Cellulose fiber-containing resin molded body
The cellulose fiber-containing resin molded article addresses the biodegradability and recyclability issues of traditional fiber-reinforced plastics by using dry papermaking and melt-kneading processes to maintain rigidity and impact resistance during recycling.
Patent Information
- Application Number
- JP2023155644
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2023-09-21
- Publication Date
- 2024-11-07
AI Technical Summary
Fiber-reinforced plastic molded bodies using reinforcing fibers like carbon and glass fibers have low biodegradability, leading to environmental challenges during disposal and incineration, and recycled products exhibit reduced rigidity and impact resistance.
A cellulose fiber-containing resin molded article with controlled flexural modulus decrease and high recyclability is achieved by manufacturing fiber aggregates through dry papermaking, compressing them into sheets, and melt-kneading to form pellets, ensuring uniform dispersion and maintaining strength and impact resistance.
The cellulose fiber-containing resin molded article maintains excellent bending rigidity and impact resistance while allowing for effective recycling with minimal loss in mechanical properties.
Smart Images

Figure 2024157503000002 
Figure 2024157503000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a cellulose fiber-containing resin molded article. [Background technology]
[0002] Fiber-reinforced plastic molded products made from nonwoven fabrics (also called sheets for fiber-reinforced plastic molded products) containing reinforcing fibers such as carbon fiber and glass fiber are already used in various fields such as sports and leisure goods, aircraft materials, electronic device components, etc. Thermosetting resins and thermoplastic resins are used as the resins that serve as the matrix in fiber-reinforced plastic molded products, but in recent years, development of fiber-reinforced plastic molded products using thermoplastic resins has been progressing.
[0003] Carbon fiber, glass fiber, aramid fiber, etc. are used as reinforcing fibers. Such reinforcing fibers work to increase the strength of fiber-reinforced plastic molded bodies. When such molded products are to be disposed of, they are usually disposed of in landfills or incinerated. However, molded products using the above-mentioned reinforcing fibers have low biodegradability after being disposed of in landfills, and there is a problem that a large load is placed on incinerators during incineration.
[0004] For this reason, in recent years, the use of pulp fibers as reinforcing fibers has been proposed (for example, Patent Documents 1 to 3). In Patent Documents 1 and 2, a slurry containing pulp fibers and a thermoplastic resin is made into a paper and the molded intermediate product is heated and pressurized to obtain a molded article. Patent Document 3 proposes forming pellets from a slurry containing pulp fibers and a thermoplastic resin and injection molding the pellets to produce a molded article. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 6-322699 [Patent Document 2] Japanese Patent Application Publication No. 6-346399 [Patent Document 3] Japanese Patent Application Publication No. 6-345944 Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, the recycling of fiber-reinforced plastic molded bodies has also been studied. It has been found that when fiber-reinforced plastic molded bodies are crushed and then used as raw materials to re-use molded bodies, the recycled molded bodies have a problem of reduced bending rigidity compared to the molded bodies before recycling. An object of the present invention is to provide a cellulose fiber-containing resin molded article that is excellent in bending rigidity and recyclability. [Means for solving the problem]
[0007] The present inventors have found that the above-mentioned problems can be solved by controlling the rate of decrease in bending rigidity to a certain value or less when a cellulose fiber-containing resin molded article is recycled. The present invention relates to the following <1> ~ <12> Regarding. <1> A cellulose fiber-containing resin molding having a flexural modulus of 2.5 GPa or more as measured in accordance with JIS K 7171:2016, and a recycled cellulose fiber-containing resin molding obtained by melt-kneading the cellulose fiber-containing resin molding and re-molding the same, in which the flexural modulus decreases by 10% or less as compared to the cellulose fiber-containing resin molding. <2> The reduction rate of bending strength of the recycled cellulose fiber-containing resin molded body is 10% or less compared to that of the cellulose fiber-containing resin molded body. <1> The cellulose fiber-containing resin molded body according to claim 1. <3> The reduction rate of Charpy impact strength in the recycled cellulose fiber-containing resin molded body is 30% or less compared to that of the cellulose fiber-containing resin molded body. <1> or <2> The cellulose fiber-containing resin molded body according to claim 1. <4> The cellulose fiber content is 10% by mass or more and 90% by mass or less. <1> The cellulose fiber-containing resin molded product according to any one of items 1 to 3. <5> Density is 0.8g / cm 3 More than 1.5g / cm 3 Below is the <1> ~ <4> 10. The cellulose fiber-containing resin molded article according to claim 9, <6> The thickness is 2mm or more. <1> ~ <5> 10. The cellulose fiber-containing resin molded article according to claim 9, <7> Charpy impact strength of 2.0 kJ / m at a thickness of 4 mm, measured according to JIS K 7111-1:2012 2 That's all. <1> ~ <6> 10. The cellulose fiber-containing resin molded article according to claim 9, <8> The initial cellulose fiber-containing resin molded body before the first recycling is a molded body obtained by a method including the following steps 1, 2, 3, and 4 in this order. <1> ~ <7> 10. The cellulose fiber-containing resin molded article according to claim 9, Step 1: A fiber assembly manufacturing process in which a fiber assembly containing cellulose fiber and resin A is manufactured by dry papermaking. Step 2: A cellulose fiber-containing resin sheet manufacturing step of compressing the fiber assembly to manufacture a cellulose fiber-containing resin sheet. Step 3: A step of producing cellulose fiber-containing resin pellets by melt-kneading the cellulose fiber-containing resin sheet to produce pellets. Step 4: Molding the cellulose fiber-containing resin pellets <9> The resin A contains resin fibers. <8> The cellulose fiber-containing resin molded body according to claim 1. <10> When the tensile strength of the cellulose fiber-containing resin sheet in a first direction is T and the tensile strength of the cellulose fiber-containing resin sheet in a second direction perpendicular to the first direction is Y, T / Y is 0.5 or more and 1.5 or less. <8> or <9> The cellulose fiber-containing resin molded body according to claim 1. <11> In step 2, the bulk density of the cellulose fiber-containing resin sheet to be subjected to step 3 is 0.10 g / mL or more and 0.60 g / mL or less; <8> ~ <10> 10. The cellulose fiber-containing resin molded article according to claim 9, <12> The step 4 is a step of injection molding the cellulose fiber-containing resin pellets. <8> ~ <11> 10. The cellulose fiber-containing resin molded article according to claim 9, Effect of the Invention
[0008] According to the present invention, there is provided a cellulose fiber-containing resin molded article having excellent bending rigidity and excellent recyclability. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 shows the web forming apparatus used in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] [Cellulose fiber-containing resin molding] The cellulose fiber-containing resin molded body of this embodiment (hereinafter simply referred to as the "molded body") has a flexural modulus of 2.5 GPa or more as measured in accordance with JIS K 7171:2016, and a recycled cellulose fiber-containing resin molded body (hereinafter simply referred to as the "recycled molded body") obtained by melt-kneading the cellulose fiber-containing resin molded body and molding it again has a flexural modulus reduction rate of 10% or less compared to the cellulose fiber-containing resin molded body. According to the present invention, there is provided a cellulose fiber-containing resin molded article having excellent bending rigidity and excellent recyclability. Until now, the decrease in bending rigidity that occurs during recycling has not been considered. In the present invention, the decrease in bending rigidity due to recycling has been considered, and it has been found that by setting this within a specific range, it is possible to provide a cellulose fiber-containing resin molding that has extremely excellent recyclability, in which not only the decrease in bending rigidity and strength but also the decrease in impact resistance, etc. are suppressed. In the following explanation, the first molded body will be referred to as the "molded body (initial)", the recycled cellulose fiber-containing resin molded body obtained by melting and kneading the molded body (initial) and remolding it will be referred to as the "molded body (first recycled)", the recycled cellulose fiber-containing resin molded body obtained by melting and kneading the molded body (first recycled) and remolding it will be referred to as the "molded body (second recycled)", and similarly hereinafter, all of these will be referred to as the "molded body (nth recycled)". In this embodiment, the flexural modulus of the molded body (initial) and the molded body (nth recycled) measured in accordance with JIS K 7171:2016 is 2.5 GPa or more. In addition, the reduction rate of the flexural modulus of the molded body (first recycled) compared to the molded body (initial) is 10% or less. In addition, the reduction rate of the flexural modulus of the molded body (n+1th recycled) compared to the molded body (nth recycled) is 10% or less. The present invention will be described in further detail below.
[0011] <Characteristics of molded products> (Flexural modulus) The molded body of this embodiment has a flexural modulus of 2.5 GPa or more measured in accordance with JIS K 7171: 2016. The flexural modulus of the molded body is preferably 3.0 GPa or more, more preferably 3.3 GPa or more, and even more preferably 3.5 GPa or more. The upper limit is not particularly limited, but from the viewpoint of ease of production, it is preferably 10 GPa or less. It does not mean that only the flexural modulus of the molded body (initial stage) is 2.5 GPa or more, but that the flexural modulus of the molded body before recycling is 2.5 GPa or more. Therefore, for example, when recycling is performed twice in total, the flexural modulus of the molded body (initial stage) and the molded body (recycled once) is 2.5 GPa or more.
[0012] (Bending strength) The molded article of the present embodiment preferably has high bending strength, and since the molded article has high bending strength, it is preferable that the molded article has excellent rigidity. The bending strength of the molded article is preferably 20 MPa or more, more preferably 30 MPa or more, and even more preferably 35 MPa or more. The upper limit is not particularly limited, but from the viewpoint of ease of production, it is preferably 150 MPa or less. The bending strength of the molded body is measured in accordance with JIS K 7171:2016.
[0013] (Charpy impact strength) The molded article of the present embodiment preferably has high Charpy impact strength, and the Charpy impact strength of a molded article having a thickness of 4 mm is preferably 1.5 kJ / m 2 More preferably, 2.0 kJ / m 2 More preferably, 3.0 kJ / m 2 More preferably, 4.0 kJ / m 2 The upper limit is not particularly limited, but from the viewpoint of ease of production, it is preferably 100 kJ / m 2 Less than or equal to 30 kJ / m 2 Less than 20 kJ / m, more preferably 20 kJ / m 2 The following is the result. The larger the Charpy impact strength value, the more excellent the impact resistance. The Charpy impact strength is measured in accordance with JIS K 7111-1:2012, and in detail, is measured by the method described in the examples.
[0014] (density) In this embodiment, the density of the molded body is preferably 0.5 g / cm 3 More preferably, 0.8 g / cm 3 More preferably, 0.85 g / cm 3 More preferably, 0.90 g / cm 3 The density of the molded body is preferably 2.0 g / cm 3 Less than or equal to 1.5 g / cm 3 Less than 1.2 g / cm, more preferably 1.2 g / cm 3 The following is the result.
[0015] (Thickness) The thickness of the molded body is not particularly limited, but is 0.5 mm or more, more preferably 1 mm or more, even more preferably 2 mm or more, and is preferably 200 mm or less, more preferably 100 mm or less, even more preferably 50 mm or less, even more preferably 20 mm or less, and particularly preferably 10 mm or less. Incidentally, by making the thickness of the molded article 2 mm or more, it can be suitably used in applications requiring impact resistance, and therefore it is particularly preferable that the thickness of the molded article is 2 mm or more.
[0016] (Composition of Molded Body) The molded body contains at least cellulose fibers and a resin component. From the viewpoint of obtaining a molded body that has excellent recyclability, a high degree of biomass conversion, excellent bending rigidity and strength, and excellent impact resistance, the cellulose fiber content in the molded body is preferably 10 mass% or more, more preferably 15 mass% or more, even more preferably 20 mass% or more, even more preferably 25 mass% or more, and is preferably 90 mass% or less, more preferably 80 mass% or less, even more preferably 70 mass% or less, and even more preferably 60 mass% or less. Other components contained in the molded product will be described later.
[0017] <Recycling characteristics> (Decrease in flexural modulus) In the molded article of this embodiment, when the molded article is melt-kneaded and molded again, the reduction in bending modulus of the molded article from the bending modulus of the molded article before recycling is 10% or less. The rate of decrease in flexural modulus after the first recycling is expressed by the following formula. Decrease in bending modulus after first recycling = (flexural modulus of molded body (initial) - flexural modulus of molded body (first recycled)) ÷ flexural modulus of molded body (initial) × 100 Similarly, the decrease in the flexural modulus after the second recycling is expressed by the following formula: Decrease in bending modulus after second recycling = (flexural modulus of molded body (first recycled) - flexural modulus of molded body (second recycled)) ÷ flexural modulus of molded body (first recycled) × 100 The decrease rate of the flexural modulus is preferably 7% or less, more preferably 5% or less, and further preferably 3% or less, with no particular lower limit. The flexural modulus is measured in accordance with JIS K 7171:2016.
[0018] (Decrease in bending strength) In the molded article of this embodiment, the molded article is melt-kneaded and molded again to produce a recycled molded article, and the bending strength of the molded article before recycling is preferably reduced by 10% or less. The rate of decrease in bending strength after the first recycling is expressed by the following formula. Decrease in bending strength after first recycling = (Bending strength of molded body (initial) - bending strength of molded body (first recycled)) ÷ bending strength of molded body (initial) × 100 Similarly, the rate of decrease in bending strength after the second recycling is expressed by the following formula. Decrease in bending strength after second recycling = (Bending strength of molded body (first recycled) - bending strength of molded body (second recycled)) ÷ bending strength of molded body (first recycled) × 100 The rate of decrease in bending strength is preferably 8% or less, more preferably 7% or less, and further preferably 5% or less, with no particular lower limit. The bending strength of the molded body is measured in accordance with JIS K 7171:2016.
[0019] (Charpy impact strength reduction rate) The molded article of the present embodiment is preferably a recycled molded article obtained by melt-kneading the molded article and molding it again, and the Charpy impact strength of the recycled molded article is preferably reduced by 30% or less from the Charpy impact strength of the molded article before recycling. Note that the Charpy impact strength is the Charpy impact strength of a molded article having a thickness of 4 mm. The rate of decrease in Charpy impact strength after the first recycling is expressed by the following formula. Decrease rate of Charpy impact strength after first recycling = (Charpy impact strength of compact (initial) - Charpy impact strength of compact (first recycled)) ÷ Charpy impact strength of compact (initial) × 100 Similarly, the rate of decrease in Charpy impact strength after the second recycling is expressed by the following formula: Decrease rate of Charpy impact strength after second recycling = (Charpy impact strength of compact (recycled for the first time) - Charpy impact strength of compact (recycled for the second time)) ÷ Charpy impact strength of compact (recycled for the first time) × 100 The rate of decrease in the Charpy impact strength is preferably 25% or less, more preferably 20% or less, even more preferably 17% or less, and still more preferably 15% or less, with no particular lower limit. The Charpy impact strength is measured in accordance with JIS K 7111-1:2012, and in detail, is measured by the method described in the examples.
[0020] [Method of manufacturing the molded body (initial stage)] In this embodiment, the initial cellulose fiber-containing resin molded body before the first recycling, i.e., the molded body (initial), may be a molded body obtained by any method, but is preferably a molded body obtained by a method including the following steps 1 to 4 in this order. It is difficult to directly specify the molded body (initial) by its structure or characteristics. Compared with the conventional method of simply melt-kneading cellulose fibers and resin to produce pellets, a fiber aggregate is produced by dry papermaking, and the pellets are produced by compressing the fiber aggregate to produce a cellulose fiber-containing resin sheet. Since the cellulose fibers are uniformly dispersed in advance in the cellulose fiber-containing resin sheet, aggregation and poor dispersion of the cellulose fibers during melt-kneading are suppressed, and the cellulose fibers are highly dispersible in the cellulose fiber-containing resin pellets, and the high dispersibility of the cellulose fibers is maintained in the molded body. As a result, a molded body having excellent bending rigidity and strength, and excellent impact resistance is obtained. Step 1: A fiber assembly manufacturing process in which a fiber assembly containing cellulose fiber and resin A is manufactured by dry papermaking. Step 2: A cellulose fiber-containing resin sheet manufacturing step of compressing the fiber assembly to manufacture a cellulose fiber-containing resin sheet. Step 3: A step of producing cellulose fiber-containing resin pellets by melt-kneading the cellulose fiber-containing resin sheet to produce pellets. Step 4: Molding the cellulose fiber-containing resin pellets Each step will be described below.
[0021] <Process 1> Step 1 is a fiber assembly production step in which a fiber assembly containing cellulose fibers and resin A is produced by dry papermaking. (Cellulose fiber) The cellulose fibers are not particularly limited in terms of the manufacturing method and type. The cellulose fibers are preferably pulp fibers, and may be, for example, chemical pulps such as hardwood and / or softwood kraft pulp, mechanical pulps such as SGP, RGP, BCTMP and CTMP, waste paper pulps such as deinked pulp, and non-wood pulps such as kenaf, jute, bagasse, bamboo, straw, and hemp. Chlorine-free pulps such as ECF pulp and TCF pulp can also be used. The cellulose fiber is preferably pulp fiber, but is not limited thereto. For example, paper powder, wood powder, etc. may be used.
[0022] Among the above pulp fibers, kraft pulp fibers, particularly softwood kraft pulp fibers (NBKP) having long fiber length, are preferably used as the cellulose fibers because the resulting molded article has excellent flexural modulus and impact resistance.
[0023] From the viewpoint of improving the flexural modulus and impact resistance of the obtained molded body and from the viewpoint of ease of production of the fiber assembly, the average fiber length of the cellulose fibers is preferably 0.1 mm or more, more preferably 0.5 mm or more, even more preferably 1 mm or more, and is preferably 50 mm or less, more preferably 10 mm or less, even more preferably 5 mm or less, and even more preferably 2.5 mm or less. The average fiber length of the cellulose fibers is measured by the method described in the Examples.
[0024] From the viewpoint of improving the bending rigidity and impact resistance of the obtained molded body and from the viewpoint of ease of production of the fiber assembly, the average fiber width of the cellulose fibers is preferably 1 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, still more preferably 15 μm or more, and is preferably 150 μm or less, more preferably 100 μm or less, even more preferably 80 μm or less, and still more preferably 50 μm or less. The average fiber width of the cellulose fibers is measured by the method described in the Examples.
[0025] In this embodiment, when the fiber aggregate is formed by an airlaid method, the cellulose fibers can be in the form of, for example, defibrated dry pulp.
[0026] The cellulose fibers are preferably unbeaten cellulose fibers in order to improve the impact resistance of the resulting molded article. In order for a molded body to exhibit impact resistance, the cellulose fibers must be properly pulled out of the resin when an impact is applied. For this purpose, unbeaten cellulose fibers having a low ratio of fine fibers are preferable, and unbeaten pulp fibers are even more preferable. From the above-mentioned viewpoints, the fine fiber ratio of the cellulose fibers is preferably 50% or less, more preferably 30% or less, and further preferably 20% or less, with no particular lower limit. The fine fiber ratio of the cellulose fibers is measured by the method described in the Examples.
[0027] The cellulose fiber content in the cellulose fiber-containing resin sheet is, from the viewpoint of obtaining a molded product having excellent flexural modulus and impact resistance, and from the viewpoint of the productivity and ease of production of the cellulose fiber-containing resin sheet, preferably 10% by mass or more and 90% by mass or less, more preferably 15% by mass or more, even more preferably 20% by mass or more, still more preferably 25% by mass or more, and more preferably 85% by mass or less, even more preferably 80% by mass or less, and still more preferably 75% by mass or less.
[0028] (Resin A) Examples of resin A components include polyolefin, polyvinyl chloride, polystyrene, ABS (acrylonitrile-butadiene-styrene), acrylonitrile-styrene, polyester, acrylic resin, polyamide, polyacetal, polycarbonate, polybutylene succinate, and polylactic acid. In addition, resins or elastomers exemplified as lubricants, plasticizers, nucleating agents, flame retardants, antistatic agents, fillers, and papermaking chemicals described in [Other components] below may also be used. In other words, resin A refers to the resin component contained in the molded product. As shown in the manufacturing method of the molded body described later, the molded body of this embodiment is preferably manufactured through a process in which a cellulose fiber aggregate containing cellulose fibers and resin A is manufactured by dry papermaking, and then compressed to manufacture a cellulose fiber-containing resin sheet. That is, it is preferable that at least resin A is blended with the cellulose fiber aggregate. In the manufacturing of the molded body, further resin or elastomer may be added.
[0029] In the present invention, the resin A contained in the fiber assembly can be any of fibers, powder, granules, and pellets. Among these, from the viewpoint of ease of papermaking in step 1 described below and the viewpoint of dispersibility of cellulose fibers in pellets and molded bodies, the resin A contained in the fiber assembly is preferably fiber or powder, and more preferably fiber. That is, the resin A contained in the fiber assembly preferably contains resin fiber or resin powder, more preferably contains resin fiber, and further preferably contains resin fiber. Preferred examples of the fibers of resin A contained in the fiber assembly include polyolefin fibers, polyvinyl chloride fibers, polyester fibers, acrylic fibers, polyamide fibers, polycarbonate fibers and polylactic acid fibers. Preferred examples of the powder, granules, and pellets of resin A to be contained in the fiber assembly include polyolefin, polyvinyl chloride, polyester, acrylic, polyamide, polycarbonate, polylactic acid, polystyrene, ABS, acrylonitrile-styrene powder, polyacetal, and polybutylene succinate. Particularly preferred examples of the powder of resin A include polyolefin powder, polystyrene powder, ABS powder, acrylonitrile-styrene powder, polyacetal powder, and polybutylene succinate powder. The polyolefin may be the same as the specific examples of polyolefin in the polyolefin fiber shown below. Among these, polyolefin fibers are preferred as the resin A contained in the fiber assembly. The resin A contained in the fiber assembly may be one or a combination of two or more resins. For example, the resin A may be a combination of two types of resins, namely, polylactic acid fiber and polybutylene succinate powder.
[0030] [Polyolefin fiber] In this embodiment, when polyolefin fibers are used as the resin A contained in the fiber assembly, the polyolefin constituting the polyolefin fibers is not particularly limited, and examples thereof include polyolefins (unmodified polyolefins) and modified polyolefins. The melting point of the polyolefin constituting the polyolefin fiber is preferably 200°C or lower, more preferably 195°C or lower, and even more preferably 180°C or lower, from the viewpoint of ease of molding and suppressing deterioration of the cellulose fiber, and is preferably 80°C or higher, more preferably 90°C or higher, and even more preferably 100°C or higher.
[0031] Examples of polyolefins include polyethylene, polypropylene, and ethylene-propylene copolymers (also called propylene-ethylene copolymers), with polyethylene and polypropylene being preferred. In the modified polyolefin, the method of modifying the polyolefin includes, for example, acid modification, chlorination, etc., and among these, acid modification is preferred from the viewpoint of improving the affinity with cellulose fibers. The acid-modifying component used for the acid modification of the acid-modified polyolefin is preferably an unsaturated carboxylic acid component. The unsaturated carboxylic acid component is a component derived from an unsaturated carboxylic acid and its acid anhydride. Examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, maleic acid, maleic anhydride, itaconic acid, itaconic anhydride, fumaric acid, and crotonic acid. Among them, the unsaturated carboxylic acid component is preferably at least one selected from acrylic acid, methacrylic acid, maleic acid, and maleic anhydride, and is particularly preferably at least one selected from maleic acid and maleic anhydride. A polyolefin modified with at least one of maleic acid and maleic anhydride is also called a maleic acid-modified polyolefin. The acid-modified polyolefin is preferably a maleic acid-modified polyolefin, more preferably a maleic acid-modified polyethylene or a maleic acid-modified polypropylene. Note that it is sufficient that the acid-modified polyolefin is at least partially modified with an acid.
[0032] The polyolefin is particularly preferably at least one selected from the group consisting of polyethylene, polypropylene, polyethylene at least partially modified with maleic acid, polypropylene at least partially modified with maleic acid, and ethylene-propylene copolymer. From the viewpoint of improving the flexural modulus of the obtained molded article, it is preferable that the polyolefin contains an acid-modified polyolefin, it is more preferable that the polyolefin contains at least one of polyethylene at least partially modified with maleic acid and polypropylene at least partially modified with maleic acid, and it is even more preferable that the polyolefin contains polyethylene at least partially modified with maleic acid. From the viewpoint of improving the impact resistance of the resulting molded article, it is preferable that the composition does not contain an acid-modified polyolefin, and it is more preferable that the polyolefin contains only polyethylene, polypropylene, and an ethylene-propylene copolymer. The polyolefin fibers may be used alone or in combination of two or more kinds.
[0033] The polyolefin fiber may be a composite fiber made of two or more polyolefins, and examples thereof include split fibers, sea-island fibers, core-sheath fibers, and laminated fibers. Among these, from the viewpoint of obtaining a molded product having excellent bending rigidity and impact resistance, the core-sheath fibers are preferred. In the case of the core-sheath fibers, fibers having a concentric cross-sectional structure or an eccentric cross-sectional structure are used, and the fibers having a concentric cross-sectional structure are preferred. The use of the fibers having a concentric cross-sectional structure is preferred because a more uniform fiber assembly can be obtained.
[0034] From the viewpoint of obtaining a uniform fiber assembly and ease of production of the fiber assembly, the fiber length of the polyolefin fiber is preferably 0.1 mm or more, more preferably 1.0 mm or more, even more preferably 2.0 mm or more, even more preferably 3.0 mm or more, and is preferably 50 mm or less, more preferably 20 mm or less, even more preferably 10 mm or less. The fiber length of the polyolefin fiber is measured by the method described in the Examples.
[0035] From the viewpoint of obtaining a uniform fiber assembly and ease of production of the fiber assembly, the fiber diameter of the polyolefin fiber is preferably 0.1 μm or more, more preferably 1 μm or more, and even more preferably 10 μm or more, and is preferably 100 μm or less, more preferably 80 μm or less, and even more preferably 50 μm or less. The fiber diameter of the polyolefin fiber is measured by the method described in the Examples.
[0036] From the viewpoint of obtaining a uniform fiber assembly and from the viewpoint of ease of production of the fiber assembly, the fineness of the polyolefin fiber is preferably 0.01 dtex or more, more preferably 0.1 dtex or more, even more preferably 1 dtex or more, and is preferably 100 dtex or less, more preferably 50 dtex or less, even more preferably 10 dtex or less.
[0037] When the resin A contained in the fiber assembly is a polyolefin fiber, the content of the polyolefin fiber in the fiber assembly is preferably 90% by mass or less from the viewpoint of obtaining a molded product having excellent bending rigidity and impact resistance, more preferably 80% by mass or less, even more preferably 65% by mass or less from the viewpoint of productivity and ease of production, and even more preferably 50% by mass or less, particularly preferably 45% by mass or less from the viewpoint of the degree of biomass conversion and productivity. Also, from the same viewpoint, it is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, and even more preferably 25% by mass or more. When two or more kinds of polyolefin fibers are used, the above content means the total content of the polyolefin fibers.
[0038] When resin A is a fiber other than a polyolefin fiber, the preferred fiber length, fiber diameter, fineness and content of the fiber are the same as the preferred fiber length, fiber diameter, fineness and content of the polyolefin fiber, respectively. In addition, when the resin A is a powder, granule, or pellet, the preferred content of the powder, granule, or pellet is the same as the preferred content of the polyolefin fiber. In addition, when the resin A is a powder, granule, or pellet, the particle size of the powder, granule, or pellet is not particularly limited.
[0039] [Other ingredients] When the resin A in the fiber assembly of the present embodiment is a polyolefin fiber, the fiber assembly may contain other components in addition to the cellulose fiber and polyolefin fiber described above, such as an elastomer or binder component described below. When the binder component is contained, the content of the binder component is preferably 0.1% by mass or more and 40% by mass or less, more preferably 0.3% by mass or more and 30% by mass or less, even more preferably 0.4% by mass or more and 20% by mass or less, and even more preferably 0.5% by mass or more and 10% by mass or less, based on the total mass of the fiber assembly. By setting the content of the binder component within the above range, the handleability and the like during the production of a molded product can be improved. Examples of binder components that can be used include various starches, casein, sodium alginate, hydroxyethyl cellulose, carboxymethyl cellulose, acrylic resins, styrene-(meth)acrylic acid ester copolymer resins, urethane resins, polyvinyl alcohol (PVA) resins, cellulose derivatives, sodium polyacrylate, polyacrylamide, polyvinylpyrrolidone, acrylamide-acrylic acid ester-methacrylic acid ester copolymers, styrene-maleic anhydride copolymer alkali salts, isobutylene-maleic anhydride copolymer alkali salts, polyvinyl acetate resins, vinyl chloride-vinyl acetate copolymers, ethylene-vinyl acetate copolymers, and the like.
[0040] The fiber assembly may further contain fillers, papermaking chemicals, and fatty acid metal salts. Examples of the filler include mineral pigments such as kaolin, calcined kaolin, calcium carbonate, calcium sulfate, barium sulfate, titanium dioxide, talc, zinc oxide, alumina, magnesium carbonate, magnesium oxide, silica, white carbon, bentonite, zeolite, sericite, and smectite, as well as organic pigments such as polystyrene-based resins, urea-based resins, melamine-based resins, acrylic-based resins, and vinylidene chloride-based resins. Examples of papermaking chemicals include paper strength enhancers, retention improvers, drainage improvers, dyes, fluorescent whitening agents, pH adjusters, defoamers, pitch control agents, slime control agents, etc. Examples of paper strength enhancers include polyacrylamide, etc. Furthermore, wet strength enhancers can also be used in combination, such as polyamide resins, melamine-formaldehyde resins, urea-formaldehyde resins, polyamide-polyamine-epichlorohydrin resins, and polyethyleneimine resins.
[0041] The fatty acid metal salt is preferably a metal salt of an aliphatic carboxylic acid, and the aliphatic carboxylic acid is preferably a saturated aliphatic carboxylic acid or an unsaturated aliphatic carboxylic acid having 12 to 24 carbon atoms, and specific examples thereof include lauric acid, myristic acid, pentadecylic acid, palmitic acid, margaric acid, stearic acid, arachidic acid, heneicosylic acid, behenic acid, lignoceric acid, cerotic acid, montanic acid, melissic acid, myristoleic acid, palmitoleic acid, sapienic acid, oleic acid, and elaidic acid. Examples of metal elements that form metal salts include Group 1 elements (alkali metals) such as sodium and potassium; Group 2 elements (alkaline earth metals) such as calcium, magnesium and barium; and Group 3 elements such as zinc and aluminum, with calcium, magnesium, zinc and aluminum being preferred. Examples of fatty acid metal salts include magnesium stearate, calcium stearate, zinc stearate, barium stearate, aluminum stearate, lithium stearate, zinc laurate, and barium laurate. Among these, from the viewpoint of excellent bending rigidity and impact resistance, calcium stearate, magnesium stearate, zinc stearate, aluminum stearate, calcium oleate, magnesium oleate, zinc oleate, aluminum oleate, zinc laurate, and calcium laurate are preferred, and calcium stearate is more preferred. From the viewpoint of bending rigidity and impact resistance, the content of fatty acid metal salt in the molded body is 0.1 mass% or more and 10 mass% or less, preferably 0.3 mass% or more, more preferably 0.5 mass% or more, even more preferably 0.8 mass% or more, and preferably 9 mass% or less, more preferably 8 mass% or less, even more preferably 7 mass% or less, and even more preferably 6 mass% or less.
[0042] When other components are contained, the content of the other components excluding cellulose fibers and polyolefin fibers is preferably 0.1 mass% or more and 40 mass% or less, more preferably 0.3 mass% or more and 30 mass% or less, even more preferably 0.4 mass% or more and 20 mass% or less, and even more preferably 0.5 mass% or more and 10 mass% or less, relative to the total mass of the fiber assembly.
[0043] [Fiber assembly manufacturing process] Next, the manufacturing process of the fiber assembly will be described. In the following description of the manufacturing process of the fiber assembly, the description will be made assuming that polyolefin fiber, which is considered to be preferable, is used as resin A. When a resin other than polyolefin fiber is used as resin A, the resin used will be read as above instead of polyolefin fiber, and the other description will be the same. Note that resin A can be used alone or in combination of two or more types, as described later.
[0044] In step 1 of the present embodiment, which is a process for producing a fiber assembly, cellulose fibers and resin A are produced by dry papermaking. The manufacturing process of the fiber assembly preferably includes a process of mixing cellulose fibers and polyolefin fibers in air and depositing the mixture. That is, the fiber assembly of the present embodiment is preferably a dry nonwoven fabric.
[0045] When manufacturing a fiber aggregate using a dry papermaking method, it is preferable to adopt an airlaid method. The airlaid method is a method in which an airflow containing raw fibers, such as polyolefin fibers and cellulose fibers defibrated in the air and mixed uniformly in the airflow, is discharged onto a mesh-like endless belt equipped with a suction box on the lower side to form an airlaid web. That is, the airlaid method is a method including a step of mixing cellulose fibers and polyolefin fibers in the air and depositing them. In the airlaid method, the above operation may be repeated multiple times as necessary.
[0046] The web formed by the above method is made into a sheet by a fiber bonding process as described below. For example, the fiber bonding process includes a method of forming a sheet by entangling polyolefin fibers or cellulose fibers with each other by passing needles perpendicularly to the web surface, such as a needle punching method. Such a bonding process is preferably used in combination with a web forming method by a carding method. In addition, the fiber bonding process may employ a process of bonding raw fibers by fusing a heat-fusible adhesive blended in a dry method web by heating (thermal bond method), a process of applying an adhesive to the obtained dry method web to bond raw fibers (chemical bond method), or a method combining the thermal bond method and the chemical bond method (multi-bond method).
[0047] In the thermal bonding method, it is preferable to heat at a temperature 20° C. higher than the melting point of the heat-fusible adhesive. Examples of the heat treatment include hot air treatment and hot pressure treatment at low pressure after hot air treatment.
[0048] When the thermal bond method or the multi-bond method is employed, it is preferable to use a particulate or fibrous heat-sealing adhesive, which may be the polyolefin fiber or binder component described above. As the particulate heat-fusible adhesive, heat-fusible resin particles such as polyethylene, polypropylene, polyester low-melting polyethylene terephthalate, low-melting polyamide, low-melting polylactic acid, polybutylene succinate, etc. are used. Examples of fibrous heat-fusible adhesives that can be used include low-melting polyethylene terephthalate, low-melting polylactic acid, polybutylene succinate (PBS), polyethylene terephthalate (PET), and other polyesters, low-melting polyamides, acrylic resins, and polyvinyl acetate (PVAc) resins. Also, as the heat-fusible synthetic fiber, a heat-fusible composite synthetic fiber having a core-sheath structure, which is obtained by combining two types of resins with different melting points and in which only the surface of the fiber melts, can be preferably used. The heat-fusible composite synthetic fiber having a core-sheath structure has a structure in which a sheath made of a resin with a low melting point is formed on the outer periphery of a core made of a resin with a high melting point. Specifically, examples include a form in which two types of resins with different melting points are combined (PET / PET composite fiber, PE / PET composite fiber, MAPE / PP composite fiber, PP / PET composite fiber, PE / PP composite fiber, PVAc / PET composite resin).
[0049] In addition, when a chemical bond method is used to bond the fibers, it is preferable to add a binder component to fix the fibers together. The binder component can be appropriately selected as needed, and for example, a solution type binder such as starch, casein, sodium alginate, hydroxyethyl cellulose, sodium carboxymethyl cellulose, polyvinyl alcohol (PVA), and sodium polyacrylate, and an emulsion type binder such as polyacrylic acid ester, acrylic styrene copolymer, polyvinyl acetate, ethylene vinyl acetate copolymer, acrylonitrile butadiene copolymer, methyl methacrylate butadiene copolymer, urea-melamine resin, and styrene-butadiene copolymer resin can be used. It is also preferable to use the above-mentioned binder component. The above-mentioned binder can be in various forms such as fiber, powder, granule, solution, or emulsion, and two or more types can be used in combination.
[0050] In the fiber aggregate produced by the above-mentioned dry papermaking method, the fibers constituting the fiber aggregate are three-dimensionally oriented randomly in the longitudinal, transverse and thickness directions. Therefore, in this embodiment, the tensile strength of the fiber aggregate in the first direction and the tensile strength in the second direction are approximately the same. That is, in this embodiment, a fiber aggregate having excellent isotropy in the planar direction is obtained.
[0051] In the manufacturing process of the fiber assembly, any sheet that does not impair moldability may be laminated on the fiber assembly to manufacture a laminated sheet. For example, any sheet may be laminated on the surface of the fiber assembly or between sheets when laminating the fiber assembly. As the any sheet to be laminated, a sheet such as tissue or nonwoven fabric can be used. These any sheets are laminated for the purpose of improving the surface properties of the fiber assembly or the cellulose fiber-containing resin sheet in the manufacturing process, improving productivity, and imparting other functions.
[0052] <Process 2> Step 2 is a cellulose fiber-containing resin sheet production step in which a cellulose fiber-containing resin sheet is produced by compressing the fiber aggregate obtained in step 1. By compressing the fiber aggregate obtained in step 1, a sheet-shaped cellulose fiber-containing resin sheet is obtained. The compression may be carried out simultaneously with the heat treatment or after the heat treatment.
[0053] Compression of the fiber aggregate can be achieved by pressing the fiber aggregate with a roll press. In addition, heating may be performed simultaneously during the roll press treatment to perform a heat and pressure treatment. The roll press treatment can be performed by pressing with a metal roll or a resin roll, so that the density of the resulting cellulose fiber-containing resin sheet can be controlled as desired. Specifically, the number of rolls used for the roll press treatment can be set to any desired number, temperature, and clearance, and the sheet can be heated and pressed to obtain a cellulose fiber-containing resin sheet of any desired density. The sheet may be compressed to a desired density by passing through multiple rolls.
[0054] Compression of the fiber assembly can also be achieved by pressure treatment using a hot press. The density of the resulting cellulose fiber-containing resin sheet can be controlled as desired by pressure treatment using an autoclave method or a mold press method on a fiber assembly cut to an appropriate size or a cellulose fiber-containing resin sheet that has been subjected to the above-mentioned roll press treatment. By heating to a temperature of 100°C or higher and applying pressure to 2 MPa or higher, a cellulose fiber-containing resin sheet with a higher density than that obtained by pressure treatment using a roll press can be obtained. In addition, a pre-pressing step may be included before obtaining the above heating and pressing conditions, and it is also preferable to carry out pre-pressing at a lower pressure under the desired heating conditions, and then increase the pressure and carry out a pressing treatment by hot pressing.
[0055] The pressurizing process by hot pressing may be a stamping molding method. In the stamping molding method, a fiber assembly is heated in advance, and the polyolefin is placed in a melted and softened state inside a mold, and then the mold is closed to clamp the assembly, and then the assembly is pressurized and cooled. For heating, a heating device such as a far-infrared heater, a heating plate, a high-temperature oven, or a dielectric heater may be used.
[0056] The pressure treatment step by hot pressing may be a vacuum molding method. In the vacuum molding method, the space between the fiber assembly and the mold is made vacuum, thereby increasing the adhesion between the fiber assembly and the mold and improving moldability. The vacuum molding is preferably performed in the mold clamping step of the stamping molding method described above. Specifically, the fiber assembly is heated, the polyolefin is melted and softened, and placed inside the mold, and then the mold is closed and clamped to perform vacuum molding. In the vacuum molding, vacuum suction is performed from the mold side. The molding pressure in the vacuum molding is usually 1.0 kg / cm. 2 The molding is carried out in about 0.1 to 60 seconds.
[0057] The pressure treatment step by hot pressing may be a pressure molding method. In the pressure molding method, compressed air is blown onto the fiber assembly to make it adhere to the mold, thereby increasing the adhesion between the fiber assembly and the mold. The pressure molding is preferably performed in the mold clamping step of the stamping molding method described above. Specifically, the fiber assembly is heated, and the polyolefin is placed in a molding die in a melted and softened state, and then compressed air is blown onto the fiber assembly side to perform molding. Pressure molding is performed at a pressure of 3 kg / cm. 2 More than 8kg / cm 2 The compressed air pressure is often as follows, and molding is preferably carried out for 0.1 to 60 seconds.
[0058] Compression of the fiber assembly can also be achieved by a supercalendering process. In the supercalendering, the fiber aggregate is molded by passing it between heated rollers while applying nip pressure. The heating temperature of the rollers used is preferably 10° C. or higher, more preferably 20° C. or higher, and even more preferably 30° C. or higher than the melting point of the polyolefin fiber, and is preferably 100° C. or lower, more preferably 90° C. or lower, and even more preferably 80° C. or lower than the melting point of the polyolefin fiber. The nip pressure is preferably 100 kg / cm or more, more preferably 150 kg / cm or more, and even more preferably 200 kg / cm or more, and is preferably 450 kg / cm or less, more preferably 400 kg / cm or less, and even more preferably 350 kg / cm or less. The number of nip stages is preferably 1 stage or more, more preferably 3 stages or more, and even more preferably 5 stages or more, and is preferably 20 stages or less, more preferably 18 stages or less, and even more preferably 16 stages or less. When compressing the fiber assembly to produce a cellulose fiber-containing sheet, a plurality of cellulose fiber-containing sheets may be appropriately laminated and compressed depending on the desired thickness of the cellulose fiber-containing sheet, etc.
[0059] In this embodiment, the cellulose fiber-containing resin sheet preferably has a T / Y ratio of 0.5 to 1.5, where T is the tensile strength in a first direction and Y is the tensile strength in a second direction perpendicular to the first direction. By setting the T / Y ratio at 0.5 to 1.5, the fibers constituting the cellulose fiber-containing resin sheet are mixed extremely uniformly, and thus a molded product having excellent impact resistance in addition to bending rigidity and strength can be obtained, which is preferable. T / Y is preferably 0.60 or more, more preferably 0.70 or more, even more preferably 0.80 or more, still more preferably 0.85 or more, and is preferably 1.40 or less, more preferably 1.30 or less, even more preferably 1.20 or less, and still more preferably 1.15 or less. The first direction of the cellulose fiber-containing resin sheet is any one direction in the planar direction of the cellulose fiber-containing resin sheet. However, when the fibers contained in the cellulose fiber-containing resin sheet are oriented in any direction in the planar direction, the orientation direction is defined as the first direction. In addition, when the flow direction in the manufacturing process of the fiber aggregate by dry papermaking is known, the flow direction is defined as the first direction. When the flow direction in the manufacturing process of the fiber aggregate is known, the flow direction in the manufacturing process is called the first direction (MD direction), and the flow direction in the obtained fiber aggregate and cellulose fiber-containing resin sheet is sometimes called the T-grain. The second direction of the fiber assembly is one direction in the planar direction of the fiber assembly and is a direction perpendicular to the first direction. When the flow direction in the manufacturing process of the fiber assembly is known, the direction perpendicular to the flow direction in the manufacturing process is called the second direction (CD direction), and the second direction in the obtained fiber assembly and cellulose fiber-containing resin sheet is sometimes called Y direction. The tensile strength of the cellulose fiber-containing resin sheet in the first and second directions is measured in accordance with JIS P 8113: 2006. The tensile strength in each direction is measured using a 15±0.1 mm × 180±1 mm strip at a speed of 20±5 mm / min using a Tensilon tensile tester manufactured by A&D Co., Ltd.
[0060] In this embodiment, the cellulose fiber-containing resin sheet is a sheet-shaped product obtained by mixing at least cellulose fibers and resin A (preferably polyolefin fibers) and then dry-pressing the mixture. The sheet is obtained by pressing a cotton-like fiber aggregate (hereinafter also referred to as a cotton-like fiber aggregate) after dry-pressing, and may have various bulk specific gravities (densities). The bulk density of the cellulose fiber-containing resin sheet to be fed to the screw-type kneader is preferably 0.10 g / mL or more, more preferably 0.15 g / mL or more, from the viewpoints of ease of compression in step 2, ease of subsequent melt-kneading, ease of cutting when cutting for feeding to the melt-kneader, etc., and is preferably 0.60 g / mL or less, more preferably 0.50 g / mL or less, and even more preferably 0.40 g / mL or less. The bulk density of the cellulose fiber-containing resin sheet is measured by the method described in the Examples.
[0061] <Process 3> Step 3 is a cellulose fiber-containing resin pellet production step in which the cellulose fiber-containing resin sheet is melt-kneaded to produce cellulose fiber-containing resin pellets (hereinafter, also simply referred to as "pellets"). From the viewpoint of facilitating feeding to a melt kneader before melt kneading, it is preferable to cut, crush, or the like the cellulose fiber-containing resin sheet before feeding it into the melt kneader. The cutter is not particularly limited, and examples thereof include a shredder. The size of the material after cutting, crushing, etc. is not particularly limited as long as it is a size that can be fed into a mold kneader.
[0062] The method for producing the pellets is not particularly limited, and it is sufficient to supply a cellulose fiber-containing resin sheet and melt-knead it, and is not particularly limited. Examples of the device used for melt kneading include a single screw extruder, a twin screw extruder, a kneader, a Banbury mixer, a mixing roll mill, an open roll mill, and a glass mixer. After supplying a cellulose fiber-containing resin sheet and melt kneading it, (1) A method in which the resin is extruded into a strand shape and then cooled and solidified to obtain cellulose fiber-containing resin pellets; (2) A method in which the molten mixture is cooled and solidified as it is or after being stretched into a sheet, and then crushed in a crusher to obtain cellulose fiber-containing resin pellets. (3) A method in which the resin is extruded into a rod or cylinder and cooled to obtain cellulose fiber-containing resin pellets. (4) A method in which a cellulose fiber-containing resin is extruded through a T-die to obtain a sheet or film-like cellulose fiber-containing resin, and then cut or crushed to obtain cellulose fiber-containing resin pellets; or (5) A method in which the molten kneaded product immediately after extrusion is cut with a rotary blade in air or water to obtain cellulose fiber-containing resin pellets. Examples include:
[0063] The size of the pellets obtained in step 3 is not particularly limited, but is preferably 1 to 10 mm from the viewpoint of ease of insertion into an injection molding machine.
[0064] The melt-kneading temperature (barrel set temperature) is not particularly limited, but it is preferable to adjust the barrel set temperature so that the temperature of the molten kneaded product (the temperature of the actually obtained kneaded product, the resin temperature) is at least 5°C higher than the melting point of the polyolefin, more preferably at least 10°C higher, and even more preferably at least 15°C higher.From the viewpoint of deterioration of the cellulose fibers, it is preferable that the barrel set temperature is not more than 100°C higher than the melting point of the polyolefin, more preferably not more than 90°C higher, and even more preferably not more than 80°C higher. The temperature of the melt-kneaded product is higher than the melt-kneading temperature (barrel set temperature) due to shear heat generated during melt-kneading. That is, it varies depending on various conditions during melt-kneading, such as the melt-kneading temperature (barrel set temperature), discharge speed, rotation speed, and screw design of the melt-kneader. In the case of the method described in the examples, the temperature of the melt-kneaded product is higher by about 20 to 40°C than the melt-kneading temperature (barrel set temperature), so the melt-kneading temperature (barrel set temperature) is lower by about 20 to 40°C than the preferred temperature of the melt-kneaded product.
[0065] Various conditions during melt kneading, such as the discharge speed and rotation speed, may be adjusted according to known techniques. When the device used for melt kneading is a twin-screw extruder, it is desirable to design the screw so that the kneading force is as weak as possible. In the present invention, the cellulose fibers and resin A are uniformly dispersed in the cellulose fiber-containing resin sheet in advance, and even if melt kneading is performed without applying high shear force, the dispersion state of the cellulose fibers in the cellulose fiber-containing resin sheet is maintained as it is, and pellets with excellent dispersion of the cellulose fibers are obtained. Therefore, by using a weak kneading force, cutting of the cellulose fibers can be avoided. Specifically, the kneading parts mainly use R-type kneading parts, and it is preferable that the number of L-type and N-type kneading parts is the same as or less than the number of R-type kneading parts, and it is even more preferable that the number is less than the number of R-type kneading parts. The kneading parts are preferably 5 or less, and more preferably 3 or less, out of the 10 parts into which the entire screw is divided.
[0066] In step 3, a resin component may be further blended and melt-kneaded together with the cellulose fiber-containing resin sheet, and the resin component is preferably a polyolefin resin or the above-mentioned elastomer. By blending at least one selected from a polyolefin resin and an elastomer in step 3, a molded product having superior impact resistance can be obtained, which is preferable. That is, the obtained cellulose fiber-containing resin pellets contain the components blended in step 3 in addition to the components derived from the cellulose fiber-containing resin sheet.
[0067] The elastomer that may be blended in the melt kneading refers to a polymeric compound that exhibits elastic deformation, and refers to a substance that has the property of softening and becoming fluid when heated and returning to a rubber-like state when cooled. Specifically, elastomers have a structure consisting of two polymers, hard segments and soft segments, where the hard segments act as cross-linking points and the soft segments exhibit rubber elasticity, resulting in elasticity. Therefore, at room temperature, the hard segments gather together to form a pseudo-cross-linked state, exhibiting rubber-like physical properties, but at high temperatures they melt, losing the function of the cross-linking points and allowing plastic deformation. Depending on the combination of hard segment polymers and soft segment polymers, they are classified into polystyrene-based, olefin / alkene-based, polyester-based, polyvinyl chloride-based, polyurethane-based, polyamide-based, polyacrylic elastomers, silicone-based, polyimide-based, etc. Even within the same system, the characteristics differ depending on the ratio of hard and soft segments and the molecular weight. For example, polystyrene-based elastomers use styrene in the hard segment and butadiene in the soft segment. In this case, a large amount of styrene results in high hardness and improved compatibility with polystyrene and polyphenylene ether, while a small amount of styrene results in low hardness, high flexibility, and improved compatibility with polyolefins. In addition, a high molecular weight improves temperature characteristics and mechanical properties, while a low molecular weight improves processability and transparency. Examples of polystyrene-based elastomers include the Tuftec series manufactured by Asahi Kasei Corporation. For example, there is an olefin / alkene-based elastomer that combines ethylene, propylene, and 1-butene. The density, elastic modulus, and melting point can be changed by changing the combination and ratio. The structure when mixed with resin also differs, and it may be dispersed like islands in the sea or may be compatible. An example of an olefin / alkene-based elastomer is the Toughmer series manufactured by Mitsui Chemicals, Inc. Among these, polystyrene-based elastomers and olefin / alkene-based elastomers are preferred from the standpoint of impact resistance and the like. Examples of the elastomer include various elastomers described in paragraphs 0043 to 0065 of REP.2020 / 080328. The method for adding the elastomer is not particularly limited, and it is preferable to supply the elastomer together with the cellulose fiber-containing resin sheet during melt-kneading of the cellulose fiber-containing resin sheet, and then melt-knead the elastomer.
[0068] When the cellulose fiber-containing resin pellets contain the elastomer, the content of the elastomer is preferably 55% by mass or less, more preferably 50% by mass or less, even more preferably 45% by mass or less, still more preferably 40% by mass or less, and particularly preferably 35% by mass or less, based on the total mass of resin A and the elastomer, from the viewpoint of improving the flexural modulus. Also, when the cellulose fiber-containing resin pellets contain the elastomer, the content of the elastomer is preferably 5% by mass or more, more preferably 8% by mass or more, even more preferably 10% by mass or more, still more preferably 12% by mass or more, and particularly preferably 15% by mass or more, based on the total mass of resin A and the elastomer, from the viewpoint of improving the impact resistance.
[0069] <Step 4> Step 4 is a step of molding the cellulose fiber-containing resin pellets obtained in step 3. In addition, various molding methods are adopted in the molding process, for example, injection molding (e.g., injection compression molding (press injection, hot flow stamping molding, gas injection compression molding), gas injection molding, and ultra-high speed injection molding), various extrusion moldings (cold runner method or hot runner method), compression (press) molding, insert molding, in-mold coating molding, heat-insulating mold molding, rapid heating and cooling mold molding, various profile extrusion moldings (e.g., two-color molding and sandwich molding), etc. can be exemplified. For example, various extrusion moldings are suitable for molding sheets, films, fibers, etc. Inflation method, calendar method, casting method, etc. can also be used for molding sheets or films. Furthermore, a specific stretching operation may be applied. It is also possible to make a hollow molded product by rotational molding or blow molding, etc. In addition, a plurality of molding steps may be combined, or a plurality of steps may be simultaneously performed as one step. For example, the cellulose fiber-containing resin pellets may be formed into a sheet and then heat-pressed to obtain a molded product, or the cellulose fiber-containing resin pellets may be formed into a sheet and then supercalendered to obtain a molded product. After forming into a sheet, the product may be molded by vacuum forming, compressed air forming, or the like. Among these, injection molding is a preferred example.
[0070] When the molding step is an injection molding step, the injection molding step involves, for example, melt-kneading the above-mentioned cellulose fiber-containing resin pellets using a known injection molding machine, and injecting the molten mixture into a mold to perform molding. When melt-kneading, a known kneading machine may be used, for example, a single-screw kneading machine or a twin-screw kneading machine. Examples of known injection molding machines include screw type injection molding machines, screw pre-plasticizing type injection molding machines, plunger pre-plasticizing type injection molding machines, plunger type injection molding machines, etc. Examples of the drive system include hydraulic, electric, and hydraulic-electric hybrid systems.
[0071] The temperature conditions for injection molding are appropriately determined depending on the type of resin contained in the pellets, and it is preferable to set the cylinder temperature of the injection molding machine to a temperature 0 to 100° C. higher than the flow start temperature of the resin used. The temperature of the mold may be appropriately selected from the viewpoints of the cooling rate and productivity of the resin used. For example, in the case of polyolefin, it is preferable to set the temperature within the range of room temperature (eg, 23°C) to 120°C. Other injection conditions such as the screw rotation speed, back pressure, injection speed, pressure holding, and pressure holding time may be appropriately adjusted.
[0072] The cellulose fiber-containing resin pellets of the present embodiment may contain other resins such as elastomers by adding other resins, for example elastomers, during molding and melt-kneading the mixture. In the manufacturing process of the molded article, other resins, various additives, masterbatches containing various additives, etc. may be added in addition to the cellulose fiber-containing resin pellets during injection molding. The additives include those typically used in resin compositions, such as stabilizers, ultraviolet absorbers, plasticizers, flame retardants, flame retardant assistants, antistatic agents, surfactants, colorants, lubricants, and mold release agents. The stabilizers include, for example, hindered phenols, hydroquinone, phosphites and substituted versions thereof. Examples of ultraviolet absorbers include resorcinol, salicylate, benzotriazole, and benzophenone. Colorants include materials including dyes, such as nitrosine, and pigments, such as cadmium sulfide, phthalocyanines, and carbon black. Examples of the lubricant include fatty acids such as stearic acid and montanic acid, their amides, their esters, their half esters with polyhydric alcohols, stearyl alcohol, stearamide, polyethylene wax, and paraffin wax.
[0073] [Method of manufacturing a resin molded product containing recycled cellulose fibers] We will explain as an example a method for producing a recycled cellulose fiber-containing resin molded body (molded body (recycled n+1 times)) by recycling a molded body (recycled nth time), but the same applies to the production of a molded body (initial) and a molded body (recycled 1st time). When recycling the molded body (recycled n-th time), it is preferable to pulverize the molded body (recycled n-th time). The pulverization is not particularly limited as long as it can be pulverized to a size that can be fed to an injection molding machine or a kneading machine, and various pulverizers may be appropriately selected. If necessary, before pulverizing the molded body (n-th recycling), a cleaning step or removal of unnecessary parts may be performed. The pulverized material is preferably molded as it is, and more preferably injection molded as it is. The recycled cellulose fiber-containing resin molded body (recycled n+1 times) of this embodiment is obtained by molding the pulverized material of the cellulose fiber-containing resin molded body (recycled n times) as it is in the same manner as the molded body (recycled n times).
[0074] In actual recycling, various aspects as shown below may be adopted. 1. In addition to the crushed product of the molded body (recycled n-th time), one or more of the following is supplied to the molding machine and molded: cellulose fiber-containing resin pellets newly obtained from a cellulose fiber-containing resin sheet; and when n is 2 or more, crushed product of the molded body (recycled nm-th time). Here, m is a natural number smaller than n. 2. The ground compact (nth recycling) is fed to a kneader to produce pellets, which are then molded. 3. In addition to the pulverized product of the molded body (recycled n-th time), at least one of newly cut pieces of a cellulose fiber-containing resin sheet, cellulose fiber-containing resin pellets obtained from a cellulose fiber-containing resin sheet, and, when n is 2 or more, pulverized product of a molded body (recycled nm-th time) is added to produce pellets, and then the pellets are molded, where m is a natural number smaller than n. 4. Various components are further added to the molding machine or kneader to satisfy the physical properties required for the molded body (recycle n+1). In actual recycling, a combination of the above-mentioned modes may be adopted. For example, a method of combining 3. and 4., in which a cut piece of a cellulose fiber-containing resin sheet and the above-mentioned elastomer are added to the crushed molded body (recycled n-th time), to produce pellets, and then the pellets are molded, may be mentioned.
[0075] (Application) The molded article of the present embodiment is preferably used for electrical and electronic equipment, office automation equipment, home appliances, civil engineering and construction, automobiles, aircraft parts, structural parts and housings, containers (e.g., food containers, drug packaging containers, cosmetic packaging containers, medical device packaging containers), furniture, daily necessities, medical tools, etc. Among these, it is suitable for applications requiring impact resistance, such as civil engineering and construction, automobile or aircraft parts, structural parts, and housings. EXAMPLES
[0076] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.
[0077] Example 1 <Preparation of fiber assembly> NBKP was defibrated using a swirling jet airflow defibrator to obtain defibrated dry pulp. The air speed in the defibrator was 45 m / min, and turbulence was achieved using a baffle installed in the device. The average fiber length of the obtained defibrated dry pulp was 2.38 mm, the average fiber width was 34.3 μm, and the fine fiber ratio was 11.4%.
[0078] Next, the obtained defibrated dry pulp, polypropylene fiber (melting point 160°C, fineness 6.6 dtex, fiber length 5 mm, fiber diameter 30 μm, also referred to as PP fiber), and polyethylene / polypropylene composite core-sheath fiber (core melting point 160°C, sheath melting point 110°C, fineness 1.7 dtex, fiber length 5 mm, fiber diameter 15 μm, also referred to as PE / PP composite fiber) were uniformly mixed in a ratio (mass ratio) of 30 / 55 / 15 using an air flow to obtain a fiber mixture.
[0079] Next, an airlaid web was formed from the fiber mixture using the web forming apparatus 1 shown in FIG. 1. Specifically, a first carrier sheet 41 was fed by a first carrier sheet supplying means 40 onto an air permeable endless belt 20 that was attached to a conveyor 10 and running. In Example 1, tissue (basis weight 14 g / m) was used as the first carrier sheet 41. 2 The "basis weight" was measured according to "Paper and paperboard - Method of measurement of basis weight" described in JIS P8124:2011.
[0080] While sucking the air-permeable endless belt 20 with the suction box 60, the fiber mixture was dropped and deposited on the first carrier sheet 41 together with the air flow from the fiber mixture supplying means 30, to obtain a cotton-like fiber aggregate. At that time, the basis weight (set basis weight) of the air-laid web portion was 400 g / m 2 The fiber mixture was supplied so that
[0081] Next, a second carrier sheet 51 was laminated on the cotton-like fiber assembly on the first carrier sheet 41 by a second carrier sheet supplying means 50 to obtain a fiber assembly containing an air-laid web. In Example 1, tissue (basis weight 14 g / m2) was used as the second carrier sheet 51. 2 That is, in Example 1, the same sheet was used for first carrier sheet 41 and second carrier sheet 51.
[0082] <Preparation of cellulose fiber-containing resin sheet> The resulting fiber assembly containing the airlaid web was passed through a box-type dryer with a hot air circulation conveyor oven system and subjected to hot air treatment at a temperature of 140°C. The density was then adjusted by roll press treatment so that the bulk specific gravity was 0.3 g / mL, and the basis weight was 449.5 g / m 2 The cellulose fiber-containing resin sheet had a T / Y of 0.88, a bulk density of 0.29 g / mL, and a thickness of 1.55 mm. The cellulose fiber-containing resin sheet was cut with a shredder (AFS100M, manufactured by Iris Ohyama Corporation) to obtain cut chips of about 4 mm×13 mm.
[0083] <Preparation of Molded Product of the Present Embodiment> The cut chips were fed to a twin-screw kneading extruder (Parker Corporation, HK-25D (41D)) and melt-kneaded and dispersed at a kneading temperature of 180°C and an output of 2.5 kg / hour. The screw used for kneading was a weak kneading configuration consisting of a 6-part kneading part used only in the 5th part counting from the raw material inlet side, out of the 7 parts divided into the entire screw. All the kneading parts were R type. After melt-kneading and dispersion, the mixture was air-cooled to produce pellets. The pellets were injection molded into a type A1 multipurpose test piece specified in JIS K 7139:2009 at a molding temperature of 170°C and an injection speed of 30 mm / sec, to obtain a cellulose fiber-containing resin molded body (initial) having a thickness of 4 mm.
[0084] Example 2 A cellulose fiber-containing resin molded body (initial) having a thickness of 4 mm was obtained in the same manner as in Example 1, except that in <Preparation of fiber aggregate> in Example 1, the fiber mixture was changed to a ratio (mass ratio) of 50 / 35 / 15, the discharge amount was changed to 3.0 kg / hour, and in <Preparation of molded body of this embodiment>, the molding temperature was changed to 180° C. The basis weight of the cellulose fiber-containing resin sheet before obtaining the cut chips was 438.9 g / m 2 , T / Y was 0.88, bulk density was 0.33 g / mL, and thickness was 1.33 mm.
[0085] Comparative Example 1 A type A1 multipurpose test piece as specified in JIS K 7139:2009 was injection molded using pellets of glass fiber reinforced polypropylene (Prime Polypro R-200G, manufactured by Prime Polymer Co., Ltd.) containing 20% by mass of glass fiber at a molding temperature of 220°C and an injection speed of 100 mm / sec to obtain a glass fiber-containing resin molded body (initial state) having a thickness of 4 mm.
[0086] <Preparation of molded bodies for evaluating recyclability> A portion of the initial molded products obtained by the methods of the above examples and comparative examples was crushed using a single-axis low-speed crusher (SCUTTER SX-250-T, manufactured by Stolz Co., Ltd.) and then injection molded under the conditions of each example and comparative example to obtain cellulose fiber-containing resin molded bodies and glass fiber-containing resin molded bodies for the first recycling cycle. A portion of this first recycled molded product was crushed using a single-axis low-speed crusher (SCUTTER SX-250-T, manufactured by Stolz Co., Ltd.) and then injection molded under the conditions of each example and comparative example to obtain a second recycled cellulose fiber-containing resin molded body and a glass fiber-containing resin molded body.
[0087] <Measurement and Evaluation> (Method of measuring fiber length and diameter of polyolefin fibers) Twenty randomly selected polyolefin fibers were observed under an optical microscope and the fiber length and fiber diameter were measured.
[0088] (Method of measuring average fiber length, average fiber diameter, and fine fiber ratio of cellulose fibers) The average fiber length and average fiber diameter of cellulose fibers were measured using a fiber image analyzer (Valmet FS5, manufactured by Valmet Ltd.) in accordance with ISO16065-2. The ratio of fine fibers with a length of 0.1 mm or less in the measured length-weighted average fiber length distribution was defined as the fine fiber ratio.
[0089] (Measuring method for melting point of polyolefin fiber) The melting point of the polyolefin fiber may be determined from a catalog value of the polyolefin fiber if such a value is available. In this embodiment, the catalog value was used. If there is no catalog value, it can be measured using the following method. 5 mg of polyolefin fiber is cut out and the melting point of the polyolefin fiber is measured using a differential scanning calorimeter (DSC). The melting point is measured by heating from 30°C to 280°C at 20°C / min under a nitrogen atmosphere using a Diamond DSC manufactured by Perkin-Elmer.
[0090] (Method for measuring bulk density of cellulose fiber-containing resin sheet) The bulk density of the cellulose fiber-containing resin sheet was calculated by measuring the thickness and mass of a 50 mm square sheet after conditioning it for 24 hours under conditions of 23°C and 50% RH. The thickness of the sheet was measured with a digital thickness gauge (DG-127, manufactured by Ozaki Seisakusho Co., Ltd.).
[0091] (Method of measuring T / Y) The flow direction (the running direction of the conveyor 10) in the manufacturing process of the obtained fiber aggregate was defined as the first direction, and the direction perpendicular to the first direction was defined as the second direction, and the tensile strength (unit: N / m) of the cellulose fiber-containing resin sheet was measured in accordance with JIS P 8113:2006. The tensile strength in each direction was divided by the thickness of the test piece to calculate the tensile strength (unit: MPa). A Tensilon manufactured by A&D Co., Ltd. was used as a tensile tester to measure a 15 mm x 180 mm strip at a speed of 20 mm / min.
[0092] (Method of measuring density of molded product) The obtained molded product (molded body) was cut into a rectangular test piece of 80 mm length x 10 mm width. The thickness of the rectangular test piece was measured with a constant pressure thickness measuring device (manufactured by Techclock Corporation, model number PG-02J), and the volume of the rectangular test piece was calculated. Furthermore, the density was calculated by measuring the mass of the rectangular test piece.
[0093] (Method of measuring flexural modulus and flexural strength of molded products) The obtained molded product was cut into a rectangular test piece of 80 mm length × 10 mm width, and a three-point bending test was carried out in accordance with JIS K 7171: 2016. The bending modulus and bending strength obtained were evaluated as being superior in rigidity and strength against bending, respectively, as the values were larger.
[0094] (Method of measuring impact resistance of molded products) The obtained molded product was cut into a rectangular test piece of 80 mm in length x 10 mm in width, and a notched Charpy impact test (strike direction: edgewise) was carried out in accordance with JIS K 7111-1: 2012. The higher the Charpy impact strength value, the better the impact resistance and the stronger the impact resistance.
[0095] [Table 1]
[0096] As shown in the examples, the cellulose fiber-containing resin molded product of the present invention has excellent bending rigidity and also has excellent recyclability. On the other hand, the molded article of Comparative Example 1 was poor in recyclability. [Explanation of symbols]
[0097] 1 Web forming device 10 Conveyor 20 Breathable endless belt 30 Fiber mixture supply means 40 First carrier sheet supply means 41 First Career Sheet 50 Second carrier sheet supply means 51 Second Career Sheet 60 Suction Box
Claims
1. A cellulose fiber-containing resin molded body, The flexural modulus measured in accordance with JIS K 7171:2016 is 2.5 GPa or more, and A recycled cellulose fiber-containing resin molded product obtained by melt-kneading the cellulose fiber-containing resin molded product and molding it again has a bending modulus reduction rate of 10% or less compared to that of the cellulose fiber-containing resin molded product. Cellulose fiber-containing resin molded body.
2. 2. The cellulose fiber-containing resin molded product according to claim 1, wherein the rate of decrease in bending strength of the recycled cellulose fiber-containing resin molded product is 10% or less compared to that of a cellulose fiber-containing resin molded product.
3. 3. The cellulose fiber-containing resin molded body according to claim 1, wherein the recycled cellulose fiber-containing resin molded body has a Charpy impact strength at a thickness of 4 mm that is reduced by 30% or less compared to a cellulose fiber-containing resin molded body.
4. The cellulose fiber-containing resin molded article according to claim 1 or 2, wherein the content of the cellulose fibers is from 10% by mass to 90% by mass.
5. Density is 0.8 g / cm 3 1.5g / cm or more 3 The cellulose fiber-containing resin molded body according to claim 1 or 2, which is as follows:
6. 3. The cellulose fiber-containing resin molded article according to claim 1, having a thickness of 2 mm or more.
7. Charpy impact strength at a thickness of 4 mm measured in accordance with JIS K 7111-1:2012 is 2.0 kJ / m 2 The cellulose fiber-containing resin molded article according to claim 1 or 2.
8. The cellulose fiber-containing resin molding according to claim 1 or 2, wherein the initial cellulose fiber-containing resin molding before the first recycling is a molding obtained by a method including the following steps 1, 2, 3, and 4 in this order. Step 1: A fiber assembly manufacturing step of manufacturing a fiber assembly containing cellulose fibers and resin A by dry papermaking. Step 2: A cellulose fiber-containing resin sheet manufacturing step of compressing the fiber assembly to manufacture a cellulose fiber-containing resin sheet. Step 3: A step of producing cellulose fiber-containing resin pellets by melt-kneading the cellulose fiber-containing resin sheet to produce pellets. Step 4: Molding the cellulose fiber-containing resin pellets
9. The cellulose fiber-containing resin molded body according to claim 8 , wherein the resin A contains resin fibers.
10. The cellulose fiber-containing resin molding of claim 8, wherein T / Y is 0.5 or more and 1.5 or less, where T is the tensile strength of the cellulose fiber-containing resin sheet in a first direction and Y is the tensile strength of the cellulose fiber-containing resin sheet in a second direction perpendicular to the first direction.
11. The cellulose fiber-containing resin molded product according to claim 8, wherein in step 2, the cellulose fiber-containing resin sheet to be subjected to step 3 has a bulk density of 0.10 g / mL or more and 0.60 g / mL or less.
12. The cellulose fiber-containing resin molded body according to claim 8 , wherein the step 4 is a step of injection molding cellulose fiber-containing resin pellets.
Citation Information
Patent Citations
Production of article formed by paper-making process
JP1994322699A
Molding made of biodegradable composite material and its production
JP1994345944A
Production of biodegradable composite paper and sheet
JP1994346399A