Method for producing cellulose fiber-containing resin pellet, and method for producing molded body

The production of cellulose fiber-containing resin pellets through controlled die opening coefficient and shear rate in a screw-type kneader addresses the biodegradability and mechanical performance issues of traditional fiber-reinforced plastics, resulting in high-quality molded articles with suppressed coloring and enhanced mechanical properties.

JP2024157415APending Publication Date: 2024-11-07OJI HLDG CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023071769
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Fiber-reinforced plastic molded bodies using thermoplastic resins have low biodegradability and pose a significant incineration load, and existing methods for using pulp fibers in resin pellets result in colored and thermally deteriorated products with inadequate flexural modulus and impact resistance.

Method used

A method for producing cellulose fiber-containing resin pellets involves melt-kneading a cellulose fiber-containing resin sheet using a screw-type kneader, setting the die opening coefficient to 0.024 or more and the shear rate in the barrel to 0.4 sec^-1, to suppress coloring and enhance dispersibility, resulting in pellets with improved thermal stability and mechanical properties.

Benefits of technology

The method produces cellulose fiber-containing resin pellets with suppressed coloring, leading to molded articles with excellent flexural modulus and impact resistance, effectively addressing the biodegradability and thermal deterioration issues of traditional fiber-reinforced plastics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157415000003
    Figure 2024157415000003
  • Figure 2024157415000001
    Figure 2024157415000001
  • Figure 2024157415000002
    Figure 2024157415000002
Patent Text Reader

Abstract

To provide a method for producing a cellulose fiber-containing resin pellet that can obtain a cellulose fiber-containing resin pellet in which coloring is suppressed, and can obtain a molded body excellent in flexural elastic modulus and impact resistance from the pellet; and a method for producing a molded body obtained by molding the pellet.SOLUTION: There is provided a method for producing a cellulose fiber-containing resin pellet includes a step of melting and kneading a cellulose fiber-containing resin sheet by a screw type kneader, and producing a cellulose fiber-containing resin pellet, wherein a die opening coefficient represented by the following expression (1) of a die provided after a kneader is 0.024 or more, and a shear rate in a barrel of the screw type kneader represented by the following formula (2) is 0.4 sec-1 or more. Expression (1): die opening coefficient={(a / 2)2×π×b} / {(R / 2)2×π}. In the expression (1), R represents a screw diameter (mm), a represents a die hole diameter (mm), and b represents a die hole number. Expression (2): shear rate in barrel (sec-1)=(4×t) / {(0.1×R / 2)3×π}. In the expression (2), t represents a flow rate (cm3 / sec) in the screw type kneader, and R represents a screw diameter (mm).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing cellulose fiber-containing resin pellets and a method for producing a molded article. [Background technology]

[0002] Fiber-reinforced plastic molded products made from nonwoven fabrics (also called sheets for fiber-reinforced plastic molded products) containing reinforcing fibers such as carbon fiber and glass fiber are already used in various fields such as sports and leisure goods, aircraft materials, electronic device components, etc. Thermosetting resins and thermoplastic resins are used as the resins that serve as the matrix in fiber-reinforced plastic molded products, but in recent years, development of fiber-reinforced plastic molded products using thermoplastic resins has been progressing.

[0003] Carbon fiber, glass fiber, aramid fiber, etc. are used as reinforcing fibers. Such reinforcing fibers work to increase the strength of fiber-reinforced plastic molded bodies. When such molded products are to be disposed of, they are usually disposed of in landfills or incinerated. However, molded products using the above-mentioned reinforcing fibers have low biodegradability after being disposed of in landfills, and there is a problem that a large load is placed on incinerators during incineration.

[0004] For this reason, in recent years, it has been proposed to use pulp fibers as reinforcing fibers (for example, Patent Documents 1 to 3). In Patent Documents 1 and 2, a slurry containing pulp fibers and a thermoplastic resin is made into a paper, and the resulting papermaking intermediate is heated and pressurized to obtain a molded article. Patent Document 3 proposes forming pellets from a slurry containing pulp fibers and a thermoplastic resin, and then injection molding the pellets to produce a molded article. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 6-322699 [Patent Document 2] Japanese Patent Application Publication No. 6-346399 [Patent Document 3] Japanese Patent Application Publication No. 6-345944 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention aims to provide a method for producing cellulose fiber-containing resin pellets, which can produce cellulose fiber-containing resin pellets with suppressed coloration and can also produce molded articles having excellent flexural modulus and impact resistance from the pellets, and a method for producing molded articles by molding the pellets. [Means for solving the problem]

[0007] The present inventors have discovered that in a method for producing cellulose fiber-containing resin pellets, which comprises a step of melt-kneading a cellulose fiber-containing resin sheet in a screw-type kneader to produce pellets, the above-mentioned problems can be solved by setting the die opening coefficient of the die provided after the kneader and the shear rate in the barrel of the kneader to be equal to or greater than specific values. The present invention relates to the following <1> ~ <13> Regarding. <1> A method for producing cellulose fiber-containing resin pellets, comprising the steps of melt-kneading a cellulose fiber-containing resin sheet with a screw-type kneader to produce cellulose fiber-containing resin pellets, wherein the die opening coefficient of a die provided downstream of the kneader, as represented by the following formula (1), is 0.024 or more, and the shear rate in the barrel of the screw-type kneader, as represented by the following formula (2), is 0.4 sec -1 The above is the method for producing cellulose fiber-containing resin pellets. Dice release coefficient = {(a / 2) 2 ×π×b} / {(R / 2) 2 ×π} (1) In formula (1), R represents the screw diameter (mm), a represents the die hole diameter (mm), and b represents the number of die holes. Shear rate in the barrel (sec -1 )=(4×t) / {(0.1×R / 2) 3×π} (2) In equation (2), t is the flow rate (cm 3 / sec), and R represents the screw diameter (mm). <2> The shear rate in the die, expressed by the following formula (3), is 1100 sec -1 Below is the <1> A method for producing cellulose fiber-containing resin pellets according to claim 1. Shear rate in the die (sec -1 )=(4×t) / {(0.1×a / 2) 3 ×π×b} (3) In equation (3), t is the flow rate (cm 3 / sec), a is the die hole diameter (mm), and b is the number of die holes. <3> The content of cellulose fibers in the cellulose fiber-containing resin pellets is 10% by mass or more and 90% by mass or less. <1> or <2> A method for producing cellulose fiber-containing resin pellets according to claim 1. <4> A cellulose fiber-containing resin sheet is produced by the following steps 1 and 2: <1> ~ <3> 13. A method for producing cellulose fiber-containing resin pellets according to any one of claims 1 to 12. Step 1: A fiber assembly manufacturing process in which a fiber assembly containing cellulose fiber and resin A is manufactured by dry papermaking. Step 2: A cellulose fiber-containing resin sheet manufacturing step of compressing the fiber assembly to manufacture a cellulose fiber-containing resin sheet. <5> The resin A contains resin fibers. <4> A method for producing cellulose fiber-containing resin pellets according to claim 1. <6> When the tensile strength of the cellulose fiber-containing resin sheet in a first direction is T and the tensile strength of the cellulose fiber-containing resin sheet in a second direction perpendicular to the first direction is Y, T / Y is 0.5 or more and 1.5 or less. <1> ~ <5> 13. A method for producing cellulose fiber-containing resin pellets according to any one of claims 1 to 12. <7> The bulk density of the cellulose fiber-containing resin sheet is 0.10 g / mL or more and 0.60 g / mL or less; <1> ~ <6> 13. A method for producing cellulose fiber-containing resin pellets according to any one of claims 1 to 12. <8> <1> ~ <7> 1. A method for producing a molded article, comprising the steps of: producing cellulose fiber-containing resin pellets by the method according to any one of the above items 1 to 7; and molding the cellulose fiber-containing resin pellets. <9> The molding step is a step of injection molding cellulose fiber-containing resin pellets. <8> A method for producing the molded article according to claim 1. <10> The density of the resulting molded body is 0.8 g / cm 3 More than 1.5g / cm 3 Below is the <8> or <9> A method for producing the molded article according to claim 1. <11> The thickness of the resulting molded body is 2 mm or more. <8> ~ <10> 13. A method for producing the molded article according to any one of the above items. <12> The flexural modulus of the obtained molded body measured in accordance with JIS K 7171:2016 is 1.5 GPa or more. <8> ~ <11> 13. A method for producing the molded article according to any one of the above items. <13> The Charpy impact strength of a 4mm thick molded product measured in accordance with JIS K 7111-1:2012 is 2.0kJ / m 2 That's all. <8> ~ <12> 13. A method for producing the molded article according to any one of the above items. Effect of the Invention

[0008] According to the present invention, there are provided a method for producing cellulose fiber-containing resin pellets that can obtain cellulose fiber-containing resin pellets with suppressed coloration and a molded article having excellent flexural modulus and impact resistance from the pellets, and a method for producing a molded article by molding the pellets. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 shows the web forming apparatus used in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] [Method of manufacturing cellulose fiber-containing resin pellets] The method for producing cellulose fiber-containing resin pellets (hereinafter simply referred to as "pellets") of this embodiment includes a step of melt-kneading a cellulose fiber-containing resin sheet with a screw-type kneader (hereinafter simply referred to as "kneader") to produce pellets, and the die opening coefficient represented by the following formula (1) of the die provided after the kneader is 0.024 or more, and the shear rate in the barrel of the screw-type kneader represented by the following formula (2) is 0.4 sec -1 That's all. Dice release coefficient = {(a / 2) 2 ×π×b} / {(R / 2) 2 ×π} (1) In formula (1), R represents the screw diameter (mm), a represents the die hole diameter (mm), and b represents the number of die holes. Shear rate in barrel = (4 x t) / {(0.1 x R / 2) 3 ×π} (2) In equation (2), t is the flow rate (cm 3 / sec), and R represents the screw diameter (mm). According to the production method of the present invention, it is possible to obtain cellulose fiber-containing resin pellets with suppressed coloration. Furthermore, a molded article obtained from the cellulose fiber-containing resin pellets has excellent flexural modulus and impact resistance.

[0011] The detailed mechanism by which the above-mentioned effects are obtained is considered to be partly as follows. The present inventors have found that in a method for producing cellulose fiber-containing resin pellets, which includes a step of melt-kneading a cellulose fiber-containing resin sheet in a screw-type kneader to produce pellets, the resulting pellets may be colored. As a result of intensive investigation into the cause, it was thought that the coloring of the cellulose fibers and the like occurs due to the temperature rise of the cellulose fiber-containing resin sheet being melt-kneaded in the kneader (hereinafter, the cellulose fiber-containing resin sheet being melt-kneaded in the kneader is also referred to as "molten resin"). As a result of investigation into the cause of the above-mentioned temperature rise, it was thought that heat is generated by the back pressure accompanying discharge from the die. On the other hand, in order to perform sufficient melt-kneading, it is necessary to set the shear rate in the barrel to a certain value or more, and further, by setting the shear rate in the barrel to a certain value or more, the residence time in the barrel can be shortened, and coloring of the resulting pellets is suppressed. In the present invention, by setting the die opening coefficient represented by the above formula (1) to 0.24 or more, heat generation accompanying the back pressure at the time of discharge from the die is suppressed, and coloring of the resulting pellets is suppressed, and the shear rate in the barrel represented by the above formula (2) is set to 0.4 sec -1 It is believed that by adjusting the above, sufficient melt-kneading is performed, uniform pellets are obtained, and the residence time in the barrel can be shortened, thereby suppressing coloration.

[0012] Furthermore, a molded article obtained by using the pellets obtained by the production method of the present invention has excellent flexural modulus and impact resistance. Since the pellets obtained by the production method of the present invention are suppressed in coloration, thermal degradation of the cellulose fibers is small. As a result, it is believed that a molded article produced from the pellets has excellent flexural modulus and impact resistance because the cellulose fibers function satisfactorily as reinforcing fibers. In addition, when cellulose fibers and resin components are fed to a screw-type kneader and melt-kneaded, the cellulose fibers are hydrophilic while the resin components are generally hydrophobic, so that the cellulose fibers aggregate and the dispersibility of the cellulose fibers in the resin components is not good. In addition, since it is necessary to apply a high shear force, the cellulose fibers are cut and fine fibers are generated. It is considered that the molded body obtained from the pellets obtained in this way has poor bending modulus and impact resistance. The mechanism by which the effects of the present invention can be obtained is not limited to the above. The present invention will be described in further detail below.

[0013] <Pellet manufacturing process> The method for producing cellulose fiber-containing resin pellets of the present embodiment includes a step of melt-kneading a cellulose fiber-containing resin sheet in a screw-type kneader to produce pellets. In the present embodiment, in the step of producing pellets, the die open coefficient represented by the above formula (1) is 0.24 or more, and the shear rate represented by the above formula (2) is 0.4 or more.

[0014] (Dice release coefficient) In this embodiment, the die opening coefficient represented by the following formula (1) is 0.024 or more. Dice release coefficient = {(a / 2) 2 ×π×b} / {(R / 2) 2 ×π} (1) In formula (1), R represents the screw diameter (mm), a represents the die hole diameter (mm), and b represents the number of die holes. The die opening factor is the ratio of the total area of ​​the die holes to the cross-sectional area of ​​the screw diameter, and if the die opening factor is small, the back pressure will be high. If the die opening factor is less than 0.024, the back pressure in the barrel will be high, which will cause heat generation and lead to coloring of the pellets. The die opening coefficient is preferably 0.025 or more, more preferably 0.040 or more, and even more preferably 0.050 or more. The upper limit is not particularly limited from the viewpoint of coloring the pellets, but is less than 1.0, and from the viewpoint of applying an appropriate back pressure to eject the pellets from the die, it is preferably 0.6 or less, more preferably 0.4 or less, and even more preferably 0.2 or less. The die opening coefficient can be adjusted to a desired range by controlling the die hole diameter and the number of die holes according to the screw diameter of the screw-type kneader used, and can be increased by increasing the die hole diameter and the number of die holes, while it can be decreased by decreasing the die hole diameter and the number of die holes.

[0015] (shear rate in barrel) In this embodiment, the shear rate in the barrel of the screw-type kneader, which is represented by the following formula (2), is 0.4 or more. Shear rate in the barrel (sec -1 ) =(4×t) / {(0.1×R / 2) 3 ×π} (2) In equation (2), t is the flow rate (cm 3 / sec), and R represents the screw diameter (mm). Here, the flow rate t (cm 3 / sec) is expressed by the following formula when the feed rate is f (kg / h) and the bulk density of the cellulose fiber-containing resin sheet is d (g / mL). t(cm 3 / sec)=f(kg / h)×1000÷(60×60)÷d(g / cm 3 )

[0016] The shear rate in the barrel is 0.4 sec -1 If the temperature is more than this, uniform melt-kneading is possible, the residence time in the barrel is shortened, and discoloration of the resulting pellets is suppressed. The shear rate in the barrel can be adjusted to a desired range by appropriately adjusting the flow rate. The shear rate in the barrel is preferably 0.5 sec. -1 More than 0.6 seconds, preferably 0.6 seconds -1 The upper limit is not particularly limited, but from the same viewpoint, it is preferably 5.0 sec -1 Less than or equal to 4.0 seconds is preferable. -1 Less than 3.0 seconds, more preferably -1 Less than 2.5 seconds, more preferably -1 The following is the result.

[0017] (shear rate in the die) In the pellet manufacturing method of this embodiment, the shear rate in the die represented by the following formula (3) is preferably 1100 sec -1 The following is the result. Shear rate in the die (sec -1 ) =(4×t) / {(0.1×a / 2) 3 ×π×b} (3) The shear rate in the die is 1100 sec -1 It is preferable that the temperature is not more than 100° C., because coloring due to a temperature rise caused by shear heating is suppressed and pellets with excellent quality can be obtained. In addition, it is preferable that a molded product made from the obtained pellets has improved flexural modulus and impact resistance. The shear rate in the die is preferably 1000 sec.sup.2 or less in order to suppress coloration of the resulting pellets. -1 Less than 800 sec, more preferably -1 More preferably, 500 sec or less -1 Below 250 sec, particularly preferred -1 The lower limit is not particularly limited, but from the viewpoint of suppressing thermal deterioration of the cellulose fiber caused by the retention of the molten resin in the die, it is preferably 5 sec or less. -1 More than 10 seconds, preferably -1 That's all.

[0018] <Cellulose fiber-containing resin sheet> The method for producing pellets according to the present embodiment includes a step of melt-kneading a cellulose fiber-containing resin sheet in a screw-type kneader to produce pellets. The cellulose fiber-containing resin sheet used as a raw material is a sheet-like raw material containing cellulose, and may be cut before being supplied to the screw-type kneader. The cellulose fiber-containing resin sheet contains, in addition to cellulose fibers, a resin component (resin A). Resin A is preferably a thermoplastic resin, and preferably contains a fibrous resin (resin fiber). The cellulose fiber-containing resin sheet may be obtained by any method, but is preferably produced by the following steps 1 and 2. Step 1: A fiber assembly manufacturing process in which a fiber assembly containing cellulose fiber and resin A is manufactured by dry papermaking. Step 2: A cellulose fiber-containing resin sheet manufacturing step of compressing the fiber assembly to manufacture a cellulose fiber-containing resin sheet. The cellulose fiber-containing resin sheet produced by the above steps 1 and 2 has cellulose fibers and a resin component uniformly dispersed therein. By melt-kneading the cellulose fiber-containing resin sheet to produce pellets, it is believed that pellets having excellent dispersion of cellulose fibers can be obtained, unlike the conventional case in which cellulose fibers and a resin component are supplied to a kneader and melt-kneaded. As a result, it is believed that a molded article produced from the pellets has excellent flexural modulus and impact resistance because the cellulose fibers function satisfactorily as reinforcing fibers. Hereinafter, a preferred method for producing a cellulose fiber-containing resin sheet in this embodiment, which includes the above steps 1 and 2, will be described in detail.

[0019] (Process 1) Step 1 is a fiber assembly production step in which a fiber assembly containing cellulose fibers and resin A is produced by dry papermaking.

[0020] [Cellulose fiber] The cellulose fibers are not particularly limited in terms of the manufacturing method and type. The cellulose fibers are preferably pulp fibers, and may be, for example, chemical pulps such as hardwood and / or softwood kraft pulp, mechanical pulps such as SGP, RGP, BCTMP and CTMP, waste paper pulps such as deinked pulp, and non-wood pulps such as kenaf, jute, bagasse, bamboo, straw, and hemp. Chlorine-free pulps such as ECF pulp and TCF pulp can also be used. The cellulose fiber is preferably pulp fiber, but is not limited thereto. For example, paper powder, wood powder, etc. may be used.

[0021] Among the above pulp fibers, kraft pulp fibers, particularly softwood kraft pulp fibers (NBKP) having long fiber length, are preferably used as the cellulose fibers because the resulting molded article has excellent flexural modulus and impact resistance.

[0022] From the viewpoint of improving the flexural modulus and impact resistance of the obtained molded body and from the viewpoint of ease of production of the fiber assembly, the average fiber length of the cellulose fibers is preferably 0.1 mm or more, more preferably 0.5 mm or more, even more preferably 1 mm or more, and is preferably 50 mm or less, more preferably 10 mm or less, even more preferably 5 mm or less, and even more preferably 2.5 mm or less. The average fiber length of the cellulose fibers is measured by the method described in the Examples.

[0023] From the viewpoint of improving the bending rigidity and impact resistance of the obtained molded body and from the viewpoint of ease of production of the fiber assembly, the average fiber width of the cellulose fibers is preferably 1 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, still more preferably 15 μm or more, and is preferably 150 μm or less, more preferably 100 μm or less, even more preferably 80 μm or less, and still more preferably 50 μm or less. The average fiber width of the cellulose fibers is measured by the method described in the Examples.

[0024] In this embodiment, when the fiber aggregate is formed by an airlaid method, the cellulose fibers can be in the form of, for example, defibrated dry pulp.

[0025] The cellulose fibers are preferably unbeaten cellulose fibers in order to improve the impact resistance of the resulting molded article. In order for a molded body to exhibit impact resistance, the cellulose fibers must be properly pulled out of the resin when an impact is applied. For this purpose, unbeaten cellulose fibers having a low ratio of fine fibers are preferable, and unbeaten pulp fibers are even more preferable. From the above-mentioned viewpoints, the fine fiber ratio of the cellulose fibers is preferably 50% or less, more preferably 30% or less, and further preferably 20% or less, with no particular lower limit. The fine fiber ratio of the cellulose fibers is measured by the method described in the Examples.

[0026] The cellulose fiber content in the cellulose fiber-containing resin sheet is preferably 10% by mass or more and 90% by mass or less, more preferably 20% by mass or more, and even more preferably 35% by mass or more, from the viewpoint of obtaining a molded body having excellent flexural modulus and impact resistance, and from the viewpoint of the productivity and ease of production of the cellulose fiber-containing resin sheet; from the viewpoint of the degree of biomass conversion, it is even more preferably 50% by mass or more, particularly preferably 55% by mass or more, and more preferably 85% by mass or less, even more preferably 80% by mass or less, and even more preferably 75% by mass or less.

[0027] [Resin A] Examples of resin A components include polyolefin, polyvinyl chloride, polystyrene, ABS (acrylonitrile-butadiene-styrene), acrylonitrile-styrene, polyester, acrylic resin, polyamide, polyacetal, polycarbonate, polybutylene succinate, and polylactic acid. In addition, resins or elastomers exemplified as lubricants, plasticizers, nucleating agents, flame retardants, antistatic agents, fillers, and papermaking chemicals described in [Other components] below may also be used. In other words, resin A refers to the resin component contained in the molded product. As shown in the manufacturing method of the molded body described later, the molded body of this embodiment is preferably manufactured through a process in which a cellulose fiber aggregate containing cellulose fibers and resin A is manufactured by dry papermaking, and then compressed to manufacture a cellulose fiber-containing resin sheet. That is, it is preferable that at least resin A is blended with the cellulose fiber aggregate. In the manufacturing of the molded body, further resin or elastomer may be added.

[0028] In the present invention, the resin A contained in the fiber assembly can be any of fibers, powder, granules, and pellets. Among these, from the viewpoint of ease of papermaking in step 1 described below, the resin A contained in the fiber assembly is preferably fiber or powder, and more preferably fiber. That is, the resin A contained in the fiber assembly preferably contains resin fiber or resin powder, more preferably contains resin fiber, and further preferably contains resin fiber. Preferred examples of the fibers of resin A contained in the fiber assembly include polyolefin fibers, polyvinyl chloride fibers, polyester fibers, acrylic fibers, polyamide fibers, polycarbonate fibers and polylactic acid fibers. Preferred examples of the powder, granules, and pellets of resin A to be contained in the fiber assembly include polyolefin, polyvinyl chloride, polyester, acrylic, polyamide, polycarbonate, polylactic acid, polystyrene, ABS, acrylonitrile-styrene powder, polyacetal, and polybutylene succinate. Particularly preferred examples of the powder of resin A include polyolefin powder, polystyrene powder, ABS powder, acrylonitrile-styrene powder, polyacetal powder, and polybutylene succinate powder. The polyolefin may be the same as the specific examples of polyolefin in the polyolefin fiber shown below. Among these, polyolefin fibers are preferred as the resin A contained in the fiber assembly. The resin A contained in the fiber assembly may be one or a combination of two or more resins. For example, the resin A may be a combination of two types of resins, namely, polylactic acid fiber and polybutylene succinate powder.

[0029] -Polyolefin fiber- In this embodiment, when polyolefin fibers are used as the resin A contained in the fiber assembly, the polyolefin constituting the polyolefin fibers is not particularly limited, and examples thereof include polyolefins (unmodified polyolefins) and modified polyolefins. The melting point of the polyolefin constituting the polyolefin fiber is preferably 200°C or lower, more preferably 195°C or lower, and even more preferably 180°C or lower, from the viewpoint of ease of molding and suppressing deterioration of the cellulose fiber, and is preferably 80°C or higher, more preferably 90°C or higher, and even more preferably 100°C or higher.

[0030] Examples of polyolefins include polyethylene, polypropylene, and ethylene-propylene copolymers (also called propylene-ethylene copolymers), with polyethylene and polypropylene being preferred. In the modified polyolefin, the method of modifying the polyolefin includes, for example, acid modification, chlorination, etc., and among these, acid modification is preferred from the viewpoint of improving the affinity with cellulose fibers. The acid-modifying component used for the acid modification of the acid-modified polyolefin is preferably an unsaturated carboxylic acid component. The unsaturated carboxylic acid component is a component derived from an unsaturated carboxylic acid and its acid anhydride. Examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, maleic acid, maleic anhydride, itaconic acid, itaconic anhydride, fumaric acid, and crotonic acid. Among them, the unsaturated carboxylic acid component is preferably at least one selected from acrylic acid, methacrylic acid, maleic acid, and maleic anhydride, and is particularly preferably at least one selected from maleic acid and maleic anhydride. A polyolefin modified with at least one of maleic acid and maleic anhydride is also called a maleic acid-modified polyolefin. The acid-modified polyolefin is preferably a maleic acid-modified polyolefin, more preferably a maleic acid-modified polyethylene or a maleic acid-modified polypropylene. Note that it is sufficient that the acid-modified polyolefin is at least partially modified with an acid.

[0031] The polyolefin is particularly preferably at least one selected from the group consisting of polyethylene, polypropylene, polyethylene at least partially modified with maleic acid, polypropylene at least partially modified with maleic acid, and ethylene-propylene copolymer. From the viewpoint of improving the flexural modulus of the obtained molded article, it is preferable that the polyolefin contains an acid-modified polyolefin, it is more preferable that the polyolefin contains at least one of polyethylene at least partially modified with maleic acid and polypropylene at least partially modified with maleic acid, and it is even more preferable that the polyolefin contains polyethylene at least partially modified with maleic acid. From the viewpoint of improving the impact resistance of the resulting molded article, it is preferable that the composition does not contain an acid-modified polyolefin, and it is more preferable that the polyolefin contains only polyethylene, polypropylene, and an ethylene-propylene copolymer. The polyolefin fibers may be used alone or in combination of two or more kinds.

[0032] The polyolefin fiber may be a composite fiber made of two or more polyolefins, and examples thereof include split fibers, sea-island fibers, core-sheath fibers, and laminated fibers. Among these, from the viewpoint of obtaining a molded product having excellent bending rigidity and impact resistance, the core-sheath fibers are preferred. In the case of the core-sheath fibers, fibers having a concentric cross-sectional structure or an eccentric cross-sectional structure are used, and the fibers having a concentric cross-sectional structure are preferred. The use of the fibers having a concentric cross-sectional structure is preferred because a more uniform fiber assembly can be obtained.

[0033] From the viewpoint of obtaining a uniform fiber assembly and ease of production of the fiber assembly, the fiber length of the polyolefin fiber is preferably 0.1 mm or more, more preferably 1.0 mm or more, even more preferably 2.0 mm or more, even more preferably 3.0 mm or more, and is preferably 50 mm or less, more preferably 20 mm or less, even more preferably 10 mm or less. The fiber length of the polyolefin fiber is measured by the method described in the Examples.

[0034] From the viewpoint of obtaining a uniform fiber assembly and ease of production of the fiber assembly, the fiber diameter of the polyolefin fiber is preferably 0.1 μm or more, more preferably 1 μm or more, and even more preferably 10 μm or more, and is preferably 100 μm or less, more preferably 80 μm or less, and even more preferably 50 μm or less. The fiber diameter of the polyolefin fiber is measured by the method described in the Examples.

[0035] From the viewpoint of obtaining a uniform fiber assembly and from the viewpoint of ease of production of the fiber assembly, the fineness of the polyolefin fiber is preferably 0.01 dtex or more, more preferably 0.1 dtex or more, even more preferably 1 dtex or more, and is preferably 100 dtex or less, more preferably 50 dtex or less, even more preferably 10 dtex or less.

[0036] When the resin A contained in the fiber assembly is a polyolefin fiber, the content of the polyolefin fiber in the fiber assembly is preferably 90% by mass or less from the viewpoint of obtaining a molded product having excellent bending rigidity and impact resistance, more preferably 80% by mass or less, and even more preferably 65% ​​by mass or less from the viewpoints of productivity and ease of production, and even more preferably 50% by mass or less, and particularly preferably 45% by mass or less from the viewpoints of biomass conversion degree and productivity. Also, from the same viewpoint, it is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, and even more preferably 25% by mass or more. When two or more kinds of polyolefin fibers are used, the above content means the total content of the polyolefin fibers.

[0037] When resin A is a fiber other than a polyolefin fiber, the preferred fiber length, fiber diameter, fineness and content of the fiber are the same as the preferred fiber length, fiber diameter, fineness and content of the polyolefin fiber, respectively. In addition, when the resin A is a powder, granule, or pellet, the preferred content of the powder, granule, or pellet is the same as the preferred content of the polyolefin fiber. In addition, when the resin A is a powder, granule, or pellet, the particle size of the powder, granule, or pellet is not particularly limited.

[0038] [Other ingredients] When the resin A in the fiber assembly of the present embodiment is a polyolefin fiber, the fiber assembly may contain other components in addition to the cellulose fiber and polyolefin fiber described above, such as an elastomer or binder component described below. When the binder component is contained, the content of the binder component is preferably 0.1% by mass or more and 40% by mass or less, more preferably 0.3% by mass or more and 30% by mass or less, even more preferably 0.4% by mass or more and 20% by mass or less, and even more preferably 0.5% by mass or more and 10% by mass or less, based on the total mass of the fiber assembly. By setting the content of the binder component within the above range, the handleability and the like during the production of a molded product can be improved. Examples of binder components that can be used include various starches, casein, sodium alginate, hydroxyethyl cellulose, carboxymethyl cellulose, acrylic resins, styrene-(meth)acrylic acid ester copolymer resins, urethane resins, polyvinyl alcohol (PVA) resins, various starches, cellulose derivatives, sodium polyacrylate, polyacrylamide, polyvinylpyrrolidone, acrylamide-acrylic acid ester-methacrylic acid ester copolymers, styrene-maleic anhydride copolymer alkali salts, isobutylene-maleic anhydride copolymer alkali salts, polyvinyl acetate resins, vinyl chloride-vinyl acetate copolymers, ethylene-vinyl acetate copolymers, and the like.

[0039] The fiber assembly may further contain fillers and papermaking chemicals. Examples of the filler include mineral pigments such as kaolin, calcined kaolin, calcium carbonate, calcium sulfate, barium sulfate, titanium dioxide, talc, zinc oxide, alumina, magnesium carbonate, magnesium oxide, silica, white carbon, bentonite, zeolite, sericite, and smectite, as well as organic pigments such as polystyrene-based resins, urea-based resins, melamine-based resins, acrylic-based resins, and vinylidene chloride-based resins. Examples of papermaking chemicals include paper strength enhancers, retention improvers, drainage improvers, dyes, fluorescent whitening agents, pH adjusters, defoamers, pitch control agents, slime control agents, etc. Examples of paper strength enhancers include polyacrylamide, etc. Furthermore, wet strength enhancers can also be used in combination, such as polyamide resins, melamine-formaldehyde resins, urea-formaldehyde resins, polyamide-polyamine-epichlorohydrin resins, and polyethyleneimine resins.

[0040] The fiber assembly may further contain a fatty acid metal salt. The fatty acid metal salt is preferably a metal salt of an aliphatic carboxylic acid, and the aliphatic carboxylic acid is preferably a saturated aliphatic carboxylic acid or an unsaturated aliphatic carboxylic acid having 12 to 24 carbon atoms, and specific examples thereof include lauric acid, myristic acid, pentadecylic acid, palmitic acid, margaric acid, stearic acid, arachidic acid, heneicosylic acid, behenic acid, lignoceric acid, cerotic acid, montanic acid, melissic acid, myristoleic acid, palmitoleic acid, sapienic acid, oleic acid, and elaidic acid. Examples of metal elements that form metal salts include Group 1 elements (alkali metals) such as sodium and potassium; Group 2 elements (alkaline earth metals) such as calcium, magnesium and barium; and Group 3 elements such as zinc and aluminum, with calcium, magnesium, zinc and aluminum being preferred. Examples of fatty acid metal salts include magnesium stearate, calcium stearate, zinc stearate, barium stearate, aluminum stearate, lithium stearate, zinc laurate, and barium laurate. Among these, from the viewpoint of excellent bending rigidity and impact resistance, calcium stearate, magnesium stearate, zinc stearate, aluminum stearate, calcium oleate, magnesium oleate, zinc oleate, aluminum oleate, zinc laurate, and calcium laurate are preferred, and calcium stearate is more preferred. From the viewpoint of bending rigidity and impact resistance, the content of fatty acid metal salt in the molded body is 0.1 mass% or more and 10 mass% or less, preferably 0.3 mass% or more, more preferably 0.5 mass% or more, even more preferably 0.8 mass% or more, and preferably 9 mass% or less, more preferably 8 mass% or less, even more preferably 7 mass% or less, and even more preferably 6 mass% or less.

[0041] When other components are contained, the content of the other components excluding cellulose fibers and polyolefin fibers is preferably 0.1 mass% or more and 40 mass% or less, more preferably 0.3 mass% or more and 30 mass% or less, even more preferably 0.4 mass% or more and 20 mass% or less, and even more preferably 0.5 mass% or more and 10 mass% or less, relative to the total mass of the fiber assembly.

[0042] [Fiber assembly manufacturing process] Next, the manufacturing process of the fiber assembly will be described. In the following description of the manufacturing process of the fiber assembly, the description will be made assuming that polyolefin fiber, which is considered to be preferable, is used as resin A. When a resin other than polyolefin fiber is used as resin A, the resin used will be read as above instead of polyolefin fiber, and the other description will be the same. Note that resin A can be used alone or in combination of two or more types, as described later.

[0043] In step 1 of the present embodiment, which is a process for producing a fiber assembly, cellulose fibers and resin A are produced by dry papermaking. The manufacturing process of the fiber assembly preferably includes a process of mixing cellulose fibers and polyolefin fibers in air and depositing the mixture. That is, the fiber assembly of the present embodiment is preferably a dry nonwoven fabric.

[0044] When manufacturing a fiber aggregate using a dry papermaking method, it is preferable to adopt an airlaid method. The airlaid method is a method in which an airflow containing raw fibers, such as polyolefin fibers and cellulose fibers defibrated in the air and mixed uniformly in the airflow, is discharged onto a mesh-like endless belt equipped with a suction box on the lower side to form an airlaid web. That is, the airlaid method is a method including a step of mixing cellulose fibers and polyolefin fibers in the air and depositing them. In the airlaid method, the above operation may be repeated multiple times as necessary.

[0045] The web formed by the above method is made into a sheet by a fiber bonding process as described below. For example, the fiber bonding process includes a method of forming a sheet by entangling polyolefin fibers or cellulose fibers with each other by passing needles perpendicularly to the web surface, such as a needle punching method. Such a bonding process is preferably used in combination with a web forming method by a carding method. In addition, the fiber bonding process may employ a process of bonding raw fibers by fusing a heat-fusible adhesive blended in a dry method web by heating (thermal bond method), a process of applying an adhesive to the obtained dry method web to bond raw fibers (chemical bond method), or a method combining the thermal bond method and the chemical bond method (multi-bond method).

[0046] In the thermal bonding method, it is preferable to heat at a temperature 20° C. higher than the melting point of the heat-fusible adhesive. Examples of the heat treatment include hot air treatment and hot pressure treatment at low pressure after hot air treatment.

[0047] When the thermal bond method or the multi-bond method is adopted, it is preferable to use a particulate or fibrous heat-sealing adhesive, which may be the polyolefin fiber or binder component described above. As the particulate heat-fusible adhesive, heat-fusible resin particles such as polyethylene, polypropylene, polyester low-melting polyethylene terephthalate, low-melting polyamide, low-melting polylactic acid, polybutylene succinate, etc. are used. Examples of fibrous heat-fusible adhesives that can be used include low-melting polyethylene terephthalate, low-melting polylactic acid, polybutylene succinate (PBS), polyethylene terephthalate (PET), and other polyesters, low-melting polyamides, acrylic resins, and polyvinyl acetate (PVAc) resins. Also, as the heat-fusible synthetic fiber, a heat-fusible composite synthetic fiber having a core-sheath structure, which is obtained by combining two types of resins with different melting points and in which only the surface of the fiber melts, can be preferably used. The heat-fusible composite synthetic fiber having a core-sheath structure has a structure in which a sheath made of a resin with a low melting point is formed on the outer periphery of a core made of a resin with a high melting point. Specifically, examples include a form in which two types of resins with different melting points are combined (PET / PET composite fiber, PE / PET composite fiber, MAPE / PP composite fiber, PP / PET composite fiber, PE / PP composite fiber, PVAc / PET composite resin).

[0048] In addition, when a chemical bond method is used to bond the fibers, it is preferable to add a binder component to fix the fibers together. The binder component can be appropriately selected as needed, and for example, a solution type binder such as starch, casein, sodium alginate, hydroxyethyl cellulose, sodium carboxymethyl cellulose, polyvinyl alcohol (PVA), and sodium polyacrylate, and an emulsion type binder such as polyacrylic acid ester, acrylic styrene copolymer, polyvinyl acetate, ethylene vinyl acetate copolymer, acrylonitrile butadiene copolymer, methyl methacrylate butadiene copolymer, urea-melamine resin, and styrene-butadiene copolymer resin can be used. It is also preferable to use the above-mentioned binder component. The above-mentioned binder can be in various forms such as fiber, powder, granule, solution, or emulsion, and two or more types can be used in combination.

[0049] In the fiber aggregate produced by the above-mentioned dry papermaking method, the fibers constituting the fiber aggregate are three-dimensionally oriented randomly in the longitudinal, transverse and thickness directions. Therefore, in this embodiment, the tensile strength of the fiber aggregate in the first direction and the tensile strength in the second direction are approximately the same. That is, in this embodiment, a fiber aggregate having excellent isotropy in the planar direction is obtained.

[0050] In the manufacturing process of the fiber assembly, any sheet that does not impair moldability may be laminated on the fiber assembly to manufacture a laminated sheet. For example, any sheet may be laminated on the surface of the fiber assembly or between sheets when laminating the fiber assembly. As the any sheet to be laminated, a sheet such as tissue or nonwoven fabric can be used. These any sheets are laminated for the purpose of improving the surface properties of the fiber assembly or the cellulose fiber-containing resin sheet in the manufacturing process, improving productivity, and imparting other functions.

[0051] (Process 2) Step 2 is a cellulose fiber-containing resin sheet production step in which a cellulose fiber-containing resin sheet is produced by compressing the fiber aggregate obtained in step 1. By compressing the fiber aggregate obtained in step 1, a sheet-shaped cellulose fiber-containing resin sheet is obtained. The compression may be carried out simultaneously with the heat treatment or after the heat treatment.

[0052] Compression of the fiber aggregate can be achieved by pressing the fiber aggregate with a roll press. In addition, heating may be performed simultaneously during the roll press treatment to perform a heat and pressure treatment. The roll press treatment can be performed by pressing with a metal roll or a resin roll, so that the density of the resulting cellulose fiber-containing resin sheet can be controlled as desired. Specifically, the number of rolls used for the roll press treatment can be set to any desired number, temperature, and clearance, and the sheet can be heated and pressed to obtain a cellulose fiber-containing resin sheet of any desired density. The sheet may be compressed to a desired density by passing through multiple rolls.

[0053] Compression of the fiber assembly can also be achieved by pressure treatment using a hot press. The density of the resulting cellulose fiber-containing resin sheet can be controlled as desired by pressure treatment using an autoclave method or a mold press method on a fiber assembly cut to an appropriate size or a cellulose fiber-containing resin sheet that has been subjected to the above-mentioned roll press treatment. By heating to a temperature of 100°C or higher and applying pressure to 2 MPa or higher, a cellulose fiber-containing resin sheet with a higher density than that obtained by pressure treatment using a roll press can be obtained. In addition, a pre-pressing step may be included before obtaining the above heating and pressing conditions, and it is also preferable to carry out pre-pressing at a lower pressure under the desired heating conditions, and then increase the pressure and carry out a pressing treatment by hot pressing.

[0054] The pressurizing process by hot pressing may be a stamping molding method. In the stamping molding method, a fiber assembly is heated in advance, and the polyolefin is placed in a melted and softened state inside a mold, and then the mold is closed to clamp the assembly, and then the assembly is pressurized and cooled. For heating, a heating device such as a far-infrared heater, a heating plate, a high-temperature oven, or a dielectric heater may be used.

[0055] The pressure treatment step by hot pressing may be a vacuum molding method. In the vacuum molding method, the space between the fiber assembly and the mold is made vacuum, thereby increasing the adhesion between the fiber assembly and the mold and improving moldability. The vacuum molding is preferably performed in the mold clamping step of the stamping molding method described above. Specifically, the fiber assembly is heated, the polyolefin is melted and softened, and placed inside the mold, and then the mold is closed and clamped to perform vacuum molding. In the vacuum molding, vacuum suction is performed from the mold side. The molding pressure in the vacuum molding is usually 1.0 kg / cm. 2 The molding is carried out in about 0.1 to 60 seconds.

[0056] The pressure treatment step by hot pressing may be a pressure molding method. In the pressure molding method, compressed air is blown onto the fiber assembly to make it adhere to the mold, thereby increasing the adhesion between the fiber assembly and the mold. The pressure molding is preferably performed in the mold clamping step of the stamping molding method described above. Specifically, the fiber assembly is heated, and the polyolefin is placed in a molding die in a melted and softened state, and then compressed air is blown onto the fiber assembly side to perform molding. Pressure molding is performed at a pressure of 3 kg / cm. 2 More than 8kg / cm 2 The compressed air pressure is often as follows, and molding is preferably carried out for 0.1 to 60 seconds.

[0057] Compression of the fiber assembly can also be achieved by a supercalendering process. In the supercalendering, the fiber aggregate is molded by passing it between heated rollers while applying nip pressure. The heating temperature of the rollers used is preferably 10° C. or higher, more preferably 20° C. or higher, and even more preferably 30° C. or higher than the melting point of the polyolefin fiber, and is preferably 100° C. or lower, more preferably 90° C. or lower, and even more preferably 80° C. or lower than the melting point of the polyolefin fiber. The nip pressure is preferably 100 kg / cm or more, more preferably 150 kg / cm or more, and even more preferably 200 kg / cm or more, and is preferably 450 kg / cm or less, more preferably 400 kg / cm or less, and even more preferably 350 kg / cm or less. The number of nip stages is preferably 1 stage or more, more preferably 3 stages or more, and even more preferably 5 stages or more, and is preferably 20 stages or less, more preferably 18 stages or less, and even more preferably 16 stages or less. When compressing the fiber assembly to produce a cellulose fiber-containing resin sheet, a plurality of cellulose fiber-containing resin sheets may be appropriately laminated and compressed depending on the desired thickness of the cellulose fiber-containing resin sheet, etc.

[0058] In the cellulose fiber-containing resin sheet of this embodiment, when the tensile strength in a first direction is T and the tensile strength in a second direction perpendicular to the first direction is Y, it is preferable that T / Y is 0.5 to 1.5. By setting the T / Y to 0.5 to 1.5, the fibers constituting the cellulose fiber-containing resin sheet are mixed extremely uniformly, and thus it is possible to obtain a molded product that is excellent in impact resistance in addition to rigidity and strength against bending, which is preferable. T / Y is preferably 0.60 or more, more preferably 0.70 or more, even more preferably 0.80 or more, still more preferably 0.85 or more, and is preferably 1.40 or less, more preferably 1.30 or less, even more preferably 1.20 or less, and still more preferably 1.15 or less. The first direction of the cellulose fiber-containing resin sheet is any one direction in the planar direction of the cellulose fiber-containing resin sheet. However, when the fibers contained in the cellulose fiber-containing resin sheet are oriented in any direction in the planar direction, the orientation direction is defined as the first direction. In addition, when the flow direction in the manufacturing process of the fiber aggregate by dry papermaking is known, the flow direction is defined as the first direction. When the flow direction in the manufacturing process of the fiber aggregate is known, the flow direction in the manufacturing process is called the first direction (MD direction), and the flow direction in the obtained fiber aggregate and cellulose fiber-containing resin sheet is sometimes called T-grain. The second direction of the fiber assembly is one direction in the planar direction of the fiber assembly and is a direction perpendicular to the first direction. When the flow direction in the manufacturing process of the fiber assembly is known, the direction perpendicular to the flow direction in the manufacturing process is called the second direction (CD direction), and the second direction in the obtained fiber assembly and cellulose fiber-containing resin sheet is sometimes called Y direction. The tensile strength of the cellulose fiber-containing resin sheet in the first and second directions is measured in accordance with JIS P 8113: 2006. The tensile strength in each direction is measured using a 15±0.1 mm × 180±1 mm strip at a speed of 20±5 mm / min using a Tensilon tensile tester manufactured by A&D Co., Ltd.

[0059] In this embodiment, the cellulose fiber-containing resin sheet is a sheet-shaped product obtained by mixing at least cellulose fibers and resin A (preferably polyolefin fibers) and then dry-pressing the mixture. The sheet is obtained by pressing a cotton-like fiber aggregate (hereinafter also referred to as a cotton-like fiber aggregate) after dry-pressing, and may have various bulk specific gravities (densities). The bulk density of the cellulose fiber-containing resin sheet to be fed to the screw-type kneader is preferably 0.10 g / mL or more, more preferably 0.15 g / mL or more, from the viewpoints of ease of compression in step 2, ease of subsequent melt-kneading, ease of cutting when cutting for feeding to the melt-kneader, etc., and is preferably 0.60 g / mL or less, more preferably 0.50 g / mL or less, and even more preferably 0.40 g / mL or less. The bulk density of the cellulose fiber-containing resin sheet is measured by the method described in the Examples.

[0060] (Pellet manufacturing process) The method for producing cellulose fiber-containing resin pellets of the present embodiment includes a step of melt-kneading a cellulose fiber-containing resin sheet in a screw-type kneader to produce pellets. Here, before melt-kneading, from the viewpoint of facilitating feeding to the melt-kneader, it is preferable to cut, crush, or the like the cellulose fiber-containing resin sheet before feeding it into the melt-kneader. The cutter is not particularly limited, and examples thereof include a shredder. The size of the material after cutting, crushing, etc. is not particularly limited as long as it is of a size that allows it to be fed into a screw-type kneader.

[0061] The method for producing the pellets is not particularly limited, and may be any method that involves supplying a cellulose fiber-containing resin sheet and melt-kneading it in a screw-type kneader. Examples of the screw type kneader include a single screw type kneader and a twin screw type kneader. The cellulose fiber-containing resin sheet is fed to a screw-type kneader and melt-kneaded, and then (1) A method in which the resin is extruded into a strand shape and then cooled and solidified to obtain cellulose fiber-containing resin pellets; (2) A method in which the resin is extruded into a rod or cylinder and cooled to obtain cellulose fiber-containing resin pellets. (3) A method in which the molten kneaded product immediately after extrusion is cut with a rotary blade in air or water to obtain cellulose fiber-containing resin pellets. Examples include:

[0062] The size of the resulting pellets is not particularly limited, but is preferably 1 to 10 mm from the viewpoint of ease of feeding into an injection molding machine when producing a molded article.

[0063] The melt-kneading temperature (barrel set temperature) is not particularly limited, but it is preferable to adjust the barrel set temperature so that the temperature of the molten kneaded product (the temperature of the actually obtained kneaded product, the resin temperature) is at least 5°C higher than the melting point of the polyolefin, more preferably at least 10°C higher, and even more preferably at least 15°C higher.From the viewpoint of deterioration of the cellulose fibers, it is preferable that the barrel set temperature is not more than 100°C higher than the melting point of the polyolefin, more preferably not more than 90°C higher, and even more preferably not more than 80°C higher. The temperature of the melt-kneaded product is higher than the melt-kneading temperature (barrel set temperature) due to shear heat generated during melt-kneading. That is, it varies depending on various conditions during melt-kneading, such as the melt-kneading temperature (barrel set temperature), discharge speed, rotation speed, and screw design of the melt-kneader. In the case of the method described in the examples, the temperature of the melt-kneaded product is higher by about 20 to 40°C than the melt-kneading temperature (barrel set temperature), so the melt-kneading temperature (barrel set temperature) is lower by about 20 to 40°C than the preferred temperature of the melt-kneaded product.

[0064] Various conditions during melt kneading, such as the discharge speed and rotation speed, may be adjusted according to known methods so that the above formulas (1) to (3) fall within the desired ranges. When the device used for melt kneading is a twin-screw extruder, it is desirable to design the screw so that the kneading force is as weak as possible. In the present invention, the cellulose fibers and resin A are uniformly dispersed in the cellulose fiber-containing resin sheet in advance, and even if melt kneading is performed without applying high shear force, the dispersion state of the cellulose fibers in the cellulose fiber-containing resin sheet is maintained as it is, and pellets with excellent dispersion of the cellulose fibers are obtained. Therefore, by using a weak kneading force, cutting of the cellulose fibers can be avoided. Specifically, the kneading parts are mainly R-type kneading parts, and the number of L-type and N-type kneading parts is preferably equal to or less than the number of R-type kneading parts, and more preferably less than the number of R-type kneading parts. When melt-kneading is performed using only cut chips of a cellulose fiber-containing resin sheet, the kneading parts may be composed of only R-type kneading parts without using L-type or N-type kneading parts. The kneading parts are preferably 5 or less, and more preferably 3 or less, out of the total 10 parts divided into which the screw is divided. When melt-kneading is performed using only cut chips of a cellulose fiber-containing resin sheet, the kneading parts may be only one part.

[0065] In the melt kneading, a resin component may be further blended and melt kneaded together with the cellulose fiber-containing resin sheet, and examples of the resin component include the resin components listed in the above-mentioned resin A and the elastomer described later, and polyolefin resins and the elastomer described later are preferred. Blending at least one selected from the resin A and the elastomer in the melt kneading is preferred because it provides a molded product with superior impact resistance. That is, the obtained cellulose fiber-containing resin pellets may contain components that are blended during melt kneading in addition to the components derived from the cellulose fiber-containing resin sheet. The elastomer that may be blended in the melt kneading refers to a polymeric compound that exhibits elastic deformation, and refers to a substance that has the property of softening and becoming fluid when heated and returning to a rubber-like state when cooled. Specifically, elastomers have a structure consisting of two polymers, hard segments and soft segments, where the hard segments act as cross-linking points and the soft segments exhibit rubber elasticity, resulting in elasticity. Therefore, at room temperature, the hard segments gather together to form a pseudo-cross-linked state, exhibiting rubber-like physical properties, but at high temperatures they melt, losing the function of the cross-linking points and allowing plastic deformation. Depending on the combination of hard segment polymers and soft segment polymers, they are classified into polystyrene-based, olefin / alkene-based, polyester-based, polyvinyl chloride-based, polyurethane-based, polyamide-based, polyacrylic elastomers, silicone-based, polyimide-based, etc. Even within the same system, the characteristics differ depending on the ratio of hard and soft segments and the molecular weight. For example, polystyrene-based elastomers use styrene in the hard segment and butadiene in the soft segment. In this case, a large amount of styrene results in high hardness and improved compatibility with polystyrene and polyphenylene ether, while a small amount of styrene results in low hardness, high flexibility, and improved compatibility with polyolefins. In addition, a high molecular weight improves temperature characteristics and mechanical properties, while a low molecular weight improves processability and transparency. Examples of polystyrene-based elastomers include the Tuftec series manufactured by Asahi Kasei Corporation. For example, there is an olefin / alkene-based elastomer that combines ethylene, propylene, and 1-butene. The density, elastic modulus, and melting point can be changed by changing the combination and ratio. The structure when mixed with resin also differs, and it may be dispersed like islands in the sea or may be compatible. An example of an olefin / alkene-based elastomer is the Toughmer series manufactured by Mitsui Chemicals, Inc. Among these, polystyrene-based elastomers and olefin / alkene-based elastomers are preferred from the standpoint of impact resistance and the like. Examples of the elastomer include various elastomers described in paragraphs 0043 to 0065 of REP.2020 / 080328. The method for adding the elastomer is not particularly limited, and it is preferable to supply the elastomer together with the cellulose fiber-containing resin sheet during melt-kneading of the cellulose fiber-containing resin sheet, and then melt-knead the elastomer.

[0066] When the cellulose fiber-containing resin pellets contain the elastomer, the content of the elastomer is preferably 55% by mass or less, more preferably 50% by mass or less, even more preferably 45% by mass or less, still more preferably 40% by mass or less, and particularly preferably 35% by mass or less, based on the total mass of resin A and the elastomer, from the viewpoint of improving the flexural modulus. Also, when the cellulose fiber-containing resin pellets contain the elastomer, the content of the elastomer is preferably 5% by mass or more, more preferably 8% by mass or more, even more preferably 10% by mass or more, still more preferably 12% by mass or more, and particularly preferably 15% by mass or more, based on the total mass of resin A and the elastomer, from the viewpoint of improving the impact resistance.

[0067] In this embodiment, the cellulose fiber content in the cellulose fiber-containing resin pellets is preferably 10% by mass or more and 90% by mass or less, more preferably 20% by mass or more, and even more preferably 35% by mass or more, from the viewpoint of obtaining a molded body having excellent bending modulus and impact resistance, and from the viewpoint of the degree of biomass conversion, it is even more preferably 50% by mass or more, particularly preferably 55% by mass or more, and more preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 65% ​​by mass or less.

[0068] <Application> The cellulose fiber-containing resin pellets of the present embodiment are suitably used as resin pellets for various molding processes.

[0069] [Method of manufacturing molded body] The method for producing a molded article of the present embodiment includes a step of producing the above-mentioned cellulose fiber-containing resin pellets, and a step of molding the cellulose fiber-containing resin pellets. In addition, various molding methods are adopted in the molding process, for example, injection molding (e.g., injection compression molding (press injection, hot flow stamping molding, gas injection compression molding), gas injection molding, and ultra-high speed injection molding), various extrusion moldings (cold runner method or hot runner method), compression (press) molding, insert molding, in-mold coating molding, heat-insulating mold molding, rapid heating and cooling mold molding, various profile extrusion moldings (e.g., two-color molding and sandwich molding), etc. can be exemplified. For example, various extrusion moldings are suitable for molding sheets, films, fibers, etc. Inflation method, calendar method, casting method, etc. can also be used for molding sheets or films. Furthermore, a specific stretching operation may be applied. It is also possible to make a hollow molded product by rotational molding or blow molding, etc. In addition, a plurality of molding steps may be combined, or a plurality of steps may be simultaneously performed as one step. For example, the cellulose fiber-containing resin pellets may be formed into a sheet and then heat-pressed to obtain a molded product, or the cellulose fiber-containing resin pellets may be formed into a sheet and then supercalendered to obtain a molded product. After forming into a sheet, the product may be molded by vacuum forming, compressed air forming, or the like. Among these, injection molding is a preferred example.

[0070] When the molding step is an injection molding step, the injection molding step involves, for example, melt-kneading the above-mentioned cellulose fiber-containing resin pellets using a known injection molding machine, and injecting the molten mixture into a mold to perform molding. When melt-kneading, a known kneading machine may be used, for example, a single-screw kneading machine or a twin-screw kneading machine. Examples of known injection molding machines include screw type injection molding machines, screw pre-plasticizing type injection molding machines, plunger pre-plasticizing type injection molding machines, plunger type injection molding machines, etc. Examples of the drive system include hydraulic, electric, and hydraulic-electric hybrid systems.

[0071] The temperature conditions for injection molding are appropriately determined depending on the type of resin contained in the pellets, and it is preferable to set the cylinder temperature of the injection molding machine to a temperature 0 to 100° C. higher than the flow start temperature of the resin used. The temperature of the mold may be appropriately selected from the viewpoints of the cooling rate and productivity of the resin used. For example, in the case of polyolefin, it is preferable to set the temperature within the range of room temperature (eg, 23°C) to 120°C. Other injection conditions such as the screw rotation speed, back pressure, injection speed, pressure holding, and pressure holding time may be appropriately adjusted.

[0072] The cellulose fiber-containing resin pellets of the present embodiment may contain other resins such as elastomers by adding other resins, for example elastomers, during molding and melt-kneading the mixture. In the process of producing a molded article, other resins, various additives, masterbatches containing various additives, and the like may be added in addition to the cellulose fiber-containing resin pellets during injection molding. The additives include those typically used in resin compositions, such as stabilizers, ultraviolet absorbers, plasticizers, flame retardants, flame retardant assistants, antistatic agents, surfactants, colorants, lubricants, and mold release agents. The stabilizers include, for example, hindered phenols, hydroquinone, phosphites and substituted versions thereof. Examples of ultraviolet absorbers include resorcinol, salicylate, benzotriazole, and benzophenone. Colorants include materials including dyes, such as nitrosine, and pigments, such as cadmium sulfide, phthalocyanines, and carbon black. Examples of the lubricant include fatty acids such as stearic acid and montanic acid, their amides, their esters, their half esters with polyhydric alcohols, stearyl alcohol, stearamide, polyethylene wax, and paraffin wax.

[0073] <Characteristics of molded products> In this embodiment, the density of the resulting molded body is preferably 0.5 g / cm 3 More preferably, 0.8 g / cm 3 More preferably, 0.95 g / cm 3 More preferably, 1.0 g / cm 3 The density of the molded body is preferably 2.0 g / cm 3 Less than or equal to 1.5 g / cm 3 Less than 1.2 g / cm, more preferably 1.2 g / cm 3 The following is the result.

[0074] The thickness of the molded body is not particularly limited, but is 0.5 mm or more, more preferably 1 mm or more, even more preferably 2 mm or more, and is preferably 200 mm or less, more preferably 100 mm or less, even more preferably 50 mm or less, even more preferably 20 mm or less, and particularly preferably 10 mm or less. Incidentally, by making the thickness of the molded article 2 mm or more, it can be suitably used in applications requiring impact resistance, and therefore it is particularly preferable that the thickness of the molded article is 2 mm or more.

[0075] The molded body of the present embodiment preferably has a high flexural modulus, and since the molded body has a high flexural modulus, it is preferable that the molded body has excellent rigidity against bending. The flexural modulus of the molded body is preferably 1.5 GPa or more, more preferably 2.0 GPa or more, even more preferably 2.5 GPa or more, even more preferably 3.0 GPa or more, and even more preferably 3.0 GPa or more. The upper limit is not particularly limited, but from the viewpoint of ease of production, it is preferably 10 GPa or less. The flexural modulus of the molded body is measured in accordance with JIS K 7171:2016.

[0076] The molded article of the present embodiment preferably has high bending strength, and since the molded article has high bending strength, it is preferable that the molded article has excellent rigidity. The bending strength of the molded article is preferably 20 MPa or more, more preferably 30 MPa or more, and even more preferably 35 MPa or more. The upper limit is not particularly limited, but from the viewpoint of ease of production, it is preferably 100 MPa or less. The bending strength of the molded body is measured in accordance with JIS K 7171:2016.

[0077] The molded article of the present embodiment preferably has high Charpy impact strength, and the Charpy impact strength of a molded article having a thickness of 4 mm is preferably 1.5 kJ / m 2 More preferably, 2.0 kJ / m 2 More preferably, 3.0 kJ / m 2 More preferably, 4.0 kJ / m 2 The upper limit is not particularly limited, but from the viewpoint of ease of production, it is preferably 100 kJ / m 2 The following is the result. The larger the Charpy impact strength value, the more excellent the impact resistance. The Charpy impact strength is measured in accordance with JIS K 7111-1:2012, and in detail, is measured by the method described in the examples.

[0078] (Application) The molded article obtained by the molded article manufacturing method of the present embodiment is preferably used for electrical and electronic equipment, office automation equipment, home appliances, civil engineering and construction, automobiles, aircraft parts, structural parts and housings, containers (e.g., food containers, drug packaging containers, cosmetic packaging containers, medical device packaging containers), furniture, daily necessities, medical tools, etc. Among these, it is suitable for applications requiring impact resistance, such as civil engineering and construction, automobile or aircraft parts, structural parts, and housings. EXAMPLES

[0079] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.

[0080] Example 1 <Preparation of fiber assembly> NBKP was defibrated using a swirling jet airflow defibrator to obtain defibrated dry pulp. The air speed in the defibrator was 45 m / min, and turbulence was achieved using a baffle installed in the device. The average fiber length of the obtained defibrated dry pulp was 2.38 mm, the average fiber width was 34.3 μm, and the fine fiber ratio was 11.4%.

[0081] Next, the obtained defibrated dry pulp, polypropylene fiber (melting point 160°C, fineness 6.6 dtex, fiber length 5 mm, fiber diameter 30 μm, also referred to as "PP fiber"), and maleic anhydride modified polyethylene / polypropylene composite core-sheath fiber (core melting point 160°C, sheath melting point 100°C, fineness 1.7 dtex, fiber length 3 mm, fiber diameter 15 μm, core diameter 10.6 μm, core mass / sheath mass = 1 / 1, also referred to as "MAPE / PP composite fiber") were uniformly mixed with an air flow in a ratio (mass ratio) of 60 / 25 / 15 to obtain a fiber mixture.

[0082] Next, an airlaid web was formed from the fiber mixture using the web forming apparatus 1 shown in FIG. 1. Specifically, a first carrier sheet 41 was fed by a first carrier sheet supplying means 40 onto an air permeable endless belt 20 that was attached to a conveyor 10 and running. In Example 1, tissue (basis weight 14 g / m) was used as the first carrier sheet 41. 2 The "basis weight" was measured according to "Paper and paperboard - Method of measurement of basis weight" described in JIS P8124:2011.

[0083] While sucking the air-permeable endless belt 20 with the suction box 60, the fiber mixture was dropped and deposited on the first carrier sheet 41 together with the air flow from the fiber mixture supplying means 30, to obtain a cotton-like fiber aggregate. At that time, the set basis weight of the air-laid web portion was 400 g / m 2 The fiber mixture was supplied so that

[0084] Next, a second carrier sheet 51 was laminated on the cotton-like fiber assembly on the first carrier sheet 41 by a second carrier sheet supplying means 50 to obtain a fiber assembly containing an air-laid web. In Example 1, tissue (basis weight 14 g / m2) was used as the second carrier sheet 51. 2 That is, in Example 1, the same sheet was used for first carrier sheet 41 and second carrier sheet 51.

[0085] <Preparation of cellulose fiber-containing resin sheet> The resulting fiber assembly containing the airlaid web was passed through a box-type dryer with a hot air circulation conveyor oven system and subjected to hot air treatment at a temperature of 140° C. Thereafter, the density was adjusted by roll press treatment so that the bulk specific gravity was 0.18 g / mL, and the fiber assembly was then dried to a basis weight of 403.2 g / m without peeling off the first carrier sheet and the second carrier sheet. 2 The cellulose fiber-containing resin sheet had a T / Y of 1.08, a bulk density of 0.18 g / mL, and a thickness of 2.24 mm. The cellulose fiber-containing resin sheet was cut with a shredder (AFS100M, manufactured by Iris Ohyama Corporation) to obtain press-cut chips of about 4 mm×13 mm.

[0086] <Preparation of cellulose fiber-containing resin pellets> The press-cut chips were mixed in a screw-type twin-screw extruder (Parker Corporation, HK-25D (41D), screw diameter 25 mm) at a mixing temperature (set temperature) of 155°C (actual resin temperature 187°C) and a feed rate of 2.1 kg / h (flow rate 3.24 cm). 3The mixture was melt-kneaded and dispersed at a rate of 1 / sec. The die used for melt-kneading had a hole diameter of 3 mm and two discharge holes. After melt-kneading and dispersion, the mixture coming out of the discharge holes was cut with a rotary blade rotating at 150 rpm while being cooled in air, to produce pellets with a length of 5 mm.

[0087] <Preparation of Molded Body> The pellets were used to injection mold a Type A1 multipurpose test piece as specified in JIS K 7139:2009 under the conditions of a molding temperature of 190°C, a mold temperature of 100°C, and an injection speed of 100mm / sec to obtain a molded body (cellulose fiber-containing molded body) having a thickness of 4mm. The density of the molded body was 1.14g / cm. 3 It was.

[0088] Example 2 In the <Preparation of cellulose fiber-containing resin pellets> of Example 1, a screw-type twin-screw kneading extruder (manufactured by Ikegai Corporation, PCM46, screw diameter 46 mm) was used, the kneading temperature (set temperature) was 145°C (actual resin temperature 177°C), and the feed rate was 6.0 kg / h (flow rate 9.26 cm 3 / sec), the hole diameter of the die used for melt kneading was 4 mm, and the number of extrusion holes was 8. The same procedure as in Example 1 was carried out to obtain a cellulose fiber-containing molded product.

[0089] Example 3 In the <Preparation of fiber assembly> of Example 2, instead of the maleic anhydride modified polyethylene / polypropylene composite sheath-core fiber (MAPE / PP composite fiber), a polyethylene / polypropylene composite sheath-core fiber (core melting point 160°C, sheath melting point 110°C, fineness 1.7 dtex, fiber length 5 mm, fiber diameter 15 μm, core diameter 10.6 μm, core mass / sheath mass=1 / 1, also referred to as "PE / PP composite fiber") was used, and the density was adjusted by roll press so that the bulk specific gravity was 0.28 g / mL to obtain a cellulose fiber-containing resin sheet. The kneading temperature (set temperature) was 145°C (actual resin temperature 199°C), and the feed speed was 6.0 kg / h (flow rate 5.95 cm 3 A cellulose fiber-containing molded product was obtained in the same manner as in Example 2, except that the mixture was melt-kneaded and dispersed at a temperature of 1000 rpm (1 / sec). The cellulose fiber-containing resin sheet has a T / Y of 0.90 and a basis weight of 394.8 g / m 2 The bulk density was 0.28 g / mL and the thickness was 1.41 mm.

[0090] Example 4 In the <Preparation of cellulose fiber-containing resin pellets> of Example 1, a screw-type twin-screw kneading extruder (Shibaura Machine Co., Ltd., TEM-26SX-9, screw diameter 26 mm) was used, the kneading temperature (set temperature) was 165°C (actual resin temperature 178°C), and the feed rate was 3.6 kg / h (flow rate 5.56 cm 3 A cellulose fiber-containing molded product was obtained in the same manner as in Example 1, except that the melt kneading speed was changed to 1.05 g / cm3 / sec, the hole diameter of the die used for melt kneading was changed to 7 mm, and the number of discharge holes was changed to two. The density of the cellulose fiber-containing molded product was 1.16 g / cm3. 3 It was.

[0091] Example 5 The cellulose fiber-containing resin sheet of Example 3 was used, and the feed rate was set at 1.1 kg / h (flow rate 1.09 cm 3 A cellulose fiber-containing molded product was obtained in the same manner as in Example 4, except that the compression rate was changed to 1.13 g / cm3 / sec. The density of the cellulose fiber-containing molded product was 1.13 g / cm3. 3 It was.

[0092] Comparative Example 1 In the <Preparation of cellulose fiber-containing resin pellets> of Example 1, a screw-type twin-screw kneading extruder (TEX30α, manufactured by The Japan Steel Works, Ltd., screw diameter 30 mm) was used, the kneading temperature (set temperature) was 145°C (actual resin temperature 201°C), and the feed rate was 2.0 kg / h (flow rate 3.09 cm 3 A cellulose fiber-containing molded product was obtained in the same manner as in Example 1, except that the melt kneading speed was 1.15 g / cm3 / sec, the hole diameter of the die used for melt kneading was 3 mm, and the number of discharge holes was 1. The density of the cellulose fiber-containing molded product was 1.14 g / cm3. 3 It was.

[0093] Comparative Example 2 In the <Preparation of Cellulose Fiber-Containing Resin Pellets> of Comparative Example 1, the feed rate was 2.5 kg / h (flow rate 3.86 cm 3 Cellulose fiber-containing resin pellets were obtained in the same manner as in Comparative Example 1, except that the heating rate was changed to 210° C. / sec. The actual resin temperature at this time was 210° C.

[0094] Comparative Example 3 In the <Preparation of cellulose fiber-containing resin pellets> of Example 1, a screw-type twin-screw kneading extruder (manufactured by Ikegai Corporation, PCM45, screw diameter 45 mm) was used, the kneading temperature (set temperature) was 145°C (actual resin temperature 243°C), and the feed rate was 1.5 kg / h (flow rate 2.31 m 3 Cellulose fiber-containing resin pellets were obtained in the same manner as in Example 1, except that the melt kneading speed was changed to 100 rpm / sec, the hole diameter of the die used for melt kneading was changed to 5 mm, and the number of extrusion holes was changed to two.

[0095] Comparative Example 4 In the <Preparation of cellulose fiber-containing resin pellets> of Example 3, a screw-type twin-screw kneading extruder (manufactured by Ikegai Corporation, PCM70-40-3V-2SF, screw diameter 69 mm) was used, the kneading temperature was 160°C (the actual resin temperature could not be measured due to carbonization and smoke generation), and the feed rate was 10.8 kg / h (flow rate 10.71 m 3 Cellulose fiber-containing resin pellets were obtained in the same manner as in Example 3, except that the melt kneading speed was changed to 100 rpm, the hole diameter of the die used for melt kneading was changed to 3 mm, and the number of extrusion holes was changed to 12.

[0096] Comparative Example 5 In the <Preparation of cellulose fiber-containing resin pellets> of Example 2, the kneading temperature (set temperature) was 145°C (actual resin temperature 191°C), and the feed rate was 1.8 kg / h (flow rate 2.78 m 3 Cellulose fiber-containing resin pellets were obtained in the same manner as in Example 2, except that the heating rate was changed to 1000 rpm / sec.

[0097] [Measurement and evaluation method] (Method of measuring fiber length and diameter of polyolefin fibers) Twenty randomly selected polyolefin fibers were observed under an optical microscope and the fiber length and fiber diameter were measured.

[0098] (Method of measuring average fiber length, average fiber diameter, and fine fiber ratio of cellulose fibers) The average fiber length and average fiber diameter of cellulose fibers were measured using a fiber image analyzer (Valmet FS5, manufactured by Valmet Ltd.) in accordance with ISO16065-2. The ratio of fine fibers with a length of 0.1 mm or less in the measured length-weighted average fiber length distribution was defined as the fine fiber ratio.

[0099] (Measuring method for melting point of polyolefin fiber) The melting point of the polyolefin fiber may be determined from a catalog value of the polyolefin fiber if such a value is available. In this embodiment, the catalog value was used. If there is no catalog value, it can be measured using the following method. 5 mg of polyolefin fiber is cut out and the melting point of the polyolefin fiber is measured using a differential scanning calorimeter (DSC). The melting point is measured by heating from 30°C to 280°C at 20°C / min under a nitrogen atmosphere using a Diamond DSC manufactured by Perkin-Elmer.

[0100] (Method of measuring bulk density of fiber assembly) The bulk density of the cellulose fiber-containing resin sheet was calculated by measuring the thickness and mass of a 50 mm square sheet after conditioning it for 24 hours under conditions of 23°C and 50% RH. The thickness of the sheet was measured with a digital thickness gauge (DG-127, manufactured by Ozaki Seisakusho Co., Ltd.).

[0101] (Method of measuring T / Y) The flow direction (the running direction of the conveyor 10) in the manufacturing process of the obtained fiber aggregate was defined as the first direction, and the direction perpendicular to the first direction was defined as the second direction, and the tensile strength (unit: N / m) of the cellulose fiber-containing resin sheet was measured in accordance with JIS P 8113:2006. The tensile strength in each direction was divided by the thickness of the test piece to calculate the tensile strength (unit: MPa). A Tensilon manufactured by A&D Co., Ltd. was used as a tensile tester to measure a 15 mm x 180 mm strip at a speed of 20 mm / min.

[0102] <Evaluation> The density, flexural modulus, flexural strength, and impact resistance of the obtained molded article were measured by the following methods. The results are shown in Table 2.

[0103] (Method of measuring density of molded products) The obtained molded product (molded body) was cut into a rectangular test piece of 80 mm length x 10 mm width. The thickness of the rectangular test piece was measured with a constant pressure thickness measuring device (manufactured by Techclock Corporation, model number PG-02J), and the volume of the rectangular test piece was calculated. Furthermore, the density was calculated by measuring the mass of the rectangular test piece.

[0104] (Method of measuring flexural modulus and flexural strength of molded products) The obtained molded product (molded body) was cut into a rectangular test piece of 80 mm length × 10 mm width, and a three-point bending test was carried out in accordance with JIS K 7171: 2016. The obtained bending modulus and bending strength were evaluated as being superior in rigidity and strength against bending, respectively, as the values ​​were larger.

[0105] (Method for measuring impact resistance of molded products (Charpy impact strength)) The obtained molded product (molded body) was cut into a rectangular test piece of 80 mm long x 10 mm wide, and a notched Charpy impact test (strike direction: edgewise) was performed in accordance with JIS K 7111-1: 2012. The larger the Charpy impact strength value, the better the impact resistance and the stronger the impact resistance.

[0106] (Pellet coloring) The pellets obtained were visually observed. If they were white or light yellow, they were rated A; if they were dark yellow or black, they were rated B.

[0107] [Table 1]

[0108] [Table 2]

[0109] As shown in Examples 1 to 5, the molded articles produced using the cellulose fiber-containing resin pellets of the present invention were less colored. On the other hand, when the value of formula (1) was small, the molded article was colored brown or black, as shown in Comparative Examples 1 to 4. Moreover, when the value of formula (2) was small, the molded article was colored brown, even if formula (1) satisfied the requirements of the present invention, as shown in Comparative Example 5. As shown in Table 2, the molded body with little coloration produced using the cellulose fiber-containing resin pellets of the present invention had superior bending rigidity, bending strength, and impact resistance compared to the molded body colored brown. [Industrial Applicability]

[0110] According to the method for producing cellulose fiber-containing resin pellets of this embodiment, pellets with suppressed coloration can be obtained, and further, a molded article having excellent flexural modulus (flexural rigidity) and impact resistance can be obtained from the pellets. [Explanation of symbols]

[0111] 1 Web forming device 10 Conveyor 20 Breathable endless belt 30 Fiber mixture supply means 40 First carrier sheet supply means 41 First Career Sheet 50 Second carrier sheet supply means 51 Second Career Sheet 60 Suction Box

Claims

1. A method for producing cellulose fiber-containing resin pellets, comprising the steps of: The method includes a step of melt-kneading a cellulose fiber-containing resin sheet in a screw-type kneader to produce cellulose fiber-containing resin pellets, The die opening coefficient of the die provided after the kneader is 0.024 or more, as represented by the following formula (1). The shear rate in the barrel of the screw type kneader represented by the following formula (2) is 0.4 sec -1 That's all. A method for producing cellulose fiber-containing resin pellets. Die opening coefficient = {(a / 2) 2 ×π×b} / {(R / 2) 2 ×π} (1) In formula (1), R represents the screw diameter (mm), a represents the die hole diameter (mm), and b represents the number of die holes. Shear rate in the barrel (sec -1 ) = (4 × t) / {(0.1 × R / 2) 3 ×π} (2) In formula (2), t is the flow rate (cm 3 / sec), and R represents the screw diameter (mm).

2. The shear rate in the die, expressed by the following formula (3), is 1100 sec -1 The method for producing cellulose fiber-containing resin pellets according to claim 1, wherein the following is true: Shear rate in the die (sec -1 ) = (4 × t) / {(0.1 × a / 2) 3 ×π×b} (3) In formula (3), t is the flow rate (cm 3 / sec), a represents the die hole diameter (mm), and b represents the number of die holes.

3. The method for producing cellulose fiber-containing resin pellets according to claim 1, wherein the cellulose fiber content in the cellulose fiber-containing resin pellets is 10% by mass or more and 90% by mass or less.

4. The method for producing cellulose fiber-containing resin pellets according to claim 1, wherein the cellulose fiber-containing resin sheet is produced by the following steps 1 and 2: Step 1: A fiber assembly manufacturing step of manufacturing a fiber assembly containing cellulose fibers and resin A by dry papermaking. Step 2: A cellulose fiber-containing resin sheet manufacturing step of compressing the fiber assembly to manufacture a cellulose fiber-containing resin sheet.

5. The method for producing cellulose fiber-containing resin pellets according to claim 4 , wherein the resin A contains resin fibers.

6. 2. The method for producing cellulose fiber-containing resin pellets according to claim 1, wherein T / Y is 0.5 or more and 1.5 or less, where T is the tensile strength of the cellulose fiber-containing resin sheet in a first direction and Y is the tensile strength of the cellulose fiber-containing resin sheet in a second direction perpendicular to the first direction.

7. The method for producing cellulose fiber-containing resin pellets according to claim 1, wherein the cellulose fiber-containing resin sheet has a bulk specific gravity of 0.10 g / mL or more and 0.60 g / mL or less.

8. A step of producing cellulose fiber-containing resin pellets by the method according to any one of claims 1 to 7; and The cellulose fiber-containing resin pellets are molded. A method for producing a molded body.

9. The method for producing a molded article according to claim 8 , wherein the molding step is a step of injection molding cellulose fiber-containing resin pellets.

10. The density of the resulting molded body is 0.8 g / cm 3 1.5g / cm or more 3 The method for producing a molded body according to claim 8, wherein:

11. The method for producing a molded article according to claim 8, wherein the thickness of the obtained molded article is 2 mm or more.

12. The method for producing a molded body according to claim 8, wherein the obtained molded body has a flexural modulus of 1.5 GPa or more as measured in accordance with JIS K 7171:2016.

13. The Charpy impact strength of a 4 mm thick molded body measured in accordance with JIS K 7111-1:2012 is 2.0 kJ / m 2 The method for producing a molded article according to claim 8 .

Citation Information

Patent Citations

  • Thermoplastic resin composition, method for producing the same and method for producing molded article

    JP2008274027A

  • Production of article formed by paper-making process

    JP1994322699A

  • Molding made of biodegradable composite material and its production

    JP1994345944A

  • Production of biodegradable composite paper and sheet

    JP1994346399A