Mold for molding plastic products and method for manufacturing thereof
A mold with a gel coat, glass fiber, and epoxy resin layers, combined with a honeycomb structure, addresses deterioration issues in resin molding, maintaining strength while reducing weight and handling difficulties.
Patent Information
- Application Number
- JP2023071738
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-07
AI Technical Summary
Conventional molds for molding resin products are prone to deterioration due to solvents and chemicals, leading to a short lifespan and increased weight, which complicates handling and poses health risks to workers.
A mold structure comprising a gel coat layer with vinyl ester resin and glass fiber, a first layer with glass cloth or mat, and a second layer with epoxy resin, carbon fiber, and a honeycomb structure, which enhances strength without excessive weight.
The mold achieves equivalent strength to conventional molds while being lighter, reducing operator burden and improving manufacturing efficiency.
Smart Images

Figure 2024157395000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a molding die used to produce resin products, particularly fiber reinforced plastic (hereinafter, FRP) products, and a method for producing said die. [Background technology]
[0002] Molds used for molding FRP are generally made by forming a gel coat resin layer using unsaturated polyester resin, vinyl ester resin, etc. on the surface of a mold (hereinafter referred to as a "master mold") that imitates the shape of the resin product to be molded, and then forming a layer of glass fiber, carbon fiber, etc. and a laminating resin on the gel coat layer.
[0003] However, most conventional molds for molding resin products have a short lifespan due to deterioration caused by trace amounts of solvents contained in the mold release agent used during molding or by chemical substances such as styrene contained in the casting resin, as well as physical fatigue caused by repeated casting and demolding and repeated drying.
[0004] Therefore, molds for molding resin products that can solve these problems have been studied. Patent Document 1 discloses a mold for molding resin products that is characterized in that short carbon fiber yarns are mixed into the gel coat resin layer on the mold surface. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 6-15660 Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the invention disclosed in Patent Document 1, although the strength of the mold in the gel coat layer can be increased, it is difficult to improve the strength of the mold for molding resin products as a whole. In order to improve the strength of the mold for molding resin products as a whole, it is necessary to make the resin layer thicker, but making the resin layer thicker increases the weight of the mold for molding resin products. If a mold with increased weight is used in this way, it becomes difficult to handle the mold when casting and demolding, which not only reduces the production efficiency of resin products but also increases the physical burden on the worker, which may harm the worker's health. Therefore, a mold that can solve such problems has been desired. [Means for solving the problem]
[0007] As a result of intensive research, the present inventors have found that the above problems can be solved by a specific structure type, and have arrived at the present invention. [1] Gel coat layer, a first layer provided on either one surface of the gel coat layer and including a vinyl ester resin and glass fibers; and a second layer including an epoxy resin, carbon fibers, and a honeycomb structure, the second layer being provided on a surface of the first layer not in contact with the gel coat layer; A mold for molding a resin product, [2] The mold for molding a resin product according to [1], wherein the glass fiber is a fiber constituting a glass cloth and / or a glass mat. [3] The mold for molding a resin product according to [1], wherein the carbon fiber is a fiber constituting a carbon cloth. [4] The mold for molding resin products according to [2], wherein two or more sheets of the glass cloth and / or glass mat are laminated. [5] The mold for molding a resin product according to [3], wherein two or more sheets of the carbon cloth are laminated. [6] The mold for molding a resin product according to [3], wherein two or more sheets of the carbon cloth are laminated, and the carbon cloth is laminated on both the front and back surfaces of the honeycomb structure. [7] A step of applying a gel coat to the surface of the master mold and curing the gel coat to form a gel coat layer; A step of laminating glass fibers on the formed gel coat layer, applying vinyl ester resin to impregnate the glass fibers, and curing the resin to form a first layer; and a step of laminating carbon fibers and a honeycomb structure on the first layer, applying an epoxy resin to the first layer to impregnate the carbon fibers and the honeycomb structure, and curing the epoxy resin to form a second layer; A method for producing a mold for molding a resin product, Regarding. Effect of the Invention
[0008] The mold for molding resin products and the mold for molding resin products obtained by the manufacturing method of the present invention are lighter in weight than conventional molds for molding resin products, while having the same strength as conventional molds. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2(a) is a perspective view of a mold for molding a resin product according to the present invention, and FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] A preferred embodiment of the present invention will be described with reference to the drawings. It goes without saying that the present invention is not limited to the following embodiments and aspects, and various modifications are possible within the technical scope of the present invention. In addition, the terms "up and down," "front and back," and "left and right" in the text refer to the directions shown in each drawing.
[0011] As described above, the present invention relates to a mold M for molding a resin product, which includes a gel coat layer 1, a first layer 2 containing vinyl ester resin and glass fiber provided on one side of the gel coat layer 1, and a second layer 3 containing epoxy resin, carbon fiber, and a honeycomb structure provided on a side of the first layer 2 not in contact with the gel coat layer 1 (see FIG. 1). Each component will be described in detail below.
[0012] 1. Gel coat layer 1 The resin forming the gel coat layer 1 can be any of the gel coat resins conventionally used in molds for resin products, without any particular restrictions. Examples of such gel coat resins include unsaturated polyester resins and vinyl ester resins. From the viewpoint of further improving the working efficiency, it is more preferable to use a thermosetting resin. The gel coat resin may be synthesized to have the desired performance, or a commercially available resin may be used. Specific examples of commercially available resins include vinyl ester resins (product name NC-72 (7A) series) manufactured by TOMATEC Corporation. The gel coat layer 1 may contain components other than the resins normally contained in the gel coat layer, such as additives such as defoamers. The thickness of the entire gel coat layer 1 can be appropriately changed, provided that the effect of the present invention is not significantly impaired. The specific thickness of the gel coat layer 1 is, for example, preferably 0.2 to 0.7 mm, more preferably 0.3 to 0.5 mm. By setting the thickness of the gel coat layer 1 within the above range, the thickness of the gel coat layer 1 is not excessively large, and therefore the weight of the mold M for molding a resin product is not excessively large.
[0013] 2. 1st layer 2 As described above, the first layer 2 is provided on either one surface of the gel coat layer 1, and is a layer containing a vinyl ester resin and glass fibers.
[0014] As the vinyl ester resin used above, vinyl ester resins that have been used in molds for molding resin products can be used without any particular restrictions. From the viewpoint of improving work efficiency, it is more preferable to use a thermosetting resin. As the vinyl ester resin, a resin having the desired performance may be synthesized, or a commercially available one may be used. As a commercially available vinyl ester resin, for example, vinyl ester resin (trade name R-806) manufactured by Resonac Co., Ltd. may be mentioned.
[0015] The glass fiber may be fibrous glass or may be a fiber constituting a glass cloth and / or a glass mat. The glass fiber may be a glass material that has been used in the past when molding a resin product, without any particular limitation. Examples of such glass materials include E glass, S glass, C glass, D glass, ECR glass, and AR glass. Among these, the use of E glass in particular can provide the first layer with more toughness, and can further increase durability against torsion applied to the mold when the mold for molding a resin product is demolded. From the viewpoint of further improving the durability of the mold for molding a resin product M, the glass fiber is preferably a fiber constituting a glass cloth and / or a glass mat.
[0016] As the glass cloth, any glass cloth that has been conventionally used in molds for molding resin products can be used without any particular limitation. As the glass cloth, a cloth-like material obtained by plain weaving, satin weaving, or leno weaving of glass fibers made of the above-mentioned materials can be used.
[0017] The thickness, density (number of glass fibers per unit area) and the like of the glass cloth used in the present invention can be appropriately changed on the condition that the effect of the present invention is not significantly impaired. The thickness of the glass cloth used in the present invention is, for example, preferably 0.2 to 0.5 mm, more preferably 0.2 to 0.3 mm. By having the thickness of the glass cloth within the above numerical range, the toughness of the first layer can be further increased without making the thickness of the first layer excessively thick.
[0018] The glass mat can be any glass mat that has been used in the past for molding resin products, without any particular limitations. The glass mat is a sheet material in which glass fibers of the above-mentioned material are cut short and randomly layered to form a cloth. The fiber diameter of the glass fibers can be appropriately changed, provided that the effect of the present invention is not significantly impaired. The thickness of the glass mat can be appropriately changed, provided that the effect of the present invention is not significantly impaired. The thickness of the glass mat used in the present invention is, for example, preferably 0.3 to 0.9 mm, more preferably 0.3 to 0.8 mm. By having the thickness of the glass mat within the above numerical range, the toughness of the first layer can be further increased without making the thickness of the first layer excessively thick.
[0019] When a glass cloth and / or a glass mat is used as the glass fiber, two or more sheets of the glass cloth and / or the glass mat may be laminated. By laminating a plurality of glass cloths and / or glass mats in this manner, the strength of the forming mold M can be further increased.
[0020] The first layer 2 contains the vinyl ester resin and glass fibers. The overall thickness of the first layer 2 can be changed as appropriate, provided that the effects of the present invention are not significantly impaired. A specific thickness of the first layer 2 is, for example, preferably 2 to 10 mm, and more preferably 2 to 5 mm. By having the thickness of the first layer 2 within the above numerical range, the thickness of the first layer 2 is not excessively large, and therefore the weight of the mold for molding a resin product is not excessively heavy, and the physical strength of the first layer 2 can be further increased.
[0021] The first layer 2 may contain components other than the vinyl ester resin and the glass sheet, for example, commonly used additives such as an anti-settling agent.
[0022] 3.Second layer 3 The second layer 3 is a layer provided on the surface of the first layer 2 that is not in contact with the gel coat layer 1, and contains an epoxy resin, carbon fibers, and a honeycomb structure.
[0023] The epoxy resin used above can be any epoxy resin that has been used in molds for molding resin products without any particular restrictions. From the viewpoint of improving work efficiency, it is more preferable to use a thermosetting resin. The epoxy equivalent of the epoxy resin used can also be appropriately selected, but in the present invention, for example, a resin with an epoxy equivalent of 160 to 180 can be suitably used. The epoxy resin may be synthesized to have the desired performance, or a commercially available one may be used. An example of a commercially available epoxy resin is an epoxy resin (trade name EPICLON830) manufactured by DIC Corporation.
[0024] The carbon fibers may be fibrous or may be fibers constituting a carbon cloth. From the viewpoint of further improving the durability of the resin product molding mold M, it is preferable that the carbon fibers are fibers constituting a carbon cloth. The carbon cloth may be a cloth-like material obtained by plain weaving, twill weaving, or open weaving of carbon fibers. Among these, the use of plain weave carbon cloth in particular can impart higher physical strength to the second layer 3. In addition, when the carbon fibers are fibers of a carbon cloth, two or more sheets of the carbon cloth may be laminated. By laminating a plurality of carbon cloths in this manner, the strength of the molding mold M can be further increased.
[0025] The thickness, density (number of carbon fibers per unit area) and the like of the carbon cloth can be appropriately changed, provided that the effect of the present invention is not significantly impaired. A specific numerical value of the thickness of the carbon cloth used in the present invention is, for example, preferably 0.2 to 0.3 mm. By making the thickness of the carbon cloth within the above numerical range, the physical strength of the second layer 3 can be further increased without making the thickness of the second layer excessively thick. In addition, the density of the carbon cloth used in the present invention (number of vertical and horizontal fibers in a 1 inch square) is, for example, preferably 11.5 to 13.5 x 11.5 to 13.5. By making the density of the carbon cloth within the above numerical range, the physical strength of the second layer 3 can be further increased.
[0026] The honeycomb structure is not particularly limited as long as it is a member having a honeycomb structure. Examples of the material of the honeycomb structure include paper materials and metal materials such as aluminum, iron, steel, and stainless steel. It is more preferable to use a honeycomb structure made of paper because the mass of the reinforcing material 4 can be reduced and the mass of the entire resin product molding mold M can be reduced. In addition, when using a honeycomb structure made of paper, it is more preferable that the paper material is a paper material impregnated with a resin, for example, a phenolic resin. By impregnating the paper material with a resin, not only the strength of the honeycomb structure can be increased, but also the water resistance and corrosion resistance of the honeycomb structure can be increased. The thickness of the honeycomb structure can be appropriately changed according to the material of the honeycomb structure, provided that the reinforcing effect can be exerted. For example, when a honeycomb structure made of paper is used as the honeycomb structure, the thickness of the honeycomb structure is, for example, preferably 3 to 15 mm, more preferably 9 to 11 mm. By setting the thickness of the honeycomb structure within the above numerical range, the physical strength of the mold for molding resin products can be increased without making the second layer 3 excessively thick and without making the weight of the mold for molding resin products excessively heavy.
[0027] Furthermore, in the case where two or more sheets of carbon cloth are laminated as described above, the carbon cloth may be laminated on both the front and back sides of the honeycomb structure. By laminating the carbon cloth on both the front and back sides of the honeycomb structure, the reinforcing effect of the honeycomb structure is further enhanced. In addition, in the case where the carbon cloth is laminated on both sides of the honeycomb structure, the carbon cloth may be laminated on a part of the front and back sides of the honeycomb structure, or may be laminated so as to cover the entire front and back sides. It is more preferable that the entire front and back sides of the honeycomb structure are covered with carbon cloth, since this has the effect of further increasing the physical strength of the finally obtained resin product molding die.
[0028] The second layer 3 contains the epoxy resin, carbon fiber, and honeycomb structure. The thickness of the entire second layer 3 can be appropriately changed on the condition that the effect of the present invention is not significantly impaired. The specific thickness of the second layer 3 is, for example, preferably 3 to 15 mm, and more preferably 9 to 13 mm. By having the thickness of the second layer 3 within the above numerical range, the thickness of the second layer 3 is not excessively large, and therefore the weight of the mold for molding a resin product is not excessively heavy, and the physical strength of the second layer 3 can be further increased.
[0029] The second layer 3 may contain components other than the epoxy resin, the carbon fiber, and the honeycomb structure, for example, commonly used additives such as an anti-settling agent.
[0030] The total thickness of the finally obtained mold M for molding resin products is, for example, preferably 10 to 30 mm, more preferably 12 to 25 mm. As described above, the mold for molding resin products of the present invention can obtain the same physical strength as a conventional mold for molding resin products even if it is thinner than the conventional mold. Therefore, when an operator uses the mold for molding resin products of the present invention to mold a resin product, the burden on the operator can be reduced by using a lighter mold.
[0031] 4. Manufacturing method of mold for resin products The mold for molding a resin product of the present invention can be produced by the following method: A step of applying a gel coat to the surface of the master mold and curing the gel coat to form a gel coat layer (hereinafter referred to as the first step); A step of laminating glass fibers on the formed gel coat layer, applying vinyl ester resin to impregnate the glass fibers, and curing the resin to form a first layer (hereinafter, the second step); and A process (hereinafter, the third process) is to laminate carbon fibers and a honeycomb structure on the first layer, apply epoxy resin to impregnate the carbon fibers and the honeycomb structure, and harden it to form a second layer. Each step will be explained below.
[0032] (1) First step The first step is a step of applying a gel coat to the surface of the master mold and heat-curing it to obtain a gel coat layer. As the master mold, any mold that has been used in the past when manufacturing a mold for molding a resin product can be used. A specific example of the master mold is a mold in which a clear paint made of polyester resin or the like is applied to the surface of a cut-processed wood to smooth the surface. The gel coat can be the same as that described for the gel coat layer 1 of the mold M for molding a resin product, without any particular restrictions. The specific amount of gel coat applied may be an amount such that the specific thickness of the gel coat layer 1 after drying is, for example, preferably 0.2 to 0.7 mm, more preferably 0.3 to 0.5 mm.
[0033] After the gel coat is applied, the coated master mold is placed in a dryer or the like and heated to harden the gel coat. The heating temperature and heating time can be appropriately adjusted based on the type of resin used in the gel coat and the amount of gel coat applied.
[0034] (2)Second process The second step is a step of laminating glass fibers on the gel coat layer formed as above, applying vinyl ester resin to impregnate the glass fibers, and curing the resin to form a first layer. The glass fibers and vinyl ester resin can be the same as those described for the first layer 2 of the resin product molding mold M, without any particular restrictions. A specific forming step is performed by laminating glass fibers on the gel coat layer formed as above, applying vinyl ester resin thereon, and impregnating the glass fibers. When the glass fibers are glass cloth and / or glass mat fibers, one or more sheets of glass cloth and / or glass mat may be laminated and vinyl ester resin may be applied. The number of glass cloth and / or glass mat sheets and the amount of vinyl ester resin applied may be adjusted so that the thickness of the first layer 2 finally formed falls within the above numerical range.
[0035] After the vinyl ester resin is applied to the glass fibers, the laminated master mold is placed in a dryer or the like and heated to harden the vinyl ester resin to form the first layer. The heating temperature and heating time can be appropriately adjusted based on the type of vinyl ester resin and the amount of the resin applied.
[0036] (3) Third step The third step is a step of laminating carbon fibers and a honeycomb structure on the first layer formed above, applying epoxy resin to impregnate the carbon fibers and honeycomb structure, and hardening the epoxy resin to form a second layer. The epoxy resin, carbon fibers, and honeycomb structure described above for the second layer 3 of the mold M for molding resin products can be used without any particular restrictions. A specific forming method is to laminate the carbon fibers and honeycomb structure on the first layer formed above, apply epoxy resin from above, and impregnate the carbon fibers and honeycomb structure. When the carbon fibers are carbon cloth fibers, one or more carbon cloths may be laminated and epoxy resin may be applied thereto. When two or more carbon cloths are used, carbon cloths may be laminated on both the front and back sides of the honeycomb structure, and epoxy resin may be applied thereto to impregnate the second layer. The number of carbon cloths and the amount of epoxy resin applied may be adjusted so that the thickness of the second layer 3 finally formed is within the above numerical range.
[0037] After laminating the epoxy resin, the laminated master mold is placed in a dryer or the like and heated to harden the epoxy resin to form the second layer. The heating temperature and heating time can be appropriately adjusted based on the type of epoxy resin and its application amount.
[0038] Finally, by removing it from the master mold, the mold M for molding a resin product is obtained.
[0039] 5. How to use the mold for resin products The mold for molding a resin product of the present invention can be used in the same manner as conventional molding dies that have been used in producing resin products such as FRP.
[0040] The present invention will be described in more detail below with reference to examples. It goes without saying that the examples do not affect the scope of the present invention. EXAMPLES
[0041] 1. Samples used (1) Gelcoat coating Vinyl ester resin (product name NC-72(7A)) manufactured by TOMATEC Corporation was used as a gel coat coating without dilution. (2) Coating for the first layer Vinyl ester resin (product name R-806) manufactured by Resonac Corporation was used as the first layer coating without dilution. (3) Coating for the second layer An epoxy resin (product name EPICLON830) (epoxy equivalent: 165 to 180 g / eq) manufactured by DIC Corporation was used as the second layer coating without dilution. (4) Glass mat: Nittobo glass mat (product number #450 MC450-AS-104SS, thickness 0.75 mm, E-glass) (5) Glass cloth: Glass cloth manufactured by Unitika Ltd. (product name M200K104JN, product number M200K104H3, thickness 0.25 mm, E glass) (6) Carbon cloth: Carbon cloth manufactured by Toray Industries, Inc. (product number C6343, fiber density (number of vertical and horizontal fibers in 1 square inch) 12.5 x 12.5, thickness 0.25 mm, plain weave) (7) Honeycomb structure (made by Shin-Nihon Feather Core Co., Ltd., made of paper, impregnated with phenolic resin, thickness 10 mm) (8) Other items used in the comparative examples Iso-based resin (manufactured by DIC Corporation: product number LP-922) was used as the first layer coating in Comparative Example 2 without dilution. Ortho resin (DIC Corporation: product number NR-2907) was used as the second layer coating in Comparative Example 2 without dilution. Roving cloth (manufactured by Unitika Ltd., product number R470 H100B) Plywood (JAS plywood, thickness 12 mm) was used instead of the honeycomb structure in Comparative Examples 1 and 2.
[0042] 2. Preparation of Example Test Pieces On the FRP plate, (1) Apply gel coat (application amount 1200g / m 2 ) and dried at 30°C for 8 hours (gel coat layer thickness after drying: approx. 0.5 mm). (2) On the gel coat layer formed above, a coating for the first layer is applied (application amount 900 g / m 2 ) → Attach one glass mat → Paint (application amount 900g / m 2 ) → Attach one glass mat → Paint (application amount 900g / m 2 ) → Attach one piece of glass cloth → Paint (application amount 900g / m 2 ) → Attach one glass mat (i.e. a total of three glass mats and one glass cloth), then dry at 30°C for 8 hours (thickness of the first layer after drying: approximately 2.5 mm), (3) The second layer coating is applied to the first layer (application amount 400 g / m 2 ) → After repeating the carbon cloth attachment process twice, the honeycomb structure is attached and the second layer coating is applied (application amount 400g / m 2 ) → The carbon cloth attachment process was repeated twice (i.e., the honeycomb structure was in the middle of the four carbon cloths), and then it was dried at 30°C for 8 hours (thickness of the second layer after drying: about 12.0 mm). (4) The dried plate was cut to a width of 31 mm and a length of 300 mm to prepare the test piece of Example 1. Ten test pieces were prepared in the above manner.
[0043] 3. Preparation of Test Pieces for Comparative Example 1 Test pieces were prepared in the same manner as in the example, except that a plywood (thickness 10 mm) was used instead of the honeycomb structure in the second layer of the example, and three sheets of roving cloth and three sheets of glass mat were used instead of the carbon cloth.
[0044] 4. Preparation of Test Pieces for Comparative Example 2 Test pieces were prepared in the same manner as in the examples, except that the glass cloth in the first layer of the examples was omitted, an iso-based resin was used instead of the vinyl ester resin, an ortho-based resin was used instead of the epoxy resin, plywood was used instead of the honeycomb structure, and a glass mat was used instead of the carbon cloth. Details of the Examples and Comparative Examples 1 and 2 are summarized in Table 1.
[0045] [Table 1] Comparing the second layer of Example 1 with the second layer of Comparative Example 1, the number of laminated sheets is greater in Comparative Example 1. This is because, in order to ensure sufficient strength and maintain a good surface condition of the gel coat layer when plywood is used, it is necessary to laminate a relatively thick roving cloth and glass mat.
[0046] 5. Measurement of the mass of the test piece The thickness and mass of the test piece prepared in the above manner were measured, and the measurement results are shown in Table 2 below. As shown in Table 2, the test pieces of the examples were thinner and had a mass that was less than half that of the test pieces of the comparative examples.
[0047] 6. Measurement of maximum bending load The maximum bending load of the test pieces of the examples and comparative examples was measured using a universal material testing machine 10 kN (model number 5966) manufactured by Instron Japan Co., Ltd. Ten samples of each were measured and the average was calculated. The results are shown in Table 2 below.
[0048] [Table 2]
[0049] As is clear from the results in Table 2, the maximum bending load of the test pieces of the Examples is comparable to that of the Comparative Examples. As described above, the molding die of the present invention is very light in mass, yet has physical strength comparable to that of conventional molds.
[0050] Further aspects of the present invention are described below. [1] Gel coat layer, a first layer provided on either one surface of the gel coat layer and including a vinyl ester resin and glass fibers; and a second layer including an epoxy resin, carbon fibers, and a honeycomb structure, the second layer being provided on a surface of the first layer not in contact with the gel coat layer; A mold for molding a resin product, [2] The mold for molding a resin product according to [1], wherein the glass fiber is a fiber constituting a glass cloth and / or a glass mat. [3] The mold for molding a resin product according to [1] or [2], wherein the carbon fiber is a fiber constituting a carbon cloth. [4] The mold for molding resin products according to [2], wherein two or more sheets of the glass cloth and / or glass mat are laminated. [5] The mold for molding a resin product according to [3], wherein two or more sheets of the carbon cloth are laminated. [6] The mold for molding a resin product according to [3] or [5], wherein two or more sheets of the carbon cloth are laminated, and the carbon cloth is laminated on both the front and back surfaces of the honeycomb structure. [7] A step of applying a gel coat to the surface of the master mold and curing the gel coat to form a gel coat layer; A step of laminating glass fibers on the formed gel coat layer, applying vinyl ester resin to impregnate the glass fibers, and curing the resin to form a first layer; and a step of laminating carbon fibers and a honeycomb structure on the first layer, applying an epoxy resin to the first layer to impregnate the carbon fibers and the honeycomb structure, and curing the epoxy resin to form a second layer; A method for producing a mold for molding a resin product, comprising the steps of: [Industrial Applicability]
[0051] The molding die of the present invention is thin and lightweight, yet has excellent physical strength, and therefore can reduce the burden on workers when manufacturing resin molded products such as FRP, and can improve the manufacturing efficiency of FRP products. [Explanation of symbols]
[0052] 1: Gel coat layer, 2: 1st layer, 3: 2nd layer, M: Mold for molding resin products
Claims
1. Gel coat layer, a first layer provided on either one surface of the gel coat layer, the first layer including a vinyl ester resin and a glass fiber; and a second layer including an epoxy resin, carbon fibers, and a honeycomb structure, the second layer being provided on a surface of the first layer not in contact with the gel coat layer; A mold for molding a resin product comprising:
2. 2. The mold for molding a resin product according to claim 1, wherein the glass fiber is a fiber constituting a glass cloth and / or a glass mat.
3. 2. The mold for molding a resin product according to claim 1, wherein the carbon fibers are fibers that constitute a carbon cloth.
4. 3. The mold for molding resin products according to claim 2, wherein two or more sheets of the glass cloth and / or the glass mat are laminated.
5. 4. The mold for molding a resin product according to claim 3, wherein two or more sheets of the carbon cloth are laminated.
6. 4. The mold for molding a resin product according to claim 3, wherein two or more sheets of said carbon cloth are laminated, and said carbon cloth is laminated on both the front and back surfaces of said honeycomb structure.
7. A step of applying a gel coat to the surface of the master mold and curing the gel coat to form a gel coat layer; A step of laminating glass fibers on the formed gel coat layer, applying vinyl ester resin to impregnate the glass fibers, and curing the resin to form a first layer; and a step of laminating carbon fibers and a honeycomb structure on the first layer, applying an epoxy resin to the first layer to impregnate the carbon fibers and the honeycomb structure, and curing the epoxy resin to form a second layer; A method for producing a mold for molding a resin product, comprising the steps of:
Citation Information
Patent Citations
Mold for molding resin article
JP1994015660A