sodium borohydride, lithium borohydride, lithium aluminum hydride, borane complexes, diborane, hydrogen, metal elements, tin compounds, ascorbic acid, hydrazine and its salts, but are not limited thereto. The above reducing agents may be used alone or in combination. It is preferable to use hydrazine because it is decomposed into nitrogen gas after the reaction and does not require a removal process. Hydrazine exists in anhydrous form and hydrate, and either may be used, or it may be in the form of a solution.

[0024] In the present invention, reduced cerium oxide means an oxide mainly composed of cerium, the average oxidation number of the cerium element being 3 or more and less than 4, as described above. One example is reduced cerium oxide having oxygen lattice defects. It is known that cerium oxide reversibly changes to a non-stoichiometric compound, and reduced cerium oxide can be obtained by keeping the oxygen partial pressure low, reducing cerium oxide by treating with a reducing agent, synthesizing cerium oxide using trivalent cerium ions and using it before it is oxidized, or the like. It is also possible to prepare reduced cerium oxide by reducing cerium oxide having an average oxidation number less than 4 to make the average oxidation number smaller than 4, that is, to prepare reduced cerium oxide in a more reduced state using reduced cerium oxide as a raw material. The valence of the cerium element in cerium oxide can be confirmed by known methods including X-ray photoelectron spectroscopy (XPS), but the most convenient method is to observe the change in color. Cerium (IV) oxide is known to be white to pale yellow, and non-stoichiometric compounds of cerium oxide having oxygen lattice defects (reduced cerium oxide) are known to be blue to black. For example, the reduced cerium oxide particles used by the inventors in the examples of the present invention were obtained as purple reduced cerium oxide using trivalent cerium ions, which became pale yellow cerium oxide (IV) when oxidized in air, and changed back to purple when treated with a reducing agent. Naturally, these changes can be clearly observed by observing the optical spectrum in the visible light region.

[0025] In the present invention, the raw material cerium oxide means, as described above, an oxide mainly composed of cerium, which is used to prepare reduced cerium oxide. The average oxidation number of the cerium element may be 4 or less.

[0026] <Step of treating the surface of reduced cerium oxide particles with acid> (Acid treatment) Following the above steps, the surfaces of the reduced cerium oxide particles are treated with an acid. The acid treatment refers to contacting an acidic substance with a substance to be treated, and does not limit the state of the acidic substance. One example of the acid treatment is stirring a particulate substance to be treated in an acidic liquid, but an acid gas may be brought into contact with the substance to be treated, or an acidic solid may be brought into contact with the substance to be treated. The type of acidic substance used in the acid treatment is not particularly limited, and for example, known acidic substances can be widely used. Examples include hydrogen halides such as hydrogen chloride and hydrochloric acid and their solutions, nitric acid, sulfur dioxide, sulfur trioxide, sulfuric acid, hydrogen sulfide, boric acid, phosphoric acid, carbonic acid, hydrofluoric acid, formic acid, acetic acid, propionic acid, butyric acid, isobutyric acid, citric acid, oxalic acid, benzoic acid, pyruvic acid, and carboxylic acids such as trifluoroacetic acid, sulfonic acids, boron trifluoride, aluminum chloride, silica, and alumina, but are not limited thereto. Preferred acids include, for example, carboxylic acids and nitric acid. The above acidic substances may be used alone or in combination. It is preferable to use acetic acid or nitric acid. Phosphoric acid, sulfuric acid, and the like are not preferable because the conjugate base is adsorbed on the cerium oxide surface (Comparative Examples 2 and 3).

[0027] The step of preparing the reduced cerium oxide particles and the step of treating the surfaces of the reduced cerium oxide particles with an acid may be carried out simultaneously, or the step of treating the surfaces of the reduced cerium oxide particles with an acid may be started first.

[0028] The method for producing acid-treated cerium oxide particles of the present invention makes it possible to easily obtain cerium oxide particles whose surfaces have been modified and which have good dispersibility in solvents, dispersants, resins, and the like.

[0029] 2. Cerium oxide particles The cerium oxide particles of the present invention correspond to the acid-treated cerium oxide described above. The cerium oxide of the present invention is as described above.

[0030] 3. Dispersion of cerium oxide particles The cerium oxide particle dispersion of the present invention is a dispersion of cerium oxide particles containing the cerium oxide particles of the present invention in a dispersion medium containing at least one of a solvent, a dispersant, and a resin. The cerium oxide particles of the present invention can be added to a solvent, a dispersant, a resin, or the like, and dispersed to prepare a dispersion liquid. Depending on the particle size of the cerium oxide used, it can be dispersed without a dispersant, and even if a dispersant is required, the amount used can be significantly reduced. It can also be dispersed in a resin only, if necessary. In the present invention, the type of solvent or resin used as the dispersion medium is not particularly limited, and for example, a wide variety of known solvents and resins can be used. For example, the solvent can be water, an organic solvent, or a mixed solvent consisting of a plurality of these. Examples of the water include tap water, ion-exchanged water, pure water, ultrapure water, RO water, and the like. Examples of the organic solvent include alcohol-based solvents such as ethanol, ethylene glycol, glycerin, and the like; ketone-based solvents such as acetone, 2-butanone, and the like; ether-based solvents such as diethyl ether, tetrahydrofuran, and the like; aromatic solvents such as toluene, xylene, and the like; amine-based solvents such as triethylamine, ethylenediamine, and the like; amide-based solvents such as N,N-dimethylformamide, and the like; aliphatic hydrocarbon-based solvents such as hexane, liquid paraffin, and the like; nitrile-based solvents such as acetonitrile, and the like; sulfoxide-based solvents such as dimethyl sulfoxide, and the like; halogen-based solvents such as dichloromethane, carbon tetrachloride, and the like; ester-based solvents such as ethyl acetate, ethylene glycol monoethyl ether acetate, and the like; carboxylic acid-based solvents such as acetic acid, propionic acid, and the like; aprotic polar solvents such as carbon disulfide, N-methyl-2-pyrrolidone, and the like; ionic liquids, sulfonic acid compounds, and the like, but are not limited thereto.

[0031] The dispersion of the cerium oxide particles of the present invention may contain a dispersant as necessary. The type of dispersant used in the dispersion is not particularly limited, and for example, a wide variety of known surfactants may be used. For example, surfactants such as cationic, anionic, nonionic, amphoteric, silicone, and fluorine-based surfactants may be used, but are not limited thereto. For example, it is preferable to use a phosphate ester-type anionic surfactant. Examples of the phosphate ester-type anionic surfactant include alkyl ether phosphate salts such as monododecyl phosphate, didodecyl phosphate, and tridodecyl phosphate, polyoxyethylene alkyl ether phosphate salts such as polyoxyethylene lauryl ether phosphate and polyoxyethylene tridecyl ether phosphate, but are not limited thereto. EXAMPLES

[0032] The present invention will be described below using examples, but the present invention is not limited to these examples.

[0033] (Reference example 1) The cerium oxide raw material solution and the cerium oxide precipitation solution were prepared using a high-speed rotary dispersion and emulsification device called Clearmix (product name: CLM-0.8S, manufactured by M-Technique). Specifically, 0.5 parts by mass of cerium nitrate (III) hexahydrate (Wako Pure Chemical Industries, special grade reagent), 1.9 parts by mass of diammonium cerium nitrate (IV) (Kishida Chemical, special grade reagent), and 97.6 parts by mass of pure water were mixed and homogenously mixed at a preparation temperature of 50°C by stirring with a Clearmix rotor at 20,000 rpm for 30 minutes to prepare a cerium oxide source solution. In addition, 2.77 parts by mass of sodium hydroxide (Kanto Chemical, special grade reagent) and 97.23 parts by mass of pure water were mixed and homogenously mixed at a preparation temperature of 45°C by stirring with a Clearmix rotor at 15,000 rpm for 30 minutes to prepare a cerium oxide deposition solution.

[0034] Next, the prepared cerium oxide raw material liquid and the cerium oxide deposition solution were mixed in a fluid treatment device (apparatus described in JP 2011-189348 A). Specifically, the cerium oxide raw material liquid was introduced into the fluid treatment device as the first fluid to be treated (liquid A) at 150 mL per minute at an introduction temperature of 122° C. between the treatment surfaces, and while the processing unit was operated at a rotation speed of 2250 rpm, the cerium oxide deposition solution was introduced into the fluid treatment device as the second fluid to be treated (liquid B) at 37.5 mL per minute at an introduction temperature of 78° C. between the treatment surfaces and mixed in the thin film fluid. Cerium oxide particles were deposited between the treatment surfaces, and a discharge liquid containing the cerium oxide particles was discharged from the treatment surfaces of the fluid treatment device. The discharge liquid containing the cerium oxide particles was collected in a beaker through a vessel.

[0035] A wet cake was prepared from the discharged liquid containing cerium oxide particles collected in a beaker. The preparation method was performed according to a known method. Specifically, the discharged liquid containing cerium oxide particles was collected by centrifugation, the cerium oxide particles were precipitated, and the supernatant liquid was removed. Then, the cerium oxide particles were washed by repeating washing with pure water (pH 6.34, conductivity 0.86 μS / cm) and precipitation by centrifugation twice to obtain a purple wet cake. Cerium (IV) oxide is white or pale yellow, and the purple color is a non-stoichiometric compound (reduced cerium oxide) having oxygen lattice defects. That is, the cerium oxide particles contained in the purple wet cake obtained here were reduced cerium oxide particles in which the average oxidation number of cerium element was 3 or more and less than 4. About four times the weight of pure water was added to the above purple wet cake, and the mixture was stirred in air for 48 hours and then centrifuged to obtain a pale yellow wet cake of raw cerium oxide (IV) particles. This color change was due to the cerium oxide particles being oxidized by oxygen in the air. In other words, the cerium oxide particles contained in the pale yellow wet cake obtained here were cerium oxide (IV) particles.

[0036] (Preparation of samples for TEM observation) A part of the wet cake of the raw material cerium (IV) oxide particles obtained in Reference Example 1 was dispersed in methanol. The obtained diluted solution was dropped onto a grid with a supporting film and dried to prepare a sample for TEM observation.

[0037] (Transmission Electron Microscope) A transmission electron microscope, JEM-2100 (manufactured by JEOL) was used for the transmission electron microscope (TEM) observation. The observation conditions were an acceleration voltage of 200 kV and an observation magnification of 10,000 to 800,000. The particle diameters of 100 particles of the raw material cerium (IV) oxide particles obtained in Reference Example 1 were measured, and the average particle diameter was 6.0 nm.

[0038] (X-ray diffraction measurement) For the X-ray diffraction (XRD) measurement, a powder X-ray diffraction measuring device EMPYREAN (manufactured by Malvern Panalytical) was used. The measurement conditions were: measurement range: 10 to 100 [°2Theta] Cu anticathode, tube voltage: 45 kV, tube current: 40 mA, and scan speed: 0.3° / min. The sample used was a wet cake of the raw material cerium (IV) oxide particles obtained in Reference Example 1, which was vacuum dried and then pulverized. XRD measurement was performed, and the diffraction pattern confirmed that it was cerium (IV) oxide. Using the peak near 28.5°, the crystallite size was calculated to be 5.7 nm using the Scherrer formula using the measurement results of a silicon polycrystalline plate.

[0039] (Reference example 2) Cerium oxide particles were prepared by batch hydrothermal synthesis. The preparation method was performed according to a known method. Specifically, 8 g of cerium nitrate (III) hexahydrate was dissolved in 92 g of boiling water to obtain a solution. 12.8 g of 20 wt% aqueous sodium hydroxide (Kanto Chemical, special grade reagent) was added over 5 minutes while stirring on a hot plate set at 80°C. After stirring for 30 minutes on the hot plate, the mixture was transferred to a sealed container and left to stand in a furnace set at 100°C for 2 hours. The mixture was collected by centrifugation, the cerium oxide particles were allowed to settle, the supernatant liquid was removed, and the cerium oxide particles were washed by repeating washing with pure water and settling by centrifugation twice to obtain a blue-purple wet cake. The cerium oxide particles contained in the obtained blue-purple wet cake were reduced cerium oxide particles. TEM observation was performed according to the above procedure, and the average particle size of 100 particles was measured, and the average value was 19.4 nm.

[0040] Example 1 In a glass vial, 10 g of the pale yellow wet cake containing the cerium (IV) oxide particles of Reference Example 1 was dispersed in 50 g of pure water, and 1 g of hydrazine monohydrate (Kanto Chemical, special grade reagent, the same applies below) was added. The mixture was stirred with a stirrer on a hot plate set at 80°C for 3 hours to obtain reduced cerium oxide particles. To the resulting slurry containing reduced cerium oxide particles, 10 g of acetic acid (special grade reagent, manufactured by Kanto Chemical; the same applies below) was added. The mixture was further stirred with a stirrer at 80°C for 16 hours. The treated liquid was pale yellow and opaque. The treated liquid was centrifuged and the supernatant was discarded to obtain a pale yellow paste containing acid-treated cerium oxide particles. TEM observation was performed using the procedure described above. A TEM photograph of the cerium oxide particles is shown in Figure 1. No change was observed in the average particle size.

[0041] Example 2 In a glass vial, 2 g of the light yellow wet cake containing the cerium (IV) oxide particles of Reference Example 1 was dispersed in 40 g of pure water, and 1 g of hydrazine monohydrate was added. The mixture was stirred with a stirrer on a hot plate set at 80° C. for 3 hours to obtain reduced cerium oxide particles. 10 g of isobutyric acid (special grade reagent, manufactured by Kanto Chemical) was added to the resulting slurry containing reduced cerium oxide particles. The mixture was further stirred at 80°C for 16 hours with a stirrer. The treated liquid was yellow and opaque. The treated liquid was centrifuged and the supernatant was discarded to obtain a yellow paste containing acid-treated cerium oxide particles.

[0042] Example 3 In a glass vial, 2 g of the light yellow wet cake containing the cerium (IV) oxide particles of Reference Example 1 was dispersed in 40 g of pure water, and 1 g of hydrazine monohydrate was added. The mixture was stirred with a stirrer on a hot plate set at 80° C. for 3 hours to obtain reduced cerium oxide particles. 10 g of nitric acid (Kishida Chemical, special grade reagent) was added to the resulting slurry containing reduced cerium oxide particles. The mixture was further stirred at 80°C for 16 hours with a stirrer. The treated liquid was white and opaque. The treated liquid was centrifuged and the supernatant was discarded to obtain a white paste containing acid-treated cerium oxide particles.

[0043] Example 4 In a glass vial, 2 g of the purple wet cake containing the reduced cerium oxide particles of Reference Example 1 was dispersed in 50 g of a 20 wt % aqueous acetic acid solution. The mixture was stirred with a stirrer on a hot plate set at 80° C. for 16 hours. The treated liquid was pale yellow and semitransparent. The treated liquid was centrifuged and the supernatant was discarded to obtain a pale yellow transparent paste containing acid-treated cerium oxide particles.

[0044] Example 5 In a glass vial, 2 g of the light yellow wet cake containing the cerium (IV) oxide particles of Reference Example 1 was dispersed in 40 g of pure water, and 1 g of hydrazine monohydrate and 10 g of acetic acid were added. The mixture was stirred with a stirrer on a hot plate set at 80° C. for 24 hours. The treated liquid was pale yellow and opaque, and was centrifuged to discard the supernatant, yielding a pale yellow paste containing acid-treated cerium oxide particles.

[0045] Example 6 In a glass vial, 2 g of the blue-purple wet cake containing the reduced cerium oxide particles of Reference Example 2 was dispersed in 20 g of pure water, and 2 g of hydrazine monohydrate was added. The mixture was stirred with a stirrer on a hot plate set at 80° C. for 3 hours to obtain more reduced reduced cerium oxide particles. 20 g of acetic acid was added to the resulting slurry containing reduced cerium oxide particles. The mixture was further stirred with a stirrer at 80° C. for 16 hours. The treated liquid was white and opaque. The treated liquid was centrifuged and the supernatant was discarded to obtain a white paste containing acid-treated cerium oxide particles.

[0046] Comparative Example 1 In a glass vial, 10 g of the pale yellow wet cake containing cerium (IV) oxide particles of Reference Example 1 was dispersed in 50 g of pure water, and the mixture was stirred with a stirrer on a hot plate set at 80°C for 3 hours, after which 10 g of acetic acid was added. The mixture was further stirred with a stirrer at 80°C for 16 hours. The treated liquid was pale yellow and transparent. The treated liquid was centrifuged, and the supernatant was discarded to obtain a pale yellow paste containing cerium oxide particles.

[0047] Comparative Example 2 In a glass vial, 2 g of the light yellow wet cake containing the cerium (IV) oxide particles of Reference Example 1 was dispersed in 40 g of pure water, and 1 g of hydrazine monohydrate was added. The mixture was stirred with a stirrer on a hot plate set at 80° C. for 3 hours to obtain reduced cerium oxide particles. To the resulting slurry containing reduced cerium oxide particles, 10 g of phosphoric acid (Kanto Chemical, special grade reagent) was added. The mixture was further stirred at 80°C for 16 hours. The treated liquid was white and opaque. The treated liquid was centrifuged and the supernatant was discarded to obtain a white paste containing cerium oxide particles.

[0048] Comparative Example 3 In a glass vial, 2 g of the light yellow wet cake containing the cerium (IV) oxide particles of Reference Example 1 was dispersed in 40 g of pure water, and 1 g of hydrazine monohydrate was added. The mixture was stirred with a stirrer on a hot plate set at 80° C. for 3 hours to obtain reduced cerium oxide particles. To the resulting slurry containing reduced cerium oxide particles, 10 g of sulfuric acid (Kishida Chemical, special grade reagent) was added. The mixture was further stirred at 80°C for 16 hours with a stirrer. The treated liquid was pale yellow and opaque. The treated liquid was centrifuged and the supernatant was discarded to obtain a pale yellow paste containing cerium oxide particles.

[0049] Comparative Example 4 In a glass vial, 2 g of the light yellow wet cake containing the cerium (IV) oxide particles of Reference Example 1 was dispersed in 40 g of pure water, and 1 g of hydrazine monohydrate was added. The mixture was stirred with a stirrer on a hot plate set at 80° C. for 3 hours to obtain reduced cerium oxide particles. 10 g of pure water was added to the resulting slurry containing reduced cerium oxide particles. The mixture was further stirred with a stirrer at 80° C. for 16 hours. The treated liquid was purple and opaque. The treated liquid was centrifuged and the supernatant was discarded to obtain a purple paste containing cerium oxide particles.

[0050] Comparative Example 5 In a glass vial, 2 g of the light yellow wet cake containing the cerium (IV) oxide particles of Reference Example 1 was dispersed in 40 g of pure water, and 1 g of hydrazine monohydrate was added. The mixture was stirred with a stirrer on a hot plate set at 80° C. for 3 hours to obtain reduced cerium oxide particles. To the resulting slurry containing reduced cerium oxide particles, 10 g of a 40 wt % aqueous solution of sodium hydroxide (Kanto Chemical, special grade reagent) was added. The mixture was further stirred at 80° C. for 16 hours with a stirrer. The treated liquid was white and opaque. The treated liquid was centrifuged and the supernatant was discarded to obtain a white paste containing cerium oxide particles.

[0051] Comparative Example 6 In a glass vial, 2 g of the light yellow wet cake containing the cerium (IV) oxide particles of Reference Example 1 was dispersed in 40 g of pure water, and 1 g of hydrazine monohydrate was added. The mixture was stirred with a stirrer on a hot plate set at 80° C. for 3 hours to obtain reduced cerium oxide particles. 10 g of aqueous ammonia (Kishida Chemical, special grade reagent) was added to the resulting slurry containing reduced cerium oxide particles. The mixture was further stirred at 80°C for 16 hours with a stirrer. The treated liquid was white and opaque. The treated liquid was centrifuged and the supernatant was discarded to obtain a white paste containing cerium oxide particles.

[0052] Comparative Example 7 In a glass vial, 2 g of the light yellow wet cake containing the cerium (IV) oxide particles of Reference Example 1 was dispersed in 40 g of pure water, and 1 g of hydrazine monohydrate was added. The mixture was stirred with a stirrer on a hot plate set at 80° C. for 3 hours to obtain reduced cerium oxide particles. To the resulting slurry containing reduced cerium oxide particles, 2 g of Plysurf A215C (registered trademark, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) was added. The mixture was further stirred with a stirrer at 80°C for 16 hours. The treated liquid was purple and opaque. The treated liquid was centrifuged and the supernatant was discarded to obtain a purple paste containing cerium oxide particles.

[0053] (Transparency of dispersion liquid) A small amount (approximately 5 mg of cerium oxide particles) of the cerium oxide particle paste obtained in each Example and Comparative Example was added to 10 mL of dispersion medium using a spatula, and the mixture was subjected to an ultrasonic disperser. If a transparent dispersion was not obtained, a drop of Plysurf A215C was added as a dispersant, and the mixture was subjected to the ultrasonic disperser again. The results are summarized in Tables 1 and 2. In Table 1, "untreated" refers to a pale yellow wet cake containing cerium (IV) oxide particles of Reference Example 1 dispersed in each dispersion medium.

[0054] [Table 1]

[0055] [Table 2]

[0056] As can be seen from Table 1, dispersions of untreated cerium oxide were not transparent in all solvents, but dispersions of the acid-treated cerium oxide particles of Examples 1 to 6 were transparent in non-polar solvents, and were also generally transparent in water and ethanol. Furthermore, as can be seen from Table 2, the cerium oxide particles or acid-treated cerium oxide particles of Comparative Examples 1 to 7 were not transparent in most of the dispersions in the solvents.

[0057] (FT-IR measurement) For the FT-IR measurement, a Fourier transform infrared spectrophotometer, FT / IR-6600 (manufactured by JASCO Corporation) was used. The measurement conditions were an ATR method under vacuum with a resolution of 4.0 cm. -1 , 128 times (4000cm -1 ~400cm -1 ) and cumulative count 256 times (400cm -1 ~50cm -1 ) The spectra obtained under the above measurement conditions are shown in Figures 2 to 7. Each sample was prepared by drying the paste in a vacuum and then pulverizing it. For reference, commercially available cerium oxide particles (Kanto Chemical, special grade, 10 μm diameter) were used.

[0058] Figure 2 shows the absorption of cerium oxide particles (450 cm -1 The infrared absorption spectra of the untreated cerium (IV) oxide particles obtained in Reference Example 1 and the acid-treated cerium oxide nanoparticles of Example 1 are shown in FIG. 3 and FIG. 4, which are converted into absorbance values ​​normalized by the peak at 1,450 cm. Further, enlarged views of the spectra are shown in FIG. 3 and FIG. 4. The reduction and acid treatment described below cause a clear change in absorption in the far-infrared region, and a change in the absorption at 1,450 cm. -1 Shift of the peak top in the absorption near (unprocessed: 1445 cm -1 Example 1: 1452 cm -1 ), 1400cm -1 Appearance of a shoulder peak near 3000 cm -1 The appearance of a peak at around 3700 cm was observed. These changes were attributed to the adsorption of acetate ions. -1 ~2500cm -1The absorption peak of the hydroxyl group, which is broadened by adsorbed water in the vicinity, is attenuated, suggesting that the surface treatment was carried out efficiently by performing the acid treatment after the reduction operation, and that the hydroxyl groups on the particle surface were removed.

[0059] In addition, the infrared absorption spectra of the commercially available reagent, the cerium oxide nanoparticles of Reference Example 1 (untreated), Example 1, and Comparative Example 1 were converted to absorbance values. -1 The results are shown in Figure 5. The peak top shift due to acid treatment (untreated: 489 cm -1 , Example 1 and Comparative Example 1: 458 cm -1 ) and 280cm -1 Attenuation of the peak near 280 cm was observed. -1 The peak around 283 cm is clearly different depending on whether or not the reduction operation is performed. -1 The absorbance at 100 nm was 0.698 for untreated, 0.490 for Comparative Example 1, and 0.413 for Example 1. This peak is attributed to the absorption of the unmodified cerium oxide surface, which supports the idea that the surface treatment was more efficient through the reduction procedure.

[0060] These absorptions are significantly different from those of the commercially available cerium oxide reference particles, which have a peak at 450 cm -1 The absorption peak top is around 449 cm -1 and 280cm -1 The nearby peak is 272cm -1 In addition, the commercially available particles showed a significantly higher intensity at 700 cm compared to the particles of Example 1. -1 ~600cm -1 From these facts, the particles of Example 1 were converted to absorbance and the absorption around 450 cm was missing. -1 It can be characterized as follows using the infrared absorption spectrum normalized to the peak top around 285 cm -1 ~270cm -1 Second, no strong absorption is observed in the 700 cm range. -1 ~600cm -1 It has absorption in the range.

[0061] The above characteristics can be specifically defined as follows using the normalized absorbance-converted spectra and peak separation results of Example 1 and Comparative Example 1 as described above. The peak separation results are shown in Figures 6 and 7. The solid line indicates the original spectrum, the long dashed line indicates the peak at 320 cm -1 The peak with the center on the lower wavenumber side, the dashed line is 700 cm -1 ~600cm -1 The dotted lines are the other separated peaks. -1 The absorbance at 320 cm was less than 0.490 (Comparative Example 1: 0.490, Example 1: 0.413) when peak separation was performed. -1 The sum of the peak areas with centers on the lower wavenumber side is 1000 cm -1 ~50cm -1 The ratio of the sum of all peak areas in the range of 663 cm to 673 cm is lower than 23.0% (Comparative Example 1: 23.0%, Example 1: 20.3%). -1 The absorbance at 610 cm is greater than 0.191 (Comparative Example 1: 0.191, Example 1: 0.201). -1 The absorbance at 700 cm was greater than 0.264 (Comparative Example 1: 0.264, Example 1: 0.274). -1 ~600cm -1 The sum of the peak areas centered at 1000 cm -1 ~50cm -1 The proportion of the sum of all peak areas in this range is higher than 4.7% (Comparative Example 1: 4.7%, Example 1: 6.8%).

[0062] (UV-vis-NIR measurement) For the UV-vis-NIR (ultraviolet-visible-near infrared absorption spectrum) measurement, a UV-visible-near infrared spectrophotometer V-770 (manufactured by JASCO Corporation) was used. The measurement conditions were a reflection method in the atmosphere, with a data width of 1 nm. Each sample was prepared by vacuum drying the paste and then pulverizing it.

[0063] FIG. 8 shows the reflectance spectrum, where the absorbance at 200 nm is set to 1. Compared with Reference Example 1 (untreated), Example 1 and Comparative Example 1, which were subjected to acid treatment, show attenuation of absorption near 400 to 500 nm. In addition, Example 1 shows a peculiar rise in absorption on the longer wavelength side than 500 nm. This feature can be specifically defined as follows using the normalized absorbance-converted spectra and peak separation results of Example 1 and Comparative Example 1 as described above. The results of peak separation are shown in FIGS. 9 and 10. The solid line shows the original spectrum, the dashed line shows the peaks centered on the longer wavelength side than 550 nm, and the dotted line shows the other separated peaks. The absorbance at 650 nm is greater than 0.055 (Comparative Example 1: 0.055, Example 1: 0.199), and when peak separation is performed, the proportion of the sum of peak areas having centers on the longer wavelength side than 550 nm to the sum of all peak areas in the range of 190 nm to 1200 nm is greater than 4.3% (Comparative Example 1: 4.3%, Example 1: 21.6%).

[0064] (Transmittance measurement) The transmittance was measured using a UV-Vis-NIR spectrophotometer V-770 (manufactured by JASCO Corporation). The measurement conditions were a cell method in air, a cell length of 1 cm, and a data width of 0.5 nm. For each sample, a toluene dispersion obtained in a dispersion test was used. The average values ​​(average transmittance) of the obtained transmittance in the visible light region (380 to 800 nm) are summarized in Table 3. [Table 3]

[0065] As can be seen from Table 3, the average transmittance of the toluene dispersion of the untreated and comparative cerium oxide particles or the acid-treated cerium oxide particles was very low. In contrast, the average transmittance of the toluene dispersion of the acid-treated cerium oxide particles of Examples 1 to 6 was very high, at 60% or more.

[0066] (Reference example 3) A solution obtained by mixing 2 parts by mass of cerium (III) nitrate hexahydrate and 98 parts by mass of pure water in Liquid A was used to produce cerium oxide particles in the same manner as in Reference Example 1. At this time, the flow rate of Liquid B was set to 30 mL per minute. A purple wet cake and a pale yellow wet cake were produced from the obtained discharged liquid in the same manner as in Reference Example 1.

[0067] (Reference Example 4, Reduced Cerium Oxide Wet Cake) In a glass vial, 2 g of the light yellow wet cake containing cerium (IV) oxide particles of Reference Example 3 was dispersed in 40 g of pure water, and 1 g of hydrazine monohydrate was added. The mixture was stirred with a stirrer on a hot plate set at 80°C for 3 hours to obtain reduced cerium oxide particles. The particles were then collected by centrifugation to obtain a purple wet cake containing reduced cerium oxide.

[0068] (Reflection spectrum measurement) Reflection spectrum measurements were performed to clarify the oxidation state of cerium oxide. A UV-Visible-Near-Infrared Spectrophotometer V-770 (manufactured by JASCO Corporation) was used for reflectance spectrum measurements. Measurements were performed in air with a data width of 1 nm. Each sample was used as is without drying the wet cake. The reflectance spectrum was converted to absorbance and normalized with the absorbance at 205 nm set to 1. The results are shown in Figure 11. All values ​​related to the reflectance spectrum hereafter are values ​​normalized with the absorbance at 205 nm set to 1.

[0069] In the purple wet cake of Reference Example 3 and the purple wet cake of Reference Example 4, absorption with a maximum near 510 to 540 nm was observed compared to the pale yellow wet cake of Reference Example 3. This absorption was observed in the purple wet cake before and after re-reduction in the atmosphere, but was not observed at all in the pale yellow wet cake after the atmosphere oxidation, and is therefore attributed to reduced cerium oxide. Although the specific oxidation number of the purple paste cannot be determined from this spectrum, it was confirmed that the cerium oxide particles were indeed converted to cerium oxide (IV) by the atmosphere oxidation. In addition, by comparing the intensity of this absorption, it is possible to determine which of two or more hydrous cerium oxide wet cakes is the more reduced cerium oxide.

[0070] Considering the mixing ratio of the materials, the purple wet cake of Reference Example 3 has an average oxidation number of cerium of 3 or more. The absorbance at 512 nm, which is the maximum absorption wavelength of the purple wet cake of Reference Example 3, is 0.851 for the purple wet cake of Reference Example 3 and 0.190 for the pale yellow wet cake of Reference Example 3. The lower limit of each average oxidation number of cerium oxide can be estimated by performing calculations assuming that the average oxidation number of cerium oxide contained in the purple wet cake of Reference Example 3 is 3. For example, when the reflectance spectrum of a hydrous cerium oxide wet cake is measured, it is found that the absorbance at 512 nm is 0.196 or more when the average oxidation number of cerium is 3.99, 0.203 or more when the average oxidation number of cerium is 3.98, 0.223 or more when the average oxidation number of cerium is 3.95, 0.256 or more when the average oxidation number of cerium is 3.90, 0.322 or more when the average oxidation number of cerium is 3.80, 0.454 or more when the average oxidation number of cerium is 3.60, and 0.520 or more when the average oxidation number of cerium is 3.50. However, these are values ​​based on the reflectance spectrum of hydrous cerium oxide, and do not mean that cerium oxide with the same average oxidation number will not fall below these absorbances in other states or when measured by other methods.

[0071] As will be seen from the examples, the present invention makes it possible to easily perform surface treatment of cerium oxide and produce a transparent dispersion of cerium oxide particles. [Industrial Applicability]

[0072] According to the present invention, it is possible to produce cerium oxide particles having good dispersibility in a solvent, a dispersant, a resin, etc. Furthermore, cerium oxide particles and a dispersion of well-dispersed cerium oxide particles are provided.

Claims

1. preparing reduced cerium oxide particles having an average oxidation number of cerium element of 3 or more and less than 4; A step of treating the surface of the reduced cerium oxide particles with an acid. A method for producing acid-treated cerium oxide particles, comprising:

2. The method according to claim 1 , wherein in the step of preparing the reduced cerium oxide particles, the reduced cerium oxide particles are prepared by reducing a raw material cerium oxide.

3. The method according to claim 1 , wherein in the step of preparing the reduced cerium oxide particles, the reduced cerium oxide particles are prepared by reducing raw material cerium oxide with a reducing agent.

4. The method according to claim 3, wherein the reducing agent is hydrazine.

5. The method according to claim 1 , wherein the acid used in the acid treatment step is a carboxylic acid or nitric acid.

6. The method according to claim 1, wherein the particle diameter of the acid-treated cerium oxide particles is 1 nm to 100 nm.

7. The acid-treated cerium oxide particles are produced by the method according to any one of claims 1 to 6, The method for producing a dispersion of acid-treated cerium oxide particles includes dispersing the obtained acid-treated cerium oxide particles in a dispersion medium containing at least one of a solvent, a dispersant, and a resin.

8. In the infrared absorption spectrum converted into absorbance, -1 ~500cm -1 When the maximum absorbance of -1 Cerium oxide particles having an absorbance of less than 0.490 at .

9. In the infrared absorption spectrum converted into absorbance, -1 ~500cm -1 When the maximum absorbance of -1 The absorbance at 610 cm is greater than 0.

191. -1 Cerium oxide particles having an absorbance of greater than 0.

264.

10. In the infrared absorption spectrum converted into absorbance, when peak separation was performed, -1 The sum of the peak areas with the center on the lower wavenumber side is 1000 cm -1 ~50cm -1 Cerium oxide particles, in which the proportion of the sum of all peak areas in the range is less than 23.0%.

11. In the infrared absorption spectrum converted into absorbance, when peak separation was performed, -1 ~600cm -1 The sum of the peak areas with the center at 1000 cm -1 ~50cm -1 Cerium oxide particles, wherein the proportion of the sum of all peak areas in the range is higher than 4.7%.

12. Cerium oxide particles having an absorbance at 650 nm of greater than 0.055 when the absorbance at 200 nm is taken as 1 in an ultraviolet-visible-near infrared reflectance spectrum converted into absorbance.

13. Cerium oxide particles, in which the sum of peak areas having centers on the longer wavelength side than 550 nm in an absorbance-converted ultraviolet-visible-near-infrared reflectance spectrum accounts for more than 4.3% of the sum of all peak areas in the range of 190 nm to 1200 nm.

14. 14. The cerium oxide particles according to claim 8, having an average particle size of 1 nm to 100 nm.

15. A dispersion of cerium oxide particles, comprising the cerium oxide particles according to any one of claims 8 to 13 in a dispersion medium containing at least one of a solvent, a dispersant, and a resin.

Citation Information

Patent Citations

  • JP20020A

  • JP145057A