Heat dissipation molding agent and heat dissipation film formed by using the same
The two-component heat dissipation molding agent with silicone resin and varying fillers addresses layer separation and caking issues, ensuring high thermal conductivity and stability in heat dissipation films.
Patent Information
- Application Number
- JP2023073933
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-07
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional heat dissipation films suffer from layer separation and caking phenomena due to differences in specific gravity between the polymer matrix and heat dissipation fillers, leading to reduced heat dissipation properties and increased load, which affects the stability and efficiency of devices like battery packs.
A two-component heat dissipation molding agent comprising silicone resin, heat dissipation fillers with varying sizes and types, a crosslinking agent, and a suspending agent to ensure uniform distribution and prevent layer separation, along with a retarder to control viscosity and prevent caking, is used to form a heat dissipation film.
The solution ensures high thermal conductivity, prevents layer separation and caking, and maintains film stability, enhancing the long-term performance and efficiency of heat dissipation films.
Smart Images

Figure 2024157491000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a heat-dissipating molding material having improved heat transfer performance and a heat-dissipating film manufactured using the same, and more particularly to a heat-dissipating molding material having improved heat-dissipating properties and a heat-dissipating film manufactured using the heat-dissipating molding material. [Background technology]
[0002] A heat dissipation film is a material that is attached to a heat-generating device to transfer the heat to the outside. To perform heat dissipation, a material with excellent heat transfer properties must be used, and it is required to effectively disperse heat and prevent heat accumulation.
[0003] In recent years, various problems have arisen due to heat generation in LED lighting, computers, smartphones, and battery packs. In particular, heat generated from battery packs is one factor that reduces battery performance. Heat generated in secondary batteries can cause thermal runaway. When thermal shock occurs, the internal temperature of the secondary battery rises, adversely affecting the operation of the electrolyte. In severe cases, the electrolyte vaporizes, increasing the internal pressure of the battery, and after a certain stage, the venting phenomenon occurs, where the battery surface opens or explodes.
[0004] To prevent this, a heat dissipation material is introduced into the exterior or surface of the battery pack. The heat dissipation material must be attached to the surface of the battery pack and must have shape controllability. That is, it must be attached in the form of a film tightly along the surface regardless of the various shapes of the battery pack. Therefore, a heat dissipation molding agent in which the heat dissipation material is dispersed in a polymer matrix is used.
[0005] The heat dissipation molding agent is coated on a substrate and adheres to the battery pack in the form of a film through a curing process. The heat dissipation molding agent is made of a thermally conductive resin, and polyurethane is used as the thermally conductive resin.
[0006] Korean Patent No. 10-1848895 discloses a heat dissipation composite material that uses a porous polyurethane resin and contains a thermally conductive filler inside. The thermally conductive filler is dispersed in a urethane monomer, and a film is produced through drying and heat compression.
[0007] However, even if conventional heat dissipation films can ensure heat dissipation properties at an early stage, various problems arise over time.
[0008] The first is layer separation and caking. Even if a molding agent with heat-dissipating filler dispersed in a polymer matrix is processed into a film and cured, the heat-dissipating filler cannot maintain its dispersed state in the polymer matrix due to the difference in specific gravity between the polymer matrix and the heat-dissipating filler, and is formed in layers. In other words, the heat dissipation properties are reduced due to the heat-dissipating filler having reduced dispersibility. In addition, caking is a phenomenon in which a cured film hardens due to contact with air, and the heat-dissipating film peels off from the substrate due to thermal expansion or mechanical impact.
[0009] The second problem is caused by excessive load. For example, when a heat dissipation film is applied to a vehicle battery, if heat dissipation films are formed on multiple battery packs and each heat dissipation film bears a high load, the fuel efficiency of the vehicle may decrease.
[0010] Among the above problems, layer separation and caking are causes of impairing the long-term stability of the heat-dissipating film. Therefore, there is a need to develop a heat-dissipating molding agent and a heat-dissipating film to which the heat-dissipating molding agent is applied, which can solve the layer separation and caking phenomena. Summary of the Invention [Problem to be solved by the invention]
[0011] The first technical objective of the present invention is to provide a two-liquid type heat dissipating molding agent capable of improving heat dissipation characteristics.
[0012] The second technical objective of the present invention is to provide a heat-dissipating film using the heat-dissipating molding agent provided through the achievement of the first technical objective. [Means for solving the problem]
[0013] In order to achieve the first technical objective described above, the present invention provides a heat-dissipating molding agent, which includes a first liquid type heat-dissipating molding agent and a second liquid type heat-dissipating molding agent, wherein the first liquid type heat-dissipating molding agent has a first silicone resin, a first heat-dissipating filler, a crosslinking agent, and a first suspending agent, and the second liquid type heat-dissipating molding agent has a second silicone resin, a second heat-dissipating filler, a catalyst, and a second suspending agent, and the first liquid type heat-dissipating molding agent and the second liquid type heat-dissipating molding agent are mixed to provide a heat-dissipating molding agent.
[0014] In order to achieve the second technical objective described above, the present invention provides a heat-dissipating film comprising: a polymer matrix in which a silicone resin is hardened by a crosslinking agent; and a heat-dissipating filler dispersed within the polymer matrix, the heat-dissipating filler comprising spherical alumina having a size of 3 μm to 7 μm, plate-like alumina having a size of 0.1 μm to 1 μm, first spherical AlN having a size of 50 μm to 60 μm, second spherical AlN having a size of 80 μm to 100 μm, and plate-like silica having a size of 0.1 μm to 0.5 μm. Effect of the Invention
[0015] According to the present invention, thermally conductive fillers having various sizes and types are introduced. In addition, the surface of the thermally conductive filler is hydrophobically treated by a crosslinking agent, so that the thermally conductive filler is evenly distributed in the thermally conductive molding material. In addition, a precipitation inhibitor is introduced to prevent layer separation caused by thermally conductive fillers having different specific gravities, so that the thermally conductive filler is evenly distributed by the precipitation inhibitor. This ensures high thermal conductivity.
[0016] In addition, caking of the heat-dissipating film can be prevented by adjusting the viscosity of the liquid heat-dissipating molding agent and using a retarder. The viscosity of the molding agent affects the thickness, surface flatness, and shape control of the heat-dissipating film during the coating process. If the viscosity of the molding agent is low, the thickness is reduced and the surface flatness is improved, but shape control is difficult. If a retarder is introduced into the curing process, rapid curing that can occur in localized areas is prevented, and the phenomenon of excessive curing of parts of the surface is prevented. In other words, caking, in which parts of the surface harden and the heat-dissipating film is destroyed or peeled off due to mechanical impact, can be prevented. [Brief description of the drawings]
[0017] [Figure 1] 1 is a schematic diagram for explaining the heat dissipation operation of a heat dissipation film according to a preferred embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present invention can be modified in various ways and can have various forms, and specific embodiments are illustrated in the drawings and described in detail in the text. However, it is not intended to limit the present invention to the specific disclosed form, and it should be understood that the present invention includes all modifications, equivalents, and alternatives within the spirit and technical scope of the present invention. Similar reference numerals are used to refer to similar components in the description of the various drawings.
[0019] Unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention pertains. Terms as commonly used and predefined should be interpreted as having a meaning consistent with the meaning they have in the context of the relevant art, and should not be interpreted as having an ideal or overly formal meaning unless expressly defined in this application.
[0020] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. EXAMPLES
[0021] The heat-dissipating molding agent of the present invention comprises a silicone resin, a crosslinking agent, a catalyst, a heat-dissipating filler, a suspending agent and a retarder.
[0022] The silicone resin is a polymer matrix.
[0023] The silicone resin is a mixture of a first polydiorganosiloxane of the following chemical formula 1, a second polydiorganosiloxane of the following chemical formula 2, a first polydihydrogensiloxane of the following chemical formula 3, and a second polydihydrogensiloxane of the following chemical formula 4.
[0024] [ka]
[0025] In the above Chemical Formula 1, R1 is preferably a non-substituted group having no aliphatic unsaturated bond or a substituted group having 1 to 5 hydrocarbons, and examples of such groups include lower alkyl groups such as methyl, ethyl, propyl, and butyl groups; aryl groups such as phenyl, xylene, and benzene groups; and cycloalkyl groups such as cyclohexyl groups; and groups in which some or all of the hydrogen atoms are substituted with halogen or cyano groups, such as a chloromethyl group, a cyanomethyl group, and a 3,3,3-trifluoropropyl group, and n is 0 or a positive integer.
[0026] The first polydiorganosiloxane of the above Chemical Formula 1 has both ends of the molecular chain blocked with dimethylvinylsiloxane groups, and is dimethylsiloxane, dimethylsiloxane methylphenylsiloxane, or a copolymer thereof, and preferably has a viscosity of 1,000 cp to 100,000 cp at room temperature.
[0027] [ka]
[0028] In the above chemical formula 2, R1 is preferably a non-substituent group containing no aliphatic unsaturated bonds or a group having 1 to 5 substituted hydrocarbon groups, and examples of such groups include lower alkyl groups such as methyl, ethyl, propyl, and butyl groups; aryl groups such as phenyl, xylene, and benzene groups; and cycloalkyl groups such as cyclohexyl groups; and groups in which some or all of the hydrogen atoms have been substituted with halogen elements or cyano groups, such as a chloromethyl group, a cyanomethyl group, and a 3,3,3-trifluoropropyl group, and n is 0 or a positive integer.
[0029] The second polydiorganosiloxane of the above formula 2 has both ends of the molecular chain blocked with dimethylhydroxysiloxane groups, is dimethylsiloxane, a dimethylsiloxane-methylphenylsiloxane copolymer, or a dimethylsiloxane-methyltrifluoropropylsiloxane copolymer, does not contain an unsaturated hydrocarbon group, and preferably has a viscosity of 100 cp to 200,000 cp at room temperature.
[0030] [ka]
[0031] In the above chemical formula 3, R1 is preferably a non-substituent group containing no aliphatic unsaturated bonds or a group having 1 to 5 substituted hydrocarbons, and examples of such groups include lower alkyl groups such as methyl, ethyl, propyl, and butyl groups; aryl groups such as phenyl, xylene, and benzene groups; and cycloalkyl groups such as cyclohexyl groups; and groups in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms or cyano groups, such as a chloromethyl group, a cyanomethyl group, or a 3,3,3-trifluoropropyl group, and n is 0 or a positive integer.
[0032] The polydihydrogensiloxane of the above formula 3 is dimethylsiloxane, a dimethylsiloxane-methylphenylsiloxane copolymer, or a dimethylsiloxane-methyltrifluoropropylsiloxane copolymer, in which both ends of the molecular chain are blocked with dimethylhydrogensiloxane groups, and preferably does not contain an aliphatic unsaturated hydrocarbon group and has a viscosity of 100 cp to 100,000 cp.
[0033] [ka]
[0034] In the above chemical formula 4, R1 and R4 are preferably unsubstituted groups not containing an aliphatic unsaturated bond, or substituted with 1 to 5 hydrocarbons, and examples of such groups include lower alkyl groups such as methyl, ethyl, propyl, and butyl groups; aryl groups such as phenyl, xylene, and benzene groups; and cycloalkyl groups such as cyclohexyl groups; and groups in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms or cyano groups, such as chloromethyl groups, cyanomethyl groups, or 3,3,3-trifluoropropyl groups, and n and m are 0 or a positive integer.
[0035] The second polydihydrogensiloxane of the above formula 4 is a copolymer of dimethylsiloxane and methylhydrogensiloxane, both ends of the molecular chain of which are blocked with trimethylsiloxane groups, and preferably has at least two hydrogen atoms bonded to silicon atoms in one molecule and a viscosity of 100 cp to 20,000 cp at room temperature.
[0036] The silicone resin may further include HPDMS (a,w-hydrogen poly(dimethyl-methylphenyl)siloxane). HPDMS is used to adjust the viscosity of the heat-dissipating molding agent.
[0037] In the silicone resin, the first polydiorganosiloxane is added at 15 wt% to 25 wt%, the second polydiorganosiloxane is added at 20 wt% to 35 wt%, the first polydihydrogensiloxane is added at 40 wt% to 48 wt%, and the fourth polydihydrogensiloxane is added at 0.1 wt% to 1.5 wt%.
[0038] The crosslinking agent used is vinyltrimethoxysilane (CH2=CHSi(OCH3)3) or phenyltrimethoxysilane (C6H5Si(OCH3)3). The crosslinking agent connects the silicone resin to each other to form a network, and modifies the surface of the heat-dissipating filler to have hydrophobic properties. The crosslinking agent improves the miscibility and dispersibility between the silicone resin and the heat-dissipating filler.
[0039] The catalyst contains Pt and is provided in the form of a hydrate. Examples of the catalyst that can be used include HPtCl6·nH2O, NaHPtCl6·nH2O, KHPtCl6·nH2O, Na2PtCl6·nH2O, K2PtCl6·nH2O, PtCl4·nH2O, PtCl2, Na2PtCl4·nH2O, or HPtCl4·nH2O. The catalyst induces a crosslinking reaction with the crosslinker during the curing process to form the heat dissipation film.
[0040] The heat dissipation filler has a heat dissipation main agent and a heat dissipation auxiliary agent. The heat dissipation main agent is spherical alumina, and the heat dissipation auxiliary agent includes plate-like alumina and spherical AlN. The heat dissipation auxiliary agent may be added with spherical BN and / or plate-like silica.
[0041] The spherical alumina has a size of 3 to 7 μm, and is contained in the heat dissipating molding agent at 450 wt % to 850 wt % relative to the silicone resin.
[0042] The plate-like alumina has a size of 0.1 μm to 1 μm, and is contained in the silicone resin at a content ratio of 10 wt% to 45 wt%. The spherical AlN has two sizes, the first spherical AlN has a size of 50 to 60 μm, and is contained in the silicone resin at a content ratio of 80 wt% to 300 wt%, and the second spherical AlN has a size of 80 μm to 100 μm, which is larger than the first spherical AlN, and is mixed at a weight ratio of 300 wt% to 550 wt%. The plate-like silica has a size of 0.1 μm to 0.5 μm, and is contained in the silicone resin at a content ratio of 0.1 wt% to 1 wt%.
[0043] In the present invention, the spherical AlN has a relatively large size, and the plate-like alumina and plate-like silica have a small size. The spherical alumina, which is the heat dissipation main material, has an intermediate size. The very small plate-like heat dissipation material and the intermediate-sized heat dissipation material are arranged between the substantially large-sized heat dissipation materials. This allows for smooth heat dissipation.
[0044] The thermally conductive filler also affects the viscosity and thixotropy index (TI) value of the thermally conductive molding agent. If the size of the thermally conductive filler is small, the viscosity and TI value increase, and if the size of the thermally conductive filler increases relatively, the viscosity and TI value decrease. Therefore, those skilled in the art can adjust the weight ratio of each thermally conductive filler to obtain a viscosity and TI value suitable for the thermally conductive film manufacturing process. This is related to the overall surface area of the thermally conductive filler. If the overall surface area of the thermally conductive filler increases, the viscosity and TI value increase.
[0045] In the present invention, the surface reaction between the crosslinker and the heat-dissipating filler is described by the following reaction formula:
[0046] [Reaction Scheme 1] R-Si(OR')3+3H2O→R-Si(OH)3+3R'OH
[0047] First, hydrolysis occurs in the crosslinker R-Si(OR')3 (R: alkyl group), and the silanol group R-Si(OH)3 is adsorbed onto the surface of the thermally conductive filler. Through heating in the curing process, a siloxane bond is formed and fixed on the surface of the thermally conductive filler as shown in Reaction Scheme 2 below.
[0048] [Reaction Scheme 2] R-SiOH+HO-filler→R-Si-O-filler
[0049] Through the above reaction scheme, the surface of the heat-dissipating filler is treated to be hydrophobic.
[0050] The precipitation inhibitor prevents the heat-dissipating fillers having different loads from settling in the silicone resin, which is the polymer matrix, and allows the fillers to be uniformly dispersed in the heat-dissipating molding material through stirring.
[0051] Polysiloxane is used as the precipitation inhibitor. The precipitation inhibitor is included in the amount of 0.2wt% to 0.5wt% of the silicone resin. If the precipitation inhibitor is less than the set range, a phenomenon occurs in which a part of the heat dissipation filler precipitates, and if it exceeds the set range, the adhesive strength of the silicone resin decreases, causing the formed heat dissipation film to peel off from the substrate.
[0052] The retarder used is tetravinyl tetramethyl cyclo tetrasiloxane ([CH3(CH2=CH)SiO]4). The retarder can retard the hardening of the heat-conductive molding agent. If the hardening proceeds too quickly, the surface roughness of the heat-conductive film increases and the hardening of the surface proceeds with the internal hardening of the heat-conductive film incomplete, causing cracks inside the film. The retarder is included in an amount of 0.1wt% to 0.6wt% relative to the silicone resin. If the retarder is less than the range described above, the hardening is not retarded smoothly and the surface roughness increases. Also, if the retarder is more than the set range, the efficiency of the process decreases due to excessive hardening time.
[0053] The heat dissipating molding agent having the above-mentioned composition is formed as a two-liquid type. That is, a first syringe and a second syringe are prepared, and the heat dissipating molding agent is separately charged into each syringe. A first liquid type heat dissipating molding agent is introduced into the first syringe. The first liquid type heat dissipating molding agent has a silicone resin, a heat dissipating filler, a crosslinking agent, a precipitation inhibitor, and a retarder. A second liquid type heat dissipating molding agent is charged into the second syringe. The second liquid type heat dissipating molding agent includes a silicone resin, a heat dissipating filler, a catalyst, and a precipitation inhibitor. The silicone resin, the heat dissipating filler, and the precipitation inhibitor are commonly charged into the two types of syringes. The precipitation inhibitor is for ensuring uniform dispersion of the heat dissipating filler, and is essentially introduced.
[0054] In addition, the first liquid type heat dissipating molding agent has a crosslinking agent and a retarder, compared to the second liquid type heat dissipating molding agent. The retarder may be added to the second syringe, but is mixed with the crosslinking agent in advance in the first syringe to effectively delay the crosslinking action of the crosslinking agent during the curing process. The crosslinking agent introduced into the first syringe makes the surface of the heat dissipating filler hydrophobic, thereby preventing layer separation of the heat dissipating filler during the subsequent mixing and coating process of the two types of heat dissipating molding agents.
[0055] A catalyst is also placed in the second syringe. By placing the crosslinker and catalyst in different syringes, no curing action occurs within each syringe.
[0056] The two types of heat-dissipating molding agents are then mixed together to form a heat-dissipating film, which is then coated onto the substrate, after which a curing process is performed.
[0057] In the present invention, curing is performed using heat or light. Heat curing is performed at 80°C to 200°C for 5 to 20 minutes. Alternatively, hybrid type curing in which heat curing and light curing are mixed may be performed. For example, curing may be performed by irradiating near infrared rays under conditions of 80°C to 200°C.
[0058] Mixing Example 1: Silicone Resin Production A silicone resin is produced by mixing 20 wt % of the first polydiorganosiloxane, 30 wt % of the second polydiorganosiloxane, 45.5 wt % of the first polydihydrogensiloxane, and 0.5 wt % of the second polydihydrogensiloxane.
[0059] Preparation Example 1: Preparation of first liquid type heat dissipating molding agent and second liquid type heat dissipating molding agent 1 The silicone resin of the mixture example is poured into the first container, and spherical alumina of 5 μm size, plate-like alumina of 0.5 μm size, first AlN of 55 μm size, and second AlN of 80 μm size are used.
[0060] The spherical alumina is mixed with the silicon resin at 500 wt %, the plate-like alumina is mixed with the silicon resin at 10 wt %, the first AlN is mixed with the silicon resin at 102.3 wt %, and the second AlN is mixed with the silicon resin at 300 wt %.
[0061] The cross-linking agent, vinyltrimethoxysilane, is mixed at 1.58 wt % relative to the silicone resin, the precipitation inhibitor, polysiloxane, is mixed at 0.348 wt % relative to the silicone resin, and the retarder, tetravinyltetramethylcyclotetrasiloxane, is mixed at 0.4 wt % relative to the silicone resin.
[0062] The mixed solution in the first container is stirred by a suitable means to produce a first liquid type heat-dissipating molding agent, which is then poured into a first syringe.
[0063] The silicone resin manufactured by the mixing example is put into the second container, and the spherical alumina is 5 μm in size, the plate-like alumina is 0.5 μm in size, the first AlN is 55 μm in size, and the second AlN is 80 μm in size.
[0064] The spherical alumina is mixed with the silicon resin at 500 wt %, the plate-like alumina is mixed with the silicon resin at 10 wt %, the first AlN is mixed with the silicon resin at 102.3 wt %, and the second AlN is mixed with the silicon resin at 300 wt %.
[0065] The catalyst, H2PtCl6·nH2O, is mixed at 4.2 wt% with the silicone resin.
[0066] The mixed solution in the second container is stirred using an appropriate means to prepare a second liquid type heat-dissipating molding agent, which is then poured into a second syringe.
[0067] Preparation Example 2: Preparation of first liquid type heat dissipating molding agent and second liquid type heat dissipating molding agent 2 The content ratio of the heat dissipating filler is changed in the first and second liquid heat dissipating molding agents in the manufacturing example 1. The composition and content are the same as those in manufacturing example 1, except that the spherical alumina in the first and second liquid types is mixed in the same syringe as 450 wt% of the silicone resin, the plate-like alumina is mixed in 15 wt% of the silicone resin, the first AlN is mixed in 100 wt% of the silicone resin, and the second AlN is mixed in 350 wt% of the silicone resin.
[0068] Preparation Example 3: Preparation of first liquid type heat dissipating molding agent and second liquid type heat dissipating molding agent 3 The content ratio of the heat dissipating filler is changed in the first and second liquid heat dissipating molding agents in the manufacturing example 1. The composition and content are the same as those in manufacturing example 1, except that the spherical alumina in the first and second liquid types is mixed in the same syringe as 500 wt% of the silicone resin, the plate-like alumina is mixed in 10 wt% of the silicone resin, the first AlN is mixed in 102.3 wt% of the silicone resin, and the second AlN is mixed in 500 wt% of the silicone resin.
[0069] Preparation Example 4: Preparation of first liquid type heat dissipating molding agent and second liquid type heat dissipating molding agent 4 The content ratio of the heat dissipating filler is changed in the first and second liquid heat dissipating molding agents in the manufacturing example 1. The composition and content are the same as those in manufacturing example 1, except that the spherical alumina in the first and second liquid types is mixed in the same syringe as 450 wt% of the silicone resin, the plate-like alumina is mixed in 15 wt% of the silicone resin, the first AlN is mixed in 100 wt% of the silicone resin, and the second AlN is mixed in 35 wt% of the silicone resin.
[0070] Preparation Example 5: Preparation of first liquid type heat dissipating molding agent and second liquid type heat dissipating molding agent 5 The content ratio of the heat dissipating filler is changed in the first and second liquid heat dissipating molding agents in the manufacturing example 1. The composition and content are the same as those in manufacturing example 1, except that the spherical alumina in the first and second liquid types is mixed in the same syringe as 450 wt% of the silicone resin, the plate-like alumina is mixed in 10 wt% of the silicone resin, the first AlN is mixed in 90 wt% of the silicone resin, and the second AlN is mixed in 400 wt% of the silicone resin.
[0071] Preparation Example 6: Preparation of first liquid type heat dissipating molding agent and second liquid type heat dissipating molding agent 6 The content ratio of the heat dissipating filler is changed in the first and second liquid heat dissipating molding agents in the manufacturing example 2. The composition and content are the same as those in manufacturing example 1, except that the spherical alumina in the first and second liquid types is mixed in the same syringe as 500 wt% of the silicone resin, the plate-like alumina is mixed in 10 wt% of the silicone resin, the first AlN is mixed in 80 wt% of the silicone resin, and the second AlN is mixed in 500 wt% of the silicone resin.
[0072] The first and second syringes of Preparation Examples 1 to 6 are stored separately, then mixed in a discharge nozzle and coated onto a substrate. After coating, the mixture is cured at 250°C for 10 minutes. After the curing process is completed, the thermal conductivity of the manufactured heat-dissipating film is measured. Table 1 below shows the thermal conductivity of the heat-dissipating films manufactured using the heat-dissipating molding agents of Preparation Examples 1 to 6.
[0073] [Table 1]
[0074] Preparation Example 7: Preparation of first liquid type heat dissipating molding agent and second liquid type heat dissipating molding agent-7 The content ratio of the heat dissipating filler is changed in the first and second liquid heat dissipating molding agents in the manufacturing example 1. The composition and content are the same as those in manufacturing example 1, except that the spherical alumina in the first and second liquid types is mixed in the same syringe with 780 wt% of the silicone resin, the plate-like alumina is mixed with 20.4 wt% of the silicone resin, the first AlN is mixed with 100 wt% of the silicone resin, and the second AlN is mixed with 430 wt% of the silicone resin.
[0075] Production Example 8: Production of first liquid type heat dissipating molding agent and second liquid type heat dissipating molding agent-8 The content ratio of the heat dissipating filler is changed in the first and second liquid heat dissipating molding agents in the manufacturing example 1. The composition and content are the same as those in manufacturing example 1, except that the spherical alumina in the first and second liquid types is mixed in the same syringe at 800 wt% with respect to the silicone resin, the plate-like alumina is mixed at 18 wt% with respect to the silicone resin, the first AlN is mixed at 100 wt% with respect to the silicone resin, and the second AlN is mixed at 450 wt% with respect to the silicone resin.
[0076] Production Example 9: Production of first liquid type heat dissipating molding agent and second liquid type heat dissipating molding agent-9 The content ratio of the heat dissipating filler is changed in the first and second liquid heat dissipating molding agents in the manufacturing example 1. The composition and content are the same as those in manufacturing example 1, except that the spherical alumina in the first and second liquid types is mixed in the same syringe with 750 wt% of the silicone resin, the plate-like alumina is mixed with 20 wt% of the silicone resin, the first AlN is mixed with 200 wt% of the silicone resin, and the second AlN is mixed with 500 wt% of the silicone resin.
[0077] Preparation Example 10: Preparation of first liquid type heat dissipating molding agent and second liquid type heat dissipating molding agent-10 The content ratio of the heat dissipating filler is changed in the first and second liquid heat dissipating molding agents in the manufacturing example 1. The composition and content are the same as those in manufacturing example 1, except that the spherical alumina in the first and second liquid types is mixed in the same syringe with 780 wt% of the silicone resin, the plate-like alumina is mixed with 20.4 wt% of the silicone resin, the first AlN is mixed with 100 wt% of the silicone resin, and the second AlN is mixed with 430 wt% of the silicone resin.
[0078] Production Example 11: Production of first liquid type heat dissipating molding agent and second liquid type heat dissipating molding agent-11 The content ratio of the heat dissipating filler is changed in the first and second liquid heat dissipating molding agents in the manufacturing example 1. The composition and content are the same as those in manufacturing example 1, except that the spherical alumina in the first and second liquid types is mixed in the same syringe with 800 wt% of the silicone resin, the plate-like alumina is mixed with 30 wt% of the silicone resin, the first AlN is mixed with 220 wt% of the silicone resin, and the second AlN is mixed with 510 wt% of the silicone resin.
[0079] Production Example 12: Production of first liquid type heat dissipating molding agent and second liquid type heat dissipating molding agent-12 The content ratio of the heat dissipating filler is changed in the first and second liquid heat dissipating molding agents in the manufacturing example 1. The composition and content are the same as those in manufacturing example 1, except that the spherical alumina in the first and second liquid types is mixed in the same syringe with 810 wt% of the silicone resin, the plate-like alumina is mixed with 45 wt% of the silicone resin, the first AlN is mixed with 300 wt% of the silicone resin, and the second AlN is mixed with 480 wt% of the silicone resin.
[0080] The first and second syringes of Preparation Examples 7 to 12 were stored separately, then mixed in a discharge nozzle and coated onto a substrate. After coating, the substrate was cured at 250°C for 10 minutes. After the curing process was completed, the thermal conductivity of the heat-dissipating film was measured. Table 2 below shows the thermal conductivity of the heat-dissipating film manufactured according to each preparation example.
[0081] [Table 2]
[0082] Comparing Tables 1 and 2, the heat dissipation films of Production Examples 7 to 12 show high thermal conductivity of 10 W / (mK) or more. In the data of Table 2, the weight ratio of spherical alumina is increased compared to the data of Table 1, and the weight ratio of plate-like alumina is also increased.
[0083] In the production example, the spherical alumina has a size of 5 μm and the plate alumina has a size of 0.5 μm. It is confirmed that the slight increase in the smallest size of plate alumina while increasing the content ratio of the relatively large size of spherical alumina is an important factor in improving thermal conductivity.
[0084] That is, it is preferable that the spherical alumina is contained in the silicone resin at 750 wt % to 830 wt %, and the plate-like alumina is contained in the silicone resin at 18 wt % to 45 wt %.
[0085] It can also be seen that even if the content ratio of the second AlN having the largest particle size is changed, it does not have a large effect on the thermal conductivity. Even if the content ratio of the second AlN having the largest particle size in the heat transfer system is changed to 400w% to 510wt%, it does not have a large effect on the thermal conductivity.
[0086] FIG. 1 is a schematic diagram for explaining the heat dissipation operation of a heat dissipation film according to a preferred embodiment of the present invention.
[0087] 1, a heat-dissipating film 300 is formed on a substrate 10. In the heat-dissipating film 300, a filler 100 is disposed within a silicone polymer matrix 200 that has been cross-linked through a curing process.
[0088] The polymer matrix 200 made of silicone resin has strong adhesive strength with the substrate 10 due to the action of the crosslinking agent and catalyst. The crosslinking agent induces crosslinking between silicone resins and performs hydrophobic treatment of the thermally conductive filler 100. As the thermally conductive filler 100 is hydrophobic treated, the effect of moisture penetrating the polymer matrix 200 is minimized. In addition, the long-term stability of the thermally conductive film 300 is ensured by blocking external moisture, etc.
[0089] In particular, the polymer matrix 200 has a specific gravity of about 1.0, and the alumina has a specific gravity of about 4.0. Also, the AlN has a specific gravity of 2.8 to 2.9. In the present invention, a precipitation inhibitor is added to the heat-dissipating molding agent. The precipitation inhibitor prevents layer separation caused by the difference in specific gravity between the types of heat-dissipating fillers 100. Therefore, the heat-dissipating fillers 100 having different sizes and specific gravities can be arranged in an evenly dispersed form.
[0090] In addition, the content of alumina having a high specific gravity compared to the polymer matrix 200 is relatively decreased, and the content of AlN having a relatively low specific gravity is significantly increased, so that even if a small amount of a precipitation inhibitor is added, the phase separation phenomenon can be prevented.
[0091] In addition, when examining the thermal conductivity of each type of material, alumina has a conductivity of 25 W / (mK), and AlN has a conductivity of 270 W / (mK).
[0092] AlN, which has high thermal conductivity, has the largest size, and alumina, which has relatively low thermal conductivity, has the smallest size. Heat is transferred mainly through AlN, but spherical AlN 120 is disposed between spherical alumina 110, and a significant portion of the surface of the spherical AlN 120 comes into contact with the spherical alumina 110 to perform heat dissipation. Also, a small amount of plate-like alumina 130 is disposed between the spherical alumina 110 or between the spherical alumina 110 and the spherical AlN 120. In addition to the heat transfer function by the plate-like alumina 130, the plate-like alumina 130 can increase the viscosity of the heat dissipation molding agent, and is therefore also used for viscosity adjustment.
[0093] In the present invention, a two-liquid type heat-dissipating molding agent is prepared, and two different types of liquid type heat-dissipating molding agents are stored in separate syringes. In the process of forming a heat-dissipating film, the two types of heat-dissipating molding agents charged in the different syringes are combined and discharged through a nozzle to form a heat-dissipating film.
[0094] The first liquid type heat dissipating molding agent has a lower viscosity than the second liquid type heat dissipating molding agent because a retarder and a crosslinking agent are added. The first liquid type heat dissipating molding agent preferably has a viscosity of 320,000cp to 370,000cp, and the second liquid type heat dissipating molding agent preferably has a viscosity of 450,000cp to 530,000cp. In addition, it is preferable that the second liquid type heat dissipating molding agent has a high viscosity, and the difference in viscosity between the two types of heat dissipating molding agents is 200,000cp or less. If a viscosity difference of more than 200,000cp occurs, there is no problem with the miscibility of the heat dissipating filler, but the retarder and crosslinking agent in the first liquid type heat dissipating molding agent cannot be dispersed evenly in the mixed heat dissipating molding agent, causing a localized rapid curing phenomenon. Therefore, bubbles are generated inside the polymer matrix due to the rapid curing of some areas, and the mechanical properties of the polymer matrix are reduced due to excessive shrinkage.
[0095] According to the present invention, thermally conductive fillers having various sizes and types are introduced. In addition, the surface of the thermally conductive fillers is hydrophobically treated by a crosslinking agent, and the thermally conductive fillers are evenly distributed in the thermally conductive molding material. In addition, a precipitation inhibitor is introduced to prevent layer separation caused by thermally conductive fillers having different specific gravities, and the thermally conductive fillers are evenly distributed by the precipitation inhibitor.
[0096] In addition, caking of the heat-dissipating film can be prevented by adjusting the viscosity of the liquid heat-dissipating molding agent and by using a retarder. The viscosity of the molding agent affects the thickness, surface flatness, and shape control of the heat-dissipating film during the coating process. If the viscosity of the molding agent is low, the thickness is reduced and the surface flatness is improved, but it is difficult to control the shape. If a retarder is introduced into the curing process, rapid curing that occurs in localized areas is prevented, and the phenomenon of excessive curing of parts of the surface is prevented. In other words, caking, in which parts of the surface harden and the heat-dissipating film is destroyed or peeled off due to mechanical impact, can be prevented. [Explanation of symbols]
[0097] 10: Base material 100: Heat dissipation filler 200: Polymer matrix 300: Heat dissipation film
Claims
1. A first liquid type heat dissipating molding agent and a second liquid type heat dissipating molding agent are included, The first liquid heat-dissipating molding agent includes a first silicone resin, a first heat-dissipating filler, a cross-linking agent, and a first suspending agent; the second liquid heat-dissipating molding agent comprises a second silicone resin, a second heat-dissipating filler, a catalyst and a second suspending agent; A heat-dissipating molding agent, which is formed by mixing the first liquid type heat-dissipating molding agent and the second liquid type heat-dissipating molding agent.
2. The heat-dissipating molding material according to claim 1, characterized in that the first heat-dissipating filler includes spherical alumina having a size of 3 μm to 7 μm, plate-shaped alumina having a size of 0.1 μm to 1 μm, first spherical AlN having a size of 50 μm to 60 μm, second spherical AlN having a size of 80 μm to 100 μm, and plate-shaped silica having a size of 0.1 μm to 0.5 μm.
3. 3. The heat dissipation molding agent of claim 2, wherein the spherical alumina is contained in an amount of 450 wt % to 850 wt % with respect to the first silicone resin, the plate-shaped alumina is contained in an amount of 10 wt % to 45 wt % with respect to the first silicone resin, the first spherical AlN is contained in an amount of 80 wt % to 300 wt % with respect to the first silicone resin, the second spherical AlN is contained in an amount of 300 wt % to 550 wt % with respect to the first silicone resin, and the plate-shaped silica is contained in an amount of 0.1 wt % to 1 wt % with respect to the first silicone resin.
4. 4. The heat dissipation molding material of claim 3, wherein the spherical alumina is contained in the first silicone resin at 750 wt % to 830 wt % and the plate-like alumina is contained in the first silicone resin at 18 wt % to 45 wt %.
5. 2. The heat sink molding material of claim 1, wherein the suspending agent is polysiloxane.
6. The heat dissipation molding material according to claim 1 , wherein the cross-linking agent comprises vinyltrimethoxysilane or phenyltrimethoxysilane.
7. The heat-dissipating molding material according to claim 6, wherein the crosslinking agent is adsorbed to the surface of the heat-dissipating filler by forming a silanol group through hydrolysis on the surface of the heat-dissipating filler.
8. The heat-dissipating molding material according to claim 7 , wherein the silanol groups form siloxane bonds on the surface of the heat-dissipating filler through a subsequent curing process.
9. 2. The heat-dissipating molding material according to claim 1, wherein the second liquid type heat-dissipating molding material has a higher viscosity than the first liquid type heat-dissipating molding material, and the difference in viscosity between the first liquid type heat-dissipating molding material and the second liquid type heat-dissipating molding material is 200,000 cp or less.
10. The first liquid type heat dissipation molding agent further includes a retarder for delaying a hardening action, 2. The heat sink molding material of claim 1, wherein the retarder is tetravinyltetramethylcyclotetrasiloxane.
11. A polymer matrix in which the silicone resin is hardened by a crosslinking agent; and a thermally conductive filler dispersed within the polymer matrix; The heat dissipation filler includes spherical alumina of 3 μm to 7 μm in size, plate-like alumina of 0.1 μm to 1 μm in size, first spherical AlN of 50 μm to 60 μm in size, second spherical AlN of 80 μm to 100 μm in size, and plate-like silica of 0.1 μm to 0.5 μm in size.
12. 12. The heat dissipation film of claim 11, wherein the spherical alumina is contained at 450 wt % to 850 wt % of the first silicone resin, the plate-shaped alumina is contained at 10 wt % to 45 wt % of the first silicone resin, the first spherical AlN is contained at 80 wt % to 300 wt % of the first silicone resin, the second spherical AlN is contained at 300 wt % to 550 wt % of the first silicone resin, and the plate-shaped silica is contained at 0.1 wt % to 1 wt % of the first silicone resin.
13. 13. The heat dissipation film of claim 12, wherein the spherical alumina is contained in the first silicone resin at 750 wt % to 830 wt %, and the plate-like alumina is contained in the first silicone resin at 18 wt % to 45 wt %.
14. The heat dissipation film according to claim 13, characterized in that it has a thermal conductivity of 10.1 W / (mK) to 10.43 W / (mK).
15. The heat dissipation film of claim 10, wherein the cross-linking agent comprises vinyltrimethoxysilane or phenyltrimethoxysilane.
16. The heat-dissipating film of claim 15, wherein the crosslinking agent forms a silanol group on the surface of the heat-dissipating filler by hydrolysis and is adsorbed to the surface of the heat-dissipating filler, and the silanol group forms a siloxane bond on the surface of the heat-dissipating filler through a subsequent curing process.
Citation Information
Patent Citations
Heat-conductive silicone composition, and method for producing heat-conductive member using the composition
JP2023183384A
Multicomponent-curable thermally-conductive silicone gel composition, thermally-conductive member and heat dissipation structure
WO2019021826A1
Thermally conductive composition package, and two-component curing type thermally conductive composition
WO2020262407A1
Thermally conductive silicone composition and method for producing gap filler using said composition
WO2023053760A1