Method for producing polystyrene resin extruded foam board
A specialized resin composition with brominated styrene-butadiene and phosphorus-based flame retardants addresses the challenge of achieving high flame retardancy and heat resistance in polystyrene foam boards, ensuring good moldability and formability even in wider boards.
Patent Information
- Application Number
- JP2023071636
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2043-04-25
AI Technical Summary
Polystyrene resin extruded foam boards require higher flame retardancy and heat resistance, but increasing the amount of brominated flame retardant to achieve this leads to deteriorated formability, especially in boards wider than 300 mm.
A method involving a foamable molten resin composition containing a brominated styrene-butadiene copolymer and a phosphorus-based flame retardant with a melting point of 80°C or less, along with specific mass ratios and additives, is used to produce extruded polystyrene foam boards with improved flame retardancy and heat resistance while maintaining moldability.
The method produces extruded foam boards with desired flame retardancy, heat resistance, and good moldability, even in widths of 300 mm or more, by optimizing the composition and additives in the resin mixture.
Smart Images

Figure 2024157337000001 
Figure 2024157337000002 
Figure 2024157337000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an extruded polystyrene foam board. [Background technology]
[0002] Conventionally, a method is known in which a cell regulator is added to a base resin, the mixture is heated and kneaded in an extruder, a physical foaming agent is then injected into the extruder and further kneaded, the resulting foamable molten resin composition is extruded from a high pressure region to a low pressure region (usually into the atmosphere), and shaped into a plate shape by a shaping device connected to the die outlet of the extruder to obtain an extruded polystyrene resin foam board. The extruded polystyrene resin foam board has a low thermal conductivity and excellent heat insulation, and is therefore suitably used as an insulation material for the walls, floors, roofs, etc. of buildings.
[0003] The present applicant has proposed a method for producing an extruded polystyrene resin foam board having excellent heat insulation and flame retardancy (for example, Patent Document 1). In the method for producing an extruded polystyrene resin foam board of Patent Document 1, a bromine-based flame retardant is added to a foamable molten resin composition in order to impart flame retardancy to the extruded foam board. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2022-110748 A Summary of the Invention [Problem to be solved by the invention]
[0005] On the other hand, in the case of extruded polystyrene resin foam boards, there are cases where higher flame retardancy and heat resistance are required. In such cases, for example, in the method for producing extruded polystyrene resin foam boards of Patent Document 1, it is considered to increase the amount of brominated flame retardant added to the foamable molten resin composition in order to more reliably impart the desired flame retardancy.
[0006] However, increasing the amount of brominated flame retardant added tends to deteriorate the moldability of the extruded foam board. In particular, in the production of extruded foam boards with a width of 300 mm or more, it was thought that there was room for further improvement in that the moldability of the widthwise ends of the extruded foam boards was further deteriorated.
[0007] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a method for producing an extruded polystyrene foam board, which can produce an extruded foam board having desired flame retardancy and heat resistance, and which has good moldability even when producing an extruded foam board with a width of 300 mm or more. [Means for solving the problem]
[0008] In order to solve the above problems, the following method for producing an extruded polystyrene foam board is provided.
[0009] [1] A foaming method comprising extruding and foaming a foamable molten resin composition containing a base resin containing a polystyrene resin, a flame retardant and a physical foaming agent, and molding the composition into a plate shape using a molding tool. 3 More than 50kg / m 3 The following is a method for producing an extruded polystyrene foam board having a width of 300 mm or more: The flame retardant includes a brominated styrene-butadiene copolymer and a phosphorus-based flame retardant having a melting point of 80° C. or less, the amount of the brominated styrene-butadiene copolymer added is 2 parts by mass or more and 12 parts by mass or less per 100 parts by mass of the base resin, A method for producing an extruded polystyrene foam board, wherein a mass ratio of the phosphorus-based flame retardant having a melting point of 80° C. or lower to the brominated styrene-butadiene copolymer is more than 0.15 and 0.5 or lower. [2] The method for producing an extruded polystyrene foam board according to [1], wherein the mass ratio of the phosphorus-based flame retardant having a melting point of 80°C or lower to the brominated styrene-butadiene copolymer is 0.18 or more and 0.5 or less. [3] The method for producing an extruded polystyrene resin foam plate according to [1] or [2], wherein the foamable molten resin composition contains graphite, and the amount of the graphite added is 0.3 parts by mass or more and 5 parts by mass or less per 100 parts by mass of the base resin. [4] The method for producing an extruded polystyrene foam board according to any one of [1] to [3] above, wherein the phosphorus-based flame retardant having a melting point of 80°C or less is one or more selected from the group consisting of triphenyl phosphate and cresyl diphenyl phosphate. [5] The method for producing a polystyrene-based resin extruded foam board according to any one of [1] to [4], wherein the base resin contains a styrene-(meth)acrylic acid ester copolymer, and the content of the (meth)acrylic acid ester component derived from the styrene-(meth)acrylic acid ester copolymer in the base resin is 8% by mass or more and 40% by mass or less. [6] The method for producing an extruded polystyrene resin foam board according to any one of [1] to [5] above, wherein a mass ratio of the phosphorus-based flame retardant having a melting point of 80°C or lower to the (meth)acrylic acid ester component in the foamable molten resin composition is 0.03 to 0.15. [7] The method for producing an extruded polystyrene resin foam board according to any one of [1] to [6], wherein the foamable molten resin composition contains a hydrofluoroolefin as the physical foaming agent, and the amount of the hydrofluoroolefin added per kg of the base resin is 0.1 mol or more and 1.3 mol or less. Effect of the Invention
[0010] The method for producing an extruded polystyrene foam board of the present invention can produce an extruded foam board having the desired flame retardancy and heat resistance, and the extruded foam board also has good moldability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, one embodiment of the method for producing an extruded polystyrene foam board of the present invention will be described.
[0012] The method for producing an extruded polystyrene foam board of the present invention includes a step of extruding and foaming a foamable molten resin composition containing a base resin containing a polystyrene resin, a flame retardant, and a physical foaming agent, and molding the composition into a board using a molding tool. 3 More than 50kg / m 3 Hereinafter, a polystyrene resin extruded foam board having a width of 300 mm or more (hereinafter sometimes referred to as "extruded foam board") is manufactured.
[0013] Specifically, for example, a base resin is added with additives such as a flame retardant and a bubble regulator, and then fed to an extruder, heated and kneaded, and then a physical foaming agent is pressed into the extruder and further kneaded to obtain a foamable resin composition. This foamable resin composition is extruded from a high pressure region to a low pressure region (usually in the atmosphere) to foam, and the resulting foam is shaped into a plate using a shaping device (such as a guider) connected to the die outlet of the extruder, to produce a polystyrene resin extruded foam plate. As the shaping device, for example, a device consisting of a pair of upper and lower polytetrafluoroethylene plates can be used.
[0014] <Base resin> The base resin contains a polystyrene resin as a main component. In this specification, "containing as a main component" means that the content of a specific component in 100% by mass of the composition is 50% by mass or more. Specifically, the content of the polystyrene resin in the base resin is 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more.
[0015] (Polystyrene resin) The polystyrene resin is a polymer containing styrene as a main component, and a styrene homopolymer or a copolymer of styrene and a vinyl monomer copolymerizable with styrene can be used.
[0016] Specifically, examples of the polystyrene resin include one or more types selected from polystyrene, styrene-(meth)acrylic acid ester copolymers, styrene-acrylic acid copolymers, styrene-maleic anhydride copolymers, styrene-polyphenylene ether copolymers, styrene-acrylonitrile copolymers, styrene-methylstyrene copolymers, styrene-dimethylstyrene copolymers, styrene-ethylstyrene copolymers, and styrene-diethylstyrene copolymers.
[0017] The content of the styrene component in the copolymer is preferably 50 mol% or more, more preferably 60 mol% or more, and further preferably 70 mol% or more. The polystyrene resin may contain a polyfunctional monomer unit component such as divinylbenzene or a multibranched macromonomer.
[0018] In addition, the melt viscosity of polystyrene resin is set at 200℃ and a shear rate of 100sec from the viewpoint of foaming and moldability. -1 Under these conditions, the viscosity is preferably 500 to 3000 Pa·s, more preferably 1000 to 2500 Pa·s, and further preferably 1500 to 2300 Pa·s.
[0019] The base resin preferably contains a styrene-(meth)acrylic acid ester copolymer as a main component. In this case, a relatively large amount of hydrofluoroolefin as a physical foaming agent described later, for example 0.5 mol / kg or more, can be added, and an extruded foam board exhibiting higher thermal insulation can be obtained. On the other hand, conventional extruded foam boards containing a styrene-(meth)acrylic acid ester copolymer as a main component tend to have reduced flame retardancy due to the (meth)acrylic acid ester component. In contrast, the present invention contains a specific flame retardant described later, so that the resulting extruded foam board has excellent flame retardancy even when the base resin contains a styrene-(meth)acrylic acid ester copolymer as a main component.
[0020] The styrene-(meth)acrylic acid ester copolymer is a copolymer of styrene and a lower alkyl ester of (meth)acrylic acid. Specific examples thereof include styrene-methyl acrylate copolymer, styrene-ethyl acrylate copolymer, styrene-propyl acrylate copolymer, styrene-methyl methacrylate copolymer, styrene-ethyl methacrylate copolymer, and styrene-propyl methacrylate copolymer. Among them, the styrene-(meth)acrylic acid ester copolymer is preferably a styrene-methyl acrylate copolymer or a styrene-methyl methacrylate copolymer, and more preferably a styrene-methyl methacrylate copolymer. These styrene-(meth)acrylic acid ester copolymers can be used alone or in combination of two or more. In this specification, "(meth)acrylic acid" is a concept that includes "acrylic acid" and "methacrylic acid", and means one or both of them.
[0021] The content of the (meth)acrylic acid ester component in the styrene-(meth)acrylic acid ester copolymer can be exemplified as a range of 10% by mass or more and 80% by mass or less. In addition, from the viewpoint of ensuring flame retardancy, heat resistance, and moldability, it is preferable that the base resin contains a styrene-(meth)acrylic acid ester copolymer with a small amount of the (meth)acrylic acid ester component. In this case, the content of the (meth)acrylic acid ester component in the styrene-(meth)acrylic acid ester copolymer is preferably 5% by mass or more and less than 40% by mass, and more preferably 15% by mass or more and 30% by mass or less. The content of the (meth)acrylic acid ester component in the styrene-(meth)acrylic acid ester copolymer can be determined by a known method such as pyrolysis gas chromatography analysis.
[0022] The styrene-(meth)acrylic acid ester copolymer may be used alone as a base resin if the content of the (meth)acrylic acid ester component in the copolymer is in the range of 10% by mass to 50% by mass. Specifically, the content of the styrene-(meth)acrylic acid ester copolymer in the base resin, which is in the range of 10% by mass to 50% by mass, is, for example, 20% by mass or more, preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, particularly preferably 80% by mass or more, including 100% by mass. On the other hand, if the content of the (meth)acrylic acid ester component in the copolymer is in the range of more than 50% by mass, it can be used as a material for adjusting the content of the (meth)acrylic acid ester component (M component) derived from the styrene-(meth)acrylic acid ester copolymer in the base resin by using it in combination with other polystyrene-based resins such as polystyrene.
[0023] The content of the (meth)acrylic acid ester component (M component) derived from the styrene-(meth)acrylic acid ester copolymer in the base resin is preferably 3% by mass or more, more preferably 8% by mass or more, even more preferably 10% by mass or more, and particularly preferably 15% by mass or more, from the viewpoint of stably obtaining an extruded foam board with good moldability even when a relatively large amount of hydrofluoroolefin is added as a physical foaming agent, and from the viewpoint of further improving the heat resistance of the obtained extruded foam board. On the other hand, the content of the (meth)acrylic acid ester component (M component) derived from the styrene-(meth)acrylic acid ester copolymer in the base resin is preferably 45% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less, from the viewpoint of more reliably ensuring the flame retardancy of the extruded foam board. It is to be noted that two or more types of styrene-(meth)acrylic acid ester copolymers having different contents of (meth)acrylic acid ester components can be used in combination. In this case, the content of the (meth)acrylic acid ester component (M component) derived from the styrene-(meth)acrylic acid ester copolymer in the base resin is the total amount of the (meth)acrylic acid ester component contained in each styrene-(meth)acrylic acid ester copolymer.
[0024] From the viewpoint of ensuring the flame retardancy, heat resistance and moldability of the extruded foam board, the content of the styrene component (St component) in the base resin is preferably 50% by mass or more and 97% by mass or less, more preferably 60% by mass or more and 95% by mass or less, and even more preferably 70% by mass or more and 90% by mass or less.
[0025] (Other polymers) The base resin may contain an amorphous polyethylene terephthalate copolymer to further improve the heat insulation, flame retardancy and heat resistance of the extruded foam board. In this case, the amorphous polyethylene terephthalate resin is preferably added to the base resin so as to be 5% by mass or more and less than 50% by mass, more preferably 10% by mass or more and 40% by mass or less, and even more preferably 15% by mass or more and 30% by mass or less. In the amorphous polyethylene terephthalate copolymer, the heat of fusion accompanying the melting of the resin based on JIS K7122 is less than 5 J / g. The heat of fusion is measured based on the DSC curve obtained using a heat flux differential scanning calorimeter, employing "the case where the heat of fusion is measured after a certain heat treatment" (the heating rate and the cooling rate in the condition adjustment of the test piece are both 10°C / min) described in JIS K7122 (1987).
[0026] In addition, other polymers than polystyrene resins may be added to the base resin within a range that does not impair the object of the present invention. Examples of other polymers include thermoplastic resins such as polyester resins, polyolefin resins, and polyphenylene ether resins, and thermoplastic elastomers such as styrene elastomers. The amount of other polymers than polystyrene resins added is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and particularly preferably 5% by mass or less in the base resin (based on the base resin being 100% by mass).
[0027] <Flame retardants> In the present invention, the flame retardant is a specific bromine-based flame retardant and a phosphorus-based flame retardant. Specifically, the flame retardant includes a brominated styrene-butadiene copolymer as the bromine-based flame retardant and a phosphorus-based flame retardant having a melting point of 80° C. or less. By using the above bromine-based flame retardant and phosphorus-based flame retardant in a specific amount and ratio, a wide extruded foam board having excellent moldability, flame retardancy, and heat resistance can be produced.
[0028] Examples of the brominated styrene-butadiene copolymer include one or more of brominated styrene-butadiene block copolymers, brominated styrene-butadiene random copolymers, and brominated styrene-butadiene graft copolymers. Such brominated styrene-butadiene copolymers are produced, for example, by brominating a polystyrene-polybutadiene copolymer. Examples of the brominated styrene-butadiene copolymers preferably used in the present invention include commercially available products such as Emerald 3000 from Chemtura and FR122P from ICL-IP.
[0029] Considering dispersibility in polystyrene resins, the weight average molecular weight of the brominated styrene-butadiene copolymer is preferably 100,000 to 200,000 in terms of polystyrene. From the viewpoint of flame retardancy, the bromine content is preferably 50 to 80% by weight. The bromine content can be determined based on JIS K7392:2009.
[0030] The amount of the brominated styrene-butadiene copolymer added is 2 parts by mass or more and 12 parts by mass or less per 100 parts by mass of the base resin. By using the brominated styrene-butadiene copolymer in the above-mentioned amount range together with a specific phosphorus-based flame retardant described later, the flame retardancy, heat resistance and moldability of the extruded foam board can be improved. Therefore, the brominated flame retardant added to the base resin preferably contains the brominated styrene-butadiene copolymer as a main component, and when a brominated flame retardant other than the brominated styrene-butadiene copolymer is used as a main component as the brominated flame retardant, it may be difficult to satisfy the flame retardancy, heat resistance and moldability of the extruded foam board. In addition, from the viewpoint of expressing a higher level of flame retardancy, the amount of the brominated styrene-butadiene copolymer added is preferably 3 parts by mass or more, more preferably 4 parts by mass or more, per 100 parts by mass of the base resin. On the other hand, from the viewpoint of further improving the moldability of the resulting extruded foam board, the amount of the brominated styrene-butadiene copolymer added is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, per 100 parts by mass of the base resin.
[0031] The phosphorus-based flame retardant used in the present invention contains a phosphorus-based flame retardant having a melting point of 80°C or less as a main component. If a phosphorus-based flame retardant having a melting point of 80°C or less is not added, the flame retardancy of the resulting extruded foam board may be reduced. If a phosphorus-based flame retardant having a melting point of 80°C or less is not added, the moldability may be reduced, and when a wide extruded foam board is produced, the surface properties and the shapeability of the end of the extruded foam board may be impaired. If a phosphorus-based flame retardant having a melting point of more than 80°C is added as a main component of the phosphorus-based flame retardant, the flame retardancy of the resulting extruded foam board may be reduced and the desired flame retardancy may not be exhibited. From this viewpoint, the melting point of the phosphorus-based flame retardant is preferably 70°C or less, more preferably 60°C or less, and even more preferably 55°C or less. The lower limit of the melting point of the phosphorus-based flame retardant is not particularly limited, but can be set at -70°C as a guideline, and is preferably -50°C. The melting point of phosphorus-based flame retardants is determined based on JIS K7121:1987. Specifically, the conditioning is performed by "(2) Measuring the melting temperature after a certain heat treatment", and the conditioned test piece is heated to obtain a DSC curve, and the apex temperature of the melting peak is taken as the melting point. The heating rate and cooling rate are 10°C / min. If multiple melting peaks appear on the DSC curve, the apex temperature of the melting peak with the largest area is taken as the melting point.
[0032] Preferred examples of phosphorus-based flame retardants having a melting point of 80°C or less include phosphoric acid esters such as triphenyl phosphate (TPP), tricresyl phosphate (TCP), cresyl diphenyl phosphate (CDP), trixylenyl phosphate (TXP), xylyl diphenyl phosphate, resorcinol bis(diphenyl)phosphate, tris(chloroethyl)phosphate (TCEP), and tris(chloropropyl)phosphate (TCPP). These may be added alone or in combination of two or more. Among these, the phosphorus-based flame retardant is preferably an aromatic phosphoric acid ester, more preferably one or more selected from the group consisting of triphenyl phosphate (TPP) and cresyl diphenyl phosphate (CDP), and even more preferably triphenyl phosphate (TPP). When two or more phosphorus-based flame retardants having a melting point of 80°C or less are added, the melting points of each phosphorus-based flame retardant are measured separately.
[0033] In the method for producing an extruded polystyrene foam board of the present invention, the ratio of the amount of phosphorus-based flame retardant having a melting point of 80° C. or less to the amount of brominated styrene-butadiene copolymer (in other words, the mass ratio of the phosphorus-based flame retardant having a melting point of 80° C. or less to the brominated styrene-butadiene copolymer) is more than 0.15 and 0.5 or less. If the mass ratio of the phosphorus-based flame retardant having a melting point of 80° C. or less to the brominated styrene-butadiene copolymer is 0.15 or less, the flame retardancy of the extruded foam board may decrease or the moldability may decrease, and especially when a wide extruded foam board is to be produced, the shapeability of the edge may be insufficient. From the viewpoint of sufficiently increasing the shapeability of the edge even in a wide extruded foam board, it is preferable that the mass ratio of the phosphorus-based flame retardant having a melting point of 80° C. or less to the brominated styrene-butadiene copolymer is 0.18 or more. On the other hand, if the mass ratio of the phosphorus-based flame retardant having a melting point of 80° C. or less to the brominated styrene-butadiene copolymer exceeds 0.5, the heat resistance of the extruded foam board may decrease. From this viewpoint, the mass ratio of the phosphorus-based flame retardant having a melting point of 80° C. or less to the brominated styrene-butadiene copolymer is preferably 0.4 or less.
[0034] The amount of phosphorus-based flame retardant added is preferably 0.3 parts by mass or more and 3 parts by mass or less, more preferably 0.5 parts by mass or more and 2 parts by mass or less, and even more preferably 0.8 parts by mass or more and 1.5 parts by mass or less, relative to 100 parts by mass of the base resin, from the viewpoint of ensuring that the flame retardancy, heat resistance, and moldability of the extruded foam board are good. The phosphorus-based flame retardant may contain a phosphorus-based flame retardant having a melting point of more than 80°C within a range that does not impair the intended effect of the present invention. However, the amount of phosphorus-based flame retardant having a melting point of more than 80°C added is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less, relative to 100 parts by mass of phosphorus-based flame retardant having a melting point of 80°C or less, and it is particularly preferable that the phosphorus-based flame retardant having a melting point of more than 80°C is not substantially contained.
[0035] In order to satisfy a high level of flame retardancy, such as the flammability standard for extruded polystyrene foam insulation boards described in "Test Method A" of the flammability test method of JIS A9521:2017, the amount of flame retardant added is preferably 3 to 15 parts by mass, and more preferably 5 to 12 parts by mass, per 100 parts by mass of the base resin.
[0036] In the case where the base resin contains a styrene-(meth)acrylic acid ester copolymer, the ratio of the amount (parts by mass) of the phosphorus-based flame retardant to the content (% by mass) of the (meth)acrylic acid ester component (M component) derived from the styrene-(meth)acrylic acid ester copolymer in the base resin (in other words, the mass ratio (phosphorus-based flame retardant / M component) of the phosphorus-based flame retardant having a melting point of 80° C. or less to the (meth)acrylic acid ester component (M component) in the foamable molten resin composition) is preferably 0.03 to 0.15. When the ratio (phosphorus-based flame retardant / M component) is in this range, even when the base resin contains a (meth)acrylic acid ester component derived from a styrene-(meth)acrylic acid ester copolymer, the flame retardancy can be further improved and the moldability can be more reliably improved.
[0037] Furthermore, in the present invention, other brominated flame retardants or flame retardant assistants may be added in combination for the purpose of further improving the flame retardancy of the extruded foam board.
[0038] Other bromine-based flame retardants include one or more of tetrabromobisphenol A, tetrabromobisphenol-A-bis(2,3-dibromopropyl ether), tetrabromobisphenol-A-bis(2-bromoethyl ether), tetrabromobisphenol-A-bis(allyl ether), tetrabromobisphenol-A-bis(2,3-dibromo-2-methylpropyl ether), tetrabromobisphenol S, tetrabromobisphenol-S-bis(2,3-dibromopropyl ether), hexabromocyclododecane, tetrabromocyclooctane, tris(2,3-dibromopropyl)isocyanurate, tribromophenol, decabromodiphenyl oxide, and tris(tribromoneopentyl)phosphate. The amount of these other brominated flame retardants added is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less, per 100 parts by mass of the brominated styrene-butadiene copolymer, and it is particularly preferable that the composition does not substantially contain any other brominated flame retardants other than the brominated styrene-butadiene copolymer.
[0039] Examples of the flame retardant auxiliary include one or more of diphenylalkanes and diphenylalkenes such as 2,3-dimethyl-2,3-diphenylbutane, 2,3-diethyl-2,3-diphenylbutane, 3,4-dimethyl-3,4-diphenylhexane, 3,4-diethyl-3,4-diphenylhexane, 2,4-diphenyl-4-methyl-1-pentene, and 2,4-diphenyl-4-ethyl-1-pentene; nitrogen-containing cyclic compounds such as antimony trioxide, diantimony pentoxide, ammonium sulfate, zinc stannate, cyanuric acid, isocyanuric acid, triallyl isocyanurate, melamine cyanurate, melamine, melam, and melem; inorganic compounds such as silicone compounds, boron oxide, zinc borate, and zinc sulfide; and phosphorus compounds such as red phosphorus, ammonium polyphosphate, and phosphazene. When a flame retardant auxiliary is added, the amount added is, for example, 0.01 to 1 part by mass, and preferably 0.05 to 0.5 parts by mass, relative to 100 parts by mass of the base resin.
[0040] As a method for adding a flame retardant to a thermoplastic resin containing a base resin, a method in which a predetermined ratio of the flame retardant is supplied together with the thermoplastic resin to a raw material supply section provided upstream of the extruder and kneaded together with the thermoplastic resin in the extruder can be exemplified. In addition, the flame retardant can be supplied to the thermoplastic resin melt from a flame retardant supply section provided in the extruder. When the flame retardant is supplied to the extruder, a method in which a dry blend of the flame retardant and the thermoplastic resin is supplied to the extruder, a method in which a liquid flame retardant that has been heated and melted in advance is supplied to the extruder, or a method in which a master batch containing the flame retardant and the thermoplastic resin as the base resin is prepared and supplied to the extruder can be adopted. In particular, from the viewpoint of dispersibility, it is preferable to adopt a method in which a master batch containing the flame retardant is prepared and supplied to the extruder. When a master batch containing the flame retardant is prepared and supplied to the extruder, the brominated styrene-butadiene copolymer and the phosphorus-based flame retardant may be supplied as a master batch blended in the same master batch, or each may be supplied as a separate master batch. The same applies to the blending method of the flame retardant auxiliary.
[0041] <Physical foaming agent> The physical foaming agent preferably has zero or extremely low ozone depletion potential and low global warming potential. For the purpose of lowering the thermal conductivity of the extruded polystyrene foam board, it is preferable to use one or more physical foaming agents selected from the group consisting of saturated hydrocarbons having at least 3 to 5 carbon atoms and hydrofluoroolefins (HFOs).
[0042] Specific examples of saturated hydrocarbons having 3 to 5 carbon atoms include propane, butane, and pentane. These blowing agents can be used alone or in combination of two or more. The saturated hydrocarbons having 3 to 5 carbon atoms have an ozone depletion potential of zero, a very small global warming potential, and a low thermal conductivity in a gaseous state.
[0043] Specific examples of hydrofluoroolefins include 1,3,3,3-tetrafluoropropene (hereinafter also referred to as HFO1234ze), 1-chloro-3,3,3-trifluoropropene (hereinafter also referred to as HFO1233zd), 1-chloro-2,3,3,3-tetrafluoropropene (hereinafter also referred to as HFO1224yd), 2,3,3,3-tetrafluoropropene (HFO-1234yf), 1,1,1,4,4,4-hexafluoro-2-butene (HFO-1336mzz), etc. These blowing agents can be used alone or in combination of two or more. The hydrofluoroolefins have an ozone depletion potential of zero, a very small global warming potential, a low thermal conductivity in a gaseous state, and are non-flammable.
[0044] Among the hydrofluoroolefins, from the viewpoint of obtaining an extruded foam board having particularly low thermal conductivity, it is preferable to use one or more selected from HFO1234ze, HFO1233zd, and HFO1224yd. From the viewpoint of further improving the moldability of the obtained extruded foam board and further improving the long-term heat insulation, it is preferable to use HFO1234ze and HFO1233zd in combination as the hydrofluoroolefin.
[0045] The amount of hydrofluoroolefin added is preferably 0.1 mol or more and 1.5 mol or less per 1 kg of base resin. When the amount of hydrofluoroolefin added is within this range, the moldability of the extruded foam board is stable and good, and an effective amount of hydrofluoroolefin remains in the foam insulation board after extrusion foaming, resulting in an extruded foam board with long-term heat insulation. From this perspective, the amount of hydrofluoroolefin added is more preferably 0.3 mol or more and 1.3 mol or less per 1 kg of base resin, more preferably 0.5 mol or more and 1.3 mol or less, and even more preferably 0.7 mol or more and 1.3 mol or less. In particular, when the base resin contains a styrene-(meth)acrylic acid ester copolymer as the main component, good moldability can be ensured even when a relatively large amount of hydrofluoroolefin, for example 0.5 mol / kg or more, is added.
[0046] In the method for producing an extruded polystyrene foam board of the present invention, when a hydrofluoroolefin is added as a physical foaming agent, sufficient flame retardancy can be ensured even if the ratio of the amount of phosphorus-based flame retardant added to the amount of brominated styrene-butadiene copolymer added is in the range of more than 0.15. From this viewpoint, the amount of hydrofluoroolefin added is preferably 0.1 mol or more and 1.5 mol or less, more preferably 0.3 mol or more and 1.3 mol or less, and even more preferably 0.5 mol or more and 1.3 mol or less per 1 kg of base resin.
[0047] Furthermore, the ratio of the amount of hydrofluoroolefin added to the total amount of physical foaming agents added (100 mol %) is preferably 50 mol % or more, more preferably 60 mol % or more, and even more preferably 70 mol % or more.
[0048] Examples of physical blowing agents other than hydrofluoroolefin include aliphatic alcohols having 1 to 5 carbon atoms, water, dialkyl ethers having an alkyl chain with 1 to 3 carbon atoms, and carbon dioxide. These physical blowing agents are preferably added together with hydrofluoroolefin. A preferred example of the aliphatic alcohols having 1 to 5 carbon atoms is ethanol. A preferred example of the dialkyl ethers having an alkyl chain with 1 to 3 carbon atoms is dimethyl ether.
[0049] In particular, from the viewpoint of being able to quickly stabilize the shape of the extruded foam board with high early dissipation properties and being able to stably obtain an extruded foam board with a lower apparent density by using it in combination with hydrofluoroolefin, it is preferable to use water and / or alcohol as the physical foaming agent, and it is even more preferable to use both water and alcohol. The amount of water and / or alcohol added is preferably 0.01 mol or more and 0.6 mol or less, more preferably 0.03 mol or more and 0.3 mol or less, per 1 kg of the base resin. The amount of water and / or alcohol added means the amount added when only one of water and alcohol is used, and means the total amount added when both water and alcohol are used. From the viewpoint of more reliably achieving the above effects, it is preferable to use both water and alcohol and to set the total amount added within the above range. There is no limitation on the blending ratio of the two, but water:alcohol=90mol%:10mol%-50mol%:50mol%, is preferable, and 80mol%:20mol%-60mol%:40mol% is more preferable.
[0050] In addition, it is preferable to use dimethyl ether as a physical foaming agent because it has high compatibility with polystyrene resins and is easy to obtain a lightweight extruded foam board with good appearance when used in combination with hydrofluoroolefin. The amount of dimethyl ether added is preferably 0.05 mol or more and 0.5 mol or less, and more preferably 0.1 mol or more and 0.3 mol or less, per 1 kg of base resin.
[0051] (Radiation suppressant) The heat insulating property can be further improved by adding a radiation suppressant to the base resin. Examples of radiation suppressants include graphite, metal oxides such as titanium oxide, metals such as aluminum, ceramics, carbon black, infrared shielding pigments, hydrotalcite, etc. These can be used alone or in combination. Among them, the radiation suppressant is preferably graphite. Examples of graphite include flake graphite, flake graphite, artificial graphite, and earthy graphite, and it is preferable to use one whose main component is flake graphite.
[0052] The amount of the radiation suppressor added is, for example, in the range of 0.3 to 5 parts by mass, preferably 0.5 to 4 parts by mass, relative to 100 parts by mass of the base resin. When the base resin contains graphite as the radiation suppressor, the content of graphite in the foamable molten resin composition is preferably 0.3 parts by mass or more and 5.0 parts by mass or less, relative to 100 parts by mass of the base resin.
[0053] In general, when the base resin contains graphite as a radiation suppressant, the flame retardancy and moldability of the extruded foam board are likely to be reduced, and especially when a wide extruded foam board is produced, the shapeability of the end of the extruded foam board is likely to be reduced.However, in the method for producing the polystyrene-based resin extruded foam board of the present invention, as described above, the amount of brominated styrene-butadiene copolymer added is 2 parts by mass or more and 12 parts by mass or less per 100 parts by mass of the base resin, and the ratio of the amount of the phosphorus-based flame retardant added to the amount of brominated styrene-butadiene copolymer added is more than 0.15 and 0.5 or less, so that even when the base resin contains graphite as a radiation suppressant, the extruded foam board has excellent flame retardancy and moldability.
[0054] (Other additives) In the present invention, various additives such as cell regulators, colorants such as pigments and dyes, heat stabilizers, and fillers may be added to the base resin as required.
[0055] As the bubble regulator, for example, inorganic powders such as talc, kaolin, mica, silica, calcium carbonate, barium sulfate, aluminum oxide, clay, bentonite, diatomaceous earth, and conventionally known chemical foaming agents such as azodicarbodiamide can be used. Among them, talc is preferable because it does not inhibit flame retardancy and is easy to adjust the bubble size. In particular, it is preferable to use talc having a particle size of 0.1 to 20 μm, more preferably 0.5 to 15 μm, as specified in JIS Z8901 (2006). The amount of the bubble regulator to be added varies depending on the type of bubble regulator, the target bubble size, and the like, but is generally 0.01 to 8 parts by mass, more preferably 0.01 to 5 parts by mass, and particularly preferably 0.05 to 3 parts by mass, relative to 100 parts by mass of the base resin.
[0056] The physical properties of the extruded foam board are described in detail below.
[0057] [Apparent Density] The apparent density of the extruded foam board is set at a lower limit of 20 kg / m from the viewpoint of improving the manufacturing stability and mechanical strength of the foam board. 3 It is preferable that the thickness is 25 kg / m 3 More preferably, it is 30 kg / m 3 From the viewpoint of improving the heat insulating property and ensuring the light weight, the upper limit of the apparent density is 50 kg / m 3 Preferably, it is 45 kg / m 3 More preferably, it is 40 kg / m 3 The apparent density of the extruded foam board can be measured in accordance with JIS K6767 (1999).
[0058] Thickness The thickness of the extruded foam board is appropriately set depending on the purpose of use, and is not particularly limited, but from the viewpoint of use as a heat insulating material, it is preferably 25 mm or more, more preferably 35 mm or more, and even more preferably 45 mm or more. The upper limit of the thickness is about 150 mm.
[0059] [width] The width of the extruded foam plate is 300 mm or more. The upper limit of the width of the extruded foam plate is not particularly limited, but is, for example, 2000 mm or less. The width of the extruded foam plate refers to the width of the foam plate when the foamable molten resin composition is extruded and foamed and molded into a plate shape by a molding tool. Generally, the wider the width of the extruded foam plate, the worse the moldability of the end of the width direction of the extruded foam plate. However, in the manufacturing method of the polystyrene-based resin extruded foam plate of the present invention, the moldability of the end of the extruded foam plate in the width direction is also good. In addition, an extruded foam plate with poor moldability of the end can be made into a product without problems by cutting the end, but in that case, there is a problem that the yield of the extruded foam plate is impaired.
[0060] [Closed bubble rate] From the viewpoint of long-term heat insulation, the closed cell ratio of the extruded foam board is preferably 85% or more, more preferably 90% or more, and even more preferably 92% or more. The closed cell ratio of the extruded foam board is measured by cutting out cut samples from a total of five randomly selected locations of the extruded foam board, determining the closed cell ratio for each measurement sample, and adopting the arithmetic average value of the closed cell ratio at the five locations. The cut sample is a sample without a skin cut into a size of 45 mm length x 20 mm width x 25 mm thickness from the extruded foam board. If the sample is too thin to cut out a 25 mm sample in the thickness direction, for example, two samples (cut samples) cut into a size of 45 mm length x 20 mm width x 12.5 mm thickness are stacked and measured. The closed cell ratio S (%) is calculated by the following formula (1) using the true volume Vx of the extruded polystyrene resin foam board measured using an air comparison type specific gravity meter (for example, Toshiba Beckman Co., Ltd., air comparison type specific gravity meter, model: 930) according to procedure C of ASTM-D2856-70. S(%)=(Vx-W / ρ)×100 / (VA-W / ρ)···(1) Vx: The true volume (cm) of the cut sample determined by measurement using an air-comparison type hydrometer 3 ) (This corresponds to the sum of the volume of the resin constituting the cut sample of the foam and the total volume of the air bubbles in the closed cell portion of the cut sample.) VA: Apparent volume (cm) of the cut sample calculated from the outer dimensions of the cut sample used in the measurement 3 ) W: Total weight of cut sample used for measurement (g) ρ: Density of the base resin constituting the polystyrene resin extruded foam board (g / cm 3 )
[0061] [Thermal Conductivity] The thermal conductivity of the extruded foam board 10 days after production is preferably 0.024 W / (m·K) or less, more preferably 0.023 W / (m·K) or less, and even more preferably 0.022 W / (m·K) or less.
[0062] Thermal conductivity can be measured by cutting a test piece (length 200 mm × width 200 mm × thickness) without any skin from the extruded foam board immediately after production, and storing the test piece for 10 days in an atmosphere of 23°C and 50% humidity, according to the flat plate heat flow meter method (two heat flow meter method, high temperature side 38°C, low temperature side 8°C, average temperature 23°C) described in JIS A 1412-2 (1999).
[0063] [Heat resistance (rate of dimensional change due to heating)] The thermal dimensional change rate of the extruded foam board is within 20%, preferably within 10%, more preferably within 5% in each of the thickness direction, width direction, and length direction when heated in an atmosphere of 80 ° C for 22 hours. If the dimensional change rate at 80 ° C is within the above range, the dimensional change is small, so that even if the extruded foam board is placed flat under the sunlight in summer, the dimensions are unlikely to change and the workability is excellent. The thermal dimensional change rate means the change rate of dimensions due to shrinkage and expansion caused by heating.
[0064] The thermal dimensional deformation rate can be measured by the following method. First, the foamed board is divided into two equal parts at the center in the width direction parallel to the length direction, and a rectangular parallelepiped test piece with a length of 100 mm, a width of 100 mm, and a thickness of 50 mm is cut out from the center including the surface exposed by the division. This test piece is then left at 23°C for at least one day, and the dimensions of each part of the length and width of the test piece are measured with a vernier caliper. Next, the test piece after the dimension measurement is heated for 22 hours in an oven adjusted to an atmosphere of 80°C, and then the heated test piece is left at 23°C for one day, and the dimensions of the same part as before heating are measured.
[0065] The method for producing an extruded polystyrene foam plate of the present invention is not limited to the above-mentioned embodiment. EXAMPLES
[0066] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.
[0067] In the examples and comparative examples, extruded foam boards were produced using the following equipment and raw materials.
[0068] <Extrusion equipment> A manufacturing device was used in which a first extruder with an inner diameter of 180 mm and a second extruder with an inner diameter of 225 mm were connected in series, a physical foaming agent injection port was provided near the end of the first extruder, and a flat die with a resin discharge port (die lip) with a rectangular cross section and a gap of 2.5 mm and a width of 400 mm or 1000 mm was connected to the outlet of the second extruder.
[0069] A shaping device (guider) consisting of a pair of upper and lower polytetrafluoroethylene resin plates was attached to the resin outlet of the flat die so that the upper and lower resin plates were parallel to each other.
[0070] The base resins, flame retardants, physical foaming agents, cell regulators and radiation suppressants used in the examples and comparative examples are shown below. <Base resin> MS750: Styrene-methyl methacrylate copolymer, manufactured by Toyo Styrene Co., Ltd., MS750 M component-75% by mass, styrene component-25% by mass, melt viscosity (200°C, 100 sec -1 )2440 Pa·s MS600: Styrene-methyl methacrylate copolymer, manufactured by Toyo Styrene Co., Ltd., MS600 M component-60% by mass / styrene component-40% by mass, melt viscosity (200°C, 100 sec -1 )2570 Pa·s MS200: Styrene-methyl methacrylate copolymer, manufactured by Toyo Styrene Co., Ltd., MS200 M component-20% by mass / styrene component-80% by mass, melt viscosity (200°C, 100 sec -1 )1980 Pa·s SPET: amorphous polyethylene terephthalate copolymer (ethylene glycol / spiroglycol = 70 mol% / 30 mol%) ALTESTER30 (manufactured by Mitsubishi Gas Chemical Company, Inc.) PS: GPPS, DIC, HP600ANJ, melt viscosity (200℃, 100sec -1 ), 1420 Pa·s <Flame retardants> (Brominated flame retardants) Brominated butadiene-styrene block copolymer: "Emerald innovation 3000" (E3000) manufactured by LANXESS AG Tetrabromobisphenol-A-bis(2,3-dibromo-2-methylpropyl ether): Daiichi Kogyo Seiyaku's "SR-130" / [Tetrabromobisphenol-A-bis(2,3-dibromopropyl ether): Daiichi Kogyo Seiyaku's "SR-720" = 60% by mass / Flame retardant masterbatch containing 40% by mass of mixed flame retardant: Daiichi Kogyo Seiyaku Co., Ltd.'s "GR-134B" (Phosphorus-based flame retardants) TPP (triphenyl phosphate) melting point 50℃, phosphorus content 9.5%, manufactured by Daihachi Chemical Industry Co., Ltd. TPPO (triphenylphosphine oxide), melting point 157°C, phosphorus content 11.0%, manufactured by Hokko Chemical Industry Co., Ltd. PX-200 (aromatic condensed phosphate ester), melting point 95°C, phosphorus content 9.0%, manufactured by Daihachi Chemical Industry Co., Ltd. CDP (cresyl diphenyl phosphate), melting point -38°C, phosphorus content 9.1%, manufactured by Daihachi Chemical Industry Co., Ltd. <Foam regulator> Talc: "Hi-Filler #12" manufactured by Matsumura Sangyo Co., Ltd. <Physical foaming agent> Hydrofluoroolefins (HFO): 1,3,3,3-tetrafluoropropene (HFO-1234ze), 1-chloro-3,3,3-trifluoropropene (HFO1233zd) Isobutane (i-Bu) Dimethyl Ether (DME) Carbon Dioxide (CO2) Ethanol (EtOH) water <Radiation suppressant> Graphite: "CP-N" (flake graphite) manufactured by Nippon Graphite Industries Co., Ltd., primary particle size (d50) = 10 μm Titanium oxide: "JR-405" manufactured by Teika Co., Ltd., primary particle size (d50) = 0.2 μm
[0071] In order to confirm the effect of improving flame retardancy when a brominated styrene-butadiene copolymer is used in combination with a phosphorus-based flame retardant, a non-foamed resin sheet was prepared by the following procedure, and the oxygen index was measured. Specifically, MS200 as a base resin and the type and amount of flame retardant shown in Table 1 were fed to an extruder, melt-kneaded at 200°C, and extruded into a sheet with a thickness of 4 mm. The LOI (oxygen index) was measured using the sheet by the method described below. As shown in Table 1, it was confirmed that the oxygen index was improved to the same extent regardless of the use of any phosphorus-based flame retardant in combination with the brominated styrene-butadiene copolymer. [Table 1]
[0072] The base resin, flame retardant, cell regulator, and radiation suppressant were each fed to an extruder in the blending ratios shown in Tables 1 to 4 below, and a physical foaming agent was further fed from a physical foaming agent feed port, melted and kneaded, and the molten mixture was extruded under atmospheric pressure from a die lip at the tip of the extruder, and then molded into a plate (original plate) having a width shown in Tables 1 to 4 and a thickness of 55 mm using a shaping device (guider). Next, the molded skins on both sides were evenly cut off to a thickness of 50 mm, thereby producing the polystyrene resin extruded foam plates of Examples 1 to 14 and Comparative Examples 1 to 12.
[0073] The extruded foam boards thus produced were measured for apparent density, closed cell ratio, flame retardancy, moldability (surface, edge), LOI (oxygen index), and heat resistance (rate of dimensional change upon heating) by the following methods. <Apparent density> The apparent density was measured in accordance with JIS K6767 (1999). Rectangular samples measuring 50 mm long x 50 mm wide x 50 mm thick were cut from three locations, namely the center and both ends in the width direction of each extruded foam board, and the apparent density of each sample was measured. The arithmetic mean of the measurements at the three locations was used as the apparent density. <Closed bubble rate> Cut samples were cut from three locations, the center and both ends of the width direction of the extruded foam board, to prepare measurement samples. The closed cell ratio of each measurement sample was measured, and the arithmetic average of the closed cell ratios at the three locations was used. The cut samples were cut from the extruded foam board to a size of 25 mm length x 25 mm width x 25 mm thickness. The closed cell ratio of the sample was measured using an air comparison specific gravity meter (Toshiba Beckman Co., Ltd., Model: 930) according to Procedure C of ASTM-D2856-70, and calculated from the above formula (1), and the arithmetic average of the three locations was used as the closed cell ratio. <Thermal insulation> Test pieces measuring 200 mm long x 200 mm wide x 25 mm thick were cut out from the extruded foam boards immediately after production and stored for 10 days in an atmosphere of 23°C and 50% humidity. The thermal conductivity of the test pieces was measured according to the flat plate heat flow meter method (two heat flow meter method, high temperature side 38°C, low temperature side 8°C, average temperature 23°C) described in JIS A1412-2 (1999), and the insulation properties were evaluated according to the following criteria. ○: Thermal conductivity 10 days after manufacture is 0.024 W / (m K) or less ×: Thermal conductivity exceeds 0.024 W / (m K) 10 days after manufacture <Flame retardancy (JIS flammability)> After production, the extruded foam boards were left in an atmosphere of 23°C and 50% humidity for 7 days, and then a flammability test was conducted in accordance with measurement method A of the flammability test method of JIS A9521:2017. For the measurement, 5 test pieces were randomly cut out from each extruded foam board, and the flame retardancy was evaluated according to the following criteria. ○: For all test specimens, the flame goes out within 3 seconds, there is no residual dust, and the specimen does not burn beyond the flammability limit line. ×: The average burning time of the five test pieces exceeds 3 seconds. <Moldability (surface)> Regarding moldability (surface), the surfaces of the original plate before cutting the molded skin and the extruded foam plate after cutting the molded skin were visually observed and evaluated as follows. ⊚: The surfaces of the original plate and the extruded foam plate were extremely good. ◯: Although cracks and tears occurred on the surface of the original plate, the surface of the extruded foam plate was extremely good. △: Cracks and fissures occurred on the surface of the original plate, and even after the original plate was cut, cracks and fissures occasionally remained on the surface of the extruded foam plate. ×: Numerous cracks and tears were observed on the surface of the original plate, and good extruded foam plates could not be obtained stably. <Moldability (ends)> Regarding formability (edges), the width direction edges (side surface) of the original sheet before cutting the molded skin were visually observed and evaluated as follows. ◯: Base plates with smooth edge surfaces were stably produced, and good extruded foam plates were obtained. △: It was possible to manufacture stably, but cracks and fissures rarely occurred on the end surface of the original plate. ×: Cracks and fissures were observed on the end surface of the original plate, and good extruded foam plates could not be obtained stably. <LOI (Oxygen Index)> The extruded foam plate immediately after manufacturing was transferred to a room with a temperature of 23°C and a relative humidity of 50%, and after leaving it in that room for 4 weeks, test pieces were cut out from the extruded foam plate, measured in accordance with JIS K7201 - 2007, and the flame retardancy was evaluated. The type of heat source of the igniter used was liquefied petroleum gas (LPG), the ignition procedure used was Method A, and the test pieces were made to stand independently at a predetermined position inside the testing machine. The temperature of the test location was 23°C and the humidity was 50%. <Heat Resistance (Heating Dimension Change Rate)> For each of the thickness direction, width direction, and length direction of the sample, the 80°C dimension change rate was measured as follows. The measurement of the dimensional deformation rate was first parallel to the length direction of the foam plate, bisected at the center in the width direction, and a rectangular parallelepiped - shaped test piece with a length of 100 mm, a width of 100 mm, and a thickness of 25 mm was cut out from the central part including the surface exposed by the bisection. After leaving this test piece at 23°C for more than one day, the dimensions of each part of the test piece in the thickness direction, width direction, and length direction were measured with a vernier caliper. The test pieces after dimension measurement were each heated in an oven at 80°C for 22 hours, and then, after leaving the heated test pieces at 23°C for one day, the dimensions at the same locations as before heating were measured, and the absolute values of the dimension change rates before and after heating in the thickness direction, width direction, and length direction were respectively obtained from the following formula. Dimension change rate = (1 - [dimension of the test piece after heating / dimension of the test piece before heating]) × 100 The above operations were performed on three test pieces, and the arithmetic - mean value of the absolute values in the thickness direction, width direction, and length direction was taken as the heating dimension change rate. The heat resistance of the extruded foam plate was evaluated based on the following criteria according to the results of the heating dimension change rate (%) of the extruded foam plate calculated above. 〇 (Good): The heating dimension change rate is 20% or less. × (Bad): The heating dimension change rate exceeds 20%.
[0074] The results are shown in Tables 2 to 5.
[0075] [Table 2] [Table 3] [Table 4] [Table 5]
[0076] The extruded foam boards of Examples 1-12 and Comparative Examples 1-8 contain a styrene-(meth)acrylic acid ester copolymer as a base resin, whereas the extruded foam boards of Examples 13 and 14 and Comparative Examples 9-12 contain only polystyrene as a base resin.
[0077] The extruded foam board of Example 1-14 contains a brominated flame retardant consisting of a brominated styrene-butadiene copolymer and a phosphorus-based flame retardant having a melting point of 80° C. or less, the amount of the brominated styrene-butadiene copolymer added is 2 parts by mass or more and 12 parts by mass or less per 100 parts by mass of the base resin, and the ratio of the amount of the phosphorus-based flame retardant having a melting point of 80° C. or less to the amount of the brominated styrene-butadiene copolymer added (the mass ratio of the phosphorus-based flame retardant having a melting point of 80° C. or less to the brominated styrene-butadiene copolymer) is more than 0.15 and 0.5 or less. It was confirmed that the extruded foam board of Example 1-14 has excellent flame retardancy and heat resistance, and also has good moldability.
[0078] In contrast, it was confirmed that Comparative Example 1, which did not contain a phosphorus-based flame retardant, had insufficient flame retardancy and moldability.It was confirmed that Comparative Example 2, in which the ratio of the amount of phosphorus-based flame retardant added to the amount of brominated styrene-butadiene copolymer added was more than 0.5, had insufficient heat resistance.
[0079] It was confirmed that Comparative Examples 3 and 4, in which the melting point of the phosphorus-based flame retardant exceeds 80° C., had insufficient flame retardancy. As shown in Table 1, in the case of a non-foamed resin sheet, the combined use of brominated styrene-butadiene copolymer (bromine-based flame retardant) and each phosphorus-based flame retardant (TPP, TPPO, PX-200, CDP) had the same effect (oxygen index measurement results) for each. Considering this, the above effect in Examples 1-14 is considered to be an effect specific to the extruded foam board, and cannot be predicted from the results in Table 1.
[0080] Comparative Example 5, in which the brominated flame retardant was a brominated bisphenol flame retardant, had insufficient flame retardancy, and Comparative Example 6, in which the amount of the brominated bisphenol flame retardant added was increased, was not moldable. Comparative Example 7, in which the ratio of the amount of the phosphorus-based flame retardant with a melting point of 80° C. or less to the amount of the brominated styrene-butadiene copolymer added (the mass ratio of the phosphorus-based flame retardant with a melting point of 80° C. or less to the amount of the brominated styrene-butadiene copolymer added) was 0.15 or less, was confirmed to have insufficient flame retardancy and moldability. Comparative Example 8, in which the ratio of the amount of the phosphorus-based flame retardant added to the amount of the brominated styrene-butadiene copolymer added was increased but still 0.15 or less, was confirmed to have poor shapeability at the end and insufficient moldability.
[0081] The oxygen index of Comparative Example 9, in which the ratio of the amount of phosphorus-based flame retardant added to the amount of brominated styrene-butadiene copolymer added was 0.15 or less, and that of Comparative Example 10, which did not contain a phosphorus-based flame retardant, was lower than that of Example 13. In addition, it was confirmed that the shapeability at the end was poor in Comparative Example 9 and Comparative Example 10, and the moldability was insufficient. The oxygen index of Comparative Example 11, in which PX-200 having a melting point of more than 80°C was used as the phosphorus-based flame retardant, was lower than that of Example 14. The oxygen index of Comparative Example 12, in which TPPO having a melting point of more than 80°C was used as the phosphorus-based flame retardant, was lower than that of Example 13.
Claims
1. The foaming method includes a step of extruding and foaming a foamable molten resin composition containing a base resin containing a polystyrene resin, a flame retardant, and a physical foaming agent, and molding the composition into a plate shape using a molding tool. 3 More than 50kg / m 3 The following is a method for producing an extruded polystyrene foam board having a width of 300 mm or more, The flame retardant includes a brominated styrene-butadiene copolymer and a phosphorus-based flame retardant having a melting point of 80° C. or less, the amount of the brominated styrene-butadiene copolymer added is 2 parts by mass or more and 12 parts by mass or less per 100 parts by mass of the base resin, A method for producing an extruded polystyrene foam board, wherein the mass ratio of the phosphorus-based flame retardant having a melting point of 80° C. or lower to the brominated styrene-butadiene copolymer is more than 0.15 and is 0.5 or less.
2. The method for producing a polystyrene-based resin extruded foam board according to claim 1, wherein the mass ratio of the phosphorus-based flame retardant having a melting point of 80° C. or less to the brominated styrene-butadiene copolymer is 0.18 or more and 0.5 or less.
3. 3. The method for producing an extruded polystyrene resin foam plate according to claim 1, wherein the foamable molten resin composition contains graphite, and the amount of the graphite added is 0.3 parts by mass or more and 5 parts by mass or less per 100 parts by mass of the base resin.
4. 3. The method for producing an extruded polystyrene foam board according to claim 1, wherein the phosphorus-based flame retardant having a melting point of 80° C. or lower is at least one selected from the group consisting of triphenyl phosphate and cresyl diphenyl phosphate.
5. The method for producing a polystyrene-based resin extruded foam board according to claim 1 or 2, wherein the base resin contains a styrene-(meth)acrylic acid ester copolymer, and the content of the (meth)acrylic acid ester component derived from the styrene-(meth)acrylic acid ester copolymer in the base resin is 8% by mass or more and 40% by mass or less.
6. The method for producing a polystyrene-based resin extruded foam board according to claim 5, wherein the mass ratio of the phosphorus-based flame retardant having a melting point of 80°C or less to the (meth)acrylic acid ester component in the foamable molten resin composition is 0.03 to 0.
15.
7. 3. The method for producing an extruded polystyrene-based resin foam board according to claim 1, wherein the foamable molten resin composition contains a hydrofluoroolefin as the physical foaming agent, and the amount of the hydrofluoroolefin added per 1 kg of the base resin is 0.1 mol or more and 1.3 mol or less.
Citation Information
Patent Citations
Foamable styrene resin particle, its manufacturing method and styrene resin foamed particle molded article
JP2014148558A
Method for producing polystyrene resin expanded material
JP2014227462A
Styrene-based resin extrusion molding
JP2019094472A
Polystyrene-based resin foamed plate and method for producing the same
JP2021080424A
Method for producing polystyrenic resin extrusion foam board, and polystyrenic resin extrusion foam board
JP2022044963A