Production method of low hemicellulose bamboo powder for resin additive

By pulverizing and fermenting bamboo powder with indigenous bacteria to reduce hemicellulose content, the method addresses the deterioration issue in resin molded products, enhancing long-term strength and reducing costs.

JP2024157379AInactive Publication Date: 2024-11-07TAKEX LABO CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023071709
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-07
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Hemicellulose in bamboo powder contributes to the deterioration of resin molded products due to decomposition at low temperatures, producing organic acids that reduce long-term strength, and existing methods to reduce hemicellulose content are costly and resource-intensive.

Method used

A method involving pulverization, aerobic fermentation by indigenous bacteria, and a fermentation stopping step to reduce hemicellulose content by 30% or more, followed by drying, to produce low hemicellulose bamboo powder suitable as a resin additive.

Benefits of technology

The method effectively reduces hemicellulose content, suppressing organic acid generation and enhancing the long-term strength of resin molded products, while being cost-effective without requiring large-scale equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157379000001
    Figure 2024157379000001
Patent Text Reader

Abstract

To provide a method for producing a low hemicellulose bamboo powder for a resin additive suitable as a resin additive (filler), which can be expected to maintain the strength of a resin molding for a long term by reducing the hemicellulose content contained in a bamboo powder.SOLUTION: A method comprises: a powdering step in which a bamboo material is pulverized to produce a bamboo powder which can pass through a sieve with a mesh opening of 2.0 mm; a fermentation step in which the bamboo powder is subjected to aerobic fermentation by resident bacteria derived from the bamboo material; and a fermentation stop step in which the bamboo powder is subjected to drying treatment in a state where the hemicellulose content in the dry weight is 12 wt.% or less to stop the aerobic fermentation.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing low-hemicellulose bamboo powder for use as a resin additive. [Background technology]

[0002] Conventionally, resin additives (fillers) have been used to improve the strength of resin molded articles.

[0003] In particular, in recent years, plant-based materials have been attracting attention as fillers from the perspective of reducing the environmental impact, and against the backdrop of the promotion of plastic-free manufacturing, demand for wood-plastic composites (WPCs), which are made by adding wood or bamboo powder to resin and molding it, is expected to increase further in the future (see, for example, Patent Document 1).

[0004] Furthermore, among these plant-based materials, bamboo grows quickly and can be said to be suitable as a filler raw material from the perspective of stable supply as an industrial material. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2023-022453 A Summary of the Invention [Problem to be solved by the invention]

[0006] Incidentally, bamboo fiber contributes to improving the strength of resin moldings containing bamboo powder, and its main components are cellulose, lignin, and hemicellulose.

[0007] However, among these components, hemicellulose may have an adverse effect in terms of maintaining the strength of the resin molded article for a long period of time.

[0008] In other words, hemicellulose decomposes at a relatively low temperature of around 190°C and organic acids are produced. For example, when heated to around 190°C during resin molding, organic acids are produced from the hemicellulose in the bamboo powder added as a filler, which accelerates the deterioration of the resin molding and leads to a decrease in strength.

[0009] Of course, if the bamboo powder is heated in advance to decompose the hemicellulose, then by using such heat-treated low-hemicellulose bamboo powder as a filler, the amount of organic acids produced by heating during resin molding can be reduced, thereby avoiding the problem of long-term strength reduction of the resin molding.

[0010] However, in order to carry out such pre-heating, large-scale equipment such as heating tanks and boilers, as well as fuel oil, are required, and the expenses required for these ultimately result in an increase in the production cost of low-hemicellulose bamboo powder.

[0011] It is also possible to consider using chemicals to break down hemicellulose, but this would require not only the expense of the chemicals but also a huge amount of money for the chemical treatment equipment after use, which would also increase the production cost of low-hemicellulose bamboo powder.

[0012] The present invention has been made in consideration of the above circumstances, and provides a method for producing low-hemicellulose bamboo powder suitable as a resin additive (filler), which is expected to maintain the strength of resin moldings over the long term by reducing the hemicellulose content contained in the bamboo powder. [Means for solving the problem]

[0013] In order to solve the above-mentioned conventional problems, the manufacturing method of low hemicellulose bamboo powder for use as a resin additive of the present invention comprises a powdering process in which bamboo material is crushed to produce bamboo powder that can pass through a sieve with 2.0 mm mesh openings, a fermentation process in which the bamboo powder is aerobically fermented using resident bacteria derived from the bamboo material, and a fermentation stopping process in which the bamboo powder is subjected to a drying treatment in a state in which the hemicellulose content of the bamboo powder has been reduced by 30% or more by dry weight compared to before the aerobic fermentation, thereby stopping the aerobic fermentation. Effect of the Invention

[0014] In addition, according to the manufacturing method for low hemicellulose bamboo powder for use as a resin additive of the present invention, the method includes a powdering step in which bamboo material is crushed to produce bamboo powder that can pass through a sieve with 2.0 mm mesh size, a fermentation step in which the bamboo powder is aerobically fermented using resident bacteria derived from the bamboo material, and a fermentation stopping step in which the aerobic fermentation is stopped by subjecting the bamboo powder to a drying treatment in a state in which the hemicellulose content of the bamboo powder has been reduced by 30% or more by dry weight compared to before the aerobic fermentation.Therefore, by reducing the hemicellulose content in the bamboo powder, it is possible to provide a manufacturing method for low hemicellulose bamboo powder for use as a resin additive (filler), which is suitable for use as a resin additive, and is expected to maintain the strength of resin moldings for the long term.

[0015] In particular, by fermenting bamboo powder, the hemicellulose contained in the bamboo material can be reduced as much as possible, suppressing the generation of organic acids from hemicellulose, and relatively increasing the content of cellulose and lignin, thereby improving the strength of the resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention provides a method for producing low-hemicellulose bamboo powder suitable as a resin additive (filler), which is expected to maintain the strength of resin moldings for the long term by reducing the hemicellulose content in the bamboo powder.

[0017] Traditionally, building materials made from bamboo have been used in the form of particle board, for example, which is made by molding small pieces (particles) of wood or other plant fibers together with an adhesive resin component, and then thermocompressing the product into a specific area, thickness, and shape. This product is widely used not only as a building material but also as a material for everyday items.

[0018] However, as times have changed, resin materials have replaced wood-based materials and are now used not only in construction materials but also in most everyday items and industrial products.

[0019] In particular, due to its ease of molding and cost advantages, it is widely used as a universal material for products in fields other than metal materials.

[0020] However, the biggest drawback to such diversity of resins is the strength of the resin material. Of course, various reinforcing materials are mixed into the resin to reinforce its strength, but these reinforcing materials have both advantages and disadvantages.

[0021] In particular, as mentioned above, bamboo is a material that is expected to be used as a resin additive; however, when bamboo powder is mixed with resin, the hemicellulose contained in bamboo generates organic acids when heated during product molding, which can cause resin denaturation and damage to the resin strength.

[0022] In this regard, a feature of the manufacturing method for low-hemicellulose bamboo powder for use as a resin additive according to this embodiment is that fermentation is carried out until the hemicellulose content is reduced by 30% or more by dry weight.

[0023] By adopting such a structure, the content of cellulose and lignin in the fiber components constituting the bamboo powder can be relatively increased, and the strength of the resin molding can be improved.

[0024] Furthermore, a feature of the manufacturing method for low hemicellulose bamboo powder for use as a resin additive according to this embodiment is that it includes a powdering process, a fermentation process, and a fermentation stopping process.

[0025] The powdering process is a process in which the bamboo is crushed to produce bamboo powder that can pass through a sieve with 2.0 mm openings. The means for crushing the bamboo is not particularly limited, and any crushing device such as a cutter type, hammer type, or mill type can be used.

[0026] The crushed pieces obtained by the crushing means are preferably passed through a sieve with 2.0 mm openings, more preferably a sieve with 1.5 mm openings, and even more preferably a sieve with 1.0 mm openings, to obtain bamboo powder. However, the bamboo powder should contain as few long fibers of 3.0 mm or more as possible (for example, 0.1% by weight or less). As a standard for more strict control, the average particle size of the bamboo powder (particle size at which the cumulative volume is 50% as measured by the laser diffraction scattering method in accordance with JIS R1629) can be set to 10 μm or more and 2000 μm or less.

[0027] The fermentation process is a process in which the bamboo powder is aerobically fermented by the indigenous bacteria derived from the bamboo material. Fermentation may be achieved by piling the bamboo powder in a fermentation yard, and aerobically fermenting the bamboo powder by the indigenous bacteria derived from the bamboo for 3 to 7 days while turning it over as necessary. If necessary, a fermentation yard with ventilation equipment installed on the floor can be used, and fermentation can be performed while ventilation and turning over at appropriate times.

[0028] Furthermore, when fermenting on a smaller scale, the material can be stored in a piled state in a thermostatic chamber set at about 30 to 45°C, and fermentation can be carried out while maintaining aeration, keeping the material warm and maintaining aerobic conditions.

[0029] The fermentation stopping step is a step in which the bamboo powder is subjected to a drying treatment in a state in which the hemicellulose content of the bamboo powder has been reduced by 30% or more by dry weight compared to before the aerobic fermentation, thereby stopping the aerobic fermentation.

[0030] Drying may be performed by ventilation or heating. The degree of drying may be such that fermentation is substantially stopped, and it is desirable to dry the mixture to a moisture content of, for example, 5 to 15% by weight.

[0031] Furthermore, the low-hemicellulose bamboo powder for resin additives produced through this process can maintain the strength of resin moldings for the long term, making it suitable as a resin additive (filler).

[0032] The pH of low hemicellulose bamboo powder for resin additives is 7.0 or more, preferably 8.5 or more, to suppress biological deterioration. The pH of bamboo powder is measured by adding 9 to 10 parts by weight of water to 1 part by weight of bamboo powder and stirring thoroughly (for example, for about 2 minutes), and measuring the pH of the resulting aqueous solution.

[0033] In addition, when using the low hemicellulose bamboo powder for resin additives produced by the method of this embodiment as a resin additive (filler), the base resin is not particularly limited, and can be, for example, a thermoplastic resin such as polyethylene or polypropylene, or a thermosetting resin such as phenolic resin.

[0034] The ratio of resin to low hemicellulose bamboo powder for use as a resin additive is not particularly limited, but the weight ratio of resin to low hemicellulose bamboo powder for use as a resin additive can be 99:1 to 30:70.

[0035] If resin moldings are manufactured using resin molding raw material pellets with this composition, the low hemicellulose bamboo powder for resin additives can be mixed with the resin as a biomass-based resin additive to maintain or improve strength. In addition, the amount of fossil raw materials used can be reduced, which contributes to the suppression of CO2 emissions. In addition, by reducing hemicellulose and lowering the amount of organic acids generated during molding, it is expected that the acidic odor derived from organic acids in the molded resin product will be reduced.

[0036] Below, the manufacturing method of low hemicellulose bamboo powder for use as a resin additive according to this embodiment will be specifically explained, following the actual manufacturing process.

[0037] [1. Powdering process] Moso bamboo, which was cut down from a bamboo forest and was 3 years old or older, was processed into powder using a chip saw type grinder. The crushed pieces were then passed through a sieve with a mesh size of 2.0 mm, preferably 1.0 mm, and the crushed pieces that passed through the sieve were used as bamboo powder. However, care was taken to ensure that the bamboo powder did not contain long fibers of 3.0 mm or more.

[0038] [2. Fermentation process] 5.0 kg of bamboo powder was placed in a thermostatic chamber set at a temperature of 35-40°C, and fermentation was carried out using resident bamboo bacteria while maintaining aerobic conditions by turning the chamber once every 1-2 days.

[0039] During the fermentation process, samples were taken once every 10 days to measure the cellulose, lignin, and hemicellulose content of the bamboo powder in dry weight. In this embodiment, samples were taken once every 10 days for verification purposes, but in actual production, samples can be taken at a frequency and timing required for quality control to measure the content of each component. In addition, the fermentation stopping process described below does not necessarily have to be performed after the analysis results of the hemicellulose content are obtained, and can be performed under the condition that, for example, the number of days that are empirically considered to have reduced the hemicellulose content by 30% or more by dry weight has passed.

[0040] [3. Fermentation stopping process] In the above [2. Fermentation process], it was confirmed that the hemicellulose content of the bamboo powder had decreased by more than 30% by dry weight, and the fermentation was stopped by drying treatment to obtain low-hemicellulose bamboo powder. Drying was performed by heating in an incubator. The moisture content after drying was 9.8% by weight, and the pH of the low-hemicellulose bamboo powder was 8.5 or higher, which is expected to be anti-fungal and suppress biological deterioration.

[0041] [4. Component analysis] Table 1 shows the results of measuring the cellulose, lignin, and hemicellulose content in dry weight of bamboo powder before the fermentation process described above (hereinafter referred to as unfermented bamboo powder) and samples taken during fermentation (10 and 20 days after the start of fermentation). [Table 1]

[0042] As can be seen from Table 1, it was shown that the hemicellulose content was reduced by fermentation, and the cellulose and lignin contents were relatively increased. In particular, in the sample 20 days after the start of fermentation, the hemicellulose content was reduced by 40% compared to the unfermented bamboo powder, and efficient reduction of hemicellulose by fermentation was realized. In addition, from these results, the bamboo powder subjected to fermentation, especially the bamboo powder 20 days after the start of fermentation in which the hemicellulose content was reduced by 30% or more by dry weight compared to before aerobic fermentation, was expected to have a long-term effect of maintaining the strength of resin moldings when used as a resin additive (filler). In Table 1, at least 10 days or more have passed for the hemicellulose content to decrease by 30% or more by weight, but this is a result at the laboratory level, and in a field test conducted separately by the present inventors, it was confirmed that the hemicellulose content was reduced by 30% or more by weight in 3 to 7 days in the fermentation yard mentioned above by using 200 kg or more of bamboo powder.

[0043] In particular, no large-scale equipment such as heating tanks or boilers or fuel oil are required to reduce hemicellulose, and the low-hemicellulose bamboo powder for resin additives in accordance with this embodiment, i.e., fermented bamboo powder for resin additives, can be produced inexpensively.

[0044] As described above, the manufacturing method for low hemicellulose bamboo powder for use as a resin additive in this embodiment includes a powdering process in which bamboo material is crushed to produce bamboo powder that can pass through a sieve with 2.0 mm mesh size, a fermentation process in which the bamboo powder is aerobically fermented using resident bacteria derived from the bamboo material, and a fermentation stopping process in which the bamboo powder is subjected to a drying treatment in a state in which the hemicellulose content of the bamboo powder has been reduced by 30% or more by dry weight compared to before the aerobic fermentation, thereby stopping the aerobic fermentation.Therefore, by reducing the hemicellulose content in the bamboo powder, it is possible to provide a manufacturing method for low hemicellulose bamboo powder for use as a resin additive (filler), which is suitable for use as a resin additive, and is expected to maintain the strength of resin moldings for the long term.

[0045] Finally, the above-mentioned embodiments are merely examples of the present invention, and the present invention is not limited to the above-mentioned embodiments. Therefore, even if the above-mentioned embodiments are different, various modifications can be made depending on the design, etc., as long as they do not deviate from the technical idea of ​​the present invention.

Claims

[Claim 1] A powdering step of crushing the bamboo material to produce bamboo powder that can pass through a sieve with 2.0 mm openings; A fermentation step of aerobically fermenting the bamboo powder using indigenous bacteria derived from the bamboo material; A fermentation stopping process in which the bamboo powder is subjected to a drying process in a state in which the hemicellulose content of the bamboo powder has been reduced by 30% or more by dry weight compared to before the aerobic fermentation to stop the aerobic fermentation. A method for producing low-hemicellulose bamboo powder for use as a resin additive, characterized by having:

Citation Information

Patent Citations

  • Polypropylene resin composition

    JP2023022453A