Solid carbon deposition method, gas mixture production method and solid carbon deposition system

JP2024157350APending Publication Date: 2024-11-07TAIHEIYO CEMENT CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023071666
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-07

AI Technical Summary

Benefits of technology

【0019】 本発明によれば、より簡便に固体炭素を析出させることができ、CO2の固定化において原料ガスから析出される固体炭素の回収率を向上させることができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157350000001_ABST
    Figure 2024157350000001_ABST
Patent Text Reader

Abstract

To provide a solid carbon deposition method, a gas mixture production method and a solid carbon deposition system that allow for simplified deposition of solid carbon, while enabling enhanced rates of recovery of solid carbon deposited from a raw gas through CO2 fixation.SOLUTION: A solid carbon deposition method includes a first step in which a raw gas containing carbon dioxide and hydrogen is exposed to a catalyst that activates the reverse shift reaction, producing carbon monoxide and water from the raw gas, a second step in which a gas containing the produced carbon monoxide is exposed to a catalyst that activates the solid carbon deposition reaction, depositing solid carbon from the produced carbon monoxide. The raw gas has a H2 / CO2 molar ratio of 4.5 or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for depositing solid carbon, a method for producing a mixed gas, and a system for depositing solid carbon. [Background technology]

[0002] At present, there is an urgent need worldwide to reduce and fix carbon dioxide, which is a greenhouse gas that has a negative impact on the environment. In response to this, various technologies, such as CO2 emission reduction technology, CO2 separation and capture technology, CO2 useful resource conversion technology, and CO2 fixation technology, are being researched and developed for practical use in various places.

[0003] Known methods for effectively utilizing carbon dioxide include, for example, a technique for converting carbon dioxide into carbon monoxide or methane and using it as fuel, and a technique for precipitating solid carbon. Known techniques for converting carbon dioxide into carbon monoxide include, for example, a method for producing carbon monoxide from carbon dioxide and hydrogen by utilizing a reverse shift reaction (see Patent Documents 1 to 5).

[0004] Patent Documents 1 and 2 disclose a method for producing a synthesis gas by contacting a feed gas containing carbon dioxide and hydrogen with a reverse shift reaction catalyst made of a composite oxide containing at least one of Ca, Sr, and Ba, and at least one of Ti and Zr, at a temperature of 700° C. or higher.

[0005] Patent Documents 3 and 4 disclose a reaction vessel having a reverse shift catalyst capable of converting a gas containing carbon dioxide and hydrogen into a gas containing carbon monoxide and water vapor, and an adsorbent that adsorbs water vapor.

[0006] Patent Document 5 discloses a fuel synthesis device that removes water vapor by a water-gas shift reaction from a gas that has passed through a reactor having a reverse shift reaction catalyst, and returns the gas from which water vapor has been removed upstream of the reactor, thereby improving the fuel production rate by the reverse shift reaction catalyst. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] International Publication No. 2011 / 065194 [Patent Document 2] International Publication No. 2012 / 153762 [Patent Document 3] Patent Publication No. 2021-070616 [Patent Document 4] Patent Publication No. 2022-171010 [Patent Document 5] JP 2022-143792 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, in the above Patent Documents 1 to 5, the composition ratio of the raw material gas supplied to the reactor in which the reverse shift reaction occurs is not fully considered. In Patent Documents 1 to 4, the ratio of hydrogen to carbon dioxide in the raw material gas is 2 to 4, but the composition ratio of the raw material gas and the results are not considered. Therefore, there is still room for improvement in the conditions including the composition ratio of the raw material gas.

[0009] Furthermore, methods for precipitating solid carbon using the reverse shift reaction have not been fully investigated. Known solid carbon precipitation methods include, for example, a method using a methanation reaction, a dry reforming reaction, and a solid carbon precipitation reaction, in which solid carbon is precipitated from a feed gas containing carbon dioxide and hydrogen through a three-stage reaction. In addition to the fact that three reactors are required for the three-stage reaction, stable operation and management are difficult due to the long process involved in solid carbon precipitation. Therefore, there is a demand for a technology that can precipitate solid carbon from carbon dioxide in a simpler way.

[0010] The present invention has been made in consideration of the above circumstances, and aims to provide a solid carbon deposition method, a mixed gas production method, and a solid carbon deposition system that can more easily deposit solid carbon and improve the recovery rate of solid carbon deposited from a raw material gas in the fixation of CO2. [Means for solving the problem]

[0011] (1) In order to achieve the above object, the method for precipitating solid carbon of the present invention includes a first step of contacting a feed gas containing carbon dioxide and hydrogen with a catalyst that activates a reverse shift reaction to produce carbon monoxide and water from the feed gas, and a second step of contacting the produced carbon monoxide-containing gas with a catalyst that activates a solid carbon deposition reaction to precipitate solid carbon from the produced carbon monoxide, wherein the feed gas has an H2 / CO2 molar ratio of 4.5 or more.

[0012] (2) In the method for precipitating solid carbon described in (1) above, the raw material gas has a H2 / CO2 molar ratio of 2.1 or more and 3.2 or less.

[0013] (3) Moreover, the method for precipitating solid carbon according to (1) or (2) above further comprises a step of separating hydrogen from the gas produced in the first step, and as a result of adjusting the amount of separated hydrogen, the produced gas containing carbon monoxide has an H / CO molar ratio of 1.0 or more and 2.0 or less.

[0014] (4) In the method for precipitating solid carbon according to any one of the above (1) to (3), the catalyst for activating the reverse shift reaction is any one of a simple substance, a compound, and a mixture thereof, containing at least one of Mn, Fe, Co, Ni, Cu, and Zn.

[0015] (5) In addition, in the method for precipitating solid carbon according to any one of the above (1) to (4), the catalyst for activating the reverse shift reaction is supported on the surface of a structure whose main raw material is a material having a melting point of 700° C. or higher.

[0016] (6) Furthermore, the method for producing a mixed gas of the present invention includes a step of contacting a raw material gas containing carbon dioxide and hydrogen with a catalyst that activates a reverse shift reaction to produce carbon monoxide and water from the raw material gas, wherein the raw material gas has a H2 / CO2 molar ratio of 4.5 or more.

[0017] (7) Further, a solid carbon deposition system of the present invention is a solid carbon deposition system for depositing solid carbon from a feed gas containing carbon dioxide and hydrogen, comprising: a first reactor for bringing the feed gas into contact with a catalyst for activating a reverse shift reaction to produce carbon monoxide and water from the feed gas; a second reactor for bringing the produced carbon monoxide into contact with a catalyst for activating a solid carbon deposition reaction to precipitate solid carbon from the produced carbon monoxide; and a control unit for controlling the flow rate of each gas circulating within the solid carbon deposition system, wherein the control unit controls the H2 / CO2 molar ratio in the feed gas within a specified range.

[0018] (8) Moreover, the solid carbon system described in (7) above is characterized in that it further comprises a hydrogen separation flow path that separates hydrogen from the gas discharged from the first reactor, and the control unit controls each gas flow rate, including the gas flow rate of the hydrogen separation flow path, so that the H2 / CO molar ratio in the mixed gas supplied to the second reactor is within a specified range. Effect of the Invention

[0019] According to the present invention, solid carbon can be precipitated more simply, and the recovery rate of solid carbon precipitated from a feed gas in the fixation of CO2 can be improved. [Brief description of the drawings]

[0020] [Figure 1] 1 is a schematic diagram showing a configuration of a solid carbon deposition device according to the present invention. [Diagram 2] 1 is a schematic diagram showing the configuration of a solid carbon deposition system according to the present invention. [Diagram 3] 1 is a table showing various conditions and measurement results in Examples 1 to 3 and Comparative Examples 1 to 6. [Figure 4] FIG. 2 is a schematic diagram showing a spiral catalyst. [Diagram 5] 1 is a table showing various conditions and measurement results in Examples 4 to 11 and Comparative Example 7. [Figure 6] 1 is a table showing various conditions and measurement results in Examples 12 to 20 and Comparative Example 8. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] [principle] The method for depositing solid carbon of the present invention utilizes a solid carbon deposition reaction including a reverse shift reaction and a Boudoir reaction. The method for depositing solid carbon utilizing the reverse shift reaction and the solid carbon deposition reaction can be represented by the following reaction formula: CO2+H2→CO+2H2O…(Formula 1) 2CO→C+CO2…(Formula 2)

[0022] As shown in formula 1, first, a reverse shift reaction occurs to convert carbon dioxide and hydrogen into carbon monoxide. Next, as shown in formula 2, solid carbon is precipitated from the carbon monoxide by a solid carbon precipitation reaction, and the solid carbon is recovered. In this way, solid carbon can be precipitated from carbon dioxide through a two-stage reaction.

[0023] The reverse shift reaction is an equilibrium reaction. In the low temperature range, the forward shift reaction shown in Equation 3 is favored, and in the high temperature range, the reverse shift reaction is favored. Therefore, in order to produce a mixed gas, it is necessary to make the reverse shift reaction proceed at high temperatures. CO+2H2O→H2+CO2…(Formula 3)

[0024] In addition, the methanation reaction shown in Equation 4 and Equation 5 may occur as a side reaction of the reverse shift reaction, and if the methanation reaction occurs, methane is produced and the carbon monoxide concentration decreases. Therefore, it is required to suppress the methanation reaction by using a reverse shift reaction catalyst at high temperatures and to allow only the reverse shift reaction to proceed. CO2+4H2→CH4+2H2O…(Formula 4) CO2+3H2→CH4+H2O…(Formula 5)

[0025] [Configuration of solid carbon deposition device] An embodiment of the present invention will be described below.

[0026] Fig. 1 shows a solid carbon deposition apparatus according to the present invention. The solid carbon deposition apparatus 1 is an apparatus for depositing solid carbon from process exhaust gas containing carbon dioxide. The process exhaust gas refers to exhaust gas containing carbon dioxide emitted from a cement clinker burning process, a quicklime manufacturing process, a thermal power plant, a waste incineration treatment facility, a ceramics burning facility, an ironworks, and a chemical plant.

[0027] As shown in Fig. 1, the solid carbon deposition apparatus 1 has two reactors in which different reactions occur, and the two reactors are connected in series. When the reactor to which the raw material gas is supplied is designated as the first reactor 10, the reaction proceeds in the order of the first reactor 10 and the second reactor 20, and solid carbon is deposited in the second reactor 20.

[0028] In addition to the two reactors, the solid carbon deposition apparatus 1 includes a hydrogen supplying equipment 3, a hydrogen flowmeter 4, a gas mixer 5, a hydrogen separator 7, water vapor removal equipment 41, 42 and a flowmeter 50 provided at the outlet of each reactor. The solid carbon deposition apparatus 1 also preferably includes equipment 61 for removing sulfur oxides that cause catalyst deterioration, a carbon dioxide concentration equipment 62, a gas circulation equipment 70 that can recycle and reuse the gas discharged from each reactor, and the like. If nitrogen or oxygen is contained in the process exhaust gas, the absolute amount of the raw material gas will be large, so the apparatus may further include equipment for removing nitrogen or oxygen from the process exhaust gas upstream of the first reactor.

[0029] The gas mixer 5 mixes hydrogen supplied from the hydrogen supply equipment 3 with the process exhaust gas containing carbon dioxide to generate a raw material gas to be supplied to the first reactor 10. At this time, the raw material gas is mixed so that the molar ratio of H2 / CO2 is 4.5 or more. The molar ratio of H2 / CO2 in the raw material gas is preferably 5.0 or more, more preferably 6.0 or more, and even more preferably 7.0 or more. Since the molar ratio of H2 / CO2 in the raw material gas is 4.5 or more, the conversion rate to carbon monoxide in the first reactor 10 can be improved, and the recovery rate of solid carbon precipitated from the raw material gas can be improved. In addition, it is preferable that the process exhaust gas is supplied to the gas mixer 5 after removing sulfur oxides by the sulfur oxide removal equipment 61 and concentrating carbon dioxide by the carbon dioxide concentration equipment 62. In addition, when the gas circulation equipment 70 is provided, the off-gas discharged from the second reactor 20 may be mixed with the raw material gas. In addition, it is preferable that the gas mixer 5 is provided with a flowmeter that measures the flow rate of the gas supplied to the first reactor 10.

[0030] The first reactor 10 contacts the raw gas supplied from the gas mixer 5 with a catalyst that activates the reverse shift reaction, and produces carbon monoxide and water from the raw gas as shown in formula 1. The raw gas is preferably supplied to the first reactor 10 so that the space velocity is 2000 to 20000 / h. The first reactor 10 includes a gas flow reaction tube filled with a catalyst that activates the reverse shift reaction, and a heating furnace that can heat the gas flow reaction tube to 700°C or higher. The heating furnace is preferably capable of heating the gas flow reaction tube to 750°C or higher, more preferably 800°C or higher, and even more preferably 850°C or higher. The first reactor 10 is, for example, a normal pressure flow reactor that is a fixed gas flow tube, since the gas flow path is not blocked by solid products.

[0031] The catalyst for activating the reverse shift reaction is any one of a simple substance, a compound, and a mixture thereof, containing at least one of Mn, Fe, Co, Ni, Cu, and Zn. An example of the compound is calcium aluminoferrite (C4AF). An example of the mixture is cement clinker, hydrated cement clinker, cement paste, mortar, concrete, and the like. In addition, various oxides and aluminosilicates such as CeO2, ZrO2, Y2O3, and Al2O3 can be used as the carrier. The shape of the catalyst may be any shape as long as a predetermined space velocity can be achieved, but a spiral shape is preferable because it requires a small volume of the catalyst.

[0032] The catalyst for activating the reverse shift reaction may be supported on the surface of a structure made mainly of a material having a melting point of 700°C or more. The structure is required to be made mainly of a material that can withstand heating by a heating furnace, and is therefore required to have a melting point of at least 700°C or more. Examples of materials having a melting point of 700°C or more include steel, copper, titanium, nickel, etc., and stainless steel is preferable because it reduces material costs. The main material of the structure is preferably selected according to the temperature at which the catalyst is heated, and when the heating temperature is 1000°C, it is preferable to use a material having a melting point of 1000°C or more as the main material of the structure. As described above, since the catalyst is preferably spiral, a plate-shaped structure may be formed into a spiral shape and a paste-like catalyst may be applied to the spiral structure to produce a catalyst for activating the reverse shift reaction.

[0033] The mixed gas supplied to the second reactor is preferably adjusted so that the H2 / CO molar ratio is 1.0 or more and 2.0 or less. The H2 / CO molar ratio in the mixed gas supplied to the second reactor is more preferably 1.1 or more and 2.0 or less. Since the mixed gas supplied to the second reactor has an H2 / CO molar ratio of 1.0 or more and 2.0 or less, the deposition rate of solid carbon can be improved. The mixed gas supplied to the second reactor is adjusted by separating hydrogen using the hydrogen separator 7, mixing off-gas using the second gas mixer, etc.

[0034] The hydrogen separator 7 separates hydrogen from the gas discharged from the first reactor 10. In the example shown in Fig. 1, the hydrogen separated by the hydrogen separator 7 is supplied to the gas mixer 5 through a hydrogen circulation line 75. The hydrogen separator 7 may be one that utilizes, for example, a PSA method, a membrane separation method, or a chemical adsorption method.

[0035] The second reactor 20 brings the mixed gas containing carbon monoxide supplied from the first reactor 10 into contact with a catalyst that activates a solid carbon deposition reaction, and deposits solid carbon from the carbon monoxide as shown in formula 2. The mixed gas supplied to the second reactor 20 is preferably supplied so that the space velocity is a maximum of 2000 / h. The second reactor 20 includes a gas flow reaction tube filled with a catalyst that activates a solid carbon deposition reaction, and a heating furnace that can heat the gas flow reaction tube to 400 to 500°C. The second reactor 20 is preferably one that can continuously discharge the catalyst on which solid carbon has been deposited, and can continuously supply new catalyst into the reactor, and is preferably, for example, a fluidized bed, a moving bed, or a rotary kiln.

[0036] The catalyst that activates the solid carbon deposition reaction can be one that can deposit solid carbon from carbon monoxide, and can be Ni or Fe, but iron-based catalysts are preferable from an environmental perspective. Various oxides and aluminosilicates, such as CeO2, ZrO2, Y2O3, and Al2O3, can be used as supports. The catalyst can be of any shape as long as it can achieve a predetermined space velocity, but a spiral shape is preferable because it requires a small catalyst volume. When making the catalyst into a spiral shape, it is produced by forming a metal plate member, such as stainless steel, into a spiral shape and applying a paste-like catalyst to it.

[0037] The gas circulation equipment 70 has a first off-gas circulation path 71 that supplies the off-gas discharged from the second reactor 20 to the first reactor 10, and a hydrogen circulation path 75 that supplies the hydrogen separated by the hydrogen separator 7 to the first reactor 10. The off-gas discharged from the second reactor 20 contains carbon dioxide. Therefore, when the off-gas is supplied to the first reactor 10 through the first off-gas circulation path 71, the mixed gas can be used as a raw material for the raw material gas without being discharged to the outside, and the emission of carbon dioxide can be prevented.

[0038] 1, water vapor removal equipment 41, 42 is provided at the outlet of each reactor. The water vapor removal equipment 41, 42 cools the gas discharged from the outlet of the target reactor to condense the water vapor, and discharges it as industrial wastewater.

[0039] In the reverse shift reaction in the first reactor 10, water vapor is generated, and if the mixed gas containing water vapor is transferred to the second reactor 20, the solid carbon deposition rate may decrease. Therefore, it is preferable to provide a first water vapor removal device 41 at the outlet of the first reactor 10 to actively remove water vapor. In addition, although the solid carbon deposition reaction is dominant in the second reactor 20, it is considered that a reaction generating water vapor may occur in some part. Therefore, it is preferable to provide a second water vapor removal device 42 at the outlet of the second reactor 20 as well.

[0040] In order to adjust the composition ratio of the mixed gas, it is preferable to install a sensor that measures the composition ratio of the gas supplied to the gas mixer 5, a valve capable of adjusting the flow rate of each mixed gas, and the gas mixer 5. The sensor may be one that can grasp at least the component ratios of hydrogen, methane, carbon dioxide, and carbon monoxide, and it is preferable that the valve capable of adjusting the flow rate of each mixed gas is installed not only at the outlet where the process exhaust gas is discharged and at the hydrogen supply facility 3, but also when the mixed gas discharged from the first reactor 10 and the mixed gas discharged from the second reactor 20 are recycled to each gas mixer.

[0041] In addition, in the solid carbon deposition apparatus 1, the reaction in the first reactor 10 is an endothermic reaction, whereas the reaction in the second reactor 20 is an exothermic reaction. Therefore, it is preferable to recover the sensible heat of the mixed gas discharged from the second reactor 20 by a heat exchanger and use it as an energy source for the first reactor 10.

[0042] [Solid carbon deposition system] Next, the solid carbon deposition system will be described. Fig. 2 is a schematic diagram showing the configuration of the solid carbon deposition system. The solid carbon deposition system 500 controls the composition ratio of the mixed gas supplied to each reactor in the solid carbon deposition device 1 to be within a specified range. The specification may be made by a user, but may also be made by a previous setting, a setting by automatic calculation, or an instruction via a network.

[0043] The solid carbon deposition system 500 includes a solid carbon deposition apparatus 1 and a gas composition ratio control device 100. The gas composition ratio control device 100 includes a memory unit 110, an operation unit 120, and a control unit 130. The memory unit 110 records values ​​measured in the solid carbon deposition apparatus 1. The values ​​measured in the solid carbon deposition apparatus 1 include, for example, the composition ratio of the gas supplied to the gas mixer 5, such as the composition ratio of the mixed gas and the process exhaust gas discharged from each reactor.

[0044] The operation unit 120 is a device that allows the user to input as desired, such as a keyboard, a mouse, or a touch panel. The user can input any range for the composition ratio of the mixed gas supplied to each reactor via the operation unit 120. The control unit 130 controls the composition ratio of the mixed gas to be within the specified range based on the data recorded in the storage unit 110. Specifically, the control unit 130 recognizes the gas flow rate from each facility and controls the valves of the gas supplied to the gas mixer 5 and the hydrogen separator 7, thereby controlling the composition ratio of the mixed gas in the gas mixer 5 to be within the specified range.

[0045] In this embodiment, an example has been described in which the composition ratio of the mixed gas in all reactors is controllable, but it is sufficient that the molar ratio of H2 / CO2 in the raw material gas supplied to at least the first reactor 10 is controllable within a specified range, and it is not necessary that the composition ratio of the mixed gas supplied to the second reactor 20 is controllable.

[0046] [Solid carbon deposition method] Next, a method for precipitating solid carbon will be described.

[0047] First, the raw material gas to be supplied to the first reactor 10 is adjusted. The raw material gas is prepared by mixing hydrogen supplied from the hydrogen supply equipment 3 with process exhaust gas containing carbon dioxide, and is adjusted so that the molar ratio of H2 / CO2 is 4.5 or more.

[0048] Next, the raw material gas is supplied to the first reactor 10, and the raw material gas is passed through the gas flow reaction tube of the first reactor 10. The gas flow reaction tube is filled with a catalyst heated to 700°C or higher by a heating furnace, and the raw material gas comes into contact with the catalyst that activates the reverse shift reaction, generating carbon monoxide from the raw material gas. By heating the catalyst that activates the reverse shift reaction to 700°C or higher, the methanation reaction can be suppressed. In addition, since the conversion rate to carbon monoxide can be improved, it is preferable that the molar ratio of the raw material gas H2 / CO2 supplied to the first reactor is 8.0 or higher and the catalyst is heated to 800°C or higher. In addition, since the conversion rate to carbon monoxide becomes 1.00, it is more preferable that the molar ratio of the raw material gas H2 / CO2 supplied to the first reactor is 9.97 or higher and the catalyst is heated to 850°C or higher.

[0049] Next, the mixed gas discharged from the first reactor 10 is supplied to the second reactor 20, and the mixed gas is caused to flow through the gas flow reaction tube of the second reactor 20. The gas flow reaction tube is filled with a catalyst heated to about 450°C by a heating furnace, and the mixed gas comes into contact with the catalyst that activates the solid carbon deposition reaction, carbon monoxide becomes solid carbon, and solid carbon deposits on the surface of the catalyst. Then, the solid carbon can be recovered by recovering the catalyst on which the solid carbon has been deposited.

[0050] From the above, in the method for precipitating solid carbon in the present invention, the raw material gas can be continuously reacted from the supply to the first reactor until solid carbon is precipitated in the second reactor. This makes the treatment more efficient than when each reaction is independent. In addition, since solid carbon is precipitated by a two-stage reaction, not only can the equipment cost be reduced, but operation management can also be made easier. As a result, solid carbon can be precipitated more simply than when solid carbon is precipitated by a three-stage reaction. In addition, since the molar ratio of H2 / CO2 in the raw material gas is 4.5 or more, the ratio of carbon dioxide converted to carbon monoxide is 0.8 or more.

[0051] In addition, the mixed gas discharged from the first reactor contains a large amount of carbon monoxide. Therefore, it may be used as an industrial raw material gas or a fuel gas used for producing chemical products other than solid carbon. In the above embodiment, all of the mixed gas discharged from the first reactor is flowed into the second reactor to precipitate solid carbon, but a configuration in which a part of the mixed gas can be taken out to the outside may also be used. In addition, the first reactor and the second reactor may be independent from each other.

[0052] [Example] The present inventors used calcium aluminoferrite, magnetite and a Ni-based catalyst as a catalyst for activating the reverse shift reaction, and investigated the molar ratio of the raw material gas and the reaction temperature.

[0053] (Calcium Aluminoferrite) Comparative Example 1 The heating furnace constituting the first reactor was a one-zone electric furnace (ceramic electric tubular furnace manufactured by Asahi Rika Seisakusho, effective length 300 mm) capable of temperature control, and the atmospheric pressure flow reaction tube was a quartz tube with an inner diameter of 8 mm and a length of 600 mm. Granular calcium aluminoferrite (C4AF) was placed at the position of the thermocouple for temperature control of the heating furnace inside the atmospheric pressure flow reaction tube as a catalyst for activating the reverse shift reaction.

[0054] The manufacturing procedure and conditions of granular calcium aluminoferrite are explained below. CaCO3, Al(OH)3, and Fe2O3 were placed in a mortar and wet mixed with ethanol. At this time, CaCO3, Al(OH)3, and Fe2O3 were placed in the mortar so that the molar ratio was CaCO3:Al(OH)3:Fe2O3=4:2:1. After wet mixing, the mixture was dried for about 12 hours and molded. The molded product was fired at 1350°C for 2 hours in an electric furnace, cooled, crushed in a ball mill, and molded again. The firing, crushing, and molding were repeated until the firing in the electric furnace was performed a total of three times. After the third firing in the electric furnace was completed and cooled, the product was crushed in a ball mill and classified using a sieve to obtain a calcium aluminoferrite (C4AF) catalyst.

[0055] The raw materials for the calcium aluminoferrite catalyst, CaCO3, Al(OH)3, and Fe2O3, were as follows: CaCO3: Reagent manufactured by Kanto Chemical Co., Ltd. Al(OH)3: Reagent manufactured by Kanto Chemical Co., Ltd. Fe2O3: Reagent manufactured by Fujifilm Wako Pure Chemical Corporation

[0056] After preparing the first reactor, the temperature was kept at 550°C for 1 hour while flowing hydrogen at 200 ml / min in order to reduce the catalyst. Next, after the first reactor reached the controlled temperature of 850°C, a standard hydrogen gas cylinder was used as hydrogen supply equipment 3, and a standard carbon dioxide gas cylinder was used instead of the process exhaust gas, and the raw material gas was supplied to the first reactor via a mass flow controller and a gas mixer.

[0057] At this time, the flow rate of carbon dioxide was set to 247 ml / min, the flow rate of hydrogen was set to 73 ml / min, and the total flow rate of the raw material gas was set to 320 ml / min by mass flow controllers so that the H2 / CO2 molar ratio in the raw material gas was 0.30, and the raw material gases were supplied to the first reactor.

[0058] A water vapor removal device and a sampling hole were installed at the outlet of the first reactor. Thirty minutes after the indicated temperature of the first reactor reached the set temperature, a syringe was used to sample from the sampling hole, and hydrogen, nitrogen, oxygen, methane, carbon monoxide, and carbon dioxide were quantitatively analyzed using a gas chromatograph GC-2014 (Shimadzu Corporation).

[0059] The conversion rate to CO was calculated by the following formula 6. A conversion rate to CO of less than 0.80 was evaluated as failing, 0.80 or more as good, and 1.00 as very good. In addition, the methane concentration in the mixed gas discharged from the first reactor was evaluated as failing when it exceeded 5%, and passing when it was 5% or less. Conversion rate to CO = (CO concentration) / (CO concentration + CO2 concentration + CH4 concentration)...(Equation 6)

[0060] Comparative Example 2 The same procedure as in Comparative Example 1 was carried out, except that the flow rates of carbon dioxide and hydrogen were set to 201 ml / min, 112 ml / min, and the molar ratio of H2 / CO2 in the raw material gas was set to 0.56.

[0061] Comparative Example 3 The same procedure as in Comparative Example 1 was carried out, except that the flow rates of carbon dioxide and hydrogen were 143 ml / min, 161 ml / min, and the molar ratio of H2 / CO2 in the raw material gas was 1.13.

[0062] Comparative Example 4 The same procedure as in Comparative Example 1 was carried out, except that the flow rates of carbon dioxide and hydrogen were 108 ml / min, 190 ml / min, and the molar ratio of H2 / CO2 in the raw material gas was 1.76.

[0063] Comparative Example 5 The same procedure as in Comparative Example 1 was carried out, except that the flow rates of carbon dioxide and hydrogen were 85 ml / min, 210 ml / min, and the molar ratio of H2 / CO2 in the raw material gas was 2.47.

[0064] Example 1 The same procedure as in Comparative Example 1 was carried out, except that the flow rates of carbon dioxide and hydrogen were 47 ml / min, 237 ml / min, and the molar ratio of H2 / CO2 in the raw material gas was 5.04.

[0065] Example 2 The same procedure as in Comparative Example 1 was carried out, except that the flow rates of carbon dioxide and hydrogen were 39 ml / min, 248 ml / min, and the molar ratio of H2 / CO2 in the raw material gas was 6.36.

[0066] Example 3 The same procedure as in Comparative Example 1 was carried out, except that the flow rates of carbon dioxide and hydrogen were 39 ml / min, 389 ml / min, and the molar ratio of H2 / CO2 in the raw material gas was 9.97.

[0067] Comparative Example 6 The same procedure as in Comparative Example 1 was repeated, except that the flow rates of carbon dioxide and hydrogen were 143 ml / min, 161 ml / min, the H2 / CO2 molar ratio in the raw material gas was 1.13, and the control temperature was 1000°C.

[0068] (Experimental Results) The experimental results of Examples 1 to 3 and Comparative Examples 1 to 6 are shown in Figure 3. Figure 3 shows the H2 / CO2 molar ratio in the raw material gas, the gas concentrations of hydrogen, methane, carbon dioxide and carbon monoxide in the mixed gas sampled from a sampling hole provided at the outlet of the first reactor, and the CO conversion rate.

[0069] In Examples 1 to 3, the conversion rate to CO was 0.8 or more, which was good. In Example 3, in which the molar ratio of H2 / CO2 in the raw material gas was 9.97 and the control temperature was 850°C, the conversion rate to CO was 1.0, which was very good. In contrast, in Comparative Examples 1 to 6, in which the molar ratio of H2 / CO2 in the raw material gas was less than 5.0, the conversion rate to CO was less than 0.8. In addition, the concentration of methane in the mixed gas discharged from the first reactor was 0% in all of Examples 1 to 3 and Comparative Examples 1 to 6. From this, it was confirmed that the conversion rate to CO can be improved by setting the molar ratio of H2 / CO2 in the raw material gas to 4.5 or more.

[0070] (Magnetite) Example 4 The preparation was the same as in Comparative Example 1, except that magnetite was used as a catalyst instead of calcium aluminoferrite to activate the reverse shift reaction, the flow rates of carbon dioxide and hydrogen were 57 ml / min, 343 ml / min, the H2 / CO2 molar ratio in the raw gas was 6.02, and the control temperature was 750°C.

[0071] The manufacturing procedure and conditions for the catalyst using magnetite are explained below. Magnetite (Fe3O4 reagent: 98% Wako Pure Chemical Industries) was mixed with distilled water to make a paste. As shown in Figure 4, two spirally twisted stainless steel plates (SUS304, width 7 mm x length 50 mm, thickness 0.5 mm) were prepared, and the magnetite paste was applied to the surface of each stainless steel plate and dried to create the catalyst.

[0072] Example 5 The same procedure as in Example 4 was carried out, except that the controlled temperature was set to 800°C.

[0073] Example 6 The same operations as in Example 4 were carried out except that the flow rates of carbon dioxide and hydrogen were 45 ml / min, 355 ml / min, and the molar ratio of H2 / CO2 in the raw material gas was 7.89.

[0074] Example 7 The same procedure as in Example 4 was carried out, except that the flow rate of carbon dioxide was 45 ml / min, the flow rate of hydrogen was 355 ml / min, the molar ratio of H2 / CO2 in the raw material gas was 7.89, and the control temperature was 800°C.

[0075] Comparative Example 7 The procedure was the same as in Example 4, except that the flow rate of carbon dioxide was 112 ml / min, the flow rate of hydrogen was 94 ml / min, the molar ratio of H2 / CO2 in the raw material gas was 0.84, and the control temperature was 850°C.

[0076] Example 8 The same procedure as in Example 4 was carried out, except that the flow rate of carbon dioxide was 67 ml / min, the flow rate of hydrogen was 333 ml / min, the molar ratio of H2 / CO2 in the raw material gas was 4.97, and the control temperature was 850°C.

[0077] Example 9 The same procedure as in Example 4 was carried out, except that the flow rate of carbon dioxide was 57 ml / min, the flow rate of hydrogen was 343 ml / min, the molar ratio of H2 / CO2 in the raw material gas was 6.02, and the control temperature was 850°C.

[0078] Example 10 The same procedure as in Example 4 was carried out, except that the flow rate of carbon dioxide was 50 ml / min, the flow rate of hydrogen was 350 ml / min, the molar ratio of H2 / CO2 in the raw material gas was 7.00, and the control temperature was 850°C.

[0079] Example 11 The same procedure as in Example 4 was carried out, except that the flow rate of carbon dioxide was 45 ml / min, the flow rate of hydrogen was 355 ml / min, the molar ratio of H2 / CO2 in the raw material gas was 7.89, and the control temperature was 850°C.

[0080] (Experimental Results) The experimental results of Examples 4 to 11 and Comparative Example 7 are shown in Fig. 5. Fig. 5 shows the H2 / CO2 molar ratio in the raw material gas, the gas concentrations of hydrogen, methane, carbon dioxide and carbon monoxide in the mixed gas sampled from a sampling hole provided at the outlet of the first reactor, and the CO conversion rate.

[0081] In Examples 4 to 11, the conversion rate to CO was 0.8 or more, which was good. In Example 11, in which the molar ratio of H2 / CO2 in the raw material gas was 7.89 and the control temperature was 850°C, the conversion rate to CO was 1.0, which was very good. In contrast, in Comparative Example 7, in which the molar ratio of H2 / CO2 in the raw material gas was less than 4.5, the conversion rate to CO was less than 0.8. In addition, the concentration of methane in the mixed gas discharged from the first reactor was 0% in both Examples 4 to 11 and Comparative Example 7. From this, it was confirmed that the conversion rate to CO can be improved by setting the molar ratio of H2 / CO2 in the raw material gas to 4.5 or more.

[0082] (Ni-based catalyst) Comparative Example 8 The preparation was the same as in Comparative Example 1, except that a Ni-based catalyst was used instead of calcium aluminoferrite as a catalyst for activating the reverse shift reaction, the flow rates of carbon dioxide and hydrogen were 57 ml / min, 343 ml / min, the H2 / CO2 molar ratio in the raw gas was 6.02, and the control temperature was 600°C.

[0083] The manufacturing procedure and conditions for the Ni-based catalyst are explained below. γAl2O3 (a reagent manufactured by Showa Denko K.K.) was used as a support, and 10 wt% of Ni(NO3)2·6H2O (98% manufactured by Wako Pure Chemical Industries) was supported by the evaporation-to-dry method. After supporting, the catalyst was fired at 500℃ for 2 hours in an air atmosphere to separate the nitric acid component. After cooling the fired product, distilled water was added and it was ground in a mortar to produce a Ni / γAl2O3 paste.

[0084] In addition to the Ni / γAl2O3 paste, two stainless steel plates (SUS304, width 7 mm x length 50 mm, thickness 0.5 mm) were prepared and twisted into a spiral shape as shown in Figure 4. The Ni / γAl2O3 paste was applied to the surface of each stainless steel plate and then dried to create the film.

[0085] Example 12 The same procedure as in Comparative Example 8 was carried out, except that the controlled temperature was set to 750°C.

[0086] (Example 13) The same procedure as in Comparative Example 8 was carried out, except that the controlled temperature was set to 800°C.

[0087] Example 14 The same procedure as in Comparative Example 8 was carried out, except that the controlled temperature was set to 850°C.

[0088] Example 15 The same procedure as in Comparative Example 8 was repeated, except that the flow rate of carbon dioxide was 45 ml / min, the flow rate of hydrogen was 355 ml / min, the molar ratio of H2 / CO2 in the raw material gas was 7.89, and the control temperature was 800°C.

[0089] (Example 16) The same procedure as in Comparative Example 8 was repeated, except that the flow rate of carbon dioxide was 45 ml / min, the flow rate of hydrogen was 355 ml / min, the molar ratio of H2 / CO2 in the raw material gas was 7.89, and the control temperature was 850°C.

[0090] (Example 17) The same procedure as in Comparative Example 8 was repeated, except that the flow rate of carbon dioxide was 67 ml / min, the flow rate of hydrogen was 333 ml / min, the molar ratio of H2 / CO2 in the raw material gas was 4.97, and the control temperature was 700°C.

[0091] (Example 18) The same procedure as in Comparative Example 8 was carried out, except that the controlled temperature was set to 700°C.

[0092] (Example 19) The same procedure as in Comparative Example 8 was repeated, except that the flow rate of carbon dioxide was 50 ml / min, the flow rate of hydrogen was 350 ml / min, the molar ratio of H2 / CO2 in the raw material gas was 7.00, and the control temperature was 700°C.

[0093] (Example 20) The same procedure as in Comparative Example 8 was repeated, except that the flow rate of carbon dioxide was 45 ml / min, the flow rate of hydrogen was 355 ml / min, the molar ratio of H2 / CO2 in the raw material gas was 7.89, and the control temperature was 700°C.

[0094] (Experimental Results) The experimental results of Examples 12 to 20 and Comparative Example 8 are shown in Fig. 6. Fig. 6 shows the H2 / CO2 molar ratio in the raw material gas, the gas concentrations of hydrogen, methane, carbon dioxide and carbon monoxide in the mixed gas sampled from the sampling hole provided at the outlet of the first reactor, and the CO conversion rate.

[0095] In Examples 12 to 20, the conversion rate to CO was 0.8 or more, and the concentration of methane in the mixed gas discharged from the first reactor was less than 5%, which was good. In Example 16, in which the molar ratio of H2 / CO2 in the raw material gas was 7.89 and the control temperature was 850°C, the conversion rate to CO was 1.0, which was very good. In Examples 14 and 16, in which the control temperature was 850°C or more, the concentration of methane in the mixed gas discharged from the first reactor was 0%. In contrast, in Comparative Example 8, in which the control temperature of the raw material gas was 700°C or less, the concentration of methane in the mixed gas discharged from the first reactor was 5% or more. From this, it was confirmed that the methanation reaction can be suppressed by setting the control temperature in the first reactor to 700°C or more, and that methane is not generated by setting the control temperature to 850°C or more. [Explanation of symbols]

[0096] 1. Solid carbon deposition device 3 Hydrogen supply equipment 4. Hydrogen flow meter 5 Gas Mixer 7 Hydrogen separator 10 First Reactor 20 Second Reactor 41 First Water Vapor Removal Facility 42 Second Water Vapor Removal Facility 50 flow meter 61 Equipment for removing sulfur oxides 62 Carbon Dioxide Concentration Equipment 70 Gas Circulation Equipment 71 First off-gas circulation line 75 Hydrogen Circulation 100 Gas composition ratio control device 110 Storage section 120 Operation section 130 Control section 500 Solid Carbon Deposition System

Claims

1. A first step of contacting a feed gas containing carbon dioxide and hydrogen with a catalyst that activates a reverse shift reaction to produce carbon monoxide and water from the feed gas; a second step of contacting the produced carbon monoxide-containing gas with a catalyst that activates a solid carbon deposition reaction to deposit solid carbon from the produced carbon monoxide, The source gas is H 2 / CO 2 A method for depositing solid carbon, characterized in that the molar ratio is 4.5 or more.

2. 2. The method for depositing solid carbon according to claim 1, wherein the temperature of the region in which the first step is carried out is 700° C. or higher.

3. The method further comprises the step of separating hydrogen from the gas produced in the first step; As a result of the adjustment of the amount of hydrogen separated, the generated gas containing carbon monoxide is 2 3. The method for depositing solid carbon according to claim 1, wherein the molar ratio of H2O to CO is 1.0 or more and 2.0 or less.

4. 3. The method for depositing solid carbon according to claim 1, wherein the catalyst for activating the reverse shift reaction is any one of a simple substance, a compound, and a mixture thereof, containing at least one of Mn, Fe, Co, Ni, Cu, and Zn.

5. 3. The method for depositing solid carbon according to claim 1, wherein the catalyst for activating the reverse shift reaction is supported on a surface of a structure whose main raw material is a material having a melting point of 700° C. or higher.

6. contacting a feed gas containing carbon dioxide and hydrogen with a catalyst that activates a reverse shift reaction to produce carbon monoxide and water from the feed gas; The source gas is H 2 / CO 2 A method for producing a mixed gas, wherein the molar ratio is 4.5 or more.

7. A solid carbon deposition system for depositing solid carbon from a feed gas containing carbon dioxide and hydrogen, comprising: a first reactor for contacting the raw material gas with a catalyst for activating a reverse shift reaction to produce carbon monoxide and water from the raw material gas; a second reactor in which the generated carbon monoxide is contacted with a catalyst that activates a solid carbon deposition reaction to deposit the solid carbon from the generated carbon monoxide; a control unit that controls a flow rate of each gas flowing through the solid carbon deposition system; The control unit is configured to 2 / CO 2 A solid carbon deposition system that controls the molar ratio within a specified range.

8. A hydrogen separation flow path is further provided to separate hydrogen from the gas discharged from the first reactor, The control unit is configured to adjust H in the mixed gas supplied to the second reactor. 2 8. The solid carbon deposition system according to claim 7, wherein the flow rates of each gas, including the gas flow rate in the hydrogen separation channel, are controlled so that the H2O / CO molar ratio is within a specified range.

Citation Information

Patent Citations

  • Apparatus for producing carbon monoxide, chemical plant and plant

    JP2021070616A

  • Fuel synthesis equipment

    JP2022143792A

  • Carbon monoxide production device and carbon monoxide production system

    JP2022171010A

  • Anti-shift reaction catalyst, and process for production of synthetic gas using same

    WO2011065194A1

  • Reverse shift reaction catalyst, and method for producing synthetic gas using same

    WO2012153762A1